Two-part curing thermally conductive grease composition, thermally conductive grease, and electronic device
The two-component curing thermally conductive grease composition balances thermal conductivity and electrical insulation by using specific particle sizes and polyorganosiloxanes, addressing the viscosity and applicability issues of existing greases, achieving efficient heat dissipation and insulation for electronic components.
Patent Information
- Application Number
- JP2022528839
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-06-05
- Filing Date
- 2021-06-01
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2041-06-01
AI Technical Summary
Existing thermally conductive greases face challenges in achieving high thermal conductivity while maintaining electrical insulation and low viscosity, as adding conductive fillers for conductivity increases viscosity, and adding insulating fillers for insulation reduces applicability.
A two-component curing thermally conductive grease composition is developed, using metal aluminum powder and thermally conductive fillers with specific particle sizes, combined with polyorganosiloxanes and a hydrosilyl addition reaction catalyst, to balance thermal conductivity, electrical insulation, and low viscosity.
The composition achieves high thermal conductivity (0.5 W/mK or more) with low viscosity, ensuring easy application and effective heat dissipation, while maintaining dielectric breakdown voltage of 1 kV or more, suitable for electronic components.
Smart Images

Figure 0007565354000001 
Figure 0007565354000002 
Figure 0007565354000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a two-part curing type thermally conductive grease composition, a thermally conductive grease, and an electronic device. [Background technology]
[0002] As heat-generating electronic components such as the CPU (Central Processing Unit) of a personal computer become smaller and more powerful, the amount of heat generated per unit area from these electronic components has become very large. The amount of heat generated by these electronic components is about 20 times that of an iron. In order to prevent these heat-generating electronic components from breaking down over the long term, they need to be cooled. Metal heat sinks and cases are used for cooling, and thermally conductive materials are used to efficiently transfer heat from the heat-generating electronic components to cooling parts such as heat sinks and cases. The reason for using these thermally conductive materials is that when a heat-generating electronic component and a heat sink are brought into contact without a thermally conductive material, air is present at the interface when viewed microscopically, which becomes an obstacle to heat transfer. Therefore, by placing a thermally conductive material between the heat-generating electronic component and the heat sink, instead of the air at the interface, heat can be efficiently transferred.
[0003] Thermally conductive materials include thermally conductive pads and sheets made by filling thermosetting resin with thermally conductive powder and forming it into a sheet; thermally conductive grease made by filling flowable resin with thermally conductive powder and allowing it to be spread or made into a thin film; and phase-change type thermally conductive materials that soften or flow at the operating temperature of heat-generating electronic components.
[0004] In recent years, with the increasing speed and miniaturization of SiC and GaN power semiconductors, the temperature of elements has risen to 200°C or higher, creating a great need for thermally conductive materials with high thermal conductivity. In addition, the use of thermally conductive grease is increasing from the viewpoint of reducing the thickness of the material used.
[0005] However, when a large amount of conductive filler with high thermal conductivity such as metal aluminum powder, copper powder, silver powder, etc. is mixed in to improve the thermal conductivity, the thermal conductivity of the thermal conductive grease can be improved, but the insulation deteriorates, making it unusable for electronic devices that require insulation. Also, when a large amount of insulating filler powder such as alumina, aluminum nitride, silica, etc. is mixed in to improve the thermal conductivity, the insulation can be secured, but the viscosity of the thermal conductive grease increases significantly, making it difficult to apply when in use.
[0006] Patent Document 1 describes a thermally conductive grease that contains two types of fine aluminum powder with different average particle sizes and fine alumina as essential components to reduce thermal resistance, and Patent Document 2 proposes a thermally conductive grease that contains metallic aluminum, aluminum nitride, and zinc oxide as essential components, but does not mention whether it has insulating properties. Meanwhile, Patent Document 3 describes that a thermally conductive silicone grease composition that is excellent in both thermal conductivity and electrical insulation can be obtained by optimizing the blending amount of metal powder and the blending amount of zinc oxide powder in liquid silicone. However, zinc oxide powder has a large specific surface area, and when it is highly filled in liquid silicone, the viscosity increases, which causes problems with the coating surface. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2005-170971 A [Patent Document 2] JP 2010-248669 A [Patent Document 3] JP 2007-099821 A Summary of the Invention Problem that the invention is trying to solve
[0008] The present invention has been made in consideration of the above problems, and has an object to provide a two-component curing thermally conductive grease composition that has low viscosity and excellent coatability, and that combines high thermal conductivity and electrical insulation properties, a thermally conductive grease, and an electronic device using the same. [Means for solving the problem]
[0009] As a result of intensive research into achieving the above-mentioned object, the inventors have found that the above-mentioned problems can be solved by mixing metallic aluminum powder having a specific average particle size and thermally conductive filler having a specific average particle size in an appropriate mixing ratio in a two-component curing thermally conductive grease composition, thereby completing the present invention.
[0010] That is, the present invention is as follows. [1] A first agent and a second agent are provided, the first agent comprises 100 parts by weight of a liquid resin (A-1), 140 to 560 parts by weight of metallic aluminum (B-1) having an average particle size of 15 to 100 μm, one or more thermally conductive fillers (C-1) selected from the group consisting of aluminum oxide, aluminum nitride, and boron nitride and having an average particle size in the range of 0.3 to 10 μm, and a hydrosilylation addition reaction catalyst (D-1); the second agent comprises 100 parts by weight of a liquid resin (A-2), 140 to 560 parts by weight of metallic aluminum (B-2) having an average particle size of 15 to 100 μm, and one or more thermally conductive fillers (C-2) selected from the group consisting of aluminum oxide, aluminum nitride, and boron nitride, and having an average particle size in the range of 0.3 to 10 μm; At least one of the thermally conductive filler (C-1) or the thermally conductive filler (C-2) contains a first thermally conductive filler (C-1-1) or a first thermally conductive filler (C-2-1) which is at least one type selected from the group consisting of aluminum oxide, aluminum nitride, and boron nitride and has an average particle size of 0.3 to 1.5 μm. A composition for a two-part curing type thermally conductive grease. [2] The liquid resin (A-1) has two or more alkenyl groups in the molecule, and is -1 The polyorganosiloxane (A-1-1) has a viscosity of 50 to 3000 mPa s at The hydrosilyl addition reaction catalyst (D-1) contains a platinum compound catalyst. The two-component curing thermally conductive grease composition according to [1]. [3] The liquid resin (A-2) has two or more alkenyl groups in the molecule, and is -1 Polyorganosiloxane (A-2-1) having a viscosity of 50 to 3000 mPa s at Contains a polyorganosiloxane (A-2-2) having three or more Si-H groups in the molecule; The two-component curing thermally conductive grease composition according to [1] or [2]. [4] the ratio of the sum of the number of moles of alkenyl groups in the liquid resin (A-1) and the liquid resin (A-2) contained in the first agent and the second agent to the number of moles of Si-H groups in the liquid resin (A-2) contained in the second agent is 0.1 to 5.0. The two-component curing thermally conductive grease composition according to any one of [1] to [3]. [5] The first agent and the second agent are subjected to a shear rate of 10 s at 25°C. -1 The viscosity at is 20 Pa·s to 300 Pa·s. The two-component curing thermally conductive grease composition according to any one of [1] to [4]. [6] [1] to [5], wherein the first and second components of the two-component curing thermally conductive grease composition are cured. Thermally conductive grease. [7] The thermal conductivity is 0.5 W / mK or more, and The dielectric breakdown voltage per mm of thickness is 1 kV or more. The thermal conductive grease according to [6]. [8] A heating element and a metal housing are arranged via the thermal conductive grease according to [6] or [7]. electronic equipment. Effect of the Invention
[0011] According to the present invention, it is possible to provide a two-component curing thermally conductive grease composition that has low viscosity and excellent coatability, and that combines high thermal conductivity with electrical insulation properties, a thermally conductive grease, and an electronic device using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Below, we will explain in detail the embodiment of the present invention (hereinafter referred to as the "present embodiment"); however, the present invention is not limited to this embodiment, and various modifications are possible without departing from the gist of the present invention.
[0013] [Two-component curing type thermally conductive grease composition] The two-part curing thermally conductive grease composition of this embodiment includes a first part and a second part. The first part includes 100 parts by weight of a liquid resin (A-1), 140 to 560 parts by weight of metallic aluminum (B-1) having an average particle size of 15 to 100 μm, one or more thermally conductive fillers (C-1) selected from the group consisting of aluminum oxide, aluminum nitride, and boron nitride and having an average particle size in the range of 0.3 to 10 μm, and a catalyst for hydrosilylation addition reaction (D-1), and may include other components as necessary. The second agent contains 100 parts by weight of a liquid resin (A-2), 140 to 560 parts by weight of metallic aluminum (B-2) having an average particle size of 15 to 100 μm, and one or more thermally conductive fillers (C-2) selected from the group consisting of aluminum oxide, aluminum nitride, and boron nitride and having an average particle size in the range of 0.3 to 10 μm, and may contain other components as necessary.
[0014] Furthermore, in this embodiment, at least one of the thermally conductive filler (C-1) contained in the first agent and the thermally conductive filler (C-2) contained in the second agent includes a first thermally conductive filler (C-1-1) or a first thermally conductive filler (C-2-1) having an average particle size of 0.3 to 1.5 μm and being at least one selected from the group consisting of aluminum oxide, aluminum nitride, and boron nitride. The thermally conductive filler having an average particle size of 0.3 to 1.5 μm contained in the first agent is referred to as the first thermally conductive filler (C-1-1), and the thermally conductive filler having an average particle size of 0.3 to 1.5 μm contained in the second agent is referred to as the first thermally conductive filler (C-2-1).
[0015] First agent, 25℃, shear rate 10s -1 The viscosity in is preferably 20 to 300 Pa·s, more preferably 20 to 250 Pa·s, even more preferably 20 to 200 Pa·s, and even more preferably 20 to 150 Pa·s. When the viscosity of the first agent is 20 Pa·s or more, even when the thermally conductive grease is used in a vertical position, dripping of the thermally conductive grease can be suppressed until the curing reaction occurs, and handling tends to be improved. In addition, when the viscosity of the first agent is 300 Pa·s or less, the applicability when the first agent and the second agent are mixed with a static mixer tends to be improved.
[0016] Second agent, 25℃, shear rate 10s -1 The viscosity in is preferably 20 to 300 Pa·s, more preferably 20 to 250 Pa·s, even more preferably 20 to 200 Pa·s, and even more preferably 20 to 150 Pa·s. When the viscosity of the second agent is 20 Pa·s or more, even when the thermally conductive grease is used in a vertical position, dripping of the thermally conductive grease can be suppressed until the curing reaction occurs, and handling tends to be improved. In addition, when the viscosity of the second agent is 300 Pa·s or less, the applicability when the first agent and the second agent are mixed with a static mixer tends to be improved.
[0017] In addition, when the first and second agents were mixed, the shear rate was 10 s at 25°C. -1 The viscosity in is preferably 20 Pa·s to 300 Pa·s, more preferably 20 Pa·s to 250 Pa·s, even more preferably 20 Pa·s to 200 Pa·s, and still more preferably 20 Pa·s to 150 Pa·s.
[0018] Below, each component contained in the first and second agents will be described in detail.
[0019] (Liquid resins (A-1) and (A-2)) The liquid resins (A-1) and (A-2) are not particularly limited, but may be, for example, silicone resin, epoxy resin, acrylic resin, urethane resin, or phenol resin. Among these, silicone resin is preferred in terms of heat resistance and flexibility. The liquid resins (A-1) and (A-2) may be used alone or in combination of two or more. The term "liquid" refers to a liquid state in which the resin alone has fluidity at room temperature and normal pressure.
[0020] The silicone resin is preferably an addition reaction type silicone resin that is liquid at room temperature.The addition reaction type silicone resin is not particularly limited, but may be, for example, polyorganosiloxane having two or more alkenyl groups in the molecule, or polyorganosiloxane having three or more Si-H groups in the molecule.The alkenyl group of the polyorganosiloxane is preferably vinyl group.
[0021] The first agent preferably contains one of these polyorganosiloxanes as the liquid resin (A-1), and more preferably contains a polyorganosiloxane having an alkenyl group. This prevents the addition reaction of the alkenyl group and the Si-H group caused by the hydrosilyl addition reaction catalyst (D-1) in the first agent. The second agent preferably contains one of these polyorganosiloxanes as the liquid resin (A-2), and more preferably contains a polyorganosiloxane having an Si-H group, and even more preferably contains both a polyorganosiloxane having an alkenyl group and a polyorganosiloxane having an Si-H group.
[0022] In the polyorganosiloxane having an alkenyl group, the bonding position of the alkenyl group is not particularly limited, and the alkenyl group can be bonded to the side chain and / or the terminal of the polyorganosiloxane. The number of alkenyl groups in the polyorganosiloxane having an alkenyl group is not particularly limited as long as it is 2 or more, but is preferably 2 to 10, and more preferably 2 to 5. By having the number of alkenyl groups within the above range, the hardness change at high temperatures of the obtained thermal conductive grease is more suppressed, and the viscosity is reduced, which tends to improve the applicability.
[0023] Furthermore, the alkenyl group content of the polyorganosiloxane having an alkenyl group is preferably 0.10 to 2.0 mol / kg, more preferably 0.10 to 1.0 mol / kg, and even more preferably 0.10 to 0.6 mol / kg. By having the alkenyl group content within the above range, the hardness change at high temperatures of the obtained thermal conductive grease is more suppressed, and the viscosity is reduced, so that the applicability tends to be more improved. In addition, when the polyorganosiloxane has a vinyl group as the alkenyl group, the alkenyl group content is also called the vinyl group content.
[0024] In the polyorganosiloxane having a Si-H group, the bonding position of the Si-H group is not particularly limited, and the Si-H group can be bonded to the side chain and / or the terminal of the polyorganosiloxane. The number of Si-H groups in the polyorganosiloxane having a Si-H group is not particularly limited as long as it is 3 or more, but is preferably 3 to 60, more preferably 10 to 50, and further preferably 25 to 45. By having the number of Si-H groups within the above range, the hardness change at high temperatures of the obtained thermal conductive grease is further suppressed, and the viscosity is reduced, so that the coatability tends to be further improved.
[0025] Furthermore, the Si-H group content of the polyorganosiloxane having Si-H groups is preferably 1.0 to 15 mol / kg, more preferably 3.0 to 12 mol / kg, and even more preferably 5.0 to 10 mol / kg. By having the Si-H group content within the above range, the hardness change at high temperatures of the obtained thermal conductive grease is further suppressed, and the viscosity is reduced, which tends to further improve the applicability.
[0026] The polyorganosiloxane having an alkenyl group in the side chain may have, for example, a constitutional unit represented by the following formula (1). The polyorganosiloxane having an Si-H group in the side chain may have, for example, a constitutional unit represented by the following formula (2). [ka]
[0027] In the above formulas (1) and (2), each R independently represents an alkyl group such as a methyl group, ethyl group, propyl group, hexyl group, octyl group, decyl group, dodecyl group, tetradecyl group, hexadecyl group, or octadecyl group; a cycloalkyl group such as a cyclopentyl group or cyclohexyl group; an aryl group such as a phenyl group or tolyl group; an aralkyl group such as a 2-phenylethyl group or 2-methyl-2-phenylethyl group; or a halogenated hydrocarbon group such as a 3,3,3-trifluoropropyl group, a 2-(perfluorobutyl)ethyl group, a 2-(perfluorooctyl)ethyl group, or a p-chlorophenyl group.
[0028] Among these, R is preferably an alkyl group or an aryl group, and more preferably a methyl group, a phenyl group, or an alkyl group having 6 to 18 carbon atoms.
[0029] In the above formulas (1) and (2), n represents the number of repeating structural units, and can be set to be approximately the same as the number of alkenyl groups or Si-H groups that the polyorganosiloxane has in its side chain.
[0030] Among the above, the liquid resin (A-1) has two or more alkenyl groups in the molecule and is a resin having a shear rate of 10 s at 25°C. -1 The liquid resin (A-2) preferably contains a polyorganosiloxane (A-1-1) having a viscosity of 50 to 3000 mPa·s at 25°C and a shear rate of 10 s. -1 It is preferable that the first agent and the second agent contain a polyorganosiloxane (A-2-1) having a viscosity of 50 to 3000 mPa s at 20° C. and a polyorganosiloxane (A-2-2) having at least three Si-H groups at both ends or in the side chains. This allows the hydrosilylation reaction to proceed more effectively by mixing the first agent and the second agent, and a crosslinked cured product having a three-dimensional network structure with crosslinking bonds can be obtained.
[0031] Polyorganosiloxanes (A-1-1) and (A-2-1) at 25°C and a shear rate of 10 s -1 The viscosity at each of the polyorganosiloxanes (A-1-1) and (A-2-1) is preferably 50 to 3000 mPa·s, more preferably 50 to 1000 mPa·s, and even more preferably 50 to 500 mPa·s. When the viscosity of the polyorganosiloxanes (A-1-1) and (A-2-1) is 50 mPa·s or more, the hardness change at high temperatures of the obtained thermally conductive grease tends to be further suppressed. Also, when the viscosity of the polyorganosiloxanes (A-1-1) and (A-2-1) is 3000 mPa·s or less, the viscosity of the obtained thermally conductive grease tends to be reduced, and the applicability tends to be further improved.
[0032] In addition, polyorganosiloxane (A-2-2) was heated at 25°C and a shear rate of 10 s -1 The viscosity at is preferably 10 to 1000 mPa·s, more preferably 10 to 500 mPa·s, and even more preferably 10 to 200 mPa·s. When the viscosity of the polyorganosiloxane (A-2-2) is 10 mPa·s or more, the hardness change of the obtained thermal conductive grease at high temperatures tends to be more suppressed. In addition, when the viscosity of the polyorganosiloxane (A-2-2) is 1000 mPa·s or less, the viscosity of the obtained thermal conductive grease tends to be reduced and the applicability tends to be further improved. In addition, when the first agent contains a polyorganosiloxane having a Si-H group, the viscosity of the polyorganosiloxane can be the same as that of the polyorganosiloxane (A-2-2).
[0033] The viscosity of each component contained in the liquid resins (A-1) and (A-2) can be measured by a conventional method using a viscometer.
[0034] The content of the liquid resin (A-1) or (A-2) is preferably 2.0 to 25 mass%, more preferably 4.0 to 18 mass%, and even more preferably 6.0 to 13 mass%, based on the total amount of the first agent or the second agent, respectively. By having the content of the liquid resin (A-1) or (A-2) within the above range, the hardness change at high temperatures of the obtained thermal conductive grease is further suppressed, and the viscosity is reduced, which tends to improve the coatability.
[0035] Furthermore, the content of polyorganosiloxane (A-1-1) or (A-2-1) is preferably 70 to 100 mass%, more preferably 80 to 100 mass%, and even more preferably 90 to 100 mass%, based on the total amount of liquid resin (A-1) or (A-2), respectively. By having the content of polyorganosiloxane (A-1-1) or (A-2-1) within the above range, the hardness change at high temperatures of the obtained thermal conductive grease is further suppressed, and the viscosity is reduced, which tends to improve the applicability.
[0036] When the second agent contains both a polyorganosiloxane having an alkenyl group and a polyorganosiloxane having a Si-H group, the content of the polyorganosiloxane having a Si-H group in the second agent is preferably 0.5 to 15 parts by weight, more preferably 1.5 to 10 parts by weight, and even more preferably 2.5 to 5.0 parts by weight, per 100 parts by weight of the total of the polyorganosiloxane having an alkenyl group and the polyorganosiloxane having a Si-H group.
[0037] In addition, the ratio of the total number of moles of alkenyl groups in the liquid resin (A-1) and the liquid resin (A-2) contained in the first and second agents to the number of moles of Si-H groups in the liquid resin (A-2) contained in the second agent is preferably 0.1 to 5.0, more preferably 1.0 to 4.0, and even more preferably 1.5 to 3.5. When the ratio is 0.1 or more, the curing property of the thermal conductive grease tends to be further improved. In addition, when the ratio is 5.0 or less, the embrittlement of the thermal conductive grease is further suppressed, and a suitable elastomer tends to be obtained.
[0038] (Metallic Aluminum (B-1) and (B-2)) The average particle size of the metallic aluminum (B-1) and (B-2) is 15 to 100 μm, preferably 20 to 80 μm, more preferably 20 to 60 μm, and even more preferably 20 to 40 μm. When the average particle size of the metallic aluminum (B-1) and (B-2) is 15 μm or more, the thermal conductivity of the obtained thermal conductive grease can be improved. Furthermore, when the average particle size of the metallic aluminum (B-1) and (B-2) is 100 μm or less, the storage stability of the obtained thermal conductive grease is improved, and separation between the liquid resins (A-1) and (A-2) and the metallic aluminum (B-1) and (B-2) is further suppressed.
[0039] The average particle size of the metallic aluminum (B-1) and (B-2) is a median size and can be measured by the method described in the Examples. The metallic aluminum (B-1) and (B-2) may be the same or different.
[0040] In addition, the metallic aluminum (B-1) and (B-2) may each be used alone or in combination of two or more types with different average particle sizes. When multiple types of metallic aluminum (B-1) and (B-2) are used, each of them is considered to be within the above range. Therefore, for example, even if metallic aluminum having an average particle size of less than 15 μm is mixed with metallic aluminum having an average particle size of more than 100 μm, the metallic aluminum after the mixing does not fall under the metallic aluminum (B-1) and (B-2) of this embodiment.
[0041] The shape of the metallic aluminum (B-1) and (B-2) is not particularly limited, but may be, for example, spherical or irregular. Among these, spherical is preferred. By having such a shape, the viscosity tends to be lowered while increasing the loading amount of the metallic aluminum (B-1) and (B-2).
[0042] The content of metallic aluminum (B-1) or (B-2) is 140 to 560 parts by weight, preferably 200 to 500 parts by weight, and more preferably 200 to 400 parts by weight, per 100 parts by weight of liquid resin (A-1) or (A-2). When the content of metallic aluminum (B-1) or (B-2) is 140 parts by weight or more, the thermal conductivity of the obtained thermal conductive grease is further improved. Also, when the content of metallic aluminum (B-1) or (B-2) is 560 parts by weight or less, the insulating property of the thermal conductive grease is further improved.
[0043] Furthermore, the volume ratio of the metallic aluminum (B-1) or (B-2) is preferably 5 to 70 volume %, more preferably 15 to 50 volume %, and even more preferably 20 to 40 volume %, based on the total of the thermally conductive filler (C-1) and the metallic aluminum (B-1), or the total of the thermally conductive filler (C-2) and the metallic aluminum (B-2), respectively. By having the volume ratio of the metallic aluminum (B-1) or (B-2) within the above range, the thermal conductivity of the thermally conductive grease is improved, and the viscosity is reduced, tending to improve the applicability.
[0044] (Thermal conductive fillers (C-1) and (C-2)) The thermally conductive fillers (C-1) and (C-2) are at least one selected from the group consisting of aluminum oxide, aluminum nitride, and boron nitride. The thermally conductive fillers (C-1) and (C-2) may be of different materials and used alone or in combination of two or more. Among these, it is preferable to use at least aluminum oxide. By using such thermally conductive fillers (C-1) and (C-2), the thermally conductive fillers (C-1) and / or (C-2) penetrate into the gaps of the metallic aluminum (B-1) and / or (B-2), and the thermal conductivity of the obtained thermally conductive grease is further improved.
[0045] The average particle size of the thermally conductive fillers (C-1) and (C-2) is 0.30 to 10 μm, preferably 0.40 to 7.0 μm. When the average particle size of the thermally conductive fillers (C-1) and (C-2) is within the above range, the thermally conductive fillers (C-1) and / or (C-2) can easily enter the gaps of the metallic aluminum (B-1) and / or (B-2). When the average particle size of the thermally conductive fillers (C-1) and (C-2) is 0.30 μm or more, the viscosity of the thermally conductive grease is reduced and the applicability is further improved. When the average particle size of the thermally conductive fillers (C-1) and (C-2) is 10 μm or less, the thermally conductive fillers can enter the gaps of the metallic aluminum (B-1) and / or (B-2) and can be highly filled, so that the thermal conductivity of the thermally conductive grease is further improved.
[0046] The thermally conductive fillers (C-1) and (C-2) may each be used alone or in combination of two or more different average particle sizes or materials. When multiple types of thermally conductive fillers (C-1) and (C-2) are used, each of them is considered to be within the above range. Therefore, for example, even if aluminum oxide having an average particle size of less than 0.30 μm is mixed with aluminum oxide having an average particle size of more than 10 μm, the aluminum oxide after mixing does not fall under the thermally conductive fillers (C-1) and (C-2) of this embodiment.
[0047] The average particle size of the thermally conductive fillers (C-1) and (C-2) is a median size and can be measured by the method described in the Examples. The thermally conductive fillers (C-1) and (C-2) may be the same or different.
[0048] Furthermore, the thermally conductive filler (C-1) may contain at least one of a first thermally conductive filler (C-1-1) having an average particle size of 0.30 to 1.5 μm, a second thermally conductive filler (C-1-2) having an average particle size of 1.6 to 3.5 μm, and a third thermally conductive filler (C-1-3) having an average particle size of 3.7 to 10 μm. Among these, it is preferable to contain the first thermally conductive filler (C-1-1), and it is more preferable to contain the first thermally conductive filler (C-1-1), the second thermally conductive filler (C-1-2), and the third thermally conductive filler (C-1-3). This tends to lower the viscosity of the thermally conductive grease, improve the applicability, and improve the thermal conductivity.
[0049] The thermally conductive filler (C-2) may contain at least one of a first thermally conductive filler (C-2-1) having an average particle size of 0.30 to 1.5 μm, a second thermally conductive filler (C-2-2) having an average particle size of 1.6 to 3.5 μm, and a third thermally conductive filler (C-2-3) having an average particle size of 3.7 to 10 μm. Among these, it is preferable to contain the first thermally conductive filler (C-2-1), and it is more preferable to contain the first thermally conductive filler (C-2-1), the second thermally conductive filler (C-2-2), and the third thermally conductive filler (C-2-3). This tends to lower the viscosity of the thermally conductive grease, improve the applicability, and improve the thermal conductivity.
[0050] In this embodiment, at least one of the thermally conductive filler (C-1) contained in the first agent and the thermally conductive filler (C-2) contained in the second agent contains the first thermally conductive filler (C-1-1) or the first thermally conductive filler (C-2-1). By containing the first thermally conductive filler in the first agent and / or the second agent, the viscosity of the thermally conductive grease is reduced, the applicability is improved, and the thermal conductivity is improved.
[0051] The content of the first thermally conductive filler (C-1-1) or (C-2-1) is preferably 10 to 400 parts by weight, more preferably 50 to 300 parts by weight, and even more preferably 100 to 250 parts by weight, per 100 parts by weight of the liquid resin (A-1) or (A-2), respectively. By having the content of the first thermally conductive filler (C-1-1) or (C-2-1) within the above range, the viscosity of the thermally conductive grease tends to be lowered, the applicability is improved, and the thermal conductivity tends to be improved.
[0052] The content of the second thermally conductive filler (C-1-2) or (C-2-2) is preferably 50 to 700 parts by weight, more preferably 100 to 500 parts by weight, and even more preferably 150 to 450 parts by weight, per 100 parts by weight of the liquid resin (A-1) or (A-2), respectively. By having the content of the second thermally conductive filler (C-1-2) or (C-2-2) within the above range, the viscosity of the thermally conductive grease tends to be lowered, the applicability is improved, and the thermal conductivity tends to be improved.
[0053] The content of the third thermally conductive filler (C-1-3) or (C-2-3) is preferably 200 to 900 parts by weight, more preferably 300 to 800 parts by weight, and even more preferably 400 to 700 parts by weight, per 100 parts by weight of the liquid resin (A-1) or (A-2), respectively. By having the content of the third thermally conductive filler (C-1-3) or (C-2-3) within the above range, the viscosity of the thermally conductive grease is lowered, the applicability is improved, and the thermal conductivity tends to be improved.
[0054] The shape of the thermally conductive filler (C-1) and (C-2) is not particularly limited, but may be, for example, spherical, irregular, etc. Among these, spherical is preferred. By having such a shape, the viscosity tends to be lowered while increasing the loading amount of the thermally conductive filler (C-1) and (C-2).
[0055] The content of the thermally conductive filler (C-1) or (C-2) is preferably 300 to 1800 parts by weight, more preferably 400 to 1700 parts by weight, even more preferably 700 to 1500 parts by weight, and even more preferably 800 to 1250 parts by weight, relative to 100 parts by weight of the liquid resin (A-1) or (A-2). By having the content of the thermally conductive filler (C-1) or (C-2) of 300 parts by weight or more, the gaps of the metallic aluminum (B-1) and / or (B-2) can be filled, and the thermal conductivity of the obtained thermally conductive grease tends to be improved. In addition, by having the content of the thermally conductive filler (C-1) or (C-2) of 1800 parts by weight or less, the viscosity of the obtained thermally conductive grease tends to be lowered, and the applicability tends to be improved.
[0056] (Catalyst for hydrosilation reaction (D-1)) The hydrosilyl addition reaction catalyst (D-1) is not particularly limited, but may be, for example, a platinum compound catalyst, a rhodium compound catalyst, or a palladium compound catalyst. Among these, a platinum compound catalyst is preferred. By using such a hydrosilyl addition reaction catalyst (D-1), the curing property of the liquid resin (A-1) and (B-1) tends to be further improved.
[0057] The platinum compound catalyst is not particularly limited, but may be, for example, a single platinum, a platinum compound, or a platinum-supported inorganic powder. The platinum compound is not particularly limited, but may be, for example, chloroplatinic acid, a platinum-olefin complex, a platinum-alcohol complex, or a platinum coordination compound. The platinum-supported inorganic powder is not particularly limited, but may be, for example, a platinum-supported alumina powder, a platinum-supported silica powder, or a platinum-supported carbon powder. The platinum compound catalyst may be mixed alone when preparing the first agent, or may be mixed in advance with other components, such as a liquid resin (A-1).
[0058] The content of the hydrosilyl addition reaction catalyst (D-1) is preferably 0.1 to 500 ppm, more preferably 1.0 to 400 ppm, and even more preferably 10 to 200 ppm, based on 100 parts by weight of the total of the liquid resins (A-1) and (A-2). By having the content of the hydrosilyl addition reaction catalyst (D-1) within the above range, the curability of the liquid resins (A-1) and (B-1) tends to be further improved.
[0059] (Other Additives (E-1) and (E-2)) In addition to the above components, the first and second agents may contain, as necessary, additives (E-1) and (E-2), such as organosilanes other than the liquid resins (A-1) and (A-2), colorants, and reaction retarders.
[0060] The organosilane is not particularly limited, and examples thereof include organosilanes represented by the following general formula (3): By using such organosilanes, the wettability of the liquid resins (A-1) and (A-2) to the thermally conductive fillers (C-1) and (C-2) is improved, the viscosity is reduced, and the thermal conductivity tends to be improved. R 1 a R 2 b Si(OR 3 ) 4-(a+b) (3) (R 1 are each independently an alkyl group having 1 to 15 carbon atoms; R 2 are each independently a saturated or unsaturated monovalent hydrocarbon group having 1 to 8 carbon atoms; R 3 are each independently an alkyl group having 1 to 6 carbon atoms, a is 1 to 3, b is 0 to 2, and a+b is 1 to 3.
[0061] In formula (3), R 1 are each independently an alkyl group having 1 to 15 carbon atoms, and examples thereof include, but are not limited to, a methyl group, an ethyl group, a propyl group, a hexyl group, a nonyl group, a decyl group, a dodecyl group, and a tetradecyl group. 1is preferably an alkyl group having 6 to 12 carbon atoms.
[0062] R 2 is a saturated or unsaturated monovalent hydrocarbon group having 1 to 8 carbon atoms, and examples thereof include, but are not limited to, alkyl groups such as methyl, ethyl, propyl, hexyl, and octyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; alkenyl groups such as vinyl and allyl; aryl groups such as phenyl and tolyl; aralkyl groups such as 2-phenylethyl and 2-methyl-2-phenylethyl; and halogenated hydrocarbon groups such as 3,3,3-trifluoropropyl, 2-(perfluorobutyl)ethyl, 2-(perfluorooctyl)ethyl, and p-chlorophenyl.
[0063] R 3 represents one or more alkyl groups having 1 to 6 carbon atoms, such as a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, or a hexyl group, and is preferably a methyl group or an ethyl group.
[0064] a is an integer of 1 to 3, and preferably 1. Furthermore, b is an integer of 0 to 2, and preferably 0. Furthermore, a+b is an integer of 1 to 3, and preferably 1.
[0065] The content of organosilane contained in the first or second agent is preferably 0.01 to 10 parts by weight, more preferably 0.1 to 5.0 parts by weight, per 100 parts by weight of the total amount of the metallic aluminum (B-1) or (B-2) and the thermally conductive filler (C-1) or (C-2). If the content of organosilane is within the above range, the wettability can be effectively improved.
[0066] The content of the colorant contained in the first agent or the second agent is preferably 0.05 to 0.2 parts by weight, respectively, relative to 100 parts by weight of the total of the first agent or the second agent.
[0067] The reaction retarder is not particularly limited, but may be, for example, 1-ethynyl-1-cyclohexanol.
[0068] The content of the reaction retarder is preferably 0.05 to 0.2 parts by weight, respectively, relative to 100 parts by weight in total of the first agent and the second agent.
[0069] [Thermal conductive grease] The thermally conductive grease of this embodiment is obtained by curing the first and second parts of the two-part curing thermally conductive grease composition. "Cured" also includes semi-curing of the first and second parts. For example, a two-part curing thermally conductive grease composition in which the hydrosilylation reaction has been partially advanced in advance can be used as the thermally conductive grease.
[0070] The thermal conductivity of the thermally conductive grease at 25°C is preferably 0.5 W / mK or more, more preferably 1.0 W / mK or more, and even more preferably 2.0 W / mK or more. By having a thermal conductivity of 0.5 W / mK or more, good heat dissipation properties can be obtained for electronic components. The thermal conductivity can be measured by the method described in the examples.
[0071] The thermal conductive grease preferably has a breakdown voltage per mm of thickness of 1.0 kV or more, more preferably 1.5 kV or more. A breakdown voltage of 1.0 kV or more ensures sufficient electrical insulation. The breakdown voltage can be measured in accordance with JIS C2110.
[0072] [Electronic equipment] In the electronic device of this embodiment, a heat generating element and a metal housing are disposed with the above-mentioned thermally conductive grease interposed therebetween.
[0073] Here, the heating element is not particularly limited, and examples thereof include heating electronic components such as motors, battery packs, circuit boards used in in-vehicle power systems, power transistors, and microprocessors. Among these, electronic components used in in-vehicle power systems for vehicles are preferred. Also, the metal housing is not particularly limited, and examples thereof include heat sinks configured for the purpose of heat dissipation or heat absorption.
Example
[0074] Hereinafter, the present invention will be described in more detail with reference to examples, but the present invention is not limited to the following examples.
[0075] <A: Liquid resin> a-1: Vinyl group-containing polyorganosiloxane (manufactured by Elkem Silicones: product name "621V100", 25 ° C, shear rate 10 s -1 Viscosity at: 100 mPa·s, vinyl group content: 0.33 mol / kg, average number of vinyl groups in the molecule: 2) a-2: SiH group-containing polyorganosiloxane (manufactured by Elkem Silicones: product name "626V25H7", 25 ° C, shear rate 10 s -1 Viscosity at: 25 mPa·s, Si-H group content: 7 mol / kg, average number of Si-H groups in the molecule: 36)
[0076] <B: Metal aluminum> b-1: Average particle size: 25 μm, spherical, manufactured by Hikari Zairyo Kogyo Co., Ltd., product name "Al-99.7% (-38μm)" b-2: Average particle size: 20 μm, spherical, manufactured by Toyo Aluminium Co., Ltd., product name "TFH-A20P" b-3: Average particle size: 48 μm, spherical, manufactured by Hikari Zairyo Kogyo Co., Ltd., product name "Al-99.7% (-63μm)" b-4: Average particle size: 66 μm, spherical, manufactured by Hikari Zairyo Kogyo Co., Ltd., product name "Al-99.7% (-150μm)"
[0077] <C: Thermal conductive filler> c-1: Aluminum oxide, average particle size: 5 μm, spherical, manufactured by Sumitomo Chemical Co., Ltd., product name "AA-5" c-2: Aluminum oxide, average particle size: 2 μm, spherical, manufactured by Sumitomo Chemical Co., Ltd., product name "AA-2" c-3: Aluminum oxide, average particle size: 0.5 μm, spherical, manufactured by Sumitomo Chemical Co., Ltd., product name "AA-0.5" c-4: Aluminum nitride, average particle size: 5 μm, spherical, manufactured by MARUWA Co., Ltd., product name "A-05-F" c-5: Aluminum nitride, average particle size: 1 μm, spherical, manufactured by MARUWA Co., Ltd., product name "A-01-F" c-6: Boron nitride, average particle size: 5 μm, flaky, manufactured by Denka Co., Ltd., product name "HGP" c-7: Zinc oxide, average particle size: 0.5 μm, spherical, manufactured by Motomura Chemical Co., Ltd., product name "Zinc Oxide Type 1"
[0078] <D: Catalyst for hydrosilylation reaction> Platinum compound catalyst: manufactured by Elkem, product name "Silicol Release Cata 12070"
[0079] <E: Organosilane> e-1: n-Decyltrimethoxysilane (manufactured by Dow Corning Toray Co., Ltd., product name "Z-6210")
[0080] 〔Examples 1 to 10 and Comparative Examples 1 to 3〕 Each raw material was blended in the ratios shown in Tables 1 to 3 in a 2 L trimmix apparatus and kneaded under reduced pressure at room temperature to prepare the first agent and the second agent of each thermally conductive grease composition. In addition, the description regarding the amounts of each component in the table means parts by weight unless otherwise specified.
[0081] (Measurement of average particle size) The average particle size of metallic aluminum B and thermally conductive filler C was measured using a laser diffraction particle size distribution analyzer SALD-20 manufactured by Shimadzu Corporation. The evaluation sample was prepared by adding 50 mL of pure water and 5 g of metallic aluminum B or thermally conductive filler C to be measured to a glass beaker, stirring with a spatula, and then dispersing for 10 minutes in an ultrasonic cleaner. The dispersion of metallic aluminum B or thermally conductive filler C that had been subjected to the dispersion treatment was added drop by drop to the sampler part of the device using a dropper, and measurements were performed when the absorbance stabilized. The average particle size was measured using D50 (median diameter).
[0082] (Viscosity measurement) The viscosity of each of the polyorganosiloxanes a-1, a-2, the first agent, the second agent, and the thermally conductive grease was measured using a rotational rheometer "HANKE MARSIII" (manufactured by Thermo Fisher Scientific). The viscosity was measured using parallel plates with a diameter of 35 mm, a gap of 0.5 mm, a temperature of 25 °C, and a shear rate of 10 s -1 The values obtained under the conditions above were used. The viscosity of the thermally conductive grease obtained by mixing the first and second agents in a static mixer at a volume ratio of 1:1, i.e., the mixed viscosity of the first and second agents, was also measured in the same manner as above.
[0083] [Evaluation of Coatability] The first and second agents were filled into two-liquid syringes (capacity 25cc x 2, manufactured by MIX PAC), and discharged at 25°C using a handgun and a static mixer. Based on the discharge state, the applicability of the first and second agents when mixed was evaluated. The evaluation criteria are as follows: ○: Easier to extrude than static mixer △: It was possible to extrude from a static mixer, but a certain amount of force (approximately 10 kgf) was required. ×: Cannot be discharged from the static mixer
[0084] [Evaluation of thermal conductivity] The thermal conductivity of the thermal conductive grease was measured by a method conforming to ASTM D5470 using a resin material thermal resistance measuring device (manufactured by Hitachi Technology Co., Ltd.). Specifically, the mixture obtained by mixing the first agent and the second agent in a volume ratio of 1:1 using a static mixer was sandwiched between copper jigs with thicknesses of 0.2 mm, 0.5 mm, and 1.0 mm and an area of 10 mm x 10 mm, and the thermal resistance value of each thickness was measured. The thermal conductivity of the thermal conductive resin composition was calculated from the following formula using the slope L of the straight line obtained by taking the thermal resistance value (°C / W) as the vertical axis and the thickness (mm) of the thermal conductive resin composition as the horizontal axis. Thermal conductivity (W / mK)=10 / L
[0085] [Evaluation of dielectric breakdown voltage] For the breakdown voltage sample, the first and second agents were mixed in a static mixer at a volume ratio of 1:1, molded to a thickness of 1 mm, and held for 24 hours to allow the curing reaction to proceed, resulting in a thermally conductive grease cured body. Next, the obtained thermally conductive grease cured body was punched out into a 50 mm square, a 25 mmφ weight was placed on the thermally conductive grease cured body, and a voltage was applied to the weight from 0 kV to 0.2 kV (DC) increments in accordance with JIS C2101. If each voltage could be held for 20 seconds, the voltage was judged to be clear, and the maximum clear value was taken as the breakdown voltage.
[0086] [Table 1] *1: Content (ppm) of components B and C combined
[0087] [Table 2] *1: Content (ppm) of components B and C combined
[0088] [Table 3] *1: Content (ppm) of components B and C combined [Industrial Applicability]
[0089] The two-part curing thermally conductive grease composition of the present invention is a composition for constituting a thermally conductive grease by mixing a first part and a second part and curing the mixture, and has industrial applicability as a thermally conductive grease material used to thermally bond a heating element and a metal housing.
Claims
1. A first agent and a second agent are provided, the first agent comprises 100 parts by weight of a liquid resin (A-1), 140 to 560 parts by weight of metallic aluminum (B-1) having an average particle size of 15 to 100 μm, one or more thermally conductive fillers (C-1) selected from the group consisting of aluminum oxide, aluminum nitride, and boron nitride and having an average particle size in the range of 0.3 to 10 μm, and a hydrosilylation reaction catalyst (D-1); the second agent comprises 100 parts by weight of a liquid resin (A-2), 140 to 560 parts by weight of metallic aluminum (B-2) having an average particle size of 15 to 100 μm, and one or more thermally conductive fillers (C-2) selected from the group consisting of aluminum oxide, aluminum nitride, and boron nitride, and having an average particle size in the range of 0.3 to 10 μm; At least one of the thermally conductive filler (C-1) or the thermally conductive filler (C-2) contains a first thermally conductive filler (C-1-1) or a first thermally conductive filler (C-2-1) which is at least one selected from the group consisting of aluminum oxide, aluminum nitride, and boron nitride and has an average particle size of 0.3 to 1.5 μm. A composition for a two-part curing type thermally conductive grease.
2. The liquid resin (A-1) has two or more alkenyl groups in the molecule, and is -1 The polyorganosiloxane (A-1-1) has a viscosity of 50 to 3000 mPa·s at The hydrosilyl addition reaction catalyst (D-1) contains a platinum compound catalyst. The two-component curing thermally conductive grease composition according to claim 1.
3. The liquid resin (A-2) has two or more alkenyl groups in the molecule, and is -1 Polyorganosiloxane (A-2-1) having a viscosity of 50 to 3000 mPa·s at Contains a polyorganosiloxane (A-2-2) having three or more Si-H groups in the molecule; The two-component curing thermally conductive grease composition according to claim 1 or 2.
4. the ratio of the sum of the number of moles of alkenyl groups in the liquid resin (A-1) and the liquid resin (A-2) contained in the first agent and the second agent to the number of moles of Si—H groups in the liquid resin (A-2) contained in the second agent is 0.1 to 5.0; The two-component curing type thermally conductive grease composition according to any one of claims 1 to 3.
5. The first agent and the second agent are subjected to a shear rate of 10 s at 25° C. -1 The viscosity at is 20 Pa s to 300 Pa s. The two-component curing thermally conductive grease composition according to any one of claims 1 to 4.
6. The two-component curing thermally conductive grease composition according to any one of claims 1 to 5, wherein the first and second components are cured. Thermally conductive grease.
7. The thermal conductivity is 0.5 W / mK or more, and The dielectric breakdown voltage per 1 mm of thickness is 1 kV or more. The thermally conductive grease according to claim 6.
8. A heat generating element and a metal housing are arranged via the thermal conductive grease according to claim 6 or 7. electronic equipment.
Citation Information
Patent Citations
Grease
JP2005170971A
Heat-conductive silicone grease composition and semiconductor device using the same
JP2007099821A
Damping material and damping composite material
JP2010248669A
Thermally conductive silicone composition and cured product of the same
JP2013124257A
Two-pack curable composition set, thermally conductive cured product, and electronic device
WO2020080256A1