Ceramic Electronic Components

By using BaTiO3 and (Ba1-xCa x )TiO3 (0.01≦x≦0.15) in the dielectric layer and cover/margin parts, the ceramic electronic components achieve enhanced high temperature reliability and moisture resistance, addressing the limitations of barium titanate.

JP7562935B2Active Publication Date: 2024-10-08SAMSUNG ELECTRO MECHANICS CO LTD

Patent Information

Application Number
JP2022210581
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-08
Filing Date
2022-12-27
Publication Date
2024-10-08
Estimated Expiration
2042-12-27

AI Technical Summary

Technical Problem

Existing ceramic electronic components face challenges with moisture resistance and reliability, particularly at high temperatures, due to the limitations of barium titanate (BaTiO3) which has a Curie temperature of 125°C and a sharp drop in dielectric constant above this temperature, and the use of barium titanate (BCT) can lead to reduced moisture resistance reliability.

Method used

Incorporating a dielectric layer made of BaTiO3 and (Ba1-xCa x )TiO3 (0.01≦x≦0.15) in the capacitor forming part, and using BaTiO3 for cover and margin parts to lower porosity, ensuring S1

Benefits of technology

The solution enhances the high temperature reliability and moisture resistance of ceramic electronic components by maintaining density and blocking moisture penetration paths, resulting in improved performance even at elevated temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562935000001
    Figure 0007562935000001
  • Figure 0007562935000002
    Figure 0007562935000002
  • Figure 0007562935000003
    Figure 0007562935000003
Patent Text Reader

Abstract

To provide a ceramic electronic component with excellent moisture resistance and high temperature reliability.SOLUTION: A ceramic electronic component includes a capacitor forming portion Ac and cover portions 112 and 113 disposed on both end surfaces of the capacitor forming portion in the first direction. A dielectric layer 111 in the forming portion includes BaTiO3 and (Ba1-xCax)TiO3 (0.01≤x≤0.15). The cover portion contains BaTiO3. In the cross section of the main body in the first and third directions, when the area ratio occupied by pores in the cover portion is S1, and the area ratio occupied by pores in the dielectric layer of the capacitor forming portion is S2, S1<S2 is satisfied.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ceramic electronic component. [Background technology]

[0002] Multi-layered ceramic capacitors (MLCCs), a type of ceramic electronic component, are chip-type capacitors that are mounted on printed circuit boards of various electronic products such as visual devices such as liquid crystal displays (LCDs) and plasma display panels (PDPs), computers, smartphones, and mobile phones, and serve to charge and discharge electricity.

[0003] In general, the dielectric material used in multilayer ceramic high-capacity capacitors is a ferroelectric material based on barium titanate (BaTiO3), which has a high dielectric constant at room temperature, a relatively small dissipation factor, and excellent insulation resistance characteristics. Recently, with the development of the electrical equipment industry, there has been a rapid demand for ceramic electronic components with excellent withstand voltage, capacitance temperature characteristics at high temperatures, and reliability. As a result, in addition to general high-capacity ceramic electronic components guaranteed up to 85°C according to the EIA standard, there is a demand for X7R ceramic electronic components guaranteed up to 125°C, X8R ceramic components guaranteed up to 150°C, and even X9M ceramic electronic components guaranteed up to 200°C.

[0004] However, barium titanate (BT, BaTiO3) has a Curie temperature of only 125°C, and there is a limit to the dielectric constant above that temperature. To solve this problem, barium titanate (BCT, (Ba 1-x Ca x A method to improve the temperature coefficient of capacitance (TCC) by using a base powder made of a mixture of titanium dioxide (TiO3) and barium titanate (BT, BaTiO3) is being researched.

[0005] However, when using a base powder containing a mixture of BCT and BT, the TCC can be improved, but the moisture resistance reliability may decrease. A solution to this problem is needed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] KR10-2006-0110603A Summary of the Invention [Problem to be solved by the invention]

[0007] One of several objects of the present invention is to provide a ceramic electronic component having excellent moisture resistance reliability.

[0008] One of several objects of the present invention is to provide a ceramic electronic component having excellent high-temperature reliability.

[0009] However, the scope of the present invention is not limited to the above, and can be more easily understood in the course of describing specific embodiments of the present invention. [Means for solving the problem]

[0010] A ceramic electronic component according to an embodiment of the present invention includes a dielectric layer, and a first internal electrode and a second internal electrode that are alternately arranged in the first direction with the dielectric layer interposed therebetween, a first surface and a second surface facing each other in the first direction, a third surface and a fourth surface facing each other in the second direction and connected to the first surface and the second surface, and a fifth surface and a sixth surface facing each other in the third direction and connected to the first surface to the fourth surface, a main body, a first external electrode disposed on the third surface and connected to the first internal electrode, and a second external electrode disposed on the fourth surface and connected to the second internal electrode. The main body includes a capacitance forming portion in which capacitance is formed including the first internal electrode and the second internal electrode, and a cover portion disposed on both end surfaces of the capacitance forming portion in the first direction. The dielectric layer of the capacitance forming portion includes BaTiO3 and (Ba 1-x Ca x )TiO3 (0.01 ≦ x ≦ 0.15), the cover portion includes BaTiO3, and when the area ratio occupied by pores in the cover portion is S1 and the area ratio occupied by pores in the dielectric layer of the capacitance forming portion is S2 in the cross sections of the main body in the first direction and the third direction, S1 < S2 can be satisfied.

[0011] A ceramic electronic component according to an embodiment of the present invention includes a dielectric layer, and a first internal electrode and a second internal electrode that are alternately arranged in the first direction with the dielectric layer interposed therebetween, a first surface and a second surface facing each other in the first direction, a third surface and a fourth surface facing each other in the second direction and connected to the first surface and the second surface, a fifth surface and a sixth surface facing each other in the third direction and connected to the first surface to the fourth surface, a main body, a first external electrode disposed on the third surface and connected to the first internal electrode, and a second external electrode disposed on the fourth surface and connected to the second internal electrode. The main body includes a capacitance forming portion in which capacitance is formed including the first internal electrode and the second internal electrode, a cover portion disposed on both end surfaces of the capacitance forming portion in the first direction, and a margin portion disposed on both end surfaces of the capacitance forming portion in the third direction. The dielectric layer of the capacitance forming portion includes BaTiO3 and (Ba 1-x Ca x)It contains TiO3 (0.01 ≤ x ≤ 0.15), the margin part contains BaTiO3, and when the area ratio occupied by pores in the margin part is S3 and the area ratio occupied by pores in the dielectric layer of the capacitance forming part is S2 in the cross-sections of the main body in the first direction and the third direction, S3 < S2 can be satisfied.

Advantages of the Invention

[0012] One of the several advantages of the present invention is that by including BaTiO3 and (Ba 1-x Ca x )TiO3 (0.01 ≤ x ≤ 0.15) in the dielectric layer of the capacitance forming part, the high-temperature reliability has been improved.

[0013] One of the several advantages of the present invention is that by including BaTiO3 in the cover part and / or the margin part to reduce the porosity, the moisture resistance reliability has been improved.

[0014] However, the various and beneficial advantages and effects of the present invention are not limited to the above-described content, and can be more easily understood in the process of describing the specific embodiments of the present invention.

Brief Description of the Drawings

[0015] [Fig. 1] It is a diagram schematically showing a perspective view of a ceramic electronic component according to an embodiment of the present invention. [Fig. 2] It is a diagram schematically showing a cross-sectional view taken along the line I-I' of FIG. 1. [Fig. 3] It is a diagram schematically showing a cross-sectional view taken along the line II-II' of FIG. 1. [Fig. 4] It is an enlarged view of the K1 region in FIG. 2. [Fig. 5] It is an enlarged view of the K2 region in FIG. 2. [Fig. 6] It is a diagram schematically showing a perspective view of a ceramic electronic component according to an embodiment of the present invention. [Fig. 7] It is a diagram schematically showing a cross-sectional view taken along the line III-III' of FIG. 6. [Fig. 8] FIG. 1 is a schematic perspective view of a ceramic electronic component according to an embodiment of the present invention. [Fig. 9] FIG. 9 is a schematic cross-sectional view taken along line IV-IV' in FIG. [Fig. 10] This is an image obtained by scanning a cross section of a cover part including BaTiO3 and (Ba1-xCax)TiO3 (0.01≦x≦0.15) using a scanning electron microscope. [Fig. 11] This is an image of a cross section of the cover containing BaTiO3, scanned with a scanning electron microscope. [Fig. 12] The image in Figure 10 was analyzed for porosity using an image analysis program. [Fig. 13] The image in Figure 11 was analyzed for porosity using an image analysis program. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, the embodiments of the present invention will be described with reference to specific embodiments and the accompanying drawings. However, the embodiments of the present invention can be modified into various other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those skilled in the art. Therefore, the shape and size of elements in the drawings may be exaggerated for clearer explanation, and elements indicated by the same reference numerals in the drawings are the same elements.

[0017] In addition, in the drawings, parts that are not relevant to the description are omitted in order to clearly explain the present invention, and the size and thickness of each component shown in the drawings are arbitrarily shown for convenience of explanation, so the present invention is not necessarily limited to those shown in the drawings. Components having the same function within the same concept will be described using the same reference numerals. Furthermore, throughout the specification, when a part is said to "include" a certain component, this does not mean that other components are excluded, but that the part may further include other components, unless otherwise specified to the contrary.

[0018] In the drawings, the first direction can be defined as the stacking direction or thickness T direction, the second direction can be defined as the length L direction, and the third direction can be defined as the width W direction.

[0019] Ceramic Electronic Components FIG. 1 is a schematic perspective view of a ceramic electronic component according to one embodiment of the present invention, FIG. 2 is a schematic cross-sectional view taken along line I-I' in FIG. 1, FIG. 3 is a schematic cross-sectional view taken along line II-II' in FIG. 1, FIG. 4 is an enlarged view of area K1 in FIG. 2, and FIG. 5 is an enlarged view of area K2 in FIG. 2.

[0020] A ceramic electronic component 100 according to one embodiment of the present invention will be described in detail below with reference to Figures 1 to 5. Also, a multi-layered ceramic capacitor (hereinafter referred to as "MLCC") will be described as an example of a ceramic electronic component, but the present invention is not limited thereto and can also be applied to various ceramic electronic components that use ceramic materials, such as inductors, piezoelectric elements, varistors, and thermistors.

[0021] A ceramic electronic component 100 according to an embodiment of the present invention includes a dielectric layer 111 and first internal electrodes 121 and second internal electrodes 122 arranged alternately in a first direction with the dielectric layer sandwiched therebetween, and includes a main body 110 including a first surface 1 and a second surface 2 facing the first direction, a third surface 3 and a fourth surface 4 connected to the first surface and the second surface and facing the second direction, and a fifth surface 5 and a sixth surface 6 connected to the first surface to the fourth surface and facing the third direction, a first external electrode 131 disposed on the third surface and connected to the first internal electrode, and a second external electrode 132 disposed on the fourth surface and connected to the second internal electrode, the main body including a capacitance forming portion Ac including the first internal electrode and the second internal electrode to form a capacitance, and cover portions 112, 113 disposed on both end surfaces in the first direction of the capacitance forming portion, and the dielectric layer 111 of the capacitance forming portion is made of BaTiO3 and (Ba 1-x Ca x)It contains TiO3 (0.01 ≦ x ≦ 0.15), the cover parts 112 and 113 contain BaTiO3, and in the cross-sections of the main body in the first direction and the third direction, when the area ratio occupied by pores P in the cover parts 112 and 113 is S1 and the area ratio occupied by pores in the dielectric layer of the capacitance forming part is S2, S1 < S2 can be satisfied.

[0022] The main body 110 may have a dielectric layer 111 and internal electrodes 121 and 122 laminated alternately.

[0023] There is no particular limitation on the specific shape of the main body 110, but as shown in the figure, the main body 110 can be formed in a hexahedron shape or a shape similar thereto. Due to the shrinkage of the ceramic powder contained in the main body 110 during the firing process, the main body 110 does not have a hexahedron shape with perfect straight lines, but can have a substantially hexahedron shape.

[0024] The main body 110 can have a first surface 1 and a second surface 2 facing each other in the first direction, a third surface 3 and a fourth surface 4 connected to the first surface and the second surface 2 and facing each other in the second direction, and a fifth surface 5 and a sixth surface 6 connected to the first surface 1 and the second surface 2, connected to the third surface and the fourth surface 4, and facing each other in the third direction.

[0025] The plurality of dielectric layers 111 forming the main body 110 are in a fired state, and the boundary between adjacent dielectric layers 111 can be integrated to such an extent that it is difficult to confirm without using a scanning electron microscope (SEM). The number of laminated dielectric layers does not need to be particularly limited and can be determined in consideration of the size of the ceramic electronic component. For example, the main body can be formed by laminating 400 or more dielectric layers.

[0026] The main body 110 can include a capacitance forming part Ac disposed inside the main body 110 and including a first internal electrode 121 and a second internal electrode 122 to form a capacitance, and cover parts 112 and 113 disposed on both end faces of the capacitance forming part Ac in the first direction.

[0027] The capacitance forming portion Ac is a portion that contributes to forming the capacitance of the capacitor, and may be formed by repeatedly stacking a plurality of first internal electrodes 121 and second internal electrodes 122 with a dielectric layer 111 sandwiched therebetween. The dielectric layer 111 of the capacitance forming portion Ac may be made of BaTiO3 and (Ba 1-x Ca x The dielectric layer 111 of the capacitance forming portion Ac may contain BaTiO3 powder and (Ba 1-x Ca x ) TiO3 (0.01≦x≦0.15) powder may be mixed with various ceramic additives, organic solvents, binders, dispersants, etc. to form the ceramic ceramic.

[0028] The cover parts 112 and 113 may include an upper cover part 112 disposed on an upper part of the capacitance forming part Ac in the first direction, and a lower cover part 113 disposed on a lower part of the capacitance forming part Ac in the first direction. The cover parts 112 and 113 may include barium titanate (BaTiO3). In addition, the cover parts 112 and 113 may include (Ba 1-x Ca x ) TiO3 may not be included. The covers 112, 113 may be formed using a raw material in which various ceramic additives, organic solvents, binders, dispersants, etc. are added to BaTiO3 powder.

[0029] Barium titanate (BT, BaTiO3) has a Curie temperature of only 125°C, and there is a limit to the dielectric constant above that temperature. To solve this problem, barium titanate with Ca in solid solution (BCT(Ba 1-x Ca x A method to improve the temperature coefficient of capacitance (TCC) by using a base powder made of a mixture of titanium dioxide (TiO3) and barium titanate (BT, BaTiO3) is being researched.

[0030] However, the cover that constitutes the exterior of the main body is made of barium titanate (BCT, (Ba1-x Ca x When a base powder made of a mixture of titanium dioxide (TiO3) and barium titanate (BT, BaTiO3) is used, pores may develop in the cover, reducing its density. The pores in the cover may act as a path for moisture to penetrate, reducing the moisture resistance reliability.

[0031] That is, the entire body 110 is made of barium titanate (BCT, (Ba 1-x Ca x When a base powder made of a mixture of titanium dioxide (TiO3) and barium titanate (BT, BaTiO3) was used, the TCC could be improved, but the moisture resistance reliability could be reduced.

[0032] Therefore, in one embodiment of the present invention, the cover portions 112 and 113 are made to contain BaTiO3 to reduce the porosity of the cover portions 112 and 113, and the dielectric layer 111 of the capacitance forming portion Ac is made to contain BaTiO3 and (Ba 1-x Ca x ) TiO3 (0.01≦x≦0.15) ensures high temperature reliability as well as moisture resistance.

[0033] The cover portions 112 and 113 may contain BaTiO3 as a main component, and may contain Mg, Dy, Y, Mn, Cr, V, Si, Al, Zr, etc. as secondary components. The dielectric layer 111 of the capacitance forming portion Ac may contain BaTiO3 and (Ba 1-x Ca x )TiO3 (0.01≦x≦0.15) as the main component, and Mg, Dy, Y, Mn, Cr, V, Si, Al, Zr, etc. as the subcomponents. Here, the meaning of the main component may mean that the number of moles of the remaining components excluding the main component is 30 moles or less per 100 moles of the main component. In the present invention, (Ba 1-x Ca x It can be said that it is preferable for the amount of Ca modification x of TiO3 to be in the range of 0.01 to 0.15.

[0034] BaTiO3 and (Ba 1-x Cax ) TiO3 (0.01≦x≦0.15) can be produced by a method such as a hydrothermal synthesis method, a solid phase method, a coprecipitation method, or a sol-gel method, but is not limited to these.

[0035] On the other hand, there is no need to particularly limit the thickness of the covers 112 and 113. However, in a ceramic electronic component having a size of 1608 (length×width, 1.6 mm×0.8 mm) or more, the thickness tc of the covers 112 and 113 may generally be 100 μm or more.

[0036] The average thickness tc of the cover parts 112, 113 may mean the size in the first direction, and may be the average value of the sizes in the first direction of the cover parts 112, 113 measured at five equally spaced points on the upper or lower part of the capacitance forming part Ac.

[0037] Moreover, margin portions 114 and 115 can be disposed on the side surfaces of the capacitance forming portion Ac.

[0038] The margin portions 114, 115 may include a first margin portion 114 disposed on the fifth surface 5 of the body 110 and a second margin portion 115 disposed on the sixth surface 6. That is, the margin portions 114, 115 may be disposed on both end surfaces of the ceramic body 110 in the width direction.

[0039] The margin portions 114, 115 may refer to the regions between both ends of the first internal electrode 121 and the second internal electrode 122 and the boundary surface of the body 110 in a cross-section of the body 110 cut in the width-thickness (WT) direction, as shown in FIG. 3.

[0040] The margins 114 and 115 essentially serve to prevent damage to the internal electrodes due to physical or chemical stress.

[0041] The margin portions 114 and 115 may be formed by applying a conductive paste to form internal electrodes except for the locations where the margin portions are formed on the ceramic green sheet.

[0042] Also, in order to suppress the step caused by the internal electrodes 121 and 122, after cutting so that the internal electrodes after lamination are exposed on the fifth surface 5 and the sixth surface 6 of the main body, a single dielectric layer or two or more dielectric layers may be laminated in the third direction (width direction) on both side surfaces of the capacitance forming portion Ac to form the margin portions 114 and 115.

[0043] The margin portions 114 and 115 may contain BaTiO3, or may contain both BaTiO3 and (Ba 1-x Ca x )TiO3 (0.01 ≦ x ≦ 0.15). The margin portions 114 and 115 can be composed of substantially the same composition as the cover portions 112 and 113, or can be composed of substantially the same composition as the capacitance forming portion Ac. When the margin portions 114 and 115 contain BaTiO3 as the main component, the moisture resistance reliability can be further improved.

[0044] In the cross-section of the main body 110 in the first direction and the third direction, when the area ratio occupied by the pores P in the cover portions 112 and 113 is S1, and the area ratio occupied by the pores P in the dielectric layer 111 of the capacitance forming portion Ac is S2, S1 < S2 can be satisfied. By satisfying S1 < S2, the density of the cover portions 112 and 113 can be improved to block the moisture penetration path, and the moisture resistance reliability can be improved.

[0045] In one embodiment, the above S1 can be 0.2 area% or less, and the above S2 can be more than 0.2 area% and 0.4 area% or less. When S1 exceeds 0.2 area%, the effect of improving the moisture resistance reliability may be insufficient. When S2 is 0.2 area% or less, the effect of improving the high-temperature reliability may be insufficient, and when S4 exceeds 0.4 area%, the dielectric constant may decrease or the breakdown voltage may decrease.

[0046] FIG. 10 shows the structure of BaTiO3 and (Ba 1-x Ca x 10 and 11 are images obtained by scanning a cross section of a cover part containing BaTiO3 (0.01≦x≦0.15) with a scanning electron microscope, and FIG. 11 is an image obtained by scanning a cross section of a cover part containing BaTiO3 with a scanning electron microscope. The size of the sample chips in FIG. 10 and FIG. 11 is 2012 (length×width, 2.0 mm×1.2 mm), and the thickness of the sample chips is 1.2 mm. Comparing FIG. 10 and FIG. 11, it is clear that the thickness of the sample chips containing BaTiO3 and (Ba 1-x Ca x 10, which contains both TiO3 (0.01≦x≦0.15), has more pores than Figure 11.

[0047] After obtaining images such as those shown in Figs. 10 and 11, S1 and S2 can analyze the proportion of pores using an image analysis program. For example, the proportion of pores can be analyzed using the ImageJ program. Figs. 12 and 13 show the images of Figs. 10 and 11, respectively, analyzed for the proportion of pores using the ImageJ program. As shown in Figs. 12 and 13, pores are represented in black, and the proportion of pores can be confirmed by measuring the area proportion occupied by black. In the case of Fig. 12, the proportion of pores was measured to be 0.38 area %, and in the case of Fig. 13, the proportion of pores was measured to be 0.09 area %.

[0048] In addition, the high-temperature reliability and moisture-resistant reliability of the sample chip of FIG. 10 and the sample chip of FIG. 11 were evaluated. As a result, it was confirmed that the high-temperature reliability was at a similar level, but the moisture-resistant reliability of the sample chip of FIG. 11 was superior.

[0049] For the moisture resistance reliability, a sample chip was judged to be "defective" if a voltage of 4 V was applied for 12 hours at a temperature of 85°C and a relative humidity of 85% and the insulation resistance value fell to 1 / 10 or less of the initial value. For the sample chips in Figure 10, 10 out of a total of 400 sample chips were judged to be "defective" in terms of moisture resistance reliability, while for the sample chips in Figure 11, 0 out of a total of 400 sample chips were judged to be "defective."

[0050] In one embodiment, the dielectric layer 111 of the capacitance forming portion Ac is (Ba 1-x Ca x ) TiO3 (0.01≦x≦0.15) may be contained in an amount of 30 mol to 300 mol per 100 mol of BaTiO3.

[0051] (Ba 1-x Ca x If the amount of )TiO3 (0.01≦x≦0.15) is less than 30 moles relative to 100 moles of BaTiO3, the effect of improving high temperature reliability may be insufficient, and if the amount of )TiO3 (0.01≦x≦0.15) is more than 300 moles relative to 100 moles of BaTiO3, the dielectric constant may decrease. 1-x Ca x ) TiO3 (0.01≦x≦0.15) can be contained in an amount of 80 mol or more and 220 mol or less per 100 mol of BaTiO3, and more preferably, in an amount of 100 mol or more and 150 mol or less per 100 mol of BaTiO3.

[0052] In one embodiment, (Ba 1-x Ca x When the first crystal grains G1 are crystal grains mainly composed of (BaTiO3 (0.01≦x≦0.15) and the second crystal grains G2 are crystal grains mainly composed of BaTiO3, the dielectric layer 111 of the capacitance forming portion includes the first crystal grains G1 and the second crystal grains G2, and the cover portions 112 and 113 include the second crystal grains G2. 1-x Ca x )TiO3 (0.01≦x≦0.15), the first crystal grains G1 are not included. Here, the main component can mean that the number of moles of the remaining components excluding the main component is 30 moles or less per 100 moles of the main component.

[0053] In one embodiment, the average size of the first crystal grains G1 can be larger than the average size of the second crystal grains G2. Since the BCT powder is larger than the BT powder, the average size of the first crystal grains G1 can be larger than the average size of the second crystal grains G2. 1-x Ca xThe size of the first crystal grains G1, which are crystal grains mainly composed of TiO3 (0.01≦x≦0.15), may be larger than the size of the second crystal grains G2, and pores P may be formed due to this size difference.

[0054] In one embodiment, the first crystal grains G1 may have an average size of 210 to 340 nm, and the second crystal grains G2 may have an average size of 160 to 290 nm.

[0055] The grain size of the first crystal grain G1 and the second crystal grain G2 can be determined by drawing a straight line from one point to another point on the grain boundary of the crystal grain, with the line having the maximum value being the major axis and the line perpendicular to the major axis having the maximum value being the minor axis, and the average value of the major axis and minor axis can be determined as the grain size. The average value of the sizes of 500 or more crystal grains can be determined as the average grain size of the dielectric crystal grains.

[0056] The grain sizes of the first crystal grains G1 and the second crystal grains G2 can be measured from an image obtained by scanning a cross section of the body 110 in the width and thickness direction (WT) with a scanning electron microscope (SEM). At this time, the magnification can be varied according to the size of the crystal grains, and the magnification can be adjusted so that the sizes of 500 or more crystal grains can be measured. However, it is not necessary to adjust the magnification so that one image contains 500 or more crystal grains, and the grain sizes can be measured from multiple images by adjusting the magnification so that the total number of crystal grains contained in multiple images is 500 or more.

[0057] The average thickness td of the dielectric layer does not need to be particularly limited, and may be, for example, 0.5 to 3 μm.

[0058] The average thickness td of the dielectric layer 111 may refer to the average thickness of the dielectric layer 111 disposed between the first internal electrode 121 and the second internal electrode 122 .

[0059] The average thickness td of the dielectric layer 111 can be measured by scanning an image of a cross section of the body 110 in the length and thickness direction (LT) using a scanning electron microscope (SEM) with a magnification of 10,000. More specifically, in the scanned image, the thickness of one dielectric layer can be measured at 30 equally spaced points in the length direction, and an average value can be calculated. The 30 equally spaced points can be designated as the capacitance forming portion Ac. Furthermore, if such an average value measurement is extended to 10 dielectric layers and an average value is measured, the average thickness of the dielectric layer can be further generalized.

[0060] The internal electrodes 121, 122 may include a first internal electrode 121 and a second internal electrode 122. The first internal electrodes 121 and the second internal electrodes 122 are alternately arranged to face each other with the dielectric layer 111 constituting the body 110 therebetween, and may be exposed to a third surface 3 and a fourth surface 4 of the body 110, respectively.

[0061] 3, the first internal electrode 121 may be spaced apart from the fourth surface 4 and exposed through the third surface 3, and the second internal electrode 122 may be spaced apart from the third surface 3 and exposed through the fourth surface 4. A first external electrode 131 may be disposed on the third surface 3 of the body and connected to the first internal electrode 121, and a second external electrode 132 may be disposed on the fourth surface 4 of the body and connected to the second internal electrode 122.

[0062] That is, the first internal electrode 121 is not connected to the second external electrode 132 but is connected to the first external electrode 131, and the second internal electrode 122 is not connected to the first external electrode 131 but is connected to the second external electrode 132. Therefore, the first internal electrode 121 may be formed at a certain distance apart on the fourth surface 4, and the second internal electrode 122 may be formed at a certain distance apart on the third surface 3. In addition, the first internal electrode 121 and the second internal electrode 122 may be disposed at a certain distance apart from the fifth and sixth surfaces of the body 110.

[0063] At this time, the first internal electrode 121 and the second internal electrode 122 can be electrically isolated from each other by the dielectric layer 111 disposed therebetween.

[0064] The body 110 may be formed by alternately stacking ceramic green sheets on which the first internal electrodes 121 are printed and ceramic green sheets on which the second internal electrodes 122 are printed, and then firing the stacked ceramic green sheets.

[0065] There is no particular limitation on the material forming the internal electrodes 121 and 122, and any material having excellent electrical conductivity may be used. For example, the internal electrodes 121 and 122 may include one or more of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof.

[0066] The internal electrodes 121 and 122 may be formed by printing a conductive paste for internal electrodes, which contains at least one of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof, on a ceramic green sheet. The method for printing the conductive paste for internal electrodes may be a screen printing method or a gravure printing method, but the present invention is not limited thereto.

[0067] There is no need to particularly limit the average thickness te of the internal electrodes 121, 122. For example, the average thickness te of the internal electrodes 121, 122 may be 0.6 μm or more and 2.0 μm or less.

[0068] The average thickness te of the internal electrodes 121, 122 may be measured by scanning an image of a cross section of the body 110 in the length and thickness direction (LT) using a scanning electron microscope (SEM) with a magnification of 10,000. More specifically, in the scanned image, the thickness of one internal electrode may be measured at 30 equally spaced points in the length direction, and an average value may be calculated. The 30 equally spaced points may be designated as the capacitance forming portion Ac. Furthermore, if such an average value measurement is extended to 10 internal electrodes and an average value is measured, the average thickness of the internal electrodes may be further generalized.

[0069] The external electrodes 131 , 132 may be disposed on the third surface 3 and the fourth surface 4 of the body 110 .

[0070] The external electrodes 131, 132 may include a first external electrode 131 and a second external electrode 132 disposed on the third surface 3 and the fourth surface 4 of the body 110, respectively, and connected to the first internal electrode 121 and the second internal electrode 122, respectively.

[0071] Referring to FIG. 1, the external electrodes 131 and 132 may be disposed to cover both end surfaces of the side margin portions 114 and 115 in the second direction.

[0072] In this embodiment, a structure in which the ceramic electronic component 100 has two external electrodes 131, 132 is described, but the number and shapes of the external electrodes 131, 132 can be changed depending on the configuration of the internal electrodes 121, 122 and other purposes.

[0073] Meanwhile, the external electrodes 131 and 132 may be formed using any material having electrical conductivity, such as a metal, and the specific material may be determined taking into consideration electrical characteristics, structural stability, etc., and may further have a multi-layer structure.

[0074] For example, the external electrodes 131 and 132 may include electrode layers 131a and 132a disposed on the body 110 and plating layers 131b and 132b formed on the electrode layers 131a and 132a.

[0075] As a more specific example of the electrode layers 131a and 132a, the electrode layers 131a and 132a may be fired electrodes including a conductive metal and glass, or may be resin-based electrodes including a conductive metal and resin.

[0076] The electrode layers 131a and 132a may be formed by sequentially forming a fired electrode and a resin-based electrode on the main body. The electrode layers 131a and 132a may be formed by transferring a sheet containing a conductive metal onto the main body, or by transferring a sheet containing a conductive metal onto a fired electrode.

[0077] The conductive metal contained in the electrode layers 131a and 132a may be, but is not limited to, a material having excellent electrical conductivity. For example, the conductive metal may be one or more of nickel (Ni), copper (Cu), and alloys thereof.

[0078] The plating layers 131b and 132b serve to improve mounting characteristics. The type of the plating layers 131b and 132b is not particularly limited, and may be a plating layer containing one or more of Ni, Sn, Pd, and alloys thereof, or may be formed of multiple layers.

[0079] As a more specific example of the plating layers 131b, 132b, the plating layers 131b, 132b may be Ni plating layers or Sn plating layers, and may be in a form in which a Ni plating layer and a Sn plating layer are sequentially formed on the electrode layers 131a, 132a, or in a form in which a Sn plating layer, a Ni plating layer and a Sn plating layer are sequentially formed. The plating layers 131b, 132b may also include a plurality of Ni plating layers and / or a plurality of Sn plating layers.

[0080] The size of the ceramic electronic component 100 does not need to be particularly limited.

[0081] However, the present invention can be suitably applied to ceramic electronic components 100 having a size of 1608 (length×width, 1.6 mm×0.8 mm) or more, which is the size of products that particularly require high-temperature reliability.

[0082] Taking into consideration manufacturing errors, the size of the external electrodes, etc., this can be suitably applied to ceramic electronic component 100 having a length of 1.54 mm or more and a width of 0.72 mm or more. Here, the length of ceramic electronic component 100 may refer to the maximum size of ceramic electronic component 100 in the second direction, and the width of ceramic electronic component 100 may refer to the maximum size of ceramic electronic component 100 in the third direction.

[0083] FIG. 6 is a diagram that roughly shows a perspective view of a ceramic electronic component 100' according to one embodiment of the present invention, and FIG. 7 is a diagram that roughly shows a cross-sectional view taken along line III-III' in FIG.

[0084] Hereinafter, a ceramic electronic component 100' according to one embodiment of the present invention will be described in detail with reference to Figures 6 and 7. However, content that overlaps with the above description will be omitted.

[0085] A ceramic electronic component 100' according to an embodiment of the present invention includes a dielectric layer 111, and a first internal electrode 121 and a second internal electrode 122 that are alternately arranged in a first direction with the dielectric layer interposed therebetween. The ceramic electronic component 100' includes a first surface 1 and a second surface 2 that face each other in the first direction, a third surface 3 and a fourth surface 4 that are connected to the first surface and the second surface and face each other in a second direction, and a fifth surface 5 and a sixth surface 6 that are connected to the first surface to the fourth surface and face each other in a third direction. The ceramic electronic component 100' also includes a main body 110', a first external electrode 131 that is disposed on the third surface and connected to the first internal electrode, and a second external electrode 132 that is disposed on the fourth surface and connected to the second internal electrode. The main body includes a capacitance forming portion Ac that includes the first internal electrode and the second internal electrode and forms a capacitance, cover portions 112', 113' that are disposed on both end faces of the capacitance forming portion in the first direction, and margin portions 114', 115' that are disposed on both end faces of the capacitance forming portion in the third direction. The dielectric layer 111 of the capacitance forming portion includes BaTiO3 and (Ba 1-x Ca x )TiO3 (0.01 ≦ x ≦ 0.15). The margin portions 114', 115' include BaTiO3. When the area ratio occupied by pores P in the margin portions 114', 115' is S3 and the area ratio occupied by pores P in the dielectric layer 111 of the capacitance forming portion Ac is S2 in cross-sections of the main body in the first and third directions, S3 < S2 can be satisfied.

[0086] When the margin portions 114', 115' that constitute the exterior of the main body are formed by applying a base material powder in which barium calcium titanate (BCT, (Ba 1-x Ca x )TiO3) and barium titanate (BT, BaTiO3) are mixed, there is a possibility that the number of pores in the margin portions 114', 115' increases and the density decreases. The pores in the margin portions 114', 115' may act as a moisture penetration path, and there is a possibility that the moisture resistance reliability decreases.

[0087] That is, the entire main body 110' is made of barium calcium titanate (BCT, (Ba 1-x Ca x)When forming by applying a base material powder in which TiO3 and barium titanate (BT, BaTiO3) are mixed, although the TCC can be improved, the moisture resistance reliability may decrease.

[0088] Therefore, in one embodiment of the present invention, BaTiO3 is included in the margin portions 114' and 115' to reduce the porosity of the margin portions 114' and 115', and BaTiO3 and (Ba 1-x Ca x )TiO3 (0.01 ≦ x ≦ 0.15) are included in the dielectric layer 111 of the capacitance forming portion Ac, thereby ensuring high-temperature reliability and moisture resistance reliability.

[0089] At this time, the margin portions 114' and 115' contain BaTiO3, and (Ba 1-x Ca x )TiO3 may not be included. The margin portions 114' and 115' can contain BaTiO3 as a main component, and the dielectric layer 111 of the capacitance forming portion Ac can contain BaTiO3 and (Ba 1-x Ca x )TiO3 (0.01 ≦ x ≦ 0.15) as a main component.

[0090] In the cross-sections of the main body 110' in the first direction and the third direction, when the area ratio occupied by the pores P in the margin portions 114', 115' is S3, and the area ratio occupied by the pores in the dielectric layer of the capacitance forming portion is S2, S3 < S2 can be satisfied. By satisfying S3 < S2, the density of the margin portions 114' and 115' can be improved to block the moisture penetration path, and the moisture resistance reliability can be improved.

[0091] In one embodiment, S3 can be 0.2 area% or less, and S2 can be more than 0.2 area% and 0.4 area% or less. When S3 exceeds 0.2 area%, the effect of improving the moisture resistance reliability may be insufficient, and when S2 is 0.2 area% or less, the effect of improving the high-temperature reliability may be insufficient. S3 can be measured in the same manner as S1 and S2 described above.

[0092] In one embodiment, (Ba 1-x Ca x )TiO3 (0.01≦x≦0.15) as the first crystal grains G1 and BaTiO3 as the second crystal grains G2, the dielectric layer 111 of the capacitance forming portion includes the first crystal grains G1 and the second crystal grains G2, and the margin portions 114', 115' can include the second crystal grains G2. That is, the dielectric layer 111 of the capacitance forming portion Ac can have the shape of the dielectric crystal grains shown in FIG. 4, and the margin portions 114', 115' can have the shape of the dielectric crystal grains shown in FIG. 5.

[0093] FIG. 8 is a diagram that roughly shows a perspective view of a ceramic electronic component 100'' according to one embodiment of the present invention, and FIG. 9 is a diagram that roughly shows a cross-sectional view taken along line IV-IV' in FIG.

[0094] As shown in FIG. 8 and FIG. 9, according to an embodiment of the present invention, the dielectric layer 111 of the capacitance forming portion is made of BaTiO3 and (Ba 1-x Ca x ) TiO3 (0.01≦x≦0.15), and the cover portions 112'', 113'' and margin portions 114'', 115'' may include BaTiO3.

[0095] The covers 112'', 113'' and margins 114'', 115'', which form the exterior of the body 110'', all contain BaTiO3, thereby reducing the porosity of the covers 112'', 113'' and margins 114'', 115'', and improving the moisture resistance reliability. The covers 112'', 113'' and margins 114'', 115'' may contain BaTiO3 as a main component, but may also contain (Ba 1-x Ca x ) TiO3 (0.01≦x≦0.15) may not be included. In this case, the dielectric layer 111 of the capacitance forming portion Ac may have the dielectric crystal grain shape shown in FIG. 4, and the cover portions 112″, 113″ and the margin portions 114″, 115″ may have the dielectric crystal grain shape shown in FIG.

[0096] In one embodiment, in the cross-sections of the main body 110'' in the first and third directions, when the area ratio occupied by the pores in the cover parts 112'', 113'' is S1, S1 < S2 can be satisfied. At this time, the above S1 and S3 can be 0.2 area % or less, and the above S2 can be more than 0.2 area % and 0.4 area % or less.

[0097] As described above, the embodiments of the present invention have been described in detail. However, the present invention is not limited by the above-described embodiments and the attached drawings, but is limited by the attached claims. Therefore, within the scope not departing from the technical idea of the present invention described in the claims, various forms of substitution, modification, and change are possible by those having ordinary knowledge in the art, and it can be said that these also belong to the scope of the present invention.

[0098] In addition, the expression "one embodiment" used in the present invention does not mean the same embodiment, but is provided to emphasize and explain each different unique feature. However, the above-presented one embodiment does not exclude being realized in combination with the features of other one embodiments. For example, even if a matter described in a specific one embodiment is not described in another one embodiment, it can be understood as being related to the description of the other one embodiment as long as there is no description contrary to or conflicting with that matter in the other one embodiment.

[0099] The terms used in the present invention are merely used to explain one embodiment and are not intended to limit the present invention. At this time, the singular expression includes the plural expression unless the context clearly has a different meaning. According to this specification, the following items are also disclosed. [Item 1] It includes a dielectric layer, and a first internal electrode and a second internal electrode that are alternately arranged in the first direction with the dielectric layer interposed therebetween, a first surface and a second surface facing each other in the first direction, a third surface and a fourth surface connected to the first surface and the second surface and facing each other in the second direction, and a fifth surface and a sixth surface connected to the first surface to the fourth surface and facing each other in the third direction, and a main body, a first external electrode disposed on the third surface and connected to the first internal electrode, a second external electrode disposed on the fourth surface and connected to the second internal electrode, the main body includes a capacitance forming portion in which capacitance is formed including the first internal electrode and the second internal electrode, and a cover portion disposed on both end faces in the first direction of the capacitance forming portion, the dielectric layer of the capacitance forming portion is BaTiO 3 and (Ba 1-xCa x )TiO 3 (0.01 ≦ x ≦ 0.15), the cover portion includes BaTiO 3 , in a cross section in the first direction and the third direction of the main body, when the area ratio occupied by pores in the cover portion is S1 and the area ratio occupied by pores in the dielectric layer of the capacitance forming portion is S2, a ceramic electronic component satisfying S1 < S2. [Item 2] S1 is 0.2 area% or less, the ceramic electronic component according to Item 1, wherein S2 is more than 0.2 area% and 0.4 area% or less. [Item 3] The cover portion does not include (Ba 1-x Ca x )TiO 3 (0.01 ≦ x ≦ 0.15), the ceramic electronic component according to Item 1. [Item 4] The dielectric layer of the capacitance forming portion includes (Ba 1-x Ca x )TiO 3 (0.01 ≦ x ≦ 0.15) in an amount of 30 mol or more and 300 mol or less with respect to 100 mol of BaTiO 3 , the ceramic electronic component according to Item 1. [Item 5] When the crystal grains mainly composed of (Ba 1-x Ca x )TiO 3 (0.01 ≦ x ≦ 0.15) are the first crystal grains and the crystal grains mainly composed of BaTiO 3 are the second crystal grains, the dielectric layer of the capacitance forming portion includes the first crystal grains and the second crystal grains, the ceramic electronic component according to any one of Items 1 to 4, wherein the cover portion includes the second crystal grains. [Item 6] The average size of the first crystal grains is larger than the average size of the second crystal grains, the ceramic electronic component according to Item 5. [Item 7] The average size of the first crystal grains is 210 to 340 nm, and the average size of the second crystal grains is 160 to 290 nm. The ceramic electronic component according to item 6. [Item 8] A main body including a dielectric layer, a first internal electrode and a second internal electrode alternately arranged in a first direction with the dielectric layer interposed therebetween, a first surface and a second surface facing each other in the first direction, a third surface and a fourth surface connected to the first surface and the second surface and facing each other in a second direction, and a fifth surface and a sixth surface connected to the first surface to the fourth surface and facing each other in a third direction, A first external electrode disposed on the third surface and connected to the first internal electrode, A second external electrode disposed on the fourth surface and connected to the second internal electrode, The main body includes a capacitance forming portion in which capacitance is formed including the first internal electrode and the second internal electrode, a cover portion disposed on both end faces of the capacitance forming portion in the first direction, and a margin portion disposed on both end faces of the capacitance forming portion in the third direction, The dielectric layer of the capacitance forming portion is BaTiO 3 And (Ba 1-x Ca x )TiO 3 (0.01 ≦ x ≦ 0.15), and the margin portion includes BaTiO 3 , In a cross section of the main body in the first direction and the third direction, when the area ratio occupied by pores in the margin portion is S3 and the area ratio occupied by pores in the dielectric layer of the capacitance forming portion is S2, a ceramic electronic component satisfying S3 < S2. [Item 9] S3 is 0.2 area% or less, The S2 is more than 0.2 area% and 0.4 area% or less. The ceramic electronic component according to item 8. [Item 10] The margin portion does not include (Ba 1-x Ca x )TiO 3 (0.01 ≦ x ≦ 0.15). The ceramic electronic component according to item 8. [Item 11] The dielectric layer of the capacitance forming portion contains (Ba 1-x Ca x )TiO 3 (0.01 ≦ x ≦ 0.15) in an amount of 30 mol or more and 300 mol or less with respect to 100 mol of BaTiO 3 . The ceramic electronic component according to item 8. [Item 12] When the crystal grains mainly composed of (Ba 1-x Ca x )TiO 3 (0.01 ≦ x ≦ 0.15) are the first crystal grains and the crystal grains mainly composed of BaTiO 3 are the second crystal grains, The dielectric layer of the capacitance forming portion includes the first crystal grains and the second crystal grains, The margin portion includes the second crystal grains. The ceramic electronic component according to any one of items 8 to 11. [Item 13] The average size of the first crystal grains is larger than the average size of the second crystal grains. The ceramic electronic component according to item 12. [Item 14] The average size of the first crystal grains is 210 to 340 nm, and the average size of the second crystal grains is 160 to 290 nm. The ceramic electronic component according to item 13. [Item 15] The cover portion contains BaTiO 3 and In the cross sections of the main body in the first direction and the third direction, when the area ratio occupied by pores in the cover portion is S1, the ceramic electronic component according to item 8, which satisfies S1 < S2. [Item 16] S1 and S3 are 0.2 area% or less, The ceramic electronic component according to item 15, wherein S2 is more than 0.2 area% and 0.4 area% or less. [Explanation of symbols]

[0100] 100: Ceramic electronic components 110: Main unit 111: Dielectric layer 112, 113: Cover part 114, 115: Margin 121, 122: Internal electrode 131, 132: External electrode 131a, 132a: Electrode layer 131b, 132b: plating layer

Claims

1. a main body including a dielectric layer, and first and second internal electrodes arranged alternately in a first direction with the dielectric layer therebetween, the main body including a first surface and a second surface facing the first direction, a third surface and a fourth surface connected to the first surface and the second surface and facing the second direction, and a fifth surface and a sixth surface connected to the first surface to the fourth surface and facing the third direction; a first external electrode disposed on the third surface and connected to the first internal electrode; a second external electrode disposed on the fourth surface and connected to the second internal electrode, the body includes a capacitance forming portion including the first internal electrode and the second internal electrode to form a capacitance, and a cover portion disposed on both end surfaces of the capacitance forming portion in a first direction, The dielectric layer of the capacitance forming portion is BaTiO 3 And (Ba 1-x Ca x ) TiO 3 (0.01≦x≦0.15), and the cover portion is BaTiO 3 Including, In a cross section of the main body in the first direction and the third direction, when an area ratio of the pores in the cover portion is S1 and an area ratio of the pores in the dielectric layer of the capacitance forming portion is S2, S1<S2 is satisfied, The S1 is 0.2 area% or less, The S2 is more than 0.2 area % and not more than 0.4 area %.

2. The cover portion is (Ba 1-x Ca x ) TiO 3 The ceramic electronic component according to claim 1 , wherein x does not include (0.01≦x≦0.15).

3. The dielectric layer of the capacitance forming portion is (Ba 1-x Ca x ) TiO 3 (0.01≦x≦0.15) 3 2. The ceramic electronic component according to claim 1, wherein the content is 30 moles or more and 300 moles or less per 100 moles.

4. (Ba 1-x Ca x ) TiO 3 The crystal grains mainly composed of (0.01≦x≦0.15) are called the first crystal grains, and BaTiO 3 the second crystal grains are crystal grains mainly composed of the above, the dielectric layer of the capacitance forming portion includes the first crystal grains and the second crystal grains, The ceramic electronic component according to claim 1 , wherein the cover portion includes second crystal grains.

5. The ceramic electronic component according to claim 4 , wherein an average size of the first crystal grains is larger than an average size of the second crystal grains.

6. 6. The ceramic electronic component according to claim 5, wherein the first crystal grains have an average size of 210 to 340 nm, and the second crystal grains have an average size of 160 to 290 nm.

7. a main body including a dielectric layer, and first and second internal electrodes arranged alternately in a first direction with the dielectric layer therebetween, the main body including a first surface and a second surface facing the first direction, a third surface and a fourth surface connected to the first surface and the second surface and facing the second direction, and a fifth surface and a sixth surface connected to the first surface to the fourth surface and facing the third direction; a first external electrode disposed on the third surface and connected to the first internal electrode; a second external electrode disposed on the fourth surface and connected to the second internal electrode, the main body includes a capacitance forming portion in which a capacitance is formed including the first internal electrode and the second internal electrode, a cover portion disposed on both end surfaces of the capacitance forming portion in a first direction, and a margin portion disposed on both end surfaces of the capacitance forming portion in a third direction, The dielectric layer of the capacitance forming portion is BaTiO 3 And (Ba 1-x Ca x ) TiO 3 (0.01≦x≦0.15), and the margin portion is BaTiO 3 Including, In cross sections of the main body in the first direction and the third direction, when an area ratio of the pores in the margin portion is S3 and an area ratio of the pores in the dielectric layer of the capacitance forming portion is S2, S3<S2 is satisfied; The S3 is 0.2 area% or less, The S2 is more than 0.2 area % and not more than 0.4 area %.

8. The margin portion is (Ba 1-x Ca x ) TiO 3 The ceramic electronic component according to claim 7 , wherein (0.01≦x≦0.15) is not included.

9. The dielectric layer of the capacitance forming portion is (Ba 1-x Ca x ) TiO 3 (0.01≦x≦0.15) 3 The ceramic electronic component according to claim 7 , wherein the content is 30 moles or more and 300 moles or less per 100 moles.

10. (Ba 1-x Ca x ) TiO 3 The crystal grains mainly composed of (0.01≦x≦0.15) are called the first crystal grains, and BaTiO 3 When the crystal grains mainly composed of are defined as the second crystal grains, the dielectric layer of the capacitance forming portion includes first crystal grains and second crystal grains, The ceramic electronic component according to claim 7 , wherein the margin portion includes second crystal grains.

11. The ceramic electronic component according to claim 10 , wherein an average size of the first crystal grains is larger than an average size of the second crystal grains.

12. The ceramic electronic component according to claim 11, wherein the first crystal grains have an average size of 210 to 340 nm, and the second crystal grains have an average size of 160 to 290 nm.

13. The cover is made of BaTiO 3 Including, The ceramic electronic component according to claim 7 , wherein when an area ratio of the pores in the cover portion in the cross sections of the main body taken in the first and third directions is S1, S1<S2 is satisfied.

14. The ceramic electronic component according to claim 13 , wherein the S1 is 0.2 area % or less.

Citation Information

Patent Citations

  • Laminated ceramic capacitor

    JP2007266223A

  • Inductor

    JP2018098489A

  • Multilayer ceramic electronic component

    JP2019175938A

  • Dielectric ceramic composition and multilayer ceramiccapacitor using the same

    KR1020060110603A

  • inductor

    US20180166198A1

Cited By

  • Multilayer ceramic capacitor

    US12603228B2

  • Multilayer ceramic capacitor

    US20250292966A1