Metallic material connector and metal material connecting method

By using a thermoplastic resin film to melt and solidify connections between metal materials, the method addresses the inefficiencies of existing connection methods, enabling rapid, repairable, and contamination-free connections with minimal thickness change, suitable for roll-to-roll manufacturing.

JP7563611B2Active Publication Date: 2024-10-08RESONAC CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023541815
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-07-27
Filing Date
2023-07-05
Publication Date
2024-10-08
Estimated Expiration
2043-07-05

AI Technical Summary

Technical Problem

Existing methods for connecting metal materials in roll-to-roll manufacturing, such as welding, liquid adhesive, thermosetting adhesive film, and adhesive tape, face issues with long process times, inability to repair, contamination of production lines, and thickness changes at connection points, making them inconvenient and unsuitable for continuous processing.

Method used

A method involving butting cross sections of metal materials and covering the opposing parts with a film containing a thermoplastic resin as the main component, which is melted and solidified to form a connection, utilizing amorphous thermoplastic resins like thermoplastic epoxy or phenoxy resins with specific properties to achieve strong, repairable, and thin connections.

Benefits of technology

The method provides a quick connection process that is repairable, prevents production line contamination, maintains minimal thickness changes, and offers high bonding strength without the need for adhesives, suitable for roll materials in manufacturing lines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563611000002
    Figure 0007563611000002
  • Figure 0007563611000003
    Figure 0007563611000003
  • Figure 0007563611000004
    Figure 0007563611000004
Patent Text Reader

Abstract

A connected body of metal materials obtained by matching a cross-section A of a flat metal material A and a cross-section B of a flat metal material B, covering at least part of the opposing portion, which is a region spanning both the edge portion A of the metal material A and the edge portion B of the metal material B, with a film that includes a layer composed mainly of a thermoplastic resin, and connecting the metal material A and the metal material B, wherein the film is one that has been melted and solidified on the opposing portion.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a metal material connection body formed by butting a cross section of a metal material with a cross section of another metal material, and a method for connecting metal materials that is suitable for applications in which a cross section of a metal material is butted with a cross section of another metal material, and In this specification, the term "edge portion" refers to a flat portion on at least one of the front and back surfaces near the end of the metal material to be connected. In this specification, the "opposing portion" refers to a region spanning the "edge portion" and including both the flat surface portions on the front and back sides of the metal material. In this specification, "cross section" is not limited to a cut surface, and "butting the cross section of a metal material with the cross section of another metal material" also includes abutting the end or beginning of a metal material that does not have a cut surface. In this specification, the term "butt" means to face each other, and is not limited to a mode in which the entire surfaces are in contact with each other. [Background technology]

[0002] In roll-to-roll manufacturing equipment that transports and continuously processes rolled metal sheet and / or metal foil (hereinafter referred to as roll material), when the amount of wound roll material becomes small or at a point where the roll material is discontinued, it is necessary to join the old roll material being continuously processed with a new roll material. As a technique for connecting the starting end of a strip-shaped metal material to the end of another strip-shaped metal material, a joining method has been disclosed in which a backing material is placed on the back side of the butt joint where the ends are butted together, and an arc welding torch is run along the front side of this butt joint to weld the butt joint (Patent Document 1).

[0003] However, the technology in Patent Document 1 involves connections by welding, and once connected, they cannot be dismantled without being destroyed. This poses the problem that it is not easy to reconnect (hereinafter also referred to as repair) the connections in case of a failure such as misalignment of the connections.

[0004] Possible connection means other than welding include connection using a liquid adhesive, connection using a film-like thermosetting adhesive (hereinafter referred to as a thermosetting adhesive film), connection using adhesive tape, connection using crimping, etc., but each of these has the following problems.

[0005] Connection using a liquid adhesive requires a coating process in which a liquid thermosetting resin composition is applied, and a curing process in which the resin composition is polymerized and cured after application. The coating process takes time to apply the resin composition, and the curing process takes time for the polymerization reaction. Thus, connection using a liquid adhesive has a problem of lack of convenience because the process time for connection is long. In addition, repair is either impossible or difficult in the case of a liquid thermosetting adhesive.

[0006] When connecting using a thermosetting adhesive film, the coating step is unnecessary and the process time can be shortened, but repairs cannot be made after connecting. When the thermosetting adhesive film is a B-stage film, the polymerization reaction easily proceeds at room temperature, resulting in poor storage stability and making it impossible to store the film for a long time at room temperature. That is, when the thermosetting adhesive film is a B-stage film, it must be stored at low temperature, requiring a low-temperature storage cabinet, making it difficult to store a large amount of the film for a long time and lacking in convenience.

[0007] In connection using adhesive tape, there is a problem that adhesive components (hereinafter referred to as adhesive substances) such as a matrix resin, which is a resin composition constituting the adhesive layer of the adhesive tape, and a tackifier, etc., adhere to the conveying path and the mold in the production line, thereby contaminating the conveying path and the mold. In addition, if the adhesive tape is accidentally peeled off, the adhesive layer of the peeled adhesive tape will be exposed, and there is a concern that the adhesive substances will contaminate the conveying path and the mold.

[0008] When connecting by crimping, metal materials are stacked together to perform the crimping, and protrusions are created by the crimping. This increases the thickness at the crimped part, which is the connection part, making it difficult to apply to low-profile manufacturing lines. In addition, crimping requires a flat metal space larger than the crimp diameter, which makes it difficult to obtain sufficient connection strength with metal materials of complex shapes or narrow pitches. In addition, when passing through multiple chemical tanks, there is a problem that more chemicals are carried over to the next tank, which causes contamination of the chemicals and shortens the life of the chemicals. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2012-61511 A Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention has been made in consideration of the above technical background, and aims to provide a connection technology that allows repair, has a short process time, is free of risk of contamination of the production line by adhesive components, and has little change in thickness at the connection part. [Means for solving the problem]

[0011] In order to achieve the above object, the present invention provides the following means.

[0012] <Metal material connector> [1] A connected metal material formed by butting a cross section A of a flat metal material A with a cross section B of a flat metal material B, covering at least a part of the opposing portion, which is an area spanning both an edge portion A of the metal material A and an edge portion B of the metal material B, with a film containing a layer mainly composed of a thermoplastic resin, and connecting the metal material A and the metal material B, wherein the film is a film that has been melted and solidified at the opposing portion. [2] The metal material connection according to [1], wherein the metal material A and the metal material B are at least one selected from the group consisting of a metal plate having a thickness of 1 mm or less and a metal foil having a thickness of 1 mm or less. [3] A connection of metal materials [1] or [2] in which the metal material A and the metal material B are in a strip shape and the metal material A and the metal material B are butted together so as to be continuous in the longitudinal direction. [4] The metal material linkage according to any one of [1] to [3], wherein the metal material A and the metal material B are rolled materials each formed by winding at least one selected from the group consisting of a metal plate and a metal foil into a roll. [5] A connection body of any of the metal materials [1] to [4], in which the coating is applied to both the front flat surfaces of the metal material A and the metal material B and the back flat surfaces of the metal material A and the metal material B. [6] The metal material linked body according to any one of [1] to [5], wherein the thermoplastic resin is an amorphous thermoplastic resin. [7] The metal connector according to [6], wherein the amorphous thermoplastic resin is at least one of a thermoplastic epoxy resin and a phenoxy resin. [8] The metal connector according to [7], wherein the amorphous thermoplastic resin is an amorphous thermoplastic resin having an epoxy equivalent of 1,600 or more, or an amorphous thermoplastic resin not containing an epoxy group. [9] The film is a connected body of metal materials according to any one of [1] to [8], having a thickness of 10 μm to 3 mm.

[10] the film has an adhesive on a surface covering the facing portion, The adhesive material has a function of temporarily fixing the film and does not have an adhesive function, and is a connected body of metal materials according to any one of [1] to [9].

[0013] <Metal material connection method>

[11] A method for joining metal materials, comprising butting a cross section A of a flat metal material A against a cross section B of a flat metal material B, covering at least a portion of the opposing area, which is an area spanning both an edge portion A of metal material A and an edge portion B of metal material B, with a film including a layer whose main component is a thermoplastic resin, and melting and solidifying the film to join said metal material A and said metal material B.

[12] The method for connecting metal materials according to

[11] , wherein the metal material A and the metal material B are at least one selected from the group consisting of a metal plate having a thickness of 1 mm or less and a metal foil having a thickness of 1 mm or less.

[13] The method for connecting metal materials according to

[11] or

[12] , wherein the metal material A and the metal material B are in a strip shape, and the metal material A and the metal material B are butted together so as to be continuous in the longitudinal direction.

[14] The method for connecting metal materials according to any one of

[11] to

[13] , wherein the metal material A and the metal material B are rolled materials obtained by winding at least one selected from the group consisting of a metal plate and a metal foil into a roll.

[15] The method for connecting metal materials according to any one of

[11] to

[14] , wherein the coating is applied to both the flat surfaces of the front side of the metal material A and the metal material B and the flat surfaces of the back side of the metal material A and the metal material B.

[16] The method for connecting metal materials according to any one of

[11] to

[15] , wherein the thermoplastic resin is an amorphous thermoplastic resin.

[17] The method for connecting metal materials according to

[16] , wherein the amorphous thermoplastic resin is at least one selected from the group consisting of thermoplastic epoxy resins and phenoxy resins.

[18] The method for connecting metal materials according to

[17] , wherein the amorphous thermoplastic resin is an amorphous thermoplastic resin having an epoxy equivalent of 1,600 or more, or an amorphous thermoplastic resin not containing an epoxy group.

[19] The method for connecting metal materials according to any one of

[11] to

[18] , wherein the film has a thickness of 10 μm to 3 mm.

[20] the film has an adhesive on a surface covering the facing portion, The method for connecting metal materials according to any one of

[11] to

[19] , wherein the adhesive has a function of temporarily fixing the film and does not have an adhesive function. Effect of the Invention

[0014] It is possible to provide a connection technique that requires a short process time, is repairable, requires a short process time, is free from the risk of contamination of the production line by an adhesive component, and causes little change in thickness at the connection portion. [Brief description of the drawings]

[0015] [Figure 1] This is a plan view of a connected body of metal materials in one embodiment of the present invention, and is a schematic diagram of a connected body in which flat metal material A and flat metal material B, both of which are strip-shaped, are joined by butting together their widthwise cross sections. [Diagram 2] This is a front view of a connected body of metal materials in one embodiment of the present invention, and is a schematic diagram of a connected body in which flat metal material A and flat metal material B, both of which are strip-shaped, are joined by butting together their widthwise cross sections. [Diagram 3] This is a front view of a connected body of metal materials in another embodiment of the present invention, and is a schematic diagram of a connected body in which flat metal material A and flat metal material B, both of which are strip-shaped, are butted together and joined by their widthwise cross sections. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment of the present invention will be described in detail. In this specification, "connection" means connecting objects to form a continuous piece, and "bonding" is a subordinate concept. In this specification, "bonding" means connecting objects so that they come into contact with each other, and "adhesion" and "welding" are subordinate concepts. "Adhesion" means bonding two adherends (objects to be bonded) together using an organic material such as tape or adhesive (such as thermosetting resin or thermoplastic resin). "Welding" means melting the surface of a thermoplastic resin or the like with heat, and then cooling it to cause entanglement through molecular diffusion, resulting in a bonded state.

[0017] [Metal material connector] The connected metal material of the present invention is a connected metal material formed by butting a cross section A:5 of a flat metal material A:1 with a cross section B:6 of a flat metal material B:2, and covering at least a portion of an opposing portion 9, which is an area spanning both an edge portion A:7 of the metal material A:1 and an edge portion B:8 of the metal material B:2, with a film 3 including a layer mainly composed of a thermoplastic resin, and connecting the metal material A and the metal material B, wherein the film 3 is a film that has been melted and solidified at the opposing portion 9. In this specification, the term "main component" refers to the component that is contained in the largest amount among the resin components in the film. The film preferably contains 50% by mass or more of the resin component, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more.

[0018] By melting and solidifying the film 3 at the opposing portion 9, the film 3 is joined to the edge portion A:7 of the metal material A:1, and the film 3 is joined to the edge portion B:8 of the metal material B:2, thereby connecting the metal materials A and B and obtaining a connected body exhibiting excellent connecting strength. The film 3 melted at the opposing portion 9 penetrates into the gap between cross section A:5 of metal material A:1 and cross section B:6 of metal material B:2 and solidifies, thereby providing a connected body in which the butt surfaces 4 of cross sections A:5 and B:6 are joined, exhibiting even superior connection strength; however, in the connected body of the present invention, a gap may exist between cross section A:5 and cross section B:6. Since the strength of the connection is affected by many factors, such as the thickness of the film, the molecular weight and chemical structure of the polymer constituting the film, the mechanical properties, and the viscoelastic properties, in addition to the strength of the interfacial interaction between the film and the metal material, the details of the mechanism by which the connector of the present invention exhibits excellent connection strength are not clear, but it is presumed that the main factor is the formation of chemical bonds or intermolecular forces, such as hydrogen bonds or van der Waals forces, at the interfaces between the film and metal material A and between the film and metal material B. However, since the state or characteristics of the interface between the film and the metal material in the connector are specified by analyzing the chemical structure of an extremely thin interface at the nanometer level or less, it is impossible or impractical with current technology to specify it in a strict numerical range and express it in a distinguishable manner.

[0019] As described above, with current technology it is difficult to strictly distinguish by analysis or the like between a connected body connected by film 3 that has been melted and solidified at the opposing portion 9 and a connected body connected by adhesive tape. However, in practice, they are distinguished based on whether the corners of the film are rounded, whether there is variation in thickness, and the surface properties of the film surface that comes into contact with the edge, as described below. A film before melting and solidifying has sharp cut surfaces formed during the manufacturing process of the film, but the film 3 that constitutes the metal material connection body of the present invention is a film 3 that has been melted and solidified at the opposing portion 9, and therefore does not have sharp cut surfaces formed during the manufacturing process of the film, and it is presumed that the corners of the film are rounded. Since a film is usually manufactured to have a uniform thickness, there is no variation in thickness before melting and solidification. However, since the film 3 constituting the metal material joint of the present invention is a film 3 that has undergone melting and solidification at the opposing portion 9, it is presumed that there is a variation in thickness that inevitably occurs during the melting and solidification process. Any appropriate method can be adopted as a method for measuring the thickness variation, such as measuring the thickness of any multiple points on the surface of the measurement object and performing statistical processing. Examples of such a method for measuring the thickness include a method involving physical contact such as a micrometer, a micro caliper, a dial gauge, etc.; a non-contact method for measuring the transmittance or reflectance of alpha rays, X-rays, infrared rays, electromagnetic waves, etc. for the measurement object; a method for cutting the measurement object at any measurement point and observing it with an optical microscope or an electron microscope; and the like, and a combination of these may be adopted. It is presumed that after melting and solidifying at the facing portion 9, the film 3 has the surface texture of edge portion A:7 transferred to the film surface in contact with edge portion A:7, and the surface texture of edge portion B:8 transferred to the film surface in contact with edge portion B:8. Here, the surface texture refers to the fine irregularities created on the surface of the metal material during the machining process or the like of the metal material.

[0020] The connection of the present invention utilizes the phase change (solid-liquid-solid) of a film mainly composed of a thermoplastic resin, and is a connection that does not involve a chemical reaction such as a polymerization reaction. Since the film is used in a state where the polymerization reaction is completed, the polymerization reaction does not proceed even at room temperature, and the film can be stored for a long time at room temperature. The film can be softened and melted by heat and can be easily peeled off, so it has excellent dismantling properties. In addition, since a film mainly composed of a thermoplastic resin has thermoplastic properties, it can be reversibly softened, melted, and solidified repeatedly, and has excellent repairability. The connection using a film mainly composed of a thermoplastic resin utilizes the phase change (solid-liquid-solid) of the film, and has the advantage that it takes a short time compared to a polymerization reaction involving the formation of chemical bonds, and the process time is short. In addition, since a thermoplastic resin is not a liquid at room temperature but a solid where the polymerization reaction is completed, and adheres by a mechanism different from adhesion, it is unnecessary to use an adhesive for the purpose of adhesion, and there is no need to worry about contamination of the production line by an adhesive. In addition, since the polymerization reaction is completed, it has excellent heat resistance and chemical resistance. In addition, because the connection is made using a thin film, there is an advantage that there is less change in thickness at the connection compared to rivets, etc.

[0021] 1 to 3 are schematic diagrams of a connected body in which a flat metal material A: 1 and a flat metal material B: 2, both of which are strip-shaped, are joined by butting together their widthwise cross sections. As shown in Figure 2, it is preferable that the film is the opposing portion 9, and covers the metal material A:1 and the metal material B:2 on at least one of the flat portions of the front side of the metal material A and the metal material B and the flat portions of the back side of the metal material A and the metal material B. As shown in Figure 3, it is particularly preferable that the opposing portion 9 covers the metal material A:1 and the metal material B:2 with both the flat surface portions on the front side of the metal material A and the metal material B and the flat surface portions on the back side of the metal material A and the metal material B.

[0022] <Metal materials> The shapes of the metal material A and the metal material are not particularly limited as long as they are flat, but the present invention is suitable for applications in which metal plates having a thickness of 1 mm or less or metal foils having a thickness of 1 mm or less are connected, and the metal material A and the metal material B are both strip-shaped (long), and are suitable for applications in which opposing portions opposed to each other so as to be continuous in the longitudinal direction are connected. Specifically, the present invention is suitable for applications in which rolled material in which metal foil is wound in a roll shape is connected, and is particularly suitable for applications in which the end of a preceding rolled material being fed into a production line is connected to the start of a following rolled material, and for applications in which the end and start of a rolled material having a break in the roll is connected. In this specification, the metal foil means a highly ductile metal that is stretched into a thin paper shape.

[0023] The type of metal for metal material A and metal material B is not particularly limited, but is preferably at least one selected from the group consisting of aluminum, iron, copper, magnesium, and alloys thereof. From the viewpoint of the strength of the interfacial adhesion with the film, it is particularly preferable to use at least one selected from the group consisting of aluminum alloys and iron alloys, since this can achieve a strong connection. Furthermore, the surface of the metal material A or the metal material B may be metal plated or may be coated with resin.

[0024] By pretreating the opposing portions of metal material A and metal material B that are to be covered with the film, high adhesive strength may be obtained between the film and the metal material. As the pretreatment, a treatment for cleaning the surface of the metal material or a treatment for making the surface uneven is preferable. When the metal material is made of aluminum or iron, at least one pretreatment selected from the group consisting of degreasing treatment, UV ozone treatment, blasting treatment, polishing treatment, plasma treatment, and etching treatment is preferable. The pretreatment may be performed by one type alone or by two or more types. As the specific method of these pretreatments, known methods can be used.

[0025] <Film> In this specification, the term "film" refers to a thin film of a resin whose main component is a thermoplastic resin, or a thin film of a resin composition whose main component is a thermoplastic resin.

[0026] In order to fully impart the properties of a thermoplastic resin to the film, the content of the thermoplastic resin is preferably 60 mass % or more of the resin components in the film, more preferably 70 mass % or more, even more preferably 80 mass % or more, and most preferably 90 mass % or more.

[0027] The thermoplastic resin is preferably an amorphous thermoplastic resin. In this embodiment, the amorphous thermoplastic resin means a resin in which no crystals are present or the content of crystals is very small, specifically, the heat of fusion of the crystals is 15 J / g or less.

[0028] The heat of fusion is calculated from the area of ​​the endothermic peak of DSC (differential scanning calorimeter) and the weight of the thermoplastic resin component. When an inorganic filler or the like is contained in the film, it is calculated from the weight of the thermoplastic resin component excluding the inorganic filler. Specifically, 2-10 mg of a sample is weighed out, placed in an aluminum pan, and heated from 23°C to 200°C or higher at 10°C / min using a DSC (DSC8231 manufactured by Rigaku Corporation) to obtain a DSC curve, and then the heat of fusion can be calculated from the area of ​​the endothermic peak at the time of melting obtained from the DSC curve and the weighed value. The heat of fusion of the amorphous thermoplastic resin is more preferably 11 J / g or less, even more preferably 7 J / g or less, even more preferably 4 J / g or less, and most preferably the melting peak is below the detection limit.

[0029] In a film whose main component is an amorphous thermoplastic resin with a heat of fusion of 15 J / g or less, when heated to melt it, there is no sudden drop in viscosity as seen in conventional hot melt adhesives, and it does not reach a low viscosity state (0.001 to 100 Pa s) even in high temperature ranges exceeding 200°C. Therefore, the film does not melt and flow out, and the thickness after solidification can be maintained within a specified range, making it possible to stably obtain high bonding strength.

[0030] When the amorphous thermoplastic resin, which is the main component of the film, contains a small amount of crystals, the melting point is preferably 50 to 400° C., more preferably 60 to 350° C., and even more preferably 70 to 300° C. By having a melting point in the range of 50 to 400° C., the film efficiently deforms and melts when heated, and effectively wets and spreads over the respective bonding surfaces of the film and metal material A and the film and metal material B, thereby obtaining a high bonding strength. In this specification, the melting point of a thermoplastic resin means the melting peak temperature measured by DSC. If the melting peak is not obtained or the heat of fusion is 15 J / g or less, the melting point is the glass transition point plus 70°C. The glass transition point means the temperature at which the DSC curve starts to drop in the second cycle after heating to 200°C by DSC, cooling to 40°C or less, and further heating to 200°C.

[0031] The amorphous thermoplastic resin is preferably at least one selected from the group consisting of thermoplastic epoxy resins and phenoxy resins. Thermoplastic epoxy resins and phenoxy resins have low cohesive strength within the resin, and therefore have strong interactions with metal materials, and can connect metal materials with a stronger connecting strength than conventional crystalline hot melt adhesives. In addition, thermoplastic epoxy resins and phenoxy resins have excellent flexibility and toughness, and therefore can provide a high-strength connection.

[0032] The amorphous thermoplastic resin preferably has an epoxy equivalent of 1,600 or more, or does not contain an epoxy group. The epoxy equivalent (weight of the thermoplastic resin containing 1 mole of epoxy groups) is the epoxy equivalent of the thermoplastic resin contained in the film before linking, and is a value (unit: g / eq.) measured by the method specified in JIS-K7236:2001. Specifically, a potentiometric titrator is used to add brominated tetraethylammonium acetate solution, and a 0.1 mol / L perchloric acid-acetic acid solution is used, and the solvent-diluted product (resin varnish) is calculated as a solid content equivalent value from the non-volatile content. In the case of a mixture of two or more resins, it can also be calculated from the content and epoxy equivalent of each resin. The epoxy equivalent of the amorphous thermoplastic resin is more preferably 2,000 or more, even more preferably 5,000 or more, and even more preferably 9,000 or more, and most preferably is equal to or more than the detection limit so that the epoxy group is not substantially detected. Note that the epoxy equivalent being equal to or more than the detection limit means that the epoxy group is not detected when the epoxy equivalent is measured based on JIS K 7236:2001 described later.

[0033] By using a film whose main component is an amorphous thermoplastic resin with an epoxy equivalent of 1,600 or more, the sudden decrease in viscosity can be more effectively suppressed, and a higher bonding strength can be stably obtained.

[0034] <Thermoplastic epoxy resin> The thermoplastic epoxy resin is preferably a polymer of (a) a difunctional epoxy resin monomer or oligomer and (b) a difunctional compound having two identical or different functional groups selected from the group consisting of a phenolic hydroxyl group, a carboxyl group, a mercapto group, an isocyanato group, and a cyanate ester group. By using such a compound, the polymerization reaction for forming a linear polymer proceeds preferentially, making it possible to obtain a thermoplastic epoxy resin having the desired properties.

[0035] The (a) difunctional epoxy resin monomer or oligomer refers to an epoxy resin monomer or oligomer having two epoxy groups in the molecule. Specific examples of the (a) include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bifunctional phenol novolac type epoxy resins, bisphenol AD ​​type epoxy resins, biphenyl type epoxy resins, bifunctional naphthalene type epoxy resins, bifunctional alicyclic epoxy resins, bifunctional glycidyl ester type epoxy resins (e.g., diglycidyl phthalate, diglycidyl tetrahydrophthalate, dimer acid diglycidyl ester, etc.), bifunctional glycidyl amine type epoxy resins (e.g., diglycidyl aniline, diglycidyl toluidine, etc.), bifunctional heterocyclic epoxy resins, bifunctional diarylsulfone type epoxy resins, hydroquinone type epoxy resins (e.g., hydroquinone diglycidyl ether, 2,5-di-tert-butyl ether, etc.), t-Butylhydroquinone diglycidyl ether, resorcin diglycidyl ether, etc.), bifunctional alkylene glycidyl ether compounds (e.g. butanediol diglycidyl ether, butenediol diglycidyl ether, butynediol diglycidyl ether, etc.), bifunctional glycidyl group-containing hydantoin compounds (e.g. 1,3-diglycidyl-5,5-dialkylhydantoin, 1-glycidyl-3-(glycidoxyalkyl)-5,5-dialkylhydantoin, etc.), bifunctional glycidyl group-containing siloxanes (e.g. 1,3-bis(3-glycidoxypropyl)-1,1,3,3-tetramethyldisiloxane, α,β-bis(3-glycidoxypropyl)polydimethylsiloxane, etc.) and modified products thereof. Among these, bisphenol A type epoxy resins, bisphenol F type epoxy resins, and biphenyl type epoxy resins are preferred in terms of reactivity and workability. Examples of the bifunctional compound having a phenolic hydroxyl group in (b) include mononuclear aromatic dihydroxy compounds having one benzene ring, such as catechol, resorcin, and hydroquinone; bisphenols, such as bis(4-hydroxyphenyl)propane (bisphenol A), bis(4-hydroxyphenyl)methane (bisphenol F), and bis(4-hydroxyphenyl)ethane (bisphenol AD); compounds having a condensed ring, such as dihydroxynaphthalene; Examples include bifunctional phenol compounds having an allyl group introduced therein, such as resorcinol, diallyl bisphenol A, and triallyl dihydroxybiphenyl, and dibutyl bisphenol A. Specific examples of the (b) carboxy group-containing compound include adipic acid, succinic acid, malonic acid, cyclohexanedicarboxylic acid, phthalic acid, isophthalic acid, and terephthalic acid. Examples of the (b) bifunctional compound having a mercapto group include ethylene glycol bisthioglycolate and ethylene glycol bisthiopropionate. Specific examples of the (b) isocyanato group-containing bifunctional compound include diphenylmethane diisocyanate (MDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HMDI), and tolylene diisocyanate (TDI). Specific examples of the (b) cyanate ester group-containing bifunctional compound include 2,2-bis(4-cyanatophenyl)propane, 1,1-bis(4-cyanatophenyl)ethane, and bis(4-cyanatophenyl)methane. Among the above (b), a bifunctional compound having a phenolic hydroxyl group is preferred from the viewpoint of obtaining a thermoplastic polymer, a bifunctional compound having two phenolic hydroxyl groups and a bisphenol structure or a biphenyl structure is preferred from the viewpoint of heat resistance and connectability, and at least one selected from the group consisting of bisphenol A, bisphenol F and bisphenol S is preferred from the viewpoint of heat resistance and cost.

[0036] When the (a) is a bisphenol A type epoxy resin, a bisphenol F type epoxy resin, a bisphenol S type epoxy resin, or a biphenyl type epoxy resin, and the (b) is at least one selected from the group consisting of bisphenol A, bisphenol F, and bisphenol S, the polymer obtained by polymerization of the (a) and (b) has a main chain having a paraphenylene structure and an ether bond as a main skeleton, the main chain being linked by an alkylene group, and a structure in which a hydroxyl group generated by polyaddition is arranged in a side chain. The linear structure of the paraphenylene skeleton can increase the mechanical strength of the polymer after polymerization, and the hydroxyl groups arranged in the side chains can improve adhesion to metal materials. As a result, high bond strength can be achieved while maintaining the adhesiveness of the thermosetting resin. Furthermore, in the case of a thermoplastic resin, recycling and repair are possible by softening and melting with heat, improving the recyclability and repairability that are problems with thermosetting resins.

[0037] Phenoxy resin Phenoxy resin is a polyhydroxy polyether synthesized from bisphenols and epichlorohydrin, and has thermoplastic properties. For the production of phenoxy resin, a method of direct reaction of dihydric phenols with epichlorohydrin and a method of addition polymerization reaction of diglycidyl ether of dihydric phenols with dihydric phenols are known, but the phenoxy resin used in the present invention may be obtained by either method. In the case of direct reaction of dihydric phenols with epichlorohydrin, examples of dihydric phenols include phenols such as bisphenol A, bisphenol F, bisphenol S, biphenol, biphenylenediol, and fluorenediphenyl; and aliphatic glycols such as ethylene glycol, propylene glycol, and diethylene glycol. Among them, bisphenol A, bisphenol F, and bisphenol S are preferred from the viewpoints of cost, connectivity, viscosity, and heat resistance. These may be used alone or in combination of two or more. Phenoxy resin has a chemical structure similar to that of epoxy resin, with a paraphenylene structure and an ether bond as the main skeleton, a main chain connecting these, and a structure in which hydroxyl groups are arranged in the side chains.

[0038] <Physical properties of thermoplastic epoxy resin and phenoxy resin> The thermoplastic epoxy resin and the phenoxy resin preferably have a weight average molecular weight of 10,000 to 500,000, more preferably 18,000 to 300,000, and even more preferably 20,000 to 200,000, which is a value calculated in terms of polystyrene by GPC (gel permeation chromatography). The weight average molecular weight is calculated from the elution peak position detected by GPC, and each is a value of the molecular weight calculated in terms of standard polystyrene. When the weight average molecular weight is within this range, the balance between thermoplasticity and heat resistance is good, and a linker can be efficiently obtained by melting, and the heat resistance is also high. When the weight average molecular weight is 10,000 or more, the heat resistance is excellent, and when it is 500,000 or less, the viscosity during melting is low and the linkage is high.

[0039] <Components other than the resin component in the film> If necessary, the film may or may not contain fillers and additives as components other than the resin component, provided that the object of the present invention is not impaired.

[0040] The filler includes inorganic fillers and organic fillers (resin powder). Examples of inorganic fillers include spherical fused silica, metal powders such as iron, silica sand, talc, calcium carbonate, mica, acid clay, diatomaceous earth, kaolin, quartz, titanium oxide, silica, phenolic resin microballoons, and glass balloons. When the film contains a filler, the content of the filler in the total amount (100 volume %) of the film is preferably 50 volume % or less, more preferably 30 volume % or less, further preferably 20 volume % or less, and most preferably 10 volume % or less. The volume of the filler can be calculated by dividing the weight of the filler contained in the film by the apparent volume of the filler. The content of the resin component in the total amount (100 volume%) of the film is preferably 10 volume% or more, more preferably 20 volume% or more, even more preferably 30 volume% or more, and even more preferably 50 volume% or more, in one embodiment 80 volume% or more, in another embodiment 90 volume% or more, and in another embodiment 99 volume% or more.

[0041] Examples of the additives include antifoaming agents, coupling agents such as silane coupling agents, pigments, etc., and these may be contained alone or in combination of two or more. The content of the additive in the film is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less. The content of the resin component in the film is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and still more preferably 50% by mass or more, in one embodiment 80% by mass or more, in another embodiment 90% by mass or more, and in another embodiment 99% by mass or more.

[0042] Film morphology and physical properties The film preferably has a thickness of 10 μm to 3 mm. From the viewpoint of obtaining a linker with excellent connectivity in a short process time, the thickness of the film is more preferably 1 mm or less, even more preferably 0.5 mm or less, even more preferably 0.3 mm or less, particularly preferably 0.2 mm or less, and most preferably 0.1 mm or less. By making the film 10 μm to 3 mm thick, it can be efficiently spread by heating, pressing, etc. between the bonding surfaces of the film and metal material A and between the film and metal material B, and a high bonding strength can be obtained.

[0043] The film may be a single layer or a laminate of multiple layers, but from the viewpoint of ease of production and improvement of the connecting strength, the thermoplastic resin layer is preferably a single layer. Alternatively, the film may be a multi-layer film in which the thermoplastic resin is laminated on a film substrate made of a resin having a melting point higher than that of the resin composition. In such a case, the resin film substrate does not melt when heat-welded to the metal substrate, and the thickness of the resin film substrate remains, so that good connecting strength can be maintained.

[0044] The film may also have tackiness to the extent that it does not impair its binding strength or its heat resistance. Tackiness may be imparted by mixing a tackifier into the thermoplastic resin, or by applying an adhesive to the film. The adhesive preferably functions to temporarily hold the film but does not have an adhesive function. An adhesive that temporarily holds the film but does not have an adhesive function is, for example, an adhesive that remains within the surface of the film that covers the facing portion 9 and is not exposed outside the surface. The adhesive may be applied to the entire surface of the surface covering the facing portion 9, or may be applied to a part of the surface covering the facing portion 9 in a striped, dotted, lattice, tiled, or other pattern (a shape in which multiple squares are arranged with gaps between them). The smaller the application area, the lower the tackiness, but the lower the risk that the adhesive will be exposed to the outside from the end face of the film after connection and become a cause of contamination.

[0045] In conventional adhesive tapes, the adhesive strength between the metal material and the film is provided only by the adhesiveness of the adhesive layer of the adhesive tape, but in the case of the thermoplastic film, the adhesive strength is provided by the adhesion caused by the melting and solidification of the thermoplastic resin as described above, so the tackiness is preferably such that it provides the temporary fixing function as described above. In other words, when the film is placed on the metal material, the film does not need to stick to the metal material, and it is sufficient that the resistance is increased (it becomes less slippery) when a force in the shear direction is applied. For the purpose of imparting tackiness sufficient to provide a temporary fixing function, it is preferable to limit the amount of adhesive applied to the minimum amount necessary to temporarily hold the film (to prevent slipping).

[0046] With conventional adhesive tapes that have an adhesive layer on only one side, the adhesive layer is generally not exposed to the outside of the joining surface after metal materials are joined. However, if there are areas where the adhesive layer protrudes onto the edge of the joining surface, the adhesive can adhere to the transport path or mold in the production line, causing contamination. In addition, the end faces of strip-shaped metal material are not necessarily straight. In such cases, gaps will form between the end faces of the two metal materials to be joined. If adhesive tape is applied to such a gap, the adhesive layer will be exposed from the gap and the adhesive may adhere to the transport path or molds in the production line, causing contamination. Furthermore, when the substrate is laminated with a single-sided adhesive tape, the adhesive portion is less exposed, but it is difficult to completely match both the front and back surfaces. In addition, when the substrate is butted, the shape of the end surface may be irregular, and the adhesive layer may be exposed in that area, causing contamination by adhering to the conveying path or mold of the production line. According to the present invention, in which bonding strength is achieved by adhesion through melting and solidifying a thermoplastic resin, adhesives are basically not required for bonding purposes, and even if an adhesive is used for purposes such as positioning, it can be used only to a minimum extent, thereby avoiding all of the above-mentioned problems associated with conventional adhesive tapes.

[0047] The breaking strength of the film in the connected body of the metal material A and the metal material B connected by the film is preferably 20 to 1000 N / 25 mm. When the connected body is connected by two films on the front and back, the breaking strength is the strength when the film is first broken.

[0048] The breaking strength of the film in the connected body is more preferably 50 to 1000 N / 25 mm, and most preferably 100 to 1000 N / 25 mm.

[0049] The breaking strength when the metal material A and the metal material B are connected using the film is the tensile strength at break per 25 mm film width measured under the conditions described in the Examples section.

[0050] <Film manufacturing method> The method for producing a film including a layer mainly composed of a thermoplastic resin is not particularly limited. For example, a resin composition may be obtained by heating and polymerizing a monomer or oligomer of a bifunctional epoxy compound, adding a solvent to the obtained resin composition as necessary, applying the composition to a release film or the like, curing and drying, and applying pressure as necessary to obtain a film. The polymerization reaction may be carried out after application to a release film or after the film is obtained, or a combination of these may be used.

[0051] [Metal material connection method] The method for producing a connected body according to this embodiment includes the steps of butting a cross section A of a flat metal material A against a cross section B of a flat metal material B, covering at least a part of the opposing portion, which is a region spanning both an edge portion A of metal material A and an edge portion B of metal material B, with a film including a layer mainly composed of a thermoplastic resin, and melting and solidifying the film to connect the metal material A and the metal material B. By melting and solidifying the film, the film and the metal material A and the film and the metal material B are bonded to each other, and the metal material A and the metal material B are connected to each other. The metal material and film are the same as those constituting the above-mentioned connecting body, and therefore a description thereof will be omitted.

[0052] <Melting and solidifying the film> The method for melting the film is not particularly limited as long as it is a means capable of heating and melting the film. Specifically, the film may be melted by at least one method selected from the group consisting of contact heating, hot air heating, heat pressing, impulse heater heating, hot plate welding, infrared heating, ultrasonic welding, vibration welding, and high-frequency induction welding. Among these, melting by an impulse heater or heat pressing is preferred from the viewpoint of ease of production and shortening the process.

[0053] In the case of hot pressing, it is more preferable to carry out the heating and pressing under conditions of 100 to 400° C. and 0.001 to 20 MPaG. The heating conditions are more preferably 100 to 300° C., even more preferably 120 to 250° C., and most preferably 150 to 220° C. By heating at 100 to 400° C., the film efficiently deforms and melts, effectively wetting and spreading over the respective bonding surfaces of the film and metal material A and the film and metal material B, thereby obtaining a high bonding strength. The pressure is preferably from 0.001 to 20 MPaG, more preferably from 0.005 to 10 MPaG, and most preferably from 0.01 to 5 MPaG. By applying a pressure of from 0.001 to 20 MPaG, the film is efficiently deformed and effectively wetted and spread, thereby obtaining a high connecting strength. By melting and solidifying the film, the film and metal material A and the film and metal material B are bonded to each other, and metal material A and metal material B are connected to each other.

[0054] In the case of ultrasonic welding, the transmission frequency is preferably 10 to 70 kHz, and more preferably 15 to 40 kHz. From the viewpoints of adhesion and appearance, the ultrasonic application time is preferably 0.1 to 3 seconds, and more preferably 0.2 to 2 seconds. When pressure is applied during ultrasonic application, the pressure is preferably 0.01 to 20 MPaG, more preferably 0.1 to 10 MPaG, and even more preferably 0.2 to 5 MPaG. Within this pressure range, the film is efficiently deformed and effectively wets and spreads across the adhesive surface, resulting in high adhesive strength. In the case of high-frequency induction welding, the output may be in the range of 100 to 5000 W, and the oscillation time may be adjusted according to the size and type of the resin substrate, and is, for example, preferably 1.0 to 10.0 seconds, and more preferably 1.5 to 8.0 seconds.

[0055] Methods for solidifying the molten film include a method of cooling at room temperature or a method of cooling using a cooling device. Here, "room temperature" means a general room temperature within the range of 5 to 30° C. Among these, the method of cooling at room temperature is preferred from the viewpoint of ease of production.

[0056] In this specification, "solidified" means that the film is solid at room temperature, that is, has no fluidity in the absence of pressure at 23° C. However, the film after solidification may have tackiness. EXAMPLES

[0057] Next, specific examples of the present invention will be described, but the present invention is not particularly limited to these examples.

[0058] <Metal material A and metal material B> As metal material A and metal material B, C1100 (tough pitch copper) having a width of 25 mm, a length of 100 mm and a thickness of 0.1 mm was prepared.

[0059] <Weight average molecular weight, heat of fusion and epoxy equivalent of thermoplastic epoxy resin and phenoxy resin> The weight average molecular weight, heat of fusion and epoxy equivalent of the thermoplastic epoxy resin and the phenoxy resin were determined as follows.

[0060] (Weight average molecular weight) Thermoplastic epoxy resin or phenoxy resin was dissolved in tetrahydrofuran, and measurement was performed under the following conditions using Prominence 501 (manufactured by Showa Science Co., Ltd., Detector: Shodex (registered trademark) RI-501 (manufactured by Showa Denko K.K.)). Column: Showa Denko LF-804 x 2 Column temperature: 40℃ Sample: 0.4% by mass of resin in tetrahydrofuran Flow rate: 1ml / min Eluent: Tetrahydrofuran Calibration method: Conversion using standard polystyrene

[0061] (Heat of fusion) 2 to 10 mg of thermoplastic epoxy resin or phenoxy resin was weighed out and placed in an aluminum pan, and the temperature was raised from 23°C to 200°C at 10°C / min using a DSC (DSC8231 manufactured by Rigaku Corporation) to obtain a DSC curve. The heat of fusion was calculated from the area of ​​the endothermic peak at the time of melting in the DSC curve and the weighed value.

[0062] (epoxy equivalent) The values ​​were measured in accordance with JIS K-7236:2001 and converted into values ​​based on the resin solid content. In the case of simple mixtures that did not involve reactions, the values ​​were calculated from the epoxy equivalent and content of each.

[0063] < Reference example 1> (Film P-1) In a reaction apparatus equipped with a stirrer, reflux condenser, gas inlet tube, and thermometer, 1.0 equivalent (203 g) of jER (registered trademark) 1007 (manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, weight average molecular weight about 10,000), 1.0 equivalent (12.5 g) of bisphenol S, 2.4 g of triphenylphosphine, and 1,000 g of methyl ethyl ketone were charged, and the temperature was raised to 100°C while stirring under a nitrogen gas atmosphere. After visually confirming that the mixture had dissolved, the mixture was cooled to 40°C to obtain a resin composition with a solid content of about 20% by mass. The solvent was removed from this to obtain a solid. A non-adhesive fluororesin film (Nitoflon (registered trademark) No. 900UL, manufactured by Nitto Denko Corporation) was placed on the upper and lower plates of a press machine, and the solid was placed on the non-adhesive fluororesin film of the lower plate. The press machine was then heated to 160°C, and the resin composition or phenoxy resin was heat-compressed for 2 hours to obtain a solid adhesive (P-1) in the form of a film having a thickness of 100 μm and a solid content of 100 mass%. The weight-average molecular weight was about 37,000. The epoxy equivalent was above the detection limit (i.e., almost no epoxy groups were present). No heat of fusion peak was detected in DSC, confirming that the material was amorphous. (concatenation) The cross section A of the metal material A and the cross section B of the metal material B were butted against each other, and the facing portions of the edge portion A of the metal material A and the edge portion B of the metal material B were covered with the film P-1 cut to a size of 20 x 25 mm across the width direction (25 mm) on each of the front and back sides, and the metal material was placed on a hot plate set at 200 ° C. with the metal material facing down. A 3 x 3 cm glass plate was placed on the film P-1 covering the facing portion, and a 2 kg weight was placed on the glass plate to perform welding for 1 minute. After the welding, the glass plate and the weight were removed and the film P-1 was cooled to room temperature. After cooling, the film was turned over and placed on the hot plate set at 200 ° C. again, and a 3 x 3 cm glass plate was placed on the film P-1 covering the facing portion, and a 2 kg weight was placed on the glass plate to perform welding for 1 minute, to produce a connected body.

[0064] <Example 2> (Film P-2) A reactor equipped with a stirrer, reflux condenser, gas inlet tube, and thermometer was charged with 20 g of Phenototo (registered trademark) YP-50S (manufactured by Nippon Steel Chemical & Material Co., Ltd., phenoxy resin, weight average molecular weight about 50,000) and 80 g of cyclohexanone, and the mixture was heated to 60°C while stirring, and the mixture was confirmed to have dissolved by visual inspection, and cooled to 40°C to obtain a resin composition with a solid content of 20% by mass. The resin composition was applied onto a release film and dried at 120°C for 30 minutes to obtain a film P-2 with a solid content of 100% by mass and a thickness of 100 μm. The epoxy equivalent was above the detection limit (i.e., almost no epoxy groups were present). No heat of fusion peak was detected in DSC, and it was confirmed to be amorphous. (concatenation) Other than using P-2 as the film Reference example A conjugate was prepared in the same manner as in 1.

[0065] <Example 3> (Film P-3) A reactor equipped with a stirrer, reflux condenser, gas inlet tube, and thermometer was charged with 20 g of Phenototo (registered trademark) YPS-007A (manufactured by Nippon Steel Chemical & Material Co., Ltd., phenoxy resin, weight average molecular weight about 42000) and 80 g of cyclohexanone, and the mixture was heated to 60°C while stirring, and the mixture was confirmed to have dissolved by visual inspection, and cooled to 40°C to obtain a resin composition with a solid content of 20% by mass. The resin composition was applied onto a release film and dried at 120°C for 30 minutes to obtain a film P-3 with a solid content of 100% by mass and a thickness of 100 μm. The epoxy equivalent was above the detection limit (i.e., almost no epoxy groups were present). No heat of fusion peak was detected in DSC, and it was confirmed to be amorphous. (concatenation) Other than using P-3 as film Reference example A conjugate was prepared in the same manner as in 1.

[0066] < Reference example 4> (concatenation) Except for the fact that a PET film (thickness 25 μm) was placed on top of the solid adhesive P-1, Reference example 1 A conjugate was prepared in the same manner as described above.

[0067] <Comparative Example 1> (concatenation) Cross section A of metal material A and cross section B of metal material B were butted together, and the opposing portions of edge portion A of metal material A and edge portion B of metal material B were covered and adhered to each other across the width (25 mm) on both the front and back with adhesive tape cut to a size of 20 x 25 mm (Sekisui Cellotape (registered trademark) No. 252 manufactured by Sekisui Chemical Co., Ltd., thickness 50 μm before the connector was made) to create a connector.

[0068] <Comparative Example 2> (concatenation) The film used was a crystalline olefin-based hot melt adhesive film (Elfan (registered trademark) NT-120, manufactured by Nihon Matai Co., Ltd., thickness 80 μm before linking) and the temperature of the hot plate was set to 150 ° C. Reference exampleThe conjugate was prepared in the same manner as in 1. The heat of fusion peak in DSC was 60 J / g.

[0069] <Comparative Example 3> (concatenation) A linked body was prepared in the same manner as in Comparative Example 1, except that a heat-resistant adhesive tape (polyimide tape PB416-20-30, manufactured by AS ONE Corporation) cut to a size of 20×25 mm was used as the adhesive tape.

[0070] [Breaking strength measurement_tensile test] The tensile strength of the connected bodies obtained in Examples 1 to 4 and Comparative Examples 1 to 3 was measured. The measurement conditions were a gripping distance of 13 cm and a tensile speed of 5 mm / min, using a Shimadzu Corporation universal testing machine Autograph AG-X Plus. The measurement results (breaking strength) are shown in Table 1. The measurements were taken under the conditions of "room temperature: 23°C", "hot at 80°C", and "soaked in ethylene glycol". In Table 1, the measurements under the "hot at 80°C" condition are values ​​measured in an atmosphere at 80°C. In Table 1, the measurements under the "soaked in ethylene glycol" condition are values ​​measured after soaking in ethylene glycol at 40°C for 5 days, removing the sample, soaking it in water for 5 seconds, wiping off the ethylene glycol, photographing the appearance, leaving it to stand for 20 to 30 minutes, and then measuring at room temperature.

[0071] [Line contamination] After the tensile test, it was observed whether the adhesive surface was exposed on the surface. If the adhesive surface was exposed on the surface, it could contaminate the line, so those with the adhesive surface exposed were rated as "X" and those without the adhesive surface exposed were rated as "O". The evaluation results are shown in Table 1.

[0072] [Table 1] [Industrial Applicability]

[0073] The present invention is suitable for applications such as connecting frame materials in a production line for LED lead frames and connecting board materials in a production line for flexible printed circuit boards, but is not limited to these exemplary applications. [Explanation of symbols]

[0074] 1 Metal material A 2 Metal material B 3. Film (film that constitutes the connecting body) 4. Mating surface 5 Cross section A 6 Cross section B 7 Edge A 8 Edge B 9 Opposing Part

Claims

1. A connected body of metal materials is formed by butting a cross section A of a flat metal material A against a cross section B of a flat metal material B, covering at least a part of an opposing portion, which is a region spanning both an edge portion A of the metal material A and an edge portion B of the metal material B, with a film including a layer mainly composed of a thermoplastic resin, and connecting the metal material A and the metal material B, the film is a film that has undergone melting and solidification at the opposing portion, The thermoplastic resin is an amorphous thermoplastic resin, the amorphous thermoplastic resin is at least one selected from the group consisting of a thermoplastic epoxy resin and a phenoxy resin, The thermoplastic epoxy resin is (a) a polymer of a bifunctional epoxy resin monomer or oligomer and (b) a bifunctional compound having two identical or different functional groups selected from the group consisting of a phenolic hydroxyl group, a carboxyl group, a mercapto group, an isocyanate group, and a cyanate ester group (excluding bisphenols and polyhydroxy polyethers synthesized from epichlorohydrin), The phenoxy resin is a polyhydroxy polyether synthesized from a bisphenol and epichlorohydrin, The film is produced by removing the solvent from a resin composition dissolved in a solvent to form a film. A metal connector.

2. 2. The metal material linkage according to claim 1, wherein the metal material A and the metal material B are at least one selected from the group consisting of a metal plate having a thickness of 1 mm or less and a metal foil having a thickness of 1 mm or less.

3. 2. The metal material connection according to claim 1, wherein the metal material A and the metal material B are in a strip shape, and the metal material A and the metal material B are butted together so as to be continuous in the longitudinal direction.

4. The connected body of metal materials according to claim 3 , wherein the metal material A and the metal material B are rolled materials each formed by winding at least one selected from the group consisting of a metal plate and a metal foil into a roll shape.

5. The metal material connection body according to claim 1, wherein the coating is formed on both the flat surface portions of the front side of the metal material A and the flat surface portions of the back side of the metal material A and the flat surface portions of the metal material B.

6. 2. The metal material linkage according to claim 1, wherein the amorphous thermoplastic resin is an amorphous thermoplastic resin having an epoxy equivalent of 1,600 or more, or an amorphous thermoplastic resin containing no epoxy groups.

7. The metal material connector according to claim 1, wherein the film has a thickness of 10 μm to 3 mm.

8. the film has an adhesive on a surface covering the facing portion, The metal material connector according to claim 1 , wherein the adhesive material functions to temporarily fasten the film but does not function as an adhesive.

9. A method for connecting metal materials, comprising: butting a cross section A of a flat metal material A against a cross section B of a flat metal material B; covering at least a part of an opposing portion, which is a region spanning both an edge portion A of the metal material A and an edge portion B of the metal material B, with a film including a layer mainly composed of a thermoplastic resin; and melting and solidifying the film to connect the metal material A and the metal material B, the film is a film that has undergone melting and solidification at the opposing portion, The thermoplastic resin is an amorphous thermoplastic resin, the amorphous thermoplastic resin is at least one selected from the group consisting of a thermoplastic epoxy resin and a phenoxy resin, The thermoplastic epoxy resin is (a) a polymer of a bifunctional epoxy resin monomer or oligomer and (b) a bifunctional compound having two identical or different functional groups selected from the group consisting of a phenolic hydroxyl group, a carboxyl group, a mercapto group, an isocyanate group, and a cyanate ester group (excluding bisphenols and polyhydroxy polyethers synthesized from epichlorohydrin), The phenoxy resin is a polyhydroxy polyether synthesized from a bisphenol and epichlorohydrin, The film is produced by removing the solvent from a resin composition dissolved in a solvent to form a film. A method for connecting metal materials.

Citation Information

Patent Citations

  • process for joining components

    DE102016212622A1

  • JP1973021724B1

  • Bonding method of metal plate

    JP1981089520A

  • Base material connecting method and base material connecting device

    JP1998157896A

  • Method of producing sheet joined body, and sheet joined body

    JP2009298136A