Tablet-shaped epoxy resin composition for sealing semiconductor elements and semiconductor device sealed using the same

The tablet-shaped epoxy resin composition with optimized size and filler content addresses thermal conductivity and contamination issues in semiconductor devices, improving heat dissipation and reducing defects in compression molding.

JP7564618B2Active Publication Date: 2024-10-09SAMSUNG SDI CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2019230681
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-20
Filing Date
2019-12-20
Publication Date
2024-10-09
Estimated Expiration
2039-12-20

AI Technical Summary

Technical Problem

Existing epoxy resin compositions for sealing semiconductor devices in compression molding face challenges such as reduced thermal conductivity, equipment contamination, and wire sweep, especially in high-density and thin semiconductor packages, which are exacerbated by the use of heat sinks that increase costs and reduce productivity.

Method used

A tablet-shaped epoxy resin composition with specific size, density, and composition ratios, including inorganic fillers like alumina and silica, is used to enhance thermal conductivity, prevent scattering, and reduce wire sweep during compression molding.

Benefits of technology

The composition achieves high thermal conductivity, minimizes equipment contamination, and significantly reduces wire sweep, enhancing heat dissipation and reducing package malfunctions and cracks due to heat generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564618000009
    Figure 0007564618000009
  • Figure 0007564618000010
    Figure 0007564618000010
  • Figure 0007564618000011
    Figure 0007564618000011
Patent Text Reader

Abstract

To provide a highly thermally conductive tableted epoxy resin composition for encapsulation of semiconductor devices.SOLUTION: A tableted epoxy resin composition for encapsulation of semiconductor devices satisfies the following conditions: (i) a proportion of the tablets having a diameter greater than or equal to 0.1 mm and less than 2.8 mm and a height greater than or equal to 0.1 mm and less than 2.8 mm is 97 wt.% or more, as measured by flour sieves using ASTM standard sieves; (ii) the tablets have a packed density greater than 1.7 g / mL; and (iii) the ratio of the packed density to the cured density of the tablets is from 0.6 to 0.87 inclusive.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a tablet-shaped epoxy resin composition for sealing semiconductor elements and a semiconductor device sealed with the same. [Background technology]

[0002] In recent years, as the electronic device market has shifted to mobile devices such as smartphones and tablet PCs, technological development of electronic devices has also focused on mobile devices that are smaller, lighter, and have high performance. Accordingly, thinner and more highly integrated semiconductor devices are being developed to realize mobile devices that meet the trends of high stacking, high performance, high density, multi-function, and slimness. When such highly stacked and highly dense semiconductor devices are sealed in small and thin semiconductor packages, the heat generated during operation of the semiconductor device can cause the package to malfunction and crack more frequently. To solve this problem, heat sinks are used, but heat sinks are only possible in some packages and have the disadvantages of reduced productivity and high costs due to additional processes. Therefore, there is a demand for epoxy resin compositions for sealing semiconductor devices that can increase thermal conductivity.

[0003] Meanwhile, in response to this trend, a method of encapsulating semiconductor devices by compression molding is under development. Compression molding is a molding method that has been attracting attention in recent years because it can suppress the generation of voids even when semiconductor devices are stacked in a multi-stack by compressing the material in a mold. During compression molding, an epoxy resin composition for encapsulating semiconductor devices may be poured into a mold in the form of a film or sheet, but is currently poured in the form of powder or granules, taking into consideration the moldability and mobility of the composition. However, the powder or granules have only a certain degree of size distribution, which causes problems such as wire sweep and / or package warpage.

[0004] Conventional methods for producing epoxy resin compositions for compression molding of semiconductor devices include centrifugal milling and hot cut methods. However, these methods for compression molding of semiconductor devices require high thermal conductivity, making it difficult to produce the epoxy resin composition. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6616201 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a tablet-shaped epoxy resin composition having high thermal conductivity for sealing semiconductor elements.

[0007] Another object of the present invention is to provide a tablet-shaped epoxy resin composition for sealing semiconductor devices, which can prevent the composition from sticking and / or scattering in compression molding equipment and reduce equipment contamination when sealing semiconductor devices by compression molding.

[0008] It is still another object of the present invention to provide a tablet-shaped epoxy resin composition for sealing semiconductor elements, which can significantly reduce wire sweep when sealing semiconductor elements by compression molding. [Means for solving the problem]

[0009] The present invention provides a tablet-shaped epoxy resin composition for sealing semiconductor elements.

[0010] In a first specific example, with respect to the entire tablet-shaped epoxy resin composition for sealing semiconductor elements, (i) the ratio of tablets having a diameter of 0.1 mm or more and less than 2.8 mm and a height of 0.1 mm or more and less than 2.8 mm when measured by powder sieving using ASTM standard sieves is 97% by weight or more, (ii) the tablets have a compressed density of more than 1.7 g / mL, and (iii) the ratio of the compressed density to the cured density of the tablets is 0.6 or more and 0.87 or less.

[0011] In a second embodiment, in the first embodiment, the tablet may have a cylindrical shape.

[0012] In a third specific example, in the first or second specific example, the tablet-shaped epoxy resin composition for sealing semiconductor elements may contain an inorganic filler including one or more of silica, alumina, aluminum nitride, calcium carbonate, magnesium carbonate, magnesia, clay, talc, calcium silicate, titanium oxide, antimony oxide, glass fiber, and boron nitride.

[0013] In a fourth specific example, in the third specific example, the inorganic filler may be contained in an amount of 70% by weight to 99% by weight of the tablet-shaped epoxy resin composition for sealing semiconductor elements.

[0014] In a fifth embodiment, in the third or fourth embodiment, the silica may be contained in an amount of 90% by weight or less of the inorganic filler.

[0015] In a sixth specific example, in any one of the third to fifth specific examples, the aluminum nitride may be contained in an amount of 50% by weight or less of the inorganic filler.

[0016] In a seventh specific example, in any one of the third to sixth specific examples, the inorganic filler may have an average particle size (D50) of 3 μm to 15 μm.

[0017] In an eighth specific example, in any one of the third to seventh specific examples, the alumina may be contained in an amount of 10% by weight to 100% by weight of the inorganic filler.

[0018] In a ninth specific example, in any one of the third to eighth specific examples, the alumina may be contained in an amount of 75% by weight to 98% by weight in the tablet-shaped epoxy resin composition for sealing a semiconductor element.

[0019] In a tenth specific example, in any one of the third to ninth specific examples, the tablet-shaped epoxy resin composition for sealing a semiconductor element may contain a mixture of alumina and silica as the inorganic filler.

[0020] In an eleventh specific example, in the tenth specific example, the mixture of alumina and silica may be contained in an amount of 75% by weight to 98% by weight in the tablet-shaped epoxy resin composition for sealing semiconductor elements.

[0021] In a twelfth specific example, in any one of the third to eleventh specific examples, the tablet-shaped epoxy resin composition for sealing a semiconductor element may contain a mixture of silica and aluminum nitride as the inorganic filler.

[0022] In a thirteenth specific example, in the twelfth specific example, the mixture of silica and aluminum nitride may be contained in an amount of 75% by weight to 98% by weight in the tablet-shaped epoxy resin composition for sealing semiconductor elements.

[0023] In a fourteenth specific example, in any one of the first to thirteenth specific examples, the cured density may be 1.9 g / mL to 4 g / mL.

[0024] In a fifteenth specific example, in any one of the first to fourteenth specific examples, the tablet-shaped epoxy resin composition for sealing a semiconductor element may be produced by tablet compression molding.

[0025] The semiconductor device of the present invention is sealed using the tablet-shaped epoxy resin composition for sealing semiconductor elements of the present invention. Effect of the Invention

[0026] The present invention provides a tablet-shaped epoxy resin composition having high thermal conductivity for sealing semiconductor elements.

[0027] The present invention provides a tablet-shaped epoxy resin composition for sealing semiconductor devices, which can prevent the composition from sticking and / or scattering in compression molding equipment when sealing semiconductor devices by compression molding, thereby reducing equipment contamination.

[0028] The present invention provides a tablet-shaped epoxy resin composition for sealing semiconductor elements, which can significantly reduce wire sweep when sealing semiconductor elements by compression molding. [Brief description of the drawings]

[0029] [Figure 1] FIG. 2 is a diagram illustrating the shape of a tablet and the diameter and height of the tablet in question in the present invention. [Diagram 2] 1A to 1C are diagrams illustrating an example of a method for sealing a semiconductor element by compression molding. [Diagram 3] 1A and 1B are diagrams illustrating an example of a semiconductor device sealed by compression molding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] The present invention will now be described in detail with reference to the accompanying drawings, by way of embodiments and examples, so that those skilled in the art can easily carry out the present invention. The present invention may be embodied in various different forms, and is not limited to the embodiments and examples set forth herein.

[0031] In this specification, the term "tablet" refers to a shape that is composed of a first surface, a second surface, and a side surface that connects the first surface and the second surface, and the first surface and the second surface are opposed to each other. In one embodiment, the first surface and the second surface may each be a flat surface, and the side surface may be a curved surface. In one specific example, the tablet may be a cylinder. Referring to FIG. 1, the tablet may be a cylinder, and the cylinder may have a diameter (D) at the first surface (or the second surface) and a height (H) at the side surface. In the present invention, the term "tablet" may include not only a case where the diameter (D) is equal to or smaller than the height (H), but also a case where the diameter (D) is greater than the height (H).

[0032] As used herein, the "aspect ratio" of a tablet may be the ratio of the height (H) to the diameter (D) (height (H) / diameter (D)).

[0033] In this specification, "a tablet-shaped epoxy resin composition for sealing a semiconductor element" may mean a composition in which 98% by weight or more, for example, 99% by weight or more of the epoxy resin composition for sealing a semiconductor element is in the form of tablets.

[0034] In this specification, "compressed density" is a value measured for tablets that belong to a powder sieve of 0.1 mm or more and less than 2.8 mm when sieved using an ASTM standard sieve. A sample is obtained by weighing a portion of the tablets that belong to a powder sieve of 0.1 mm or more and less than 2.8 mm, and the weight (W) is measured using an electronic balance. A 50 ml graduated cylinder is half-filled with water, a silicone surfactant is added, and the exact volume (V1) is measured. The tablets whose weight has been measured are placed in the graduated cylinder, and the changed volume (V2) is accurately measured. The compressed density (unit: g / mL) is calculated according to the following formula 1. At this time, the graduated cylinder is shaken to remove the air between the tablets, and the volume is measured, and the compressed density can be calculated as the average value after five measurements.

[0035]

number

[0036] In this specification, the "cured density" can be calculated as the ratio of mass to volume (mass / volume, g / mL) by molding an epoxy resin composition for sealing semiconductor elements into a disk of 50 mm in diameter and 3 mm in thickness using a transfer molding machine at a mold temperature of 175±5°C, injection pressure of 7 MPa, and curing time of 120 seconds, and then determining the mass and volume after a post mold curing (PMC) process at 175°C for 4 hours.

[0037] In this specification, the "thermal conductivity" is a value measured at 25°C according to ASTM D5470 on a test piece formed from an epoxy resin composition for sealing semiconductor elements.

[0038] In this specification, when describing a numerical range, "X to Y" means X or more and Y or less.

[0039] The tablet-shaped epoxy resin composition for sealing semiconductor elements according to an embodiment of the present invention satisfies all of the following (i), (ii) and (iii). By satisfying all of (i), (ii) and (iii), it is possible to reduce the possibility of contamination of equipment such as a vibrating feeder due to scattering of fine powder during compression molding of a semiconductor element, to significantly reduce wire sweep, and to significantly increase thermal conductivity. In one embodiment, the tablet-shaped epoxy resin composition for sealing semiconductor elements according to the present invention may have a thermal conductivity of 2 W / mK or more, for example, 2 W / mK to 10 W / mK, for example, 2 W / mK to 7.5 W / mK. Within this range, the heat dissipation effect during sealing of a semiconductor element is improved, and the frequency of package malfunction and crack occurrence due to heat generated during operation can be reduced.

[0040] In particular, the inventors of the present invention have confirmed that even if an epoxy resin composition for encapsulating semiconductor devices contains the same type and amount of inorganic filler, if it does not satisfy one or more of the following (i), (ii) and (iii), it will be impossible to obtain all of the effects of improving thermal conductivity, reducing wire sweep and reducing the possibility of equipment contamination due to scattering of fine powder.

[0041] (i) The proportion of tablets having a diameter of 0.1 mm or more but less than 2.8 mm and a height of 0.1 mm or more but less than 2.8 mm is 97% or more by weight, as measured by powder sieving using ASTM standard sieves.

[0042] (ii) the tablet has a compressed density of greater than 1.7 g / mL;

[0043] (iii) The tablet has a ratio of compressed density to hardened density (compressed density / hardened density) of 0.6 or greater and 0.87 or less.

[0044] The tablet-shaped epoxy resin composition for sealing semiconductor devices of the present invention has a ratio of tablets having a diameter of 0.1 mm or more and less than 2.8 mm and a height of 0.1 mm or more and less than 2.8 mm, when measured by powder sieving using ASTM standard sieves, of 97% by weight or more of the total tablet-shaped epoxy resin composition. If the tablets having a diameter or height of less than 0.1 mm exceed 3% by weight, the content of fine powder increases, and the fine powder may adhere to the compression molding equipment, causing contamination. If the tablets having a diameter or height of 2.8 mm or more exceed 3% by weight, the tablet-shaped epoxy resin composition for sealing semiconductor devices may crumble during transportation, causing contamination of the compression molding equipment. In addition, the tablet-shaped composition may have an uneven shape, which may cause errors when measuring tablets in the compression molding equipment, which may cause differences in thickness of semiconductor packages and defects due to deviations in warpage. In one specific example, the ratio of tablets having a diameter of 0.1 mm or more and less than 2.8 mm and a height of 0.1 mm or more and less than 2.8 mm may be 97% by weight to 99% by weight of the entire tablet-shaped epoxy resin composition.

[0045] According to powder sieving using ASTM standard sieves, 0.1 mm corresponds to ASTM mesh No. 140, and 2.8 mm corresponds to ASTM mesh No. 7.

[0046] The tablet-shaped epoxy resin composition for sealing semiconductor elements of the present invention has a compressed density of more than 1.7 g / mL. If the compressed density is 1.7 g / mL or less, the thermal conductivity is low, and as a result, the heat dissipation effect is low when sealing a semiconductor element, and the frequency of package malfunction and crack occurrence due to heat generated during operation may increase. The method for measuring the compressed density is as described above. The compressed density may be preferably more than 1.7 g / mL and less than 3.2 g / mL, more preferably 1.71 g / mL to 3.2 g / mL, and most preferably 1.71 g / mL to 3 g / mL.

[0047] The tablet-shaped epoxy resin composition for sealing semiconductor elements of the present invention has a density ratio between the compressed density and the cured density (ratio of the compressed density to the cured density) of 0.6 to 0.87. If the density ratio is less than 0.6, the melting property and compatibility during compression molding may be poor. If the density ratio exceeds 0.87, the thermal conductivity improvement effect may be weak and wire sweep may be large.

[0048] In one embodiment, the cured density may be 1.9 g / mL to 4 g / mL, preferably 1.95 g / mL to 3.5 g / mL, and more preferably 1.95 g / mL to 3.2 g / mL. In the above range, the melting property and compatibility during compression molding are good, and the occurrence of wire sweep and voids can be reduced. The method for measuring the cured density is as described above.

[0049] The tablet-shaped epoxy resin composition for sealing semiconductor elements of the present invention may have an aspect ratio of 0.1 to 5, preferably 0.25 to 4. Within the above range, there may be an additional effect of reducing the thickness deviation of the semiconductor package and reducing the warpage deviation.

[0050] The tablet-shaped epoxy resin composition for sealing semiconductor elements of the present invention may be cylindrical in shape.

[0051] The tablet-shaped epoxy resin composition for sealing semiconductor elements of the present invention described above can be produced by the tablet compression molding method described below. The tablet compression molding method may use a tablet compression molding device. For example, the epoxy resin composition for sealing semiconductor elements is melted and kneaded at 90°C to 110°C using a continuous kneader, and then cooled and pulverized to produce a powdered composition. The produced powdered preliminary composition is fed into a tablet press equipment feeder, and the powdered composition in the die is compressed by lowering the upper punch, and then the tablet-shaped composition is produced by raising and lowering the upper punch. The epoxy resin composition for sealing semiconductor elements can be produced by adjusting the compression load applied to the composition by lowering the upper punch and raising and lowering the lower punch, the diameter and height of the die, etc.

[0052] In one embodiment, the compression load may vary depending on the diameter of the die, the height of the die, the height and diameter of the composition injected into the die, etc., and may be 0.1 to 1 ton. In one embodiment, the diameter of the die may be 0.1 mm or more and less than 2.8 mm, and the height of the die may be 0.1 mm or more and less than 2.8 mm.

[0053] Meanwhile, a conventional centrifugal milling method is known as a method for molding epoxy resin compositions for semiconductor element encapsulation. In the case of centrifugal milling, even if the composition passes through a uniform punched iron screen by the centrifugal force of the rotor, it is molded in a molten and mixed state, so melting does not occur reliably during compression and molding, which can result in wire sweep defects. In addition, deviations in the size of granules can cause package warpage problems.

[0054] In addition, a conventional hot cut method is known as another method for molding an epoxy resin composition for sealing semiconductor devices. In the hot cut method, an epoxy resin composition in a molten and kneaded state is cut to produce the composition, so melting is not performed reliably during compression molding, which can result in wire sweep defects.

[0055] The components of the tablet-form epoxy resin composition for sealing semiconductor elements of the present invention will be described below.

[0056] The tablet-shaped epoxy resin composition for sealing semiconductor elements of the present invention may contain an epoxy resin, a curing agent, a curing catalyst, and an inorganic filler.

[0057] The epoxy resin may be a mixture of monomers, oligomers, polymers, etc. having two or more epoxy groups in one molecule. For example, the epoxy resin may be a bisphenol type epoxy resin such as a bisphenol A type epoxy resin or a bisphenol F type epoxy resin, a phenol novolac type epoxy resin, a tert-butylcatechol type epoxy resin, a naphthalene type epoxy resin, a glycidylamine type epoxy resin, a phenol aralkyl type epoxy resin, a cresol novolac type epoxy resin, a biphenyl type epoxy resin, a linear aliphatic epoxy resin, an alicyclic epoxy resin, a heterocyclic epoxy resin, a spiro ring-containing epoxy resin, a cyclohexane dimethanol type epoxy resin, a halogenated epoxy resin, a biphenyl type novolac epoxy resin, etc., which may be included alone or in a mixture of two or more.

[0058] The curing agent is not particularly limited as long as it can cure the epoxy resin. Examples of the curing agent include phenol aralkyl type phenolic resin, phenol novolac type phenolic resin, biphenyl type novolac phenolic resin, Xylok type phenolic resin, cresol novolac type phenolic resin, naphthol type phenolic resin, terpene type phenolic resin, polyfunctional phenolic resin, dicyclopentadiene type phenolic resin, novolac type phenolic resin synthesized from bisphenol A and resol, polyhydric phenolic compounds including tris(hydroxyphenyl)methane and dihydroxybiphenyl, acid anhydrides including maleic anhydride and phthalic anhydride, and aromatic amines such as meta-phenylenediamine, diaminodiphenylmethane, and diaminodiphenylsulfone.

[0059] Any curing catalyst can be used without limitation as long as it can accelerate the curing reaction between the epoxy group of the epoxy resin and the curing agent. For example, tertiary amines, organometallic compounds, organophosphorus compounds, imidazoles, and boron compounds can be used as curing catalysts. Tertiary amines include benzyldimethylamine, triethanolamine, triethylenediamine, diethylaminoethanol, tri(dimethylaminomethyl)phenol, 2-2-(dimethylaminomethyl)phenol, 2,4,6-tris(diaminomethyl)phenol, and tri-2-ethylhexyl salt. Organometallic compounds include chromium acetylacetonate, zinc acetylacetonate, and nickel acetylacetonate. Organophosphorus compounds include tris(4-methoxyphenyl)phosphine, triphenylphosphine, triphenylborane, and triphenylphosphine-1,4-benzoquinone adduct. Imidazoles include 2-methylimidazole, 2-phenylimidazole, 2-aminoimidazole, 2-methyl-1-vinylimidazole, 2-ethyl-4-methylimidazole, and 2-heptadecylimidazole. Boron compounds include triphenylphosphine tetraphenylborate, tetraphenylborate, trifluoroborane-n-hexylamine, trifluoroborane monoethylamine, tetrafluoroborane triethylamine, and tetrafluoroborane amine. Other usable compounds include 1,5-diazabicyclo[4.3.0]non-5-ene (DBN), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), and phenol novolac resin salt. As the curing catalyst, it is also possible to use an adduct made by pre-reaction with the epoxy resin or the curing agent.

[0060] As the inorganic filler, inorganic fillers that are commonly used in epoxy resin compositions for sealing semiconductor elements may be used.

[0061] In one embodiment, the inorganic filler may include one or more of silica, alumina, aluminum nitride, calcium carbonate, magnesium carbonate, magnesia, clay, talc, calcium silicate, titanium oxide, antimony oxide, glass fiber, and boron nitride. Preferably, the inorganic filler includes alumina to increase the thermal conductivity of the epoxy resin composition for sealing semiconductor elements. The inorganic filler may be included alone or in combination with two or more kinds. When two or more kinds of inorganic fillers are included, the inorganic fillers may have the same or different average particle diameters (D50). Preferably, when two or more kinds of inorganic fillers are included, the inorganic fillers may have different average particle diameters (D50).

[0062] In one embodiment, only alumina may be used as the inorganic filler. Specifically, alumina may be contained in the tablet-shaped epoxy resin composition for sealing semiconductor elements in an amount of 70% by weight to 99% by weight, preferably 75% by weight to 98% by weight. In the above range, the thermal conductivity of the epoxy resin composition for sealing semiconductor elements is improved, and the effects of the present invention can be obtained.

[0063] In another embodiment, a mixture of alumina and silica may be used as the inorganic filler. Specifically, the mixture of alumina and silica may be contained in the tablet-shaped epoxy resin composition for sealing semiconductor elements in an amount of 70% by weight to 99% by weight, preferably 75% by weight to 98% by weight. In the above range, the thermal conductivity of the epoxy resin composition for sealing semiconductor elements is improved while the effects of the present invention can be obtained.

[0064] In still another embodiment, a mixture of alumina and aluminum nitride may be used as the inorganic filler. Specifically, the mixture of alumina and aluminum nitride may be contained in an amount of 70% by weight to 99% by weight, preferably 75% by weight to 98% by weight, of the tablet-shaped epoxy resin composition for sealing semiconductor elements.

[0065] In still another embodiment, a mixture of silica and aluminum nitride may be used as the inorganic filler. Specifically, the mixture of silica and aluminum nitride may be contained in the tablet-shaped epoxy resin composition for sealing semiconductor elements in an amount of 70% by weight to 99% by weight, preferably 75% by weight to 98% by weight. In the above range, the thermal conductivity of the epoxy resin composition for sealing semiconductor elements is improved while the effects of the present invention can be obtained.

[0066] In one embodiment, the content of alumina in the inorganic filler may be 10% by weight or more, preferably 10% by weight to 100% by weight of the inorganic filler. Within this range, the thermal conductivity of the epoxy resin composition for sealing semiconductor elements can be improved while the effects of the present invention can be obtained.

[0067] In one embodiment, the content of silica in the inorganic filler may be 90% by weight or less, preferably 10% to 90% by weight, of the inorganic filler. Within this range, the thermal conductivity of the epoxy resin composition for sealing semiconductor elements can be improved while the effects of the present invention can be obtained.

[0068] In one embodiment, the content of aluminum nitride in the inorganic filler may be 50% by weight or less, preferably 30% by weight or less, and more preferably 5% to 30% by weight of the inorganic filler. Within this range, the thermal conductivity of the epoxy resin composition for sealing semiconductor elements can be improved while the effects of the present invention can be obtained.

[0069] The inorganic filler may have an average particle size (D50) of 3 μm to 15 μm, preferably 5 μm to 15 μm, and more preferably 5 μm to 12 μm. In this range, the flowability of the epoxy resin composition may be good. The "average particle size" refers to the usual particle size D50 known to those skilled in the art, and means the particle size of the inorganic filler that corresponds to 50% by weight when the inorganic filler is distributed on a weight basis.

[0070] The epoxy resin composition for sealing semiconductor elements may further contain a common additive in addition to the above-mentioned components. In a specific example, the additive may include one or more of a coupling agent, a release agent, a stress relaxation agent, a crosslinking promoter, a leveling agent, and a colorant. The coupling agent may be one or more selected from the group consisting of epoxy silane, amino silane, mercapto silane, alkyl silane, and alkoxy silane, but is not limited thereto. The release agent may be one or more selected from the group consisting of paraffin wax, ester wax, higher fatty acid, higher fatty acid metal salt, natural fatty acid, and natural fatty acid metal salt. The stress relaxation agent may be one or more selected from the group consisting of modified silicone oil, silicone elastomer, silicone powder, and silicone resin, but is not limited thereto. The colorant may be carbon black or the like.

[0071] The epoxy resin composition for sealing semiconductor elements may contain 0.5 wt % to 20 wt %, specifically 3 wt % to 15 wt %, epoxy resin, 0.1 wt % to 13 wt %, specifically 0.1 wt % to 10 wt %, curing agent, 70 wt % to 99 wt %, for example, 75 wt % to 98 wt %, inorganic filler, 0.01 wt % to 2 wt %, specifically 0.02 wt % to 1.5 wt %, and various additives, each of which may be contained in an amount of 0.1 wt % to 10 wt %.

[0072] The semiconductor element of the present invention can be encapsulated by compression molding using the tablet-shaped epoxy resin composition for encapsulating semiconductor elements of the present invention. The semiconductor element may include an integrated circuit, a transistor, a thyristor, a diode, a solid-state imaging element, etc.

[0073] Hereinafter, a method for sealing an epoxy resin composition for sealing a semiconductor element by compression molding will be described with reference to FIG. 2. Referring to FIG. 2, in (a), an epoxy resin composition for sealing a semiconductor element 1 is fed into a composition supply container 3 by a vibration feeder 2. The vibration feeder 2 vibrates at a constant or variable feed speed, thereby allowing a predetermined amount of an epoxy resin composition for sealing a semiconductor element to be fed into the composition supply container 3 at a constant speed. In (b), a shutter 4 or other means is attached to the composition supply container 3, and by moving the shutter 4 or the like, the epoxy resin composition for sealing a semiconductor element 1 in the composition supply container 3 can be instantly fed into the lower molding cavity 5. An upper substrate 7 on which a semiconductor element 6 and the like are mounted on the lower molding cavity 5 and a lower substrate 8 on which the lower molding cavity 5 is formed are compressed against each other. At this time, the composition supply container 3 moves toward a side that does not interfere with the compression of the upper substrate 7 and the lower substrate 8. In addition, the lower substrate 7 rises, thereby compressing the upper substrate 7 and the lower substrate 8. The epoxy resin composition 1 for sealing semiconductor elements introduced into the lower molding cavity 5 is melted by the heater 9 embedded in the lower substrate 8, and as the upper substrate 7 on which the semiconductor elements 6 and other components are mounted is lowered, the semiconductor elements and other components are gradually dipped into the molten material, completing the compression molding.

[0074] Fig. 3 illustrates an example of a semiconductor device sealed by compression molding. Referring to Fig. 3, a semiconductor element 101 is sealed with a sealant 102 formed from an epoxy resin composition for sealing semiconductor elements. The semiconductor element 101 is fixed on a die pad 103 with a die bonding material 104. An electrode pad of the semiconductor element 101 and a lead frame 105 are connected with a wire 106. The semiconductor device of the present invention is sealed with a sealant formed from the epoxy resin composition for sealing semiconductor elements of the present invention, and thus the deviation in thickness (T) of the semiconductor package is small, and thus the deviation in warpage is low. EXAMPLES

[0075] Hereinafter, the configuration and operation of the present invention will be described in more detail through preferred embodiments of the present invention. However, the following examples are provided to facilitate understanding of the present invention, and the scope of the present invention is not limited to the following examples.

[0076] Example 1 The epoxy resins used were 7.01% by weight of phenol aralkyl type epoxy resin NC-3000 (manufactured by Nippon Kayaku Co., Ltd.) and 5.73% by weight of biphenyl type epoxy resin YX-4000 (manufactured by Japan Epoxy Resins Co., Ltd.); the curing agents used were 4.32% by weight of phenol novolac resin DL-92 (manufactured by Meiwa Kasei Co., Ltd.) and 1.08% by weight of phenol aralkyl type phenol resin MEH-7851S (manufactured by Meiwa Kasei Co., Ltd.); the curing catalyst used was triphenylphosphine ( A master batch composition was prepared by mixing 0.89 wt% of 10 wt% alumina and 70 wt% silica as an inorganic filler, 0.3 wt% epoxy silane KBM-303 (Shin-Etsu Chemical Co., Ltd.) and 0.2 wt% amino silane KBM-573 (Shin-Etsu Chemical Co., Ltd.) as coupling agents, 0.37 wt% carbon black MA-600B (Mitsubishi Chemical Co., Ltd.) as a colorant, and 0.1 wt% carnauba wax as a mold release agent using a Henschel mixer (KEUM SUNG MACHINERY CO., LTD (KSM-22)). In this case, "wt%" indicates the content of each component in the epoxy resin composition for sealing semiconductor elements.

[0077] The prepared composition was melted and kneaded at 90°C to 110°C using a continuous kneader, and then cooled and pulverized to prepare a powdered composition. The prepared powdered preliminary composition was made into a tablet-shaped epoxy resin composition for sealing semiconductor elements using a tablet compression molding machine.

[0078] Specifically, the powdered composition prepared above was fed into a tablet press feeder, and the powdered composition in the die was compressed by lowering the upper punch, and then the upper punch was raised and lowered to prepare a tableted composition. The compression load applied to the composition by lowering the upper punch and raising and lowering the lower punch was 0.6 tons. In addition, by adjusting the diameter and height of the die, tableted epoxy resin compositions for sealing semiconductor devices having the physical properties shown in Table 4 below were prepared.

[0079] (Examples 2 to 9) An epoxy resin composition for encapsulating a semiconductor device was prepared in the same manner as in Example 1, except that the content of each component in the epoxy resin composition for encapsulating a semiconductor device was changed as shown in Table 1 below.

[0080] The epoxy resin composition for encapsulating semiconductor devices thus prepared was subjected to tablet compression molding by adjusting the compression load, die diameter, and / or die height, and as a result, tablet-shaped epoxy resin compositions for encapsulating semiconductor devices having the physical properties shown in Table 4 below were prepared.

[0081] (Comparative Example 1 to Comparative Example 12) An epoxy resin composition for encapsulating a semiconductor device was prepared in the same manner as in Example 1, except that the content of each component in the epoxy resin composition for encapsulating a semiconductor device was changed as shown in Tables 2 and 3 below.

[0082] The epoxy resin composition for sealing semiconductor elements thus prepared was subjected to tablet compression molding by adjusting the compression load, die diameter, and / or die height, thereby preparing tablet-shaped epoxy resin compositions for sealing semiconductor elements having the physical properties shown in Tables 5 and 6 below. In Comparative Example 8, tablets could not be produced during tablet compression molding.

[0083] Comparative Example 13 An epoxy resin composition for encapsulating a semiconductor device was prepared in the same manner as in Example 1, except that the content of each component in the epoxy resin composition for encapsulating a semiconductor device was changed as shown in Table 3 below.

[0084] A punched iron net with small holes of 2.5 mm diameter was used as the material for the cylindrical outer periphery. A punched iron net with a height of 25 mm and a thickness of 1.5 mm was placed on the outer periphery of a rotor with a diameter of 20 cm to form the cylindrical outer periphery. The rotor was rotated at 3000 RPM, and the cylindrical outer periphery was heated to 115°C by an excitation coil. After the rotor rotation speed and the temperature of the cylindrical outer periphery became normal, the master batch was melted and kneaded by a twin-screw extruder while being degassed by a degassing device, and the melt obtained was supplied to the inside of the rotor at a rate of 2 kg / hr through a double-tube cylinder above the rotor, and passed through multiple small holes in the cylindrical outer periphery by centrifugal force obtained by rotating the rotor, thereby obtaining a resin composition having the physical properties shown in Table 6 below by a centrifugal milling method. The kneading temperature of the twin-screw extruder was 90°C to 110°C.

[0085] (Comparative Examples 14 to 16) An epoxy resin composition for encapsulating a semiconductor device was prepared in the same manner as in Example 1, except that the content of each component in the epoxy resin composition for encapsulating a semiconductor device was changed as shown in Table 3 below.

[0086] The epoxy resin compositions for sealing semiconductor elements thus produced were subjected to the same centrifugal milling as in Comparative Example 13. When centrifugal milling was performed on the epoxy resin compositions for sealing semiconductor elements in Comparative Examples 14 to 16, production was impossible.

[0087] [Table 1]

[0088] [Table 2]

[0089] [Table 3]

[0090] In Tables 1 to 3, Epoxy resin 1 is a phenol aralkyl type epoxy resin. Epoxy resin 2 is a biphenyl type epoxy resin. Hardener 1 is a phenol novolac type resin. Hardener 2 is a phenol aralkyl type phenolic resin. The curing catalyst is triphenylphosphine. The alumina has an average particle size (D50) of 9 μm. The silica has an average particle size (D50) of 8 μm. The aluminum nitride has an average grain size (D50) of 3 μm. Coupling agent 1 is an epoxy silane, Coupling agent 2 is an aminosilane.

[0091] The epoxy resin compositions for sealing semiconductor elements molded in the Examples and Comparative Examples were evaluated for the following physical properties, and the results are shown in Tables 4, 5, and 6 below.

[0092] (1) Tablet size of the epoxy resin composition for sealing semiconductor devices prepared: Using ASTM standard MESH, a vibrating sieve was used with sieve meshes of 0.1 mm [ASTM No 140] and 2.8 mm [ASTM No 7], and the sample was vibrated at 100 hammer strokes per minute for 10 minutes to pass through a powder sieve. The weight of the tablets filtered through the powder sieve of 0.1 mm or more and less than 2.8 mm, and the weight of the tablets filtered through the powder sieve of less than 0.1 mm and 2.8 mm or more were measured, and the content (%) of the tablets of the epoxy resin composition for sealing semiconductor devices corresponding to 0.1 mm or more and less than 2.8 mm was measured.

[0093] (2) Compressed density: When sieved using an ASTM standard sieve, it was measured for those filtered through a powder sieve of 0.1 mm or more and less than 2.8 mm. Specifically, a sample was obtained by weighing a portion of the powder sieve of 0.1 mm or more and less than 2.8 mm, and the weight (W) was measured using an electronic balance. A 50 ml graduated cylinder was half-filled with water, 0.1 g of a silicone surfactant (product name: BYK-378, manufacturer: BYK) was added, and the exact volume (V1) was measured. The tablets whose weights were measured were placed in the graduated cylinder, and the changed volume (V2) was accurately measured. At this time, the density of the tablets was calculated as the compressed density (unit: g / mL) according to the following formula 1. At this time, the cylinder was shaken to remove the air between the tablets, and then the volume was measured, and the compressed density can be calculated as the average value after five measurements.

[0094]

number

[0095] (3) Cured density: The epoxy resin composition for sealing semiconductor elements was molded into a disk of 50 mm in diameter and 3 mm in thickness using a transfer molding machine at a mold temperature of 175±5°C, injection pressure of 7 MPa, and curing time of 120 seconds. The PMC (post mold curing) process was carried out in an oven at 175°C for 4 hours, after which the mass and volume were determined and calculated as the ratio of mass to volume (mass / volume, g / mL).

[0096] (4) Thermal conductivity: The epoxy resin composition for sealing semiconductor elements was injected into a transfer molding machine under the conditions of a mold temperature of 175°C, an injection pressure of 9 MPa, and a curing time of 120 seconds to prepare a thermal conductivity test piece. The thermal conductivity test piece was then evaluated at 25°C using a QTM-500 measuring device manufactured by Kyoto Electronics Manufacturing Co., Ltd. in accordance with ASTM D5470.

[0097] (5) Degree of contamination of equipment for fine powder scattering during compression molding: Compression molding equipment (PMC-1040, manufactured by TOWA Corporation) was used as the compression molding equipment. 25 g of the epoxy resin composition produced in the examples and comparative examples was placed in the vibration feeder, and the operation of constantly feeding at a feed rate of 1.0 g / sec was repeated 20 times. After the feeding was completed, the vibration feeder was separated and the weight of the epoxy resin composition attached to the wall of the vibration feeder was measured. When the weight of the attached epoxy resin composition was less than 150 mg in total and the adhesion state of the vibration feeder inner tube was not visible with the naked eye, it was judged as ×, when the weight of the attached epoxy resin composition was less than 150 mg in total and the adhesion state of the vibration feeder inner tube was observed with the naked eye, it was judged as △, and when the weight of the attached epoxy resin composition was 150 mg or more in total, the vibration feeder inner tube turned black with the naked eye, and the adhesion of the epoxy resin composition occurred significantly, it was judged as ○.

[0098] (6) Wire sweep: A die (10 mm x 10 mm x 0.5 mm) was mounted on a printed wiring board (board size: 240 mm x 77.5 mm, unit size: 14 mm x 18 mm). A gold wire with a diameter of 0.8 mm was used for connection. A compression molding machine (PMC-1040, manufactured by TOWA Corporation) was used. The epoxy resin compositions for sealing semiconductor elements of the examples and comparative examples were charged into the molding machine in the same amount, and a semiconductor device was molded under the conditions of a molding thickness of 0.7 mm, a mold temperature of 175°C, a curing time of 100 seconds, and a molding pressure of 10 tons. Analysis was performed using an X-ray transmission machine (Tosmicron-S4090, manufactured by Toshiba IT Control Systems Corporation) to evaluate wire sweep for 10 wires (wire length of 3 mm) of the package.

[0099] [Table 4]

[0100] [Table 5]

[0101] [Table 6]

[0102] As shown in Table 4, the tablet-shaped epoxy resin compositions of Examples 1 to 9 of the present invention were able to prevent the composition from sticking and / or scattering in compression molding equipment when sealing semiconductor elements by compression molding, thereby reducing contamination of the equipment. In addition, wire sweep was significantly reduced when sealing semiconductor elements by compression molding. In addition, by having a thermal conductivity of 2 W / mK or more, the heat dissipation effect was improved when sealing semiconductor elements, and the frequency of package malfunction and crack occurrence due to heat generated during operation was reduced.

[0103] On the other hand, as shown in Tables 5 and 6, even when using the tablet compression molding method, referring to Comparative Examples 1 to 12, when any one of (i), (ii), and (iii) of the present application is not satisfied, the wire sweep reduction effect is low, the thermal conductivity is low, or the equipment contamination due to dust is high.

[0104] Simple modifications and variations of the present invention can be easily implemented by those having ordinary skill in the art, and all such modifications and variations can be considered to be included within the scope of the present invention. [Explanation of symbols]

[0105] 1. Epoxy resin composition for sealing semiconductor elements, 2 Vibratory feeder, 3 composition supply container, 4 shutter, 5 Lower molding cavity, 6 Semiconductor elements, 7 Top board, 8 Lower Board, 9 Heater, 101 Semiconductor element, 102 Sealing materials, 103 die pad, 104 Die bonding materials, 105 electrode pads and lead frames, 106 wires.

Claims

1. With respect to the entire tablet-form epoxy resin composition for sealing semiconductor elements, (i) the proportion of tablets having a diameter of 0.1 mm or more and less than 2.8 mm and a height of 0.1 mm or more and less than 2.8 mm is 97% or more by weight, as measured by powder sieving using ASTM standard sieves; (ii) the tablet has a compressed density of greater than 1.7 g / mL; (iii) the tablet has a ratio of compressed density to hardened density of 0.6 to 0.87; It contains an inorganic filler containing one or more of alumina and aluminum nitride. A tablet-shaped epoxy resin composition for sealing semiconductor elements.

2. 2. The tablet-shaped epoxy resin composition for sealing semiconductor elements according to claim 1, wherein the tablet has a cylindrical shape.

3. The tablet-shaped epoxy resin composition for sealing semiconductor elements according to claim 1 or 2, wherein the inorganic filler is contained in an amount of 70% by weight to 99% by weight of the tablet-shaped epoxy resin composition for sealing semiconductor elements.

4. A tablet-form epoxy resin composition for sealing semiconductor elements described in any one of claims 1 to 3, wherein the inorganic filler contains silica, and the silica is contained in the inorganic filler in an amount of 90 weight % or less.

5. 5. The tablet-shaped epoxy resin composition for sealing semiconductor elements according to claim 1, wherein the aluminum nitride is contained in an amount of 50% by weight or less of the inorganic filler.

6. The tablet-shaped epoxy resin composition for sealing semiconductor elements according to any one of claims 1 to 5, wherein the inorganic filler has an average particle size (D50) of 3 µm to 15 µm.

7. 7. The tablet-shaped epoxy resin composition for sealing semiconductor elements according to claim 1, wherein the alumina is contained in an amount of 10% by weight to 100% by weight of the inorganic filler.

8. The tablet-shaped epoxy resin composition for sealing semiconductor elements according to any one of claims 1 to 7, wherein the alumina is contained in an amount of 75% by weight to 98% by weight of the tablet-shaped epoxy resin composition for sealing semiconductor elements.

9. The tablet-shaped epoxy resin composition for sealing semiconductor elements according to any one of claims 1 to 8, wherein the tablet-shaped epoxy resin composition for sealing semiconductor elements contains a mixture of alumina and silica as the inorganic filler.

10. The tablet-shaped epoxy resin composition for sealing semiconductor elements according to claim 9, wherein the mixture of alumina and silica is contained in an amount of 75% by weight to 98% by weight of the tablet-shaped epoxy resin composition for sealing semiconductor elements.

11. The tablet-shaped epoxy resin composition for sealing semiconductor elements according to any one of claims 1 to 10, which contains a mixture of silica and aluminum nitride as the inorganic filler.

12. The tablet-shaped epoxy resin composition for sealing semiconductor elements according to claim 11, wherein the mixture of silica and aluminum nitride is contained in an amount of 75% by weight to 98% by weight of the tablet-shaped epoxy resin composition for sealing semiconductor elements.

13. The tablet-shaped epoxy resin composition for sealing semiconductor elements according to any one of claims 1 to 12, wherein the cured density is 1.9 g / mL to 4 g / mL.

14. The tablet-shaped epoxy resin composition for sealing semiconductor elements according to any one of claims 1 to 13, wherein the tablet-shaped epoxy resin composition for sealing semiconductor elements is produced by tablet compression molding.

15. A semiconductor device sealed with the tablet-shaped epoxy resin composition for sealing semiconductor elements according to any one of claims 1 to 14.

Citation Information

Patent Citations

  • Molding material for sealing semiconductor part

    JP1984204614A

  • Manufacture of semiconductor device

    JP1985224234A

  • Manufacturing method of epoxy resin molding material for sealing, epoxy resin molding material for sealing and electronic part unit

    JP2007077333A

  • Sealing material tablet

    JP2007258744A

  • Granulated epoxy resin composition for semiconductor encapsulation, semiconductor device using the same, and method for manufacturing the semiconductor device

    JP2010159400A