Weld metal and weld joints
A weld metal with controlled alloy components and oxide inclusions addresses the toughness issue in high-strength applications, achieving enhanced mechanical properties through refined microstructure.
Patent Information
- Application Number
- JP2020147561
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-02
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-09-02
AI Technical Summary
Existing weld metals with high Al content tend to have coarse structures, leading to insufficient toughness when used in high-strength applications.
A weld metal composition with controlled amounts of C, Si, Mn, Ni, Cr, Mo, Ti, and O, along with specific oxide inclusions, ensures high strength and toughness by acting as intragranular transformation nuclei, refining the weld metal structure.
The refined structure enhances the weld metal's toughness and strength, providing a weld joint with improved mechanical properties.
Smart Images

Figure 0007564428000008 
Figure 0007564428000009 
Figure 0007564428000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a weld metal and a weld joint. [Background technology]
[0002] Demand for natural gas is on the rise due to the increase in global energy demand and the need to reduce CO2 emissions. Long-distance pipelines are necessary to transport natural gas. From the perspective of cost reduction, the development and application of high-strength steel pipes that enable higher operating pressures and reduced steel usage is being promoted. In addition, in recent years, pipelines have become larger and are increasingly used in cold regions, so there is a demand for steel plates used in pipelines with even higher strength and toughness.
[0003] In addition, welding is essential for the construction of long-distance pipelines, so the development of a weld metal with high strength and toughness is an important issue in the development of high-strength steel pipes.
[0004] For example, Patent Document 1 discloses a technology for suppressing the growth of unstable brittle cracks and improving the crack tip opening displacement (CTOD) characteristics by appropriately controlling the contents of particularly Al, Ti, and O in the weld metal and controlling the average circular equivalent diameter and number density of Al-containing oxides within predetermined ranges.
[0005] Furthermore, Patent Document 1 discloses a technique for obtaining a weld metal having high strength by controlling the individual contents of the chemical components of the weld metal as well as the contents of C, Mn, Cu, Ni, Cr, and Mo relative to one another. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2018 / 043455 Summary of the Invention [Problem to be solved by the invention]
[0007] However, the weld metal described in Patent Document 1 has a large amount of Al-containing oxides, and therefore the structure of the weld metal tends to become coarse. Therefore, when the technology described in Patent Document 1 is applied to a weld metal that requires high strength, there is a problem that sufficient toughness cannot be obtained.
[0008] The present invention has been made to solve the above problems, and has an object to provide a weld metal and a weld joint that have high strength and excellent toughness. [Means for solving the problem]
[0009] In order to solve the above problems, the present invention provides the following means. (1) A weld metal according to one aspect of the present invention has a chemical composition, by mass%, of C: 0.02 to 0.12%, Si: 0.10 to 0.70%, Mn: 0.5 to 2.0%, P: 0.03% or less, S: 0.02% or less, N: 0.03% or less, Ni: 1.0 to 3.5%, Cr: more than 0% and 1.0% or less, Mo: 0.3 to 2.0%, Ti: more than 0.005% and 0.500% or less, and O: 0.005 to 0.050%, with the balance being Fe and impurities. The oxides having an equivalent circle diameter of 0.10 μm or more have an average chemical composition comprising 10 to 70 mass% Mn, 10 to 50 mass% Ti, 0 to 20 mass% Si, and 5 mass% or less Al, and in the average chemical composition, the total amount of Mn, Ti, and Si is 60 mass% or more, the oxides having an equivalent circle diameter of 0.10 μm or more have an average equivalent circle diameter of 0.30 to 1.00 μm, and the number density of the oxides having an equivalent circle diameter of 0.10 μm or more is 0.005 to 0.05 / μm 2 and α defined by the following formula (1) is 0.40% or more and 0.80% or less. α=[C]+[Si] / 24+[Mn] / 6+[Ni] / 40+[Cr] / 5+[Mo] / 4+[V] / 14...(1) However, the elements in brackets in formula (1) indicate the content of each element in mass % in the chemical composition of the weld metal, and 0 is substituted for elements that are not contained. (2) The weld metal described in (1) above may further contain, in mass%, one or more of Al: 0.010% or less, Cu: 0.200% or less, Nb: 0.100% or less, V: 0.100% or less, and B: 0.0020% or less, in place of a portion of the Fe. In the case where the weld metal contains V, α defined by the following formula (2) may be 0.40% or more and 0.80% or less, instead of the α defined by the formula (1) above. α=[C]+[Si] / 24+[Mn] / 6+[Ni] / 40+[Cr] / 5+[Mo] / 4+[V] / 14...(2) However, the elements in brackets in formula (2) indicate the content of each element in the chemical composition of the weld metal, expressed as mass%, and 0 is substituted for elements that are not contained. (3) A welded joint according to another aspect of the present invention comprises the weld metal according to (1) or (2). Effect of the Invention
[0010] According to the present invention, it is possible to provide a weld metal and a weld joint having high strength and excellent toughness. [Brief description of the drawings]
[0011] [Figure 1] 1 shows the results of measuring the chemical composition of oxides in a weld metal according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing test piece processing positions of a weld metal and a weld joint according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] In order to improve the toughness of weld metal, the present inventors have investigated the effects of alloy components and inclusions on toughness and have obtained the following findings. In weld metal with a tensile strength of about 600 MPa, the inclusion of a large amount of B promotes intragranular transformation, refines the structure of the weld metal, and improves the toughness of the weld metal. However, conversely, in weld metal with a tensile strength of about 980 MPa, the inclusion of a large amount of B suppresses intragranular transformation and inhibits the refinement of the weld metal structure. Therefore, in weld metal with a tensile strength of 980 MPa or more, the inclusion of a large amount of B reduces the toughness of the weld metal. In addition, it was found that by making the chemical composition of the inclusions in the weld metal mainly oxides of Mn, Ti, and Si, the inclusions act as intragranular transformation nuclei, which is extremely effective in refining the structure of the weld metal. By finely dispersing these inclusions in the weld metal, good toughness can be obtained.
[0013] The present invention has been made as a result of the above-mentioned investigations, and the reasons for limiting the characteristic technical requirements and preferable aspects of the embodiments of the present invention will be described below. First, the weld metal according to the embodiment of the present invention will be described.
[0014] (Chemical composition of weld metal) The alloy components contained in the weld metal according to this embodiment and the reasons for limiting the content of each component will be described below. In the following description, "%" means "mass %" unless otherwise specified.
[0015] C: 0.02-0.12% C has the effect of improving the strength of the weld metal by dissolving in the weld metal. Furthermore, C has the effect of improving the hardenability of the weld metal. In order to ensure the strength of the weld metal, the C content is set to 0.02% or more. The lower limit of the C content may be set to 0.05%. On the other hand, when an excessive amount of C is present in the weld metal, hard structures such as carbides and martensite are likely to form. Therefore, an excessive amount of C may reduce the toughness of the weld metal. In addition, an excessive amount of C may make the weld metal more susceptible to hot welding cracking. Therefore, the C content is set to 0.12% or less. The upper limit of the C content may be set to 0.11%.
[0016] Silicon: 0.10 to 0.70% Since Si is an element having a deoxidizing effect, it has the effect of improving the cleanliness of the weld metal and suppressing the occurrence of welding defects such as blowholes. Furthermore, Si dissolves in the weld metal, thereby improving the strength of the weld metal. In addition, Si, together with Mn and Ti described below, forms oxides that become intragranular transformation nuclei in the weld metal. The presence of intragranular transformation nuclei in the weld metal makes the structure of the weld metal finer. As a result, the toughness of the weld metal is improved. To obtain these effects, the Si content is set to 0.10% or more. The lower limit of the Si content may be set to 0.20%. On the other hand, when an excessive amount of Si dissolves in the weld metal, hard structures such as island martensite are likely to form. Therefore, an excessive amount of Si may reduce the toughness of the weld metal. Therefore, the Si content is set to 0.70% or less. The upper limit of the Si content may be set to 0.50%.
[0017] Mn: 0.5-2.0% Mn has the effect of improving the strength of the weld metal by dissolving in the weld metal. In addition, Mn, together with Si and Ti described later, forms oxides that become intragranular transformation nuclei in the weld metal. The presence of intragranular transformation nuclei in the weld metal makes the structure of the weld metal finer. As a result, the toughness of the weld metal is improved. To obtain these effects, the Mn content is set to 0.5% or more. The lower limit of the Mn content may be set to 0.8%. On the other hand, when an excessive amount of Mn dissolves in the weld metal, it becomes easier for hard structures such as martensite to form, and therefore an excessive amount of Mn may reduce the toughness of the weld metal. Therefore, the Mn content is set to 2.0% or less. The upper limit of the Mn content may be set to 1.5%.
[0018] P:0.03% or less P is an impurity. Therefore, the lower limit of the P content is set to 0%. Since excessive reduction leads to increased costs, it may be set to, for example, 0.001% or more. On the other hand, if the P content exceeds 0.03%, the toughness of the weld metal is deteriorated. Therefore, the upper limit of the P content is set to 0.03%.
[0019] S: 0.02% or less S is an impurity. Therefore, the lower limit of the S content is set to 0%. Since excessive reduction leads to increased costs, it may be set to, for example, 0.001% or more. On the other hand, if the S content exceeds 0.02%, the toughness of the weld metal is deteriorated. Therefore, the upper limit of the S content is set to 0.02%.
[0020] N: 0.03% or less N is an impurity. Therefore, the lower limit of the N content is set to 0%. Excessive reduction leads to increased costs, so it may be set to, for example, 0.002% or more. On the other hand, if the N content exceeds 0.03%, coarse nitrides are formed in the weld metal, deteriorating the toughness of the weld metal. Therefore, the upper limit of the N content is set to 0.03%.
[0021] Ni: 1.0~3.5% Ni has the effect of improving the toughness of the weld metal by dissolving in the weld metal. To obtain this effect, the Ni content is set to 1.0% or more. The lower limit of the Ni content may be set to 2.0%. On the other hand, when an excessive amount of Ni dissolves in the weld metal, hard structures such as martensite are likely to form. Therefore, an excessive amount of Ni may reduce the toughness of the weld metal. Furthermore, an excessive amount of Ni may make the weld metal more susceptible to hot welding cracking. Therefore, the Ni content is set to 3.5% or less. The upper limit of the Ni content may be set to 3.2%.
[0022] Cr: More than 0% and 1.0% or less Cr has the effect of improving the strength of the weld metal by dissolving in the weld metal. To obtain this effect, the Cr content is set to more than 0%. The lower limit of the Cr content may be set to 0.1%. On the other hand, an excessive amount of Cr reacts with C or N to form Cr carbides or Cr nitrides, which are the starting points of fracture. Therefore, an excessive amount of Cr may reduce the toughness of the weld metal. Therefore, the Cr content is set to 1.0% or less. The upper limit of the Cr content may be set to 0.7%.
[0023] Mo: 0.3-2.0% Mo has the effect of improving the strength of the weld metal by dissolving in the weld metal. In addition, Mo has the effect of strengthening grain boundaries. Therefore, Mo improves the toughness of the weld metal. To obtain these effects, the Mo content is set to 0.3% or more. The lower limit of the Mo content may be set to 0.5%. On the other hand, when an excessive amount of Mo dissolves in the weld metal, it becomes easier for hard structures such as martensite to form. Therefore, an excessive amount of Mo may reduce the toughness of the weld metal. Therefore, the Mo content is set to 2.0% or less. The upper limit of the Mo content may be set to 1.5%.
[0024] Ti: more than 0.005% and less than 0.500% Ti, together with Si and Mn, forms oxides in the weld metal that become intragranular transformation nuclei. The presence of intragranular transformation nuclei in the weld metal refines the structure of the weld metal. As a result, the toughness of the weld metal is improved. To obtain this effect, the Ti content is set to more than 0.005%. The lower limit of the Ti content may be set to 0.007%, 0.010%, or 0.013%. On the other hand, an excessive amount of Ti reacts with C or N to form Ti carbides or Ti nitrides, which are the starting points of fracture. Therefore, an excessive amount of Ti may reduce the toughness of the weld metal. Therefore, the Ti content is set to 0.500% or less. The upper limit of the Ti content may be set to 0.470%, 0.430%, or 0.400%.
[0025] O: 0.005 to 0.050% O reacts with Ti, Si, and Mn to form oxides that become intragranular transformation nuclei. The presence of intragranular transformation nuclei in the weld metal makes the structure of the weld metal finer. As a result, the toughness of the weld metal is improved. To obtain this effect, O is set to 0.005% or more. The lower limit of the O content may be set to 0.010%. On the other hand, an excessive amount of O increases the number density of inclusions that are the starting points of fracture. Therefore, an excessive amount of O may reduce the toughness of the weld metal. Therefore, the O content is set to 0.050% or less. The upper limit of the O content may be set to 0.040%.
[0026] Al: 0.010% or less Al does not have to be contained in the weld metal, so the lower limit of the Al content is set to 0%. However, since Al is an element having a deoxidizing effect, Al may be contained in the weld metal. The lower limit of the Al content may be set to 0.001%. On the other hand, the affinity of Al with O is higher than the affinity of Ti, Si, and Mn with O. As a result, an excessive amount of Al inhibits the formation of complex oxides containing Ti, Si, and Mn that act as intragranular transformation nuclei. Therefore, an excessive amount of Al may reduce the toughness of the weld metal. Therefore, the Al content is set to 0.010% or less. The upper limit of the Al content may be set to 0.0070%.
[0027] Cu:0.200% or less Cu does not have to be contained in the weld metal, so the lower limit of the Cu content is set to 0%. However, Cu has the effect of improving the strength of the weld metal by dissolving in the weld metal. Furthermore, Cu improves the toughness of the weld metal by dissolving in the weld metal. To obtain these effects, the lower limit of the Cu content may be set to 0.001%. On the other hand, an excessive amount of Cu makes it easier to form precipitates that become the starting point of fracture. Therefore, an excessive amount of Cu may reduce the toughness of the weld metal. Therefore, the Cu content is set to 0.200% or less. The upper limit of the Cu content may be set to 0.150%.
[0028] Nb: 0.100% or less Nb does not have to be contained in the weld metal, so the lower limit of the Nb content is set to 0%. However, Nb has the effect of improving the strength of the weld metal by dissolving in the weld metal. To obtain this effect, Nb may be contained in the weld metal. The lower limit of the Nb content may be set to 0.001%. On the other hand, an excessive amount of Nb is undesirable because it forms precipitates and reduces the toughness of the weld metal. Therefore, the Nb content is set to 0.100% or less. The upper limit of the Nb content may be set to 0.070%.
[0029] V:0.100% or less V does not have to be contained in the weld metal. Therefore, the lower limit of the V content is set to 0%. However, V has the effect of improving the strength of the weld metal by dissolving in the weld metal. To obtain this effect, V may be contained in the weld metal. The lower limit of the V content may be set to 0.001%. On the other hand, an excessive amount of V makes it easier to form precipitates that become the starting point of fracture. Therefore, an excessive amount of V is undesirable because it reduces the toughness of the weld metal. Therefore, the V content is set to 0.100% or less. The upper limit of the V content may be set to 0.070%.
[0030] B: 0.0020% or less B does not have to be contained in the weld metal. Therefore, the lower limit of the B content is set to 0%. It is generally believed that B promotes intragranular transformation by dissolving in the weld metal. However, in high-strength weld metal, excessive B segregates at the interface between the parent phase and oxides that become the nuclei for intragranular transformation. B that segregates at the interface between the parent phase and oxides that become the nuclei for intragranular transformation suppresses intragranular transformation. This causes the weld metal structure to become coarse. Therefore, excessive B may reduce the toughness of the weld metal. For this reason, the B content is set to 0.0020% or less. On the other hand, B has the effect of improving the hardenability of the weld metal by dissolving in the weld metal. To obtain these effects, B may be contained in the weld metal. The lower limit of the B content may be 0.0001%, 0.0003%, or 0.0010%.
[0031] The balance of the weld metal is Fe and impurities. The impurities are components that are mixed in from the welding material, base metal, and surrounding atmosphere such as shielding gas, and do not impair the properties of the weld metal according to this embodiment.
[0032] (α: 0.40% or more and 0.80% or less) The weld metal of this embodiment contains the above-mentioned elements. In addition, in order to ensure the strength and toughness of the weld metal, the weld metal of this embodiment further contains α, which is represented by the following formula (1), in the range of 0.40% to 0.80%. α=[C]+[Si] / 24+[Mn] / 6+[Ni] / 40+[Cr] / 5+[Mo] / 4...(1) However, the elements in brackets in formula (1) indicate the content of each element in the chemical composition of the weld metal, expressed as mass%, and 0 is substituted for elements that are not contained. However, if the weld metal contains V, the following formula (2) is used. α=[C]+[Si] / 24+[Mn] / 6+[Ni] / 40+[Cr] / 5+[Mo] / 4+[V] / 14...(2)
[0033] The method for measuring the chemical composition of weld metal is as follows: For elements other than O and N, first, a 15mm square sample is taken 2mm from the surface of the weld bead and from the center of the weld metal. Then, the chemical composition is measured using the countback method in accordance with JIS G 1256 (Method for fluorescent X-ray analysis of iron and steel), 2013. If it is not possible to take a 15mm square sample from the weld metal, JIS G 1258 (Method for inductively coupled plasma atomic emission spectrometry analysis of iron and steel), 2017, may be used instead of JIS G 1256 (Method for fluorescent X-ray analysis of iron and steel), 2013. In addition, O is measured for the above samples using JIS G 1239 (inert gas fusion-infrared absorption method) of 2014. N is measured for the above samples using JIS G 1228 (iron and steel-nitrogen determination method) of 2006.
[0034] (Chemical composition of oxides) The reasons for limiting the average chemical composition of oxides in the weld metal according to this embodiment will be described below.
[0035] The average chemical composition of the oxide having an equivalent circle diameter of 0.10 μm or more is Mn: 10-70 mass%, Ti: 10-50 mass%, Si: 0-20 mass%, and Al: 5 mass% or less. In the average chemical composition of this oxide, the total amount of Mn, Ti, and Si is 60 mass% or more. Hereinafter, unless otherwise specified, "oxide" means an oxide having an equivalent circle diameter of 0.10 μm or more. The average chemical composition of an oxide refers to the average value of the chemical compositions of multiple oxides obtained by measurement. In addition, oxides with a circle equivalent diameter of less than 0.10 μm are not very effective as intragranular transformation nuclei. Therefore, the calculation of the average chemical composition of an oxide does not take into account the chemical composition of oxides with a circle equivalent diameter of less than 0.10 μm.
[0036] By setting the chemical composition of the oxides within the above range, the oxides finely dispersed in the weld metal are extremely effective as intragranular transformation nuclei. The intragranular transformation nuclei have the effect of refining the structure of the weld metal. As a result, the toughness of the weld metal is improved. In addition, Al oxides do not act as intragranular transformation nuclei. Furthermore, if the Al content of the oxides is excessively high, the effect of the oxides in refining the structure is impaired. Therefore, the average chemical composition of oxides having a circle equivalent diameter of 0.10 μm or more is set to Al: 5 mass% or less. Furthermore, if the average chemical composition of the oxides is outside the above range, the oxides will not be effective as intragranular transformation nuclei, but will rather become the starting points of fracture, thereby reducing the toughness of the weld metal. As long as the above requirements are met, the oxide having an equivalent circle diameter of 0.10 μm or more may contain elements other than those mentioned above.
[0037] The method for measuring the average chemical composition of oxides having a circle-equivalent diameter of 0.10 μm or more is as follows. For mass%, first, the chemical composition of the oxides is measured at a magnification of 5000 times or more using a SEM (scanning electron microscope) and EDS (energy dispersive X-ray analysis). Here, oxides having a circle-equivalent diameter of less than 0.10 μm are not measured. An example of the measurement result is shown in FIG. 1. The average value of the chemical composition of oxides having a circle-equivalent diameter of 0.10 μm or more is calculated to obtain the average chemical composition of oxides having a circle-equivalent diameter of 0.10 μm or more. The size of the measurement field is not particularly limited, but the number of oxides having a circle-equivalent diameter of 0.10 μm or more used when calculating the average chemical composition is 200 or more.
[0038] (Oxide form) The reasons for limiting the form of oxides in the weld metal according to this embodiment will be described below.
[0039] Average equivalent circle diameter of oxides with an equivalent circle diameter of 0.10 μm or more: 0.30 to 1.00 μm Oxides with an equivalent circle diameter of 0.10 μm or more are effective as intragranular transformation nuclei. Intragranular transformation nuclei have the effect of refining the structure of the weld metal. Therefore, oxides with an equivalent circle diameter of 0.10 μm or more improve the toughness of the weld metal. If the average equivalent circle diameter of oxides with an equivalent circle diameter of 0.10 μm or more is less than 0.30 μm, the effect of intragranular transformation nuclei decreases. Therefore, the average equivalent circle diameter of oxides with an equivalent circle diameter of 0.10 μm or more is set to 0.30 μm or more. On the other hand, an excessive amount of coarse oxides can become the starting point of fracture. Therefore, if the average equivalent circle diameter of oxides having an equivalent circle diameter of 0.10 μm or more exceeds 1.00 μm, the toughness of the weld metal decreases. Therefore, the average equivalent circle diameter of oxides having an equivalent circle diameter of 0.10 μm or more is set to 1.00 μm or less. The upper limit of the average equivalent circle diameter of oxides having an equivalent circle diameter of 0.10 μm or more may be 0.80 μm.
[0040] The method for measuring the average equivalent circle diameter of oxides having a circle equivalent diameter of 0.10 μm or more is as follows. First, a photograph of the oxide is taken using SEM and EDS. The photograph is taken 2 mm from the surface layer of the weld bead and at the center of the weld metal. The photograph is analyzed using an image to measure the area of each oxide. The equivalent circle diameter of the oxide is calculated using the measured area of the oxide and a formula for calculating the area of a circle. Among the measured oxides, oxides having an equivalent circle diameter of less than 0.10 μm are not measured. The average value of the equivalent circle diameters of oxides having an equivalent circle diameter of 0.10 μm or more is calculated. The calculated average value is the average equivalent circle diameter of oxides having an equivalent circle diameter of 0.10 μm or more. The size of the measurement field of view is not particularly limited, but the number of oxides having an equivalent circle diameter of 0.10 μm or more used when calculating the average equivalent circle diameter is 200 or more.
[0041] Number density of oxides with a circle equivalent diameter of 0.10 μm or more: 0.005 to 0.05 / μm 2 Oxides with a circle equivalent diameter of 0.10 μm or more are effective as intragranular transformation nuclei. To obtain this effect, the number density of oxides with a circle equivalent diameter of 0.10 μm or more is 0.005 μm or less. 2 The number density of oxides with a circle equivalent diameter of 0.10 μm or more is 0.005 μm or more. 2 If it is less than 0.008 / μm, the number of intragranular transformation nuclei becomes excessively small. This causes the structure of the weld metal to become coarse. As a result, the toughness of the weld metal decreases. The lower limit of the number density of oxides with a circle equivalent diameter of 0.10 μm or more is 0.008 / μm 2 It is also possible to use the following. On the other hand, an excessive amount of oxides can become the starting point of fracture. Therefore, the number density of an excessive amount of oxides may reduce the toughness of the weld metal. Therefore, the number density of oxides with a circle equivalent diameter of 0.10 μm or more is 0.05 / μm. 2 The upper limit of the number density of oxides with a circle equivalent diameter of 0.10 μm or more is 0.045 / μm 2 It is also possible to use the following.
[0042] The method for measuring the number density of oxides having an equivalent circle diameter of 0.10 μm or more is as follows. First, the number of oxides having an equivalent circle diameter of 0.10 μm or more is measured using SEM and EDS. The measurement location is 2 mm from the surface layer of the weld bead and at the center of the weld metal. Then, the number of oxides having an equivalent circle diameter of 0.10 μm or more is divided by the measurement area to obtain the number density of oxides having an equivalent circle diameter of 0.10 μm or more. The size of the measurement field of view is not particularly limited, but the number of oxides having an equivalent circle diameter of 0.10 μm or more used to measure the number density of oxides is 200 or more.
[0043] Next, a welded joint according to an embodiment of the present invention will be described.
[0044] The welded joint according to the embodiment of the present invention includes the weld metal according to the embodiment of the present invention described above. The base steel plate is not particularly limited. When the base steel plate is a steel plate having excellent strength and toughness, it is preferable because a welded joint having high strength and excellent toughness can be obtained.
[0045] Next, a method for producing a weld metal and a weld joint according to an embodiment of the present invention will be described.
[0046] The method for producing the weld metal and the weld joint according to the embodiment of the present invention is not particularly limited, but for example, shielded metal arc welding and gas shielded metal arc welding may be used. The chemical composition and structure of the base material and the welding material are not particularly limited as long as the chemical composition and oxides of the weld metal after welding satisfy the requirements of the chemical composition and structure of the weld metal according to the embodiment of the present invention. When the steel plate serving as the base material is a steel plate having excellent strength and toughness, it is preferable because a weld joint having high strength and excellent toughness can be obtained.
[0047] The method for producing the weld metal and weld joint according to the embodiment of the present invention is not particularly limited, but for example, they can be suitably produced by setting the heat input to 1.5 to 2.3 kJ / mm. If the heat input is less than 1.5 kJ / mm, the cooling rate of the weld metal increases, and the average equivalent circle diameter of oxides may decrease. In other words, the number of oxides large enough to contribute as intragranular transformation nuclei decreases, and the effect of refining the microstructure is not sufficiently obtained, so that the toughness of the weld metal and weld joint may be insufficient. On the other hand, if the heat input exceeds 2.3 kJ / mm, the cooling rate of the weld metal will be slow, and the oxide density may be low. In other words, the number of intragranular transformation nuclei will be reduced, and the effect of refining the microstructure will not be sufficient, so that the toughness of the weld metal and welded joint may be insufficient. Furthermore, when the heat input exceeds 2.3 kJ / mm, the cooling rate of the weld metal slows down, and the average circle equivalent diameter of the oxides may increase, which may increase the number of coarse inclusions that can be the starting points of fracture, resulting in insufficient toughness of the weld metal and welded joint.
[0048] Welding conditions such as welding speed, welding current, arc voltage, groove shape, and backing metal are not particularly limited as long as the heat input falls within the above-mentioned range.
[0049] According to the weld metal and weld joint of the embodiments of the present invention, the chemical compositions of the weld metal and oxides, and the morphology of the oxides are set to predetermined modes, and oxides with an equivalent circle diameter of 0.10 μm or more that serve as intragranular transformation nuclei are finely dispersed in the weld metal, so that a weld metal having high strength and excellent toughness can be provided.
[0050] In particular, by specifying the content of Al, which has a high affinity with O, it is possible to control the number of oxides in the weld metal without inhibiting the formation of oxides having an equivalent circle diameter of 0.10 μm or more, thereby making it possible to provide a weld metal and weld joint with high strength and excellent toughness. EXAMPLES
[0051] Next, an embodiment of the present invention will be described. The conditions shown in the embodiment are an example adopted to confirm the feasibility and effects of the present invention. Therefore, the present invention is not limited to this example. Various conditions can be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.
[0052] A groove was prepared using a base material having the chemical composition shown in Table 1. A number of steel plates were prepared with different amounts of Al, Cu, Nb, V, and B added. A rod (Table 5) was prepared with different amounts of Ti added to the flux of a covered metal arc welding rod (welding material). However, the balance of the chemical composition of the base material shown in Table 1 is Fe and impurities. The prepared groove was subjected to covered metal arc welding. As a result, a total of 10 types of weld metal and weld joints were obtained, which are Examples 1 to 6 and Comparative Examples 1 to 4. The chemical composition of the weld metal is shown in Table 2. The chemical composition, number density, and average circle equivalent diameter of the oxide are shown in Tables 3 and 4. The tensile strength and impact value of the weld metal and weld joint are shown in Table 4. In addition, the welding material and welding conditions are shown in Tables 5 to 7. In Table 2, even if Al was not intentionally added, the composition analysis of the weld metal was performed and the values were shown. In addition, the description "<0.002" in Table 2 indicates that it was below the lower limit of analysis.
[0053] The method for measuring the chemical composition of the weld metal was as follows. For elements other than O and N, a 15 mm square sample was first taken 2 mm from the surface of the weld bead and from the center of the weld metal. The chemical composition was then measured using the countback method in accordance with JIS G 1256 (Method for fluorescent X-ray analysis of iron and steel) in 2013. The O content of the above samples was measured using JIS G 1239 (inert gas fusion-infrared absorption method) in 2014. The N content of the above samples was measured using JIS G 1228 (iron and steel-nitrogen determination method) in 2006.
[0054] [Table 1]
[0055] [Table 2]
[0056] The method for measuring the average equivalent circle diameter of oxides having a circle equivalent diameter of 0.10 μm or more was as follows. First, a photograph of the oxide was taken using an SEM. The photograph was taken 2 mm from the surface layer of the weld bead and at the center of the weld metal. The photograph was analyzed to measure the area of each oxide. The equivalent circle diameter of the oxide was calculated using the measured area of the oxide and a formula for calculating the area of a circle. Among the measured oxides, oxides having an equivalent circle diameter of less than 0.10 μm were not measured. The average value of the equivalent circle diameter of oxides having an equivalent circle diameter of 0.10 μm or more was calculated. The calculated average value was taken as the average equivalent circle diameter of oxides having an equivalent circle diameter of 0.10 μm or more. The size of the measurement field of view is not particularly limited, but the number of oxides having an equivalent circle diameter of 0.10 μm or more used to calculate the average equivalent circle diameter was 217. The measurement results are shown in Table 3.
[0057] The method for measuring the chemical composition of oxides with a circle equivalent diameter of 0.10 μm or more was as follows. First, a photograph of the oxide was taken using an SEM. The photograph was taken 2 mm from the surface layer of the weld bead and at the center of the weld metal. The photograph was analyzed to measure the area of each oxide. The circle equivalent diameter of the oxide was calculated using the measured area of the oxide and a formula for calculating the area of a circle. Among the measured oxides, oxides with a circle equivalent diameter of less than 0.10 μm were not measured. The chemical composition of the oxide was measured by EDS point analysis, aiming at the center of each oxide with a circle equivalent diameter of 0.10 μm or more. The size of the measurement field of view was not particularly limited, but the number of oxides with a circle equivalent diameter of 0.10 μm or more used to calculate the chemical composition of the oxide was 217. The measurement results are shown in Table 4.
[0058] The method for measuring the number density of oxides having a circle-equivalent diameter of 0.10 μm or more was as follows. First, the number of oxides having a circle-equivalent diameter of 0.10 μm or more was measured using an SEM. The measurement location was 2 mm from the surface layer of the weld bead and at the center of the weld metal. Then, the number of oxides having a circle-equivalent diameter of 0.10 μm or more was divided by the measurement area to obtain the number density of oxides having a circle-equivalent diameter of 0.10 μm or more. The size of the measurement field of view was not particularly limited, but the number of oxides having a circle-equivalent diameter of 0.10 μm or more used to measure the number density of oxides was 217. The measurement results are shown in Table 3.
[0059] Tensile test pieces and Charpy impact test pieces were taken from the positions shown in Figure 2. Tensile tests of weld metals were conducted in accordance with JIS Z 3121 (tensile test method for butt welded joints) in 2013. Charpy impact tests of weld metals were conducted in accordance with JIS Z 2242 (Charpy impact test method for metallic materials) in 2018. Toughness was judged to be good when the impact value was 80J or more. The results of the tensile test and Charpy impact test are shown in Table 3.
[0060] [Table 3]
[0061] [Table 4]
[0062] [Table 5]
[0063] [Table 6]
[0064] [Table 7]
[0065] The weld metals and weld joints of Inventive Examples 1 to 6 were within the range of the present invention, and therefore exhibited a tensile strength of 980 MPa or more and a Charpy impact test value of 80 J or more. In Comparative Example 1, the weld metal contained a small amount of Ti. Therefore, the Ti concentration in the oxide was outside the range of the present invention, and the oxide did not effectively serve as a nucleus for intragranular transformation, resulting in coarsening of the microstructure. As a result, the toughness of the weld metal and welded joint was insufficient. In Comparative Example 2, the welding heat input was excessively high, the cooling rate of the weld metal was slow, and the oxide number density was low. In other words, the number of intragranular transformation nuclei was reduced, and the effect of refining the microstructure was not sufficient, so the toughness of the weld metal and welded joint was insufficient. In Comparative Example 3, the welding heat input was excessively low, the cooling rate of the weld metal was fast, and the average equivalent circular diameter of the oxides was small. In other words, the number of oxides large enough to contribute as intragranular transformation nuclei was reduced, and the effect of refining the microstructure was not sufficient, so the toughness of the weld metal and welded joint was insufficient. In Comparative Example 4, the welding heat input was excessively high, the cooling rate of the weld metal was slow, and the average circle equivalent diameter of the oxides was large. In other words, the number of coarse inclusions that could be the starting points of fracture was increased, and the toughness of the weld metal and welded joint was insufficient. [Industrial Applicability]
[0066] As described above, according to the present invention, it is possible to provide a weld metal and a weld joint having high strength and excellent toughness, and thus the present invention has high industrial applicability.
Claims
1. The chemical composition, in mass%, is C: 0.02-0.12%, Si: 0.10-0.70%, Mn: 0.5-2.0%, P: 0.03% or less, S: 0.02% or less, N: 0.03% or less, Ni: 1.0 to 3.5%, Cr: more than 0% and 1.0% or less; Mo: 0.3-2.0%, Ti: more than 0.005% and not more than 0.500%, and O: 0.005 to 0.040%; The balance is Fe and impurities, The average chemical composition of the oxide having an equivalent circle diameter of 0.10 μm or more includes Mn: 10 to 70 mass%, Ti: 10 to 50 mass%, Si: 0 to 20 mass%, and Al: 5 mass% or less, In the average chemical composition, the total amount of Mn, Ti, and Si is 60 mass% or more, the average equivalent circular diameter of the oxide having an equivalent circular diameter of 0.10 μm or more is 0.30 to 1.00 μm; The number density of the oxides having a circle equivalent diameter of 0.10 μm or more is 0.005 to 0.05 / μm 2 and A weld metal, characterized in that α defined by the following formula (1) is 0.40% or more and 0.80% or less. α=[C]+[Si] / 24+[Mn] / 6+[Ni] / 40+[Cr] / 5+[Mo] / 4...(1) In the formula (1), the elements in brackets [ ] indicate the content of each element in the chemical composition of the weld metal, expressed as mass %, and 0 is substituted for elements that are not contained.
2. The chemical composition of the weld metal further contains, in mass %, Al: 0.010% or less, Cu: 0.200% or less, Nb: 0.100% or less, V: 0.100% or less, and B: 0.0020% or less, Contains one or more of the following:
2. The weld metal according to claim 1, characterized in that, when the weld metal contains V, α defined by the following formula (2) is 0.40% or more and 0.80% or less, instead of the α defined by the formula (1): α=[C]+[Si] / 24+[Mn] / 6+[Ni] / 40+[Cr] / 5+[Mo] / 4+[V] / 14...(2) In the formula (2), the elements in brackets [ ] indicate the content of each element in the chemical composition of the weld metal, expressed as mass %, and 0 is substituted for elements that are not contained.
3. A welded joint comprising the weld metal according to claim 1 or 2.
Citation Information
Patent Citations
Flux-cored wire for gas shield arc welding, and weld metal
JP2018039025A
Flux-containing wire
JP2019089131A
Weld metal having excellent sensitivity to hydrogen embrittlement resistance
WO2012105617A1
High strength welded metal
WO2018043455A1