Conductive polymer-containing liquid and method for producing same, and conductive laminate and method for producing same

A conductive composite modified with epoxy and quaternary ammonium compounds addresses adhesion and dispersibility issues, enabling the formation of highly conductive layers in ester solvents, improving coating efficiency and conductivity.

JP7565777B2Active Publication Date: 2024-10-11SHIN ETSU POLYMER CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020205853
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-11
Publication Date
2024-10-11
Estimated Expiration
2040-12-11

AI Technical Summary

Technical Problem

Conductive polymer dispersions face issues with low adhesion to hydrophobic film substrates, long drying times, and poor dispersibility in ester solvents, leading to challenges in forming conductive layers with high conductivity.

Method used

A conductive composite containing a π-conjugated conductive polymer and polyanion, modified with an epoxy compound and quaternary ammonium compound, is stabilized in organic solvents like esters using an ester group-containing compound, allowing for improved dispersibility and conductivity.

Benefits of technology

The modified conductive composite achieves stable dispersion in ester solvents, enabling the formation of conductive layers with excellent conductivity and adhesion to film substrates, enhancing productivity and applicability in various coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565777000001
    Figure 0007565777000001
  • Figure 0007565777000002
    Figure 0007565777000002
  • Figure 0007565777000003
    Figure 0007565777000003
Patent Text Reader

Abstract

To provide a conductive polymer-containing liquid containing a conductive complex that is well dispersed in a silicone solution and can be stably dispersed even in an ester solvent such as ethyl acetate and a method for producing the same; and a conductive laminate having a cured layer of the conductive polymer-containing liquid and a method for producing the same.SOLUTION: A conductive polymer-containing liquid contains a conductive complex containing a π-conjugated conductive polymer and a polyanion, and an organic solvent. The polyanion is modified by the reaction between some anion groups of the polyanion and epoxy compounds and quaternary ammonium compounds. The organic solvent contains an ester group-containing compound.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive polymer-containing liquid that contains a π-conjugated conductive polymer and a method for producing the same, and a conductive laminate and a method for producing the same. [Background technology]

[0002] As a coating material for forming a conductive layer, a conductive polymer aqueous dispersion in which poly(3,4-ethylenedioxythiophene) is doped with polystyrene sulfonic acid may be used. Usually, the film substrate on which the conductive layer is applied is made of a hydrophobic plastic film. Therefore, the conductive polymer aqueous dispersion, which is a water-based paint, tends to have low adhesion to the film substrate. In addition, the conductive polymer aqueous dispersion takes a long time to dry, which tends to reduce the productivity of the conductive layer formation. In view of this, a conductive polymer organic solvent dispersion may be used in which the water, which is the dispersion medium of a conductive polymer aqueous dispersion, is replaced with an organic solvent. A known conductive polymer organic solvent dispersion is obtained by freeze-drying a conductive polymer aqueous dispersion containing a conductive complex composed of a π-conjugated conductive polymer and a polyanion to obtain a dried body, and then adding an organic solvent and an amine compound to the dried body (Patent Document 1). However, when an addition curing type silicone is blended into a conductive polymer organic solvent dispersion in order to impart releasability to the conductive layer, the presence of an amine compound can inhibit the curing of the addition curing type silicone.Therefore, in a conductive polymer organic solvent dispersion using an amine compound, there is a problem that the conductive release film is difficult to cure when an addition curing type silicone is blended.

[0003] As a countermeasure to the above problem, it is known to obtain a conductive polymer organic solvent dispersion by adding a cyclic ether compound having at least one of an oxirane group and an oxetane group to a conductive polymer aqueous dispersion containing a conductive complex consisting of a π-conjugated conductive polymer and a polyanion (Patent Document 2). In the method described in Patent Document 2, the anion groups not doped in the π-conjugated conductive polymer are reacted with the oxirane group or oxetane group of the cyclic ether compound to hydrophobize the conductive complex, thereby making the conductive complex dispersible in an organic solvent. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2011-032382 A [Patent Document 2] International Publication No. 2014 / 125827 Summary of the Invention [Problem to be solved by the invention]

[0005] However, even with the method described in Patent Document 2, the dispersibility of the conductive composite in the silicone solution was sometimes insufficient.

[0006] Meanwhile, ester solvents such as ethyl acetate can be mixed in any ratio with many organic solvents such as alcohols, ethers, aromatic compounds, and hydrocarbons, and many of them are fast drying, have low odor, and are low toxicity, making them industrially important solvents. For example, they are widely used as raw materials for printing inks, adhesives, coating materials, etc. On the other hand, even if the conductive complex is hydrophobized so as to dissolve in an organic solvent such as toluene as disclosed in Patent Documents 1 and 2, it is insoluble in an ester-based solvent, and even if it is dispersed with a high-pressure homogenizer, it separates within a few minutes. Therefore, there is a problem that it is difficult to add the conductive complex to raw materials containing an ester-based solvent.

[0007] The present invention provides a conductive polymer-containing liquid containing a conductive complex that has excellent dispersibility in a silicone solution and can be stably dispersed in an ester solvent such as ethyl acetate, and a method for producing the same, a conductive laminate including a cured layer of the conductive polymer-containing liquid, and a method for producing the same. [Means for solving the problem]

[0008] [1] A conductive polymer-containing liquid comprising a conductive complex including a π-conjugated conductive polymer and a polyanion, and an organic solvent, wherein the polyanion is modified by a reaction between a portion of an anion group of the polyanion and an epoxy compound and a quaternary ammonium compound, and the organic solvent contains an ester group-containing compound. [2] The conductive polymer-containing liquid according to [1], wherein the ester group-containing compound is one or more compounds selected from the group of compounds represented by the following formula 1: Formula 1:R 21 -C(=O)-OR 22 [In the formula, R 21 represents a hydrogen atom, a methyl group, or an ethyl group; R 22 represents a linear or branched alkyl group having 1 to 6 carbon atoms.] [3] The conductive polymer-containing liquid according to [1] or [2], wherein the π-conjugated conductive polymer contains poly(3,4-ethylenedioxythiophene) or the polyanion contains polystyrenesulfonic acid. [4] The conductive polymer-containing liquid according to any one of [1] to [3], wherein the epoxy compound has 4 or more carbon atoms, or the quaternary ammonium compound has a substituent on a nitrogen atom having 4 or more carbon atoms. [5] The conductive polymer-containing liquid according to any one of [1] to [4], further comprising an adhesive or a binder component other than the adhesive. [6] A method for producing a conductive polymer-containing liquid, comprising: a precipitation / recovery step of adding an epoxy compound and a quaternary ammonium compound to a conductive polymer aqueous dispersion in which a conductive complex containing a π-conjugated conductive polymer and a polyanion is contained in an aqueous dispersion medium, and then recovering the precipitated reaction product; and an organic solvent adding step of adding an organic solvent to the reaction product to obtain a conductive polymer-containing liquid, wherein the organic solvent contains an ester group-containing compound. [7] The method for producing a conductive polymer-containing liquid according to [6], wherein the ester group-containing compound is one or more selected from the group of compounds represented by the following formula 1: Formula 1:R 21 -C(=O)-OR 22 [In the formula, R 21 represents a hydrogen atom, a methyl group, or an ethyl group; R 22 represents a linear or branched alkyl group having 1 to 6 carbon atoms.] [8] The method for producing a conductive polymer-containing liquid according to [6] or [7], further comprising the step of adding an adhesive or a binder component other than the adhesive. [9] A conductive laminate comprising a substrate and a conductive layer formed on at least one surface thereof, the conductive layer being a cured layer of the conductive polymer-containing liquid according to any one of [1] to [5].

[10] A method for producing a conductive laminate, comprising applying the conductive polymer-containing liquid according to any one of [1] to [5] to at least one surface of a substrate. Effect of the Invention

[0009] In the conductive polymer-containing liquid of the present invention, the conductive complex is stably dispersed in an organic solvent, particularly in a hydrocarbon solvent such as toluene or an ester solvent such as ethyl acetate. This makes the liquid suitable for use as a paint or for mixing with other raw materials containing a hydrocarbon solvent or an ester solvent. When used as a paint, a conductive layer with excellent conductivity can be easily formed. The conductive polymer-containing liquid of the present invention has excellent dispersibility in silicone solutions and can easily form a conductive layer with excellent conductivity. According to the method for producing a conductive polymer-containing liquid of the present invention, a conductive polymer-containing liquid having the above-mentioned effects can be easily produced. According to the method for producing a conductive laminate of the present invention, a conductive laminate having a conductive layer with excellent conductivity can be easily formed.

[0010] This invention is believed to contribute to SDGs Goal 12, "Responsible Consumption and Production."

[0011] In this specification and claims, the lower limit and upper limit of a numerical range indicated with "to" are included in the numerical range. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] ≪Conductive polymer-containing liquid≫ A first aspect of the present invention is a conductive polymer-containing liquid that contains a conductive complex containing a π-conjugated conductive polymer and a polyanion, and an organic solvent, wherein the polyanion has been modified by a reaction between a portion of an anion group of the polyanion and an epoxy compound and a quaternary ammonium compound, and the organic solvent contains an ester group-containing compound. In the conductive polymer-containing liquid of this embodiment, the conductive complex may be in a dispersed state or a dissolved state. In this specification, unless otherwise specified, the dispersed state and the dissolved state are not distinguished, and may simply be referred to as the dispersed state.

[0013] [Conductive composite] The conductive complex contained in the conductive polymer-containing liquid of this embodiment contains a π-conjugated conductive polymer and a polyanion. The polyanion in the conductive complex is doped into the π-conjugated conductive polymer to form a conductive complex having electrical conductivity. In the polyanion, only a part of the anionic groups is doped into the π-conjugated conductive polymer, and there are excess anionic groups that are not involved in the doping. Since the excess anionic groups are hydrophilic groups, the conductive composite in which the excess anionic groups are not modified has water dispersibility.

[0014] (π-conjugated conductive polymer) The π-conjugated conductive polymer may be an organic polymer whose main chain is composed of a π-conjugated system, and examples thereof include polypyrrole-based conductive polymers, polythiophene-based conductive polymers, polyacetylene-based conductive polymers, polyphenylene-based conductive polymers, polyphenylenevinylene-based conductive polymers, polyaniline-based conductive polymers, polyacene-based conductive polymers, polythiophenevinylene-based conductive polymers, and copolymers thereof. From the viewpoint of stability in air, polypyrrole-based conductive polymers, polythiophenes, and polyaniline-based conductive polymers are preferred, and from the viewpoint of transparency, polythiophene-based conductive polymers are more preferred.

[0015] Polythiophene-based conductive polymers include polythiophene, poly(3-methylthiophene), poly(3-ethylthiophene), poly(3-propylthiophene), poly(3-butylthiophene), poly(3-hexylthiophene), poly(3-heptylthiophene), poly(3-octylthiophene), poly(3-decylthiophene), poly(3-dodecylthiophene), poly(3-octadecylthiophene), poly(3-bromothiophene), poly(3-chlorothiophene), and poly(3-iodothiophene). thiophene), poly(3-cyanothiophene), poly(3-phenylthiophene), poly(3,4-dimethylthiophene), poly(3,4-dibutylthiophene), poly(3-hydroxythiophene), poly(3-methoxythiophene), poly(3-ethoxythiophene), poly(3-butoxythiophene), poly(3-hexyloxythiophene), poly(3-heptyloxythiophene), poly(3-octyloxythiophene), poly(3-decyloxythiophene), poly(3-dodecyloxythiophene), oxythiophene), poly(3-octadecyloxythiophene), poly(3,4-dihydroxythiophene), poly(3,4-dimethoxythiophene), poly(3,4-diethoxythiophene), poly(3,4-dipropoxythiophene), poly(3,4-dibutoxythiophene), poly(3,4-dihexyloxythiophene), poly(3,4-diheptyloxythiophene), poly(3,4-dioctyloxythiophene), poly(3,4-didecyloxythiophene), poly(3,4-di dodecyloxythiophene), poly(3,4-ethylenedioxythiophene), poly(3,4-propylenedioxythiophene), poly(3,4-butylenedioxythiophene), poly(3-methyl-4-methoxythiophene), poly(3-methyl-4-ethoxythiophene), poly(3-carboxythiophene), poly(3-methyl-4-carboxythiophene), poly(3-methyl-4-carboxyethylthiophene), and poly(3-methyl-4-carboxybutylthiophene). Examples of polypyrrole-based conductive polymers include polypyrrole, poly(N-methylpyrrole), poly(3-methylpyrrole), poly(3-ethylpyrrole), poly(3-n-propylpyrrole), poly(3-butylpyrrole), poly(3-octylpyrrole), poly(3-decylpyrrole), poly(3-dodecylpyrrole), poly(3,4-dimethylpyrrole), poly(3,4-dibutylpyrrole), poly(3-carboxypyrrole), poly(3-methyl-4-carboxypyrrole), poly(3-methyl-4-carboxyethylpyrrole), poly(3-methyl-4-carboxybutylpyrrole), poly(3-hydroxypyrrole), poly(3-methoxypyrrole), poly(3-ethoxypyrrole), poly(3-butoxypyrrole), poly(3-hexyloxypyrrole), and poly(3-methyl-4-hexyloxypyrrole). Examples of polyaniline-based conductive polymers include polyaniline, poly(2-methylaniline), poly(3-isobutylaniline), poly(2-anilinesulfonic acid), and poly(3-anilinesulfonic acid). Among these π-conjugated conductive polymers, poly(3,4-ethylenedioxythiophene) is particularly preferable because of its excellent conductivity, transparency, and heat resistance. The conductive composite may contain one type of π-conjugated conductive polymer, or two or more types of polymers.

[0016] (Polyanion) A polyanion is a polymer having two or more monomer units each having an anionic group in the molecule. The anionic group of the polyanion functions as a dopant for a π-conjugated conductive polymer, improving the conductivity of the π-conjugated conductive polymer. The anion group of the polyanion is preferably a sulfo group or a carboxy group. Specific examples of such polyanions include polymers having a sulfo group, such as polystyrene sulfonic acid, polyvinyl sulfonic acid, polyallyl sulfonic acid, polyacrylic acid esters having a sulfo group, polymethacrylic acid esters having a sulfo group (for example, poly(4-sulfobutyl methacrylate, polysulfoethyl methacrylate, polymethacryloyloxybenzenesulfonic acid), poly(2-acrylamido-2-methylpropanesulfonic acid), and polyisoprene sulfonic acid; and polymers having a carboxy group, such as polyvinyl carboxylic acid, polystyrene carboxylic acid, polyallyl carboxylic acid, polyacrylic acid, polymethacrylic acid, poly(2-acrylamido-2-methylpropanecarboxylic acid), and polyisoprene carboxylic acid. The polyanion may be a homopolymer in which a single monomer is polymerized, or a copolymer in which two or more monomers are polymerized. Among these polyanions, polymers having a sulfo group are preferred, and polystyrene sulfonic acid is more preferred, since they can provide higher electrical conductivity. The polyanions may be used alone or in combination of two or more kinds. The mass average molecular weight of the polyanion is preferably from 20,000 to 1,000,000, and more preferably from 100,000 to 500,000. The mass average molecular weight is the average molecular weight based on mass measured by gel filtration chromatography and calculated in terms of pullulan.

[0017] When the number of all anionic groups in the polyanion is taken as 100 mol %, the excess anionic groups are preferably from 30 mol % to 90 mol %, more preferably from 45 mol % to 75 mol %.

[0018] The polyanion of the present invention is modified by the reaction of the excess anionic groups (hereinafter also referred to as "partial anionic groups") of the polyanion that are not involved in the dope with both an epoxy compound and a quaternary ammonium compound. That is, the polyanion of the present invention has at least one selected from the group consisting of a substituent (A) formed by the reaction of an epoxy compound with a partial anionic group and a substituent (C) formed by the reaction of a quaternary ammonium compound with a partial anionic group.

[0019] (Substituent A) The substituent (A) is presumed to be a group represented by the following formula (A1) or a group represented by the following formula (A2).

[0020] [ka]

[0021] [In formula (A1), R 1 , R 2 , R 3 , and R 4 are each independently a hydrogen atom or any substituent.

[0022] [ka]

[0023] [In formula (A2), m is an integer of 2 or more, 5 , multiple R 6 , multiple R 7 , and multiple R 8 are each independently a hydrogen atom or an arbitrary substituent, and multiple R 5 may be the same or different, and multiple R 6 may be the same or different, and multiple R 7 may be the same or different, and multiple R 8 may be the same or different.]

[0024] In formulae (A1) and (A2), the bond at the left end represents that the substituent (A) is substituted with a proton of an anionic group. Examples of the anionic group having a substituted proton include an anionic group having an active proton bonded to an oxygen atom, such as "-SO3H".

[0025] In formula (A1), R 1 , R 2 , R 3 , and R 4 Examples of the optional substituent of R include an aliphatic hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, and an aromatic hydrocarbon group having 6 to 20 carbon atoms which may have a substituent. 1 and R 3 may be bonded to form a ring which may have a substituent. For example, R 1 and R 3 and R 1 and a divalent hydrocarbon group obtained by removing any one hydrogen atom from the monovalent hydrocarbon group of R 3 and a divalent hydrocarbon group obtained by removing any one hydrogen atom from the monovalent hydrocarbon group above, are bonded to each other at the carbon atoms from which the hydrogen atom has been removed to form a ring. In formula (A2), R 5 , R 6 , R 7 , and R 8 Examples of the optional substituent of R include an aliphatic hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, and an aromatic hydrocarbon group having 6 to 20 carbon atoms which may have a substituent. 5 and R 7 and may be bonded to form a ring which may have a substituent. Examples of the ring are the same as those mentioned above. In this specification, the term "optionally substituted" includes both cases where a hydrogen atom (-H) is replaced with a monovalent group and cases where a methylene group (-CH2-) is replaced with a divalent group. Examples of monovalent groups as substituents include alkyl groups having 1 to 4 carbon atoms, alkenyl groups having 2 to 4 carbon atoms, halogen atoms (such as fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms), and trialkoxysilyl groups (such as trimethoxysilyl groups). Examples of the divalent group as a substituent include an oxygen atom (-O-), -C(=O)-, and -C(=O)-O-. m is an integer of 2 or more, preferably 2 to 100, more preferably 2 to 50, and even more preferably 2 to 25. When m is equal to or more than the lower limit, the hydrophobicity of the conductive composite is sufficiently high. When m is equal to or less than the upper limit, it is possible to prevent the hydrophobicity from becoming too high or the conductivity from decreasing.

[0026] The epoxy compound is a compound having one or more epoxy groups in one molecule (an epoxy group-containing compound). From the viewpoint of preventing aggregation or gelation, the epoxy compound is preferably a compound having one epoxy group in one molecule. The epoxy compound that reacts with the conductive composite may be one type or two or more types.

[0027] Examples of monofunctional epoxy compounds having one epoxy group per molecule include ethylene oxide, propylene oxide, 2,3-butylene oxide, isobutylene oxide, 1,2-butylene oxide, 1,2-epoxyhexane, 1,2-epoxyheptane, 1,2-epoxypentane, 1,2-epoxyoctane, 1,2-epoxydecane, 1,3-butadiene monoxide, 1,2-epoxytetradecane, glycidyl methyl ether, 1,2-epoxyoctadecane, 1,2-epoxyhexadecane, and ethylene oxide. glycidyl ether, glycidyl isopropyl ether, tert-butyl glycidyl ether, 1,2-epoxyeicosane, 2-(chloromethyl)-1,2-epoxypropane, glycidol, epichlorohydrin, epibromohydrin, butyl glycidyl ether, 1,2-epoxyhexane, 1,2-epoxy-9-decane, 2-(chloromethyl)-1,2-epoxybutane, 2-ethylhexyl glycidyl ether, 1,2-epoxy-1H,1H,2H,2H,3H,3H-trifluorobutane, allyl glycidyl ether, tetracyanoethylene oxide, glycidyl butyrate, 1,2-epoxycyclooctane, glycidyl methacrylate, 1,2-epoxycyclododecane, 1-methyl-1,2-epoxycyclohexane, 1,2-epoxycyclopentadecane, 1,2-epoxycyclopentane, 1,2-epoxycyclohexane, 1,2-epoxy-1H,1H,2H,2H,3H,3H-heptadecafluorobutane, 3,4-epoxytetrahydrofuran, glycidyl stearate, 3-glycidyloxypropyl trimer Epoxysilane, epoxysuccinic acid, glycidyl phenyl ether, isophorone oxide, α-pinene oxide, 2,3-epoxynorbornene, benzyl glycidyl ether, diethoxy(3-glycidyloxypropyl)methylsilane, 3-[2-(perfluorohexyl)ethoxy]-1,2-epoxypropane, 1,1,1,3,5,5,5-heptamethyl-3-(3-glycidyloxypropyl)trisiloxane, 9,10-epoxy-1,5-cyclododecadiene, glycidyl 4-tert-butylbenzoate, 2,2-Bis(4-glycidyloxyphenyl)propane, 2-tert-butyl-2-[2-(4-chlorophenyl)]ethyloxirane, styrene oxide, glycidyl trityl ether, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-phenylpropylene oxide, cholesterol-5α,6α-epoxide, stilbene oxide, p-toluenesulfonic acid glycidyl, 3-methyl-3-phenylglycidic acid ethyl, N-propyl-N-(2,3-epoxypropyl)perfluoro-n- Examples of the glycidyl ethers include octyl sulfonamide, (2S,3S)-1,2-epoxy-3-(tert-butoxycarbonylamino)-4-phenylbutane, (R)-glycidyl 3-nitrobenzenesulfonate, glycidyl 3-nitrobenzenesulfonate, parthenolide, N-glycidylphthalimide, endrin, dieldrin, 4-glycidyloxycarbazole, 7,7-dimethyloctanoic acid [oxiranylmethyl], 1,2-epoxy-4-vinylcyclohexane, and higher alcohol glycidyl ethers having 10 to 16 carbon atoms.

[0028] The higher alcohol glycidyl ether is preferably at least one type of higher alcohol glycidyl ether having 10 to 16 carbon atoms, more preferably at least one type of higher alcohol glycidyl ether having 12 to 14 carbon atoms, and further preferably at least one type of C12 (12 carbon atoms) higher alcohol glycidyl ether and C13 (13 carbon atoms) higher alcohol glycidyl ether.

[0029] Examples of polyfunctional epoxy compounds having two or more epoxy groups in one molecule include 1,6-hexanediol diglycidyl ether, 1,7-octadiene diepoxide, neopentyl glycol diglycidyl ether, 4-butanediol diglycidyl ether, 1,2:3,4-diepoxybutane, 1,2-cyclohexanedicarboxylate diglycidyl, triglycidyl isocyanurate, neopentyl glycol diglycidyl ether, 1,2:3,4-diepoxybutane, polyethylene glycol diglycidyl ether, ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, and the like. Examples of the glycidyl ether include glycidyl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, glycerin diglycidyl ether, trimethylolpropane triglycidyl ether, trimethylolpropane polyglycidyl ether, hydrogenated bisphenol A diglycidyl ether, hexahydrophthalic acid diglycidyl ester, glycerin polyglycidyl ether, diglycerin polyglycidyl ether, polyglycerin polyglycidyl ether, sorbitol-based polyglycidyl ether, and ethylene oxide lauryl alcohol glycidyl ether.

[0030] Since the epoxy compound has high dispersibility in organic solvents, the molecular weight is preferably from 50 to 2000. Furthermore, since the epoxy compound has high dispersibility in low-polarity hydrocarbon solvents and ester solvents, the epoxy compound preferably has a carbon number of from 4 to 120, more preferably from 7 to 100, even more preferably from 10 to 80, and particularly preferably from 15 to 50.

[0031] (Substituent C) The substituent (C) is presumed to be a group represented by the following formula (C).

[0032] -N + R 11 R 12 R 13 R 14 (C) [In formula (C), R 11 ~R 14 each independently represents a hydrocarbon group which may have a substituent.

[0033] In the substituent (C), the bond at the left end represents the bond between the negative charge of the anion group and the positive charge of the quaternary ammonium cation. Examples of an anion group that can be negatively charged include "-SO3 - " is an anionic group in which an active proton is bonded to an oxygen atom.

[0034] R in chemical formula (C) 11 ~R 14 R in chemical formula (C) is a hydrocarbon group which may have a substituent. 11 ~R 14 is a substituent derived from a quaternary ammonium compound. Examples of the hydrocarbon group in the chemical formula (C) include an aliphatic hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, and an aromatic hydrocarbon group having 6 to 20 carbon atoms which may have a substituent. Examples of the aliphatic hydrocarbon group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, and an octyl group. Examples of the substituent on the aliphatic hydrocarbon group include a phenyl group and a hydroxyl group. Examples of the aromatic hydrocarbon group include a phenyl group and a naphthyl group. Examples of the substituent on the aromatic hydrocarbon group include an alkyl group having 1 to 5 carbon atoms and a hydroxyl group.

[0035] In order to improve dispersibility in organic solvents and conductivity, the quaternary ammonium compound preferably has a substituent on the nitrogen atom having 3 or more carbon atoms, more preferably has a substituent on the nitrogen atom having 5 or more carbon atoms, and even more preferably has a substituent on the nitrogen atom having 7 or more carbon atoms. The upper limit of the carbon number of each substituent on the nitrogen atom is not particularly limited, and taking into consideration solubility in solvents and reactivity, it is, for example, preferably 40 or less, more preferably 30 or less, and even more preferably 20 or less. In addition, the R 11 ~R 14 The total number of carbon atoms is preferably 8 to 44, more preferably 12 to 40, and further preferably 16 to 36. The number of carbon atoms in each of the substituents on the nitrogen atom may be the same or different.

[0036] Specific examples of quaternary ammonium compounds include quaternary ammonium salts such as tetramethylammonium salt, tetraethylammonium salt, tetrapropylammonium salt, tetrabutylammonium salt, tetra-n-octylammonium salt, tetraphenylammonium salt, tetrabenzylammonium salt, and tetranaphthylammonium salt. Examples of the counter anion of the ammonium cation include halogen ions such as bromide ion and chloride ion, and hydroxy ion.

[0037] In the polyanion, the mass ratio represented by [substituent (A)]:[substituent (C)] (hereinafter also referred to as A / C ratio) is preferably 10:90 to 90:10, more preferably 20:80 to 80:20, and even more preferably 25:75 to 75:25. When the A / C ratio is within the above range, it is easy to balance the dispersibility and the conductivity. The mass of the [substituent (A)] can be calculated by [(mass of reactant A obtained by reacting an epoxy compound with a conductive complex)-(mass of the conductive complex before reacting with an epoxy compound)]. The mass of the [anion group to which the substituent (C) is bonded] can be calculated by [(mass of reactant C obtained by reacting the reactant A with a quaternary ammonium compound)-(mass of the reactant A)].

[0038] The content of the polyanion in the conductive complex is preferably in the range of 1 part by mass to 1000 parts by mass, more preferably 10 parts by mass to 700 parts by mass, and even more preferably 100 parts by mass to 500 parts by mass, relative to 100 parts by mass of the π-conjugated conductive polymer. If the content of the polyanion is equal to or greater than the lower limit, the doping effect on the π-conjugated conductive polymer tends to be stronger, and the conductivity becomes higher. On the other hand, if the content of the polyanion is equal to or less than the upper limit, the amount of anion groups not involved in doping is appropriately suppressed, and the anion groups can be easily converted to hydrophobicity when reacting with an epoxy compound and a quaternary ammonium compound.

[0039] The content of the conductive complex relative to the total mass of the conductive polymer-containing liquid is, for example, preferably 0.01 mass % or more and 10 mass % or less, more preferably 0.1 mass % or more and 5 mass % or less, and even more preferably 0.2 mass % or more and 2 mass % or less.

[0040] [Dispersion medium] The dispersion medium contained in the conductive polymer-containing liquid of this embodiment may be an organic solvent or a mixture of water and an organic solvent. As described above, since the polyanion of the conductive composite is hydrophobically modified, a dispersion medium containing an organic solvent is preferred. The content of the organic solvent relative to the total mass of the dispersion medium is preferably from 50% by mass to 100% by mass, more preferably from 90% by mass to 100% by mass, and even more preferably from 95% by mass to 100% by mass.

[0041] <Organic solvent> The organic solvent contained in the conductive polymer-containing liquid of this embodiment contains an ester group-containing compound (ester-based solvent) having an ester group (-C(=O)-O-).

[0042] From the viewpoint of enhancing the dispersibility of the conductive composite, the conductive polymer-containing liquid of this embodiment preferably contains one or more ester solvents represented by the following formula 1. Formula 1:R 21 -C(=O)-OR 22 [In the formula, R 21represents a hydrogen atom, a methyl group, or an ethyl group; R 22 represents a linear or branched alkyl group having 1 to 6 carbon atoms.]

[0043] In order to enhance the dispersibility of the conductive composite of this embodiment, R 21 is preferably a methyl group or an ethyl group, more preferably a methyl group. 22 The number of carbon atoms is preferably 2 to 5, and more preferably 2 to 4.

[0044] Preferred specific examples of the ester-based solvent include ethyl acetate, propyl acetate, butyl acetate, isopropyl acetate, and isobutyl acetate.

[0045] The content of the ester solvent in the organic solvent is preferably 40% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, most preferably 90% by mass or more, and may be 100% by mass, based on the total mass of the organic solvent. When the content of the ester solvent is within the above range, the dispersibility of the conductive composite can be increased.

[0046] The conductive polymer-containing liquid of this embodiment may further contain one or more organic solvents other than the ester-based solvent. Examples of organic solvents other than ester-based organic solvents include hydrocarbon-based solvents, ketone-based solvents, alcohol-based solvents, ether-based solvents, and nitrogen atom-containing compound-based solvents. Examples of the hydrocarbon solvent include aliphatic hydrocarbon solvents and aromatic hydrocarbon solvents. Examples of the aliphatic hydrocarbon solvent include pentane, hexane, heptane, octane, decane, cyclohexane, methylcyclohexane, etc. Examples of the aromatic hydrocarbon solvent include benzene, toluene, xylene, ethylbenzene, propylbenzene, isopropylbenzene, etc. Examples of the ketone solvent include diethyl ketone, methyl propyl ketone, methyl butyl ketone, methyl isopropyl ketone, methyl isobutyl ketone, methyl amyl ketone, diisopropyl ketone, methyl ethyl ketone, acetone, and diacetone alcohol. Examples of the alcohol solvent include methanol, ethanol, isopropanol, n-butanol, t-butanol, and allyl alcohol. Examples of the ether solvent include diethyl ether, dimethyl ether, and propylene glycol dialkyl ether. Examples of the nitrogen atom-containing compound solvent include N-methylpyrrolidone, dimethylacetamide, and dimethylformamide.

[0047] When the conductive polymer-containing liquid of this embodiment contains a hydrocarbon solvent, the wettability of the conductive polymer-containing liquid to the plastic film substrate is increased, and a binder component with low polarity can be easily added, which is preferable.

[0048] Among the hydrocarbon solvents, toluene is preferred because it is versatile, and when a silicone compound is added as a binder component, at least one of heptane and toluene is preferred because it has excellent solubility for the silicone compound.

[0049] It is preferable to further contain methyl ethyl ketone in addition to the hydrocarbon solvent, since the dispersibility of the conductive composite is increased. For example, the content of methyl ethyl ketone is preferably 20 parts by mass or more and 120 parts by mass or less, more preferably 30 parts by mass or more and 100 parts by mass or less, and even more preferably 40 parts by mass or more and 80 parts by mass or less, relative to 100 parts by mass of the hydrocarbon solvent.

[0050] The content of the hydrocarbon solvent is preferably 10% by mass or more and 80% by mass or less, more preferably 20% by mass or more and 70% by mass or less, and even more preferably 30% by mass or more and 60% by mass or less, based on the total mass of the organic solvent contained in the conductive polymer-containing liquid of this embodiment. When the content of the hydrocarbon solvent is within the above range, the dispersibility of the conductive composite can be improved.

[0051] <Binder components> The conductive polymer-containing liquid of this embodiment may contain a binder component. By using a conductive polymer-containing liquid containing a binder component, the strength of the conductive layer to be formed can be improved and adhesiveness and releasability can be imparted. The binder component is a resin or a precursor thereof other than the π-conjugated conductive polymer and the polyanion, and is a thermoplastic resin or a curable monomer or oligomer that is cured when the conductive layer is formed. The thermoplastic resin becomes the binder resin as it is, and the curable monomer or oligomer becomes the resin formed by curing. The binder component may be a pressure-sensitive adhesive, which will be described later. The conductive polymer-containing liquid of this embodiment may contain one type of binder component or two or more types of binder components.

[0052] Specific examples of binder resins derived from binder components include epoxy resins, acrylic resins (acrylic compounds), polyester resins, polyurethane resins, polyimide resins, polyether resins, melamine resins, and silicones.

[0053] The curable monomer or oligomer may be a thermosetting monomer or oligomer, or a photocurable monomer or oligomer. Here, the oligomer refers to a polymer having a mass average molecular weight of less than 10,000. Examples of the curable monomer include an acrylic monomer (acrylic compound), an epoxy monomer, an organosiloxane, etc. Examples of the curable oligomer include an acrylic oligomer (acrylic compound), an epoxy oligomer, a silicone oligomer (curable silicone), etc. When an acrylic monomer or an acrylic oligomer is used as the binder component, it can be easily cured by heating or irradiating with light.

[0054] When a curable monomer or oligomer is included, it is preferable to further include a curing catalyst. For example, when a thermosetting monomer or oligomer is included, it is preferable to include a thermal polymerization initiator that generates radicals by heating, and when a photocurable monomer or oligomer is included, it is preferable to include a photopolymerization initiator that generates radicals by light irradiation.

[0055] The content ratio of the binder component (excluding the silicone compound described later) contained in the conductive polymer-containing liquid of this embodiment is, for example, preferably 1 part by mass or more and 10,000 parts by mass or less, more preferably 10 parts by mass or more and 1,000 parts by mass or less, and even more preferably 50 parts by mass or more and 500 parts by mass or less, relative to 1 part by mass of the conductive composite. When the content is equal to or greater than the lower limit of the above range, the characteristics of the binder component contained in the conductive layer formed from the conductive polymer-containing liquid of this embodiment can be fully exhibited. When it is equal to or less than the upper limit of the above range, sufficient conductivity of the conductive layer formed from the conductive polymer-containing liquid of this embodiment can be ensured.

[0056] (Silicone compounds) Since the conductive polymer-containing liquid of this embodiment uses an organic solvent as a dispersion medium, a silicone compound having low polarity can be added as a binder component to sufficiently disperse the silicone compound. When the organic solvent contains a hydrocarbon-based solvent or an ester-based solvent, the dispersibility of the silicone compound is further improved, which is preferable. Examples of the silicone compound include curable silicone. When the binder component is curable silicone, releasability can be imparted to the conductive layer by curing the curable silicone.

[0057] The curable silicone may be either an addition curable silicone or a condensation curable silicone. In this embodiment, the addition curable silicone is preferred because it is less likely to cause curing inhibition.

[0058] The addition curing silicone may be a linear polymer having a siloxane bond, which includes polydimethylsiloxane having vinyl groups at both ends of the linear chain, and hydrogen silane. Such addition curing silicone forms a three-dimensional crosslinked structure by addition reaction and cures. A platinum-based curing catalyst may be used to accelerate the cure. Specific examples of addition curing silicones include KS-3703T, KS-847T, KM-3951, X-52-151, X-52-6068, and X-52-6069 (manufactured by Shin-Etsu Chemical Co., Ltd.). The addition curing type silicone is preferably dissolved or dispersed in an organic solvent.

[0059] The content ratio of the silicone compound contained in the conductive polymer-containing liquid of this embodiment is preferably 10 parts by mass or more and 50,000 parts by mass or less, more preferably 50 parts by mass or more and 10,000 parts by mass or less, and even more preferably 100 parts by mass or more and 5,000 parts by mass or less, relative to 100 parts by mass of the conductive composite. When the content is equal to or greater than the lower limit of the above range, sufficient releasability can be imparted to the conductive layer formed from the conductive polymer-containing liquid of this embodiment. When it is equal to or less than the upper limit of the above range, sufficient conductivity of the conductive layer formed from the conductive polymer-containing liquid of this embodiment can be ensured.

[0060] [Adhesive] The conductive polymer-containing liquid of this embodiment may contain an adhesive as a binder component. By using a conductive polymer-containing liquid containing an adhesive, a conductive layer having adhesive properties can be formed. Since the conductive polymer-containing liquid of this embodiment contains an ester-based solvent, it can be easily mixed with a pressure-sensitive adhesive that has been dispersed in advance in a hydrocarbon-based solvent or an ester-based solvent, and the conductive complex can be stably dispersed in the mixed liquid.

[0061] The degree of adhesion of the adhesive of this embodiment is not particularly limited, and may be adhesion that can be easily peeled off by hand after application, or adhesion that is difficult to peel off after application. Adhesion that is difficult to peel off can be rephrased as adhesion. In other words, the adhesion may be such that it can be adhered semi-permanently.

[0062] As the pressure-sensitive adhesive, known pressure-sensitive adhesives can be used, and from the viewpoint of exhibiting good adhesiveness while maintaining electrical conductivity, acrylic pressure-sensitive adhesives are preferred.

[0063] (Acrylic adhesive) The acrylic adhesive can bond and integrate the surfaces of the same or different solids. The acrylic adhesive contains an acrylic resin (acrylic polymer).

[0064] Specific examples of acrylic monomers that form acrylic resins include acrylic acid, methacrylic acid, methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, 2-ethylhexyl acrylate, 2-methoxyethyl acrylate, ditrimethylolpropane tetraacrylate, 2-hydroxy-3-phenoxypropyl acrylate, bisphenol A·ethylene oxide modified diacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, dipentaerythritol monohydroxypentaacrylate, dipropylene glycol diacrylate, trimethylolpropane triacrylate, glycerol propoxy triacrylate, 4-hydroxybutyl acrylate, 1,6-hexanediol diacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, acrylate, isobornyl acrylate, polyethylene glycol diacrylate, pentaerythritol triacrylate, tetrahydrofurfuryl acrylate, tripropylene glycol diacrylate, and other acrylates; methacrylates, such as tetraethylene glycol dimethacrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, t-butyl methacrylate, allyl methacrylate, 1,3-butylene glycol dimethacrylate, benzyl methacrylate, cyclohexyl methacrylate, diethylene glycol dimethacrylate, 2-ethylhexyl methacrylate, glycidyl methacrylate, 1,6-hexanediol dimethacrylate, 2-hydroxyethyl methacrylate, isobornyl methacrylate, lauryl methacrylate, phenoxyethyl methacrylate, tetrahydrofurfuryl methacrylate, and trimethylolpropane trimethacrylate, and other methacrylates;Examples of (meth)acrylamides include diacetone acrylamide, N,N-dimethylacrylamide, dimethylaminopropyl acrylamide, dimethylaminopropyl methacrylamide, methacrylamide, N-methylolacrylamide, acryloylformolin, N-methylacrylamide, N-isopropylacrylamide, Nt-butylacrylamide, N-phenylacrylamide, acryloylpiperidine, and 2-hydroxyethylacrylamide. The acrylic resin may be formed of one type of acrylic monomer or two or more types of acrylic monomers. By combining two or more types of acrylic monomers, the adhesiveness can be adjusted.

[0065] The acrylic resin may be a copolymer of an acrylic monomer and a vinyl monomer other than the acrylic monomer. Examples of vinyl monomers include styrene, α-methylstyrene, vinyl acetate, acrylonitrile, methacrylonitrile, and maleic anhydride. The content of the acrylic monomer unit in the copolymer is preferably 50 mol % or more and less than 100 mol %, and more preferably 70 mol % or more and 98 mol % or less. When the content of the acrylic monomer unit is equal to or more than the lower limit, adhesiveness can be easily exhibited. The content of the vinyl monomer unit in the copolymer can be, for example, from 2 mol % to 20 mol %.

[0066] The glass transition temperature of the acrylic resin is preferably 80° C. or lower, more preferably 50° C. or lower, and even more preferably 0° C. or lower. An acrylic resin having a glass transition temperature of more than 80° C. has low adhesion. The glass transition temperature of an acrylic resin is −80° C. or higher, and it is difficult to obtain an acrylic resin having a glass transition temperature lower than that. The glass transition temperature of an acrylic resin can be determined by differential scanning calorimetry or dynamic viscoelasticity measurement. Examples of acrylic monomers that tend to lower the glass transition temperature of acrylic resins include ethyl acrylate, butyl acrylate (particularly n-butyl acrylate), 2-ethylhexyl acrylate, etc. In acrylic resins, the higher the ratio of these monomer units, the lower the glass transition temperature.

[0067] The mass average molecular weight of the acrylic resin is preferably 10,000 to 2,000,000, and more preferably 30,000 to 1,000,000. If the mass average molecular weight of the acrylic resin is equal to or greater than the lower limit, sufficient cohesive strength can be ensured. If the mass average molecular weight is equal to or less than the upper limit, adhesion can be further improved.

[0068] When the acrylic resin has an acrylic monomer unit having a reactive functional group, it may be cured by reacting with a curing agent. When the acrylic resin is cured, the cohesive force of the conductive layer containing the adhesive is improved, and the strength can be improved. In addition, by improving the cohesive force of the conductive layer, it is possible to make the conductive layer removably capable of repeated adhesion and peeling. Examples of the reactive functional group include a hydroxy group, a carboxy group, an amino group, an amide group, an epoxy group, etc. When reacting with a polyfunctional isocyanate described later, the reactive functional group is preferably a hydroxy group, a carboxy group, or an amino group, and more preferably a hydroxy group. Examples of acrylic monomers having a hydroxy group include 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl acrylate, 3-hydroxypropyl methacrylate, 4-hydroxybutyl acrylate, and 4-hydroxybutyl methacrylate. Examples of the acrylic monomer having a carboxy group include acrylic acid, methacrylic acid, and itaconic acid. Examples of the acrylic monomer having an amino group include dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, diethylaminoethyl acrylate, and diethylaminoethyl methacrylate. Examples of acrylic monomers having an amide group include acrylamide, methacrylamide, N-methylol acrylamide, and N-methylol methacrylamide. Examples of the acrylic monomer having an epoxy group include glycidyl acrylate and glycidyl methacrylate. When a polyfunctional isocyanate is used as a curing agent, among the acrylic monomers having a reactive functional group, taking into consideration curability and cost, an acrylic monomer having a hydroxy group is preferred, and 2-hydroxyethyl acrylate and 2-hydroxyethyl methacrylate are more preferred. The acrylic monomer having a reactive functional group that forms the acrylic resin may be of one type or of two or more types.

[0069] The content of the adhesive contained in the conductive polymer-containing liquid of this embodiment is preferably 1 part by mass or more and 1,000 parts by mass or less, more preferably 10 parts by mass or more and 500 parts by mass or less, and even more preferably 30 parts by mass or more and 250 parts by mass or less, relative to 1 part by mass of the conductive composite. When it is equal to or greater than the lower limit of the above range, sufficient adhesion can be imparted to the conductive layer formed by the conductive polymer-containing liquid of this embodiment. When it is equal to or less than the upper limit of the above range, sufficient conductivity of the conductive layer formed from the conductive polymer-containing liquid of this embodiment can be ensured.

[0070] (hardening agent) When the adhesive contained in the conductive polymer-containing liquid of this embodiment has a reactive functional group, the conductive polymer-containing liquid of this embodiment preferably contains a curing agent. Examples of the curing agent include isocyanate-based curing agents such as polyfunctional isocyanates having two or more isocyanate groups in one molecule, and epoxy-based curing agents such as epoxy compounds having two or more epoxy groups in one molecule. Among these curing agents, polyfunctional isocyanates are preferred from the viewpoint of reactivity. In particular, when the adhesive has an acrylic monomer unit having a hydroxyl group, it is preferred that the curing agent is a polyfunctional isocyanate.

[0071] Examples of the polyfunctional isocyanate include aliphatic polyfunctional isocyanates, alicyclic polyfunctional isocyanates, and aromatic polyfunctional isocyanates. Specific examples of polyfunctional isocyanates include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, polyphenylene polymethylene polyisocyanate, 1,6-hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, p-phenylene diisocyanate, transcyclohexane 1,4-diisocyanate, 4,4'-dicyclomethane diisocyanate, 3, Examples of the isocyanate include 3'-dimethyl-4,4'-diphenylmethane diisocyanate, dianisidine diisocyanate, m-xylylene diisocyanate, isophorone diisocyanate, 1,5-naphthalene diisocyanate, 1,4-cyclohexane diisocyanate, lysine diisocyanate, lysine ester triisocyanate, tetramethylxylene diisocyanate, 1,6,11-undecane triisocyanate, 1,3,6-hexamethylene triisocyanate, bicyclohepta triisocyanate, and trimethylhexamethylene diisocyanate. The polyfunctional isocyanate may be a modified diisocyanate formed from a modified polyfunctional isocyanate obtained by modifying the diisocyanate so that the NCO / OH molar ratio becomes 2 / 1 or more. The polyfunctional isocyanate may be a modified polyisocyanate. Examples of the modified polyisocyanate include polyurethane polyisocyanates obtained by reacting the polyfunctional isocyanate with polyhydric alcohols, polyisocyanates containing an isocyanurate ring obtained by polymerizing a polyfunctional isocyanate, and polyisocyanates containing a biuret bond obtained by reacting a polyfunctional isocyanate with water. The conductive polymer-containing liquid of this embodiment may contain one type of curing agent, or two or more types of curing agents.

[0072] The content ratio of the curing agent contained in the conductive polymer-containing liquid of this embodiment is, for example, preferably 1 part by mass or more and 100 parts by mass or less, more preferably 2 parts by mass or more and 50 parts by mass or less, and even more preferably 3 parts by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the adhesive. When the content is within the above range, sufficient adhesion can be imparted to the conductive layer formed by the conductive polymer-containing liquid of this embodiment.

[0073] (Highly conductive agent) The conductive polymer-containing liquid of this embodiment may contain a conductivity enhancing agent. Here, the above-mentioned π-conjugated conductive polymer, polyanion, organic solvent, adhesive, curing agent, and binder component are not classified as a high-conductivity agent. Note that the above-mentioned epoxy compound and quaternary ammonium compound may be included in the high-conductivity agent described here. The conductive agent is preferably at least one compound selected from the group consisting of saccharides, nitrogen-containing aromatic cyclic compounds, compounds having two or more hydroxyl groups, compounds having one or more hydroxyl groups and one or more carboxyl groups, compounds having an amide group, compounds having an imide group, lactam compounds, and compounds having a glycidyl group. The conductive polymer-containing liquid of this embodiment may contain one type of highly conductive agent, or two or more types of highly conductive agents. The content of the conductive agent is preferably 1 part by mass or more and 10,000 parts by mass or less, more preferably 10 parts by mass or more and 5,000 parts by mass or less, and even more preferably 100 parts by mass or more and 2,500 parts by mass or less, per 100 parts by mass of the conductive composite. When the content ratio of the conductive agent is equal to or more than the lower limit, the effect of improving the conductivity by adding the conductive agent is sufficiently exhibited, and when the content ratio is equal to or less than the upper limit, a decrease in the conductivity caused by a decrease in the concentration of the π-conjugated conductive polymer can be prevented.

[0074] (Other additives) The conductive polymer-containing liquid of this embodiment may contain other known additives. The additives are not particularly limited as long as the effects of the present invention can be obtained. For example, surfactants, inorganic conductive agents, antifoaming agents, coupling agents, antioxidants, ultraviolet absorbing agents, etc. can be used. The surfactant may be a nonionic, anionic or cationic surfactant, with the nonionic surfactant being preferred from the standpoint of storage stability. A polymer surfactant such as polyvinylpyrrolidone may also be added. Examples of the inorganic conductive agent include metal ions, conductive carbon, etc. Metal ions can be generated by dissolving a metal salt in water. The antifoaming agent includes silicone resin, polydimethylsiloxane, silicone oil, and the like. The coupling agent may be a silane coupling agent having a vinyl group or an amino group. Examples of the antioxidant include phenol-based antioxidants, amine-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, and sugars. Examples of the ultraviolet absorber include benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, salicylate-based ultraviolet absorbers, cyanoacrylate-based ultraviolet absorbers, oxanilide-based ultraviolet absorbers, hindered amine-based ultraviolet absorbers, and benzoate-based ultraviolet absorbers. When the conductive polymer-containing liquid of this embodiment contains the above-mentioned additive, the content ratio thereof is appropriately determined depending on the type of additive, but can be, for example, in the range of 0.001 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the conductive composite. Furthermore, the conductive polymer-containing liquid of this embodiment may or may not contain an unsaturated aliphatic alcohol compound having an unsaturated bond between carbon atoms and a hydroxyl group in the molecule.

[0075] <Method for producing conductive polymer-containing liquid> A second aspect of the present invention is a method for producing a conductive polymer-containing liquid, comprising the steps of adding at least one epoxy compound and at least one quaternary ammonium compound to a conductive polymer aqueous dispersion in which a conductive complex containing a π-conjugated conductive polymer and a polyanion is contained in an aqueous dispersion medium, and then recovering the precipitated reaction product (precipitation and recovery step), and adding an organic solvent to the recovered reaction product to obtain a conductive polymer-containing liquid (addition step). According to the production method of this embodiment, the conductive polymer-containing liquid of the first embodiment can be produced.

[0076] The manufacturing method of this embodiment may further include a washing step between the precipitation / recovery step and the organic solvent adding step. In addition, a binder component or the like may be further added in the organic solvent adding step.

[0077] [Precipitation recovery process] The precipitation and recovery process is a process in which an epoxy compound and a quaternary ammonium compound are added to a conductive polymer aqueous dispersion to precipitate a reaction product between the conductive composite and the epoxy compound and the quaternary ammonium compound, and then the reaction product is recovered as a precipitate. The recovery method is not particularly limited, and the product can be recovered, for example, by filtration.

[0078] When an epoxy compound is added to a conductive polymer aqueous dispersion, the epoxy group of the epoxy compound reacts with some of the anion groups of the polyanion, forming a substituent (A) and making the conductive complex hydrophobic, making it difficult to stably disperse in the aqueous dispersion and causing it to precipitate out as a precipitate. When the epoxy compound is added, heating may be performed to promote the reaction. The heating temperature is preferably 40° C. or higher and 100° C. or lower. The amount of the epoxy compound added is preferably 10 parts by mass or more and 10,000 parts by mass or less, more preferably 100 parts by mass or more and 5,000 parts by mass or less, and even more preferably 500 parts by mass or more and 3,000 parts by mass or less, relative to 100 parts by mass of the conductive composite. When it is at least the lower limit of the above range, the hydrophobicity of the conductive composite is sufficiently high, and the dispersibility in organic solvents is improved. When the content is equal to or less than the upper limit of the above range, a decrease in electrical conductivity due to unreacted epoxy compound can be prevented.

[0079] An organic solvent may be added before, simultaneously with, or after the epoxy compound is added to the conductive polymer aqueous dispersion. The organic solvent is preferably a water-soluble organic solvent. Here, the water-soluble organic solvent is an organic solvent that dissolves in an amount of 1 g or more per 100 g of water at a temperature of 20° C. Examples of the water-soluble organic solvent include alcohol-based solvents, ketone-based solvents, and ester-based solvents. The organic solvent to be added may be one type or two or more types.

[0080] When a quaternary ammonium compound is added to a conductive polymer aqueous dispersion, the quaternary ammonium compound reacts with some of the anion groups of the polyanion, forming a substituent (C) and making the conductive complex hydrophobic, making it difficult to stably disperse it in the aqueous dispersion. The amount of the quaternary ammonium compound added is preferably 1 part by mass or more and 10,000 parts by mass or less, more preferably 10 parts by mass or more and 5,000 parts by mass or less, and even more preferably 50 parts by mass or more and 1,000 parts by mass or less, per 100 parts by mass of the conductive composite. When it is at least the lower limit of the above range, the hydrophobicity of the conductive composite is sufficiently high, and the dispersibility in organic solvents is improved. When the content is equal to or less than the upper limit of the above range, a decrease in electrical conductivity due to unreacted quaternary ammonium compound can be prevented. The quaternary ammonium compound has a reaction mechanism similar to that of the amine compound, and exhibits good reactivity with the conductive complex even at a smaller amount than the amine compound. The conductivity of the conductive layer containing the conductive complex modified with the quaternary ammonium compound tends to be superior to that of the conductive layer modified with the amine compound.

[0081] In the precipitation recovery process, the order of addition of the epoxy compound and the quaternary ammonium compound is not particularly limited. Since the synthetic intermediate (reaction intermediate) is easy to handle, it is preferable to add the epoxy compound to the conductive polymer aqueous dispersion liquid to react with a part of the anion group of the polyanion, and then add the quaternary ammonium compound to react with the other part of the anion group of the polyanion.

[0082] The conductive polymer aqueous dispersion is a dispersion in which a conductive complex containing a π-conjugated conductive polymer and a polyanion is contained in an aqueous dispersion medium. Here, the aqueous dispersion medium is water or a mixture of water and a water-soluble organic solvent. Examples of the water-soluble organic solvent include alcohol-based solvents, ketone-based solvents, and ester-based solvents. The aqueous dispersion medium may contain one type of water-soluble organic solvent or two or more types of water-soluble organic solvents. The content of water relative to the total mass of the aqueous dispersion medium is preferably more than 50% by mass, more preferably 60% by mass or more, even more preferably 80% by mass or more, and may be 100% by mass.

[0083] The conductive polymer aqueous dispersion can be obtained, for example, by chemically oxidizing a monomer that forms a π-conjugated conductive polymer in an aqueous solution of a polyanion. Alternatively, a commercially available conductive polymer aqueous dispersion can be used. A known catalyst may be used in the chemical oxidative polymerization. For example, a catalyst and an oxidizing agent may be used. Examples of the catalyst include transition metal compounds such as ferric chloride, ferric sulfate, ferric nitrate, and cupric chloride. Examples of the oxidizing agent include persulfates such as ammonium persulfate, sodium persulfate, and potassium persulfate. The oxidizing agent can return the reduced catalyst to its original oxidized state.

[0084] The reaction product (precipitate) recovered in the precipitation recovery step preferably has as little moisture as possible, and most preferably contains no moisture at all, but from a practical standpoint, it may contain moisture in the range of 10 mass % or less. Methods for reducing the moisture content include, for example, washing off the precipitate with an organic solvent, drying the precipitate, and the like.

[0085] [Cleaning process] The washing step between the precipitate recovery step and the organic solvent addition step is a step of washing the precipitate with an organic solvent for washing, which removes residual water, unreacted epoxy compounds, unreacted quaternary ammonium compounds, hydrolyzates of epoxy compounds, and the like. The organic solvent for cleaning is preferably one that can clean the precipitate while minimizing dissolution of the precipitate. For this reason, the organic solvent for cleaning is preferably an alcohol-based solvent. The organic solvent for cleaning may contain one type of organic solvent or two or more types of organic solvents. The washing method is not particularly limited, and for example, the precipitate may be washed by pouring an organic washing solvent over the precipitate, or the precipitate may be washed by stirring in the organic washing solvent.

[0086] [Organic solvent addition process] The organic solvent adding step is a step of adding an organic solvent to the precipitate to obtain a conductive polymer-containing liquid.

[0087] The organic solvent in this step can be the organic solvent contained in the conductive polymer-containing liquid of the first embodiment. Since the conductive complex is modified with an epoxy compound and a quaternary ammonium compound, an ester-based solvent is used to thoroughly disperse the conductive complex. In addition to the ester-based solvent, an optional organic solvent, for example, one or more selected from hydrocarbon-based solvents, may be added. Specifically, the ester solvent represented by the formula 1 and at least one selected from heptane and toluene as an optional organic solvent are preferred. When the organic solvent contains heptane or toluene, it may further contain methyl ethyl ketone. By using these suitable organic solvents, the dispersibility of the conductive composite can be further improved in the conductive polymer-containing liquid of this embodiment. The content of each solvent contained in the organic solvent is preferably within the preferred range exemplified in the first embodiment.

[0088] The conductive polymer-containing liquid obtained by adding an organic solvent to the precipitate may be stirred and dispersed. The stirring method is not particularly limited, and may be a weak shear stirring such as with a stirrer, or may be a high shear stirring using a dispersing machine (homogenizer, etc.).

[0089] The content of the conductive complex relative to the total mass of the conductive polymer-containing liquid dispersed by the high-pressure homogenizer is, for example, preferably from 0.01% by mass to 5% by mass, more preferably from 0.05% by mass to 2% by mass, and even more preferably from 0.1% by mass to 1% by mass. When the concentration is within the above range, the dispersibility of the conductive composite can be sufficiently increased.

[0090] [Solvent replacement method] The above-mentioned precipitation / recovery step and organic solvent addition step may be the following solvent replacement method. The reaction product precipitated in the reaction solution to which the quaternary ammonium compound has been added tends to naturally settle to the bottom layer of the reaction solution. Although the details of the mechanism by which the precipitation occurs have not been elucidated, it is believed that the relationship between the specific gravity of the reaction product and the specific gravity of the reaction solution is an influence.

[0091] When the reaction product settles to the bottom layer of the reaction liquid, the upper layer of the reaction liquid contains almost no reaction product. By removing the upper layer by suction, decantation, etc., the concentration of the precipitated reaction product increases, and a residual liquid with a reduced volume is obtained. This operation corresponds to the step of recovering the reaction product. The resulting residual liquid contains moisture derived from the conductive polymer aqueous dispersion. Next, an organic solvent containing an ester-based solvent is added to the residual liquid to obtain the desired conductive polymer-containing liquid. This operation corresponds to the organic solvent addition step. Here, if the residual liquid has a high water content or if the amount of the upper layer removed is small, the reaction product (conductive composite) is not dispersed in the mixed liquid after the organic solvent is added, and can be precipitated again into the lower layer. In this case, by removing the upper layer again, the concentration of the reaction product is increased, the water content is reduced, and a residual liquid with a reduced volume is obtained. By adding an organic solvent containing an ester-based solvent to the residual liquid again, a conductive polymer-containing liquid is obtained in which the organic solvent concentration is increased (water content is reduced) compared to the first solvent replacement. This "solvent replacement method" is not limited to one time, and may be repeated two or more times. When performing the solvent replacement method two or more times, it is preferable that the organic solvent added in the final solvent replacement method contains an ester-based solvent, but the organic solvent added in the solvent replacement method before the final one may or may not contain an ester-based solvent.

[0092] By the solvent replacement method described above, it is possible to obtain the desired conductive polymer-containing liquid having a water content of preferably 20 mass % or less, more preferably 10 mass % or less, and even more preferably 5 mass % or less, relative to the total mass of the dispersion medium. For the purpose of improving the dispersibility of the conductive composite in the obtained conductive polymer-containing liquid, it is preferable to carry out a dispersion treatment using a dispersing machine such as a high-pressure homogenizer.

[0093] (Addition of binder components) The binder component may be added to the conductive polymer-containing liquid. In this case, an arbitrary organic solvent may be added together with the binder component. It is preferable to stir the mixture after the addition of the binder component to enhance the dispersibility of the binder component. The curing agent may be added simultaneously with or after the addition of the adhesive. When the binder component is an addition-curing silicone, it is preferable to add a platinum-based curing catalyst simultaneously with or after the addition of the binder component.

[0094] (Addition of high conductivity agents and other additives) The conductive polymer-containing liquid may contain the conductive agent and other additives.

[0095] <Conductive laminate> A third aspect of the present invention is a conductive laminate comprising a substrate and a conductive layer formed on at least one surface of the substrate, the conductive layer being a cured layer of the conductive polymer-containing liquid of the first aspect.

[0096] [Conductive layer] The average thickness of the conductive layer provided on at least one surface of the substrate is, for example, preferably 10 nm to 100 μm, more preferably 20 nm to 50 μm, and even more preferably 30 nm to 30 μm. When the average thickness of the conductive layer is equal to or greater than the lower limit, high conductivity can be exhibited, and when the average thickness is equal to or less than the upper limit, the adhesion of the conductive layer to the substrate is further improved.

[0097] The conductive layer included in the conductive laminate of this embodiment contains a conductive complex containing a π-conjugated conductive polymer and a polyanion. When the conductive polymer-containing liquid applied to the substrate contains a binder component, the conductive layer contains the binder component or a cured product of the binder component.

[0098] [Base material] The substrate constituting the conductive laminate of this embodiment may be a substrate made of an insulating material or a substrate made of a conductive material. The shape of the substrate is not particularly limited, and examples thereof include a shape mainly having a flat surface such as a film or a substrate. Examples of insulating materials include glass, synthetic resin, and ceramics. The conductive material may be a metal, a conductive metal oxide, carbon, or the like.

[0099] (Film substrate) When a film substrate is used as the substrate, the conductive laminate becomes a conductive film. The film substrate may be, for example, a plastic film made of a synthetic resin, such as ethylene-methyl methacrylate copolymer resin, ethylene-vinyl acetate copolymer resin, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinyl alcohol, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyacrylate, polycarbonate, polyvinylidene fluoride, polyarylate, styrene-based elastomer, polyester-based elastomer, polyethersulfone, polyetherimide, polyetheretherketone, polyphenylene sulfide, polyimide, cellulose triacetate, cellulose acetate propionate, etc. From the viewpoint of improving the adhesion between the film substrate and the conductive layer, the synthetic resin for the film substrate is preferably the same type of resin as the binder resin, and among these, a polyester resin such as polyethylene terephthalate is preferred.

[0100] The synthetic resin for the film substrate may be either amorphous or crystalline. The film substrate may be either unstretched or stretched. The film substrate may be subjected to a surface treatment such as a corona discharge treatment, a plasma treatment, or a flame treatment in order to further improve the adhesiveness of the conductive layer formed from the conductive polymer-containing liquid.

[0101] The average thickness of the film substrate is preferably 5 μm to 500 μm, more preferably 20 μm to 200 μm. If the average thickness of the film substrate is equal to or more than the lower limit, the film is less likely to break, and if the average thickness is equal to or less than the upper limit, the film can have sufficient flexibility. The average thickness of the film substrate is calculated by measuring the thickness at 10 randomly selected points and averaging the measured values.

[0102] (Glass substrate) Examples of the glass substrate include an alkali-free glass substrate, a soda-lime glass substrate, a borosilicate glass substrate, and a quartz glass substrate. If the substrate contains an alkali component, the conductivity of the conductive layer tends to decrease, so among the above glass substrates, an alkali-free glass is preferred. Here, the alkali-free glass refers to a glass composition in which the content of the alkali component is 0.1 mass% or less with respect to the total mass of the glass composition.

[0103] The average thickness of the glass substrate is preferably 100 μm or more and 3000 μm or less, and more preferably 100 μm or more and 1000 μm or less. If the average thickness of the glass substrate is equal to or more than the lower limit, the substrate is less likely to be broken, and if the average thickness is equal to or less than the upper limit, the substrate can contribute to making the conductive laminate thinner. The average thickness of the glass substrate is calculated by measuring the thickness at 10 randomly selected points and averaging the measured values.

[0104] <Method for manufacturing conductive laminate> A fourth aspect of the present invention is a method for producing a conductive laminate, the method including applying the conductive polymer-containing liquid of the first aspect to at least one surface of a substrate. The conductive laminate of the third aspect can be produced by the production method of this aspect.

[0105] Examples of a method for applying (coating) the conductive polymer-containing liquid of the first embodiment to an arbitrary surface of a substrate include a method using a coater such as a gravure coater, a roll coater, a curtain flow coater, a spin coater, a bar coater, a reverse coater, a kiss coater, a fountain coater, a rod coater, an air doctor coater, a knife coater, a blade coater, a cast coater, or a screen coater; a method using a sprayer such as an air spray, an airless spray, or a rotor dampening; and an immersion method such as dipping.

[0106] The amount of conductive polymer-containing liquid applied to the substrate is not particularly limited, but taking into consideration uniform and even application, conductivity, and film strength, a solid content of 0.01 g / m 2 More than 10.0g / m 2 The following ranges are preferred:

[0107] The coating film made of the conductive polymer-containing liquid applied onto the substrate is dried to remove the dispersion medium, thereby obtaining a conductive laminate in which a conductive layer (conductive film) is formed by hardening the coating film. Methods for drying the coating film include heat drying, vacuum drying, etc. Examples of heat drying that can be used include hot air heating and infrared heating. When applying heat drying, the heating temperature is appropriately set depending on the dispersion medium used, but is usually within the range of 50° C. to 150° C. Here, the heating temperature is the set temperature of the drying device. A suitable drying time within the above heating temperature range is preferably 1 minute to 30 minutes, more preferably 5 minutes to 15 minutes.

[0108] In the case where the conductive polymer-containing liquid contains an active energy ray-curable binder component, the method may further include an active energy ray irradiation step of irradiating the dried conductive polymer coating film with active energy rays after the drying step. By including the active energy ray irradiation step, the rate of forming the conductive layer can be increased, and the productivity of the conductive film can be improved. In the case where the active energy ray irradiation step is included, examples of the active energy ray used include ultraviolet rays, electron beams, visible light, etc. Examples of the light source of the ultraviolet ray that can be used include light sources such as ultra-high pressure mercury lamps, high pressure mercury lamps, low pressure mercury lamps, carbon arcs, xenon arcs, and metal halide lamps. The illuminance of ultraviolet light is 100mW / cm 2 Illuminance of 100mW / cm or more is preferable. 2 If the radiation dose is less than 50 mJ / cm2, the active energy ray-curable binder component may not be cured sufficiently. 2 More than 50mJ / cm is preferable. 2 If the irradiance is less than 100 nm, crosslinking may not be sufficient. In this specification, the illuminance and the integrated light amount are values ​​measured using a Topcon UVR-T1 (industrial UV checker, photoreceiver: UD-T36, measurement wavelength range: 300 nm to 390 nm, peak sensitivity wavelength: about 355 nm). EXAMPLES

[0109] (Production Example 1) Production of polystyrene sulfonic acid 206 g of sodium styrenesulfonate was dissolved in 1000 ml of ion-exchanged water, and while stirring at 80° C., 1.14 g of an oxidizing agent solution of ammonium persulfate previously dissolved in 10 ml of water was added dropwise over 20 minutes, and the solution was stirred for 12 hours. 1000ml of sulfuric acid diluted to 10% by mass was added to the obtained sodium styrene sulfonate-containing solution, and about 1000ml of the solvent was removed from the polystyrene sulfonic acid-containing solution by ultrafiltration. Next, 2000ml of ion-exchanged water was added to the remaining liquid, and about 2000ml of the solvent was removed by ultrafiltration, and the polystyrene sulfonic acid was washed with water. This washing operation was repeated three times. Water in the resulting solution was removed under reduced pressure to obtain colorless solid polystyrene sulfonic acid.

[0110] (Production Example 2) Synthesis of a conductive polymer dispersion containing a π-conjugated conductive polymer and a polyanion 14.2 g of 3,4-ethylenedioxythiophene and a solution in which 36.7 g of polystyrene sulfonic acid was dissolved in 2000 ml of ion-exchanged water were mixed at 20°C. The resulting mixed solution was kept at 20° C., and while stirring, 29.64 g of ammonium persulfate and 8.0 g of an oxidation catalyst solution of ferric sulfate dissolved in 200 ml of ion-exchanged water were slowly added, followed by stirring for 3 hours to allow the reaction to proceed. To the reaction solution, 2000 ml of ion-exchanged water was added, and about 2000 ml of the solvent was removed by ultrafiltration. This operation was repeated three times. Next, 200 ml of sulfuric acid diluted to 10% by mass and 2000 ml of ion-exchanged water were added to the obtained solution, and about 2000 ml of the solvent was removed by ultrafiltration. 2000 ml of ion-exchanged water was added to the remaining liquid, and about 2000 ml of the solvent was removed by ultrafiltration. This operation was repeated three times. Furthermore, 2000 ml of ion-exchanged water was added to the obtained solution, and about 2000 ml of the solvent was removed by ultrafiltration. This operation was repeated five times to obtain an aqueous dispersion of polystyrene sulfonate-doped poly(3,4-ethylenedioxythiophene) (PEDOT-PSS) with a concentration of 1.2 mass%.

[0111] Example 1 200g of methanol and 25g of an epoxy compound (Epolite M-1230, C12, C13 mixed higher alcohol glycidyl ether, manufactured by Kyoeisha Chemical Co., Ltd.) were added to 100g of the aqueous dispersion of PEDOT-PSS obtained in Production Example 2, and the mixture was heated and stirred at 60°C for 4 hours. At this time, the epoxy compound reacted and bonded to a part of the excess sulfonic acid groups in PEDOT-PSS that were not bonded to PEDOT of PSS. Next, 100g of isopropanol and 1.0g of tetraoctylammonium bromide were added. At this time, a quaternary ammonium compound bonded to the excess sulfonic acid groups in PEDOT-PSS that were not bonded to PEDOT of PSS. As a result, the water dispersibility of PEDOT-PSS decreased, and a conductive complex containing PEDOT-PSS modified by the reaction of the epoxy compound and the quaternary ammonium compound was precipitated. The precipitate was collected by filtration to obtain 2.0g of a conductive complex. Next, the conductive complex was added to 798.0 g of ethyl acetate and dispersed using a high-pressure homogenizer to obtain a conductive polymer-containing liquid. The obtained conductive polymer-containing liquid was applied onto a PET film (Lumirror T60, manufactured by Toray Industries, Inc.) using a bar coater #4, and dried for 1 minute at 100° C. The surface resistance of the obtained conductive film was measured, and the results are shown in Table 1. Moreover, the conductive polymer-containing liquid obtained above was allowed to stand at room temperature (25° C.) for 24 hours, and the results of observation thereafter are shown in Table 1.

[0112] Example 2 A conductive film was prepared in the same manner as in Example 1, except that ethyl acetate was replaced with butyl acetate, and the surface resistance value was measured. The results are shown in Table 1.

[0113] Example 3 A conductive film was prepared in the same manner as in Example 1, except that ethyl acetate was replaced with isopropyl acetate, and the surface resistance value was measured. The results are shown in Table 1.

[0114] Example 4 A conductive film was prepared in the same manner as in Example 1, except that ethyl acetate was replaced with isobutyl acetate, and the surface resistance value was measured. The results are shown in Table 1.

[0115] Example 5 200g of methanol and 25g of butyl glycidyl ether were added to 100g of the aqueous dispersion of PEDOT-PSS obtained in Production Example 2, and the mixture was heated and stirred at 60°C for 4 hours. At this time, an epoxy compound reacted and bonded to a part of the excess sulfonic acid groups in PEDOT-PSS that were not bonded to PEDOT of PSS. Next, 100g of isopropanol and 1.0g of tetraoctylammonium bromide were added. At this time, a quaternary ammonium compound bonded to the excess sulfonic acid groups in PEDOT-PSS that were not bonded to PEDOT of PSS. As a result, the water dispersibility of PEDOT-PSS decreased, and a conductive complex containing PEDOT-PSS modified by the reaction of an epoxy compound and a quaternary ammonium compound was precipitated. The precipitate was collected by filtration to obtain 1.9g of a conductive complex. Next, the conductive complex was added to 798.1 g of ethyl acetate and dispersed using a high-pressure homogenizer to obtain a conductive polymer-containing liquid. The obtained conductive polymer-containing liquid was applied onto a PET film (Lumirror T60, manufactured by Toray Industries, Inc.) using a bar coater #4, and dried for 1 minute at 100° C. The surface resistance of the obtained conductive film was measured, and the results are shown in Table 1.

[0116] Example 6 200g of methanol and 25g of an epoxy compound (Epolite M-1230, C12, C13 mixed higher alcohol glycidyl ether, manufactured by Kyoeisha Chemical Co., Ltd.) were added to 100g of the aqueous dispersion of PEDOT-PSS obtained in Production Example 2, and the mixture was heated and stirred at 60°C for 4 hours. At this time, the epoxy compound reacted and bonded to a part of the excess sulfonic acid groups in PEDOT-PSS that were not bonded to PEDOT of PSS. Next, 100g of isopropanol and 1.0g of tetrabutylammonium bromide were added. At this time, a quaternary ammonium compound bonded to the excess sulfonic acid groups in PEDOT-PSS that were not bonded to PEDOT of PSS. As a result, the water dispersibility of PEDOT-PSS decreased, and a conductive complex containing PEDOT-PSS modified by the reaction of the epoxy compound and the quaternary ammonium compound was precipitated. The precipitate was collected by filtration, and 1.9g of a conductive complex was obtained. Next, the conductive complex was added to 798.1 g of ethyl acetate and dispersed using a high-pressure homogenizer to obtain a conductive polymer-containing liquid. The obtained conductive polymer-containing liquid was applied onto a PET film (Lumirror T60, manufactured by Toray Industries, Inc.) using a bar coater #4, and dried for 1 minute at 100° C. The surface resistance of the obtained conductive film was measured, and the results are shown in Table 1.

[0117] Example 7 200g of methanol and 25g of an epoxy compound (Epolite M-1230, C12, C13 mixed higher alcohol glycidyl ether, manufactured by Kyoeisha Chemical Co., Ltd.) were added to 100g of the aqueous dispersion of PEDOT-PSS obtained in Production Example 2, and the mixture was heated and stirred at 60°C for 4 hours. At this time, the epoxy compound reacted and bonded to a part of the excess sulfonic acid groups in PEDOT-PSS that were not bonded to PEDOT of PSS. Next, 100g of isopropanol and 1.0g of tetraethylammonium bromide were added. At this time, a quaternary ammonium compound bonded to the excess sulfonic acid groups in PEDOT-PSS that were not bonded to PEDOT of PSS. As a result, the water dispersibility of PEDOT-PSS decreased, and a conductive complex containing PEDOT-PSS modified by the reaction of the epoxy compound and the quaternary ammonium compound was precipitated. The precipitate was collected by filtration, and 1.8g of a conductive complex was obtained. Next, the conductive complex was added to 798.2 g of ethyl acetate and dispersed using a high-pressure homogenizer to obtain a conductive polymer-containing liquid. The obtained conductive polymer-containing liquid was applied onto a PET film (Lumirror T60, manufactured by Toray Industries, Inc.) using a bar coater #4, and dried for 1 minute at 100° C. The surface resistance of the obtained conductive film was measured, and the results are shown in Table 1.

[0118] Example 8 200g of methanol and 25g of an epoxy compound (Epolite M-1230, C12, C13 mixed higher alcohol glycidyl ether, manufactured by Kyoeisha Chemical Co., Ltd.) were added to 100g of the aqueous dispersion of PEDOT-PSS obtained in Production Example 2, and the mixture was heated and stirred at 60°C for 4 hours. At this time, the epoxy compound reacted and bonded to a part of the excess sulfonic acid groups in PEDOT-PSS that were not bonded to PEDOT of PSS. Next, 100g of isopropanol and 1.0g of tetradecylammonium bromide were added. At this time, a quaternary ammonium compound bonded to the excess sulfonic acid groups in PEDOT-PSS that were not bonded to PEDOT of PSS. As a result, the water dispersibility of PEDOT-PSS decreased, and a conductive complex containing PEDOT-PSS modified by the reaction of the epoxy compound and the quaternary ammonium compound was precipitated. The precipitate was collected by filtration, and 2.2g of a conductive complex was obtained. Next, the conductive complex was added to 797.8 g of ethyl acetate and dispersed using a high-pressure homogenizer to obtain a conductive polymer-containing liquid. The obtained conductive polymer-containing liquid was applied onto a PET film (Lumirror T60, manufactured by Toray Industries, Inc.) using a bar coater #4, and dried for 1 minute at 100° C. The surface resistance of the obtained conductive film was measured, and the results are shown in Table 1.

[0119] Example 9 174g of methanol and 25g of an epoxy compound (Epolite M-1230, C12, C13 mixed higher alcohol glycidyl ether, manufactured by Kyoeisha Chemical Co., Ltd.) were added to 100g of the aqueous dispersion of PEDOT-PSS obtained in Production Example 2, and the mixture was heated and stirred at 60°C for 4 hours. At this time, the epoxy compound reacted and bonded to a part of the excess sulfonic acid groups in PEDOT-PSS that were not bonded to PEDOT of PSS. Next, 1.0g of tetraoctylammonium bromide was added. At this time, a quaternary ammonium compound bonded to the excess sulfonic acid groups in PEDOT-PSS that were not bonded to PEDOT of PSS. As a result, the aqueous dispersibility of PEDOT-PSS decreased, and a conductive complex containing PEDOT-PSS modified by the reaction of the epoxy compound and the quaternary ammonium compound precipitated and precipitated in the solution. Next, 150g of the upper layer (supernatant) of the solution was removed. Further, 300 g of ethyl acetate was added, 300 g of the upper layer (supernatant) of the solution was removed, 300 g of ethyl acetate was added, 300 g of the upper layer (supernatant) of the solution was removed, and 650 g of ethyl acetate was added. Next, the mixture was further dispersed using a high-pressure homogenizer to obtain a conductive polymer-containing liquid. The obtained conductive polymer-containing liquid was applied onto a PET film (Lumirror T60, manufactured by Toray Industries, Inc.) using a bar coater #4, and dried for 1 minute at 100° C. The surface resistance of the obtained conductive film was measured, and the results are shown in Table 1.

[0120] Comparative Example 1 200g of methanol and 25g of an epoxy compound (Epolite M-1230, C12, C13 mixed higher alcohol glycidyl ether, manufactured by Kyoeisha Chemical Co., Ltd.) were added to 100g of the aqueous dispersion of PEDOT-PSS obtained in Production Example 2, and the mixture was heated and stirred at 60°C for 4 hours. At this time, the epoxy compound reacted and bonded to some of the excess sulfonic acid groups in PEDOT-PSS that were not bonded to PEDOT of PSS. Next, 100g of isopropanol was added. As a result, the water dispersibility of PEDOT-PSS decreased, and a conductive complex containing PEDOT-PSS modified by the reaction of the epoxy compound was precipitated. The precipitate was collected by filtration to obtain 1.5g of a conductive complex. Next, the above conductive complex was added to 798.5 g of ethyl acetate and dispersed using a high-pressure homogenizer. However, all of the conductive complex settled and separated within a few minutes, and the study was discontinued.

[0121] Comparative Example 2 200g of methanol, 100g of isopropanol, and 1g of tetraoctylammonium bromide were added to 100g of the aqueous dispersion of PEDOT-PSS obtained in Production Example 2. As a result, the aqueous dispersibility of PEDOT-PSS decreased, and a conductive complex containing PEDOT-PSS and a quaternary ammonium compound bonded thereto was precipitated. The precipitate was collected by filtration to obtain 1.8g of the conductive complex. Next, the above conductive complex was added to 798.2 g of ethyl acetate and dispersed using a high-pressure homogenizer. However, all of the conductive complex settled and separated within a few minutes, and the study was discontinued.

[0122] [Surface resistance measurement] For the conductive films prepared in each example, the surface resistance value of the conductive layer was measured using a resistivity meter (Hiresta manufactured by Nitto Seiko Analytech Co., Ltd.) under the condition of an applied voltage of 10 V. In the table, "1.0E+06" means "1.0×10 6 " and so on.

[0123] [Table 1]

[0124] <Consideration 1> In the conductive polymer-containing liquids of Examples 1 to 9, the conductive complex is modified with an epoxy compound and a quaternary ammonium compound, and therefore has excellent dispersibility in ester solvents such as ethyl acetate. When these conductive polymer-containing liquids were applied to a film substrate, a conductive layer having excellent conductivity could be formed. In Example 9, the conductive polymer-containing liquid was obtained by the solvent replacement method (decantation method) without performing a filtration process, and thus a conductive film with even more excellent conductivity was obtained. The conductive composite of Comparative Example 1 was modified only with an epoxy compound, and was not modified with a quaternary ammonium compound, and therefore could not be dispersed in an ester-based solvent. The conductive composite of Comparative Example 2 was modified only with a quaternary ammonium compound, and was not modified with an epoxy compound, and therefore could not be dispersed in an ester-based solvent.

[0125] Example 10 A coating material was obtained by mixing 60 g of SK Dyne 1499M (manufactured by Soken Chemical Industries, Ltd., acrylic adhesive, solid content 35 mass%, ethyl acetate, butyl acetate mixed solution) and 1.6 g of hardener L-45 (manufactured by Soken Chemical Industries, Ltd., toluene diisocyanate-trimethylolpropane adduct, solid content 45 mass%, toluene, ethyl acetate mixed solution) with 40 g of the conductive polymer-containing liquid of Example 1. This coating material was applied onto a PET film (Toray Industries, Ltd., Lumirror T60) using a bar coater #16, dried at 100°C for 1 minute, and the surface resistance value of the formed conductive layer was measured. Next, a PET film was pressure-bonded to a part of the conductive layer, and alkali-free glass (thickness 0.7 mm) was pressure-bonded to the other part of the conductive layer, and the resultant was aged at room temperature for 48 hours. Next, the bonded PET film was cut into 10 mm wide strips and a 180° peel test was performed to measure the peel strength. Furthermore, the surface of the alkali-free glass bonded to the conductive layer was rubbed with a nonwoven fabric to measure the electrostatic charge. The results of these measurements are shown in Table 2.

[0126] Comparative Example 3 A test sample was prepared and measured in the same manner as in Example 10, except that the conductive polymer-containing liquid was changed to ethyl acetate in Example 10. The measurement results are shown in Table 2.

[0127] [Peel force measurement] For the coating film formed on the test sample of each example, the peel strength was measured by the following method to evaluate the releasability. According to JIS Z0237, a PET film (width 10 mm) pressed onto the surface of the conductive layer was peeled off at an angle of 180° (peel speed 0.3 m / min) using a tensile tester to measure the peel force (unit: N). The smaller the peel force, the higher the releasability of the coating film.

[0128] [Charged voltage] The electrostatic potential on the surface of the non-alkali glass attached to the coating film of each test sample was measured by the following method to evaluate the antistatic properties. According to JIS C61340-2-2:2006, the surface potential of the alkali-free glass plate that was charged by rubbing with the nonwoven fabric as described above was measured using a digital low potential meter (KSD-3000, manufactured by Kasuga Electric Co., Ltd.). This surface potential was taken as the charging voltage of the alkali-free glass plate. The lower the charging voltage, the better the antistatic properties.

[0129] [Table 2]

[0130] <Consideration 2> In the conductive polymer-containing liquid of Example 10, an adhesive was added to the conductive polymer-containing liquid of Example 1. In the conductive polymer-containing liquid before the adhesive was added, the conductive complex was sufficiently dispersed in the ester-based solvent. Therefore, even in the conductive polymer-containing liquid (paint) after the adhesive containing the ester-based solvent was added, the conductive complex did not settle and was stably dispersed. As a result, the paint was applied to a film substrate to form a conductive layer that exhibited excellent conductivity, adhesion, and antistatic properties. In Comparative Example 3, since the paint did not contain a conductive complex, the formed coating film did not exhibit conductivity.

[0131] Example 11 To 60 g of the conductive polymer-containing liquid obtained in Example 1, 1.5 g of KS-3703T (addition curing silicone, solid content 30 mass%, toluene solution), 25.5 g of toluene, and 0.3 g of CAT-PL-50T (Platinum catalyst, Shin-Etsu Chemical Co., Ltd.) were added to obtain a coating material. This coating material was applied onto a PET film using a #8 bar coater and dried at 150°C for 1 minute to obtain a conductive film. The results of measuring the surface resistance and peel strength of the obtained conductive film are shown in Table 3.

[0132] Comparative Example 4 A test sample was prepared and measured in the same manner as in Example 11, except that the conductive polymer-containing liquid was changed to ethyl acetate in Example 11. The measurement results are shown in Table 3.

[0133] [Peel force measurement] For the coating film formed on the film of each example, the peel strength was measured by the following method to evaluate the releasability. A 25 mm wide polyester adhesive tape (No. 31B, manufactured by Nitto Denko Corporation) was placed on the surface of the coating of each film example, and a load of 1976 Pa was placed on the adhesive tape and pressure treated at 25°C for 20 hours. Next, in accordance with JIS Z0237, the adhesive tape attached to the coating was peeled off at an angle of 180° (peel speed 0.3 m / min) using a tensile tester to measure the peel force (unit: N). The smaller the peel force, the higher the releasability of the coating.

[0134] [Table 3]

[0135] <Consideration 3> In the conductive polymer-containing liquid of Example 11, a silicone compound was added to the conductive polymer-containing liquid of Example 1. In the conductive polymer-containing liquid before the silicone compound was added, the conductive complex was sufficiently dispersed in the ester-based solvent. Therefore, even in the conductive polymer-containing liquid (paint) after the silicone compound was added together with toluene, which is a non-polar solvent, the conductive complex did not settle and was stably dispersed. As a result, the paint was applied to a film substrate to form a conductive layer that exhibited excellent conductivity and releasability. In Comparative Example 4, since the paint did not contain a conductive complex, the formed coating film did not exhibit conductivity.

[0136] Example 12 10g of Artresin UN-904M (manufactured by Negami Chemical Industries, urethane acrylate, solid content 80 mass%, methyl ethyl ketone solution), 30g of pentaerythritol triacrylate, 10g of diacetone alcohol, and 1.6g of Irgacure 184 (manufactured by BASF, photopolymerization initiator) were added to 50g of the conductive polymer-containing liquid obtained in Example 1 to obtain a paint. This paint was applied onto a PET film using a #8 bar coater, dried at 100°C for 1 minute, and irradiated with 400mJ of ultraviolet light to obtain a conductive film. The results of measuring the surface resistance of the obtained conductive film are shown in Table 4.

[0137] Comparative Example 5 A test sample was prepared and measured in the same manner as in Example 12, except that the conductive polymer-containing liquid was changed to ethyl acetate in Example 12. The measurement results are shown in Table 4.

[0138] [Table 4]

[0139] <Consideration 4> In the conductive polymer-containing liquid of Example 12, a photocurable acrylic compound was added to the conductive polymer-containing liquid of Example 1. In the conductive polymer-containing liquid before the acrylic compound was added, the conductive complex was sufficiently dispersed in the ester-based solvent. Therefore, even in the conductive polymer-containing liquid (paint) after the acrylic compound was added together with the polar solvent methyl ethyl ketone, the conductive complex did not settle and was stably dispersed. As a result, the paint was applied to a film substrate to form a conductive layer exhibiting excellent conductivity and hardness (hard coat properties). In Comparative Example 5, since the paint did not contain a conductive complex, the formed coating film did not exhibit conductivity.

Claims

1. The conductive composite material includes a π-conjugated conductive polymer and a polyanion, and an organic solvent, the polyanion being modified by a reaction between a part of an anion group of the polyanion, an epoxy compound, and a quaternary ammonium compound, The quaternary ammonium compound is a quaternary ammonium salt having one nitrogen atom and four hydrocarbon groups bonded to the nitrogen atom, The conductive polymer-containing liquid, wherein the organic solvent contains an ester group-containing compound.

2. The conductive polymer-containing liquid according to claim 1 , wherein the ester group-containing compound is one or more compounds selected from the group consisting of compounds represented by the following formula 1: Formula 1: R 21 -C(=O)-OR 22 [In the formula, R 21 represents a hydrogen atom, a methyl group, or an ethyl group; R 22 represents a linear or branched alkyl group having 1 to 6 carbon atoms.

3. 3. The conductive polymer-containing liquid according to claim 1, wherein the π-conjugated conductive polymer contains poly(3,4-ethylenedioxythiophene), or the polyanion contains polystyrenesulfonic acid.

4. The conductive polymer-containing liquid according to any one of claims 1 to 3, wherein the epoxy compound has 4 or more carbon atoms, or the quaternary ammonium compound has a substituent having 4 or more carbon atoms on a nitrogen atom.

5. The conductive polymer-containing liquid according to any one of claims 1 to 4, further comprising an adhesive or a binder component other than the adhesive.

6. a precipitation recovery step of adding an epoxy compound and a quaternary ammonium compound to a conductive polymer aqueous dispersion in which a conductive complex containing a π-conjugated conductive polymer and a polyanion is contained in an aqueous dispersion medium, and then recovering the precipitated reaction product; and an organic solvent adding step of obtaining a conductive polymer-containing liquid by adding an organic solvent to the reaction product, The quaternary ammonium compound is a quaternary ammonium salt having one nitrogen atom and four hydrocarbon groups bonded to the nitrogen atom, The method for producing a conductive polymer-containing liquid, wherein the organic solvent contains an ester group-containing compound.

7. 7. The method for producing a conductive polymer-containing liquid according to claim 6, wherein the ester group-containing compound is one or more compounds selected from the group of compounds represented by the following formula 1: Formula 1: R 21 -C(=O)-OR 22 [In the formula, R 21 represents a hydrogen atom, a methyl group, or an ethyl group; R 22 represents a linear or branched alkyl group having 1 to 6 carbon atoms.

8. The method for producing a conductive polymer-containing liquid according to claim 6 or 7, further comprising the step of adding an adhesive or a binder component other than the adhesive.

9. A conductive laminate comprising a substrate and a conductive layer formed on at least one surface thereof, the conductive layer being a cured layer of the conductive polymer-containing liquid according to any one of claims 1 to 5.

10. A method for producing a conductive laminate, comprising applying the conductive polymer-containing liquid according to any one of claims 1 to 5 to at least one surface of a substrate.

Citation Information

Patent Citations

  • Electroconductive composition, electroconductive film obtained by using the same and laminated product comprising the conductive film

    JP2009275088A

  • Conductive polymer solution and method for producing the same

    JP2011032382A

  • Conductive polymer solution, conductive coated film and input device

    JP2012201837A

  • Conductive polymer dispersion liquid and conductive coating film

    JP2015131890A

  • Electroconductive polymer-containing liquid, manufacturing method thereof and manufacturing method of conductive film

    JP2020097680A