Temporary fixing substrate, manufacturing method thereof, and method for temporarily fixing electronic components
The substrate with a dent formation region on its outer periphery addresses peeling failures in semiconductor packages by enhancing adhesion and preventing air bubbles, thereby maintaining high yield.
Patent Information
- Application Number
- JP2022058844
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-03-31
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2042-03-31
AI Technical Summary
Conventional temporarily fixed substrates experience peeling failures during the semiconductor package manufacturing process, leading to decreased yield.
A temporarily fixed substrate with a dent formation region on its outer periphery, featuring a large number of depressions of varying shapes and sizes, is used to enhance adhesion and prevent peeling.
The substrate effectively suppresses peeling between the resin and the substrate, maintaining high yield by ensuring proper adhesion and preventing air bubble formation.
Smart Images

Figure 0007561157000001 
Figure 0007561157000002 
Figure 0007561157000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a temporary fixing substrate used in a manufacturing process of a semiconductor package. [Background technology]
[0002] FOWLP (Fan-out Wafer Level Package) technology is known as a semiconductor package manufacturing technology. FOWLP technology is a process of obtaining a semiconductor package with a lower height than conventional ones by performing a process of resin molding on a temporary fixing substrate on which a semiconductor chip is temporarily fixed with an adhesive, a process of grinding the resin mold to expose the electrode ends of the semiconductor chip, a process of forming a thin-film rewiring layer (multilayer wiring) and solder balls on the surface where the electrode ends are exposed, and a process of singulating each package and peeling it off from the temporary fixing substrate.
[0003] An embodiment using a translucent ceramic substrate as a temporary fixing substrate for chips in such FOWLP technology is already known (see, for example, Patent Documents 1 and 2). The translucent ceramic substrate satisfies all of the requirements required for a temporary fixing substrate, namely, high flatness required for exposing electrode ends, high rigidity and reverse warpage required for suppressing warpage during multilayer wiring formation, translucency that allows the transmission of laser light for hardening the adhesive, and chemical resistance for cleaning and reuse after use. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6430081 [Patent Document 2] Patent No. 6420023 Summary of the Invention [Problem to be solved by the invention]
[0005] However, conventional temporary fixing substrates have a problem in that peeling defects occur in which the resin portion peels off from the outer periphery, resulting in a decrease in yield.
[0006] The present invention has been made in consideration of the above problems, and has an object to provide a temporary fixing substrate that suppresses peeling defects and enables semiconductor packages to be obtained with a higher yield than in the past. [Means for solving the problem]
[0007] In order to solve the above problems, a first aspect of the present invention is a temporary fixing substrate having a plurality of electronic components bonded to one main surface and temporarily fixed by a resin mold, characterized in that the temporary fixing substrate has a dent formation region in which a large number of depressions of the same or different shapes are present regularly or irregularly around the entire outer periphery of the one main surface.
[0008] A second aspect of the present invention is a temporary fixing substrate related to the first aspect, characterized in that the dent formation area is provided in a range of 3% or less of the radius of the temporary fixing substrate from the side end of the temporary fixing substrate.
[0009] A third aspect of the present invention is a temporary fixing substrate relating to the first or second aspect, characterized in that the radial size of the numerous recesses is 0.1 mm to 5 mm, the circumferential size is 0.01 mm to 60 mm, and the depth is 1 μm to 20 μm.
[0010] A fourth aspect of the present invention is a temporary fixing substrate according to any one of the first to third aspects, characterized in that the spacing between the numerous recesses is 0.2 mm or more and equal to or less than the diameter of the temporary fixing substrate.
[0011] A fifth aspect of the present invention is the temporary fixing substrate according to the fourth aspect, Around It is characterized by its directional size being 3mm to 60mm.
[0012] A sixth aspect of the present invention is a method for manufacturing a temporary fixing substrate having a plurality of electronic components bonded to one main surface and temporarily fixed by a resin mold, the method comprising the steps of: producing a disk-shaped molded body mainly composed of a translucent ceramic; forming a plurality of recesses regularly or irregularly within a predetermined range of the entire outer periphery of one main surface of the molded body; firing the molded body with the plurality of recesses formed therein to obtain a sintered body; and polishing the sintered body.
[0013] A seventh aspect of the present invention is a method for temporarily fixing an electronic component to a temporary fixing substrate, comprising the steps of: preparing a temporary fixing substrate having a dent formation area in which a large number of depressions of the same or different shapes are present regularly or irregularly around the entire outer periphery of one main surface; forming an adhesive layer on the temporary fixing substrate; arranging a plurality of electronic components on the adhesive layer; bonding the plurality of electronic components to the temporary fixing substrate by hardening the adhesive layer to form an adhesive layer; and forming a resin mold on the adhesive layer and the plurality of electronic components. Effect of the Invention
[0014] According to the first to seventh aspects of the present invention, it is possible to suitably suppress the occurrence of peeling between the temporary fixing substrate and the resin during the process of temporarily fixing an electronic component to the temporary fixing substrate with a resin mold. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a plan view of one main surface (front surface) 1a of the temporary fixing substrate 1. [Diagram 2] 2 is a schematic enlarged view of a portion A shown in FIG. 1 showing variations of dents in a dent formation region 2. FIG. [Diagram 3] 1A to 1C are schematic cross-sectional views showing stages during a process of manufacturing a semiconductor package by FOWLP technology using a temporary fixing substrate 1. [Figure 4] FIG. 2 is a flow diagram illustrating a manufacturing process of the temporary fixing substrate 1. [Diagram 5] 1 is a box plot showing the distribution of measurement values for the recesses formed in the dent formation region 2 of the temporary fixing substrate 1 in Example 1. FIG. [Figure 6] 13 is a box plot showing the distribution of measurement values for the recesses formed in the dent formation region 2 of the temporary fixing substrate 1 in Example 2. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] <Temporary fixing board> 1 is a plan view of one main surface (front surface) 1a of a temporary fixing substrate 1 according to the present embodiment. The temporary fixing substrate 1 is a substrate to which a semiconductor chip is temporarily fixed when a semiconductor package is manufactured by a fan-out wafer level package (FOWLP) technique.
[0017] The temporary fixing substrate 1 is a translucent ceramic substrate having a diameter of several hundred mm (e.g., 300 mm), a thickness of several hundred μm to several mm (e.g., 1 mm), an in-plane thickness difference of several μm or less (e.g., 3 μm or less), and a warpage of several hundred μm or less (e.g., 200 μm). In this embodiment, the translucent ceramic is a ceramic having a forward total light transmittance of 20% or more in the entire wavelength range of 200 nm to 1500 nm. Examples of such translucent ceramic include alumina, silicon nitride, aluminum nitride, and silicon oxide. For example, a suitable example of the temporary fixing substrate 1 is one having alumina as the main component and a forward total light transmittance of 70% or more at a wavelength of 1500 nm. When alumina is the main component, it is preferable to use high-purity alumina powder of 99.9% or more (preferably 99.95% or more) as the raw material, and it is preferable to add magnesium oxide and zirconia (ZrO2) and yttria (Y2O3) as sintering aids to such alumina powder.
[0018] The front surface 1a, on which the semiconductor chip is arranged, and the other main surface (back surface) 1b are both polished to be approximately flat surfaces. As a result, the front surface 1a achieves the above-mentioned in-plane thickness difference of within a few μm and an arithmetic mean roughness Ra of 20 nm or less. More specifically, both the front surface 1a and the back surface 1b are surfaces that have been subjected to lapping.
[0019] However, in the temporary fixing substrate 1 according to this embodiment, an area of a predetermined width a from the side end 1e on the entire outer periphery of the surface 1a is a dent formation area 2 where numerous dents exist regularly or irregularly. Therefore, strictly speaking, the arithmetic mean roughness Ra of the surface 1a of 20 nm or less is realized in the area excluding the dent formation area 2.
[0020] FIG. 2 is a diagram showing variations of dents in the dent formation region 2 as a schematic enlarged view of a portion A shown in FIG.
[0021] FIG. 2(a) shows a state in which a plurality of linear recesses D1 are formed discretely at a predetermined pitch p along the radial direction of the temporary fixing substrate 1.
[0022] However, each recess does not have to have the same shape, and recesses of various shapes may be present. Also, recesses of the same or different shapes may be present at various pitches in both the radial and circumferential directions.
[0023] 2(b) illustrates recesses D2 to D4 of several different shapes. The recess D2 is rectangular. The recess D3 is linear along the circumferential direction of the temporary fixing substrate 1. The recess D4 is dot-shaped. Recesses of different irregular diameters may also be formed.
[0024] Also, it is not essential that the individual depressions are discrete, and they may overlap each other. Fig. 2(c) illustrates a state in which a large number of linear depressions D5 overlap each other to form a mesh. More specifically, the mesh-like depressions D5 are formed by a large number of depressions D5a aligned in a certain direction and a large number of depressions D5b perpendicular to the depressions D5a.
[0025] <Semiconductor package manufacturing process and the effect of dent formation> 3A to 3C are schematic cross-sectional views showing, in stages, intermediate steps of a process for producing a semiconductor package by the FOWLP technique using the temporary fixing substrate 1. FIG.
[0026] In the process of manufacturing a semiconductor package, first, as shown in Fig. 3(a), a layer (adhesive layer) 3α made of an adhesive is formed on a temporary fixing substrate 1 having a dent formation region 2 on the outer periphery of its surface 1a. Examples of the adhesive include double-sided tape and hot melt adhesives, and various known methods such as roll coating, spray coating, screen printing, and spin coating can be used for forming the adhesive. In more detail, the temporary fixing substrate 1 has a warped shape that is slightly convex toward the surface 1a side, but in Fig. 3, for convenience of illustration, such warping is ignored.
[0027] Next, as shown in FIG. 3(b), a plurality (a large number) of semiconductor chips 4 are placed on the adhesive layer 3α. The semiconductor chips 4 are placed in an area inside the dent formation area 2. The adhesive layer 3α is then cured to form the adhesive layer 3. The curing method is selected from heating, ultraviolet irradiation, and the like, depending on the material of the adhesive used in the adhesive layer 3α. As a result, the semiconductor chips 4 are adhesively fixed to the temporary fixing substrate 1.
[0028] When the semiconductor chip 4 is fixed to the temporary fixing substrate 1 in this manner, a molding resin is poured onto the entire upper surface of the temporary fixing substrate 1, that is, into the gaps 5 between the semiconductor chips 4 and the entire upper surface of the semiconductor chip 4. The molding resin is cured to form a resin mold 6, as shown in Fig. 3(c). Examples of the molding resin include epoxy resin, polyimide resin, polyurethane resin, and urethane resin.
[0029] Thereafter, the resin mold 6 is ground until the electrode ends of the semiconductor chip 4 are exposed, and then a rewiring layer and solder balls are formed on the ground surface. Finally, the substrate is divided into individual packages, and the temporary fixing substrate 1 is separated by laser lift-off.
[0030] The dent formation region 2 provided on the outer periphery of the temporary fixing substrate 1 has the effect of suppressing the occurrence of defects (peeling defects) in which the resin (adhesive layer 3 and resin mold 6) peels off from the temporary fixing substrate 1 (peeling suppression effect) during the semiconductor package manufacturing process described above, until the time when individualization and laser lift-off are performed.
[0031] In the case of conventional temporary fixing substrates, during the manufacturing process of the above-mentioned semiconductor package, air can get in between the temporary fixing substrate and the resin from the outside near the outer periphery of the temporary fixing substrate, forming air bubbles, which can cause peeling between the temporary fixing substrate and the resin.
[0032] However, when the temporary fixing substrate 1 according to the present embodiment is used, the adhesive and further the mold resin enter the recesses in the dent formation region 2 provided on the outer periphery of the front surface 1a, and an anchor effect is generated between the adhesive and the resin in the dent formation region 2. This anchor effect suppresses the formation of air bubbles on the outer periphery of the temporary fixing substrate 1 and the peeling of the resin. The presence or absence of air bubbles can be confirmed by observing the temporary fixing substrate 1 from the back surface 1b side with the naked eye or with a stereomicroscope. In this embodiment, the resin is deemed to have peeled off not only when the temporary fixing substrate 1 is visually observed from the side end portion 1e side and a portion where the resin and the temporary fixing substrate 1 are separated is confirmed, but also when air bubbles having a size of 3 mm or more in the longitudinal or lateral direction are confirmed as a result of observing the temporary fixing substrate 1 from the back surface 1b side with the naked eye or with a stereomicroscope.
[0033] The width a of the dent formation region 2 in the temporary fixing substrate 1 from the outer periphery is at most 3% of the radius r of the temporary fixing substrate 1. Even if the width a from the outer periphery is 3% or less of the radius r, as long as the recess is provided sufficiently, the peeling suppression effect can be obtained well. Furthermore, the laser lift-off is not hindered. Note that the recess may be present on the surface 1a inside the dent formation region 2 as long as the arithmetic mean roughness of the surface 1a does not exceed 20 nm. The recess may have a longitudinal size of 2 mm or less and a depth of 20 μm or less, for example. It is not preferable that the recess is present in such a manner that the arithmetic mean roughness of the surface 1a exceeds 20 nm, since it is not possible to obtain a good semiconductor package.
[0034] As shown in FIG. 2(b) for the recess D2, when the radial size L and circumferential size W of each recess are defined, it is preferable that the radial size L is 0.1 mm to 5 mm, and the circumferential size W is 0.01 mm to 60 mm. It is preferable that the depth of each recess is about 1 μm to 20 μm. Furthermore, it is preferable that the interval between each recess (when there is overlap as in the recess D5, the size of the area surrounded by each recess) is 0.2 mm or more and the substrate diameter or less. When these conditions are satisfied, the occurrence rate of peeling failure (peeling failure rate) counted per substrate is suppressed to 1% or less. Note that the case where the interval between the recesses is equal to the substrate diameter generally means the case where the interval is about 1 / 3 of the total circumferential length of the dent formation region 2. If the maximum interval between the recesses is about the same as the substrate diameter, the number of recesses to be formed is at least three, but even in this case, a certain degree of peeling suppression effect can be obtained. On the other hand, if the interval between the recesses is less than 0.2 mm, the dent formation region 2 becomes too rough, which is undesirable as it makes the region more susceptible to peeling.
[0035] It should be noted that, so long as there are sufficient recesses satisfying the above range and peeling is effectively suppressed, the presence of recesses below or above the range is permissible.
[0036] Moreover, it is more preferable that the circumferential dimension W is 3 mm to 60 mm. In this case, the anchor effect is more preferably exhibited, and the peeling failure rate is suppressed to 0.5% or less.
[0037] <Temporary Fixation Substrate Manufacturing Process> Next, a description will be given of a manufacturing process of the temporary fixing substrate 1 having the dent formation region 2. Fig. 4 is a flow diagram that shows an outline of the manufacturing process of the temporary fixing substrate 1. The temporary fixing substrate 1 is generally manufactured through a green body preparation step (step S1), a dent formation step (step S2), a firing step (step S3), and a polishing step (step S4).
[0038] In manufacturing the temporary fixing substrate 1, first, a molded body mainly composed of a light-transmitting ceramic powder is prepared (step S1). For example, the above-mentioned alumina or other light-transmitting ceramic raw material powder, ceramic powder such as magnesium or a sintering aid, and organic materials such as a binder and a solvent are kneaded in a ball mill or the like to produce a slurry, and the slurry is molded into a tape. The obtained tape is sheared (cut) to obtain rectangular sheets of a predetermined size, which are laminated and pressed, and the pressed laminate is punched into a circle. This produces a disk-shaped molded body. Alternatively, the molded body may be obtained by a doctor blade method, an extrusion method, a gel cast method, or the like.
[0039] Once the molded body is obtained, a large number of dents are then formed regularly or irregularly over the entire outer periphery of one main surface of the molded body, in an area that will become the dent formation region 2 in the ultimately obtained temporary fixing substrate 1 (step S2).
[0040] The recesses can be formed, for example, by making streak-like scratches with a tool with a sharp tip such as a diamond pen, by pressing a tool with a tip that is harder than the molded body such as a grindstone against the molded body, or by repeating such a procedure at predetermined intervals or randomly, or by pressing and rolling a knurl along the outer periphery of the molded body. For example, the mesh-like recesses D5 can be formed by using a twill knurl.
[0041] In addition, since some of the formed dents will shrink or disappear due to firing shrinkage in the subsequent firing process or due to removal of the surface region of surface 1a in the polishing process, it is desirable to form dents in the molded body with a size, depth, number, and range that take this into consideration.
[0042] Next, the molded body with the recesses formed therein is fired (step S3), whereby the organic components are eliminated and a ceramic sintered body (temporarily fixed substrate 1 before polishing) is obtained.
[0043] The firing is preferably performed by first calcining in an air furnace and then firing in a hydrogen furnace. The sintering temperature in the firing is preferably 1700°C to 1900°C, more preferably 1750°C to 1850°C, from the viewpoint of densifying the sintered body.
[0044] After the firing, the sintered body may be annealed in a hydrogen furnace to adjust (correct) the warpage. From the viewpoint of preventing deformation and abnormal grain growth while accelerating the discharge of the sintering aid, the annealing is preferably performed at a temperature within ±100°C of the maximum temperature during firing, and more preferably at 1900°C or less. The annealing time is preferably 1 to 6 hours.
[0045] Finally, the front and back surfaces of the sintered body obtained by firing are polished (step S4). First, the front and back surfaces of the sintered body are lapped. The lapped polishing is performed using a water-based or oil-based diamond slurry. Examples of the material of the polishing plate include copper, resin copper, tin, or a metal plate with a polishing pad attached. Examples of the polishing pad include a hard urethane pad, a nonwoven fabric pad, and a suede pad.
[0046] Prior to the polishing, the outer peripheral edge of the sintered body may be beveled (chamfered).
[0047] By going through the above steps, the temporary fixing substrate 1 according to this embodiment having the dent formation regions 2 is obtained.
[0048] Instead of forming a recess in the molded body before firing, a recess may be formed in the sintered body after firing or polishing. However, since such a sintered body has a higher hardness than the molded body, it is preferable to form a recess in the molded body from the viewpoint of ease of formation.
[0049] As described above, according to this embodiment, by making the outer periphery of the temporary fixing substrate used for temporarily fixing a semiconductor chip in the semiconductor package manufacturing process using FOWLP technology into a dent formation area having a large number of dents, it is possible to effectively suppress peeling between the temporary fixing substrate and the resin during the process.
[0050] (Modification) In the above-described embodiment, the temporary fixing substrate having the dent formation region is used as a substrate on which a plurality of semiconductor chips are temporarily fixed when a semiconductor package is manufactured by the FOWLP technique, but the use of the temporary fixing substrate is not limited thereto, and the temporary fixing substrate may be used for temporarily fixing electronic components other than semiconductor chips. That is, the temporary fixing substrate according to the above-described embodiment may be used for the purpose of suppressing peeling between the resin and the temporary fixing substrate when a resin mold is formed after a plurality of electronic components are bonded to the temporary fixing substrate with an adhesive.
[0051] In the above-described embodiment, the dent formation region is provided on one main surface of the temporary fixing substrate. In addition, the dent formation region may be formed on the other main surface as well. EXAMPLES
[0052] Example 1 Using alumina as the raw material for the translucent ceramics, we attempted to fabricate a temporary fixing substrate 1 having a dent formation region 2. Specifically, a diamond pen was used to form randomly sized dents at approximately 10 mm pitch along the diameter of the green body, and then sintering and polishing processes were performed to obtain a temporary fixing substrate 1 with a diameter of 300 mm. The width a of the dent formation region 2 was set to 4.5 mm or less.
[0053] When the obtained temporary fixing substrate 1 was visually observed, it was confirmed that it had dent formation regions 2.
[0054] In addition, a laser microscope was used to measure the radial size L, circumferential size W, and depth of the recesses formed in the dent formation region 2. The number of recesses measured was 24.
[0055] Fig. 5 is a box plot showing the distribution of each measurement value. As shown in Fig. 5(a), the radial size L was in the range of about 0.3 mm to 3.5 mm, with an average value of about 1.25 mm. As shown in Fig. 5(b), the circumferential size W was in the range of about 0.01 mm to 0.92 mm, with an average value of about 0.05 mm. As shown in Fig. 5(c), the depth was in the range of about 1.6 μm to 7.0 μm, with an average value of about 3.2 μm.
[0056] The above results show that the use of a diamond pen makes it possible to satisfactorily form the dent formation region 2, which is mainly a recess along the radial direction.
[0057] Example 2 An attempt was made to manufacture a temporary fixing substrate 1 having a dent formation region 2 in the same manner as in Example 1, except that the recesses were formed along the circumferential direction.
[0058] When the obtained temporary fixing substrate 1 was visually observed, it was confirmed that it had dent formation regions 2.
[0059] Moreover, the measurement of the depressions formed in the dent formation region 2 was also carried out in the same manner as in Example 1. The number of depressions measured was 11.
[0060] FIG. 6 is a box plot showing the distribution of each measurement value. As shown in FIG. 6(a), the radial size L was in the range of about 0.3 mm to 4.0 mm, with an average value of about 2.0 mm. As shown in FIG. 6(b), the circumferential size W was in the range of about 0.9 mm to 12.7 mm, with an average value of about 8.0 mm. As shown in FIG. 6(c), the depth was in the range of about 3.8 μm to 14.8 μm, with an average value of about 8.5 μm.
[0061] The above results show that the use of a diamond pen can also satisfactorily form the dent formation region 2, which is mainly a recess along the circumferential direction.
[0062] Example 3 In order to confirm that the provision of the dent formation region 2 in the temporary fixing substrate 1 is effective in suppressing peeling failure, the peeling failure rate was evaluated. The temporary fixing substrate 1 was prepared in the same manner as in Example 1.
[0063] Specifically, 800 temporary fixing substrates 1 were fabricated, and for each of them, a resin mold 6 was formed in accordance with the manufacturing process of a semiconductor package using the FOWLP technology, and then the presence or absence of peeling was confirmed by visual observation from the side end 1e side and the back surface 1b side. If separation between the resin mold 6 and the temporary fixing substrate 1 was confirmed at the side end 1e, and if air bubbles of 3 mm or more in size were confirmed in the longitudinal or lateral direction when observed from the back surface 1b side, it was determined that peeling defects had occurred.
[0064] As a result, peeling failure occurred in seven of the temporary fixing substrates 1. That is, the peeling failure rate was 7 / 800=0.00875, which was below 1%.
[0065] Comparative Example 1 For comparison with Example 3, 800 temporary fixing substrates 1 were produced in the same manner as in Example 3 except that the dent formation region 2 was not provided, and the peeling failure rate was also evaluated for these.
[0066] As a result, peeling failure occurred in 27 of the temporary fixing substrates 1. That is, the peeling failure rate was 27 / 800=0.0338, which exceeded 1%.
[0067] Comparing these results with those of Example 3, it can be said that providing the dent formation region 2 as in Example 3 is effective in preventing the occurrence of peeling defects.
[0068] Comparative Example 2 800 temporary fixing substrates 1 were produced using the same procedure as in Example 3, except that the entire surface 1a was made into the dent formation region 2 and the arithmetic mean roughness of the surface 1a was made into 25 nm, and the peeling failure rate was also evaluated for these.
[0069] As a result, peeling failure occurred in six temporary fixing substrates 1. That is, the peeling failure rate was 6 / 800=0.0075, which was below 1%.
[0070] Comparing these results with Example 3, it is confirmed that there is no significant difference between the peeling failure rate when the dent formation region 2 is provided only on the periphery of the temporary fixing substrate 1 as in Example 3 and when the dent formation region 2 is provided over almost the entire surface as in Comparative Example 2. This means that by simply providing the dent formation region 2 only on the periphery of the temporary fixing substrate 1 as in Example 3, it is possible to obtain almost the same effect of suppressing peeling failure as when the dent formation region 2 is provided over almost the entire surface as in Comparative Example 2. [Explanation of symbols]
[0071] 1 Temporary fixing board 1a (Temporary Fixing Board) Surface 1b (Temporary Fixing Board) Backside 1e Side end (of temporary fixing board) 2 dent formation area 3α Adhesive layer 3 Adhesive layer 4. Semiconductor chips 5 Gap 6 Resin mold
Claims
1. A temporary fixing substrate having a plurality of electronic components bonded to one main surface thereof and temporarily fixed by a resin mold, The one main surface has a dent formation region in which a large number of recesses of the same or different shapes are present regularly or irregularly around the entire outer periphery. A temporary fixing substrate,
2. The temporary fixing substrate according to claim 1 , The dent formation region is provided in a range of 3% or less of a radius of the temporary fixing substrate from a side end of the temporary fixing substrate. A temporary fixing substrate,
3. The temporary fixing substrate according to claim 1 or 2, The multiple recesses have a radial size of 0.1 mm to 5 mm, a circumferential size of 0.01 mm to 60 mm, and a depth of 1 μm to 20 μm. A temporary fixing substrate,
4. The temporary fixing substrate according to any one of claims 1 to 3, The intervals between the multiple recesses are 0.2 mm or more and are equal to or less than the diameter of the temporary fixing substrate. A temporary fixing substrate,
5. The temporary fixing substrate according to claim 4, The circumferential size of the multiple recesses is 3 mm to 60 mm; A temporary fixing substrate,
6. A method for manufacturing a temporary fixing substrate having a plurality of electronic components bonded to one main surface thereof and temporarily fixed by a resin mold, comprising: A step of preparing a disk-shaped molded body mainly composed of a translucent ceramic; forming a large number of recesses regularly or irregularly in a predetermined range over the entire outer periphery of one main surface of the molded body; sintering the molded body having the numerous recesses formed therein to obtain a sintered body; polishing the sintered body; A method for manufacturing a temporary fixing substrate, comprising:
7. A method for temporarily fixing an electronic component to a temporary fixing substrate, comprising the steps of: a step of preparing a temporary fixing substrate having a dent formation region in which a large number of dents of the same or different shapes are present regularly or irregularly on the entire outer periphery of one main surface; forming an adhesive layer on the temporary fixing substrate; placing a plurality of electronic components on the adhesive layer; a step of bonding the plurality of electronic components to the temporary fixing substrate by curing the adhesive layer to form an adhesive layer; forming a resin mold on the adhesive layer and the plurality of electronic components; A method for temporarily fixing an electronic component, comprising:
Citation Information
Patent Citations
Hand for harvesting fruit vegetables
JP1989020023A
Head moving device for hard disk
JP1989030081A
Method of manufacturing semiconductor device
JP2008258303A
Substrate support plate and method of bonding wafer temporarily to substrate support plate
JP2012049274A
Method for sealing semiconductor chip with resin
JP2014011268A