Anode and zinc secondary battery

By using Zn particles, ZnO particles, and solder as a conductive aid in the negative electrode, the microstructural changes and dendrite formation issues are mitigated, enhancing the durability and cycle life of zinc secondary batteries.

JP7564668B2Active Publication Date: 2024-10-09NGK CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020154999
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-24
Filing Date
2020-09-15
Publication Date
2024-10-09
Estimated Expiration
2040-09-15

AI Technical Summary

Technical Problem

Zinc secondary batteries face shortened lifespan due to zinc dendrite formation causing short circuits and morphological changes in the negative electrode, leading to increased resistance and decreased active material availability during charging and discharging.

Method used

Incorporating Zn particles, ZnO particles, and solder as a conductive aid in the negative electrode to stabilize the microstructure and maintain electron conduction paths, thereby suppressing zinc accumulation and maintaining active material availability.

Benefits of technology

The proposed solution extends the cycle life of zinc secondary batteries by preventing zinc dendrite penetration and maintaining electrode functionality despite repeated charging and discharging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564668000002
    Figure 0007564668000002
  • Figure 0007564668000003
    Figure 0007564668000003
  • Figure 0007564668000001
    Figure 0007564668000001
Patent Text Reader

Abstract

To provide a negative electrode, and a zinc secondary battery including the negative electrode which suppress deterioration of the negative electrode due to repeated charging and discharging to improve durability in the zinc secondary battery, and thereby prolonging the cycle life.SOLUTION: A negative electrode 10 used for a zinc secondary battery includes a negative electrode active material 12 including Zn particles and ZnO particles, and a conductive aid 14 including solder.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a negative electrode and a zinc secondary battery. [Background technology]

[0002] In zinc secondary batteries such as nickel-zinc secondary batteries and air-zinc secondary batteries, it is known that metallic zinc precipitates in the form of dendrites from the negative electrode during charging, penetrates the voids in the separator such as nonwoven fabric, and reaches the positive electrode, resulting in a short circuit. Such a short circuit caused by zinc dendrites shortens the repeated charge-discharge life.

[0003] In order to address the above problems, a battery has been proposed that includes a layered double hydroxide (LDH) separator that selectively allows hydroxide ions to pass through while preventing the penetration of zinc dendrites. For example, Patent Document 1 (WO 2013 / 118561) discloses that an LDH separator is provided between the positive and negative electrodes in a nickel-zinc secondary battery. In addition, Patent Document 2 (WO 2016 / 076047) discloses a separator structure that includes an LDH separator fitted or joined to a resin outer frame, and that the LDH separator has such high density that it is gas impermeable and / or water impermeable. This document also discloses that the LDH separator can be composited with a porous substrate. Furthermore, Patent Document 3 (WO 2016 / 067884) discloses various methods for obtaining a composite material by forming an LDH dense membrane on the surface of a porous substrate. This method includes the steps of uniformly attaching an initiator substance capable of providing an initiation point for the crystal growth of LDH to a porous substrate, and subjecting the porous substrate to hydrothermal treatment in a raw material aqueous solution to form a dense LDH membrane on the surface of the porous substrate. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2013 / 118561 [Patent Document 2] International Publication No. 2016 / 076047 [Patent Document 3] International Publication No. 2016 / 067884 Summary of the Invention

[0005] Another factor that shortens the lifespan of zinc secondary batteries is the change in the morphology of zinc, which is the negative electrode active material. That is, as zinc dissolves and precipitates repeatedly during charging and discharging, the morphology of the negative electrode changes, causing high resistance due to blockage of pores and a decrease in the charge active material due to accumulation of isolated zinc, which results in problems such as difficulty in charging and discharging.

[0006] The present inventors have now discovered that by using solder as a conductive additive in the negative electrode together with Zn particles and ZnO particles, it is possible to suppress the deterioration of the negative electrode due to repeated charging and discharging in a zinc secondary battery, thereby improving durability and thereby extending the cycle life.

[0007] Therefore, an object of the present invention is to provide a negative electrode in a zinc secondary battery that can suppress deterioration of the negative electrode due to repeated charging and discharging, improve durability, and thereby extend the cycle life.

[0008] According to one aspect of the present invention, there is provided a negative electrode for use in a zinc secondary battery, comprising: A negative electrode active material including Zn particles and ZnO particles; A conductive assistant containing solder; A negative electrode is provided, comprising:

[0009] According to another aspect of the present invention, A positive electrode and The negative electrode; a separator that separates the positive electrode and the negative electrode in a manner capable of conducting hydroxide ions; An electrolyte; A zinc secondary battery is provided, comprising: [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a conceptual diagram for explaining a presumed mechanism of microstructural change during charging and discharging of a negative electrode containing the solder according to the present invention. [Diagram 2] FIG. 1 is a conceptual diagram for explaining a presumed mechanism of microstructural change in a conventional negative electrode not including solder during charging and discharging. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The negative electrode of the present invention is a negative electrode used in a zinc secondary battery. This negative electrode includes a negative electrode active material and a conductive assistant. The negative electrode active material includes Zn particles and ZnO particles. The conductive assistant includes solder. By using solder as a conductive assistant in the negative electrode together with Zn particles and ZnO particles in this way, the deterioration of the negative electrode due to repeated charging and discharging in the zinc secondary battery can be suppressed, and durability can be improved, thereby extending the cycle life.

[0012] As mentioned above, in conventional negative electrodes, as zinc dissolves and precipitates repeatedly during charging and discharging, the morphology of the negative electrode changes, causing high resistance due to blockage of pores and a decrease in the charge active material due to the accumulation of isolated zinc, which results in problems such as difficulty in charging and discharging. The estimated mechanism for this is as follows. In the negative electrode, the charge and discharge reaction formula is: ZnO+H2O+2OH - +2e - ⇔ Zn+4OH - … Formula (1) According to the above, ZnO changes to Zn during charging, while Zn changes to ZnO during discharging. However, not all of the Zn particles generated by charging can return to ZnO particles during discharging, and some of the Zn remains and accumulates. Then, as charging and discharging are repeated, the required ZnO particles gradually decrease, and the capacity decreases. This series of estimated mechanisms is conceptually shown in FIG. 2. In FIG. 2, a conventional negative electrode 10' (not including solder) including a negative electrode active material 12 containing Zn particles (discharge active material) and ZnO particles (charge active material and electron conductive material) and a current collector 16 is shown together with an electrolyte 18 and a separator 20. First, before the start of the charge and discharge cycle, as shown in FIG. 2(a), the negative electrode 10' contains more ZnO particles than Zn particles. Next, when charging, the reaction of formula (1) proceeds to the right, and as a result, the ZnO particles change to Zn particles and the Zn particles increase, as shown in FIG. 2(b). Since the Zn particles function not only as a charge active material but also as an electron conductive material, the increase in the Zn particles increases the electron conductive path. On the other hand, during discharge, the reaction of formula (1) proceeds to the left, and as a result, the Zn particles are converted to ZnO particles and the amount of Zn particles decreases, as shown in FIG. 2(c). However, at that time, the Zn particles near the surface of the negative electrode 10' far from the current collector 16 (area marked A in the figure) become electrically isolated, and cannot be discharged and accumulate as Zn particles, which is thought to result in a decrease in the amount of ZnO. Then, when charging and discharging are repeated, the amount of Zn accumulation gradually increases, as shown in FIG. 2(d), while the amount of ZnO required for charging gradually decreases, making it impossible to charge to the rated capacity.

[0013] In contrast, as conceptually shown in FIG. 1, the negative electrode 10 of the present invention contains solder as a conductive assistant 14 together with Zn particles and ZnO particles, and it is believed that this conductive assistant 14, i.e., solder, suppresses the increase in the amount of Zn accumulation (i.e., the decrease in the amount of ZnO). First, before the start of the charge-discharge cycle, as shown in FIG. 1(a), the negative electrode 10 contains more ZnO particles than Zn particles. Next, when the battery is charged, the reaction of formula (1) proceeds to the right, and as shown in FIG. 1(b), the ZnO particles change to Zn particles and the Zn particles increase. Since the Zn particles function not only as a charging active material but also as an electronic conductive material, the increase in the Zn particles increases the electronic conductive path. On the other hand, during discharge, the reaction of formula (1) proceeds to the left, and as shown in FIG. 2(c), the Zn particles change to ZnO particles and the Zn particles decrease. At this time, even if the Zn particles are reduced, the conductive assistant 14 (solder) ensures an electronic conduction path, so that the Zn particles near the surface of the negative electrode 10 far from the current collector 16 (area marked A in the figure) can be electrically connected, and a larger portion (ideally almost all) of the Zn particles generated by charging can be involved in the discharge, and as a result, the reduction in the ZnO particles is effectively suppressed. That is, the electrical isolation and accumulation of the Zn particles near the surface of the negative electrode 10 far from the current collector 16, and the resulting reduction in the amount of ZnO can be effectively suppressed. Thus, even if charging and discharging are repeated, the amount of Zn accumulation does not gradually increase as shown in FIG. 1(d), and therefore the amount of ZnO required for charging can be sufficiently secured, and charging to the rated capacity can be performed. In this way, the deterioration of the negative electrode 10 due to repeated charging and discharging can be suppressed, the durability can be improved, and the cycle life can be extended.

[0014] In FIG. 1, the area of ​​conductive additive 14 (solder) is depicted as not being connected between the upper and lower surfaces of negative electrode 10. However, this is because it is depicted two-dimensionally as a cross section. Taking depth into account, in three dimensions, it is preferable that the area of ​​conductive additive 14 is connected between the upper and lower surfaces of negative electrode 10, thereby ensuring an electronic conduction path for conductive additive 14.

[0015] The negative electrode active material 12 includes Zn particles and ZnO particles. The Zn particles are typically metal Zn particles, but particles of a Zn alloy or a Zn compound may be used. Metal Zn particles generally used in zinc secondary batteries can be used as the metal Zn particles, but it is more preferable to use metal Zn particles smaller than the metal Zn particles from the viewpoint of extending the cycle life of the battery. Specifically, the D50 particle size of the metal Zn particles is preferably 5 to 200 μm, more preferably 8 to 100 μm, and even more preferably 10 to 50 μm. The preferred content of the Zn particles in the negative electrode 10 is preferably 1 to 50 parts by weight, more preferably 2 to 45 parts by weight, and even more preferably 5 to 35 parts by weight, when the content of the ZnO particles is taken as 100 parts by weight. Alternatively, the preferred content of the Zn particles in the negative electrode 10 is preferably 1 to 40 parts by volume, more preferably 2 to 35 parts by volume, and even more preferably 4 to 30 parts by volume, when the content of the ZnO particles is taken as 100 parts by volume. As described later, the metal Zn particles may be doped with a dopant such as In or Bi. The ZnO particles are not particularly limited and may be a commercially available zinc oxide powder used in zinc secondary batteries or a zinc oxide powder obtained by growing particles by a solid-phase reaction using the commercially available zinc oxide powder as a starting material. The D50 particle size of the ZnO particles is preferably 0.1 to 20 μm, more preferably 0.1 to 10 μm, and even more preferably 0.1 to 5 μm.

[0016] The content of the negative electrode active material 12 with respect to the total volume of the negative electrode active material 12, the conductive assistant 14, and the binder resin (if the negative electrode 10 contains a binder resin) is preferably 40 to 95% by volume, more preferably 50 to 90% by volume, and further preferably 60 to 80% by volume. In calculating the solder content, the amount of metal components in the solder (converted value) is used as the solder content, while the amount of the binder resin is used as the solid content (converted value) of the binder resin.

[0017] The conductive assistant 14 includes solder. Any kind of solder can be used as long as it does not impair the function of the zinc secondary battery. A preferred solder includes at least one selected from the group consisting of Sn, Pb, Bi, In, and Zn, and more preferably includes at least Sn. By using a solder with such a composition, undesirable reactions (e.g., hydrogen generation) are less likely to occur in a strong alkaline electrolyte (e.g., potassium hydroxide aqueous solution). Specific examples of such preferred solder include Sn-Pb solder, Sn-Bi solder, Sn-In solder, Sn-Zn solder, and combinations thereof. The compositions of Sn-Pb solder, Sn-Bi solder, Sn-In solder, and Sn-Zn solder can be generally known compositions and are not particularly limited, but typically contain 40 to 95% by weight of Sn, with the remainder being other elements such as Pb, Bi, In, and Zn. A particularly preferred composition is a eutectic composition in that it can be melted at the lowest temperature. The eutectic compositions (weight %) of Sn-Pb solder, Sn-Bi solder, Sn-In solder, and Sn-Zn solder are Sn63%-Pb37%, Sn42%-Bi58%, Sn48%-In52%, and Sn91%-Zn9%, respectively. However, the composition of the solder does not have to be a eutectic composition as long as the desired characteristics are obtained. The solder is preferably in the form of particles with a particle size of 0.1 to 100 μm, more preferably 3 to 100 μm, further preferably 3 to 50 μm, and particularly preferably 5 to 30 μm. In particular, the solder forms a three-dimensional network, and Zn particles and ZnO particles are incorporated into the three-dimensional network. In this way, undesirable movement of the conductive assistant 14 due to repeated charging and discharging can be effectively suppressed, and the conductive assistant 14 can be effectively held at the desired position. The three-dimensional network of the solder can be formed by melting the solder particles and bonding them to each other. Although the conductive assistant 14 is preferably composed only of solder, the negative electrode 10 may contain other conductive assistants to the extent that the above-mentioned effects are not impaired.

[0018] The content of the solder with respect to the total volume of the negative electrode active material 12, the conductive assistant 14, and (when the negative electrode 10 contains a binder resin) the binder resin is preferably 5 to 60% by volume, more preferably 10 to 50% by volume, and further preferably 20 to 40% by volume. Note that, in calculating the content of the solder, the amount of the metal components of the solder (converted value) is used as the content of the solder, whereas the amount of the solid content of the binder resin (converted value) is used as the content of the binder resin.

[0019] The negative electrode 10 may further contain a binder resin (not shown). When the negative electrode 10 contains a binder, the shape of the negative electrode is easily maintained. As the binder resin, various known binders can be used, and preferred examples include polyvinyl alcohol (PVA) and polytetrafluoroethylene (PTFE). It is particularly preferred to use a combination of both PVA and PTFE as the binder.

[0020] The negative electrode 10 is preferably a sheet-like pressed body. This can prevent the negative electrode active material 12 from falling off, improve the electrode density, and more effectively suppress the change in shape of the negative electrode 10. Such a sheet-like pressed body can be produced by adding a binder to the negative electrode material and kneading the mixture, and then subjecting the resulting kneaded mixture to press molding such as roll pressing to form it into a sheet.

[0021] The negative electrode 10 is preferably provided with a current collector 16. Preferable examples of the current collector 16 include copper punched metal and copper expanded metal. In this case, for example, a mixture containing Zn particles, ZnO particles, solder, and optionally a binder resin (e.g., polytetrafluoroethylene particles) can be applied onto the copper punched metal or copper expanded metal to preferably prepare a negative electrode plate consisting of the negative electrode 10 / current collector 16. In this case, it is also preferable to perform a press treatment on the negative electrode plate (i.e., the negative electrode 10 / current collector 16) after drying to prevent the negative electrode active material 12 from falling off and to improve the electrode density. Alternatively, the above-mentioned sheet-like press molded body may be pressure-bonded to the current collector 16 such as copper expanded metal.

[0022] Zinc secondary battery The negative electrode 10 of the present invention is preferably applied to a zinc secondary battery. Therefore, according to a preferred embodiment of the present invention, a zinc secondary battery is provided, which includes a positive electrode (not shown), a negative electrode 10, a separator 20 that separates the positive electrode and the negative electrode 10 so as to be capable of conducting hydroxide ions, and an electrolyte 18. The zinc secondary battery of the present invention is not particularly limited as long as it is a secondary battery that uses the above-mentioned negative electrode 10 and uses the electrolyte 18 (typically an aqueous alkali metal hydroxide solution). Therefore, it can be a nickel-zinc secondary battery, a silver oxide zinc secondary battery, a manganese oxide zinc secondary battery, a zinc-air secondary battery, or any other type of alkaline zinc secondary battery. For example, it is preferable that the positive electrode contains nickel hydroxide and / or nickel oxyhydroxide, thereby forming a nickel-zinc secondary battery. Alternatively, the positive electrode may be an air electrode, thereby forming a zinc secondary battery.

[0023] The separator 20 is preferably a layered double hydroxide (LDH) separator. That is, as described above, LDH separators are known in the field of nickel-zinc secondary batteries and air-zinc secondary batteries (see Patent Documents 1 to 3), and this LDH separator can be preferably used in the zinc secondary battery of the present invention. The LDH separator can selectively allow hydroxide ions to pass through while preventing the penetration of zinc dendrites. Combined with the effect of employing the negative electrode of the present invention, the durability of the zinc secondary battery can be further improved.

[0024] The LDH separator may be a composite with a porous substrate as disclosed in Patent Documents 1 to 3. The porous substrate may be made of any of ceramic materials, metal materials, and polymer materials, but is particularly preferably made of a polymer material. The polymer porous substrate has the following advantages: 1) flexibility (so it is difficult to break even if it is made thin); 2) porosity can be easily increased; 3) conductivity can be easily increased (because the thickness can be reduced while increasing the porosity); and 4) it is easy to manufacture and handle. Particularly preferred polymer materials are polyolefins such as polypropylene and polyethylene, which are excellent in hot water resistance, acid resistance, and alkali resistance, and are low cost, and polypropylene is the most preferred. When the porous substrate is made of a polymer material, it is particularly preferred that the functional layer is incorporated throughout the entire thickness direction of the porous substrate (for example, most or almost all of the pores inside the porous substrate are filled with LDH). In this case, the preferred thickness of the polymer porous substrate is 5 to 200 μm, more preferably 5 to 100 μm, and even more preferably 5 to 30 μm. As such a polymeric porous substrate, a microporous membrane such as that commercially available as a lithium battery separator can be preferably used.

[0025] The electrolyte 18 preferably contains an aqueous solution of an alkali metal hydroxide. Examples of the alkali metal hydroxide include potassium hydroxide, sodium hydroxide, lithium hydroxide, and ammonium hydroxide, with potassium hydroxide being more preferred. Zinc oxide, zinc hydroxide, and the like may be added to the electrolyte to suppress self-dissolution of the zinc-containing material. EXAMPLES

[0026] The present invention will now be further illustrated by the following examples.

[0027] Examples 1-16 (1) Preparation of the positive electrode Paste-type nickel hydroxide positive electrode (capacity density: approx. 700 mAh / cm 3 ) was prepared.

[0028] (2) Preparation of the negative electrode The following various raw material powders were prepared. <Negative electrode active material> ZnO powder (manufactured by Seido Chemical Industry Co., Ltd., JIS standard class 1 grade, average particle size D50: 0.2 μm) Metallic Zn powder (Mitsui Mining & Smelting Co., Ltd., doped with Bi and In, Bi: 1000 ppm by weight, In: 1000 ppm by weight, average particle size D50: 50 μm) <Conductive assistant> Solder (powder or paste) of various compositions and particle sizes shown in Table 1 <Resin binder> Polytetrafluoroethylene (PTFE) aqueous dispersion (Daikin Industries, Ltd., solids content 60%)

[0029] In Examples 1 to 15, ZnO powder was mixed with ZnO metal powder and solder, and PTFE was added and kneaded with propylene glycol according to the mixing ratio (solder is calculated as metal component, PTFE is calculated as solid content) shown in Table 1. Meanwhile, in Example 16, ZnO powder was mixed with ZnO metal powder, and PTFE was added and kneaded with propylene glycol according to the mixing ratio (solder is calculated as metal component, PTFE is calculated as solid content) shown in Table 1.

[0030] The obtained kneaded material was rolled with a roll press to obtain a negative electrode active material sheet. The negative electrode active material sheet was pressure-bonded to a tin-plated copper expand metal. The samples with added solder (Examples 1 to 15) were heat-treated under conditions suitable for the solder components and used as negative electrodes, while the sample without added solder (Example 16) was used as negative electrodes without heat treatment.

[0031] (3) Preparation of electrolyte Ion-exchanged water was added to a 48% aqueous potassium hydroxide solution (special grade, manufactured by Kanto Chemical Co., Ltd.) to adjust the KOH concentration to 5.4 mol%, and then 0.42 mol / L of zinc oxide was dissolved therein by heating and stirring to obtain an electrolyte.

[0032] (4) Preparation of evaluation cell The positive and negative electrodes were wrapped in nonwoven fabric, and a current extraction terminal was welded to them. The positive and negative electrodes thus prepared were placed opposite each other via an LDH separator, sandwiched between a laminate film with a current extraction port, and three sides of the laminate film were heat-sealed. An electrolyte was added to the cell container with the top open in this way, and the electrolyte was allowed to fully penetrate the positive and negative electrodes by evacuation or the like. The remaining side of the laminate film was then heat-sealed to form a simple sealed cell.

[0033] (5) Evaluation Using a charge / discharge device (TOSCAT3100, manufactured by Toyo Systems Co., Ltd.), the simple sealed cell was subjected to formation by charging at 0.1C and discharging at 0.2C. Then, a 1C charge / discharge cycle was performed. The charge / discharge cycle was repeated under the same conditions, and the number of charge / discharge cycles until the discharge capacity of the prototype battery decreased to 70% of the discharge capacity of the first cycle was recorded. The number of charge / discharge cycles for each example is shown in Table 1 as a relative value when the number of charge / discharge cycles in Example 16 is set to 1.0.

[0034] [Table 1] [Explanation of symbols]

[0035] 10,10' negative pole 12 Negative electrode active material 14 Conductive additives 16 Current collector 18 Electrolyte 20 Separator

Claims

1. A negative electrode for use in a zinc secondary battery, a negative electrode active material including Zn particles and ZnO particles; A conductive assistant containing solder; Including, The solder contains one or more elements selected from the group consisting of Sn, Pb, Bi, In, and Zn, including at least Sn; A negative electrode, wherein the solder forms a three-dimensional network, and Zn particles and ZnO particles are embedded in the three-dimensional network.

2. 2. The negative electrode according to claim 1, wherein the solder is at least one selected from the group consisting of Sn-Pb solder, Sn-Bi solder, Sn-In solder, and Sn-Zn solder.

3. 3. The negative electrode according to claim 1, wherein the solder is in the form of particles having a particle size of 0.1 to 100 μm.

4. 4. The negative electrode according to claim 3, wherein the solder has a particle size of 3 to 100 μm.

5. 4. The negative electrode according to claim 3, wherein the solder has a particle size of 3 to 50 μm.

6. The negative electrode according to any one of claims 1 to 5, wherein the negative electrode further comprises a binder resin.

7. The negative electrode according to any one of claims 1 to 6, wherein a content ratio of the solder with respect to a total volume of the negative electrode active material, the conductive assistant, and (if the negative electrode contains a binder resin) the binder resin is 5 to 60 volume %.

8. A positive electrode and The negative electrode according to any one of claims 1 to 7, a separator that separates the positive electrode and the negative electrode in a manner capable of conducting hydroxide ions; An electrolyte; A zinc secondary battery comprising:

9. 9. The zinc secondary battery of claim 8, wherein the separator is a layered double hydroxide (LDH) separator.

10. The zinc secondary battery according to claim 9 , wherein the LDH separator is composited with a porous substrate.

11. The zinc secondary battery according to any one of claims 8 to 10, wherein the positive electrode contains nickel hydroxide and / or nickel oxyhydroxide, thereby making the zinc secondary battery a nickel-zinc secondary battery.

12. The zinc secondary battery according to any one of claims 8 to 10, wherein the positive electrode is an air electrode, thereby forming the zinc secondary battery into a zinc-air secondary battery.

Citation Information

Patent Citations

  • Zinc electrode

    JP1984042775A

  • Negative active material for secondary battery, electrode and secondary battery using it

    JP1997092277A

  • Electrode structural body, secondary battery, and their manufacture

    JP1999242954A

  • Conductive composition

    JP2013201133A