Sputtering target material and its manufacturing method

A Co-Fe-B alloy with controlled boron and rare earth elements forms an intermetallic compound phase, enhancing the toughness of sputtering target materials, enabling efficient production of high-performance magnetic films for magnetic devices.

JP7564626B2Active Publication Date: 2024-10-09SANYO SPECIAL STEEL CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020022183
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-02-13
Publication Date
2024-10-09
Estimated Expiration
2040-02-13

Smart Images

  • Figure 0007564626000003
    Figure 0007564626000003
  • Figure 0007564626000001
    Figure 0007564626000001
  • Figure 0007564626000002
    Figure 0007564626000002
Patent Text Reader

Abstract

To provide a sputtering target material having exceptional cracking resistance, and a method for manufacturing the sputtering target material.SOLUTION: Provided is a sputtering target material, the substance of which is an alloy including B and one or more rare-earth elements, the balance being Co and / or Fe, and unavoidable impurities. The B content of the alloy is 15-30 at.% (inclusive); the one or more rare-earth elements are selected from the group consisting of Pr, Nd, Sm, Gd, Tb, Dy, and Ho; and the total content of the selected rare-earth element(s) is 0.1-10 at.% (inclusive). The sputtering target material is produced through a sintering step to sinter the base powder made up of the alloy of the composition.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sputtering target material, and more particularly to a sputtering target material used in the production of a magnetic layer and a method for producing the same. [Background technology]

[0002] Magnetic tunnel junction (MTJ) elements are used in magnetic devices such as magnetic heads and magnetic random access memories (MRAMs), etc. MTJ elements exhibit characteristics such as a high tunnel magnetoresistance (TMR) signal and low switching current density (Jc).

[0003] A magnetic tunnel junction (MTJ) element has a structure in which a shielding layer made of MgO is sandwiched between two magnetic layers made of, for example, a Co-Fe-B alloy. A magnetic material containing boron (B) is known as a material for this magnetic layer. For example, it is a magnetic material having a composition of Co-B, Fe-B, Co-Fe-B, or a composition in which Al, Cu, Mn, Ni, etc. are added to these.

[0004] The magnetic layer constituting a magnetic tunnel junction (MTJ) element is usually obtained by sputtering using a target material made of a Co-Fe-B alloy. JP 2004-346423 A (Patent Document 1) discloses a Co-Fe-B alloy target material in which a boride phase is finely dispersed in a cross-sectional microstructure. International Publication WO2015-080009 (Patent Document 2) proposes a magnetic sputtering target that includes a high concentration phase of B and a low concentration phase of B, and in which the high concentration phase of B is finely dispersed.

[0005] JP 2017-057477 A (Patent Document 3) proposes a sputtering target material that reduces the formation of (CoFe)3B, Co3B, and Fe3B. International Publication WO2016-140113 (Patent Document 4) discloses a magnetic sputtering target with an oxygen content of 100 atppm or less.

[0006] In recent years, there has been a demand for further improvements in the performance of MTJ elements. Japanese Patent Laid-Open No. 2017-82330 (Patent Document 5) and Japanese Patent Laid-Open No. 2014-156639 (Patent Document 6) disclose sputtering target materials made of alloys for soft magnetic film layers containing rare earth (lanthanoid) elements. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2004-346423 A [Patent Document 2] International Publication No. WO2015-080009 [Patent Document 3] JP 2017-057477 A [Patent Document 4] International Publication No. WO2016-140113 [Patent Document 5] JP 2017-82330 A [Patent Document 6] JP 2014-156639 A Summary of the Invention [Problem to be solved by the invention]

[0008] As shown in Patent Documents 5 and 6, the addition of rare earth elements to the CoFe alloy that constitutes the target material improves the magnetic performance of the resulting magnetic layer, achieving a high TMR signal from the MTJ element. However, the target material made of an alloy containing rare earth elements is very brittle and easily breaks during its manufacture and use, hindering productivity.

[0009] An object of the present invention is to provide a sputtering target material which is made of a Co-Fe-B based alloy containing a rare earth element and has excellent crack resistance, and a method for producing the same. [Means for solving the problem]

[0010] In a target material obtained by sintering a Co-Fe-B alloy powder, a metal structure containing a CoFe phase, which is an alloy phase, is formed. This CoFe phase contributes to improving the toughness of the target material. As a result of intensive research, the inventors of the present invention have focused on the fact that the addition of a rare earth element produces an intermetallic compound between the CoFe phase, which is responsible for the toughness, and the rare earth element, and have completed the present invention.

[0011] That is, the material of the sputtering target material according to the present invention is an alloy containing B and rare earth elements (hereinafter referred to as "rare earth elements RE" or simply "RE"), with the remainder being made of Co and / or Fe and unavoidable impurities. The content of B in this alloy is 15 at.% or more and 30 at.% or less. The rare earth elements RE are one or more elements selected from the group consisting of Pr, Nd, Sm, Gd, Tb, Dy and Ho. In this alloy, the total content of the selected rare earth elements RE is 0.1 at.% or more and 10 at.% or less.

[0012] Preferably, the intermetallic compound phase is formed from Co and / or Fe and the rare earth element, and the randomly selected areas 3250 μm 2 In the field of view, the number of intermetallic compound phases that can draw the maximum inscribed circle having a diameter of 5 μm or more is one or less.

[0013] From another viewpoint, a method for producing a sputtering target material according to the present invention includes a sintering step of sintering a raw material powder whose material is an alloy containing B and a rare earth element RE, with the balance being Co and / or Fe and unavoidable impurities. In this production method, the content of B in the alloy is 15 at.% or more and 30 at.% or less. The rare earth element RE is one or more selected from the group consisting of Pr, Nd, Sm, Gd, Tb, Dy and Ho. In this alloy, the total content of the selected rare earth elements RE is 0.1 at.% or more and 10 at.% or less. Effect of the Invention

[0014] The sputtering target material according to the present invention has an appropriate content of boron and rare earth elements in the alloy that is the material of the target material. This target material has excellent crack resistance. This target material is prevented from being damaged during its manufacture and sputtering. This target material has high production efficiency. A magnetic film obtained by sputtering using this target material has excellent magnetic performance. With this target material, a high-performance, high-quality magnetic film can be efficiently obtained. This target material is suitable for manufacturing magnetic films used in magnetic devices such as magnetic heads and MRAMs.

[0015] From another viewpoint, the manufacturing method according to the present invention makes it possible to obtain a magnetic film having improved magnetic performance, and moreover to efficiently and easily manufacture a target material having excellent crack resistance. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a scanning electron microscope image showing the metal structure of an alloy constituting a sputtering target material according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, the present invention will be described in detail based on preferred embodiments. In the present specification, the term "X to Y" indicating a range means "X or more and Y or less."

[0018] The sputtering target material according to the present invention is an alloy containing B and a rare earth element RE, with the balance being Co and / or Fe and unavoidable impurities. In other words, this alloy is a Co-Fe-B alloy containing a rare earth element RE. In the present invention, the rare earth element RE is one or more elements selected from the group consisting of Pr, Nd, Sm, Gd, Tb, Dy and Ho. These rare earth elements RE can contribute to improving the magnetic performance of the magnetic film obtained. As long as the effect of the present invention is not impaired, this alloy can contain other elements as optional components. Examples of unavoidable impurities include O, S, C, N, etc.

[0019] The B content in this alloy is 15 at.% or more and 30 at.% or less. By making the B content 15 at.% or more, sufficient amorphousness is imparted to the obtained magnetic film. This magnetic film has excellent magnetic performance. If the B content is 30 at.% or less, a metal structure containing a CoFe phase can be formed even when a rare earth element RE is added.

[0020] The content of the rare earth element RE in this alloy is 0.1 at.% or more and 10 at.% or less. When this alloy contains two or more selected from the group consisting of Pr, Nd, Sm, Gd, Tb, Dy and Ho, the total content is 0.1 at.% or more and 10 at.% or less. By making the total content of the rare earth element RE 0.1 at.% or more, the performance improvement effect of the obtained magnetic film is fully exhibited. By making the total content of the rare earth element RE 10 at.% or less, the formation of the CoFe phase in the metal structure is not inhibited.

[0021] The sputtering target material according to the present invention has an appropriate content of boron B and rare earth element RE in the alloy that is the material of the target material. The formation of the CoFe phase is not inhibited in the metal structure of this alloy. The CoFe phase in the metal structure contributes to improving the toughness of the target material and the magnetic performance of the magnetic film obtained. This target material has excellent crack resistance during manufacture and use. By sputtering using this target material, a magnetic film having high magnetic performance can be efficiently manufactured. By incorporating this magnetic film, a high TMR signal of the MTJ element is achieved. This target material is suitable for manufacturing magnetic films used in magnetic devices such as magnetic heads and MRAMs.

[0022] Preferably, the alloy constituting the sputtering target material has the following composition formula: (1-yz)(Co-xFe)-yB-zRE

[0023] In the above composition formula, x is the ratio (at.%) of Fe to the total of Co and Fe in this alloy. As long as the effects of the present invention can be obtained, x can be appropriately selected within the range of 0 at.% or more and 100 at.% or less. The (1-x) before Co is omitted.

[0024] In the above composition formula, RE is a collective term for rare earth elements selected from the group consisting of Pr, Nd, Sm, Gd, Tb, Dy, and Ho. y is the ratio (at.%) of B to the total of Co, Fe, B, and RE (i.e., the total content of rare earth elements selected from the group consisting of Pr, Nd, Sm, Gd, Tb, Dy, and Ho), and z is the ratio (at.%) of RE to this total.

[0025] In the target material according to the present invention, y is 15 at.% or more and 30 at.% or less. From the viewpoint of magnetic properties, y is more preferably 20 at.% or more.

[0026] In the target material according to the present invention, z is 0.1 at.% or more and 10 at.% or less. From the viewpoint of magnetic properties, z is more preferably 3 at.% or more.

[0027] In the Co-Fe-B alloy containing the rare earth element RE represented by the above composition formula, a metal structure containing the (CoFe)RE phase can be formed. The (CoFe)RE phase is a phase of an intermetallic compound (CoFe)RE formed by a reaction between the rare earth element RE and Co and / or Fe. The ratio of Co and / or Fe to RE in the (Co+Fe)RE phase varies depending on the type of rare earth element RE. In this specification, the intermetallic compound formed from Co and / or Fe and the rare earth element RE is defined as (CoFe)RE regardless of the ratio.

[0028] In the metal structure of a Co-Fe-B alloy containing a rare earth element RE, the formation and increase of the (CoFe)RE phase leads to a decrease and disappearance of the CoFe phase, which is responsible for the toughness of the target material. The decrease and disappearance of the CoFe phase reduces the crack resistance of the target material. A target material having a metal structure in which the formation and increase of the (CoFe)RE phase is suppressed and in which the toughness derived from the CoFe phase is not inhibited is preferable.

[0029] When observing the metal structure formed in this target material using a scanning electron microscope (SEM), it is preferable to observe a randomly selected field of view (area) of 50 μm in length and 65 μm in width. 3250 μm 2 ), the number of (CoFe)RE phases capable of drawing a maximum inscribed circle having a diameter of 5 μm or more therein is 1 or less. "The number of (CoFe)RE phases capable of drawing a maximum inscribed circle having a diameter of 5 μm or more therein" means, in other words, that the formation and increase of the (CoFe)RE phase in the metal structure is suppressed. In a target material having this metal structure, the toughness derived from the CoFe phase is not inhibited. This target material has excellent crack resistance. From this viewpoint, "the number of (CoFe)RE phases capable of drawing a maximum inscribed circle having a diameter of 5 μm or more therein" is more preferably zero.

[0030] The diameter of the maximum inscribed circle that can be drawn inside the (CoFe)RE phase is measured by image processing of the SEM image of the test piece taken from the target material. Commercially available image analysis software can be used for the image processing.

[0031] FIG. 1 is a part of a scanning electron microscope image obtained for a target material according to a preferred embodiment of the present invention. In FIG. 1, the white parts are (CoFe)RE phases. In this SEM image, the largest (CoFe)RE phase is indicated by an arrow 1. The diameter of the largest inscribed circle that can be drawn inside this largest (CoFe)RE phase is less than 5 μm. The dark parts indicated by an arrow 2 are boride phases (CoFe boride phases) formed from Co and / or Fe and B, and CoFe phases formed from Co and / or Fe. A circle with a diameter of 5 μm is shown at the bottom of the image for comparison.

[0032] In the present specification, "the number of (CoFe)RE phases within which a maximum inscribed circle with a diameter of 5 μm or more can be drawn" is determined by observing a test piece with a microscope and determining the field area of ​​the test piece. 3250 μm 2 For example, a field of view of 50 μm in length and 65 μm in width is randomly selected so that the number of (CoFe)RE phases having a maximum inscribed circle diameter of 5 μm or more is counted.

[0033] As long as the effects of the present invention are obtained, the metal structure may have other phases in addition to the (CoFe)RE phase. Examples of other phases include the (CoFe)2B phase and the CoFe phase.

[0034] The method for producing a sputtering target material according to the present invention includes a sintering step of sintering a raw material powder. In detail, this production method includes a step of forming a sintered body by so-called powder metallurgy, in which the raw material powder is heated under high pressure and solidified. The target material is obtained by processing this sintered body into an appropriate shape by mechanical means or the like.

[0035] The raw material powder is composed of a large number of particles. In the manufacturing method according to the present invention, the material of each particle constituting the raw material powder is an alloy containing B and a rare earth element RE, with the remainder being Co and / or Fe and unavoidable impurities. The content of B in this alloy is 15 at.% or more and 30 at.% or less. The rare earth element RE is one or more elements selected from the group consisting of Pr, Nd, Sm, Gd, Tb, Dy and Ho. The total content of the selected rare earth elements RE in this alloy is 0.1 at.% or more and 10 at.% or less.

[0036] In this manufacturing method, raw material powders having boron B and rare earth element RE contents each within the above-mentioned ranges are used, thereby suppressing the formation and increase of the (CoFe)RE phase in the metal structure of the target material obtained by sintering the raw material powder. The CoFe phase that contributes to toughness can be properly formed in the metal structure of the target material. The target material obtained by this manufacturing method has excellent crack resistance. This manufacturing method can prevent damage during the manufacturing of the target material.

[0037] This raw material powder can be produced by an atomization method. The type of atomization method is not particularly limited, and may be a gas atomization method, a water atomization method, or a centrifugal atomization method. When carrying out the atomization method, a known atomization device and production conditions are appropriately selected and used.

[0038] Preferably, the raw material powder is sieved before the sintering step. The purpose of this sieving is to remove particles (coarse powder) with a particle diameter of 500 μm or more that inhibit sintering. With this raw material powder, the effects of the present invention can be obtained even if no particle size adjustment is performed other than removing the coarse powder.

[0039] In producing the target material, the method and conditions for obtaining a sintered body by solidifying the raw material powder are not particularly limited. For example, hot isostatic pressing (HIP), hot pressing, spark plasma sintering (SPS), hot extrusion, etc. may be appropriately selected. In addition, the method for processing the obtained sintered body is not particularly limited, and known mechanical processing means may be used.

[0040] The target material obtained by the manufacturing method according to the present invention is suitable for use in sputtering to form a magnetic thin film used in an MTJ element, for example. This target material suppresses cracking of the target material during sputtering, even though it contains rare earth elements. This makes it possible to efficiently obtain high-performance, high-quality magnetic films suitable for magnetic devices such as magnetic heads and MRAMs. EXAMPLES

[0041] The effects of the present invention will be clarified by the following examples, but the present invention should not be construed as being limited based on the description of these examples.

[0042] [Production of raw powder] Each raw material was weighed so as to obtain the composition shown in Table 1-2, and placed in a crucible made of refractory material, and melted by induction heating under reduced pressure in an Ar gas atmosphere or a vacuum atmosphere. The molten metal was then made to flow out from a small hole (diameter 8 mm) provided at the bottom of the crucible, and gas atomized using high-pressure Ar gas to obtain raw material powder for manufacturing the target material.

[0043] [Manufacturing of sputtering target materials] The obtained raw material powder was sintered according to the following procedure to produce target materials Nos. 1-12 of the embodiment and target materials Nos. 13-15 of the comparative example.

[0044] First, the raw powder obtained by gas atomization was sieved to remove coarse powder with a diameter of 500 μm or more. Next, the raw powder after sieving was filled into a can (outer diameter 220 mm, inner diameter 210 mm, length 200 mm) made of carbon steel and vacuum degassed, and then sintered using a HIP device at a temperature of 900 to 1200 ° C, a pressure of 100 to 150 MPa, and a holding time of 1 to 5 hours to produce a sintered body. The obtained sintered body was processed into a disk shape with a diameter of 180 mm and a thickness of 7 mm by wire cutting, lathe processing, and surface grinding to prepare a sputtering target material.

[0045] [Scanning electron microscope observation] Test pieces were taken from each of the target materials No. 1-12 of the embodiment and the target materials No. 13-15 of the comparative example, and the cross section of each test piece was polished. The cross section of each test piece was observed with a scanning electron microscope (SEM) to measure the area of ​​50 μm vertically and 65 μm horizontally. 3250 μm 2 ) were taken in five fields of view. After that, image analysis was performed to measure the diameter of the largest inscribed circle drawn in the intermetallic compound (CoFe)RE phase, and the number of (CoFe)RE phases with a diameter of 5 μm or more was recorded. The results obtained are shown in Table 1-2 below as the number N of inscribed circles. This number N is the average value of the values ​​measured in the five fields of view.

[0046] [Crack resistance evaluation] The crack resistance of the sputtering target material was evaluated based on the flexural strength measured by the following procedure.

[0047] First, test pieces were cut out by wire cutting from each of the target materials No. 1-12 of the embodiment and the target materials No. 13-15 of the comparative example. Then, a flexural test was performed in accordance with the provisions of JIS Z 2511 "Metal powder - Method for measuring green strength by flexural test". The test conditions were as follows. Test piece shape: thickness 2mm, width 2mm, length 20mm Distance between fulcrums: 10mm

[0048] The load (kN) when the test piece broke was measured, and the flexural strength (MPa) was calculated using the following formula. The average of the values ​​obtained from three measurements is shown in Table 1-2 below. BS = (3 / 2) × P × L / (t 2 × W) BS: bending strength (MPa) t: thickness of test piece (mm) W: Width of test piece (mm) L: Distance between fulcrums (mm) P: Load at break (kN)

[0049] [Table 1]

[0050] [Table 2]

[0051] One of the SEM images obtained by photographing five fields of view for the target material No. 5 of the embodiment is shown in FIG. 1. The white area indicated by the arrow in FIG. 1 is the (CoFe)RE phase. As shown in Table 1, in the metal structure of the target material of the embodiment No. 5, the field of view of 50 μm vertical and 65 μm horizontal (area 3250 μm 2 ), the number N of (CoFe)RE phases having a maximum inscribed circle diameter of 5 μm or more is 0.

[0052] Using the target materials No. 1-12 of the embodiment and the target materials No. 13-15 of the comparative example, sputtering was performed by DC magnetron sputtering under the following sputtering conditions. Substrate: Aluminum substrate (diameter 95 mm, thickness 1.75 mm) Chamber atmosphere: Argon gas Chamber pressure: 0.9 Pa After sputtering, the condition of each target material was visually observed.

[0053] In the target materials No. 1-12 of the embodiment, no cracks were observed during sputtering, whereas in the target materials No. 13-15 of the comparative examples, which have a flexural strength of 90 MPa or less, cracks were observed after sputtering.

[0054] As described above, the target materials of the examples were evaluated higher than the target materials of the comparative examples. From these evaluation results, the superiority of the present invention is clear. [Industrial Applicability]

[0055] The sputtering target materials described above can be applied to the production of magnetic layers for various applications. [Explanation of symbols]

[0056] 1...(CoFe)RE phase 2. CoFe boride phase

Claims

1. The material is an alloy containing B and a rare earth element, with the balance being Co and / or Fe and unavoidable impurities, The content of B in the alloy is 15 at. % or more and 30 at. % or less, The rare earth element is one or more selected from the group consisting of Sm, Gd, Tb, Dy and Ho, and the total content of the selected rare earth element RE is 0.1 at. % or more and 10 at. % or less; A sputtering target material comprising an intermetallic compound phase formed from Co and / or Fe and the rare earth element, the intermetallic compound phase having a maximum inscribed circle having a diameter of 5 μm or more being one or less in a randomly selected visual field having an area of ​​3250 μm 2 .

2. The material includes a sintering step of sintering a raw material powder that is an alloy containing B and a rare earth element, with the balance being Co and / or Fe and unavoidable impurities, The content of B in the alloy is 15 at. % or more and 30 at. % or less, The rare earth element is one or more selected from the group consisting of Sm, Gd, Tb, Dy and Ho, and the total content of the selected rare earth element RE is 0.1 at. % or more and 10 at. % or less; A method for producing a sputtering target material, comprising the steps of: forming an intermetallic compound phase from Co and / or Fe and the rare earth element; and in a randomly selected field of 3250 μm 2 , there is one or less intermetallic compound phase capable of drawing a maximum inscribed circle having a diameter of 5 μm or more.

Citation Information

Patent Citations

  • Formation of thin film of ferromagnetic alloy

    JP1989156466A

  • Magnetic recording medium, target for forming magnetic recording film, and formation of magnetic recording film

    JP1994215941A

  • Fe-Co-B ALLOY TARGET MATERIAL, ITS MANUFACTURING METHOD, SOFT MAGNETIC FILM, MAGNETIC RECORDING MEDIUM AND TMR ELEMENT

    JP2004346423A

  • Sputtering target for permanent magnet thin film and method for producing the same

    JP2012207274A

  • CoFe-BASED ALLOY FOR SOFT MAGNETIC FILM LAYERS IN PERPENDICULAR MAGNETIC RECORDING MEDIA, AND SPUTTERING TARGET MATERIAL