Ceramic electronic components and their manufacturing method

The ceramic electronic component with recessed external electrodes and differential material densities addresses the bonding strength issue by stabilizing solder volume, enhancing the reliability of the ceramic capacitor-circuit board interface.

JP7562249B2Active Publication Date: 2024-10-07TAIYO YUDEN KK
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2019208102
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-11-18
Publication Date
2024-10-07
Estimated Expiration
2039-11-18

AI Technical Summary

Technical Problem

The bonding strength between multilayer ceramic capacitors and circuit boards is compromised due to reduced solder bonding areas, which can be exacerbated by inconsistent formation of recessed portions in external electrodes, leading to potential instability in the bonding process.

Method used

A ceramic electronic component design featuring a laminated structure with external electrodes having recesses on specific side surfaces, utilizing different material densities for side margin and cover layers to stabilize the formation of recesses, ensuring a controlled depth and increased solder volume for enhanced bonding.

Benefits of technology

The proposed design ensures stable and robust bonding strength between the ceramic electronic component and the circuit board by increasing the solder volume in the bonding area, thereby improving reliability and consistency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562249000003
    Figure 0007562249000003
  • Figure 0007562249000004
    Figure 0007562249000004
  • Figure 0007562249000005
    Figure 0007562249000005
Patent Text Reader

Abstract

To provide a ceramic electronic component which allows for securement of bonding strength between the ceramic electronic component and a circuit board, and a manufacturing method of a ceramic electronic component.SOLUTION: A multilayer ceramic capacitor 100 comprises: laminated structure in which a dielectric layer 11 containing ceramic as a main component and an internal electrode layer 12 are alternately laminated; and cover layers 13 provided on the upper surface and the lower surface in the lamination direction, of the laminated structure, and further comprises: a laminated chip 10 having a substantially rectangular parallelepiped shape and formed in such a manner that a plurality of laminated internal electrode layers are exposed to two opposite end facing each other alternately; and a pair of external electrodes 20a and 20b formed from the two end faces to the four sides of the laminated chip. The external electrode has recesses 24 on at least one of the two side surfaces facing each other in the lamination direction or one of the other two side surfaces, and has no recess on the other two side surfaces.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ceramic electronic component and a method for manufacturing the same. [Background technology]

[0002] As electronic devices become smaller and more powerful, proposals have been made to reduce the mounting space required for electronic components such as multilayer ceramic capacitors on circuit boards, including control of the shape of solder fillets formed by the wetting and rising of solder onto the end faces of external electrodes (e.g., Patent Documents 1 and 2) and reduction of land patterns (e.g., Patent Documents 3 and 4). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-026392 A [Patent Document 2] JP 2017-103321 A [Patent Document 3] JP 2014-086606 A [Patent Document 4] JP 2016-219624 A [Patent Document 5] JP 2013-012561 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the techniques described in Patent Documents 1 to 4, the solder joint area in the multilayer ceramic capacitor and the circuit board is small, which raises concerns about a decrease in the joint strength between the multilayer ceramic capacitor and the circuit board.

[0005] Therefore, for example, as shown in Patent Document 5, a concave portion may be formed on the peripheral surface of the external electrode to increase the amount of solder between the multilayer ceramic capacitor and the circuit board, thereby improving the bonding strength between the multilayer ceramic capacitor and the circuit board.

[0006] In Patent Document 5, the amount of binder in the conductive paste for forming the external electrodes is adjusted to form recesses on the peripheral surfaces of the external electrodes. In this case, it is not possible to stably form recesses with a predetermined depth, and depending on the finished product, sufficient bonding strength may not be obtained.

[0007] The present invention has been made in view of the above-mentioned problems, and has an object to provide a ceramic electronic component that can ensure the bonding strength between the ceramic electronic component and a circuit board, and a manufacturing method thereof. [Means for solving the problem]

[0008] A ceramic electronic component according to the present invention comprises a laminated chip having a laminated structure in which ceramic-based dielectric layers and internal electrode layers are alternately laminated, and cover layers provided on upper and lower surfaces in a lamination direction of the laminated structure, the laminated chip having a substantially rectangular parallelepiped shape and formed so that a plurality of the laminated internal electrode layers are exposed on two end surfaces that alternately face each other, and a pair of external electrodes formed from the two end surfaces to four side surfaces of the laminated chip, the external electrodes having a recess on at least one of the two side surfaces that face each other in the lamination direction and the other two side surfaces. and when the external electrode has a recess on at least one of the two side surfaces opposing each other in the stacking direction, a first side margin portion that faces each other in a direction perpendicular to the stacking direction and the opposing direction in which the two end faces face each other and covers the end faces of the dielectric layer, the internal electrode layer, and the cover layer of the stacked structure from the upper surface to the lower surface constitutes the other two side surfaces, and the second side margin portion and the cover layer constitute two side surfaces opposing each other in the stacking direction, and have different characteristics from the first side margin portion and the cover layer, the recess is formed by a difference between a characteristic of the ceramic dielectric layer green sheet which is a material of the first side margin portion and a characteristic of a cover sheet which is a material of the cover layer,When the external electrode has a recess on at least one of the other two side surfaces, the cover layers provided on the upper surface and the lower surface constitute two side surfaces opposing each other in the lamination direction, a second side margin portion extending from each of the other two side surfaces of the laminated structure to the internal electrode layer and the cover layers provided on the upper surface and the lower surface constitute the other two side surfaces, and the second side margin portion and the cover layer have different characteristics. The recess is formed by the difference between the characteristics of the ceramic dielectric layer green sheet, which is the material of the second side margin portion, and the characteristics of the cover sheet, which is the material of the cover layer. , characterized in that

[0009] When the external electrode has a recess on at least one of two side surfaces opposing each other in the stacking direction, the density of the first side margin portion is smaller than the density of the cover layer, the density of the first side margin portion is uniform, and the density of the cover layer is uniform; when the external electrode has a recess on at least one of the other two side surfaces, the density of the cover layer is smaller than the density of the second side margin portion, the density of the cover layer is uniform, and the density of the second side margin portion is uniform. It is also possible to use the following.

[0011] In the above ceramic electronic component, when the distance between the midpoint of a line connecting the vertex at the periphery of the recess where the external electrode is farthest from the side surface of the laminated chip having the recess and the vertex at the periphery of the laminated chip where the external electrode is closest to the side surface of the laminated chip having the recess and the side surface of the laminated chip where the external electrode is located having the recess, and the distance between the midpoint and the point at which the recess is deepest, and d, a recess level X expressed by X=d / t may be 25% or more and 75% or less.

[0012] In the ceramic electronic component, the surface on which the recess is formed may be a mounting surface for mounting on a circuit board.

[0013] The ceramic electronic component may include a covering portion that covers five of six faces of the ceramic electronic component excluding the face on which the recess is formed.

[0014] The method for producing a ceramic electronic component according to the present invention includes alternately laminating ceramic dielectric layer green sheets and conductive pastes for forming internal electrode layers, and forming the outermost layer by The density is lower than that of the ceramic dielectric layer green sheet, and the density is uniform. A cover sheet is used, and the laminated conductive pastes for forming internal electrode layers are exposed on two end faces that are alternately opposed to each other to form a ceramic laminate having a substantially rectangular parallelepiped shape, and a metal paste is applied from the two end faces of the ceramic laminate to four side faces of the ceramic laminate; Due to the difference in density between the ceramic dielectric layer green sheet and the cover sheet,The present invention is characterized in that a recess is formed in the metal paste on at least one of two opposing side surfaces in a direction perpendicular to the stacking direction of the ceramic laminate and the opposing direction of the two end faces, and no recess is formed in the metal paste on the two opposing side surfaces in the stacking direction, and the metal paste and the ceramic laminate are fired simultaneously.

[0016] The method for producing a ceramic electronic component according to the present invention includes forming a laminated structure by alternately laminating ceramic dielectric layer green sheets and conductive paste for forming internal electrode layers, and forming a laminated structure on the upper and lower surfaces of the laminated structure in the lamination direction. The density is uniform A cover sheet is arranged and the laminated structure is cut to form two end faces where the internal electrode layers are exposed every other one, and two side faces where all of the internal electrode layers are exposed, and on the two side faces where all of the internal electrode layers are exposed, The density is lower than the density of the cover sheet, and the density is uniform. By disposing a side margin sheet, a ceramic laminate having a substantially rectangular parallelepiped shape is formed in which the laminated conductive pastes for forming internal electrode layers are exposed on two end faces that are alternately opposed to each other, and a metal paste is applied from the two end faces of the ceramic laminate to four side faces of the ceramic laminate; The difference in density between the cover sheet and the side margin sheet The method is characterized in that a recess is formed in the metal paste on at least one of two opposing side surfaces in the stacking direction, and no recess is formed in the metal paste on side surfaces other than the two opposing side surfaces among the four side surfaces, and the metal paste and the ceramic laminate are fired simultaneously. Effect of the Invention

[0018] According to the present invention, it is possible to ensure the bonding strength between the ceramic electronic component and the circuit board. [Brief description of the drawings]

[0019] [Figure 1] 1 is a partial cross-sectional perspective view of a multilayer ceramic capacitor in accordance with a first embodiment. [Diagram 2]2A is a partial cross-sectional view taken along line CC in FIG. 1, and FIG. 2B is a cross-sectional view taken along line CC in FIG. [Diagram 3] 3A is a cross-sectional view taken along line AA in FIG. 1, and FIG. 3B is a cross-sectional view taken along line BB in FIG. [Figure 4] FIG. 4 is a diagram for explaining the recess level X. As shown in FIG. [Diagram 5] FIG. 5 is a diagram showing a state in which the multilayer ceramic capacitor in accordance with the first embodiment is mounted on a mounting surface of a substrate. [Figure 6] FIG. 6 is a flowchart illustrating the method for manufacturing the multilayer ceramic capacitor in accordance with the first embodiment. [Figure 7] 7(A) to 7(C) are diagrams illustrating the mechanism by which recesses are formed. [Figure 8] FIG. 8 is a partial cross-sectional perspective view of the multilayer ceramic capacitor 100 in accordance with the second embodiment. [Figure 9] 9(A) is a cross-sectional view taken along line AA in FIG. 8, and FIG. 9(B) is a cross-sectional view taken along line CC in FIG. [Figure 10] FIG. 10 is a diagram showing a state in which the multilayer ceramic capacitor in accordance with the second embodiment is mounted on a mounting surface of a substrate. [Figure 11] FIG. 11 is a flowchart illustrating the method for manufacturing the multilayer ceramic capacitor in accordance with the second embodiment. [Figure 12] FIG. 12A is a perspective view of a multilayer ceramic capacitor according to a modified example, and FIG. 12B is a cross-sectional view taken along line CC in FIG. 12A. [Figure 13] FIG. 13 is a flowchart illustrating a method for manufacturing a multilayer ceramic capacitor according to a modified example. [Figure 14] 14(A) to 14(D) are diagrams illustrating a method for manufacturing a multilayer ceramic capacitor according to a modified example. [Figure 15] FIG. 15 is a graph showing the actual measured values ​​of the dent level relative to the design values ​​of the dent level in the embodiment and the modified example. [Figure 16]FIG. 16 is a graph showing the bonding strength versus the dent level X. [Figure 17] FIG. 17 is a diagram for explaining the length of the exposed portion. [Figure 18] FIG. 18 is a graph showing the relationship between the recess level X and the bonding strength for different lengths of the exposed portion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, an embodiment will be described with reference to the drawings.

[0021] (First embodiment) First, the multilayer ceramic capacitor will be described. Fig. 1 is a partial cross-sectional perspective view of a multilayer ceramic capacitor 100 according to a first embodiment. As illustrated in Fig. 1, the multilayer ceramic capacitor 100 includes a laminated chip 10 having a rectangular parallelepiped shape, and external electrodes 20a, 20b provided on any two opposing end faces of the laminated chip 10. The four faces of the laminated chip 10 other than the two end faces are referred to as side faces. The external electrodes 20a, 20b extend to the four side faces. However, the external electrodes 20a, 20b are spaced apart from each other on the four side faces.

[0022] The laminated chip 10 has a configuration in which dielectric layers 11 containing a ceramic material that functions as a dielectric and internal electrode layers 12 are alternately laminated. The edges of the internal electrode layers 12 are alternately exposed to the end face on which the external electrode 20a of the laminated chip 10 is provided and the end face on which the external electrode 20b is provided. As a result, the internal electrode layers 12 are alternately conductive to the external electrodes 20a and the external electrodes 20b. In addition, of the four side surfaces of the laminated chip 10, two side surfaces corresponding to the upper and lower surfaces in the lamination direction of the dielectric layers 11 and the internal electrode layers 12 (hereinafter referred to as the lamination direction) are formed by the cover layer 13. The cover layer 13 is mainly composed of a ceramic material. For example, the main component material of the cover layer 13 is the same as the main component material of the dielectric layer 11.

[0023] The size of the multilayer ceramic capacitor 100 is, for example, 0.25 mm in length, 0.125 mm in width, and 0.125 mm in height, or 0.4 mm in length, 0.2 mm in width, and 0.2 mm in height, or 0.6 mm in length, 0.3 mm in width, and 0.3 mm in height, or 1.0 mm in length, 0.5 mm in width, and 0.5 mm in height, or 3.2 mm in length, 1.6 mm in width, and 1.6 mm in height, or 4.5 mm in length, 3.2 mm in width, and 2.5 mm in height, but is not limited to these sizes.

[0024] The dielectric layer 11 is mainly composed of a ceramic material having a perovskite structure represented by the general formula ABO3. 3-α For example, the ceramic material includes BaTiO3 (barium titanate), CaZrO3 (calcium zirconate), CaTiO3 (calcium titanate), SrTiO3 (strontium titanate), BaTiO3 (strontium titanate) which forms a perovskite structure, 1-x-y Ca x Sr y Ti 1-z Zr z O3 (0≦x≦1, 0≦y≦1, 0≦z≦1) can be used. The average thickness of the dielectric layer 11 is, for example, 1 μm or less.

[0025] The internal electrode layer 12 is mainly composed of base metals such as Ni (nickel), Cu (copper), and Sn (tin). The internal electrode layer 12 may be mainly composed of precious metals such as Pt (platinum), Pd (palladium), Ag (silver), and Au (gold), or alloys containing these metals. The average thickness of the internal electrode layer 12 is, for example, 1 μm or less.

[0026] 2(A) is a cross-sectional view of the external electrode 20b, and is a partial cross-sectional view taken along the line CC in FIG. 1. The ceramic material is mainly exposed on the surface of the laminated chip 10. Therefore, it is difficult to form a plating layer on the surface of the laminated chip 10 without a base layer. Therefore, as illustrated in FIG. 2(A), the external electrode 20b has a structure in which a plating layer is formed on an underlying conductor layer 21 formed on the surface of the laminated chip 10. The plating layer includes a first plating layer 22 that contacts and covers the underlying conductor layer 21, and a second plating layer 23 that contacts and covers the first plating layer 22. An underlying plating layer may be provided between the underlying conductor layer 21 and the first plating layer 22. The base conductor layer 21 mainly contains a metal such as Cu, Ni, Al (aluminum), Zn (zinc), Ag, Au, Pd, Pt, etc., or an alloy of two or more of these (for example, an alloy of Cu and Ni), and contains ceramics such as a glass component for densifying the base conductor layer 21 and a co-material for controlling the sinterability of the base conductor layer 21. The glass component is an oxide such as Ba (barium), Sr (strontium), Ca (calcium), Zn, Al, Si (silicon), B (boron), etc. The co-material is, for example, a ceramic component mainly containing the same material as the main component of the ceramic dielectric layer 11. The plating layer mainly contains a metal such as Cu, Ni, Al, Zn, Sn, etc., or an alloy of two or more of these.

[0027] Fig. 2(B) is a cross-sectional view taken along line CC in Fig. 1, Fig. 3(A) is a cross-sectional view taken along line AA in Fig. 1, and Fig. 3(B) is a cross-sectional view taken along line BB in Fig. 1. As shown in Fig. 3(A), in the laminated chip 10, the portions extending from the two side surfaces of the laminated chip 10 to the internal electrode layers 12 are referred to as side margin portions 16. That is, the side margin portions 16 are portions provided in a laminated structure in which the dielectric layers 11 and the internal electrode layers 12 are laminated, so as to cover the ends of the laminated multiple internal electrode layers 12 extending to the two side surfaces of the laminated chip 10.

[0028] As shown in FIG. 1, FIG. 2(B), FIG. 3(A), and FIG. 3(B), each of the external electrodes 20a and 20b has a recess 24 on at least one of two side surfaces other than the two side surfaces facing each other in the stacking direction, and does not have a recess 24 on the two side surfaces (upper and lower surfaces) facing each other in the stacking direction of the laminated chip 10. Here, not having a recess 24 means that when the ratio of the depth d of the recess 24 to the thickness t of the external electrodes 20a and 20b is defined as the recess level X (=(d / t)×100[%]), the recess level X is less than 25%. Note that the thickness t of the external electrodes 20a and 20b is the distance between the midpoint CP of a line connecting the vertex P1, which is the furthest from the side surface of the laminated chip 10 where the external electrodes 20a and 20b have the recess 24, and the vertex P2, which is the closest to the side surface of the laminated chip 10, on the periphery of the recess 24, and the side surface of the laminated chip 10, as shown in FIG. Further, the depth d of the recess 24 is the distance between the midpoint CP and the point where the recess 24 is deepest (the point where the external electrodes 20a, 20b are thinnest). Since the recess 24 is formed in the external electrodes 20a, 20b on the side surfaces formed of the side margin portion 16 and the cover layer 13 using materials having different properties (e.g., density), the recess 24 can have a desired recess level X. Since the side surfaces in the stacking direction of the laminated chip 10 (the upper and lower surfaces in the stacking direction) are formed of the cover layer 13 with uniform properties, it is difficult to form the recess 24 with the desired recess level X.

[0029] In the multilayer ceramic capacitor 100 according to the first embodiment, a pair of external electrodes 20a, 20b formed over the four side surfaces of the multilayer chip 10 has a recess 24 on at least one of the two side surfaces (the other two side surfaces in the first embodiment) between the two side surfaces facing each other in the stacking direction of the multilayer chip 10 and the other two side surfaces, and does not have a recess 24 on the other two side surfaces (the two side surfaces facing each other in the stacking direction in the first embodiment). As shown in Fig. 5, by soldering (mounting) the multilayer ceramic capacitor 100 on the mounting surface 101 of the circuit board S with the recess 24 facing the circuit board, the recess 24 can increase the amount of solder H between the multilayer ceramic capacitor 100 and the circuit board S compared to a case where the recess 24 is not present, and therefore the bonding strength between the multilayer ceramic capacitor 100 and the circuit board S can be ensured.

[0030] As the recess level X becomes smaller, the depth d of the recess 24 becomes smaller, so that the amount of solder H becomes smaller when mounting the multilayer ceramic capacitor 100 on a circuit board, and it is possible that a predetermined bonding strength cannot be ensured. Therefore, the recess level X is preferably 25% or more. On the other hand, if the recess level X is too large, the thickness of the external electrodes 20a, 20b becomes insufficient, and the element body may be exposed or the reliability may be reduced. Therefore, the recess level X is preferably 75% or less.

[0031] The external electrodes 20a, 20b of the multilayer ceramic capacitor 100 may have recesses on two end faces, so long as the thickness of the external electrodes 20a, 20b at their thinnest portions is ensured to be equal to or greater than a predetermined value.

[0032] Next, a method for manufacturing the multilayer ceramic capacitor 100 in accordance with the first embodiment will be described. Fig. 6 is a flowchart showing the method for manufacturing the multilayer ceramic capacitor 100 in accordance with the first embodiment.

[0033] (Raw powder production process) First, a predetermined additive compound is added to the powder of the ceramic material, which is the main component of the dielectric layer 11, according to the purpose. Examples of the additive compound include oxides of Mg (magnesium), Mn (manganese), V (vanadium), Cr (chromium), rare earth elements (Y (yttrium), Sm (samarium), Eu (europium), Gd (gadolinium), Tb (terbium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium), and Yb (ytterbium)), as well as oxides or glasses of Co (cobalt), Ni, Li (lithium), B, Na (sodium), K (potassium), and Si. For example, first, a compound containing the additive compound is mixed with the powder of the ceramic material and calcined. Then, the particles of the obtained ceramic material are wet-mixed with the additive compound, and the mixture is dried and pulverized to prepare a powder of the ceramic material.

[0034] (Lamination process) Next, a binder such as polyvinyl butyral (PVB) resin, an organic solvent such as ethanol or toluene, and a plasticizer are added to the obtained ceramic material powder and wet mixed. The obtained slurry is used to coat a strip-shaped dielectric green sheet, for example, with a thickness of 1.0 μm or less, on a substrate by, for example, a die coater method or a doctor blade method, and then dried.

[0035] Next, the pattern of the internal electrode layer 12 is arranged by printing the conductive paste for forming the internal electrode layer on the surface of the dielectric green sheet by screen printing, gravure printing, or the like. The conductive paste for forming the internal electrode layer contains the main component metal of the internal electrode layer 12, a binder, a solvent, and other auxiliary agents as necessary. It is preferable to use a binder and a solvent different from the above-mentioned ceramic slurry. In addition, the ceramic material that is the main component of the dielectric layer 11 may be dispersed in the conductive paste for forming the internal electrode layer as a co-material.

[0036] Next, the dielectric green sheet on which the internal electrode layer pattern is printed is punched out to a predetermined size, and the punched dielectric green sheet is laminated, with the base material peeled off, to a predetermined number of layers (e.g., 200 to 500 layers) such that the internal electrode layers 12 and the dielectric layers 11 are alternated and the edges of the internal electrode layers 12 are alternately exposed at both longitudinal end faces of the dielectric layers 11 and alternately drawn out to a pair of external electrodes having opposite polarities.

[0037] Cover sheets that will become the cover layers 13 are pressed onto the top and bottom of the laminated pattern forming sheets, and then cut to a predetermined chip size (for example, 1.0 mm x 0.5 mm). At this time, a cover sheet with a density lower than that of the dielectric green sheets that form the side margin portion 16 is used. This results in a ceramic laminate having an approximately rectangular parallelepiped shape.

[0038] (Coating process) The ceramic laminate obtained in the lamination process is subjected to binder removal in an N2 atmosphere at 250 to 500°C, and then, as shown in FIG. 7(A), a metal paste 21a that will become the base conductor layer 21 of the external electrodes 20a, 20b is applied to both end faces and four side faces of the ceramic laminate by a dipping method or the like, and then dried.

[0039] At this time, as shown in FIG. 7(B), the density of the cover sheet 13a that becomes the cover layer 13 is lower than the density of the dielectric green sheet 11a that forms the side margin portion 16, so the moisture in the metal paste 21a permeates into the cover sheet 13a at a faster permeation rate (see arrow AR1) than into the side margin portion 16 (see arrow AR2). As a result, the metal paste 21a dries from the cover sheet 13a side (outside) and shrinks. As a result, as shown by arrow AR3, the metal paste 21a that is not yet dried in the center is pulled outward (to the cover sheet 13a side). This reduces the solvent concentration at the end of the metal paste 21a that is not yet dried, and increases the surface tension. Therefore, as shown in FIG. 7(C), the end of the metal paste 21a that is not yet dried becomes thicker due to mass transfer from the center, and the center becomes recessed, forming a recess 24. In this way, since materials with different properties can be used for the cover sheet 13a and the dielectric green sheet 11a, it is possible to form recesses 24 having a desired recess level X in the external electrodes 20a, 20b on the side surfaces formed by the cover sheet 13a and the dielectric green sheet 11a by utilizing the difference in properties between the cover sheet 13a and the dielectric green sheet 11a. On the other hand, since the upper and lower surfaces in the lamination direction of the ceramic laminate are formed by the cover sheet 13a, it is not possible to form the recesses 24 by utilizing the difference in properties, and it is difficult to form the recesses 24 having the desired recess level X.

[0040] (Firing process) Thereafter, the metal paste and ceramic laminate are fired for about 2 hours at a temperature of about 900°C to 1050°C in a reducing atmosphere with about 1.5% by volume of H2. This allows the firing of the dielectric layers 11 and the internal electrode layers 12 and the baking of the base conductor layers 21 to be performed simultaneously, and a semi-finished multilayer ceramic capacitor 100 can be obtained.

[0041] (Reoxidation treatment process) After that, a re-oxidation treatment may be performed at 600°C to 1000°C in an N2 gas atmosphere.

[0042] (Plating layer formation process) Next, a first plating layer 22 is formed by electrolytic plating on the underlying conductor layer 21 of the semi-finished product. Furthermore, a second plating layer 23 is formed on the first plating layer 22 by electrolytic plating.

[0043] As described above, according to the manufacturing method of the multilayer ceramic capacitor 100 according to the first embodiment shown in FIG. 6, the multilayer ceramic capacitor 100 can be manufactured in which the external electrodes 20a, 20b formed on the two end faces to the four side faces of the multilayer chip 10 have the recess 24 on at least one of the two side faces other than the two side faces facing each other in the stacking direction of the multilayer chip 10, and the two side faces facing each other in the stacking direction of the multilayer chip 10 do not have the recess 24. By soldering (mounting) the multilayer ceramic capacitor 100 on the mounting surface of the circuit board with the recess 24 facing the circuit board, the recess 24 can increase the amount of solder between the multilayer ceramic capacitor 100 and the circuit board compared to a case where the recess 24 is not present, so that the bonding strength between the multilayer ceramic capacitor 100 and the circuit board can be ensured. Note that not forming the recess 24 in the metal paste on the side faces other than the two facing side faces among the four side faces of the ceramic laminate means not forming the recess 24 with the recess level X of 25% or more.

[0044] In the first embodiment, the density of the cover sheet 13a is smaller than that of the dielectric green sheet 11a. This makes it possible to stably form the recesses 24 having a depth sufficient to ensure a predetermined bonding strength, compared to when the same material is used for the cover sheet 13a and the dielectric green sheet 11a and the recesses 24 are formed by adjusting the amount of binder in the conductive paste for forming the base conductor layer. This makes it possible to ensure the bonding strength between the multilayer ceramic capacitor 100 and the circuit board.

[0045] Second embodiment Fig. 8 is a partial cross-sectional perspective view of a multilayer ceramic capacitor 100A in accordance with the second embodiment, Fig. 9(A) is a cross-sectional view taken along line AA in Fig. 8, and Fig. 9(B) is a cross-sectional view taken along line CC in Fig. 8.

[0046] The multilayer ceramic capacitor 100A differs from the multilayer ceramic capacitor 100 (see FIG. 1) in that a recess 24 is formed on at least one of two side surfaces (upper and lower surfaces in the stacking direction) facing each other in the stacking direction among the four side surfaces of the laminated chip 10, and no recess 24 is formed on the other two side surfaces. Note that "no recess 24 is formed" means that the recess level X described in the first embodiment is less than 25%.

[0047] As shown in FIG. 9(A), in the multilayer ceramic capacitor 100A, the two side surfaces of the multilayer chip 10 facing each other in the stacking direction are formed by the cover layer 13 and the third margin portion 16. Meanwhile, the other two side surfaces of the multilayer chip 10 are formed by the side margin portion 16. Since the recesses 24 are formed in the external electrodes 20a, 20b on the side surfaces (upper and lower surfaces in the stacking direction) formed by the side margin portion 16 and the cover layer 13 using materials having different properties (e.g., density), the recesses 24 can have a desired recess level X. Meanwhile, since the two side surfaces in the facing direction of the two end faces of the multilayer chip 10 and in the direction perpendicular to the stacking direction are formed by the side margin portion 16 having uniform properties, it is difficult to form the recesses 24 having the desired recess level X. Since the other configurations are the same as those of the multilayer ceramic capacitor 100, detailed description thereof will be omitted.

[0048] In the multilayer ceramic capacitor 100A according to the second embodiment, a pair of external electrodes 20a, 20b formed over the four side surfaces of the laminated chip 10 has a recess 24 on at least one of two side surfaces between the two side surfaces facing each other in the stacking direction and the other two side surfaces (in the second embodiment, the two side surfaces facing each other in the stacking direction), and does not have a recess 24 on the other two side surfaces (in the second embodiment, the two side surfaces facing each other in the facing direction of the two end faces and in the direction perpendicular to the stacking direction). As shown in FIG. 10, by soldering (mounting) the multilayer ceramic capacitor 100A on the mounting surface 101 of the circuit board S with the recess 24 facing the circuit board, the recess 24 can increase the amount of solder H between the multilayer ceramic capacitor 100 and the circuit board S compared to a case where the recess 24 is not present, and therefore the bonding strength between the multilayer ceramic capacitor 100A and the circuit board S can be ensured.

[0049] In the multilayer ceramic capacitor 100A as well, the external electrodes 20a, 20b may have recesses on two end faces as long as the thickness of the external electrodes 20a, 20b at their thinnest portions is ensured to be equal to or greater than a predetermined value.

[0050] Next, a method for manufacturing the multilayer ceramic capacitor 100A in accordance with the second embodiment will be described. Fig. 11 is a flowchart showing the method for manufacturing the multilayer ceramic capacitor 100A in accordance with the second embodiment. Note that only differences from the method for manufacturing the multilayer ceramic capacitor 100 shown in Fig. 6 will be described, and detailed descriptions of the rest will be omitted.

[0051] (Raw powder production process) In the raw powder preparation process, a side margin material for forming the side margin portion 16 is prepared. A specific additive compound is added to a ceramic powder of barium titanate obtained by a process similar to that of the dielectric material preparation process for forming the dielectric layer 11, depending on the purpose. The additive compound may be oxides of Mn, V, Cr, and rare earth elements, as well as oxides or glasses of Co, Ni, Li, B, Na, K, and Si.

[0052] (Lamination process) A conductive paste for forming an internal electrode layer is printed on the surface of the dielectric green sheet by screen printing, gravure printing, or the like to arrange the pattern of the internal electrode layer 12. Next, the dielectric green sheet on which the pattern of the internal electrode layer 12 is printed is punched out to a predetermined size, and the punched dielectric green sheet is laminated by a predetermined number of layers (for example, 200 to 500 layers) in a state where the base material is peeled off so that the internal electrode layer 12 and the dielectric layer 11 are alternately arranged, and the internal electrode layer 12 is alternately drawn to a pair of external electrodes having different polarities by exposing the end edges alternately at both end faces in the length direction of the dielectric layer 11. Next, cover sheets to become the cover layer 13 are laminated on the top and bottom and pressed. Thereafter, the obtained laminate is cut to a predetermined dimension to form a laminate having two end faces where the patterns of the internal electrode layer 12 are exposed every other one, and two side faces where the patterns of all the internal electrode layers 12 are exposed.

[0053] (Side margin forming process) A binder such as polyvinyl butyral (PVB) resin, an organic solvent such as ethanol or toluene, and a plasticizer are added to the side margin material and wet mixed. The obtained slurry is used to coat, for example, a strip-shaped side margin sheet on a substrate by, for example, a die coater method or a doctor blade method, and then dried. Side margin sheets that become the side margin portions 16 are attached to two side surfaces on which the patterns of all the internal electrode layers 12 of the laminate are exposed. At this time, by using a side margin sheet that has a lower density than the cover sheet, it is possible to form a recess 24 having a desired recess level X in the external electrodes 20a, 20b on the side surfaces formed by the cover sheet and the side margin sheet.

[0054] As described above, according to the manufacturing method of the multilayer ceramic capacitor 100A according to the second embodiment shown in FIG. 11, the multilayer ceramic capacitor 100A can be manufactured in which the external electrodes 20a, 20b formed on the two end faces to the four side faces of the laminated chip 10 have the recess 24 on at least one of the two side faces facing each other in the lamination direction, and the other two side faces (the two side faces facing each other in the direction perpendicular to the facing direction of the two end faces and the lamination direction of the laminated chip 10) do not have the recess 24. By soldering (mounting) the multilayer ceramic capacitor 100A on the mounting surface of the circuit board with the recess 24 facing the circuit board, the recess 24 can increase the amount of solder between the multilayer ceramic capacitor 100A and the circuit board compared to the case where the recess 24 is not present, so that the bonding strength between the multilayer ceramic capacitor 100A and the circuit board can be ensured. Note that not forming the recess 24 in the metal paste on the side faces other than the two opposing side faces among the four side faces of the ceramic laminate means not forming the recess 24 with the recess level X of 25% or more.

[0055] In addition, in the manufacturing method according to the present embodiment, the density of the side margin sheet is smaller than that of the cover sheet 13a. This makes it possible to stably form the recesses 24 having a depth sufficient to ensure a predetermined bonding strength, compared to the case where the recesses 24 are formed by adjusting the amount of binder in the conductive paste for forming the base conductor layer. Therefore, the bonding strength between the multilayer ceramic capacitor 100A and the circuit board can be ensured. In addition, since the side margin portion 16 can use a side margin sheet having a different composition from the ceramic dielectric layer green sheet that becomes the dielectric layer 11, the freedom of material selection for the cover sheet and the side margin sheet is improved.

[0056] In the manufacturing methods according to the first and second embodiments, the concave portions 24 are formed by making the density of the cover sheet smaller than that of the ceramic dielectric layer green sheet or by making the density of the side margin sheet smaller than that of the cover sheet, but the present invention is not limited to this. As long as the concave portions 24 can be formed before firing the metal paste and the ceramic laminate, the concave portions 24 may be formed by other methods such as surface treatment.

[0057] (Modification) Fig. 12(A) is a perspective view of a multilayer ceramic capacitor 100B according to a modified example, and Fig. 12(B) is a cross-sectional view taken along line CC in Fig. 12(A). The multilayer ceramic capacitor 100B according to the modified example includes a multilayer ceramic capacitor 100 and a covering portion 60. Note that the multilayer ceramic capacitor 100 may be replaced with a multilayer ceramic capacitor 100A.

[0058] The covering portion 60 is made of, for example, resin, and covers five of the six faces of the multilayer ceramic capacitor 100 excluding one of the two faces in which the recesses 24 are formed. Therefore, in the multilayer ceramic capacitor 100B, as shown in Fig. 12(B), exposed portions 25a, 25b are formed where the external electrodes 20a, 20b of the multilayer ceramic capacitor 100 are exposed without being covered by the covering portion 60.

[0059] The resin forming the covering portion 60 may be, for example, a thermosetting resin such as an epoxy resin, a polyimide resin, a phenol resin, or an amino resin, or an ultraviolet-curing resin such as a radical polymerization type or a cationic polymerization type. In this embodiment, the covering portion 60 is formed using a thermosetting resin. Although FIG. 12(A) shows an example in which the covering portion 60 is formed from a transparent or semitransparent resin, the covering portion 60 may be formed from an opaque resin or may be colored.

[0060] The multilayer ceramic capacitor 100B according to the modified example includes a covering portion 60 that covers five of the six faces of the multilayer ceramic capacitor 100 except for the face on which the recess 24 is formed. Solder cannot wet up the areas of the external electrodes 20a, 20b covered by the covering portion 60. This reduces the amount of solder that wets up, making it possible to reduce the mounting space. In addition, if the amount of solder that wets up is reduced by the covering portion 60, there is a concern that the bonding strength will decrease. However, since the multilayer ceramic capacitor 100B has the recess 24 formed on the mounting surface to the circuit board, the amount of solder between the multilayer ceramic capacitor 100B and the circuit board can be increased compared to a case in which the recess 24 is not formed, and the bonding strength can be ensured. Furthermore, since the five faces except for the face on which the recess 24 is formed are covered by the covering portion 60, it is easy to identify the mounting surface of the multilayer ceramic capacitor 100B to the circuit board.

[0061] Next, a method for manufacturing the multilayer ceramic capacitor 100B according to the modified example will be described below. Fig. 13 is a flowchart showing a method for manufacturing the multilayer ceramic capacitor 100B.

[0062] (Tape application process) As shown in FIG. 14(A), in the multilayer ceramic capacitor 100 manufactured by the manufacturing method of FIG. 6 or FIG. 11, one of the two faces on which the recesses 24 are formed in the external electrodes 20a, 20b is attached to a tape T.

[0063] (Resin coating process) The laminated ceramic capacitor 100 attached to the tape T is covered with the uncured resin 60a. For example, as shown in FIG. 14(B), the surface of the tape T opposite to the surface to which the laminated ceramic capacitor 100 is attached is fixed to a holding plate F, the holding plate F is arranged so that the laminated ceramic capacitor 100 faces downward, and the laminated ceramic capacitor 100 faces a bath containing the uncured resin 60a. Next, as shown in FIG. 14(C), the holding plate F is moved downward to immerse the laminated ceramic capacitor 100 in the uncured resin 60a. At this time, the tape T is prevented from contacting the uncured resin 60a. After that, as shown in FIG. 14(D), the laminated ceramic capacitor 100 is pulled upward. As a result, the uncured resin 60a adheres to the surface of the laminated ceramic capacitor 100, and the laminated ceramic capacitor 100 is covered with the uncured resin 60a.

[0064] (hardening process) After the uncured resin 60a is temporarily cured, the multilayer ceramic capacitor 100 is peeled off from the tape T. The temporarily cured resin is then permanently cured. Through the above steps, a multilayer ceramic capacitor 100B according to the modified example is obtained.

[0065] In the above embodiment and modified examples, a multilayer ceramic capacitor is described as an example of a ceramic electronic component, but the present invention is not limited to this. For example, other electronic components such as a varistor or a thermistor may be used. EXAMPLES

[0066] A multilayer ceramic capacitor according to the embodiment was fabricated, and the variation in the dent level X was examined.

[0067] (Examples 1 to 3) In Examples 1 to 3, a multilayer ceramic capacitor 100 having recesses 24 on two side surfaces of the external electrodes 20a, 20b was fabricated by making the density of the cover sheet smaller than the density of the ceramic dielectric green sheet forming the side margin portion 16. 100 multilayer ceramic capacitors 100 were fabricated with design values ​​of recess level X of 25, 50, and 75. The multilayer ceramic capacitor 100 had a length of 1.0 mm, a width of 0.5 mm, and a height of 0.5 mm.

[0068] In Comparative Examples 1 to 3, the density of the dielectric green sheet and the density of the cover sheet were made the same, and the binder amount of the metal paste for forming the base conductor layer was changed to form recesses 24 on the four side surfaces of the external electrodes 20a, 20b. 100 multilayer ceramic capacitors were manufactured with design values ​​of recess level X of 25, 50, and 75. In Comparative Examples 1 to 3, the recess level X of the recess 24 formed on the upper surface in the stacking direction among the recesses 24 formed on the four side surfaces was measured. This is because the binder amount of the metal paste for forming the base conductor layer was changed so that the recess level X of the recess 24 formed on the upper surface in the stacking direction was the design value.

[0069] Table 1 shows the actual measured value of the dent level X relative to the design value of the dent level X. Fig. 15 is a graph showing the variation of the actual measured value of the dent level X relative to the design value of the dent level X. [Table 1]

[0070] As shown in Table 1 and Fig. 15, by making the density of the cover sheet lower than the density of the side margin portion 16 and forming the recesses 24 on the two side surfaces of the external electrodes 20a, 20b, it is found that the variation in the recess level X from the design value can be reduced. In other words, it was found that the recesses 24 having the desired recess level X can be stably formed. On the other hand, in Comparative Examples 1 to 3, the variation in the recess level X from the design value is large, and there is a concern that the defective rate will increase if the recesses 24 are formed by changing the amount of binder in the metal paste for forming the base conductor layer.

[0071] Example 4 By varying the density difference between the density of the dielectric green sheet and the density of the cover sheet, multilayer ceramic capacitors 100 with different recess levels X were fabricated. The fabricated multilayer ceramic capacitors 100 were soldered to a circuit board with the recesses 24 facing the circuit board, and the bonding strength between the multilayer ceramic capacitor 100 and the circuit board was measured with a push-pull gauge. The multilayer ceramic capacitor 100 was 1.0 mm long, 0.5 mm wide, and 0.5 mm high.

[0072] Fig. 16 is a graph showing the relationship between the dent level X and the bonding strength. As shown in Fig. 16, it can be seen that the bonding strength tends to increase as the dent level X increases. Compared to the bonding strength when no recess 24 is formed (dent level X = 0%), when the dent level X is 25%, the bonding strength increases by about 5%, when the dent level X is 50%, the bonding strength increases by about 16%, and when the dent level X is 75%, the bonding strength increases by about 37%. It was also found that when the dent level X is less than 25%, there is almost no effect of increasing the bonding strength.

[0073] (Examples 5 to 16) A laminated ceramic capacitor 100B according to a modified example was fabricated by changing the length of exposed portions 25a, 25b by changing the distance between the surface of uncured resin 60a and tape T when the laminated ceramic capacitor 100 shown in Fig. 14(C) was immersed in uncured resin 60a. The length of exposed portions 25a, 25b was set to the distance L from the side surface of the laminated chip 10 to the end of the covering portion 60, as shown in Fig. 17.

[0074] In Examples 5 to 7, the covering portion 60 was formed on the multilayer ceramic capacitor 100 having different recess levels X obtained by setting the design value of the recess level X to 25%, 50%, and 75%, and the length of the exposed portions 25a and 25b was set to 30 μm. In Examples 8 to 10, the covering portion 60 was formed on the multilayer ceramic capacitor 100 having different recess levels X obtained by setting the design value of the recess level X to 25%, 50%, and 75%, and the length of the exposed portions 25a and 25b was set to 50 μm. In Examples 11 to 13, the covering portion 60 was formed on the multilayer ceramic capacitor 100 having different recess levels X obtained by setting the design value of the recess level X to 25%, 50%, and 75%, and the length of the exposed portions 25a and 25b was set to 100 μm. In Examples 14 to 16, the covering portion 60 was formed on the multilayer ceramic capacitors 100 having different recess levels X obtained by setting the design value of the recess level X to 25%, 50%, and 75%, and the length of the exposed portions 25a and 25b was set to 150 μm.

[0075] (Comparative Examples 4 to 7) In Comparative Examples 4 to 7, the covering portion 60 was formed on the multilayer ceramic capacitor 100 in which the recess 24 was not formed, that is, the recess level X was 0%, and the lengths of the exposed portions 25a, 25b were set to 30 μm, 50 μm, 100 μm, and 150 μm, respectively.

[0076] The laminated ceramic capacitor 100B thus fabricated was soldered to the circuit board with the recess 24 facing the circuit board, and the bonding strength between the laminated ceramic capacitor 100B and the circuit board was measured using a push-pull gauge. The laminated ceramic capacitor 100A was 1.0 mm long, 0.5 mm wide, and 0.5 mm high.

[0077] Table 2 and FIG. 18 show the relationship between the recess level X and the bonding strength for each length of the exposed portion. [Table 2]

[0078] 18, it can be seen that the higher the dent level X, the higher the bonding strength tends to be. It can also be seen that when the dent level X is 25% or more, the bonding strength increases.

[0079] When the covering portion 60 is provided to a multilayer ceramic capacitor that does not have the recess 24, if the multilayer ceramic capacitor has a small shape (especially a low-profile product), the manufacturing yield may be reduced depending on the accuracy of the manufacturing device. Specifically, if the multilayer ceramic capacitor is covered with the covering portion 60 more than the target value, and the length of the exposed portions 25a, 25b of the manufactured multilayer ceramic capacitor is shorter (for example, less than 50 μm) than the length of the exposed portions 25a, 25b that can ensure the bonding strength with the circuit board while suppressing the wet-up of the solder (for example, 50 to 150 μm), the bonding strength between the multilayer ceramic capacitor and the circuit board will be equal to or less than the reference value. Therefore, the multilayer ceramic capacitor 100A having the length of the exposed portions 25a, 25b below the lower limit must be treated as a defective product. On the other hand, since the multilayer ceramic capacitor 100A according to the modified example has the recess 24, the bonding strength can be ensured even if the length of the exposed portions 25a, 25b is shorter than the target value. Therefore, the decrease in the yield can be suppressed.

[0080] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]

[0081] 10 Stacked Chip 11 Dielectric layer 12 Internal electrode layer 13 Cover Layer 16 Side margin 20a,20b external electrode 21 Undercoat conductor layer 24 Recess 60 Covering part 100,100A,100B Multilayer Ceramic Capacitors

Claims

1. a laminated chip having a laminated structure in which dielectric layers mainly composed of ceramic and internal electrode layers are alternately laminated, and cover layers provided on upper and lower surfaces in a lamination direction of the laminated structure, the laminated chip having a substantially rectangular parallelepiped shape, the laminated chip being formed so that a plurality of the laminated internal electrode layers are exposed on two end surfaces that face each other alternately; a pair of external electrodes formed from the two end faces to four side faces of the laminated chip; the external electrode has a recess on at least one of two side surfaces between the two side surfaces facing each other in the stacking direction and the other two side surfaces, and has no recess on the other two side surfaces; When the external electrode has the recess on at least one of two side surfaces opposing each other in the stacking direction, a first side margin portion opposing in a direction perpendicular to the stacking direction and the opposing direction in which the two end faces oppose each other and covering the end faces of the dielectric layer, the internal electrode layer, and the cover layer of the stacked structure from the upper surface to the lower surface constitutes the other two side surfaces, the first side margin portion and the cover layer constitute two side surfaces opposing each other in the stacking direction, the first side margin portion and the cover layer have different characteristics, and the recess is formed by the difference in characteristics between the ceramic dielectric layer green sheet which is the material of the first side margin portion and the cover sheet which is the material of the cover layer, When the external electrode has the recess on at least one of the other two side surfaces, the cover layers provided on the upper surface and the lower surface constitute two side surfaces opposing each other in the stacking direction, a second side margin portion extending from each of the other two side surfaces of the stacked structure to the internal electrode layer and the cover layers provided on the upper surface and the lower surface constitute the other two side surfaces, the second side margin portion and the cover layer have different characteristics, and the recess is formed by the difference between the characteristics of the ceramic dielectric layer green sheet which is the material of the second side margin portion and the characteristics of the cover sheet which is the material of the cover layer. A ceramic electronic component comprising:

2. When the external electrode has the recess on at least one of two side surfaces opposing each other in the stacking direction, a density of the first side margin portion is smaller than a density of the cover layer, the density of the first side margin portion is uniform, and the density of the cover layer is uniform, When the external electrode has the recess on at least one of the other two side surfaces, the density of the cover layer is smaller than the density of the second side margin portion, the density of the cover layer is uniform, and the density of the second side margin portion is uniform.

2. The ceramic electronic component according to claim 1.

3. on the periphery of the recess, a distance between the midpoint of a line connecting a vertex where the external electrode is farthest from the side surface of the laminated chip having the recess and a vertex where the external electrode is closest to the side surface of the laminated chip having the recess, and the side surface of the laminated chip where the external electrode has the recess, is t, and a distance between the point where the recess is deepest and the midpoint is d, a recess level X expressed by X=d / t is 25% or more and 75% or less.

3. The ceramic electronic component according to claim 1 or 2.

4. The surface on which the recess is formed is a mounting surface for a circuit board.

4. The ceramic electronic component according to claim 1, wherein the ceramic electronic component is made of a material selected from the group consisting of fluororesin, ...

5. a covering portion that covers five of six surfaces of the ceramic electronic component except for the surface on which the recess is formed; The ceramic electronic component according to any one of claims 1 to 4.

6. a ceramic dielectric layer green sheet and an internal electrode layer forming conductive paste are alternately laminated, the outermost layer is a cover sheet having a uniform density and a density lower than that of the ceramic dielectric layer green sheet, and the laminated plurality of internal electrode layer forming conductive pastes are exposed on two end faces alternately facing each other to form a ceramic laminate having a substantially rectangular parallelepiped shape; A metal paste is applied from the two end faces of the ceramic laminate to four side faces of the ceramic laminate; a recess is formed in the metal paste on at least one of two side surfaces opposing each other in a direction perpendicular to the stacking direction of the ceramic laminate and the opposing direction of the two end faces due to a difference between the density of the ceramic dielectric layer green sheet and the density of the cover sheet, and no recess is formed in the metal paste on the two side surfaces opposing each other in the stacking direction, The metal paste and the ceramic laminate are fired simultaneously. A method for producing a ceramic electronic component comprising the steps of:

7. A laminated structure is formed by alternately laminating ceramic dielectric layer green sheets and conductive paste for forming internal electrode layers, A cover sheet having a uniform density is placed on the upper and lower surfaces of the laminated structure in the lamination direction; by cutting the laminated structure, two end faces at which every other internal electrode layer is exposed and two side faces at which all of the internal electrode layers are exposed are formed; By disposing side margin sheets having a uniform density and a lower density than the density of the cover sheet on two side surfaces on which all of the internal electrode layers are exposed, a ceramic laminate having a substantially rectangular parallelepiped shape is formed in which the laminated conductive pastes for forming the internal electrode layers are exposed on two end surfaces that face each other alternately, A metal paste is applied from the two end faces of the ceramic laminate to four side faces of the ceramic laminate; A recess is formed in the metal paste on at least one of two side surfaces facing each other in the stacking direction due to a difference between the density of the cover sheet and the density of the side margin sheet, and no recess is formed in the metal paste on side surfaces other than the two facing side surfaces among the four side surfaces, The metal paste and the ceramic laminate are fired simultaneously. A method for producing a ceramic electronic component comprising the steps of:

Citation Information

Patent Citations

  • Multilayer ceramic electronic component

    JP2006278557A

  • Multilayer ceramic electronic component

    JP2013012561A

  • Electronic component and manufacturing method therefor

    JP2013026392A

  • Mounting structure of multilayer ceramic capacitor

    JP2014086606A

  • Multilayer ceramic electronic part

    JP2015008313A