Zinc secondary battery
The zinc secondary battery design with a hydroxide ion conductive separator and additives enhances cycle performance by preventing dendrite penetration and maintaining electrode shape, thus extending battery life.
Patent Information
- Application Number
- JP2023508457
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-26
- Filing Date
- 2021-11-25
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2041-11-25
AI Technical Summary
Zinc secondary batteries suffer from shortened lifespan due to zinc dendrite formation causing short circuits and negative electrode shape changes, leading to inadequate charge/discharge cycle performance.
A zinc secondary battery design incorporating a hydroxide ion conductive separator to isolate positive and negative electrodes, using additives like nonionic water-absorbing polymers and electrolyte components that form complexes with zinc to suppress shape changes, and optimizing charge/discharge parameters to fall within specific performance ranges.
Improves charge/discharge cycle performance by preventing zinc dendrite penetration and maintaining electrode integrity, extending the battery's cycle life and reliability.
Smart Images

Figure 0007564941000012 
Figure 0007564941000013 
Figure 0007564941000014
Abstract
Description
[Technical field]
[0001] The present invention relates to a zinc secondary battery. [Background technology]
[0002] In zinc secondary batteries such as nickel-zinc secondary batteries and air-zinc secondary batteries, it is known that metallic zinc precipitates in the form of dendrites from the negative electrode during charging, penetrates the voids in the separator such as nonwoven fabric, and reaches the positive electrode, resulting in a short circuit. Such a short circuit caused by zinc dendrites shortens the repeated charge-discharge life.
[0003] In order to address the above problems, a battery equipped with a layered double hydroxide (LDH) separator that selectively allows hydroxide ions to pass through while preventing the penetration of zinc dendrites has been proposed (see, for example, Patent Document 1 (WO 2016 / 076047) and Patent Document 2 (WO 2019 / 124270)). In addition, although they cannot be called LDHs, LDH-like compounds are known as hydroxides and / or oxides with a layered crystal structure similar to LDHs, and exhibit hydroxide ion conductive properties similar enough to be collectively referred to as hydroxide ion conductive layered compounds together with LDHs. For example, Patent Document 3 (WO 2020 / 255856) discloses a hydroxide ion conductive separator that includes a porous substrate and a layered double hydroxide (LDH)-like compound that blocks the pores of the porous substrate.
[0004] Meanwhile, another factor that shortens the life of zinc secondary batteries is the shape change of zinc, which is the negative electrode active material. That is, as zinc dissolves and precipitates repeatedly due to repeated charging and discharging, the shape of the negative electrode changes, causing high resistance due to blockage of pores, a decrease in the charge active material due to accumulation of isolated zinc, etc., resulting in a problem that charging and discharging becomes difficult. In order to address this problem, Patent Document 4 (WO 2020 / 049902) proposes using ZnO particles in combination with at least two selected from (i) metal Zn particles of a predetermined particle size, (ii) a predetermined metal element, and (iii) a binder resin having a hydroxyl group for use in the negative electrode. It is said that this negative electrode can suppress the deterioration of the negative electrode due to repeated charging and discharging in a zinc secondary battery, improve durability, and thereby extend the cycle life.
[0005] Furthermore, Patent Document 5 (Japanese Patent No. 6190101) discloses a negative electrode composite material containing a negative electrode active material such as metallic Zn or ZnO, a polymer such as an aromatic group-containing polymer, an ether group-containing polymer, or a hydroxyl group-containing polymer, and a conductive assistant, and describes that the negative electrode composite material is suitable for forming a storage battery that exhibits excellent battery performance such as high cycle characteristics, rate characteristics, and Coulombic efficiency while suppressing shape change of the electrode active material, morphological changes of the electrode active material such as dendrites, dissolution, corrosion, and passivation.
[0006] Furthermore, Patent Document 6 (International Publication No. 2020 / 049901) discloses a zinc secondary battery in which the electrolyte further contains a protein capable of forming a complex with Zn and / or a derivative and / or decomposition product thereof, or a polyphenol capable of forming a complex with Zn and / or a derivative and / or decomposition product thereof, and preferred examples of such substances include casein, leucine, and tannic acid. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2016 / 076047 [Patent Document 2] International Publication No. 2019 / 124270 [Patent Document 3] International Publication No. 2020 / 255856 [Patent Document 4] International Publication No. 2020 / 049902 [Patent Document 5] Patent No. 6190101 [Patent Document 6] International Publication No. 2020 / 049901 Summary of the Invention
[0008] However, the charge-discharge cycle performance of existing zinc secondary batteries is not necessarily sufficient, and further improvement in the charge-discharge cycle performance is required.
[0009] The present inventors have now discovered that the charge-discharge cycle performance can be improved by constructing a zinc secondary battery so that the results of a specified charge-discharge cycle test fall within a range that satisfies y≧−0.10x+100 and y≦−0.01x+100 in a coordinate system consisting of an x-axis to which the cycle number is assigned and a y-axis to which the remaining area ratio (%) of the negative electrode plate according to the cycle number is assigned.
[0010] It is therefore an object of the present invention to provide a zinc secondary battery that exhibits improved charge-discharge cycle performance.
[0011] According to one aspect of the present invention, a positive electrode plate including a positive electrode active material; A negative electrode plate including a negative electrode active material including at least one selected from the group consisting of zinc, zinc oxide, zinc alloys, and zinc compounds; a hydroxide ion conductive separator that separates the positive electrode plate and the negative electrode plate so as to be capable of conducting hydroxide ions; An electrolyte; A zinc secondary battery having a unit cell including the above-mentioned, wherein the zinc secondary battery is subjected to a charge-discharge cycle test under the following conditions: - Current density: 12.5mA / cm 2 - Temperature: 25℃ - Charge / discharge rate: 0.5C - Depth of discharge (DOD): 70% - Charging: constant current (CC) charging (cutoff voltage 1.9V) followed by constant voltage (CV) charging - Discharge: Constant current (CC) discharge (cut-off voltage 1.4V) - Pause time when switching between charging and discharging: 5 minutes - Number of cycles: 40 or more If you go with In a coordinate system consisting of an x-axis to which the number of cycles is assigned and a y-axis to which the remaining area ratio (%) of the negative electrode plate according to the number of cycles is assigned, the results of the charge-discharge cycle test are y ≧ -0.10x+100, and y≦-0.01x+100 The zinc secondary battery is provided within the range of the above. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a nickel-zinc secondary battery according to the present invention. [Diagram 2] FIG. 2 is a diagram showing an example of a cross section of the nickel-zinc secondary battery shown in FIG. 1 taken along line AA'. [Diagram 3] 1 is a graph plotting the residual area ratio of the negative electrode at each cycle number obtained in Examples 1 to 85. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Zinc secondary battery The zinc secondary battery of the present invention is not particularly limited as long as it is a secondary battery using zinc as the negative electrode and an alkaline electrolyte (typically an aqueous alkali metal hydroxide solution). Therefore, it can be a nickel-zinc secondary battery, a silver oxide zinc secondary battery, a manganese oxide zinc secondary battery, an air zinc secondary battery, or any other type of alkaline zinc secondary battery. For example, it is preferable that the positive electrode plate contains nickel hydroxide and / or nickel oxyhydroxide, thereby making the zinc secondary battery a nickel-zinc secondary battery. Alternatively, the positive electrode plate may be an air electrode layer, thereby making the zinc secondary battery an air zinc secondary battery.
[0014] 1 and 2 show an embodiment of a zinc secondary battery according to the present invention. The zinc secondary battery 10 shown in FIGS. 1 and 2 includes a battery element 11 in a sealed container 20, and the battery element 11 includes a unit cell 10a including a positive electrode plate 12, a negative electrode plate 14, a hydroxide ion conductive separator 16, and an electrolyte 18. The positive electrode plate 12 includes a positive electrode active material. The negative electrode plate 14 includes a negative electrode active material, which includes at least one selected from the group consisting of zinc, zinc oxide, zinc alloys, and zinc compounds. The hydroxide ion conductive separator 16 separates the positive electrode plate 12 and the negative electrode plate 14 so as to be conductive to hydroxide ions. The zinc secondary battery 10 is then subjected to a charge-discharge cycle test under the following conditions: - Current density: 12.5mA / cm 2 - Temperature: 25℃ - Charge / discharge rate: 0.5C - Depth of discharge (DOD): 70% - Charging: constant current (CC) charging (cutoff voltage 1.9V) followed by constant voltage (CV) charging - Discharge: Constant current (CC) discharge (cut-off voltage 1.4V) - Pause time when switching between charging and discharging: 5 minutes - Number of cycles: 40 or more When the charge-discharge cycle test is performed, in a coordinate system having an x-axis to which the cycle number is assigned and a y-axis to which the remaining area rate (%) of the negative electrode plate according to the cycle number is assigned, the result of the charge-discharge cycle test falls within a range that satisfies y≧−0.10x+100 and y≦−0.01x+100.
[0015] In this way, by configuring a zinc secondary battery so as to fall within the range of the above-mentioned region, the charge-discharge cycle performance is improved. By using such parameters or indicators, a zinc secondary battery with excellent charge-discharge cycle performance can be conveniently identified. For example, according to the present invention, when configuring a zinc secondary battery with desired specifications, it is possible to relatively accurately predict the long-term performance of the cycle performance, such as the cycle life, of the zinc secondary battery by simply checking whether or not the range of the above-mentioned region is satisfied by a relatively small number of charge-discharge cycle tests (for example, 40 times, 100 times, 150 times, 200 times, etc.).
[0016] y≧-0.10x+100 is a formula that defines the lower limit of the above region, more preferably y≧-0.09x+100, and even more preferably y≧-0.05x+100. On the other hand, y≦-0.01x+100 is a formula that defines the upper limit of the above region, and the preferred upper limit is y≦-0.02x+100, and more preferably y≦-0.03x+100. That is, the preferred region is a region that satisfies y≧-0.09x+100 and y≦-0.02x+100, and more preferably a region that satisfies y≧-0.05x+100 and y≦-0.03x+100. In these preferred regions, a zinc secondary battery exhibiting further improved charge-discharge cycle performance can be provided. It goes without saying that the above region satisfies x≧40 (because there is a condition of 40 or more cycles), but the upper limit is not particularly limited. However, the above range typically satisfies x≦1200, x≦1000, x≦800, x≦600, x≦400, x≦200, x≦150, or x≦100.
[0017] In order to configure a zinc secondary battery so as to fall within the above range, it is preferable to add an additive to the negative electrode plate 14 and / or the electrolyte 18, which has an effect of suppressing negative electrode shape change.
[0018] A preferred additive to be added to the negative electrode plate 14 is a nonionic water-absorbing polymer. Preferred examples of the nonionic water-absorbing polymer include polyalkylene oxide water-absorbing resin, polyvinyl acetamide water-absorbing resin, polyvinyl alcohol (PVA resin), and polyvinyl butyral (PVB resin), and more preferably, polyalkylene oxide water-absorbing resin. Commercially available polyalkylene oxide water-absorbing resins can be used. The nonionic water-absorbing polymer may contain at least one selected from hydrophilic ether groups, hydroxyl groups, amide groups, and acetamide groups. The presence of these functional groups can provide a water-absorbing and releasing function that is more favorable for the battery reaction. The nonionic water-absorbing polymer may remain as particles in the negative electrode, or may cover the active material. When the active material is covered with the nonionic water-absorbing polymer, a method of adding the nonionic water-absorbing polymer in a slurry form, or a method of heating and melting the nonionic water-absorbing polymer during production can be considered. In the latter case, the melting point of the nonionic water-absorbing polymer is preferably 45°C to 350°C, more preferably 45°C to 200°C, and even more preferably 50°C to 100°C. The content of the nonionic water-absorbing polymer in the negative electrode plate 14 is preferably 0.01 to 6.0 parts by weight in terms of solid content, more preferably 0.01 to 5.5 parts by weight, even more preferably 0.05 to 5.0 parts by weight, and particularly preferably 0.07 to 4.0 parts by weight, when the content of the ZnO particles is 100 parts by weight. In addition, the nonionic water-absorbing polymer is preferably particulate. In this case, the particle size of the nonionic water-absorbing polymer is preferably 10 to 200 μm, more preferably 15 to 180 μm, even more preferably 20 to 160 μm, and particularly preferably 30 to 150 μm. It is not necessary that all the particles of the nonionic water-absorbing polymer are within the above numerical range, and it is sufficient that the average particle size D50 falls within the above numerical range.
[0019] Examples of preferred additives to be added to the electrolyte 18 include proteins capable of forming a complex with Zn and / or derivatives and / or decomposition products thereof, or polyphenols capable of forming a complex with Zn and / or derivatives and / or decomposition products thereof (see Patent Document 6). That is, the electrolyte may contain proteins capable of forming a complex with Zn, but a part or all of the proteins may exist as derivatives and / or decomposition products thereof (e.g., peptides and amino acids). Alternatively, the electrolyte may contain polyphenols capable of forming a complex with Zn, but a part or all of the proteins may exist as derivatives and / or decomposition products of polyphenols. The protein as an additive is not particularly limited as long as it is capable of forming a complex with Zn. Examples of such proteins include casein and gelatin, and casein is particularly preferred. Proteins such as casein may form micelles in the electrolyte. Derivatives of proteins such as casein are not particularly limited as long as they are compounds modified to an extent that the structure or properties of the protein are not significantly changed by the introduction or substitution of functional groups, oxidation, reduction, or substitution of atoms, and examples thereof include sodium salts and potassium salts. Examples of decomposition products of proteins such as casein include polypeptides, tripeptides, dipeptides, and amino acids such as glutamic acid, aspartic acid, leucine, isoleucine, histidine, methionine, glycine, proline, tyrosine, and lysine. From the viewpoint of extending the cycle life, preferred examples of amino acids include aspartic acid, methionine, glycine, leucine, and isoleucine, more preferably glycine, leucine, and isoleucine, particularly preferably leucine and isoleucine, and most preferably leucine. The polyphenol as an additive is not particularly limited as long as it can form a complex with Zn. Examples of such polyphenols include hydrolyzed (pyrogallol-type) tannins and condensed (catechol-based) tannins, preferably hydrolyzed (pyrogallol-type) tannins, and more preferably tannic acid, which is one of the hydrolyzed (pyrogallol-type) tannins.The derivatives of polyphenols such as tannic acid are not particularly limited as long as they are modified to such an extent that the structure and properties of the polyphenols are not significantly changed by the introduction or substitution of functional groups, oxidation, reduction, atomic substitution, etc. Examples of derivatives of tannic acid include compounds having a molecular structure in which at least a portion of the hydroxyl groups contained in the tannic acid molecule is substituted with an alkyl ether group or an alkyl ester group, etc. Examples of decomposition products of tannic acid include compounds produced by hydrolyzing at least a portion of the ester bonds in the tannic acid molecule.
[0020] In addition to the additives described above, various additives shown in Table 1 below can be used to configure a zinc secondary battery so as to fall within the range described above. All of these additives are well known and are considered to be effective in suppressing the shape change of the negative electrode.
[0021] [Table 1]
[0022] The positive electrode plate 12 includes a positive electrode active material. The positive electrode active material includes nickel hydroxide and / or nickel oxyhydroxide. Typically, the positive electrode plate 12 further includes a positive electrode current collector (not shown), and the positive electrode current collector preferably has a positive electrode current collector tab 13 extending from an end (e.g., an upper end) of the positive electrode plate 12. A preferred example of the positive electrode current collector is a nickel porous substrate such as a foamed nickel plate. In this case, for example, a paste containing an electrode active material such as nickel hydroxide is uniformly applied onto a nickel porous substrate and dried to preferably produce a positive electrode plate consisting of a positive electrode / positive electrode current collector. At that time, it is also preferred to perform a press treatment on the dried positive electrode plate (i.e., the positive electrode / positive electrode current collector) to prevent the electrode active material from falling off and improve the electrode density. The positive electrode plate 12 shown in FIG. 2 includes a positive electrode current collector (e.g., foamed nickel), but is not shown. This is because in the case of a nickel-zinc secondary battery, the positive electrode current collector is integrated with the positive electrode active material, and therefore the positive electrode current collector cannot be depicted separately. The nickel-zinc secondary battery 10 preferably further includes a positive electrode current collector plate connected to the tip of the positive electrode current collector tab 13, and more preferably, a plurality of positive electrode current collector tabs 13 are connected to one positive electrode current collector plate. This allows current collection to be performed with a simple configuration and with good space efficiency, and also makes it easier to connect to the positive electrode terminal 26. The positive electrode current collector plate itself may be used as the positive electrode terminal 26.
[0023] The positive electrode plate 12 may contain at least one additive selected from the group consisting of silver compounds, manganese compounds, and titanium compounds, which can promote a positive electrode reaction that absorbs hydrogen gas generated by a self-discharge reaction. The positive electrode plate 12 may further contain cobalt. Cobalt is preferably contained in the positive electrode plate 12 in the form of cobalt oxyhydroxide. In the positive electrode plate 12, cobalt functions as a conductive additive, thereby contributing to an improvement in charge / discharge capacity.
[0024] The negative electrode plate 14 includes a negative electrode active material. The negative electrode active material includes at least one selected from the group consisting of zinc, zinc oxide, zinc alloy, and zinc compound. Zinc may be included in any form of zinc metal, zinc compound, or zinc alloy, so long as it has electrochemical activity suitable for the negative electrode. Preferred examples of the negative electrode material include zinc oxide, zinc metal, calcium zincate, and the like, and a mixture of zinc metal and zinc oxide is more preferred. The negative electrode active material may be configured in a gel form, or may be mixed with the electrolyte 18 to form a negative electrode mixture. For example, a gelled negative electrode can be easily obtained by adding an electrolyte and a thickener to the negative electrode active material. Examples of the thickener include polyvinyl alcohol, polyacrylate, CMC, alginic acid, and the like, and polyacrylic acid is preferred because of its excellent chemical resistance to strong alkali.
[0025] As the zinc alloy, a zinc alloy containing no mercury or lead, known as a mercury-free zinc alloy, can be used. For example, a zinc alloy containing 0.01 to 0.1 mass% indium, 0.005 to 0.02 mass% bismuth, and 0.0035 to 0.015 mass% aluminum is preferable because it has an effect of suppressing hydrogen gas generation. In particular, indium and bismuth are advantageous in terms of improving discharge performance. The use of a zinc alloy for the negative electrode can improve safety by suppressing hydrogen gas generation by slowing down the self-dissolution rate in an alkaline electrolyte.
[0026] The shape of the negative electrode material is not particularly limited, but it is preferably in powder form, which increases the surface area and allows for high-current discharge. The average particle size of the negative electrode material is preferably in the range of 3 to 100 μm in minor axis in the case of a zinc alloy, and within this range, the large surface area makes it suitable for high-current discharge, and it is easy to mix uniformly with the electrolyte and gelling agent, and is easy to handle when assembling a battery.
[0027] Preferably, the negative electrode plate 14 further includes a negative electrode current collector 15, and the negative electrode current collector 15 has a negative electrode current collector tab 15a extending from an end (for example, an upper end) of the negative electrode plate 14. The negative electrode current collector tab 15a is preferably provided at a position that does not overlap with the positive electrode current collector tab 13. The zinc secondary battery 10 preferably further includes a negative electrode current collector plate connected to the tip of the negative electrode current collector tab 15a, and more preferably, a plurality of negative electrode current collector tabs 15a are connected to one negative electrode current collector plate. This allows current collection to be performed with a simple configuration and with good space efficiency, and also makes it easier to connect to the negative electrode terminal 28. The negative electrode current collector plate itself may be used as the negative electrode terminal 28.
[0028] Preferred examples of the negative electrode current collector 15 include copper foil, copper expand metal, and copper punched metal, and more preferably copper expand metal. In this case, for example, a mixture containing zinc oxide powder and / or zinc powder, and optionally a binder (e.g., polytetrafluoroethylene particles) can be applied onto the copper expand metal to preferably produce a negative electrode plate consisting of a negative electrode / negative electrode current collector. In this case, it is also preferable to press the negative electrode plate (i.e., a negative electrode / negative electrode current collector) after drying to prevent the electrode active material from falling off and improve the electrode density.
[0029] The zinc secondary battery 10 may further include a liquid-retaining member 17 in contact with the positive electrode plate 12 and / or the negative electrode plate 14. For example, it is preferable that not only the hydroxide ion conductive separator 16 but also the liquid-retaining member 17 is interposed between the positive electrode plate 12 and the negative electrode plate 14. As shown in FIG. 2, it is preferable that the positive electrode plate 12 and / or the negative electrode plate 14 is covered or wrapped with the liquid-retaining member 17. However, a simple configuration in which the liquid-retaining member 17 is disposed on one side of the positive electrode plate 12 or the negative electrode plate 14 may also be used. In any case, by interposing the liquid-retaining member 17, the electrolyte 18 can be evenly present between the positive electrode plate 12 and / or the negative electrode plate 14 and the hydroxide ion conductive separator 16, and the hydroxide ions can be efficiently exchanged between the positive electrode plate 12 and / or the negative electrode plate 14 and the hydroxide ion conductive separator 16. The liquid-retaining member 17 is not particularly limited as long as it is a member capable of retaining the electrolyte solution 18, but is preferably a sheet-like member. Preferred examples of the liquid-retaining member 17 include nonwoven fabric, water-absorbent resin, liquid-retaining resin, porous sheet, and various spacers, but nonwoven fabric is particularly preferred because it allows the production of a negative electrode structure with good performance at low cost. The liquid-retaining member 17 or nonwoven fabric preferably has a thickness of 10 to 200 μm, more preferably 20 to 200 μm, even more preferably 20 to 150 μm, particularly preferably 20 to 100 μm, and most preferably 20 to 60 μm. If the thickness is within the above range, a sufficient amount of electrolyte solution 18 can be retained in the liquid-retaining member 17 while keeping the overall size of the positive electrode structure and / or negative electrode structure compact and without waste.
[0030] The hydroxide ion conductive separator 16 is provided so as to separate the positive electrode plate 12 and the negative electrode plate 14 in a manner allowing hydroxide ion conductivity. For example, as shown in FIG. 2, the negative electrode plate 14 may be configured to be covered or wrapped with the hydroxide ion conductive separator 16. This makes it possible to fabricate a nickel-zinc secondary battery (particularly a laminated battery thereof) capable of preventing zinc dendrite extension extremely easily and with high productivity, without the need for a complicated sealing joint between the hydroxide ion conductive separator 16 and the battery case. However, a simple configuration in which the hydroxide ion conductive separator 16 is disposed on one side of the positive electrode plate 12 or the negative electrode plate 14 may also be used.
[0031] The hydroxide ion conductive separator 16 is not particularly limited as long as it is a separator capable of isolating the positive electrode plate 12 and the negative electrode plate 14 in a hydroxide ion conductive manner, but is typically a separator that includes a hydroxide ion conductive solid electrolyte and selectively passes hydroxide ions solely by utilizing hydroxide ion conductivity. A preferred hydroxide ion conductive solid electrolyte is a layered double hydroxide (LDH) and / or an LDH-like compound. Therefore, the hydroxide ion conductive separator 16 is preferably an LDH separator. In this specification, an "LDH separator" is defined as a separator that includes an LDH and / or an LDH-like compound and selectively passes hydroxide ions solely by utilizing the hydroxide ion conductivity of the LDH and / or the LDH-like compound. In this specification, an "LDH-like compound" is a hydroxide and / or oxide with a layered crystal structure similar to LDH, which may not be called LDH, and can be said to be equivalent to LDH. However, in a broad sense, "LDH" can be interpreted as including not only LDH but also LDH-like compounds. The LDH separator is preferably composited with a porous substrate. Therefore, the LDH separator preferably further comprises a porous substrate, and is composited with the porous substrate in a form in which the pores of the porous substrate are filled with LDH and / or LDH-like compounds. That is, in a preferred LDH separator, the pores of the porous substrate are blocked with LDH and / or LDH-like compounds so as to exhibit hydroxide ion conductivity and gas impermeability (and therefore function as an LDH separator exhibiting hydroxide ion conductivity). The porous substrate is preferably made of a polymer material, and it is particularly preferred that the LDH is incorporated over the entire thickness of the porous substrate made of a polymer material. For example, known LDH separators such as those disclosed in Patent Documents 1 to 4 can be used. The thickness of the LDH separator is preferably 5 to 100 μm, more preferably 5 to 80 μm, even more preferably 5 to 60 μm, and particularly preferably 5 to 40 μm.
[0032] When the positive electrode plate 12 and / or the negative electrode plate 14 are covered or wrapped with the liquid retaining member 17 and / or the separator 16, it is preferable that the outer edge of the positive electrode plate 12 and / or the negative electrode plate 14 is closed (except for the edge from which the positive electrode current collecting tab 13 and the negative electrode current collecting tab 15a extend). In this case, it is preferable that the closed edge of the outer edge of the liquid retaining member 17 and / or the separator 16 is realized by folding the liquid retaining member 17 and / or the separator 16, or by sealing the liquid retaining members 17 together and / or the separators 16 together. Examples of the preferred sealing method include adhesives, heat welding, ultrasonic welding, adhesive tape, sealing tape, and combinations thereof. In particular, since the LDH separator including the porous base material made of a polymer material has an advantage that it is flexible and therefore easy to bend, it is preferable to form the LDH separator into a long shape and fold it to form a state in which one side of the outer edge is closed. Thermal welding and ultrasonic welding may be performed using a commercially available heat sealer or the like, but in the case of sealing between LDH separators, it is preferable to perform thermal welding and ultrasonic welding by sandwiching the outer peripheral portion of the liquid retaining member 17 between the LDH separators constituting the outer peripheral portion, in order to perform more effective sealing. On the other hand, the adhesive, adhesive tape, and sealing tape may be commercially available products, but it is preferable to use those containing a resin having alkali resistance in order to prevent deterioration in an alkaline electrolyte. From this viewpoint, examples of preferable adhesives include epoxy resin adhesives, natural resin adhesives, modified olefin resin adhesives, and modified silicone resin adhesives, and among them, epoxy resin adhesives are more preferable because they are particularly excellent in alkali resistance. An example of a product of an epoxy resin adhesive is the epoxy adhesive Hysol (registered trademark) (manufactured by Henkel).
[0033] It is preferable that the outer edge of one side, which is the upper end of the separator 16, is open. This open-top structure makes it possible to deal with the problem of overcharging in nickel-zinc batteries and the like. That is, when a nickel-zinc battery or the like is overcharged, oxygen (O 2 ) may occur, but the LDH separator is highly dense and allows only hydroxide ions to pass through, so O 2In this respect, the open-top structure does not allow O 2 can be released above the positive electrode plate 12 and sent to the negative electrode plate 14 side through the upper open portion, thereby 2 The negative electrode active material Zn can be oxidized to ZnO by this oxygen reaction cycle. By using the open-top battery element 11 in a sealed nickel-zinc secondary battery, the overcharge resistance can be improved. Even if the outer edge of one side that is the upper end of the separator 16 or the liquid-retaining member 17 is closed, the same effect as that of the open-type configuration can be expected by providing a vent hole in a part of the closed outer edge. For example, the vent hole may be opened after sealing the outer edge of one side that is the upper end of the LDH separator, or when sealing, a part of the outer edge may be left unsealed so that a vent hole is formed.
[0034] The electrolyte 18 preferably contains an aqueous solution of an alkali metal hydroxide. In FIG. 2, the electrolyte 18 is only partially illustrated because it is distributed throughout the positive and negative plates 12 and 14. Examples of alkali metal hydroxides include potassium hydroxide, sodium hydroxide, lithium hydroxide, and ammonium hydroxide, with potassium hydroxide being more preferable. In order to suppress the self-dissolution of zinc and / or zinc oxide, a zinc compound such as zinc oxide or zinc hydroxide may be added to the electrolyte. As described above, the electrolyte may be mixed with the positive electrode active material and / or the negative electrode active material to be present in the form of a positive electrode mixture and / or a negative electrode mixture. The electrolyte may be gelled to prevent leakage of the electrolyte. As the gelling agent, it is preferable to use a polymer that absorbs the solvent of the electrolyte and swells, and polymers such as polyethylene oxide, polyvinyl alcohol, and polyacrylamide, or starch are used.
[0035] As shown in Fig. 2, the battery element 11 preferably has a positive / negative electrode laminate including a plurality of positive plates 12, a plurality of negative plates 14, and a plurality of separators 16, and is laminated so that the unit of positive plate 12 / separator 16 / negative plate 14 is repeated. That is, the zinc secondary battery 10 preferably has a plurality of unit cells 10a, and the plurality of unit cells 10a as a whole form a multi-layer cell. This is the configuration of a so-called assembled battery or laminated battery, and is advantageous in that a high voltage and a large current can be obtained.
[0036] The sealed container 20 is preferably made of resin. The resin constituting the sealed container 20 is preferably a resin resistant to alkali metal hydroxides such as potassium hydroxide, more preferably a polyolefin resin, ABS resin, or modified polyphenylene ether, and even more preferably ABS resin or modified polyphenylene ether. The sealed container 20 has an upper lid 20a. The sealed container 20 (e.g., the upper lid 20a) may have a pressure relief valve for releasing gas. Also, a group of cases in which two or more sealed containers 20 are arranged may be housed in an outer frame to form a battery module.
[0037] LDH-like compounds According to a preferred embodiment of the present invention, the LDH separator may contain an LDH-like compound. The definition of the LDH-like compound is as described above. Preferred LDH-like compounds are: (a) a hydroxide and / or oxide having a layered crystal structure containing Mg and one or more elements including at least Ti selected from the group consisting of Ti, Y, and Al, or (b) a hydroxide and / or oxide having a layered crystal structure containing (i) Ti, Y, and optionally Al and / or Mg, and (ii) an additional element M which is at least one selected from the group consisting of In, Bi, Ca, Sr, and Ba; or (c) a hydroxide and / or oxide having a layered crystal structure containing Mg, Ti, Y, and optionally Al and / or In, wherein the LDH-like compound in (c) is In(OH) 3 It exists in the form of a mixture with
[0038] According to a preferred embodiment (a) of the present invention, the LDH-like compound may be a hydroxide and / or oxide having a layered crystal structure containing Mg and one or more elements including at least Ti selected from the group consisting of Ti, Y, and Al. Thus, a typical LDH-like compound is a composite hydroxide and / or composite oxide of Mg, Ti, optionally Y, and optionally Al. The above elements may be replaced with other elements or ions to the extent that the basic properties of the LDH-like compound are not impaired, but it is preferable that the LDH-like compound does not contain Ni. For example, the LDH-like compound may further contain Zn and / or K. This can further improve the ionic conductivity of the LDH separator.
[0039] LDH-like compounds can be identified by X-ray diffraction. Specifically, when X-ray diffraction is performed on the surface of the LDH separator, peaks derived from LDH-like compounds are typically detected in the range of 5°≦2θ≦10°, more typically in the range of 7°≦2θ≦10°. As described above, LDH has exchangeable anions and H as intermediate layers between stacked hydroxide base layers. 2 O is present. In this regard, when LDH is measured by X-ray diffraction, a peak due to the crystal structure of LDH (i.e., the (003) peak of LDH) is essentially detected at 2θ=11-12°. In contrast, when an LDH-like compound is measured by X-ray diffraction, a peak is typically detected in the above-mentioned range shifted to the lower angle side from the above-mentioned peak position of LDH. In addition, the interlayer distance of the layered crystal structure can be determined by the Bragg formula using 2θ corresponding to the peak derived from the LDH-like compound in X-ray diffraction. The interlayer distance of the layered crystal structure constituting the LDH-like compound determined in this way is typically 0.883-1.8 nm, more typically 0.883-1.3 nm.
[0040] In the LDH separator according to the above aspect (a), the atomic ratio of Mg / (Mg+Ti+Y+Al) in the LDH-like compound determined by energy dispersive X-ray analysis (EDS) is preferably 0.03 to 0.25, more preferably 0.05 to 0.2. The atomic ratio of Ti / (Mg+Ti+Y+Al) in the LDH-like compound is preferably 0.40 to 0.97, more preferably 0.47 to 0.94. The atomic ratio of Y / (Mg+Ti+Y+Al) in the LDH-like compound is preferably 0 to 0.45, more preferably 0 to 0.37. The atomic ratio of Al / (Mg+Ti+Y+Al) in the LDH-like compound is preferably 0 to 0.05, more preferably 0 to 0.03. Within the above ranges, the alkali resistance is more excellent, and the effect of suppressing short circuits caused by zinc dendrites (i.e., dendrite resistance) can be more effectively realized. Regarding LDH separators, conventionally known LDHs have the general formula: M 2+ 1-x M 3+ x (OH) 2 A n- x / n mH 2 O(in the formula, M 2+ is a divalent cation, M 3+ is a trivalent cation, and A n- is an n-valent anion, n is an integer of 1 or more, x is 0.1 to 0.4, and m is 0 or more). In contrast, the above atomic ratio in the LDH-like compound generally deviates from the above general formula of LDH. For this reason, it can be said that the LDH-like compound in this embodiment generally has a composition ratio (atomic ratio) different from that of conventional LDH. It is preferable to perform the EDS analysis using an EDS analyzer (e.g., X-act, manufactured by Oxford Instruments) by 1) capturing an image at an accelerating voltage of 20 kV and a magnification of 5,000 times, 2) performing three-point analysis with an interval of about 5 μm in the point analysis mode, 3) repeating the above 1) and 2) once more, and 4) calculating the average value of a total of six points.
[0041] According to another preferred embodiment (b) of the present invention, the LDH-like compound may be a hydroxide and / or oxide having a layered crystal structure, comprising (i) Ti, Y, and optionally Al and / or Mg, and (ii) an additional element M. Thus, a typical LDH-like compound is a composite hydroxide and / or composite oxide of Ti, Y, the additional element M, optionally Al, and optionally Mg. The additional element M is In, Bi, Ca, Sr, Ba, or a combination thereof. The above elements may be replaced with other elements or ions to the extent that the basic properties of the LDH-like compound are not impaired, but it is preferred that the LDH-like compound does not contain Ni.
[0042] In the LDH separator according to the above aspect (b), the atomic ratio of Ti / (Mg+Al+Ti+Y+M) in the LDH-like compound determined by energy dispersive X-ray analysis (EDS) is preferably 0.50 to 0.85, more preferably 0.56 to 0.81. The atomic ratio of Y / (Mg+Al+Ti+Y+M) in the LDH-like compound is preferably 0.03 to 0.20, more preferably 0.07 to 0.15. The atomic ratio of M / (Mg+Al+Ti+Y+M) in the LDH-like compound is preferably 0.03 to 0.35, more preferably 0.03 to 0.32. The atomic ratio of Mg / (Mg+Al+Ti+Y+M) in the LDH-like compound is preferably 0 to 0.10, more preferably 0 to 0.02. The atomic ratio of Al / (Mg+Al+Ti+Y+M) in the LDH-like compound is preferably 0 to 0.05, more preferably 0 to 0.04. Within the above range, the alkali resistance is more excellent, and the effect of suppressing short circuits caused by zinc dendrites (i.e., dendrite resistance) can be more effectively realized. Incidentally, LDHs conventionally known as LDH separators are represented by the general formula: M 2+ 1-x M 3+ x (OH) 2 A n- x / n mH 2 O(in the formula, M 2+ is a divalent cation, M 3+ is a trivalent cation, and A n-is an n-valent anion, n is an integer of 1 or more, x is 0.1 to 0.4, and m is 0 or more). In contrast, the above atomic ratio in the LDH-like compound generally deviates from the above general formula of LDH. For this reason, it can be said that the LDH-like compound in this embodiment generally has a composition ratio (atomic ratio) different from that of conventional LDH. It is preferable to perform the EDS analysis using an EDS analyzer (e.g., X-act, manufactured by Oxford Instruments) by 1) capturing an image at an accelerating voltage of 20 kV and a magnification of 5,000 times, 2) performing three-point analysis with an interval of about 5 μm in the point analysis mode, 3) repeating the above 1) and 2) once more, and 4) calculating the average value of a total of six points.
[0043] According to yet another preferred embodiment (c) of the present invention, the LDH-like compound is a hydroxide and / or oxide of a layered crystal structure containing Mg, Ti, Y, and optionally Al and / or In, and the LDH-like compound is In(OH) 3 The LDH-like compound of this embodiment is a hydroxide and / or oxide having a layered crystal structure containing Mg, Ti, Y, and optionally Al and / or In. Thus, a typical LDH-like compound is a composite hydroxide and / or composite oxide of Mg, Ti, Y, optionally Al, and optionally In. The In that can be contained in the LDH-like compound includes not only In that is intentionally added to the LDH-like compound, but also In(OH) 3 The above elements may be unavoidably mixed into the LDH-like compound due to the formation of Ni. The above elements may be replaced with other elements or ions to the extent that the basic properties of the LDH-like compound are not impaired, but it is preferable that the LDH-like compound does not contain Ni. Incidentally, the LDH conventionally known for the LDH separator has the general formula: M 2+ 1-x M 3+ x (OH) 2 A n- x / n mH 2 O(in the formula, M 2+ is a divalent cation, M 3+ is a trivalent cation, and A n-is an n-valent anion, n is an integer of 1 or more, x is 0.1 to 0.4, and m is 0 or more). In contrast, the atomic ratio in the LDH-like compound generally deviates from the above general formula of LDH. Therefore, it can be said that the LDH-like compound in this embodiment generally has a composition ratio (atomic ratio) different from that of conventional LDH.
[0044] The mixture according to embodiment (c) contains not only LDH-like compounds but also In(OH) 3 (typically LDH-like compounds and In(OH) 3 It consists of In(OH) 3 The inclusion of In(OH) in the mixture can effectively improve the alkali resistance and dendrite resistance of the LDH separator. 3 The content of In(OH) is preferably an amount that can improve the alkali resistance and dendrite resistance of the LDH separator without substantially impairing the hydroxide ion conductivity, and is not particularly limited. 3 may have a cubic crystal structure, In(OH) 3 The crystal may be surrounded by an LDH-like compound. 3 can be identified by X-ray diffraction. EXAMPLES
[0045] The present invention will now be further illustrated by the following examples.
[0046] Examples 1 to 75 Simple nickel-zinc secondary battery cells of various specifications were fabricated using the following procedure, and charge-discharge cycle tests were performed.
[0047] (1) Preparation of the positive electrode Paste-type nickel hydroxide positive electrode (capacity density: approx. 700 mAh / cm 3 ) was prepared.
[0048] (2) Preparation of the negative electrode The following various raw materials were prepared. <Negative electrode active material> ZnO powder (Seido Chemical Industry Co., Ltd., JIS standard class 1 grade, average particle size D50: 0.2 μm) Metallic Zn powder (manufactured by DOWA Electronics Co., Ltd., doped with Bi and In, Bi: 70 ppm by weight, In: 200 ppm by weight, average particle size D50: 120 μm) <Additive 1> Milled carbon fiber (product name: DonaCarbo Milt, manufactured by Osaka Gas Chemicals) Acetylene black (product name: Denka Black, manufactured by Denka Co., Ltd.) Carbon nanotubes (product name: VGCF, manufactured by Showa Denko K.K.) S-100 / g (Product name: Chemi-Q S-100, manufactured by Chemic Co., Ltd.) Powdered PTFE (product name: Lubron, manufactured by Daikin Industries, Ltd.) In 2 O 3 Powder (product name: indium oxide, manufactured by Takanami Inorganic Co., Ltd.) <Additive 2> Propylene glycol (PG) (product name: propylene glycol, manufactured by Kanto Chemical Co., Ltd.) <Additive 3> Polyvinyl alcohol (PVA) (product name: Polyvinyl alcohol, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) Polyolefin aqueous dispersion (product name: Chemipearl S100, manufactured by Mitsui Chemicals, Inc.) Polyolefin aqueous dispersion (product name: Chemipearl S650, manufactured by Mitsui Chemicals, Inc.) <Additive 4> PTFE (Product name: Polyflon PTFE F Series, manufactured by Daikin Industries, Ltd.)
[0049] According to the compounding ratios shown in Tables 2A and 2B, ZnO powder was mixed with metal Zn powder and various additives. The resulting mixture was rolled with a roll press to obtain a negative electrode active material sheet. The negative electrode active material sheet was pressed onto a tin-plated copper expand metal to obtain a negative electrode. In this way, 21 types of negative electrode plates shown in Tables 2A and 2B were produced.
[0050] (3) Preparation of electrolyte Ion-exchanged water was added to a 48% aqueous potassium hydroxide solution (special grade, manufactured by Kanto Chemical Co., Ltd.) to adjust the KOH concentration to 5.4 mol%, and then zinc oxide was dissolved at 0.42 mol / L by heating and stirring to obtain an electrolyte solution. In Examples 30 to 32, casein was added to this electrolyte solution in an amount of 2.0 / 50 CC.
[0051] (4) Preparation of evaluation cell As shown in Tables 3 to 8, various negative electrodes were used to prepare cells in the following manner. First, the positive and negative electrodes were wrapped in nonwoven fabric, and current extraction terminals were welded to them. The positive and negative electrodes thus prepared were placed opposite each other via an Mg-Al-Ti-Y-LDH separator, sandwiched between laminate films provided with current extraction ports, and three sides of the laminate film were heat-sealed. An electrolyte was added to the cell container thus obtained with the top open, and the electrolyte was sufficiently permeated into the positive and negative electrodes by evacuation or the like. Thereafter, the remaining side of the laminate film was also heat-sealed to form a simple sealed cell.
[0052] (5) Charge / discharge cycle test A charge-discharge cycle test was carried out on the simple sealed cell at 25°C using a charge-discharge device (TOSCAT3100, manufactured by Toyo Systems Co., Ltd.). This cycle test was carried out at a discharge rate of 0.5C (current density of 12.5mA / cm 2 ) until the battery voltage reached 1.9 V, then continued with constant voltage (CV) charging at 1.9 V until the battery capacity reached 63% of the positive electrode capacity. After a 5-minute charge rest period, the battery was charged at a charge rate of 0.5 C (current density 12.5 mA / cm 2 The charge-discharge cycle was performed the number of times shown in Tables 3 to 8, including discharging at a constant current (CC) at a cutoff voltage of 1.4 V until the depth of discharge (DOD) reached 70%, followed by a 5-minute discharge rest period.
[0053] A planar image of the negative plate of the battery after the charge-discharge cycle test was taken, and the image was analyzed to calculate the remaining area ratio (%) of the negative plate. Specifically, the remaining area ratio of the negative plate is the value obtained by dividing the area of the part (visually recognized as black) where the negative active material (ZnO) remains in the negative plate after the cycle test by the area (visually recognized as black) that was covered with the negative active material (ZnO) in the negative plate before the cycle test, and multiplying the result by 100. The results are shown in Tables 3 to 8 and FIG. 3. [Table 2A]
[0054] [Table 2B]
[0055] [Table 3]
[0056] [Table 4]
[0057] [Table 5]
[0058] [Table 6]
[0059] [Table 7]
[0060] [Table 8]
[0061] Examples 76-85 Simple nickel-zinc secondary battery cells of various specifications were fabricated using the following procedure, and charge-discharge cycle tests were performed.
[0062] (1) Preparation of the positive electrode Paste-type nickel hydroxide positive electrode (capacity density: approx. 700 mAh / cm 3 ) was prepared.
[0063] (2) Preparation of the negative electrode The following various raw materials were prepared. <Negative electrode active material> ZnO powder (Seido Chemical Industry Co., Ltd., JIS standard class 1 grade, average particle size D50: 0.2 μm) Metallic Zn powder (manufactured by DOWA Electronics Co., Ltd., doped with Bi and In, Bi: 70 ppm by weight, In: 200 ppm by weight, average particle size D50: 120 μm) <Additives> Nonionic water-absorbing polymer (sodium polyacrylate, product name: Aquacork C-PF, manufactured by Sumitomo Seika Chemicals Co., Ltd.) In 2 O 3 Powder (product name: indium oxide, manufactured by Takanami Inorganic Co., Ltd.) Propylene glycol (PG) (product name: propylene glycol, manufactured by Kanto Chemical Co., Ltd.) PTFE (Product name: Polyflon PTFE F Series, manufactured by Daikin Industries, Ltd.)
[0064] According to the blending ratios shown in Tables 9 and 10, ZnO powder was mixed with metal Zn powder, polytetrafluoroethylene (PTFE), and other additives, and kneaded with propylene glycol. The resulting mixture was rolled with a roll press to obtain a negative electrode active material sheet. The negative electrode active material sheet was pressed onto a tin-plated copper expand metal to obtain a negative electrode. Various negative electrode plates were thus produced.
[0065] (3) Preparation of electrolyte Ion-exchanged water was added to a 48% aqueous potassium hydroxide solution (special grade, manufactured by Kanto Chemical Co., Ltd.) to adjust the KOH concentration to 5.4 mol%, and then 0.42 mol / L of zinc oxide was dissolved therein by heating and stirring to obtain an electrolyte.
[0066] (4) Preparation of evaluation cell As shown in Tables 9 and 10, various negative electrodes were used to prepare cells in the following manner. First, two positive electrodes and one negative electrode were wrapped in nonwoven fabric, and a current extraction terminal was welded to each electrode. The two positive electrodes and one negative electrode thus prepared were laminated in the order of positive electrode / negative electrode / positive electrode with an Mg-Al-Ti-Y-LDH separator interposed therebetween, and the laminate film was sandwiched between the electrodes and the current extraction port, and the three sides of the laminate film were heat-sealed. An electrolyte was added to the cell container thus obtained with the top open, and the electrolyte was sufficiently permeated into the positive and negative electrodes by evacuation or the like. Then, the remaining side of the laminate film was also heat-sealed to form a simple sealed cell.
[0067] (5) Charge / discharge cycle test A charge-discharge cycle test was carried out in the same manner as in Examples 1 to 75, and the remaining area ratio (%) of the negative electrode plate was measured. The results are shown in Tables 9 and 10 and FIG.
[0068] [Table 9]
[0069] [Table 10]
[0070] result 3 is a graph plotting the results of each of Examples 1 to 85 in a coordinate system consisting of an x-axis to which the cycle number is assigned, and a y-axis to which the remaining area ratio (%) of the negative electrode plate according to the cycle number is assigned. From FIG. 3, it can be seen that when evaluated by a predetermined charge-discharge cycle test, a zinc secondary battery configured to be within the range of a region satisfying y≧-0.10x+100 (preferably y≧-0.09x+100, more preferably y≧-0.05x+100) and y≦-0.01x+100 (preferably y≦-0.02x+100, more preferably y≦-0.03x+100) exhibits improved cycle characteristics (prolonged cycle life).
Claims
1. a positive electrode plate including a positive electrode active material; A negative electrode plate including a negative electrode active material including at least one selected from the group consisting of zinc, zinc oxide, a zinc alloy, and a zinc compound; a hydroxide ion conductive separator that separates the positive electrode plate and the negative electrode plate so as to be capable of conducting hydroxide ions; An electrolyte; A zinc secondary battery having a unit cell including the above-mentioned. The zinc secondary battery is subjected to a charge-discharge cycle test under the following conditions: - Current density: 12.5mA / cm 2 - Temperature: 25℃ - Charge / discharge rate: 0.5C - Depth of discharge (DOD): 70% - Charging: constant current (CC) charging (cut-off voltage 1.9V) followed by constant voltage (CV) charging - Discharge: constant current (CC) discharge (cut-off voltage 1.4V) - Pause time when switching between charging and discharging: 5 minutes - Number of cycles: 40 or more If you go with In a coordinate system having an x-axis to which the number of cycles is assigned and a y-axis to which the remaining area ratio (%) of the negative electrode plate according to the number of cycles is assigned, the results of the charge-discharge cycle test are y≧−0.05x+100, and y≦-0.03x+100 Zinc secondary batteries fall within the range of the above.
2. 2. The zinc secondary battery of claim 1, wherein the hydroxide ion conducting separator is a layered double hydroxide (LDH) separator comprising an LDH and / or an LDH-like compound.
3. The zinc secondary battery of claim 2, wherein the LDH separator further comprises a porous substrate, and the LDH and / or LDH-like compound is composited with the porous substrate in a form filled in the pores of the porous substrate.
4. The zinc secondary battery according to claim 3 , wherein the porous substrate is made of a polymeric material.
5. The zinc secondary battery according to any one of claims 1 to 4, wherein the positive electrode plate contains nickel hydroxide and / or nickel oxyhydroxide, thereby making the zinc secondary battery a nickel-zinc secondary battery.
6. The zinc secondary battery according to any one of claims 1 to 5, wherein the positive electrode plate is an air electrode, thereby forming the zinc secondary battery into an air-zinc secondary battery.
7. 7. The zinc secondary battery according to claim 1, comprising a plurality of said unit cells, the plurality of said unit cells forming a multi-layer cell as a whole.
Citation Information
Patent Citations
Polarization splitter
JP1986090101A
Sealed secondary battery
JP1994096796A
Separator structure body for use in zinc secondary battery
WO2016076047A1
LDH separator and zinc secondary battery
WO2019124270A1
Zinc secondary battery
WO2020049901A1