Austenitic stainless steel welding filler metal
The controlled chemical composition of the filler metal addresses hot cracking and hydrogen embrittlement in austenitic stainless steel welding, improving weld metal resistance and ductility while optimizing element ratios for enhanced performance.
Patent Information
- Application Number
- JP2020201605
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-04
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-12-04
AI Technical Summary
Existing filler metals for austenitic stainless steel welding face challenges in suppressing hot cracking, ductility loss, and hydrogen embrittlement, particularly under low-temperature, high-pressure hydrogen environments, despite improvements in chemical composition to enhance hydrogen embrittlement resistance.
A filler metal with controlled chemical composition, including specific ranges of elements such as Mn, Ni, Cr, and f-value optimization, to improve cracking resistance and hydrogen embrittlement resistance, with elements like B and Mg to enhance ductility and reduce impurities like P, S, and O.
The filler metal effectively enhances the cracking resistance and hydrogen embrittlement resistance of weld metal, ensuring stability and durability in harsh hydrogen environments, maintaining ductility and reducing manufacturing costs.
Smart Images

Figure 0007564696000005 
Figure 0007564696000001 
Figure 0007564696000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a filler metal for welding austenitic stainless steel. [Background technology]
[0002] In recent years, hydrogen energy has been attracting attention as a clean energy source that does not emit greenhouse gases such as carbon dioxide. However, the use of hydrogen energy can cause a problem of material embrittlement caused by hydrogen gas, known as hydrogen embrittlement.
[0003] Therefore, various materials have been developed to suppress hydrogen embrittlement. For example, Patent Document 1 discloses the development of an austenitic stainless steel with improved hydrogen embrittlement resistance. The austenitic stainless steel used in such hydrogen-related technologies is often joined by welding and used as a component in the form of a welded joint.
[0004] Even if a steel has excellent hydrogen embrittlement resistance in its raw state, cracks and reduced ductility, or reduced hydrogen embrittlement resistance may occur after welding, so when welding, it is desirable for the welded joint to have good properties. In this case, the performance of the weld metal, which melts during welding and then solidifies, is likely to deteriorate. Therefore, improving the performance of the weld metal is important.
[0005] In light of the above, an austenitic stainless steel welded joint with improved hydrogen embrittlement resistance has been developed by controlling the chemical composition of the weld metal, as described in Patent Document 2. This welded joint has improved hydrogen embrittlement resistance by not only containing Cu but also increasing the Mn content. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2018 / 180788 [Patent Document 2] JP 2015-171729 A [Non-patent literature]
[0007] [Non-Patent Document 1] Tatsuya Hashimoto et al. (1965) “Methods for measuring the temperature of molten metal pool and examples of measurements” Journal of the Japan Welding Society 34, pp654-664. Summary of the Invention [Problem to be solved by the invention]
[0008] Thus, in order to improve properties such as hydrogen embrittlement resistance, it is effective to increase the Mn content and to add Cu, but for example, depending on the welding conditions, hot cracking and reduced ductility of the weld may occur. In addition, in recent years, hydrogen environments have become lower in temperature and pressure, and in such cases, hydrogen embrittlement resistance may also decrease.
[0009] The performance of the weld metal is affected by the filler metal, which is supplied to the molten pool during welding and becomes the weld metal after welding. Therefore, when austenitic stainless steel is used as a weld joint, a filler metal is required that can suppress hot cracking and a decrease in ductility in the weld metal, that is, that has good cracking resistance. In addition, the filler metal is naturally required to suppress the decrease in hydrogen embrittlement resistance as described above.
[0010] An object of the present invention is to solve the above problems and to provide a filler metal for welding austenitic stainless steels, which can improve the cracking resistance and hydrogen embrittlement resistance of the weld metal when welding austenitic stainless steels. [Means for solving the problem]
[0011] The present invention has been made in order to solve the above problems, and the gist of the invention is the following austenitic stainless steel welding filler metal.
[0012] (1) Chemical composition, in mass%, C: 0.10% or less, Si: 1.0% or less, Mn: 8.0-11.0%, P:0.030% or less, S: 0.0030% or less, Cr: 15.0-18.0%, Ni: 7.0-9.0%, N: 0.15-0.25%, B: 0.0002~0.01%, Mg: 0.0001 to 0.0050%, Cu: less than 1.00% Mo: 0.5% or less O: 0.0050% or less, Al: 0-0.20%, Ca: 0-0.01%, Nb: 0-0.50%, Ti: 0 to 0.50%, V: 0~0.50%, W: 0 to 0.50%, Zr: 0-0.50%, Co: 0-0.50%, Ga: 0 to 0.010%, Hf: 0~0.10%, REM: 0~0.10%, The balance is Fe and impurities. An austenitic stainless steel welding filler metal, whose f-value, calculated by the following formula (i), is greater than 30.0 and less than 33.5. f value=Ni+0.72Cr+0.88Mo+1.11Mn-0.27Si+12.93C+7.55N (i) In the above formula (i), each element symbol represents the content (mass%) of each element contained in the steel, and when no element is contained, it is set to zero.
[0013] (2) The chemical composition is, in mass%, Al: 0.003-0.20%, Ca: 0.0002~0.01%, Nb: 0.002 to 0.50%, Ti: 0.002 to 0.50%, V: 0.01 to 0.50%, W: 0.001 to 0.50%, Zr: 0.01 to 0.50%, Co: 0.01 to 0.50%, Ga: 0.001 to 0.010%, Hf: 0.01 to 0.10%, and REM: 0.01~0.10%, The filler metal for welding austenitic stainless steel according to the above (1), comprising one or more selected from the following:
[0014] (3) The chemical composition is P: 0.025% or less, S: 0.0020% or less, B: 0.0002~0.0020%, Mg: 0.0001 to 0.0020%, Cu: 0.50% or less, O: 0.0030% or less, The austenitic stainless steel welding filler metal according to the above (1) or (2). Effect of the Invention
[0015] According to the present invention, it is possible to obtain a filler metal for welding austenitic stainless steel, which can improve the cracking resistance and hydrogen embrittlement resistance of the weld metal. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a schematic diagram showing the groove shape in a welding test in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The present inventors performed welding using a filler metal for austenitic stainless steels that can increase the Mn content and improve hydrogen embrittlement resistance. Then, the crack resistance and hydrogen embrittlement resistance of the weld metal of the obtained welded joint were investigated. As a result, the following findings (a) to (d) were obtained regarding the chemical composition of the filler metal.
[0018] (a) Weld metal of welded joints with a high Mn content was prone to hot cracking as well as reduced ductility after welding. In order to suppress hot cracking, it is effective to reduce low melting point elements such as P and S in the filler metal. Also, in order to suppress the decrease in ductility after welding, it is effective to reduce elements such as P and S. In addition, it is desirable to reduce O, which has a negative effect on ductility. It was also revealed that reducing Cu is extremely effective in preventing the decrease in ductility after welding.
[0019] In improving the ductility of the weld metal, it was also effective to add small amounts of B and Mg. The reason for this is that when the chemical composition of the filler metal is controlled as described above, B suppresses the grain boundary segregation of Cu in the weld metal of the weld joint, and Mg acts as a deoxidizer to reduce the O content.
[0020] (b) In addition, it is also effective to optimize the contents of Al, Ca, Nb, and Ti, which affect the penetration of the weld metal, for both hot crack resistance and ductility degradation after welding. The reason for this is that controlling the contents of the above elements improves the penetration of the weld metal, thereby suppressing the occurrence of cracks. Furthermore, these elements can also prevent the formation of welding slag that is difficult to peel off.
[0021] (c) In particular, when welding steel plates, the above-mentioned control of chemical composition is extremely effective because, since the heat input is relatively small in welding steel plates, elements such as Mn, Ni, Cu, and Mo are likely to induce cracks in the weld metal due to solidification segregation or grain boundary segregation.
[0022] (d) In a severe hydrogen environment, for example, a high-temperature, low-pressure hydrogen gas environment, in order to improve the hydrogen embrittlement resistance of the weld metal, it is necessary to limit the value of the f-value in the filler metal, which will be described later. In addition, in order to achieve both the crack resistance and hydrogen embrittlement resistance of the weld metal in the above environment, it is necessary to optimize the range of the above-mentioned elements and the f-value. This is because the contents of the above-mentioned elements and the contents of the elements that affect the f-value mutually affect each other.
[0023] The present invention has been made based on the above findings. Each of the features of the present invention will be described in detail below.
[0024] 1.Chemical composition The reasons for limiting the content of each element are as follows. In the following description, "%" for the content means "mass %."
[0025] C: 0.10% or less C is an element effective in stabilizing the austenite phase and also contributes to improving hydrogen embrittlement resistance. However, excessive C content makes the weld metal more susceptible to hot cracking and reduces the ductility of the weld metal, impairing cracking resistance. For this reason, the C content is set to 0.10% or less. The C content is preferably set to 0.08% or less, and more preferably set to 0.07% or less. On the other hand, in order to obtain the above effects, the C content is preferably set to 0.01% or more.
[0026] Si: 1.0% or less Silicon has the effect of suppressing undercutting, which is a defect that is hollowed out above the notch at the bead toe of the weld metal, and suppressing the formation of slag on the surface of the weld metal. However, excessive silicon content not only generates slag that is poorly removable during welding, but also reduces the ductility of the weld metal. For this reason, the silicon content is set to 1.0% or less. It is more preferable that the silicon content is set to 0.7% or less. On the other hand, in order to obtain the above effects, the silicon content is preferably set to 0.2% or more.
[0027] Mn: 8.0-11.0% Mn is an element effective in stabilizing the austenite phase, and contributes to improving hydrogen embrittlement resistance. In addition, since it increases the solid solubility limit of N, it contributes to saving expensive Ni and has the effect of preventing denitrification during welding. Furthermore, it has the effect of improving the cracking resistance of the weld metal. For this reason, the Mn content is set to 8.0% or more. The Mn content is preferably set to 8.5% or more, and more preferably set to 9.0% or more. However, excessive Mn content leads to a decrease in the ductility of the weld metal. For this reason, the Mn content is set to 11.0% or less, and preferably set to 10.0% or less.
[0028] P:0.030% or less P is an impurity contained in steel, which is concentrated during the final solidification process and lowers the melting point of the steel. As a result, it promotes hot cracking and reduces the cracking resistance of the weld metal. It also reduces hydrogen embrittlement resistance. For this reason, the P content is set to 0.030% or less. From the viewpoint of improving the cracking resistance of the weld metal, the P content is preferably set to 0.025% or less, and more preferably set to 0.015% or less. On the other hand, excessive reduction of P leads to an increase in raw material costs, so the P content is preferably set to 0.005% or more.
[0029] S: 0.0030% or less Like P, S is an impurity contained in steel and reduces the cracking resistance of the weld metal. It also reduces hydrogen embrittlement resistance. For this reason, the S content is set to 0.0030% or less. The S content is preferably set to 0.0020% or less, and more preferably set to 0.0010% or less. However, excessive reduction of S increases manufacturing costs. For this reason, the S content is preferably set to 0.0001% or more.
[0030] Cr: 15.0~18.0% Cr is a basic element that improves the corrosion resistance, especially the weather resistance, required for the weld metal. For this reason, the Cr content is set to 15.0% or more. However, Cr is a ferrite forming element. For this reason, excessive Cr content destabilizes the austenite phase, which leads to the formation of δ ferrite, resulting in a decrease in the ductility of the weld metal and a decrease in hydrogen embrittlement resistance. For this reason, the Cr content is set to 18.0% or less. The Cr content is preferably set to 17.0% or less.
[0031] Ni: 7.0~9.0% Ni, together with Mn, is an element necessary for ensuring the ductility and hydrogen embrittlement resistance of the weld metal. For this reason, the Ni content is set to 7.0% or more. However, excessive Ni content increases the raw material cost. For this reason, the Ni content is set to 9.0% or less. The Ni content is preferably set to 8.5% or less, and more preferably set to 8.0% or less.
[0032] N: 0.15~0.25% N is an element effective in improving the strength and hydrogen embrittlement resistance of the weld metal. For this reason, the N content is set to 0.15% or more. However, excessive N content makes it easier for internal defects such as blowholes to occur in the weld metal, and also reduces the ductility of the weld metal. For this reason, the N content is set to 0.25% or less. The N content is preferably set to 0.22% or less, and more preferably set to 0.20% or less.
[0033] B: 0.0002 to 0.01% B has the effect of strengthening grain boundaries and improving the ductility deterioration of the weld metal. For this reason, the B content is set to 0.0002% or more. The B content is preferably set to 0.0003% or more. However, even if B is contained in excess, not only does the effect saturate, but it also promotes the precipitation of boron compounds (BN, BC, Cr2B) at grain boundaries, reducing the hot cracking resistance of the weld metal. For this reason, the B content is set to 0.01% or less. The B content is preferably set to 0.0050% or less, and more preferably set to 0.0020% or less.
[0034] Mg: 0.0001 to 0.0050% Mg is an element effective in deoxidizing, and has the effect of improving the decrease in ductility of the weld metal. Therefore, the Mg content is set to 0.0001% or more. The Mg content is preferably set to 0.0003% or more. However, excessive Mg content reduces manufacturability such as refining. In addition, the crack resistance of the weld metal also decreases. Therefore, the Mg content is set to 0.0050% or less. From the viewpoint of effect and manufacturability, the Mg content is preferably set to 0.0020% or less.
[0035] Cu: Less than 1.00% Cu is an element that is mixed in from raw materials such as scrap, and has the effect of stabilizing the austenite phase and improving hydrogen embrittlement resistance. However, Cu is a low melting point element that is prone to segregation at grain boundaries, promoting hot cracking of the weld metal and making it prone to ductility reduction. For this reason, the Cu content is less than 1.00%. The Cu content is preferably 0.50% or less. However, excessive reduction of the Cu content leads to restrictions on the melting raw materials and increases the manufacturing cost. For this reason, the Cu content is preferably 0.01% or more.
[0036] Mo: 0.5% or less Mo is an element that is mixed in from raw materials such as scrap, and has the effect of improving strength and corrosion resistance. On the other hand, excessive inclusion of Mo promotes the formation of the δ-ferrite phase, reducing the crack resistance and hydrogen embrittlement resistance of the weld metal. For this reason, the Mo content is set to 0.5% or less. On the other hand, excessive reduction of Mo leads to restrictions on the melted raw materials and increases manufacturing costs. For this reason, the Mo content is preferably set to 0.01% or more.
[0037] O: 0.0050% or less O is an impurity contained in steel, which easily causes cracking and a decrease in ductility of the weld metal. Furthermore, it easily causes non-peelable slag to form on the surface of the weld metal. For this reason, the O content is set to 0.0050% or less. As a result, the weldability is improved, and the crack resistance is also improved. For this reason, the O content is preferably set to 0.0040% or less, and more preferably set to 0.0030% or less. However, excessive reduction of O makes it easy for undercut to occur. For this reason, the O content is preferably set to 0.0005% or more.
[0038] In addition to the above elements, one or more elements selected from Al, Ca, Nb, Ti, V, W, Zr, Co, Ga, Hf and REM may be contained within the ranges shown below. The reasons for limiting each element will be explained.
[0039] Al: 0 to 0.20% In addition to being an effective deoxidizing element, Al also has the effect of improving the penetration of the weld metal and suppressing undercut. Therefore, it may be contained as necessary. However, if an excessive amount of Al is contained, it inhibits the penetration during welding and makes it easier for non-peelable slag to form on the weld metal surface. For this reason, the Al content is set to 0.20% or less. The Al content is preferably set to 0.10% or less. On the other hand, in order to obtain the above effect, the Al content is preferably set to 0.003% or more, and more preferably set to 0.005% or more.
[0040] Ca: 0-0.01% Like Al, Ca is an effective deoxidizing element, and also has the effect of improving the penetration of the weld metal and suppressing undercut. Therefore, Ca may be contained as necessary. However, excessive Ca content inhibits the penetration during welding and makes it easier for non-peelable slag to form on the weld metal surface. For this reason, the Ca content is set to 0.01% or less. On the other hand, in order to obtain the above effect, the Ca content is preferably 0.0002% or more, and more preferably 0.0005% or more.
[0041] Nb: 0 to 0.50% Nb has the effect of forming carbonitrides, refining crystal grains, and improving the crack resistance of the weld metal. Therefore, it may be contained as necessary. However, if an excessive amount of Nb is contained, the ductility of the weld metal decreases. For this reason, the Nb content is set to 0.50% or less. The Nb content is preferably set to 0.30% or less. On the other hand, in order to obtain the above effect, the Nb content is preferably set to 0.002% or more, and more preferably set to 0.010% or more.
[0042] Ti: 0 to 0.50% Ti has the effect of forming carbonitrides, refining crystal grains, and improving the crack resistance of the weld metal. Therefore, it may be contained as necessary. However, if Ti is contained in excess, the ductility of the weld metal decreases. For this reason, the Ti content is set to 0.50% or less. The Ti content is preferably set to 0.30% or less. On the other hand, in order to obtain the above effect, the Ti content is preferably set to 0.002% or more, and more preferably set to 0.010% or more.
[0043] V: 0~0.50% V precipitates as a solid solution or carbonitride and has the effect of improving the strength of the weld metal. Therefore, V may be contained as necessary. However, if an excessive amount of V is contained, carbonitrides are formed in excess, which reduces the ductility of the weld metal. For this reason, the V content is preferably 0.50% or less. On the other hand, in order to obtain the above effect, the V content is preferably 0.01% or more, and more preferably 0.02% or more.
[0044] W: 0~0.50% W has the effect of improving the strength and corrosion resistance of the weld metal. Therefore, it may be contained as necessary. However, excessive W content reduces the ductility of the weld metal. For this reason, the W content is set to 0.50% or less. The W content is preferably set to 0.30% or less. On the other hand, in order to obtain the above effect, the W content is preferably set to 0.001% or more.
[0045] Zr: 0 to 0.50% Zr has a deoxidizing effect and has an effect of improving the ductility of the weld metal. Therefore, it may be contained as necessary. However, if Zr is contained in excess, an excessive amount of oxide is formed, and the crack resistance of the weld metal decreases. Therefore, the Zr content is set to 0.50% or less. The Zr content is preferably set to 0.30% or less. On the other hand, in order to obtain the above effect, the Zr content is preferably set to 0.01% or more.
[0046] Co: 0 to 0.50% Co has the effect of stabilizing the austenite phase of the weld metal and improving hydrogen embrittlement resistance. Therefore, it may be contained as necessary. However, excessive Co content reduces the ductility of the weld metal. For this reason, the Co content is set to 0.50% or less. On the other hand, in order to obtain the above effect, the Co content is preferably set to 0.01% or more.
[0047] Ga: 0 to 0.010% Ga has a deoxidizing effect and has the effect of improving the ductility of the weld metal. Therefore, it may be contained as necessary. However, if Ga is contained in excess, oxides are formed in excess, and the crack resistance of the weld metal decreases. For this reason, the Ga content is set to 0.010% or less. On the other hand, in order to obtain the above effect, the Ga content is preferably set to 0.001% or more.
[0048] Hf: 0~0.10% Hf has a deoxidizing effect and has the effect of improving the ductility of the weld metal. Therefore, it may be contained as necessary. However, if an excessive amount of Hf is contained, an excessive amount of oxide is formed, and the crack resistance of the weld metal decreases. Therefore, the Hf content is set to 0.10% or less. On the other hand, in order to obtain the above effect, the Hf content is preferably set to 0.01% or more.
[0049] REM: 0~0.10% REM has a deoxidizing effect and has the effect of improving the ductility of the weld metal. Therefore, it may be contained as necessary. However, if an excessive amount of REM is contained, an excessive amount of oxide is formed, and the cracking resistance of the weld metal decreases. For this reason, the REM content is set to 0.10% or less. On the other hand, in order to obtain the above effect, the REM content is preferably set to 0.01% or more.
[0050] REM refers to a total of 17 elements, including Sc, Y and lanthanides, and the above REM content refers to the total content of these elements. In industry, REM is often added in the form of misch metal.
[0051] In the chemical composition of the present invention, the balance is Fe and impurities. Here, the term "impurities" refers to components that are mixed in due to various factors in raw materials such as ores and scraps and manufacturing processes during industrial production of austenitic stainless steel filler metal, and are permissible within a range that does not adversely affect the present invention.
[0052] f-Score In the austenitic stainless steel welding filler metal according to the present invention, the f-value calculated below is specified as an index representing the stability of the austenite phase related to hydrogen embrittlement resistance. Specifically, the f-value calculated by the following formula (i) is set to be more than 30.0 and less than 33.5.
[0053] f value=Ni+0.72Cr+0.88Mo+1.11Mn-0.27Si+12.93C+7.55N (i) In the above formula (i), each element symbol represents the content (mass%) of each element contained in the steel, and when no element is contained, it is set to zero.
[0054] Here, if the f-value is 30.0 or less, the stability of the austenite phase is low and the hydrogen embrittlement resistance of the weld metal is reduced. For this reason, the f-value is set to be greater than 30.0. However, if the f-value is 33.5 or more, the cracking resistance of the weld metal is reduced due to the high alloying. In addition, the raw material cost increases, and the manufacturing cost of the filler metal also increases. Furthermore, the hydrogen embrittlement resistance may also decrease. For this reason, the f-value is set to be less than 33.5. From the viewpoints of the hydrogen embrittlement resistance and cracking resistance of the weld metal, and economic efficiency, the f-value is preferably set to be greater than 30.0 and equal to or less than 32.5.
[0055] 2.Applications The austenitic stainless steel welding filler metal according to the present invention is preferably used to produce austenitic stainless steel welded joints for use in hydrogen equipment such as high pressure hydrogen.
[0056] The chemical composition of the austenitic stainless steel, that is, the chemical composition of the base steel plate used for welding (base material excluding the heat-affected zone and weld metal in a welded joint), is, for example, C: 0.10% or less, Si: 1.0% or less, Mn: 8.0 to 10.0%, P: 0.030% or less, S: 0.0030% or less, Cr: 15.0 to 18.0%, Ni: 7.0 to 9.0%, N: 0.15 to 0.25%, B: 0 to 0.01%, Mg: 0 to 0.005%, and the like. %, Cu: less than 1.0%, Mo: less than 1.0%, Al: 0-0.20%, Ca: 0-0.01%, Nb: 0-0.50%, Ti: 0-0.50%, V: 0-0.50%, W: 0-0.50%, Zr: 0-0.50%, Co: 0-0.50%, Ga: 0-0.010%, Hf: 0-0.10%, REM: 0-0.10%, balance: Fe and impurities, and the F value calculated by the following formula (I) is preferably greater than 29.5 and less than 32.5.
[0057] F value=Ni+0.72Cr+0.88Mo+1.11Mn-0.27Si+0.53Cu+12.93C+7.55N...(I) In the above formula (I), each element symbol represents the content (mass%) of each element contained in the steel, and when no element is contained, it is set to zero.
[0058] In addition, the weld metal of the welded joint is as follows: C: 0.10% or less, Si: 1.0% or less, Mn: 8.0-11.0%, P: 0.030% or less, S: 0.0030% or less, Cr: 15.0-18.0%, Ni: 7.0-9.0%, N: 0.15-0.25%, B: 0-0.01%, Mg: 0-0.005%, Al: 0-0.20%, Cu: less than 1.0%, Mo: less than 1.0%, Ca: 0-0.01%, The filler metal, base steel plate, welding conditions, and the like are preferably adjusted as appropriate so that the F value calculated by the following formula (I) is greater than 29.5 and less than 32.5, and the filler metal, base steel plate, welding conditions, and the like are Nb: 0-0.50%, Ti: 0-0.50%, V: 0-0.50%, W: 0-0.50%, Zr: 0-0.50%, Co: 0-0.50%, Ga: 0-0.010%, Hf: 0-0.10%, REM: 0-0.10%, and the balance: Fe and impurities.
[0059] F value=Ni+0.72Cr+0.88Mo+1.11Mn-0.27Si+0.53Cu+12.93C+7.55N...(I) In the above formula (I), each element symbol represents the content (mass%) of each element contained in the steel, and when no element is contained, it is set to zero.
[0060] The chemical composition of the weld metal is the average chemical composition of the entire weld metal. Here, the weld metal in a welded joint refers to the metal part that melts and solidifies during welding. The weld metal and the weld heat-affected zone in the base material that is affected by the welding heat are collectively called the weld zone.
[0061] The austenitic stainless steel welding filler metal according to the present invention is used for welding steel plates, steel pipes, bars and wire rods, and is particularly preferably used for welding steel plates.
[0062] 3. Manufacturing method A preferred method for producing the austenitic stainless steel welding filler metal according to the present invention will now be described.
[0063] The filler metal according to the present invention is preferably produced by melting steel having the above-mentioned chemical composition and producing a billet or the like. The billet is preferably hot forged at 900 to 1300°C, heat treated in the range of 950 to 1150°C, and drawn into a steel wire by wire drawing. This steel wire is often wound on a spool. Other specific production conditions may be appropriately adjusted as long as they do not impair the effect of the filler metal.
[0064] When welding austenitic stainless steel using the filler metal according to the present invention, the welding conditions are not limited as long as the effects of the present invention are not impaired. In order to obtain a weld metal that provides the effects of the present invention, it is preferable to use, for example, gas tungsten arc welding (TIG welding).
[0065] In order to improve the crack resistance of the weld metal, it is effective to suppress the solidification segregation and grain boundary segregation of Mn, Ni, Cu, and Mo. For this reason, it is desirable to control the cooling rate to slow cooling after welding. Specifically, in the temperature range of 1300 to 800°C where the diffusion and movement of alloy elements progress in the weld metal, it is preferable to control the cooling rate to 20°C / sec or less, and more preferably to a range of 1 to 10°C / sec. The cooling rate after welding as described above can be controlled, for example, by the welding speed.
[0066] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. EXAMPLES
[0067] Steels having the chemical compositions shown in Table 1 were melted, and cold-rolled and annealed steel sheets (also called "base steel sheets") with thicknesses of 1.0 mm and 2.0 mm were manufactured by hot rolling, annealing, cold rolling, and annealing. Filler metals were melted from W1 to W22 with the various compositions shown in Table 2, and then hot forged at 1000 to 1250°C, heat-treated in the range of 1000 to 1100°C, drawn to a diameter of 1.0 mm, and wound on a spool.
[0068] [Table 1]
[0069] [Table 2]
[0070] Using the obtained base steel plate and filler metal, two steel plates each having a plate thickness t of 1.0 mm and 2.0 mm were prepared as shown in Fig. 1, and a gapless I-groove 3 was formed between each of the steel plates 1, and a copper backing 2 was attached to the back side to prepare a test specimen. This test specimen was TIG welded using the filler metal listed in Table 2 under the conditions listed in Table 3 to prepare a welded joint.
[0071] The cooling rate in the temperature range of 1300 to 800°C of the weld metal was obtained by direct measurement using a thermocouple as described in Non-Patent Document 1. In addition, by setting the welding conditions as described in Table 3, the cooling rate was adjusted in the range of 15 to 25°C / sec in the above temperature range in condition 1, and the cooling rate was adjusted in the range of 3 to 10°C / sec in condition 2. Thereafter, in order to evaluate the cracking resistance and hydrogen embrittlement resistance of the weld metal, a tensile test and the like were performed under the conditions described below. In addition, the test specimen with a plate thickness t of 1.0 mm was used to evaluate the cracking resistance, and the test specimen with a plate thickness t of 2.0 mm was used to evaluate the hydrogen embrittlement resistance.
[0072] [Table 3]
[0073] (Crack resistance) The crack resistance of the weld metal was evaluated by visual observation of the bead appearance and by a tensile test in air. For the tensile test, the excess weld was removed and a plate-shaped test piece 25 mm wide and 94 mm long was taken in the longitudinal direction of the bead, with the parallel part of the test piece being 4 mm wide and 20 mm long. The test piece was also adjusted so that the weld metal was located near the center of the length of the parallel part. A plate-shaped test piece of the base steel plate was prepared as a comparison material. The tensile test was carried out at room temperature and at a strain rate of 2.5 x 10 -3It was done at / s.
[0074] When no cracks were observed by visual observation of the bead appearance, and when the tensile test showed that the fracture occurred not in the weld metal but in the base metal, the specimen was marked with "◎" as an example of particularly excellent crack resistance. Except for the above, when the fracture occurred in the weld metal, the specimen was marked with "○" as an example of good crack resistance when the relative fracture elongation was ≥ 0.90. On the other hand, when cracks were observed visually, or when no cracks were observed visually but the relative fracture elongation was < 0.90, the specimen was marked with "×" as the specimen had poor crack resistance. The relative fracture elongation was calculated using the following formula (a). Relative fracture elongation = fracture elongation in tensile test including weld metal / fracture elongation in tensile test of base metal (a)
[0075] (Hydrogen embrittlement resistance) The hydrogen embrittlement resistance of the weld metal was evaluated by a slow strain rate tensile test at 0°C, 70 MPa, H2 and at 0.1 MPa, N2. For the tensile test, as shown in Figure 1, the excess reinforcement of the welded part of the steel plate 1 with a thickness of 2.0 mm was removed, and the plate-shaped test specimens described above were taken. The tensile test was performed at 0°C, a strain rate of 10 -5 The tensile test was performed at 1000 s / s. The breaking strength (TS) and breaking elongation (EL) were measured in the tensile test, and the hydrogen embrittlement resistance was evaluated using the breaking strength-breaking elongation balance (TS × EL) given by equation (a).
[0076] Evaluation value = {(TS × EL in 70 MPa H2) / (TS × EL in 0.1 MPa N2) (b) When the evaluation value calculated from formula (b) exceeds 0.9, the hydrogen embrittlement resistance is deemed to be particularly excellent, and is marked with a double circle. In addition, except for the above, when the evaluation value is 0.8 or more, the hydrogen embrittlement resistance is deemed to be good, and is marked with a circle. On the other hand, when the evaluation value is less than 0.8, the hydrogen embrittlement resistance is deemed to be poor, and is marked with a cross. The results are summarized in Table 4 below.
[0077] [Table 4]
[0078] Test Nos. 1 to 17, which satisfied the chemical composition of the present invention, were rated as ◎ or ◯ for the cracking resistance and hydrogen embrittlement resistance of the weld metal, which were the same as the examples of the present invention. Test Nos. 2, 6, 10, 11, and 14 to 17 satisfied the preferred ranges of P, S, B, Mg, Cu, and O of the present invention, and the cracking resistance and hydrogen embrittlement resistance of the weld metal were rated as ◎. On the other hand, Test Nos. 5, 9, and 13 were welding under more preferred conditions, and although they fell outside the preferred ranges of P, S, B, Mg, Cu, and O of the present invention, the cracking resistance and hydrogen embrittlement resistance of the weld metal were rated as ◎.
[0079] Test Nos. 18 to 25, which do not satisfy the chemical composition of the present invention, were poor in at least one of the cracking resistance and hydrogen embrittlement resistance of the weld metal even when the preferable welding conditions were implemented. Test Nos. 18, 19, 21, 22, 23, and 24 had poor cracking resistance because any of P, S, B, Mg, Cu, and O related to the cracking resistance of the weld metal did not satisfy the provisions of the present invention. Test No. 20 satisfied the provisions of P, S, B, Mg, Cu, and O, but had a low f value, so had poor hydrogen embrittlement resistance. Test No. 25 satisfied the provisions of P, S, B, Mg, Cu, and O, but had a low Ni content, so had poor hydrogen embrittlement resistance. [Industrial Applicability]
[0080] The welding filler metal according to the present invention has excellent resistance to cracking and hydrogen embrittlement of the weld metal, and is suitable for welding austenitic stainless steels for high-pressure hydrogen gas applications.
Claims
1. The chemical composition, in mass%, is C: 0.10% or less, Si: 1.0% or less, Mn: 8.0 to 11.0%, P: 0.030% or less, S: 0.0030% or less, Cr: 15.0-18.0%, Ni: 7.0-9.0%, N: 0.15-0.25%, B: 0.0002-0.01%, Mg: 0.0001 to 0.0050%, Cu: less than 1.00% Mo: 0.5% or less, O: 0.0050% or less, Al: 0-0.20%, Ca: 0-0.01%, Nb: 0 to 0.50%, Ti: 0 to 0.50%, V: 0-0.50%, W: 0-0.50%, Zr: 0 to 0.50%, Co: 0 to 0.50%, Ga: 0 to 0.010%, Hf: 0-0.10%, REM: 0-0.10%, The balance is Fe and impurities. An austenitic stainless steel welding filler metal, having an f-value calculated by the following formula (i) of more than 30.0 and less than 33.5: f value=Ni+0.72Cr+0.88Mo+1.11Mn-0.27Si+12.93C+7.55N...(i) In the above formula (i), each element symbol represents the content (mass%) of each element contained in the steel, and when the element is not contained, it is set to zero.
2. The chemical composition, in mass%, Al: 0.003-0.20%, Ca: 0.0002-0.01%, Nb: 0.002 to 0.50%, Ti: 0.002 to 0.50%, V: 0.01-0.50%, W: 0.001-0.50%, Zr: 0.01-0.50%, Co: 0.01 to 0.50%, Ga: 0.001 to 0.010%, Hf: 0.01 to 0.10%, and REM: 0.01-0.10%, The austenitic stainless steel welding filler metal according to claim 1, comprising at least one selected from the group consisting of:
3. The chemical composition is P: 0.025% or less, S: 0.0020% or less, B: 0.0002 to 0.0020%, Mg: 0.0001 to 0.0020%, Cu: 0.50% or less, O: 0.0030% or less, 3. The austenitic stainless steel welding filler metal according to claim 1 or 2,
Citation Information
Patent Citations
Gas shielded welding wire for austenitic stainless steel
JP1995314178A
HIGH-Mn AUSTENITIC STAINLESS STEEL AND METAL PART FOR CLOTHING
JP2010196142A
AUSTENITIC HIGH Mn STAINLESS STEEL WELD JOINT FOR HIGH-PRESSURE HYDROGEN GAS AND LIQUID HYDROGEN AND METHOD OF PRODUCING THE SAME
JP2015171729A
Austenitic stainless steel wire material and wire for nonmagnetic game ball
JP2015196837A
Austenite stainless steel cast slab, and steel pipe, bar steel, and plank including the same
JP2021109998A