Electronic devices

The use of a thermosetting resin composition with inorganic filler and non-conductive metal compounds in a core-shell structure addresses the limitations of existing LDS technologies, enhancing the reliability and circuit formability of electronic devices, particularly MIDs, by forming a stable and flexible encapsulation.

JP7562989B2Active Publication Date: 2024-10-08SUMITOMO BAKELITE CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020088189
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-12
Filing Date
2020-05-20
Publication Date
2024-10-08
Estimated Expiration
2040-05-20

AI Technical Summary

Technical Problem

Existing technologies for manufacturing electronic devices using Laser Direct Structuring (LDS) face challenges in achieving reliable and flexible circuit formation, particularly in molded interconnect devices (MIDs), due to limitations in the materials and processes used for encapsulation and sealing.

Method used

The use of a thermosetting resin composition for LDS, comprising a thermosetting resin, inorganic filler, and a non-conductive metal compound that forms a metal nucleus upon active energy ray irradiation, is applied as a first and second encapsulant to seal semiconductor elements, allowing for the formation of a core-shell structure that enhances reliability and circuit formability.

Benefits of technology

This approach results in electronic devices with improved reliability and circuit formability, enabling finer and more complex wiring structures, while reducing the device size, weight, and number of parts through effective use of space.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562989000005
    Figure 0007562989000005
  • Figure 0007562989000006
    Figure 0007562989000006
  • Figure 0007562989000007
    Figure 0007562989000007
Patent Text Reader

Abstract

To provide an electronic apparatus with excellent reliability and circuit formability.SOLUTION: A semiconductor device 100 includes a substrate 101, a semiconductor device 103 mounted on the substrate 101, a first encapsulating layer 105 that encapsulates the semiconductor device 103, a second encapsulating layer 107 that covers the surface of the first encapsulating layer 105 and is composed of a cured material of a thermosetting resin composition for LDS. The thermosetting resin composition for LDS includes a thermosetting resin, an inorganic filler, and a non-conductive metal compound that forms metal nuclei upon irradiation with an active energy beam.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to electronic devices. [Background technology]

[0002] Patent Document 1 (JP 2015-134903 A) describes a technology related to resin materials used in LASER DIRECT STRUCTURE (LDS). This document describes a fiber-reinforced resin material obtained by impregnating continuous fibers with a thermoplastic resin composition containing an LDS additive, and uses a polyamide resin as the thermoplastic resin. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-134903 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present inventors have investigated the use of microfabrication by LDS in the manufacture of electronic devices such as molded interconnect devices (MIDs). The present invention provides an electronic device having excellent reliability and circuit formability. [Means for solving the problem]

[0005] According to the present invention, Electronic components, a first sealing material covering at least a portion of a surface of the electronic component; a second sealing material covering at least a portion of the surface of the electronic component and the first sealing material; Including, At least one of the first and second sealing materials is made of a cured product of a thermosetting resin composition for LDS (LASER DIRECT STRUCTURE), The thermosetting resin composition for LDS, A thermosetting resin; An inorganic filler; a non-conductive metal compound which forms a metal nucleus when irradiated with active energy rays; An electronic device is provided, comprising:

[0006] According to the present invention, A substrate; A semiconductor element mounted on the substrate; a first encapsulant that encapsulates the semiconductor element; A second sealing material that covers a surface of the first sealing material and is made of a cured product of a thermosetting resin composition for LDS (LASER DIRECT STRUCTURE), Including, The thermosetting resin composition for LDS, A thermosetting resin; An inorganic filler; a non-conductive metal compound which forms a metal nucleus when irradiated with active energy rays; There is provided an electronic device which is a semiconductor device, comprising:

[0007] According to the present invention, preparing a structure in which a semiconductor element mounted on a substrate is sealed with a first sealing material; forming a second sealing material composed of a cured product of a thermosetting resin composition for LDS (LASER DIRECT STRUCTURE) on the first sealing material; Including, The thermosetting resin composition for LDS, A thermosetting resin; An inorganic filler; a non-conductive metal compound which forms a metal nucleus when irradiated with active energy rays; A method for manufacturing a semiconductor device is provided, comprising:

[0008] According to the present invention, forming a second sealing material on the first sealing material so as to cover at least a portion of a surface of the first sealing material; disposing the electronic component such that the first and second encapsulants cover at least a portion of the electronic component; Including, At least one of the first and second sealing materials is made of a cured product of a thermosetting resin composition for LDS (LASER DIRECT STRUCTURE), The thermosetting resin composition for LDS, A thermosetting resin; An inorganic filler; a non-conductive metal compound which forms a metal nucleus when irradiated with active energy rays; A method for manufacturing an electronic device is provided, comprising:

[0009] According to the present invention, preparing a structure having an electronic component provided on a first sealing material; forming a second sealing material on the first sealing material so as to cover at least a portion of the electronic component; Including, The first sealing material is composed of a cured product of a thermosetting resin composition for LDS (LASER DIRECT STRUCTURE), The thermosetting resin composition for LDS, A thermosetting resin; An inorganic filler; a non-conductive metal compound which forms a metal nucleus when irradiated with active energy rays; A method for manufacturing an electronic device is provided, comprising:

[0010] Any combination of these configurations and conversion of the present invention between methods, devices, etc. are also valid aspects of the present invention. For example, according to the present invention, it is also possible to obtain a thermosetting resin composition for LDS used in the second encapsulating material of the semiconductor device of the present invention, and a cured product thereof. Effect of the Invention

[0011] According to the present invention, it is possible to provide an electronic device having excellent reliability and circuit formability. [Brief description of the drawings]

[0012] [Figure 1] 1 is a cross-sectional view showing a configuration example of a semiconductor device according to an embodiment; [Diagram 2] 1 is a cross-sectional view showing a configuration example of a semiconductor device according to an embodiment; [Diagram 3] 1 is a perspective view showing a configuration example of a thin film inductor according to an embodiment; [Figure 4] 1A to 1C are schematic cross-sectional views showing steps of an example of a method for manufacturing a thin-film inductor. [Diagram 5] 1A to 1C are schematic cross-sectional views showing steps of an example of a method for manufacturing a thin-film inductor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given the same reference numerals, and the description will be omitted as appropriate. The drawings are schematic and do not necessarily correspond to the actual dimensional ratios. Unless otherwise specified, the numerical range "A to B" means "A or more and B or less". The composition may contain each component alone or in combination of two or more kinds. Furthermore, the configurations of the following embodiments can be used in appropriate combination.

[0014] (First embodiment) In this embodiment, an example in which the electronic device is a semiconductor device will be described. Fig. 1(a) is a cross-sectional view showing an example of the configuration of a semiconductor device according to the present embodiment, Fig. 1(b) is a diagram showing a modified example of the semiconductor device 100 shown in Fig. 1(a). The electronic device (semiconductor device 100) includes an electronic component (semiconductor element 103), a first sealing material (first sealing layer 105) covering at least a part of the surface of the semiconductor element 103, and a second sealing material (second sealing layer 107) covering at least a part of the surfaces of the semiconductor element 103 and the first sealing layer 105. At least one of the first sealing layer 105 and the second sealing layer 107 is composed of a cured product of a thermosetting resin composition for LDS (LASER DIRECT STRUCTUREING). The thermosetting resin composition for LDS includes a thermosetting resin, an inorganic filler, and a non-conductive metal compound that forms a metal nucleus by irradiation with active energy rays. 1(a) and 1(b), specifically, the second encapsulation layer 107 is made of a thermosetting resin composition for LDS. That is, the semiconductor device 100 includes a substrate 101, a semiconductor element 103 mounted on the substrate 101, a first encapsulation material (first encapsulation layer 105) that encapsulates the semiconductor element 103, and a second encapsulation material (second encapsulation layer 107) that covers the surface of the first encapsulation layer 105 and is made of a cured product of a thermosetting resin composition for LDS (LASER DIRECT STRUCTURE). The thermosetting resin composition for LDS includes a thermosetting resin, an inorganic filler, and a non-conductive metal compound that forms a metal nucleus by irradiation with active energy rays. Specific examples of the components of the thermosetting resin composition for LDS will be described later in the sixth embodiment.

[0015] Specific examples of the semiconductor device 100 include molded circuit components and various semiconductor packages. Specific examples of molded circuit components include those used in portable electronic devices such as mobile phones, vehicles such as automobiles, and medical devices. Specific examples of semiconductor packages include semiconductor packages such as MAP (Mold Array Package), QFP (Quad Flat Package), SOP (Small Outline Package), CSP (Chip Size Package), QFN (Quad Flat Non-leaded Package), SON (Small Outline Non-leaded Package), BGA (Ball Grid Array), LF-BGA (Lead Flame BGA), FCBGA (Flip Chip BGA), MAPBGA (Molded Array Process BGA), eWLB (Embedded Wafer-Level BGA), Fan-In type eWLB, Fan-Out type eWLB, and SIP (System In package).

[0016] Moreover, the semiconductor device 100 is, for example, a three-dimensional molded circuit component (Molded Interconnect Device: MID). The MID has three elements: a three-dimensional shape, the above-mentioned resin molded product, and a three-dimensional circuit, and is, for example, a component in which a circuit is formed with a metal film on the surface of a resin molded product with a three-dimensional structure. Specifically, the MID can include a resin molded product with a three-dimensional structure and a three-dimensional circuit formed on the surface of this resin molded product. By using such an MID, it is possible to effectively utilize space and reduce the number of parts and make the device lighter, thinner, shorter, and smaller.

[0017] The semiconductor element 103 is mounted on the substrate 101. Here, the semiconductor element 103 may be provided on the substrate 101 in the form of a semiconductor chip or a semiconductor package. The substrate 101 is, for example, a wiring board such as an interposer, or a lead frame. Fig. 1(b) is a cross-sectional view showing a modified example of the semiconductor device 100. In Fig. 1(b), the substrate is a lead frame 109. The semiconductor element 103 is electrically connected to the substrate 101 by, for example, wire bonding or flip chip connection. For example, a conductor portion (not shown) provided on the semiconductor element 103 may be electrically connected to a conductor portion (lead frame 109 in FIG. 1(b)) provided on the substrate 101. The conductor portion is wiring or the like. Specifically, the conductor portion is made of a conductive material, for example, Cu or a Cu alloy.

[0018] In semiconductor device 100, the encapsulant includes first encapsulation layer 105 and second encapsulation layer 107, which are laminated together. First sealing layer 105 is composed of a cured product of a thermosetting resin composition. From the viewpoint of improving the dielectric properties of the entire sealing material and improving the adhesion between first sealing layer 105 and a conductive member (for example, lead frame 109 in FIG. 1(b)), first sealing layer 105 or the thermosetting resin composition used for first sealing layer 105 preferably does not contain a non-conductive metal compound.

[0019] The thickness of first sealing layer 105 can be adjusted according to, for example, the shape and size of semiconductor element 103, and specifically, can be set to a thickness that can stably seal semiconductor element 103.

[0020] The linear expansion coefficient of the first sealing layer 105 in the temperature region below the glass transition temperature, as measured by thermomechanical analysis (TMA), is preferably 6 ppm / °C or more, more preferably 7 ppm / °C or more, and even more preferably 9 ppm / °C or more, from the viewpoint of improving adhesion with adjacent conductor portions. From a similar viewpoint, the linear expansion coefficient of first sealing layer 105 in the temperature region below the glass transition temperature, as measured by thermomechanical analysis (TMA), is preferably 20 ppm / °C or less, more preferably 18 ppm / °C or less, and even more preferably 15 ppm / °C or less.

[0021] Here, the linear expansion coefficients of the first sealing layer 105 and the second sealing layer 107 described below can be measured using a TMA device (e.g., TMA6100 manufactured by Hitachi High-Technologies Corporation) at a temperature increase rate of 10°C / min in the temperature range of 30°C to 350°C.

[0022] The second sealing layer 107 is composed of a cured product of a thermosetting resin composition for LDS described later. Specific examples of the shape of the thermosetting resin composition for LDS include solid shapes such as a sheet shape and a particulate shape (e.g., granules or tablets); and liquid shapes. In the present embodiment, the following description will be given taking as an example a case where a sheet-shaped thermosetting resin composition for LDS is used. In this embodiment, second sealing layer 107 is specifically a sheet-shaped cured product of a thermosetting resin composition for LDS. Second sealing layer 107 is provided in contact with and covers first sealing layer 105. Second sealing layer 107 only needs to cover at least a portion of first sealing layer 105, and may cover at least a portion of the top surface and side surfaces of first sealing layer 105, for example. In semiconductor device 100, second sealing layer 107 seals the entire surface of first sealing layer 105 above substrate 101. That is, second sealing layer 107 covers the entire surface of first sealing layer 105 above substrate 101. Also, end portions of second sealing layer 107 contact the surface of substrate 101. This configuration can further increase the degree of freedom in forming circuits outside the sealing material.

[0023] From the viewpoint of enhancing the stability of circuit formation, second sealing layer 107 has a thickness of preferably 30 μm or more, more preferably 40 μm or more, even more preferably 50 μm or more, and still more preferably 80 μm or more. In addition, from the viewpoint of solidifying the entire semiconductor device 100 and improving the dielectric properties of the entire sealing material, the thickness of the second sealing layer 107 is preferably 500 μm or less, more preferably 400 μm or less, even more preferably 300 μm or less, even more preferably 200 μm or less, and even more preferably 150 μm or less.

[0024] The linear expansion coefficient of the second sealing layer 107 in the temperature region below the glass transition temperature, as measured by thermomechanical analysis (TMA), is preferably 6 ppm / °C or more, more preferably 7 ppm / °C or more, and even more preferably 8 ppm / °C or more, from the viewpoint of improving adhesion to the first sealing layer 105. From a similar viewpoint, the linear expansion coefficient of the second sealing layer 107 in the temperature region below the glass transition temperature, as measured by thermomechanical analysis (TMA), is preferably 20 ppm / °C or less, more preferably 18 ppm / °C or less, and even more preferably 15 ppm / °C or less.

[0025] From the viewpoint of improving the adhesion between first sealing layer 105 and second sealing layer 107, the difference between the linear expansion coefficient in a temperature region below the glass transition temperature of first sealing layer 105 and the linear expansion coefficient in a temperature region below the glass transition temperature of second sealing layer 107 is preferably 5 ppm / ° C. or less, more preferably 3 ppm / ° C. or less, and further preferably 1 ppm / ° C. or less. The linear expansion coefficient difference may be, for example, more than 0 ppm / ° C., and is preferably 0 ppm / ° C. Here, the linear expansion coefficients of first sealing layer 105 and second sealing layer 107 can be adjusted, for example, by adjusting the content of inorganic filler in the thermosetting resin composition used in these sealing layers.

[0026] In addition, from the viewpoint of improving the heat resistance reliability of semiconductor device 100, the glass transition temperature (Tg) of each of first sealing layer 105 and second sealing layer 107 is preferably 100°C or higher, more preferably 120°C or higher, and is preferably 250°C or lower, more preferably 220°C or lower.

[0027] Next, a method for manufacturing the semiconductor device 100 will be described. Specifically, the manufacturing method of the electronic device (semiconductor device 100) includes the steps of preparing a structure in which an electronic component (semiconductor element 103) is sealed with a first sealing layer 105, and forming a second sealing layer 107 on the first sealing layer 105, and at least one of the first sealing layer 105 and the second sealing layer 107 is composed of a cured product of a thermosetting resin composition for LDS. Hereinafter, a more specific description will be given of an example in which second sealing layer 107 is made of a cured product of a thermosetting resin composition for LDS. In this case, the method for producing semiconductor device 100 includes, for example, the following steps 1 and 2. (Step 1) A step of preparing a structure in which a semiconductor element 103 mounted on a substrate 101 is sealed with a first sealing layer 105. (Step 2) A step of forming a second sealing layer 107 made of a cured product of a thermosetting resin composition for LDS on the first sealing layer 105.

[0028] In step 1, for example, semiconductor element 103 is mounted on substrate 101 according to a conventional method, and semiconductor element 103 is encapsulated with first encapsulating layer 105. From the viewpoint of improving production stability, compression molding or transfer molding is preferably used to form first encapsulating layer 105.

[0029] In step 2, a molding method for second sealing layer 107 can be selected depending on, for example, the shape of the thermosetting resin composition for LDS. In this embodiment, specifically, the entire first sealing layer 105 may be sealed using a sheet-shaped thermosetting resin composition for LDS.

[0030] At this time, second sealing layer 107 can be formed by, for example, compression molding or lamination molding. In the case of compression molding, for example, the structure obtained in step 1 is fixed to one of the upper and lower dies of a compression molding die by a fixing means such as clamping or suction. In the following, an example will be described in which the structure is fixed to the upper die of the compression molding die so that the surface of the structure on which the first sealing layer 105 is formed faces the resin material supply container.

[0031] Next, the sheet-shaped thermosetting resin composition for LDS is placed in the lower mold cavity of the mold so as to be at a position corresponding to the structure fixed to the upper mold of the mold. Next, the gap between the upper and lower molds of the mold is narrowed under reduced pressure, so that the sheet-shaped thermosetting resin composition for LDS is heated to a predetermined temperature in the lower mold cavity and becomes molten. Thereafter, the upper and lower molds of the mold are joined together to press the molten thermosetting resin composition for LDS against the structure fixed to the upper mold. In this way, the structure can be filled with the thermosetting resin composition for LDS, and the surface of the structure can be covered with the thermosetting resin composition for LDS in the molten state. Then, while maintaining the state in which the upper and lower molds of the mold are joined together, the thermosetting resin composition for LDS is cured for a predetermined time. In this way, the second sealing layer 107 that seals the first sealing layer 105 can be formed.

[0032] When compression molding is performed, it is preferable to perform resin sealing while reducing the pressure inside the mold, and more preferably under vacuum conditions, so that first sealing layer 105 can be embedded with second sealing layer 107 without leaving any filled portion.

[0033] The molding temperature in compression molding is preferably 50 to 200° C., more preferably 80 to 180° C. The molding pressure is preferably 0.5 to 12 MPa, more preferably 1 to 10 MPa. The molding time is preferably 30 seconds to 15 minutes, more preferably 1 to 10 minutes. By setting the molding temperature, pressure, and time within the above ranges, it is possible to prevent the occurrence of areas where the molten sealing material is not filled.

[0034] The post-cure temperature, which is performed after the structure obtained in step 1 is encapsulated by compression molding using the sheet-shaped thermosetting resin composition for LDS, is preferably 150 to 200° C., and more preferably 165 to 185° C. The post-cure time is preferably 1 to 5 hours, and more preferably 2 to 4 hours.

[0035] In the case of lamination molding, first, a sheet-like LDS thermosetting resin composition prepared in a roll shape is attached to an unwinding device of a vacuum pressure laminator and connected to a winding device. Next, the structure obtained in step 1 is conveyed to a diaphragm (elastic membrane) type laminator section. Next, when pressing is started under reduced pressure, the sheet-like LDS thermosetting resin composition is heated to a predetermined temperature and becomes molten. Thereafter, the sheet-like LDS thermosetting resin composition in the molten state is pressed against the first sealing layer 105 formation surface of the structure by pressing through a diaphragm, so that the second sealing layer 107 can be filled in and the surface of the first sealing layer 105 can be covered with the second sealing layer 107 in the molten state. Then, the second sealing layer 107 is cured for a predetermined time. In this way, the first sealing layer 105 can be sealed. If more precise flatness is required for second sealing layer 107, a pressing step using a highly precisely adjusted flat pressing device can be added after pressing with a diaphragm-type laminator.

[0036] When carrying out the above-mentioned lamination molding, the molding temperature by the diaphragm (elastic film) type laminator part is preferably 50 to 120°C, more preferably 80 to 110°C. The molding pressure by the diaphragm (elastic film) type laminator part is preferably 0.5 to 1 MPa, more preferably 0.6 to 0.9 MPa. The molding time by the diaphragm (elastic film) type laminator part is preferably 30 seconds to 5 minutes, more preferably 1 to 3 minutes. By setting the molding temperature, pressure, and time by the diaphragm (elastic film) type laminator part within the above ranges, it is possible to prevent the occurrence of portions that are not filled with the thermosetting resin composition for LDS in a molten state.

[0037] When carrying out the above-mentioned lamination molding, the pressing temperature by the flat press is preferably 80 to 130°C, more preferably 90 to 120°C. The molding pressure by the flat press is preferably 0.5 to 2 MPa, more preferably 0.8 to 1.5 MPa. The molding time by the flat press is preferably 30 seconds to 5 minutes, more preferably 1 to 3 minutes. By setting the pressing temperature, molding pressure, and time by the flat press in the above ranges, it is possible to prevent the occurrence of areas where the molten thermosetting resin composition for LDS is not filled.

[0038] Furthermore, the post-cure temperature, which is performed after the first sealing layer 105 is sealed and molded by a lamination molding method using a sheet-shaped thermosetting resin composition for LDS, is preferably 150 to 200° C., and more preferably 165 to 185° C. The post-cure time is preferably 1 hour to 5 hours, and more preferably 2 hours to 4 hours.

[0039] After step 2, for example, the following steps 3 and 4 may be carried out. (Step 3) A step of irradiating a specific portion of the surface of second sealing layer 107 with active energy rays (Step 4) A step of forming a conductor layer such as a wiring layer by selectively forming a metal layer in the area (recess) on the surface of the second sealing layer 107 irradiated with active energy rays. In addition, a surface cleaning step may be added after step 3 and before step 4.

[0040] In step 3, specific portions of the surface of second sealing layer 107 are selectively irradiated with active energy rays such as a laser. By irradiating with the laser, for example, recesses can be formed in the laser irradiated portions of second sealing layer 107. The laser can be appropriately selected from known lasers such as YAG laser, excimer laser, electromagnetic rays, etc., and YGA laser is preferred. The wavelength of the laser is not specified, but is, for example, 200 nm or more and 2000 nm or less, and from the viewpoint of thinning, is preferably 240 nm or more and 1100 nm or less. Among these, preferred lasers include those with wavelengths of 248 nm, 308 nm, 355 nm, 515 nm, 532 nm, 1064 nm, or 1060 nm.

[0041] In step 4, a metal film is selectively formed in a predetermined region of second sealing layer 107 by LDS. Specifically, in LDS, active energy rays are irradiated onto the surface of second sealing layer 107 containing an LDS additive to generate metal nuclei, and the metal nuclei are used as seeds to form a plating pattern in the energy ray irradiated region by plating treatment such as electroless plating. Based on this plating pattern, conductive members such as wiring and circuits can be formed. This will be explained in more detail below.

[0042] In step 4, a conductor layer such as a wiring layer is selectively formed in the laser irradiated portions, specifically in the recesses, of the surface of second sealing layer 107. Specifically, the conductor layer is made of a plating film. Moreover, step 4 specifically includes a step of applying a metal to the recessed portion, and a step of growing a plating layer of the metal in the recessed portion.

[0043] The plating process may be either electrolytic plating or electroless plating. A circuit (plating layer) can be formed by plating the area irradiated with the laser in step 2. The plating solution is not specified and any known plating solution can be widely used, and a plating solution containing a mixture of copper, nickel, gold, silver, and palladium as metal components may be used.

[0044] Through the above steps, the semiconductor device 100 is obtained. In this embodiment, since the encapsulant for the semiconductor element 103 has a core-shell structure of the first encapsulating layer 105 and the second encapsulating layer 107, the semiconductor device 100 can be obtained with excellent reliability and circuit formability. For example, different resin compositions are used for the first encapsulating layer 105 and the second encapsulating layer 107, and preferably the resin composition for the first encapsulating layer 105 does not contain a non-conductive metal compound, so that the adhesion between the semiconductor element 103 or the conductor and the first encapsulating layer 105 can be excellent, while the moldability and dielectric properties of the entire encapsulant can be more favorable. In addition, since the second encapsulating layer 107 is composed of a cured product of the thermosetting resin composition for LDS, for example, the wiring formation by the LDS process can be stably performed by the above-mentioned steps 3 and 4, and it is also possible to provide the semiconductor device 100 with a finer or more complicated wiring structure.

[0045] In the following embodiment, the differences from the first embodiment will be mainly described.

[0046] Second Embodiment Fig. 2(a) is a cross-sectional view showing an example of the configuration of the semiconductor device according to this embodiment, and Fig. 2(b) is a diagram showing a modified example of the semiconductor device 110 shown in Fig. 2(a). In Figures 2(a) and 2(b), the basic configuration of semiconductor device 110 is similar to that of semiconductor device 100 shown in Figures 1(a) and 1(b), respectively, except that a second sealing layer 111 is provided instead of second sealing layer 107 as the second sealing material. In this embodiment, second sealing layer 111 is specifically a cured product of a liquid thermosetting resin composition for LDS. Second sealing layer 111 is provided in contact with the upper part of first sealing layer 105 , and covers the entire upper surface of first sealing layer 105 .

[0047] From the same viewpoint as in the first embodiment, the thickness of second sealing layer 111 can be set to approximately the thickness of second sealing layer 107 described above in the first embodiment. The linear expansion coefficient in the temperature region below the glass transition temperature of second sealing layer 111, the difference between the linear expansion coefficient in the temperature region below the glass transition temperature of first sealing layer 105 and the linear expansion coefficient in the temperature region below the glass transition temperature of second sealing layer 111, and the glass transition temperature of second sealing layer 111, which are measured by thermomechanical analysis (TMA), can each be approximately as large as described above in the first embodiment, for example.

[0048] The semiconductor device 110 can also be manufactured, for example, in accordance with the manufacturing method of the semiconductor device 100 described above in the first embodiment, and more specifically, the manufacturing method can include the above-mentioned steps 1 and 2.

[0049] Step 1 can be, for example, the same method as in the first embodiment. In step 2, for example, a liquid thermosetting resin composition for LDS is applied to the upper surface of first encapsulating layer 105 to form a film, which can be cured to form second encapsulating layer 111. Specific examples of the method for applying the thermosetting resin composition for LDS include printing such as offset printing and screen printing; jet dispensing such as air dispensing and mechanical dispensing; and the like, with printing being preferred. It is also preferable to obtain second sealing layer 111 by compression molding.

[0050] In semiconductor device 110, the sealing material of semiconductor element 103 has a core-shell structure of first sealing layer 105 and second sealing layer 111, and therefore the same effects as those of the first embodiment can be obtained. Furthermore, according to this embodiment, for example, it is possible to suitably suppress warping of the sealing material.

[0051] Although an example in which semiconductor element 103 is embedded in first sealing layer 105 has been described above, first sealing layer 105 and second sealing layer 111 may each cover at least a part of the surface of the electronic component. A part of the electronic component may be exposed on the surface of at least one of first sealing layer 105 and second sealing layer 111. In addition, although the above describes an example in which second sealing layer 111 is provided in contact with the surface of first sealing layer 105, one or more intervening layers may be provided between first sealing layer 105 and second sealing layer 111.

[0052] Although the above description has been given by taking the case where the electronic device is a semiconductor device as an example, the electronic device is not limited to a semiconductor device. Another specific example of the electronic device is an inductor such as a thin film inductor. In the following, a thin film inductor will be taken as an example for explanation. In the following embodiments, the MID circuit can be formed by, for example, at least a part of the method described above in the first embodiment, more specifically, at least a part of steps 3 and 4.

[0053] (Third embodiment) Fig. 3 is a perspective view showing an example of the configuration of a thin-film inductor according to this embodiment. The thin-film inductor 10 shown in Fig. 3 includes a soft magnetic thin film 12 (38) made of a resin molding material and an MID (Molded Interconnect Device) circuit 14 on the upper surface thereof.

[0054] 4(a) to 4(d) are cross-sectional views showing an example of a manufacturing process for the thin-film inductor 10. The thin-film inductor 10 can be manufactured by a method including the following steps, for example. (Step 11) A step of forming a second sealing material (insulating layer 13) on the first sealing material (soft magnetic thin film 12) so as to cover at least a part of the surface of the soft magnetic thin film 12. (Step 12) A step of disposing the copper layer 16 so that the soft magnetic thin film 12 and the insulating layer 13 cover at least a part of the electronic component (copper layer 16). In this embodiment, for example, the soft magnetic thin film 12 may be made of a cured product of a thermosetting resin composition for LDS. In this case, the thermosetting resin composition for LDS may contain a non-conductive metal compound that forms a metal nucleus when irradiated with active energy rays, as described later in the fifth embodiment.

[0055] In step 11, first, the soft magnetic thin film 12 is formed by transfer molding or compression molding of a resin molding material (FIG. 4(a)). The thickness of the soft magnetic thin film 12 is about 200 μm.

[0056] Here, a known resin composition for molding an inductor can be used as the resin molding material for obtaining the soft magnetic thin film 12. The resin composition for molding an inductor contains, for example, a thermosetting resin such as an epoxy resin, and a magnetic powder. Furthermore, from the viewpoint of making the soft magnetic thin film 12 a magnetic material having a high saturation magnetic flux density and excellent mechanical strength such as bending strength, the resin composition for molding inductors preferably contains an epoxy resin, a curing agent, a compound represented by the following general formula (1), and soft magnetic particles.

[0057] [ka]

[0058] (In the above general formula (1), R 1 represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkenyl group having 1 to 10 carbon atoms, an alkynyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aryl group, or a substituted or unsubstituted aralkyl group; R 2 represents an alkylene group having 1 to 10 carbon atoms, an alkenylene group having 1 to 10 carbon atoms, or an alkynylene group having 1 to 10 carbon atoms. Each A is independently an alkoxy group having 1 to 3 carbon atoms or an alkyl group having 1 to 3 carbon atoms, and at least one A is an alkoxy group having 1 to 3 carbon atoms.

[0059] The epoxy resin, hardener, and soft magnetic particles may be, for example, any of those known as resin compositions for molding inductors. Specific examples of the compound represented by the general formula (1) include N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane (KBM-602, Shin-Etsu Chemical Co., Ltd.), N-2-(aminoethyl)-3-aminopropyltrimethoxysilane (KBM-603, Shin-Etsu Chemical Co., Ltd.), 3-aminopropyltrimethoxysilane (KBM-903, Shin-Etsu Chemical Co., Ltd.), 3-aminopropyltriethoxysilane (KBE-903, Shin-Etsu Chemical Co., Ltd.), 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine (KBE-9103P, Shin-Etsu Chemical Co., Ltd.), and N-phenyl-3-aminopropyltrimethoxysilane (KBM-573, Shin-Etsu Chemical Co., Ltd. / CF-4083: manufactured by Dow Corning Toray Co., Ltd.).

[0060] Returning to the explanation of the manufacturing method, next, an insulating layer 13 is formed on the upper surface of the soft magnetic thin film 12 (FIG. 4(b)). The thickness of the insulating layer 13 is about 200 μm. The insulating layer 13 can be formed from a conventionally known material by a spray method, a coating method, or the like.

[0061] Then, specific portions of the soft magnetic thin film 12 are selectively irradiated with active energy rays such as a laser to form recesses (openings 15) extending from the soft magnetic thin film 12 to the insulating layer 13 (FIG. 4(c)). In addition, after forming the soft magnetic thin film 12, specific portions of the soft magnetic thin film 12 can be selectively irradiated with active energy rays to form a circuit pattern, an insulating layer can be formed on the entire upper surface of the soft magnetic thin film 12, and the pattern portion can be selectively irradiated with active energy rays again to form an insulating layer on the inner wall of the opening 15.

[0062] Next, a plating process is performed to form a copper layer 16 in the opening 15, thereby obtaining a thin-film inductor 10 having a MID circuit 14 on the soft magnetic thin film 12 (FIG. 4(d)). The thin-film inductor 10 can also have a structure shown in FIG. 4(d1).

[0063] (Fourth embodiment) This embodiment relates to another method for manufacturing the thin film inductor 10 (FIG. 3) described above in the third embodiment. Figures 5(a) to 5(d) are cross-sectional views showing an example of a manufacturing process for the thin film inductor 10. The thin film inductor 10 can also be manufactured by a method including the following steps, for example. (Step 21) A step of preparing a structure in which an electronic component (copper layer 36) is provided on a first sealing material (MID film 32). (Step 22) A step of forming a second sealing material (soft magnetic layer (thin film) 38) on the MID film 32 so as to cover at least a part of the copper layer 36. In this embodiment, specifically, the MID film 32 is made of a cured product of a thermosetting resin composition for LDS.

[0064] First, the thermosetting resin composition for LDS is applied by a die coater and dried to form the MID film 32 (FIG. 5(a)). The thickness of the MID film 32 is about 200 μm. The thermosetting resin composition for LDS can have a configuration described later in the fifth embodiment, for example.

[0065] Specific portions of the MID film 32 are selectively irradiated with active energy rays such as a laser to form openings 34 (FIG. 5(b)).

[0066] Then, a plating process is performed to form a copper layer 36 in the opening 34, thereby forming the MID circuit 14 on the MID film 32 (FIG. 5(c)). Note that after this process, an insulating layer can also be formed on the surface of the copper layer 36.

[0067] Next, the soft magnetic layer (thin film) 38 is formed on the MID film 32 and the copper layer 36 by the above-mentioned transfer molding or compression molding, and these are sealed to obtain the thin film inductor 10 having the MID circuit 14 in the soft magnetic layer (thin film) 38 (FIG. 5(d)). The material of the soft magnetic layer (thin film) 38 may be, for example, the material of the soft magnetic thin film 12 in the third embodiment. The thin film inductor 10 may also have the structure shown in FIG. 5(d1).

[0068] Fifth embodiment In this embodiment, the thermosetting resin composition used in the first sealing layer 105 and the second sealing layer in each embodiment will be described.

[0069] (First sealing layer) The thermosetting resin composition used for the first sealing layer 105 can be, specifically, a semiconductor sealing resin composition, and more specifically, can contain a thermosetting resin and an inorganic filler.

[0070] In addition, the thermosetting resin composition used in the first sealing layer 105 may be any of those widely used as semiconductor sealing materials. In addition, the thermosetting resin composition used in the first sealing layer 105 may be a composition composed of components obtained by excluding the non-conductive metal compound from the thermosetting resin composition used in the second sealing layer described below.

[0071] Furthermore, when first sealing layer 105 is a cured product of a thermosetting resin composition for LDS, the configuration of the thermosetting resin composition used for the second sealing layer described below can also be adopted.

[0072] (Second sealing layer) The thermosetting resin composition used in the second sealing layer is a thermosetting resin composition for laser direct structuring (LDS). LDS is one of the methods for manufacturing MID. Specifically, in LDS, the surface of a resin molded product containing an LDS additive is irradiated with active energy rays to generate metal nuclei, and the metal nuclei are used as seeds to form a plating pattern in the energy ray irradiated area by plating treatment such as electroless plating. Based on this plating pattern, conductive members such as wiring and circuits can be formed.

[0073] In this embodiment, the thermosetting resin composition for LDS (hereinafter, also simply referred to as "thermosetting resin composition") contains a thermosetting resin, an inorganic filler, and a non-conductive metal compound that forms a metal nucleus when irradiated with active energy rays. The components and the composition of the thermosetting resin composition can be selected depending on, for example, the shape of the second sealing layer and the method of application onto first sealing layer 105, respectively.

[0074] The shape of the thermosetting resin composition can also be selected depending on, for example, the shape of the second sealing layer and the method of application onto first sealing layer 105. Examples of the shape of the thermosetting resin composition include solid shapes such as granules and sheets; and liquid shapes. When the second sealing layer is formed by transfer molding, for example, a granular or sheet-like thermosetting resin composition can be used. When the second sealing layer is formed by compression molding, for example, a granular, sheet-like or liquid thermosetting resin composition can be used.

[0075] The configuration of the second sealing layer can also be applied to, for example, the MID film 32 in the fourth embodiment.

[0076] In addition, when the second sealing layer is a cured product of a resin composition that does not contain a non-conductive metal compound that forms a metal nucleus upon irradiation with active energy rays, the configuration of the thermosetting resin composition used for the first sealing layer 105 described above can also be adopted as such a resin composition.

[0077] (thermosetting resin) Examples of the thermosetting resin include one or more selected from the group consisting of epoxy resin, bismaleimide resin, benzoxazine resin, phenol resin, urea resin, melamine resin, unsaturated polyester resin, polyurethane resin, diallyl phthalate resin, silicone resin, cyanate resin, polyimide resin, polyamideimide resin, and benzocyclobutene resin. The thermosetting resin may contain a resin curing agent such as a phenolic resin curing agent described later. From the viewpoint of improving curability, storage stability, heat resistance, moisture resistance, and chemical resistance, the thermosetting resin preferably contains an epoxy resin, and is more preferably an epoxy resin.

[0078] As the epoxy resin, any monomer, oligomer, or polymer having two or more epoxy groups in one molecule can be used, and there are no limitations on the molecular weight or molecular structure. Examples of the epoxy resin include biphenyl type epoxy resins; bisphenol type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, and tetramethylbisphenol F type epoxy resins; stilbene type epoxy resins; novolac type epoxy resins such as phenol novolac type epoxy resins and cresol novolac type epoxy resins; polyfunctional epoxy resins such as trisphenol type epoxy resins exemplified by triphenol methane type epoxy resins and alkyl-modified triphenol methane type epoxy resins; phenol aralkyl type epoxy resins having a phenylene skeleton, naphthol aralkyl type epoxy resins having a phenylene skeleton, and the like. the epoxy resins include one or more selected from the group consisting of phenol aralkyl-type epoxy resins such as phenol aralkyl-type epoxy resins having a biphenylene skeleton, and naphthol aralkyl-type epoxy resins having a biphenylene skeleton; naphthol-type epoxy resins such as dihydroxynaphthalene-type epoxy resins and epoxy resins obtained by glycidyl etherifying a dimer of dihydroxynaphthalene; triazine nucleus-containing epoxy resins such as triglycidyl isocyanurate and monoallyl diglycidyl isocyanurate; and bridged cyclic hydrocarbon compound-modified phenol-type epoxy resins such as dicyclopentadiene-modified phenol-type epoxy resins. Of these, from the viewpoint of suppressing warping of a molded article obtained by curing the thermosetting resin composition and improving the balance of various properties such as fluidity, filling property, heat resistance, and moisture resistance, one or more types selected from the group consisting of biphenyl aralkyl type epoxy resins, orthocresol novolac type epoxy resins, polybiphenylene skeleton-containing phenol aralkyl type epoxy resins, and bisphenol F type epoxy resins are preferably used.

[0079] The content of the thermosetting resin in the thermosetting resin composition is preferably 1 mass % or more, more preferably 2 mass % or more, and even more preferably 2.5 mass % or more, based on the total thermosetting resin composition, from the viewpoint of improving fluidity during molding and improving filling property and molding stability. On the other hand, from the viewpoint of improving the moisture resistance reliability and reflow resistance, and from the viewpoint of suppressing warping of the molded body, the content of the thermosetting resin is preferably 15 mass % or less, more preferably 14 mass % or less, and even more preferably 13 mass % or less, based on the entire thermosetting resin composition. In this embodiment, the content relative to the entire thermosetting resin composition refers to the content relative to the entire solid content of the thermosetting resin composition excluding the solvent when the thermosetting resin composition contains a solvent. The solid content of the thermosetting resin composition refers to the non-volatile content in the thermosetting resin composition, and refers to the remainder excluding volatile components such as water and solvent.

[0080] (hardening agent) The thermosetting resin composition may contain a curing agent. The curing agents can be roughly divided into three types: polyaddition type curing agents, catalyst type curing agents, and condensation type curing agents. These may be used alone or in combination of two or more.

[0081] The polyaddition type curing agent includes, for example, one or more selected from the group consisting of aliphatic polyamines such as diethylenetriamine (DETA), triethylenetetramine (TETA), and metaxylylenediamine (MXDA), aromatic polyamines such as diaminodiphenylmethane (DDM), m-phenylenediamine (MPDA), and diaminodiphenylsulfone (DDS), as well as polyamine compounds including dicyandiamide (DICY) and organic acid dihydrazides; alicyclic acid anhydrides such as hexahydrophthalic anhydride (HHPA), methyltetrahydrophthalic anhydride (MTHPA), and aromatic acid anhydrides such as trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), and benzophenonetetracarboxylic acid (BTDA); phenolic resin curing agents; polymercaptan compounds such as polysulfides, thioesters, and thioethers; isocyanate compounds such as isocyanate prepolymers and blocked isocyanates; and organic acids such as carboxylic acid-containing polyester resins.

[0082] Among these, the phenolic resin curing agent includes, for example, one or more selected from the group consisting of resol type phenolic resins; novolac type phenolic resins such as phenol novolac resins, cresol novolac resins, and bisphenol novolac; polyfunctional type phenolic resins such as polyvinylphenol and triphenolmethane type phenolic resins; modified phenolic resins such as terpene modified phenolic resins and dicyclopentadiene modified phenolic resins; phenol aralkyl type phenolic resins such as phenol aralkyl resins having at least one of a phenylene skeleton and a biphenylene skeleton, and naphthol aralkyl resins having at least one of a phenylene skeleton and a biphenylene skeleton; and bisphenol compounds such as bisphenol A and bisphenol F. Among these, from the viewpoint of suppressing warpage of the molded body, it is more preferable to include novolac type phenolic resins, multifunctional type phenolic resins, and phenol aralkyl type phenolic resins. In addition, phenol novolac resins, phenol aralkyl resins having a biphenylene skeleton, and triphenylmethane type phenolic resins modified with formaldehyde can also be preferably used.

[0083] The catalyst type curing agent includes, for example, one or more selected from the group consisting of imidazole compounds such as 2-methylimidazole, 2-ethyl-4-methylimidazole (EMI24), and Lewis acids such as BF3 complexes.

[0084] The condensation type curing agent includes, for example, one or more selected from the group consisting of urea resins such as methylol group-containing urea resins; and melamine resins such as methylol group-containing melamine resins.

[0085] When the thermosetting resin composition is in a liquid state, from the viewpoint of improving heat resistance, the thermosetting resin composition preferably contains one or more curing agents selected from the group consisting of polyamine compounds and acid anhydrides, and more preferably contains one or more compounds selected from acid anhydrides. When the thermosetting resin composition is in the form of particles or a sheet, it is more preferable that the composition contains a phenol resin curing agent from the viewpoint of improving the balance of flame resistance, moisture resistance, electrical properties, curability, storage stability, and the like.

[0086] From the viewpoint of realizing excellent fluidity during molding and improving filling property and moldability, the content of the curing agent in the thermosetting resin composition is preferably 0.5 mass % or more, more preferably 1 mass % or more, even more preferably 2 mass % or more, and still more preferably 3 mass % or more, based on the entire thermosetting resin composition. On the other hand, from the viewpoint of improving the moisture resistance reliability and reflow resistance of the electronic component and from the viewpoint of suppressing warping of the obtained molded body, the content of the curing agent is preferably 9 mass % or less, more preferably 8 mass % or less, and even more preferably 7 mass % or less, based on the entire thermosetting resin composition.

[0087] (Inorganic filler) The inorganic filler includes, for example, one or more materials selected from the group consisting of fused silica such as fused crushed silica and fused spherical silica, silica (silicon dioxide) such as crystalline silica and amorphous silica, alumina, aluminum hydroxide, silicon nitride, and aluminum nitride. From the viewpoint of making the mechanical properties or thermal properties of the cured product of the thermosetting resin composition favorable, the inorganic filler preferably includes silica such as fused crushed silica, fused spherical silica, and crystalline silica, and more preferably is silica.

[0088] Inorganic filler d 50 From the viewpoint of favorable fluidity, the particle size is, for example, 1 μm or more, preferably 5 μm or more, more preferably 10 μm or more, even more preferably 12 μm or more, and still more preferably 15 μm or more. On the other hand, from the viewpoint of reducing the plating wiring width after laser processing, the inorganic filler d 50 The particle size is preferably 40 μm or less, more preferably 30 μm or less, even more preferably 27 μm or less, and even more preferably 25 μm or less.

[0089] Here, the particle size distribution of the inorganic filler can be measured on a volume basis by using a commercially available laser diffraction particle size distribution measuring device (for example, SALD-7000, manufactured by Shimadzu Corporation).

[0090] From the viewpoint of improving dimensional stability, the content of the inorganic filler in the thermosetting resin composition is 40 mass% or more, preferably 50 mass% or more, more preferably 60 mass% or more, even more preferably 65 mass% or more, and still more preferably 70 mass% or more, based on the entire thermosetting resin composition. On the other hand, from the viewpoint of obtaining favorable viscosity and fluidity, the content of the inorganic filler is 85 mass % or less, preferably 80 mass % or less, more preferably 78 mass % or less, even more preferably 75 mass % or less, and still more preferably 73 mass % or less, based on the entire thermosetting resin composition.

[0091] (Non-conductive metal compounds that form metal nuclei when irradiated with active energy rays) A non-conductive metal compound that forms a metal nucleus by irradiation with active energy rays (hereinafter, also simply referred to as a "non-conductive metal compound") is a non-conductive metal compound that forms a metal nucleus by irradiation with active energy rays. Such a compound acts as an LDS additive. The non-conductive metal compound is not limited as long as it can form a metal nucleus by irradiation with active energy rays. Although the detailed mechanism is unclear, it is considered that when such a non-conductive metal compound is irradiated with active energy rays such as a YAG laser having an absorbable wavelength range, the metal nucleus is activated (for example, reduced) to generate a metal nucleus that can be plated with metal. Then, when the surface of the cured product of the thermosetting resin composition in which the non-conductive metal compound is dispersed is irradiated with active energy rays, a seed region having a metal nucleus that can be plated with metal is formed on the irradiated surface. By using the obtained seed region, it is possible to form a plating pattern such as a circuit on the surface of the cured product of the thermosetting resin composition.

[0092] The non-conductive metal compound includes, for example, one or more selected from the group consisting of (i) spinel-type metal oxides, (ii) metal oxides selected from Groups 3 to 12 of the periodic table, which have two or more adjacent transition metal elements, and (iii) tin-containing oxides.

[0093] In the above (i), the spinel structure is one of the typical crystal structures found in AB2O4 type compounds (A and B are metal elements) in double oxides. The spinel structure may be either a normal spinel structure or an inverse spinel structure (B(AB)O4) (where A and B are partially interchanged), but the normal spinel structure is more preferably used. In this case, A in the normal spinel structure may be copper.

[0094] The metal atom constituting the spinel metal oxide can be, for example, copper or chromium. In other words, the non-conductive metal compound can contain a spinel metal oxide containing copper or chromium. For example, copper can be used as the metal atom from the viewpoint of improving adhesion with a copper plating pattern.

[0095] In addition to copper and chromium, the metal atoms may contain trace amounts of metal atoms such as antimony, tin, lead, indium, iron, cobalt, nickel, zinc, cadmium, silver, bismuth, arsenic, manganese, magnesium, and calcium. These trace metal atoms may be present as oxides. The content of each trace metal atom may be 0.001 mass% or less based on the total metal atoms in the metal oxide.

[0096] Spinel-type metal oxides have high thermal stability and can be durable in acidic or alkaline aqueous metallization baths. For example, by appropriately controlling the dispersibility of the thermosetting resin composition, the spinel-type metal oxide can be present in a highly oxidized state in the unirradiated area on the surface of the cured product of the thermosetting resin composition. An example of such a spinel-type metal oxide is described in JP-A-2004-534408.

[0097] The metal oxide having the transition metal element (ii) is a metal oxide having two or more transition metal elements selected from Groups 3 to 12 of the periodic table and adjacent to each other. Here, the metal belonging to the transition metal element can be expressed as containing a metal of Group n and a metal of Group n+1 of the periodic table. The metal oxide having the transition metal element may be a single oxide of these metals or a combination of two or more of them.

[0098] Examples of metals belonging to group n of the periodic table include group 3 (scandium, yttrium), group 4 (titanium, zirconium, etc.), group 5 (vanadium, niobium, etc.), group 6 (chromium, molybdenum, etc.), group 7 (manganese, etc.), group 8 (iron, ruthenium, etc.), group 9 (cobalt, rhodium, iridium, etc.), group 10 (nickel, palladium, platinum), group 11 (copper, silver, gold, etc.), group 12 (zinc, cadmium, etc.), and group 13 (aluminum, gallium, indium, etc.).

[0099] Examples of metals in group n+1 of the periodic table include group 4 (titanium, zirconium, etc.), group 5 (vanadium, niobium, etc.), group 6 (chromium, molybdenum, etc.), group 7 (manganese, etc.), group 8 (iron, ruthenium, etc.), group 9 (cobalt, rhodium, iridium, etc.), group 10 (nickel, palladium, platinum), group 11 (copper, silver, gold, etc.), group 12 (zinc, cadmium, etc.), and group 13 (aluminum, gallium, indium, etc.). An example of the metal oxide containing such a transition metal element is described in JP-A-2004-534408.

[0100] The tin-containing oxide (iii) is a metal oxide containing at least tin. The metal atoms constituting the tin-containing oxide may contain antimony in addition to tin. Such a tin-containing oxide may contain tin oxide and antimony oxide. More specifically, the metal components contained in the tin-containing oxide may be 90% by mass or more of tin and 5% by mass or more of antimony. This tin-containing oxide may further contain lead and / or copper as the metal component. Specifically, the metal components contained in the tin-containing oxide may be, for example, 90% by mass or more of tin, 5 to 9% by mass of antimony, 0.01 to 0.1% by mass of lead, and 0.001 to 0.01% by mass of copper. Such a tin-containing oxide may contain, for example, tin oxide, antimony oxide, and one or more of lead oxide and copper oxide. The tin-containing oxide may contain trace metal atoms exemplified in the spinel-type metal oxide. The tin-containing oxide may be used in combination with the above-mentioned (i) spinel-type metal oxide or the above-mentioned (ii) metal oxide having a transition metal element.

[0101] The content of the non-conductive metal compound in the thermosetting resin composition is, for example, 2% by mass or more, preferably 4% by mass or more, and more preferably 8% by mass or more, based on the entire thermosetting resin composition, from the viewpoint of improving plating characteristics in the cured product of the thermosetting resin composition. Also, from the viewpoint of suppressing a decrease in insulation and an increase in dielectric tangent in the cured product of the thermosetting resin composition, and from the viewpoint of improving the fluidity of the thermosetting resin composition when the shape of the non-conductive metal compound is non-spherical, the content of the non-conductive metal compound is, for example, 20% by mass or less, preferably 18% by mass or less, and more preferably 15% by mass or less, based on the entire thermosetting resin composition.

[0102] Furthermore, from the viewpoint of improving the resin mechanical properties and resin strength, the total content of the inorganic filler and the non-conductive metal compound in the thermosetting resin composition is preferably 70 mass % or more, more preferably 75 mass % or more, even more preferably 80 mass % or more, and still more preferably 82 mass % or more, based on the entire thermosetting resin composition. On the other hand, from the viewpoint of improving moldability, the total content of the inorganic filler and the non-conductive metal compound is preferably 98 mass % or less, more preferably 95 mass % or less, and even more preferably 90 mass % or less, based on the entire thermosetting resin composition.

[0103] (Other Ingredients) In this embodiment, the thermosetting resin composition may contain components other than the above-mentioned components. For example, the thermosetting resin composition may further contain one or more selected from the group consisting of a coupling agent, a curing accelerator, and a (meth)acrylic compound.

[0104] (Coupling Agent) From the viewpoint of improving the moldability of the second sealing layer, the thermosetting resin composition preferably further contains a coupling agent. From the same viewpoint, the coupling agent preferably contains one or more selected from the group consisting of mercaptosilane, aminosilane, and epoxysilane. From the viewpoint of continuous moldability, mercaptosilane is preferred, from the viewpoint of fluidity, secondary aminosilane is preferred, and from the viewpoint of adhesion, epoxysilane is preferred.

[0105] Among these, examples of epoxy silanes include γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and the like, with γ-glycidoxypropylmethyldimethoxysilane being preferred.

[0106] Examples of aminosilanes include phenylaminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, N-phenyl-γ-aminopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltriethoxysilane, N-(6-aminohexyl)3-aminopropyltrimethoxysilane, and N-(3-(trimethoxysilylpropyl)-1,3-benzenedimethanane, with N-phenyl-γ-aminopropyltriethoxysilane being preferred. The primary amino site of the aminosilane may be protected by reacting it with a ketone or aldehyde to be used as a latent aminosilane coupling agent. The aminosilane may also have a secondary amino group.

[0107] Examples of mercaptosilanes include γ-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, and silane coupling agents that exhibit the same function as a mercaptosilane coupling agent upon thermal decomposition, such as bis(3-triethoxysilylpropyl)tetrasulfide and bis(3-triethoxysilylpropyl)disulfide, with γ-mercaptopropyltrimethoxysilane being preferred.

[0108] These silane coupling agents may be hydrolyzed in advance and then blended in. These silane coupling agents may be used alone or in combination of two or more.

[0109] The content of the coupling agent in the thermosetting resin composition is preferably 0.01 mass % or more, more preferably 0.05 mass % or more, and even more preferably 0.1 mass % or more, based on the total amount of the thermosetting resin composition, from the viewpoint of improving moldability by increasing the flow length of the thermosetting resin composition. On the other hand, from the viewpoint of suppressing an increase in water absorption of the cured product of the thermosetting resin composition and obtaining good rust prevention properties, the content of the coupling agent is preferably 1 mass % or less, more preferably 0.8 mass % or less, even more preferably 0.6 mass % or less, and even more preferably 0.4 mass % or less, based on the total amount of the thermosetting resin composition.

[0110] (Cure accelerator) The curing accelerator may be any accelerator that accelerates the crosslinking reaction between the thermosetting resin and the curing agent, and any accelerator that is generally used in thermosetting resin compositions may be used.

[0111] The curing accelerator may contain one or more of phosphorus atom-containing compounds such as organic phosphines, tetra-substituted phosphonium compounds, phosphobetaine compounds, adducts of phosphine compounds and quinone compounds, and adducts of phosphonium compounds and silane compounds; tertiary amine compounds such as amidines, exemplified by 1,8-diazabicyclo[5.4.0]undecene-7 and benzyldimethylamine (BDMA), and 2,4,6-trisdimethylaminomethylphenol (DMP-30); and nitrogen atom-containing compounds such as tertiary amines and quaternary salts of the above amidines and amines. Among these, it is more preferable to contain a phosphorus atom-containing compound from the viewpoint of improving the curability. In addition, it is more preferable to contain a compound having latency, such as a tetra-substituted phosphonium compound, a phosphobetaine compound, an adduct of a phosphine compound and a quinone compound, or an adduct of a phosphonium compound and a silane compound, from the viewpoint of improving the balance between moldability and curability. From a similar viewpoint, the curing accelerator preferably includes one or more selected from triphenylphosphine, tetraphenylphosphonium bis(naphthalene-2,3-dioxy)phenylsilicate, and tetraphenylphosphonium-4,4′-sulfonyldiphenolate.

[0112] When the thermosetting resin composition contains a curing accelerator, the content of the curing accelerator is preferably 0.1 mass % or more, more preferably 0.15 mass % or more, and even more preferably 0.25 mass % or more, based on the total amount of the thermosetting resin composition, from the viewpoint of effectively improving the curability during molding. On the other hand, from the viewpoint of improving fluidity during molding, the content of the curing accelerator is preferably 1 mass % or less, more preferably 0.8 mass % or less, and even more preferably 0.5 mass % or less, based on the total thermosetting resin composition.

[0113] ((Meth)acrylic compounds) Examples of the (meth)acrylic compound include a (meth)acrylic resin, a (meth)acrylic oligomer, a (meth)acrylic monomer, etc. When the thermosetting resin composition contains a (meth)acrylic compound, the effect of suppressing cracking or chipping of the sheet when the thermosetting resin composition is formed into a sheet can be improved. From the viewpoint of preventing cracks and chips in the sheet, the (meth)acrylic compound preferably contains a (meth)acrylic monomer. The (meth)acrylic monomer is preferably a monomer having a boiling point higher than that of the solvent used in producing the sheet-shaped thermosetting resin composition of the present embodiment. In order to suppress volatilization of the (meth)acrylic monomer in the manufacturing process of the sheet-shaped thermosetting resin composition and to generate an interaction between the (meth)acrylic monomer, the solvent, and the resin composition through a chemical reaction, the boiling point of the (meth)acrylic monomer is preferably more than 100° C., and more preferably 110° C. or higher. This allows the sheet-shaped thermosetting resin composition to have excellent flexibility to an extent that the workability during use can be improved.

[0114] Examples of (meth)acrylic monomers include 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxypropyl succinic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl methyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl methyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl methyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxypropyl phthalic acid, 2-(meth)acryloyloxyethyl tetra ... p) acryloyloxypropyl tetrahydrophthalic acid, 2-(meth)acryloyloxyethyl methyl tetrahydrophthalic acid, 2-(meth)acryloyloxypropyl methyl tetrahydrophthalic acid, 2-hydroxy-1,3-di(meth)acryloxypropane, tetramethylolmethane tri(meth)acrylate, 2-hydroxyethyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, 2-hydroxybutyl(meth)acrylate, glycerin di(meth)acrylate, 2-hydroxy-3-(meth)acryloyloxypropyl(meth)acrylate, 1,4-Cyclohexanedimethanol mono(meth)acrylate, ethyl-α-(hydroxymethyl)(meth)acrylate, 4-hydroxybutyl(meth)acrylate, methyl(meth)acrylate, ethyl(meth)acrylate, n-butyl(meth)acrylate, isobutyl(meth)acrylate, tertiary butyl(meth)acrylate, isodecyl(meth)acrylate, lauryl(meth)acrylate, tridecyl(meth)acrylate, cetyl(meth)acrylate, stearyl(meth)acrylate, isoamyl(meth)acrylate, isostearyl(meth)acrylate, behenyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, other alkyl(meth)acrylates, cyclohexyl(meth)acrylate, tertiary butylcyclohexyl(meth)acrylate, tetrahydrofurfuryl(meth)acrylate, benzyl(meth)acrylate, phenoxyethyl(meth)acrylate acrylate, isobornyl (meth)acrylate, glycidyl (meth)acrylate, trimethylolpropane tri(meth)acrylate, zinc mono(meth)acrylate, zinc di(meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, neopentyl glycol (meth)acrylate, trifluoroethyl (meth)acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, 2,2, 3,3,4,4-Hexafluorobutyl (meth)acrylate, perfluorooctyl (meth)acrylate, perfluorooctylethyl (meth)acrylate, ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,10-Decanediol di(meth)acrylate, tetramethylene glycol di(meth)acrylate, methoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxypolyalkylene glycol mono(meth)acrylate, octoxypolyalkylene glycol mono(meth)acrylate, lauroxypolyalkylene glycol mono(meth)acrylate, stearoxypolyalkylene glycol mono(meth)acrylate, aryloxypolyalkylene glycol mono(meth)acrylate, nonylphenoxypolyalkylene glycol mono(meth)acrylate, N, Examples of polyfunctional monomers include N'-methylene bis(meth)acrylamide, N,N'-ethylene bis(meth)acrylamide, 1,2-di(meth)acrylamidoethylene glycol, di(meth)acryloyloxymethyl tricyclodecane, 2-(meth)acryloyloxyethyl, N-(meth)acryloyloxyethyl maleimide, N-(meth)acryloyloxyethyl hexahydrophthalimide, N-(meth)acryloyloxyethyl phthalimide, N-vinyl-2-pyrrolidone, ethoxylated bisphenol A (meth)acrylate, propoxylated bisphenol A (meth)acrylate, and trimethylolpropane tri(meth)acrylate.

[0115] From the viewpoint of suppressing cracking or chipping of the sheet, the content of the (meth)acrylic monomer in the thermosetting resin composition is preferably 0.01 mass % or more, more preferably 0.05 mass % or more, and even more preferably 0.5 mass % or more, based on the entire thermosetting resin composition. From the same viewpoint, the content of the (meth)acrylic monomer is preferably 3% by mass or less, more preferably 2% by mass or less, and further preferably 1% by mass or less, based on the entire thermosetting resin composition.

[0116] The thermosetting resin composition may contain at least one type of organic, heat-stable metal chelate complex salt in addition to the non-conductive metal compound described above. The thermosetting resin composition may contain additives such as surfactants, silicones, release agents, flame retardants, ion scavengers, colorants, low stress materials, adhesion aids, and antioxidants, as necessary. These may be used alone or in combination of two or more. The amount of each of these components in the thermosetting resin composition can be about 0.01 to 10% by mass based on the entire thermosetting resin composition.

[0117] In this embodiment, the method for producing the thermosetting resin composition can be selected depending on the shape and ingredients of the thermosetting resin composition. For example, a method for producing a sheet-shaped thermosetting resin composition may include applying a varnish of the thermosetting resin composition prepared by blending the respective components onto a film, drying the varnish to form a sheet, and then volatilizing the solvent. Examples of methods for applying the varnish include a coating method using a coater such as a comma coater or a die coater, and a printing method such as stencil printing or gravure printing. The thermosetting resin composition may also be extruded and formed into a sheet.

[0118] Examples of a method for producing a liquid thermosetting resin composition include a method in which each component, additive, etc. are dispersed and kneaded using an apparatus such as a planetary mixer, a three-roll mill, a two-roll mill, or a mortar and pestle mixer, and then the mixture is degassed under vacuum.

[0119] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. For example, in the above embodiment, the sealing material has a two-layer structure of the first sealing layer 105 and the second sealing layer, but there is no limit to the number of sealing layers provided outside the first sealing layer 105, and for example, a third sealing layer may be further provided. In this case, for example, it is preferable that the outermost sealing layer is composed of a cured product of the thermosetting resin composition for LDS. In the first and second embodiments, examples using a sheet-like and liquid thermosetting resin composition for LDS, respectively, have been mainly described. However, the form of the thermosetting resin composition for LDS is not limited thereto, and the composition may be in other forms, such as granular form.

[0120] Below, examples of reference forms are given. (Reference form A) A 1. A substrate; A semiconductor element mounted on the substrate; a first encapsulant that encapsulates the semiconductor element; A second sealing material that covers a surface of the first sealing material and is made of a cured product of a thermosetting resin composition for LDS (LASER DIRECT STRUCTURE), Including, The thermosetting resin composition for LDS, A thermosetting resin; An inorganic filler; a non-conductive metal compound which forms a metal nucleus when irradiated with active energy rays; 13. A semiconductor device comprising: A 2. The first encapsulant does not contain the non-conductive metal compound; A 1. A semiconductor device according to claim 1. A 3. The thickness of the second sealing material is 30 μm or more and 500 μm or less. A 1. Or A 2. The semiconductor device according to claim 1. A 4. The linear expansion coefficient of the second encapsulating material in a temperature range below the glass transition temperature, as measured by thermomechanical analysis (TMA), is 7 ppm / °C or more and 20 ppm / °C or less. A 1.~ A 3. A semiconductor device according to any one of claims 1 to 3. A 5. The linear expansion coefficient of the first encapsulating material in a temperature range below the glass transition temperature, as measured by thermomechanical analysis (TMA), is 7 ppm / °C or more and 20 ppm / °C or less. A 1.~ A4. A semiconductor device according to any one of claims 1 to 4. A 6. The second encapsulant encapsulates the entire surface of the first encapsulant on top of the substrate; A 1.~ A 5. A semiconductor device according to any one of claims 1 to 5. A 7. The thermosetting resin composition for LDS further contains a coupling agent. A 1.~ A 6. A semiconductor device according to any one of claims 1 to 6. A 8. A step of preparing a structure in which a semiconductor element mounted on a substrate is sealed with a first sealing material; forming a second sealing material composed of a cured product of a thermosetting resin composition for LDS (LASER DIRECT STRUCTURE) on the first sealing material; Including, The thermosetting resin composition for LDS, A thermosetting resin; An inorganic filler; a non-conductive metal compound which forms a metal nucleus when irradiated with active energy rays; A method for manufacturing a semiconductor device comprising the steps of: (Reference form B) B1. Electronic components and a first sealing material covering at least a portion of a surface of the electronic component; a second sealing material covering at least a portion of the surface of the electronic component and the first sealing material; Including, At least one of the first and second sealing materials is made of a cured product of a thermosetting resin composition for LDS (LASER DIRECT STRUCTURE), The thermosetting resin composition for LDS is A thermosetting resin; An inorganic filler; a non-conductive metal compound which forms a metal nucleus when irradiated with active energy rays; 23. An electronic device comprising: B2. A substrate; A semiconductor element mounted on the substrate; a first encapsulant that encapsulates the semiconductor element; A second sealing material that covers a surface of the first sealing material and is made of a cured product of a thermosetting resin composition for LDS (LASER DIRECT STRUCTURE), Including, The thermosetting resin composition for LDS is A thermosetting resin; An inorganic filler; a non-conductive metal compound which forms a metal nucleus when irradiated with active energy rays; The electronic device is a semiconductor device comprising: B3. The electronic device of B1. or B2., wherein the first encapsulant does not include the non-conductive metal compound. B4. The electronic device according to any one of B1 to B3, wherein the thickness of the second sealing material is 30 μm or more and 500 μm or less. B5. An electronic device described in any one of B1 to B4, wherein the second sealing material has a linear expansion coefficient of 7 ppm / °C or more and 20 ppm / °C or less in a temperature range below the glass transition temperature, as measured by thermomechanical analysis (TMA). B6. An electronic device according to any one of B1 to B5, wherein the first sealing material has a linear expansion coefficient of 7 ppm / °C or more and 20 ppm / °C or less in a temperature range below the glass transition temperature, as measured by thermomechanical analysis (TMA). B7. The electronic device according to any one of B1. to B6., wherein the second encapsulant encapsulates the entire surface of the first encapsulant on top of the substrate. B8. An electronic device according to any one of B1 to B7, wherein the thermosetting resin composition for LDS further contains a coupling agent. B9. A process of preparing a structure in which a semiconductor element mounted on a substrate is sealed with a first sealing material; forming a second sealing material composed of a cured product of a thermosetting resin composition for LDS (LASER DIRECT STRUCTURE) on the first sealing material; Including, The thermosetting resin composition for LDS, A thermosetting resin; An inorganic filler; a non-conductive metal compound which forms a metal nucleus when irradiated with active energy rays; A method for manufacturing a semiconductor device comprising the steps of: EXAMPLES

[0121] Hereinafter, the embodiments will be described in detail with reference to examples, but the present invention is not limited to the description of these examples.

[0122] Example 1 A sheet-shaped thermosetting resin composition for LDS was prepared according to the composition shown in Table 1. Specifically, first, the raw material components except for the solvent and acrylic monomer were kneaded according to the composition shown in Table 1 below to obtain a resin mixture, which was then dissolved in a predetermined amount of propylene glycol monomethyl ether and the amount of acrylic monomer shown in Table 1 to prepare a varnish. Next, the prepared varnish was applied to the upper surface of a PET film (Unitika Co., Ltd., TR1) using a die coater, and then dried until propylene glycol monomethyl ether was evaporated. In this way, the resin sheet of this example was produced. The thickness of the obtained resin sheet was 100 μm, and the width was 500 mm.

[0123] (Examples 2 and 3) A granular thermosetting resin composition for LDS was prepared according to the formulation shown in Table 2. The raw materials shown in Table 2 were mixed at room temperature using a mixer, and then roll-kneaded at 70 to 100° C. The resulting kneaded product was then cooled and pulverized to obtain a granular thermosetting resin composition.

[0124] Example 4 A liquid thermosetting resin composition for LDS was prepared according to the formulation shown in Table 3. The raw materials shown in Table 3 were placed in a beaker and mixed with a spatula, then kneaded three times with a triple roll, and then placed in a beaker and degassed in a vacuum oven (room temperature, 5 mmHg) for 10 minutes to obtain a liquid thermosetting resin composition.

[0125] Details of the components listed in Tables 1 to 3 are shown below. (thermosetting resin) Epoxy resin 1: Biphenyl aralkyl type epoxy resin, NC-3000L, manufactured by Nippon Kayaku Co., Ltd. Epoxy resin 2: Orthocresol novolac type epoxy resin, EOCN-1020, manufactured by Nippon Kayaku Co., Ltd. Epoxy resin 3: phenol aralkyl type epoxy resin containing biphenylene skeleton, NC3000, manufactured by Nippon Kayaku Co., Ltd. Epoxy resin 4: Bisphenol F type epoxy resin, YDF-870GS, manufactured by Tohto Kasei Co., Ltd. (hardener) Hardener 1: Trihydroxyphenylmethane type phenolic resin, HE910-20, manufactured by Air Water Chemical Co., Ltd. Hardener 2: Novolac type phenolic resin, PR-HF-3, manufactured by Sumitomo Bakelite Co., Ltd. Hardener 3: Phenol aralkyl resin containing biphenylene skeleton, MEH-7851SS, manufactured by Meiwa Kasei Co., Ltd. Hardener 4: Acid anhydride, HN-2200R, Hitachi Chemical (Cure accelerator) Curing accelerator 1: Triphenylphosphine Curing accelerator 2: Tetraphenylphosphonium bis(naphthalene-2,3-dioxy)phenylsilicate Curing accelerator 3: Tetraphenylphosphonium-4,4'-sulfonyldiphenolate (Inorganic filler) Inorganic filler 1: Fused spherical silica, MUF-046, manufactured by Tatsumori Co., Ltd., average particle size 4.1 μm Inorganic filler 2: amorphous silica / crystalline silica, MUF-4V, manufactured by Tatsumori Co., Ltd., average particle size 3.8 μm Inorganic filler 3: silicon dioxide, SC-2500-SQ, manufactured by Admatechs Co., Ltd., average particle size 0.6 μm Inorganic filler 4: silicon dioxide, SC-5500-SQ, manufactured by Admatechs Co., Ltd., average particle size 1.6 μm Inorganic filler 5: silicon dioxide, MSR-SC3-TS, manufactured by Tatsumori Co., Ltd., average particle size 12 μm Inorganic filler 6: silicon dioxide, SO-E2 / 24C, manufactured by Admatechs, average particle size 0.5 μm (Acrylic Compounds) Acrylic monomer 1: Trimethylolpropane trimethacrylate, Light Ester TMP, manufactured by Kyoeisha Chemical Co., Ltd., boiling point 200°C or higher (Additives) Additive 1 (non-conductive metal compound): Inorganic composite oxide, Black 3702, manufactured by Asahi Chemical Industry Co., Ltd. Additive 2: Nonionic surfactant, BYK-A506, manufactured by BYK-Chemie (Coloring agent) Colorant 1: Carbon black, Carbon #5, manufactured by Mitsubishi Chemical Corporation (Coupling Agent) Coupling agent 1: 3-mercaptopropyltrimethoxysilane, S810, manufactured by Chisso Corporation Coupling agent 2: 3-glycidoxypropyltrimethoxysilane, S510, manufactured by Chisso Corporation Coupling agent 3: N-phenyl-γ-aminopropyltrimethoxysilane, CF-4083, manufactured by Dow Corning Toray Co., Ltd. Coupling agent 4: γ-glycidylpropyltrimethoxysilane, KBM-403E, manufactured by Shin-Etsu Chemical Co., Ltd. (Release agent) Release agent 1: Glycerol trimontanic acid ester, Lycorb-WE-4, Clariant Japan (silicone) Silicone 1: Polyoxyalkylene epoxy modified dimethylpolysiloxane, FZ-3730, manufactured by Dow Corning Toray Co., Ltd. Silicone 2: Silicone rubber composite particles, KMP600, manufactured by Shin-Etsu Chemical Co., Ltd. (Low stress material) Low stress material 1: Epoxidized polybutadiene, JP-200, manufactured by Nippon Soda Co., Ltd.

[0126] (Measurement of size of inorganic filler) For the examples listed in Table 3, the d 50 was measured using a laser diffraction particle size distribution analyzer (Shimadzu Corporation, SALD-7000).

[0127] (Viscosity of Thermosetting Resin Composition) The viscosity of the thermosetting resin compositions obtained in the examples shown in Table 3 was measured using an E-type viscometer (Toki Sangyo Co., Ltd., TVB-10) equipped with a 3°×R7.7 type cone at 25° C. and 2.5 rpm.

[0128] (glass transition temperature (Tg), linear expansion coefficient) The thermosetting resin composition obtained in each example was compression molded under conditions of a molding temperature of 175°C for 3 minutes and a PMC of 175°C for 4 hours to obtain a cured product. The glass transition temperature and linear expansion coefficient of the cured material were measured using a TMA (Hitachi High-Technologies Corporation, TMA6100) at a heating rate of 10°C / min over the temperature range of 30°C to 350°C. In each table, the linear expansion coefficient of the cured material in the temperature range below Tg is also referred to as CTE1.

[0129] (evaluation) For the thermosetting resin composition obtained in each example, an evaluation sample was prepared by the following method and evaluated.

[0130] (Moldability) The thermosetting resin composition obtained in each example was used to form a second sealing layer. First, the first thermosetting resin composition was molded using a compression molding machine under the conditions of 175°C / 180 seconds to obtain a molded product of 240 mm x 70 mm. Here, Sumicon (registered trademark) EME-G700H Type C manufactured by Sumitomo Bakelite Co., Ltd. was used as the first thermosetting resin composition. The cured product of the thermosetting resin composition obtained in each example was laminated on the obtained molded product to obtain a molded product. The manufacturing method and conditions are as follows. Example 1: A sheet-shaped encapsulating material prepared according to the composition shown in Table 1 was compression molded using a compression molding machine at a molding thickness of 50 μm and at 175° C. for 180 seconds, using the first thermosetting composition prepared earlier as a substrate. Examples 2 and 3: The granular sealing material prepared according to the formulation shown in Table 2 was compression molded using a compression molding machine at a molding thickness of 100 μm and 175° C. / 180 seconds, using the first thermosetting composition prepared previously as the substrate. Example 4: The liquid encapsulant prepared according to the formulation shown in Table 3 was compression molded using a compression molding machine at a molding thickness of 100 μm and at 175° C. for 180 seconds, using the first thermosetting composition prepared earlier as a substrate.

[0131] The obtained molded products were observed and evaluated according to the following criteria. ◎: No internal or external voids ○: Internal voids observed, but no external voids △: External voids are observed ×: Some filling is not completed

[0132] (warp) The thermosetting resin compositions obtained in the examples shown in Table 3 were used to form the second sealing layer. First, the first thermosetting resin composition was molded using a compression molding machine under the conditions of 175°C / 180 seconds to obtain a molded product of 240 mm x 70 mm. Here, Sumicon (registered trademark) EME-G700H Type C manufactured by Sumitomo Bakelite Co., Ltd. was used as the first thermosetting resin composition. The obtained molded product was compression molded under the conditions of 175°C / 180 seconds to obtain a molded product with a second sealing layer laminated thereon. The magnitude of warpage of the obtained molded product was evaluated based on the height from the reference plane to the bottom end of the molded product. The evaluation criteria are shown below. ○: Height is 5mm or less △: Height is over 5mm and 10mm or less ×: Height exceeds 10 mm

[0133] (Plating ability) The resin composition obtained in each example was molded and cured at 150° C. to obtain a cured product. The surface of the obtained cured product was irradiated with a YAG laser (wavelength 1064 nm) to perform electroless copper plating, and the plating adhesion in the laser irradiated area was evaluated according to the following criteria. ◎: No unevenness on the plating surface ○: Some unevenness is visible on the plated surface, but there are no unplated areas. △: Unevenness is visible on the plated surface, but there are no unplated areas. ×: Severe unevenness is visible on the plating surface and there are areas where the plating has not adhered.

[0134] (L / S) Molded products were prepared in the same manner as in the plating adhesion evaluation described above, and the surfaces of the obtained resin molded products were irradiated with a YAG laser (wavelength 1064 nm) to create circuits of each line width. The circuit with the narrowest pitch that achieved conductivity is shown in each table as the result for each example. The evaluation standards were seven levels: L / S = 20, 30, 40, 50, 75, 100 and 200 μm.

[0135] [Table 1]

[0136] [Table 2]

[0137] [Table 3] [Explanation of symbols]

[0138] 10 Thin film inductors 12, 38 Soft magnetic thin film 13 Insulating layer 14 MID circuit 15, 34 Opening 16, 36 copper layers 32 MID membrane 100 Semiconductor device 101 Substrate 103 Semiconductor elements 105 First sealing layer 107 Second sealing layer 109 Lead Frame 110 Semiconductor device 111 Second sealing layer

Claims

1. A substrate; A semiconductor element mounted on the substrate; a first encapsulant that encapsulates the semiconductor element and is composed of a cured product of a curable resin composition; a second sealing material covering a surface of the first sealing material and made of a compression molded cured product of a thermosetting resin composition for LDS (LASER DIRECT STRUCTURE); Including, The thermosetting resin composition for LDS, A thermosetting resin; An inorganic filler; a non-conductive metal compound which forms a metal nucleus when irradiated with active energy rays; Including, The thickness of the second sealing material is 30 μm or more and 500 μm or less, An electronic device which is a semiconductor device, wherein the second sealing material has a linear expansion coefficient of 7 ppm / ° C. or more and 20 ppm / ° C. or less in a temperature range below the glass transition temperature as measured by thermomechanical analysis (TMA).

2. The electronic device of claim 1 , wherein the first encapsulant is free of the non-conductive metal compound.

3. 3 . The electronic device according to claim 1 , wherein the first sealing material has a linear expansion coefficient of 7 ppm / ° C. or more and 20 ppm / ° C. or less in a temperature range below a glass transition temperature, as measured by thermomechanical analysis (TMA).

4. 4. The electronic device of claim 1, wherein the second encapsulant encapsulates the entire surface of the first encapsulant on top of the substrate.

5. The electronic device according to claim 1 , wherein the thermosetting resin composition for LDS further comprises a coupling agent.

6. A method for manufacturing an electronic device according to any one of claims 1 to 5, comprising: preparing a structure in which the semiconductor element mounted on the substrate is sealed with the first sealing material; forming the second sealing material composed of the compression molded cured product of the thermosetting resin composition for LDS on the first sealing material; A method for manufacturing an electronic device, comprising:

Citation Information

Patent Citations

  • Semiconductor device

    JP2008270454A

  • Semiconductor package

    JP2013038410A

  • Semiconductor device manufacturing method and semiconductor device

    JP2014192170A

  • Fiber-reinforced resin material, resin molding, resin molding with plated layer, method of producing resin molding with plated layer, and method of producing fiber-reinforced resin material

    JP2015134903A

  • Coating composition, composite material prepared by using the coating composition, and method for preparing the same