Wire Harness
By integrating a nitrogen-containing monomer into the resin composition of wire harness waterproof parts, the adhesion and waterproof integrity of wire harnesses are maintained in high temperature and high humidity environments, addressing plasticizer migration issues.
Patent Information
- Application Number
- JP2020215820
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-24
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-12-24
AI Technical Summary
Existing wire harnesses using urethane (meth)acrylate for waterproofing in high temperature and high humidity environments face adhesion issues due to plasticizer migration from the insulation coating, leading to decreased waterproof performance.
Incorporating a nitrogen-containing monomer into the resin composition of the waterproof part, specifically a urethane (meth)acrylate oligomer, to enhance the solubility parameter and prevent plasticizer migration, maintaining adhesion and waterproof integrity.
The addition of a nitrogen-containing monomer to the resin composition effectively suppresses plasticizer migration, ensuring high adhesion and waterproof performance even in harsh environmental conditions.
Smart Images

Figure 0007563171000012 
Figure 0007563171000013 
Figure 0007563171000014
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a wire harness. [Background technology]
[0002] In a wire harness including a plurality of electric wires, the conductors exposed from the insulating coating of each electric wire may be joined to each other using a crimp terminal or the like to form a splice portion. Wire harnesses including such a splice portion are disclosed in Patent Documents 1 to 3, etc. In order to protect the splice portion from contact with water, the portion including the splice portion may be covered with a resin material that is difficult for water to permeate. In particular, when the wire harness is used in an environment where contact with water is likely to occur, such as an automobile, it is important to waterproof the splice portion. In Patent Documents 1 to 3, constituent materials of the waterproof portion are considered so as to obtain desired characteristics such as high waterproof performance. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2015-159070 A [Patent Document 2] International Publication No. 2014 / 112157 [Patent Document 3] JP 2016-91629 A [Patent Document 4] JP 2019-85394 A [Patent Document 5] JP 2015-182912 A Summary of the Invention [Problem to be solved by the invention]
[0004] As described in Patent Documents 1 to 3, urethane (meth)acrylate is often used to form a waterproof part in a portion of a wire harness where an electric conductor is exposed from an insulating coating, such as a splice part. Urethane (meth)acrylate is an excellent material that can provide high waterproof performance while maintaining flexibility. However, when a wire harness is placed in a high-temperature and high-humidity environment, the waterproof performance exhibited by urethane (meth)acrylate may be affected. For example, the insulating coating constituting a wire harness is often made of polyvinyl chloride (PVC) containing a plasticizer, and when the waterproof part is placed in a high-temperature and high-humidity environment in a state where the waterproof part is in contact with the insulating coating, the plasticizer may migrate from the insulating coating to the waterproof part. The migration of the plasticizer reduces the adhesion of the waterproof part to the insulating coating, which may lead to a decrease in waterproof performance. In Patent Document 2, the solubility parameter of the curable material constituting the waterproof part is set to a predetermined value or more to suppress the migration of the plasticizer. However, from the viewpoint of effectively suppressing the decrease in adhesion due to migration of the plasticizer, particularly in high-temperature and high-humidity environments, there is room for further consideration of the constituent materials of the waterproof part.
[0005] Therefore, the objective of the present invention is to provide a wire harness in which the exposed portions of the electric conductors from the insulating coating are covered with a waterproof part, and which can maintain the adhesion of the waterproof part to the insulating coating containing a plasticizer even when placed in a high-temperature and high-humidity environment. [Means for solving the problem]
[0006] The wire harness of the present disclosure comprises an electric wire having a conductor and an insulating coating covering the outer periphery of the conductor, the electric wire having a conductor exposed portion where the conductor is exposed from the insulating coating, and a waterproof portion integrally covering the conductor exposed portion and a surface of the insulating coating, the insulating coating containing a plasticizer, and the waterproof portion being configured as a cured body of a resin composition containing a urethane (meth)acrylate oligomer and a nitrogen-containing monomer which is a radical polymerizable monomer containing a nitrogen atom. Effect of the Invention
[0007] The wire harness of the present disclosure is a wire harness in which the portions of the electric conductor exposed from the insulating coating are covered with a waterproof portion, and the waterproof portion can maintain adhesion to the insulating coating containing a plasticizer even when placed in a high-temperature and high-humidity environment. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a side view showing a wire harness according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a graph showing the change in adhesive strength over time in a high-temperature, high-humidity environment in the cases where a nitrogen-containing monomer (ACMO) was added to the resin composition and where no nitrogen-containing monomer (ACMO) was added. [Diagram 3] FIG. 3 is a diagram showing infrared absorption spectra before and after being left in a high-temperature and high-humidity environment, in the case where a nitrogen-containing monomer (ACMO) is added to a resin composition and in the case where a nitrogen-containing monomer (ACMO) is not added to the resin composition. [Figure 4] 4A to 4D are diagrams showing the relationship between the solubility parameter of a resin composition and the adhesive strength after being left in a high-temperature and high-humidity environment. Fig. 4A shows the relationship between the SP value, and Figs. 4B to 4D show the relationship between the dispersion term, polar term, and hydrogen bond term of the Hansen solubility parameter and the adhesive strength, respectively. [Diagram 5] 5A to 5D are diagrams showing the relationship between the solubility parameter of a resin composition and the rate of decrease in adhesive strength due to exposure to a high-temperature, high-humidity environment. Fig. 5A shows the relationship between the SP value and the dispersion term, polar term, and hydrogen bond term of the Hansen solubility parameter, respectively, and the rate of decrease in adhesive strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [Description of the embodiments of the present disclosure] First, embodiments of the present disclosure will be listed and described. The wire harness according to the present disclosure comprises an electric wire having a conductor and an insulating coating covering the outer periphery of the conductor, the electric wire having a conductor exposed portion where the conductor is exposed from the insulating coating, and a waterproof portion integrally covering the conductor exposed portion and a surface of the insulating coating, the insulating coating containing a plasticizer, and the waterproof portion being configured as a cured body of a resin composition containing a urethane (meth)acrylate oligomer and a nitrogen-containing monomer which is a radically polymerizable monomer containing a nitrogen atom.
[0010] In the above-mentioned wire harness, the resin composition constituting the waterproof part contains a nitrogen-containing monomer. By containing the nitrogen-containing monomer in the resin composition, migration of the plasticizer from the insulating coating of the electric wire to the waterproof part is suppressed even after exposure to a high-temperature and high-humidity environment. As a result, the adhesive strength of the waterproof part to the insulating coating containing the plasticizer is less likely to decrease even after exposure to a high-temperature and high-humidity environment, and high waterproof performance is maintained.
[0011] Here, the urethane (meth)acrylate oligomer is preferably a polycarbonate-based urethane (meth)acrylate oligomer, in which case the effect of suppressing the decrease in adhesive strength of the waterproof part in a high-temperature and high-humidity environment due to the addition of a nitrogen-containing monomer is particularly enhanced.
[0012] The nitrogen-containing monomer may be a (meth)acrylamide compound. By adding a (meth)acrylamide compound as the nitrogen-containing monomer to the resin composition constituting the waterproof part, the effect of suppressing a decrease in adhesion of the waterproof part to the insulating coating when exposed to a high-temperature and high-humidity environment is particularly excellent.
[0013] The resin composition constituting the waterproof part may have a dispersion term of the Hansen solubility parameter of 17.1 or more. As will be shown later, in the phenomenon in which the migration of the plasticizer from the insulating coating in a high-temperature, high-humidity environment is suppressed by adding a nitrogen-containing monomer to the resin composition constituting the waterproof part, it has been made clear from the examples that the addition of the nitrogen-containing monomer contributes greatly to increasing the solubility parameter of the resin composition, particularly the dispersion term. By constituting the waterproof part using a resin composition having a dispersion term of the solubility parameter of 17.1 or more, migration of the plasticizer from the insulating coating to the waterproof part and the resulting decrease in the adhesive strength of the waterproof part are particularly effectively suppressed when the waterproof part is subjected to a high-temperature, high-humidity environment.
[0014] The resin composition constituting the waterproof part may have a solubility parameter of 19.5 or more. Not only the variance term of the Hansen solubility parameter, but also the solubility parameter of the resin composition itself has a correlation with the migration of the plasticizer in a high-temperature and high-humidity environment, and by constituting the waterproof part using a resin composition with a large solubility parameter, a high effect can be obtained in suppressing the decrease in the adhesive strength of the waterproof part by suppressing the migration of the plasticizer.
[0015] The content of the nitrogen-containing monomer in the resin composition constituting the waterproof part is preferably 10% by mass or more, whereby the addition of the nitrogen-containing monomer significantly exerts the effect of suppressing migration of plasticizer into the waterproof part.
[0016] The wire harness may include a plurality of the electric wires, a splice portion at which the exposed conductor portions of the plurality of electric wires are joined, and the waterproof portion may integrally cover the splice portion and a surface of the insulating coating. In this case, the waterproof portion maintains high adhesion to the insulating coating of the electric wires even after exposure to a high temperature and high humidity environment, thereby maintaining high waterproofing at the splice portion.
[0017] [Details of the embodiment of the present disclosure] Hereinafter, a wire harness according to an embodiment of the present disclosure will be described with reference to the drawings. In this specification, various characteristics are values obtained in the atmosphere at room temperature unless otherwise specified. In addition, when a certain component is the main component of a certain material, this component refers to a state in which the component accounts for 50% by mass or more of the entire material. In this specification, "(meth)acrylate" refers to acrylate and methacrylate.
[0018] <Outline of wire harness> First, an outline of a wire harness according to an embodiment of the present disclosure will be described. An outline of a wire harness 1 according to an embodiment of the present disclosure is shown in Fig. 1. The structure of the wire harness 1 can be the same as those disclosed in Patent Documents 1 to 3.
[0019] The wire harness 1 includes a plurality of electric wires 4. Each electric wire 4 has a conductor 2 and an insulating coating 3 that covers the outer periphery of the conductor 2. The wire harness 1 has an intermediate splice portion 20 at a midway point in the longitudinal direction. In each electric wire 4, the insulating coating 3 is removed to form an exposed conductor portion 5 where the conductor 2 is exposed from the insulating coating 3. Then, each electric wire 4 is joined at the exposed conductor portion 5 by a crimp terminal 21, thereby forming the intermediate splice portion 20.
[0020] In the wire harness 1, the periphery of the intermediate splice portion 20 is covered by a waterproof portion 10. The periphery of the waterproof portion 10 is further covered by a protective sheet 30 to form a waterproof structure. In a bundle of a plurality of electric wires 4 (two in the figure), the waterproof portion 10 integrally covers the surface of the intermediate splice portion 20 to which the exposed conductor portion 5 is joined and the surface of the insulating coating 3 in the area adjacent to the exposed conductor portion 5. The exposed conductor portion 5 is provided with waterproofness by being covered by the waterproof portion 10. In other words, the exposed conductor portion 5 is sealed from the external environment by the waterproof portion 10, and the intrusion of electrolytes such as water into the exposed conductor portion 5 from the outside is suppressed.
[0021] A brief description will be given of the materials constituting each part of the wire harness 1. The conductor 2 constituting the electric wire 4 is not particularly limited, but is preferably made of a metal material such as copper, a copper alloy, aluminum, or an aluminum alloy.
[0022] The insulating coating 3 constituting the electric wire 4 is made of an insulating material mainly composed of a polymer material and contains a plasticizer. The type of polymer material is not particularly limited, but polyvinyl chloride (PVC) can be mentioned as a polymer material to which a plasticizer is added and which is often used for electric wire coating. The type of plasticizer is also not particularly limited, and examples thereof include phthalate ester plasticizers such as diisononyl phthalate (DINP), trimellitate ester plasticizers such as tris(2-ethylhexyl) trimellitate (TOTM), aliphatic dibasic acid ester plasticizers such as 2-ethylhexyl adipate and dibutyl sebacate, epoxy plasticizers such as epoxidized soybean oil, and phosphate ester plasticizers such as tricresyl phosphate. DINP and TOTM are plasticizers that are widely used in electric wire coating materials mainly composed of PVC, and it is preferable to use DINP or TOTM for the insulating coating 3 in this embodiment. The plasticizer may be used alone or in combination of two or more kinds. The content of the plasticizer in the insulating coating 3 is not particularly limited, but the content in a typical insulating coating is, for example, 25 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the polymer component.
[0023] The size of the electric wire 4 is not particularly limited. However, when the electric wire 4 is thick, as will be described later, the effect of suppressing the decrease in adhesive strength at the interface between the waterproof part 10 and the insulating coating 3 when exposed to a high temperature and high humidity environment by selecting the constituent material of the waterproof part 10 is greater. For example, when the conductor cross-sectional area of each electric wire 4 is 2 mm 2 The above embodiment is preferable.
[0024] The waterproof part 10 is configured as a cured product of a curable resin composition. The resin composition, which will be described in detail later, contains a urethane (meth)acrylate oligomer and a radical polymerizable monomer containing a nitrogen atom. The resin composition is preferably at least one of photocurable and thermosetting, and more preferably photocurable.
[0025] The material constituting the protective sheet 30 is not particularly limited as long as it is an insulating polymer material. When the resin composition constituting the waterproof part 10 is photocurable, the protective sheet 30 is preferably one that can transmit the irradiated light when photocuring the resin composition constituting the waterproof part 10. Specifically, as the protective sheet 30, a wrap sheet of an olefin resin such as polyethylene, polypropylene, polyvinyl chloride, polyvinylidene chloride, and polyvinylidene fluoride, or a wrap sheet of a general-purpose resin such as polyester, polyethylene terephthalate, or nylon can be used. In particular, it is preferable to use a sheet of polyvinyl chloride resin, polyvinylidene chloride resin, or polyvinylidene fluoride resin that has good self-adhesion (tackiness) as the protective sheet 30. Alternatively, it is preferable to provide a layer of adhesive or pressure-sensitive adhesive on the inner surface of the protective sheet 30.
[0026] The wire harness 1 according to the present embodiment can be manufactured by the same method as disclosed in Patent Documents 1 to 3. For example, first, a bundle of electric wires is prepared by joining a plurality of electric wires 4 at the conductor exposed portion 5 to form an intermediate splice portion 20. Then, the intermediate splice portion 20 of the bundle of electric wires is placed on a protective sheet 30 made of a material that transmits irradiated light together with the portions covered with the insulating coating 3 on both sides. Next, a resin composition that becomes the waterproof portion 10 is supplied on the intermediate splice portion 20. At this time, the resin composition may be supplied to the protective sheet 30, and then the bundle of electric wires may be placed on the resin composition. Alternatively, a part of the resin composition may be supplied to the protective sheet 30, and the resin composition may be cured by light irradiation or the like, and the remaining resin composition may be supplied and the intermediate splice portion 20 may be placed on the protective sheet 30.
[0027] Next, protective sheet 30 is folded or wrapped around intermediate splice portion 20 so that the outer periphery of intermediate splice portion 20 and the areas on both sides covered with insulating coating 3 are covered with the resin composition, and protective sheet 30 is further disposed on the outer periphery. Then, protective sheet 30 is irradiated with light or heated from the outside to cure the resin composition.
[0028] In the above-described embodiment, the wire harness 1 has the intermediate splice portion 20, and the waterproof portion 10 is formed in the region including the intermediate splice portion 20. However, the wire harness according to the embodiment of the present disclosure is not limited to such a form, as long as a waterproof portion is formed to integrally cover the conductor exposed portion where the conductor is exposed from the insulating coating and the surface of the insulating coating in the region adjacent to the conductor exposed portion. For example, when the conductor exposed portions of a plurality of electric wires constituting an electric wire bundle are joined to form a terminal splice portion at the terminal portion of the wire harness, the terminal splice portion may be covered to provide a waterproof portion. Furthermore, the present invention is not limited to a splice portion that joins the conductor exposed portions of a plurality of electric wires, but may also include a form in which a waterproof portion is provided by covering a conductor exposed portion where a conductor is exposed from an insulating coating in a single electric wire. For example, a waterproof portion may be provided at the boundary between the connection terminal and the electric wire in a form in which a connection terminal is connected to a conductor exposed portion provided at the terminal of one electric wire. Alternatively, a conductor exposed portion may be provided in the middle of one electric wire, and a waterproof portion may be provided in a region including the conductor exposed portion.
[0029] <Waterproof section materials> Next, there will be described a constituent material of the waterproof portion 10 provided in the wire harness 1. The waterproof portion 10 is formed as a cured body of a curable resin composition.
[0030] The resin composition constituting the waterproof part 10 contains a urethane (meth)acrylate oligomer and a nitrogen-containing monomer. By adding the nitrogen-containing monomer to the resin composition, when the wire harness 1 is placed in a high-temperature and high-humidity environment, the phenomenon in which a plasticizer migrates from the insulating coating 3 to the waterproof part 10 and the adhesion of the waterproof part 10 to the insulating coating 3 decreases is suppressed.
[0031] The urethane (meth)acrylate oligomer is a compound in which a hydroxy (meth)acrylate is bonded to the end of an oligomer obtained by polymerizing an isocyanate compound and a polyol compound. The urethane (meth)acrylate oligomer has excellent adhesiveness and waterproof properties when cured, and is also excellent in flexibility, so that it can be suitably used to form the waterproof part 10.
[0032] As the urethane (meth)acrylate oligomer, polyester-based urethane (meth)acrylate oligomers having a polyester skeleton at a site derived from a polyol compound and polyether-based urethane (meth)acrylate oligomers having a polyether structure at a site derived from a polyol compound are representative. In this embodiment, any of these may be used as the urethane (meth)acrylate oligomer, but it is preferable to use a polyester-based, particularly a polycarbonate-based urethane (meth)acrylate oligomer. As shown in the following examples, by using a polyester-based, particularly a polycarbonate-based urethane (meth)acrylate oligomer, the effect of suppressing plasticizer migration and adhesiveness reduction in a high-temperature and high-humidity environment due to the addition of a nitrogen-containing monomer can be particularly highly obtained. As the urethane (meth)acrylate oligomer, only one type may be used, or two or more types may be used in combination.
[0033] The nitrogen-containing monomer added to the resin composition is a radical polymerizable monomer containing a nitrogen atom. The radical polymerizable monomer is a monomer capable of radical polymerization by light or heat, and examples thereof include molecules containing an ethylenic double bond in the form of a (meth)acryloyl group or a (meth)acrylamide group. The specific type of the nitrogen-containing monomer is not particularly limited, but from the viewpoints of high plasticizer migration suppression effect, high curing property, easy availability, etc., it is preferable to use a (meth)acrylamide compound or a compound containing a nitrogen atom in a ring structure. The nitrogen-containing monomer may be used alone or in combination of two or more kinds.
[0034] A (meth)acrylamide compound is a compound having an acrylamide group or a methacrylamide group, and has the structure of Formula 1 below. [ka] In formula 1, R1 is a hydrogen atom or a methyl group. R2 and R3 are not particularly limited, but may each independently be a hydrogen atom or a hydrocarbon group. This form includes the case where R2 and R3 are bonded to each other by a ring structure, and includes the case where the skeleton of the ring structure is composed only of carbon atoms, as well as the case where it has an oxygen atom. The number of carbon atoms in R2 and R3 is not particularly limited, but is preferably 1 to 18.
[0035] Examples of (meth)acrylamide compounds applicable as nitrogen-containing monomers include the following molecules. 4-Acryloylmorpholine (ACMO) [ka] N,N-Dimethylacrylamide (DMAA) [ka]
[0036] Examples of compounds containing nitrogen atoms in a ring structure that can be used as nitrogen-containing monomers include those in which a ring structure containing a nitrogen atom and an ethylenically unsaturated bond coexist in one molecule. The ring structure is preferably a saturated ring structure. In addition, it is preferable that the carbon atom constituting the ethylenically unsaturated bond is bonded to the nitrogen atom constituting the ring structure. Examples of saturated ring structures containing nitrogen atoms include caprolactam rings, pyrrolidone rings, morpholine rings, and isocyanuric acid skeletons. Among these ring structures, those having a caprolactam ring or a morpholine ring are particularly preferred in terms of the high plasticizer migration suppression effect, etc.
[0037] Examples of compounds containing a nitrogen atom in a ring structure that can be used as a nitrogen-containing monomer include the following molecules: Note that the above-listed 4-acryloylmorpholine is an acrylamide represented by formula 1, and is also a compound containing a nitrogen atom in a ring structure. N-vinyl-ε-caprolactam (NVC) [ka] N-vinyl-2-pyrrolidone (NVP) [ka] Tris(2-acryloyloxyethyl)isocyanurate [ka]
[0038] In the resin composition constituting the waterproof part 10, the content of the nitrogen-containing monomer is not particularly limited, but from the viewpoint of enhancing the effect of suppressing plasticizer migration and adhesive strength reduction when exposed to a high-temperature and high-humidity environment, it is preferable that the content of the nitrogen-containing monomer is 10 mass % or more, and further 25 mass % or more of the entire resin composition. On the other hand, from the viewpoint of ensuring a sufficient content of urethane (meth)acrylate oligomer, the content of the nitrogen-containing monomer is preferably 85 mass % or less.
[0039] The resin composition constituting the waterproof part 10 preferably contains a photopolymerization initiator or a thermal polymerization initiator as a radical polymerization initiator in addition to the urethane (meth)acrylate oligomer and the nitrogen-containing monomer. The resin composition is a urethane (meth)acrylate composition having the following properties: waterproofness, suppression of plasticizer migration, etc. Oligomers As long as the properties exhibited by the nitrogen-containing monomer are not significantly impaired, urethane (meth)acrylates, other than radical polymerization initiators, Oligomers and may contain components other than the nitrogen-containing monomer as appropriate. Examples of such components include (meth)acrylate oligomers other than the above-mentioned urethane (meth)acrylate oligomers. Also, examples of radical polymerizable monomers other than the nitrogen-containing monomer, including (meth)acrylate monomers, such as those used as reactive diluents, may be mentioned. Furthermore, the resin composition may contain additives such as stabilizers, plasticizers, softeners, pigments, dyes, antistatic agents, flame retardants, adhesion promoters, sensitizers, dispersants, solvents, and antibacterial and antifungal agents as appropriate.
[0040] In the wire harness 1 according to the present embodiment, the waterproof part 10 integrally covers the intermediate splice part 20 to which the conductor exposed part 5 is joined and the surface of the insulating coating 3 of the electric wire 4 constituting the electric wire bundle, and the waterproof part 10 is in contact with the surface of the insulating coating 3. In this state, when the part including the waterproof part 10 in the wire harness 1 is placed in a high-temperature and high-humidity environment, the plasticizer contained in the insulating coating 3 may migrate to the waterproof part 10. When the plasticizer migrates, the constituent materials of the insulating coating 3 and the waterproof part 10 may be altered, and the adhesive strength of the waterproof part 10 at the interface between the waterproof part 10 and the insulating coating 3 may decrease. For example, when the plasticizer migrates after a high-temperature and high-humidity environment, the plasticizer contained in the insulating coating 3 decreases when the temperature returns to normal temperature, and the insulating coating 3 shrinks, generating thermal stress at the interface with the waterproof part 10, and the adhesive strength at the interface with the waterproof part 10 decreases. In this way, if the adhesive strength at the interface between the waterproof part 10 and the insulating coating 3 is reduced, it may become impossible to sufficiently prevent water from entering through the interface. In fact, as shown in the examples below, when the waterproof part 10 is made of a resin composition that does not contain a nitrogen-containing monomer, the adhesive strength is reduced in a high-temperature and high-humidity environment due to migration of the plasticizer.
[0041] In response to this, by adding a nitrogen-containing monomer to the resin composition constituting the waterproof part 10, even if a portion of the wire harness 1 including the waterproof part 10 is placed in a high-temperature, high-humidity environment, the plasticizer is less likely to migrate from the insulating coating 3 to the waterproof part 10. As a result, even after exposure to a high-temperature, high-humidity environment, the waterproof part 10 can maintain high adhesion to the insulating coating 3 and maintain a state in which it exhibits high waterproofing. For example, when the wire harness 1 is used in an automobile, it is expected that the waterproof part 10 will be exposed to a high-temperature, high-humidity environment, and it is important that the waterproofing can be maintained high even after exposure to a high-temperature, high-humidity environment.
[0042] The adhesive strength between the waterproof part 10 and the insulating coating 3 can be evaluated by performing a shear adhesion test on a model sample in which an adhesive joint is formed between the respective constituent materials, observing the failure mode, and measuring the adhesive strength. For example, the adhesive joint may be left in a humid and hot environment at a temperature of 85°C and a humidity of 85%RH for 250 hours, and then a shear adhesion test may be performed in accordance with JIS K6850. In this case, if the failure mode is not an interfacial failure but a cohesive failure of the constituent materials of the waterproof part 10, or if the insulating coating 3 breaks or stretches before the cohesive failure, it can be said that a sufficiently high adhesive strength is obtained even after the humid and hot environment. The mode in which the insulating coating 3 breaks or stretches is particularly preferable. In addition, it is preferable that the adhesive strength of the adhesive joint after being left in the humid and hot environment for 250 hours is 1.5 MPa or more, and more preferably 2.0 MPa or more.
[0043] <Migration of plasticizers to waterproof parts and solubility parameters> As described above, by adding a nitrogen-containing monomer to the resin composition constituting the waterproof part 10, migration of the plasticizer from the insulating coating 3 to the waterproof part 10 can be suppressed even in a high-temperature and high-humidity environment. As shown in the following examples, this suppression of plasticizer migration can be associated with an increase in the solubility parameter due to the addition of a nitrogen-containing monomer to the resin composition. The greater the difference between the solubility parameters of two substances, the less likely the compatibility phenomenon between those substances will occur. Therefore, the greater the difference between the solubility parameter of the waterproof part 10 and the solubility parameter of the plasticizer contained in the insulating coating 3, the less likely the plasticizer will migrate to the waterproof part 10. A plasticizer is a substance having a relatively low solubility parameter, and by adding a nitrogen-containing monomer to the resin composition constituting the waterproof part 10, the solubility parameter of the waterproof part 10 increases, and the solubility parameter of the waterproof part 10 becomes higher than the solubility parameter of the plasticizer. This is thought to suppress migration of the plasticizer. In the resin composition constituting the waterproof part 10, the solubility parameter and δ, which will be described next, are used. D , δ P , δ H As the values of each of the above terms become larger, the waterproof part 10 formed as a cured product of the resin composition also becomes larger in solubility parameter and each of the above terms.
[0044] The solubility parameter can be separated into contributions according to the type of intermolecular interaction, as shown in Equation 2 below. SP 2 = δ D 2 +δ P 2 +δ H 2 (2) Here, δ D , δ P , δ H are the dispersion term, polar term, and hydrogen bonding term of the Hansen solubility parameter, respectively. The dispersion term δ D represents the contribution of intermolecular interactions due to dispersion forces such as van der Waals forces, and the polar term δ P represents the contribution of intermolecular interactions due to molecular polarity, such as dipole interactions, and the hydrogen bond term δ H represents the contribution of intermolecular interactions due to hydrogen bonds. SP in Equation 2 is the total solubility parameter, which corresponds to the Hildebrand solubility parameter (SP value).
[0045] In this embodiment, the contribution of the dispersion term, among the solubility parameters, is considered to be particularly large in the phenomenon in which the addition of a nitrogen-containing monomer to the waterproof part 10 suppresses plasticizer migration and adhesive strength reduction in a high-temperature, high-humidity environment. As shown in the examples, the suppression of adhesive strength reduction shows a clear correlation with the dispersion term of the solubility parameter, but does not show a very clear correlation with the polar term or hydrogen bond term. It is considered that the addition of a nitrogen-containing monomer increases the dispersion term of the solubility parameter of the resin composition constituting the waterproof part 10, and there is a large difference in the dispersion term between the resin composition and the plasticizer, thereby suppressing the migration of the plasticizer to the waterproof part 10.
[0046] The more nitrogen-containing monomer is added to the resin composition constituting the waterproof part 10, the larger the solubility parameter of the resin composition, particularly the dispersion term. By selecting the type and amount of the nitrogen-containing monomer so that the dispersion term of the solubility parameter of the resin composition is 17.1 or more, further 17.3 or more, or 17.5 or more, a significant effect can be obtained in suppressing the migration of the plasticizer to the waterproof part 10 in a high-temperature and high-humidity environment and suppressing the resulting decrease in adhesive strength. The SP value should be 19.5 or more, further 20.5 or more.
[0047] The solubility parameter of the nitrogen-containing monomer itself is not particularly limited as long as the resin composition constituting the waterproof part 10 can have a large solubility parameter sufficient to suppress the migration of the plasticizer. However, the larger the solubility parameter of the nitrogen-containing monomer itself, the greater the effect of increasing the solubility parameter of the resin composition. For example, the nitrogen-containing monomer may have a solubility parameter of 17.0 or more, or even 17.5 or more, or 18.0 or more, in terms of the dispersion term, or 19.0 or more, 21.0 or more, or 22.0 or more in terms of the SP value.
[0048] As described above, the type of plasticizer contained in the insulating coating 3 is not particularly limited. However, from the viewpoint of relatively increasing the effect of suppressing plasticizer migration obtained by adding a nitrogen-containing monomer to the waterproof part 10 compared to the case where no nitrogen-containing monomer is added, it is preferable that the plasticizer itself is one that is likely to migrate to the waterproof part 10 to which no nitrogen-containing monomer is added, that is, one that has a relatively small solubility parameter. For example, DINP has a solubility parameter dispersion term of 16.3 and an SP value of 17.2. TOTM has a dispersion term of 16.8 and an SP value of 17.7. EXAMPLES
[0049] Examples are shown below. Here, the effect of adding a nitrogen-containing monomer to the resin composition constituting the waterproof part was confirmed, and the relationship with the solubility parameter of the resin composition constituting the waterproof part was examined. Unless otherwise specified, the preparation and evaluation of samples were performed at room temperature in the atmosphere. Note that the present invention is not limited to these examples.
[0050] [1] Change in adhesive properties due to the addition of nitrogen-containing monomers First, for a resin composition in which a polymerizable monomer is added to a urethane acrylate oligomer, it was confirmed how the adhesiveness at the interface with an insulating coating material changes after exposure to a high-temperature and high-humidity environment.
[0051] [Test 1-1] Effect of resin composition on adhesion <Sample preparation> The resin compositions to be used as samples were prepared by blending and uniformly mixing the urethane acrylate oligomer and the nitrogen-containing monomer or the nitrogen-free polymerizable monomer as shown in Table 1. In each sample, the blending amount of the monomer was 50 mass % of the entire resin composition.
[0052] The materials used in preparing the resin composition are as follows: (Urethane acrylate oligomer) Polycarbonate-based urethane acrylate oligomer Polyether-based urethane acrylate oligomer (Nitrogen-containing monomer) ACMO: 4-Acryloylmorpholine ·DMAA: N,N-Dimethylacrylamide NVC: N-vinyl-ε-caprolactam MN1: Tris(2-acryloyloxyethyl)isocyanurate (Non-nitrogen-containing monomer) IBXA: Isobornyl acrylate ·BCHA: tert-Butyl cyclohexanol acrylate ·HPA: Hydroxypropyl acrylate MN2: Tricyclodecane dimethanol diacrylate ·MN3: 3,3,5-trimethylcyclohexyl acrylate
[0053] <Evaluation of adhesive strength> As a model of the adhesive part between the waterproof part and the insulating coating of the wire harness, the adhesive strength between the PVC coating material and the cured product of the resin composition prepared above was measured. Specifically, the above resin composition was placed between the surfaces of two PVC coating materials (thickness 0.4 mm), and the resin material was cured by ultraviolet light irradiation to prepare a test piece for measuring adhesive strength. A shear adhesion test was performed on this test piece in accordance with JIS K6850 to measure the tensile shear adhesive strength and observe the fracture morphology. This evaluation result was taken as the result of the shear adhesion test in the initial state. The PVC coating material used contained DINP or TOTM as a plasticizer.
[0054] Furthermore, the same test pieces as above were left in a humid heat environment at a temperature of 85°C and a humidity of 85%RH for 250 hours. After the test pieces were allowed to cool to room temperature, a shear adhesion test was performed in the same manner as above. The evaluation results were used as the results of the shear adhesion test after humid heat.
[0055] <Evaluation Results> Table 1 below shows the adhesive strength and fracture morphology obtained in the shear adhesion test in the initial state and after wet heat for samples A1 to A15, together with the material type used in the preparation of the resin composition and the type of plasticizer added to the coating material. As described above, the content of monomer in the resin composition is 50 mass% for all samples. Regarding the fracture morphology, "interface" refers to interfacial fracture, and "cohesion" refers to cohesive fracture in the cured resin composition. "Coating break" and "coating elongation" refer to the phenomenon in which the coating material breaks and elongates before the occurrence of interfacial fracture or cohesive fracture. The value shown as "adhesive strength" indicates the shear strength when the coating break and coating elongation occur, and the adhesive strength at the sample interface is greater than the value shown.
[0056] [Table 1]
[0057] According to Table 1, in the case of using polycarbonate-based urethane acrylate oligomer, in the case of samples A5 to A7 to which a non-nitrogen-containing monomer was added, all of the samples showed interface failure in the shear adhesion test after wet heat. Furthermore, in the case of samples A6 and A7, the adhesive strength after wet heat was clearly lower than that in the initial state, and the adhesive strength value after wet heat was small, at 1.3 MPa or less. In contrast, in the case of samples A1 to A4 to which a nitrogen-containing monomer was added, the adhesive strength measured after wet heat was higher than that measured in the initial state, and showed a large value of 2.6 MPa or more. In particular, in the case of samples A1 to A3, the form of failure after wet heat was coating breakage, and no interface failure occurred. As described above, when coating elongation or coating breakage is observed, the actual adhesive strength at the sample interface should be higher than the measured adhesive strength, and the phenomenon in which the adhesive strength measured after wet heat is higher than that measured in the initial state does not necessarily mean that the adhesive strength at the interface has increased. When polyether-based urethane acrylate oligomers were used, a comparison of samples A8 to A10 containing added nitrogen-containing monomers and samples A11 to A14 containing added nitrogen-free monomers showed that in all cases the failure mode after moist heat was interfacial failure, but the adhesive strength after moist heat was 0.3 MPa or less in samples A11 to A14 containing added nitrogen-free monomers, while the adhesive strength after moist heat was 0.6 MPa or more in samples A8 to A10 containing added nitrogen-containing monomers.
[0058] From these results, it can be said that, whether a polycarbonate-based or polyether-based urethane acrylate oligomer is used, the addition of a nitrogen-containing monomer to the oligomer results in higher adhesion at the interface between the cured body and the coating material after exposure to moist heat than the addition of a nitrogen-free monomer to the oligomer. In other words, it can be seen that the addition of a nitrogen-containing monomer to the urethane acrylate oligomer has the effect of suppressing the decrease in adhesion in a moist heat environment.
[0059] When comparing the effect of suppressing the decrease in adhesiveness in a humid and hot environment depending on the type of urethane acrylate oligomer, the adhesive strength value after humid and hot exposure is higher when the urethane acrylate oligomer is polycarbonate-based than when it is polyether-based. In addition, in the case of polyether-based, although the decrease is suppressed to a small extent by adding a nitrogen-containing monomer, the adhesive strength decreases after being left in a humid and hot environment, whereas in the case of polycarbonate-based, the adhesive strength does not decrease after being left in a humid and hot environment, and the destruction form may be coating cracking. Thus, the effect of suppressing the decrease in adhesiveness in a humid and hot environment by adding a nitrogen-containing monomer is particularly large when the urethane acrylate oligomer is polycarbonate-based.
[0060] The samples A1 to A4 are different from each other in the type of nitrogen-containing monomer added to the resin composition. Among them, the destruction mode after moist heat in sample A4 is interfacial destruction, whereas the destruction mode in samples A1 to A3 is coating breakage. From this, it can be said that the adhesive strength of the interface after moist heat is higher in samples A1 to A3 than in sample A4. In other words, it can be said that the effect of suppressing the decrease in adhesive strength due to leaving in moist heat environment is particularly large by using, among nitrogen-containing monomers, (meth)acrylamide compounds having the structure of the above formula 1 as in samples A1 and A2, or one containing a nitrogen atom in a caprolactam ring as in A3.
[0061] Sample A1 and Sample A15 differ in the type of plasticizer contained in the coating material. However, for both samples, in the shear adhesion test after moist heat, the destruction mode observed was coating breakage, and no decrease in adhesive strength was observed. As shown in the test in [2] below, the decrease in adhesive strength after exposure to moist heat is thought to be due to the migration of plasticizer from the coating material to the cured resin composition. However, regardless of the type of plasticizer added to the coating material, it is clear that the addition of a nitrogen-containing monomer to the resin composition has the effect of suppressing the decrease in adhesiveness due to moist heat.
[0062] [Test 1-2] Change over time in a hot and humid environment <Sample preparation> A resin composition was prepared by adding ACMO to a polycarbonate-based urethane acrylate oligomer so that the content was 20 mass % of the total. For comparison, the urethane acrylate oligomer itself was also prepared as a resin composition without ACMO.
[0063] <Evaluation of adhesive strength> In the same manner as in Test 1-1 above, the adhesive strength between the PVC coating material and the cured product of the resin composition was measured in the initial state and in the state where the material was left in a humid and hot environment at a temperature of 85°C and a humidity of 85%RH for a predetermined time and then cooled to room temperature. The time of leaving the material in the humid and hot environment was set to four times: 100 hours, 300 hours, 500 hours, and 1000 hours. The PVC coating material used contained DINP as a plasticizer.
[0064] <Evaluation Results> Figure 2 shows the change in adhesive strength when left in a humid and hot environment for resin compositions containing and not containing ACMO. The horizontal axis shows the time left in the humid and hot environment, and the vertical axis shows the measured adhesive strength. The error bars in the figure show the variation in the evaluation results for multiple individual samples.
[0065] According to Fig. 2, in the initial state (0 hours), the adhesive strength is about the same regardless of whether ACMO is present or not. However, when placed in a humid and hot environment, when the resin composition does not contain ACMO (no ACMO in the figure), the adhesive strength drops rapidly over the humid and hot exposure period of up to about 300 hours, whereas when the resin composition contains ACMO (ACMO added in the figure), the drop in adhesive strength stops after about 100 hours, and the amount of drop is significantly smaller. Thereafter, the adhesive strength starts to increase, and even after 1000 hours, the measured adhesive strength remains stably higher than when ACMO is not added.
[0066] In this way, by adding ACMO, a nitrogen-containing monomer, to the urethane acrylate oligomer, the effect of suppressing the decrease in adhesive strength at the interface with the coating material in a moist heat environment becomes evident from a relatively short time period of 100 hours or less. And, even if the sample is left in a moist heat environment for a long time period of 1000 hours, the effect is stably maintained. In addition, in the above test 1-1, the time of leaving in a moist heat environment was 250 hours, but according to Figure 2, the decrease in adhesive strength had already converged at 250 hours in the sample with ACMO added, and it is considered that the effect of suppressing the decrease in adhesive strength after moist heat by adding a nitrogen-containing polymer observed in the above test 1-1 will be maintained even if the time of leaving in a moist heat environment is further extended.
[0067] [2] Changes in plasticizer behavior due to the addition of nitrogen-containing monomers Next, we investigated how the plasticizer in the coating material behaved at the interface between the cured body and the coating material after exposure to a high-temperature and high-humidity environment.
[0068] <Sample preparation> A resin composition was prepared by using the same polycarbonate-based urethane acrylate oligomer as used in Test 1-1 as the urethane acrylate oligomer and ACMO as the nitrogen-containing monomer. The resin composition was prepared by adding ACMO to the urethane acrylate oligomer in an amount of 20 mass% of the total.
[0069] <Evaluation of migration of plasticizers> In the same manner as in Test 1, a resin composition was placed between the surfaces of two PVC coating materials, and a sample was prepared in which the resin material was cured by irradiation with ultraviolet light. The PVC coating material used contained DINP as a plasticizer. The sample was left in a humid and hot environment at a temperature of 85°C and a humidity of 85% RH for 250 hours. Then, a shear adhesion test was performed on the initial state before being left in the humid and hot environment and the state after being left in the humid and hot environment. Furthermore, infrared absorption spectroscopy measurement by total reflection measurement (ATR-IR measurement) was performed on the cured portion of the sample after the shear adhesion test. For reference, infrared absorption spectroscopy measurement was also performed on the plasticizer DINP itself.
[0070] <Evaluation Results> Figure 3 shows the infrared absorption spectra of the urethane acrylate oligomer in the initial state and after wet heating, in the range of 800 to 700 cm, with and without ACMO added. -1 The spectrum of the plasticizer itself is also shown in the figure (thin solid line). In FIG. 3, as indicated by the arrow, DINP is -1 When the growth of the peak at this wavenumber is observed in the spectrum of the cured product of the resin composition after being left in a humid and hot environment, it can be determined that migration of the plasticizer from the coating material to the cured product has occurred.
[0071] First, when looking at the spectrum when the urethane acrylate oligomer does not contain ACMO, in the initial state (gray solid line), -1No peak is seen in the vicinity of this wavelength. However, after moist heat treatment (gray dashed line), a peak structure is seen in this wavenumber region. This result indicates that DINP is migrating from the coating material to the cured resin composition after exposure to moist heat. On the other hand, when looking at the spectrum in which ACMO is included, a peak is seen at 740 cm in the initial state (black solid line) and after moist heat treatment (black dashed line). -1 The spectral intensity around 740 cm hardly changes. This result indicates that the migration of DINP from the coating material to the cured resin composition hardly occurs even after exposure to a humid and hot environment. In the sample containing ACMO, the spectral intensity around 740 cm hardly changes from the initial state. -1 A weak peak structure is observed around 1000 nm, which is thought to be due to the fact that ACMO itself has a weak absorption peak in this region.
[0072] As described above, when the cured product of the urethane acrylate oligomer to which the nitrogen-containing monomer is not added is exposed to a humid and hot environment, the plasticizer migrates from the coating material, whereas when the nitrogen-containing monomer ACMO is added, the plasticizer is less likely to migrate even when the cured product is exposed to a humid and hot environment. Considering the results of the test in [1] above, which showed that the addition of the nitrogen-containing monomer suppresses the decrease in adhesive strength at the interface between the cured product and the coating material when exposed to a humid and hot environment, it can be said that the addition of the nitrogen-containing monomer suppresses the migration of the plasticizer in a humid and hot environment, which leads to the suppression of the decrease in adhesive strength. When the plasticizer migrates from the coating material to the cured product of the resin composition in a humid and hot environment, the coating material shrinks when the temperature is returned to room temperature, causing thermal stress at the interface with the cured product, which reduces the adhesive strength. However, it is believed that the addition of the nitrogen-containing monomer to the resin composition suppresses the migration of the plasticizer, and therefore the adhesive strength at the interface is maintained at a high level even when exposed to a humid and hot environment.
[0073] [3] Contribution of solubility parameters Finally, the relationship between the solubility parameter of the resin composition and the change in adhesive strength when exposed to a humid and hot environment was examined.
[0074] <Sample preparation> The components were blended and mixed uniformly according to the compositions shown in Tables 3 to 5 below to prepare sample resin compositions. The urethane acrylate oligomers and monomers used were the same as those used in the test [1] above. Regarding the urethane acrylate oligomer, "Polycarbonate-based oligomer 1" was the same as that used in the test 1-1 above (weight average molecular weight: 5.4×10 4 ), "Polycarbonate-based oligomer 2" is the same as that used in Test 1-2 above (weight average molecular weight: 1.2 × 10 4 ). In addition, the following non-nitrogen-containing monomers were used as reactive diluents: MN4: (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl acrylate
[0075] <Evaluation of adhesive strength> The adhesive strength between the PVC coating material and the cured resin composition was measured by a shear adhesion test in the same manner as in the test [1] above. The measurements were performed in the initial state and in the state after being left in a humid and hot environment of 85°C and 85% RH for 250 hours and then cooled to room temperature. The PVC coating material used contained DINP as a plasticizer.
[0076] <Estimation of solubility parameters> The solubility parameter of each sample resin composition was estimated by calculation. In addition to determining the Hildebrand solubility parameter (SP value), the dispersion term δ of the Hansen solubility parameter was calculated as shown in the above formula 2. D , polarity term δ P , hydrogen bond term δ H The contributions of were separated.
[0077] When calculating the solubility parameter of each sample, the solubility parameter values of each component shown in Table 2 below were added together according to the volume ratio of the components. The solubility parameter values in Table 2 were estimated using Hansen solubility parameter in practice (HSPiP), a software for calculating solubility parameters. The solubility parameter values of each component calculated by HSPiP are calculated based on values obtained from latent heat of vaporization, dipole-dipole forces, intermolecular forces, etc.
[0078] [Table 2]
[0079] <Evaluation Results> Tables 3 to 5 show the amount of each component (unit: mass %) for resin compositions with various formulations, as well as the estimated SP value and Hansen solubility parameter for each term, and the measured adhesive strength and failure mode in the initial state and after moist heat treatment. The reduction rate of adhesive strength is also shown. This reduction rate is calculated as the reduction in adhesive strength from the initial state to the state after moist heat treatment as a ratio to the initial value, and a negative value indicates that the adhesive strength after moist heat treatment is greater than the initial state. Samples A1 to A4 and A7 in Table 5 are the same as the samples used in Test 1-1 shown in Table 1.
[0080] [Table 3]
[0081] [Table 4]
[0082] [Table 5]
[0083] Based on the data in Tables 3 to 5, Figures 4A to 4D show the relationship between the estimated values of the SP value, the dispersion term, polarity term, and hydrogen bond term of the Hansen solubility parameters, and the measured adhesive strength after the moist heat treatment. Figures 5A to 5D show the relationship between the estimated values of the SP value, the dispersion term, polarity term, and hydrogen bond term of the Hansen solubility parameters, and the decrease rate of adhesive strength due to the moist heat environment. In each figure, samples B1 to B18 in Table 3, which use polycarbonate oligomer 1, ACMO, and MN4 as components, are shown with black circles (●). Samples C1 to C5 in Table 4, which use polycarbonate oligomer 2 and ACMO as components, are shown with white circles (○). Samples A1 to A4 and A7 in Table 5, which use polycarbonate oligomer 1 and various monomers, are shown with white squares (□).
[0084] Looking at the relationship between the adhesive strength and the decrease rate of adhesive strength after moist heat (vertical axis) and the SP value (horizontal axis) shown in Figures 4A and 5A, although the data points are widely dispersed, it can be seen that as the SP value of the resin composition increases, the adhesive strength after moist heat increases and the decrease rate of adhesive strength decreases. In addition, these trends are generally saturated in the region where the SP value is 19.5 or more. Considering this result together with the test results of [1] and [2] above, it can be said that the addition of a nitrogen-containing monomer increases the solubility parameter of the resin composition, which suppresses the migration of the plasticizer from the coating material to the cured resin composition after exposure to moist heat, and further suppresses the decrease in the adhesive strength at the interface.
[0085] Furthermore, when looking at the relationship between the adhesive strength and the decrease rate of the adhesive strength after moist heat treatment (vertical axis) in Figures 4B and 5B and the dispersion term of the solubility parameter (horizontal axis), the dispersion of the data points is smaller than that of the relationship with the SP value in Figures 4A and 5A, and the tendency that the adhesive strength after moist heat treatment increases and the decrease rate of the adhesive strength decreases as the dispersion term increases, and the behavior that these tendencies saturate in the region where the magnitude of the dispersion term is approximately 17.1 or more, are more clearly seen. On the other hand, when the polarity term in Figures 4C and 5C is used as the horizontal axis, or when the hydrogen bond term in Figures 4D and 5D is used as the horizontal axis, there is no clear correlation between the adhesive strength after moist heat treatment and the decrease rate of the adhesive strength, as in the case of the dispersion term in Figures 4B and 5B. Rather, it can be said that the dispersion of the data points is larger than when the SP value in Figures 4A and 5A is used as the horizontal axis, and the correlation is lower. In particular, when the hydrogen bond term in Figures 4D and 5D is used as the horizontal axis, the distribution regions of the data points are separated due to differences in the component types.
[0086] From these results, it can be seen that the phenomenon in which the addition of a nitrogen-containing monomer suppresses the migration of plasticizers and the decrease in adhesive strength when exposed to a humid and hot environment is highly correlated with the dispersion term, among the solubility parameters of the resin composition. Furthermore, in the graphs in which the horizontal axis is the SP value in Figures 4A and 5A, and the graphs in which the horizontal axis is the dispersion term in Figures 4B and 5B, the data points of different component types plotted with different symbols all follow a common trend. This shows that the suppression of the migration of plasticizers and the decrease in adhesive strength can be organized by the solubility parameter, which is a macroscopic physical property value, especially the dispersion term, without taking into account the detailed molecular structure.
[0087] Furthermore, the results summarized in Tables 3 and 4 also show the effect of the amount of nitrogen-containing monomer added to the resin composition. According to Tables 3 and 4, as the amount of nitrogen-containing monomer (ACMO) added increases, the adhesive strength after moist heat treatment increases and the decrease in the adhesive strength decreases. In addition, the fracture morphology changes from interface fracture to cohesive fracture, and then to coating breakage and coating elongation, which indicates that the adhesiveness at the interface is strong. In general, in the region where the nitrogen-containing monomer content is 10% by mass or more, the tendency of the adhesive strength to increase after moist heat treatment and the decrease in the amount of decrease in adhesive strength begins to saturate, and the fracture morphology changes to cohesive fracture, and then to coating breakage and coating elongation. In the region where the nitrogen-containing monomer content is 25% by mass or more, these behaviors become even clearer. In addition, in Table 3, when comparing cases where the amount of nitrogen-containing monomer (ACMO) added is the same and the amount of nitrogen-free monomer (MN4) added is different, the adhesive strength after moist heat treatment increases and the decrease in the adhesive strength decreases as the amount of nitrogen-free monomer added decreases.
[0088] Although the embodiments of the present disclosure have been described in detail above, the present invention is not limited to the above-described embodiments, and various modifications are possible without departing from the gist of the present invention. [Explanation of symbols]
[0089] 1 Wire harness 2 Conductors 3. Insulation coating 4 electric wire 5 Exposed conductor 10 Waterproof part 20 Intermediate splice 21 Crimp terminal 30 Protective Sheet
Claims
1. An electric wire having a conductor and an insulating coating covering an outer periphery of the conductor, the electric wire having a conductor exposed portion where the conductor is exposed from the insulating coating; a waterproof portion that integrally covers the conductor exposed portion and a surface of the insulating coating, The insulating coating contains a plasticizer, The waterproof portion is A polycarbonate-based urethane (meth)acrylate oligomer; a nitrogen-containing monomer which is a radical polymerizable monomer containing a nitrogen atom; A wire harness comprising a cured body of a resin composition comprising the above-mentioned.
2. The wire harness according to claim 1 , wherein the nitrogen-containing monomer is a (meth)acrylamide compound.
3. 3. The wire harness according to claim 1, wherein the resin composition constituting the waterproof portion has a variance term of a Hansen solubility parameter of 17.1 or more.
4. The wire harness according to claim 1 , wherein the resin composition constituting the waterproof portion has a solubility parameter of 19.5 or more.
5. The wire harness according to claim 1 , wherein the resin composition constituting the waterproof portion has a content of the nitrogen-containing monomer of 10 mass % or more.
6. the wire harness includes a plurality of the electric wires and has a splice portion at which the exposed conductor portions of the plurality of the electric wires are joined, The wire harness according to claim 1 , wherein the waterproof portion integrally covers the splice portion and a surface of the insulating coating.
Citation Information
Patent Citations
Wire harness
JP2015159070A
Optical fiber
JP2015182912A
Wire harness
JP2016058317A
Wire harness
JP2016091629A
Sealed electric terminal assembly
JP2018049814A