Method for highly selectively depositing metal films
The described ALD method using controlled purge times and annealing techniques addresses the challenge of selective metal deposition on patterned substrates, achieving high selectivity and conformal deposition of metals like cobalt and ruthenium, reducing grain boundaries and surface roughness for improved semiconductor performance.
Patent Information
- Application Number
- JP2021531326
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-03
- Filing Date
- 2019-12-03
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2039-12-03
AI Technical Summary
Existing methods for selective metal deposition, particularly at the nanoscale on patterned substrates, face challenges in maintaining selectivity between metal and insulator surfaces due to diffusion of molecularly adsorbed metal precursors, leading to non-selective deposition and the need for high temperatures incompatible with low-k dielectrics.
A method involving atomic layer deposition (ALD) using organometallic precursors and coreactants like formic acid or tert-butylamine, combined with controlled purge times, reduced precursor feed rates, and periodic annealing, to achieve selective deposition of metals such as cobalt and ruthenium on specific surfaces, minimizing unwanted nucleation on insulators.
The method achieves nearly infinite selectivity and superselectivity, reducing grain boundaries and surface roughness, enabling conformal deposition of metals with large grains suitable for via filling and interconnects in semiconductor devices.
Smart Images

Figure 0007561127000001 
Figure 0007561127000002 
Figure 0007561127000003
Abstract
Description
[Technical field]
[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of U.S. Provisional Patent Application No. 62 / 774,695, filed December 3, 2018, which is incorporated by reference in its entirety.
[0002] [Statement regarding Federal Assistance] This invention was made with Government support under Grant No. HR0011-18-3-0004 awarded by the Department of Defense / Defense Advanced Research Projects Agency (DARPA). The United States Government has certain rights in this invention.
[0003] The field of the invention is semiconductor device manufacturing, in particular the highly selective deposition of metal films. Applications of the invention include bottom-up filling of vias, patterning of integrated circuits, application of barrier layers, and formation of seed layers for copper deposition. [Background technology]
[0004] Selective metal deposition is desirable for bottom-up fill for both middle-of-line (MOL or MEOL) and back-end-of-line (BEOL) processing. Successful implementation induces the formation and growth of larger grains, which would be expected to reduce via and line resistance by reducing grain boundaries and reducing surface roughness. In addition, bottom-up growth has the potential to eliminate the need for a nucleation layer on low-k dielectrics (SiCOH) since nucleation occurs only on the bottom surface. Important metals for bottom-up growth include cobalt and ruthenium. Cobalt is particularly important because it is used as a capping layer on Cu to protect it from oxidation [Yang, CC., et al. “Characterization of copper electromigration dependence on selective chemical vapor deposited cobalt capping layer thickness”, IEEE Electron Device Letters 32.4(2011): 560-562], and also in vias below 10 nm where Co is considered a better conductor than Cu because Co has a shorter electron mean free path than Cu and Cu electroplating is problematic in vias below 10 nm [Gall, Daniel, “Electron mean free path in elemental metals”, Journal of Applied Physics 119.8(2016):085101].
[0005] Cobalt atomic layer deposition (ALD) has been previously reported by Charles Winter and coworkers. Klesko, Joseph P., Marissa M. Kerrigan, and Charles H. Winter, “Low Temperature Thermal Atomic Layer Deposition of Cobalt Metal Films”, Chemistry of Materials 28.3 (2016): 700-703 (Non-Patent Document 3); Kerrigan, Marissa M. et al., “Substrate selectivity in the low temperature atomic layer deposition of cobalt metal films from bis(1,4-di-tert-butyl-1,3-diazadienyl)cobalt and formic acid”, The Journal of Chemical Physics 146.5 (2017): 052813 (Non-Patent Document 4); Kerrigan, Marissa M., Joseph P. Klesko, and Charles H. Winter, “Low Temperature, Selective Atomic Layer Deposition of Cobalt Metal Films Using Bis(1,4-di-tert-butyl-1,3-diazadienyl)cobalt and Alkylamine Precursors”, Chemistry of Materials 29.17 (2017): 7458-7466 (Non-Patent Document 5); Winter et al., US9,255,327 (Patent Document 1); Winter et al., US20180265975 (Patent Document 2). Selectivity was not quantified in the study by Winter et al.In the cobalt layer ALD described by Winter et al., it was concluded that HCOOH dissociatively chemisorbed to generate atomic H, which removed the ligand from Co(DAD)2. Other CoALD techniques exist, but they often require elevated temperatures and co-reactants such as O2, which are incompatible with low-k dielectrics such as SiCOH (methyl-terminated porous SiO2) used in mid- and back-of-line processing (MOL and BEOL). Furthermore, for MOL and BEOL, selectivity must be maintained at the nanoscale between the metal growth surface and the insulator. On patterned samples / substrates, selectivity is often limited under the same ALD conditions due to diffusion of molecularly adsorbed metal precursors from reactive to non-reactive surfaces. Therefore, improved methods for selective deposition of metal films at the nanoscale, especially on patterned samples, are needed. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] US9,255,327 [Patent Document 2] US20180265975 [Non-patent literature]
[0007] [Non-Patent Document 1] Yang, CC., et al. “Characterization of copper electromigration dependence on selective chemical vapor deposited cobalt capping layer thickness”, IEEE Electron Device Letters 32.4(2011): 560-562) [Non-Patent Document 2] Gall, Daniel, “Electron mean free path in elemental metals”, Journal of Applied Physics 119.8 (2016): 085101 [Non-Patent Document 3] Klesko, Joseph P., Marissa M. Kerrigan, and Charles H. Winter, “Low Temperature Thermal Atomic Layer Deposition of Cobalt Metal Films,” Chemistry of Materials 28.3 (2016): 700-703 [Non-Patent Document 4] Kerrigan, Marissa M. et al., “Substrate selectivity in the low temperature atomic layer deposition of cobalt metal films from bis(1,4-di-tert-butyl-1,3-diazadienyl)cobalt and formic acid”, The Journal of Chemical Physics 146.5(2017):052813 [Non-Patent Document 5] Kerrigan, Marissa M., Joseph P. Klesko, and Charles H. Winter, “Low Temperature, Selective Atomic Layer Deposition of Cobalt Metal Films Using Bis (1,4-di-tert-butyl-1,3-diazadienyl)cobalt and Alkylamine Precursors,” Chemistry of Materials (2017) 29.17: 7458-7466. Summary of the Invention
[0008] Selective metal deposition is desirable for bottom-up fill for both middle-of-line (MOL or MEOL) and back-end-of-line (BEOL) processes. Successful implementation induces the formation and growth of larger grains, which is expected to reduce via and line resistance by reducing grain boundaries and reducing surface roughness. In addition, bottom-up growth has the potential to eliminate the need for a nucleation layer on low-k dielectrics (SiCOH) since nucleation occurs only on the bottom surface. Important metals for bottom-up growth include cobalt and ruthenium. Cobalt is particularly important because it is used as a capping layer on Cu to protect it from oxidation [Yang, CC., et al. “Characterization of copper electromigration dependence on selective chemical vapor deposited cobalt capping layer thickness”, IEEE Electron Device Letters 32.4(2011):560-562] (Non-Patent Document 1), and also in vias below 10 nm where Co is considered to be a better conductor than Cu [Gall, Daniel, “Electron mean free path in elemental metals”, Journal of Applied Physics 119.8(2016):085101] (Non-Patent Document 2).
[0009] According to one aspect of the invention, a method for atomic layer deposition (ALD) of a metal is provided, the method comprising at least one cycle of a) exposing a substrate to an organometallic precursor, the substrate comprising a surface including metal portions and insulator portions, b) depositing the organometallic precursor onto the surfaces of the metal portions of the substrate to selectively provide a metal precursor layer on the surfaces of the metal portions of the substrate, c) exposing the metal precursor layer to a co-reactant, and d) depositing the co-reactant onto the metal precursor layer, wherein the co-reactant participates in ligand exchange with the metal precursor layer.
[0010] According to another aspect of the present invention, a method for atomic layer deposition (ALD) of metal is provided, the method includes at least one cycle of a) exposing a substrate to a liquid organometallic precursor in a zero oxidation state, the substrate comprising a surface including a metal portion and an insulator portion, b) depositing the liquid organometallic precursor in a zero oxidation state on the surface of the metal portion of the substrate to selectively provide a metal precursor layer on the surface of the metal portion of the substrate, c) exposing the metal precursor layer to a co-reactant, and d) depositing the co-reactant on the metal precursor layer, the co-reactant being formic acid (HCOOH) or tert-butylamine (TBA). It is noted that similar co-reactants such as other organic acids and other organic amines also work.
[0011] According to another aspect of the present invention, there is provided a method for atomic layer deposition (ALD) of metals, comprising at least one cycle of: a) exposing a surface of a substrate to a metal organic precursor comprising cobalt (Co) or ruthenium (Ru), wherein the substrate surface comprises a metal portion comprising copper (Cu) or platinum (Pt) or cobalt (Co) or ruthenium (Ru) or other metal, and an insulator portion comprising SiO2, SiN or SiCOH, b) depositing a metal organic precursor on the surface of the metal portion of the substrate to selectively provide a metal precursor layer on the surface of the metal portion of the substrate, c) exposing the metal precursor layer to a co-reactant, and d) depositing the co-reactant on the metal precursor layer, wherein the co-reactant is formic acid (HCOOH) or tert-butylamine (TBA), and the deposition is performed between about 140° C. and about 230° C. It is noted that similar co-reactants such as other organic acids, other organic amines will work as well. [Brief description of the drawings]
[0012] [Figure 1] XPS of UHV annealed Pt and SiO2 substrates after 100 cycles and then subjected to an additional 100 ALD cycles of Co(DAD)2 + HCOOH at 180 °C. In the case of the Pt substrate, the loss of the Pt signal in the XPS is consistent with a deposited cobalt film with a thickness of more than 10 nm, whereas no cobalt signal is observed on the SiO2, suggesting that no deposition has occurred, consistent with infinite selectivity. [Diagram 2] AFM imaging before and after ALD cycling on SiO2 and Pt. No changes were observed on SiO2, but the Co film on Pt had an RMS surface roughness of less than 2 nm. [Diagram 3] Saturation study of Co(DAD)2 and HCOOH at 180 °C. The self-limiting exposure was consistent with ALD. The increase in C and O after HCOOH feeding was consistent with formate deposition on the surface. The decrease in C and O and the increase in Co after Co(DAD)2 feeding suggested a ligand exchange mechanism for this reaction. [Figure 4]Co2p raw XPS peak. After formic acid addition, a higher binding energy (BE) component is shown, consistent with formate being deposited on the Co surface. This formate is removed after Co(DAD)2 addition. [Figure 5A] CoALD with HCOOH vs TBA on Cu vs SiO2. No attenuation of the substrate Cu signal with HCOOH is consistent with etching of Cu / CuOx. [Figure 5B] CoALD with HCOOH vs. TBA on Cu vs. SiO2. When ALD was performed with TBA, the Cu was completely filled, consistent with it not being etched. [Figure 5C] CoALD with HCOOH vs. TBA on Cu vs. SiO2. 4% CoOx was observed after 50 cycles of Co(DAD)2 + TBA. No additional CoOx was observed after 250 additional ALD cycles, consistent with superselectivity. [Figure 6] Non-selectivity in high temperature deposition with HCOOH. [Figure 7] Strong selectivity when the temperature is reduced to 215°C and HCOOH is used. Significant deposition occurs only on Cu and not on SiO2. [Figure 8] Strong selectivity when temperature is reduced to 215°C and HCOOH is used. AFM on the left shows deposition on Cu (miniature and magnification); consistent with potential etching, larger grains have formed. Need to repeat with TBA. On the right is SiO2, which only shows small nuclei. [Figure 9] Selective deposition with TBA. XPS on SiO2 and passivated SiO2 shows much less deposition after 600 total cycles compared to deposition on Pt samples. A selectivity of approximately 20:1 is seen for Pt vs. SiO2. [Figure 10] AFM showing a smooth film formed on Pt. Left: AFM showing a smooth Ru film formed on Pt. Right: AFM shows the Ru film formed on SiO2, which appears to have more grains, consistent with the selectivity seen in XPS. [Figure 11]Raw XPS Ru 3d peaks on SiO2 and Pt. The raw XPS peaks give further insight into the oxidation state of the deposited Ru. On Pt the oxidation state is consistent with metallic Ru (BE of 279.8 eV), whereas on SiO2 the oxidation state of Ru is more consistent with that of an oxide (BE of 280.3 eV). This allows us to gain insight into the mechanism of selectivity by forming an oxide on the surface that prevents deposition. [Figure 12] 200 cycles of Co(DAD)2+TBA at 180 °C on patterned Cu / SiO2 structures. The Cu strips are grey, the SiO2 areas are black. (Left) After 200 cycles in the non-passivated sample, unwanted Co nuclei are observed near the Co / Cu strips. (Right) In the passivated sample, the density of unwanted nuclei is 4 times lower and more uniform across the SiO2. [Figure 13a] 200 cycles of Co(DAD)2 + TBA at 180 °C on patterned Cu / SiO2 sample. The Cu strips are gray and the SiO2 areas are black. Increasing the pump-out time has a weak effect on the nucleation density. [Figure 13b] 200 cycles of Co(DAD)2+TBA at 180 °C on a patterned Cu / SiO2 sample. The Cu strips are grey, the SiO2 areas are black. The Co(DAD)2 supply was reduced by 4x with each cycle. Note: Selectivity was nearly complete, but the overall growth rate was reduced by 2x. [Figure 14] 200 cycles of Co(DAD)2+TBA at 180 °C on a patterned Cu / SiO2 sample with cyclic anneal at 260 °C. Cu strips are grey and SiCOH areas are black. (Left) Note: Near perfect selectivity. No passivation was employed, only a 5 second pump-out was used, and a saturating Co(DAD)2 feed rate was used to obtain maximum growth rate and conformal deposition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The above and other aspects of the present invention will be described in more detail with respect to other embodiments described herein. It should be understood that the present invention can be embodied in many different forms and should not be construed as being limited to the embodiments described herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the invention to those skilled in the art.
[0014] The terms used in the detailed description of the present invention are intended to describe only certain embodiments and are not intended to limit the present invention. When used in the detailed description of the present invention and the appended claims, the singular form is intended to include the plural form unless the context clearly indicates otherwise. In addition, when used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items and may be abbreviated as " / ".
[0015] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0016] Aspects of the invention provide ALD techniques that allow selective deposition of metals on a first surface or portion of a substrate, e.g., a metal surface, preferentially over a second surface of the substrate, e.g., an insulator surface, such as, but not limited to, a SiO2 surface on the substrate. In some aspects, deposition of metals can be performed, e.g., with Co and Ru, on metals such as Pt, Cu, Co, and / or Ru, with selectivity over insulators, e.g., SiO2 or SiCOH (porous low-k dielectrics), but this mechanism of selectivity can be extended to other metal precursors through co-reactants of formic acid or tert-butylamine (TBA) or related co-reactants such as organic carboxylic acids and organic aminos. In some aspects, the substrate can be an unpatterned substrate. In other aspects, the substrate can be a patterned substrate.
[0017] Embodiments of the present invention provide highly selective Co and Ru metal deposition, e.g., from Co(DAD)2 or Ru(DMBD)(CO)3 metal precursors and two different co-reactants (HCOOH and TBA). In some embodiments, e.g., Co deposition, e.g., Co deposition on Pt or Cu using HCOOH as a co-reactant, no deposition was observed on SiO2, consistent with infinite selectivity on flat samples, but HCOOH was observed to etch Cu. By switching to TBA, no Cu etching was observed and similar metallic Co films were deposited on SiO2 with only 4% CoOx regardless of the number of CoALD cycles. The self-limiting deposition on SiO2 is a novel mechanism of selectivity via the formation of oxide particles, which results in ultraselectivity.
[0018] The number of ALD cycles performed in the methods according to the invention is not particularly limited, and can be as few as 1 cycle, and as many as about 2, 5, 10, 20, 30, 40, 50, 100, 150, 200, 300, 400, 500, 600, 700, 800, 900, up to about 1,000 cycles or more, or any number of cycles in between.
[0019] In an embodiment of the invention, deposition of metals by ALD occurs via ligand exchange that occurs between a metal precursor layer, e.g., a metal surface or portion of a substrate, and a co-reactant. For example, exposing a metal surface or portion of a substrate to a metal precursor, e.g., Co(DAD)2, to deposit / form a metal precursor layer on the substrate, and then exposing the metal precursor layer to a co-reactant, e.g., HCOOH, to deposit the co-reactant on the metal precursor layer, e.g., forming a formate on the metal precursor layer, i.e., the co-reactant participates in ligand exchange with the metal precursor layer.
[0020] HCOOH and TBA were disclosed by Winter et al. to give selective CoALD with Co(DAD)2, but in accordance with the present invention, ALD selectivity approaches and is infinite due to specific control of pumping, purging and wall temperature to remove CVD components and achieve ligand exchange or molecular chemisorption, in contrast to the ALD described by Winter et al., who concluded that HCOOH is dissociatively chemisorbed to produce atomic H that removes the ligand from Co(DAD)2. Important aspects of such specific control include: (a) reducing background water, other reactive gases and co-reactants (all of which can induce non-selective CVD) by, for example, about 1×10 -6 These include using a chamber base pressure of 10 Torr (which may be provided, for example, by the use of a turbomolecular pump); (b) reducing surface contamination (which may be provided, for example, by the use of a turbomolecular pump); (c) using a long purge cycle (e.g., for about 15-30 seconds) to reduce residual co-reactants from the previous half cycle that may induce CVD; (d) using a UHV high temperature pre-anneal, for example, for 30 minutes, at a temperature of about 250°C to about 350°C to reduce undesired metal deposits on the insulator surface; (e) controlling the chamber wall temperature between about 80°C and about 100°C to reduce precursor remaining in the chamber after each pulse; and (f) using optimized pulse times for each precursor. Pulse and pump times were optimized to about 1 second (pulse time) for the precursors, which were separated by about 15 seconds of pumping (pump time).
[0021] In some embodiments, to enhance selectivity, particularly for nanoscale patterned samples, a relatively long purge time can be used, for example, the purge time after exposing the substrate / sample to the organometallic precursor can be increased from about 5 seconds to about 10 seconds, about 15 seconds, about 20 seconds, about 30 seconds, about 40 seconds, about 50 seconds, or even about 60 seconds. In other embodiments, to enhance selectivity, particularly for nanoscale patterned samples, the supply amount of the organometallic precursor can be reduced, for example, by decreasing the number of pulses per cycle. In some embodiments, to enhance selectivity, particularly for nanoscale patterned samples, the supply amount of the organometallic precursor can be less than the saturation supply amount. For example, the supply amount can be less than about 0.7×saturation supply amount, less than about 0.6×saturation supply amount, less than about 0.5×saturation supply amount, less than about 0.4×saturation supply amount, less than about 0.3×saturation supply amount, or less than about 0.2×saturation supply amount. Furthermore, in some embodiments, a cyclic anneal between two cycles of ALD may be performed, for example, but not limited to, after about 10, 20, 50, 100, 150, or 200 ALD cycles, at a temperature below the reflow temperature of the deposited metal (e.g., about 260° C. for Co), followed by one or more additional ALD cycles, for example, about 10, 20, 50, 100, 150, or 200 ALD cycles, to increase selectivity, especially for nanoscale patterned samples. In the case of Ru, the cyclic anneal may be performed at a temperature, for example, near about 250° C. to 350° C. in the presence of O2, or near about 350° C. to about 400° C. in the absence of O2.
[0022] In addition, the temperature at which the deposition is performed can be important for selectivity. In some embodiments, selective ALD of Co may be performed between about 160° C. and about 280° C. In some embodiments, selective ALD of Co is performed at a temperature of about 180° C. In other embodiments, selective ALD of Ru may be performed between about 160° C. and about 230° C. In some embodiments, selective ALD of Ru is performed at about 215° C.±15° C.
[0023] Furthermore, an aspect of the present invention provides a mechanism for ultraselective ALD that is extensible to nearly any metal with a DAD ligand precursor. ALD cobalt metal was deposited on Cu, Pt, and SiO2 substrates at 180 °C using bis(1,4-di-tert-butyl-1,3-diazadienyl)cobalt (Co(DAD)2) as the organometallic cobalt precursor and either formic acid (HCOOH) or tert-butylamine (TBA) as the co-reactant. The deposited Co films were investigated using in situ X-ray photoelectron spectroscopy (XPS) and atomic force microscopy (AFM). Cross-sectional scanning electron microscopy (SEM) and four-point probe measurements were performed to examine the film thickness and resistivity, respectively. η as the zero oxidation state liquid precursor was used. 4 ALD ruthenium metal was deposited using -2,3-dimethylbutadiene ruthenium tricarbonyl [Ru(DMBD)(CO)3] and again either formic acid or TBA. Selectivity was again observed as Ru metal was deposited on the metal substrates (Pt and Cu) versus SiO2. ALD was performed at 215°C. Deposition on both of these metals via a selective ALD process allows for via metal deposition with relatively large grains that degrade via metal deposition.
[0024] Selective Co from HCOOH: For 180°C ALD using Co(DAD)2 and HCOOH, it was found that there is almost infinite selective deposition of Co on the conductor but not on SiO2. The ALD was performed at a wall temperature of 80°C and a base pressure of 1×10 -6 The experiments were carried out using a turbomolecular pump system at 100 Torr. The Co(DAD)2 precursor was heated to a bottle temperature of 150 °C to achieve sufficient vapor pressure, while HCOOH was delivered at room temperature. The ALD pulse time and pumping time were optimized to 1 s for the precursors, which were separated by 15 s of pumping.
[0025] FIG. 1 shows XPS of 100 ALD cycles followed by 100 additional cycles on UHV annealed Pt vs. SiO2. +0A film is deposited, but not substantially on SiO2. AFM images show no change on SiO2 before and after the CoALD cycle, consistent with no nucleation, while the roughness for Co on Pt surface remains below 1.8 nm (FIG. 2). To demonstrate self-limiting precursor exposure consistent with ALD, a saturation study was performed and monitored with XPS. FIG. 3 highlights the effect of each additional half-cycle dose resulting in self-limiting Co(DAD)2 and HCOOH exposure, consistent with ALD. Additionally, this study revealed a novel mechanism for the reaction. Unlike the cobalt layer ALD of Winter et al., where it was concluded that HCOOH dissociatively chemisorbs to generate atomic H, which removes the ligand from Co(DAD)2, in the present invention's ALD, XPS shows that HCOOH does not remove the ligand, but instead induces a ligand exchange process. FIG. 4 shows the Co2p peak, which suggests that HCOOH leaves behind a relatively high binding energy component, consistent with the presence of formate on the surface that is removed upon exposure to Co(DAD)2.
[0026] Deposition with selective Co:HCOOH from TBA was attempted on Cu substrates (FIG. 5A); however, the substrate Cu signal did not decrease to zero, consistent with etching with HCOOH, so an alkylamine coreactant (TBA) was also examined. With Co(DAD)2+TBA ALD at 180° C., reduced Co metal films were deposited on Cu and Pt substrates with superselectivity to SiO2. Films as thick as 30 nm were grown on the conductor without etching of the substrate (FIG. 5B). On SiO2, only 4% CoOx was deposited after the initial 50 ALD cycles. After an additional 250 ALD cycles, there was still only 4% CoOx present (FIG. 5C), consistent with saturation and superselectivity (i.e., infinite selectivity). AFM imaging from ALD with TBA confirmed the low surface roughness ALD on Pt and Cu, whereas only small (<5 nm) CoOx particles were present on SiO2.
[0027] For RuALD, Figure 6 shows the reaction at high temperature (325°C). No metal vs. insulator selectivity is observed. However, lowering the temperature to 215°C results in strong selectivity of Ru deposition over metal with very little deposition on SiO2. ALD was performed at a wall temperature of 80°C and a base pressure of 1x10 -6 The ALD pulse times were set at 1 s for the precursors and separated by 15 s of pumping.
[0028] When the AFM was examined to see the surface topography, the Ru deposition on Cu shows some relatively large grains consistent with the deposition, whereas there are only a few nuclei on the SiO2, consistent with good selectivity (Figure 8). The film was a little rougher than ideal, so the precursor was switched from formic acid (as with Co) to TBA. When TBA was used with Ru(DMBD)(CO)3, the selectivity was still very strong in XPS. Figure 9 shows the amount of Ru deposited on each of the various substrates. Figure 10 shows an AFM image switching to a smoother platinum sample compared to the deposition on SiO2. The AFM shows very little surface roughness, consistent with a very smooth film of Ru being deposited. This smooth film is expected to be a very good option for bottom-up filling in vias. Figure 11 shows the XPS chemical shift data for the Ru 3d peak in XPS for both Pt and SiO2 substrates. For SiO2, the peak is at 280.3 eV, whereas for Pt, the peak is at 279.8 eV, which is highly consistent with RuOx formation on the SiO2 surface, whereas more strongly reduced (metallic) Ru is formed on the Pt surface, suggesting that the deposition of reduced metal species is reduced by the formation of oxidized metal components on the surface, but the adsorption of the precursor is not completely prevented because RuOx is not fully oxidized.
[0029] In another aspect of the present invention, an ALD process is provided that can be used in MOL and BEOL where selectivity is maintained at the nanoscale level between the metal growth surface and the insulator, i.e., on a patterned surface / substrate. Exemplary aspects are now described below.
[0030] According to some aspects of the present invention, atomic layer deposition of cobalt using Co(DAD)2 and tertiary butylamine (TBA) has nearly infinite selectivity (>1000 cycles) on metal-to-insulator (SiO2 or low-kSiCOH) flat samples. However, on patterned samples, the selectivity may be limited under identical ALD conditions due to diffusion of molecularly adsorbed metal precursors from reactive to non-reactive surfaces. Three strategies were found to improve CoALD selectivity: increasing purge time, reducing precursor feed rate, and cyclic annealing. While reducing precursor feed rate may be considered a conventional strategy, the other two strategies are unconventional. Increasing purge time is particularly effective for the Co(DAD)2 precursor because it allows reversible adsorption and desorption from the sample; conversely, most precursors undergo rapid dissociative chemistry. The cyclic annealing technique has not been reported before for any system. The cyclic annealing technique allows for resorption of Co nuclei from the insulator surface to the growth surface and is compatible with the low temperature reflow process.
[0031] CoALD was performed using Co(DAD)2 + TBA at 180 °C on 85 nm wide Cu strips on SiO2. The flat structure of these strips is used to demonstrate the passivation effect because top-down SEM imaging and XPS quantification can be used to monitor the growth and presence of unwanted Co nuclei on the insulator. To control the precursor dosage, multiple precursor pulses were employed in each cycle to limit the maximum pressure. XPS is performed without breaking vacuum to prevent oxidation of Co.
[0032] Reduced selectivity at the nanoscale: The Co(DAD)2+TBA ALD process was employed on patterned substrates with 85 nm wide Cu lines separated by SiO2. XPS quantification shows Cu decay and Si remaining consistent with selective deposition, while SEM imaging shows Co nuclei on the non-reactive SiO2 surface (see Figure 12). The nuclei are dense near the Cu and taper away from the strip. In addition, nearly all nuclei have a similar diameter. This is consistent with unwanted nuclei forming by diffusion of the Co(DAD)2 precursor from the Co growth surface on Cu to the SiO2 where it is reduced to Co by a subsequent TBA pulse. On unpatterned SiO2 surfaces, the observed superselectivity is consistent with a lack of molecular adsorption, but it is hypothesized that hydroxyl groups on the SiO2 combined with the close proximity of the Co / Cu surfaces may lead to unwanted adsorption of the Co precursor and thus unwanted nucleation.
[0033] To confirm this, Cu / SiO2 patterned samples were passivated with gas-phase dimethylamino-dimethyl-silazane (DMADMS) and tetramethyl-disilazane (TMDS) at 70 °C for 10 min and subjected to 200 cycles of CoALD. As shown in Figure 12, the number of undesired nuclei was reduced by at least 4x and the uniformity of nuclei on SiO2 was increased. This is consistent with the defect sites on SiO2 being passivated, leaving Co(DAD)2 with a longer surface diffusion path and more amenable to readsorption on the metal stripes.
[0034] The two-way diffusion-controlled:Co(DAD)2+TBA ALD is unusual because the XPS data are consistent with molecular adsorption rather than dissociative chemisorption of Co(DAD)2 at 180 °C. This suggests that Co(DAD)2 adsorption is reversible; therefore, it was hypothesized that selectivity could also be improved by increasing the purge time, so that Co(DAD)2 diffused onto SiO2 could desorb before the pulse of TBA stripped the (DAD) ligand from Co(DAD)2 and induced irreversible adsorption. As shown in Figure 13a, increasing the purge time from 5 to 20 s reduced the density of undesired nuclei, consistent with Co(DAD)2 diffusion and reversible adsorption, but the effect is less dramatic than that of passivation.
[0035] Although Co(DAD)2 tends to strongly adsorb on the Co metal growth surface, during each ALD cycle, excess Co(DAD)2 is used to ensure saturation, so that the growth surface is not metallic Co at the end of the Co(DAD)2 supply. It was hypothesized that once the growth surface was saturated with Co(DAD)2, further supply of Co(DAD)2 would lead to diffusion into SiO2. To test this, a lower Co(DAD)2 supply was employed by decreasing the number of pulses per cycle. As shown in Figure 13b, this was very effective in reducing the number of undesired nuclei on SiO2, but also slowed the growth rate. These results confirm that the loss of selectivity at the nanoscale is due to surface precursor diffusion.
[0036] Removal of unwanted nuclei by nano-reflow: A third method to improve selectivity was tested; after each 100 CoALD cycles, an anneal to 260 °C was performed; this is about 100 °C lower than the normal Co reflow temperature. However, according to a simple Ostwald ripening model, atoms from small nuclei can diffuse more easily than atoms from large nuclei; therefore, it may be possible to induce Co diffusion from the nuclei into the Co / Cu strip by annealing the sample when the nuclei are small. As shown in Figure 14, cyclic annealing led to almost perfect selectivity on the Cu / SiO2 patterns without passivation. This technique has the added advantage of allowing lower temperatures for reflow, potentially removing the diffusion barrier between Co and SiCOH that is usually employed. It is noted that this method of increasing selectivity to Co and reducing the need for high temperature reflow may also be useful for other selective CoALD and CVD processes. Note that this method as well as the other two methods (increasing the purge time and decreasing the metal supply) may be effective for increasing selectivity at the nanoscale and also for Ru(DMBD)(CO)3+HCOOH or TBA RuALD processes. Note that for Ru reflow, annealing during O2 supply may be acceptable since RuOx may diffuse faster than Ru at a given temperature.
[0037] While particular embodiments of the present invention have been shown and described, it will be understood that other modifications, substitutions and alterations will be apparent to those of ordinary skill in the art. Such modifications, substitutions and alterations can be made without departing from the spirit and scope of the present invention, which should be determined from the appended claims.
[0038] Various features of the invention are set forth in the following claims. While this application is directed to the invention set forth in the claims, the disclosure of this application also includes: 1. A method for atomic layer deposition (ALD) of a metal, comprising: a) exposing a substrate to an organometallic precursor, wherein the substrate comprises a surface including metal portions and insulator portions; b) depositing an organometallic precursor onto the surface of the metal portion of the substrate to selectively provide a metal precursor layer on the surface of the metal portion of the substrate; c) exposing the metal precursor layer to a co-reactant; and d) depositing a co-reactant onto the metal precursor layer; The method includes at least one cycle, wherein the co-reactant participates in ligand exchange with the metal precursor layer. 2. The method according to claim 1, wherein the cycle of a), b), c), and d) is carried out more than once. 3. The method according to claim 2, wherein cyclic annealing is performed between the two cycles of a), b), c), and d). 4. Cyclic annealing is performed at about 260 °C if the organometallic precursor contains Co, or at about 100 °C if the organometallic precursor contains O. 2 At about 250°C to about 350°C in the presence of Ru, or at about 100°C in the presence of Ru, 2 The method according to claim 3, wherein the method is carried out at about 350° C. to about 400° C. in the absence of 5. The method of any one of claims 1 to 4, wherein the exposure of the substrate to the organometallic precursor comprises a pulse time of about 1 second. 6. The method according to any one of 1. to 5. above, wherein the substrate is exposed to less than a saturation supply of the organometallic precursor (<0.7×saturation). 7. The method according to any one of 1. to 5. above, further comprising purging excess organometallic precursor after step a) for a period of about 20 seconds to about 60 seconds. 8. The method of any one of 1. to 7. above, wherein the co-reactant is formic acid (HCOOH) or tert-butylamine (TBA), or a similar organic carboxylic acid or organic amine. 9. The organometallic precursor is bis(1,4-di-tert-butyl-1,3-diazadienyl)cobalt [Co(DAD)] 2 9. The method according to any one of 1. to 8. above, 10. The method according to any one of 1. to 9. above, wherein the deposition is carried out at between about 160°C and about 200°C. 11. The method according to claim 10, wherein the deposition is carried out at about 180°C. 12. The substrate comprises a metal portion comprising copper (Cu), or platinum (Pt), or cobalt (Co), or ruthenium (Ru), and the deposition on the metal portion of the substrate is SiO 2 12. The method according to any one of 1. to 11. above, wherein the deposition is more selective than deposition on insulating portions of a substrate comprising SiN or SiCOH. 13. The insulating part of the substrate is SiO 2 13. The method according to claim 12, further comprising: 14. The method according to any one of 1. to 13. above, wherein the ligand exchange is induced through control of gas-phase CVD. 15. A method for atomic layer deposition (ALD) of a metal, comprising: a) exposing a substrate to a liquid organometallic precursor in a zero oxidation state, wherein the substrate comprises a surface including metal portions and insulator portions; b) depositing a zero oxidation state liquid organometallic precursor on the top surface of the metal portion of the substrate to selectively provide a metal precursor layer on the top surface of the metal portion of the substrate; c) exposing the metal precursor layer to a co-reactant; and d) depositing a co-reactant onto the metal precursor layer; A process comprising at least one cycle, wherein the co-reactant is formic acid (HCOOH) or tert-butylamine (TBA), or a similar organic carboxylic acid or organic amine. 16. The method according to claim 15, wherein the cycle of a), b), c) and d) is carried out more than once. 17. The method according to claim 15, wherein cyclic annealing is performed between two cycles of a), b), c), and d). 18. The substrate includes a metal portion including copper (Cu) or platinum (Pt), and deposition on the metal portion of the substrate is SiO 2 18. The method according to any one of claims 15 to 17, wherein the deposition is more selective than deposition on insulating portions of a substrate comprising SiN or SiCOH. 19. The insulating part of the substrate is SiO 2 17. The method according to claim 16, further comprising: 20. Liquid organometallic precursors in the zero oxidation state are η 4 -2,3-Dimethylbutadiene ruthenium tricarbonyl [Ru(DMBD)(CO) 3 20. The method according to any one of 15. to 19. above, 21. The method of claim 19, wherein the metal moiety comprises Cu, Pt, Co, or Ru, and the co-reactant is HCOOH or TBA. 22. The method according to any one of claims 15 to 21, wherein the deposition is carried out at between about 160°C and about 230°C. 23. The method according to claim 22, wherein the deposition is carried out at about 215°C. 24. A method for atomic layer deposition (ALD) of a metal, comprising: a) exposing a surface of a substrate to an organometallic precursor containing cobalt (Co) or ruthenium (Ru), wherein the surface of the substrate is formed of a metal moiety containing copper (Cu), platinum (Pt), cobalt (Co) or ruthenium (Ru) and a metal moiety containing SiO 2 and an insulating portion including SiN or SiCOH, b) depositing an organometallic precursor on the top surface of the metal portion of the substrate to selectively provide a metal precursor layer on the top surface of the metal portion of the substrate; c) exposing the metal precursor layer to a co-reactant; and d) depositing a co-reactant onto the metal precursor layer; 13. A method comprising at least one cycle, wherein the co-reactant is formic acid (HCOOH) or tert-butylamine (TBA), and the deposition is carried out at between about 160° C. and about 230° C. 25. The method according to claim 24, wherein the cycle of a), b), c) and d) is carried out more than once. 26. The method according to claim 24 or 25, wherein the coreactant participates in ligand exchange with the metal precursor layer. 27. The organometallic precursor is bis(1,4-di-tert-butyl-1,3-diazadienyl)cobalt [Co(DAD) 2 27. The method of claim 26, wherein the co-reactant is HCOOH, the metal portion of the substrate comprises Pt, Cu, Co or Ru, and the deposition is carried out at about 180°C. 28. The organometallic precursor is bis(1,4-di-tert-butyl-1,3-diazadienyl)cobalt [Co(DAD) 2 27. The method of claim 26, wherein the co-reactant is TBA, the metal portion of the substrate comprises Cu, Pt, Co or Ru, and the deposition is carried out at about 180°C. 29. A method according to any one of claims 26 to 28, wherein the cycle of a), b), c) and d) is carried out more than once, and cyclic annealing is carried out between two cycles of a), b), c) and d). 30. The method according to claim 29, wherein the cyclic annealing is carried out at about 260°C. 31. Organometallic precursor is η 4 -2,3-Dimethylbutadiene ruthenium tricarbonyl [Ru(DMBD)(CO) 3 25. The method according to claim 24, wherein the deposition is carried out at about 215°C. 32. The method of any one of claims 24 to 31, wherein the exposure of the substrate to the organometallic precursor comprises a pulse time of about 1 second. 33. The method according to any one of 24. to 32. above, wherein the substrate is exposed to less than a saturation supply of the organometallic precursor (<0.7×saturation). 34. The method according to any one of claims 24 to 33, further comprising purging excess organometallic precursor after step a) for a period of about 20 seconds to about 60 seconds.
Claims
1. 1. A method for atomic layer deposition (ALD) of a metal, comprising: a) exposing a substrate to an organometallic precursor, wherein the substrate comprises a surface including metal portions and insulator portions; b) depositing an organometallic precursor onto a surface of the metal portion of the substrate to selectively provide a metal precursor layer on the surface of the metal portion of the substrate; c) exposing the metal precursor layer to a co-reactant; and d) depositing a co-reactant onto the metal precursor layer; at least one cycle, with the proviso that a co-reactant participates in ligand exchange with the metal precursor layer, and the cycles of a), b), c), and d) are performed more than once, and a cyclic anneal is performed between two cycles of a), b), c), and d).
2. The cyclic anneal is performed at about 260° C. if the organometallic precursor contains Co, or at about 100° C. if the organometallic precursor contains O. 2 at about 250° C. to about 350° C. in the presence of, or when the organometallic precursor comprises Ru, O 2 The method of claim 1, wherein the method is carried out at about 350° C. to about 400° C. in the absence of
3. 3. The method of claim 1 or 2, wherein the exposure of the substrate to the organometallic precursor comprises a pulse time of about 1 second.
4. The method according to any one of claims 1 to 3, wherein the substrate is exposed to less than a saturation dose (<0.7 x saturation dose) of the organometallic precursor.
5. The method of any one of claims 1 to 3, further comprising purging excess organometallic precursor after step a) for a period of about 20 seconds to about 60 seconds.
6. The process according to any one of claims 1 to 5, wherein the co-reactant is an organic carboxylic acid or an organic amine.
7. The method of claim 1, wherein the co-reactant is formic acid (HCOOH) or tert-butylamine (TBA).
8. The organometallic precursor was bis(1,4-di-tert-butyl-1,3-diazadienyl)cobalt [Co(DAD) 2 8. The method according to claim 1, wherein 9. The method of claim 1, wherein the co-reactant is selected from an organic carboxylic acid and an organic amine, and the organometallic precursor has a DAD (1,4-di-tert-butyl-1,3-diazadienyl) ligand.
10. The method of any one of claims 1 to 9, wherein the deposition is carried out at between about 160°C and about 200°C.
11. The method of claim 10, wherein the deposition is performed at about 180°C.
12. The substrate includes a metal portion including copper (Cu), or platinum (Pt), or cobalt (Co), or ruthenium (Ru), and deposition on the metal portion of the substrate includes deposition of SiO 2 12. The method according to claim 1, wherein the deposition is more selective towards deposition on insulating parts of the substrate comprising SiN or SiCOH.
13. The insulating part of the substrate is SiO 2 The method of claim 12, comprising:
14. The method according to any one of claims 1 to 13, wherein the ligand exchange is induced via control of gas phase CVD.
15. 1. A method for atomic layer deposition (ALD) of a metal, comprising: a) exposing a substrate to a liquid organometallic precursor in a zero oxidation state, wherein said substrate comprises a surface including metal portions and insulator portions; b) depositing a zero oxidation state liquid organometallic precursor on an upper surface of the metal portion of the substrate to selectively provide a metal precursor layer on the upper surface of the metal portion of the substrate; c) exposing the metal precursor layer to a co-reactant; and d) depositing a co-reactant onto the metal precursor layer; wherein the co-reactant is an organic carboxylic acid or an organic amine, and wherein the cycles of a), b), c) and d) are carried out more than once, and wherein a cyclic anneal is carried out between two cycles of a), b), c) and d).
16. 16. The method of claim 15, wherein the co-reactant is formic acid (HCOOH) or tert-butylamine (TBA).
17. The substrate includes a metal portion including copper (Cu) or platinum (Pt), and deposition on the metal portion of the substrate includes SiO 2 17. The method of claim 15 or 16, wherein the method is more selective for deposition on insulating portions of a substrate comprising SiN or SiCOH.
18. The insulating part of the substrate is SiO 2 17. The method of claim 15 or 16, comprising:
19. The liquid organometallic precursor in the zero oxidation state is η 4 -2,3-Dimethylbutadiene ruthenium tricarbonyl [Ru(DMBD)(CO) 3 19. The method according to any one of claims 15 to 18, wherein
20. 20. The method of claim 18, wherein the metal moiety comprises Cu, Pt, Co or Ru and the co-reactant is HCOOH or TBA.
21. The method of any one of claims 15 to 20, wherein the deposition is carried out at between about 160°C and about 230°C.
22. The method of claim 21 , wherein the deposition is performed at about 215° C.
23. 1. A method for atomic layer deposition (ALD) of a metal, comprising: a) exposing a surface of a substrate to an organometallic precursor comprising cobalt (Co) or ruthenium (Ru), wherein the surface of the substrate is formed of a metal moiety comprising copper (Cu), platinum (Pt), cobalt (Co) or ruthenium (Ru) and a SiO 2 and an insulating portion including SiN or SiCOH, b) depositing an organometallic precursor on the top surface of the metal portion of the substrate to selectively provide a metal precursor layer on the top surface of the metal portion of the substrate; c) exposing the metal precursor layer to a co-reactant; and d) depositing a co-reactant onto the metal precursor layer; wherein the co-reactant is formic acid (HCOOH) or tert-butylamine (TBA) and the deposition is performed at between about 160° C. and about 230° C. and the cycles of a), b), c) and d) are performed more than once and a cyclic anneal is performed between two cycles of a), b), c) and d).
24. The method of claim 23 , wherein the co-reactant participates in ligand exchange with the metal precursor layer.
25. The organometallic precursor was bis(1,4-di-tert-butyl-1,3-diazadienyl)cobalt [Co(DAD) 2 25. The method of claim 24, wherein the co-reactant is HCOOH, the metal portion of the substrate comprises Pt, Cu, Co or Ru, and the deposition is performed at about 180°C.
26. The organometallic precursor was bis(1,4-di-tert-butyl-1,3-diazadienyl)cobalt [Co(DAD) 2 25. The method of claim 24, wherein the co-reactant is TBA, the metal portion of the substrate comprises Cu, Pt, Co or Ru, and the deposition is performed at about 180°C.
27. The method according to any one of claims 23 to 26, wherein the cyclic annealing is performed at about 260°C.
28. The organometallic precursor was η 4-2,3-dimethylbutadiene ruthenium tricarbonyl [Ru(DMBD)(CO) 3 and the deposition is performed at about 215° C.
29. The method of any one of claims 23 to 28, wherein exposing the substrate to the organometallic precursor comprises a pulse time of about 1 second.
30. The method of any one of claims 23 to 29, wherein the substrate is exposed to less than a saturation dose (<0.7 x saturation dose) of the organometallic precursor.
31. The method of any one of claims 23 to 30, further comprising purging excess organometallic precursor after step a) for a period of about 20 seconds to about 60 seconds.
Citation Information
Patent Citations
Organometallic compounds useful for chemical phase deposition
JP2018515694A
Thermally stable volatile precursors
US20180265975A1
Thermally stable volatile precursors
US9255327B2
Thin film formation method
WO2011114989A1