Dental zirconia sintered body, laminate, and zirconia calcined body for dental processing, and dental prosthesis
By laminating zirconia powders with varying compositions and stabilizers, the method enhances bonding and strength at layer boundaries in zirconia sintered bodies, addressing separation issues and achieving high mechanical properties and natural color gradation.
Patent Information
- Application Number
- JP2023076564
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2013-05-10
- Filing Date
- 2023-05-08
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2034-05-08
AI Technical Summary
Zirconia sintered bodies with laminated structures experience separation and reduced strength at layer boundaries due to differences in composition, leading to potential breakage during calcination or sintering.
Laminating zirconia powders with varying compositions and pigment contents, incorporating yttria as a stabilizer, and forming mixed layers at boundaries to enhance bonding strength through partial mixing and controlled sintering temperatures.
The method produces zirconia sintered bodies with increased bending strength and fracture toughness, maintaining integrity at layer boundaries, resembling natural tooth color gradation and reducing deformation during sintering.
Smart Images

Figure 0007561912000045 
Figure 0007561912000046 
Figure 0007561912000047
Abstract
Description
[Technical field]
[0001] [Related Application Description] The present invention is based on Japanese Patent Application No. 2013-100617 (filed May 10, 2013), the entire contents of which are incorporated herein by reference. The present invention relates to Dental The present invention also relates to a zirconia sintered body. Dental Laminate for producing zirconia sintered body and For dental processing The present invention further relates to a zirconia calcined body. Dental The present invention relates to a dental prosthesis (prosthetic material) having a zirconia sintered body. [Background technology]
[0002] In dental treatment, artificial teeth are used as substitutes for natural teeth, and these artificial teeth are required to have the same appearance as natural teeth.
[0003] Patent Document 1 discloses a multi-colored molded body having layers arranged on top of each other to produce a dental restoration. The molded body described in Patent Document 1 comprises (a) at least two continuous and differently colored main layers, and (b) at least two differently colored intermediate layers between the at least two continuous and differently colored main layers, where the change in color between the intermediate layers occurs in a direction opposite to the direction of the change in color between the main layers. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2008-68079 A Summary of the Invention [Problem to be solved by the invention]
[0005] The entire disclosure of the above-mentioned Patent Document 1 is incorporated herein by reference. The following analysis is provided in view of the present invention.
[0006] When preparing a zirconia sintered body having a laminated structure as described in Patent Document 1, the first layer is compression molded, the second layer is compression molded on top of the first layer, and so on. The zirconia powders of each layer are compression molded while being laminated, and then sintered. However, even if the composition of each layer is the same except for a trace amount of pigment, peeling may occur at the boundary between adjacent layers during calcination or sintering of the zirconia powder. In addition, in the sintered body, the strength of the boundary between adjacent layers is reduced, making it easy to break partially. [Means for solving the problem]
[0007] According to a first aspect of the present invention, there is provided a zirconia sintered body in a state in which a laminate formed by stacking a plurality of zirconia powders, each having a different composition due to a different pigment content, and vibrating the stack to form a mixed layer in which the zirconia powders in the upper and lower layers are partially mixed at each boundary between the zirconia powders, and sintering the laminate, the laminate being molded, and the zirconia sintered body is in a sintered state, the laminate being in a state in which a test piece cut out from the zirconia sintered body in the longitudinal direction along the stacking direction satisfies a test condition in accordance with JIS R1601 in which the bending strength measured by aligning the load point of a three-point bending test with the position of the mixed layer is 1100 MPa or more for the test piece in which the mixed layer exists so as to cross the test piece along the load application direction. According to a variation of the first aspect, there is provided a dental zirconia sintered body, which contains zirconia and yttria as a stabilizer for suppressing a phase transition of zirconia, and is in a state in which a laminate formed by stacking and molding a plurality of zirconia powders having different compositions due to different pigment contents is sintered, and the dental zirconia sintered body satisfies a test condition that a sintered body test piece cut out from the dental zirconia sintered body in the longitudinal direction along the stacking direction conforms to JIS R1601, and that the bending strength measured by aligning the load point of a three-point bending test with the position of the boundary for the sintered body test piece that exists so as to cross the sintered body test piece along the load application direction is 1100 MPa or more, and the dental zirconia sintered body contains at most 0.3 wt % aluminum oxide. According to another variation of the first aspect, there is provided a dental zirconia sintered body, which contains zirconia and yttria as a stabilizer for suppressing a phase transition of zirconia, and is in a state in which a laminate formed by stacking and molding a plurality of zirconia powders having different compositions due to different pigment contents is sintered, and the dental zirconia sintered body is provided with a sintered body test piece cut out from the dental zirconia sintered body in the longitudinal direction along the stacking direction, which satisfies a test condition in accordance with JIS R1601, in which the bending strength measured by matching the load point of a three-point bending test to the position of the boundary of the plurality of zirconia powders is 90% or more of the bending strength of another sintered body test piece obtained by sintering one of the zirconia powders alone at the same temperature as the sintering temperature of the sintered body test piece, and which contains at most 0.3% by weight of aluminum oxide.
[0008] According to a second aspect of the present invention, there is provided a zirconia calcined body for producing a zirconia sintered body, which becomes the zirconia sintered body according to the first aspect by sintering at 1400°C to 1600°C. According to the variant of the second aspect, there is provided a zirconia calcined body for dental processing, which becomes the dental zirconia sintered body according to the variant of the first aspect or another variant by sintering at 1400°C to 1600°C.
[0009] According to a third aspect of the present invention, there is provided a zirconia calcined body, which contains zirconia and yttria as a stabilizer for suppressing a phase transition of zirconia, and which is obtained by stacking a plurality of zirconia powders having different compositions due to different pigment contents, applying vibration to the stacked bodies to form mixed layers in which the zirconia powders in the upper and lower layers are partially mixed at each boundary between the zirconia powders, and molding the stacked body, and which is in a state where the stacked body is calcined at 800°C to 1200°C, and which satisfies a test condition in accordance with JIS R1601 in which a test piece is cut out from the zirconia calcined body in the longitudinal direction along the lamination direction, and the bending strength of the test piece, which is measured with the load point of a three-point bending test aligned with the position of the mixed layer, for the test piece in which the mixed layer exists so as to cross the test piece in the load application direction, is 90% or more of the bending strength of another test piece obtained by calcining one of the zirconia powders alone at the same temperature as the calcination temperature of the test piece. According to a variation of the third aspect, there is provided a zirconia calcined body for dental processing, which contains zirconia and yttria as a stabilizer for suppressing a phase transition of zirconia, and is in a state in which a laminate formed by stacking and shaping a plurality of zirconia powders having different compositions due to different pigment contents is calcined, wherein a calcined body test piece cut out longitudinally from the zirconia calcined body for dental processing along the lamination direction satisfies a test condition in accordance with JIS R1601 in which the bending strength measured in a three-point bending test with the load point aligned with the position of the boundary between the plurality of zirconia powders is 90% or more of the bending strength of another calcined body test piece obtained by calcining one of the zirconia powders alone at the same temperature as the calcination temperature of the calcined body test piece, and contains at most 0.3% by weight of aluminum oxide.
[0010] According to a fourth aspect of the present invention, there is provided a zirconia sintered body in a state obtained by sintering the zirconia calcined body according to the second aspect.
[0011] According to a fifth aspect of the present invention, there is provided a laminate for producing a zirconia sintered body, which becomes the zirconia sintered body according to the first aspect by sintering at 1400°C to 1600°C. According to the variant of the fifth aspect, there is provided a laminate for producing a dental zirconia sintered body, which becomes the dental zirconia sintered body according to the variant of the first aspect or another variant by sintering at 1400°C to 1600°C.
[0012] According to a sixth aspect of the present invention, there is provided a laminate for producing a zirconia sintered body, which becomes the zirconia calcined body according to the second aspect by firing at 800° C. to 1200° C. According to the variant of the sixth aspect, there is provided a laminate for producing a dental zirconia sintered body, which becomes the zirconia calcined body for dental processing according to the variant of the second or third aspect by calcining.
[0013] According to a seventh aspect of the present invention, there is provided a dental prosthesis in a state in which the zirconia calcined body according to the second aspect is cut and then sintered. According to the seventh aspect, there is provided a dental prosthesis in a state in which the calcined zirconia for dental processing according to the second or third aspect is cut and then sintered.
[0014] According to an eighth aspect of the present invention, there is provided a zirconia sintered body, which contains yttria as a stabilizer for suppressing the phase transition of zirconia and zirconia, and is in a state in which a laminate formed by stacking a plurality of zirconia powders having different compositions due to different pigment contents and applying vibration to form a mixed layer in which the zirconia powders of the upper and lower layers are partially mixed at each boundary between the zirconia powders and molding the laminate is sintered at 1400 ° C to 1600 ° C, and the zirconia sintered body satisfies a test condition that a test piece cut out from the zirconia sintered body in the longitudinal direction along the stacking direction conforms to JIS R 1601, the mixed layer exists so as to cross the test piece along the load application direction, and the bending strength measured by adjusting the load point of a three-point bending test to the position of the mixed layer is 90% or more of the bending strength of another test piece obtained by sintering one of the zirconia powders alone at the same temperature as the sintering temperature of the test piece.
[0015] According to a ninth aspect of the present invention, there is provided a zirconia calcined body, which contains zirconia and yttria as a stabilizer for suppressing a phase transition of zirconia, and which is obtained by stacking a plurality of zirconia powders having different compositions due to different pigment contents, applying vibration to the stacked bodies to form mixed layers in which the zirconia powders in the upper and lower layers are partially mixed at each boundary between the zirconia powders, and molding the stacked body, and which is in a state where the stacked body is calcined at 800°C to 1200°C, and which satisfies a test condition in accordance with JIS R1601 that the bending strength of the test piece, which is measured with the load point of a three-point bending test aligned with the position of the mixed layer, for the test piece in which the mixed layer exists so as to cross the test piece in the load application direction, is 90% or more of the bending strength of another test piece obtained by calcining one of the zirconia powders alone at the same temperature as the calcination temperature of the test piece. Effect of the Invention
[0016] The present invention has at least one of the following advantages.
[0017] According to the zirconia sintered body of the present invention, even when the zirconia sintered body is produced by laminating zirconia powders having different compositions, it is possible to obtain a zirconia sintered body in which the strength of the boundary between the layers is not reduced.
[0018] According to the laminate and zirconia calcined body of the present invention, the above-mentioned zirconia sintered body can be obtained. [Brief description of the drawings]
[0019] [Figure 1] FIG. 2 is a schematic diagram for explaining a three-point bending test method. [Diagram 2] Schematic diagram of zirconia sintered body. [Diagram 3] FIG. 1 is a schematic diagram of a test piece for measuring the amount of deformation during sintering. [Figure 4] FIG. 1 is a schematic diagram of a test piece for measuring the amount of deformation during sintering. [Diagram 5] FIG. 4 is a schematic diagram for explaining a method for measuring the amount of deformation. [Figure 6] Schematic diagram of a test piece in Example 5 and measurement results. [Figure 7] Schematic diagram of a test piece in Comparative Example 3 and measurement results. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Preferred embodiments of each of the above aspects are described below.
[0021] According to a preferred embodiment of the first aspect, the bending strength is 1200 MPa or more.
[0022] According to a preferred embodiment of the first aspect, when a zirconia calcined body is produced by calcining the laminate at 800°C to 1200°C, the bending strength measured in accordance with JIS R1601, in a three-point bending test for a test piece of the calcined body in which boundaries between a plurality of zirconia powder particles exist across the test piece in the load application direction, with the load point aligned with the position of the boundary, is 90% or more of the bending strength of a zirconia calcined body obtained by calcining one of the zirconia powder particles alone at the same temperature as the calcination temperature of the test piece.
[0023] According to a preferred embodiment of the first aspect, the plurality of zirconia powders contain a pigment and each of the zirconia powders has a different pigment content.
[0024] According to a preferred embodiment of the first aspect, each of the sintered bodies obtained by sintering a plurality of zirconia powders individually at 1500° C. has a bending strength of 1100 MPa or more as measured in accordance with JIS R1601.
[0025] According to a preferred embodiment of the first aspect, a zirconia calcined body is produced by calcining the laminate at 800°C to 1200°C, and the zirconia calcined body is molded into a rectangular parallelepiped shape having dimensions of width 50 mm x height 10 mm x depth 5 mm to prepare a test piece. When the surface of the test piece that is 50 mm wide x 5 mm deep is taken as the bottom surface, the boundary surface formed by the lamination of zirconia powder extends in the same direction as the bottom surface. When the test piece is sintered at 1500°C for 2 hours and placed with the bottom surface that has been deformed into a concave shape facing down, (maximum distance between the bottom surface that has been deformed into a concave shape and the ground surface) / (distance between the ground portions in the width direction) x 100 is 0.15 or less.
[0026] According to a preferred embodiment of the first aspect, the L of a first point in a section from one end to 25% of the total length on a straight line extending in a first direction from one end to the other end * a * b * Chromaticity according to color system (L * ,a * ,b * ) is (L1, a1, b1), and the second point L in the section from the other end to 25% of the total length is * a * b * Chromaticity according to color system (L * ,a * ,b *) is (L2, a2, b2), L1 is 58.0 or more and 76.0 or less, a1 is -1.6 or more and 7.6 or less, b1 is 5.5 or more and 26.7 or less, L2 is 71.8 or more and 84.2 or less, a2 is -2.1 or more and 1.8 or less, b2 is 1.9 or more and 16.0 or less, and L1<L2であり、a1> a2, b1>b2, and L from the first point to the second point * a * b * The tendency for chromaticity to increase or decrease due to the color system does not change.
[0027] According to a preferred embodiment of the first aspect, on a straight line connecting the first point and the second point, L is provided from the first point to the second point. * There is no interval where the value decreases by 1 or more, and a * There is no interval where the value increases by 1 or more, and b * There is no interval where the value increases by 1 or more.
[0028] According to a preferred embodiment of the first aspect, a third point between the first point and the second point on a straight line connecting the first point and the second point is located at a distance L. * a * b * Chromaticity according to color system (L * ,a * ,b * ) is (L3, a3, b3), L3 is 62.5 or more and 80.5 or less, a3 is -1.8 or more and 5.5 or less, b3 is 4.8 or more and 21.8 or less, and L1 <L3<L2であり、a1> a3>a2 and b1>b3>b2.
[0029] According to a preferred embodiment of the first aspect, a fourth point L between the third point and the second point on a straight line connecting the first point and the second point is * a * b * Chromaticity according to color system (L * ,a * ,b *) is (L4, a4, b4), then L4 is 69.1 or more and 82.3 or less, a4 is -2.1 or more and 1.8 or less, b4 is 3.5 or more and 16.2 or less, a1>a3>a4>a2, and b1>b3>b4>b2.
[0030] According to a preferred embodiment of the first aspect, the third point is located at a distance of 45% of the total length from the one end, and the fourth point is located at a distance of 55% of the total length from the one end.
[0031] According to a preferred embodiment of the first aspect, the first point, the third point, the fourth point and the second point are adjacent to each other. * The difference in values is ΔL * Let a be the distance between two adjacent points. * The difference between the values is Δa * Then, b at two adjacent points * The difference between the values is Δb * Then, from the following formula 1, ΔE * When ab is calculated, ΔE between the first and third points * ab is between 3.7 and 14.3, and ΔE between the third and fourth points is * ab is 1.8 to 17.9, and ΔE between the 4th point and the 2nd point is * ab is 1.0 or more and 9.0 or less. Formula 1
[0032] TIFF0007561912000001.tif866
[0033] According to a preferred embodiment of the first aspect, a third point between the first point and the second point on a straight line connecting the first point and the second point is located at a distance L. * a * b * Chromaticity according to color system (L * ,a * ,b * ) is (L3, a3, b3), L3 is 69.1 or more and 82.3 or less, a3 is -2.1 or more and 1.8 or less, b3 is 3.5 or more and 16.2 or less, and L1 <L3<L2であり、a1> a3>a2 and b1>b3>b2.
[0034] According to a preferred embodiment of the first aspect, the color changes in a first direction from one end to the other end, and L * a * b * The tendency for chromaticity to increase or decrease due to the color system does not change.
[0035] According to a preferred embodiment of the first aspect, on a straight line connecting one end and the other end, L is provided from a first point to a second point. * The value is on the rise, * value and b * The value is on a downward trend.
[0036] According to a preferred mode of the first aspect, the distance from one end to the other end is 5 mm to 18 mm.
[0037] According to a preferred mode of the first aspect, the color does not change along a second direction perpendicular to the first direction.
[0038] According to a preferred embodiment of the first aspect, at two points on a line extending in the second direction, L between the two points is * The difference in values is ΔL * Let a be the distance between the two points. * The difference between the values is Δa * Then, b between two points * The difference between the values is Δb * From the above formula 1, ΔE * When ab is calculated, ΔE * ab is less than 1.
[0039] According to a preferred embodiment of the first aspect, the fracture toughness measured in accordance with JIS R1607 is 3.5 MPa m 1 / 2 That's all.
[0040] According to a preferred embodiment of the first aspect, in an X-ray diffraction pattern of a zirconia sintered body after a hydrothermal treatment test at 180°C and 1 MPa for 5 hours, the ratio of the height of a peak existing near the position where a tetragonal crystal-derived
[0111] peak occurs at 2θ of about 30° to the height of a peak existing near the position where a monoclinic crystal-derived [11-1] peak occurs at 2θ of about 28° is 1 or less.
[0041] According to a preferred embodiment of the third aspect, the plurality of zirconia powders contain a pigment, and each of the zirconia powders has a different pigment content.
[0042] According to a preferred embodiment of the third aspect, a zirconia calcined body is produced by calcining the laminate at 800°C to 1200°C, and the zirconia calcined body is molded into a rectangular parallelepiped shape having dimensions of width 50 mm x height 10 mm x depth 5 mm to prepare a test piece. When the surface of the test piece that is 50 mm wide x 5 mm deep is taken as the bottom surface, the boundary surface formed by the lamination of the zirconia powder extends in the same direction as the bottom surface. When the test piece is sintered at 1500°C for 2 hours and placed with the bottom surface that has been deformed into a concave shape facing down, (maximum distance between the bottom surface that has been deformed into a concave shape and the ground surface) / (distance between the ground portions in the width direction) x 100 is 0.15 or less.
[0043] According to a preferred embodiment of the seventh aspect, the cutting process is carried out using a CAD / CAM system.
[0044] In the present invention, for example, when the zirconia sintered body has a crown shape, the above-mentioned "one end" and "other end" preferably refer to one point on the end on the incisal side and one point on the end on the root side. The one point may be a point on the end face or a point on the cross section. The point in the section from one end or the other end to 25% of the total length refers to, for example, a point away from one end or the other end at a distance equivalent to 10% of the height of the crown.
[0045] When the zirconia sintered body has a disk shape or a hexahedral shape such as a rectangular parallelepiped, the above-mentioned "one end" and "the other end" preferably refer to a point on the upper and lower surfaces (bottom surfaces). The point may be a point on an end face or a point on a cross section. A point located within 25% of the total length from one end or the other end refers to, for example, a point away from one end or the other end at a distance equivalent to 10% of the thickness of the hexahedron or disk.
[0046] In the present invention, the "first direction from one end to the other end" means the direction in which the color changes. For example, the first direction is preferably the direction in which the powder is layered in the manufacturing method described below. For example, when the zirconia sintered body has a crown shape, the first direction is preferably the direction connecting the incisal side and the root side.
[0047] The zirconia sintered body of the present invention will be described. The zirconia sintered body of the present invention is a sintered body in which partially stabilized zirconia crystal particles are mainly sintered, and has partially stabilized zirconia as a matrix phase. In the zirconia sintered body of the present invention, the main crystal phase of zirconia is a tetragonal system or a tetragonal and cubic system. It is preferable that the zirconia sintered body does not substantially contain a monoclinic system (at a stage before the hydrothermal treatment test described later).
[0048] The zirconia sintered body of the present invention includes not only a sintered body obtained by sintering molded zirconia particles under normal pressure or under no pressure, but also a sintered body densified by a high-temperature pressure treatment such as HIP (Hot Isostatic Pressing) treatment.
[0049] The zirconia sintered body of the present invention contains zirconia and a stabilizer therefor. The stabilizer inhibits the phase transition of tetragonal zirconia to monoclinic. By inhibiting the phase transition, strength, durability and dimensional accuracy can be improved. Examples of the stabilizer include oxides such as calcium oxide (CaO), magnesium oxide (MgO), yttrium oxide (Y2O3) (hereinafter referred to as "yttria") and cerium oxide (CeO2). It is preferable to add the stabilizer in an amount that can partially stabilize the tetragonal zirconia particles. For example, when yttria is used as the stabilizer, the content of yttria is preferably 2.5 mol% to 5 mol%, more preferably 3 mol% to 4.5 mol%, and even more preferably 3.5 mol% to 4.5 mol%, based on the total molar number of zirconia and yttria. If the content of the stabilizer is too high, even if the phase transition can be inhibited, bending strength and fracture toughness will decrease. On the other hand, if the content of the stabilizer is too low, even if the decrease in bending strength and fracture toughness can be suppressed, the suppression of the progress of the phase transition is insufficient. Note that tetragonal zirconia partially stabilized by adding a stabilizer is called partially stabilized zirconia (PSZ).
[0050] The zirconia sintered body of the present invention preferably contains aluminum oxide (Al2O3; alumina). The aluminum oxide is preferably α-alumina. The strength can be increased by containing aluminum oxide. The content of aluminum oxide in the zirconia sintered body is preferably 0 mass% (not contained) to 0.3 mass% based on the total mass of zirconia and the stabilizer. If the aluminum oxide is contained in an amount of more than 0.3 mass%, the transparency decreases.
[0051] The zirconia sintered body of the present invention preferably contains titanium oxide (TiO2; titania). The inclusion of titanium oxide can promote grain growth. The content of titanium oxide in the zirconia sintered body is preferably 0 mass% (not contained) to 0.6 mass% based on the total mass of zirconia and the stabilizer. If titanium oxide is contained in an amount of more than 0.6 mass%, the strength decreases.
[0052] In the zirconia sintered body of the present invention, the content of silicon oxide (SiO2; silica) is preferably 0.1 mass% or less based on the total mass of zirconia and the stabilizer, and the zirconia sintered body preferably does not substantially contain silicon oxide. If silicon oxide is contained, the transparency of the zirconia sintered body decreases. Here, "substantially does not contain" means that it is within a range that does not particularly affect the properties and characteristics of the present invention, and preferably does not contain more than the impurity level, and does not necessarily mean that it is below the detection limit.
[0053] The zirconia sintered body of the present invention may contain a pigment for coloring. When the zirconia sintered body is used as a dental material, the pigment may be, for example, chromium oxide (Cr2O3), erbium oxide (Er2O3), iron oxide (Fe2O3), praseodymium oxide (Pr6O 11 ) can be used. These pigments may be used in combination. The pigment content can be partially different.
[0054] For example, when the zirconia sintered body used as a dental material contains chromium oxide, the partial content of chromium oxide in the region containing chromium oxide is preferably 0.001% by mass or less with respect to the total mass of zirconia and the stabilizer. When the zirconia sintered body used as a dental material contains erbium oxide, the partial content of erbium oxide in the region containing erbium oxide is preferably 2% by mass or less with respect to the total mass of zirconia and the stabilizer. For example, when the zirconia sintered body used as a dental material contains iron oxide, the partial content of iron oxide in the region containing iron oxide is preferably 0.1% by mass or less with respect to the total mass of zirconia and the stabilizer. For example, when the zirconia sintered body used as a dental material contains praseodymium oxide, the partial content of praseodymium oxide in the region containing praseodymium oxide is preferably 0.1% by mass or less with respect to the total mass of zirconia and the stabilizer.
[0055] After sintering the zirconia sintered body, the X-ray diffraction pattern of the untreated zirconia sintered body in a hydrothermal treatment test (described later), which is an accelerated deterioration test, is measured using CuKα radiation. The ratio of the height of the peak (hereinafter referred to as the "second peak") near the position where the monoclinic [11-1] peak occurs at 2θ of approximately 28° to the height of the peak (hereinafter referred to as the "first peak") near the position where the tetragonal
[0111] peak occurs at 2θ of approximately 30° (i.e., "height of the second peak / height of the first peak"; hereinafter referred to as the "monoclinic peak ratio") is preferably 0.1 or less, and more preferably 0.05 or less.
[0056] The zirconia sintered body of the present invention is inhibited from undergoing a phase transition from tetragonal to monoclinic even when subjected to a hydrothermal treatment test. For example, when the zirconia sintered body of the present invention is subjected to a hydrothermal treatment at 180°C and 1 MPa for 5 hours, the monoclinic peak ratio in the X-ray diffraction pattern measured with CuKα radiation on the surface of the zirconia sintered body after the hydrothermal treatment is preferably 1 or less, more preferably 0.8 or less, even more preferably 0.7 or less, and even more preferably 0.6 or less.
[0057] In this document, "hydrothermal treatment test" refers to a test conforming to ISO13356. However, while the conditions specified in ISO13356 are "134°C, 0.2 MPa, 5 hours," in the present invention, in order to make the test conditions more severe, the conditions are set to "180°C, 1 MPa," and the test time is set appropriately according to the purpose. The hydrothermal treatment test is also called the "low-temperature accelerated deterioration test" or the "hydrothermal deterioration test."
[0058] The bending strength of the zirconia sintered body of the present invention measured in accordance with JIS R1601 is preferably 1000 MPa or more, more preferably 1100 MPa or more, and even more preferably 1200 MPa or more. Note that these values are those in a state before the hydrothermal treatment test.
[0059] In the zirconia sintered body of the present invention, the above bending strength can be obtained in a three-point bending test even when the load point is located at the boundary between layers in the manufacturing method described below. FIG. 1 shows a schematic diagram of a three-point bending test. For example, in a test piece, the boundary when zirconia powders with different compositions are laminated is located at the center of the test piece (middle in the longitudinal direction). The boundary extends along the load application direction (along the smallest area direction) and crosses the test piece. The load point in the three-point bending test is aligned with the position of the boundary. Even if the bending strength is measured by a test in which a load is applied to the boundary in this way, a strength similar to that of a sintered body that is not laminated (without a boundary) can be obtained. For example, in the sintered body of the present invention, the bending strength measured by applying a load to the boundary between layers is preferably 90% or more, more preferably 95% or more, of the bending strength of the region other than the boundary (for example, the bending strength of a calcined body produced under similar conditions (for example, the same calcination temperature and calcination time) from a composition that is not a laminate).
[0060] The fracture toughness of the zirconia sintered body of the present invention, measured in accordance with JIS R1607, is 3.5 MPa m 1 / 2 It is preferable that the pressure is 3.8MPa m or more. 1 / 2 More preferably, it is 4 MPa m 1 / 2More preferably, it is 4.2 MPa m 1 / 2 It is more preferable that the value is equal to or more than this. Note that these values are for the case where the hydrothermal treatment test has not been carried out.
[0061] In the zirconia sintered body of the present invention, the above-mentioned fracture toughness can be obtained in the fracture toughness measurement test even when the load point is located at the boundary between layers in the manufacturing method described below. For example, in the test piece, the boundary when zirconia powders with different compositions are laminated is located at the center (middle in the longitudinal direction) of the test piece. The boundary extends along the load application direction (along the smallest area direction) and crosses the test piece. The diamond indenter for the measurement test is positioned on the boundary. Even if the fracture toughness is measured by a test in which a load is applied to the boundary in this way, the fracture toughness can be obtained similar to that of a sintered body that is not laminated (without a boundary).
[0062] The zirconia sintered body of the present invention preferably satisfies the above-mentioned values for all of the monoclinic peak ratio, bending strength, and fracture toughness after hydrothermal treatment. For example, the zirconia sintered body of the present invention has a monoclinic peak ratio of 1 or less and a fracture toughness of 3.5 MPa m 1 / 2 More preferably, the zirconia sintered body of the present invention has a monoclinic peak ratio of 0.6 or less and a fracture toughness of 4 MPa m after hydrothermal treatment. 1 / 2 and the bending strength is 1000 MPa or more.
[0063] When the zirconia sintered body of the present invention is colored, particularly when the color gradually changes in one direction (has a gradation), it is preferable that the zirconia sintered body of the present invention has a direction in which the color does not change substantially. FIG. 2 shows a schematic diagram of a zirconia sintered body. For example, in the zirconia sintered body 10 shown in FIG. 2, it is preferable that the color does not change substantially in the first direction X. For example, between any two points on a straight line extending in the first direction X, L * a * b * L, which is the chromaticity in the color system (JISZ8729)* Value, a * value and b * The difference between the values is ΔL * , Δa * and Δb * Then, from the following formula, ΔE * When ab is calculated, ΔE * ab is preferably less than 1, and more preferably less than 0.5.
[0064] TIFF0007561912000002.tif866
[0065] In addition, when the zirconia sintered body of the present invention is colored, it is preferable that the color changes (has a gradation) from one end connecting both ends to the other end. * Value, a * value and b * It is preferable that the increasing or decreasing trend of the value does not change in the opposite direction. That is, on a straight line from one end P to the other end Q, * If the value is increasing, L * It is preferable that there is no section in which the value substantially decreases. For example, on a straight line from one end P to the other end Q, * If the value is increasing, L * It is preferable that there is no interval where the value decreases by 1 or more, and more preferable that there is no interval where the value decreases by 0.5 or more. * If the value is on a decreasing trend, a * It is preferable that there is no section in which the value increases substantially. For example, on a line from one end P to the other end Q, * If the value is on a decreasing trend, a * It is preferable that there is no interval where the value increases by 1 or more, and more preferable that there is no interval where the value increases by 0.5 or more. * If the value is decreasing, b * It is preferable that there is no section in which the value substantially increases. For example, on a straight line from one end P to the other end Q, *If the value is decreasing, b * It is preferable that there is no interval where the value increases by 1 or more, and it is more preferable that there is no interval where the value increases by 0.5 or more.
[0066] The color change direction of the zirconia sintered body 10 is from one end P to the other end Q, * When the value is increasing, a * value and b * For example, when the zirconia sintered body 10 is used as a dental prosthetic material, it is preferable that the color changes from light yellow, light orange, or light brown to white from one end P to the other end Q.
[0067] In FIG. 2, the points on the line connecting one end P to the other end Q are designated as the first point A, the second point B, the third point C, and the fourth point D, in order from the one end P side. When the zirconia sintered body 10 is used as a dental prosthetic material, the first point A is preferably in a section from the one end P to 25% to 45% of the length between the one end P and the other end Q (hereinafter referred to as "total length"). The second point B is preferably in a section from a point 30% of the total length from the one end P to 70% of the total length from the one end P. The fourth point D is preferably in a section from the other end Q to 25% to 45% of the total length. The third point C is preferably in a section from a point 30% of the total length from the other end Q to 70% of the total length from the other end Q.
[0068] L at the first point A, the second point B, the third point C and the fourth point D * a * b * Color of zirconia sintered body 10 according to the color system (JIS Z8729) (L * ,a * ,b * ) are (L1, a1, b1), (L2, a2, b2), (L3, a3, b3) and (L4, a4, b4). At this time, it is preferable that the following magnitude relationship is established. The chromaticity of each point can be obtained by producing a zirconia sintered body of the composition corresponding to each point alone and measuring the chromaticity of the zirconia sintered body.
[0069] L1 <L2<L3<L4 a1>a2>a3>a4 b1>b2>b3>b4
[0070] When the zirconia sintered body of the present invention is applied to a dental material, for example, L1 is preferably 58.0 or more and 76.0 or less. L2 is preferably 62.5 or more and 80.5 or less. L3 is preferably 69.1 or more and 82.3 or less. L4 is preferably 71.8 or more and 84.2 or less.
[0071] When the zirconia sintered body of the present invention is applied to a dental material, for example, a1 is preferably -1.6 or more and 7.6 or less, a2 is preferably -1.8 or more and 5.5 or less, a3 is preferably -2.1 or more and 1.6 or less, and a4 is preferably -2.1 or more and 1.8 or less.
[0072] When the zirconia sintered body of the present invention is applied to a dental material, for example, b1 is preferably 5.5 or more and 26.7 or less, b2 is preferably 4.8 or more and 21.8 or less, b3 is preferably 3.5 or more and 16.2 or less, and b4 is preferably 1.9 or more and 16.0 or less.
[0073] When the zirconia sintered body of the present invention is applied to a dental material, preferably, L1 is 60.9 or more and 72.5 or less, a1 is 0.2 or more and 5.9 or less, b1 is 11.5 or more and 24.9 or less, L4 is 72.2 or more and 79.2 or less, a4 is -1.2 or more and 1.7 or less, and b4 is 6.0 or more and 15.8 or less. More preferably, L1 is 63.8 or more and 68.9 or less, a1 is 2.0 or more and 4.1 or less, b1 is 17.5 or more and 23.4 or less, L4 is 72.5 or more and 74.1 or less, a4 is -0.2 or more and 1.6 or less, and b4 is 10.1 or more and 15.6 or less. This allows the color tone of the average tooth to be matched.
[0074] Color difference between two adjacent points ΔE * ab can be expressed by the following formula: ΔL * is the L in two adjacent layers *The difference between the values (e.g. L1-L2). Δa * is the a in two adjacent layers * The difference between the values (e.g. a1-a2). Δb * is the b * The difference between the color values (e.g. b1-b2). The color difference between the first point A and the second point B is ΔE * ab1, the color difference between the second point B and the third point C is ΔE * ab2, and the color difference between the third point C and the fourth point D is ΔE * ab3, if the chromaticities of the first point A, the second point B, the third point C, and the fourth point D have the above relationship, for example, ΔE * ab1 is preferably 3.7 or more and 14.3 or less. * ab2 is preferably 1.8 or more and 17.9 or less. * It is preferable that ab3 is 1.0 or more and 9.0 or less. This makes it possible to reproduce the same color change as that of natural teeth.
[0075] TIFF0007561912000003.tif866
[0076] The color difference between the first point A and the fourth point D is ΔE * When the chromaticities of the first point A, the second point B, the third point C, and the fourth point D have the above relationship, for example, ΔE * It is preferable that ab4 is 36 or less. Color difference ΔE between first point A and second point B * ab1, color difference ΔE between second point B and third point C * ab2 and the color difference ΔE between the third point C and the fourth point * From the sum of ab3, the color difference ΔE between the first point A and the fourth point D * The value obtained by subtracting ab4 is preferably equal to or less than 1. This allows a natural color change to be displayed.
[0077] In the zirconia sintered body of the present invention, when powders of different compositions are laminated in a manufacturing method described later, a straight line is formed so as to cross the layers (intersect with the boundary), i.e., along the second direction Y shown in FIG. * a * b * Color space (JISZ8729) b *By measuring the continuous change in value, the b * It is preferable that the value is not constant, but shows a gradual increasing (or decreasing) trend. Also, even if the boundary portion is crossed, b * It is preferable that no sudden increase or decrease in the value is observed. * The change in value can be measured, for example, using a two-dimensional colorimeter RC-300 manufactured by Paparab Co., Ltd. In this measurement, the interval between adjacent measurement points can be set to, for example, 13 μm.
[0078] When the zirconia sintered body of the present invention is applied to a dental material, if the chromaticity of the fourth point D is within the above range, the zirconia sintered body is prepared from the composition corresponding to the fourth point alone, and a sample having a thickness of 0.5 mm and mirror-finished on both sides is preferably 27% or more in light transmittance measured in accordance with JIS K 7361. Also, if the chromaticity of the first point A is within the above range, the zirconia sintered body is prepared from the composition corresponding to the first point alone, and a sample having a thickness of 0.5 mm and mirror-finished on both sides is preferably 10% or more in light transmittance measured in accordance with JIS K 7361.
[0079] When the zirconia sintered body of the present invention is applied to a dental material, the length L in the first direction Y of the zirconia sintered body 10 of the present invention preferably satisfies at least the length corresponding to the exposed part of a natural tooth. For example, the length L of the zirconia sintered body 10 is preferably 5 mm to 18 mm.
[0080] Next, the composition and calcined body for producing the zirconia sintered body of the present invention will be described. The composition and calcined body are precursors (intermediate products) of the zirconia sintered body of the present invention described above. The calcined body is obtained by firing (i.e., calcining) the composition at a temperature that does not lead to sintering. The calcined body also includes a molded product. For example, a dental prosthesis (e.g., a crown shape) obtained by processing a calcined zirconia disk using a CAD / CAM (Computer-Aided Design / Computer-Aided Manufacturing) system is also included in the calcined body.
[0081] The composition and calcined body of the present invention are produced by laminating zirconia powders having different compositions.
[0082] The composition and the calcined body contain (mainly monoclinic) zirconia crystal particles, a stabilizer, and titanium oxide. The composition may contain aluminum oxide. The aluminum oxide is preferably alpha alumina.
[0083] The average particle size of the zirconia powder (in a granular state) in the composition is preferably 20 μm to 40 μm.
[0084] Examples of the stabilizer in the composition and the calcined body include oxides such as calcium oxide (CaO), magnesium oxide (MgO), yttria, and cerium oxide (CeO2). The stabilizer is preferably added in an amount that can partially stabilize the zirconia particles in the sintered body. For example, when yttria is used as the stabilizer, the content of yttria is preferably 2.5 mol% to 4.5 mol%, more preferably 3 mol% to 4.5 mol%, and more preferably 3.5 mol% to 4.5 mol%, based on the total moles of zirconia and yttria.
[0085] The content of aluminum oxide in the composition and the calcined body is preferably 0% by mass (not contained) to 0.3% by mass based on the total mass of the zirconia crystal particles and the stabilizer. This is to increase the strength of the zirconia sintered body. If it is more than 0.3% by mass, the transparency of the zirconia sintered body decreases.
[0086] The content of titanium oxide in the composition and the calcined body is preferably 0% by mass (not contained) to 0.6% by mass based on the total mass of the zirconia crystal particles and the stabilizer. This is to grow the zirconia crystal grains. If it is more than 0.6% by mass, the strength of the zirconia sintered body decreases.
[0087] In the composition and calcined body of the present invention, the content of silicon oxide is preferably 0.1 mass % or less based on the total mass of the zirconia crystal particles and the stabilizer, and the composition and calcined body preferably do not substantially contain silicon oxide (SiO2; silica). This is because the transparency of the zirconia sintered body decreases if silicon oxide is contained. Here, "substantially does not contain" means that it is within a range that does not particularly affect the properties and characteristics of the present invention, and preferably does not contain more than the impurity level, and does not necessarily mean that it is below the detection limit.
[0088] The composition and calcined body of the present invention may contain a pigment for coloring. For example, when the zirconia sintered body produced from the composition and calcined body of the present invention is used as a dental material, examples of the pigment include chromium oxide (Cr2O3), erbium oxide (Er2O3), iron oxide (Fe2O3), praseodymium oxide (Pr6O 11 ) can be used. These pigments may be used in combination. The pigment content can be partially different.
[0089] For example, in the molded composition and calcined body, when the entirety is divided into four layers, with a region from the bottom end that accounts for 25% to 45% of the entire thickness being the first layer, a region on the first layer that accounts for 5% to 25% of the entire thickness being the second layer, a region on the second layer that accounts for 5% to 25% of the entire thickness being the third layer, and a region from the top of the third layer to the top end that accounts for 25% to 45% of the entire thickness being the fourth layer, it is preferable that the pigment content decreases from the first layer to the fourth layer.
[0090] For example, when the sintered body produced from the composition and the calcined body is used as a dental material, erbium oxide and iron oxide can be added as pigments. In this case, the first layer preferably has an erbium oxide content of 0.33 mass% to 0.52 mass% and an iron oxide content of 0.05 mass% to 0.12 mass% relative to the total mass of zirconia and the stabilizer. The second layer preferably has an erbium oxide content of 0.26 mass% to 0.45 mass% and an iron oxide content of 0.04 mass% to 0.11 mass% relative to the total mass of zirconia and the stabilizer. The third layer preferably has an erbium oxide content of 0.05 mass% to 0.24 mass% and an iron oxide content of 0.012 mass% to 0.08 mass% relative to the total mass of zirconia and the stabilizer. In the fourth layer, the content of erbium oxide is preferably 0% by mass to 0.17% by mass and the content of iron oxide is preferably 0% by mass to 0.07% by mass relative to the total mass of zirconia and the stabilizer. The contents of erbium oxide and iron oxide preferably decrease in order from the first layer to the fourth layer.
[0091] For example, when the sintered body produced from the composition and the calcined body is used as a dental material, erbium oxide, iron oxide, and chromium oxide can be added as pigments. For example, when the sintered body produced from the composition and the calcined body is used as a dental material, the first layer preferably has an erbium oxide content of 0.08% by mass to 0.37% by mass, an iron oxide content of 0.08% by mass to 0.15% by mass, and an chromium oxide content of 0.0008% by mass to 0.0012% by mass, relative to the total mass of zirconia and the stabilizer. The second layer preferably has an erbium oxide content of 0.06% by mass to 0.42% by mass, an iron oxide content of 0.06% by mass to 0.18% by mass, and an chromium oxide content of 0.0006% by mass to 0.001% by mass, relative to the total mass of zirconia and the stabilizer. In the third layer, the content of erbium oxide is preferably 0.06% by mass to 0.17% by mass, the content of iron oxide is preferably 0.018% by mass to 0.042% by mass, and the content of chromium oxide is preferably 0.0001% by mass to 0.0003% by mass, relative to the total mass of zirconia and the stabilizer. In the fourth layer, the content of erbium oxide is preferably 0% by mass to 0.12% by mass, the content of iron oxide is preferably 0% by mass to 0.001% by mass, and the content of chromium oxide is preferably 0% by mass to 0.0001% by mass, relative to the total mass of zirconia and the stabilizer. The contents of erbium oxide, iron oxide, and chromium oxide preferably decrease in order from the first layer to the fourth layer.
[0092] For example, when the sintered body produced from the composition and the calcined body is used as a dental material, erbium oxide, iron oxide and praseodymium oxide can be added as pigments. For example, when the sintered body produced from the composition and the calcined body is used as a dental material, the first layer preferably has an erbium oxide content of 0.08% by mass to 2.2% by mass, an iron oxide content of 0.003% by mass to 0.12% by mass, and an praseodymium oxide content of 0.003% by mass to 0.12% by mass, relative to the total mass of zirconia and the stabilizer. The second layer preferably has an erbium oxide content of 0.06% by mass to 1.9% by mass, an iron oxide content of 0.002% by mass to 0.11% by mass, and an praseodymium oxide content of 0.002% by mass to 0.11% by mass, relative to the total mass of zirconia and the stabilizer. In the third layer, it is preferable that the content of erbium oxide is 0.018 mass% to 1 mass%, the content of iron oxide is 0.008 mass% to 0.06 mass%, and the content of praseodymium oxide is 0.0008 mass% to 0.06 mass%, relative to the total mass of zirconia and the stabilizer. In the fourth layer, it is preferable that the content of erbium oxide is 0 mass% to 0.7 mass%, the content of iron oxide is 0 mass% to 0.05 mass%, and the content of praseodymium oxide is 0 mass% to 0.05 mass%, relative to the total mass of zirconia and the stabilizer. It is preferable that the contents of erbium oxide, iron oxide, and praseodymium oxide decrease in order from the first layer to the fourth layer.
[0093] The content of the pigment can be theoretically calculated from the amount added relative to the total mass of zirconia and stabilizer and the production method.
[0094] The calcined body of the present invention has a bending strength measured in accordance with JIS R1601 of preferably 38 MPa or more, more preferably 40 MPa or more, and even more preferably 42 MPa or more.
[0095] In the calcined body of the present invention, the above bending strength can be obtained in a three-point bending test, even if the load point is located at the boundary between layers when zirconia powders of different compositions are laminated, as shown in the manufacturing method described later. For example, when the bending strength is measured by the same test as the bending test of the sintered body described above, a higher strength can be obtained compared to a calcined body produced by simply laminating powders. In addition, even when the bending strength is measured by a test in which a load is applied to the boundary, a strength similar to that of a calcined body that is not laminated (without boundaries) can be obtained. In addition, even when the bending strength is measured by a test in which a load is applied to the boundary, a strength similar to that of a calcined body that is not laminated (without boundaries) can be obtained. In the calcined body of the present invention, the bending strength measured by applying a load to the boundary between layers is preferably 90% or more, more preferably 95% or more, of the bending strength of the region other than the boundary (for example, the bending strength of a calcined body produced under similar conditions (for example, the same calcination temperature and calcination time) from a composition that is not a laminate).
[0096] Even if the composition and calcined body of the present invention are subjected to a heat treatment for calcination or sintering, peeling does not occur at the boundary between layers of zirconia powders having different compositions, and overall deformation can be suppressed. Schematic diagrams of a test piece for measuring the amount of deformation during sintering are shown in Figs. 3 and 4. Fig. 3 is a schematic diagram of a two-layered laminate. Fig. 4 is a schematic diagram of a four-layered laminate. Fig. 5 is a schematic diagram for explaining a method for measuring the amount of deformation. For example, a composition is formed by laminating a plurality of zirconia powders having different compositions, and the composition is fired at 800°C to 1200°C for 2 hours to produce a calcined body. Then, as shown in Figs. 3 and 4, the calcined body is formed into a rectangular parallelepiped shape with dimensions of 50 mm wide x 10 mm high x 5 mm deep using a CAD / CAM system. This becomes the test piece. For example, the test piece 20 of the two-layered laminate shown in Fig. 3 has a first layer 21a and a second layer 21b. The thickness of the first layer 21a and the thickness of the second layer 21b are each 50% of the total thickness. The four-layer laminate test piece 22 shown in FIG. 4 has a first layer 23a, a second layer 23b, a third layer 23c, and a fourth layer 23d. The thickness of the first layer 23a and the fourth layer 23d are each 35% of the total thickness. The thickness of the second layer 23b and the third layer 23c are each 15% of the total thickness. In the test pieces 20 and 22, if the 50 mm×5 mm surface is the bottom surface (upper surface and lower surface), each layer extends in the same direction as the bottom surface 20a, 22a, and preferably extends parallel to the bottom surface 20a, 22a. In other words, the boundary between the layers is parallel to the bottom surface 20a, 22a. When this test piece is fired and sintered at 1500° C. for 2 hours, the bottom surfaces 20a, 22a are deformed so as to be curved. The test pieces 20, 22 are placed on a flat surface (ground surface 30) with the concave side of the bottom surface 20a, 22a facing down. Then, the width of the test pieces 20, 22 after deformation, that is, the distance L between the ground contact portions in the width direction, is measured. Also, the largest distance d between the bottom surface 20a, 22a deformed into a concave shape and the ground contact surface 30 is measured. Then, the amount of deformation is calculated as (d / L×100). This amount of deformation is preferably 0.15 or less, more preferably 0.1 or less, more preferably 0.05 or less, and even more preferably 0.03 or less.
[0097] The composition and calcined body produced by laminating zirconia powders with different compositions are easily deformed when sintered, but the composition and calcined body of the present invention can reduce the amount of deformation compared to the composition and calcined body produced by simply laminating. This can improve the dimensional accuracy of the final product. For example, the composition and calcined body of the present invention can be suitably applied to dental prostheses that vary greatly from person to person. In addition, in Figures 3 and 4, the mixed layer of the upper and lower layers that is assumed to be formed at the boundary between each layer is not shown for simplification.
[0098] The composition of the present invention includes powder, a fluid in which a powder is added to a solvent, and a molded body in which a powder is molded into a predetermined shape. That is, the composition may be in a powder form, a paste form, or a wet composition (that is, it may be in a solvent or may contain a solvent). The composition may also contain additives such as binders and pigments. In addition, the mass of additives such as solvents and binders is not taken into consideration in calculating the above content.
[0099] When the composition of the present invention is a molded product, it may be molded by any molding method, for example, press molding, injection molding, or stereolithography, or may be molded in multiple stages. For example, the composition of the present invention may be press molded and then further subjected to CIP (Cold Isostatic Pressing) treatment.
[0100] The calcined body of the present invention can be obtained by firing the composition of the present invention at 800° C. to 1200° C. under normal pressure.
[0101] The calcined body of the present invention becomes the zirconia sintered body of the present invention by firing at 1350° C. to 1600° C. under normal pressure.
[0102] It is preferable to determine the length (thickness) of the composition and the calcined body in the stacking direction, taking into consideration sintering shrinkage, so that the sintered body achieves a target length. For example, when the sintered body produced from the composition and the calcined body is used as a dental material, the target length of the sintered body in the stacking direction is 5 mm to 18 mm, and the length (thickness) of the composition and the calcined body in the stacking direction can be set to 10 mm to 26 mm.
[0103] Next, an example of a method for producing the composition, calcined body, and sintered body of the present invention will be described. Here, a method for gradually changing the color of the sintered body (creating gradation) will also be described.
[0104] First, zirconia and a stabilizer are wet mixed in water to form a slurry. The slurry is then dried and granulated. The granulated material is then calcined to produce the primary powder.
[0105] Next, in the case where a sintered body is to have a gradation, the primary powder is divided into two. Next, a pigment is added to at least one of the two primary powders so that there is a difference in the pigment addition rate. For example, one of the primary powders may not have a pigment added, and the other may have a pigment added. Hereinafter, the powder with a lower specific pigment addition rate is referred to as a low-addition rate powder, and the secondary powder with a higher specific pigment addition rate is referred to as a high-addition rate powder. It is preferable that the pigment addition amount in the high-addition rate powder is matched to the addition amount in the darkest color region of the sintered body. Then, for each of the powders, zirconia is crushed and mixed in water until it has a desired particle size to form a zirconia slurry. Next, the slurry is dried and granulated to produce a secondary powder. When additives such as aluminum oxide, titanium oxide, and binder are added, they may be added when producing the primary powder or when producing the secondary powder.
[0106] Next, a plurality of powders with different pigment content ratios are prepared based on the secondary powders of low and high additive ratio powders. For example, when preparing the above-mentioned four-layer composition and calcined body, the first powder for the first layer is 100% high additive ratio powder without mixing low additive ratio powder. The second powder for the second layer is mixed in a ratio of low additive ratio powder: high additive ratio powder = 5:95 to 15:85. The third powder for the third layer is mixed in a ratio of low additive ratio powder: high additive ratio powder = 35:65 to 45:55. The fourth powder for the fourth layer is mixed in a ratio of low additive ratio powder: high additive ratio powder = 45:55 to 55:45. As another mixing ratio, for example, when preparing the above-mentioned four-layer composition and calcined body, the first powder for the first layer is 100% high additive ratio powder without mixing low additive ratio powder. The second powder for the second layer is mixed in a ratio of low additive powder: high additive powder = 10:90 to 30:70. The third powder for the third layer is mixed in a ratio of low additive powder: high additive powder = 70:30 to 90:10. The fourth powder for the fourth layer is 100% low additive powder without mixing in the high additive powder.
[0107] When the zirconia sintered body is used as a dental material, it is preferable to make the blending difference between the second and third layers larger than the blending difference between the first and second layers and the blending difference between the third and fourth layers. This makes it possible to reproduce the same color change as that of natural teeth.
[0108] In this way, by using two types of powder that have different colors as the base for the sintered body and adjusting the pigment content of each layer, it is possible to naturally change color (create a gradation) by layering each powder in sequence.
[0109] When layering for purposes other than coloring, the secondary powder is divided into layers according to the number of layers to be layered. Desired additives may be added to each powder.
[0110] Next, multiple powders with different pigment contents are layered in order. When forming a gradation in the sintered body, it is preferable to layer the powders so that the addition rate of a specific pigment increases or decreases stepwise in the order of layering. First, the first layer of powder is filled into the mold, and then the top surface of the powder of the first layer is made flat. As a method for making the surface flat, for example, a method of vibrating the mold or a method of grinding the top surface of the powder of the first layer can be adopted. However, it is preferable not to perform a pressing process until all layers are layered. Next, the powder of the second layer is filled on top of the powder of the first layer. Next, vibration is applied to the mold. The vibration is transmitted to the powder in the mold. As a method for applying vibration, for example, a mechanical vibration is applied to the mold, the mold is manually shaken, the mold is hit with a hammer, or any other suitable method can be adopted. As a result, it is considered that the powder of the first layer and the powder of the second layer are partially mixed at the boundary between the powder of the first layer and the powder of the second layer. That is, the number and strength of vibrations, or in the case of mechanical vibration, the frequency and amplitude, etc., can be appropriately set according to the particle size, particle size distribution, particle shape, etc. of the powder so that the powders of the upper and lower layers are mixed at the boundary between the layers. Next, the top surface of the powder of the second layer is smoothed in the same manner as the powder of the first layer. This process is repeated until all layers are laminated.
[0111] For example, when preparing the above-mentioned composition and calcined body having a total of four layers, the first powder is filled into a mold to a predetermined thickness (for example, 25% to 45% of the total thickness). At this time, the upper surface of the first powder is made flat and level, but is not subjected to a pressing process. Next, the second powder is filled on the first powder to a predetermined thickness (for example, 5% to 25% of the total thickness). Next, vibration is applied to the mold. It is presumed that this vibration forms a first boundary layer in which the first powder and the second powder are mixed at the boundary between the upper surface of the first powder and the lower surface of the second powder. Next, the upper surface of the second powder is made flat and level. The second powder is not subjected to a pressing process before filling with the third powder. Next, the third powder is filled on the second powder to a predetermined thickness (for example, 5% to 25% of the total thickness). Next, vibration is applied to the mold. It is presumed that this vibration forms a second boundary layer in which the second powder and the third powder are mixed at the boundary between the upper surface of the second powder and the lower surface of the third powder. Next, the upper surface of the third powder is made flat and level. The third powder is not subjected to a pressing process before the fourth powder is filled. Next, the fourth powder is filled on top of the third powder to a predetermined thickness (for example, 25% to 45% of the total thickness). Next, vibration is applied to the mold. It is presumed that this vibration forms a third boundary layer in which the third powder and the fourth powder are mixed at the boundary between the upper surface of the third powder and the lower surface of the fourth powder.
[0112] After all layers are laminated, the laminate is press molded to produce a molded product of the composition of the present invention. The molded product may further be subjected to CIP treatment.
[0113] By not performing a pressing process before filling the powder of the next layer and by applying vibration each time a layer is filled, it is believed that a boundary layer where the powders of the upper and lower layers are mixed can be formed between adjacent layers. This can increase the adhesion between adjacent layers in the sintered body. The amount or speed of shrinkage during heat treatment can be made equal for each layer, preventing peeling between layers during heat treatment and preventing the sintered body from deforming distortedly relative to the target shape. Furthermore, the color difference between adjacent layers can be mitigated. This allows the color to change naturally in the stacking direction in the sintered body (creating a gradation).
[0114] In addition, this method does not require an intermediate layer between each of the main layers. In other words, when stacking four main layers, it is sufficient to stack only four layers. Also, there is no need to press each layer. This greatly reduces the labor and time required, and reduces the manufacturing cost.
[0115] When the calcined body is not prepared, the zirconia powder is sintered by firing the composition at 1400° C. to 1600° C., preferably 1450° C. to 1550° C., to produce the zirconia sintered body of the present invention. The zirconia sintered body may be formed into a desired shape at the stage of the molded product.
[0116] When preparing the calcined body, the composition is fired at 800°C to 1200°C to prepare the calcined body. Next, the calcined body is fired at 1400°C to 1600°C, preferably 1450°C to 1550°C, to sinter the zirconia powder and produce the zirconia sintered body of the present invention. The shaping may be performed by cutting or the like at the stage of the calcined body, or may be performed after sintering. The shaping may be performed by a CAD / CAM system.
[0117] The method for producing a dental prosthesis is the same as the above-mentioned method for producing a sintered body, except that the calcined body or sintered body is formed into a crown shape.
[0118] In the above embodiment, the composition, calcined body, and sintered body based on a four-layer laminate are exemplified, but are not limited to four layers. For example, the composition, calcined body, and sintered body may be made from a two-layer laminate of the first and fourth layers described above. Alternatively, the composition, calcined body, and sintered body may be made from a three-layer laminate of the first, second, and fourth layers, or the first, third, and fourth layers described above. Also, FIG. 2 is intended to facilitate the explanation of the positional relationship and direction of each point, and the shape and dimensions are not limited to the form shown in FIG. 2. EXAMPLES
[0119] [Examples 1 to 4] [Production of composition, calcined body and sintered body] Zirconia powders with different compositions were layered to produce sintered bodies, and their bending strength, color, and deformation were measured.
[0120] First, zirconia powder containing a stabilizer was prepared. 7.2 mass% (4 mol%) of yttria was added as a stabilizer to 92.8 mass% of mainly monoclinic zirconia powder. Alumina sol was added to the mixed powder of zirconia and yttria (100 mass%) so that 0.1 mass% of alumina was added, and 150 mass% of water, 0.2 mass% of antifoaming agent, and 1 mass% of dispersing agent were added to the mixed powder of zirconia and yttria (100 mass%), and this mixture was pulverized in a ball mill for 10 hours. The average particle size of the slurry obtained after pulverization was 0.12 μm. Next, the mixture was granulated using a spray dryer, and the granules obtained were calcined at 1000° C. for 2 hours to produce a primary powder.
[0121] Next, the primary powder was divided into two, and a pigment was added to at least one of them. The one with a lower pigment addition rate was designated as the low-addition rate powder, and the one with a higher pigment addition rate was designated as the high-addition rate powder. Table 1 shows the addition rates of Examples 1 to 3. Table 4 shows the addition rate of Example 4. The values shown in Tables 1 and 2 are the addition rates relative to the mixed powder of zirconia and yttria (100 mass%). In addition, 0.2 mass% of titania, 200 mass% of water, 0.2 mass% of an antifoaming agent, and 1 mass% of a dispersing agent were added to each powder relative to the mixed powder of zirconia and yttria (100 mass%), and the mixture was pulverized in a ball mill for 15 hours. The average particle size of the slurry obtained after pulverization was 0.13 μm. Next, 6 mass% of a binder and 0.5 mass% of a release agent were added, and mixed in a ball mill for 15 minutes. Next, the resulting slurry was granulated using a spray dryer to produce secondary powders of low and high additive ratio powders.
[0122] Next, the low-addition ratio powder and the high-addition ratio powder were mixed in the ratios shown in Tables 3 to 6 to prepare first to fourth powders.
[0123] Next, a molded body was produced. In Examples 1, 3, and 4, 35 g of the first powder was filled into a mold having an inner dimension of 82 mm x 25 mm, and the upper surface of the first powder was smoothed by grinding the upper surface. Next, 15 g of the second powder was filled on the first powder, and the mold was vibrated by a vibration device. Then, the upper surface of the second powder was smoothed by grinding the upper surface of the second powder. Next, 15 g of the third powder was filled on the second powder, and the mold was vibrated by a vibration device. Then, the upper surface of the third powder was smoothed by grinding the upper surface of the third powder. Next, 35 g of the fourth powder was filled on the third powder, and the mold was vibrated by a vibration device. Then, the upper surface of the fourth powder was smoothed by grinding the upper surface of the fourth powder. In Example 2, 50 g of the first powder was filled, and 50 g of the second powder was filled, but the same as in Examples 1, 3, and 4. Next, the upper mold is set and the uniaxial press molding machine is used to apply a surface pressure of 200 kg / cm 2 The primary press molding was then performed at 1500 kg / cm for 90 seconds. 2 The mixture was subjected to CIP molding at 40° C. for 5 minutes to prepare a green body.
[0124] Next, the molded body was fired at 1000°C for 2 hours to produce a calcined body. Next, it was molded into a crown shape using a CAD / CAM system (Katana System, Kuraray Noritake Dental Co., Ltd.). Next, the calcined body was fired at 1500°C for 2 hours to produce a sintered body. The length of the sintered body in the layering direction of the first to fourth powders was 18 mm.
[0125] In all of the sintered bodies of Examples 1 to 4, a gradation was formed in which the color changed from light yellow to yellow-white from the region corresponding to the first layer of the composition to the region corresponding to the fourth layer, and the bodies had an appearance similar to that of natural teeth.
[0126] [Table 1]
[0127] [Table 2]
[0128] [Table 3]
[0129] [Table 4]
[0130] [Table 5]
[0131] [Table 6]
[0132] [Measurement of bending strength] The bending strength of the calcined body and the sintered body produced in Example 4 was measured in accordance with JISR1601. As a comparative example, the bending strength of the calcined body and the sintered body to which no vibration was applied when filling each powder was also measured. Comparative Example 1 is a calcined body and a sintered body produced from a composition that was not subjected to a press treatment each time each layer was filled. Comparative Example 2 is a calcined body and a sintered body produced from a composition that was subjected to a press treatment each time each layer was filled. The bending strength was measured in accordance with JISR1601. However, the test piece was cut out along the lamination direction in the longitudinal direction. The part of the test piece that corresponds to the boundary (mixed layer) between the powders extends along the load application direction (along the smallest area direction) and crosses the test piece. The bending strength was measured by adjusting the load point of the three-point bending test to the position of the part of the test piece that corresponds to the mixed layer between the second powder and the third powder, and the results are shown in Table 7.
[0133] For the calcined body, the bending strength of Example 4 was 40 MPa or more, while the bending strength of the comparative example was 36 MPa or less. This shows that the bonding strength between layers can be increased at the calcined body stage by applying vibration when stacking the powder. For the sintered body, the bending strength was 1200 MPa or more in Example 4, while Comparative Examples 1 and 2 were less than 1100 MPa, which was 100 MPa or more lower than Example 4. It can be seen that the bonding strength between layers can be increased for the sintered body as well.
[0134] In addition, as shown in Example 9 below, the bending strength of Example 4 is the same as that of a sintered body produced without lamination, for both the sintered body and the calcined body, and it is found that lamination does not cause a decrease in bonding strength. This shows that by applying vibration during powder lamination, the boundaries between the layers have the same strength as the areas other than the boundaries, for both the sintered body and the calcined body.
[0135] This is believed to be primarily because vibration was applied when the powder layers were stacked, causing the powders in the upper and lower layers to partially mix at the boundaries, increasing the bonding strength between the layers, and secondarily because the first to fourth powders were made by mixing two types of powder, which reduced the difference in properties between the powders and made them easier to blend.
[0136] [Table 7]
[0137] [Measurement of fracture toughness] The fracture toughness of the sintered body produced in Example 4 was measured in accordance with JIS R 1607. The position of the boundary in the test piece was the same as in the bending test described above. The pressing tool was also aligned with the position of the boundary between the second powder and the third powder. As a result, the fracture toughness was 4.3 MPa m 1 / 2 As shown in Example 9 below, this value is similar to the fracture toughness of a sintered body produced without lamination, and it is understood that lamination does not cause a decrease in fracture toughness.
[0138] [Measurement of shrinkage and deformation during sintering] In Example 4, the calcined body was calcined at 1000°C for 2 hours to prepare the test pieces shown in Figs. 3 and 4, which were then fired at 1500°C for 2 hours to measure the deformation (d / L x 100). The method for measuring the deformation was the same as that described above. As comparative examples, the same test pieces were prepared for Comparative Example 1 and Comparative Example 2 in the same manner as in the bending test, and the deformation after sintering was measured. Table 8 shows the measurement results.
[0139] In the comparative examples, the deformation amount was 0.15 or more. On the other hand, in Example 4, the deformation amount was 0.05 or less, and it can be seen that the deformation amount was significantly suppressed compared to the comparative examples. From this, it is considered that shrinkage deformation during sintering can be suppressed by applying vibration to the composition when powders with different compositions are layered.
[0140] In addition, comparing Comparative Example 1 and Comparative Example 2, the amount of deformation is smaller in Comparative Example 1. From this, it is considered that shrinkage deformation during sintering can be more effectively suppressed by not carrying out the press treatment after filling each layer.
[0141] Furthermore, when comparing the 2-layer laminate with the 4-layer laminate, the amount of deformation is smaller in the 4-layer laminate than in the 2-layer laminate, which suggests that shrinkage deformation can be suppressed more effectively by increasing the number of layers.
[0142] [Table 8]
[0143] [Measurement of chromaticity and color difference] For each of the first, second, third, and fourth powders in Examples 1 to 4, a single sintered body was produced, and the L * a * b *The chromaticity was measured according to the color system. The sintered body was processed into a disk with a diameter of 14 mm and a thickness of 1.2 mm, both sides of which were polished, and then the chromaticity was measured using an Olympus measuring device CE100-DC / US. Based on the chromaticity measurement results, the color difference ΔE between adjacent layers was also measured. * ab 1~3 In addition, the color difference ΔE between the first and fourth layers was calculated. * ab4 was calculated. Then, (ΔE * ab1+ΔE * ab2+ΔE * ab3)-ΔE * ab4 was calculated. Chromaticity is shown in Tables 9 to 12. Color difference is shown in Table 13.
[0144] The chromaticity of the sintered body of each powder is considered to represent the chromaticity of the color partially exhibited by the zirconia sintered body.
[0145] In the sintered body of the first layer of the four-layer laminate, L * 58~73, a * is 0 to 8, b * In the sintered body of the second layer, L * 64~73, a * is 0 to 6, b * In the sintered body of the third layer, L * 70~78, a * is -2 to 2, b * In the sintered body of the fourth layer, L * 72~84, a * is -2 to 1, b * was 4 to 15.
[0146] The color difference between the sintered body of the first layer and the sintered body of the second layer was 7 to 14. The color difference between the sintered body of the second layer and the sintered body of the third layer was 10 to 18. The color difference between the sintered body of the third layer and the sintered body of the fourth layer was 4 to 9. The color difference between the sintered body of the first layer and the sintered body of the fourth layer was 28 to 36. The value obtained by subtracting the color difference between the sintered body of the first layer and the sintered body of the fourth layer from the sum of the color differences between the sintered body of the first layer and the sintered body of the second layer, the sintered body of the second layer and the sintered body of the third layer, and the sintered body of the third layer and the sintered body of the fourth layer was 1 or less.
[0147] [Table 9]
[0148] [Table 10]
[0149] [Table 11]
[0150] [Table 12]
[0151] [Table 13]
[0152] [Example 5] [b * Measurement of change in value A low-addition powder and a high-addition powder were prepared by adding pigments to a mixed powder of zirconia and yttria (100 mass%) at the addition rates shown in Table 14, and compositions were prepared at the blending ratios shown in Table 15. Sintered bodies were prepared in the same manner as in Examples 1 to 4, and the L * a * b * Color space b * The change in the value was measured. Figure 6 shows a schematic diagram of the prepared test piece and the measurement results. The upper diagram of Figure 6 is a schematic diagram of the test piece, showing the dimensions and the measurement direction. The lower diagram of Figure 6 is a graph showing the measurement results. The sintered test piece was prepared to have dimensions of 20 mm x 20 mm x 1 mm after sintering. The first layer is the area filled with the first powder, and the fourth layer is the area filled with the fourth powder. b *The values were measured using a Paparab RC-300 two-dimensional colorimeter, with a test piece placed in the center of an image measuring 29 mm x 22 mm, and scanned in a direction perpendicular to the boundary surface of each layer at intervals of about 13 μm. The values on the X-axis of the graph in the lower part of FIG. 6 indicate the number of measurement points. As Comparative Example 3, a sintered body was produced by applying no vibration when stacking the powder for each layer, and by carrying out a press treatment each time each layer was filled, and the b * The composition and blending ratio of the low-addition rate powder and the high-addition rate powder in Comparative Example 3 are the same as those in Example 5. Fig. 7 shows a schematic diagram of the test piece and the measurement results.
[0153] Looking at the graph in Figure 7, in the center of each layer, b * The value tends to be flat. Also, at the boundary between layers, there is a steep step-like * The value also changes. This is thought to be because the powders in each layer, which have different pigment compositions, are sintered independently. According to this, the appearance of the test piece in Comparative Example 3 does not show a clear gradation. On the other hand, looking at the graph in Figure 6, even in the center of each layer, * The value shows a gradual increase. In addition, at the boundaries between layers, there is a step-like b * No change in value is observed, making it difficult to determine where the boundaries are. In particular, there is a linear transition at the boundaries between the first and second layers and between the third and fourth layers. This shows that a beautiful gradation is formed in the appearance of the sintered body of the present invention. This result is believed to be due to the fact that, in the present invention, vibration is applied when the first to fourth powders are packed, which causes the powders to mix between adjacent layers near the boundaries between the upper and lower layers, thereby reducing the difference in pigment content between adjacent layers. Note that, since the difference in pigment content between the second and third powders is large, the b in the graph * It is believed that the change in value is also more rapid than in other areas.
[0154] [Table 14]
[0155] [Table 15]
[0156] [Examples 6 to 15] A sintered body for a dental prosthesis was produced based on a composition produced by laminating zirconia powders with different pigment compositions. The chromaticity of the sintered body of each powder used as the base of each layer was measured. Furthermore, the bending strength, fracture toughness, and monoclinic peak ratio after hydrothermal treatment were measured for the sintered body of Example 9.
[0157] First, a primary powder was prepared in the same manner as in Examples 1 to 4. Next, the primary powder was divided into four. These powders were designated as the first to fourth powders. In Examples 6 to 15, pigments shown in Tables 6 to 16 below were added to each powder. The values shown in the tables are the addition rates relative to the mixed powder of zirconia and yttria (100 mass%). Then, secondary powders of the first to fourth powders were prepared in the same manner as in Examples 1 to 4, except that low and high addition rate powders were not prepared and the pigment addition rates were different.
[0158] Next, a green body was produced in the same manner as in Examples 1 to 4. The green body was then fired at 1000°C for 2 hours to produce a calcined body. The green body was then formed into a crown shape using a CAD / CAM system (Katana System, Kuraray Noritake Dental Co., Ltd.). The calcined body was then fired at 1500°C for 2 hours to produce a sintered body. The length of the sintered body in the layering direction of the first to fourth powders was 8 mm.
[0159] In all of the sintered bodies of Examples 6 to 16, a gradation was formed in which the color changed from light yellow to yellow-white from the region corresponding to the first layer of the composition to the region corresponding to the fourth layer, and the bodies had an appearance similar to that of natural teeth.
[0160] [Table 16]
[0161] [Table 17]
[0162] [Table 18]
[0163] [Table 19]
[0164] [Table 20]
[0165] [Table 21]
[0166] [Table 22]
[0167] [Table 23]
[0168] [Table 24]
[0169] [Table 25]
[0170] The chromaticity and color difference of the sintered bodies of the first powder, the second powder, the third powder, and the fourth powder were measured in the same manner as in Examples 1 to 4. The chromaticity is shown in Tables 26 to 35. The color difference is shown in Tables 36 to 37.
[0171] The chromaticity of each powder is considered to represent the chromaticity of each point of the zirconia sintered body made from a laminate of multiple powders. The combination of the four sintered bodies in Example 9 exhibited a light color as a whole. The combination of the four sintered bodies in Example 10 exhibited a dark color as a whole.
[0172] In the first layer of sintered body, L * 58~76, a * -2 to 8, b * In the sintered body of the second layer, L * 66~81, a * -2 to 6, b * In the sintered body of the third layer, L * 69-83, a * is -2 to 2, b * In the sintered body of the fourth layer, L * 71-84, a * is -2 to 1, b * was 2 to 15.
[0173] The color difference between the sintered body of the first layer and the sintered body of the second layer was 3 to 15. The color difference between the sintered body of the second layer and the sintered body of the third layer was 1 to 11. The color difference between the sintered body of the third layer and the sintered body of the fourth layer was 1 to 4. The color difference between adjacent layers tended to become smaller from the first layer to the fourth layer. In addition, the color difference between the sintered body of the first layer and the sintered body of the fourth layer was 8 to 29. The value obtained by subtracting the color difference between the sintered body of the first layer and the sintered body of the fourth layer from the total color difference between the sintered body of the first layer and the sintered body of the second layer, the color difference between the sintered body of the second layer and the sintered body of the third layer, and the color difference between the sintered body of the third layer and the sintered body of the fourth layer was 1 or less.
[0174] [Table 26]
[0175] [Table 27]
[0176] [Table 28]
[0177]
Table 29
[0178]
Table 30
[0179]
Table 31
[0180]
Table 32
[0181]
Table 33
[0182]
Table 34
[0183]
Table 35
[0184]
Table 36
[0185]
Table 37
[0186] For each of the first, second, third, and fourth powders in Example 9, a single zirconia sintered body was prepared, and the bending strength, fracture toughness, and monoclinic peak ratio after hydrothermal treatment were measured. The measurement results are shown in Table 38. The bending strength of the zirconia sintered body was measured in accordance with JIS R1601. The fracture toughness of the zirconia sintered body was measured in accordance with JIS R1607. The hydrothermal treatment test was performed in accordance with ISO 13356 under conditions of 180°C, 1 MPa, and 5 hours. After the hydrothermal treatment test, the X-ray diffraction pattern of the zirconia sintered body was measured using CuKα radiation, and the monoclinic peak ratio, i.e., the degree of phase transition to monoclinic due to the hydrothermal treatment test, was measured. All sintered bodies had a bending strength of 1200 MPa or more and a fracture toughness of 4 MPa m 1 / 2 The peak ratio of the monoclinic phase was also less than 1. The zirconia sintered bodies in the other examples have the same composition, so it is expected that similar results will be obtained. The test results for bending strength and fracture toughness were similar to the values obtained when a load was applied to the boundary of the laminate.
[0187] The bending strength of the calcined body produced by firing the second powder at 1000°C for 2 hours was also measured in accordance with JIS R 1601. The bending strength of the calcined body of the second powder was 41 MPa. This value was the same as the value when a load was applied to the boundary of the laminate.
[0188] [Table 38]
[0189] [Example 16] In the above examples, the content of yttria was 4 mol% in terms of the total mole number of zirconia and yttria, but in Example 16, a sintered body with 3 mol% yttria was produced and the chromaticity was measured. The sintered body used for the measurement was the same as that in Example 4 shown in Tables 14 and 15, except for the yttria content. Table 39 shows the measurement results. Compared with the chromaticity shown in Table 12, when the yttria content was reduced, the L * tends to decrease, and a * and b * There was a tendency for the number of cases to increase.
[0190] [Table 39]
[0191] The zirconia sintered body, and the composition and calcined body for the zirconia sintered body of the present invention have been described based on the above embodiment, but needless to say, they are not limited to the above embodiment and can include various modifications, changes, and improvements to the various disclosed elements (including each element of each claim, each element of each embodiment or example, each element of each drawing, etc.) within the scope of the present invention and based on the basic technical idea of the present invention. Furthermore, various combinations, substitutions, or selections of the various disclosed elements (including each element of each claim, each element of each embodiment or example, each element of each drawing, etc.) are possible within the scope of the claims of the present invention.
[0192] Further objects, objectives and developments of the present invention will become apparent from the entire disclosure of the present invention, including the claims.
[0193] For numerical ranges set forth herein, any numerical value or subrange contained within the range should be construed as specifically set forth unless expressly stated otherwise.
[0194] A part or all of the above-described embodiments may be described as follows, but is not limited to the following description. [Appendix 1] A plurality of zirconia powders having different compositions containing zirconia and a stabilizer that inhibits phase transition of zirconia are formed, The plurality of zirconia powders are laminated to form a zirconia composition; A zirconia calcined body produced by firing the zirconia composition at 800 ° C to 1200 ° C, The calcined body was molded into a rectangular parallelepiped shape having dimensions of 50 mm in width × 10 mm in height × 5 mm in depth to prepare a test piece, and when the surface of the test piece that is 50 mm in width × 5 mm in depth is set as a bottom surface, the boundary surface formed by the lamination of the zirconia powder is parallel to the bottom surface, The test piece was sintered at 1500°C for 2 hours. When the bottom surface that is deformed into a concave shape is placed on the bottom, A zirconia calcined body, characterized in that (maximum distance between the bottom surface deformed into a concave surface and the ground surface) / (distance between the ground contact portions in the width direction)×100 is 0.15 or less. [Appendix 2] The zirconia calcined body according to the appendix, characterized in that (maximum distance between the bottom surface deformed into a concave surface and the ground surface) / (distance between the grounding portions in the width direction)×100 is 0.1 or less. [Appendix 3] The zirconia calcined body according to the appendix, wherein the plurality of zirconia powders contain a pigment, and each of the zirconia powders has a different pigment content. [Appendix 4] A zirconia sintered body, characterized in that it is produced by a method including a step of sintering the zirconia calcined body described in the appendix at 1400°C to 1600°C. [Appendix 5] A step of preparing a plurality of lamination powders containing zirconia, a stabilizer for suppressing a phase transition of the zirconia, and a pigment, the plurality of lamination powders having different pigment contents; and a lamination step of laminating a plurality of the lamination powders in a mold, A method for producing a zirconia composition, wherein in the lamination step, after filling at least two of the lamination powders into the mold, the mold is vibrated. [Appendix 6] The method for producing a zirconia composition according to the appendix, wherein in the lamination step, the mold is vibrated every time one of the lamination powders is filled into the mold. [Appendix 7] A step of preparing a low-additive powder and a high-additive powder containing zirconia, a stabilizer for suppressing a phase transition of the zirconia, and a pigment, the low-additive powder and the high-additive powder having different contents of the pigment; a mixing step of mixing the low-additive powder and the high-additive powder to produce at least one lamination powder; a lamination step of laminating at least two powders among the low additive ratio powder, the high additive ratio powder, and the lamination powder in a mold; A method for producing a zirconia composition comprising the steps of: [Appendix 8] The method for producing a zirconia composition according to the appendix, wherein in the lamination step, after filling the at least two powders into the mold, the mold is vibrated. [Appendix 9] In the mixing step, two or more lamination powders having different mixing ratios of the low-additive powder and the high-additive powder are prepared, The method for producing a zirconia composition according to the appendix, characterized in that in the layering step, a plurality of powders are layered so that the content of the low addition rate powder or the high addition rate powder changes in sequence. [Appendix 10] The method for producing a zirconia composition according to the appendix, wherein in the layering step, after one powder is filled into the mold, the upper surface of the powder is smoothed. [Appendix 11] The method for producing a zirconia composition according to the appendix, wherein in the layering step, the powder is layered so that the pigment content in the powder changes sequentially. [Appendix 12] A method for producing a zirconia composition according to the appendix; Firing the composition at 800°C to 1200°C; A method for producing a zirconia calcined body, comprising: [Appendix 13] A method for producing a zirconia composition according to the appendix; Firing the composition at 1400°C to 1600°C; A method for producing a zirconia sintered body, comprising: [Appendix 14] A method for producing a zirconia calcined body according to the appendix; Firing the calcined body at 1400 ° C to 1600 ° C; A method for producing a zirconia sintered body, comprising: [Industrial Applicability]
[0195] The zirconia sintered body of the present invention can be used for various applications such as dental materials such as prostheses, optical fiber connection parts such as ferrules and sleeves, various tools (e.g., grinding balls, grinding tools), various parts (e.g., screws, bolts and nuts), various sensors, electronics parts, decorative items (e.g., watch bands), etc. When the zirconia sintered body is used as a dental material, it can be used, for example, for copings, frameworks, crowns, crown bridges, abutments, implants, implant screws, implant fixtures, implant bridges, implant bars, brackets, denture bases, inlays, onlays, onlays, orthodontic wires, laminate veneers, etc. [Explanation of symbols]
[0196] 10 Zirconia sintered body 20,22 Calcined body 20a, 22a Bottom 21a, 21b 1st layer, 2nd layer 23a~23d 1st~4th layer 30 Ground plane A~D 1st point~4th point P one end Q Other end X 1st direction Y Second direction
Claims
1. A dental zirconia sintered body, which contains zirconia and yttria as a stabilizer for suppressing phase transition of zirconia, and is in a state of being sintered by laminating and molding a plurality of zirconia powders having different compositions due to different pigment contents, A sintered body test piece cut out from the dental zirconia sintered body along the lamination direction in the longitudinal direction, The test condition is that the flexural strength of the sintered compact test piece is 1100 MPa or more, the flexural strength being measured by adjusting the load point of a three-point bending test to the position of the boundary between the sintered compact test pieces in accordance with JIS R1601 and the boundary between the sintered compact test pieces is in a load application direction. Contains at most 0.3% by weight of aluminum oxide, A dental zirconia sintered body characterized by:
2. A dental zirconia sintered body, which contains zirconia and yttria as a stabilizer for suppressing phase transition of zirconia, and is in a state in which a laminate formed by laminating and molding a plurality of zirconia powders having different compositions due to different pigment contents is sintered, A sintered body test piece cut out from the dental zirconia sintered body along the lamination direction in the longitudinal direction, The test condition is satisfied in accordance with JIS R1601, in which the flexural strength of the sintered compact test piece, in which the boundaries of the plurality of zirconia powders are present across the sintered compact test piece in the load application direction, is measured by adjusting the load point of a three-point bending test to the position of the boundaries, and is 90% or more of the flexural strength of another sintered compact test piece obtained by sintering one of the zirconia powders alone at the same sintering temperature as the sintering temperature of the sintered compact test piece. Contains at most 0.3% by weight of aluminum oxide, A dental zirconia sintered body characterized by:
3. A calcined body test piece cut out from the dental zirconia calcined body in the calcined state of the laminated body along the lamination direction in the longitudinal direction is The calcined test piece is in conformity with JIS R1601, and the boundaries of the plurality of zirconia powders are present so as to cross the calcined test piece in the load application direction. The bending strength measured by adjusting the load point of a three-point bending test to the position of the boundaries is 90% or more of the bending strength of another calcined test piece obtained by calcining one of the zirconia powders alone at the same calcination temperature as the calcined test piece. The dental zirconia sintered body according to claim 1 or 2.
4. A dental zirconia sintered body as described in any one of claims 1 to 3, characterized in that the laminate has a mixed layer in which the zirconia powder of the upper and lower layers is partially mixed at the boundary between each layer.
5. On a straight line extending in a first direction from one end to the other end, L of the first point in the section from the one end to 25% of the total length * a * b * Chromaticity according to the color system (L * , a * , b * ) is (L1, a1, b1), The second point L in the section from the other end to 25% of the total length * a * b * Chromaticity according to the color system (L * , a * , b * ) is (L2, a2, b2), On the straight line connecting the first point and the second point, L from the first point to the second point * There is no interval where the value decreases by 1 or more, From the first point to the second point, * There is no interval where the value increases by 1 or more, b from the first point to the second point * There is no interval where the value increases by 1 or more. The dental zirconia sintered body according to any one of claims 1 to 4.
6. A third point between the first point and the second point on a straight line connecting the first point and the second point is L * a * b * Chromaticity according to the color system (L * , a * , b * ) is (L3, a3, b3), L of a fourth point between the third point and the second point * a * b * Chromaticity according to the color system (L * , a * , b * ) is (L4, a4, b4), At the first point, the third point, the fourth point, and the second point, L at two adjacent points * The difference between the values is ΔL * year, a at two adjacent points * The difference between the values is Δa * year, b at two adjacent points * The difference between the values is Δb * year, From the following formula 1, ΔE * When ab is calculated, ΔE between the first point and the third point * ab is equal to or greater than 3.7 and equal to or less than 14.3; ΔE between the third point and the fourth point * ab is equal to or greater than 1.8 and equal to or less than 10.5, ΔE between the fourth point and the second point * ab is 1.0 or more and 9.0 or less; The dental zirconia sintered body according to claim 5 . [Formula 1]
7. The color changes in a first direction from one end to the other end, On the straight line from the one end to the other end, * a * b *The dental zirconia sintered body according to any one of claims 1 to 6, characterized in that the tendency of chromaticity to increase or decrease according to a color system does not change.
8. On a straight line connecting the one end and the other end, a distance L is measured from a first point located in a section from the one end to 25% of the total length to a second point located in a section from the other end to 25% of the total length. * The value is on the rise, * Value and b * The dental zirconia sintered body according to claim 7, characterized in that the value tends to decrease.
9. The dental zirconia sintered body according to any one of claims 5 to 8, characterized in that the color does not change along a second direction perpendicular to the first direction.
10. At two points on a line extending in the second direction, L between the two points * The difference between the values is ΔL * year, a between the two points * The difference between the values is Δa * year, b between the two points * The difference between the values is Δb * year, From the following formula 2, ΔE * When ab is calculated, ΔE * The dental zirconia sintered body according to claim 9, characterized in that ab is less than 1. [Formula 2]
11. Fracture toughness measured according to JIS R1607 is 3.5 MPa m 1/2 The dental zirconia sintered body according to any one of claims 1 to 10, characterized in that
12. In the X-ray diffraction pattern of the dental zirconia sintered body after a hydrothermal treatment test at 180 ° C. and 1 MPa for 5 hours, the ratio of the height of the peak existing near the position where the monoclinic crystal-derived [11-1] peak occurs at 2θ of about 28 ° to the height of the peak existing near the position where the tetragonal crystal-derived [111] peak occurs at 2θ of about 30 ° is 1 or less. The dental zirconia sintered body according to any one of claims 1 to 11.
13. A zirconia calcined body for dental processing, for producing a dental zirconia sintered body, characterized in that the dental zirconia sintered body according to any one of claims 1 to 12 is obtained by sintering at 1400 ° C to 1600 ° C.
14. A dental calcined zirconia body containing zirconia and yttria as a stabilizer for suppressing a phase transition of zirconia, the laminate being formed by laminating and molding a plurality of zirconia powders having different compositions due to different pigment contents, and the laminate being in a calcined state, A calcined body test piece cut out from the dental zirconia calcined body along the lamination direction in the longitudinal direction, The test condition is satisfied in accordance with JIS R1601, in which the bending strength of the calcined test piece, in which the boundaries of the plurality of zirconia powders are present across the calcined test piece in the load application direction, is measured by adjusting the load point of a three-point bending test to the position of the boundaries, and is 90% or more of the bending strength of another calcined test piece obtained by calcining one of the zirconia powders alone at the same calcination temperature as the calcined test piece, Contains at most 0.3% by weight of aluminum oxide, A zirconia calcined body for dental processing, characterized in that
15. A zirconia calcined body for dental processing as described in Claim 14, characterized in that the laminate has a mixed layer in which the zirconia powder of the upper and lower layers is partially mixed at the boundary between each layer.
16. A laminate for producing a dental zirconia sintered body, characterized in that the dental zirconia sintered body according to any one of claims 1 to 12 is obtained by sintering at 1400 ° C. to 1600 ° C.
17. A laminate for producing a dental zirconia sintered body, characterized in that by calcining it becomes the zirconia calcined body for dental processing described in any one of claims 13 to 15.
18. 16. A dental prosthesis, which is in a state in which the zirconia calcined body for dental processing according to any one of claims 13 to 15 is cut and then sintered.
Citation Information
Patent Citations
Ceramic block
JP2004035332A
Process for preparing colored blank and die part
JP2007314536A
Multi-colored shaped body
JP2008068079A