Dilatancy Composition

The dilatancy composition with specific base oils and fillers addresses the limitations of conventional compositions by enhancing dilatancy and temperature range while preventing electrical contact issues, suitable for automobile parts.

JP7561425B2Active Publication Date: 2024-10-04NIPPON KOYU LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021019694
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-10
Publication Date
2024-10-04
Estimated Expiration
2041-02-10

AI Technical Summary

Technical Problem

Conventional dilatancy compositions face challenges in achieving desired dilatancy properties when using fluorine oil or silicone oil as dispersion media, particularly in automobile parts due to issues like electrical contact failure and limited temperature range.

Method used

A dilatancy composition using mineral oil, synthetic hydrocarbon oil, diester oil, polyol ester oil, or alkylene glycol oil as base oil, combined with spherical silica or calcium carbonate filler and dispersants like sorbitan fatty acid ester or glycerin fatty acid ester, ensuring a viscosity ratio of 1.5 or higher at a shear rate of 0-200 s^-1.

Benefits of technology

The composition achieves excellent dilatancy properties with a wider temperature range and reduces electrical contact failures, making it suitable for automobile parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561425000001
    Figure 0007561425000001
  • Figure 0007561425000002
    Figure 0007561425000002
  • Figure 0007561425000003
    Figure 0007561425000003
Patent Text Reader

Abstract

To provide a dilatancy composition that can be used in a wide temperature range and can suppress electrical contact failure.SOLUTION: A dilatancy composition of the present invention comprises: a base oil as a dispersion medium; a filler; and a dispersant, wherein the base oil is at least one selected from a mineral oil, a synthetic hydrocarbon oil, a diester oil, a polyol ester oil, a diphenyl ether oil, and an alkylene glycol oil. In the present invention, the filler is preferably at least one selected from resin fine particles and inorganic fine particles.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dilatancy composition that is applied to parts of automobiles, home appliances, industrial machinery, and the like. [Background technology]

[0002] 2. Description of the Related Art Dilatancy compositions have been known for some time and are widely used in automobiles, home appliances, industrial machinery parts, and the like.

[0003] The invention described in Patent Document 1 discloses a grease composition comprising fluorinated oil and boron nitride, and having a worked penetration of 220 to 340. In addition, the invention described in Patent Document 2 discloses a dilatant composition comprising inorganic particles and silicone oil. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-201718 A [Patent Document 2] JP 2010-24420 A [Patent Document 3] JP 2006-2027 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, it has been found that when the base oil is a fluorinated oil or when no dispersant is contained, the desired dilatancy cannot be obtained.

[0006] There are also known known examples of using silicone oil as a dispersion medium for dilatancy compositions (see Patent Document 3). However, when a composition using silicone oil as a dispersion medium is applied to a part, there is a concern that low molecular weight siloxane may cause poor electrical contact, making it difficult to use in automobile-related parts in particular. In addition, dispersants compatible with silicone oil can only be effective with silicone oil, and cannot be applied to dispersion media other than silicone oil.

[0007] The present invention has been made in view of the above-mentioned points, and an object of the present invention is to provide a dilatancy composition capable of obtaining excellent dilatancy properties. [Means for solving the problem]

[0008] The dilatancy composition of the present invention is a dilatancy composition containing a base oil as a dispersion medium, a filler, and a dispersant, wherein the base oil is at least one selected from mineral oils, synthetic hydrocarbon oils, diester oils, polyol ester oils, diphenyl ether oils, and alkylene glycol oils; The filler includes at least one of spherical silica and spherical calcium carbonate, the dispersant is at least one selected from sorbitan fatty acid ester, alkyl glycerol, and glycerin fatty acid ester, and the shear rate is 0 to 200 S. -1 the maximum viscosity measured by changing the viscosity from (A) to (B) and the viscosity at the starting point where the viscosity of (A) begins to increase, the viscosity ratio calculated as (A) / (B) is 3.5 or more; It is characterized by:

[0009] Books In the present invention, it is preferable that the average particle size of the filler is 0.4 μm or more and 10 μm or less.

[0010] In the present invention, It is preferable that the content of the base oil in the dilatancy composition is 11.6 mass% or more and 27.7 mass% or less, the content of the filler is 69.6 mass% or more and 87.4 mass% or less, and the content of the dispersant is 1.0 mass% or more and 2.9 mass% or less. In the present invention, the grease may contain 3 mass % or less of a grease thickener. The present invention is preferably used for parts in the automobile-related field. Effect of the Invention

[0011] According to the dilatancy composition of the present invention, by containing at least one of mineral oil, synthetic hydrocarbon oil, diester oil, polyol ester oil, diphenyl ether oil, and alkylene glycol oil in the base oil as a dispersion medium, it is possible to obtain good dilatancy. In addition, compared to the case where silicone oil is used in the base oil, the concern of electrical contact failure can be reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] An embodiment of the present invention (hereinafter, abbreviated as "embodiment") will be described in detail below. Note that the present invention is not limited to the following embodiment, and can be practiced with various modifications within the scope of the gist. In addition, the notation "to" includes both the lower limit and the upper limit as a range.

[0013] <Background to the present embodiment> The dilatancy composition contains a base oil as a dispersion medium, a filler, and a dispersant. Conventional products often use a water-based, solvent-based, or silicone-based dispersion medium. However, conventional dilatancy compositions have a problem in that it is difficult to obtain a desired dilatancy. The "desired dilatancy" will be described later.

[0014] Here, various characteristics are required for the parts of automobiles, home appliances, industrial machines, etc. to which the dilatancy composition is applied. For example, speed control characteristics are required for damper devices and conveyor brakes, power transmission characteristics are required for joints, shock prevention characteristics are required for seat belt retractors and part protection, and vibration prevention characteristics are required for preventing brake squeal.

[0015] However, in the conventional dilatancy composition, for example, when the dispersion medium is water-based or solvent-based, the temperature range of use is narrow, and the parts that can be applied to satisfy the above characteristics are limited. That is, when the dispersion medium is water-based or solvent-based, there is a problem that the dispersion medium solidifies at low temperatures and is prone to volatilization at high temperatures. Even if it does not reach that level, there is a problem that the viscosity changes drastically and it can only be used around room temperature. In addition, it is difficult to use the dilatancy composition using silicone oil as the dispersion medium for automotive parts where there is a concern of poor electrical contact.

[0016] Therefore, the inventors conducted extensive research into a dilatancy composition containing a base oil as a dispersion medium, a filler, and a dispersant, and as a result, they were able to improve the dilatancy properties by improving the composition, etc.

[0017] <Dilatancy composition of the present embodiment> The dilatancy composition in this embodiment is a dilatancy composition containing a base oil as a dispersion medium, a filler, and a dispersant, and is characterized in that the base oil is at least one selected from mineral oil, synthetic hydrocarbon oil, diester oil, polyol ester oil, diphenyl ether oil, and alkylene glycol oil.

[0018] "Dilatancy" refers to a property in which the viscosity increases rapidly as the shear rate increases. In this embodiment, the presence or absence of the desired dilatancy is defined by the following index. That is, the viscosity was measured by changing the shear rate from 0 to 200 s-1 using a rheometer (Discovery HR-2 manufactured by TA Instruments). Then, the maximum viscosity obtained by the above measurement was defined as (A), and the viscosity at the starting point where the viscosity increase of (A) began was defined as (B), and the viscosity ratio (X) calculated by (A) / (B) was obtained. Then, when the viscosity ratio (X) was 1.5 or more, it was determined that the dilatancy was present.

[0019] In this embodiment, it was found that the desired dilatancy can be obtained by using a hydrocarbon oil such as a mineral oil or a synthetic hydrocarbon oil as the base oil as the dispersion medium. In addition, the operating temperature range can be wider than when water or a solvent-based dispersion medium is used. In addition, electrical contact failure can be suppressed compared to when silicone oil is used as the dispersion medium. One of the reasons for obtaining such effects is thought to be that a sufficient amount of filler can be added to the dilatancy composition.

[0020] In this embodiment, even when ester oil, ether oil, or glycol oil is used as the base oil other than the hydrocarbon oil, the same effect as that of the hydrocarbon oil can be obtained. The ester oil is preferably selected from diester oil or polyol ester oil. The ether oil is preferably diphenyl ether oil. The glycol oil is preferably alkylene glycol oil. In this embodiment, the base oil may be selected from two or more types of mineral oil, synthetic hydrocarbon oil, diester oil, polyol ester oil, diphenyl ether oil, and alkylene glycol oil.

[0021] In this embodiment, the base oil is preferably contained in the dilatancy composition in an amount of 4.5% by mass to 45% by mass, more preferably 10% by mass to 40% by mass.

[0022] The filler (solid component) is preferably at least one selected from resin fine particles and inorganic fine particles. Although not limited thereto, the inorganic fine particles may be spherical silica, spherical calcium carbide, Zn powder, etc. Furthermore, the resin fine particles may be fine particles made of melamine cyanurate or polypropylene.

[0023] In this embodiment, the average particle size of the filler is preferably 0.4 μm or more and 10 μm or less. Preferably, the average particle size of the filler is preferably 0.4 μm or more and 5 μm or less, and more preferably 0.4 μm or more and 3 μm or less. The smaller the average particle size, the slower the settling rate and the better the stability over time (Stokes' law). On the other hand, if the average particle size is too small, the surface area becomes large and the amount of filler that can be added decreases. Therefore, it is preferable that the average particle size is within the above range. The average particle size can be measured, for example, by acquiring a cross-sectional image with a scanning electron microscope and analyzing it using commercially available image analysis software. Alternatively, if it is a commercially available product, the particle size listed in each catalog can be used as the average particle size of the filler in this embodiment.

[0024] In this embodiment, the filler is preferably contained in the dilatancy composition in a range of 50% by mass or more and 95% by mass or less. In this way, in this embodiment, the filler content can be increased, and excellent dilatancy properties can be obtained. In this embodiment, the filler content is preferably 55% by mass or more, more preferably 60% by mass or more, even more preferably 65% ​​by mass or more, and even more preferably 70% by mass or more. In addition, the filler content is preferably 90% by mass or less. This allows the base oil and the dispersant to be blended in a well-balanced manner.

[0025] In this embodiment, the dispersant is preferably at least one selected from sorbitan fatty acid esters, alkyl glycerols, and glycerin fatty acid esters. For example, sorbitan monooleate can be selected as the sorbitan fatty acid ester, for example, oleyl glyceryl can be selected as the alkyl glycerol, and for example, glyceryl stearate can be selected as the glycerin fatty acid ester.

[0026] The dispersant is preferably contained in the dilatancy composition in an amount of 0.5% by mass to 5% by mass, and more preferably in an amount of 0.5% by mass to 3% by mass.

[0027] In this embodiment, by using sorbitan fatty acid ester, alkyl glycerol or glycerin fatty acid ester as the dispersant, it is possible to realize a combination of the base oil such as hydrocarbon oil in this embodiment with a suitable dispersant. As a result, the total content of the base oil and dispersant can be kept at a maximum of about 50 mass %, and a sufficient amount of filler can be added to exhibit dilatancy.

[0028] That is, if silicone oil, fluorine oil, or water-based is selected as the dispersion medium, sorbitan fatty acid ester, alkyl glycerol, and glycerin fatty acid ester as the dispersant are not compatible, and therefore cannot exhibit sufficient dilatancy.In other words, for example, the dispersant that is compatible with silicone oil is not compatible with the dispersion medium other than silicone oil, and only exhibits its effect when it is silicone oil.Therefore, the combination of base oil, filler, and dispersant that constitutes dilatancy composition is very closely related to dilatancy.

[0029] The dilatancy composition of this embodiment may be liquid or semi-solid (grease type). In the case of the grease type, a thickener is further included. In this embodiment, the thickener is not limited, and a commercially available one can be used as appropriate. For example, the thickener can be selected from at least one of lithium soap, calcium soap, sodium soap, aluminum soap, lithium complex soap, calcium complex soap, aluminum complex soap, urea compound, organo-bentonite, polytetrafluoroethylene, silica gel, sodium terephthalamate, calcium sulfonate complex soap, and barium complex soap.

[0030] In this embodiment, the content of the thickener in the dilatancy composition is preferably 3% by mass or less.

[0031] If necessary, the dilatancy composition of the present embodiment may contain an antioxidant, a rust inhibitor, a metal corrosion inhibitor, an oiliness agent, an anti-wear agent, an extreme pressure agent, a solid lubricant, etc. The content of these additives in the dilatancy composition is within a range of about 0.01% by mass to 20% by weight.

[0032] The antioxidant may be selected from hindered phenols, alkylated diphenylamines, phenyl-α-naphthylamines, etc. The rust inhibitor may be selected from sodium nitrite, carboxylic acids such as stearic acid, dicarboxylic acids, metal soaps, amine carboxylates, metal salts of heavy sulfonic acids, or partial esters of carboxylic acids of polyhydric alcohols, etc. The metal corrosion inhibitor may be selected from benzotriazole, benzimidazole, thiadiazole, etc. The oiliness agent may be selected from amines such as laurylamine, higher alcohols such as myristyl alcohol, higher fatty acids such as palmitic acid, fatty acid esters such as methyl stearate, or amides such as oleylamide, etc. The anti-wear agent may be selected from zinc-based, sulfur-based, phosphorus-based, amine-based, or ester-based agents, etc. The extreme pressure agent may be selected from zinc dialkyldithiophosphate, molybdenum dialkyldithiophosphate, sulfurized olefin, sulfurized oil and fat, methyl trichlorostearate, chlorinated naphthalene, benzyl iodide, fluoroalkyl polysiloxane, lead naphthenate, etc. The solid lubricant may be selected from graphite, graphite fluoride, polytetrafluoroethylene, melamine cyanurate, molybdenum disulfide, antimony sulfide, etc.

[0033] The dilatancy composition of the present embodiment is not limited to a particular application, but may be used for parts such as speed control, power transmission, shock prevention, and vibration prevention for automobiles, home appliances, and industrial machines. The dilatancy composition of the present embodiment does not use low molecular weight siloxane (silicone oil) as a dispersion medium. Therefore, in particular in the automobile-related field, the dilatancy composition of the present embodiment can be used to eliminate concerns about poor electrical contacts caused by low molecular weight siloxane, and can be preferably applied to parts in the automobile-related field.

[0034] In addition, the dilatancy composition is liquid when no shear is applied, and therefore it is preferable to use the dilatancy composition in a sealed state, but it can be used in other than sealed states by increasing the kinetic viscosity of the base oil, increasing the amount of filler to make it harder, or adding a thickener to make it a grease type to make it semi-fluid. EXAMPLES

[0035] The effects of the present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the experiments, the following raw materials were used to prepare the dilatancy composition:

[0036] (Base oil) a: Polyalphaolefin (dynamic viscosity at 40°C is 18mm 2 / s) b: Polyalphaolefin (dynamic viscosity at 40°C is 100mm 2 / s) c: Polyalphaolefin (Kinematic viscosity at 40°C is 407mm 2 / s) d: Alkyl diphenyl ether (kinematic viscosity at 40°C is 100 mm 2 / s) e: Alkylene glycol (Kinematic viscosity at 40°C is 32mm 2 / s) f: Diester oil (kinematic viscosity at 40°C is 11mm 2 / s) g: Polyol ester oil (kinetic viscosity at 40°C is 44mm 2 / s) h: Perfluoropolyether (dynamic viscosity at 40°C is 17mm 2 / s)

[0037] (Filler) i: High-purity synthetic spherical silica (particle size 1.5 to 2.5 μm) j: High purity synthetic spherical silica (particle size 0.9~1.2μm) k: High-purity synthetic spherical silica (particle size 0.4 to 0.6 μm) l: Spherical calcium carbonate (average particle size 5 μm) m: Melamine cyanurate (particle size 3.0±1.0μm) n: Polypropylene (average particle size 10 μm)

[0038] (Dispersant) o: Oleyl glyceryl (acid value: 1.1 mg KOH / g or less) p: Sorbitan monooleate (acid value: 5mgKOH / g) q: Glyceryl stearate (acid value: 1.1 mg KOH / g)

[0039] (Thickener) r: Lithium soap (melting point: 217°C) In the experiments, the above-mentioned raw materials a to q were mixed in the mixing ratios shown in Tables 1, 2, and 3 below to prepare various compositions.

[0040] Alternatively, the lithium soap r was mixed with a base oil, heated to 220°C with stirring, cooled, and then processed with a three-roll mill to make a grease with a worked penetration of NLGI Grade No. 1 (310-340), and a composition was prepared by further mixing with a filler and a dispersant.

[0041] (Measurement of dilatancy) The dilatancy was measured by the following method. That is, a rheometer (Discovery HR-2 manufactured by TA Instruments) was used to measure the shear rate from 0 to 200 s -1 The viscosity was measured by changing the temperature to

[0042] The maximum viscosity obtained by the above measurement was designated as (A), and the viscosity at the starting point where the viscosity of (A) began to increase was designated as (B). The viscosity ratio (X) calculated as (A) / (B) was obtained. When (X) was 1.5 or more, it was determined that there was dilatancy, and when (X) was less than 1.5, it was determined that there was no dilatancy. In Tables 1 to 3, the presence of dilatancy was marked with ◯, and the absence of dilatancy was marked with ×.

[0043] (Precipitation confirmation) A 100 mL beaker was filled with 50 mL of the dilatancy composition, and after leaving it at 25° C. for 24 hours, if the filler did not settle at the bottom of the beaker, it was considered that no precipitation occurred. In Tables 1 to 3, the absence of precipitation was marked with ◯, and the absence of precipitation was marked with ×.

[0044] [Table 1]

[0045] [Table 2]

[0046] [Table 3]

[0047] As shown in Tables 1 and 2, in Examples 1 to 15, a lubricant-type dilatancy composition was obtained by mixing and stirring a base oil, a filler, and a dispersant. The contents of the base oil, the filler, and the dispersant shown in the tables are the percentages when the total amount of these is 100% by mass. Also, as shown in Table 2, in Examples 16 to 17, a grease-type dilatancy composition was obtained by mixing a base oil, a filler, a dispersant, and a thickener. The contents of the base oil, the filler, the dispersant, and the thickener shown in the tables are the percentages when the total amount of these is 100% by mass.

[0048] Comparative Example 1 is a composition in which only the base oil and the filler were mixed and stirred, and does not contain a dispersant. Comparative Example 1 became a hard paste.

[0049] In addition, Comparative Example 2 is a composition in which perfluoropolyether was used as the base oil, and a filler and a dispersant were mixed and stirred. In this Comparative Example 2 as well, the composition became a hard paste.

[0050] Moreover, Comparative Example 3 is a composition in which a base oil and a filler were mixed and stirred, but it did not contain a dispersant and, furthermore, the filler content was small, so that no dilatancy was obtained.

[0051] Thus, both Comparative Example 1 and Comparative Example 2 were in a hard paste state, and therefore the viscosity could not be measured with a rheometer, i.e., dilatancy was not obtained.

[0052] In contrast, for Examples 1 to 15, one of mineral oils, synthetic hydrocarbon oils, diester oils, polyol ester oils, diphenyl ether oils, and alkylene glycol oils was selected as the base oil. The base oil, filler, and dispersant were mixed and stirred to obtain a composition. The compositions of these Examples were liquid when no shear force was applied. The viscosity ratio (X) was 1.5 or more. The viscosity ratio (X) could be made 3 or more, and could also be made 5 or more, or 10 or more.

[0053] Examples 16 and 17 were grease types, and in these examples too, the viscosity ratio (X) was 1.5 or more. In addition, no precipitation of the filler was observed in any of the examples. From the above, it was found that the compositions of the examples had excellent and desired dilatancy properties.

[0054] In this embodiment, resin particles or inorganic particles were selected as the filler, and the average particle size of the filler was in the range of 0.4 μm to 10 μm. It was found that silica and calcium carbonate can be preferably used as the inorganic particles. In particular, it was found that the content of silica can be increased, and the dilatancy can be effectively improved.

[0055] In this example, the filler content was in the range of 50% by mass or more and 95% by mass or less. It was found that the filler content is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more.

[0056] In this embodiment, when sorbitan fatty acid ester, alkyl glycerol, or glycerin fatty acid ester was used as the dispersant, good dilatancy was obtained.

[0057] In this embodiment, a hydrocarbon oil was used as the base oil, 80% by mass or more of inorganic fine particles were added to the filler, and 0.5% by mass or more and 2.0% by mass or less of alkyl glycerol was added to the dispersant, thereby making it possible to achieve a viscosity ratio (X) of approximately 5 or more and obtaining excellent dilatancy properties.

[0058] Furthermore, as shown in Examples 15 and 16, good dilatancy properties could be obtained even when a thickener was added to prepare a grease. [Industrial Applicability]

[0059] According to the dilatancy composition of the present invention, the temperature range of use can be broadened compared to the conventional one, the risk of poor contact of electrical contacts can be reduced, and excellent dilatancy can be obtained. Therefore, the dilatancy composition of the present invention can be applied to parts of automobiles, home appliances, and industrial machines, and is particularly preferably applied to automobile-related parts.

Claims

1. A dilatancy composition comprising a base oil as a dispersion medium, a filler, and a dispersant, The base oil is at least one selected from the group consisting of mineral oils, synthetic hydrocarbon oils, diester oils, polyol ester oils, diphenyl ether oils, and alkylene glycol oils; The filler contains at least one of spherical silica and spherical calcium carbonate, The dispersant is at least one selected from a sorbitan fatty acid ester, an alkyl glycerol, and a glycerin fatty acid ester, When the maximum viscosity measured by changing the shear rate from 0 to 200 S-1 is (A) and the viscosity at the starting point where the viscosity of (A) begins to increase is (B), the viscosity ratio calculated as (A) / (B) is 3.5 or more. A dilatancy composition comprising:

2. 2. The dilatancy composition according to claim 1, characterized in that the average particle size of the filler is 0.4 μm or more and 10 μm or less.

3. The dilatancy composition according to claim 1 or 2, characterized in that the filler is contained in an amount ranging from 50% by mass to 95% by mass.

4. The content of the base oil in the dilatancy composition is 11.6 mass% or more and 27.7 mass% or less, the content of the filler is 69.6 mass% or more and 87.4 mass% or less, and the content of the dispersant is 1.0 mass% or more and 2.9 mass% or less, A dilatancy composition according to claim 1 or claim 2.

5. 5. The dilatancy composition according to claim 1, further comprising 3% by mass or less of a grease thickener.

6. A dilatancy composition as described in claims 1 to 5, characterized in that it is used for parts in the automotive related field.

Citation Information

Patent Citations

  • Dilatant liquid

    JP1996281095A

  • Dilatant fluid

    JP1998152669A

  • High thermal conductive grease composition and cooling apparatus using the same

    JP2002201483A

  • Thermally conductive grease, method for mounting the same, method for cooling electronic component, electronic device and information processing device

    JP2003027080A

  • Dilatant fluid composition

    JP2006002027A