Optical sheets and optical components
The optical sheet with continuous layers at the interface between base materials and a half mirror layer addresses peeling issues during thermal bending, ensuring excellent processability and durability.
Patent Information
- Application Number
- JP2023560774
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Existing optical sheets with a half mirror layer face challenges in maintaining excellent workability and reliability during thermal bending processes, leading to potential peeling at the interface between the base material and the half mirror layer.
The optical sheet is designed with a first and second base material bonded to a half mirror layer composed of alternately stacked high and low refractive index layers, forming continuous layers at the interfaces to prevent peeling during thermal bending, ensuring excellent processability.
The solution effectively suppresses peeling between the base materials and the half mirror layer, allowing for accurate thermal bending into curved shapes with maintained optical properties and durability.
Smart Images

Figure 0007563628000010 
Figure 0007563628000011 
Figure 0007563628000012
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical sheet and an optical component. [Background technology]
[0002] In recent years, for the purpose of improving the design of lenses for eyewear such as spectacles and sunglasses, lenses have been proposed which have on their surface an optical sheet equipped with a half-mirror layer that selectively reflects light in a specific wavelength range and transmits light in other wavelength ranges.
[0003] For example, a lens having such an optical sheet on its surface is manufactured by preparing an optical sheet having a flat plate shape in a plan view, and punching the optical sheet into a predetermined shape such as a circular shape in a plan view with protective films attached to both sides of the optical sheet. Then, the optical sheet is subjected to a thermal bending process under heating to form a curved optical sheet having a curved convex surface and a curved concave surface curved by thermal bending. Then, after peeling the protective film from the curved optical sheet, the curved optical sheet is placed in a state of being adsorbed to a mold having a curved concave surface such that the concave surface of the mold and the convex surface of the curved optical sheet come into contact with each other. In this state, a resin layer (molded layer) mainly made of a resin material is formed on the concave surface of the curved optical sheet by using an insert injection molding method, thereby manufacturing a lens having an optical sheet on its surface (see, for example, Patent Document 1).
[0004] In such a lens manufacturing method, as described above, a thermal bending process is performed in which an optical sheet is thermally bent to obtain a curved optical sheet having one surface that is curved concave and the other surface that is curved convex. In this thermal bending process, the optical sheet is required to have excellent processability.
[0005] For this reason, there has been a demand for the development of optical sheets that have excellent processability and that have a half-mirror layer that selectively reflects light in a specific wavelength range and transmits light in other wavelength ranges. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2009-294445 A Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide an optical sheet having a half mirror layer that selectively reflects light in a specific wavelength range and transmits light in other wavelength ranges, which can exhibit excellent processability, and an optical component having excellent reliability and which includes such an optical sheet. [Means for solving the problem]
[0008] Such objectives are as follows: 10 This is achieved by the present invention described in (1) a first substrate made primarily of a resin material having optical transparency; a half mirror layer provided on one surface of the first base material and made of a laminate in which high refractive index layers and low refractive index layers are alternately and repeatedly laminated; an optical sheet including a second substrate that is mainly made of the resin material and is bonded to a surface of the half mirror layer opposite to the first substrate, In the half mirror layer, the refractive index of the high refractive index layer is higher than the refractive index of the low refractive index layer, The interface between the first substrate and the half mirror layer forms a continuous layer between the first substrate and the half mirror layer, and the interface between the second substrate and the half mirror layer forms a continuous layer between the second substrate and the half mirror layer. And, The half mirror layer has a thickness direction retardation (Rth) of 300 nm or less at a wavelength of 589 nm. An optical sheet characterized by:
[0009] (2) The optical sheet according to (1) above, wherein Tg1 is a glass transition point of a main material constituting the high refractive index layer, and Tg2 is a glass transition point of a main material constituting the low refractive index layer, and Tg1, Tg2 are greater than or equal to 105° C.
[0010] (3) The optical sheet according to the above (2), wherein the glass transition point Tg1 and the glass transition point Tg2 satisfy the relationship: 0°C≦|Tg1-Tg2|≦60°C.
[0011] (4) The optical sheet according to (2) or (3), wherein the lower of the glass transition points Tg1 and Tg2 is 110° C. or higher and 250° C. or lower.
[0012] (5) An optical sheet according to any one of (1) to (4) above, wherein the refractive index difference (N1-N2) is 0.05 or more and 0.25 or less, where N1 is the refractive index of the high refractive index layer at a wavelength of 589 nm and N2 is the refractive index of the low refractive index layer at a wavelength of 589 nm.
[0013] (6) The optical sheet according to any one of (1) to (5) above, wherein the high refractive index layer and the low refractive index layer each have an average thickness of 50 nm or more and 300 nm or less.
[0014] (7) The optical sheet according to any one of (1) to (6) above, wherein the number of times the high refractive index layers and the low refractive index layers are alternately stacked in the half mirror layer is 50 to 750.
[0016] ( 8 ) the reflectance of light having a wavelength of 589 nm of the curved optical sheet when the optical sheet is curved at a curvature radius of 60 mm at a temperature 10° C. higher than the higher of the glass transition point Tg1 of the main material constituting the high refractive index layer and the glass transition point Tg2 of the main material constituting the low refractive index layer is R1 [%], The above-mentioned curved optical sheet is stored in a heat circulation oven at a temperature of 105° C. for 1000 hours, and then, when the reflectance of the curved optical sheet at a wavelength of 589 nm is R2 [%], the reflectance retention calculated by R2 / R1×100 [%] is 80% or more. 7 2. The optical sheet according to claim 1 ,
[0017] ( 9 ) the optical sheet is curved at a temperature 10° C. higher than the higher of the glass transition point Tg1 of the main material constituting the high refractive index layer and the glass transition point Tg2 of the main material constituting the low refractive index layer, and the optical sheet is curved at a curvature radius of 60 mm, and after storing the optical sheet in a heat circulation oven at a temperature environment of 105° C. for 1000 hours, the number of the curved optical sheets in which peeling has occurred between the first substrate and the half mirror layer or between the second substrate and the half mirror layer is 2 or less out of 50 curved optical sheets, 8 2. The optical sheet according to claim 1 ,
[0018] ( 10 ) (1) or ( 9 2. An optical component comprising the optical sheet according to claim 1 . Effect of the Invention
[0019] According to the present invention, the half mirror layer includes a repeating portion formed of a laminate in which high refractive index layers and low refractive index layers are alternately stacked, and the first and second substrates bonded to the half mirror layer form a continuous layer between the first substrate and the half mirror layer at the interface between the first substrate and the half mirror layer, and form a continuous layer between the second substrate and the half mirror layer at the interface between the second substrate and the half mirror layer. Therefore, even if the optical sheet is subjected to a thermal bending process to obtain a curved optical sheet with one surface of the optical sheet being a curved concave surface and the other surface being a curved convex surface, peeling between the first substrate and the half mirror layer and the second substrate and the half mirror layer can be appropriately suppressed or prevented. Therefore, an optical sheet with excellent processability can be obtained. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a perspective view showing an embodiment of sunglasses equipped with lenses having a curved optical sheet obtained by curvedly forming the optical sheet of the present invention. [Diagram 2] FIG. 2 is a schematic diagram for explaining a method for producing a lens having a curved optical sheet obtained by curvedly forming the optical sheet of the present invention. [Diagram 3] FIG. 3 is a vertical cross-sectional view showing a first embodiment of the optical sheet of the present invention. [Figure 4] FIG. 4 is an enlarged cross-sectional view of a part of the half mirror layer of the optical sheet, located in the area [B] surrounded by the dashed line in FIG. [Diagram 5] FIG. 5 is a vertical cross-sectional view showing a second embodiment of the optical sheet of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, the optical sheet and optical component of the present invention will be described in detail based on preferred embodiments shown in the accompanying drawings.
[0022] The optical sheet of the present invention comprises a first substrate mainly made of a resin material having optical transparency, a half mirror layer bonded to one surface of the first substrate and having a laminate in which high refractive index layers and low refractive index layers are alternately and repeatedly laminated, and a second substrate mainly made of the resin material and bonded to a surface of the half mirror layer opposite to the first substrate. In the half mirror layer, the refractive index of the high refractive index layer is higher than the refractive index of the low refractive index layer, the interface between the first substrate and the half mirror layer forms a continuous layer between the first substrate and the half mirror layer, and the interface between the second substrate and the half mirror layer forms a continuous layer between the second substrate and the half mirror layer.
[0023] In this way, in the present invention, the half mirror layer and the first and second substrates form a continuous layer between the first substrate and the half mirror layer at the interface between the first substrate and the half mirror layer, and form a continuous layer between the second substrate and the half mirror layer at the interface between the second substrate and the half mirror layer. Therefore, even if the optical sheet is subjected to a thermal bending process to obtain a curved optical sheet by making one surface of the optical sheet a curved concave surface and the other surface a curved convex surface, peeling between the first substrate and the half mirror layer and the second substrate and the half mirror layer can be appropriately suppressed or prevented. Therefore, an optical sheet with excellent processability can be obtained.
[0024] The curved optical sheet of the present invention, which is obtained by subjecting the optical sheet of the present invention to a thermal bending process under heating, and has a curved shape with a curved convex surface and a curved concave surface, is used as a curved resin substrate (curved resin substrate) of a lens of sunglasses, which is a type of spectacles, for example, to impart half-mirror properties to the lens. Therefore, in the following, first, the sunglasses will be described before describing the optical sheet of the present invention.
[0025] <Sunglasses> Fig. 1 is a perspective view showing an embodiment of sunglasses equipped with lenses having a curved optical sheet obtained by curvedly forming the optical sheet of the present invention. In Fig. 1, when the sunglasses are worn on the head of a user, the surface of the lens facing the user's eyes is called the back surface, and the opposite surface is called the front surface.
[0026] As shown in FIG. 1, the sunglasses 100 include a frame 20 and a lens 30 (a lens for glasses).
[0027] In this specification, the term "lens (spectacle lens)" includes both lenses having a light-collecting function and lenses having no light-collecting function.
[0028] The frame 20 is a member that is attached to the head of the user and that positions the lenses 30 in front of and near the eyes of the user.
[0029] The frame 20 has a rim portion 21, a bridge portion 22, a temple portion 23, and a nose pad portion 24.
[0030] The rim portions 21 are ring-shaped, one for each of the right and left eyes, and have lenses 30 attached to their insides. This allows the user to view external information through the lenses 30.
[0031] Furthermore, the bridge portion 22 is rod-shaped and is positioned in front of the upper part of the user's nose when the glasses are worn on the user's head, connecting the pair of rim portions 21 together.
[0032] The temple portion 23 is shaped like a temple and is connected to the edge of each rim portion 21 on the opposite side to the position where the bridge portion 22 is connected. The temple portion 23 is hung on the user's ear when wearing the glasses on the user's head.
[0033] The nose pads 24 are provided on the edges of the rims 21 that correspond to the nose of the user when the sunglasses 100 are worn on the head of the user, and come into contact with the nose of the user, forming a shape that corresponds to the contact portion of the nose of the user at this time. This allows the sunglasses 100 to be stably maintained when worn.
[0034] The constituent materials of each part constituting the frame 20 are not particularly limited, and for example, various metal materials, various resin materials, etc. may be used. The shape of the frame 20 is not limited to the shape shown in the figure, as long as it can be worn on the head of the user.
[0035] A lens 30 (optical component of the present invention) is attached to each of the rim portions 21. The lens 30 is a light-transmitting member having an overall shape of a plate curved outward, and includes a resin layer 35 (molded layer) and a curved optical sheet 10.
[0036] The resin layer 35 has optical transparency and is located on the rear side of the lens. When the lens 30 is provided with a light collecting function, the resin layer 35 has the light collecting function.
[0037] The material for the resin layer 35 is not particularly limited as long as it is a resin material having optical transparency, and examples thereof include various curable resins such as various thermoplastic resins, thermosetting resins, and photocurable resins, and one or a combination of two or more of these can be used.
[0038] Examples of the resin material include polyolefins such as polyethylene, polypropylene, and ethylene-propylene copolymers, polyvinyl chloride, polystyrene, polyamide, polyimide, polycarbonate, poly-(4-methylpentene-1), ionomers, acrylic resins, polymethyl methacrylate, acrylonitrile-butadiene-styrene copolymers (ABS resins), acrylonitrile-styrene copolymers (AS resins), butadiene-styrene copolymers, polyesters such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT), polyethers, polyether ketones (PEK), and polyether ether ketones (PEK). Examples of the resin include polyether ether ketone (PEEK), polyetherimide, polyacetal (POM), polyphenylene oxide, polysulfone, polyethersulfone, polyphenylene sulfide, polyarylate, aromatic polyester (liquid crystal polymer), polytetrafluoroethylene, polyvinylidene fluoride, other fluorine-based resins, epoxy resins, phenolic resins, urea resins, melamine resins, silicone resins, polyurethanes, etc., or copolymers, blends, polymer alloys, etc., mainly made of these resins. Among them, it is preferable that the resin material is the same as or the same as the resin material constituting the first substrate 11 of the curved optical sheet 10 described later as the main material. This can improve the adhesion between the resin layer 35 and the curved optical sheet 10. In addition, since the refractive index difference between the resin layer 35 and the curved optical sheet 10 (first substrate 11) can be set low, diffuse reflection of light between the resin layer 35 and the curved optical sheet 10 can be appropriately suppressed or prevented, and light can be transmitted between the resin layer 35 and the curved optical sheet 10 with excellent light transmittance. The refractive index difference between the resin layer 35 and the curved optical sheet 10 (first substrate 11) is preferably 0.1 or less, and more preferably 0.05 or less, so that the effect obtained by setting the refractive index difference low can be more significantly exhibited.
[0039] The thickness of the resin layer 35 is not particularly limited, and is preferably, for example, 0.5 mm to 5.0 mm, and more preferably 1.0 mm to 3.0 mm, which allows the lens 30 to have both a relatively high strength and a lightweight structure.
[0040] The curved optical sheet 10 is a curved resin substrate that is bonded to the outer surface of the resin layer 35, i.e., the curved convex surface, in a curved shape corresponding to the shape, and the lens 30 is provided with this curved optical sheet 10, thereby imparting half-mirror properties to the sunglasses 100. As a result, the sunglasses 100 exhibit the function of sunglasses having half-mirror properties. The curved optical sheet 10 is configured by making the optical sheet of the present invention into a curved shape, but a detailed explanation of this will be given later.
[0041] As described above, the lens 30 of the sunglasses 100 may be either a lens having a light-collecting function or a lens having no light-collecting function.
[0042] Furthermore, as described above, the sunglasses 100 may be sunglasses having a frame 20, or may have a frameless configuration from the standpoint of fashionability, lightweightness, and the like.
[0043] Furthermore, in this embodiment, glasses equipped with lenses 30 are applied to sunglasses 100, but this is not limited to this, and the glasses may be, for example, prescription glasses, fashion glasses, goggles that protect the eyes from wind, rain, dust, chemicals, etc.
[0044] In the sunglasses 100 (eyeglasses) configured as described above, the lenses 30 included in the sunglasses 100 are manufactured, for example, through a manufacturing method for the lenses 30 as described below.
[0045] <Lens manufacturing method> Fig. 2 is a schematic diagram for explaining a method for manufacturing a lens having a curved optical sheet obtained by curvedly forming the optical sheet of the present invention. For convenience of explanation, the upper side of Fig. 2 will be referred to as "upper" and the lower side as "lower" in the following description.
[0046] Hereinafter, each step of the method for producing the lens 30 including the curved optical sheet 10 in which the optical sheet 15 of the present invention is curved will be described in detail. [1] First, prepare an optical sheet 15 (the optical sheet of the present invention) having a flat overall shape, which includes a first substrate 11, a half mirror layer 13, and a second substrate 12, which are laminated in this order. Then, apply protective films 50 (masking tape) to both sides of the optical sheet 15 to obtain a multilayer laminate 150 in which the protective films 50 are applied to both sides of the optical sheet 15 (see FIG. 2(a)).
[0047] [2] Next, as shown in FIG. 2(b), the prepared multilayer laminate 150, i.e., the optical sheet 15 with the protective films 50 attached to both sides thereof, is punched out in its thickness direction to form the multilayer laminate 150 having a circular shape in a plan view.
[0048] 2(c), the circular multilayer laminate 150 is subjected to a thermal bending process under heating to form the multilayer laminate 150 into a curved multilayer laminate 200 having a curved shape with the first substrate 11 side (one side) being a curved concave surface and the second substrate 12 side (the other side) being a curved convex surface. This makes it possible to form the flat optical sheet 15 into the curved optical sheet 10 with the protective films 50 attached to both sides.
[0049] This heat bending is usually carried out by press forming or vacuum forming. As described above, in this embodiment, the heating temperature (molding temperature) of the multilayer laminate 150 (optical sheet 15) at this time is set to preferably about 120° C. or more and 250° C. or less, more preferably about 130° C. or more and 180° C. or less, taking into consideration the melting or softening temperatures of the substrates 11 and 12, since the optical sheet 15 comprises substrates 11 and 12. By setting the heating temperature within this range, it is possible to prevent the optical sheet 15 from being altered or deteriorated, bring the optical sheet 15 into a softened or molten state, and reliably thermally bend the optical sheet 15 into the curved optical sheet 10 having a curved shape.
[0050] [4] Next, the protective film 50 is peeled off from the thermally bent curved optical sheet 10. Thereafter, as shown in FIG. 2(d), a mold 40 having a curved concave surface with a curved shape is placed in contact with the curved convex surface of the curved optical sheet 10, and in this state, a resin layer 35 mainly made of a resin material is injection molded on the curved concave surface of the curved optical sheet 10 by, for example, an insert injection molding method. That is, the constituent material of the resin layer 35 in a molten state is cooled and solidified in a state of contact with the curved concave surface of the curved optical sheet 10, and the resin layer 35 is molded in a state of direct contact with the curved concave surface of the curved optical sheet 10 without an adhesive layer or the like. In this way, a lens 30 (optical component of the present invention) including the thermally bent curved optical sheet 10 and the resin layer 35 is manufactured.
[0051] When the resin layer 35 is injection molded, the heating temperature (molding temperature) of the constituent material of the resin layer 35 to bring it into a molten state is appropriately set according to the type of the constituent material of the resin layer 35, but when the constituent material of the resin layer 35 is the same or identical to the constituent material of the first base material 11 of the curved optical sheet 10 described later, the heating temperature is preferably set to about 180° C. or more and 320° C. or less, more preferably 230° C. or more and 300° C. or less. By setting the heating temperature within this range, the constituent material of the resin layer 35 in a molten state can be reliably supplied to the curved concave surface of the curved optical sheet 10.
[0052] Among the insert injection molding methods, the injection compression molding method is preferably used. In the injection compression molding method, the resin material for forming the resin layer 35 is injected into the mold 40 at low pressure, and then the mold 40 is closed at high pressure to apply a compressive force to the resin material. Therefore, the resin layer 35 as a molded body and the lens 30 are less likely to suffer from molding distortion or optical anisotropy due to the local orientation of the resin molecules during molding, and therefore the injection compression molding method is preferably used. In addition, by controlling the mold compression force applied uniformly to the resin material, the resin material can be cooled at a constant specific volume, and therefore the resin layer 35 with high dimensional accuracy can be obtained.
[0053] The curved optical sheet 15 of the present invention is used for the curved optical sheet 10 provided in the lens 30 manufactured by the lens manufacturing method as described above. Each embodiment of the optical sheet 15 will be described in detail below.
[0054] <<First embodiment>> FIG. 3 is a longitudinal cross-sectional view showing a first embodiment of the optical sheet of the present invention, and FIG. 4 is an enlarged cross-sectional view showing a portion of the half mirror layer of the optical sheet, located in the area [B] surrounded by a dashed line in FIG.
[0055] For convenience of explanation, the upper side in Fig. 3 will be referred to as "upper" and the lower side as "lower". Additionally, the x direction in Fig. 3 and Fig. 4 will be referred to as the "left-right direction" or "flow direction (MD)", the y direction will be referred to as the "front-back direction" or "vertical direction (TD)", and the z direction will be referred to as the "up-down direction". Additionally, the thickness direction of the optical sheet is exaggerated in Fig. 3 and Fig. 4, so the actual dimensions are significantly different.
[0056] In this embodiment, as shown in FIG. 3, the optical sheet 15 (optical substrate) comprises a first substrate 11 having optical transparency, a second substrate 12 having optical transparency provided on one side of the first substrate 11, and a half mirror layer 13 provided between the first substrate 11 and the second substrate 12.
[0057] By setting the positional relationship of the layers in the optical sheet 15 as described above, the half mirror layer 13 is located between the first substrate 11 and the second substrate 12 and is not exposed on the surface of the optical sheet 15. In other words, it does not constitute the outermost layer exposed on the upper or lower surface of the optical sheet 15. Therefore, it is possible to reliably prevent the half mirror layer 13 from being hit by dust, rain, etc., or being worn by other members, etc., as in the case where the outermost layer is constituted. Therefore, it is possible to reliably prevent the half mirror layer 13 from being damaged by this hit or friction. Therefore, the optical sheet 15 maintains its design and optical properties for a long period of time.
[0058] Furthermore, in the optical sheet 15 having such a configuration, the half mirror layer 13 is composed of a laminate in which high refractive index layers 31 and low refractive index layers 32 are alternately and repeatedly laminated. As a result, the half mirror layer 13 selectively reflects light in a specific wavelength region among the incident light and transmits the remaining portion, so that when a person is located on the back side of the optical sheet 15, that is, when the person wears the sunglasses 100, the person (wearer) can see the front side of the optical sheet 15 through the optical sheet 15. In addition, the light in the specific wavelength region reflected on the front side of the optical sheet 15 is visible to a person located on the opposite side of the wearer through the optical sheet 15, so that an optical sheet 15 with a design can be obtained.
[0059] Each layer constituting this optical sheet 15 will now be described. The first substrate 11 supports the half mirror layer 13 (laminate) and positions the half mirror layer 13 between the first substrate 11 and the second substrate 12 described later. The first substrate 11 constitutes the outermost layer of the optical sheet 15 and functions as a protective layer to protect the half mirror layer 13.
[0060] In the optical sheet 15, the first substrate 11 and the second substrate 12 described later constitute the outermost layer of the optical sheet 15, so that the half mirror layer 13 is not exposed on the surface of the optical sheet 15. Therefore, in the lens 30 including this optical sheet 15, the half mirror layer 13 constitutes the outermost layer, and it is possible to reliably prevent the half mirror layer 13 from being struck by sand, dust, or even rain, or from being worn by other members, as would occur if the half mirror layer 13 were exposed. Therefore, it is possible to reliably prevent the half mirror layer 13 from being damaged by this strike or friction. Therefore, the design and optical properties of the optical sheet 15 can be maintained for a long period of time.
[0061] This first base material 11 is not particularly limited as long as it is made mainly of a transparent resin material, but it is preferable that it contains a transparent resin (base resin) having thermoplasticity as the main material.
[0062] The transparent resin is not particularly limited, but examples thereof include transparent resins such as acrylic resins, polystyrene resins, polyethylene resins, polypropylene resins, polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polycarbonate resins, polyamide resins, cycloolefin resins, vinyl chloride resins, and polyacetal resins, and one or more of these resins may be used in combination. Among these, polycarbonate resins or polyamide resins are preferred, and polycarbonate resins are particularly preferred. Polycarbonate resins are rich in transparency (translucency) and mechanical strength such as rigidity, and further have high heat resistance, so that the use of polycarbonate resins as the transparent resin can improve the transparency of the first substrate 11 and the impact resistance and heat resistance of the first substrate 11.
[0063] As the polycarbonate resin, various resins can be used, among which aromatic polycarbonate resins are preferable. Aromatic polycarbonate resins have aromatic rings in their main chains, which allows the first base material 11 to have superior strength.
[0064] The aromatic polycarbonate resin is synthesized, for example, by an interfacial polycondensation reaction between bisphenol and phosgene, or an ester exchange reaction between bisphenol and diphenyl carbonate.
[0065] Examples of bisphenols include bisphenol A and bisphenol (modified bisphenol) which is the source of the repeating unit of polycarbonate represented by the following formula (1A).
[0066] [ka] (In formula (1A), X is an alkyl group having 1 to 18 carbon atoms, an aromatic group, or a cyclic aliphatic group; Ra and Rb are each independently an alkyl group having 1 to 12 carbon atoms; m and n are each an integer of 0 to 4; and p is the number of repeating units.)
[0067] Specific examples of bisphenols that are the source of the repeating units of the polycarbonate represented by the formula (1A) include 4,4'-(pentane-2,2-diyl)diphenol, 4,4'-(pentane-3,3-diyl)diphenol, 4,4'-(butane-2,2-diyl)diphenol, 1,1'-(cyclohexanediyl)diphenol, 2-cyclohexyl-1,4-bis(4-hydroxyphenyl)benzene, 2,3-biscyclohexyl-1,4-bis(4-hydroxyphenyl)benzene, 1,1'-bis(4-hydroxy-3-methylphenyl)cyclohexane, and 2,2'-bis(4-hydroxy-3-methylphenyl)propane, and any of these may be used alone or in combination of two or more.
[0068] In particular, the polycarbonate resin is preferably a bisphenol-type polycarbonate resin having a skeleton derived from bisphenol, which provides the first base material 11 with even greater strength.
[0069] Furthermore, as long as the first base material 11 has light transmitting properties, its color may be any color, such as colorless, red, blue, or yellow.
[0070] These colors can be selected by incorporating a dye or pigment into the first substrate 11. Examples of the dye include acid dyes, direct dyes, reactive dyes, and basic dyes, and one or more of these dyes may be used in combination.
[0071] Specific examples of dyes include CI Acid Yellow 17, 23, 42, 44, 79, 142, CI Acid Red 52, 80, 82, 249, 254, 289, CI Acid Blue 9, 45, 249, CI Acid Black 1, 2, 24, 94, CI Food Black 1, 2, CI Direct Yellow 1, 12, 24, 33, 50, 55, 58, 86, 132, 142, 144, 173, CI Direct Red 1, 4, 9, 80, 81, 225, 227, CI Direct Blue 1, 2, 15, 71, 86, 87, 98, 165, 199, 202, CI Direct Black 19, 38, 51, 71, 154, 168, 171, 195, and CI Reactive Red. 14, 32, 55, 79, 249, CI Reactive Black 3, 4, 35, etc.
[0072] If necessary, the first base material 11 may contain various additives such as an antioxidant, a filler, a plasticizer, a light stabilizer, an ultraviolet absorber, a heat absorber, and a flame retardant, in addition to the transparent resin, dye, or pigment described above.
[0073] The refractive index of the first base material 11 at a wavelength of 589 nm is preferably 1.3 to 1.8, more preferably 1.4 to 1.65. By setting the refractive index of the first base material 11 within the above numerical range, it is possible to appropriately suppress or prevent the impairment of the function of the half mirror layer 13, which transmits a part of the incident light and reflects the remainder.
[0074] The first base material 11 has an average thickness set to preferably 0.1 mm or more and 1.5 mm or less, more preferably 0.2 mm or more and 0.8 mm or less. By setting the average thickness of the first base material 11 within this range, it is possible to appropriately suppress or prevent the occurrence of bending in the optical sheet 15 while making the optical sheet 15 thinner. Therefore, the color of the light in a specific wavelength range selectively reflected by the half mirror layer 13 can be more uniformly visually recognized over the entire optical sheet 15.
[0075] The second substrate 12 supports the half mirror layer 13 (optical multilayer film) and positions the half mirror layer 13 between the first substrate 11 and the second substrate 12. The second substrate 12 constitutes the outermost layer of the optical sheet 15 and functions as a protective layer to protect the half mirror layer 13.
[0076] In the optical sheet 15, the second substrate 12 constitutes the outermost layer of the optical sheet 15, so that the half mirror layer 13 is not exposed on the surface of the optical sheet 15. Therefore, in the lens 30 including this optical sheet 15, the half mirror layer 13 constitutes the outermost layer, and it is possible to reliably prevent the half mirror layer 13 from being struck by sand, dust, or even rain, or from being worn by other members, as would occur if the half mirror layer 13 were exposed. Therefore, it is possible to reliably prevent the half mirror layer 13 from being damaged by this strike or friction. Therefore, the design and optical properties of the optical sheet 15 can be maintained for a long period of time.
[0077] The second base material 12 may be made of the same material as that mentioned for the first base material 11. The second base material 12 and the first base material 11 may be made of the same material (same type) or different materials.
[0078] Furthermore, the refractive index of the second substrate 12 at a wavelength of 589 nm may be the same as or different from the refractive index of the first substrate 11, but is preferably 1.3 to 1.8, more preferably 1.4 to 1.65. By setting the refractive index of the second substrate 12 within the above numerical range, it is possible to precisely suppress or prevent the half mirror layer 13 from impairing its function of transmitting a part of the incident light and reflecting the remainder.
[0079] The second substrate 12 may have an average thickness that is the same as or different from that of the first substrate 11, and is preferably 0.2 mm to 1.5 mm, and more preferably 0.2 mm to 0.8 mm. By setting the average thickness of the second substrate 12 within this range, it is possible to reduce the thickness of the optical sheet 15 while appropriately suppressing or preventing the optical sheet 15 from bending. Therefore, the color of the light in a specific wavelength region selectively reflected by the half mirror layer 13 can be more uniformly viewed throughout the entire optical sheet 15.
[0080] Moreover, the first substrate 11 and the second substrate 12 as described above preferably have a glass transition point of 105° C. or higher, similar to the high refractive index layer 31 and the low refractive index layer 32 of the half mirror layer 13 described later. This can further improve the heat resistance and thermal bendability of the first substrate 11 and the second substrate 12, and therefore the optical sheet 15.
[0081] The half mirror layer 13 is an intermediate layer located at the center of the thickness direction of the optical sheet 15, and in the present invention, it selectively reflects light having a specific wavelength range (specific wavelength region) and transmits the remaining light that is not reflected due to this reflection.
[0082] 4, the half mirror layer 13 has a repeating portion 33 composed of a laminate in which high refractive index layers 31 having a high refractive index and low refractive index layers 32 having a low refractive index are alternately and repeatedly stacked with respect to light in the visible light region. That is, the half mirror layer 13 has a configuration in which one high refractive index layer 31 is sandwiched between two low refractive index layers 32 by being composed of a multi-layer laminate in which the repeating portion 33 is repeatedly stacked a plurality of times.
[0083] In this half mirror layer 13, the high refractive index layer 31 contains a resin material having a high refractive index for light in the visible light region, and the low refractive index layer 32 contains a resin material having a low refractive index for light in the visible light region, so that the refractive index difference between the high refractive index layer 31 and the low refractive index layer 32 for light in the visible light region can be increased and the refractive index difference for non-reflected light can be decreased. This allows the half mirror layer 13 to function as a multilayer laminate, i.e., a multilayer laminate reflector, which selectively reflects light in a specific wavelength region in the visible light region and transmits the remaining non-reflected light as transmitted light. In other words, when light in the visible light region is incident on the half mirror layer 13 as incident light, the half mirror layer 13 functions as a multilayer laminate reflector that blocks (reflects) the reflected light (reflected light) of the incident light to the maximum extent, i.e., transmits the minimum amount, and when non-reflected light (transmitted light) is incident on the half mirror layer 13 as incident light, the half mirror layer 13 functions as a multilayer laminate reflector that blocks the transmitted light to the minimum extent, i.e., transmits the maximum amount.
[0084] Here, in order to selectively reflect light in a specific wavelength region in the visible light region and transmit the remaining unreflected light as transmitted light, specifically, in the half mirror layer 13, when the refractive index of the high refractive index layer 31 at a wavelength of 589 nm is N1 and the refractive index of the low refractive index layer 32 at a wavelength of 589 nm is N2, the refractive index difference (N1-N2) is preferably set to 0.05 or more and 0.25 or less, more preferably 0.08 or more and 0.25 or less. By setting the refractive index difference (N1-N2) at a wavelength of 589 nm within the above range, it can be said that the refractive index difference for light in the visible light region is set large between the high refractive index layer 31 and the low refractive index layer 32, and light in the visible light region can be reliably blocked (reflected) to the maximum extent.
[0085] The specific wavelength region of visible light that blocks (reflects) light in the visible light region to the maximum extent and blocks non-reflected light to the minimum extent, and the intensity of light in that wavelength region, can be adjusted to a desired magnitude (within a range) by appropriately setting the types of resin materials contained in the high refractive index layer 31 and the low refractive index layer 32, respectively, the number of repetitions of the high refractive index layer 31 and the low refractive index layer 32 in the half mirror layer 13 (repeating portion 33), and the thickness of the half mirror layer 13 (high refractive index layer 31, low refractive index layer 32), etc.
[0086] Therefore, by providing the lens 30 with the curved optical sheet 10 in which the optical sheet 15 is formed to have a curved shape, when the external light irradiated from outside the sunglasses 100, i.e., the direct light of sunlight and its reflected light, passes through the optical sheet 15, the light of a specific wavelength region in the visible light region is reflected by the optical sheet 15, and the remaining light, i.e., the light that is attenuated as the light that is not reflected, reaches the eyes of the wearer of the sunglasses 100. This suppresses the intrusion of the light of a specific wavelength region out of the visible light contained in the direct light of sunlight and the reflected light into the eyes, thereby improving the recognition of the object visually recognized by the wearer. On the other hand, the light of a specific wavelength region reflected by the optical sheet 15 (reflected light) is visible to a person positioned on the opposite side of the wearer through the lens 30 (optical sheet 15), so that the design of the sunglasses 100 can be improved. In this way, the optical sheet 15 functions as a reflector that selectively reflects light having a specific wavelength region out of the visible light and selectively transmits the remaining light.
[0087] In the above-mentioned lens manufacturing method, the optical sheet 15 undergoes a thermal history since it is subjected to the thermal bending process in the step [3] and the injection molding process in the step [4]. As described above, the heating temperature during these processes is set to preferably about 120°C to 250°C in the step [3] and preferably 180°C to 320°C in the step [4], so the half mirror layer 13 of the optical sheet 15 is required to have excellent heat resistance.
[0088] As described above, the half mirror layer 13 exhibits the property of reflecting light in a specific wavelength region in the visible light region to the maximum extent, and transmitting the remaining unreflected light to the maximum extent. Therefore, when the half mirror layer 13 exhibits excellent heat resistance, it can be said that the properties of the half mirror layer 13 are favorably maintained even when exposed to harsh conditions.
[0089] Therefore, when the glass transition point of the resin material contained in the high refractive index layer 31, which has a high refractive index for light in the visible light region, is Tg1 and the glass transition point of the resin material contained in the low refractive index layer 32, which has a low refractive index for light in the visible light region, is Tg2, it is preferable that the relationship of Tg1, Tg2 ≧ 105°C is satisfied. In this way, by preferably selecting a material with both Tg1 and Tg2 of 105°C or more, both the high refractive index layer 31 and the low refractive index layer 32 have excellent heat resistance. Therefore, it is possible to appropriately suppress or prevent the film thickness of the refractive index layer having the lower glass transition point of the low refractive index layer 32 and the high refractive index layer 31 from changing. Therefore, the half mirror layer 13 of the optical sheet 15 exhibits excellent heat resistance because the deterioration of its function as a reflector that selectively reflects light (visible light) in a specific wavelength region is appropriately suppressed or prevented. In general, the resin material having a low refractive index in the low refractive index layer 32 tends to have a lower glass transition point than the resin material having a high refractive index contained as the main material of the high refractive index layer 31. Therefore, by using a material having a glass transition point Tg2 of 105° C. or higher as the resin material having a low refractive index, the above-mentioned effect can be reliably achieved.
[0090] When optical sheet 15 having this half mirror layer 13 is pressed against a metal mold at a temperature 10° C. higher than the higher of the glass transition point Tg1 of the main material constituting high refractive index layer 31 and the glass transition point Tg2 of the main material constituting low refractive index layer 32, optical sheet 15 is made into curved optical sheet 10 having a curved shape with a curvature radius of 60 mm. When the reflectance of curved optical sheet 10 at a wavelength of 589 nm is R1 [%], and this curved optical sheet 10 is stored for 1000 hours in a heat circulation oven at a temperature environment of 105° C., the reflectance retention calculated by R2 / R1×100 [%] is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more.
[0091] As described above, even if the curved optical sheet 10 curved with a radius of curvature of 60 mm is exposed to harsh conditions such as storage for 1000 hours in a temperature environment of 105°C, the reflectance retention is maintained at or above the lower limit. Since the reflectance retention is maintained at a rate equal to or above the lower limit, the half mirror layer 13 can be said to exhibit excellent heat resistance. In addition, the reflectance R1 of the curved optical sheet 10 at a wavelength of 589 nm is preferably 40% or more, and more preferably 45% or more and 70% or less. Such a curved optical sheet 10 can be said to reflect light in the visible light region with excellent reflectance.
[0092] As described above, in the repeating portion 33 (laminate), a specific wavelength region of visible light that blocks (reflects) light in the visible light region to the maximum extent and blocks non-reflected light to the minimum extent, and further, the intensity of light in that wavelength region can be adjusted to a desired magnitude (within a range) by appropriately setting the types of resin materials contained in the high refractive index layer 31 and the low refractive index layer 32, respectively, the number of repetitions of the high refractive index layer 31 and the low refractive index layer 32 in the half mirror layer 13 (repeating portion 33), and the thickness of the half mirror layer 13 (high refractive index layer 31, low refractive index layer 32), etc.
[0093] In such a half mirror layer 13 (repeated portion 33), specifically, the sodium D line (589 nm), which is generally used as the reference wavelength of visible light, is used as a representative value, and the magnitude of the refractive index difference (N1-N2) between the refractive index N1 of the high refractive index layer 31 and the refractive index N2 of the low refractive index layer 32 at a wavelength of 589 nm is specified to be preferably 0.05 or more and 0.25 or less, so that the half mirror layer 13 (repeated portion 33), i.e., the reflector, can reflect light in a specific wavelength range of visible light, specifically, visible light in the wavelength range of 400 nm or more and 780 nm or less, to the maximum extent.
[0094] Furthermore, by selecting, as the main material of the high refractive index layer 31 and the main material of the low refractive index layer 32, materials such that the glass transition point Tg1 of the resin material contained in the high refractive index layer 31 having a high refractive index for light in the visible light range and the glass transition point Tg2 of the resin material contained in the low refractive index layer 32 having a low refractive index for light in the visible light range preferably satisfy the relationship Tg1, Tg2 ≧ 105°C, the half mirror layer 13 (repeating portion 33), i.e., the reflector (multilayer laminated reflector), can exhibit excellent heat resistance.
[0095] As described above, the main material of the high refractive index layer 31, i.e., the resin material having a high refractive index for light in the visible light region, and the main material of the low refractive index layer 32, i.e., the resin material having a low refractive index for light in the visible light region, which have a refractive index difference (N1-N2) of preferably 0.05 to 0.25 and further preferably Tg1, Tg2≧105°C, are preferably at least one of polycarbonate resin, polystyrene resin, polyether resin, styrene resin, polyester resin, and acrylic resin having amorphous properties, and more preferably at least one of polycarbonate resin, polyether resin, and polyester resin. By appropriately selecting the main materials of the high refractive index layer 31 and the low refractive index layer 32 from these resin materials, the half mirror layer 13 including the high refractive index layer 31 and the low refractive index layer 32 can relatively easily satisfy both the refractive index difference (N1-N2) of 0.05 to 0.25 and Tg1, Tg2≧105°C.
[0096] Considering the above points, the main material of the high refractive index layer 31 is preferably at least one of polyester resins such as polycarbonate (PC), polyethylene terephthalate (PET), and polyethylene naphthalate (PEN), polyethersulfone (PES), and polyarylate (PAR).
[0097] In addition, as the main material of the low refractive index layer 32, at least one of polyester resins such as polycarbonate (PC), polyethylene terephthalate (PET), and polyethylene naphthalate (PEN), acrylic resins such as polymethyl methacrylate (PMMA), styrene resins such as polystyrene (PS) and acrylonitrile-styrene copolymer (AS), and polyarylate (PAR) is suitably selected.
[0098] When such resin materials are used, specific combinations of the main materials contained in the high refractive index layer 31 and the low refractive index layer 32 include a combination of polycarbonate (PC) and polymethylmethacrylate (PMMA), a combination of polyarylate (PAR) and polymethylmethacrylate (PMMA), a combination of polyethylene terephthalate (PET) and polymethylmethacrylate (PMMA), a combination of polyethersulfone (PES) and polyarylate (PAR), a combination of polyethylene naphthalate (PEN) and acrylonitrile-styrene copolymer (AS), a combination of polyethylene naphthalate (PEN) and polymethylmethacrylate (PMMA), etc. With such combinations, it is possible to more easily satisfy both the refractive index difference (N1-N2) of 0.05 to 0.25 and Tg1, Tg2≧105°C.
[0099] In addition to the main material, the high refractive index layer 31 and the low refractive index layer 32 may each contain an additive such as a filler. This makes it easier for the half mirror layer 13 including the high refractive index layer 31 and the low refractive index layer 32 to satisfy both the refractive index difference (N1-N2) of 0.05 to 0.25 and Tg1, Tg2≧105° C.
[0100] The filler is not particularly limited, but examples thereof include inorganic fillers such as silica, alumina, calcium carbonate, strontium carbonate, calcium phosphate, kaolin, talc, and smectite, and organic fillers such as cross-linked polystyrene and styrene-divinylbenzene copolymer. One or a combination of two or more of these can be used, and among these, at least one of strontium carbonate and smectite is preferable, and strontium carbonate is more preferable.
[0101] The filler may be in any shape, such as particulate (eg, spherical or flat), granular, pellet-like, or scaly form, but is preferably contained in particulate form.
[0102] In the high refractive index layer 31 and the low refractive index layer 32 obtained by the above combination of resin materials, the glass transition point Tg1 of the resin material having a high refractive index for light in the visible light region and the glass transition point Tg2 of the resin material having a low refractive index for light in the visible light region preferably satisfy the relationship Tg1, Tg2 ≧ 105°C, in other words, the lower of the temperatures Tg1 and Tg2 is preferably 105°C or higher, and further, the lower of the temperatures Tg1 and Tg2 preferably satisfies the relationship of 110°C or higher and 250°C or lower, and more preferably the lower of the temperatures Tg1 and Tg2 satisfies the relationship of 110°C or higher and 200°C or lower. In addition, it is preferable to satisfy the relationship of 0°C ≦ |Tg1-Tg2| ≦ 60°C, and more preferably the relationship of 25°C ≦ |Tg1-Tg2| ≦ 60°C. In this way, by selecting a combination in which both Tg1 and Tg2 are within the above range and the difference between the two is not more than the above upper limit, both the high refractive index layer 31 and the low refractive index layer 32 have excellent heat resistance, and therefore it is possible to obtain a half mirror layer 13 that reliably exhibits excellent heat resistance.
[0103] In addition, the refractive index difference (N1-N2), which is the relation between the refractive index N1 at a wavelength of 589 nm of the high refractive index layer 31 and the refractive index N2 at a wavelength of 589 nm of the low refractive index layer 32, is preferably 0.05 or more and 0.25 or less, but the refractive index N1 of the high refractive index layer 31 at a wavelength of 589 nm is preferably 1.57 or more and 1.85 or less, and the refractive index N2 of the low refractive index layer 32 at a wavelength of 589 nm is preferably 1.49 or more and 1.67 or less. This makes it possible to more reliably reflect light in a specific wavelength range in the visible light range.
[0104] Furthermore, the high refractive index layer 31 and the low refractive index layer 32 each preferably have an average thickness of 50 nm or more and 300 nm or less, and more preferably have an average thickness of 50 nm or more and 200 nm or less. In the average thicknesses within this range, the optical thicknesses (average layer thickness x layer refractive index) of the high refractive index layer 31 and the low refractive index layer 32 are set to a quarter of the wavelength of light in the visible light region to be selectively reflected. This allows the lights reflected at the interface to reinforce each other, so that the half mirror layer 13 can selectively reflect light in a specific wavelength region in the visible light region.
[0105] In addition, the repeating portion 33 in which the high refractive index layer 31 and the low refractive index layer 32 are laminated is preferably laminated 50 times or more and 750 times or less, and more preferably 100 times or more and 600 times or less.
[0106] By setting the average thickness of the high refractive index layers 31 and the low refractive index layers 32, and the number of repeating sections 33 in which the high refractive index layers 31 and the low refractive index layers 32 are stacked, within the above ranges, the specific wavelength (wavelength range) of light that is maximally blocked in the visible light range can be adjusted to the desired size (range).
[0107] Furthermore, the half mirror layer 13 may be stretched or unstretched, but is preferably unstretched. Specifically, the thickness direction retardation (Rth) at a wavelength of 589 nm, as represented by the following calculation formula (A), is preferably 500 nm or less, and more preferably 300 nm or less.
[0108] Rth = [(nx + ny) / 2 - nz] · d … (A) (In the above formula (A), nx and ny represent the principal refractive indices in the plane of the half mirror layer 13, nz represents the refractive index in the thickness direction of the half mirror layer 13, and d represents the thickness of the half mirror layer 13.)
[0109] Here, by selecting a stretched half mirror layer 13, the apparent glass transition point of the half mirror layer 13 can be improved, that is, the heat resistance of the half mirror layer 13 can be improved, but on the other hand, there is a problem that the thermal bending property (processability) is reduced. In response to this, in the present invention, as described above, a resin material contained in the high refractive index layer and the low refractive index layer that preferably satisfies Tg1, Tg2≧105° C. is selected, thereby imparting excellent heat resistance to the half mirror layer 13. And, by preferably selecting a non-stretched half mirror layer 13, the thermal bending property of the half mirror layer 13 and thus the optical sheet 15 can be further improved.
[0110] The optical sheet 15 as described above is composed of a laminate in which the first substrate 11, the half mirror layer 13, and the second substrate 12 are bonded to each other and laminated in this order, and by performing the thermal bending process in the step [3] in the above-mentioned lens manufacturing method, this optical sheet 15 is thermally bent into the curved optical sheet 10 having a curved shape with the first substrate 11 side (upper side) as a curved concave surface and the second substrate 12 side (lower side) as a curved convex surface. Therefore, the optical sheet 15 is required to have excellent processability.
[0111] The first base material 11 and the second base material 12 contain a resin material as their main material. As described above, in the present invention, the half mirror layer 13 contains a resin material having a glass transition point of Tg1 and a resin material having a glass transition point of Tg2 as the main material of the high refractive index layer 31 and the main material of the low refractive index layer 32 constituting the half mirror layer 13, respectively.
[0112] In this way, by using resin materials as the main materials of the first substrate 11 and the second substrate 12, and the high refractive index layer 31 and the low refractive index layer 32 constituting the half mirror layer 13, the optical sheet 15 constituted by these laminates can be given excellent processability. Therefore, when the optical sheet 15 is thermally bent into a curved shape, it is possible to appropriately suppress or prevent cracks from occurring in the high refractive index layer 31 and the low refractive index layer 32, as in the case where the high refractive index layer 31 and the low refractive index layer 32 are made of a metallic (inorganic) material.
[0113] In the present invention, in such an optical sheet 15, the interface between the first substrate 11 and the half mirror layer 13 forms a continuous layer between the first substrate 11 and the half mirror layer 13, and the interface between the second substrate 12 and the half mirror layer 13 forms a continuous layer between the second substrate 12 and the half mirror layer 13. In this way, in the optical sheet 15, at the interface where the layers constituting the optical sheet 15 itself are bonded to each other, a continuous layer is formed in which the constituent materials contained in each of the layers to be bonded are mixed together. Therefore, the adhesion between the first substrate 11 and the half mirror layer 13 and the adhesion between the second substrate 12 and the half mirror layer 13 are improved. Therefore, even if the optical sheet 15 is subjected to a thermal bending process in order to obtain the curved optical sheet 10 having a curved shape with the first substrate 11 side (upper side) being a curved concave surface and the second substrate 12 side (lower side) being a curved convex surface in the step [3], it is possible to appropriately suppress or prevent peeling between the first substrate 11 and the half mirror layer 13 and between the second substrate 12 and the half mirror layer 13. Therefore, it is possible to impart superior processability to the optical sheet 15.
[0114] The continuous layer refers to a state where the constituent materials contained in the first substrate 11 and the half mirror layer 13 are mixed together at the interface between the first substrate 11 and the half mirror layer 13, and more specifically, refers to a state where the constituent material of the first substrate 11 is dispersed on the half mirror layer 13 side at the interface between the first substrate 11 and the half mirror layer 13, and the constituent material of the half mirror layer 13 is dispersed on the first substrate 11 side. The continuous layer refers to a state where the constituent materials contained in the second substrate 12 and the half mirror layer 13 are mixed together at the interface between the second substrate 12 and the half mirror layer 13, and more specifically, refers to a state where the constituent material of the second substrate 12 is dispersed on the half mirror layer 13 side at the interface between the second substrate 12 and the half mirror layer 13, and the constituent material of the half mirror layer 13 is dispersed on the second substrate 12 side.
[0115] This optical sheet 15 is pressed against a metal mold at a temperature 10° C. higher than the higher of the glass transition point Tg1 of the main material constituting the high refractive index layer 31 and the glass transition point Tg2 of the main material constituting the low refractive index layer 32, to form the optical sheet 15 into a curved shape with a radius of curvature of 60 mm. After storing this curved optical sheet 10 for 1000 hours in a heat circulation oven at a temperature environment of 105° C., it is preferable that the number of curved optical sheets 10 that maintain a shape with a radius of curvature of 60±5 mm out of 50 curved optical sheets 10 is 48 or more, and more preferably 50.
[0116] As described above, even if the curved optical sheet 10 curved with a curvature radius of 60 mm is exposed to harsh conditions such as storage for 1000 hours in a temperature environment of 105° C., the shape retention of the curved optical sheet 10 is maintained at or above the lower limit. Since the shape retention is maintained at a rate equal to or above the lower limit, it can be said that the curved optical sheet 10 exhibits excellent processability.
[0117] Furthermore, as described above, after the curved optical sheets 10 are stored for 1,000 hours in a heat circulation oven at a temperature of 105°C, the number of curved optical sheets 10 in which peeling has occurred between the first substrate 11 and the half mirror layer 13, or between the second substrate 12 and the half mirror layer 13, among the 50 curved optical sheets is preferably 2 or less, and more preferably 0.
[0118] As described above, even if the curved optical sheet 10 curved with a curvature radius of 60 mm is exposed to harsh conditions such as storage for 1000 hours in a temperature environment of 105° C., the occurrence of peeling in the curved optical sheet 10 remains below the upper limit. Since the occurrence of peeling is suppressed to a rate below the upper limit, it can be said that the curved optical sheet 10 suppresses the occurrence of peeling between the substrates 11 and 12 and the half mirror layer 13 and exhibits excellent processability.
[0119] Furthermore, the total thickness of the optical sheet 15 is not particularly limited, but is preferably about 0.2 mm to 3.0 mm, and more preferably about 0.4 mm to 1.6 mm, which imparts excellent strength to the optical sheet 15 and also imparts excellent thermoformability to the optical sheet 15 when the optical sheet 15 is molded into the curved optical sheet 10 having a curved shape.
[0120] The optical sheet 15 of this embodiment having such a configuration is obtained by integrally forming a laminate in which a first substrate 11, a half mirror layer 13 having a plurality of repeating sections 33 in which high refractive index layers 31 and low refractive index layers 32 are alternately stacked, and a second substrate 12 are bonded to each other in the stated order, and more specifically, it can be manufactured, for example, as follows.
[0121] That is, first, materials containing a resin material having a high refractive index for light in the visible light region and a resin material having a low refractive index for light in the visible light region as the main material are prepared as resin compositions for forming the high refractive index layer 31 and the low refractive index layer 32. Then, by alternately laminating these, a multiple laminate is obtained in which a repeating portion 33 (laminate) in which the high refractive index layer 31 and the low refractive index layer 32 are alternately laminated is laminated multiple times, and then a resin composition containing a resin material for forming the first base material 11 and the second base material 12 as the main material is laminated on the upper surface and the lower surface of the obtained multiple laminate. As a result, an integrated product is obtained in which the first base material 11, the multiple laminate, and the second base material 12 are laminated in this order (lamination process). In other words, an integrated product is obtained in which the upper surface and the lower surface of the multiple laminate are covered with the first base material 11 and the second base material 12 as a covering layer (skin layer), respectively.
[0122] The method for obtaining an integrated product in which the first substrate 11, the multiple laminates, and the second substrate 12 are laminated in this order is not particularly limited, but examples thereof include a feed block method in which resin compositions containing the resin materials that are the raw materials for each layer are melt-extruded by several extruders, a co-extrusion T-die method such as a multi-manifold method, and an air-cooled or water-cooled co-extrusion inflation method, and among these, the co-extrusion T-die method is particularly preferred. The co-extrusion T-die method is preferably used because it is excellent in controlling the thickness of each layer that is formed so as to overlap each other in the thickness direction.
[0123] Next, the obtained integrated body is cooled to be dried and solidified (cooling step), whereby the first base material 11, the half mirror layer 13, and the second base material 12 are bonded to one another in this order to obtain an integrated laminate, namely, the optical sheet 15.
[0124] <Second embodiment> Further, the optical sheet 15 may have the following configuration in addition to the configuration described in the first embodiment. FIG. 5 is a vertical cross-sectional view showing a second embodiment of the optical sheet of the present invention.
[0125] For convenience of explanation, the upper side of Fig. 5 will be referred to as "upper" and the lower side as "lower". The x direction in Fig. 5 will be referred to as "left-right direction", the y direction as "front-rear direction", and the z direction as "up-down direction". Furthermore, the thickness direction of the optical sheet is exaggerated in Fig. 5, so the dimensions are significantly different from the actual dimensions.
[0126] Hereinafter, the second embodiment of the optical sheet of the present invention will be described with reference to this figure, but the differences from the above-described embodiment will be mainly described, and a description of the similar points will be omitted.
[0127] The optical sheet 15 of this embodiment is similar to the optical sheet 15 of the first embodiment, except that it further includes, as the outermost layer, a coating layer 17 (hard coat layer) that coats the first substrate 11 and the second substrate 12, respectively.
[0128] 5, in this embodiment, the optical sheet 15 further has a covering layer 17 on one surface side (upper surface side) of the first substrate 11 as an outermost layer, which covers the first substrate 11. Also, the optical sheet 15 further has a covering layer 17 on the other surface side (lower surface side) of the second substrate 12 as an outermost layer, which covers the second substrate 12. In other words, the optical sheet 15 of this embodiment is configured as a laminate in which the covering layer 17, the second substrate 12, the half mirror layer 13, the first substrate 11, and the covering layer 17 are laminated in this order from the lower surface side to the upper surface side of the optical sheet 15.
[0129] By providing the coating layers 17 that respectively cover the first substrate 11 and the second substrate 12 as in this embodiment, it is possible to reliably prevent the first substrate 11 and the second substrate 12 from being damaged.
[0130] This coating layer 17 (coat layer) is a so-called hard coat layer formed using a resin composition, and as this resin composition, for example, a resin composition containing a silicon-modified (meth)acrylic resin is preferably used. Hereinafter, the resin composition containing the silicon-modified (meth)acrylic resin will be described.
[0131] (Silicone modified (meth)acrylic resin) Silicone-modified (meth)acrylic resin (siloxane-modified (meth)acrylate) is a polymer (prepolymer) having a main chain in which structural units derived from a (meth)acrylic monomer having a (meth)acryloyl group are repeated, and a repeating body (side chain) in which structural units having a siloxane bond are repeated and linked to this main chain.
[0132] That is, it is a polymer (prepolymer) in which a (meth)acrylic compound as the main chain and a compound having a siloxane bond (-Si-O-Si-) as the side chain are linked together.
[0133] The silicon-modified (meth)acrylic resin, having the above-mentioned main chain, imparts excellent transparency to the coating layer 17, and further, having a repeating unit in which structural units having the above-mentioned siloxane bonds are repeated, imparts excellent scratch resistance and weather resistance to the coating layer 17, i.e., the resin can reliably impart the functionality of the coating layer 17.
[0134] Specific examples of the main chain of the silicon-modified (meth)acrylic resin include structures composed of repeating structural units derived from monomers having at least one of the (meth)acryloyl groups of the following formula (1) and formula (2). An example of a structure having repeating structural units derived from both of these monomers is a structure having the chemical formula shown in the following formula (12).
[0135] [ka] (In formula (1), n is an integer of 1 or more, R1 independently represents a hydrocarbon group, an organic group, or a hydrogen atom, and R0 independently represents a hydrocarbon group or a hydrogen atom.)
[0136] [ka] (In formula (2), m represents an integer of 1 or more, R2 independently represents a hydrocarbon group, an organic group, or a hydrogen atom, and R0 independently represents a hydrocarbon group or a hydrogen atom.)
[0137] [ka] (In formula (12), m and n are integers of 1 or more, R1, R2, and R3 each independently represent a hydrocarbon group, an organic group, or a hydrogen atom, and R0 independently represents a hydrocarbon group or a hydrogen atom.)
[0138] Furthermore, at least one end of the main chain or side chain of such a structure is bonded to a repeating unit (sub-chain) in which a structural unit having a siloxane bond is repeated.
[0139] Since siloxane bonds have a high bonding strength, a silicon-modified (meth)acrylic resin having a repeating body in which structural units having siloxane bonds are repeated can provide a coating layer 17 with better heat resistance and weather resistance. In addition, the high bonding strength of the siloxane bonds can provide a hard coating layer 17, further increasing the scratch resistance of the optical sheet 15.
[0140] Specific examples of repeating units having siloxane bonds include structures having repeating units having siloxane bonds of at least one of the following formulas (3) and (4).
[0141] [ka] (In formula (3), X1 represents a hydrocarbon group or a hydroxyl group.)
[0142] [ka] (In formula (4), X2 represents a hydrocarbon group or a hydroxyl group, and X3 represents a divalent group in which a hydrogen atom has been removed from a hydrocarbon group or a hydroxyl group.)
[0143] Specific examples of the repeating body in which the structural unit having a siloxane bond is repeated include a structure having a polyorganosiloxane and a structure having a silsesquioxane. The silsesquioxane structure may be any structure such as a random structure, a cage structure, or a ladder structure.
[0144] Examples of the hydrocarbon group include alkyl groups such as a methyl group, an ethyl group, a propyl group, and an isopropyl group; cycloalkyl groups such as a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group; aryl groups such as a phenyl group, a naphthyl group, and a 2-methylphenyl group; aralkyl groups such as a benzyl group, a diphenylmethyl group, and a naphthylmethyl group; and a biphenyl group.
[0145] In addition, it is preferable that an unsaturated double bond is introduced into the end or side chain of the repeating body in which the structural unit having a siloxane bond is repeated. As a result, when the resin composition contains a urethane (meth)acrylate described later, the double bond can be bonded to the (meth)acryloyl group of the urethane (meth)acrylate to form a network of the silicon-modified (meth)acrylic resin and the urethane (meth)acrylate. Therefore, the silicon-modified (meth)acrylic resin and the urethane (meth)acrylate are more uniformly dispersed in the coating layer 17, and as a result, the coating layer 17 can exhibit the above-mentioned characteristics more uniformly throughout its entirety.
[0146] The content of the silicon-modified (meth)acrylic resin in the resin composition is not particularly limited, but is preferably 5 parts by mass or more and 45 parts by mass or less, and more preferably 11 parts by mass or more and 28 parts by mass or less, in 100 parts by mass of the resin composition. If the content of the silicon-modified (meth)acrylic resin in the resin composition is less than the lower limit, the hardness of the coating layer 17 obtained by the resin composition may decrease. In addition, if the content of the silicon-modified (meth)acrylic resin in the resin composition exceeds the upper limit, the content of materials other than the silicon-modified (meth)acrylic resin in the resin composition may relatively decrease, and the flexibility of the coating layer 17 formed by using the resin composition may decrease.
[0147] Examples of the silicon-modified (meth)acrylic resin having the above-mentioned structure include compounds represented by the following formulas (5) and (6).
[0148] [ka] (In formula (5), Me represents a methyl group, and m, n, and p each represent an integer of 1 or more.)
[0149] [ka] (In formula (6), Me represents a methyl group, m, n, and p each represent an integer of 1 or more, and R1, R2, R3, and R4 each independently represent a hydrocarbon group, an organic group, or a hydrogen atom.)
[0150] (Urethane (meth)acrylate) Moreover, it is preferable that the resin composition further contains urethane (meth)acrylate.
[0151] When an unsaturated double bond is introduced at the end or side chain of a repeating unit having a siloxane bond, which is included in the silicon-modified (meth)acrylic resin, the (meth)acryloyl group and the unsaturated double bond of the urethane (meth)acrylate are bonded to form a network of the silicon-modified (meth)acrylic resin and the urethane (meth)acrylate by containing the urethane (meth)acrylate in the resin composition. As a result, the resin composition is cured to obtain a cured product, and the coating layer 17 composed of the cured product is formed. The curing of the resin composition by the binding of the (meth)acryloyl group and the unsaturated double bond is performed by photocuring, which cures the resin composition by irradiating it with energy rays such as ultraviolet rays.
[0152] By containing urethane (meth)acrylate in the coating layer 17 formed as described above, the flexibility of the coating layer 17 can be improved, and since optical sheet 15 is applied, in part or in whole, to a structure having a curved shape, the occurrence of cracks on the surface of coating layer 17 can be effectively suppressed when optical sheet 15 is thermally bent, thereby imparting excellent thermoformability to optical sheet 15.
[0153] Furthermore, by combining the above-mentioned silicon-modified (meth)acrylic resin with this urethane (meth)acrylate, it is possible to obtain an optical sheet 15 that has both excellent scratch resistance and thermoformability at a high level.
[0154] The urethane (meth)acrylate is a compound having a main chain with a urethane bond (-OCONH-) and a (meth)acryloyl group linked to the main chain. The urethane (meth)acrylate is a monomer or oligomer.
[0155] The urethane (meth)acrylate of this composition has urethane bonds, and is therefore a compound with excellent flexibility. Therefore, by including urethane (meth)acrylate in the covering layer 17, it is possible to impart further flexibility (softness) to the covering layer 17. Therefore, when the optical sheet 15 is molded into the curved optical sheet 10 having a curved shape, it is possible to appropriately suppress the occurrence of cracks in the bent portion.
[0156] The urethane (meth)acrylate can be obtained, for example, as a reaction product between an isocyanate compound obtained by reacting a polyol with a diisocyanate, and a (meth)acrylate monomer having a hydroxyl group.
[0157] Examples of the polyol include polyether polyol, polyester polyol, and polycarbonate diol.
[0158] The polyester polyol can be obtained, for example, by polycondensation of a diol with a dicarboxylic acid or a dicarboxylic acid chloride, or by esterifying a diol or a dicarboxylic acid and then transesterifying it. Examples of the dicarboxylic acid include adipic acid, succinic acid, glutaric acid, pimelic acid, sebacic acid, azelaic acid, maleic acid, terephthalic acid, isophthalic acid, and phthalic acid, and examples of the diol include ethylene glycol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tetraethylene glycol, tripropylene glycol, and tetrapropylene glycol.
[0159] Furthermore, examples of polycarbonate diols include reaction products of diols and carbonate esters. Examples of diols that can be used include 1,4-butanediol, 1,6-hexanediol, ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, dipropylene glycol, 2-ethyl-1,3-hexanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,4-cyclohexanediol, and polyoxyethylene glycol. These can be used alone or in combination of two or more.
[0160] Examples of (meth)acrylate monomers having a hydroxyl group include trimethylolpropane triacrylate, pentaerythritol triacrylate, dipentaerythritol triacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxybutyl acrylate, 3-hydroxybutyl acrylate, and polyethylene glycol monoacrylate.
[0161] The content of the urethane (meth)acrylate in the resin composition is not particularly limited, but is preferably 10 parts by mass or more and 75 parts by mass or less, and more preferably 17 parts by mass or more and 50 parts by mass or less, in 100 parts by mass of the resin composition. If the content of the urethane (meth)acrylate in the resin composition is less than the lower limit, the flexibility of the coating layer 17 may be poor depending on the type of the urethane (meth)acrylate. If the content of the urethane (meth)acrylate in the resin composition exceeds the upper limit, the content of materials other than the urethane (meth)acrylate in the resin composition may relatively decrease depending on the type of the urethane (meth)acrylate, and the scratch resistance of the optical sheet 15 may decrease.
[0162] ((Meth)acrylate Monomer) In addition, the resin composition preferably further contains a (meth)acrylate monomer.
[0163] When an unsaturated double bond is introduced at the end or side chain of a repeating unit having a siloxane bond, which is contained in the silicon-modified (meth)acrylic resin, the (meth)acryloyl group of the (meth)acrylate monomer is bonded to the unsaturated double bond to form a network of the silicon-modified (meth)acrylic resin and the (meth)acrylate monomer, and as a result, the resin composition hardens to form coating layer 17.
[0164] The (meth)acrylate monomer is not particularly limited, but may be, for example, pentaerythritol tetraacrylate, ditrimethylolpropane triacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, dipentaerythritol triacrylate, ethoxylated trimethylolpropane triacrylate, ethoxylated pentaerythritol triacrylate, ethoxylated pentaerythritol tetraacrylate, polyethylene glycol diacrylate, ethoxylated bisphenol A diacrylate, ethoxylated hydrogenated bisphenol A diacrylate, ethoxylated cyclohexane dimethanol diacrylate, tricyclodecane dimethanol diacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxybutyl acrylate, 3-hydroxybutyl acrylate, isobornyl acrylate, etc., and one or more of these may be used in combination. Among these, from the viewpoint of improving the weather resistance of the optical sheet 15, it is preferable to use a resin that does not contain aromatics.
[0165] The content of the (meth)acrylate monomer in the resin composition is not particularly limited, but is preferably 15 parts by mass or more and 55 parts by mass or less, and more preferably 27 parts by mass or more and 55 parts by mass or less, per 100 parts by mass of the resin composition.
[0166] (Isocyanate) In addition, the resin composition preferably further contains an isocyanate. As a result, in the resin composition, the isocyanate functions as a crosslinking agent that bonds (crosslinks) between the molecules of the silicon-modified (meth)acrylic resin. That is, by including the isocyanate as a crosslinking agent, the hydroxyl group of the main chain of the silicon-modified (meth)acrylic resin, which is a repeating structural unit derived from a (meth)acrylic monomer having a (meth)acryloyl group, reacts with the isocyanate group of the isocyanate to form a crosslinked structure composed of urethane bonds, and as a result, a coating layer 17 composed of a cured product of the resin composition is formed. The curing of the resin composition by the bonding of the hydroxyl group and the isocyanate group is performed by thermal curing, which cures the resin composition by heating it.
[0167] In the coating layer 17 formed as described above, a network can be constructed by bonding hydroxyl groups and isocyanate groups, so that the scratch resistance and weather resistance of the coating layer 17 can be further improved.
[0168] The content of isocyanate in the resin composition is not particularly limited, but is preferably 3 parts by mass or more and 40 parts by mass or less, and more preferably 10 parts by mass or more and 25 parts by mass or less, per 100 parts by mass of the resin composition.
[0169] (Other materials) Furthermore, the resin composition may contain other materials in addition to the various materials described above. The other materials are not particularly limited, but examples thereof include resin materials other than the silicon-modified (meth)acrylic resin, photopolymerization initiators, ultraviolet absorbers, colorants, sensitizers, stabilizers, surfactants, antioxidants, reduction inhibitors, antistatic agents, surface conditioners, hydrophilic additives, fillers, and solvents, and one or more of these may be used in combination.
[0170] The average thickness of the coating layer 17 composed of the cured product of the resin composition as described above is not particularly limited, but is preferably 1 μm to 40 μm, more preferably 2 μm to 30 μm, and even more preferably 5 μm to 20 μm. If the thickness of the coating layer 17 is less than the lower limit, the weather resistance of the optical sheet 15 may be reduced. On the other hand, if the thickness of the coating layer 17 exceeds the upper limit, when the optical sheet 15 is made into a curved optical sheet 10 having a curved shape, cracks may occur in the curved optical sheet 10 during molding of the curved optical sheet 10.
[0171] The optical sheet 15 of the second embodiment as described above also provides the same effects as those of the first embodiment.
[0172] Although the optical sheet and optical component of the present invention have been described above, the present invention is not limited thereto. For example, each layer constituting the optical sheet 15 having the half mirror layer 13 as a reflector can be replaced with a layer of any configuration that can exert the same function. Furthermore, when it is necessary to impart superior strength or the like to the optical sheet 15, other substrates or the like may be laminated on the substrates 11 and 12, respectively, via adhesive layers.
[0173] Furthermore, in the above embodiment, the optical sheet 15 of the present invention is applied to a lens 30 having a curved optical sheet 10 having a curved shape as a curved resin substrate, i.e., the optical component of the present invention is composed of a lens 30, but the optical sheet 15 can also be attached to, for example, a cover film provided in a display device such as a liquid crystal display or a head-up display, a window member provided in a means of transportation such as a motorcycle, a car, an airplane, or a train, a machine tool, or a building, a cover member provided in a headlight or a fog lamp, a brightness enhancement film or a cold mirror provided in a light source provided in a head-up display, a reflector provided in an in-vehicle sensor such as an infrared sensor, or the like. In these cases, the optical component is composed of the cover film, the window member, the cover member, the brightness enhancement film, the cold mirror, or the reflector, and the curved optical sheet 10 attached thereto. EXAMPLES
[0174] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples in any way.
[0175] 1. Preparation of raw materials <Polycarbonate (PC1)> As the polycarbonate (PC1), Iupilon E2000 (manufactured by Mitsubishi Engineer Plastics Corporation) was prepared.
[0176] <Polymethylmethacrylate (heat-resistant PMMA1)> As polymethyl methacrylate (heat-resistant PMMA1), Delpet PM120N (manufactured by Asahi Kasei Corporation) was prepared.
[0177] <Polyethylene terephthalate (heat-resistant PETG1)> As heat-resistant amorphous polyethylene terephthalate (heat-resistant PETG1), Tritan TX2001 (glycol-modified polyethylene terephthalate, manufactured by Eastman Chemical Company) was prepared.
[0178] <Polyethylene terephthalate (PETG2)> As the amorphous polyethylene terephthalate copolymer (PETG2), Sky Green K2012 (manufactured by SK Chemicals) was prepared.
[0179] <Polyarylate (PAR1)> As the polyarylate (PAR1), U-polymer P-5001 (manufactured by Unitika Ltd.) was prepared.
[0180] <Polyethersulfone (PES)> As polyethersulfone (PES), Sumikaexcel 3600G (manufactured by Sumitomo Chemical Co., Ltd.) was prepared.
[0181] <Polyethylene naphthalate (PEN1)> Teonex TN8065S (manufactured by Teijin Ltd.) was prepared as the polyethylene naphthalate (PEN1).
[0182] <Polyethylene terephthalate (APET1)> As the polyethylene terephthalate (APET1), Novapex GM700Z (Mitsubishi Chemical Corporation, crystalline polyethylene terephthalate) was prepared.
[0183] <Acrylonitrile-styrene copolymer (AS1)> As the acrylonitrile-styrene copolymer (AS1), Denka AS-XGS (manufactured by Denka Co., Ltd.) was prepared.
[0184] <Styrene-N-phenylmaleimide-maleic anhydride copolymer (IP1)> As the styrene-N-phenylmaleimide-maleic anhydride copolymer (IP1), Denka IP-ND (manufactured by Denka Co., Ltd.) was prepared.
[0185] 2. Manufacturing of optical sheets Example 1 [1] First, polycarbonate (PC1) was prepared as a resin material for forming the substrates 11 and 12 and the high refractive index layer 31, and polymethyl methacrylate (heat-resistant PMMA1) was prepared as a resin material for forming the low refractive index layer 32.
[0186] [2] Next, polycarbonate (PC1, Tg 150°C) and polymethyl methacrylate (heat-resistant PMMA1, Tg 123°C) were melted at 270°C in an extruder (manufactured by Sun NT, "SNT40-28") and co-extruded using a feed block and a die to form a film. After that, these films were cooled to obtain the optical sheet 15 of Example 1, in which the upper and lower surfaces of the half mirror layer 13, which is composed of a laminate (multilayer laminate) in which high refractive index layers 31 and low refractive index layers 32 are alternately laminated and has a total of 1023 layers (repeated 511 times), are covered with the first substrate 11 and the second substrate 12, respectively. Here, the discharge amount was adjusted so that the laminate thickness ratio was high refractive index layer 31:low refractive index layer 32=1:1.
[0187] In the obtained half mirror layer 13, the refractive index of the low refractive index layer 32 at a wavelength of 589 nm was measured using an Appe refractometer (manufactured by ATAGO, "NA-1T SOLID") and was 1.510. In addition, the refractive index of the high refractive index layer 31 at a wavelength of 589 nm was measured using an Appe refractometer (manufactured by ATAGO, "NA-1T SOLID") and was 1.585. Furthermore, the average thickness of the half mirror layer 13 was 100 μm, and the average thicknesses of the first substrate 11 and the second substrate 12 were 0.3 mm.
[0188] (Examples 2 to 5, Reference Examples 1 to 3) In the step [1], the materials shown in Table 1 were prepared as the resin materials for forming the first substrate 11, the second substrate 12, the high refractive index layer 31 and the low refractive index layer 32, respectively, and the optical sheets 15 of Examples 2 to 5 and Reference Examples 1 to 3 were obtained in the same manner as in Example 1, except that the half mirror layer 13 obtained in the step [3] was subjected to a stretching treatment in MD as necessary.
[0189] 3. Evaluation The optical sheets 15 of the respective Examples and Reference Examples were evaluated by the following methods.
[0190] <1A> Measurement of reflectance R1 (%) of curved optical sheet 10 before heating First, the optical sheet 15 of each embodiment and each reference example was pressed against a metal mold at a temperature 10°C higher than the higher of the glass transition point Tg1 of the main material constituting the high refractive index layer 31 and the glass transition point Tg2 of the main material constituting the low refractive index layer 32, thereby making the optical sheet 15 (laminate) into a curved optical sheet 10 (curved laminate) having a curved shape with a curvature radius of 60 mm.
[0191] Next, the curved optical sheet 10 was placed between a light source emitting light of 589 nm and the light receiving unit so that the angle between the upper surface of the curved optical sheet and the straight line connecting the light source and the light receiving unit was 90°.
[0192] Next, the emitted light (transmitted light) emitted from the light source and transmitted through the curved optical sheet 10 was received by the light receiving section, and the transmittance (%) of this transmitted light was measured to determine the initial (before heating) reflectance R1 (%).
[0193] <2A> Measurement of reflectance R2 (%) of curved optical sheet 10 after heating First, the optical sheet 15 of each embodiment and each reference example was pressed against a metal mold at a temperature 10°C higher than the higher of the glass transition point Tg1 of the main material constituting the high refractive index layer 31 and the glass transition point Tg2 of the main material constituting the low refractive index layer 32, thereby making the optical sheet 15 (laminate) into a curved optical sheet 10 (curved laminate) having a curved shape with a curvature radius of 60 mm.
[0194] Next, the curved optical sheet 10 was stored in a heat circulation oven at a temperature environment of 105°C for 1000 hours, and then it was placed between a light source emitting light of 589 nm and a light receiving unit so that the angle between the upper surface of the curved optical sheet and the straight line connecting the light source and the light receiving unit was 90°.
[0195] Next, the emitted light (transmitted light) emitted from the light source and transmitted through the curved optical sheet 10 was received by the light receiving section, and the transmittance (%) of this transmitted light was measured to determine the reflectance R2 (%) after heating.
[0196] Then, the reflectance retention (R2 / R1×100[%]) was calculated using the reflectance R2 (%) after heating obtained here and the initial (before heating) reflectance R1 (%) obtained in <1A> above.
[0197] <3A> Confirmation of heat resistance of optical sheets in the visible light region First, the reflectance at a wavelength of 590 nm was measured for the optical sheet 15 of each of the examples and reference examples. Then, a durability test (105°C x 1000 hr) was performed, and the reflectance of the sample (optical sheet) after the test was also measured in the same manner.
[0198] The reflectances before and after the durability test were defined as R3 and R4, respectively. Based on these, the rate of change in reflectance was calculated as shown below.
[0199] Reflectance change rate: R4 / R3 x 100 (%) Thereafter, the obtained rate of change in reflectance was evaluated based on the following evaluation criteria.
[0200] [Evaluation Criteria] A: R4 / R3×100 is 85% or more B: R4 / R3×100 is 80% or more but less than 85% C: R4 / R3×100 is less than 80%
[0201] <5A> Confirmation of thermal bending properties of optical sheets First, the optical sheet 15 of each of the examples and reference examples was subjected to a thermal bending process by heating it to a temperature 10°C higher than the higher of the glass transition points Tg1 and Tg2 and pressing it against a metal mold having a curvature radius of 60 mm. The thermally bent curved optical sheet 10 was then stored in a heat circulation oven at a temperature of 105° C. for 1000 hours, after which the radius of curvature was measured and evaluated based on the following evaluation criteria.
[0202] [Evaluation Criteria] The number of curved optical sheets that maintain a radius of curvature of 60±5 mm after being stored for 1000 hours in a heat circulation oven at a temperature of 105°C is A: 50 out of 50 curved optical sheets B: Of 50 curved optical sheets, there are 48 or more but less than 50 C: Less than 48 out of 50 curved optical sheets
[0203] In addition, after storing the curved optical sheet 10 for 1,000 hours in a temperature environment of 105°C, the presence or absence of peeling between the substrates 11 and 12 and the half mirror layer 13 of the curved optical sheet 10 was visually confirmed and evaluated based on the evaluation criteria shown below. [Evaluation Criteria] The number of curved optical sheets in which peeling between the substrates 11 and 12 and the half mirror layer 13 was confirmed after storing the curved optical sheets for 1000 hours in a temperature environment of 105° C. in a heat circulation oven is A: 0 out of 50 curved optical sheets B: 1 to less than 3 out of 50 curved optical sheets C: 3 or more out of 50 curved optical sheets
[0204] The evaluation results of the optical sheets 15 of the respective Examples and Reference Examples thus obtained are shown in Table 1 below.
[0205] [Table 1]
[0206] As shown in Table 1, in the optical sheets in each embodiment, continuous layers are formed at the interface between the first substrate 11 and the half mirror layer 13 and at the interface between the second substrate 12 and the half mirror layer 13, respectively. This prevents peeling at each interface during excellent thermal bending processing, and the results show that the optical sheets have excellent processability. [Industrial Applicability]
[0207] According to the present invention, the half mirror layer having a repeating portion composed of a laminate in which high refractive index layers and low refractive index layers are alternately stacked, and the first substrate and the second substrate bonded to the half mirror layer form a continuous layer of the first substrate and the half mirror layer at the interface between the first substrate and the half mirror layer, and form a continuous layer of the second substrate and the half mirror layer at the interface between the second substrate and the half mirror layer. Therefore, even if the optical sheet is subjected to a thermal bending process to obtain a curved optical sheet by making one surface of the optical sheet a curved concave surface and the other surface a curved convex surface, peeling between the first substrate and the half mirror layer and the second substrate and the half mirror layer can be appropriately suppressed or prevented, and an optical sheet with excellent processability can be obtained. Therefore, the present invention has industrial applicability. [Explanation of symbols]
[0208] 10 Curved optical sheet 11 First base material 12 Second base material 13 Half mirror layer 15 Optical Sheet 17 Covering layer 20 Frames 21 Rim 22 Bridge section 23 Temple Section 24 Nose pad section 30 Lenses 31 High refractive index layer 32 Low refractive index layer 33 Repeat Section 35 Resin layer 40 Mold 50 Protective Film 100 Sunglasses 150 Multilayer laminate 200 Curved multi-layer laminate
Claims
1. A first base material mainly made of a resin material having optical transparency; a half mirror layer provided on one surface of the first base material and made of a laminate in which high refractive index layers and low refractive index layers are alternately and repeatedly laminated; an optical sheet including a second substrate that is mainly made of the resin material and is bonded to a surface of the half mirror layer opposite to the first substrate, In the half mirror layer, the refractive index of the high refractive index layer is higher than the refractive index of the low refractive index layer, an interface between the first substrate and the half mirror layer forms a continuous layer between the first substrate and the half mirror layer, and an interface between the second substrate and the half mirror layer forms a continuous layer between the second substrate and the half mirror layer, The half mirror layer has a thickness direction retardation (Rth) of 300 nm or less at a wavelength of 589 nm.
2. 2. The optical sheet according to claim 1, wherein Tg1 is a glass transition point of a main material constituting the high refractive index layer, and Tg2 is a glass transition point of a main material constituting the low refractive index layer, and Tg1, Tg2 are greater than or equal to 105° C.
3. 3. The optical sheet according to claim 2, wherein the glass transition point Tg1 and the glass transition point Tg2 satisfy the relationship: 0° C.≦|Tg1−Tg2|≦60° C.
4. 4. The optical sheet according to claim 2, wherein the lower of the glass transition points Tg1 and Tg2 is 110° C. or higher and 250° C. or lower.
5. 4. The optical sheet according to claim 1, wherein the refractive index difference (N1-N2) is 0.05 or more and 0.25 or less, where N1 is the refractive index of the high refractive index layer at a wavelength of 589 nm and N2 is the refractive index of the low refractive index layer at a wavelength of 589 nm.
6. 4. The optical sheet according to claim 1, wherein the high refractive index layer and the low refractive index layer each have an average thickness of 50 nm or more and 300 nm or less.
7. 4. The optical sheet according to claim 1, wherein the number of times the high refractive index layers and the low refractive index layers are alternately laminated in the half mirror layer is 50 to 750.
8. the optical sheet is curved into a curved shape with a curvature radius of 60 mm at a temperature 10° C. higher than the higher of a glass transition point Tg1 of a main material constituting the high refractive index layer and a glass transition point Tg2 of a main material constituting the low refractive index layer, the reflectance of the curved optical sheet at a wavelength of 589 nm is R1 [%], 4. The optical sheet according to claim 1, wherein after storing the curved optical sheet for 1,000 hours in a temperature environment of 105°C in a heat circulation oven, the reflectance retention calculated by R2 / R1 x 100 [%] is 80% or more, where R2 [%] is the reflectance of the curved optical sheet at light with a wavelength of 589 nm.
9. 4. The optical sheet according to claim 1, wherein the optical sheet is curved at a temperature 10° C. higher than the higher of a glass transition point Tg1 of a main material constituting the high refractive index layer and a glass transition point Tg2 of a main material constituting the low refractive index layer, and after storing the optical sheet for 1,000 hours in a temperature environment of 105° C. in a heat circulation oven, the number of the curved optical sheets in which peeling has occurred between the first substrate and the half mirror layer or between the second substrate and the half mirror layer is 2 or less out of 50 curved optical sheets.
10. An optical component comprising the optical sheet according to claim 1 .
Citation Information
Patent Citations
Polarizing layer laminate and its manufacturing method
JP2009294445A
Optical film, polarizing plate and image display device
JP2013101330A
Infrared ray shield film and manufacturing method thereof
JP2015055818A
Multilayered laminated film
JP2021045924A
Optical film for eyewear, and functional film for eyewear, optical laminate for eyewear, and eyewear which have same
WO2017086067A1