Active energy ray polymerization initiator, active energy ray curable composition, active energy ray curable ink, ink container, image forming method and image forming apparatus
The active energy ray polymerization initiator with a thioxanthone-glucamine structure addresses sensitivity and solubility issues, enhancing UV-LED compatibility and performance in water-based inks.
Patent Information
- Application Number
- JP2020117238
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-07
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2040-07-07
AI Technical Summary
Existing polymerization initiators exhibit insufficient sensitivity to UV-LED light sources with wavelengths of 350 nm to 400 nm and low water solubility, limiting their effectiveness in water-based inks.
Development of an active energy ray polymerization initiator with a specific structure represented by general formula (1), featuring a thioxanthone moiety and glucamine group, which enhances sensitivity to UV light and solubility in water.
The new initiator demonstrates high sensitivity to UV light within the 350 nm to 400 nm range and improved water solubility, enabling effective polymerization in water-based inks.
Smart Images

Figure 0007562078000027 
Figure 0007562078000028 
Figure 0007562078000029
Abstract
Description
[Technical field]
[0001] The present invention relates to an active energy ray polymerization initiator, an active energy ray curable composition, an active energy ray curable ink, an ink container, an image forming method, and an image forming apparatus. [Background technology]
[0002] In general, the use of volatile organic compounds is a cause of air pollution and may be subject to legal restrictions. In printing inks, water-based ink compositions containing water as a vehicle are also required. Many water-based inks contain a thermoplastic resin emulsion in order to fix an image on a medium, and the resin emulsion forms a film by heating and drying to form an image. In order to further strengthen the resistance of the image, for example, the prevention of bleeding (beading) during printing, the prevention of bleeding of the image due to contact with ethanol or the like after image formation, and the resistance to physical scratching and rubbing, water-based inks are used that contain a water-soluble monomer, water-soluble oligomer, or resin emulsion that can be polymerized by active energy rays such as electron beams (EB) and ultraviolet rays (UV), and a water-soluble polymerization initiator that generates free radicals by active energy rays. The light source of the active energy rays is preferably a UV light emitting diode (LED) of 350 nm to 400 nm in terms of energy saving and space saving. Patent Document 1 proposes a photopolymerization initiator having high sensitivity to UV rays and high solubility in water, and an ink composition using the same. Summary of the Invention [Problem to be solved by the invention]
[0003] However, the polymerization initiator exemplified in Patent Document 1 has a maximum absorption wavelength (λmax) of 301 nm to 318 nm, and its sensitivity to a UV-LED light source of 350 nm to 400 nm is insufficient. Therefore, an object of the present invention is to provide an active energy ray polymerization initiator having high sensitivity to UV rays of 350 nm to 400 nm and high solubility in water. [Means for solving the problem]
[0004] The above problem is solved by the invention having the following configuration (1). (1) An active energy ray polymerization initiator having a structure represented by the following general formula (1): [ka] (In the general formula (1), R1 is H or a methoxy group, R2 is H or a C1-8 hydrocarbon group, Alk is a C3-12 hydrocarbon group, and Lnk is a bond or a group represented by the following structural formula (1).) [ka] Effect of the Invention
[0005] According to the present invention, it is possible to provide an active energy ray polymerization initiator having high sensitivity to UV rays of 350 nm to 400 nm and high solubility in water. [Brief description of the drawings]
[0006] [Figure 1] FIG. 2 is a diagram showing an example of an absorption spectrum of the active energy ray polymerization initiator of the present invention. [Diagram 2] FIG. 2 is a diagram showing an example of an absorption spectrum of the active energy ray polymerization initiator of the present invention. [Diagram 3] FIG. 1 is a diagram showing an example of the absorption spectrum of a conventional active energy ray polymerization initiator. [Figure 4] FIG. 1 is a diagram showing an example of the absorption spectrum of a conventional active energy ray polymerization initiator. [Diagram 5] FIG. 1 is a diagram showing an example of the absorption spectrum of a conventional active energy ray polymerization initiator. [Figure 6]FIG. 1 is a schematic diagram illustrating an example of an image forming apparatus according to the present invention. [Figure 7] FIG. 2 is a schematic diagram showing an example of another image forming apparatus according to the present invention. [Figure 8] FIG. 11 is a schematic diagram showing yet another example of an image forming apparatus according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] Hereinafter, an embodiment for carrying out the present invention will be described, however, the present invention is not limited to the following embodiment. The active energy ray polymerization initiator of the present invention has a structure represented by the following general formula (1). [ka] (In the general formula (1), R1 is H or a methoxy group, R2 is H or a C1-8 hydrocarbon group, Alk is a C3-12 hydrocarbon group, and Lnk is a bond or a group represented by the following structural formula (1).) [ka]
[0008] In the active energy ray polymerization initiator having the structure represented by general formula (1), the thioxanthone moiety having an alkoxy group represented by R1 or Alk-O- absorbs light, abstracts hydrogen from the polymerization initiator itself or from a second compound, and generates free radicals. Hydrogen abstraction by the thioxanthone moiety is likely to occur from the hydrocarbon adjacent to the nitrogen atom, so the hydrocarbon adjacent to the nitrogen atom of the glucamine moiety acts effectively. In addition, the glucamine portion of general formula (1) confers water solubility. In terms of water solubility, it is preferable that Alk and R2 in general formula (1) have fewer carbon atoms. Moreover, Lnk in general formula (1) is preferably a group represented by structural formula (1) from the viewpoints of synthesis and purification.
[0009] The active energy ray-curable composition of the present invention comprises at least an active energy ray polymerization initiator having a structure represented by the above general formula (1) and other components appropriately selected according to the desired properties of the polymerization product. The other components include a polymerizable monomer, a polymerization initiator, an organic solvent, water, a surfactant, a resin, etc.
[0010] In the active energy ray-curable composition of the present invention, the content of the active energy ray polymerization initiator having the structure represented by the general formula (1) may be appropriately determined depending on the application of the composition, etc., but is preferably 1 to 30 mass %, more preferably 5 to 15 mass %.
[0011] As the polymerizable monomer, the following (meth)acrylate, (meth)acrylamide, vinyl ether, etc. can also be used in combination. Ethylene glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, γ-butyrolactone acrylate, isobornyl (meth)acrylate, formalized trimethylolpropane mono(meth)acrylate, polytetramethylene glycol di(meth)acrylate, trimethylolpropane (meth)acrylic acid benzoate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol diacrylate [CH2=CH-CO -(OC2H4)n-OCOCH=CH2(n≒4)】, (n≒9), (n≒14), (n≒23), dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol dimethacrylate [CH2=C(CH3)-CO-(OC3H6)n-OCOC(CH3)=CH2(n≒7)], 1,3-butanediol di(meth)acrylate, 1,4-butanediol diacrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate , neopentyl glycol diacrylate, tricyclodecane dimethanol diacrylate, propylene oxide modified bisphenol A di(meth)acrylate, polyethylene glycol di(meth)acrylate, dipentaerythritol hexa(meth)acrylate, (meth)acryloylmorpholine, propylene oxide modified tetramethylolmethane tetra(meth)acrylate, dipentaerythritol hydroxypenta(meth)acrylate, caprolactone modified dipentaerythritol hydroxypenta(meth)acrylate, ditrimethylol Tyrolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, trimethylolpropane triacrylate, ethylene oxide modified trimethylolpropane tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, caprolactone modified trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, neopentyl glycol diacrylate,Ethoxylated neopentyl glycol di(meth)acrylate, propylene oxide modified neopentyl glycol di(meth)acrylate, propylene oxide modified glyceryl tri(meth)acrylate, polyester di(meth)acrylate, polyester tri(meth)acrylate, polyester tetra(meth)acrylate, polyester penta(meth)acrylate, polyester poly(meth)acrylate, polyurethane di(meth)acrylate, polyurethane tri(meth)acrylate, polyurethane tetra(meth)acrylate, polyurethane penta(meth)acrylate, polyurethane poly(meth)acrylate, 2-hydroxypropyl(meth)acrylamide, N-vinyl caprolactam, N-vinyl pyrrolidone, N-vinyl formamide, cyclohexane dimethanol monovinyl ether, cyclohexane dimethanol divinyl ether, hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, diethylene glycol divinyl ether, dicyclopentadiene vinyl ether, tricyclodecane vinyl ether, benzyl vinyl ether, ethyl oxetane methyl vinyl ether, etc.,
[0012] In the active energy ray-curable composition of the present invention, the content of the polymerizable monomer may be appropriately determined depending on the application of the composition, etc., but is preferably from 70 to 99 mass %, more preferably from 85 to 95 mass %.
[0013] The active energy ray curable composition of the present invention may contain a polymerization initiator other than the active energy ray polymerization initiator having the structure represented by the general formula (1). The polymerization initiator may be any one that can generate active species such as radicals and cations by the energy of active energy rays and initiate polymerization of a polymerizable compound (monomer or oligomer). As such a polymerization initiator, known radical polymerization initiators, cationic polymerization initiators, base generators, etc. can be used alone or in combination of two or more kinds, and among them, it is preferable to use a radical polymerization initiator. Examples of the radical polymerization initiator include aromatic ketones, acylphosphine oxide compounds, aromatic onium salt compounds, organic peroxides, thio compounds (thioxanthone compounds, thiophenyl group-containing compounds, etc.), hexaarylbiimidazole compounds, ketoxime ester compounds, borate compounds, azinium compounds, metallocene compounds, active ester compounds, compounds having a carbon-halogen bond, and alkylamine compounds.
[0014] In the active energy ray-curable composition of the present invention, the content of the polymerization initiator other than the active energy ray polymerization initiator having the structure represented by the general formula (1) may be appropriately determined depending on the application of the composition, and is, for example, 0 to 5 mass %.
[0015] In addition to the polymerization initiator, a polymerization accelerator (sensitizer) can also be used in combination. The polymerization accelerator is not particularly limited, but for example, amine compounds such as trimethylamine, methyldimethanolamine, triethanolamine, p-diethylaminoacetophenone, ethyl p-dimethylaminobenzoate, 2-ethylhexyl p-dimethylaminobenzoate, N,N-dimethylbenzylamine, and 4,4'-bis(diethylamino)benzophenone are preferred, and the content thereof may be appropriately set according to the polymerization initiator used and its amount.
[0016] Since the active energy ray polymerization initiator of the present invention is water-soluble, it can be used in combination with a hydrophilic organic solvent.
[0017] Specific examples of the water-soluble organic solvent include ethylene glycol, diethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,3-butanediol, triethylene glycol, polyethylene glycol, polypropylene glycol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, 2,4-pentanediol, 1,5-pentanediol, and the like. polyhydric alcohols such as pentanediol, 1,2-hexanediol, 1,6-hexanediol, 1,3-hexanediol, 2,5-hexanediol, 1,5-hexanediol, glycerin, 1,2,6-hexanetriol, 2-ethyl-1,3-hexanediol, ethyl-1,2,4-butanetriol, 1,2,3-butanetriol, 2,2,4-trimethyl-1,3-pentanediol, and petriol, ethylene glycol monoethyl ether, and ethylene glycol monobutyl ether. polyhydric alcohol alkyl ethers such as diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and propylene glycol monoethyl ether; polyhydric alcohol aryl ethers such as ethylene glycol monophenyl ether and ethylene glycol monobenzyl ether; nitrogen-containing heterocyclic compounds such as 2-pyrrolidone, N-methyl-2-pyrrolidone, N-hydroxyethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, ε-caprolactam, and γ-butyrolactone; amides such as formamide, N-methylformamide, N,N-dimethylformamide, 3-methoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide; amines such as monoethanolamine, diethanolamine, and triethylamine; sulfur-containing compounds such as dimethyl sulfoxide, sulfolane, and thiodiethanol; propylene carbonate, and ethylene carbonate.
[0018] In the active energy ray-curable composition of the present invention, the content of the organic solvent may be appropriately determined depending on the application of the composition, and is, for example, 10 to 60 mass %.
[0019] The active energy ray-curable composition of the present invention may contain a surfactant. Examples of the surfactant include silicone surfactants, fluorine surfactants, and nonionic surfactants.
[0020] Silicone surfactants are not particularly limited and can be appropriately selected according to purpose.Among them, those that do not decompose even at high pH are preferred, such as side chain modified polydimethylsiloxane, both end modified polydimethylsiloxane, one end modified polydimethylsiloxane, side chain both end modified polydimethylsiloxane, etc., and those having polyoxyethylene group or polyoxyethylene polyoxypropylene group as modified group are particularly preferred because they show good properties as aqueous surfactants.In addition, polyether modified silicone surfactants can also be used as the silicone surfactant, such as a compound in which a polyalkylene oxide structure is introduced into the Si part side chain of dimethylsiloxane. As the fluorosurfactant, for example, perfluoroalkyl sulfonic acid compounds, perfluoroalkyl carboxylic acid compounds, perfluoroalkyl phosphate compounds, perfluoroalkyl ethylene oxide adducts, and polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups on the side chain are particularly preferred because they have low foaming properties. As the perfluoroalkyl sulfonic acid compounds, for example, perfluoroalkyl sulfonic acid, perfluoroalkyl sulfonate, etc. are included. As the perfluoroalkyl carboxylic acid compounds, for example, perfluoroalkyl carboxylic acid, perfluoroalkyl carboxylate, etc. are included. As the polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups on the side chain, for example, sulfate ester salts of polyoxyalkylene ether polymers having perfluoroalkyl ether groups on the side chains, salts of polyoxyalkylene ether polymers having perfluoroalkyl ether groups on the side chains, etc. are included. As counter ions of the salts in these fluorosurfactants, Li, Na, K, NH4, NH3CH2CH2OH, NH2(CH2CH2OH)2, NH(CH2CH2OH)3, etc. are included.
[0021] In the active energy ray-curable composition of the present invention, the content of the surfactant may be appropriately determined depending on the application of the composition, and is, for example, 1 to 5 mass %.
[0022] The active energy ray-curable composition of the present invention may contain a resin emulsion in which a resin is dispersed in water as a dispersion medium. The type of resin is not particularly limited and can be appropriately selected depending on the purpose. Examples of the resin include urethane resin, polyester resin, acrylic resin, vinyl acetate resin, styrene resin, butadiene resin, styrene-butadiene resin, vinyl chloride resin, acrylic styrene resin, and acrylic silicone resin. These resin particles may be used alone or in combination of two or more kinds.
[0023] In the active energy ray-curable composition of the present invention, the content of the resin may be appropriately determined depending on the application of the composition, and is, for example, 10 to 90% by mass.
[0024] The active energy ray-curable composition of the present invention can be prepared using the various components described above. The preparation means and conditions are not particularly limited. For example, the active energy ray-curable composition can be prepared by putting a polymerizable monomer, a pigment, a dispersant, etc. into a dispersing machine such as a ball mill, a Kitty mill, a disk mill, a pin mill, or a Dyno mill, dispersing the ingredients to prepare a pigment dispersion, and further mixing a polymerizable monomer, a polymerization initiator, a polymerization inhibitor, a surfactant, etc. into the pigment dispersion.
[0025] The active energy rays applied to the active energy ray polymerization initiator of the present invention are not particularly limited, and may be any rays that can provide the energy required to advance the polymerization reaction, such as ultraviolet rays, electron beams, α rays, β rays, γ rays, and X-rays. In the case of ultraviolet irradiation, mercury-free devices are strongly desired from the viewpoint of environmental protection, and replacement with GaN-based semiconductor ultraviolet light-emitting devices is very useful industrially and environmentally. Furthermore, ultraviolet light-emitting diodes (UV-LEDs) and ultraviolet laser diodes (UV-LDs) are small, have a long life, are highly efficient, and are low cost, making them preferable as ultraviolet light sources.
[0026] The active energy ray-curable ink of the present invention may contain an active energy ray-curable composition, a coloring material, and, if necessary, other components.
[0027] <Coloring material> The coloring material is not particularly limited, and pigments and dyes can be used. The pigment may be an inorganic pigment or an organic pigment. These may be used alone or in combination of two or more. Mixed crystals may also be used. Examples of pigments that can be used include black pigments, yellow pigments, magenta pigments, cyan pigments, white pigments, green pigments, orange pigments, glossy pigments such as gold and silver pigments, and metallic pigments. As inorganic pigments, titanium oxide, iron oxide, calcium carbonate, barium sulfate, aluminum hydroxide, barium yellow, cadmium red, chrome yellow, as well as carbon black produced by known methods such as the contact method, furnace method, and thermal method can be used. As organic pigments, azo pigments, polycyclic pigments (e.g., phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, indigo pigments, thioindigo pigments, isoindolinone pigments, quinophthalone pigments, etc.), dye chelates (e.g., basic dye chelates, acid dye chelates, etc.), nitro pigments, nitroso pigments, aniline black, etc. can be used. Among these pigments, those having good affinity with the solvent are preferably used. In addition, resin hollow particles and inorganic hollow particles can also be used. Specific examples of pigments for black colors include carbon blacks (CI Pigment Black 7) such as furnace black, lamp black, acetylene black, and channel black; metals such as copper, iron (CI Pigment Black 11), and titanium oxide; and organic pigments such as aniline black (CI Pigment Black 1). In addition, for color, CI Pigment Yellow 1, 3, 12, 13, 14, 17, 24, 34, 35, 37, 42 (yellow iron oxide), 53, 55, 74, 81, 83, 95, 97, 98, 100, 101, 104, 108, 109, 110, 117, 120, 138, 150, 153, 155, 180, 185, 213, CI Pigment Yellow Range 5, 13, 16, 17, 36, 43, 51, CI Pigment Red 1, 2, 3, 5, 17, 22, 23, 31, 38, 48:2, 48:2 (Permanent Red 2B (Ca)), 48:3, 48:4, 49:1, 52:2, 53:1, 57:1 (Brilliant Carmine 6B), 60:1, 63:1, 63:2, 64:1, 81, 83, 88 , 101 (red oxide), 104, 105, 106, 108 (cadmium red), 112, 114, 122 (quinacridone magenta), 123, 146, 149, 166, 168, 170, 172, 177, 178, 179, 184, 185, 190, 193, 202, 207, 208, 209, 213, 219, 224, 254, 264, CI Pigment Violet 1 (Rhodamine Lake), 3, 5:1, 16, 19, 23, 38; CI Pigment Blue 1, 2, 15 (Phthalocyanine Blue), 15:1, 15:2, 15:3, 15:4 (Phthalocyanine Blue), 16, 17:1, 56, 60, 63; CI Pigment Green 1, 4, 7, 8, 10, 17, 18, 36, etc. The dye is not particularly limited, and acid dyes, direct dyes, reactive dyes, and basic dyes can be used. One type of dye may be used alone, or two or more types may be used in combination. Examples of the dyes include CI Acid Yellow 17, 23, 42, 44, 79, 142, CI Acid Red 52, 80, 82, 249, 254, 289, CI Acid Blue 9, 45, 249, CI Acid Black 1, 2, 24, 94, CI Food Black 1, 2, CI Direct Yellow 1, 12, 24, 33, 50, 55, 58, 86, 132, 142, 144, 173, CI Direct Red 1, 4, 9, 80, 81, 225, 227, CI Direct Blue 1, 2, 15, 71, 86, 87, 98, 165, 199, 202, CI Direct Black 19, 38, 51, 71, 154, 168, 171, 195, and CI Reactive Red. 14, 32, 55, 79, 249, and CI Reactive Black 3, 4, and 35.
[0028] The content of the coloring material in the ink is preferably from 0.1% to 15% by mass, and more preferably from 1% to 10% by mass, from the viewpoints of improving image density, good fixing property and ejection stability.
[0029] Methods for dispersing a pigment in an ink include a method of introducing a hydrophilic functional group into the pigment to make it a self-dispersing pigment, a method of dispersing the pigment by coating the surface of the pigment with a resin, and a method of dispersing the pigment using a dispersant. As a method for making a pigment into a self-dispersing pigment by introducing a hydrophilic functional group, for example, a self-dispersing pigment that can be dispersed in water by adding a functional group such as a sulfone group or a carboxyl group to a pigment (e.g., carbon) can be used. As a method for coating the surface of a pigment with a resin and dispersing it, a method for encapsulating the pigment in a microcapsule and dispersing it in water can be used. This can be called a resin-coated pigment. In this case, it is not necessary for all the pigments blended in the ink to be coated with a resin, and uncoated or partially coated pigments may be dispersed in the ink as long as the effects of the present invention are not impaired. Examples of the method for dispersing using a dispersant include a method for dispersing using a known low molecular weight dispersant or a known polymeric dispersant, such as a surfactant. As the dispersant, for example, anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, etc. can be used depending on the pigment. RT-100 (nonionic surfactant) manufactured by Takemoto Oil Co., Ltd. and sodium naphthalenesulfonate formalin condensate can also be suitably used as dispersants. The dispersants may be used alone or in combination of two or more.
[0030] <Pigment dispersion> It is possible to obtain ink by mixing a pigment with materials such as water or an organic solvent, or it is also possible to manufacture ink by mixing a pigment with other materials such as water or a dispersant to prepare a pigment dispersion, and then mixing the resulting mixture with materials such as water or an organic solvent. The pigment dispersion is obtained by dispersing water, a pigment, a pigment dispersant, and other components as required, and adjusting the particle size. Dispersion is preferably performed using a dispersing machine. The particle size of the pigment in the pigment dispersion is not particularly limited, but the maximum frequency in terms of the maximum number is preferably 20 nm or more and 500 nm or less, more preferably 20 nm or more and 150 nm or less, in order to improve the dispersion stability of the pigment and the image quality such as ejection stability and image density. The particle size of the pigment can be measured using a particle size analyzer (Nanotrac Wave-UT151, manufactured by Microtrac Bell Co., Ltd.). The content of the pigment in the pigment dispersion is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of obtaining good ejection stability and increasing image density, the content is preferably from 0.1% by mass to 50% by mass, and more preferably from 0.1% by mass to 30% by mass. It is preferable that the pigment dispersion is degassed, if necessary, by filtering coarse particles using a filter, a centrifugal separator, or the like.
[0031] The active energy ray-curable ink of the present invention may contain an antifoaming agent, an antiseptic / antifungal agent, an antirust agent, and / or a pH adjuster.
[0032] <Antifoaming agent> The defoaming agent is not particularly limited, and examples thereof include silicone-based defoaming agents, polyether-based defoaming agents, fatty acid ester-based defoaming agents, and the like. These may be used alone or in combination of two or more. Among these, silicone-based defoaming agents are preferred because of their excellent defoaming effect.
[0033] <Antiseptic and mildew-proof agent> The antiseptic and mildew-proof agent is not particularly limited, and examples thereof include 1,2-benzisothiazolin-3-one and the like.
[0034] <Rust inhibitor> The rust inhibitor is not particularly limited, and examples thereof include acid sulfite, sodium thiosulfate, and the like.
[0035] <pH adjuster> The pH adjuster is not particularly limited as long as it can adjust the pH to 7 or higher, and examples thereof include amines such as diethanolamine and triethanolamine.
[0036] The physical properties of the ink are not particularly limited and can be appropriately selected according to the purpose. For example, it is preferable that the viscosity, surface tension, pH, etc. are in the following ranges. The viscosity of the ink at 25°C is preferably 5 mPa·s or more and 30 mPa·s or less, more preferably 5 mPa·s or more and 25 mPa·s or less, from the viewpoints of improving the printing density and the quality of characters and obtaining good ejection properties. Here, for example, a rotational viscometer (RE-80L manufactured by Toki Sangyo Co., Ltd.) can be used to measure the viscosity. The measurement conditions are as follows: at 25°C, using a standard cone rotor (1°34’×R24), a sample liquid volume of 1.2 mL, a rotation speed of 50 rpm, and it can be measured in 3 minutes. The surface tension of the ink is preferably 35 mN / m or less, more preferably 32 mN / m or less at 25°C, from the viewpoints of the ink being preferably leveled on the recording medium and shortening the drying time of the ink. The pH of the ink is preferably 7 to 12, more preferably 8 to 11, from the viewpoint of preventing corrosion of the metal members in contact with the liquid.
[0037] The use of the active energy ray-curable composition of the present invention is not particularly limited and can be appropriately selected depending on the purpose. Examples of the use include molding resins, paints, adhesives, insulating materials, release agents, coating materials, sealing materials, various resists, and various optical materials.
[0038] Furthermore, the active energy ray curable composition of the present invention can be used as an ink to form two-dimensional characters and images, and decorative coatings on various substrates, and can also be used as a material for three-dimensional modeling to form a three-dimensional image (three-dimensional object). This material for three-dimensional modeling can be used, for example, as a binder between powder particles used in a powder lamination method in which a three-dimensional modeling is performed by repeatedly curing and laminating powder layers, or as a three-dimensional construction material (model material) or a support member (support material) used in an additive manufacturing method (stereolithography) as shown in FIG. 7 or FIG. 8. FIG. 7 shows a method of discharging the active energy ray curable composition of the present invention into a predetermined area, irradiating it with active energy rays, and sequentially laminating the cured layers to perform three-dimensional modeling (described in detail later), and FIG. 8 shows a method of irradiating a storage pool (container) 1 of the active energy ray curable composition 5 of the present invention with active energy rays 4 to form a cured layer 6 of a predetermined shape on a movable stage 3, and sequentially laminating the layers to perform three-dimensional modeling.
[0039] As a three-dimensional modeling apparatus for forming a three-dimensional object using the active energy ray-curable composition of the present invention, a known one can be used, and is not particularly limited. For example, the three-dimensional modeling apparatus may be one equipped with a means for storing, supplying, and discharging the composition, and an active energy ray irradiation means.
[0040] The present invention also includes a molded article obtained by processing a cured product obtained by curing the active energy ray-curable composition of the present invention or a structure formed on a substrate with the cured product. The molded article is, for example, a cured product or structure formed in a sheet or film shape, which is molded by heat stretching, punching, or the like, and is suitably used for applications requiring molding after surface decoration, such as meters and operation panels for automobiles, office automation equipment, electric and electronic equipment, and cameras.
[0041] The substrate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the substrate include paper, thread, fiber, cloth, leather, metal, plastic, glass, wood, ceramics, and composite materials thereof. From the viewpoint of processability, a plastic substrate is preferred.
[0042] The ink container of the present invention means a container in which active energy ray-curable ink is contained, and is suitable for use in the above-mentioned applications. For example, the ink container of the present invention can be used as an ink cartridge or ink bottle, which eliminates the need to directly touch the ink during ink transport, ink replacement, and other operations, thereby preventing hands, fingers, and clothing from getting dirty. In addition, it is possible to prevent foreign matter such as dust from getting mixed into the ink. The shape, size, material, and the like of the container itself may be any suitable material for the application and usage, and are not particularly limited, but it is preferable that the material be a light-shielding material that does not transmit light, or that the container be covered with a light-shielding sheet or the like.
[0043] The image forming method of the present invention comprises a step of ejecting the active energy ray-curable ink of the present invention onto a recording medium to form an image. The image forming apparatus of the present invention comprises an ink container that contains the active energy ray-curable ink of the present invention, and a discharge means that discharges the ink contained in the ink container onto a recording medium. A specific example of an image forming method will now be described.
[0044] In order to cure the active energy ray curable ink of the present invention with active energy rays, an irradiation step of irradiating active energy rays is provided, and the image forming apparatus of the present invention includes an irradiation means for irradiating active energy rays and a storage section for storing the active energy ray curable ink of the present invention, and the storage section may store the container. Furthermore, the apparatus may include a discharge step and a discharge means for discharging the active energy ray curable ink. The discharge method is not particularly limited, and examples thereof include a continuous jet type and an on-demand type. Examples of the on-demand type include a piezo type, a thermal type, and an electrostatic type.
[0045] FIG. 6 is an example of an image forming apparatus equipped with an inkjet ejection means. The ink is ejected onto a recording medium 22 supplied from a supply roll 21 by printing units 23a, 23b, 23c, and 23d each equipped with an ink cartridge and an ejection head for each color of active energy ray curable ink of yellow, magenta, cyan, and black. Then, the ink is cured by irradiating the ink with active energy rays from light sources 24a, 24b, 24c, and 24d for curing the ink, forming a color image. Then, the recording medium 22 is conveyed to a processing unit 25 and a print winding roll 26. Each printing unit 23a, 23b, 23c, and 23d may be provided with a heating mechanism so that the ink is liquefied in the ink ejection section. If necessary, a mechanism for cooling the recording medium to about room temperature by contact or non-contact may be provided. In addition, the inkjet recording method can be either a serial method in which the head is moved to eject ink onto the recording medium, which moves intermittently according to the width of the ejection head, or a line method in which the recording medium is moved continuously and ink is ejected onto the recording medium from a head held at a fixed position.
[0046] The recording medium 22 is not particularly limited, but may be paper, film, ceramics, glass, metal, a composite material thereof, or the like, and may be in the form of a sheet. The recording medium 22 may be configured to allow only one-sided printing, or may be configured to allow both-sided printing. The recording medium 22 is not limited to those generally used as recording media, and may be appropriately made of cardboard, building materials such as wallpaper and flooring, concrete, cloth for clothing such as T-shirts, textiles, leather, or the like. Furthermore, the irradiation of active energy rays from the light sources 24a, 24b, and 24c may be weakened or omitted, and after printing multiple colors, the active energy rays may be irradiated from the light source 24d, which can save energy and reduce costs.
[0047] Recorded matters recorded with the ink of the present invention include not only those printed on smooth surfaces such as ordinary paper or resin film, but also those printed on uneven printing surfaces and those printed on printing surfaces made of various materials such as metals and ceramics. In addition, by laminating two-dimensional images, it is also possible to form an image with a partially three-dimensional effect (an image consisting of two and three dimensions) or a three-dimensional object.
[0048] Fig. 7 is a schematic diagram showing an example of another image forming apparatus (a three-dimensional solid image forming apparatus) according to the present invention. The image forming apparatus 39 in Fig. 7 uses a head unit (movable in the AB direction) in which inkjet heads are arranged, and ejects a first active energy ray curable ink from an ejection head unit 30 for a model and ejects a second active energy ray curable ink having a different composition from the first active energy ray curable ink from ejection head units 31 and 32 for a support, and laminates these compositions while curing them with adjacent ultraviolet ray irradiation means 33 and 34. More specifically, for example, the second active energy ray curable ink is discharged from the support ejection head units 31 and 32 onto the object support substrate 37, and the ink is irradiated with active energy rays to solidify the ink to form a first support layer having a reservoir. The first active energy ray curable ink is then discharged from the object ejection head unit 30 into the reservoir, and the ink is irradiated with active energy rays to solidify the ink to form a first object layer. This process is repeated several times while lowering the stage 38 movable in the vertical direction in accordance with the number of layers to laminate the support layer and the object layer to produce a three-dimensional object 35. After that, the support layer 36 is removed as necessary. Although only one object ejection head unit 30 is provided in FIG. 7, two or more object ejection head units 30 may be provided. EXAMPLES
[0049] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0050] <<Preparation of active energy ray polymerization initiator>> [Example 1] A solution of 8.42 g (150 mmol) of potassium hydroxide in 20.0 g of ion-exchanged water was prepared in a reaction vessel, and 50 mL of tetrahydrofuran (THF) and 12.34 g (50 mmol) of 2-chlorothioxanthone were added in that order. Nitrogen gas was bubbled into the resulting mixture for 15 minutes, and then 0.485 g (1 mmol) of 2-(di-tert-butylphosphino)-2',4',6'-triisopropyl-3,6-dimethoxy-1,1'-biphenyl (t-ButylBrettPhos, Merck) was added.
[0051] 6 mL of THF was added to a test tube, and nitrogen gas was bubbled through for 1 minute. Then, 0.86 g (1 mmol) of [(2-di-tert-butylphosphino-3,6-dimethoxy-2′,4′,6′-triisopropyl-1,1′-biphenyl)-2-(2′-amino-1,1′-biphenyl)]palladium(II) methanesulfonate (t-BuBrettPhos Pd G3, Merck) was added and dissolved while bubbling nitrogen. The resulting solution was added to the above reaction solution with a syringe while bubbling nitrogen, heated under reflux for 12 hours, and then cooled to room temperature. The resulting reaction solution was diluted with 300 mL of ethyl acetate, neutralized by adding 25 g of 6N hydrochloric acid, and then washed with 200 mL of brine three times. The isolated organic phase was dried over magnesium sulfate, and the solvent was distilled off. The residue was purified by silica gel column chromatography using a mixed solvent of toluene / ethyl acetate (volume ratio 8 / 2 to 5 / 5) as an eluent to obtain 7.85 g of 2-hydroxythioxanthone.
[0052] Next, 1.60 g (7 mmol) of 2-hydroxythioxanthone, 4.25 g (21 mmol) of 1,3-dibromopropane, and 1.45 g of potassium carbonate were added to 25 mL of methyl ethyl ketone (MEK), heated under reflux for 10 hours, and then cooled. The resulting reaction solution was diluted with 40 mL of ethyl acetate and filtered through filter paper. The filtrate was concentrated, and the residue was purified by silica gel column chromatography using toluene as an eluent to obtain 1.85 g of 2-(3-bromopropoxy)thioxanthone.
[0053] Next, 0.57 g (3.2 mmol) of D-glucamine (Tokyo Chemical Industry Co., Ltd.) was dissolved in a mixed solvent of 5 mL of water and 5 g of ethanol, and 0.46 g of potassium carbonate and 1.05 g (3.0 mmol) of 2-(3-bromopropyl)-9H-thioxanthen-9-one were added, and the mixture was heated under reflux for 18 hours and then cooled. The solvent was distilled off from the reaction solution, and 50 mL of methylene chloride and 50 mL of ethanol were added to the residue and dissolved. The resulting solution was washed with 100 mL of ion-exchanged water, and then the organic phase was isolated and the solvent was distilled off to obtain 1.11 g of the active energy ray polymerization initiator (TX-1) of the present invention represented by formula (1). [ka]
[0054] [Example 2] 1.60 g (7 mmol) of 2-hydroxythioxanthone, 5.13 g (21 mmol) of 1,6-dibromohexane, and 1.45 g of potassium carbonate were added to 25 mL of MEK, heated under reflux for 10 hours, and then cooled. The resulting reaction solution was diluted with 40 mL of ethyl acetate and filtered through filter paper. The filtrate was concentrated, and the residue was purified by silica gel column chromatography using toluene as an eluent to obtain 2.34 g of 2-(3-bromohexyloxy)thioxanthone. Next, 0.57 g (3.2 mmol) of D-glucamine (Tokyo Chemical Industry Co., Ltd.) was dissolved in a mixed solvent of 5 mL of water and 5 g of ethanol, and 0.46 g of potassium carbonate and 1.18 g (3 mmol) of 2-(3-bromohexyloxy)thioxanthone were added, and the mixture was heated under reflux for 18 hours and then cooled. The solvent was distilled off from the reaction solution, and 50 mL of methylene chloride and 50 mL of ethanol were added to the residue and dissolved. The resulting solution was washed with 100 mL of ion-exchanged water, and then the organic phase was isolated and the solvent was distilled off to obtain 1.26 g of the active energy ray polymerization initiator (TX-2) of the present invention represented by formula (2). [ka]
[0055] [Example 3] 1.60g (7mmol) of 2-hydroxythioxanthone, 6.90g (21mmol) of 1,12-dibromododecane, and 1.45g of potassium carbonate were added to 30mL of MEK, heated under reflux for 10 hours, and then cooled. The resulting reaction solution was diluted with 40mL of ethyl acetate and filtered through filter paper. The filtrate was concentrated, and the residue was purified by silica gel column chromatography using toluene as an eluent to obtain 2.88g of 2-(3-bromododecyloxy)thioxanthone. Next, 0.57 g (3.2 mmol) of D-glucamine (Tokyo Chemical Industry Co., Ltd.) was dissolved in a mixed solvent of 5 mL of water and 5 g of ethanol, and 0.46 g of potassium carbonate and 1.43 g (3 mmol) of 2-(3-bromododecyloxy)thioxanthone were added, and the mixture was heated under reflux for 18 hours and then cooled. The solvent was distilled off from the reaction solution, and 50 mL of methylene chloride and 50 mL of ethanol were added to the residue and dissolved. The resulting solution was washed with 100 mL of ion-exchanged water, and then the organic phase was isolated and the solvent was distilled off to obtain 1.41 g of the active energy ray polymerization initiator (TX-3) of the present invention represented by formula (3). [ka]
[0056] [Example 4] 0.62g (3.2mmol) of N-methyl-D-glucamine (Tokyo Chemical Industry Co., Ltd.) was dissolved in 5mL of a mixed solvent of water and 5g of ethanol, 0.46g of potassium carbonate and 1.05g (3.0mmol) of 2-(3-bromopropoxy)thioxanthone were added, and the mixture was heated under reflux for 18 hours and then cooled. The solvent was distilled off from the reaction solution, and 50mL of methylene chloride and 50mL of ethanol were added to the residue and dissolved. The resulting solution was washed with 100mL of ion-exchanged water, and the organic phase was isolated and the solvent was distilled off to obtain 1.05g of the active energy ray polymerization initiator (TX-4) of the present invention represented by formula (4). [ka]
[0057] [Example 5] 0.66g (3.2mmol) of N-ethyl-D-glucamine (Tokyo Chemical Industry Co., Ltd.) was dissolved in a mixed solvent of 5mL of water and 5g of ethanol, 0.46g of potassium carbonate and 1.05g (3.0mmol) of 2-(3-bromopropoxy)thioxanthone were added, and the mixture was heated under reflux for 18 hours and then cooled. The solvent was distilled off from the reaction solution, and 50mL of methylene chloride and 50mL of ethanol were added to the residue and dissolved. The resulting solution was washed with 100mL of ion-exchanged water, and the organic phase was isolated and the solvent was distilled off to obtain 1.18g of the active energy ray polymerization initiator (TX-5) of the present invention represented by formula (5). [ka]
[0058] [Example 6] 0.92g (3.2mmol) of Nn-octyl-D-glucamine (Tokyo Chemical Industry Co., Ltd.) was dissolved in a mixed solvent of 5mL of water and 5g of ethanol, 0.46g of potassium carbonate and 1.05g (3.0mmol) of 2-(3-bromopropyl)thioxanthone were added, and the mixture was heated under reflux for 18 hours and then cooled. The solvent was distilled off from the reaction solution, and 50mL of methylene chloride and 50mL of ethanol were added to the residue and dissolved. The resulting solution was washed with 100mL of ion-exchanged water, and the organic phase was isolated and the solvent was distilled off to obtain 1.36g of the active energy ray polymerization initiator (TX-6) of the present invention represented by formula (6). [ka]
[0059] [Example 7] 5.00g (40mmol) of 2-mercaptosalicylic acid was added little by little to 19.8g of concentrated sulfuric acid, and then 6.33g (40mmol) of 2-methoxyphenol was added little by little and stirred at room temperature for 22 hours. The resulting reaction solution was dropped into 200mL of water at 60°C. The precipitate was filtered, washed with 2L of water, dried, and purified by silica gel column chromatography using a mixed solvent of toluene / ethyl acetate (volume ratio 9 / 1 to 8 / 2) as an eluent to obtain 6.27g of 2-hydroxy-3-methoxythioxanthone. Next, 1.29 g (5 mmol) of 2-hydro-3-methoxythioxanthone, 5.05 g (25 mmol) of 1,3-dibromopropane, and 1.04 g of potassium carbonate were added to 30 mL of methyl ethyl ketone (MEK), heated under reflux for 10 hours, and then cooled. The resulting reaction solution was diluted with 40 mL of ethyl acetate and filtered through filter paper. The filtrate was concentrated, and the residue was purified by silica gel column chromatography using toluene as an eluent to obtain 1.54 g of 2-(3-bromopropoxy)-3-methoxythioxanthone. Next, 0.62 g (3.2 mmol) of N-methyl-D-glucamine (Tokyo Chemical Industry Co., Ltd.) was dissolved in a mixed solvent of 5 mL of water and 5 g of ethanol, and 0.46 g of potassium carbonate and 1.14 g (3.0 mmol) of 2-(3-bromopropoxy)-3-methoxythioxanthone were added, and the mixture was heated under reflux for 18 hours and then cooled. The solvent was distilled off from the reaction solution, and 50 mL of methylene chloride and 50 mL of ethanol were added to the residue and dissolved. The resulting solution was washed with 100 mL of ion-exchanged water, and then the organic phase was isolated and the solvent was distilled off to obtain 1.22 g of the active energy ray polymerization initiator (TX-7) of the present invention represented by formula (7). [ka]
[0060] [Example 8] 5.93g (40mmol) of phthalic anhydride (Tokyo Chemical Industry Co., Ltd.) was added to a mixed solvent of 30mL of anhydrous ethanol (Wako Pure Chemical Industries, Ltd.) and 30mL of ultra-dehydrated dichloromethane (Wako Pure Chemical Industries, Ltd.) under a nitrogen stream, dissolved, and then 7.25g (40mmol) of D-glucamine was added under a nitrogen stream and stirred at room temperature for 24 hours. The solvent was distilled off from the resulting reaction solution to obtain 13.12g of 2-(2,3,4,5,6-pentahydroxyhexylcarbamoyl)benzoic acid. Next, 0.12 g of potassium hydroxide was dissolved in 10 mL of ion-exchanged water, and 0.69 g (2.1 mmol) of 2-(2,3,4,5,6-pentahydroxyhexylcarbamoyl)benzoic acid was added and dissolved. A solution of 0.70 g (2.0 mmol) of 2-(3-bromopropoxy)thioxanthone dissolved in 2 mL of dimethylformamide was added to this solution, and the mixture was stirred at 100°C for 15 hours and then cooled. The solvent was distilled off from the resulting reaction solution, and 70 mL of methylene chloride and 30 mL of ethanol were added to the residue and dissolved. The resulting solution was washed with 100 mL of ion-exchanged water, and the organic phase was isolated and the solvent was distilled off to obtain 1.03 g of the active energy ray polymerization initiator (TX-8) of the present invention represented by formula (8). [ka]
[0061] [Example 9] 0.12g of potassium hydroxide was dissolved in 10mL of ion-exchanged water, and 0.70g (2.1mmol) of 2-(2,3,4,5,6-pentahydroxyhexylcarbamoyl)benzoic acid was added and dissolved. A solution of 0.79g (2.0mmol) of 2-(6-bromohexyloxy)thioxanthone dissolved in 2mL of dimethylformamide was added to this solution, and the mixture was stirred at 100°C for 15 hours and then cooled. The solvent was distilled off from the resulting reaction solution, and 70mL of methylene chloride and 30mL of ethanol were added to the residue and dissolved. The resulting solution was washed with 100mL of ion-exchanged water, and the organic phase was isolated and the solvent was distilled off to obtain 1.17g of the active energy ray polymerization initiator (TX-9) of the present invention represented by formula (9). [ka]
[0062] [Example 10] 0.12g of potassium hydroxide was dissolved in 10mL of ion-exchanged water, and 0.69g (2.1mmol) of 2-(2,3,4,5,6-pentahydroxyhexylcarbamoyl)benzoic acid was added and dissolved. A solution of 0.95g (2.0mmol) of 2-(12-bromododecyloxy)thioxanthone dissolved in 2mL of dimethylformamide was added to this solution, and the mixture was stirred at 100°C for 15 hours and then cooled. The solvent was distilled off from the resulting reaction solution, and 70mL of methylene chloride and 30mL of ethanol were added to the residue and dissolved. The resulting solution was washed with 100mL of ion-exchanged water, and the organic phase was isolated and the solvent was distilled off to obtain 1.33g of the active energy ray polymerization initiator (TX-10) of the present invention represented by formula (10). [ka]
[0063] [Example 11] 5.93g (40mmol) of phthalic anhydride (Tokyo Chemical Industry Co., Ltd.) was added to a mixed solvent of 30mL of anhydrous ethanol (Wako Pure Chemical Industries, Ltd.) and 30mL of ultra-dehydrated dichloromethane (Wako Pure Chemical Industries, Ltd.) under a nitrogen stream, dissolved, and then 7.82g (40mmol) of N-methyl-D-glucamine was added under a nitrogen stream and stirred at room temperature for 24 hours. The solvent was distilled off from the resulting reaction solution to obtain 13.66g of 2-(N-(2,3,4,5,6-pentahydroxyhexyl)-N-methylcarbamoyl)benzoic acid. Next, 0.12 g of potassium hydroxide was dissolved in 10 mL of ion-exchanged water, and 0.72 g (2.1 mmol) of 2-(N-(2,3,4,5,6-pentahydroxyhexyl)-N-methylcarbamoyl)benzoic acid was added and dissolved. To this solution, a solution of 0.70 g (2.0 mmol) of 2-(3-bromopropoxy)thioxanthone dissolved in 2 mL of dimethylformamide was added, and the mixture was stirred at 100° C. for 15 hours and then cooled. The solvent was distilled off from the resulting reaction solution, and 70 mL of methylene chloride and 30 mL of ethanol were added to the residue and dissolved. The resulting solution was washed with 100 mL of ion-exchanged water, and then the organic phase was isolated and the solvent was distilled off to obtain 1.18 g of the active energy ray polymerization initiator (TX-11) of the present invention represented by formula (11). [ka]
[0064] [Example 12] 5.93g (40mmol) of phthalic anhydride (Tokyo Chemical Industry Co., Ltd.) was added to a mixed solvent of 30mL of anhydrous ethanol (Wako Pure Chemical Industries, Ltd.) and 30mL of ultra-dehydrated dichloromethane (Wako Pure Chemical Industries, Ltd.) under a nitrogen stream, dissolved, and then 8.38g (40mmol) of N-ethyl-D-glucamine was added under a nitrogen stream and stirred at room temperature for 24 hours. The solvent was distilled off from the resulting reaction solution to obtain 14.22g of 2-(N-(2,3,4,5,6-pentahydroxyhexyl)-N-ethylcarbamoyl)benzoic acid. Next, 0.12 g of potassium hydroxide was dissolved in 10 mL of ion-exchanged water, and 0.75 g (2.1 mmol) of 2-(N-(2,3,4,5,6-pentahydroxyhexyl)-N-ethylcarbamoyl)benzoic acid was added and dissolved. To this solution, a solution of 0.70 g (2.0 mmol) of 2-(3-bromopropoxy)thioxanthone dissolved in 2 mL of dimethylformamide was added, and the mixture was stirred at 100° C. for 15 hours and then cooled. The solvent was distilled off from the resulting reaction solution, and 70 mL of methylene chloride and 30 mL of ethanol were added to the residue and dissolved. The resulting solution was washed with 100 mL of ion-exchanged water, and then the organic phase was isolated and the solvent was distilled off to obtain 1.14 g of the active energy ray polymerization initiator (TX-12) of the present invention represented by formula (12). [ka]
[0065] [Example 13] 5.93g (40mmol) of phthalic anhydride (Tokyo Chemical Industry Co., Ltd.) was added to a mixed solvent of 30mL of anhydrous ethanol (Wako Pure Chemical Industries, Ltd.) and 30mL of ultra-dehydrated dichloromethane (Wako Pure Chemical Industries, Ltd.) under a nitrogen stream, dissolved, and then 12.3g (40mmol) of N-octyl-D-glucamine was added under a nitrogen stream and stirred at room temperature for 24 hours. The solvent was distilled off from the resulting reaction solution to obtain 17.55g of 2-(N-(2,3,4,5,6-pentahydroxyhexyl)-N-octylcarbamoyl)benzoic acid. Next, 0.12 g of potassium hydroxide was dissolved in 10 mL of ion-exchanged water, and 0.929 g (2.1 mmol) of 2-(N-(2,3,4,5,6-pentahydroxyhexyl)-N-octylcarbamoyl)benzoic acid was added and dissolved. To this solution, a solution of 0.70 g (2.0 mmol) of 2-(3-bromopropoxy)thioxanthone dissolved in 2 mL of dimethylformamide was added, and the mixture was stirred at 100° C. for 15 hours and then cooled. The solvent was distilled off from the resulting reaction solution, and 70 mL of methylene chloride and 30 mL of ethanol were added to the residue and dissolved. The resulting solution was washed with 100 mL of ion-exchanged water, and then the organic phase was isolated and the solvent was distilled off to obtain 1.30 g of the active energy ray polymerization initiator (TX-13) of the present invention represented by formula (13). [ka]
[0066] [Example 14] 0.12g of potassium hydroxide was dissolved in 10mL of ion-exchanged water, and 0.64g (2.1mmol) of 2-(2,3,4,5,6-pentahydroxyhexylcarbamoyl)benzoic acid was added and dissolved. A solution of 0.76g (2.0mmol) of 2-(3-bromopropoxy)-3-methoxythioxanthone dissolved in 2mL of dimethylformamide was added to this solution, and the mixture was stirred at 100°C for 15 hours and then cooled. The solvent was distilled off from the resulting reaction solution, and 70mL of methylene chloride and 30mL of ethanol were added to the residue and dissolved. The resulting solution was washed with 100mL of ion-exchanged water, and the organic phase was isolated and the solvent was distilled off to obtain 1.14g of the active energy ray polymerization initiator (TX-14) of the present invention represented by formula (14). [ka]
[0067] [Comparative Example 1] 4.57g (20mmol) of 2-hydroxythioxanthone, 5.99g (24mmol) of 1-bromododecane, and 4.15g of potassium carbonate were added to 60mL of MEK, heated under reflux for 10 hours, and then cooled. The resulting reaction solution was diluted with 600mL of ethyl acetate and filtered through filter paper. The filtrate was concentrated, and the residue was purified by silica gel column chromatography using toluene as an eluent to obtain 6.98g of 2-dodecyloxythioxanthone as a comparative active energy ray polymerization initiator (Ref-1) represented by formula (15). [ka]
[0068] [Comparative Example 2] 3.97g (20mmol) of 2-hydroxybenzophenone (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 5.90 (24mmol) of 12-bromododecane (manufactured by Tokyo Chemical Industry Co., Ltd.), and 4.15g of potassium carbonate were added to 60mL of methyl ethyl ketone, heated under reflux for 10 hours, and then cooled to room temperature. The resulting reaction solution was filtered through filter paper. The filtrate was concentrated, and the residue was purified by silica gel column chromatography using toluene as an eluent to obtain 6.32g of (2-(dodecyloxy)phenyl)(phenyl)methanone as a comparative active energy ray polymerization initiator (Ref-2) represented by formula (16). [ka]
[0069] [Comparative Example 3] 2-Hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (manufactured by Tokyo Chemical Industry Co., Ltd.) was used as the active energy ray polymerization initiator in Comparative Example 3.
[0070] The structures of the active energy ray polymerization initiators of the present invention prepared above are summarized in Table 1.
[0071] [Table 1]
[0072] <<Evaluation of active energy ray polymerization initiators>> The polymerization initiators of Examples 1 to 14 and Comparative Examples 1 to 3 obtained above were evaluated by the following evaluation methods. <Absorption spectrum> The absorption spectra of methylene chloride solutions of the active energy ray polymerization initiators TX-1 and TX-8 of Examples 1 and 8 were measured using an ultraviolet, visible, near infrared spectrophotometer V-680 (manufactured by JASCO Corporation). The absorption spectra of TX-1 and TX-8 are shown in Figures 1 and 2, respectively. The absorption spectra of the active energy ray polymerization initiators Ref-1, Ref-2, and Ref-3 of Comparative Examples 1 to 3 were measured in the same manner as above. The results are shown in Figures 3, 4, and 5, respectively. It was confirmed that the polymerization initiators TX-1 and TX-8 of the present invention and the comparative polymerization initiator Ref-1 absorb light with wavelengths of 440 nm or less and are compatible with LED light sources of 365 nm, 385 nm, and 395 nm as active energy ray polymerization initiators. On the other hand, the comparative polymerization initiator Ref-2 absorbs light of 400 nm or less, but the absorption is significantly weaker than that of the polymerization initiators TX-1 and TX-2. In addition, the comparative polymerization initiator Ref-3 does not absorb any light of 350 nm or more, and it was confirmed that the comparative polymerization initiator Ref-3 is not compatible with light sources of 365 nm, 385 nm, and 395 nm.
[0073] <Reactivity> 365nm UV-LED irradiation device (LIGHTINGCURE TM The functions of the active energy ray polymerization initiators were evaluated using a high-sensitivity differential scanning calorimeter (DSC7020, manufactured by SII Nano Technology Co., Ltd.) equipped with a 385 nm UV-LED irradiation device (UV-LED LIGHT SOURCE EXECURE-H-1VCII, manufactured by HOYA Corporation), or a 395 nm UV-LED irradiation device (JOL-1205AIT). The active energy ray polymerization initiators of Examples 1 to 14 (TX-1 to TX-14) or the active energy ray polymerization initiators of Comparative Examples 1 to 3 (Ref-1 to Ref-3) were mixed with N-vinylacetamide (manufactured by Tokyo Chemical Industry Co., Ltd.) in a mass ratio of 1:1, and 10 mg of the mixture was weighed onto an aluminum pan and incubated at 10 mW / cm 2 The samples were irradiated with ultraviolet light of 365 nm, 385 nm, or 395 nm for 30 seconds at room temperature, and the maximum heat generation (Hmax [mW]) and the time to reach the maximum heat generation (Tmax [sec]) were measured. From the results shown in Table 2, it is clear that the active energy ray polymerization initiator of the present invention reacts faster to ultraviolet rays of each wavelength than the active energy ray polymerization initiator of the comparative example.
[0074] <Water-soluble> The active energy ray polymerization initiators of Examples 1 to 14 (TX-1 to TX-14) or the active energy ray polymerization initiators of Comparative Examples 1 to 3 (Ref-1 to Ref-3) were added to a solution in which ion-exchanged water and methanol were mixed at a ratio of 1:1 by mass, and the water solubility was evaluated and determined as follows. A: Dissolves at 5% by mass or more in the mixed solution B: Dissolves in the mixed solution at 1.5% by mass or more and less than 5% by mass. C: Dissolves in the mixed solution at 0.5% by mass or more and less than 1.5% by mass. D: Dissolves in the mixed solution at less than 0.5% by mass The results are shown in Table 2. From the results shown in Table 2, it is clear that the active energy ray polymerization initiator of the present invention has higher water solubility than the active energy ray polymerization initiator of the comparative example.
[0075] [Table 2]
[0076] The present invention relates to the active energy ray polymerization initiator of (1) below, and includes the following (2) to (8) as embodiments. (1) An active energy ray polymerization initiator having a structure represented by the following general formula (1): [ka] (In the formula, R1 is H or a methoxy group, R2 is H or a C1 to C8 hydrocarbon group, Alk is a C3 to C12 hydrocarbon group, and Lnk is a bond or a group represented by the following structural formula (1). [ka] (2) The active energy ray polymerization initiator according to the above (1), wherein the Lnk is a group represented by the above structural formula (1). (3) The active energy ray polymerization initiator according to (2) above, wherein R1 is H. (4) An active energy ray-curable composition comprising the active energy ray polymerization initiator according to any one of (1) to (3) above. (5) An active energy ray-curable ink containing the active energy ray polymerization initiator according to any one of (1) to (3) above. (6) An ink container containing the active energy ray-curable ink described in (5) above. (7) An image forming method comprising discharging the active energy ray curable ink according to (5) above onto a recording medium to form an image. (8) An image forming apparatus comprising an ink container that contains the active energy ray-curable ink described in (5) above, and a discharge means that discharges the ink contained in the ink container onto a recording medium. [Prior art documents] [Patent documents]
[0077] [Patent Document 1] Patent No. 6318111
Claims
1. An active energy ray polymerization initiator having a structure represented by the following general formula (1): [Formula 1] (In general formula (1), R 1 is H or a methoxy group, R 2 is H or a C1-8 hydrocarbon group, Alk is a C3-12 hydrocarbon group, and Lnk is a single bond or a group represented by the following structural formula (1): [chemical 2]
2. The active energy ray polymerization initiator according to claim 1 , wherein the Lnk is a group represented by the structural formula (1).
3. The R 1 The active energy ray polymerization initiator according to claim 2 , wherein
4. An active energy ray-curable composition comprising the active energy ray polymerization initiator according to claim 1 .
5. An active energy ray-curable ink comprising the active energy ray polymerization initiator according to claim 1 .
6. An ink container containing the active energy ray-curable ink according to claim 5 .
7. An image forming method comprising discharging the active energy ray curable ink according to claim 5 onto a recording medium to form an image.
8. 6. An image forming apparatus comprising: an ink container that contains the active energy ray curable ink according to claim 5; and a discharge unit that discharges the ink contained in the ink container onto a recording medium.
Citation Information
Patent Citations
Thioxanthone, manufacture and photopolymerizable composition
JP1983079991A
Manufacture of builtup cam shaft
JP1988018111A
Aqueous photocurable resin composition, waste-based ink, ink cartridge, recording unit, inkjet recording apparatus and photopolymerization initiator
JP2002187918A
Aqueous curing type ink for ink jet and recording method using the same