Lithographic printing plate precursor, method for preparing a lithographic printing plate, and lithographic printing method

The lithographic printing plate precursor with a high ethylenically unsaturated bond value in its image recording layer addresses plate skipping by enhancing film strength and polymerization, resulting in improved printing durability and reduced skipping.

JP7562527B2Active Publication Date: 2024-10-07FUJIFILM CORP
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2021528301
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-18
Filing Date
2020-06-26
Publication Date
2024-10-07
Estimated Expiration
2040-06-26

AI Technical Summary

Technical Problem

Lithographic printing plates are prone to plate skipping, where the image area is damaged due to local pressure increases from adhered solid matter, leading to incomplete ink application.

Method used

A lithographic printing plate precursor with an image recording layer containing resin particles and a compound having ethylenically unsaturated groups, featuring a high ethylenically unsaturated bond value, which promotes polymerization and enhances film strength to reduce plate skipping.

Benefits of technology

The solution results in a lithographic printing plate with reduced plate skipping and improved printing durability, especially when using ultraviolet curable ink, by ensuring high film strength and effective polymerization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562527000111
    Figure 0007562527000111
  • Figure 0007562527000112
    Figure 0007562527000112
  • Figure 0007562527000113
    Figure 0007562527000113
Patent Text Reader

Abstract

Provided is a lithographic printing plate precursor having an aluminum substrate and an image-recording layer formed on the aluminum substrate. The image-recording layer contains resin particles A having an ethylenic unsaturated group and a compound B that has an ethylenic unsaturated group and that is different from the resin particles A. The ethylenic unsaturated bond amount is 1.5 mmol / g or greater. Also provided are a method for producing a lithographic printing plate using said lithographic printing plate precursor and a lithographic printing method.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a lithographic printing plate precursor, a method for preparing a lithographic printing plate, and a lithographic printing method. [Background technology]

[0002] Generally, a lithographic printing plate consists of an oleophilic image area that accepts ink during the printing process, and a hydrophilic non-image area that accepts dampening water. Lithographic printing utilizes the mutual repulsion properties of water and oil-based ink, making the oleophilic image area of ​​the lithographic printing plate the ink-receptive area and the hydrophilic non-image area the dampening water-receptive area (i.e. the ink non-receptive area) to create a difference in ink adhesion on the surface of the lithographic printing plate, and after ink is applied only to the image area, the ink is transferred to the printing material such as paper to print. To prepare such a lithographic printing plate, a lithographic printing plate precursor (also called a PS plate) having an oleophilic photosensitive resin layer (also called an image recording layer) provided on a hydrophilic support has been widely used. Usually, the lithographic printing plate precursor is exposed to light through an original such as a lithographic film, and then the image areas of the image recording layer are left, while the other unnecessary image recording layer is dissolved and removed with an alkaline developer or an organic solvent, exposing the hydrophilic support surface to form non-image areas, thereby obtaining a lithographic printing plate.

[0003] Furthermore, due to growing concern about the global environment, environmental issues related to waste liquids accompanying wet processing such as development processing have come into focus. In response to the above environmental issues, efforts are being made to simplify development or plate making, eliminate processing, etc. One of the simple manufacturing methods is a method called "on-press development." That is, after exposing a lithographic printing plate precursor to light, it is not subjected to conventional development, but is instead mounted on a printing press as is, and unnecessary portions of the image recording layer are removed at an early stage of the normal printing process.

[0004] As an on-press development type lithographic printing plate precursor, for example, WO 2018 / 159710 discloses a lithographic printing plate precursor having an image recording layer on a support, the image recording layer containing a specific infrared absorber and thermoplastic polymer particles, but not containing a binder polymer.

[0005] As another lithographic printing plate precursor, JP2005-297305A discloses a lithographic printing plate precursor which has, on a support, a photosensitive-thermosensitive layer on which an image can be recorded by exposure to an infrared laser, and which can be printed by mounting the plate on a printing press without undergoing a development processing step after image recording, or by mounting the plate on the printing press and then recording an image thereon, and also discloses a photosensitive-thermosensitive layer which contains microcapsules in which a compound having an ethylenically unsaturated group is encapsulated. Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a lithographic printing plate precursor which can provide a lithographic printing plate which is less susceptible to plate skipping. Another problem to be solved by another embodiment of the present invention is to provide a method for producing a lithographic printing plate or a lithographic printing method in which plate skipping is less likely to occur. Here, "skip" in this disclosure refers to the following phenomenon. That is, it refers to the phenomenon where, when a lithographic printing plate is used for printing with solid matter such as paper fibers or lint from the worker's clothing adhering to the surface of the image area, the pressure on the image area increases locally at the location where the solid matter is adhered, destroying and removing part of the image area, causing ink to be removed in that area. The number of printed sheets until "skip" occurs in the lithographic printing plate is an index showing that "skip is unlikely to occur" [Means for solving the problem]

[0007] Means for solving the above problems include the following aspects. <1> an aluminum support and an image recording layer formed on the aluminum support; The lithographic printing plate precursor, wherein the image recording layer contains resin particles A having an ethylenically unsaturated group and compound B other than the resin particles A and having an ethylenically unsaturated group, and the ethylenically unsaturated bond valence is 1.5 mmol / g or more. <2> the ethylenically unsaturated bond value of the image recording layer is 2.1 mmol / g or more; <1> The lithographic printing plate precursor according to claim 1. <3> The compound B has an ethylenically unsaturated bond equivalent of 300 g / mol or less. <1> or <2> The lithographic printing plate precursor according to claim 1. <4> The molecular weight of the compound B is 2,500 or less. <1> ~ <3> 10. The lithographic printing plate precursor according to claim 9, <5> The compound B includes a compound having an ethylenically unsaturated bond valence of 5.0 mmol / g or more. <1> ~ <4> 10. The lithographic printing plate precursor according to claim 9, <6> The compound having an ethylenically unsaturated bond valence of 5.0 mmol / g or more is a compound represented by the following formula (I): <5> The lithographic printing plate precursor according to claim 1. Formula (I): X-(Y) n In formula (I), X represents an n-valent organic group having a hydrogen-bonding group, Y represents a monovalent group having two or more ethylenically unsaturated groups, n represents an integer of 2 or more, and the molecular weight of X / (molecular weight of Y×n) is 1 or less. <7> The compound having an ethylenically unsaturated bond valence of 5.0 mmol / g or more has at least one structure selected from the group consisting of an adduct structure, a biuret structure, and an isocyanurate structure. <5> or <6> The lithographic printing plate precursor according to claim 1. <8> The compound B includes a compound having one or two ethylenically unsaturated groups. <1> ~ <4> 10. The lithographic printing plate precursor according to claim 9, <9> The content of the compound B is 15% by mass to 80% by mass based on the total mass of the image recording layer. <3> ~ <8> 10. The lithographic printing plate precursor according to claim 9,

[0008] <10> The resin particles A are particles containing a resin having an ethylenically unsaturated group. <1> ~ <9> 10. The lithographic printing plate precursor according to claim 9, <11> The resin having an ethylenically unsaturated group contained in the resin particles A further has a hydrophilic structure. <10> The lithographic printing plate precursor according to claim 1. <12> The hydrophilic structure is a hydrophilic group represented by the following formula Z: <11> The lithographic printing plate precursor according to claim 1. *-QWY formula Z In formula Z, Q represents a divalent linking group, W represents a divalent group having a hydrophilic structure or a divalent group having a hydrophobic structure, Y represents a monovalent group having a hydrophilic structure or a monovalent group having a hydrophobic structure, either W or Y has a hydrophilic structure, and * represents a bonding site with another structure. <13> The hydrophilic structure of the resin having an ethylenically unsaturated group contains a polyalkylene oxide structure. <11> or <12> The lithographic printing plate precursor according to claim 1. <14> The polyalkylene oxide structure includes a polypropylene oxide structure. <13> The lithographic printing plate precursor according to claim 1. <15> The polyalkylene oxide structure includes a polyethylene oxide structure and a polypropylene oxide structure. <13> or <14> The lithographic printing plate precursor according to claim 1. <16> The resin having an ethylenically unsaturated group contained in the resin particles A is an addition polymerization type resin. <10> ~ <15> 10. The lithographic printing plate precursor according to claim 9, <17> The addition polymerization resin contains a structural unit formed from an aromatic vinyl compound. <16> The lithographic printing plate precursor according to claim 1.

[0009] <18> The resin having an ethylenically unsaturated group in the resin particles A includes a structure obtained by reacting at least an isocyanate compound represented by the following formula (Iso) with water: <10> ~ <15> 10. The lithographic printing plate precursor according to claim 9,

[0010] [ka]

[0011] In formula (Iso), n represents an integer of 0 to 10.

[0012] <19> The resin having an ethylenically unsaturated group in the resin particles A contains a structure obtained by at least reacting an isocyanate compound represented by the formula (Iso) with water, and contains a resin having a polyethylene oxide structure and a polypropylene oxide structure as a polyoxyalkylene structure. <18> The lithographic printing plate precursor according to claim 1. <20> The content of the resin particles A is 20% by mass to 60% by mass based on the total mass of the image recording layer. <1> ~ <19> 10. The lithographic printing plate precursor according to claim 9,

[0013] <21> The contact angle with water by a water drop method on the surface of the aluminum support on the side of the image recording layer is 110° or less. <1> ~ <20> 10. The lithographic printing plate precursor according to claim 9, <22> The contact angle of the surface of the aluminum support on the side of the image recording layer with water by a water drop method in the air is 80° or less. <21> The lithographic printing plate precursor according to claim 1. <23> The contact angle with water on the surface of the aluminum support on the side of the image recording layer is 50° or less by a water drop method in the air. <22> The lithographic printing plate precursor according to claim 1. <24> The layer on the aluminum support comprises a hydroxycarboxylic acid or a salt thereof. <1> ~ <23> 10. The lithographic printing plate precursor according to claim 9, <25> The above hydroxycarboxylic acid or its salt includes a compound having two or more hydroxy groups. <24> The lithographic printing plate precursor according to claim 1. <26> The above hydroxycarboxylic acid or its salt includes a compound having three or more hydroxy groups. <24> or <25> The lithographic printing plate precursor according to claim 1.

[0014] <27> The image recording layer further contains a polymerization initiator. <1> ~ <26> 10. The lithographic printing plate precursor according to claim 9, <28> The image recording layer further contains an infrared absorbing agent. <1> ~ <27> 10. The lithographic printing plate precursor according to claim 9, <29> the image recording layer further contains an electron-donating polymerization initiator and an infrared absorbing agent, The value obtained by subtracting the HOMO of the electron-donating polymerization initiator from the HOMO of the infrared absorber is 0.70 eV or less. <1> ~ <26> 10. The lithographic printing plate precursor according to claim 9, <30> The content of the electron-donating polymerization initiator is 0.1% by mass to 10% by mass based on the total mass of the image recording layer. <29> The lithographic printing plate precursor according to claim 1. <31> The infrared absorber has an organic anion having a Hansen solubility parameter Δd of 16 or more, a Δp of 16 to 32, and a Δh of 60% or less of Δp. <28> or <29> The lithographic printing plate precursor according to claim 1. <32> The polymerization initiator contains an electron-accepting polymerization initiator, The electron-accepting polymerization initiator has an organic anion having a Hansen solubility parameter δd of 16 or more, δp of 16 to 32, and δh of 60% or less of δp. <27> The lithographic printing plate precursor according to claim 1.

[0015] <33> The polymerization initiator includes an electron-accepting polymerization initiator, The electron-accepting polymerization initiator contains a compound represented by the following formula (II): <27> The lithographic printing plate precursor according to claim 1.

[0016] [ka]

[0017] In formula (II), X represents a halogen atom; 3 represents an aryl group.

[0018] <34> The image recording layer further contains a color former. <1> ~ <33> 10. The lithographic printing plate precursor according to claim 9, <35> The color former is an acid color former. <34> The lithographic printing plate precursor according to claim 1. <36> The acid color former is a leuco dye. <35> The lithographic printing plate precursor according to claim 1. <37> The leuco dye is a leuco dye having a phthalide structure or a fluoran structure. <36> The lithographic printing plate precursor according to claim 1.

[0019] <38> The leuco dye having a phthalide structure or a fluoran structure is a compound represented by any one of the following formulas (Le-1) to (Le-3): <37> The lithographic printing plate precursor according to claim 1.

[0020] [ka]

[0021] In formulae (Le-1) to (Le-3), each ERG independently represents an electron-donating group, each X1 to X4 independently represents a hydrogen atom, a halogen atom, or a dialkylanilino group, 10 each independently represents a hydrogen atom, a halogen atom, or a monovalent organic group; Y1 and Y2 each independently represent C or N; when Y1 is N, X1 is not present; and when Y2 is N, X4 is not present; Ra1 represents a hydrogen atom, an alkyl group, or an alkoxy group; and Rb1 to Rb4 each independently represent an alkyl group or an aryl group.

[0022] <39> The leuco dye having a phthalide structure or a fluoran structure is a compound represented by any one of the following formulas (Le-4) to (Le-6): <37> or <38> The lithographic printing plate precursor according to claim 1.

[0023] [ka]

[0024] In formulae (Le-4) to (Le-6), ERG each independently represents an electron donating group, X1 to X4 each independently represent a hydrogen atom, a halogen atom, or a dialkylanilino group, Y1 and Y2 each independently represent C or N, and when Y1 is N, X1 does not exist, and when Y2 is N, X4 does not exist, Ra1 represents a hydrogen atom, an alkyl group, or an alkoxy group, and Rb1 to Rb4 each independently represent an alkyl group or an aryl group.

[0025] <40> The leuco dye having a phthalide structure or a fluoran structure is a compound represented by any one of the following formulas (Le-7) to (Le-9): <37> ~ <39> 10. The lithographic printing plate precursor according to claim 9,

[0026] [ka]

[0027] In formulae (Le-7) to (Le-9), X1 to X4 each independently represent a hydrogen atom, a halogen atom, or a dialkylanilino group; Y1 and Y2 each independently represent C or N; when Y1 is N, X1 does not exist; when Y2 is N, X4 does not exist; Ra1 to Ra4 each independently represent a hydrogen atom, an alkyl group, or an alkoxy group; Rb1 to Rb4 each independently represent an alkyl group or an aryl group; and Rc1 and Rc2 each independently represent an aryl group.

[0028] <41> Ra1 to Ra4 are each independently an alkoxy group. <40> The lithographic printing plate precursor according to claim 1. <42> The leuco dye having a phthalide structure or a fluoran structure is a compound represented by the formula (Le-8) <40> The lithographic printing plate precursor according to claim 1. <43> X1 to X4 are hydrogen atoms, and Y1 and Y2 are C. <42> The lithographic printing plate precursor according to claim 1. <44> Rb1 and Rb2 are each independently an alkyl group. <42> or <43> The lithographic printing plate precursor according to claim 1.

[0029] <45> The image recording layer further contains polyvinyl acetal as a binder resin. <1> ~ <44> 10. The lithographic printing plate precursor according to claim 9, <46> The image recording layer further contains a fluoroaliphatic group-containing copolymer. <1> ~ <45> 10. The lithographic printing plate precursor according to claim 9,

[0030] <47> The fluoroaliphatic group-containing copolymer has a structural unit formed from a compound represented by any one of the following formulas (F1) and (F2): <46> The lithographic printing plate precursor according to claim 1.

[0031] [ka]

[0032] In formulas (F1) and (F2), R F1 Each X independently represents a hydrogen atom or a methyl group, and each X independently represents an oxygen atom, a sulfur atom, or -N(R F2 )-, m is an integer of 1 to 6, n is an integer of 1 to 10, l is an integer of 0 to 10, R F2 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.

[0033] <48> The fluoroaliphatic group-containing copolymer further has a structural unit formed of at least one compound selected from the group consisting of poly(oxyalkylene)acrylates and poly(oxyalkylene)methacrylates. <47> The lithographic printing plate precursor according to claim 1.

[0034] <49> The image recording layer is the outermost layer. <1> ~ <48> 10. The lithographic printing plate precursor according to claim 9,

[0035] <50> the aluminum support has an aluminum plate and an anodized aluminum coating disposed on the aluminum plate; the anodized film is located on the image recording layer side of the aluminum plate, the anodized coating has micropores extending in a depth direction from a surface on the image-recording layer side, the average diameter of the micropores on the surface of the anodized film is greater than 10 nm and not greater than 100 nm; The L of the surface of the anodized film on the image recording layer side * a * b * Lightness L in color system *The value is between 70 and 100. <1> ~ <49> 10. The lithographic printing plate precursor according to claim 9, <51> the micropores are composed of large-diameter pores extending from the surface of the anodized coating to a depth of 10 nm to 1,000 nm, and small-diameter pores communicating with the bottoms of the large-diameter pores and extending from the communicating position to a depth of 20 nm to 2,000 nm, the large diameter pores have an average diameter of 15 nm to 100 nm on the surface of the anodized film; The small diameter pores have an average diameter of 13 nm or less at the communicating position. <50> The lithographic printing plate precursor according to claim 1.

[0036] <52> <1> ~ <51> imagewise exposing the lithographic printing plate precursor according to any one of the above items; a step of supplying at least one selected from the group consisting of printing ink and fountain solution to the exposed lithographic printing plate precursor to remove the image recording layer in the non-image area on a printing press; A method for making a lithographic printing plate, comprising: <53> <1> ~ <51> imagewise exposing the lithographic printing plate precursor according to any one of the above items; a step of supplying at least one selected from the group consisting of printing ink and fountain solution to the exposed lithographic printing plate precursor on a printing press to remove the image recording layer in the non-image area, thereby preparing a lithographic printing plate; A step of printing with the prepared lithographic printing plate; A lithographic printing method comprising: Effect of the Invention

[0037] According to an embodiment of the present invention, it is possible to provide a lithographic printing plate precursor which can produce a lithographic printing plate which is less susceptible to plate skipping. According to another embodiment of the present invention, a method for producing a lithographic printing plate or a lithographic printing method in which plate skipping is unlikely to occur can be provided. [Brief description of the drawings]

[0038] [Figure 1] FIG. 2 is a schematic cross-sectional view of one embodiment of an aluminum support. [Diagram 2] FIG. 2 is a schematic cross-sectional view of another embodiment of an aluminum support. [Diagram 3] 1 is a graph showing an example of an alternating current waveform used in electrochemical graining treatment in a method for producing an aluminum support. [Figure 4] FIG. 2 is a side view showing an example of a radial cell in electrochemical graining treatment using an alternating current in a method for producing an aluminum support. [Diagram 5] FIG. 1 is a schematic diagram of an anodizing treatment apparatus used in an anodizing treatment in a method for producing an aluminum support having an anodized coating. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0039] The contents of the present disclosure will be described in detail below. The following description of the components may be based on a representative embodiment of the present disclosure, but the present disclosure is not limited to such an embodiment. In the present disclosure, the use of "to" indicating a numerical range means that the numerical values ​​before and after it are included as the lower limit and upper limit. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples. In addition, in the description of groups (atomic groups) in the present disclosure, descriptions that do not indicate whether they are substituted or unsubstituted include those that have no substituents as well as those that have a substituent. For example, an "alkyl group" includes not only an alkyl group that has no substituents (unsubstituted alkyl groups) but also an alkyl group that has a substituent (substituted alkyl groups). In the present disclosure, "(meth)acrylic" is a term used as a concept that includes both acrylic and methacrylic, and "(meth)acryloyl" is a term used as a concept that includes both acryloyl and methacryloyl. In addition, the term "step" in the present disclosure includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved. In the present disclosure, "mass %" and "weight %" are synonymous, and "parts by mass" and "parts by weight" are synonymous. Unless otherwise specified, each component in a composition or each structural unit in a polymer in the present disclosure may be contained alone or in combination of two or more types. Furthermore, in the present disclosure, the amount of each component in a composition or each structural unit in a polymer means, when a plurality of substances or structural units corresponding to each component or each structural unit in a polymer are present in the composition, the total amount of the corresponding plurality of substances present in the composition or the corresponding plurality of structural units present in the polymer, unless otherwise specified. Furthermore, in the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments.

[0040] In addition, unless otherwise specified, the weight average molecular weight (Mw) and number average molecular weight (Mn) in the present disclosure are molecular weights detected by a gel permeation chromatography (GPC) analyzer using columns of TSKgel GMHxL, TSKgel G4000HxL, or TSKgel G2000HxL (all product names manufactured by Tosoh Corporation) in a solvent of THF (tetrahydrofuran) and a differential refractometer, and converted using polystyrene as a standard substance.

[0041] In addition, unless otherwise specified, the median diameter of the resin particles in this disclosure refers to a value measured by a light scattering method, and the median diameter refers to a diameter at which the number of larger and smaller particles is equal when a powder is divided into two particles of a certain particle diameter. The measurement of the median diameter of the resin particles by the light scattering method is performed using an LA-920 (manufactured by Horiba, Ltd.) according to the manual for the above instrument.

[0042] In this disclosure, the term "lithographic printing plate precursor" includes not only lithographic printing plate precursors but also throwaway plate precursors. Furthermore, the term "lithographic printing plate" includes not only lithographic printing plates prepared by subjecting a lithographic printing plate precursor to operations such as exposure and development as necessary, but also throwaway plates. In the case of a throwaway plate precursor, the operations of exposure and development are not necessarily required. Note that a throwaway plate is a lithographic printing plate precursor that is attached to an unused plate cylinder when, for example, a portion of the page is printed in one color or two colors in color newspaper printing. In addition, in the present disclosure, "*" in a chemical structural formula indicates a bonding position with other structures. The present disclosure will be described in detail below.

[0043] <Lithographic printing plate original plate> The lithographic printing plate precursor according to the present disclosure has an aluminum support and an image recording layer formed on the aluminum support, the image recording layer containing resin particles A having an ethylenically unsaturated group and compound B other than the resin particles A having an ethylenically unsaturated group, and having an ethylenically unsaturated bond valence of 1.5 mmol / g or more. In the present disclosure, resin particles A having an ethylenically unsaturated group are also referred to as "polymerizable resin particles A", and compounds B having an ethylenically unsaturated group other than resin particles A are also referred to as "polymerizable compound B". The lithographic printing plate precursor according to the present disclosure is a negative-working lithographic printing plate precursor. In addition, the lithographic printing plate precursor according to the present disclosure can be suitably used as an on-press development type lithographic printing plate precursor. In the present disclosure, the on-press development type lithographic printing plate precursor refers to a lithographic printing plate precursor that can be developed by an on-press development method described later.

[0044] The present inventors have found that conventional lithographic printing plate precursors, for example, the lithographic printing plate precursors described in the above-mentioned International Publication No. 2018 / 159710 or JP-A-2005-297305, cannot sufficiently suppress the occurrence of plate skipping in the resulting lithographic printing plate. As a result of extensive investigations, the present inventors have found that a lithographic printing plate precursor having the above-mentioned configuration can provide a lithographic printing plate which is less susceptible to plate skipping. Although the detailed mechanism by which the above effects are obtained is unclear, it is speculated as follows. The lithographic printing plate precursor according to the present disclosure has an image recording layer with a high ethylenically unsaturated bond valence (specifically, 1.5 mmol / g or more). The image recording layer with an ethylenically unsaturated bond valence of 1.5 mmol / g or more has a high density of ethylenically unsaturated groups in the layer, and therefore it is considered that the polymerization reaction by the ethylenically unsaturated groups is promoted, and an image part with high film strength is formed. As a result, it is presumed that the lithographic printing plate precursor according to the present disclosure can provide a lithographic printing plate that is less likely to cause plate skipping. For the same reasons as above, it is presumed that the lithographic printing plate precursor according to the present disclosure can provide a lithographic printing plate that is excellent in the number of printable sheets (so-called printing durability). Furthermore, an image recording layer containing polymerizable resin particles A and polymerizable compound B and having a high ethylenically unsaturated bond valence tends to have a low content of polymer compounds such as binder polymers in order to achieve this high ethylenically unsaturated bond valence. As a result, the image recording layer is composed of relatively low molecular weight components, which is presumably why high developability is also obtained.

[0045] 2. Description of the Related Art In recent years, inks that harden when exposed to ultraviolet (UV) rays (hereinafter, also referred to as "ultraviolet-curable inks") have come to be used as printing inks. UV-curable inks have the following advantages: they can be dried instantly, which makes them highly productive; they generally contain a small amount of solvent or are solvent-free, which makes it easy to reduce environmental pollution; and they can form images without drying by heat or after a short period of heat drying, which broadens the range of applications for printing, etc. Therefore, a lithographic printing plate precursor capable of producing a lithographic printing plate which is less susceptible to plate skipping when using ultraviolet-curable ink (hereinafter also referred to as "UV plate skipping") is thought to be extremely useful industrially. Similarly, a lithographic printing plate precursor capable of producing a lithographic printing plate having excellent printing durability when ultraviolet-curable ink is used (hereinafter also referred to as "UV printing durability") would be very useful. As described above, the lithographic printing plate precursor according to the present disclosure has an image recording layer with a high ethylenically unsaturated bond value, and therefore image areas with high film strength are formed. It is therefore presumed that this makes it difficult for UV plate skipping to occur, and furthermore, makes it possible to obtain a lithographic printing plate having excellent UV printing durability.

[0046] [Image Recording Layer] The lithographic printing plate precursor according to the present disclosure has an image recording layer containing polymerizable resin particles A and a polymerizable compound B. The image recording layer in the present disclosure is a negative type image recording layer in which a hardened portion (corresponding to an exposed portion) is formed by a polymerization reaction between polymerizable resin particles A and a polymerizable compound B. From the viewpoint of on-press developability, the image recording layer according to the present disclosure preferably has a non-cured portion (corresponding to an unexposed portion) that is removable with at least one selected from the group consisting of fountain solution and printing ink.

[0047] [Ethylenically unsaturated bond valence] In the present disclosure, the ethylenically unsaturated bond valence in the image recording layer refers to the amount [mmol] of the ethylenically unsaturated group per gram of the image recording layer. The image recording layer in the present disclosure has an ethylenically unsaturated bond valence of 1.5 mmol / g or more, and from the viewpoints of suppressing the occurrence of plate skipping and improving printing durability, it is preferably 1.8 mmol / g or more, more preferably 2.1 mmol / g or more, and particularly preferably 2.5 mmol / g or more. The upper limit of the ethylenically unsaturated bond valence of the image recording layer is not particularly limited, and is preferably, for example, 10.0 mmol / g or less.

[0048] The ethylenically unsaturated bond value in the image recording layer can be determined by the following method. First, a predetermined amount of sample (for example, 200 cm2 in terms of the surface area of ​​the image recording layer) 2), for example, the image recording layer is subjected to solvent extraction, and then the components contained therein are separated using centrifugation, preparative gel permeation chromatography (preparative GPC), and preparative liquid chromatography (preparative HPLC). Next, the structures and compositions of the components contained therein are identified using pyrolysis gas chromatography mass spectrometry (pyrolysis GC / MS), liquid chromatography mass spectrometry (LC-MS), nuclear magnetic resonance spectroscopy (NMR), Fourier transform infrared spectroscopy (FT-IR), etc., and the total amount [mmol] of ethylenically unsaturated groups is calculated. The ethylenically unsaturated bond valence in the image recording layer is calculated by dividing the total amount [mmol] of ethylenically unsaturated groups thus obtained by the mass [g] of the image recording layer used in the measurement. The above operation is carried out at any three points on the image recording layer, and the average is defined as the ethylenically unsaturated bond value of the image recording layer in the present disclosure.

[0049] In addition to the polymerizable resin particles A and the polymerizable compound B, the image recording layer in the present disclosure preferably contains a polymerization initiator, an infrared absorber, etc., from the viewpoints of printing durability and photosensitivity, and may further contain other components.

[0050] Each component contained in the image recording layer will be described in detail below.

[0051] [Polymerizable resin particles A] The polymerizable resin particles A in the present disclosure are preferably particles containing a resin having an ethylenically unsaturated group (hereinafter also referred to as polymerizable resin RA). From the viewpoint of preventing plate skipping, the polymerizable resin particles A preferably contain 80% by mass or more of the polymerizable resin RA, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 100% by mass, based on the total mass of the polymerizable resin particles A. In other words, it is particularly preferable that the polymerizable resin particles A are particles made of the polymerizable resin RA (i.e., particles containing 100% by mass of the polymerizable resin RA based on the total mass of the polymerizable resin particles A). The upper limit of the content of the polymerizable resin RA is not particularly limited, and may be 100% by mass or less.

[0052] (ethylenically unsaturated bond valence) The ethylenically unsaturated bond valence in the polymerizable resin particles A is not particularly limited, but from the viewpoint of suppressing the occurrence of plate skipping, it is preferably 0.01 mmol / g or more, more preferably 0.05 mmol / g or more, and even more preferably 0.09 mmol / g or more. The ethylenically unsaturated bond valence in the polymerizable resin particles A refers to the amount of ethylenically unsaturated groups per gram of the polymerizable resin particles A [mmol]. The upper limit of the ethylenically unsaturated bond valence in the polymerizable resin particles A is, for example, 10.0 mmol / g. The ethylenically unsaturated bond value in the polymerizable resin particles A can be determined by the following method. First, for a given sample amount (e.g., 0.2 g) of polymerizable resin particles A, the structure and composition of the components contained therein are identified using, for example, pyrolysis GC / MS, FT-IR, NMR, time-of-flight secondary ion mass spectrometry (TOF-SIMS), etc., and the total amount [mmol] of ethylenically unsaturated groups is obtained. The total amount [mmol] of ethylenically unsaturated groups thus obtained is divided by the sample amount [g] of polymerizable resin particles A to calculate the ethylenically unsaturated bond valence in polymerizable resin particles A.

[0053] (Polymerizable resin RA) The polymerizable resin RA contained in the polymerizable resin particles A is not particularly limited as long as it is a resin having an ethylenically unsaturated group in the molecule, and may be an addition polymerization type resin, a polycondensation type resin, or a polyaddition type resin. From the viewpoint of suppressing plate skipping, however, it is preferable that it is an addition polymerization type resin. From the viewpoint of ease of production, the addition polymerization type resin as the polymerizable resin RA is preferably a resin obtained by polymerizing an ethylenically unsaturated compound, and more preferably a resin obtained by copolymerizing a polyfunctional ethylenically unsaturated compound and a monofunctional ethylenically unsaturated compound.

[0054] The polymerizable resin RA has at least an ethylenically unsaturated group. From the viewpoint of achieving the ethylenically unsaturated bond valence in the polymerizable resin particles A described above, the polymerizable resin RA is preferably a resin having a structural unit having an ethylenically unsaturated group. The ethylenically unsaturated group contained in the polymerizable resin RA is not particularly limited, and examples thereof include a (meth)acrylic group, an allyl group, a vinylphenyl group, a vinyl ether group, a vinyl ester group, etc. Among these, from the viewpoint of reactivity, the ethylenically unsaturated group is preferably a (meth)acrylic group, more specifically, a (meth)acryloxy group and a (meth)acrylamide group are preferred, and a (meth)acryloxy group is most preferred. The polymerizable resin RA may have only one type of ethylenically unsaturated group, or may have two or more types.

[0055] -Polymerizable resin RA1, which is an addition polymerization type resin- First, the polymerizable resin RA1 (hereinafter, also referred to as "polymerizable resin RA1"), which is an addition polymerization type resin, will be described below. The method for introducing an ethylenically unsaturated group into the polymerizable resin RA1 is not particularly limited, and examples thereof include method (1) in which a polyfunctional monomer having two or more ethylenically unsaturated groups is used during resin synthesis, and the ethylenically unsaturated group remains after resin synthesis, and method (2) in which an ethylenically unsaturated group is introduced by a polymer reaction after resin synthesis. In the present disclosure, the latter method (2) is preferred. In the case of method (2), the resin into which an ethylenically unsaturated group is introduced may be a resin having no ethylenically unsaturated groups, or a resin having fewer ethylenically unsaturated groups than the desired amount. By the above method, a polymerizable resin RA1 having a structural unit having an ethylenically unsaturated group is obtained.

[0056] (Structural Unit Having an Ethylenically Unsaturated Group) The structural unit having an ethylenically unsaturated group in the polymerizable resin RA1 is not particularly limited, and examples thereof include a structural unit represented by the following formula D1.

[0057] [ka]

[0058] In formula D1, L D1 represents a single bond or a divalent linking group; L D2 represents a linking group having a valence of m+1; X D1 -O- or -NR N - represents R N represents a hydrogen atom or an alkyl group, R D1 represents a hydrogen atom or a methyl group, R D represents an ethylenically unsaturated group, and m represents an integer of 1 or more.

[0059] In formula D1, L D1 When represents a divalent linking group, it is preferably an alkylene group, an arylene group, or a divalent group in which two or more of these are bonded, and more preferably an alkylene group having 2 to 10 carbon atoms or a phenylene group. L D1 is preferably a single bond.

[0060] In formula D1, L D2 The m+1-valent linking group represented by the following formula is preferably a linking group containing any of the groups represented by the following formulae D2 to D6, and more preferably a linking group formed by bonding any of the groups represented by the following formulae D2 to D6 to one or more groups selected from the group consisting of an ester bond, an alkylene group, and an alkyleneoxy group.

[0061] [ka]

[0062] In formulas D2 to D6, L D3 ~L D7 represents a divalent linking group, L D5 and L D6 may be the same or different, and X D5 -O- or -NR N - and R N represents a hydrogen atom or an alkyl group, and * represents X in formula D1. D1The wavy line represents the binding site with R in formula D1. D (Preferably, X in formula D7 described below D2 ) binding site.

[0063] In formula D3, L D3 is preferably an alkylene group, an arylene group, or a group in which two or more of these are bonded, and more preferably an alkylene group having 1 to 10 carbon atoms, a phenylene group, or a group in which two or more of these are bonded. In formula D4, L D4 is preferably an alkylene group, an arylene group, or a group in which two or more of these are bonded, and more preferably an alkylene group having 1 to 10 carbon atoms, a phenylene group, or a group in which two or more of these are bonded. In formula D5, L D5 is preferably an alkylene group, an arylene group, or a group in which two or more of these are bonded, and more preferably an alkylene group having 1 to 10 carbon atoms, a phenylene group, or a group in which two or more of these are bonded. In formula D5, X D5 is preferably -O- or -NH-. In formula D5, L D6 is preferably an alkylene group, an arylene group, or a group in which two or more of these are bonded, and more preferably an alkylene group having 1 to 10 carbon atoms, a phenylene group, or a group in which two or more of these are bonded. In formula D6, L D7 is preferably an alkylene group, an arylene group, or a group in which two or more of these are bonded, and more preferably an alkylene group having 1 to 10 carbon atoms, a phenylene group, or a group in which two or more of these are bonded.

[0064] In formula D1, X D1 Ga-NR N - means R N is preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and more preferably a hydrogen atom. Also, X D1 is preferably -O-.

[0065] In formula D1, R D1is preferably a methyl group. In formula D1, m is preferably an integer of 1 to 4, more preferably 1 or 2, and further preferably 1.

[0066] In formula D1, R D The ethylenically unsaturated group represented by the following formula D7 is preferred.

[0067] [ka]

[0068] In formula D7, X D2 -O- or -NR N - represents R N represents a hydrogen atom or an alkyl group. In formula D7, R D2 represents a hydrogen atom or a methyl group. In Formula D7, m has the same meaning as m in Formula D1, and the preferred embodiments are also the same. D2 At least one of these is preferably a methyl group. X in formula D7 D2 X D1 and —O— are preferred.

[0069] The number of atoms between the ethylenically unsaturated group (for example, a (meth)acryloxy group) and the main chain of the addition polymerization resin is preferably 50 to 300, more preferably 69 to 278, and more preferably 135 to 278, from the viewpoint of reactivity.

[0070] Specific examples of the structural unit having an ethylenically unsaturated group are shown below, but the present invention is not limited thereto.

[0071] [ka]

[0072] [ka]

[0073] As described above, a structural unit having an ethylenically unsaturated group (preferably a structural unit represented by formula D1) is preferably introduced into the polymerizable resin RA1 by a method of introducing an ethylenically unsaturated group by a polymer reaction after resin synthesis. A method for introducing an ethylenically unsaturated group by a polymer reaction after resin synthesis will be described below. A structural unit having an ethylenically unsaturated group can be introduced into the polymerizable resin RA1 by, for example, a method of reacting a polymer containing a structural unit having a carboxy group, such as methacrylic acid, with a compound having an epoxy group and an ethylenically unsaturated group (e.g., glycidyl methacrylate, etc.), or a method of reacting a polymer containing a structural unit having a group having active hydrogen, such as a hydroxy group or an amino group, with a compound having an isocyanate group and an ethylenically unsaturated group (e.g., 2-isocyanatoethyl methacrylate, etc.). In addition, by adjusting the reaction rate of the compound having an epoxy group and an ethylenically unsaturated group, or the compound having an isocyanate group and an ethylenically unsaturated group, with the structural unit having a carboxy group or the structural unit having a group having an active hydrogen, the structural unit having a carboxy group or the structural unit having a group having an active hydrogen may be allowed to remain in the polymerizable resin RA1. Hereinafter, the structural units having a carboxy group and the structural units having a group having an active hydrogen are collectively referred to as "structural units before the reaction", and these structural units after the introduction of the ethylenically unsaturated group are also referred to as "structural units after the reaction".

[0074] Since the structural unit before the reaction corresponds to a structural unit having a hydrophilic structure described later, by adjusting the reaction rate, a polymerizable resin RA1 having both a structural unit having an ethylenically unsaturated group and a structural unit having a hydrophilic structure (here, a carboxy group, an amino group, etc.) may be obtained. The reaction rate is, for example, preferably 10% or more and 100% or less, and more preferably 30% or more and 70% or less. The reaction rate is a value defined by the following formula R. Formula R reaction rate = (number of moles of structural units after reaction in the obtained addition polymerization type resin / total number of moles of structural units before reaction in the obtained addition polymerization type resin) × 100

[0075] In addition, a structural unit having an ethylenically unsaturated group may be introduced into the polymerizable resin RA1 by a method of reacting a polymer containing a structural unit having an epoxy group, such as glycidyl (meth)acrylate, with a compound having a carboxy group and an ethylenically unsaturated group.

[0076] Furthermore, a structural unit having an ethylenically unsaturated group may be introduced into the polymerizable resin RA1 by, for example, reacting a polymer containing a structural unit having a partial structure represented by the following formula d1 or d2 with a basic compound. In this method, an ethylenically unsaturated group is formed by an elimination reaction of the partial structure represented by the following formula d1 or d2, and thus the structural unit having an ethylenically unsaturated group is introduced into the polymerizable resin RA1.

[0077] [ka]

[0078] In formula d1 and formula d2, R d represents a hydrogen atom or an alkyl group, A d represents a halogen atom, and X d -O- or -NR N - represents R N represents a hydrogen atom or an alkyl group, and * represents a bonding site with another structure. In formula d1 and formula d2, R d is preferably a hydrogen atom or a methyl group. In formula d1 and formula d2, A d is preferably a chlorine atom, a bromine atom, or an iodine atom. In formula d1 and formula d2, Xd is preferably -O-. d Ga-NR N - means R N is preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and more preferably a hydrogen atom.

[0079] From the viewpoint of preventing plate skipping, the content of the structural unit having an ethylenically unsaturated group in the polymerizable resin RA1 is preferably 10% by mass to 70% by mass, more preferably 20% by mass to 70% by mass, even more preferably 30% by mass to 70% by mass, and particularly preferably 30% by mass to 60% by mass, relative to the total mass of the polymerizable resin RA1 (i.e., addition polymerization type resin).

[0080] (Hydrophilic structure) The polymerizable resin RA1 preferably has a hydrophilic structure in the molecule. In particular, from the viewpoint of facilitating control of the amount of hydrophilic structure introduced, the polymerizable resin RA1 preferably contains a structural unit having a hydrophilic structure. As a hydrophilic structure, the polymerizable resin RA1 preferably has an ionic group or an acid group, and more preferably has an ionic group, from the viewpoints of on-press developability, on-press development residue suppression, and dispersion stability of the polymerizable resin particles A (particularly dispersion stability in water), in addition to suppressing the occurrence of plate skipping. In the present disclosure, the ionic group refers to a group at least a part of which can be dissociated into an anion or a cation in water. In addition, the polymerizable resin RA1 preferably has a sulfonate group (salt of a sulfonic acid group) or a sulfonic acid group as a hydrophilic structure from the viewpoint of dispersion stability of the polymerizable resin particles A in water. On the other hand, the polymerizable resin RA1 preferably has a polyalkylene oxide structure or a polyester structure as a hydrophilic structure, from the viewpoints of suppressing the occurrence of plate skipping, on-press developability, on-press development residue suppression, and dispersion stability of the polymerizable resin particles A (particularly dispersion stability in organic solvents), and more preferably has a polyalkylene oxide structure. Furthermore, it is particularly preferable that the polymerizable resin RA1 has, as a hydrophilic structure, an ionic group or an acid group and a polyalkylene oxide structure from the viewpoints of on-press developability, on-press development residue suppression, and particle dispersion stability, in addition to suppressing the occurrence of plate skipping.

[0081] Specifically, from the viewpoints of on-machine developability, on-machine development residue suppression, and particle dispersion stability (particularly dispersion stability in water), the acid group is preferably a sulfonic acid group, a carboxylic acid group, a phosphoric acid group, or a sulfate monoester group, more preferably a sulfonic acid group or a carboxylic acid group, and particularly preferably a carboxylic acid group.

[0082] Specifically, from the viewpoints of on-press developability, on-press development residue suppression, and particle dispersion stability (particularly dispersion stability in water), the ionic group is preferably a group that dissociates a counter ion to generate an anion (i.e., an anionic group), more preferably a salt of an acid group, specifically, a sulfonate group, a carboxylate group, or a sulfate monoester group is further preferable, and a carboxylate group is particularly preferable. Here, the counter cation in the salt of the acid group may be an inorganic cation or an organic cation, but is preferably an inorganic cation. The counter cation may be not only a monovalent cation but also a polyvalent cation, but is preferably a monovalent cation. As the inorganic cation, an alkali metal ion or an alkaline earth metal ion is more preferable, an alkali metal ion is more preferable, and specifically, a lithium ion, a sodium ion, or a potassium ion is particularly preferable. Examples of the organic cation include a quaternary ammonium cation and a cation obtained by alkylating the nitrogen atom of an aromatic nitrogen-containing heterocycle. Examples of the quaternary ammonium cation include the tetramethylammonium cation, the tetraethylammonium cation, and the dimethylbenzylammonium cation. An example of a cation obtained by alkylating a nitrogen atom of an aromatic nitrogen-containing heterocycle is a pyridinium cation. Among these, the counter cation in the salt of the acid group is preferably an alkali metal ion or a quaternary ammonium cation, and more preferably an alkali metal ion.

[0083] Specifically, the polyalkylene oxide structure is preferably a polyethylene oxide structure, a polypropylene oxide structure, or a poly(ethylene oxide / propylene oxide) structure from the viewpoint of the dispersion stability of the polymerizable resin particles A, particularly in an organic solvent. From the viewpoints of on-press developability and suppression of development residue during on-press development, the polyalkylene oxide structure preferably contains a polypropylene oxide structure, and more preferably contains a polyethylene oxide structure and a polypropylene oxide structure. The number of alkylene oxide structures in the polyalkylene oxide structure is preferably 2 or more, more preferably 5 or more, further preferably 5 to 200, and particularly preferably 8 to 150, from the viewpoint of dispersion stability of the polymerizable resin particles A, in particular, dispersion stability in an organic solvent.

[0084] The polyester structure is not particularly limited, but preferred examples include a ring-opening polymerization chain of lactone and a polycondensation chain of hydroxycarboxylic acid. The number of hydroxycarboxylic acid structures (or lactone ring-opening structures) in the polyester structure is preferably 2 or more, more preferably 2 to 20, even more preferably 2 to 10, and particularly preferably 4 to 10, from the viewpoint of dispersion stability of the particles, particularly dispersion stability in an organic solvent.

[0085] The polymerizable resin RA1 preferably has a constituent unit represented by the following formula A-1 as a constituent unit having an ionic group or an acid group, which is a hydrophilic structure.

[0086] [ka]

[0087] In formula A-1, X1 -O- or -NR 3 - represents L 1 represents a divalent linking group having 1 to 20 carbon atoms, R 1 represents an ionic group or an acid group, R 2 represents a hydrogen atom or a methyl group, R 3 represents a hydrogen atom, an alkyl group, or an aryl group.

[0088] In formula A-1, R 1 The ionic group or acid group represented by the formula (I) is the same as the ionic group or acid group in the hydrophilic structure described above, and preferred examples are also the same. In formula A-1, X 1 is preferably -O-. In formula A-1, L 1 is preferably a divalent linking group having 2 to 10 carbon atoms, more preferably a divalent linking group having 2 to 8 carbon atoms, further preferably an alkylene group having 2 to 8 carbon atoms, and particularly preferably an alkylene group having 2 to 5 carbon atoms. Specifically, the divalent linking group is preferably an alkylene group or a group in which one or more alkylene groups are linked to one or more structures of at least one type selected from the group consisting of an ether bond and an ester bond, and more preferably an alkylene group. In formula A-1, R 3 is preferably a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a phenyl group, and more preferably a hydrogen atom.

[0089] The addition polymerization resin preferably has a structural unit represented by the following formula A-3 or A-4 as a structural unit having a hydrophilic polyalkylene oxide structure or polyester structure, and more preferably has a structural unit represented by the following formula A-3.

[0090] [ka]

[0091] In formula A-3 and formula A-4, L 2represents an ethylene group or a propylene group, L 3 represents an alkylene group having 2 to 10 carbon atoms; L 4 represents an alkylene group having 1 to 10 carbon atoms, R 4 and R 6 each independently represents a hydrogen atom, an alkyl group, or an aryl group; R 5 and R 7 each independently represents a hydrogen atom or a methyl group, m1 represents an integer of 2 to 200, and m2 represents an integer of 2 to 20.

[0092] In formula A-3, L 2 is preferably an ethylene group or a 1,2-propylene group. In formula A-4, L 3 is preferably an alkylene group having 2 to 8 carbon atoms, more preferably an alkylene group having 2 to 4 carbon atoms, and further preferably an ethylene group. In formula A-4, L 4 is preferably an alkylene group having 2 to 8 carbon atoms, more preferably an alkylene group having 3 to 8 carbon atoms, and further preferably an alkylene group having 4 to 6 carbon atoms. In formula A-3 and formula A-4, R 4 and R 6 are each independently preferably a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a phenyl group, more preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and more preferably a hydrogen atom or a methyl group. In formula A-3, m1 is preferably an integer of 5-200, and more preferably an integer of 8-150. In formula A-4, m2 is preferably an integer of 2-10, and more preferably an integer of 4-10.

[0093] From the viewpoints of on-machine developability, on-machine development residue suppression, and particle dispersion stability, it is particularly preferable that the polymerizable resin RA1 has a constitutional unit represented by the above formula A-1 and a constitutional unit represented by the above formula A-3 or formula A-4, and it is most preferable that the polymerizable resin RA1 has a constitutional unit represented by the above formula A-1 and a constitutional unit represented by the above formula A-3.

[0094] From the viewpoints of on-press developability, on-press development residue suppression, and dispersion stability of the polymerizable resin particles A, the polymerizable resin RA1 preferably has a group represented by the following formula Z as a hydrophilic structure. *-QWY formula Z In formula Z, Q represents a divalent linking group, W represents a divalent group having a hydrophilic structure or a divalent group having a hydrophobic structure, Y represents a monovalent group having a hydrophilic structure or a monovalent group having a hydrophobic structure, either W or Y has a hydrophilic structure, and * represents a bonding site with another structure.

[0095] In formula Z, Q is preferably a divalent linking group having 1 to 20 carbon atoms, and more preferably a divalent linking group having 1 to 10 carbon atoms. The divalent linking group represented by Q is preferably an alkylene group, an arylene group, an ester bond, an amide bond, or a group consisting of a combination of two or more of these, and more preferably a phenylene group, an ester bond, or an amide bond.

[0096] In formula Z, the divalent group having a hydrophilic structure represented by W is a polyalkyleneoxy group or a polyalkyleneoxy group having -CH2CH2NR at one end. W Preferably, R is a group having - bonded thereto. W represents a hydrogen atom or an alkyl group. In formula Z, the divalent group having a hydrophobic structure represented by W is -R WA -, -OR WA -O-, -R W NR WA -NR W -, -OC(=O)-R WA -O- or -OC(=O)-R WA Preferably, R is —O—. WA R each independently represents a linear, branched or cyclic alkylene group having 6 to 120 carbon atoms, a haloalkylene group having 6 to 120 carbon atoms, an arylene group having 6 to 120 carbon atoms, or an aralkylene group having 6 to 120 carbon atoms. W is the above R W is synonymous with.

[0097] In formula Z, the monovalent group having a hydrophilic structure represented by Y is -OH, -C(=O)OH, a polyalkyleneoxy group having a hydrogen atom or an alkyl group at the end, or a polyalkyleneoxy group having a hydrogen atom or an alkyl group at the other end and -CH2CH2N(R W )- is preferably a group bonded to R W is the above R W is synonymous with. The monovalent group having a hydrophobic structure represented by Y is a linear, branched or cyclic alkyl group having 6 to 120 carbon atoms, a haloalkyl group having 6 to 120 carbon atoms, an aryl group having 6 to 120 carbon atoms, an alkylaryl group having 6 to 120 carbon atoms, an aralkyl group having 6 to 120 carbon atoms, -OR WB , -C(=O)OR WB , or -OC(=O)R WB It is preferable that R WB represents an alkyl group having 6 to 20 carbon atoms.

[0098] From the viewpoints of on-machine developability, on-machine development residue suppression, and dispersion stability of the polymerizable resin particles A, the content of the structural unit having a hydrophilic structure in the polymerizable resin RA1 is preferably 1 mass % to 30 mass %, more preferably 3 mass % to 20 mass %, even more preferably 5 mass % to 15 mass %, and particularly preferably 5 mass % to 10 mass %, relative to the total mass of the polymerizable resin RA1 (i.e., addition polymerization type resin). Furthermore, when the hydrophilic structure is an ionic group, the content of the structural unit having an ionic group in the polymerizable resin RA1 is, from the viewpoints of on-machine developability, on-machine development residue suppression, and dispersion stability of the polymerizable resin particles A, preferably 1 mass % to 30 mass %, more preferably 1 mass % to 20 mass %, even more preferably 3 mass % to 15 mass %, and particularly preferably 3 mass % to 10 mass %, relative to the total mass of the polymerizable resin RA1 (i.e., addition polymerization type resin).

[0099] (Crosslinked structure) The polymerizable resin RA1 may have a crosslinked structure in the molecule. The crosslinked structure is not particularly limited, but is preferably introduced into the polymerizable resin RA1 as a structural unit obtained by polymerizing a polyfunctional ethylenically unsaturated compound, or as a structural unit in which one or more reactive groups form a covalent bond within the resin. The functionality of the polyfunctional ethylenically unsaturated compound is preferably 2 to 15, more preferably 3 to 10, even more preferably 4 to 10, and particularly preferably 5 to 10, from the viewpoint of suppressing the occurrence of plate skipping. In other words, from the viewpoint of suppressing the occurrence of plate skipping, the structural unit having a crosslinked structure is preferably a bifunctional to 15 functional branch unit, more preferably a trifunctional to 10 functional branch unit, even more preferably a tetrafunctional to 10 functional branch unit, and particularly preferably a pentafunctional to 10 functional branch unit. The n-functional branch unit refers to a branch unit having n molecular chains, in other words, a structural unit having an n-functional branch point (that is, a crosslinked structure).

[0100] The ethylenically unsaturated group in the polyfunctional ethylenically unsaturated compound is not particularly limited, but examples thereof include a (meth)acryloxy group, a (meth)acrylamide group, an aromatic vinyl group, and a maleimide group. The polyfunctional ethylenically unsaturated compound is preferably a polyfunctional (meth)acrylate compound, a polyfunctional (meth)acrylamide compound, or a polyfunctional aromatic vinyl compound.

[0101] Examples of the polyfunctional (meth)acrylate compound include diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, trimethylolpropane diacrylate, trimethylolpropane triacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, polyethylene glycol diacrylate, polypropylene glycol diacrylate, tricyclodecane dimethylol diacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol triacrylate, dipentaerythritol hexaacrylate, and tris(β-hydroxyethyl)isocyanurate triacrylate. Examples of the polyfunctional (meth)acrylamide compound include N,N'-methylenebisacrylamide, N-[tris(3-acrylamidopropoxymethyl)methyl]acrylamide, and the like. An example of the polyfunctional aromatic vinyl compound is divinylbenzene.

[0102] The number of carbon atoms in the structural unit having a crosslinked structure is not particularly limited, but is preferably 8-100, and more preferably 8-70.

[0103] From the viewpoints of UV printing durability and suppression of plate skipping, the structural unit having a crosslinked structure is preferably at least one structural unit selected from the group consisting of structural units represented by BR-1 to BR-17 below.Moreover, the structural unit having a crosslinked structure more preferably contains at least one structural unit selected from the group consisting of structural units represented by BR-1 to BR-10 or BR-13 to BR-17 below, further preferably at least one structural unit selected from the group consisting of structural units represented by BR-1 to BR-7 or BR-13 to BR-17 below, and particularly preferably the structural unit represented by BR-1 below.

[0104] [ka]

[0105] [ka]

[0106] [ka]

[0107] [ka]

[0108] Among the structural units represented by BR-1 to BR-17 above, R BR each independently represents a hydrogen atom or a methyl group, and n represents an integer of 1 to 20.

[0109] From the viewpoint of preventing plate skipping, the content of the structural unit having a crosslinked structure in the polymerizable resin RA1 is preferably 1% by mass to 50% by mass, more preferably 3% by mass to 30% by mass, even more preferably 5% by mass to 20% by mass, and particularly preferably 5% by mass to 15% by mass, relative to the total mass of the polymerizable resin RA1 (i.e., addition polymerization type resin).

[0110] -Other building blocks- The polymerizable resin RA1 may have a structural unit (other structural unit) other than the structural unit having an ethylenically unsaturated bond, the structural unit having a hydrophilic structure, and the structural unit having a crosslinked structure, which are described above. Preferred examples of compounds (i.e., monomers) that form other structural units include monofunctional ethylenically unsaturated compounds such as aromatic vinyl compounds, (meth)acrylate compounds, (meth)acrylonitrile compounds, (meth)acrylamide compounds, N-vinyl heterocyclic compounds, vinyl halide compounds, vinyl ester compounds, vinyl ether compounds, and α-olefin compounds. More preferred examples of compounds (i.e., monomers) that form other structural units include styrene, methyl methacrylate, acrylonitrile, methacrylonitrile, N,N-dimethylacrylamide, 2-hydroxyethyl acrylate, 2,3-dihydroxypropyl methacrylate, 2-ethylhexyl methacrylate, acryloylmorpholine, diacetone acrylamide, N-isopropylacrylamide, cyclohexyl methacrylate, acryloxymethyl ethylene carbonate, pt-butylstyrene, methacrylamide, and N-vinylpyrrolidone. Among them, the polymerizable resin RA1 more preferably has at least one type of structural unit selected from the group consisting of structural units derived from aromatic vinyl compounds such as styrene, structural units derived from acrylonitrile compounds such as acrylonitrile, structural units derived from N-vinyl heterocyclic compounds such as N-vinylpyrrolidone, and (meth)acrylate compounds such as 2-hydroxyethyl acrylate, and particularly preferably has a structural unit derived from an aromatic vinyl compound. Among them, the polymerizable resin RA1 particularly preferably has a structural unit derived from acrylonitrile and a structural unit derived from styrene.

[0111] A preferred example of a structural unit formed from an aromatic vinyl compound is a structural unit represented by the following formula A1.

[0112] [ka]

[0113] In formula A1, R A1 and R A2 each independently represents a hydrogen atom or an alkyl group, Ar represents an aromatic ring group, R A3 represents a substituent, and n represents an integer equal to or less than the maximum number of substituents on Ar. In formula A1, R A1 and R A2are each independently preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, more preferably a hydrogen atom or a methyl group, and further preferably all are a hydrogen atom. In formula A1, Ar is preferably a benzene ring or a naphthalene ring, and more preferably a benzene ring. In formula A1, R A3 is preferably an alkyl group or an alkoxy group, more preferably an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms, and further preferably a methyl group or a methoxy group. In formula A1, R A3 If there are multiple R A3 may be the same or different from each other. In formula A1, n is preferably an integer of 0 to 2, more preferably 0 or 1, and even more preferably 0.

[0114] The aromatic vinyl compound for obtaining the above structural unit may be any compound having a structure in which a vinyl group is bonded to an aromatic ring, and examples thereof include styrene compounds and vinylnaphthalene compounds, with styrene compounds being preferred and styrene being more preferred. Examples of the styrene compound include styrene, p-methylstyrene, p-methoxystyrene, β-methylstyrene, p-methyl-β-methylstyrene, α-methylstyrene, and p-methoxy-β-methylstyrene, with styrene being preferred. Examples of the vinylnaphthalene compound include 1-vinylnaphthalene, methyl-1-vinylnaphthalene, β-methyl-1-vinylnaphthalene, 4-methyl-1-vinylnaphthalene, 4-methoxy-1-vinylnaphthalene, and the like, with 1-vinylnaphthalene being preferred.

[0115] Moreover, as a structural unit formed from an acrylonitrile compound, a structural unit represented by the following formula B1 can be preferably mentioned.

[0116] [ka]

[0117] In formula B1, R B1 represents a hydrogen atom or an alkyl group. In formula B1, R B1 is preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, more preferably a hydrogen atom or a methyl group, and even more preferably a hydrogen atom.

[0118] Examples of the acrylonitrile compound from which the above structural unit is obtained include (meth)acrylonitrile, with acrylonitrile being preferred.

[0119] A preferred example of a structural unit formed by an N-vinyl heterocyclic compound is a structural unit represented by the following formula C1.

[0120] [ka]

[0121] In formula C1, Ar N represents a heterocyclic structure containing a nitrogen atom, and Ar N The nitrogen atom in the compound bonds to the carbon atom indicated with an *. In formula C1, Ar N The heterocyclic structure represented by the formula (I) is preferably a pyrrolidone ring, a carbazole ring, a pyrrole ring, a phenothiazine ring, a succinimide ring, a phthalimide ring, a caprolactam ring, or an imidazole ring, and more preferably a pyrrolidone ring. Also, Ar N The heterocyclic structure represented by the formula: may have a known substituent.

[0122] Examples of N-vinyl heterocyclic compounds for obtaining the above structural unit include N-vinylpyrrolidone, N-vinylcarbazole, N-vinylpyrrole, N-vinylphenothiazine, N-vinylsuccinimide, N-vinylphthalimide, N-vinylcaprolactam, and N-vinylimidazole, with N-vinylpyrrolidone being preferred.

[0123] The polymerizable resin RA1 may have one type of other structural unit alone, two or more types of other structural units, or no other structural units. From the viewpoints of suppressing plate skipping, sensitivity, on-press developability, etc., the content of other structural units in the polymerizable resin RA1 is preferably 0% by mass to 90% by mass, more preferably 10% by mass to 70% by mass, even more preferably 20% by mass to 60% by mass, and particularly preferably 30% by mass to 60% by mass, relative to the total mass of the polymerizable resin RA1 (i.e., addition polymerization type resin).

[0124] (Synthesis of polymerizable resin particles A containing polymerizable resin RA1) The method for synthesizing the polymerizable resin particles A containing the polymerizable resin RA1 is not particularly limited as long as it is a method for synthesizing particles that contain the polymerizable resin RA1 and can achieve the above-mentioned ethylenically unsaturated bond valence, and for example, known methods for synthesizing resin particles such as emulsion polymerization, suspension polymerization, dispersion polymerization, soap-free polymerization, and microemulsion polymerization can be used. In the present disclosure, from the viewpoint of suitability for synthesis with various monomers, and from the viewpoint of controlling the dispersibility (particularly dispersibility in water) and particle size of the polymerizable resin particles A described below, it is preferable to use an emulsion polymerization method as a synthesis method for the polymerizable resin particles A containing the polymerizable resin RA1.

[0125] Methods for synthesizing polymerizable resin particles A containing polymerizable resin RA1 include, for example, method (1') in which a polyfunctional monomer having two or more ethylenically unsaturated groups is used during particle synthesis to leave the ethylenically unsaturated groups after particle synthesis, and method (2') in which an ethylenically unsaturated group is introduced by a polymer reaction after particle synthesis, and in this disclosure, the latter method (2') is preferred. In the case of method (2'), polymerizable resin particles A having a large number of active ethylenically unsaturated groups on the surface are synthesized, and it is considered that the reactivity of these polymerizable resin particles A with the polymerizable compound B described later and the like increases, making it easier to form strong crosslinked parts. In the case of method (2'), the particles into which ethylenically unsaturated groups are introduced may be particles containing a resin that does not have an ethylenically unsaturated group, or may be particles containing a resin in which the amount of ethylenically unsaturated groups is less than the desired amount.

[0126] In addition, in the case of the above method (2'), if a site where an ethylenically unsaturated group is to be introduced (e.g., the aforementioned carboxy group, a group having active hydrogen, etc.) is present closer to the surface of the particle, more ethylenically unsaturated groups can be introduced onto the surface of the polymerizable resin particle A. As a method for synthesizing such polymerizable resin particles A, for example, a method in which the ratio of monomers used in the synthesis is changed and polymerized so that the aforementioned constituent units having a carboxy group such as methacrylic acid or the constituent units having a group having active hydrogen (the aforementioned constituent units before the reaction) are more present near the surface of the particles, i.e., a seed polymerization method, may be applied.

[0127] Specific examples of the polymerizable resin RA1 include those shown below, but the polymerizable resin RA1 is not limited to these. In the following specific examples, n represents an integer of 2 to 200.

[0128] [ka]

[0129] -Other polymerizable resins RA2- The polymerizable resin RA in the present invention is not limited to an addition polymerization type resin, but may be a polycondensation type resin or a polyaddition type resin. Here, the polycondensation type resin refers to a resin obtained by a polycondensation reaction, and the polyaddition type resin refers to a resin obtained by a polyaddition reaction. Examples of the polycondensation type resin include polyamide and polyester. Examples of the polyaddition type resin include polyurethane, polyurea, polyurethane urea, polycarbonate, etc. More specifically, the polymerizable resin RA2 (hereinafter also referred to as polymerizable resin RA2) other than the polymerizable resin RA1 which is an addition polymerization type resin may be a resin having at least one type of bond selected from the group consisting of a urea bond, a urethane bond, an amide bond, a carbonate bond, an ester bond, and an imide bond in the main chain and having an ethylenically unsaturated group, and the like. A resin having at least one type of bond selected from the group consisting of a urea bond, a urethane bond, an amide bond, and an ester bond in the main chain and having an ethylenically unsaturated group is preferred, and a resin having at least one type of bond selected from the group consisting of a urea bond and a urethane bond in the main chain and having an ethylenically unsaturated group is even more preferred. More specifically, the polymerizable resin RA2 is preferably a polyurea, polyurethane, polyurethane urea, polyamide, or polyester having an ethylenically unsaturated group, and more preferably a polyurea or polyurethane having an ethylenically unsaturated group.

[0130] The polymerizable resin RA2 may be in the form of a microgel (crosslinkable resin particle). The microgel may or may not have an ethylenically unsaturated group. The polymerizable resin particle A made of a microgel is preferably a microgel containing a compound (e.g., a monomer) having an ethylenically unsaturated group. However, even if exposed to light, the compound (e.g., monomer) having an encapsulated ethylenically unsaturated group remains unreacted in the microgel, or a crosslinking reaction only occurs inside the microgel. Therefore, the compound (e.g., monomer) having an encapsulated ethylenically unsaturated group encapsulated in the microgel is unlikely to react with the polymerizable compound B, and is unlikely to contribute to the curing of the exposed area.

[0131] Specifically, the microgel is preferably one obtained by reacting a polyisocyanate compound, which is an adduct of a polyphenol compound having two or more hydroxy groups in the molecule with isophorone diisocyanate, with a compound having active hydrogen. The polyhydric phenol compound is preferably a compound having a plurality of benzene rings each having a phenolic hydroxy group. The compound having the above-mentioned active hydrogen is preferably a polyol compound or a polyamine compound, more preferably a polyol compound, and even more preferably at least one compound selected from the group consisting of propylene glycol, glycerin, and trimethylolpropane. Preferred examples of resin particles obtained by reacting a polyisocyanate compound, which is an adduct of a polyphenol compound having two or more hydroxy groups in the molecule and isophorone diisocyanate, with a compound having active hydrogen include the polymer particles described in paragraphs 0032 to 0095 of JP2012-206495A.

[0132] The polymerizable resin RA2 preferably has a hydrophilic structure, and the hydrophilic structure is the same as the hydrophilic structure possessed by the polymerizable resin RA1, and the preferred embodiment is also the same.

[0133] As the polymerizable resin RA2 in the present disclosure, a resin containing a urea bond is preferable, particularly from the viewpoints of printing durability, ink adhesion, special color ink adhesion, UV plate skip suppression, on-press developability, and development residue suppression during on-press development. More specifically, the polymerizable resin RA2 is a resin containing a urea bond, and more preferably contains a structure obtained by at least reacting an isocyanate compound represented by the following formula (Iso) with water, and particularly preferably contains a resin that contains a structure obtained by at least reacting an isocyanate compound represented by the following formula (Iso) with water and has a polyethylene oxide structure and a polypropylene oxide structure as a polyoxyalkylene structure. In addition, in the polymerizable resin RA2, the particles containing the resin containing the urea bond are preferably microgels (that is, crosslinked resin particles).

[0134] [ka]

[0135] In formula (Iso), n represents an integer of 0 to 10.

[0136] An example of the reaction between the isocyanate compound represented by the above formula (Iso) and water is the reaction shown below. Note that the following example is an example in which n=0 and the 4,4-isomer is used. As shown below, when the isocyanate compound represented by the above formula (Iso) is reacted with water, a part of the isocyanate group is hydrolyzed by the water to generate an amino group, and the generated amino group reacts with the isocyanate group to generate a urea bond, forming a dimer. The following reaction is repeated to form a resin having a urea bond.

[0137] [ka]

[0138] The resin containing a urea bond, which is one of the specific resins a2, has an ethylenically unsaturated group. The ethylenically unsaturated group preferably has a group represented by the following formula (PETA).

[0139] [ka]

[0140] In formula (PETA), the wavy line portion represents the bonding position to other structures.

[0141] In addition, in the reaction of the isocyanate compound represented by the above formula (Iso) with water, by adding a compound reactive with an isocyanate group, such as an alcohol compound or an amine compound (e.g., a compound having active hydrogen), the structure of the alcohol compound, amine compound, etc. can be introduced into the polymerizable resin RA2. Examples of the compound having active hydrogen include the above-mentioned compounds having active hydrogen used in the microgel, and preferred embodiments are also the same.

[0142] (Other Ingredients) Components other than the polymerizable resin RA contained in the polymerizable resin particles A (hereinafter also referred to as other components) include, for example, compounds having an ethylenically unsaturated group (e.g., monomers), polymerization initiator residues, low molecular weight surfactants, etc. The content of other components is preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, and particularly preferably 0% by mass, based on the total mass of the polymerizable resin particles A. In other words, it is particularly preferable that the polymerizable resin particles A are particles made of the polymerizable resin RA without containing other components.

[0143] Specific examples of the polymerizable resin particles A containing the polymerizable resin RA1 include particles R-2 to R-6 synthesized in the examples, but the polymerizable resin particles A are not limited to these. Specific examples of the polymerizable resin particles A containing the polymerizable resin RA2 include particles R-1 and R-7 to 11 synthesized in the examples, but the polymerizable resin particles A are not limited to these.

[0144] -Particle characteristics- <<Dispersibility>> From the viewpoint of developability and on-machine developability, the polymerizable resin particles A preferably have water dispersibility. In the present disclosure, "water-dispersible particles" refers to particles in which, when 5.0 g of particles are mixed in 100 mL of water in an environment at 20°C, dispersed by stirring at a stirring speed of 300 rpm (revolutions per minute, the same applies below) for 10 minutes in a 20°C environment, and then allowed to stand for 1 hour in an environment at 20°C, no precipitate is visually observed or a small amount of precipitate is visually observed but the precipitate is easily redispersible. It is preferable that after the polymerizable resin particles A are allowed to stand for one hour, no precipitate is visually observed or a small amount of precipitate is visually observed but the polymerizable resin particles A are in a state that is easily redispersible, and it is more preferable that no precipitate is visually observed and the polymerizable resin particles A are in a state that is favorable in dispersibility.

[0145] In addition, from the viewpoints of printing durability, developability, and developing property, the polymerizable resin particles A preferably have dispersibility in an organic solvent. In the present disclosure, "dispersible in organic solvent" refers to dispersion in at least one organic solvent selected from MEK / MFG / methanol=48 / 30 / 22 (mass ratio, SP value=11.1), 1-propanol / water=1 / 1 (mass ratio, SP value=17.7), and a single alcoholic organic solvent (methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, MFG, etc.). These organic solvents may be used as coating solvents described below to form an image recording layer in the lithographic printing plate precursor according to the present disclosure. In this disclosure, MEK stands for methyl ethyl ketone and MFG stands for 1-methoxy-2-propanol. In the present disclosure, "particles dispersible in an organic solvent" refers to particles that, when 5.0 g of particles are mixed in 100 mL of at least one of the above organic solvents in an environment at 20°C, dispersed by stirring at a stirring speed of 300 rpm for 10 minutes, and allowed to stand for 1 hour in an environment at 20°C, a small amount of precipitate is visually confirmed, but the particles are easily redispersible. After leaving the polymerizable resin particles A for one hour, a small amount of precipitate is visually confirmed, but it is preferable that the particles are in a state that can be easily redispersed, and it is more preferable that no precipitate is visually confirmed and the particles have good dispersibility. If the polymerizable resin particles A in the present disclosure are particles having organic solvent dispersibility, the particles can be well dispersed in the coating liquid when forming the image recording layer. When the image recording layer is formed using such a coating liquid, the polymerizable resin particles A are unlikely to be coated in an aggregated state, so that the image recording layer is likely to have excellent coating surface condition, printing durability, developability, and on-machine developability.

[0146] The SP value of the organic solvent preferred as the coating solvent is from 9.3 to 18.0, more preferably from 10.0 to 15.0, and further preferably from 10.5 to 12.5. The polymerizable resin particles A in the present disclosure are preferably dispersible in an organic solvent having the above SP value. The SP values ​​of representative organic solvents are as follows: MEK (SP value = 9.3), MFG (SP value = 11.2), methanol (SP value = 14.7), ethanol (SP value = 12.4), 1-propanol (SP value = 11.9), 2-propanol (SP value = 11.2), 1-butanol (SP value = 11.4), water (SP value = 23.4) The SP value in this disclosure is calculated by the Okitsu method (Okitsu Toshinao, Journal of the Adhesion Society of Japan, 29(5)(1993)). Specifically, the SP value is calculated by the following formula: where ΔF is a value given in the literature. SP value (δ) = ΣΔF (Molar Attraction Constants) / V (Molar Volume) In addition, the unit of SP value in this disclosure is MPa. 1 / 2 It is. When a mixture of a plurality of organic solvents is used as the organic solvent, the SP value is calculated as a weighted average value according to the mass ratio of each organic solvent contained. Specifically, the weighted average value is "X" calculated by the following formula 1. Specifically, the SP value of organic solvent A containing two or more organic solvents is X, which is calculated by substituting the SP value of the i-th organic solvent (i is an integer of 1 or more) contained in Si and the mass content of the i-th organic solvent in the entire organic solvent A in Formula 1 below.

[0147]

number

[0148] <<Median diameter>> From the viewpoint of suppressing the occurrence of plate skipping, the particle diameter of the specific particles is preferably 1,000 nm or less, and more preferably 50 nm to 300 nm, in terms of median diameter. The method for measuring the median diameter is as described above.

[0149] <<Coefficient of variation>> The coefficient of variation of the particle size of the polymerizable resin particles A is preferably 100% or less, more preferably 40% or less, and even more preferably 25% or less. The lower limit of the coefficient of variation is not particularly limited, and may be 0%. The above-mentioned coefficient of variation can be reduced by appropriately setting reaction conditions such as stirring speed and temperature during particle synthesis, or, in the case of polymerizable resin RA1, by increasing the content of hydrophilic structures (particularly, the amount of polyalkylene oxide structures). In the present disclosure, the coefficient of variation of the particle size of the polymerizable resin particles A is measured by directly observing the particle size using the following microscope method.

[0150] The measurement of particle size by direct observation using the above-mentioned microscope will now be described in detail. 1. Sample Preparation 1 g of the dispersion liquid containing the polymerizable resin particles A is spread on an aluminum cup, solidified by natural drying, and pulverized in a mortar to obtain a powder sample. 2.SEM Measurement The obtained sample is measured by a scanning electron microscope (SEM, manufactured by JEOL Ltd.). After obtaining two fields of view in which the number of particles is 50 or more, the particle diameters are all measured by the Feret method (sandwiched between parallel lines: width of parallel lines = diameter) to obtain particle diameters for 100 or more particles. 3. Coefficient of variation After expanding the values ​​in order of particle size, the point where the number of large particles and the number of small particles are equal is defined as the central particle size, in the same way as for the definition of the median size, and the coefficient of variation of the particles using a microscope is calculated from the range of deviation from the central particle size.

[0151] The polymerizable resin particles A may be used alone or in combination of two or more kinds. The content of polymerizable resin particles A in the image recording layer of the lithographic printing plate precursor according to the present disclosure is, from the viewpoint of preventing plate skipping, preferably 10% by mass to 60% by mass, more preferably 20% by mass to 60% by mass, and more preferably 20% by mass to 55% by mass, and from the viewpoint of preventing plate skipping and on-press developability, further preferably 25% by mass to 55% by mass, and particularly preferably 30% by mass to 55% by mass.

[0152] [Polymerizable compound B] The polymerizable compound B in the present disclosure is a compound other than the polymerizable resin particles A that has an ethylenically unsaturated group. In the present disclosure, the polymerizable compound B is a compound having an ethylenically unsaturated group other than the polymerizable resin particles A, excluding the binder polymer described below. The ethylenically unsaturated group in the polymerizable compound B is the same as the ethylenically unsaturated group in the polymerizable resin RA, and preferred examples are also the same. The molecular weight of the polymerizable compound B (weight average molecular weight when the compound has a molecular weight distribution) is preferably 2,500 or less, more preferably 50 to 2,500, and further preferably 70 to 2,000. In one preferred embodiment, the molecular weight of the polymerizable compound B (weight average molecular weight when the compound has a molecular weight distribution) is 200 to 2,500.

[0153] The polymerizable compound B is an addition polymerizable compound (i.e., an ethylenically unsaturated compound) having at least one ethylenically unsaturated group. The polymerizable compound B preferably has two or more ethylenically unsaturated groups, and more preferably has three or more ethylenically unsaturated groups. The number of ethylenically unsaturated groups that the polymerizable compound B has is preferably, for example, 20 or less. The ethylenically unsaturated bond valence of the polymerizable compound B is, for example, preferably 1 mmol / g to 12 mmol / g, more preferably 5 mmol / g to 12 mmol / g, and even more preferably 7 mmol / g to 12 mmol / g, from the viewpoint of preventing plate skipping. The polymerizable compound B has a chemical form such as, for example, a monomer, a prepolymer, that is, a dimer, a trimer or an oligomer, or a mixture thereof.

[0154] -Oligomer- The polymerizable compound B preferably contains an oligomer. In the present disclosure, an oligomer refers to a polymerizable compound having a molecular weight (weight average molecular weight when the molecular weight has a molecular weight distribution) of 600 to 10,000 and containing at least one ethylenically unsaturated group. From the viewpoint of excellent chemical resistance and suppression of on-machine development residue, the molecular weight of the oligomer is preferably from 1,000 to 5,000, and more preferably from 1,000 to 2,500.

[0155] In addition, from the viewpoint of improving chemical resistance, the number of ethylenically unsaturated groups in one oligomer molecule is preferably 2 or more, more preferably 3 or more, even more preferably 6 or more, and particularly preferably 10 or more. The upper limit of the number of ethylenically unsaturated groups in the oligomer is not particularly limited, but is preferably 20 or less.

[0156] From the viewpoint of achieving superior chemical resistance and suppression of on-machine development residue, the oligomer preferably has 7 or more ethylenically unsaturated groups and a molecular weight of 1,000 to 10,000, and more preferably has 7 to 20 ethylenically unsaturated groups and a molecular weight of 1,000 to 5,000 (more preferably 1,000 to 2,500).

[0157] From the viewpoint of achieving better chemical resistance, the oligomer is preferably at least one type selected from the group consisting of a compound having a urethane bond, a compound having an ester bond, and a compound having an epoxy residue, and is preferably a compound having a urethane bond. In the present disclosure, the epoxy residue refers to a structure formed by an epoxy group, and means, for example, a structure similar to the structure obtained by the reaction of an acid group (such as a carboxylic acid group) with an epoxy group.

[0158] <<Compounds with urethane bonds>> The compound having a urethane bond is not particularly limited, but examples thereof include compounds obtained by reacting a polyisocyanate compound with a compound having a hydroxy group and an ethylenically unsaturated group.

[0159] The polyisocyanate compound may be a difunctional to pentafunctional polyisocyanate compound, and a difunctional or trifunctional polyisocyanate compound is preferred. Examples of polyisocyanate compounds include 1,3-bis(isocyanatomethyl)cyclohexane, isophorone diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, 1,3-cyclopentane diisocyanate, 9H-fluorene-2,7-diisocyanate, 9H-fluoren-9-one-2,7-diisocyanate, 4,4'- Preferred examples include diphenylmethane diisocyanate, 1,3-phenylene diisocyanate, tolylene-2,4-diisocyanate, tolylene-2,6-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 2,2-bis(4-isocyanatophenyl)hexafluoropropane, 1,5-diisocyanatonaphthalene, dimers and trimers (isocyanurate bonds) of these polyisocyanates, etc. Also, biuret compounds obtained by reacting the above polyisocyanate compounds with known amine compounds may be used.

[0160] As the compound having a hydroxy group and an ethylenically unsaturated group, a compound having one hydroxy group and one or more ethylenically unsaturated groups is preferable, and a compound having one hydroxy group and two or more ethylenically unsaturated groups is more preferable. Examples of compounds having a hydroxy group and an ethylenically unsaturated group include hydroxyethyl (meth)acrylate, glycerin di(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate.

[0161] The compound having a urethane bond is preferably a compound having at least a group represented by the following formula (Ac-1) or formula (Ac-2), and more preferably a compound having at least a group represented by the following formula (Ac-1).

[0162] [ka]

[0163] In formula (Ac-1) and formula (Ac-2), L 1 ~L 4 each independently represents a divalent hydrocarbon group having 2 to 20 carbon atoms, and the wavy line portion represents the bonding position to other structures. In formula (Ac-1) and formula (Ac-2), L 1 ~L 4 is preferably an alkylene group having 2 to 20 carbon atoms, more preferably an alkylene group having 2 to 10 carbon atoms, and further preferably an alkylene group having 4 to 8 carbon atoms. In addition, the alkylene group may have a branched or cyclic structure, but is preferably a linear alkylene group.

[0164] It is preferred that the wavy line portions in formula (Ac-1) or formula (Ac-2) are each independently directly bonded to the wavy line portions in the groups represented by formula (Ae-1) or formula (Ae-2) below.

[0165] [ka]

[0166] In formula (Ae-1) and formula (Ae-2), each R independently represents an acryloyloxy group or a methacryloyloxy group, and the wavy line portion represents the bonding position to the wavy line portion in formula (Ac-1) and formula (Ac-2).

[0167] In addition, as the compound having a urethane bond, a compound obtained by introducing an ethylenically unsaturated group into a polyurethane oligomer obtained by reacting a polyisocyanate compound with a polyol compound through a polymer reaction may be used. In addition, a compound having a urethane bond may be obtained by reacting a compound having an epoxy group and an ethylenically unsaturated group with a polyurethane oligomer obtained by reacting a polyol compound having an acid group with a polyisocyanate compound, for example.

[0168] <<Compounds with ester bonds>> Furthermore, the number of ethylenically unsaturated groups in the compound having an ester bond is preferably 3 or more, and more preferably 6 or more.

[0169] <<Compounds containing epoxy residues>> As the compound having an epoxy residue, a compound containing a hydroxy group within the compound is preferred. The compound having an epoxy residue preferably has 2 to 6 ethylenically unsaturated groups, and more preferably has 2 to 3 ethylenically unsaturated groups. The compound having an epoxy residue can be obtained, for example, by reacting a compound having an epoxy group with acrylic acid.

[0170] The oligomer used as the polymerizable compound B may be a commercially available product, and examples thereof include UA-510H, UA-306H, UA-306I, UA-306T (all manufactured by Kyoeisha Chemical Co., Ltd.), UV-1700B, UV-6300B, UV7620EA (all manufactured by Nippon Synthetic Chemical Industry Co., Ltd.), U-15HA (manufactured by Shin-Nakamura Chemical Co., Ltd.), EBECRYL450, EBECRYL657, EBECRYL885, EBECRYL800, EBECRYL3416, EBECRYL860 (all manufactured by Daicel-Allnex Corporation), but are not limited thereto.

[0171] From the viewpoint of improving chemical resistance and suppressing on-machine development residue, the content of the above oligomer relative to the total mass of the polymerizable compound B in the image recording layer is preferably 30% by mass to 100% by mass, more preferably 50% by mass to 100% by mass, and even more preferably 80% by mass to 100% by mass.

[0172] (Polymerizable compound B1) From the viewpoint of improving printing durability, the specific compound B may contain a compound having an ethylenically unsaturated bond valence of 5.0 mmol / g or more (hereinafter, also referred to as a polymerizable compound B1). The ethylenically unsaturated bond valence of the polymerizable compound B1 is preferably 5.5 mmol / g or more, more preferably 6.0 mmol / g or more. The upper limit of the ethylenically unsaturated bond valence of the polymerizable compound B1 is, for example, 10.0 mmol / g or less, more preferably 8.5 mmol / g or less.

[0173] Here, the ethylenically unsaturated bond valence of a compound in the present disclosure is determined by the following method. First, for a given sample amount (e.g., 0.2 g) of the compound, the structure of the compound is identified using, for example, pyrolysis GC / MS, FT-IR, NMR, TOF-SIMS, etc., and the total amount (mmol) of ethylenically unsaturated groups is determined. The determined total amount (mmol) of ethylenically unsaturated groups is divided by the sample amount (g) of the compound to calculate the ethylenically unsaturated bond valence of the compound.

[0174] From the viewpoint of satisfying the above C═C value, the polymerizable compound B1 is preferably a compound represented by the following formula (I). Formula (I): X-(Y)n In formula (I), X represents an n-valent organic group having a hydrogen-bonding group, Y represents a monovalent group having two or more ethylenically unsaturated groups, n represents an integer of 2 or more, and the molecular weight of X / (molecular weight of Y×n) is 1 or less.

[0175] The hydrogen bond group in X of formula (I) is not particularly limited, and may be a hydrogen bond donor group, a hydrogen bond acceptor group, or both, as long as it is a group capable of hydrogen bonding. Examples of the hydrogen bond group include a hydroxyl group, a carboxyl group, an amino group, a carbonyl group, a sulfonyl group, a urethane group, a urea group, an imide group, an amide group, and a sulfonamide group. Among them, the hydrogen bond group preferably contains at least one group selected from the group consisting of a urethane group, a urea group, an imide group, an amide group, and a sulfonamide group, from the viewpoint of on-press developability and printing durability, more preferably contains at least one group selected from the group consisting of a urethane group, a urea group, an imide group, and an amide group, further preferably contains at least one group selected from the group consisting of a urethane group, a urea group, and an imide group, and particularly preferably contains at least one group selected from the group consisting of a urethane group and a urea group.

[0176] X in formula (I) is preferably an organic group having no ethylenically unsaturated bond. From the viewpoints of on-press developability and printing durability, X in formula (I) is preferably a group consisting of a combination of two or more structures selected from the group consisting of monovalent to n-valent aliphatic hydrocarbon groups, monovalent to n-valent aromatic hydrocarbon groups, urethane bonds, urea bonds, biuret bonds, and allophanate bonds, and more preferably a group consisting of a combination of two or more structures selected from the group consisting of monovalent to n-valent aliphatic hydrocarbon groups, monovalent to n-valent aromatic hydrocarbon groups, urethane bonds, urea bonds, and biuret bonds.

[0177] From the viewpoints of on-press developability and printing durability, X in formula (I) is preferably a group obtained by removing a terminal isocyanate group from a polymer (including an adduct of a polyfunctional alcohol compound such as a trimethylolpropane adduct) obtained by polymerizing a polyfunctional isocyanate compound, more preferably a group obtained by removing a terminal isocyanate group from a polymer (including an adduct of a polyfunctional alcohol compound) obtained by polymerizing a bifunctional isocyanate compound, and particularly preferably a group obtained by removing a terminal isocyanate group from a polymer (including an adduct of a polyfunctional alcohol compound) obtained by polymerizing hexamethylene diisocyanate.

[0178] The molecular weight of X in formula (I) is preferably from 100 to 1,000, more preferably from 150 to 800, and particularly preferably from 150 to 500, from the viewpoints of on-press developability and printing durability.

[0179] The ethylenically unsaturated group in Y of formula (I) is not particularly limited, and from the viewpoints of reactivity, on-press developability, and printing durability, it is preferably at least one group selected from the group consisting of a vinylphenyl group, a vinyl ester group, a vinyl ether group, an allyl group, a (meth)acryloxy group, and a (meth)acrylamide group. From the same viewpoints as above, the ethylenically unsaturated group in Y of formula (I) is more preferably at least one group selected from the group consisting of a vinylphenyl group, a (meth)acryloxy group, and a (meth)acrylamide group, and is even more preferably a (meth)acryloxy group. That is, from the viewpoints of on-press developability and printing durability, it is preferable that the ethylenically unsaturated group in Y of formula (I) contains a (meth)acryloxy group.

[0180] In formula (I), Y is preferably a group having three or more (meth)acryloxy groups, more preferably a group having five or more (meth)acryloxy groups, and even more preferably a group having 5 to 12 (meth)acryloxy groups.

[0181] From the viewpoints of on-press developability and printing durability, Y in formula (I) may have a structure represented by the following formula (Y-1) or formula (Y-2).

[0182] [ka]

[0183] In formula (Y-1) and formula (Y-2), each R independently represents an acrylic group or a methacrylic group, and the wavy line portion represents the bonding position to other structures.

[0184] In formula (Y-1) or formula (Y-2), it is preferable that all R's are the same group. Also, in formula (Y-1) or formula (Y-2), it is preferable that R's are acrylic groups.

[0185] Furthermore, it is preferable that all of the n Y's in formula (I) are the same group.

[0186] The molecular weight of Y in formula (I) is preferably 200 or more and 1,000 or less, and more preferably 250 or more and 800 or less, from the viewpoints of on-press developability and printing durability.

[0187] In the formula (I), n is an integer of 2 or more, and from the viewpoints of on-press developability and printing durability, it is more preferably 2 to 3.

[0188] The molecular weight of X / (molecular weight of Y×n) is 1 or less, and from the viewpoints of on-press developability and printing durability, it is preferably 0.01 to 0.8, and more preferably 0.1 to 0.5.

[0189] As described above, the structure of the polymerizable compound B1 is preferably a structure in which the terminal isocyanate group of a polymerized product (including an adduct) of a polyfunctional isocyanate compound is blocked with a compound having an ethylenically unsaturated group. Among them, the polymerized product of a polyfunctional isocyanate compound is preferably a polymerized product of a bifunctional isocyanate compound.

[0190] In addition, from the viewpoint of on-press developability and printing durability, the polymerizable compound B1 is preferably a compound obtained by reacting a terminal isocyanate group of a polymerized product of a multifunctional isocyanate compound with a multifunctional ethylenically unsaturated compound having a hydroxyl group (also called a hydroxyl group) at the end. In addition, from the same viewpoint as above, the polymerizable compound B1 is more preferably a compound obtained by reacting a terminal isocyanate group of a polymerized product (including an adduct of a multifunctional alcohol compound) of a bifunctional isocyanate compound with a multifunctional ethylenically unsaturated compound having a hydroxyl group. Furthermore, from the same viewpoint as above, the polymerizable compound B1 is particularly preferably a compound obtained by reacting a terminal isocyanate group of a polymerized product (including an adduct of a multifunctional alcohol compound) of a hexamethylene diisocyanate with a multifunctional ethylenically unsaturated compound having a hydroxyl group.

[0191] The polyfunctional isocyanate compound is not particularly limited, and known compounds can be used, and may be aliphatic polyfunctional isocyanate compounds or aromatic polyfunctional isocyanate compounds.Specific examples of the polyfunctional isocyanate compound include 1,3-bis(isocyanatomethyl)cyclohexane, isophorone diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, 1,3-cyclopentane diisocyanate, 9H-fluorene-2,7-diisocyanate, and 9H-fluoren-9-one-2,7-diisocyanate. Preferred examples of the polyisocyanate include 4,4'-diphenylmethane diisocyanate, 1,3-phenylene diisocyanate, tolylene-2,4-diisocyanate, tolylene-2,6-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 2,2-bis(4-isocyanatophenyl)hexafluoropropane, 1,5-diisocyanatonaphthalene, and dimers and trimers (isocyanurate bonds) of these polyisocyanates. In addition, biuret compounds obtained by reacting the above polyisocyanate compounds with known amine compounds may be used. The polyfunctional ethylenically unsaturated compound having a hydroxyl group is preferably a trifunctional or higher ethylenically unsaturated compound having a hydroxyl group, more preferably a pentafunctional or higher ethylenically unsaturated compound having a hydroxyl group. The polyfunctional ethylenically unsaturated compound having a hydroxyl group is preferably a polyfunctional (meth)acrylate compound having a hydroxyl group.

[0192] From the viewpoints of on-press developability and printing durability, the polymerizable compound B1 preferably has at least one structure selected from the group consisting of an adduct structure, a biuret structure, and an isocyanurate structure. From the same viewpoints as above, the polymerizable compound B1 more preferably has at least one structure selected from the group consisting of a trimethylolpropane adduct structure, a biuret structure, and an isocyanurate structure, and particularly preferably has a trimethylolpropane adduct structure.

[0193] From the viewpoints of on-press developability and printing durability, the polymerizable compound B1 preferably has a structure represented by any one of the following formulas (A-1) to (A-3), and more preferably has a structure represented by the following formula (A-1).

[0194] [ka]

[0195] In formula (A-1), R A1 represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms, and the wavy line portion represents the bonding position to other structures.

[0196] R in formula (A-1) A1 From the viewpoints of on-press developability and printing durability, is preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, further preferably a methyl group or an ethyl group, and particularly preferably an ethyl group.

[0197] From the viewpoints of on-press developability and printing durability, the polymerizable compound B1 is preferably a (meth)acrylate compound having a urethane group, that is, a urethane (meth)acrylate oligomer.

[0198] The polymerizable compound B1 may be an oligomer having a polyester bond (hereinafter also referred to as a polyester(meth)acrylate oligomer) or an oligomer having an epoxy residue (hereinafter also referred to as an epoxy(meth)acrylate oligomer) so long as the ethylenically unsaturated bond valence is 5.0 mmol / g or more. Here, the epoxy residue in the epoxy (meth)acrylate oligomer is as described above.

[0199] The number of ethylenically unsaturated groups in the polyester (meth)acrylate oligomer which is the polymerizable compound B1 is preferably 3 or more, and more preferably 6 or more.

[0200] The epoxy (meth)acrylate oligomer, which is the polymerizable compound B1, is preferably a compound containing a hydroxyl group in the compound. The number of ethylenically unsaturated groups in the epoxy (meth)acrylate oligomer is preferably 2 to 6, more preferably 2 to 3. The epoxy (meth)acrylate oligomer can be obtained, for example, by reacting a compound having an epoxy group with acrylic acid.

[0201] The molecular weight of the polymerizable compound B1 (weight average molecular weight when the compound has a molecular weight distribution) may be more than 1,000, preferably 1,100 to 10,000, and more preferably 1,100 to 5,000.

[0202] The polymerizable compound B1 may be a synthetic product or a commercially available product. Specific examples of the polymerizable compound B1 include the following commercially available products, but the polymerizable compound B1 used in the present disclosure is not limited to these. Note that the number of functional groups (or average number of functional groups) and C=C value of the ethylenically unsaturated group are shown in parentheses. Specific examples of the polymerizable compound B1 include urethane (meth)acrylate oligomers such as U-10HA (functional group number: 10, C=C value: 8 mmol / g) and U-15HA (functional group number: 15, C=C value: 6 mmol / g) manufactured by Shin-Nakamura Chemical Co., Ltd., UA-510H (functional group number: 10, C=C value: 8 mmol / g) manufactured by Kyoeisha Chemical Co., Ltd., KRM8452 (functional group number: 10, C=C value: 7 mmol / g) manufactured by Daicel-Allnex Corporation, CN8885NS (functional group number: 9, C=C value: 6 mmol / g) and CN9013NS (functional group number: 9, C=C value: 6 mmol / g) manufactured by Sartomer Corporation. Specific examples of the polymerizable compound B1 include epoxy (meth)acrylate oligomers such as NK Oligo EA-7420 / PGMAc (functional group number: 10 to 15, C=C value: 5 mmol / g) manufactured by Shin-Nakamura Chemical Co., Ltd. and CN153 (C=C value: 5 mmol / g) manufactured by Sartomer Corporation. Further, specific examples of the polymerizable compound B1 include polyester (meth)acrylate oligomers such as CN2267 (C=C value: 5 mmol / g) manufactured by Sartomer Corporation.

[0203] When the polymerizable compound B1 is used, the content of the polymerizable compound B1 relative to the total mass of the polymerizable compound B in the image recording layer is preferably 10% by mass to 100% by mass, more preferably 50% by mass to 100% by mass, and further preferably 80% by mass to 100% by mass.

[0204] The polymerizable compound B may contain a compound other than the above oligomer and the polymerizable compound B1. The compound other than the oligomer as the polymerizable compound B is preferably a low molecular weight compound having a molecular weight (weight average molecular weight when the compound has a molecular weight distribution) of less than 1,000. The low molecular weight compound as the polymerizable compound B may be in any chemical form, such as a monomer, a dimer, a trimer, or a mixture thereof. From the viewpoint of chemical resistance, the low molecular weight compound as the polymerizable compound B is preferably at least one compound selected from the group consisting of a compound having three or more ethylenically unsaturated groups and a compound having an isocyanuric ring structure.

[0205] The low molecular weight compound as the polymerizable compound B may have a molecular weight (weight average molecular weight in the case of having a molecular weight distribution) of 50 or more and less than 1,000, preferably 50 or more and less than 600, and from the viewpoint of excellent chemical resistance and suppression of on-machine development residue, it is preferably 100 to 600, more preferably 200 to 600, and even more preferably 300 to 600.

[0206] When the polymerizable compound B contains the low molecular weight compound, from the viewpoints of chemical resistance and suppression of on-machine development residue, the ratio of the oligomer to the low molecular weight compound (oligomer / low molecular weight compound) is preferably 10 / 1 to 1 / 10, more preferably 10 / 1 to 3 / 7, and even more preferably 10 / 1 to 7 / 3, by mass.

[0207] Examples of low molecular weight compounds as the polymerizable compound B include unsaturated carboxylic acids (e.g., acrylic acid, methacrylic acid, itaconic acid, crotonic acid, isocrotonic acid, maleic acid, etc.), esters or amides thereof. Preferably, esters of unsaturated carboxylic acids and polyhydric alcohol compounds, and amides of unsaturated carboxylic acids and polyvalent amine compounds are used. In addition, unsaturated carboxylic acid esters having nucleophilic substituents such as hydroxyl groups, amino groups, and mercapto groups, or addition reaction products of amides and monofunctional or polyfunctional isocyanates or epoxy groups, and dehydration condensation reaction products of monofunctional or polyfunctional carboxylic acids are also preferably used. In addition, addition reaction products of unsaturated carboxylic acid esters or amides having electrophilic substituents such as isocyanate groups and epoxy groups and monofunctional or polyfunctional alcohols, amines, and thiols, and substitution reaction products of unsaturated carboxylic acid esters or amides having eliminable substituents such as halogen atoms and tosyloxy groups and monofunctional or polyfunctional alcohols, amines, and thiols are also suitable. As another example, it is also possible to use a compound group in which the above unsaturated carboxylic acid is replaced with an unsaturated phosphonic acid, styrene, vinyl ether, or the like. These are described in JP-T-2006-508380, JP-A-2002-287344, JP-A-2008-256850, JP-A-2001-342222, JP-A-9-179296, JP-A-9-179297, JP-A-9-179298, JP-A-2004-294935, JP-A-2006-243493, JP-A-2002-275129, JP-A-2003-64130, JP-A-2003-280187, JP-A-10-333321, and the like.

[0208] Specific examples of monomers of esters of polyhydric alcohol compounds and unsaturated carboxylic acids include acrylic esters such as ethylene glycol diacrylate, 1,3-butanediol diacrylate, tetramethylene glycol diacrylate, propylene glycol diacrylate, trimethylolpropane triacrylate, hexanediol diacrylate, tetraethylene glycol diacrylate, pentaerythritol tetraacrylate, sorbitol triacrylate, isocyanuric acid ethylene oxide (EO) modified triacrylate, polyester acrylate oligomer, etc. Specific examples of methacrylic esters include tetramethylene glycol dimethacrylate, neopentyl glycol dimethacrylate, trimethylolpropane trimethacrylate, ethylene glycol dimethacrylate, pentaerythritol trimethacrylate, bis[p-(3-methacryloxy-2-hydroxypropoxy)phenyl]dimethylmethane, bis[p-(methacryloxyethoxy)phenyl]dimethylmethane, etc. Specific examples of amide monomers of polyamine compounds and unsaturated carboxylic acids include methylene bisacrylamide, methylene bismethacrylamide, 1,6-hexamethylene bisacrylamide, 1,6-hexamethylene bismethacrylamide, diethylenetriamine trisacrylamide, xylylene bisacrylamide, and xylylene bismethacrylamide.

[0209] Also suitable are urethane-based addition polymerizable compounds produced by an addition reaction between an isocyanate and a hydroxy group. Specific examples thereof include vinyl urethane compounds containing two or more polymerizable vinyl groups in one molecule, which are obtained by adding a vinyl monomer containing a hydroxy group represented by the following formula (M) to a polyisocyanate compound having two or more isocyanate groups in one molecule, as described in JP-B-48-41708. Formula (M) CH2=C(R M4 )COOCH2CH(R M5 )OH In formula (M), R M4 and R M5 each independently represents a hydrogen atom or a methyl group.

[0210] Examples of the polymerizable compound B include urethane acrylates described in JP-A-51-37193, JP-B-2-32293, JP-B-2-16765, JP-A-2003-344997, and JP-A-2006-65210; Also suitable are urethane compounds having an ethylene oxide skeleton described in U.S. Pat. No. 7,153,632, JP-T-8-505958, JP-A-2007-293221, or JP-A-2007-293223, and urethane compounds having a hydrophilic group described in U.S. Pat. No. 7,153,632, JP-T-8-505958, JP-A-2007-293221, or JP-A-2007-293223.

[0211] (Polymerizable compound B2) The polymerizable compound B may contain, as a low molecular weight compound, a compound having one or two ethylenically unsaturated bond groups (hereinafter, also referred to as polymerizable compound B2). A preferred embodiment of the ethylenically unsaturated group in the polymerizable compound B2 is the same as the ethylenically unsaturated group in the polymerizable compound B1. Moreover, from the viewpoint of suppressing a decrease in on-press developability, the polymerizable compound B2 is preferably a compound having two ethylenically unsaturated bond groups (that is, a bifunctional polymerizable compound).

[0212] From the viewpoints of on-press developability and printing durability, the polymerizable compound B2 is preferably a methacrylate compound, that is, a compound having a methacryloxy group.

[0213] From the viewpoint of on-machine developability, the polymerizable compound B2 preferably contains an alkyleneoxy structure or a urethane bond.

[0214] The molecular weight of the polymerizable compound B2 (when the compound has a molecular weight distribution, the weight average molecular weight) is preferably 50 or more and less than 1,000, more preferably 200-900, and further preferably 250-800.

[0215] Specific examples of the polymerizable compound B2 are listed below, but the polymerizable compound B2 used in the present disclosure is not limited to these. In addition, in the compound (2) below, for example, n+m=10

[0216] [ka]

[0217] As the polymerizable compound B2, the commercially available products shown below may be used, but the polymerizable compound B2 used in the present disclosure is not limited to these. Specific examples of the polymerizable compound B2 include ethoxylated bisphenol A dimethacrylates such as BPE-80N (compound (1) above), BPE-100, BPE-200, and BPE-500 manufactured by Shin-Nakamura Chemical Co., Ltd., and CN104 (compound (1) above) manufactured by Sartomer Corporation. Specific examples of the polymerizable compound B2 include ethoxylated bisphenol A diacrylates such as A-BPE-10 (the compound (2) above) and A-BPE-4 manufactured by Shin-Nakamura Chemical Co., Ltd. Further, specific examples of the polymerizable compound B2 include bifunctional methacrylates such as FST 510 manufactured by AZ Electronics.

[0218] Here, the above-mentioned "FST 510" is a reaction product of 1 mole of 2,2,4-trimethylhexamethylene diisocyanate and 2 moles of hydroxyethyl methacrylate, and is an 82 mass % solution of the above-mentioned compound (3) in methyl ethyl ketone.

[0219] When the polymerizable compound B2 is used, the content of the polymerizable compound B2 relative to the total mass of the polymerizable compound B in the image recording layer is preferably 10% by mass to 100% by mass, more preferably 50% by mass to 100% by mass, and further preferably 80% by mass to 100% by mass.

[0220] Details of the method of use, such as the structure of the polymerizable compound B, whether it is used alone or in combination, and the amount added, can be set arbitrarily. That is, the polymerizable compound B may be used alone or in combination of two or more kinds. The content of the polymerizable compound B is preferably from 5 to 75% by mass, more preferably from 10 to 70% by mass, and particularly preferably from 15 to 60% by mass, based on the total mass of the image recording layer.

[0221] In the present disclosure, from the viewpoint of reactivity with the polymerizable resin particles A, the polymerizable compound B is preferably a compound having an ethylenically unsaturated bond equivalent of 300 g / mol or less, more preferably 150 g / mol or less. The lower limit of the ethylenically unsaturated bond equivalent of the polymerizable compound B is, for example, 50 g / mol. Here, the ethylenically unsaturated bond equivalent is a value obtained by dividing the molecular weight (g / mol) by the number of ethylenically unsaturated groups.

[0222] In the present disclosure, from the viewpoint of reactivity with the polymerizable resin particles A, the polymerizable compound B is preferably a compound having a molecular weight of 2,500 or less (more preferably, 100 to 2,500).

[0223] When the polymerizable compound B is a compound having an ethylenically unsaturated bond equivalent of 300 g / mol or less and / or a molecular weight of 2,500 or less (more preferably, 100 to 2,500), from the viewpoint of preventing plate skipping, the content is preferably 15% by mass to 80% by mass, more preferably 15% by mass to 70% by mass, and even more preferably 20% by mass to 65% by mass, relative to the total mass of the image recording layer.

[0224] In the present disclosure, the total amount of the polymerizable resin particles A and the polymerizable compound B in the image recording layer is preferably 40% by mass to 90% by mass, more preferably 50% by mass to 85% by mass, and even more preferably 50% by mass to 80% by mass.

[0225] [Polymerization initiator] The image recording layer in the present disclosure preferably contains a polymerization initiator. The polymerization initiator is not particularly limited, and examples thereof include an electron-accepting polymerization initiator and an electron-donating polymerization initiator. Among them, the polymerization initiator preferably contains at least an electron-accepting polymerization initiator.

[0226] (Electron-accepting polymerization initiator) The image recording layer preferably contains an electron-accepting polymerization initiator in order to prevent plate skipping. The electron-accepting polymerization initiator used in the present disclosure is a compound that generates a polymerization initiating species such as a radical or a cation by the energy of light, heat, or both, and can be appropriately selected from known thermal polymerization initiators, compounds having a bond with small bond dissociation energy, photopolymerization initiators, and the like. As the electron-accepting polymerization initiator, a radical polymerization initiator is preferable, and an onium compound is more preferable. The electron-accepting polymerization initiator is preferably an infrared-sensitive polymerization initiator. The electron-accepting polymerization initiator may be used alone or in combination of two or more kinds. Examples of the radical polymerization initiator include (a) organic halides, (b) carbonyl compounds, (c) azo compounds, (d) organic peroxides, (e) metallocene compounds, (f) azide compounds, (g) hexaarylbiimidazole compounds, (h) disulfone compounds, (i) oxime ester compounds, and (j) onium compounds. Among the above electron-accepting polymerization initiators, (i) oxime ester compounds and (j) onium compounds are preferred from the viewpoint of curability.

[0227] As the (a) organic halide, for example, the compounds described in paragraphs 0022 to 0023 of JP-A No. 2008-195018 are preferable. As the (b) carbonyl compound, for example, the compound described in paragraph 0024 of JP-A-2008-195018 is preferable. As the (c) azo compound, for example, the azo compounds described in JP-A-8-108621 can be used. (d) As the organic peroxide, for example, the compound described in paragraph 0025 of JP-A-2008-195018 is preferable. (e) As the metallocene compound, for example, the compound described in paragraph 0026 of JP-A-2008-195018 is preferable. (f) Examples of the azide compounds include 2,6-bis(4-azidobenzylidene)-4-methylcyclohexanone. (g) Preferred examples of the hexaarylbiimidazole compound include the compounds described in paragraph 0027 of JP-A-2008-195018. (h) Examples of disulfone compounds include the compounds described in JP-A-61-166544 and JP-A-2002-328465. (i) As the oxime ester compound, for example, the compounds described in paragraphs 0028 to 0030 of JP-A No. 2008-195018 are preferable.

[0228] In the present disclosure, the electron-accepting polymerization initiator is particularly preferably an onium compound (j). The onium compound (j) will be described in detail below. As the (j) onium compound, from the viewpoint of preventing plate skipping, an iodonium salt compound, a sulfonium salt compound, or an azinium salt compound is preferable, an iodonium salt compound or a sulfonium salt compound is more preferable, and an iodonium salt compound is even more preferable. Specific examples of these compounds are shown below, but the present disclosure is not limited thereto.

[0229] Preferred examples of the iodonium salt compound include diaryliodonium salt compounds, more preferred are diphenyliodonium salt compounds substituted with electron-donating groups such as alkyl groups or alkoxy groups, and more preferred are asymmetric diphenyliodonium salt compounds. Specific examples include diphenyliodonium hexafluorophosphate, 4-methoxyphenyl-4-(2-methylpropyl)phenyliodonium hexafluorophosphate, 4-(2-methylpropyl)phenyl-p-tolyliodonium hexafluorophosphate, 4-hexyloxyphenyl-2,4,6-trimethoxyphenyliodonium hexafluorophosphate, 4-hexyloxyphenyl-2,4-diethoxyphenyliodonium tetrafluoroborate, 4-octyloxyphenyl-2,4,6-trimethoxyphenyliodonium 1-perfluorobutanesulfonate, 4-octyloxyphenyl-2,4,6-trimethoxyphenyliodonium hexafluorophosphate, and bis(4-t-butylphenyl)iodonium hexafluorophosphate.

[0230] As an example of the sulfonium salt compound, a triarylsulfonium salt compound is preferable, particularly a triarylsulfonium salt compound in which an electron-withdrawing group, for example, at least a part of the group on the aromatic ring, is substituted with a halogen atom, and more preferably a triarylsulfonium salt compound in which the total number of halogen atoms substituted on the aromatic ring is 4 or more. Specific examples include triphenylsulfonium hexafluorophosphate, triphenylsulfonium benzoylformate, bis(4-chlorophenyl)phenylsulfonium benzoylformate, bis(4-chlorophenyl)-4-methylphenylsulfonium tetrafluoroborate, tris(4-chlorophenyl)sulfonium 3,5-bis(methoxycarbonyl)benzenesulfonate, tris(4-chlorophenyl)sulfonium hexafluorophosphate, tris(2,4-dichlorophenyl)sulfonium hexafluorophosphate, etc.

[0231] As the counter anion of the iodonium salt compound and the sulfonium salt compound, a sulfonamide anion or a sulfonimide anion is preferable, and a sulfonimide anion is more preferable. The sulfonamide anion is preferably an arylsulfonamide anion. The sulfonimide anion is preferably a bisarylsulfonimide anion. Specific examples of sulfonamide anions or sulfonimide anions are shown below, but the present disclosure is not limited thereto. In the following specific examples, Ph represents a phenyl group, Me represents a methyl group, and Et represents an ethyl group.

[0232] [ka]

[0233] Moreover, from the viewpoints of developability and UV printing durability of the resulting lithographic printing plate, the electron-accepting polymerization initiator may contain a compound represented by the following formula (II).

[0234] [ka]

[0235] In formula (II), X represents a halogen atom; 3 represents an aryl group.

[0236] Specific examples of X in the formula (II) include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Among these, a chlorine atom or a bromine atom is preferred because of its excellent sensitivity, and a bromine atom is particularly preferred. In addition, in formula (II), R 3 From the viewpoint of achieving an excellent balance between sensitivity and storage stability, an aryl group substituted with an amide group is preferred as the aryl group.

[0237] Specific examples of the electron-accepting polymerization initiator represented by the above formula (II) include compounds represented by the following formulas, but the present disclosure is not limited thereto.

[0238] [ka]

[0239] [ka]

[0240] [ka]

[0241] [ka]

[0242] [ka]

[0243] [ka]

[0244] [ka]

[0245] The lowest unoccupied molecular orbital (LUMO) of the electron-accepting polymerization initiator is preferably −3.00 eV or less, and more preferably −3.02 eV or less, from the viewpoint of preventing plate skipping. The lower limit of the LUMO of the electron-accepting polymerization initiator is preferably −3.80 eV or more, and more preferably −3.60 eV or more.

[0246] The content of the electron-accepting polymerization initiator is preferably 0.1% by mass to 50% by mass, more preferably 0.5% by mass to 30% by mass, and particularly preferably 0.8% by mass to 20% by mass, based on the total mass of the image recording layer.

[0247] (Electron-donating polymerization initiator) From the viewpoint of contributing to the chemical resistance of the lithographic printing plate and suppression of plate skipping, it is preferable that the polymerization initiator further contains an electron-donating polymerization initiator, and it is more preferable that the polymerization initiator contains both an electron-donating polymerization initiator and the above-mentioned electron-donating polymerization initiator. Examples of the electron-donating polymerization initiator include the following five types. (i) Alkyl or aryl ate complexes: It is believed that the carbon-hetero bond is oxidatively cleaved to generate active radicals. Specific examples include borate compounds. (ii) Aminoacetic acid compounds: It is believed that the C-X bond on the carbon adjacent to the nitrogen is cleaved by oxidation to generate an active radical. X is preferably a hydrogen atom, a carboxyl group, a trimethylsilyl group, or a benzyl group. Specific examples include N-phenylglycines (which may have a substituent on the phenyl group), N-phenyliminodiacetic acid (which may have a substituent on the phenyl group), etc. (iii) Sulfur-containing compounds: The above-mentioned aminoacetic acid compounds, in which the nitrogen atom is replaced with a sulfur atom, can generate active radicals by the same action. A specific example is phenylthioacetic acid (the phenyl group may have a substituent). (iv) Tin-containing compounds: Compounds in which the nitrogen atom of the above-mentioned aminoacetic acid compounds is replaced with a tin atom can generate active radicals by the same action. (v) Sulfinates: These can generate active radicals by oxidation. Specific examples include sodium arylsulfinate.

[0248] Among the electron donating polymerization initiators, the image recording layer preferably contains a borate compound. As the borate compound, a tetraarylborate compound or a monoalkyltriarylborate compound is preferable, and from the viewpoint of the stability of the compound, a tetraarylborate compound is more preferable, and a tetraphenylborate compound is particularly preferable. The counter cation of the borate compound is not particularly limited, but is preferably an alkali metal ion or a tetraalkylammonium ion, more preferably a sodium ion, a potassium ion, or a tetrabutylammonium ion. In addition, the onium ion in the electron-accepting polymerization initiator is also preferably used as the counter cation of the borate compound.

[0249] A specific example of a preferred borate compound is sodium tetraphenylborate.

[0250] Moreover, the highest occupied molecular orbital (HOMO) of the electron donating polymerization initiator used in the present disclosure is preferably −6.00 eV or more, more preferably −5.95 eV or more, and even more preferably −5.93 eV or more, from the viewpoint of preventing plate skipping. The upper limit of the HOMO of the electron-donating polymerization initiator is preferably −5.00 eV or less, and more preferably −5.40 eV or less.

[0251] In the present disclosure, the highest occupied molecular orbital (HOMO) and lowest unoccupied molecular orbital (LUMO) are calculated by the following method. First, the counter anion in the compound to be calculated is ignored. The quantum chemical calculation software Gaussian09 was used, and the structure optimization was performed using DFT (B3L YP / 6-31G(d)). MO (molecular orbital) energy calculations are performed using DFT (B3LYP / 6-31+G(d,p) / CPCM (solvent=methanol)) on the structure obtained by the above structural optimization. The MO energy Ebare (unit: hartree) obtained in the above MO energy calculation is converted to Escaled (unit: eV) used as the HOMO and LUMO values ​​in this disclosure by the following formula. Escaled=0.823168×27.2114×Ebare-1.07634 Note that 27.2114 is simply a coefficient for converting hartrees to eV, and 0.823168 and -1.07634 are adjustment coefficients that are used to determine the HOMO and LUMO of the compound being calculated so that the calculation matches the measured values.

[0252] As preferred specific examples of the electron-donating polymerization initiator, B-1 to B-8 and other compounds are shown below, but it goes without saying that the present invention is not limited to these. In the following chemical formulas, Bu represents an n-butyl group, and Z represents a counter cation. Z + As the counter cation represented by + , K + , N + (Bu)4, etc. + The counter cation represented by the formula (I) may be an onium ion in the electron-accepting polymerization initiator.

[0253] [ka]

[0254] [ka]

[0255] The electron-donating polymerization initiator may be added either alone or in combination of two or more. From the viewpoint of increasing reactivity, the content of the electron-donating polymerization initiator is preferably 0.1 to 10% by mass, more preferably 1.0 to 10% by mass, and even more preferably 3.0 to 7.0% by mass, based on the total mass of the image recording layer.

[0256] In addition, one of the preferred aspects of the present disclosure is an aspect in which the electron-accepting polymerization initiator and the electron-donating polymerization initiator form a salt. Specifically, for example, the onium compound may be a salt of an onium ion and an anion in the electron-donating polymerization initiator (e.g., tetraphenylborate anion).More preferably, the onium compound may be an iodonium borate compound in which an iodonium cation in the iodonium salt compound (e.g., di-p-tolyliodonium cation) and a borate anion in the electron-donating polymerization initiator form a salt. Specific examples of the embodiment in which the electron-accepting polymerization initiator and the electron-donating polymerization initiator form a salt are shown below, but the present disclosure is not limited thereto.

[0257] [ka]

[0258] In the present disclosure, when the image recording layer contains an onium ion and an anion in the above-mentioned electron-donating polymerization initiator, the image recording layer contains an electron-accepting polymerization initiator and the above-mentioned electron-donating polymerization initiator.

[0259] [Infrared absorbent] The image recording layer in the present disclosure preferably contains an infrared absorbing agent. The infrared absorbing agent is not particularly limited, and examples thereof include pigments and dyes. As the dye to be used as the infrared absorber, commercially available dyes and known dyes described in literature such as "Dye Handbook" (edited by the Organic Synthesis Chemistry Association, published in 1970) can be used. Specific examples of the dye include azo dyes, metal complex azo dyes, pyrazolone azo dyes, naphthoquinone dyes, anthraquinone dyes, phthalocyanine dyes, carbonium dyes, quinoneimine dyes, methine dyes, cyanine dyes, squarylium dyes, pyrylium salts, and metal thiolate complex dyes.

[0260] Particularly preferred among these dyes are cyanine dyes, squarylium dyes, pyrylium salts, nickel thiolate complexes, and indolenine cyanine dyes, of which cyanine dyes are particularly preferred.

[0261] The infrared absorbing agent is preferably a cationic polymethine dye having an oxygen or nitrogen atom at the meso position. Preferred examples of the cationic polymethine dye include cyanine dyes, pyrylium dyes, thiopyrylium dyes, and azulenium dyes, and from the viewpoints of availability, solubility in a solvent during the introduction reaction, and the like, cyanine dyes are preferred.

[0262] Specific examples of the cyanine dye include the compounds described in paragraphs 0017 to 0019 of JP-A-2001-133969, the compounds described in paragraphs 0016 to 0021 of JP-A-2002-023360, and the compounds described in paragraphs 0012 to 0037 of JP-A-2002-040638. Specific examples of the cyanine dye include the compounds described in paragraphs 0034 to 0041 of JP-A-2002-278057, or the compounds described in paragraphs 0080 to 0086 of JP-A-2008-195018, and particularly preferably the compounds described in paragraphs 0035 to 0043 of JP-A-2007-90850, or the compounds described in paragraphs 0105 to 0113 of JP-A-2012-206495. Furthermore, as the cyanine dye, the compounds described in paragraphs 0008 to 0009 of JP-A No. 5-5005 and paragraphs 0022 to 0025 of JP-A No. 2001-222101 can also be preferably used. As the pigment, the compounds described in paragraphs 0072 to 0076 of JP-A No. 2008-195018 are preferred.

[0263] The infrared absorbing agent may be used alone or in combination of two or more kinds. Also, a pigment and a dye may be used in combination as the infrared absorbing agent. The content of the infrared absorbing agent in the image recording layer is preferably from 0.1% by mass to 10.0% by mass, and more preferably from 0.5% by mass to 5.0% by mass, based on the total mass of the image recording layer.

[0264] -Relationship between electron donor polymerization initiators and infrared absorbers- From the viewpoint of preventing plate skipping, the image recording layer in the present disclosure contains the electron-donating polymerization initiator and the infrared absorber, and the value obtained by subtracting the HOMO of the electron-donating polymerization initiator from the HOMO of the infrared absorber is preferably 0.70 eV or less, and more preferably 0.70 eV to -0.10 eV. A negative value means that the HOMO of the electron-donating polymerization initiator is higher than the HOMO of the infrared absorber.

[0265] -Preferred embodiments of infrared absorber and electron-accepting polymerization initiator- In order to prevent plate skipping, the infrared absorber according to the present disclosure preferably has an organic anion in which, in Hansen solubility parameters, Δd is 16 or more, Δp is 16 to 32, and Δh is 60% or less of Δp. In terms of preventing plate skipping, a preferred embodiment of the electron-accepting polymerization initiator in the present disclosure has an organic anion in which Δd is 16 or more, Δp is 16 to 32, and Δh is 60% or less of Δp, in Hansen solubility parameters.

[0266] Here, δd, δp, and δh in the Hansen solubility parameters in this disclosure are the dispersion term δd [unit: MPa 0.5 ], polar term δp [unit: MPa 0.5 ], and hydrogen bond term δh [unit: MPa 0.5 Here, the Hansen solubility parameter is the solubility parameter introduced by Hildebrand, which is divided into three components, the dispersion term δd, the polarity term δp, and the hydrogen bond term δh, and expressed in three-dimensional space. Details of Hansen solubility parameters are described in the literature "Hansen Solubility Parameters; A Users Handbook (CRC Press, 2007)" written by Charles M. Hansen.

[0267] In the present disclosure, the δd, δp, and δh in the Hansen solubility parameters of the above organic anions are values ​​estimated from their chemical structures using computer software "Hansen Solubility Parameters in Practice (HSPiP ver.4.1.07)."

[0268] Specific examples of organic anions having a Hansen solubility parameter Δd of 16 or more, Δp of 16 to 32, and Δh of 60% or less of Δp are preferably, but needless to say, not limited to, those shown below.

[0269] [ka]

[0270] [Binder polymer] The image recording layer in the present disclosure may contain a binder polymer. As the binder polymer, any binder polymer used in a known lithographic printing plate precursor can be used without any restrictions.

[0271] The binder polymer used in the present disclosure preferably has a glass transition temperature (Tg) of 50° C. or higher, more preferably 70° C. or higher, even more preferably 80° C. or higher, and particularly preferably 90° C. or higher, from the viewpoint of suppressing deterioration of on-press developability over time. The upper limit of the glass transition temperature of the binder polymer is preferably 200° C., more preferably 120° C. or lower, from the viewpoint of ease of penetration of water into the image recording layer.

[0272] As the binder polymer having the above glass transition temperature, polyvinyl acetal is preferred from the viewpoint of further suppressing the deterioration of on-press developability over time.

[0273] Polyvinyl acetal is a resin obtained by acetalizing the hydroxyl groups of polyvinyl alcohol with an aldehyde. In particular, polyvinyl butyral obtained by acetalizing (that is, butyralizing) the hydroxyl groups of polyvinyl alcohol with butylaldehyde is preferred. The polyvinyl acetal preferably contains a structural unit represented by the following (a) obtained by acetalizing the hydroxyl group of polyvinyl alcohol with an aldehyde.

[0274] [ka]

[0275] Here, R represents the residue of the aldehyde used in the acetalization. Examples of R include a hydrogen atom, an alkyl group, and an ethylenically unsaturated group described below.

[0276] The content of the structural unit represented by (a) (also referred to as the amount of ethylene groups in the main chain contained in the structural unit represented by (a) above, and also referred to as the degree of acetalization) is preferably 50 mol% to 90 mol%, more preferably 55 mol% to 85 mol%, and even more preferably 55 mol% to 80 mol%, relative to all structural units of the polyvinyl acetal (total amount of ethylene groups in the main chain). The degree of acetalization is a molar fraction calculated by dividing the amount of ethylene groups to which acetal groups are bonded (the amount of ethylene groups in the main chain contained in the structural unit represented by (a) above) by the total amount of ethylene groups in the main chain, expressed as a percentage. The same applies to the content of each structural unit of the polyvinyl acetal described below.

[0277] From the viewpoint of improving printing durability, the polyvinyl acetal preferably has an ethylenically unsaturated group. Here, the ethylenically unsaturated group contained in the polyvinyl acetal is not particularly limited, and from the viewpoints of reactivity, on-press developability, and printing durability, it is more preferably at least one group selected from the group consisting of a vinylphenyl group (styryl group), a vinyl ester group, a vinyl ether group, an allyl group, a (meth)acryloxy group, and a (meth)acrylamide group, and a vinyl group, an allyl group, a (meth)acryloxy group, etc. are preferred.

[0278] From the viewpoint of improving printing durability, the polyvinyl acetal preferably contains a structural unit having an ethylenically unsaturated group. The structural unit having an ethylenically unsaturated group may be the above-mentioned structural unit having an acetal ring, or may be a structural unit other than the structural unit having an acetal ring. Among them, from the viewpoint of increasing the crosslink density during exposure, the polyvinyl acetal is preferably a compound having an ethylenically unsaturated group introduced into the acetal ring, i.e., in the constitutional unit represented by (a) above, it is preferable that R has an ethylenically unsaturated group.

[0279] When the structural unit having an ethylenically unsaturated group is a structural unit other than a structural unit having an acetal ring, it may be, for example, a structural unit having an acrylate group, specifically, a structural unit represented by the following (d).

[0280] [ka]

[0281] When the structural unit having an ethylenically unsaturated group is a structural unit other than a structural unit having an acetal ring, the content of this structural unit (also referred to as the amount of acrylate groups) is preferably 1 mol% to 15 mol%, and more preferably 1 mol% to 10 mol%, based on the total structural units of the polyvinyl acetal.

[0282] The polyvinyl acetal preferably further contains a structural unit having a hydroxy group from the viewpoint of on-machine developability, etc. In other words, the polyvinyl acetal preferably contains a structural unit derived from vinyl alcohol. An example of a structural unit having a hydroxy group is the structural unit represented by the following (b).

[0283] [ka]

[0284] From the viewpoint of on-machine developability, the content of the structural unit represented by (b) (also referred to as the amount of hydroxyl groups) is preferably 5 mol% to 50 mol%, more preferably 10 mol% to 40 mol%, and even more preferably 20 mol% to 40 mol%, based on the total structural units of the polyvinyl acetal.

[0285] The polyvinyl acetal may further contain other structural units. Examples of other structural units include structural units having an acetyl group, specifically, the structural unit represented by the following (c).

[0286] [ka]

[0287] The content of the structural unit represented by (c) (also referred to as the amount of acetyl groups) is preferably 0.5 mol % to 10 mol %, more preferably 0.5 mol % to 8 mol %, and even more preferably 1 mol % to 3 mol %, based on all structural units of the polyvinyl acetal.

[0288] Here, the degree of acetalization, the amount of acrylate groups, the amount of hydroxyl groups, and the amount of acetyl groups can be determined as follows. That is, 1The molar content is calculated from the proton peak area ratio of the methyl or methylene moiety of the acetal, the methyl moiety of the acrylate group, the hydroxyl group, and the methyl moiety of the acetyl group by H NMR measurement.

[0289] The weight average molecular weight of the polyvinyl acetal is preferably 10,000 to 150,000.

[0290] The Hansen solubility parameter of the above polyvinyl acetal is 17.5MPa. 1 / 2 ~20.0MPa 1 / 2 It is preferable that the pressure is 18.0 MPa. 1 / 2 ~19.5MPa 1 / 2 It is more preferable that: In the present disclosure, when a compound is a polymer of an addition polymerization type, polycondensation type, or the like, the SP value of each monomer unit is multiplied by the molar fraction to represent the total amount, and when a compound is a low molecular weight compound having no monomer units, the SP value of the entire compound is used. In the present disclosure, the SP value of a polymer may be calculated from the molecular structure of the polymer by the Hoy method described in Polymer Handbook (fourth edition).

[0291] Specific examples of the polyvinyl acetal [P-1 to P-3] are given below, but the polyvinyl acetal used in the present disclosure is not limited to these. In the following structure, "l" is 50 mol% to 90 mol%, "m" is 0.5 mol% to 10 mass%, "n" is 5 mol% to 50 mol%, and "o" is 1 mol% to 15 mol%.

[0292] [ka]

[0293] As the polyvinyl acetal, commercially available products can be used. Commercially available polyvinyl acetal products include the S-LEC BL series (specifically, S-LEC BL-10, BL-1, BL-5Z, BL-7Z, etc.), the S-LEC BM series (specifically, S-LEC BM-1, BM-S(Z), BM-5, etc.), the S-LEC BH series (specifically, S-LEC BH-S, BH-6, BH-3(Z)), the S-LEC BX series (S-LEC BX-L, etc.), and the S-LEC KS series (S-LEC KS-10, etc.), all manufactured by Sekisui Chemical Co., Ltd.

[0294] However, from the viewpoint of preventing plate skipping, it is preferable to increase the content of the polymerizable resin particles A and the polymerizable compound B in the image recording layer, and it is preferable that the image recording layer does not contain a binder polymer or contains a small amount of a binder polymer. From the viewpoint of improving developability and preventing plate skipping, the content of the binder polymer is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass, and particularly preferably 0% by mass, based on the total mass of the image recording layer.

[0295] [Color former] The image recording layer in the present disclosure preferably contains a color former, and more preferably contains an acid color former. As the color former, an acid color former is particularly preferred. The term "color former" as used in the present disclosure means a compound that has the property of changing the color of the image recording layer by developing or decoloring in response to a stimulus such as light, acid, etc. Additionally, the term "acid color former" means a compound that has the property of changing the color of the image recording layer by developing or decoloring in response to heating in a state in which it accepts an electron-accepting compound (e.g., a proton such as an acid). As the acid color former, in particular, a colorless compound having a partial skeleton such as a lactone, lactam, sultone, spiropyran, ester, or amide, which quickly undergoes ring-opening or cleavage when contacted with an electron-accepting compound, is preferred.

[0296] Examples of acid color formers include 3,3-bis(4-dimethylaminophenyl)-6-dimethylaminophthalide (also known as crystal violet lactone), 3,3-bis(4-dimethylaminophenyl)phthalide, 3-(4-dimethylaminophenyl)-3-(4-diethylamino-2-methylphenyl)-6-dimethylaminophthalide, 3-(4-dimethylaminophenyl)-3-(1,2-dimethylindol-3-yl)phthalide, and 3-(4-dimethylaminophenyl)-3-(2-methylindol-3-yl)phthalide. 3,3-bis(1,2-dimethylindol-3-yl)phthalide, 3,3-bis(1,2-dimethylindol-3-yl)-5-dimethylaminophthalide, 3,3-bis(1,2-dimethylindol-3-yl)-6-dimethylaminophthalide, 3,3-bis(9-ethylcarbazol-3-yl)-6-dimethylaminophthalide, 3,3-bis(2-phenylindol-3-yl)-6-dimethylaminophthalide, 3-(4-dimethylaminophenyl)-3-(1-methylpyrrol-3-yl)-6-dimethylaminophthalide,

[0297] 3,3-bis[1,1-bis(4-dimethylaminophenyl)ethylene-2-yl]-4,5,6,7-tetrachlorophthalide, 3,3-bis[1,1-bis(4-pyrrolidinophenyl)ethylene-2-yl]-4,5,6,7-tetrabromophthalide, 3,3-bis[1-(4-dimethylaminophenyl)-1-(4-methoxyphenyl)ethylene-2-yl]-4,5,6,7-tetrachlorophthalide, 3,3-bis[1-(4-pyrrolidinophenyl)-1-(4-methoxyphenyl)ethylene-2-yl]-4,5,6,7-tetrachlorophthalide, 3-[1,1-di(1-ethyl-2-methylindo phthalides such as 3-[1,1-di(1-ethyl-2-methylindol-3-yl)ethylene-2-yl]-3-(4-diethylaminophenyl)phthalide, 3-[1,1-di(1-ethyl-2-methylindol-3-yl)ethylene-2-yl]-3-(4-N-ethyl-N-phenylaminophenyl)phthalide, 3-(2-ethoxy-4-diethylaminophenyl)-3-(1-n-octyl-2-methylindol-3-yl)-phthalide, 3,3-bis(1-n-octyl-2-methylindol-3-yl)-phthalide, and 3-(2-methyl-4-diethylaminophenyl)-3-(1-n-octyl-2-methylindol-3-yl)-phthalide;

[0298] 4,4-Bis-dimethylaminobenzhydrin benzyl ether, N-halophenyl-leucoauramine, N-2,4,5-trichlorophenylleucoauramine, rhodamine-B-anilinolactam, rhodamine-(4-nitroanilino)lactam, rhodamine-B-(4-chloroanilino)lactam, 3,7-bis(diethylamino)-10-benzoylphenoxazine, benzoylleuco methylene blue, 4-nitrobenzoyl methylene blue,

[0299] 3,6-dimethoxyfluoran, 3-dimethylamino-7-methoxyfluoran, 3-diethylamino-6-methoxyfluoran, 3-diethylamino-7-methoxyfluoran, 3-diethylamino-7-chlorofluoran, 3-diethylamino-6-methyl-7-chlorofluoran, 3-diethylamino-6,7-dimethylfluoran, 3-N-cyclohexyl-Nn-butylamino-7-methylfluoran, 3-diethylamino-7-dibenzylaminofluoran, 3-diethylamino-7-octylaminofluoran, 3-diethylamino-7-di-n-hexylaminofluoran, 3-diethylamino-7-anilinofluoran, 3- Diethylamino-7-(2'-fluorophenylamino)fluoran, 3-diethylamino-7-(2'-chlorophenylamino)fluoran, 3-diethylamino-7-(3'-chlorophenylamino)fluoran, 3-diethylamino-7-(2',3'-dichlorophenylamino)fluoran, 3-diethylamino-7-(3'-trifluoromethylphenylamino)fluoran, 3-di-n-butylamino-7-(2'-fluorophenylamino)fluoran, 3-di-n-butylamino-7-(2'-chlorophenylamino)fluoran, 3-N-isopentyl-N-ethylamino-7-(2'-chlorophenylamino)fluoran,

[0300] 3-Nn-hexyl-N-ethylamino-7-(2'-chlorophenylamino)fluoran, 3-diethylamino-6-chloro-7-anilinofluoran, 3-di-n-butylamino-6-chloro-7-anilinofluoran, 3-diethylamino-6-methoxy-7-anilinofluoran, 3-di-n-butylamino-6-ethoxy-7-anilinofluoran, 3-pyrrolidino-6-methyl-7-anilinofluoran, 3-piperidino-6-methyl-7-anilinofluoran, 3-morpholino- 6-Methyl-7-anilinofluoran, 3-dimethylamino-6-methyl-7-anilinofluoran, 3-diethylamino-6-methyl-7-anilinofluoran, 3-di-n-butylamino-6-methyl-7-anilinofluoran, 3-di-n-pentylamino-6-methyl-7-anilinofluoran, 3-N-ethyl-N-methylamino-6-methyl-7-anilinofluoran, 3-Nn-propyl-N-methylamino-6-methyl-7-anilinofluoran, 3-Nn-propyl-N-ethyl N-butyl-N-methylamino-6-methyl-7-anilinofluoran, 3-N-butyl-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-isobutyl-N-methylamino-6-methyl-7-anilinofluoran, 3-N-isobutyl-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-isopentyl-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-hexyl-N-methylamino amino-6-methyl-7-anilinofluoran, 3-N-cyclohexyl-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-cyclohexyl-Nn-propylamino-6-methyl-7-anilinofluoran, 3-N-cyclohexyl-Nn-butylamino-6-methyl-7-anilinofluoran, 3-N-cyclohexyl-Nn-hexylamino-6-methyl-7-anilinofluoran, 3-N-cyclohexyl-Nn-octylamino-6-methyl-7-anilinofluoran,

[0301] 3-N-(2'-methoxyethyl)-N-methylamino-6-methyl-7-anilinofluoran, 3-N-(2'-methoxyethyl)-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-(2'-methoxyethyl)-N-isobutylamino-6-methyl-7-anilinofluoran, 3-N-(2'-ethoxyethyl)-N-methylamino-6-methyl-7-anilinofluoran, 3-N-(2'-ethoxyethyl)-N-ethylamino-6-methyl-7 -Anilinofluoran, 3-N-(3'-methoxypropyl)-N-methylamino-6-methyl-7-anilinofluoran, 3-N-(3'-methoxypropyl)-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-(3'-ethoxypropyl)-N-methylamino-6-methyl-7-anilinofluoran, 3-N-(3'-ethoxypropyl)-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-(3'-ethoxypropyl)-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-(2'-tetrahydrofurfuryl)- N-ethylamino-6-methyl-7-anilinofluoran, 3-N-(4'-methylphenyl)-N-ethylamino-6-methyl-7-anilinofluoran, 3-diethylamino-6-ethyl-7-anilinofluoran, 3-diethylamino-6-methyl-7-(3'-methylphenylamino)fluoran, 3-diethylamino-6-methyl-7-(2',6'-dimethylphenylamino)fluoran, 3-di-n-butylamino-6-methyl-7-(2',6'-dimethylphenylamino)fluoran, fluorans such as 3-di-n-butylamino-7-(2',6'-dimethylphenylamino)fluoran, 3-di-n-butylamino-7-(2',6'-dimethylphenylamino)fluoran, 2,2-bis[4'-(3-N-cyclohexyl-N-methylamino-6-methylfluoran)-7-ylaminophenyl]propane, 3-[4'-(4-phenylaminophenyl)aminophenyl]amino-6-methyl-7-chlorofluoran, and 3-[4'-(dimethylaminophenyl)]amino-5,7-dimethylfluoran;

[0302] 3-(2-methyl-4-diethylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, 3-(2-n-propoxycarbonylamino-4-di-n-propylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, 3-(2-methylamino-4-di-n-propylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, 3-(2-methylamino-4-di-n-propylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, 3-(2-methyl-4-di-n-hexylaminophenyl)-3-(1-n- Octyl-2-methylindol-3-yl)-4,7-diazaphthalide, 3,3-bis(2-ethoxy-4-diethylaminophenyl)-4-azaphthalide, 3,3-bis(1-n-octyl-2-methylindol-3-yl)-4-azaphthalide, 3-(2-ethoxy-4-diethylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, 3-(2-ethoxy-4-diethylaminophenyl)-3-(1-octyl-2-methylindol-3-yl)-4 or 7-azaphthalide 3-(2-ethoxy-4-diethylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)-4 or 7-azaphthalide, 3-(2-hexyloxy-4-diethylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)-4 or 7-azaphthalide, 3-(2-ethoxy-4-diethylaminophenyl)-3-(1-ethyl-2-phenylindol-3-yl)-4 or 7-azaphthalide, 3-(2-butoxy-4-diethylaminophenyl)-3-(1-ethyl-2-phenylindol-3-yl)-4 or 7-azaphthalide nilindol-3-yl)-4 or 7-azaphthalide 3-methylspirodiinaphthopyran, 3-ethylspirodiinaphthopyran, 3-phenylspirodiinaphthopyran, 3-benzylspirodiinaphthopyran, 3-methylnaphtho(3-methoxybenzo)spiropyran, 3-propylspirodibenzopyran-3,6-bis(dimethylamino)fluorene-9-spiro-3'-(6'-dimethylamino)phthalide, 3,6-bis(diethylamino)fluorene-9-spiro-3'-(6'-dimethylamino)phthalide and other phthalides;

[0303] Other examples include 2'-anilino-6'-(N-ethyl-N-isopentyl)amino-3'-methylspiro[isobenzofuran-1(3H),9'-(9H)xanthene-3-one, 2'-anilino-6'-(N-ethyl-N-(4-methylphenyl))amino-3'-methylspiro[isobenzofuran-1(3H),9'-(9H)xanthene]-3-one, 3'-N,N-dibenzylamino-6'-N,N-diethylaminospiro[isobenzofuran-1(3H),9'-(9H)xanthene]-3-one, and 2'-(N-methyl-N-phenyl)amino-6'-(N-ethyl-N-(4-methylphenyl))aminospiro[isobenzofuran-1(3H),9'-(9H)xanthene]-3-one.

[0304] Among the above, the acid color former used in the present disclosure is preferably at least one compound selected from the group consisting of spiropyran compounds, spirooxazine compounds, spirolactone compounds, and spirolactam compounds. From the viewpoint of visibility, the hue of the dye after color development is preferably green, blue, or black.

[0305] In addition, the acid color former is preferably a leuco dye from the viewpoints of color development and visibility of exposed areas. The leuco dye is not particularly limited as long as it has a leuco structure, but it preferably has a spiro structure, and more preferably has a spirolactone ring structure. From the viewpoints of color development and visibility of exposed areas, the leuco dye is preferably a leuco dye having a phthalide structure or a fluoran structure. Furthermore, from the viewpoints of color development and visibility of exposed areas, the leuco dye having the above-mentioned phthalide structure or fluoran structure is preferably a compound represented by any one of the following formulas (Le-1) to (Le-3), and more preferably a compound represented by the following formula (Le-2).

[0306] [ka]

[0307] In formulae (Le-1) to (Le-3), each ERG independently represents an electron-donating group, each X1 to X4 independently represents a hydrogen atom, a halogen atom, or a dialkylanilino group, 10 each independently represents a hydrogen atom, a halogen atom, or a monovalent organic group; Y1 and Y2 each independently represent C or N; when Y1 is N, X1 is not present; and when Y2 is N, X4 is not present; Ra1 represents a hydrogen atom, an alkyl group, or an alkoxy group; and Rb1 to Rb4 each independently represent an alkyl group or an aryl group.

[0308] From the viewpoints of color development and visibility of exposed areas, the electron-donating group in ERG of formulae (Le-1) to (Le-3) is preferably an amino group, an alkylamino group, an arylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a diarylamino group, an alkoxy group, an aryloxy group, or an alkyl group, more preferably an amino group, an alkylamino group, an arylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a diarylamino group, an alkoxy group, or an aryloxy group, still more preferably a monoalkylmonoarylamino group or a diarylamino group, and particularly preferably a monoalkylmonoarylamino group. In the formulae (Le-1) to (Le-3), X1 to X4 are each preferably independently a hydrogen atom or a chlorine atom, more preferably a hydrogen atom, from the viewpoints of color development and visibility of exposed areas. X5 to X in formula (Le-2) or formula (Le-3) 10are each independently, from the viewpoints of color development and visibility of the exposed area, preferably a hydrogen atom, a halogen atom, an alkyl group, an aryl group, an amino group, an alkylamino group, an arylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a diarylamino group, a hydroxy group, an alkoxy group, an aryloxy group, an acyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, or a cyano group, more preferably a hydrogen atom, a halogen atom, an alkyl group, an aryl group, an alkoxy group, or an aryloxy group, even more preferably a hydrogen atom, a halogen atom, an alkyl group, or an aryl group, and particularly preferably a hydrogen atom. In the formulae (Le-1) to (Le-3), from the viewpoints of color development and visibility of exposed areas, at least one of Y1 and Y2 is preferably C, and it is more preferable that both of Y1 and Y2 are C. From the viewpoints of color development and visibility of exposed areas, Ra1 in formulae (Le-1) to (Le-3) is preferably an alkyl group or an alkoxy group, more preferably an alkoxy group, and particularly preferably a methoxy group. In formulae (Le-1) to (Le-3), Rb1 to Rb4 are each independently preferably a hydrogen atom or an alkyl group, more preferably an alkyl group, and particularly preferably a methyl group, from the viewpoints of color development and visibility of exposed areas.

[0309] From the viewpoints of color development and visibility of exposed areas, the leuco dye having a phthalide structure or a fluoran structure is more preferably a compound represented by any one of the following formulas (Le-4) to (Le-6), and even more preferably a compound represented by the following formula (Le-5).

[0310] [ka]

[0311] In formulae (Le-4) to (Le-6), ERG each independently represents an electron donating group, X1 to X4 each independently represent a hydrogen atom, a halogen atom, or a dialkylanilino group, Y1 and Y2 each independently represent C or N, and when Y1 is N, X1 does not exist, and when Y2 is N, X4 does not exist, Ra1 represents a hydrogen atom, an alkyl group, or an alkoxy group, and Rb1 to Rb4 each independently represent an alkyl group or an aryl group.

[0312] In formulae (Le-4) to (Le-6), ERG, X1 to X4, Y1, Y2, Ra1, and Rb1 to Rb4 have the same meanings as ERG, X1 to X4, Y1, Y2, Ra1, and Rb1 to Rb4 in formulae (Le-1) to (Le-3), respectively, and preferred embodiments are also the same.

[0313] Furthermore, from the viewpoints of color development and visibility of exposed areas, the leuco dye having the phthalide structure or the fluoran structure is more preferably a compound represented by any one of the following formulas (Le-7) to (Le-9), and particularly preferably a compound represented by the following formula (Le-8).

[0314] [ka]

[0315] In formulae (Le-7) to (Le-9), X1 to X4 each independently represent a hydrogen atom, a halogen atom, or a dialkylanilino group; Y1 and Y2 each independently represent C or N; when Y1 is N, X1 does not exist; when Y2 is N, X4 does not exist; Ra1 to Ra4 each independently represent a hydrogen atom, an alkyl group, or an alkoxy group; Rb1 to Rb4 each independently represent an alkyl group or an aryl group; and Rc1 and Rc2 each independently represent an aryl group.

[0316] X1 to X4, Y1 and Y2 in formulae (Le-7) to (Le-9) have the same meanings as X1 to X4, Y1 and Y2 in formulae (Le-1) to (Le-3), and preferred embodiments are also the same. In formulae (Le-7) to (Le-9), Ra1 to Ra4 are each independently preferably an alkyl group or an alkoxy group, more preferably an alkoxy group, and particularly preferably a methoxy group, from the viewpoints of color development and visibility of the exposed area. In formulae (Le-7) to (Le-9), Rb1 to Rb4 are each independently preferably a hydrogen atom, an alkyl group, or an aryl group substituted with an alkoxy group, more preferably an alkyl group, and particularly preferably a methyl group, from the viewpoints of color development and visibility of the exposed area. In formulae (Le-7) to (Le-9), Rc1 and Rc2 are each independently preferably a phenyl group or an alkylphenyl group, more preferably a phenyl group, from the viewpoints of color development and visibility of exposed areas. In formula (Le-8), from the viewpoints of color development and visibility of exposed areas, it is preferable that X1 to X4 are hydrogen atoms, and Y1 and Y2 are C. Furthermore, in formula (Le-8), from the viewpoints of color development and visibility of exposed areas, it is preferred that Rb1 and Rb2 are each independently an aryl group substituted with an alkyl group or an alkoxy group.

[0317] The alkyl group in the formulae (Le-1) to (Le-9) may be linear, branched, or have a ring structure. In addition, the alkyl group in formulae (Le-1) to (Le-9) preferably has 1 to 20 carbon atoms, more preferably 1 to 8 carbon atoms, further preferably 1 to 4 carbon atoms, and particularly preferably 1 or 2 carbon atoms. The aryl group in formulae (Le-1) to (Le-9) preferably has 6 to 20 carbon atoms, more preferably 6 to 10 carbon atoms, and particularly preferably 6 to 8 carbon atoms.

[0318] In addition, each group such as a monovalent organic group, an alkyl group, an aryl group, a dialkylanilino group, an alkylamino group, and an alkoxy group in the formulae (Le-1) to (Le-9) may have a substituent. Examples of the substituent include an alkyl group, an aryl group, a halogen atom, an amino group, an alkylamino group, an arylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a diarylamino group, a hydroxy group, an alkoxy group, an aryloxy group, an acyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, and a cyano group. In addition, these substituents may be further substituted with these substituents.

[0319] Specific examples of the leuco dye having a phthalide structure or a fluoran structure that can be suitably used include the following compounds (S-1 to S-14).

[0320] [ka]

[0321] [ka]

[0322] [ka]

[0323] [ka]

[0324] [ka]

[0325] As the acid color former, commercially available products can be used. Acid color-developing agent products include ETAC, RED500, RED520, CVL, S-205, BLACK305, BLACK400, BLACK100, BLACK500, H-7001, GREEN300, NIRBLACK78, BLUE220, H-3035, BLUE203, ATP, H-1046, H-2114 (all manufactured by Fukui Yamada Chemical Co., Ltd.), ORANGE-DCF, Vermilion-DCF, and PIN. Examples of suitable dyes include K-DCF, RED-DCF, BLMB, CVL, GREEN-DCF, TH-107 (all manufactured by Hodogaya Chemical Co., Ltd.), ODB, ODB-2, ODB-4, ODB-250, ODB-BlackXV, Blue-63, Blue-502, GN-169, GN-2, Green-118, Red-40, Red-8 (all manufactured by Yamamoto Chemical Industry Co., Ltd.), and crystal violet lactone (manufactured by Tokyo Chemical Industry Co., Ltd.). Among these commercially available products, ETAC, S-205, BLACK305, BLACK400, BLACK100, BLACK500, H-7001, GREEN300, NIRBLACK78, H-3035, ATP, H-1046, H-2114, GREEN-DCF, Blue-63, GN-169, and crystal violet lactone are preferred because the films formed have good visible light absorptance.

[0326] These color formers (preferably acid color formers) may be used alone or in combination of two or more kinds. The content of the color former (preferably an acid color former) is preferably from 0.5% by mass to 10% by mass, and more preferably from 1% by mass to 5% by mass, based on the total mass of the image recording layer.

[0327] [Chain transfer agent] The image recording layer in the present disclosure may contain a chain transfer agent. The chain transfer agent contributes to improving the printing durability of the lithographic printing plate. The chain transfer agent is preferably a thiol compound, more preferably a thiol having 7 or more carbon atoms from the viewpoint of boiling point (difficulty of volatilization), and further preferably a compound having a mercapto group on an aromatic ring (aromatic thiol compound).The thiol compound is preferably a monofunctional thiol compound.

[0328] Specific examples of the chain transfer agent include the following compounds.

[0329] [ka]

[0330] [ka]

[0331] [ka]

[0332] [ka]

[0333] The chain transfer agent may be added alone or in combination of two or more kinds. The content of the chain transfer agent is preferably from 0.01% by mass to 50% by mass, more preferably from 0.05% by mass to 40% by mass, and even more preferably from 0.1% by mass to 30% by mass, based on the total mass of the image recording layer.

[0334] [Other resin particles] In order to improve the on-press developability of the lithographic printing plate precursor, the image recording layer may contain resin particles other than the polymerizable resin particles A. The other resin particles are preferably resin particles that can convert the image recording layer to a hydrophobic state when heat is applied thereto. The other resin particles are preferably at least one selected from hydrophobic thermoplastic resin particles, heat-reactive resin particles, resin particles having a polymerizable group other than the polymerizable resin particles A, microcapsules encapsulating a hydrophobic compound, and microgels (i.e., crosslinked resin particles). Among these, resin particles and microgels having a polymerizable group other than the polymerizable resin particles A are preferred.

[0335] Suitable examples of the hydrophobic thermoplastic resin particles include those described in Research Disclosure No. 33303 published in January 1992, JP-A Nos. 9-123387, 9-131850, 9-171249, and 9-171250, and European Patent No. 931647. Specific examples of the resin constituting the hydrophobic thermoplastic resin particles include homopolymers or copolymers of monomers such as ethylene, styrene, vinyl chloride, methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, vinylidene chloride, acrylonitrile, vinylcarbazole, acrylates or methacrylates having a polyalkylene structure, or mixtures thereof. Preferred examples include polystyrene, copolymers containing styrene and acrylonitrile, and polymethyl methacrylate. The volume average particle size of the hydrophobic thermoplastic resin particles is preferably 0.01 μm to 2.0 μm.

[0336] The thermally reactive resin particles include resin particles having a thermally reactive group, which form a hydrophobic region by crosslinking due to a thermal reaction and by the change in functional group at that time.

[0337] The thermoreactive group in the resin particles having a thermoreactive group can be any functional group that undergoes any reaction as long as it forms a chemical bond, and is preferably a polymerizable group.As examples thereof, the ethylenically unsaturated group that undergoes radical polymerization reaction (such as acryloyl group, methacryloyl group, vinyl group, allyl group, etc.), cationic polymerizable group (such as vinyl group, vinyloxy group, epoxy group, oxetanyl group, etc.), the isocyanato group or its block product that undergoes addition reaction, epoxy group, vinyloxy group and the functional group with active hydrogen atom that is their reaction partner (such as amino group, hydroxyl group, carboxyl group, etc.), the carboxyl group that undergoes condensation reaction and the hydroxyl group or amino group that is their reaction partner, the acid anhydride that undergoes ring-opening addition reaction and the amino group or hydroxyl group that is their reaction partner, etc. can be suitably mentioned.

[0338] As the microcapsule, for example, as described in JP-A-2001-277740 and JP-A-2001-277742, all or part of the components of the image recording layer are encapsulated in the microcapsule. The components of the image recording layer can also be contained outside the microcapsule. As the image recording layer containing the microcapsule, a preferred embodiment is one in which the hydrophobic components are encapsulated in the microcapsule and the hydrophilic components are contained outside the microcapsule.

[0339] The microgel (crosslinked resin particles) can contain a part of the components of the image recording layer at least either inside or on the surface thereof.

[0340] In order to microencapsulate or microgel the components of the image recording layer, known methods can be used. The average particle size of the microcapsules and the microgel is preferably 0.01 μm to 3.0 μm, more preferably 0.05 μm to 2.0 μm, and particularly preferably 0.10 μm to 1.0 μm. Good resolution and stability over time can be obtained within this range.

[0341] When other resin particles are contained in the image recording layer, the content of the other resin particles is preferably 0% by mass to 30% by mass with respect to the total mass of the image recording layer.

[0342] [Low molecule hydrophilic compound] The image recording layer in the present disclosure may contain a low molecular weight hydrophilic compound in order to improve on-press developability while suppressing a decrease in printing durability. The low molecular weight hydrophilic compound is preferably a compound having a molecular weight of less than 1,000, more preferably a compound having a molecular weight of less than 800, and even more preferably a compound having a molecular weight of less than 500. Examples of low molecular weight hydrophilic compounds include water-soluble organic compounds such as glycols and their ether or ester derivatives, such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, and tripropylene glycol; polyols, such as glycerin, pentaerythritol, and tris(2-hydroxyethyl)isocyanurate; organic amines and their salts, such as triethanolamine, diethanolamine, and monoethanolamine; organic sulfonic acids and their salts, such as alkylsulfonic acid, toluenesulfonic acid, and benzenesulfonic acid; organic sulfamic acids and their salts, such as alkylsulfamic acid; organic sulfuric acids and their salts, such as alkylsulfuric acid and alkyl ether sulfuric acid; organic phosphonic acids and their salts, such as phenylphosphonic acid; organic carboxylic acids and their salts, such as tartaric acid, oxalic acid, citric acid, malic acid, lactic acid, gluconic acid, and amino acids; and betaines.

[0343] As the low molecular weight hydrophilic compound, it is preferable to contain at least one selected from polyols, organic sulfates, organic sulfonates, and betaines.

[0344] Specific examples of organic sulfonates include alkyl sulfonates such as sodium n-butyl sulfonate, sodium n-hexyl sulfonate, sodium 2-ethylhexyl sulfonate, sodium cyclohexyl sulfonate, and sodium n-octyl sulfonate; alkyl sulfonates containing an ethylene oxide chain such as sodium 5,8,11-trioxapentadecane-1-sulfonate, sodium 5,8,11-trioxaheptadecane-1-sulfonate, sodium 13-ethyl-5,8,11-trioxaheptadecane-1-sulfonate, and sodium 5,8,11,14-tetraoxatetracosane-1-sulfonate. arylsulfonates such as sodium benzenesulfonate, sodium p-toluenesulfonate, sodium p-hydroxybenzenesulfonate, sodium p-styrenesulfonate, sodium isophthalate dimethyl-5-sulfonate, sodium 1-naphthylsulfonate, sodium 4-hydroxynaphthylsulfonate, disodium 1,5-naphthalenedisulfonate, and trisodium 1,3,6-naphthalenetrisulfonate; and compounds described in paragraphs 0026 to 0031 of JP-A No. 2007-276454 and paragraphs 0020 to 0047 of JP-A No. 2009-154525. The salt may be a potassium salt or a lithium salt.

[0345] The organic sulfates include sulfates of alkyl, alkenyl, alkynyl, aryl, or heterocyclic monoether of polyethylene oxide. The number of ethylene oxide units is preferably 1 to 4, and the salt is preferably a sodium salt, a potassium salt, or a lithium salt. Specific examples include the compounds described in paragraphs 0034 to 0038 of JP-A-2007-276454.

[0346] As the betaines, compounds in which the number of carbon atoms in the hydrocarbon substituent on the nitrogen atom is 1 to 5 are preferable, and specific examples include trimethylammonium acetate, dimethylpropylammonium acetate, 3-hydroxy-4-trimethylammoniobutyrate, 4-(1-pyridinio)butyrate, 1-hydroxyethyl-1-imidazolioacetate, trimethylammonium methanesulfonate, dimethylpropylammonium methanesulfonate, 3-trimethylammonio-1-propanesulfonate, and 3-(1-pyridinio)-1-propanesulfonate.

[0347] Since the structure of the hydrophobic portion of the low molecular weight hydrophilic compound is small and it has almost no surface activity, the dampening water is unlikely to penetrate into the image portion of the image recording layer and reduce the hydrophobicity of the image portion, film strength, etc. Therefore, by incorporating a low molecular weight hydrophilic compound in the image recording layer, the ink acceptance and printing durability of the image recording layer can be well maintained.

[0348] The low molecular weight hydrophilic compound may be used alone or in combination of two or more kinds. The content of the low molecular weight hydrophilic compound is preferably 0.5% by mass to 20% by mass, more preferably 1% by mass to 15% by mass, and even more preferably 2% by mass to 10% by mass, based on the total mass of the image recording layer. Within this range, good on-press developability and printing durability can be obtained.

[0349] [Oil sensitizer] The image recording layer in the present disclosure may contain an oil sensitizer such as a phosphonium compound, a nitrogen-containing low molecular weight compound, or an ammonium group-containing polymer in order to improve ink receptivity. In particular, when an inorganic layered compound is contained in the water-soluble resin layer, these compounds function as a surface coating agent for the inorganic layered compound, and can suppress a decrease in ink receptivity during printing caused by the inorganic layered compound. As the oil sensitizer, it is preferable to use a phosphonium compound, a nitrogen-containing low molecular weight compound, and an ammonium group-containing polymer in combination, and it is more preferable to use a phosphonium compound, a quaternary ammonium salt, and an ammonium group-containing polymer in combination.

[0350] Examples of the phosphonium compound include those described in JP-A-2006-297907 and JP-A-2007-50660.Specific examples include tetrabutylphosphonium iodide, butyltriphenylphosphonium bromide, tetraphenylphosphonium bromide, 1,4-bis(triphenylphosphonio)butane=di(hexafluorophosphate), 1,7-bis(triphenylphosphonio)heptane=sulfate, and 1,9-bis(triphenylphosphonio)nonane=naphthalene-2,7-disulfonate.

[0351] Examples of the nitrogen-containing low molecular weight compound include amine salts and quaternary ammonium salts. Examples of the nitrogen-containing low molecular weight compound include imidazolinium salts, benzimidazolinium salts, pyridinium salts, and quinolinium salts. Among them, quaternary ammonium salts and pyridinium salts are preferred. Specific examples include tetramethylammonium hexafluorophosphate, tetrabutylammonium hexafluorophosphate, dodecyltrimethylammonium p-toluenesulfonate, benzyltriethylammonium hexafluorophosphate, benzyldimethyloctylammonium hexafluorophosphate, benzyldimethyldodecylammonium hexafluorophosphate, and the compounds described in paragraphs 0021 to 0037 of JP-A-2008-284858 and paragraphs 0030 to 0057 of JP-A-2009-90645.

[0352] The ammonium group-containing polymer may have an ammonium group in its structure, and is preferably a polymer containing 5 mol % to 80 mol % of a (meth)acrylate having an ammonium group in a side chain as a copolymerization component. Specific examples include the polymers described in paragraphs 0089 to 0105 of JP-A-2009-208458.

[0353] The ammonium salt-containing polymer preferably has a reduced specific viscosity (unit: ml / g) value determined according to the measurement method described in JP 2009-208458 A in the range of 5 to 120, more preferably 10 to 110, and particularly preferably 15 to 100. When the reduced specific viscosity is converted into a weight average molecular weight (Mw), it is preferably 10,000 to 150,0000, more preferably 17,000 to 140,000, and particularly preferably 20,000 to 130,000.

[0354] Specific examples of the ammonium group-containing polymer are shown below. (1) 2-(trimethylammonio)ethyl methacrylate = p-toluenesulfonate / 3,6-dioxaheptyl methacrylate copolymer (molar ratio 10 / 90, Mw 45,000) (2) 2-(trimethylammonio)ethyl methacrylate = hexafluorophosphate / 3,6-dioxaheptyl methacrylate copolymer (molar ratio 20 / 80, Mw 60,000) (3) 2-(ethyldimethylammonio)ethyl methacrylate = p-toluenesulfonate / hexyl methacrylate copolymer (molar ratio 30 / 70, Mw 45,000) (4) 2-(trimethylammonio)ethyl methacrylate = hexafluorophosphate / 2-ethylhexyl methacrylate copolymer (molar ratio 20 / 80, Mw 60,000) (5) 2-(trimethylammonio)ethyl methacrylate = methyl sulfate / hexyl methacrylate copolymer (molar ratio 40 / 60, Mw 70,000) (6) 2-(butyldimethylammonio)ethyl methacrylate = hexafluorophosphate / 3,6-dioxaheptyl methacrylate copolymer (molar ratio 25 / 75, Mw 65,000) (7) 2-(butyldimethylammonio)ethyl acrylate = hexafluorophosphate / 3,6-dioxaheptyl methacrylate copolymer (molar ratio 20 / 80, Mw 65,000) (8) 2-(butyldimethylammonio)ethyl methacrylate = 13-ethyl-5,8,11-trioxa-1-heptadecanesulfonate / 3,6-dioxaheptyl methacrylate copolymer (molar ratio 20 / 80, Mw 75,000) (9) 2-(butyldimethylammonio)ethyl methacrylate = hexafluorophosphate / 3,6-dioxaheptyl methacrylate / 2-hydroxy-3-methacryloyloxypropyl methacrylate copolymer (molar ratio 15 / 80 / 5, Mw 65,000)

[0355] The content of the oil sensitizer is preferably from 0.01% by mass to 30.0% by mass, more preferably from 0.1% by mass to 15.0% by mass, and even more preferably from 1% by mass to 10% by mass, based on the total mass of the image recording layer.

[0356] [Coloring agent] The image recording layer in the present disclosure can contain a dye having a large absorption in the visible light region as an image colorant. It is preferable to add a colorant since it makes it easier to distinguish between image areas and non-image areas after image formation. Specific examples of colorants include oil yellow #101, oil yellow #103, oil pink #312, oil green BG, oil blue BOS, oil blue #603, oil black BY, oil black BS, oil black T-505 (all manufactured by Orient Chemical Industry Co., Ltd.), Victoria Pure Blue, crystal violet (CI42555), methyl violet (CI42535), ethyl violet, ethyl violet 6HNAPS, rhodamine B (CI145170B), malachite green (CI42000), methylene blue (CI52015), and dyes described in JP-A-62-293247. In addition, pigments such as phthalocyanine pigments, azo pigments, carbon black, and titanium oxide can also be suitably used. The amount of the colorant added is preferably 0.005% by mass to 10% by mass based on the total mass of the image recording layer.

[0357] [Fluorine-containing copolymer] The image recording layer in the present disclosure preferably contains a fluorine-containing copolymer, more preferably a fluorine-containing copolymer having a structural unit formed from a fluorine-containing monomer. Among the fluorine-containing copolymers, a fluoroaliphatic group-containing copolymer is preferred. By using a fluorine-containing copolymer (preferably a fluoroaliphatic group-containing copolymer), abnormal surface quality due to foaming during the formation of the image recording layer can be suppressed, the coating surface condition can be improved, and further the ink receptivity of the formed image recording layer can be improved. In addition, an image recording layer containing a fluorine-containing copolymer (preferably a fluoroaliphatic group-containing copolymer) can provide a lithographic printing plate with high gradation, high sensitivity to, for example, laser light, good fogging properties due to scattered light, reflected light, etc., and excellent printing durability.

[0358] The above-mentioned fluoroaliphatic group-containing copolymer preferably has a structural unit formed from a fluoroaliphatic group-containing monomer, and in particular, preferably has a structural unit formed from a compound represented by either of the following formula (F1) and the following formula (F2).

[0359] [ka]

[0360] In formulas (F1) and (F2), R F1 each independently represents a hydrogen atom or a methyl group, and each X independently represents an oxygen atom, a sulfur atom, or -N(R F2 )-, m is an integer of 1 to 6, n is an integer of 1 to 10, l is an integer of 0 to 10, R F2 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.

[0361] R in formulas (F1) and (F2) F2 The alkyl group having 1 to 4 carbon atoms represented by the following formula is preferably a methyl group, an ethyl group, an n-propyl group, or an n-butyl group, and more preferably a hydrogen atom or a methyl group. In formulae (F1) and (F2), X is preferably an oxygen atom. In formula (F1), m is preferably 1 or 2, and more preferably 2. In formula (F1), n ​​is preferably 2, 4, 6, 8 or 10, and more preferably 4 or 6. In formula (F2), l is preferably 0.

[0362] Specific examples of the fluoroaliphatic group-containing monomer including a compound represented by either formula (F1) or formula (F2) and the fluorine-containing monomer are shown below, but the fluoroaliphatic group-containing monomer and the fluorine-containing monomer are not limited thereto.

[0363] [ka]

[0364] [ka]

[0365] [ka]

[0366] [ka]

[0367] [ka]

[0368] [ka]

[0369] [ka]

[0370] [ka]

[0371] [ka]

[0372] [ka]

[0373] [ka]

[0374] [ka]

[0375] The above-mentioned fluorine-containing copolymer preferably has, in addition to the constituent units formed from the fluorine-containing monomer, a constituent unit formed from at least one compound selected from the group consisting of poly(oxyalkylene)acrylates and poly(oxyalkylene)methacrylates. In addition, the above-mentioned fluoroaliphatic group-containing copolymer preferably further has a structural unit formed from at least one compound selected from the group consisting of poly(oxyalkylene)acrylates and poly(oxyalkylene)methacrylates, in addition to the structural unit formed from the compound represented by either of the above-mentioned formula (F1) and formula (F2).

[0376] The polyoxyalkylene group in the poly(oxyalkylene) acrylate and poly(oxyalkylene) methacrylate is -(OR F3 ) x - can be expressed as R F3 represents an alkyl group, and x represents an integer of 2 or more. F3is preferably a linear or branched alkylene group having 2 to 4 carbon atoms. The linear or branched alkylene group having 2 to 4 carbon atoms is preferably -CH2CH2-, -CH2CH2CH2-, -CH(CH3)CH2-, or -CH(CH3)CH(CH3)-. x is preferably an integer of 2 to 100. In the polyoxyalkylene group, x "OR F3 " may be the same or different. In other words, the polyoxyalkylene group may have two or more "OR F3 " may be bonded regularly or irregularly. For example, the polyoxyalkylene group may be a group in which linear or branched oxypropylene units and oxyethylene units are bonded regularly or irregularly. More specifically, the polyoxyalkylene group may be a group in which blocks of linear or branched oxypropylene units and blocks of oxyethylene units are bonded. The polyoxyalkylene group may contain one or more linking groups (for example, -CONH-Ph-NHCO-, -S-, etc., where Ph represents a phenylene group). The molecular weight of the polyoxyalkylene group is preferably 250 to 3,000.

[0377] As the poly(oxyalkylene)acrylate and poly(oxyalkylene)methacrylate, commercially available products or synthetic products may be used. The above poly(oxyalkylene) acrylates and poly(oxyalkylene) methacrylates can be synthesized, for example, by reacting a hydroxypoly(oxyalkylene) compound with acrylic acid, methacrylic acid, acrylic chloride, methacrylic chloride, acrylic anhydride, or the like by a known method. As the hydroxypoly(oxyalkylene) compound, commercially available products may be used, such as ADEKA (registered trademark) Pluronic manufactured by ADEKA CORPORATION, ADEKA Polyether manufactured by ADEKA CORPORATION, Carbowax (registered trademark) manufactured by Union Carbide Corporation, Triton manufactured by The Dow Chemical Company, and PEG manufactured by Daiichi Kogyo Seiyaku Co., Ltd. As the poly(oxyalkylene) acrylate and poly(oxyalkylene) methacrylate, poly(oxyalkylene) diacrylate and the like synthesized by a known method may be used.

[0378] [Other ingredients] The image recording layer in the present disclosure may contain, as other components, a surfactant (other than a fluoroaliphatic group-containing copolymer), a polymerization inhibitor, a higher fatty acid derivative, a plasticizer, inorganic particles, an inorganic layered compound, etc. For details, refer to the description in paragraphs 0114 to 0159 of JP-A-2008-284817.

[0379] [Formation of image recording layer] The image recording layer in the lithographic printing plate precursor according to the present disclosure can be formed, for example, as described in paragraphs

[0142] to

[0143] of JP2008-195018A, by dispersing or dissolving each of the above-mentioned necessary components in a known solvent (coating solvent) to prepare a coating liquid, applying the coating liquid onto a support by a known method such as bar coater coating, and drying. The coating amount (solid content) of the image recording layer after coating and drying varies depending on the application, but is generally 0.3 g / m 2 ~3.0g / m 2 In this range, good sensitivity and good film properties of the image recording layer can be obtained.

[0380] Examples of the coating solvent include MEK / MFG / methanol=48 / 30 / 22 (mass ratio, SP value=11.1), 1-propanol / water=1 / 1 (mass ratio, SP value=17.7), and a single alcoholic organic solvent.

[0381] [Protective layer] The lithographic printing plate precursor according to the present disclosure may have a layer such as a protective layer (sometimes referred to as an overcoat layer, etc.) containing a water-soluble resin or the like on the image recording layer; however, the image recording layer has a high ethylenically unsaturated bond value, and therefore does not necessarily require oxygen blocking properties provided by a protective layer, etc. Therefore, the lithographic printing plate precursor according to the present disclosure is preferably in an embodiment in which no layer such as a water-soluble resin layer is provided, and the image recording layer is exposed.

[0382] [Aluminum Support] The aluminum support in the lithographic printing plate precursor according to the present disclosure can be appropriately selected from known aluminum supports for lithographic printing plate precursors. Hereinafter, the aluminum support may also be simply referred to as "support". The aluminum support is preferably an aluminum support having a hydrophilic surface (hereinafter, also referred to as "hydrophilic aluminum support").

[0043] From the viewpoint of preventing scratches and stains, the aluminum support in the lithographic printing plate precursor according to the present disclosure has a contact angle with water, as measured by a water drop method in the air, on the surface of the aluminum support on the image recording layer side, of preferably 110° or less, more preferably 90° or less, even more preferably 80° or less, even more preferably 50° or less, particularly preferably 30° or less, more particularly preferably 20° or less, and most preferably 10° or less.

[0383] In the present disclosure, the contact angle with water on the surface of the aluminum support on the side of the image recording layer is measured by the following method using a water drop method in the air. The lithographic printing plate precursor is immersed in a solvent capable of removing the image recording layer (e.g., the solvent used in the coating liquid for the image recording layer), and the image recording layer is scraped off with at least one of a sponge and cotton, thereby dissolving the image recording layer in the solvent to expose the surface of the aluminum support. The surface of the aluminum support exposed by the above method may contain a hydrophilic compound, which will be described later. Therefore, for example, the contact angle of the surface with water may be adjusted by the hydrophilic compound remaining on the surface of the aluminum support. The contact angle with water on the surface of the exposed aluminum support on the image recording layer side is measured as the contact angle of a water droplet on the surface at 25°C (after 0.2 seconds) using a fully automatic contact angle meter (e.g., DM-501 manufactured by Kyowa Interface Science Co., Ltd.) as a measuring device.

[0384] The aluminum support in the present disclosure is preferably an aluminum plate that has been subjected to a surface roughening treatment and anodization treatment by a known method. That is, the aluminum support in the present disclosure preferably has an aluminum plate and an anodized aluminum coating disposed on the aluminum plate.

[0385] [Preferred embodiment of the support] An example of a preferred embodiment of the aluminum support used in the present disclosure (the aluminum support according to this example is also referred to as "support (1)") is shown below. That is, the support (1) has an aluminum plate and an anodized aluminum film disposed on the aluminum plate, the anodized film is located closer to the image recording layer than the aluminum plate, the anodized film has micropores extending in the depth direction from the surface on the image recording layer side, the average diameter of the micropores on the surface of the anodized film is more than 10 nm and not more than 100 nm, and the L of the surface of the anodized film on the image recording layer side is * a * b * Lightness L in color system * The value is between 70 and 100.

[0386] FIG. 1 is a schematic cross-sectional view of one embodiment of an aluminum support 12a. The aluminum support 12a has a laminated structure in which an aluminum plate 18 and an aluminum anodized film 20a (hereinafter also simply referred to as "anodized film 20a") are laminated in this order. The anodized film 20a in the aluminum support 12a is located closer to the image recording layer than the aluminum plate 18. In other words, the lithographic printing plate precursor according to the present disclosure preferably has at least an anodized film, an image recording layer, and an optional protective layer, in this order, on the aluminum plate.

[0387] -Anodized film- A preferred embodiment of the anodic oxide film 20a will now be described. The anodized film 20a is a film produced on the surface of the aluminum plate 18 by anodizing, and has extremely fine micropores 22a that are approximately perpendicular to the film surface and are uniformly distributed. The micropores 22a extend from the surface of the anodized film 20a on the image recording layer side (the surface of the anodized film 20a on the side opposite to the aluminum plate 18 side) along the thickness direction (toward the aluminum plate 18).

[0388] The average diameter (average opening diameter) of the micropores 22a in the anodized coating 20a at the surface of the anodized coating is preferably more than 10 nm and not more than 100 nm. From the viewpoint of a balance between printing durability, stain resistance, and image visibility, the average diameter is more preferably 15 nm to 60 nm, even more preferably 20 nm to 50 nm, and particularly preferably 25 nm to 40 nm. The diameter inside the pores may be wider or narrower than that at the surface layer. If the average diameter exceeds 10 nm, printing durability and image visibility are further improved, whereas if the average diameter is 100 nm or less, printing durability is further improved. The average diameter of the micropores 22a is calculated as the arithmetic mean value by observing N=4 images of the surface of the anodized film 20a using a field emission scanning electron microscope (FE-SEM) at a magnification of 150,000 times, measuring the diameters of 50 micropores present in an area of ​​400 nm x 600 nm in the four images obtained. When the shape of the micropores 22a is not circular, the equivalent circle diameter is used. The "equivalent circle diameter" is the diameter of a circle when the shape of the opening is assumed to be a circle having the same projected area as the projected area of ​​the opening.

[0389] The depth of the micropores 22a is not particularly limited, but is preferably from 10 nm to 3,000 nm, more preferably from 50 nm to 2,000 nm, and further preferably from 300 nm to 1,600 nm. The above depth is calculated by taking a photograph (150,000 times) of the cross section of the anodic oxide film 20a, measuring the depth of 25 or more micropores 22a, and averaging the measured value.

[0390] The shape of the micropores 22a is not particularly limited, and although it is generally straight (cylindrical) in Fig. 2, it may be a cone whose diameter decreases in the depth direction (thickness direction). The shape of the bottom of the micropores 22a is not particularly limited, and may be curved (convex) or flat.

[0391] The L of the surface of the aluminum support 12a on the image recording layer side (the surface of the anodized film 20a on the image recording layer side) * a * b * Lightness L in color system * The value is preferably from 70 to 100. Among these, from the viewpoint of a better balance between printing durability and image visibility, a value from 75 to 100 is preferred, and a value from 75 to 90 is more preferred. Above lightness L * The measurement is carried out using a color difference meter Spectro Eye manufactured by X-Rite Corporation.

[0392] In the support (1), the micropores are preferably composed of large-diameter pores extending from the surface of the anodized film to a depth of 10 nm to 1,000 nm, and small-diameter pores that communicate with the bottoms of the large-diameter pores and extend from the communicating positions to a depth of 20 nm to 2,000 nm, and the large-diameter pores have an average diameter of 15 nm to 100 nm at the surface of the anodized film, and the small-diameter pores have an average diameter of 13 nm or less at the communicating positions (hereinafter, the support according to the above support is also referred to as "support (2)"). FIG. 2 is a schematic cross-sectional view of an aluminum support 12a according to another embodiment different from that shown in FIG. In FIG. 2, the aluminum support 12b includes an aluminum plate 18 and an anodized film 20b having micropores 22b each composed of a large diameter portion 24 and a small diameter portion . Micropores 22b in anodized film 20b are composed of large diameter pores 24 extending from the surface of the anodized film to a depth of 10 nm to 1,000 nm (depth D: see Figure 2), and small diameter pores 26 that communicate with the bottom of large diameter pore 24 and extend from the communicating position to a depth of 20 nm to 2,000 nm. The large diameter hole portion 24 and the small diameter hole portion 26 will be described in detail below.

[0393] The average diameter of the large diameter pores 24 on the surface of the anodized film 20b is the same as the average diameter of the micropores 22a in the anodized film 20a on the surface of the anodized film, that is, more than 10 nm but not more than 100 nm, and the preferred range is also the same. The method for measuring the average diameter of the large diameter pores 24 on the surface of the anodized film 20b is the same as the method for measuring the average diameter of the micropores 22a in the anodized film 20a on the surface of the anodized film.

[0394] The bottoms of the large diameter holes 24 are located at a depth of 10 nm to 1,000 nm (hereinafter also referred to as depth D) from the surface of the anodized film. That is, the large diameter holes 24 are holes that extend from the surface of the anodized film to a position 10 nm to 1,000 nm in the depth direction (thickness direction). The depth is preferably 10 nm to 200 nm. The above depth is calculated by taking a photograph (150,000 times) of a cross section of the anodic oxide coating 20b, measuring the depths of 25 or more large diameter holes 24, and averaging the measured values.

[0395] The shape of the large diameter hole portion 24 is not particularly limited, and examples thereof include a substantially straight tube shape (substantially cylindrical shape) and a cone shape whose diameter decreases in the depth direction (thickness direction), with a substantially straight tube shape being preferred.

[0396] As shown in FIG. 2, the small diameter hole portion 26 is a hole portion that communicates with the bottom of the large diameter hole portion 24 and extends further in the depth direction (thickness direction) from the communicating position. The average diameter of the small diameter holes 26 at the communicating positions is preferably 13 nm or less. In particular, it is preferably 11 nm or less, and more preferably 10 nm or less. There is no particular lower limit, but it is often 5 nm or more.

[0397] The average diameter of the small pores 26 is obtained by observing the surface of the anodized film 20a with an FE-SEM at a magnification of 150,000 times, observing the diameters (diameters) of the micropores (small pores) present in the range of 400 nm × 600 nm in the four images obtained, and calculating the arithmetic average value. If the large pores are deep, the upper part of the anodized film 20b (the area where the large pores are located) may be cut (e.g., cut with argon gas) as necessary, and then the surface of the anodized film 20b may be observed with the FE-SEM to determine the average diameter of the small pores. If the shape of the small diameter hole 26 is not circular, the equivalent circle diameter is used. The "equivalent circle diameter" is the diameter of a circle when the shape of the opening is assumed to be a circle having the same projected area as the projected area of ​​the opening.

[0398] The bottoms of the small diameter holes 26 are located at positions extending 20 nm to 2,000 nm in the depth direction from the positions where the small diameter holes 26 communicate with the large diameter holes 24. In other words, the small diameter holes 26 are holes extending in the depth direction (thickness direction) from the positions where the small diameter holes 26 communicate with the large diameter holes 24, and the depth of the small diameter holes 26 is 20 nm to 2,000 nm. The depth is preferably 500 nm to 1,500 nm. The above depth is calculated by taking a photograph (50,000 times) of the cross section of the anodic oxide coating 20b, measuring the depth of at least 25 small diameter holes, and averaging the measured value.

[0399] The shape of the small diameter hole portion 26 is not particularly limited, and examples thereof include a substantially straight tube shape (substantially cylindrical shape) and a cone shape whose diameter decreases in the depth direction, with a substantially straight tube shape being preferred.

[0400] [Method of manufacturing aluminum support] As a method for producing an aluminum support in the present disclosure, for example, a production method in which the following steps are carried out in order is preferable. Surface roughening process: A process for roughening the surface of aluminum plates. Anodizing process: A process of anodizing a roughened aluminum plate. Pore ​​widening process: A process in which the aluminum plate having the anodized film obtained in the anodizing process is brought into contact with an acidic or alkaline aqueous solution to expand the diameter of the micropores in the anodized film. The procedure for each step is described in detail below.

[0401] (Surface roughening process) The surface roughening step is a step of roughening the surface of the aluminum plate, including electrochemical roughening. This step is preferably performed before the anodizing step described below, but may not be necessary if the surface of the aluminum plate already has a desired surface shape.

[0402] The surface roughening treatment may be performed by electrochemical surface roughening alone, or may be performed by combining electrochemical surface roughening treatment with mechanical surface roughening treatment and / or chemical surface roughening treatment. When mechanical graining and electrochemical graining are combined, it is preferable to carry out the electrochemical graining after the mechanical graining. The electrochemical graining treatment is preferably carried out in an aqueous solution mainly containing nitric acid or hydrochloric acid, using a direct current or an alternating current. The method for mechanically roughening the surface is not particularly limited, but may be, for example, the method described in JP-B-50-40047. The chemical roughening treatment is not particularly limited, and known methods can be used.

[0403] After the mechanical roughening treatment, the following chemical etching treatment is preferably carried out. The chemical etching treatment carried out after the mechanical graining treatment is carried out to smooth the uneven edges of the surface of the aluminum plate, prevent the ink from catching during printing, improve the stain resistance of the printing plate, and remove any unwanted material such as abrasive particles remaining on the surface. Examples of chemical etching treatments include etching with an acid and etching with an alkali, and a method that is particularly excellent in terms of etching efficiency is a chemical etching treatment using an aqueous alkali solution (hereinafter, also referred to as "alkaline etching treatment").

[0404] The alkaline agent used in the alkaline aqueous solution is not particularly limited, but examples thereof include caustic soda, caustic potash, sodium metasilicate, sodium carbonate, sodium aluminate, and sodium gluconate. The alkaline aqueous solution may contain aluminum ions. The concentration of the alkaline agent in the alkaline aqueous solution is preferably 0.01% by mass or more, more preferably 3% by mass or more, and is preferably 30% by mass or less.

[0405] When the alkaline etching treatment is carried out, it is preferable to carry out a chemical etching treatment (hereinafter also referred to as a "desmutting treatment") using a low-temperature acidic aqueous solution in order to remove products produced by the alkaline etching treatment. The acid used in the acidic aqueous solution is not particularly limited, but examples thereof include sulfuric acid, nitric acid, and hydrochloric acid. The temperature of the acidic aqueous solution is preferably 20°C to 80°C.

[0406] As the surface roughening step, a method in which the treatments shown in embodiment A or embodiment B are carried out in the order shown below is preferred.

[0407] -A form- (2) Chemical etching treatment using an alkaline aqueous solution (first alkaline etching treatment) (3) Chemical etching treatment using an acidic aqueous solution (first desmutting treatment) (4) Electrochemical roughening treatment using an aqueous solution mainly containing nitric acid (first electrochemical roughening treatment) (5) Chemical etching treatment using an alkaline aqueous solution (second alkaline etching treatment) (6) Chemical etching treatment using an acidic aqueous solution (second desmutting treatment) (7) Electrochemical roughening treatment in an aqueous solution mainly containing hydrochloric acid (second electrochemical roughening treatment) (8) Chemical etching treatment using an alkaline aqueous solution (third alkaline etching treatment) (9) Chemical etching treatment using an acidic aqueous solution (third desmutting treatment)

[0408] -B mode- (10) Chemical etching treatment using an alkaline aqueous solution (fourth alkaline etching treatment) (11) Chemical etching treatment using an acidic aqueous solution (fourth desmutting treatment) (12) Electrochemical roughening treatment using an aqueous solution mainly containing hydrochloric acid (third electrochemical roughening treatment) (13) Chemical etching treatment using an alkaline aqueous solution (fifth alkaline etching treatment) (14) Chemical etching treatment using an acidic aqueous solution (5th desmutting treatment)

[0409] Before the treatment (2) in the above embodiment A or before the treatment (10) in the above embodiment B, a mechanical graining treatment (1) may be carried out, if necessary.

[0410] The amount of aluminum plate dissolved in the first and fourth alkaline etching treatments was 0.5 g / m 2 ~30g / m 2 is preferred, and 1.0 g / m 2 ~20g / m 2 is more preferred.

[0411] The aqueous solution mainly containing nitric acid for use in the first electrochemical graining treatment in embodiment A includes an aqueous solution for use in electrochemical graining treatment using direct or alternating current, such as an aqueous solution obtained by adding aluminum nitrate, sodium nitrate, ammonium nitrate, or the like to a 1 to 100 g / L aqueous solution of nitric acid. The aqueous solution mainly containing hydrochloric acid used in the second electrochemical graining treatment in the embodiment A and the third electrochemical graining treatment in the embodiment B includes an aqueous solution used in an ordinary electrochemical graining treatment using direct or alternating current. For example, an aqueous solution obtained by adding 0 g / L to 30 g / L of sulfuric acid to an aqueous solution of hydrochloric acid of 1 g / L to 100 g / L may be included. Note that this solution may further include nitrate ions such as aluminum nitrate, sodium nitrate, and ammonium nitrate; or chloride ions such as aluminum chloride, sodium chloride, and ammonium chloride.

[0412] The AC power waveform for the electrochemical graining treatment may be a sine wave, a square wave, a trapezoidal wave, a triangular wave, etc. The frequency is preferably 0.1 Hz to 250 Hz. FIG. 3 is a graph showing an example of an alternating current waveform used in the electrochemical graining treatment. In FIG. 3, ta is the anode reaction time, tc is the cathode reaction time, tp is the time from 0 to the peak of the current, Ia is the current at the peak on the anode cycle side, Ic is the current at the peak on the cathode cycle side, AA is the current of the anode reaction of the aluminum plate, and CA is the current of the cathode reaction of the aluminum plate. In the trapezoidal wave, the time tp from 0 to the peak of the current is preferably 1 ms to 10 ms. The conditions of one cycle of the alternating current used for electrochemical surface roughening are preferably in the range of 1 to 20 for the ratio tc / ta of the anode reaction time ta of the aluminum plate to the cathode reaction time tc, 0.3 to 20 for the ratio Qc / Qa of the quantity of electricity when the aluminum plate is the anode to the quantity of electricity Qa when the aluminum plate is the anode, and 5 ms to 1,000 ms for the anode reaction time ta. The current density is 10 A / dm2 at the peak value of the trapezoidal wave for both the anode cycle side Ia and the cathode cycle side Ic.2 ~200A / dm 2 The ratio Ic / Ia is preferably 0.3 to 20. The total amount of electricity involved in the anodic reaction of the aluminum plate at the time when the electrochemical graining is completed is 25 C / dm 2 ~1,000C / dm 2 is preferred.

[0413] For electrochemical roughening using alternating current, the device shown in FIG. 4 can be used. FIG. 4 is a side view showing an example of a radial cell in electrochemical surface roughening treatment using an alternating current. In Fig. 4, 50 is a main electrolytic cell, 51 is an AC power source, 52 is a radial drum roller, 53a and 53b are main electrodes, 54 is an electrolyte supply port, 55 is an electrolyte, 56 is a slit, 57 is an electrolyte passage, 58 is an auxiliary anode, 60 is an auxiliary anode cell, and W is an aluminum plate. In Fig. 4, arrow A1 indicates the electrolyte supply direction, and arrow A2 indicates the electrolyte discharge direction. When two or more electrolytic cells are used, the electrolysis conditions may be the same or different. The aluminum sheet W is wound around a radial drum roller 52 immersed in a main electrolytic cell 50, and is electrolyzed by main electrodes 53a and 53b connected to an AC power source 51 during transportation. An electrolyte 55 is supplied from an electrolyte supply port 54 through a slit 56 to an electrolyte passage 57 between the radial drum roller 52 and the main electrodes 53a and 53b. The aluminum sheet W treated in the main electrolytic cell 50 is then electrolyzed in an auxiliary anode cell 60. In this auxiliary anode cell 60, an auxiliary anode 58 is disposed opposite the aluminum sheet W, and the electrolyte 55 is supplied so as to flow through the space between the auxiliary anode 58 and the aluminum sheet W.

[0414] The amount of aluminum plate dissolved in the second alkaline etching treatment is set to 1.0 g / m2 in order to facilitate the production of a desired printing plate precursor. 2 More than 2.0 g / m is preferable. 2 ~10g / m 2 is more preferred.

[0415] The amount of dissolution of the aluminum plate in the third alkaline etching treatment and the fourth alkaline etching treatment is set to 0.01 g / m so that a predetermined printing plate precursor can be easily produced. 2 ~0.8g / m 2 is preferred, and 0.05 g / m 2 ~0.3g / m 2 is more preferred.

[0416] In the chemical etching treatments (first to fifth desmutting treatments) using an acidic aqueous solution, an acidic aqueous solution containing phosphoric acid, nitric acid, sulfuric acid, chromic acid, hydrochloric acid, or a mixed acid containing two or more of these acids is suitably used. The acid concentration of the acidic aqueous solution is preferably 0.5% by mass to 60% by mass.

[0417] (Anodizing process) The procedure for the anodizing treatment step is not particularly limited as long as the above-mentioned micropores can be obtained, and known methods can be used. In the anodizing process, an aqueous solution of sulfuric acid, phosphoric acid, oxalic acid, etc. can be used as an electrolytic bath. For example, the concentration of sulfuric acid can be 100 g / L to 300 g / L. The conditions for the anodizing treatment are appropriately set depending on the electrolyte used. For example, the electrolyte temperature is 5°C to 70°C (preferably 10°C to 60°C), the current density is 0.5 A / dm 2 ~60A / dm 2 (Preferably 5A / dm 2 ~60A / dm 2 ), voltage 1V to 100V (preferably 5V to 50V), electrolysis time 1 second to 100 seconds (preferably 5 seconds to 60 seconds), and coating amount 0.1g / m 2 ~5g / m 2 (Preferably 0.2 g / m 2 ~3g / m 2 ) are mentioned.

[0418] (Pore Widening Treatment) The pore widening treatment is a treatment (pore diameter enlargement treatment) for enlarging the diameter (pore diameter) of the micropores present in the anodized film formed by the above-mentioned anodizing treatment process. The pore widening treatment can be carried out by contacting the aluminum plate obtained by the above-mentioned anodizing treatment step with an acid aqueous solution or an alkaline aqueous solution. The contacting method is not particularly limited, and examples thereof include a dipping method and a spraying method.

[0419] [Undercoat layer] The lithographic printing plate precursor according to the present disclosure preferably has an undercoat layer (sometimes called an intermediate layer) between the image recording layer and the support. The undercoat layer may contribute to improving developability while suppressing a decrease in printing durability by strengthening the adhesion between the support and the image recording layer in the exposed area and facilitating peeling of the image recording layer from the support in the unexposed area. In addition, the undercoat layer may also have the effect of functioning as a heat insulating layer in the case of infrared laser exposure, preventing a decrease in sensitivity due to the diffusion of heat generated by exposure to the support.

[0420] The compound used in the undercoat layer may be a low molecular weight compound or a polymer. The compound used in the undercoat layer may be, for example, a polymer having an adsorptive group and a hydrophilic group capable of being adsorbed to the support surface. The compound used in the undercoat layer is preferably a polymer having an adsorptive group and a hydrophilic group capable of being adsorbed to the support surface, and further having a crosslinkable group. The compounds used in the undercoat layer may be used in combination of two or more kinds, if necessary.

[0421] When the compound used in the undercoat layer is a polymer, it is preferably a copolymer of a monomer having an adsorptive group, a monomer having a hydrophilic group, and a monomer having a crosslinkable group. The adsorptive group capable of being adsorbed to the surface of the support is preferably a phenolic hydroxy group, a carboxy group, -PO3H2, -OPO3H2, -CONHSO2-, -SO2NHSO2-, or -COCH2COCH3. The hydrophilic group is preferably a sulfo group or a salt thereof, or a salt of a carboxy group. The crosslinkable group is preferably an acryl group, a methacryl group, an acrylamide group, a methacrylamide group, or an allyl group. The polymer may have a crosslinkable group introduced by salt formation between a polar substituent of the polymer and a compound having an ethylenically unsaturated bond and a substituent having an opposite charge to the polar substituent, or may further be copolymerized with a monomer other than the above-mentioned monomers, preferably a hydrophilic monomer.

[0422] Specific examples of compounds suitable for use in the undercoat layer include silane coupling agents having an addition-polymerizable ethylenic double bond reactive group as described in JP-A-10-282679 and phosphorus compounds having an ethylenic double bond reactive group as described in JP-A-2-304441. Also suitable for use are low-molecular or high-molecular compounds having a crosslinkable group (preferably an ethylenic unsaturated group), a functional group that interacts with the support surface, and a hydrophilic group as described in JP-A-2005-238816, JP-A-2005-125749, JP-A-2006-239867, and JP-A-2006-215263. More preferred examples include polymers having an adsorptive group, a hydrophilic group and a crosslinkable group capable of being adsorbed onto the surface of a support, as described in JP-A Nos. 2005-125749 and 2006-188038.

[0423] The content of the ethylenically unsaturated group in the polymer used in the undercoat layer is preferably from 0.1 mmol to 10.0 mmol, and more preferably from 0.2 mmol to 5.5 mmol, per 1 g of the polymer. The weight average molecular weight (Mw) of the polymer used in the undercoat layer is preferably 5,000 or more, and more preferably from 10,000 to 300,000.

[0424] -Hydrophilic compound- From the viewpoint of developability, the undercoat layer preferably contains a hydrophilic compound. The hydrophilic compound is not particularly limited, and any known hydrophilic compound used in an undercoat layer can be used. Preferred examples of the hydrophilic compound include phosphonic acids having an amino group such as carboxymethyl cellulose and dextrin, organic phosphonic acids, organic phosphoric acids, organic phosphinic acids, amino acids, and hydrochlorides of amines having a hydroxyl group. Preferred examples of the hydrophilic compound include compounds having an amino group or a functional group having polymerization-inhibiting ability and a group that interacts with the support surface (e.g., 1,4-diazabicyclo[2.2.2]octane (DABCO), 2,3,5,6-tetrahydroxy-p-quinone, chloranil, sulfophthalic acid, ethylenediaminetetraacetic acid (EDTA) or a salt thereof, hydroxyethylethylenediaminetriacetic acid or a salt thereof, dihydroxyethylethylenediaminediacetic acid or a salt thereof, hydroxyethyliminodiacetic acid or a salt thereof, etc.).

[0425] As the hydrophilic compound, from the viewpoint of scratch and stain suppression, it is preferable to use a hydroxycarboxylic acid or a salt thereof. From the viewpoint of scratch and stain suppression, the hydrophilic compound (preferably hydroxycarboxylic acid or its salt) is preferably contained in a layer on the aluminum support, not limited to the undercoat layer. The layer on the aluminum support is preferably a layer on the side on which the image recording layer is formed, and is preferably a layer in contact with the aluminum support. As the layer on the aluminum support, a layer in contact with the aluminum support is preferably an undercoat layer or an image recording layer. In addition, a layer other than the layer in contact with the aluminum support, for example, a protective layer or an image recording layer, may contain a hydrophilic compound (preferably a hydroxycarboxylic acid or a salt thereof). In the planographic printing plate precursor according to the present disclosure, from the viewpoint of scratch and stain suppression, an embodiment in which the image recording layer contains a hydroxycarboxylic acid or a salt thereof is also preferred. In another preferred embodiment of the lithographic printing plate precursor according to the present disclosure, the surface of the aluminum support on the image recording layer side is surface-treated with a composition (e.g., an aqueous solution) containing at least a hydroxycarboxylic acid or a salt thereof. In this embodiment, at least a portion of the treated hydroxycarboxylic acid or a salt thereof can be detected in a layer (e.g., an image recording layer or an undercoat layer) on the image recording layer side in contact with the aluminum support. By including a hydroxycarboxylic acid or a salt thereof in a layer that comes into contact with the aluminum support, such as an undercoat layer, the surface of the aluminum support on the image recording layer side can be made hydrophilic, and the contact angle with water on the surface of the aluminum support on the image recording layer side can be easily adjusted to 110° or less by a water drop method in the air. As a result, a lithographic printing plate precursor with excellent scratch and stain resistance can be obtained.

[0426] Here, hydroxycarboxylic acid is a general term for an organic compound having one or more carboxy groups and one or more hydroxy groups in one molecule, and is also called hydroxy acid, oxy acid, oxycarboxylic acid, or alcohol acid (see Iwanami Dictionary of Physics and Chemistry, 5th Edition, published by Iwanami Shoten Co., Ltd. (1998)). The above hydroxycarboxylic acid or a salt thereof is preferably represented by the following formula (HC): R HC (OH) mhc (COOM HC ) nhc Formula (HC) In formula (HC), R HC represents an organic group with mhc+nhc valence, and M HC each independently represents a hydrogen atom, an alkali metal, or an onium; mhc and nhc each independently represent an integer of 1 or more; when n is 2 or more, M may be the same or different.

[0427] In formula (HC), R HC Examples of the organic group having a valence of mhc+nhc represented by the formula (1) include a hydrocarbon group having a valence of mhc+nhc. The hydrocarbon group may have a substituent and / or a linking group. Examples of the hydrocarbon group include mhc+nhc valent groups derived from aliphatic hydrocarbons, such as alkylene groups, alkanetriyl groups, alkanetetrayl groups, alkanpentyl groups, alkenylene groups, alkenetriyl groups, alkenetetrayl groups, alkenepentyl groups, alkynylene groups, alkyntriyl groups, alkyntetrayl groups, and alkynpentyl groups, and mhc+nhc valent groups derived from aromatic hydrocarbons, such as arylene groups, arenetriyl groups, arenetetrayl groups, and arenepentyl groups. Substituents that can be introduced into the hydrocarbon group are substituents other than hydroxyl and carboxyl groups, and include alkyl groups, alkenyl groups, alkynyl groups, aralkyl groups, aryl groups, etc. Specific examples of the substituent include methyl groups, ethyl groups, propyl groups, butyl groups, pentyl groups, hexyl groups, heptyl groups, octyl groups, nonyl groups, decyl groups, undecyl groups, dodecyl groups, tridecyl groups, hexadecyl groups, octadecyl groups, eicosyl groups, isopropyl groups, isobutyl groups, s-butyl groups, t-butyl groups, isopentyl groups, neopentyl groups, 1-methylbutyl groups, isohexyl groups, 2-ethylhexyl groups, 2-methylhexyl groups, cyclohexyl groups, cyclopentyl groups, 2-norbornyl groups, methoxymethyl groups, methoxyethoxyethyl groups, allyloxymethyl groups, phenoxymethyl groups, acetyloxymethyl groups, benzoyloxymethyl groups, methyl ... Examples of the alkyl group include an alkyl group, a phenyl ... The linking group is composed of at least one atom selected from the group consisting of hydrogen atoms, carbon atoms, oxygen atoms, nitrogen atoms, sulfur atoms, and halogen atoms, and the number of atoms is preferably 1 to 50. Specific examples include alkylene groups, substituted alkylene groups, arylene groups, and substituted arylene groups, and these divalent groups may have a structure in which a plurality of them are linked together by any one of amide bonds, ether bonds, urethane bonds, urea bonds, and ester bonds.

[0428] M HC Examples of the alkali metal represented by the formula (I) include lithium, sodium, potassium, etc., and sodium is particularly preferred. M HC The onium represented by the formula (I) includes ammonium, phosphonium, sulfonium, etc., and ammonium is particularly preferred. Also, M HC From the viewpoint of scratch and stain suppression, is preferably an alkali metal or an onium, and more preferably an alkali metal. The total number of mhc and nhc is preferably 3 or more, more preferably 3 to 8, and even more preferably 4 to 6.

[0429] The hydroxycarboxylic acid or salt thereof preferably has a molecular weight of 600 or less, more preferably 500 or less, and particularly preferably 300 or less. In addition, the molecular weight is preferably 76 or more. Specific examples of the hydroxycarboxylic acid constituting the above hydroxycarboxylic acid or the salt of the above hydroxycarboxylic acid include gluconic acid, glycolic acid, lactic acid, tartronic acid, hydroxybutyric acid (2-hydroxybutyric acid, 3-hydroxybutyric acid, γ-hydroxybutyric acid, etc.), malic acid, tartaric acid, citramalic acid, citric acid, isocitric acid, leucinic acid, mevalonic acid, pantoic acid, ricinoleic acid, ricineraidic acid, cerebroside acid, quinic acid, shikimic acid, monohydroxybenzoic acid derivatives (salicylic acid, creosinoic acid, etc.), and the like. Examples of the benzoic acid derivatives include benzoic acid (homosalicylic acid, hydroxy(methyl)benzoic acid), vanillic acid, syringic acid, etc.), dihydroxybenzoic acid derivatives (pyrocatechuic acid, resorcylic acid, protocatechuic acid, gentisic acid, orselliic acid, etc.), trihydroxybenzoic acid derivatives (gallic acid, etc.), phenylacetic acid derivatives (mandelic acid, benzilic acid, atrolactic acid, etc.), hydrocinnamic acid derivatives (mellitic acid, phloretic acid, coumaric acid, umbellic acid, caffeic acid, ferulic acid, sinapic acid, cerebronic acid, carminic acid, etc.).

[0430] Among these, from the viewpoint of scratch and stain suppression, the hydroxycarboxylic acid or the hydroxycarboxylic acid constituting the salt of the hydroxycarboxylic acid is preferably a compound having two or more hydroxy groups, more preferably a compound having three or more hydroxy groups, even more preferably a compound having five or more hydroxy groups, and particularly preferably a compound having 5 to 8 hydroxy groups. As an acid having one carboxy group and two or more hydroxy groups, gluconic acid or shikimic acid is preferred. As an acid having two or more carboxy groups and one hydroxy group, citric acid or malic acid is preferable. As an acid having two or more carboxy groups and two or more hydroxy groups, tartaric acid is preferred. Among these, gluconic acid is particularly preferred as the hydroxycarboxylic acid.

[0431] The hydrophilic compounds may be used alone or in combination of two or more. When the undercoat layer contains a hydrophilic compound (preferably a hydroxycarboxylic acid or a salt thereof), the content of the hydrophilic compound (preferably a hydroxycarboxylic acid or a salt thereof) is preferably 0.01% by mass to 50% by mass, more preferably 0.1% by mass to 40% by mass, and particularly preferably 1.0% by mass to 30% by mass, relative to the total mass of the undercoat layer.

[0432] In addition to the above-mentioned compounds, the undercoat layer may contain a chelating agent, a secondary or tertiary amine, a polymerization inhibitor, etc. to prevent staining over time.

[0433] The subbing layer is coated on the aluminum support by known methods. The coating amount (solid content) of the undercoat layer is 0.1 mg / m 2 ~100mg / m 2 is preferred, and 1 mg / m 2 ~30mg / m 2 is more preferred.

[0434] <Method of preparing a lithographic printing plate and method of lithographic printing> The method for making a lithographic printing plate according to the present disclosure is not particularly limited, so long as it is a method for making a lithographic printing plate using a lithographic printing plate precursor according to the present disclosure. For example, the method for producing a lithographic printing plate according to the present disclosure preferably includes a step of exposing the lithographic printing plate precursor according to the present disclosure imagewise (hereinafter also referred to as an "imagewise exposure step"), and a step of supplying at least one selected from the group consisting of printing ink and fountain solution to the exposed lithographic printing plate precursor to remove the image recording layer in the non-image area on a printing press (hereinafter also referred to as an "on-press development processing step"). The above plate making method is hereinafter also referred to as an "on-press development method". The lithographic printing method according to the present disclosure is a method of making a lithographic printing plate using the lithographic printing plate precursor according to the present disclosure and printing, and preferably includes a step of exposing the lithographic printing plate precursor according to the present disclosure in an imagewise manner (hereinafter also referred to as an "imagewise exposure step"), a step of supplying at least one selected from the group consisting of printing ink and fountain solution to the lithographic printing plate precursor after exposure to remove the image recording layer in non-image areas on a printing press (hereinafter also referred to as an "on-press development processing step"), and a step of printing with the obtained lithographic printing plate (hereinafter also referred to as a "printing step"). It should be noted that, among the planographic printing plate precursors according to the present disclosure, the disposable plate precursor is subjected to a development processing step without undergoing an image exposure step. Hereinafter, preferred aspects of each step of the method for producing a lithographic printing plate according to the present disclosure and the lithographic printing method according to the present disclosure will be described in order. Note that the lithographic printing plate precursor according to the present disclosure can also be developed with a developer.

[0435] [Image Exposure Process] The step of imagewise exposing the lithographic printing plate precursor can be carried out in accordance with a general imagewise exposure operation for a lithographic printing plate precursor. Imagewise exposure is performed by laser exposure through a transparent original having a line image, a halftone image, or the like, or by laser light scanning using digital data. The wavelength of the light source used is preferably 700 nm to 1,400 nm. As a light source of 700 nm to 1,400 nm, a solid-state laser or a semiconductor laser that emits infrared rays is suitable. With regard to the infrared laser, the output is preferably 100 mW or more, the exposure time per pixel is preferably 20 μs or less, and the irradiation energy amount is 10 mJ / cm. 2 ~300mJ / cm 2 It is preferable to use a multi-beam laser device in order to shorten the exposure time. The exposure mechanism may be any of an internal drum type, an external drum type, a flatbed type, etc. Imagewise exposure can be performed by a conventional method using a plate setter or the like.

[0436] [On-press development processing process] The lithographic printing plate precursor after exposure can be developed by a conventional method. In the case of on-press development, when at least one selected from the group consisting of printing ink and fountain solution is supplied to the exposed lithographic printing plate precursor on the printing press, the image recording layer hardened by exposure forms a printing ink receptive area (i.e., image area) having a lipophilic surface in the exposed area of ​​the image recording layer. Meanwhile, in the unexposed area, the unhardened image recording layer is dissolved or dispersed and removed by the at least one selected from the group consisting of printing ink and fountain solution, exposing a hydrophilic surface in that area. As a result, the fountain solution adheres to the exposed hydrophilic surface, and the printing ink is applied to the image recording layer in the exposed area, thereby starting printing. Here, either dampening water or printing ink may be supplied first to the surface of the lithographic printing plate precursor, but it is preferable to supply dampening water first in order to allow the dampening water to penetrate and promote on-press developability.

[0437] <Printing process> Printing with the resulting lithographic printing plate can be carried out by a conventional method. A desired printing ink and, if necessary, dampening water are supplied to the lithographic printing plate, and printing can be carried out. The supply amounts of printing ink and dampening water are not particularly limited and may be appropriately set according to the desired printing. The method for supplying the printing ink and the dampening water to the lithographic printing plate is not particularly limited, and can be carried out by any known method. The recording medium to be printed is not particularly limited, and any known recording medium can be used as desired.

[0438] [Developer development process] In the method for producing a lithographic printing plate according to the present disclosure and the lithographic printing method according to the present disclosure, a step of developing the exposed lithographic printing plate precursor with a developer (developer development process) may be carried out instead of the on-press development process step. In the developer development process, for example, a developer having a pH of 2 to 11 is preferably supplied to remove the unexposed areas of the exposed lithographic printing plate precursor. The developer development process will be described below.

[0439] (Development process using developer) The developer used in the developer development process is not particularly limited, and any conventionally known developer may be used. As the developer, for example, a developer having a pH of 2 to 11 that may contain at least one compound selected from the group consisting of surfactants and water-soluble polymer compounds is preferably used.

[0440] If necessary, the developer may contain a water-soluble polymer compound, so that the development and gum solution treatment steps can be carried out simultaneously. Therefore, a post-rinsing step is not particularly required, and the development and gum solution treatment can be carried out in a single step, followed by a drying step. Therefore, as the development treatment using a developer, it is preferable to develop the exposed lithographic printing plate precursor with a developer having a pH of 2 to 11. After the development treatment, it is preferable to remove excess developer using a squeeze roller, and then dry the plate.

[0441] As described above, in the developer development treatment step of the method for producing a lithographic printing plate according to the present disclosure, it is preferable to carry out the development treatment and the gum solution treatment in a one-liquid, one-step process. Carrying out development and gum solution treatment in one liquid step means that development treatment and gum solution treatment are not carried out as separate steps, but are carried out in one step using one liquid.

[0442] The development process using a developer can be suitably carried out by an automatic developing processor having a developer supplying means and a developing means equipped with a rubbing member. An automatic developing processor using a rotating brush roll as the rubbing member is particularly preferred. The number of rotating brush rolls is preferably two or more. Furthermore, the automatic developing processor preferably includes a means for removing excess developer, such as a squeeze roller, and a drying means, such as a hot air device, downstream of the developing means. The automatic developing processor may also include a pre-heating means for heat-treating the exposed lithographic printing plate precursor, upstream of the developing means. Processing in such an automatic developing processor has the advantage that it is not necessary to deal with development residue derived from the water-soluble resin layer and / or the image recording layer, which is generated in the so-called on-machine development processing.

[0443] In the case of manual processing in the developer development processing step, suitable examples of development processing with a developer include a method in which a sponge, absorbent cotton, or the like is soaked in the aqueous solution, the entire plate surface is rubbed while processing, and then drying is performed after completion of processing. Suitable examples of immersion processing include a method in which the lithographic printing plate precursor is immersed in a vat, deep tank, or the like containing an aqueous solution for about 60 seconds, agitated, and then dried while rubbing with absorbent cotton, a sponge, or the like.

[0444] For the development treatment using a developer, it is preferable to use an apparatus with a simplified structure and process. For example, in an alkaline development process, the water-soluble resin layer is removed in a pre-rinsing step, then development is performed with a high pH alkaline developer, followed by removal of the alkali in a post-rinsing step, gumming in a gumming step, and drying in a drying step. In a simplified development process, development and gumming can be performed simultaneously using one solution. Therefore, the post-rinsing step and gumming step can be omitted, and it is preferable to perform development and gumming (gum solution treatment) using one solution, and then perform a drying step as necessary. Furthermore, it is preferable to simultaneously remove the water-soluble resin layer, develop, and gum the film using one solution without performing a pre-rinsing step. After development and gumming, it is preferable to remove excess developer using a squeeze roller, and then dry the film.

[0445] In the development treatment using a developer, the film may be immersed in the developer once or may be immersed two or more times. Among them, the method of immersing the film in the developer once or twice is preferred. The immersion may be performed by passing the exposed lithographic printing plate precursor through a developer tank filled with the developer, or by spraying the developer onto the plate surface of the exposed lithographic printing plate precursor using a spray or the like. In addition, even if the substrate is immersed in the developer more than twice, if the substrate is immersed in the same developer or in a developer and a developer in which the components of the image recording layer have been dissolved or dispersed by the development process (fatigue liquid), this is called development processing with one liquid (one-liquid processing).

[0446] In the development treatment using a developer, it is preferable to use a rubbing member, and it is preferable that a rubbing member such as a brush is provided in the development bath for removing the non-image areas of the image recording layer. The development process using a developer can be carried out according to a conventional method, preferably at a temperature of 0°C to 60°C, more preferably 15°C to 40°C, for example, by immersing the exposed lithographic printing plate precursor in the developer and rubbing it with a brush, or by pumping up the processing solution stored in an external tank and spraying it from a spray nozzle and rubbing it with a brush. These development processes can also be carried out multiple times in succession. For example, the developer stored in an external tank can be pumped up and sprayed from a spray nozzle and rubbing it with a brush, and then the developer can be sprayed again from a spray nozzle and rubbing it with a brush. When the development process is carried out using an automatic developing machine, the developer becomes fatigued due to an increase in the processing amount, so it is preferable to restore the processing capacity by using a replenisher or fresh developer.

[0447] For development processing using a developer, a gum coater or an automatic developing machine conventionally known for PS plates (presensitized plates) and CTP (computer to plate) can be used. When an automatic developing machine is used, any of the following methods can be applied: a method in which the developer stored in a developing tank or a developer stored in an external tank is pumped up with a pump and sprayed from a spray nozzle; a method in which the printing plate is immersed and transported in a tank filled with the developer using a submerged guide roll or the like; and a so-called disposable processing method in which only the amount of substantially unused developer required for each plate is supplied for processing. In any of these methods, a rubbing mechanism using a brush, a moulton, or the like is more preferable. For example, commercially available automatic processors (Clean Out Unit C85 / C125, Clean-Out Unit+ C85 / 120, FCF 85V, FCF 125V, FCF News (manufactured by Glunz & Jensen), Azura CX85, Azura CX125, Azura CX150 (manufactured by AGFA GRAPHICS) can be used. Also, a device in which the laser exposure section and the automatic processor section are integrated can be used.

[0448] (Developer) The developer used in the development treatment with the developer preferably has a pH of 2-11, more preferably 5-9, and further preferably 7-9. From the viewpoint of developability and dispersibility of the image recording layer, it is advantageous to set the pH value higher, but in terms of printability, particularly prevention of smearing, it is more effective to set the pH value lower. Here, the pH is a value measured at 25° C. using a pH meter (model number: HM-31, manufactured by DKK-TOA Corporation).

[0449] Examples of components contained in the developer used in the development treatment with the developer include a surfactant, a water-soluble polymer compound, a wetting agent, a preservative, a chelating compound, an antifoaming agent, an organic acid, an organic solvent, an inorganic acid, and an inorganic salt.

[0450] [Other steps] The method for preparing a lithographic printing plate according to the present disclosure and the lithographic printing method according to the present disclosure may include other known steps in addition to the steps described above, such as a step of heating the entire surface of the lithographic printing plate precursor at least either before exposure, during exposure, or between exposure and development, a plate inspection step of checking the position, orientation, etc. of the lithographic printing plate precursor before each step, and a confirmation step of checking the printed image after the development processing step. By carrying out a step of heating the entire surface of the lithographic printing plate precursor, the image forming reaction in the image recording layer is promoted, and advantages such as improved sensitivity and printing durability, and stabilization of sensitivity can be obtained. In the case of heating before development, it is preferable to carry out the heating under mild conditions of 150°C or less from the viewpoint of suppressing the effects of non-image areas. In the case of heating after development, it is preferable to use very strong conditions, and a heating range of, for example, 100°C to 500°C is preferable from the viewpoint of obtaining a sufficient image strengthening effect and suppressing problems such as deterioration of the support and thermal decomposition of the image areas. EXAMPLES

[0451] The present disclosure will be described in detail below with reference to examples, but the present disclosure is not limited thereto. In the present examples, "%" and "parts" mean "mass%" and "mass parts", respectively, unless otherwise specified. In the polymer compounds, unless otherwise specified, the molecular weight is the weight average molecular weight (Mw), and the ratio of the constituent repeating units is the molar percentage. The weight average molecular weight (Mw) is a value measured as a polystyrene equivalent value by gel permeation chromatography (GPC).

[0452] <Synthesis of resin particles R-1> The method for preparing the microgel resin particles R-1 is shown below. -Preparation of polyisocyanate compound (1)- To a suspension of 17.78 g (80 mmol) of isophorone diisocyanate and 7.35 g (20 mmol) of a polyhydric phenol compound (1) having the following structure in ethyl acetate (25.31 g), 43 mg of bismuth tris(2-ethylhexanoate) (Neostan U-600, manufactured by Nitto Kasei Co., Ltd.) was added and stirred. When the heat generation subsided, the reaction temperature was set to 50° C., and the mixture was stirred for 3 hours to obtain an ethyl acetate solution (50% by mass) of the polyhydric isocyanate compound (1).

[0453] [ka]

[0454] -Preparation of microgel- The following oil phase components and water phase components were mixed and emulsified for 10 minutes at 12,000 rpm using a homogenizer. The obtained emulsion was stirred at 45°C for 4 hours, and then 5.20 g of a 10% by mass aqueous solution of 1,8-diazabicyclo[5.4.0]undec-7-ene-octylate (U-CAT SA 102, manufactured by San-Apro Co., Ltd.) was added, stirred at room temperature for 30 minutes, and allowed to stand at 45°C for 24 hours. The solid content was adjusted to 20% by mass with distilled water to obtain an aqueous dispersion of microgel. The average particle size of the microgel was measured by a light scattering method and found to be 0.28 μm.

[0455] ~Oily phase components~ (Component 1) Ethyl acetate: 12.0g (Component 2) Trimethylolpropane (6 molar equivalents) and xylylene diisocyanate (18 molar equivalents) were added to methyl-terminated polyoxyethylene (1 molar equivalent, number of repeating oxyethylene units: 90) (50% by mass solution in ethyl acetate, manufactured by Mitsui Chemicals, Inc.): 3.76 g (Component 3) Polyisocyanate compound (1) (as a 50% by mass solution in ethyl acetate): 15.0 g (Component 4) 65% by weight solution of dipentaerythritol pentaacrylate (SR399, manufactured by Sartomer Corporation) in ethyl acetate: 11.54 g (Component 5) 10% ethyl acetate solution of sulfonate surfactant (Paionin A-41-C, Takemoto Oil Co., Ltd.): 4.42 g ~Aqueous phase components~ Distilled water: 46.87g

[0456] 15 g of acetone was added to 1 g of the obtained aqueous dispersion of the microgel, and the mixture was centrifuged (radius 15 cm, 14,500 rpm). The supernatant was measured by liquid chromatography (HPLC) to detect the amount of encapsulated monomer eluted. As described above, after three washings by adding acetone and centrifuging were repeated, the monomer encapsulated in the microgel was no longer detectable. After the above washing, the ethylenically unsaturated bond value (ie, C=C value) of the microgel which is the resin particle R-1 was 0.5 mmol / g, the median diameter was 210 nm, and the variation coefficient was 24%. In addition, the dispersibility of the resin particles R-1 was confirmed by the method described above, and it was found that the resin particles R-1 were particles having dispersibility in water and dispersibility in organic solvents.

[0457] <Synthesis of resin particles R-2> Into a 1000 ml four-neck flask, 10.0 g of the following compound B-1 (n=45) serving as a dispersion unit, 85.0 g of distilled water, and 240.0 g of n-propanol were added, and the mixture was heated and stirred at 70° C. under a nitrogen atmosphere. Next, a mixture of 20.0 g of compound A-1 below, 70.0 g of compound A-2 below, and 0.7 g of 2,2'-azobisisobutyronitrile that had been mixed in advance was added dropwise to the four-neck flask over a period of 2 hours. After the dropwise addition was completed, the reaction was continued for 5 hours, and then 0.5 g of 2,2'-azobisisobutyronitrile was added and the temperature was raised to 80° C. Then, 0.4 g of 2,2'-azobisisobutyronitrile was added every 6 hours, and the reaction was continued for a total of 19 hours. The reaction liquid was allowed to cool to room temperature (25° C.) to obtain a dispersion liquid of resin particles R-2 (solid content 23%).

[0458] [ka]

[0459] The resin particles R-2 had an ethylenically unsaturated bond value (that is, a C=C value) of 0 mmol / g, a median diameter of 150 nm, and a coefficient of variation of 23%. In addition, the dispersibility of the resin particles R-2 was confirmed by the method described above, and it was found that the resin particles R-2 were particles having dispersibility in water and dispersibility in organic solvents.

[0460] <Synthesis of resin particles R-3> 20 g of 2-butanone was weighed into a 500 mL three-neck flask and heated to 70° C. under a nitrogen stream. A mixed solution consisting of 12.6 g of Karenz-MOI (2-methacryloyloxyethyl isocyanate, Showa Denko K.K.), 15 g of the above compound A-1, 15.0 g of the above compound A-2, 10 g of the above compound B-1 (n=45), 5 g of methyl methacrylate, 0.6 g of V-65 (2,2′-azobis(2,4-dimethylvaleronitrile), Fujifilm Wako Pure Chemical Industries, Ltd.), and 44 g of 2-butanone was added dropwise to this reaction vessel over 2 hours. After the dropwise addition, the reaction was continued for another 2 hours. After 2 hours, 0.1 g of V-65 was added, the temperature was raised to 80° C., and the reaction was continued for another 2 hours. After the reaction was completed, the reaction solution was cooled to room temperature (25° C., hereinafter the same), and then 30 g of 2-butanone, 0.1 g of tetramethylpiperidine N-oxide, 43 g of SR399 (manufactured by Sartomer Corporation), and 0.2 g of Neostan U-600 (manufactured by Nitto Kasei Co., Ltd.) were added to the reaction solution, thoroughly stirred, and then heated to 70° C. After 6 hours, the reaction solution was cooled to room temperature. Next, 400 ml of water was added to a 1 L stainless steel beaker, and while stirring with a mechanical stirrer, the above reaction solution was added in its entirety at a rate of 1 ml / min. The supernatant was removed leaving the resulting white precipitate, which was then washed twice with water. Without going through a drying process, 200 ml of 0.1 N (mol / L) NaOH aqueous solution and 100 ml of pure water are added to a stainless steel beaker and stirred to obtain a white dispersion. The resulting dispersion was emulsified using a homogenizer at 18,000 rpm for 12 minutes to obtain a resin particle R-3 dispersion (solid content 21%).

[0461] The resin particles R-3 had an ethylenically unsaturated bond value (that is, a C=C value) of 4.0 mmol / g, a median diameter of 140 nm, and a coefficient of variation of 23%. In addition, when the dispersibility of the resin particles R-3 was confirmed by the method already described, it was found that the resin particles R-3 were particles having dispersibility in water and dispersibility in organic solvents.

[0462] <Synthesis of resin particles R-4> Resin particles R-4 were synthesized in the same manner as for resin particles R-3, except that the type and amount of the monomers used were appropriately changed. The resin particles R-4 had an ethylenically unsaturated bond value (that is, a C=C value) of 2.8 mmol / g, a median diameter of 140 nm, and a coefficient of variation of 27%. Furthermore, when the dispersibility of the resin particles R-4 was confirmed by the method already described, the resin particles R-4 were found to be water-dispersible.

[0463] <Synthesis of resin particles R-5> -Synthesis of precursor R-5'- A three-neck flask was charged with 20 parts of ion-exchanged water, 0.3 parts of Rongalite, 0.01 parts of disodium ethylenediaminetetraacetate, and 0.0025 parts of ferrous sulfate heptahydrate, and the mixture was stirred at 250 rpm at 60° C. in a nitrogen atmosphere. Next, 4.0 parts of the above compound A-1, 4.0 parts of the above compound A-2, 2.0 parts of the following compound A-3, 6.0 parts of the following compound A-4, 1.6 parts of methacrylic acid, 0.60 parts of sodium dodecylbenzenesulfonate, 0.58 parts of a peroxide polymerization initiator (manufactured by NOF Corporation, trade name PERBUTYL H), and 17 parts of ion-exchanged water were added and stirred at room temperature for 30 minutes to prepare an emulsion. 25% of the obtained emulsion was added to the three-neck flask over 30 minutes, and then the mixture was heated and stirred for 30 minutes, after which the remaining 75% was added dropwise over 2 hours. After the addition was completed, the mixture was heated and stirred for 2 hours. The reaction solution was allowed to cool to room temperature (25°C) to obtain a dispersion of Precursor R-5' (solid content 35%). The average particle size of Precursor R-5' was 120 nm.

[0464] -Synthesis of resin particles R-5- Into a three-neck flask, 12.5 parts of the dispersion of precursor R-5', 1.0 part of glycidyl acrylate, 0.2 parts of tetrabutylammonium bromide, and 30.0 parts of 1-methoxy-2-propanol were added and stirred for 12 hours at 90° C. The reaction solution was allowed to cool to room temperature (25° C.) to obtain a dispersion of resin particles R-5 (solid content 10%).

[0465] [ka]

[0466] The resin particles R-5 had an ethylenically unsaturated bond value (that is, a C=C value) of 0.93 mmol / g, a median diameter of 124 nm, and a coefficient of variation of 30%. In addition, when the dispersibility of the resin particles R-5 was confirmed by the method already described, it was found that the resin particles R-5 were particles having dispersibility in water and dispersibility in organic solvents.

[0467] <Synthesis of resin particles R-6> Resin particles R-6 were synthesized in the same manner as for resin particles R-5, except that the type and amount of the monomers used were appropriately changed. The resin particles R-6 had an ethylenically unsaturated bond value (that is, a C=C value) of 0.93 mmol / g, a median diameter of 95 nm, and a coefficient of variation of 19%. In addition, when the dispersibility of the resin particles R-6 was confirmed by the method already described, it was found that the resin particles R-6 were particles having dispersibility in water and dispersibility in organic solvents.

[0468] The details of the resin particles R-2 to R-6 are as follows. Here, structural units A-1' to A-6' and structural units B-1' to B-3' respectively represent structural units constituting resin particles R-2 to R-6, and the amount of structural units represents the content [mass %] of each structural unit contained in resin particles R-2 to R-6.

[0469] [ka]

[0470] <Synthesis of resin particles R-7> Resin particles R-7 were synthesized by the following method. -Synthesis of wall material A-

[0471] [ka]

[0472] Into a three-neck flask were placed 9.5 g of the above MR-200 (a compound represented by formula (Iso), n=0 to 10, manufactured by Tosoh Corporation), 0.5 g of the above PETA (pentaerythritol triacrylate, manufactured by Nippon Kayaku Co., Ltd., SR444), and 10 g of ethyl acetate, and the mixture was stirred at room temperature and then heated to 60°C. Next, 0.05 g of Neostan U-600 (manufactured by Nitto Kasei Co., Ltd.) was added to the three-neck flask and heated and stirred for 3 hours, after which it was cooled to room temperature to obtain wall material A (solid content 50% by mass).

[0473] -Synthesis of wall material B- In the following formula, Me represents a methyl group.

[0474] [ka]

[0475] To a three-neck flask, 5.0 g of the above Takenate D-110N (manufactured by Mitsui Chemicals, Inc.), 5.0 g of the above Uniox (registered trademark) M-4000 (manufactured by NOF Corporation), and 10 g of ethyl acetate were added and stirred at room temperature, and then the temperature was raised to 60°C. Next, 0.05 g of Neostan U-600 (Nitto Kasei Co., Ltd.) was added to the three-neck flask and heated and stirred for 3 hours. After that, it was cooled to room temperature to obtain wall material B (solid content 50% by mass).

[0476] -Synthesis of resin particles R-7- 0.45 g of Paionin A-41-C (manufactured by Takemoto Oil Co., Ltd.), 14.99 g of wall material A, 7.49 g of SR399E (dipentaerythritol pentaacrylate, manufactured by Sartomer Corporation), 3.78 g of wall material B, and 16.56 g of ethyl acetate were added to an aluminum cup and stirred at room temperature. Then, 46.89 g of pure water was added to the aluminum cup and stirred at 12,000 rpm for 12 minutes with a homogenizer, after which 16.64 g of pure water was further added, the temperature was raised to 45° C., and the mixture was heated and stirred for 4 hours. Thereafter, 5.17 g of a 10% aqueous solution of U-CAT SA 102 (manufactured by San-Apro Co., Ltd.) was added. Next, the container was placed in a thermostatic bath and aged for 48 hours to obtain a dispersion liquid of resin particles R-7 (solid content 20%). The ethylenically unsaturated bond value (that is, C=C value) of the resin particles R-7 was 0.50 mmol / g. The median diameter of the resin particles R-7 was 190 nm, and the coefficient of variation was 27.1%. The resins contained in the resin particles R-7 are shown below. In the resins below, the subscripts under each compound (monomer) and the subscripts to the right of the parentheses indicate the content ratio (mass ratio).

[0477] [ka]

[0478] <Synthesis of resin particles R-8> Resin particles R-8 were synthesized by the following method.

[0479] -Synthesis of wall material B- It was synthesized in the same manner as in the case of wall material B of resin particle R-7.

[0480] -Synthesis of wall material C-

[0481] [ka]

[0482] Into a three-neck flask were placed 2.375 g of the above compound a, 7.125 g of the above compound b, 0.5 g of the above compound c, and 10 g of ethyl acetate, and the mixture was stirred at room temperature and then heated to 60°C. Next, 0.05 g of Neostan U-600 (manufactured by Nitto Kasei Co., Ltd.) was added to the three-neck flask and heated and stirred for 3 hours, after which it was cooled to room temperature to obtain wall material C (solid content 50% by mass).

[0483] -Synthesis of wall material D-

[0484] [ka]

[0485] 5.0 g of the above Takenate D-110N (manufactured by Mitsui Chemicals, Inc.), 5.0 g of the above Unisafe PKA5014-TF (polypropylene glycol allyl ether, manufactured by NOF Corporation), and 10 g of ethyl acetate were added to a three-neck flask and stirred at room temperature, after which the temperature was raised to 60°C. Next, 0.05 g of Neostan U-600 (manufactured by Nitto Kasei Co., Ltd.) was added to the three-neck flask and heated and stirred for 3 hours, after which it was cooled to room temperature to obtain wall material D (solid content 50% by mass).

[0486] -Synthesis of resin particles R-8- To an aluminum cup, 0.45 g of Paionin A-41-C (manufactured by Takemoto Oil Co., Ltd.), 14.99 g of wall material C, 7.49 g of SR399E (manufactured by Sartomer), 1.89 g of wall material B, 1.89 g of wall material D, and 16.56 g of ethyl acetate were added and stirred at room temperature. Then, 46.89 g of pure water was added to the aluminum cup and stirred at 12,000 rpm for 12 minutes with a homogenizer, after which 16.64 g of pure water was further added, the temperature was raised to 45° C., and the mixture was heated and stirred for 4 hours. Thereafter, 5.17 g of a 10% aqueous solution of U-CAT SA 102 (manufactured by San-Apro Co., Ltd.) was added. The container was then placed in a thermostatic bath and aged for 48 hours to obtain a dispersion of resin particles R-8 (solid content 20%). The ethylenically unsaturated bond value (that is, C=C value) of the resin particles R-8 was 0.50 mmol / g. The median diameter of the resin particles R-8 was 220 nm, and the coefficient of variation was 29.3%. The resins contained in the resin particles R-8 are shown below. In the resins below, the subscripts under each compound (monomer) and the subscripts to the right of the parentheses indicate the content ratio (mass ratio).

[0487] [ka]

[0488] <Synthesis of resin particles R-9> Resin particles R-9 were synthesized by the following method.

[0489] -Synthesis of wall material C- It was synthesized in the same manner as wall material C in resin particle R-8.

[0490] -Synthesis of wall material D- It was synthesized in the same manner as wall material D in resin particle R-8.

[0491] -Synthesis of resin particles (20)- Into an aluminum cup, 0.45 g of Paionin A-41-C (manufactured by Takemoto Oil Co., Ltd.), 14.99 g of wall material C, 7.49 g of SR399E (manufactured by Sartomer Corporation), 3.78 g of wall material D, and 16.56 g of ethyl acetate were added and stirred at room temperature. Then, 46.89 g of pure water was added to the aluminum cup and stirred at 12,000 rpm for 12 minutes with a homogenizer, after which 16.64 g of pure water was further added, the temperature was raised to 45° C., and the mixture was heated and stirred for 4 hours. Thereafter, 5.17 g of a 10% aqueous solution of U-CAT SA 102 (manufactured by San-Apro Co., Ltd.) was added. Next, the container was placed in a thermostatic bath and aged for 48 hours to obtain a dispersion liquid of resin particles R-9 (solid content 20%). The ethylenically unsaturated bond value (that is, C=C value) of the resin particles R-9 was 0.50 mmol / g. The median diameter of the resin particles R-9 was 225 nm, and the coefficient of variation was 28.7%. The resins contained in the resin particles R-9 are shown below. In the resins below, the subscripts under each compound (monomer) and the subscripts to the right of the parentheses indicate the content ratio (mass ratio).

[0492] [ka]

[0493] <Synthesis of resin particles R-10> Resin particles R-10 were synthesized by the following method.

[0494] -Synthesis of wall material A- It was synthesized in the same manner as wall material A in resin particle R-7.

[0495] -Synthesis of wall material B- It was synthesized in the same manner as in the case of wall material B of resin particle R-7.

[0496] -Synthesis of wall material D- It was synthesized in the same manner as wall material D in resin particle R-8.

[0497] -Synthesis of resin particles R-10- To an aluminum cup, 0.45 g of Paionin A-41-C (manufactured by Takemoto Oil Co., Ltd.), 14.99 g of wall material A, 7.49 g of SR399E (manufactured by Sartomer Corporation), 1.89 g of wall material B, 1.89 g of wall material D, and 16.56 g of ethyl acetate were added and stirred at room temperature. Then, 46.89 g of pure water was added to the aluminum cup and stirred at 12,000 rpm for 12 minutes with a homogenizer, after which 16.64 g of pure water was further added, the temperature was raised to 45° C., and the mixture was heated and stirred for 4 hours. Then, 5.17 g of a 10% aqueous solution of U-CAT SA 102 (manufactured by San-Apro Co., Ltd.) was added. The container was then placed in a thermostatic bath and aged for 48 hours to obtain a dispersion of resin particles R-10 (solid content 20%). The ethylenically unsaturated bond value (that is, C=C value) of the resin particles R-10 was 0.50 mmol / g. The median diameter of the resin particles R-10 was 190 nm, and the coefficient of variation was 26.5%. The resins contained in the resin particles R-10 are shown below. In the following resins, the subscripts under each compound (monomer) and the subscripts in the brackets to the right of each compound indicate the content ratio (mass ratio). Additionally, Me indicates a methyl group.

[0498] [ka]

[0499] <Synthesis of resin particles R-11> Resin particles R-11 were synthesized by the following method.

[0500] -Synthesis of wall material A- It was synthesized in the same manner as wall material A in resin particle R-7.

[0501] -Synthesis of wall material D- It was synthesized in the same manner as wall material D in resin particle R-8.

[0502] -Synthesis of resin particles R-11- Into an aluminum cup, 0.45 g of Paionin A-41-C (manufactured by Takemoto Oil Co., Ltd.), 14.99 g of wall material A, 7.49 g of SR399E (manufactured by Sartomer Corporation), 3.78 g of wall material D, and 16.56 g of ethyl acetate were added and stirred at room temperature. Then, 46.89 g of pure water was added to the aluminum cup and stirred at 12,000 rpm for 12 minutes with a homogenizer, after which 16.64 g of pure water was further added, the temperature was raised to 45° C., and the mixture was heated and stirred for 4 hours. Thereafter, 5.17 g of a 10% aqueous solution of U-CAT SA 102 (manufactured by San-Apro Co., Ltd.) was added. Next, the container was placed in a thermostatic bath and aged for 48 hours to obtain a dispersion liquid (solid content 20%) of resin particles R-11. The ethylenically unsaturated bond value (that is, C=C value) of the resin particles R-11 was 0.50 mmol / g. The median diameter of the resin particles R-11 was 185 nm, and the coefficient of variation was 29.5%. The resins contained in the resin particles R-11 are shown below. In the resins below, the subscripts under each compound (monomer) and the subscripts to the right of the parentheses indicate the content ratio (mass ratio).

[0503] [ka]

[0504] <Synthesis of resin particles R-12> A microgel dispersion (solid content 20%) was obtained by the same method as in "Preparation of microgel" in the synthesis of resin particles R-1. The obtained microgel dispersion was used as a dispersion of resin particles R-12 (solid content 20%). The resin particles R-12 are resin particles containing a monomer, and the ethylenically unsaturated bond value (that is, C=C value) was 4.00 mmol / g. The median diameter of the resin particles R-12 was 200 nm, and the coefficient of variation was 30%.

[0505] <Synthesis of resin particles R-13> -Preparation of oil phase components- Polymeric MDI WANNATE (registered trademark) PM-200 (polyfunctional isocyanate compound: manufactured by Wanka Chemical): 6.66 g, Takenate (registered trademark) D-116N (50 mass% ethyl acetate solution of adduct (structure below) of trimethylolpropane (TMP), m-xylylene diisocyanate (XDI) and polyethylene glycol monomethyl ether (EO90): manufactured by Mitsui Chemicals, Inc.): 5.46 g, SR399 (dipentaerythritol pentaacrylate: manufactured by Sartomer Co., Ltd.) 65 mass% ethyl acetate solution: 11.24 g, ethyl acetate: 14.47 g, and Paionin A-41-C (manufactured by Takemoto Oil Co., Ltd.): 0.45 g were mixed and stirred at room temperature (25 ° C.) for 15 minutes to obtain an oil phase component.

[0506] [ka]

[0507] -Preparation of aqueous phase components- As the aqueous phase component, 47.2 g of distilled water was prepared.

[0508] - Microcapsule formation - The above-mentioned aqueous phase component was added to the above-mentioned oil phase component and mixed, and the resulting mixture was emulsified using a homogenizer at 12,000 rpm for 16 minutes to obtain an emulsion. To the resulting emulsion was added 16.8 g of distilled water, and the resulting liquid was stirred at room temperature for 180 minutes. Next, the liquid after stirring was heated to 45° C. and stirred for 5 hours while maintaining the liquid temperature at 45° C., thereby distilling off ethyl acetate from the liquid. The solid content was adjusted to 20% by mass with distilled water, to obtain an aqueous dispersion of resin particles R-13.

[0509] The resin particles R-13 are microcapsules encapsulating a monomer, and have an ethylenically unsaturated bond valence of 4.00 mmol / g. The median diameter of the resin particles R-13 was 165 nm, and the coefficient of variation was 32%.

[0510] <Preparation of Support A> (Aa) Alkaline etching treatment An aluminum plate was etched by spraying an aqueous solution of caustic soda with a caustic soda concentration of 26% by mass and an aluminum ion concentration of 6.5% by mass at a temperature of 70°C. The plate was then rinsed with water by spraying. The amount of dissolved aluminum on the surface to be subsequently subjected to electrochemical graining treatment was 5 g / m 2 It was.

[0511] (Ab) Desmutting treatment using an acidic aqueous solution (first desmutting treatment) Next, a desmutting treatment was carried out using an acidic aqueous solution. The acidic aqueous solution used in the desmutting treatment was an aqueous solution of 150 g / L sulfuric acid. The liquid temperature was 30°C. The acidic aqueous solution was sprayed onto the aluminum plate to carry out the desmutting treatment for 3 seconds. After that, a water rinsing treatment was carried out.

[0512] (Ac) Electrochemical roughening treatment Next, electrochemical graining treatment was performed using an electrolytic solution with a hydrochloric acid concentration of 14 g / L, an aluminum ion concentration of 13 g / L, and a sulfuric acid concentration of 3 g / L, using an alternating current. The temperature of the electrolytic solution was 30° C. The aluminum ion concentration was adjusted by adding aluminum chloride. The AC waveform is a sine wave with symmetrical positive and negative waveforms, the frequency is 50Hz, the anode reaction time and cathode reaction time in one AC cycle are 1:1, and the current density is 75A / dm at the peak current value of the AC waveform. 2 The total amount of electricity that the aluminum plate receives in the anode reaction is 450 C / dm 2 and electrolytic treatment is 112.5C / dm 2The test was carried out four times with a four second interval between each test. A carbon electrode was used as the counter electrode for the aluminum plate. After that, the plate was washed with water.

[0513] (Ad) Alkaline etching treatment After electrochemical graining, the aluminum plate was etched by spraying an aqueous solution of caustic soda with a caustic soda concentration of 5% by mass and an aluminum ion concentration of 0.5% by mass at 45°C. The amount of aluminum dissolved from the electrochemically grained surface was 0.2 g / m 2 Then, a water washing treatment was carried out.

[0514] (Ae) Desmutting treatment using an acidic aqueous solution Next, a desmutting treatment was carried out using an acidic aqueous solution. Specifically, the acidic aqueous solution was sprayed onto the aluminum plate and the desmutting treatment was carried out for 3 seconds. The acidic aqueous solution used for the desmutting treatment was an aqueous solution with a sulfuric acid concentration of 170 g / L and an aluminum ion concentration of 5 g / L. The liquid temperature was 30°C.

[0515] (Af) Anodizing Anodizing was performed using an anodizing treatment device 610 using direct current electrolysis having the structure shown in FIG. 5, to form an anodized film. The anodizing conditions were: sulfuric acid concentration of electrolyte 170 g / L, electrolyte temperature 50°C, current density 30 A / dm 2 , film amount 2.4g / m 2 It was. In an anodizing treatment apparatus 610 shown in Fig. 5, an aluminum sheet 616 is transported as indicated by an arrow in Fig. 5. In a power supply tank 612 in which an electrolytic solution 618 is stored, the aluminum sheet 616 is charged (+) by a power supply electrode 620. Then, in the power supply tank 612, the aluminum sheet 616 is transported upward by a roller 622, and its direction is changed downward by a nip roller 624, and then the aluminum sheet 616 is transported toward an electrolytic treatment tank 614 in which an electrolytic solution 626 is stored, and its direction is changed horizontally by a roller 628. Next, the aluminum sheet 616 is charged (-) by an electrolytic electrode 630, so that an anodized film is formed on the surface of the aluminum sheet 616, and the aluminum sheet 616 that leaves the electrolytic treatment tank 614 is transported to a subsequent process. In the anodizing device 610, a roller 622, a nip roller 624, and a roller 628 constitute a direction changing means, and the aluminum sheet 616 is transported in a mountain shape and an inverted U shape by the rollers 622, 624, and 628 in the space between the power supply tank 612 and the electrolytic treatment tank 614. The power supply electrode 620 and the electrolytic electrode 630 are connected to a DC power source 634.

[0516] (Ag)Pore-wide processing The anodized aluminum plate was immersed in an aqueous solution of caustic soda with a temperature of 40° C., a caustic soda concentration of 5 mass %, and an aluminum ion concentration of 0.5 mass % for 3 seconds to perform a pore widening treatment, and then washed with water by spraying.

[0517] The details of the obtained support A are summarized below. Support A: Average diameter of micropores on the anodized film surface: 12 nm, L of the anodized film surface * a * b * Lightness L in color system * Value: 81

[0518] <Preparation of Support B> An aluminum alloy plate of material 1S having a thickness of 0.3 mm was subjected to (Aa) mechanical roughening treatment (brush grain method) described in paragraph 0126 of JP2012-158022A to (Ai) desmutting treatment in an acidic aqueous solution described in paragraph 0134 of JP2012-158022A. Next, the conditions for each of the treatments from (Aj) the first stage anodizing treatment described in paragraph 0135 of JP 2012-158022 A to (Am) the third stage anodizing treatment described in paragraph 0138 of JP 2012-158022 A were appropriately adjusted to form an anodized coating, which was designated as Support B. In addition, water rinsing was carried out between all processing steps, and after the water rinsing, the liquid was removed with nip rollers.

[0519] The details of the obtained support are summarized below. Support B: L on the anodized film surface * a * b * Lightness L in color system * value: 83, average diameter of the large-diameter pores on the oxide film surface: 35 nm (depth 100 nm), average diameter of the small-diameter pores at the communicating positions in the micropores: 10 nm (depth 1,000 nm), ratio of the depth of the large-diameter pores to the average diameter of the large-diameter pores: 2.9

[0520] <Preparation of Support C> (Ca) Alkaline etching treatment An aluminum plate was etched by spraying an aqueous solution of caustic soda (sodium hydroxide) with a concentration of 26% by mass and an aluminum ion concentration of 6.5% by mass at 70°C using a spray tube. The plate was then rinsed with water using a spray. The amount of dissolved aluminum on the surface to be electrochemically roughened was 1.0 g / m2. 2 It was.

[0521] (Cb) Desmutting in an acidic aqueous solution (first desmutting treatment) Next, desmutting treatment was performed in an acidic aqueous solution. The acidic aqueous solution used in the desmutting treatment was an aqueous solution of 150 g / L sulfuric acid. The liquid temperature was 30°C. The desmutting solution was sprayed onto the material for 3 seconds. After that, a water washing treatment was performed.

[0522] (Cc) Electrochemical roughening treatment in hydrochloric acid solution Next, an electrolytic roughening treatment was performed using an alternating current and an electrolyte solution with a hydrochloric acid concentration of 14 g / L, an aluminum ion concentration of 13 g / L, and a sulfuric acid concentration of 3 g / L. The temperature of the electrolyte solution was 30°C. The aluminum ion concentration was adjusted by adding aluminum chloride. The waveform of the alternating current was a sine wave with symmetrical positive and negative waveforms, the frequency was 50 Hz, the anode reaction time and cathode reaction time in one cycle of the alternating current were 1:1, and the current density was 75 A / dm at the peak current value of the alternating current waveform. 2 The total amount of electricity that the aluminum plate receives in the anode reaction is 450 C / dm 2 The electrolytic treatment is 125C / dm 2 The test was carried out four times with a four second interval between each test. A carbon electrode was used as the counter electrode for the aluminum plate. After that, the plate was washed with water.

[0523] (Cd) Alkaline etching treatment The aluminum plate after electrochemical graining treatment was etched by spraying an aqueous solution of caustic soda with a caustic soda concentration of 5 mass% and an aluminum ion concentration of 0.5 mass% at 45°C using a spray tube. The amount of aluminum dissolved from the surface that had been subjected to electrochemical graining treatment was 0.2 g / m 2 Then, a water washing treatment was carried out.

[0524] (Ce) Desmutting in acidic aqueous solution Next, desmutting treatment was carried out in an acidic aqueous solution. The acidic aqueous solution used in the desmutting treatment was waste liquid (aluminum ions 5.0 g / L dissolved in sulfuric acid 170 g / L aqueous solution) generated in the anodizing treatment process. The liquid temperature was 30°C. The desmutting liquid was sprayed onto the material for 3 seconds.

[0525] (Cf) First stage anodizing The first stage of anodizing treatment was carried out using an anodizing treatment apparatus using direct current electrolysis with the structure shown in Figure 5. Specifically, anodizing treatment was carried out under the conditions in the "First anodizing treatment" column in Table 1 below, and an anodized film of a specified film volume was formed.

[0526] (Cg) Pore Wide Processing The anodized aluminum plate was immersed in an aqueous solution of caustic soda with a temperature of 35° C., a caustic soda concentration of 5 mass %, and an aluminum ion concentration of 0.5 mass % under the conditions shown in Table 1 below to carry out a pore widening treatment. Then, the aluminum plate was washed with water by spraying.

[0527] (Ch) Second stage anodizing The second stage of anodizing was carried out using an anodizing treatment device using direct current electrolysis with the structure shown in Figure 5. Specifically, anodizing was carried out under the conditions in the "second anodizing treatment" column in Table 1 below, and an anodized film of a specified film volume was formed.

[0528] Through the above treatments, Support C was obtained. For the obtained support C, the L of the micropore anodized film surface was * a * b * Lightness L in color system * , the average diameter of the large pores in the anodized film surface having micropores, the average diameter (nm) at the communicating positions of the small pores, the depth (nm) of the large pores and the small pores, and the pit density (density of micropores, unit: pits / μm 2 ) and the thickness (nm) of the anodized film from the bottom of the small hole to the surface of the aluminum plate are shown in Table 2. In Table 1, the film amount in the "first anodizing treatment" column and the film amount in the "second anodizing treatment" column indicate the film amount obtained in each treatment. The electrolyte used is an aqueous solution containing the liquid components in Table 1.

[0529] [Table 1]

[0530] [Table 2]

[0531] <Preparation of Support D> -Alkaline etching treatment- An aluminum plate was etched by spraying an aqueous solution of caustic soda with a caustic soda concentration of 26% by mass and an aluminum ion concentration of 6.5% by mass at a temperature of 55°C. The aluminum was then rinsed with water by spraying. The amount of aluminum dissolved on the surface to be subsequently subjected to electrochemical graining treatment was 3 g / m 2 It was.

[0532] - Desmutting treatment using an acidic aqueous solution (first desmutting treatment) - Next, a desmutting treatment was carried out using an acidic aqueous solution. The acidic aqueous solution used in the desmutting treatment was an aqueous solution of 170 g / L sulfuric acid. The liquid temperature was 30°C. The acidic aqueous solution was sprayed onto the aluminum plate to carry out the desmutting treatment for 3 seconds. After that, a water rinsing treatment was carried out.

[0533] -Electrochemical roughening treatment- Next, electrochemical roughening was performed using an electrolytic solution of hydrochloric acid and an alternating current. The temperature of the electrolytic solution was 40°C. The waveform of the alternating current was a sine wave with symmetrical positive and negative waveforms, and the frequency was 50Hz. The total amount of electricity that the aluminum plate was exposed to in the anode reaction was 300C / dm 2 A carbon electrode was used as the counter electrode for the aluminum plate. After that, the plate was washed with water.

[0534] -Alkaline etching treatment- After electrochemical graining, an aqueous solution of caustic soda with a caustic soda concentration of 5% by mass and an aluminum ion concentration of 0.5% by mass was sprayed at 35°C to an etching amount of 0.1 g / m 2The etching process was carried out as follows: Then, a water washing process was carried out.

[0535] - Desmutting treatment using an acidic aqueous solution - Next, a desmutting treatment was carried out using an acidic aqueous solution. The acidic aqueous solution used in the desmutting treatment was an aqueous solution of 170 g / L sulfuric acid. The liquid temperature was 30°C. The acidic aqueous solution was sprayed onto the aluminum plate to carry out the desmutting treatment for 3 seconds. After that, a water rinsing treatment was carried out.

[0536] -Anodizing- Using a direct current in a sulfuric acid solution of 170 g / L and a solution temperature of 40°C, the amount of anodized film is 3 g / m 2 The anodizing treatment was carried out so that

[0537] Through the above treatments, Support D was obtained.

[0538] Here, the average diameter of the micropores (average diameter of the large diameter pores and the small diameter pores) in each support is the average value obtained by observing the surfaces of the large diameter pores and the small diameter pores in N=4 images with an FE-SEM at a magnification of 150,000 times, measuring the diameters of the micropores (large diameter pores and small diameter pores) present in the range of 400 nm × 600 nm in the obtained four images. Note that when the large diameter pores are deep and the diameter of the small diameter pores is difficult to measure, or when measuring the enlarged diameter pores in the small diameter pores, the upper part of the anodized film was cut and various diameters were then obtained. The depth of the micropores (depth of the large diameter pores and the small diameter pores) in each support was determined by observing the cross section of the support (anodic oxide film) with a FE-SEM (observation of the depth of the large diameter pores: 150,000x, observation of the depth of the small diameter pores: 50,000x), measuring the depth of 25 randomly selected micropores in the obtained image, and averaging the measured values.

[0539] [Examples 1 to 25 and Comparative Examples 1 to 5] <Preparation of lithographic printing plate precursor> The lithographic printing plate precursors of Examples 1 to 25 and Comparative Examples 1 to 5 were each prepared by the following method.

[0540] <Formation of undercoat layer> On the supports shown in Tables 3 to 5, the undercoat layer coating solution (1) having the following composition was applied in a dry coating amount of 20 mg / m 2 The coating was then dried to form an undercoat layer.

[0541] - Undercoat layer coating solution (1) - Polymer (U-1) [structure below]: 0.18 parts Hydroxyethyliminodiacetic acid: 0.10 parts ·Wednesday: 61.4 parts

[0542] [ka]

[0543] <Formation of image recording layer> An image recording layer coating liquid was prepared according to the following image recording layer coating liquid (1) and Tables 3 to 5. The content of each compound shown in Tables 3 to 5 is the solid content (parts by mass). The image recording layer coating solution containing resin particles was prepared by mixing a photosensitive solution containing the components described in the following image recording layer coating solution (1) other than the resin particles and a dispersion containing each resin particle synthesized in the above synthesis example, and stirring the mixture immediately before coating to obtain the composition shown in Tables 3 to 5. On the undercoat layer, the image recording layer coating solution (1) was applied in a dry coating amount of 959 mg / m 2 The resulting solution was applied so as to become a layer having a thickness of 100 nm and then dried to form an image recording layer.

[0544] [Image recording layer coating liquid (1)] Resin particles (resin particles shown in Tables 3 to 5): the amount shown in Tables 3 to 5 Compound having an ethylenically unsaturated group (compounds listed in Tables 3 to 5): the amount listed in Tables 3 to 5 Electron-accepting polymerization initiator (compounds shown in Tables 3 to 5): the amount shown in Tables 3 to 5 Electron-donating polymerization initiator (compounds shown in Tables 3 to 5): the amount shown in Tables 3 to 5 Infrared absorber (compounds listed in Tables 3 to 5): the amount listed in Tables 3 to 5 Binder polymer (compounds shown in Tables 3 to 5): amounts shown in Tables 3 to 5 Color former (compounds shown in Tables 3 to 5): amounts shown in Tables 3 to 5 Oil sensitizer (compounds shown in Tables 3 to 5): the amount shown in Tables 3 to 5 Low molecular weight hydrophilic compound (compounds listed in Tables 3 to 5): the amount listed in Tables 3 to 5 The following mixed solvent: Amount that results in a solid content concentration of 7% by mass

[0545] -Mixing ratio of mixed solvent- 2-Butanone: 5 parts 1-Methoxy-2-propanol: 4 parts Distilled water: 5 parts

[0546] <Formation of protective layer> If necessary, a protective layer coating solution having the following composition is applied onto the image recording layer with a bar, and dried in an oven at 120° C. for 60 seconds to obtain a dry coating amount of 0.15 g / m 2 A protective layer of For the examples in which a protective layer was formed, the column for protective layer in Tables 3 to 5 states "Yes."

[0547] [Protective Layer Coating Solution] Inorganic layered compound dispersion (1) [see below]: 1.5g Polyvinyl alcohol 6% by weight aqueous solution: 0.55g (CKS50, manufactured by Nippon Synthetic Chemical Industry Co., Ltd., sulfonic acid modified, saponification degree 99 mol% or more, polymerization degree 300) Polyvinyl alcohol 6% by weight aqueous solution: 0.03g (PVA-405, Kuraray Co., Ltd., saponification degree 81.5 mol%, polymerization degree 500) 1% by weight aqueous solution of surfactant: 0.86g (Polyoxyethylene lauryl ether, Emalex (registered trademark) 710, manufactured by Nippon Emulsion Co., Ltd.) -Ion-exchanged water: 6.0g

[0548] [Preparation of Inorganic Layered Compound Dispersion (1)] 6.4 g of synthetic mica (Somasif ME-100, Co-op Chemical Co., Ltd.) was added to 193.6 g of ion-exchanged water and dispersed using a homogenizer until the average particle size (laser scattering method) became 3 μm. The aspect ratio of the obtained dispersed particles was 100 or more.

[0549] <Evaluation of lithographic printing plate precursors> The lithographic printing plate precursor prepared as described above was exposed (irradiation energy 110 mJ / cm) using a Kodak Magnus800 Quantum (platesetter) equipped with an infrared semiconductor laser under the conditions of an output of 27 W, an outer drum rotation speed of 450 rpm, and a resolution of 2,400 dpi (dots per inch, 1 inch is 2.54 cm). 2 (equivalent). The exposure image included a solid image and an AM screen (Amplitude Modulation Screen) 3% halftone dot chart.

[0550] (1)UV printing durability The exposed original plate obtained as described above was attached to the cylinder of a Heidelberg SX-74 printing machine with a size of 636 mm x 939 mm without development. A 100 L dampening water circulation tank with a built-in nonwoven fabric filter and temperature control device was connected to this printing machine. 80 L of dampening water containing 2.0 mass % of dampening water S-Z1 (manufactured by Fujifilm Corporation) was charged into the circulation device, and T&K UV OFS K-HS ink GE-M (manufactured by T&K TOKA Corporation), which is an ultraviolet-curable ink, was used as the printing ink. After supplying the dampening water and ink using the standard automatic printing start method, printing was performed on Tokubishi Art paper (ream weight: 76.5 kg, Mitsubishi Paper Mills Co., Ltd.) at a printing speed of 10,000 sheets per hour. As the number of prints increased, the image area gradually wore away, causing the ink density on the print to decrease. Printing durability was evaluated as the number of prints completed when the dot area ratio of the AM screen 3% dots on the print, measured with a Gretag densitometer (manufactured by GretagMacbeth), fell 1% from the measurement on the 500th print. Relative printing durability was evaluated, with 50,000 prints being taken as 100. The higher the value, the better the printing durability. Relative printing durability = (number of prints of the target lithographic printing plate precursor) / 50,000 x 100

[0551] (2) UV plate skipping A 0.4 mm diameter piano wire (ESCO Co., Ltd.) was attached to the halftone dots of the exposed original plate obtained as described above in a direction perpendicular to the rotation direction of the plate cylinder, and the plate was attached to the cylinder of a Heidelberg SX-74 printing press of 1920 size without development processing. A 100 L capacity dampening water circulation tank with a built-in nonwoven fabric filter and temperature control device was connected to this printing press. 80 L of 2.0% dampening water S-Z1 (FUJIFILM Corporation) was charged into the circulation device, and T&K UV OFS K-HS Sumi GE-M (T&K TOKA Corporation) was used as printing ink. After supplying dampening water and ink using the standard automatic printing start method, printing was performed on Tokubishi Art paper (Mitsubishi Paper Mills Co., Ltd., ream weight: 76.5 kg) at a printing speed of 10,000 sheets per hour. When the number of printed sheets reached 2,000, the piano wire was removed from...

Claims

1. an aluminum support and an image recording layer formed on the aluminum support; the image recording layer contains resin particles A having an ethylenically unsaturated group and a compound B other than the resin particles A having an ethylenically unsaturated group, and the image recording layer has an ethylenically unsaturated bond valence of 1.5 mmol / g or more; the resin particles A are particles containing a resin having an ethylenically unsaturated group, The lithographic printing plate precursor, wherein the resin having an ethylenically unsaturated group contained in the resin particles A is an addition polymerization type resin.

2. The lithographic printing plate precursor according to claim 1 , wherein the compound B comprises a compound having one or two ethylenically unsaturated groups.

3. the image recording layer further contains a polymerization initiator, The polymerization initiator contains an electron-accepting polymerization initiator, 3. The lithographic printing plate precursor according to claim 1, wherein the electron-accepting polymerization initiator has an organic anion having a Hansen solubility parameter δd of 16 or more, a δp of 16 to 32, and a δh of 60% or less of δp.

4. The lithographic printing plate precursor according to any one of claims 1 to 3, wherein the image recording layer has an ethylenically unsaturated bond valence of 2.1 mmol / g or more.

5. The lithographic printing plate precursor according to any one of claims 1 to 4, wherein compound B has an ethylenically unsaturated bond equivalent of 300 g / mol or less.

6. The lithographic printing plate precursor according to any one of claims 1 to 5, wherein compound B has a molecular weight of 2,500 or less.

7. the layer on the aluminum support comprises a hydroxycarboxylic acid or a salt thereof, The lithographic printing plate precursor according to any one of claims 1 to 6, wherein the hydroxycarboxylic acid or the salt thereof comprises a compound having two or more hydroxy groups.

8. the image recording layer further contains an electron-donating polymerization initiator and an infrared absorbing agent, The lithographic printing plate precursor according to any one of claims 1 to 7, wherein a value obtained by subtracting the HOMO of the electron-donating polymerization initiator from the HOMO of the infrared absorber is 0.70 eV or less.

9. the image recording layer further contains an infrared absorbing agent, The lithographic printing plate precursor according to any one of claims 1 to 8, wherein the infrared absorber has an organic anion having a Hansen solubility parameter δd of 16 or more, a δp of 16 to 32, and a δh of 60% or less of δp.

10. the image recording layer further contains a color former, The lithographic printing plate precursor according to any one of claims 1 to 9, wherein the color former is an acid color former.

11. the acid color former contains a leuco dye having a phthalide structure or a fluoran structure, The lithographic printing plate precursor according to claim 10, wherein the leuco dye having a phthalide structure or a fluoran structure is a compound represented by any one of the following formulas (Le-7) to (Le-9): 【Chemistry 1】 In formulas (Le-7) to (Le-9), X 1 ~X 4 each independently represents a hydrogen atom, a halogen atom, or a dialkylanilino group; Y 1 and Y 2 each independently represents C or N; Y 1 If N, then X 1 does not exist, and Y 2 If N, then X 4 does not exist, and Ra 1 ~Ra 4 each independently represents a hydrogen atom, an alkyl group, or an alkoxy group; Rb 1 ~Rb 4 Each independently represents an alkyl group or an aryl group; 1 and Rc 2 each independently represents an aryl group.

12. The lithographic printing plate precursor according to any one of claims 1 to 11, wherein the image recording layer further contains polyvinyl acetal as a binder resin.

13. The aluminum support has an aluminum plate and an anodized aluminum coating disposed on the aluminum plate, the anodized film is located closer to the image recording layer than the aluminum plate, The anodized film has micropores extending in a depth direction from the surface on the image recording layer side. death, the average diameter of the micropores on the surface of the anodized coating is greater than 10 nm and not greater than 100 nm; The L of the surface of the anodized film on the image recording layer side * a * b * Lightness L in color system * The lithographic printing plate precursor according to claim 1, wherein the value of

14. A step of imagewise exposing the lithographic printing plate precursor according to any one of claims 1 to 13; a step of supplying at least one selected from the group consisting of printing ink and fountain solution to the exposed lithographic printing plate precursor to remove the image recording layer in the non-image area on a printing press; A method for making a lithographic printing plate, comprising:

15. A step of imagewise exposing the lithographic printing plate precursor according to any one of claims 1 to 13; a step of supplying at least one selected from the group consisting of printing ink and fountain solution to the exposed lithographic printing plate precursor on a printing press to remove the image recording layer in the non-image area, thereby preparing a lithographic printing plate; A step of printing with the prepared lithographic printing plate; A lithographic printing method comprising:

Citation Information

Patent Citations

  • Photopolymerizable composition

    JP1988137226A

  • Manufacture of supporting member for photosensitive lithographic press

    JP1988202497A

  • (+-)-or (+)-1-(2-n-substituted aminoethyl)-1-methyl-7-methoxy-1,2,3,4-tetrahydronaphthalene and production thereof

    JP1989061447A

  • Method for forming image and image exposure apparatus

    JP2004341500A

  • Coloring photosensitive resin composition, pattern forming method, color filter manufacturing method, color filter and display device using the same

    JP2011227311A