Magnetic tape cartridge and magnetic tape device
The magnetic tape cartridge design with controlled tension and reduced thickness addresses deformation issues, ensuring accurate data recording and playback in long-term storage by minimizing misalignment.
Patent Information
- Application Number
- JP2020214222
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-23
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-12-23
AI Technical Summary
Magnetic tapes in data storage devices are prone to deformation over time, leading to misalignment of the magnetic head during recording and playback, which can result in data overwriting and poor reproduction, especially in long-term storage applications.
A magnetic tape cartridge design that applies a tension of 0.30N or less in the longitudinal direction during rewinding onto the cartridge reel, combined with a magnetic tape thickness of 5.6 μm or less, to minimize deformation and maintain accurate track positioning.
This approach ensures successful data recording and playback on magnetic tapes after storage by reducing deformation-induced misalignment, thereby enhancing data integrity and reliability in long-term storage.
Smart Images

Figure 0007565785000013 
Figure 0007565785000014 
Figure 0007565785000015
Abstract
Description
[Technical field]
[0001] The present invention relates to a magnetic tape cartridge and a magnetic tape device. [Background technology]
[0002] Magnetic recording media include tape-type and disk-type recording media, and tape-type magnetic recording media, that is, magnetic tapes, are primarily used for data storage applications such as data backup and archiving (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 6590102 specification Summary of the Invention [Problem to be solved by the invention]
[0004] Data is usually recorded on a magnetic tape by running the magnetic tape in a magnetic tape device (usually called a "drive") and recording data on the data band by making a magnetic head follow the data band of the magnetic tape. This forms a data track on the data band. When playing back recorded data, the magnetic tape is run in the magnetic tape device and the magnetic head follows the data band of the magnetic tape to read the data recorded on the data band. After such recording or playback, the magnetic tape is stored wound on a reel (hereinafter referred to as a "cartridge reel") in a magnetic tape cartridge until the next recording and / or playback is performed.
[0005] After the above storage, when recording and / or reproducing is performed, if the magnetic head for recording and / or reproducing data deviates from the target track position due to deformation of the magnetic tape and performs recording and / or reproducing of data, phenomena such as overwriting of recorded data and reproduction failure may occur. Meanwhile, in the field of data storage, there has been an increasing need in recent years for long-term storage of data, known as archives. However, in general, the longer the storage period, the more likely the magnetic tape is to deform. Therefore, it is expected that there will be an even greater demand in the future for suppressing the occurrence of the above phenomena after storage.
[0006] In view of the above, an object of one aspect of the present invention is to provide a means for enabling good recording and / or reproduction of data on a magnetic tape after storage. [Means for solving the problem]
[0007] One aspect of the present invention is A magnetic tape cartridge including a magnetic tape and a cartridge reel, a magnetic tape cartridge in which the magnetic tape has a minimum load for causing a slippage of 250 N or less (hereinafter also simply referred to as the "minimum load for causing a slippage") measured after the magnetic tape is rewound on the cartridge reel with a tension of 0.30 N (Newton) applied in the longitudinal direction of the magnetic tape; Regarding.
[0008] In one embodiment, the magnetic tape can have a non-magnetic support and a magnetic layer containing ferromagnetic powder, and the non-magnetic support can be a polyester support.
[0009] In one embodiment, the magnetic tape can further include a non-magnetic layer containing non-magnetic powder between the non-magnetic support and the magnetic layer.
[0010] In one embodiment, the magnetic tape can further have a backcoat layer containing a nonmagnetic powder on the surface side of the nonmagnetic support opposite to the surface side having the magnetic layer.
[0011] In one embodiment, the magnetic tape may have a tape thickness of 5.6 μm or less.
[0012] In one embodiment, the magnetic tape may have a tape thickness of 5.3 μm or less.
[0013] In one embodiment, the minimum load at which a winding slippage occurs can be 10N or more and 250N or less.
[0014] In one embodiment, the squareness ratio of the magnetic tape in the perpendicular direction can be 0.60 or more.
[0015] In one embodiment, the magnetic tape cartridge can be used in a magnetic tape device, which runs the magnetic tape between a take-up reel and a cartridge reel of the magnetic tape cartridge with tension applied in the longitudinal direction of the magnetic tape, the maximum value of this tension being 0.50 N or more, and winds the magnetic tape, after running with the magnetic tape under the tension, around the cartridge reel with tension of 0.30 N or less in the longitudinal direction of the magnetic tape.
[0016] One aspect of the present invention relates to a magnetic tape device including the above-mentioned magnetic tape cartridge.
[0017] In one embodiment, the magnetic tape device comprises: The magnetic tape cartridge; A take-up reel; Including, a magnetic tape device which runs the magnetic tape between the take-up reel and a cartridge reel of the magnetic tape cartridge with tension applied in the longitudinal direction of the magnetic tape, the maximum value of this tension being 0.50 N or more, and winds the magnetic tape after running with the magnetic tape under tension of 0.30 N or less in the longitudinal direction of the magnetic tape onto the cartridge reel of the magnetic tape cartridge; It can be.
[0018] In one embodiment, the tension applied to the magnetic tape in the longitudinal direction during the running can be changed. Effect of the Invention
[0019] According to one aspect of the present invention, when recording and / or reproducing data on a magnetic tape after storage, it is possible to perform recording and / or reproducing satisfactorily. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a schematic diagram illustrating an example of a magnetic tape device. [Diagram 2] 2 shows an example of the arrangement of data bands and servo bands. [Diagram 3] An example of servo pattern arrangement on an LTO (Linear Tape-Open) Ultrium format tape is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] One aspect of the present invention relates to a magnetic tape cartridge including a magnetic tape and a cartridge reel, wherein the magnetic tape has a minimum load of 250 N or less at which a slippage occurs, measured after the magnetic tape is rewound onto the cartridge reel with a tension of 0.30 N applied in the longitudinal direction of the magnetic tape.
[0022] Another aspect of the present invention relates to a magnetic tape device including the above magnetic tape cartridge.
[0023] The magnetic tape cartridge includes a magnetic tape and a cartridge reel. In an unused magnetic tape cartridge before being attached to a magnetic tape device for recording and / or reproducing data, the magnetic tape is usually housed in a state wound around the cartridge reel. In the magnetic tape device, the magnetic tape is run between a cartridge reel (supply reel) and a take-up reel to record data on the magnetic tape and / or reproduce the recorded data. After recording or reproducing data, the magnetic tape is rewound onto the cartridge reel and stored in the magnetic tape cartridge in a state wound around the cartridge reel until the next recording and / or reproduction is performed. During storage, it is presumed that the magnetic tape housed in the magnetic tape cartridge undergoes deformation that differs depending on the position, with the portion close to the cartridge reel deforming wider than the initial width due to compressive stress in the tape thickness direction, and the portion farther from the cartridge reel deforming narrower than the initial width due to tensile stress in the tape longitudinal direction. If deformation that differs greatly depending on the position occurs, it is considered that this could cause the magnetic head to record and / or reproduce data while shifting from the target track position when recording and / or reproducing after storage. Regarding the above modification, the inventor has considered the following: (1) The tension applied to the magnetic tape in the longitudinal direction when rewinding it onto the cartridge reel must be a low tension of 0.30 N or less; and (2) The magnetic tape contained in the magnetic tape cartridge is a magnetic tape that is wound around the cartridge reel without being tightly wound when rewound at such low tension; It has been thought that it is possible to suppress the occurrence of the above-mentioned deformation of the magnetic tape during storage. In this regard, the above-mentioned magnetic tape cartridge has a minimum load at which a winding slippage occurs of 250 N or less, measured after the magnetic tape is rewound onto a cartridge reel with a tension of 0.30 N applied in the longitudinal direction of the magnetic tape. The inventors believe that the above-mentioned minimum load at which a winding slippage occurs of 250 N or less indicates that the magnetic tape can be wound onto a cartridge reel without being tightly wound when rewound with the above-mentioned low tension. As a result of extensive research by the inventors, it has been newly discovered that such a magnetic tape cartridge enables good recording and / or reproduction of data on the magnetic tape after storage.
[0024] The magnetic tape cartridge and the magnetic tape device will be described in more detail below. An embodiment of the magnetic tape cartridge and the magnetic tape device will be described below with reference to the drawings. However, the magnetic tape cartridge and the magnetic tape device are not limited to the embodiment shown in the drawings.
[0025] [Magnetic tape device configuration] A magnetic tape device 10 shown in FIG. 1 controls a recording / reproducing head unit 12 in response to commands from a control device 11, and records and reproduces data on a magnetic tape MT. The magnetic tape device 10 has a configuration capable of detecting and adjusting tension applied to the magnetic tape in the longitudinal direction by spindle motors 17A, 17B that control the rotation of the cartridge reel 130 and take-up reel 16 and their drive devices 18A, 18B. The magnetic tape device 10 has a configuration in which a magnetic tape cartridge 13 can be mounted. The magnetic tape device 10 has a cartridge memory read / write device 14 capable of reading from and writing to a cartridge memory 131 in the magnetic tape cartridge 13 . From the magnetic tape cartridge 13 attached to the magnetic tape device 10, the end or leader pin of the magnetic tape MT is pulled out by an automatic loading mechanism or manually, and the magnetic tape MT passes over the recording / playback head via guide rollers 15A and 15B with the magnetic layer surface in a direction facing the recording / playback head surface of the recording / playback head unit 12, and the magnetic tape MT is wound onto the take-up reel 16. The rotation and torque of spindle motors 17A and 17B are controlled by signals from control device 11, and magnetic tape MT runs at any speed and tension. A servo pattern formed in advance on the magnetic tape can be used to control the tape speed. A tension detection mechanism may be provided between magnetic tape cartridge 13 and take-up reel 16 to detect the tension. The tension may be adjusted using guide rollers 15A and 15B in addition to the control by spindle motors 17A and 17B. The cartridge memory read / write device 14 is configured to be able to read and write information from and to the cartridge memory 131 in response to commands from the control device 11. As a communication method between the cartridge memory read / write device 14 and the cartridge memory 131, for example, the ISO (International Organization for Standardization) 14443 method can be adopted.
[0026] The control device 11 includes, for example, a control unit, a storage unit, a communication unit, and the like.
[0027] The recording and reproducing head unit 12 is composed of, for example, a recording and reproducing head, a servo tracking actuator that adjusts the position of the recording and reproducing head in the track width direction, a recording and reproducing amplifier 19, a connector cable for connecting to the control device 11, etc. The recording and reproducing head is composed of, for example, a recording element that records data on the magnetic tape, a reproducing element that reproduces the data on the magnetic tape, and a servo signal reading element that reads the servo signal recorded on the magnetic tape. One magnetic head is equipped with, for example, one or more of each of the recording element, reproducing element, and servo signal reading element. Alternatively, each element may be provided separately in a plurality of magnetic heads according to the running direction of the magnetic tape.
[0028] The recording / reproducing head unit 12 is configured to be capable of recording data onto the magnetic tape MT in response to a command from the control device 11. Also, the recording / reproducing head unit 12 is configured to be capable of reproducing the data recorded onto the magnetic tape MT in response to a command from the control device 11.
[0029] The control device 11 has a mechanism for determining the running position of the magnetic tape from the servo signals read from the servo bands while the magnetic tape MT is running, and for controlling the servo tracking actuator so that the recording element and / or the reproducing element are positioned at the target running position (track position). The control of this track position is performed, for example, by feedback control. The control device 11 has a mechanism for determining the servo band interval from the servo signals read from two adjacent servo bands while the magnetic tape MT is running. The control device 11 also has a mechanism for controlling the torque of the spindle motor 17A and the spindle motor 17B and / or the guide rollers 15A and 15B to adjust and change the tension applied in the longitudinal direction of the magnetic tape so that the servo band interval becomes a target value. The adjustment of this tension is performed, for example, by feedback control. The control device 11 can also store information on the determined servo band interval in a storage unit inside the control device 11, a cartridge memory 131, an external connected device, or the like.
[0030] In the above magnetic tape device, tension can be applied in the longitudinal direction of the magnetic tape during recording and / or playback. In one embodiment, the tension applied in the longitudinal direction of the magnetic tape during recording and / or playback is a constant value, and in another embodiment, it varies. With respect to tension in the present invention and this specification, the value of the tension applied in the longitudinal direction of the magnetic tape in the magnetic tape device is the value of tension used by the control device of the magnetic tape device to control the mechanism for adjusting the above tension as the tension to be applied in the longitudinal direction of the magnetic tape. In addition, the tension actually applied in the longitudinal direction of the magnetic tape in the magnetic tape device can be detected, for example, by providing a tension detection mechanism between the magnetic tape cartridge 13 and the take-up reel 16 in FIG. 1, as described above. Furthermore, for example, the minimum tension can be controlled by the control device of the magnetic tape device so that it does not fall below a value or a recommended value set by a standard, etc., and / or the maximum tension does not exceed a value or a recommended value set by a standard, etc.
[0031] [Magnetic tape cartridge] Before being loaded into a magnetic tape device and after being removed from the magnetic tape device, a magnetic tape cartridge generally contains a magnetic tape wound around a cartridge reel inside the cartridge body. The cartridge reel is rotatably provided inside the cartridge body. As magnetic tape cartridges, single-reel type magnetic tape cartridges having one reel inside the cartridge body and twin-reel type magnetic tape cartridges having two reels inside the cartridge body are widely used. The magnetic tape cartridge included in the magnetic tape device can be a single-reel type magnetic tape cartridge in one form, and can be a twin-reel type magnetic tape cartridge in another form. In the case of a twin-reel type magnetic tape cartridge, the cartridge reel refers to the reel on which the magnetic tape is mainly wound when it is stored after data is recorded and / or played back, and the other reel is referred to as the winding reel. When a single-reel magnetic tape cartridge is loaded into a magnetic tape device for recording and / or reproducing data on the magnetic tape, the magnetic tape is pulled out from the magnetic tape cartridge and wound around the take-up reel of the magnetic tape device, as shown in FIG. 1 for example. A magnetic head is disposed in the magnetic tape transport path from the magnetic tape cartridge to the take-up reel. The magnetic tape runs by being fed out and taken up between the cartridge reel (also called the "supply reel") of the magnetic tape cartridge and the take-up reel of the magnetic tape device. During this time, the magnetic head comes into contact with and slides against the magnetic layer surface of the magnetic tape, thereby recording and / or reproducing data. In contrast, a dual-reel magnetic tape cartridge is provided with both a supply reel and a take-up reel inside the magnetic tape cartridge.
[0032] In one embodiment, the magnetic tape cartridge may include a cartridge memory. The cartridge memory may be, for example, a non-volatile memory, in which tension adjustment information is already recorded or tension adjustment information is to be recorded. The tension adjustment information is information for adjusting the tension applied in the longitudinal direction of the magnetic tape. For the cartridge memory, the above description may also be referred to.
[0033] [Tension during running, tension during winding onto cartridge reel] In the magnetic tape device, the magnetic tape is run between a cartridge reel (supply reel) and a take-up reel, and data can be recorded on the magnetic tape and / or the recorded data can be reproduced. In the magnetic tape device, tension can be applied in the longitudinal direction of the magnetic tape during the running. The greater the tension applied in the longitudinal direction of the magnetic tape, the greater the shrinkage of the widthwise dimension of the magnetic tape (i.e., the narrower the width can be), and the smaller the tension, the smaller the degree of shrinkage can be. Therefore, the widthwise dimension of the magnetic tape can be controlled by the value of the tension applied in the longitudinal direction of the magnetic tape running in the magnetic tape device. In one embodiment, the magnetic tape device can run the magnetic tape with a maximum tension of 0.50 N or more applied in the longitudinal direction. If the magnetic tape is stored in the magnetic tape cartridge after running in such a state of being subjected to a large tension, it is considered that the magnetic tape is likely to be deformed during storage. As described above, it is presumed that during storage, the magnetic tape contained in a magnetic tape cartridge undergoes deformation that varies depending on position, with the portion close to the cartridge reel deforming wider than initial due to compressive stress in the tape thickness direction, and the portion farther from the cartridge reel deforming narrower than initial due to tensile stress in the tape longitudinal direction, and that magnetic tape stored under large tension is more likely to experience greater differences in deformation depending on position. Therefore, in one embodiment, in the magnetic tape device, when the magnetic tape is wound onto the cartridge reel after running with a tension of 0.50 N or more applied in the longitudinal direction, it is preferable that the tension applied in the longitudinal direction of the magnetic tape is 0.30 N or less. This makes it possible to wind the magnetic tape onto the cartridge reel with a tension smaller than the tension applied in the longitudinal direction during running and store it in the magnetic tape cartridge, and therefore the inventor believes that the occurrence of the phenomenon that may occur due to the deformation described above can be suppressed. Furthermore, the inventor presumes that, regardless of whether tension was applied during running or not and the value of the tension, it is preferable to apply a tension of 0.30 N or less in the longitudinal direction of the magnetic tape when winding the magnetic tape onto the cartridge reel after running in order to suppress the occurrence of the phenomenon that may occur due to the deformation described above.
[0034] When tension is applied in the longitudinal direction of the magnetic tape in the above magnetic tape device, the maximum value of the tension can be 0.50N or more, 0.60N or more, 0.70N or more, or 0.80N or more. The maximum value can be, for example, 1.50N or less, 1.40N or less, 1.30N or less, 1.20N or less, 1.10N or less, or 1.00N or less. The tension applied in the longitudinal direction of the magnetic tape during running can be a constant value or can be changed. In the case of a constant value, the tension applied in the longitudinal direction of the magnetic tape can be controlled, for example, by a control device of the magnetic tape device, so that a constant value of tension is applied in the longitudinal direction of the magnetic tape. On the other hand, when the tension applied in the longitudinal direction of the magnetic tape during running is changed, for example, a servo signal can be used to obtain dimensional information in the width direction of the magnetic tape during running, and the tension applied in the longitudinal direction of the magnetic tape can be adjusted and changed according to the obtained dimensional information. This makes it possible to control the dimension in the width direction of the magnetic tape. One form of such tension adjustment has been described above with reference to FIG. 1. However, the above magnetic tape device is not limited to the above-mentioned embodiment. In the above magnetic tape device, when the tension applied in the longitudinal direction of the running magnetic tape is changed, the minimum value can be, for example, 0.10 N or more, 0.20 N or more, 0.30 N or more, or 0.40 N or more. In one embodiment, the minimum value can be, for example, 0.40 N or less or less than 0.40 N, and in another embodiment, it can be 0.60 N or less or 0.50 N or less.
[0035] In a magnetic tape device, when a magnetic tape is run for recording and / or reproducing data, the following specific modes of running the magnetic tape can be given. Type 1: At the end of a run for recording and / or reproducing data, the entire length of the magnetic tape is wound onto the take-up reel. Type 2: At the end of a run for recording and / or reproducing data, the entire length of the magnetic tape is wound onto the cartridge reel. Mode 3: At the end of running for recording and / or reproducing data, a portion of the magnetic tape is wound on the cartridge reel and a portion is wound on the take-up reel.
[0036] The tension applied to the magnetic tape after it has been run in the longitudinal direction when it is wound onto the cartridge reel (hereinafter also referred to as "rewind tension") refers to the following tension. In the first embodiment, the rewinding tension is a tension applied in the longitudinal direction of the magnetic tape when the entire length of the magnetic tape is wound onto a cartridge reel to be housed in a magnetic tape cartridge. In form 2, first, the magnetic tape is wound from the cartridge reel onto the take-up reel. The tension applied to the magnetic tape in the longitudinal direction at this time is not particularly limited. It may be a constant value or may be variable, and may or may not follow the above description regarding the tension value during running. The tension applied to the magnetic tape in the longitudinal direction when it is subsequently wound onto the cartridge reel is the rewind tension. This tension is the tension applied to the magnetic tape in the longitudinal direction when the entire length of the magnetic tape is wound from the take-up reel onto the cartridge reel. Configuration 3 can be either of the following two configurations. In the first configuration (configuration 3-1), when the running for recording and / or reproducing data is completed, the portion of the magnetic tape wound around the cartridge reel is wound with tension in the longitudinal direction when it is wound around the cartridge reel. This tension during winding is the rewinding tension. In the second configuration (configuration 3-2), the configuration is a configuration other than configuration 3-1 of configuration 3. In configuration 3-1, in order to wind the entire length of the magnetic tape around the cartridge reel and accommodate it in the cartridge, the tension applied in the longitudinal direction of the magnetic tape when the magnetic tape that is not wound around the cartridge reel is wound around the cartridge reel is the rewinding tension. Configuration 3-2 is the same as configuration 2. That is, first, the magnetic tape is wound from the cartridge reel to the take-up reel. Then, the tension applied in the longitudinal direction of the magnetic tape when the entire length of the magnetic tape is wound from the take-up reel to the cartridge reel is the rewinding tension. In any of the above-mentioned forms 1, 2, and 3, the tension applied in the longitudinal direction of the magnetic tape when it is wound around the cartridge reel (rewinding tension) is preferably 0.30 N or less. The rewinding tension may be a constant value or may be changed. In one form, the rewinding tension may be a constant value of 0.30 N or less, or may be changed within a range of 0.30 N or less. When it is changed, the maximum value of the tension applied in the longitudinal direction of the magnetic tape when it is wound around the cartridge reel is preferably 0.30 N or less, and may be, for example, 0.25 N or less. The minimum value of the tension applied in the longitudinal direction of the magnetic tape when it is wound around the cartridge reel may be, for example, 0.10 N or more, 0.20 N or more, or more than 0.20 N, or may be less than the value exemplified here. The tension (rewinding tension) when it is wound around the cartridge reel can be controlled, for example, by a control device of the magnetic tape device. In addition, an operating program may be recorded in the cartridge memory so that the magnetic tape is wound onto the cartridge reel with the set rewinding tension applied in the longitudinal direction after recording and / or playback of data on the magnetic tape, and the control device may read this program to perform the winding operation.
[0037] [Magnetic tape] <Minimum load for occurrence of winding slippage> The magnetic tape contained in the magnetic tape cartridge has a minimum load for causing shearing of 250N or less, measured after being rewound on a cartridge reel with a tension of 0.30N in the longitudinal direction of the magnetic tape. The minimum load for causing shearing of 250N or less can contribute to enabling good recording and / or reproduction of data on the magnetic tape after storage. From this point of view, the minimum load for causing shearing of 200N or less is more preferable, 150N or less is even more preferable, and 100N or less is even more preferable. In addition, from the viewpoint of improving the winding stability of the magnetic tape when it is housed in a magnetic tape cartridge, the minimum load for causing shearing of 5N or more is more preferable, 10N or more is more preferable, 15N or more is even more preferable, and 20N or more is even more preferable.
[0038] In the present invention and this specification, the minimum load at which winding slippage occurs is determined by the following method in an environment with an atmospheric temperature of 23° C. and a relative humidity of 50%. The magnetic tape cartridge to be measured is an unused magnetic tape cartridge that is not installed in a magnetic tape device. The magnetic tape wound on the cartridge reel in the magnetic tape cartridge is temporarily taken out of the magnetic tape cartridge by winding it onto a temporary take-up reel. The magnetic tape is taken out by applying a tension of 0.30 N in the longitudinal direction. Thereafter, the magnetic tape temporarily wound on the take-up reel is rewound onto the cartridge reel with a tension of 0.30 N applied in the longitudinal direction of the magnetic tape, so that the entire length of the magnetic tape is wound again onto the cartridge reel and housed in the magnetic tape cartridge. The above winding and rewinding can be performed, for example, by using a magnetic tape device having the above-described tension adjusting mechanism. The temporary winding reel can be, for example, the take-up reel of the magnetic tape device. The tension applied in the longitudinal direction during winding and rewinding is, similar to the tension described above, a tension value used by the control device of the magnetic tape device to control the above-described tension adjusting mechanism as the tension to be applied in the longitudinal direction of the magnetic tape. Thereafter, the cartridge reel on which the entire length of the magnetic tape is wound is removed from the magnetic tape cartridge. The cartridge reel includes at least a reel hub, which is a cylindrical member constituting the axial center. The cartridge reel also usually has flanges (upper flange and lower flange) that extend radially outward from the upper and lower ends of the reel hub. For cartridge reels that have flanges, the flanges are removed by a known cutting means (such as an ultrasonic cutter) to expose both sides of the tape winding surface on which the magnetic tape is wound. The flanges are removed with care so that no vertical load is applied to the tape winding surface. The side closer to the reel hub is called the "inner side" and the side farther away is called the "outer side", with the inner end of the magnetic tape being called the "inner end" and the other end being called the "outer end". If a leader pin is attached to the outer end, the leader pin is removed and the outer end of the magnetic tape is fixed to the inner tape with adhesive tape to maintain the wound state. When the magnetic tape is pulled during fixing, it is pulled with a low tension (approximately 0.1 N or less in the longitudinal direction) that can remove the slack in the magnetic tape. After that, the reel hub is placed on the support stand. If the gear is integrally formed in the reel hub, the reel hub can be placed on the support stand so that it is supported by the gear surface. When placing it on the support stand, the reel hub is placed on the support stand so that the tape winding surface on the side on which the plate is placed and the load is applied as described below is vertically separated by 5 cm or more from the floor surface on which the support stand is placed. The tape winding surface on the side on which the load is applied may be either tape winding surface, and is selected at random. An aluminum ring with an outer diameter of 90 mm and an inner diameter of 80 mm is placed on the tape winding surface of the wound magnetic tape placed on the support stand so that the center of rotation of the reel hub and the center of the aluminum ring are aligned. The "alignment" here is not limited to a perfect alignment, and a deviation of 3 mm or less is permitted. An aluminum plate having a square shape of 100 mm x 100 mm in plan view and a thickness of 3 mm is placed on the aluminum ring. A load is applied from above the plate and maintained for 10 minutes, after which the load is removed. The load can be applied by a known method.For example, the load can be applied by placing a weight on the plate or by pressing the plate with a pressing device. The load is preferably applied so that a uniform load is applied to the entire surface of the plate. Here, "uniform" includes the presence of parts where the load is different within a range that can normally occur when applying a load by a known method. In addition, in the case of a concentrated load, the area on the plate to which the load is applied is a part or all of a circular area located above the center of the ring in a range of up to 25 mm in the radial direction. The vertical position of the upper surface of the plate before the load is applied is A, and the vertical position of the upper surface of the plate after the load is removed is B. If "AB ≥ 1 mm", it is determined that a winding slippage has occurred in the wound magnetic tape. The vertical position is measured at a position on the ring to avoid being affected by deformation of the plate. The measurement is performed at a total of six positions every 60° in the circumferential direction of the ring, and the arithmetic average of the values obtained at the six positions before the load is applied is A, and the arithmetic average of the values obtained at the six positions after the load is removed is B. The position for measuring A and the position for measuring B may be the same or different. For the same magnetic tape, the load is started from 5N and increased in increments of 5N while performing the above measurements, and the minimum load at which slippage occurs is defined as the "minimum load at which slippage occurs."
[0039] Regarding the control of the minimum load at which the magnetic tape is wound, the inventors have investigated the following trends. The thinner the magnetic tape is, the smaller the minimum load at which winding slippage occurs tends to be. Increasing the dispersibility of the ferromagnetic powder in the magnetic layer can contribute to reducing the value of the minimum load at which winding slippage occurs. This is presumably because the smoother the magnetic layer surface is, the less likely it is that winding tightness will occur. In magnetic tapes having a backcoat layer, increasing the dispersibility of the nonmagnetic powder in the backcoat layer can contribute to reducing the minimum load at which slippage occurs. This is presumably because increasing the surface smoothness of the backcoat layer can prevent the surface roughness of the backcoat layer from being transferred to the surface of the magnetic layer, thereby preventing the surface smoothness of the magnetic layer from being reduced. The above points will be described in detail later.
[0040] <Vertical squareness ratio> In one embodiment, the perpendicular squareness of the magnetic tape can be, for example, 0.55 or more, and is preferably 0.60 or more. It is preferable that the perpendicular squareness of the magnetic tape is 0.60 or more from the viewpoint of improving electromagnetic conversion characteristics. The upper limit of the squareness is, in principle, 1.00 or less. The perpendicular squareness of the magnetic tape can be 1.00 or less, and can be 0.95 or less, 0.90 or less, 0.85 or less, or 0.80 or less. It is preferable that the perpendicular squareness of the magnetic tape has a large value from the viewpoint of improving electromagnetic conversion characteristics. The perpendicular squareness of the magnetic tape can be controlled by a known method such as performing a perpendicular orientation process.
[0041] In the present invention and this specification, the "perpendicular squareness" refers to the squareness measured in the perpendicular direction of the magnetic tape. The "perpendicular direction" described in relation to the squareness is the direction perpendicular to the magnetic layer surface, and can also be called the thickness direction. In the present invention and this specification, the perpendicular squareness is determined by the following method. A sample piece of a size that can be introduced into a vibration sample magnetometer is cut out from the magnetic tape to be measured. A magnetic field is applied to this sample piece in a vertical direction (perpendicular to the magnetic layer surface) using a vibration sample magnetometer at a maximum applied magnetic field of 3979 kA / m, a measurement temperature of 296 K, and a magnetic field sweep speed of 8.3 kA / m / sec, and the magnetization strength of the sample piece against the applied magnetic field is measured. The measured value of the magnetization strength is obtained as a value after demagnetization field correction and a value obtained by subtracting the magnetization of the sample probe of the vibration sample magnetometer as background noise. When the magnetization strength at the maximum applied magnetic field is Ms and the magnetization strength at zero applied magnetic field is Mr, the squareness ratio SQ is a value calculated as SQ=Mr / Ms. The measurement temperature refers to the temperature of the sample piece, and by setting the ambient temperature around the sample piece to the measurement temperature, the temperature equilibrium is established and the temperature of the sample piece can be set to the measurement temperature.
[0042] The above magnetic tape will now be described in more detail.
[0043] <Magnetic layer> (Ferromagnetic powder) The magnetic tape may have a non-magnetic support and a magnetic layer containing ferromagnetic powder. As the ferromagnetic powder contained in the magnetic layer, one or more of known ferromagnetic powders used in the magnetic layers of various magnetic recording media may be used in combination. It is preferable to use ferromagnetic powders with a small average particle size from the viewpoint of improving recording density. From this viewpoint, the average particle size of the ferromagnetic powder is preferably 50 nm or less, more preferably 45 nm or less, even more preferably 40 nm or less, even more preferably 35 nm or less, even more preferably 30 nm or less, even more preferably 25 nm or less, and even more preferably 20 nm or less. On the other hand, from the viewpoint of magnetization stability, the average particle size of the ferromagnetic powder is preferably 5 nm or more, more preferably 8 nm or more, even more preferably 10 nm or more, even more preferably 15 nm or more, and even more preferably 20 nm or more.
[0044] Hexagonal Ferrite Powder A preferred specific example of the ferromagnetic powder is hexagonal ferrite powder. For details of the hexagonal ferrite powder, see, for example, JP2011-225417A, paragraphs 0012-0030, JP2011-216149A, paragraphs 0134-0136, JP2012-204726A, paragraphs 0013-0030, and JP2015-127985A, paragraphs 0029-0084.
[0045] In the present invention and this specification, the term "hexagonal ferrite powder" refers to a ferromagnetic powder in which a hexagonal ferrite type crystal structure is detected as the main phase by X-ray diffraction analysis. The main phase refers to a structure to which the most intense diffraction peak belongs in the X-ray diffraction spectrum obtained by X-ray diffraction analysis. For example, when the most intense diffraction peak in the X-ray diffraction spectrum obtained by X-ray diffraction analysis is assigned to a hexagonal ferrite type crystal structure, it is determined that the hexagonal ferrite type crystal structure has been detected as the main phase. When only a single structure is detected by X-ray diffraction analysis, the detected structure is regarded as the main phase. The hexagonal ferrite type crystal structure contains at least an iron atom, a divalent metal atom, and an oxygen atom as constituent atoms. The divalent metal atom is a metal atom that can become a divalent cation as an ion, and examples of such include alkaline earth metal atoms such as strontium atoms, barium atoms, and calcium atoms, and lead atoms. In the present invention and this specification, the hexagonal strontium ferrite powder refers to a powder in which the main divalent metal atom contained therein is a strontium atom, and the hexagonal barium ferrite powder refers to a powder in which the main divalent metal atom contained therein is a barium atom. The main divalent metal atom refers to the divalent metal atom that is the most abundant of the divalent metal atoms contained in the powder on an atomic % basis. However, the above divalent metal atoms do not include rare earth atoms. In the present invention and this specification, the "rare earth atom" is selected from the group consisting of scandium atoms (Sc), yttrium atoms (Y), and lanthanoid atoms. The lanthanide atom is selected from the group consisting of a lanthanum atom (La), a cerium atom (Ce), a praseodymium atom (Pr), a neodymium atom (Nd), a promethium atom (Pm), a samarium atom (Sm), a europium atom (Eu), a gadolinium atom (Gd), a terbium atom (Tb), a dysprosium atom (Dy), a holmium atom (Ho), an erbium atom (Er), a thulium atom (Tm), a ytterbium atom (Yb), and a lutetium atom (Lu).
[0046] Hereinafter, hexagonal strontium ferrite powder, which is one form of hexagonal ferrite powder, will be described in more detail.
[0047] The activation volume of the hexagonal strontium ferrite powder is preferably 800 to 1600 nm 3 The finely divided hexagonal strontium ferrite powder having an activation volume in the above range is suitable for producing a magnetic tape exhibiting excellent electromagnetic conversion characteristics. The activation volume of the hexagonal strontium ferrite powder is preferably 800 nm 3 For example, 850 nm or more. 3 From the viewpoint of further improving the electromagnetic conversion characteristics, the activation volume of the hexagonal strontium ferrite powder can be 1500 nm or more. 3 More preferably, it is 1400 nm or less. 3 More preferably, it is 1300 nm or less. 3 More preferably, it is 1200 nm or less. 3 More preferably, it is equal to or less than 1100 nm. 3 It is even more preferable that the activation volume of the hexagonal barium ferrite powder is equal to or less than 1000 nm. The same is true for the activation volume of the hexagonal barium ferrite powder.
[0048] "Activation volume" is a unit of magnetization reversal and is an index showing the magnetic size of a particle. The activation volume described in this invention and this specification and the anisotropy constant Ku described below are values obtained by measuring the coercive force Hc measurement section at magnetic field sweep speeds of 3 minutes and 30 minutes (measurement temperature: 23°C ± 1°C) using a vibrating sample magnetometer, and calculating from the following relationship between Hc and activation volume V. The unit of the anisotropy constant Ku is 1 erg / cc = 1.0 x 10 -1 J / m 3 It is. Hc=2Ku / Ms{1-[(kT / KuV)ln(At / 0.693)] 1 / 2} [In the above formula, Ku: anisotropy constant (unit: J / m 3 ), Ms: saturation magnetization (unit: kA / m), k: Boltzmann constant, T: absolute temperature (unit: K), V: activation volume (unit: cm 3), A: spin precession frequency (unit: s -1 ), t: magnetic field reversal time (unit: s)]
[0049] The anisotropy constant Ku can be used as an index of reduction in thermal fluctuation, in other words, improvement in thermal stability. The hexagonal strontium ferrite powder is preferably 1.8×10 5 J / m 3 More preferably, the Ku is 2.0×10 or more. 5 J / m 3 The Ku of the hexagonal strontium ferrite powder can be, for example, 2.5×10 5 J / m 3 However, since a higher Ku value means higher thermal stability and is preferable, the Ku value is not limited to the above-mentioned values.
[0050] The hexagonal strontium ferrite powder may or may not contain rare earth atoms. When the hexagonal strontium ferrite powder contains rare earth atoms, it is preferable that the rare earth atoms are contained at a content (bulk content) of 0.5 to 5.0 atomic % relative to 100 atomic % of iron atoms. In one embodiment, the hexagonal strontium ferrite powder containing rare earth atoms can have uneven distribution of rare earth atoms in the surface layer portion. In the present invention and this specification, the term "surface distribution of rare earth atoms" refers to the rare earth atom content relative to 100 atomic % of iron atoms in a solution obtained by partially dissolving a hexagonal strontium ferrite powder in an acid (hereinafter referred to as "surface content of rare earth atoms" or simply "surface content" for rare earth atoms), which is greater than the rare earth atom content relative to 100 atomic % of iron atoms in a solution obtained by completely dissolving a hexagonal strontium ferrite powder in an acid (hereinafter referred to as "bulk content of rare earth atoms" or simply "bulk content" for rare earth atoms), Rare earth atom surface content / rare earth atom bulk content>1.0 The rare earth atom content of the hexagonal strontium ferrite powder described later is synonymous with the rare earth atom bulk content. In contrast, partial dissolution using an acid dissolves the surface layer of the particles constituting the hexagonal strontium ferrite powder, so the rare earth atom content in the solution obtained by partial dissolution is the rare earth atom content in the surface layer of the particles constituting the hexagonal strontium ferrite powder. The rare earth atom surface layer content satisfying the ratio of "rare earth atom surface layer content / rare earth atom bulk content>1.0" means that the rare earth atoms are unevenly distributed (i.e., more present in the surface layer) in the particles constituting the hexagonal strontium ferrite powder. In the present invention and this specification, the surface layer refers to a portion of the region extending from the surface of the particles constituting the hexagonal strontium ferrite powder toward the inside.
[0051] When the hexagonal strontium ferrite powder contains rare earth atoms, the rare earth atom content (bulk content) is preferably in the range of 0.5 to 5.0 atomic % relative to 100 atomic % of iron atoms. It is considered that the rare earth atoms contained in the bulk content in the above range and the rare earth atoms unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder contribute to suppressing the decrease in the reproduction output during repeated reproduction. This is presumed to be because the hexagonal strontium ferrite powder contains rare earth atoms in the bulk content in the above range and the rare earth atoms unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder can increase the anisotropy constant Ku. The higher the value of the anisotropy constant Ku, the more the occurrence of a phenomenon called thermal fluctuation can be suppressed (in other words, the thermal stability can be improved). By suppressing the occurrence of thermal fluctuation, the decrease in the reproduction output during repeated reproduction can be suppressed. It is speculated that the uneven distribution of rare earth atoms in the surface layer of hexagonal strontium ferrite powder particles contributes to stabilizing the spin of the iron (Fe) sites in the crystal lattice of the surface layer, thereby increasing the anisotropy constant Ku. In addition, it is presumed that using the hexagonal strontium ferrite powder having rare earth atom uneven distribution on the surface as the ferromagnetic powder of the magnetic layer also contributes to suppressing the wear of the magnetic layer surface due to sliding with the magnetic head. That is, it is presumed that the hexagonal strontium ferrite powder having rare earth atom uneven distribution on the surface can also contribute to improving the running durability of the magnetic tape. This is presumed to be because the uneven distribution of rare earth atoms on the surface of the particles constituting the hexagonal strontium ferrite powder contributes to improving the interaction between the particle surface and the organic substance (e.g., binder and / or additive) contained in the magnetic layer, and as a result, the strength of the magnetic layer is improved. From the viewpoint of suppressing a decrease in the reproduction output during repeated reproduction and / or from the viewpoint of further improving running durability, the rare earth atom content (bulk content) is more preferably in the range of 0.5 to 4.5 atomic %, even more preferably in the range of 1.0 to 4.5 atomic %, and even more preferably in the range of 1.5 to 4.5 atomic %.
[0052] The bulk content is the content obtained by completely dissolving the hexagonal strontium ferrite powder. In the present invention and this specification, unless otherwise specified, the content of an atom refers to the bulk content obtained by completely dissolving the hexagonal strontium ferrite powder. The hexagonal strontium ferrite powder containing rare earth atoms may contain only one rare earth atom as a rare earth atom, or may contain two or more rare earth atoms. When two or more rare earth atoms are contained, the bulk content is obtained for the total of two or more rare earth atoms. This point is the same for other components in the present invention and this specification. That is, unless otherwise specified, a certain component may be used in only one type, or in two or more types. When two or more types are used, the content or content refers to the total of two or more types.
[0053] When the hexagonal strontium ferrite powder contains rare earth atoms, the rare earth atoms contained therein may be any one or more of rare earth atoms. From the viewpoint of suppressing the decrease in the reproduction output during repeated reproduction, preferred rare earth atoms include neodymium atoms, samarium atoms, yttrium atoms and dysprosium atoms, more preferred are neodymium atoms, samarium atoms and yttrium atoms, and further preferred are neodymium atoms.
[0054] In the hexagonal strontium ferrite powder having rare earth atom uneven distribution in the surface layer, the rare earth atoms may be unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder, and the degree of uneven distribution is not limited. For example, for the hexagonal strontium ferrite powder having rare earth atom uneven distribution in the surface layer, the ratio of the surface content of rare earth atoms obtained by partial dissolution under the dissolution conditions described below to the bulk content of rare earth atoms obtained by complete dissolution under the dissolution conditions described below, "surface content / bulk content", is more than 1.0 and can be 1.5 or more. The "surface content / bulk content" being greater than 1.0 means that the rare earth atoms are unevenly distributed in the surface layer (i.e., more than in the interior) in the particles constituting the hexagonal strontium ferrite powder. In addition, the ratio of the surface layer content of rare earth atoms obtained by partial dissolution under the dissolution conditions described later to the bulk content of rare earth atoms obtained by total dissolution under the dissolution conditions described later, "surface layer content / bulk content", can be, for example, 10.0 or less, 9.0 or less, 8.0 or less, 7.0 or less, 6.0 or less, 5.0 or less, or 4.0 or less. However, in a hexagonal strontium ferrite powder having rare earth atom surface layer uneven distribution, it is sufficient that the rare earth atoms are unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder, and the above "surface layer content / bulk content" is not limited to the upper or lower limit exemplified.
[0055] The partial and total dissolution of hexagonal strontium ferrite powder will be described below. For hexagonal strontium ferrite powder present as powder, the sample powders to be partially and completely dissolved are taken from the same lot of powder. On the other hand, for hexagonal strontium ferrite powder contained in the magnetic layer of a magnetic tape, a part of the hexagonal strontium ferrite powder taken out from the magnetic layer is subjected to partial dissolution, and the other part is subjected to total dissolution. The hexagonal strontium ferrite powder can be taken out from the magnetic layer by, for example, the method described in paragraph 0032 of JP 2015-91747 A. The above-mentioned partial dissolution means that the hexagonal strontium ferrite powder is dissolved to such an extent that the remaining powder can be visually confirmed in the liquid at the end of dissolution. For example, the partial dissolution can dissolve a region of 10 to 20 mass% of the particles constituting the hexagonal strontium ferrite powder, with the whole particles being 100 mass%. On the other hand, the above-mentioned complete dissolution means that the hexagonal strontium ferrite powder is dissolved to such an extent that the remaining powder cannot be visually confirmed in the liquid at the end of dissolution. The partial dissolution and the surface layer content are measured, for example, by the following method. Note that the dissolution conditions such as the amount of sample powder are merely examples, and any dissolution conditions that allow partial or complete dissolution can be used. A container (e.g., a beaker) containing 12 mg of sample powder and 10 mL of 1 mol / L hydrochloric acid is placed on a hot plate set at 70°C for 1 hour. The resulting solution is filtered through a 0.1 μm membrane filter. Elemental analysis of the filtrate thus obtained is performed using an inductively coupled plasma (ICP) analyzer. In this way, the surface layer content of rare earth atoms relative to 100 atomic % of iron atoms can be determined. When multiple types of rare earth atoms are detected by elemental analysis, the total content of all rare earth atoms is taken as the surface layer content. This is also true for the measurement of bulk content. On the other hand, the total dissolved and bulk contents are measured, for example, by the following method. A container (e.g., a beaker) containing 12 mg of sample powder and 10 mL of 4 mol / L hydrochloric acid is placed on a hot plate set at 80° C. for 3 hours. After that, the bulk content relative to 100 atomic % of iron atoms can be calculated by carrying out the same procedure as the partial dissolution and surface layer content measurement described above.
[0056] From the viewpoint of increasing the reproduction output when reproducing data recorded on a magnetic tape, it is desirable for the mass magnetization σs of the ferromagnetic powder contained in the magnetic tape to be high. In this regard, hexagonal strontium ferrite powder that contains rare earth atoms but does not have uneven distribution of rare earth atoms in the surface layer has a tendency to have a significantly lower σs than hexagonal strontium ferrite powder that does not contain rare earth atoms. In contrast, hexagonal strontium ferrite powder that has uneven distribution of rare earth atoms in the surface layer is considered to be preferable in terms of suppressing such a large decrease in σs. In one embodiment, the σs of the hexagonal strontium ferrite powder is 45 A·m 2 / kg or more, and 47A·m 2 / kg or more. On the other hand, from the viewpoint of noise reduction, σs is 80A·m 2 / kg or less, and 60A·m 2 / kg or less. σs can be measured using a known measuring device capable of measuring magnetic properties, such as a vibrating sample magnetometer. In the present invention and this specification, unless otherwise specified, the mass magnetization σs is a value measured at a magnetic field strength of 15 kOe. 1 [kOe]=10 6 / 4π[A / m].
[0057] Regarding the content (bulk content) of the constituent atoms of the hexagonal strontium ferrite powder, the strontium atom content can be, for example, in the range of 2.0 to 15.0 atomic % relative to 100 atomic % of iron atoms. In one embodiment, the divalent metal atoms contained in the hexagonal strontium ferrite powder can be only strontium atoms. In another embodiment, the hexagonal strontium ferrite powder can also contain one or more other divalent metal atoms in addition to strontium atoms. For example, it can contain barium atoms and / or calcium atoms. When divalent metal atoms other than strontium atoms are contained, the barium atom content and calcium atom content in the hexagonal strontium ferrite powder can each be, for example, in the range of 0.05 to 5.0 atomic % relative to 100 atomic % of iron atoms.
[0058] Known crystal structures of hexagonal ferrite include magnetoplumbite type (also called "M type"), W type, Y type, and Z type. The hexagonal strontium ferrite powder may have any of the crystal structures. The crystal structure can be confirmed by X-ray diffraction analysis. The hexagonal strontium ferrite powder may be one in which a single crystal structure or two or more types of crystal structures are detected by X-ray diffraction analysis. For example, in one embodiment, the hexagonal strontium ferrite powder may be one in which only the M-type crystal structure is detected by X-ray diffraction analysis. For example, M-type hexagonal ferrite is AFe 12 O 19Here, A represents a divalent metal atom, and when the hexagonal strontium ferrite powder is of the M type, A is only a strontium atom (Sr), or when A contains a plurality of divalent metal atoms, the strontium atom (Sr) accounts for the largest proportion on an atomic % basis as described above. The divalent metal atom content of the hexagonal strontium ferrite powder is usually determined by the type of crystal structure of the hexagonal ferrite, and is not particularly limited. The same applies to the iron atom content and the oxygen atom content. The hexagonal strontium ferrite powder contains at least an iron atom, a strontium atom, and an oxygen atom, and may further contain a rare earth atom. Furthermore, the hexagonal strontium ferrite powder may or may not contain atoms other than these atoms. As an example, the hexagonal strontium ferrite powder may contain an aluminum atom (Al). The content of aluminum atoms can be, for example, 0.5 to 10.0 atomic % relative to 100 atomic % of iron atoms. From the viewpoint of suppressing the decrease in the reproduction output during repeated reproduction, the hexagonal strontium ferrite powder contains iron atoms, strontium atoms, oxygen atoms, and rare earth atoms, and the content of atoms other than these atoms is preferably 10.0 atomic % or less relative to 100 atomic % of iron atoms, more preferably in the range of 0 to 5.0 atomic %, and may be 0 atomic %. That is, in one embodiment, the hexagonal strontium ferrite powder may not contain atoms other than iron atoms, strontium atoms, oxygen atoms, and rare earth atoms. The content expressed in atomic % above is obtained by converting the content (unit: mass %) of each atom obtained by completely dissolving the hexagonal strontium ferrite powder into a value expressed in atomic % using the atomic weight of each atom. In addition, in the present invention and this specification, "not containing" a certain atom means that the content measured by an ICP analyzer after completely dissolving is 0 mass %. The detection limit of an ICP analyzer is usually 0.01 ppm (parts per million) or less on a mass basis. The above term "free" is used to mean that the content is below the detection limit of the ICP analyzer.In one form, the hexagonal strontium ferrite powder can be one that does not contain bismuth atoms (Bi).
[0059] metal powder A specific preferred example of the ferromagnetic powder is a ferromagnetic metal powder. For details of the ferromagnetic metal powder, reference can be made to, for example, paragraphs 0137 to 0141 of JP 2011-216149 A and paragraphs 0009 to 0023 of JP 2005-251351 A.
[0060] ε-iron oxide powder A preferred specific example of the ferromagnetic powder is ε-iron oxide powder. In the present invention and this specification, the term "ε-iron oxide powder" refers to a ferromagnetic powder in which an ε-iron oxide type crystal structure is detected as the main phase by X-ray diffraction analysis. For example, when the highest intensity diffraction peak in the X-ray diffraction spectrum obtained by X-ray diffraction analysis is attributed to an ε-iron oxide type crystal structure, it is determined that the ε-iron oxide type crystal structure is detected as the main phase. Known methods for producing ε-iron oxide powder include a method of producing it from goethite and a reverse micelle method. All of the above production methods are publicly known. In addition, for a method for producing ε-iron oxide powder in which a part of Fe is replaced by a substitution atom such as Ga, Co, Ti, Al, or Rh, reference can be made to, for example, J. Jpn. Soc. Powder Metallurgy Vol. 61 Supplement, No. S1, pp. S280-S284, J. Mater. Chem. C, 2013, 1, pp.5200-5206, etc. However, the method for producing the ε-iron oxide powder that can be used as the ferromagnetic powder in the magnetic layer of the magnetic tape is not limited to the method given here.
[0061] The activation volume of the ε-iron oxide powder is preferably 300 to 1500 nm 3 The finely divided ε-iron oxide powder exhibiting an activation volume in the above range is suitable for producing a magnetic tape exhibiting excellent electromagnetic conversion characteristics. The activation volume of the ε-iron oxide powder is preferably 300 nm 3For example, 500 nm or more. 3 From the viewpoint of further improving the electromagnetic conversion characteristics, the activation volume of the ε-iron oxide powder can be 1400 nm or more. 3 More preferably, it is 1300 nm or less. 3 More preferably, it is 1200 nm or less. 3 More preferably, it is equal to or less than 1100 nm. 3 It is even more preferred that:
[0062] The anisotropy constant Ku can be used as an index of the reduction in thermal fluctuation, in other words, the improvement in thermal stability. The ε-iron oxide powder is preferably 3.0×10 4 J / m 3 More preferably, the Ku is 8.0×10 or more. 4 J / m 3 The Ku of the ε-iron oxide powder can be, for example, 3.0×10 5 J / m 3 However, since a higher Ku value means higher thermal stability and is preferable, the Ku value is not limited to the above-mentioned values.
[0063] From the viewpoint of increasing the reproduction output when reproducing data recorded on a magnetic tape, it is desirable that the mass magnetization σs of the ferromagnetic powder contained in the magnetic tape is high. In this regard, in one embodiment, the σs of the ε-iron oxide powder is 8 A m 2 / kg or more, and 12 A m 2 On the other hand, the σs of ε-iron oxide powder is 40 A m 2 / kg or less, and 35A·m 2 It is more preferable that the amount is not more than 1 / kg.
[0064] In the present invention and this specification, unless otherwise specified, the average particle size of various powders such as ferromagnetic powders is a value measured by the following method using a transmission electron microscope. The powder is photographed at a magnification of 100,000 times using a transmission electron microscope, and a photograph of the particles that make up the powder is obtained by printing it on photographic paper or displaying it on a display so that the total magnification is 500,000 times. From the obtained particle photograph, the target particle is selected, and the particle outline is traced with a digitizer to measure the particle (primary particle) size. Primary particles are independent particles that are not aggregated. The above measurements are carried out for 500 randomly selected particles. The arithmetic mean of the particle sizes of the 500 particles thus obtained is the average particle size of the powder. As the transmission electron microscope, for example, a Hitachi transmission electron microscope H-9000 type can be used. The particle size can be measured using known image analysis software, for example, Carl Zeiss image analysis software KS-400. The average particle size shown in the examples described below is a value measured using a Hitachi transmission electron microscope H-9000 type as the transmission electron microscope and Carl Zeiss image analysis software KS-400 as the image analysis software, unless otherwise specified. In the present invention and this specification, powder means a collection of multiple particles. For example, ferromagnetic powder means a collection of multiple ferromagnetic particles. In addition, the collection of multiple particles is not limited to a form in which the particles constituting the collection are in direct contact with each other, and also includes a form in which a binder, additive, etc., described later, are interposed between the particles. The term particle is sometimes used to refer to powder.
[0065] As a method for collecting sample powder from the magnetic tape for particle size measurement, for example, the method described in paragraph 0015 of JP 2011-048878 A can be used.
[0066] In the present invention and this specification, unless otherwise specified, the size of the particles constituting the powder (particle size) is determined by the shape of the particles observed in the particle photograph. (1) In the case of needle-shaped, spindle-shaped, columnar (where the height is greater than the maximum major axis of the base), etc., it is expressed by the length of the major axis that constitutes the particle, i.e., the major axis length. (2) In the case of a plate or columnar shape (where the thickness or height is smaller than the maximum long diameter of the plate or base), it shall be expressed by the maximum long diameter of the plate or base. (3) In the case of a particle having a spherical, polyhedral, or amorphous shape, and in which the major axis of the particle cannot be identified from its shape, the particle is expressed as the equivalent circle diameter, which is determined by the circle projection method.
[0067] The average acicular ratio of a powder refers to the arithmetic average of the short axis length of the particles, i.e., the short axis length, the (long axis length / short axis length) value of each particle, and the values obtained for the 500 particles. Here, unless otherwise specified, the short axis length refers to the length of the short axis constituting the particle in the above definition of particle size (1), and to the thickness or height in the above definition of particle size (2), and in the above definition of particle size (3), since there is no distinction between the long axis and the short axis, (long axis length / short axis length) is considered to be 1 for the sake of convenience. Unless otherwise specified, when the particle shape is specific, for example, in the case of the above definition of particle size (1), the average particle size is the average major axis length, in the case of definition (2), the average particle size is the average plate diameter, and in the case of definition (3), the average particle size is the average diameter (also called the average particle diameter or average particle size).
[0068] The content (filling rate) of the ferromagnetic powder in the magnetic layer is preferably in the range of 50 to 90 mass % and more preferably in the range of 60 to 90 mass % relative to the total mass of the magnetic layer. A high filling rate of the ferromagnetic powder in the magnetic layer is preferable from the viewpoint of improving recording density.
[0069] (Binding Agent) The magnetic tape may be a coated magnetic tape, and may contain a binder in the magnetic layer. The binder is one or more kinds of resin. As the binder, various resins that are usually used as binders for coated magnetic recording media may be used. For example, as the binder, a resin selected from polyurethane resin, polyester resin, polyamide resin, vinyl chloride resin, acrylic resin copolymerized with styrene, acrylonitrile, methyl methacrylate, etc., cellulose resin such as nitrocellulose, epoxy resin, phenoxy resin, polyvinyl acetal, polyvinyl butyral, etc. may be used alone or in combination. Among these, polyurethane resin, acrylic resin, cellulose resin, and vinyl chloride resin are preferred. These resins may be homopolymers or copolymers. These resins may also be used as binders in the non-magnetic layer and / or backcoat layer described below. For the above binders, reference can be made to paragraphs 0028 to 0031 of JP 2010-24113 A. The average molecular weight of the resin used as the binder can be, for example, 10,000 to 200,000 in weight average molecular weight. The binder can be used in an amount of, for example, 1.0 to 30.0 parts by mass relative to 100.0 parts by mass of the ferromagnetic powder.
[0070] (hardening agent) A curing agent can be used together with the resin usable as a binder. In one embodiment, the curing agent can be a thermosetting compound, which is a compound in which a curing reaction (crosslinking reaction) proceeds by heating, and in another embodiment, the curing agent can be a photocuring compound in which a curing reaction (crosslinking reaction) proceeds by light irradiation. As the curing reaction proceeds in the magnetic layer forming process, at least a part of the curing agent can be contained in the magnetic layer in a state of reacting (crosslinking) with other components such as the binder. This point is also true for layers formed using a composition used to form other layers that contains a curing agent. A preferred curing agent is a thermosetting compound, and polyisocyanate is suitable. For details on polyisocyanate, refer to paragraphs 0124 to 0125 of JP 2011-216149 A. The curing agent can be used in an amount of, for example, 0 to 80.0 parts by mass relative to 100.0 parts by mass of the binder, and preferably 50.0 to 80.0 parts by mass from the viewpoint of improving the strength of the magnetic layer.
[0071] (Additives) The magnetic layer may contain one or more additives as necessary. An example of the additive is the curing agent described above. Examples of additives contained in the magnetic layer include non-magnetic powders (e.g., inorganic powders, carbon black, etc.), lubricants, dispersants, dispersion aids, antifungal agents, antistatic agents, antioxidants, etc. For example, reference can be made to paragraphs 0030 to 0033, 0035, and 0036 of JP2016-126817A for lubricants. The non-magnetic layer described below may contain a lubricant. Reference can be made to paragraphs 0030, 0031, 0034 to 0036 of JP2016-126817A for lubricants that may be contained in the non-magnetic layer. Reference can be made to paragraphs 0061 and 0071 of JP2012-133837A for dispersants. Compounds having polyalkyleneimine chains and vinyl polymer chains can act as dispersants to improve the dispersibility of ferromagnetic powders. Furthermore, the above compound may also contribute to improving the strength of the magnetic layer. Increasing the strength of the magnetic layer may suppress the occurrence of back-transmission, which will be described later, and increase the surface smoothness of the magnetic layer. For compounds having polyalkyleneimine chains and vinyl polymer chains, refer to paragraphs 0024 to 0064 of JP 2019-169225 A and the Examples of the same publication. The above compound is preferably contained in the magnetic layer in an amount of 18.0 parts by mass or more, more preferably 20.0 parts by mass or more, per 100.0 parts by mass of ferromagnetic powder. In addition, the content of the above compound in the magnetic layer is preferably 35.0 parts by mass or less, more preferably 30.0 parts by mass or less, per 100.0 parts by mass of ferromagnetic powder. In addition, one or more dispersants such as the above compounds may be added to the nonmagnetic layer forming composition. For dispersants that can be added to the nonmagnetic layer forming composition, refer to paragraph 0061 of JP 2012-133837 A. In addition, examples of non-magnetic powders that can be contained in the magnetic layer include non-magnetic powders that can function as abrasives, and non-magnetic powders (e.g., non-magnetic colloidal particles) that can function as protrusion-forming agents that form protrusions that protrude appropriately on the magnetic layer surface.The average particle size of colloidal silica (silica colloid particles) shown in the examples described later is a value obtained by the method described in paragraph 0015 of JP-A-2011-048878 as a method for measuring the average particle size. The additives can be appropriately selected from commercially available products according to the desired properties, or can be manufactured by known methods and used in any amount. Examples of additives that can be used to improve the dispersibility of an abrasive in a magnetic layer containing an abrasive include dispersants described in paragraphs 0012 to 0022 of JP-A-2013-131285.
[0072] The magnetic layer described above can be provided directly on the surface of the non-magnetic support, or indirectly via a non-magnetic layer.
[0073] <Nonmagnetic layer> Next, the non-magnetic layer will be described. The magnetic tape may have a magnetic layer directly on the surface of the non-magnetic support, or may have a magnetic layer on the surface of the non-magnetic support via a non-magnetic layer containing non-magnetic powder. The non-magnetic powder used in the non-magnetic layer may be an inorganic powder or an organic powder. Carbon black or the like may also be used. Examples of inorganic powder include powders of metals, metal oxides, metal carbonates, metal sulfates, metal nitrides, metal carbides, metal sulfides, and the like. These non-magnetic powders are commercially available, and can also be produced by known methods. For details, refer to paragraphs 0146 to 0150 of JP-A-2011-216149. For carbon black usable in the non-magnetic layer, refer to paragraphs 0040 and 0041 of JP-A-2010-24113. The content (filling rate) of the non-magnetic powder in the non-magnetic layer is preferably in the range of 50 to 90% by mass, more preferably in the range of 60 to 90% by mass, based on the total mass of the non-magnetic layer.
[0074] The non-magnetic layer may contain a binder and may also contain an additive. For other details of the binder, additive, etc. of the non-magnetic layer, known techniques related to non-magnetic layers can be applied. In addition, for example, for the type and content of the binder, the type and content of the additive, known techniques related to magnetic layers can also be applied.
[0075] In the present invention and this specification, the nonmagnetic layer also includes a substantially nonmagnetic layer that contains a small amount of ferromagnetic powder, for example as an impurity or intentionally, together with the nonmagnetic powder. Here, the substantially nonmagnetic layer refers to a layer having a residual magnetic flux density of 10 mT or less, a coercive force of 7.96 kA / m (100 Oe) or less, or a layer having a residual magnetic flux density of 10 mT or less and a coercive force of 7.96 kA / m (100 Oe) or less. It is preferable that the nonmagnetic layer has no residual magnetic flux density or coercive force.
[0076] <Backcoat layer> In one embodiment, the magnetic tape may have a backcoat layer containing a nonmagnetic powder on the surface side opposite to the surface side having the magnetic layer of the nonmagnetic support. In another embodiment, the magnetic tape may be a magnetic tape without a backcoat layer. When the magnetic tape has a backcoat layer, the following description can be referred to for the nonmagnetic powder of the backcoat layer. The backcoat layer may contain a binder and may also contain one or more additives. For the binder and various additives that may be contained in the backcoat layer, known techniques related to the backcoat layer can be applied, and known techniques related to the formulation of the magnetic layer and / or nonmagnetic layer can also be applied. For example, the description in paragraphs 0018 to 0020 of JP 2006-331625 A and in column 4, line 65 to column 5, line 38 of the specification of U.S. Pat. No. 7,029,774 can be referred to for the backcoat layer.
[0077] In the manufacturing process of a magnetic tape, when the magnetic layer surface and the back surface are in contact with each other in a rolled state, the surface shape of the back surface is transferred to the magnetic layer surface (so-called "show-through"), which may form a recess on the magnetic layer surface. Inhibiting the formation of such recesses and increasing the surface smoothness of the magnetic layer can contribute to reducing the value of the minimum load at which the winding slippage occurs. The back surface is the back coat layer surface when a back coat layer is present, and is the support surface when no back coat layer is present. One example of a means for inhibiting the formation of recesses on the magnetic layer surface is, for example, the selection of the type of component to be added to the composition for forming the back coat layer in order to adjust the surface shape of the back surface. From this point of view, it is preferable to use carbon black and a non-magnetic powder other than carbon black in combination, or to use carbon black (i.e., the non-magnetic powder of the back coat layer is made of carbon black). Examples of non-magnetic powders other than carbon black include the non-magnetic powders exemplified above as those that can be contained in the non-magnetic layer. For the non-magnetic powder in the backcoat layer, the proportion of carbon black in 100.0 parts by mass of the total amount of non-magnetic powder is preferably in the range of 50.0 to 100.0 parts by mass, more preferably in the range of 70.0 to 100.0 parts by mass, and even more preferably in the range of 90.0 to 100.0 parts by mass. It is also preferable that the total amount of non-magnetic powder in the backcoat layer is carbon black. The content (filling rate) of non-magnetic powder in the backcoat layer is preferably in the range of 50 to 90% by mass, more preferably in the range of 60 to 90% by mass, relative to the total mass of the backcoat layer.
[0078] In order to suppress the occurrence of the above-mentioned show-through, the composition for forming the backcoat layer preferably contains a component (dispersant) capable of increasing the dispersibility of the non-magnetic powder contained in the composition. An example of such a dispersant is a compound having an ammonium salt structure of an alkyl ester anion represented by the following formula 1. The compound having an ammonium salt structure of an alkyl ester anion represented by the following formula 1 can contribute to improving the dispersibility of carbon black. The "alkyl ester anion" can also be called an "alkyl carboxylate anion".
[0079] [ka]
[0080] In formula 1, R represents an alkyl group having 7 or more carbon atoms or a fluorinated alkyl group having 7 or more carbon atoms; Z + represents an ammonium cation.
[0081] In one embodiment, two or more components capable of forming the compound having the above-mentioned salt structure can be used when preparing the composition for forming a backcoat layer, whereby at least a part of the components can form the compound having the above-mentioned salt structure when preparing the composition for forming a backcoat layer.
[0082] Unless otherwise specified, the groups described below may have a substituent or may be unsubstituted. In addition, the "carbon number" of a group having a substituent means the carbon number not including the carbon number of the substituent, unless otherwise specified. In the present invention and this specification, examples of the substituent include an alkyl group (e.g., an alkyl group having 1 to 6 carbon atoms), a hydroxyl group, an alkoxy group (e.g., an alkoxy group having 1 to 6 carbon atoms), a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, etc.), a cyano group, an amino group, a nitro group, an acyl group, a carboxy group, a salt of a carboxy group, a sulfonic acid group, a salt of a sulfonic acid group, etc.
[0083] Formula 1 will now be described in more detail.
[0084] In formula 1, R represents an alkyl group having 7 or more carbon atoms or a fluorinated alkyl group having 7 or more carbon atoms. The fluorinated alkyl group has a structure in which some or all of the hydrogen atoms constituting the alkyl group are substituted with fluorine atoms. The alkyl group or fluorinated alkyl group represented by R may have a straight-chain structure, may have a branched structure, or may be a cyclic alkyl group or fluorinated alkyl group, and is preferably a straight-chain structure. The alkyl group or fluorinated alkyl group represented by R may have a substituent or may be unsubstituted, and is preferably unsubstituted. The alkyl group represented by R is, for example, C n H 2n+1 Here, n is an integer of 7 or more. The fluorinated alkyl group represented by R can be, for example, C n H 2n+1 The alkyl group or fluorinated alkyl group represented by R may have a structure in which some or all of the hydrogen atoms constituting the alkyl group represented by - are substituted with fluorine atoms. The number of carbon atoms in the alkyl group or fluorinated alkyl group represented by R is 7 or more, preferably 8 or more, more preferably 9 or more, even more preferably 10 or more, still more preferably 11 or more, even more preferably 12 or more, and even more preferably 13 or more. The number of carbon atoms in the alkyl group or fluorinated alkyl group represented by R is preferably 20 or less, more preferably 19 or less, and even more preferably 18 or less.
[0085] In equation 1, Z + represents an ammonium cation. More specifically, the ammonium cation has the following structure: In the present invention and this specification, "*" in a formula representing a part of a compound represents the bonding position between the part of the structure and the adjacent atom.
[0086] [ka]
[0087] Nitrogen cation N of ammonium cation + and the oxygen anion O in Eq.- and form a salt bridging group to form an ammonium salt structure of an alkyl ester anion represented by formula 1. The inclusion of a compound having an ammonium salt structure of an alkyl ester anion represented by formula 1 in the backcoat layer can be confirmed by analyzing the magnetic tape using X-ray photoelectron spectroscopy (ESCA; Electron Spectroscopy for Chemical Analysis), infrared spectroscopy (IR; infrared spectroscopy), etc.
[0088] In one form, Z + The ammonium cation represented by the formula (I) can be obtained, for example, by the nitrogen atom of a nitrogen-containing polymer becoming a cation. The nitrogen-containing polymer means a polymer containing a nitrogen atom. In the present invention and this specification, the terms "polymer" and "polymeric polymer" are used to include homopolymers and copolymers. In one form, the nitrogen atom can be included as an atom constituting the main chain of the polymer, and in another form, the nitrogen atom can be included as an atom constituting the side chain of the polymer.
[0089] One example of the nitrogen-containing polymer is polyalkyleneimine, which is a ring-opening polymer of alkyleneimine and has a plurality of repeating units represented by the following formula 2.
[0090] [ka]
[0091] The nitrogen atom N constituting the main chain in formula 2 is a nitrogen cation N + So, Z in Eq. + This can result in an ammonium cation represented by the formula: and can form an ammonium salt structure with an alkyl ester anion, for example as follows:
[0092] [ka]
[0093] Formula 2 will now be described in more detail.
[0094] In formula 2, R 1 and R 2 each independently represents a hydrogen atom or an alkyl group, and n1 represents an integer of 2 or greater.
[0095] R 1 or R 2 Examples of the alkyl group represented by the formula (I) include alkyl groups having 1 to 6 carbon atoms, preferably alkyl groups having 1 to 3 carbon atoms, more preferably a methyl group or an ethyl group, and even more preferably a methyl group. 1 or R 2 The alkyl group represented by the formula (2) is preferably an unsubstituted alkyl group. 1 and R 2 The combination of includes a form in which one is a hydrogen atom and the other is an alkyl group, a form in which both are hydrogen atoms, and a form in which both are alkyl groups (same or different alkyl groups), and preferably a form in which both are hydrogen atoms. As an alkyleneimine that results in a polyalkyleneimine, the structure with the smallest number of carbon atoms constituting the ring is ethyleneimine, and the number of carbon atoms in the main chain of the alkyleneimine (ethyleneimine) obtained by ring-opening of ethyleneimine is 2. Therefore, n1 in formula 2 is 2 or more. n1 in formula 2 can be, for example, 10 or less, 8 or less, 6 or less, or 4 or less. The polyalkyleneimine may be a homopolymer containing only the same structure as the repeating structure represented by formula 2, or a copolymer containing two or more different structures as the repeating structure represented by formula 2. The number average molecular weight of the polyalkyleneimine that can be used to form a compound having an ammonium salt structure of an alkyl ester anion represented by formula 1 can be, for example, 200 or more, preferably 300 or more, and more preferably 400 or more. The number average molecular weight of the polyalkyleneimine can be, for example, 10,000 or less, preferably 5,000 or less, and more preferably 2,000 or less.
[0096] In the present invention and this specification, the average molecular weight (weight average molecular weight and number average molecular weight) refers to a value measured by gel permeation chromatography (GPC) and calculated in terms of standard polystyrene. The average molecular weight shown in the examples described later is a value (polystyrene-equivalent value) calculated in terms of standard polystyrene from a value measured by GPC under the following measurement conditions, unless otherwise specified. GPC equipment: HLC-8220 (Tosoh Corporation) Guard column: TSKguardcolumn Super HZM-H Columns: TSKgel Super HZ 2000, TSKgel Super HZ 4000, TSKgel Super HZ-M (Tosoh Corporation, 4.6 mm (inner diameter) x 15.0 cm, three columns connected in series) Eluent: Tetrahydrofuran (THF), containing stabilizer (2,6-di-t-butyl-4-methylphenol) Eluent flow rate: 0.35mL / min Column temperature: 40℃ Inlet temperature: 40℃ Refractive Index (RI) measurement temperature: 40℃ Sample concentration: 0.3% by mass Sample injection volume: 10 μL
[0097] Another example of the nitrogen-containing polymer is polyallylamine, which is a polymer of allylamine and has a plurality of repeating units represented by the following formula 3.
[0098] [ka]
[0099] The nitrogen atom N constituting the amino group in the side chain in formula 3 is a nitrogen cation N + So, Z in Eq. +This can result in an ammonium cation represented by the formula: and can form an ammonium salt structure with an alkyl ester anion, for example as follows:
[0100] [ka]
[0101] The weight-average molecular weight of the polyallylamine usable for forming the compound having an ammonium salt structure of an alkyl ester anion represented by formula 1 can be, for example, 200 or more, preferably 1,000 or more, and more preferably 1,500 or more. The weight-average molecular weight of the polyalkyleneimine can be, for example, 15,000 or less, preferably 10,000 or less, and more preferably 8,000 or less.
[0102] The fact that the backcoat layer contains a compound having a structure derived from polyalkyleneimine or polyallylimine as a compound having an ammonium salt structure of an alkyl ester anion represented by formula 1 can be confirmed by analyzing the surface of the backcoat layer using time-of-flight secondary ion mass spectrometry (TOF-SIMS) or the like.
[0103] The compound having an ammonium salt structure of an alkyl ester anion represented by formula 1 can be a salt of a nitrogen-containing polymer and one or more fatty acids selected from the group consisting of fatty acids having 7 or more carbon atoms and fluorinated fatty acids having 7 or more carbon atoms. The nitrogen-containing polymer forming the salt can be one or more nitrogen-containing polymers, for example, a nitrogen-containing polymer selected from the group consisting of polyalkyleneimine and polyallylamine. The fatty acids forming the salt can be one or more fatty acids selected from the group consisting of fatty acids having 7 or more carbon atoms and fluorinated fatty acids having 7 or more carbon atoms. The fluorinated fatty acid has a structure in which some or all of the hydrogen atoms constituting the alkyl group bonded to the carboxy group COOH in the fatty acid are replaced with fluorine atoms. For example, the salt-forming reaction can easily proceed by mixing the nitrogen-containing polymer and the above-mentioned fatty acids at room temperature. The room temperature is, for example, about 20 to 25°C. In one embodiment, one or more nitrogen-containing polymers and one or more fatty acids are used as components of the composition for forming a backcoat layer, and the salt-forming reaction can be promoted by mixing them in the preparation process of the composition for forming a backcoat layer. In another embodiment, before preparing the composition for forming a backcoat layer, one or more nitrogen-containing polymers and one or more fatty acids are mixed to form a salt, and then the salt can be used as a component of the composition for forming a backcoat layer to prepare the composition for forming a backcoat layer. When the nitrogen-containing polymer and the fatty acids are mixed to form the ammonium salt of the alkyl ester anion represented by formula 1, the nitrogen atom constituting the nitrogen-containing polymer and the carboxyl group of the fatty acid may also react to form the following structure, and the form including such a structure is also included in the above compound.
[0104] [ka]
[0105] Examples of the fatty acids include fatty acids having an alkyl group as described above for R in formula 1 and fluorinated fatty acids having a fluorinated alkyl group as described above for R in formula 1.
[0106] The mixing ratio of the nitrogen-containing polymer and the fatty acid used to form the compound having an ammonium salt structure of an alkyl ester anion represented by formula 1 can be 3:97 to 97:3 as the mass ratio of the nitrogen-containing polymer: the fatty acid. In addition, the compound having an ammonium salt structure of an alkyl ester anion represented by formula 1 can be used, for example, 1.0 to 20.0 parts by mass, and preferably 1.0 to 10.0 parts by mass, per 100.0 parts by mass of carbon black, when preparing the composition for forming a backcoat layer. In addition, for example, the nitrogen-containing polymer can be used, for example, 0.1 to 10.0 parts by mass, per 100.0 parts by mass of carbon black, and preferably 0.5 to 8.0 parts by mass, of the nitrogen-containing polymer. The fatty acid can be used, for example, 0.05 to 10.0 parts by mass, and preferably 0.1 to 5.0 parts by mass, per 100.0 parts by mass of carbon black, when preparing the composition for forming a backcoat layer.
[0107] <Nonmagnetic support> Examples of the non-magnetic support (hereinafter also simply referred to as "support") include known supports such as polyethylene terephthalate, polyethylene naphthalate, polyamide, polyamideimide, aromatic polyamide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred.
[0108] In one embodiment, the non-magnetic support of the magnetic tape may be a polyester support. In the present invention and this specification, "polyester" means a resin containing a plurality of ester bonds. "Polyester support" means a support containing at least one layer of polyester film. "Polyester film" means a film in which the component that constitutes this film in the largest proportion by mass is polyester. In the present invention and this specification, the "polyester support" includes a support in which all the resin films contained in this support are polyester films, and a support containing a polyester film and another resin film. Specific forms of the polyester support include a single-layer polyester film, a laminated film of two or more layers of polyester films having the same constituent components, a laminated film of two or more layers of polyester films having different constituent components, a laminated film containing one or more layers of polyester films and one or more layers of resin films other than polyester, and the like. In the laminated film, an adhesive layer or the like may be optionally included between two adjacent layers. In addition, the polyester support may optionally include a metal film and / or a metal oxide film formed by deposition or the like on one or both surfaces. The above also applies to the "aromatic polyester support", "polyethylene terephthalate support" and "polyethylene naphthalate support" in the present invention and this specification.
[0109] The polyester support can be an aromatic polyester support. In the present invention and this specification, "aromatic polyester" means a resin containing an aromatic backbone and a plurality of ester bonds, and "aromatic polyester support" means a support comprising at least one layer of an aromatic polyester film.
[0110] The aromatic ring contained in the aromatic skeleton of the aromatic polyester is not particularly limited, but specific examples of the aromatic ring include a benzene ring and a naphthalene ring. For example, polyethylene terephthalate (PET) is a polyester containing a benzene ring, and is a resin obtained by polycondensation of ethylene glycol with terephthalic acid and / or dimethyl terephthalate. In the present invention and this specification, "polyethylene terephthalate" also includes structures having one or more other components (e.g., copolymerized components, components introduced into the terminals or side chains, etc.) in addition to the above components. Polyethylene naphthalate (PEN) is a polyester containing a naphthalene ring, and is a resin obtained by esterification of dimethyl 2,6-naphthalenedicarboxylate with ethylene glycol, followed by transesterification and polycondensation. In the present invention and this specification, "polyethylene naphthalate" also includes structures having one or more other components (e.g., copolymer components, components introduced into the terminals or side chains, etc.) in addition to the above components.
[0111] The non-magnetic support may be a biaxially stretched film, and may be a film that has been subjected to corona discharge, plasma treatment, easy-adhesion treatment, heat treatment, or the like.
[0112] <Various thicknesses> With regard to the thickness (total thickness) of the magnetic tape, with the enormous increase in the amount of information in recent years, there is a demand for the magnetic tape to have an increased recording capacity (high capacity). As a means for increasing the capacity, there is a demand for a thinner magnetic tape and an increased length of the magnetic tape accommodated in one magnetic tape cartridge. From this point of view, the thickness (total thickness) of the magnetic tape is preferably 5.6 μm or less, more preferably 5.5 μm or less, more preferably 5.4 μm or less, even more preferably 5.3 μm or less, even more preferably 5.2 μm or less, and even more preferably 5.1 μm or less. As described above, reducing the thickness of the magnetic tape can contribute to reducing the value of the minimum load at which the winding slippage occurs. Moreover, from the viewpoint of ease of handling, the thickness of the magnetic tape is preferably 3.0 μm or more, more preferably 3.5 μm or more.
[0113] The thickness (total thickness) of the magnetic tape can be measured by the following method. Ten tape samples (e.g., 5 to 10 cm long) are cut out from any part of the magnetic tape, and the tape samples are stacked and the thickness is measured. The measured thickness is divided by 10 to obtain the value (thickness per tape sample), which is the tape thickness. The thickness measurement can be performed using a known measuring device capable of measuring thickness to the order of 0.1 μm.
[0114] The thickness of the non-magnetic support is preferably 3.0 to 5.0 μm. The thickness of the magnetic layer can be optimized depending on the saturation magnetization amount of the magnetic head used, the head gap length, the band of the recording signal, etc., and is generally 0.01 μm to 0.15 μm, and from the viewpoint of high density recording, is preferably 0.02 μm to 0.12 μm, and more preferably 0.03 μm to 0.1 μm. At least one magnetic layer is sufficient, and the magnetic layer may be separated into two or more layers having different magnetic properties, and a known configuration related to a multilayer magnetic layer can be applied. When the magnetic layer is separated into two or more layers, the thickness of the magnetic layer is the total thickness of these layers. The thickness of the nonmagnetic layer is, for example, 0.1 to 1.5 μm, and preferably 0.1 to 1.0 μm. The thickness of the backcoat layer is preferably 0.9 μm or less, and more preferably 0.1 to 0.7 μm. Various thicknesses such as the thickness of the magnetic layer can be determined by the following method. After exposing the cross section of the magnetic tape in the thickness direction with an ion beam, the exposed cross section is observed with a scanning electron microscope or a transmission electron microscope. The thicknesses can be calculated as the arithmetic average of the thicknesses measured at any two points in the cross section observation. Alternatively, the thicknesses can be calculated as the design thickness calculated from the manufacturing conditions, etc.
[0115] <Manufacturing process> (Preparation of compositions for forming each layer) The process of preparing the composition for forming the magnetic layer, non-magnetic layer or backcoat layer can usually include at least a kneading process, a dispersion process, and a mixing process provided before or after these processes as necessary. Each process may be divided into two or more stages. The components used in the preparation of the composition for forming each layer may be added at the beginning or during any process. As the solvent, one or more of various solvents usually used in the manufacture of coating-type magnetic recording media can be used. For the solvent, refer to paragraph 0153 of JP-A-2011-216149. Also, each component may be added in two or more steps in a divided manner. For example, the binder may be added in a divided manner in the kneading process, the dispersion process, and the mixing process for adjusting the viscosity after dispersion. In order to manufacture the magnetic tape, known manufacturing techniques can be used in various processes. In the kneading process, it is preferable to use a kneader with a strong kneading force, such as an open kneader, a continuous kneader, a pressure kneader, or an extruder. For details of the kneading treatment, reference can be made to JP-A-1-106338 and JP-A-1-79274. A known dispersing machine can be used. At any stage of preparing each layer-forming composition, filtration may be performed by a known method. Filtration can be performed, for example, by filter filtration. As the filter used for filtration, for example, a filter with a pore size of 0.01 to 3 μm (for example, a glass fiber filter, a polypropylene filter, etc.) can be used.
[0116] (coating process) The magnetic layer can be formed by directly applying the magnetic layer-forming composition onto the surface of the non-magnetic support, or by successively or simultaneously applying the magnetic layer-forming composition and the non-magnetic layer-forming composition in a multi-layer manner. The backcoat layer can be formed by applying the backcoat layer-forming composition onto the surface of the non-magnetic support opposite to the surface having the non-magnetic layer and / or magnetic layer (or the non-magnetic layer and / or magnetic layer will be provided later). For details of the coating for forming each layer, refer to paragraph 0066 of JP2010-231843A.
[0117] (Other processes) Known techniques can be applied to other various steps for manufacturing a magnetic tape. For various steps, see, for example, paragraphs 0067-0070 of JP-A-2010-231843. For example, the coating layer of the magnetic layer-forming composition can be subjected to an orientation treatment in an orientation zone while the coating layer is in a wet state. For the orientation treatment, various known techniques, including those described in paragraph 0052 of JP-A-2010-24113, can be applied. For example, the vertical orientation treatment can be performed by a known method such as a method using magnets with different poles facing each other. In the orientation zone, the drying speed of the coating layer can be controlled by the temperature and volume of the drying air and / or the transport speed in the orientation zone. In addition, the coating layer may be pre-dried before being transported to the orientation zone. A long magnetic tape roll can be obtained through various processes. The obtained magnetic tape roll is cut (slit) to the width of the magnetic tape to be wound into a magnetic tape cartridge by a known cutter. The width is determined according to standards and is usually 1 / 2 inch. 1 / 2 inch = 12.65 mm. A servo pattern is usually formed on the magnetic tape obtained by slitting, as will be described in detail later.
[0118] (Heat treatment) In one embodiment, the magnetic tape may be a magnetic tape manufactured through the following heat treatment. In another embodiment, the magnetic tape may be a magnetic tape manufactured without the following heat treatment.
[0119] The heat treatment can be carried out by winding the magnetic tape, which has been slit and cut to a width determined in accordance with a standard, around a core member and carrying out the heat treatment in the wound state.
[0120] In one form, the above-mentioned heat treatment is performed with the magnetic tape wound around a core-shaped member for heat treatment (hereinafter referred to as the "heat treatment core"), and the magnetic tape after heat treatment is wound onto a cartridge reel of a magnetic tape cartridge, thereby producing a magnetic tape cartridge in which the magnetic tape is wound around the cartridge reel. The heat treatment core may be made of metal, resin, paper, or the like. The material of the heat treatment core is preferably a material with high rigidity from the viewpoint of suppressing the occurrence of winding failures such as sporking. From this viewpoint, the heat treatment core is preferably made of metal or resin. As an index of rigidity, the flexural modulus of the material of the heat treatment core is preferably 0.2 GPa (gigapascal) or more, more preferably 0.3 GPa or more. On the other hand, since high rigidity materials are generally expensive, using a heat treatment core of a material having a rigidity exceeding the rigidity that can suppress the occurrence of winding failures leads to an increase in cost. In consideration of the above, the flexural modulus of the material of the heat treatment core is preferably 250 GPa or less. The flexural modulus is a value measured according to ISO (International Organization for Standardization) 178, and the flexural modulus of various materials is publicly known. The heat treatment core may be a solid or hollow core-shaped member. In the case of a hollow core, the wall thickness is preferably 2 mm or more from the viewpoint of maintaining rigidity. The core for heat treatment may or may not have a flange. It is preferable to prepare a magnetic tape having a length equal to or greater than the length (hereinafter referred to as the "final product length") to be finally accommodated in a magnetic tape cartridge as the magnetic tape to be wound around the core for heat treatment, and to perform heat treatment by placing this magnetic tape wound around the core for heat treatment in a heat treatment environment. The length of the magnetic tape to be wound around the core for heat treatment is equal to or greater than the final product length, and from the viewpoint of ease of winding around the core for heat treatment, it is preferable that the length is "final product length + α". From the viewpoint of ease of winding, this α is preferably 5 m or more. The tension during winding around the core for heat treatment is preferably 0.1 N or more. In addition, from the viewpoint of suppressing excessive deformation during manufacturing, the tension during winding around the core for heat treatment is preferably 1.5 N or less, and more preferably 1.0 N or less. The outer diameter of the core for heat treatment is preferably 20 mm or more, and more preferably 40 mm or more, from the viewpoint of ease of winding and suppression of coiling (curl in the longitudinal direction). The outer diameter of the heat treatment core is preferably 100 mm or less, more preferably 90 mm or less. The width of the heat treatment core may be equal to or greater than the width of the magnetic tape wound around the core. After the heat treatment, when removing the magnetic tape from the heat treatment core, it is preferable to remove the magnetic tape from the heat treatment core after the magnetic tape and the heat treatment core have been sufficiently cooled in order to prevent unintended deformation of the tape during the removal operation. It is preferable to once wind the removed magnetic tape around another core (called the "temporary winding core"), and then wind the magnetic tape from the temporary winding core onto a cartridge reel of a magnetic tape cartridge (generally with an outer diameter of about 40 to 50 mm). This allows the magnetic tape to be wound around the cartridge reel of a magnetic tape cartridge while maintaining the relationship between the inside and outside of the magnetic tape with respect to the heat treatment core during the heat treatment. For details of the temporary winding core and the tension when winding the magnetic tape around this core, the above description of the heat treatment core can be referred to. In a form in which the above-mentioned heat treatment is performed on a magnetic tape having a length of "final product length + α", the length of "+ α" can be cut off at any stage. For example, in one form, the magnetic tape of the final product length is wound from a temporary winding core onto a reel of a magnetic tape cartridge, and the remaining length of "+ α" can be cut off.From the viewpoint of reducing the portion that is cut off and discarded, the above α is preferably 20 m or less.
[0121] A specific embodiment of the heat treatment performed in the state where the material is wound around the core member as described above will be described below. The atmospheric temperature at which the heat treatment is performed (hereinafter referred to as "heat treatment temperature") is preferably 40° C. or higher, and more preferably 50° C. or higher. On the other hand, from the viewpoint of suppressing excessive deformation, the heat treatment temperature is preferably 75° C. or lower, more preferably 70° C. or lower, and even more preferably 65° C. or lower. The weight absolute humidity of the atmosphere in which the heat treatment is carried out is preferably 0.1 g / kg dry air or more, more preferably 1 g / kg dry air or more. An atmosphere with a weight absolute humidity in the above range is preferable because it can be prepared without using a special device for reducing moisture. On the other hand, the weight absolute humidity is preferably 70 g / kg dry air or less, more preferably 66 g / kg dry air or less, from the viewpoint of suppressing the occurrence of condensation and the deterioration of workability. The heat treatment time is preferably 0.3 hours or more, more preferably 0.5 hours or more. Moreover, the heat treatment time is preferably 48 hours or less from the viewpoint of production efficiency.
[0122] (Servo pattern) "Forming a servo pattern" can also be called "recording a servo signal." By using the servo signal to obtain dimensional information about the width of the magnetic tape while it is running, and adjusting and changing the tension applied to the magnetic tape in the longitudinal direction according to the obtained dimensional information, the width of the magnetic tape can be controlled.
[0123] The formation of the servo pattern will be described below.
[0124] The servo pattern is usually formed along the longitudinal direction of the magnetic tape. Control methods that use servo signals (servo control) include timing-based servo (TBS), amplitude servo, and frequency servo.
[0125] As shown in ECMA (European Computer Manufacturers Association)-319 (June 2001), magnetic tapes (generally called "LTO tapes") conforming to the LTO (Linear Tape-Open) standard employ a timing-based servo system. In this timing-based servo system, a servo pattern is formed by a pair of non-parallel magnetic stripes (also called "servo stripes") arranged continuously in the longitudinal direction of the magnetic tape. A servo system is a system that performs head tracking using a servo signal. In this invention and this specification, the "timing-based servo pattern" refers to a servo pattern that enables head tracking in a servo system of the timing-based servo system. As described above, the servo pattern is formed by a pair of non-parallel magnetic stripes in order to inform the servo signal reading element that passes over the servo pattern of its passing position. Specifically, the pair of magnetic stripes is formed so that the interval between them changes continuously along the width direction of the magnetic tape, and the servo signal reading element can know the relative position between the servo pattern and the servo signal reading element by reading the interval. This relative position information enables tracking of the data track. For this reason, a plurality of servo tracks are usually set on the servo pattern along the width direction of the magnetic tape.
[0126] A servo band is made up of a continuous servo pattern in the longitudinal direction of the magnetic tape. Usually, multiple servo bands are provided on a magnetic tape. For example, there are five servo bands on an LTO tape. The area between two adjacent servo bands is the data band. The data band is made up of multiple data tracks, and each data track corresponds to one servo track.
[0127] Also, in one embodiment, as shown in JP 2004-318983 A, information indicating the number of the servo band (also called "servo band ID (identification)" or "UDIM (Unique Data Band Identification Method) information") is embedded in each servo band. This servo band ID is recorded by shifting a specific one of a plurality of pairs of servo stripes in the servo band so that its position is displaced relatively in the longitudinal direction of the magnetic tape. Specifically, the way in which a specific one of a plurality of pairs of servo stripes is shifted is changed for each servo band. As a result, the recorded servo band ID is unique for each servo band, so that the servo band can be uniquely identified simply by reading one servo band with a servo signal reading element.
[0128] Incidentally, there is also a method for uniquely identifying servo bands that uses the staggered method as shown in ECMA-319 (June 2001). In this staggered method, a group of pairs of non-parallel magnetic stripes (servo stripes) arranged continuously in the longitudinal direction of the magnetic tape are recorded so that they are shifted in the longitudinal direction of the magnetic tape for each servo band. The combination of the shift between adjacent servo bands is unique across the entire magnetic tape, so when the servo pattern is read by two servo signal reading elements, it is possible to uniquely identify the servo bands.
[0129] Also, as specified in ECMA-319 (June 2001), information indicating the longitudinal position of the magnetic tape (also called "LPOS (Longitudinal Position) information") is usually embedded in each servo band. Like UDIM information, this LPOS information is also recorded by shifting the positions of a pair of servo stripes in the longitudinal direction of the magnetic tape. However, unlike UDIM information, the same signal is recorded in each servo band with this LPOS information.
[0130] It is also possible to embed information other than the above UDIM information and LPOS information in the servo bands. In this case, the embedded information may be different for each servo band, such as UDIM information, or may be common to all servo bands, such as LPOS information. Also, methods other than those described above can be used to embed information in the servo bands. For example, a predetermined code may be recorded by thinning out a predetermined pair from a group of pairs of servo stripes.
[0131] The head for forming a servo pattern is called a servo write head. The servo write head usually has a pair of gaps corresponding to the pair of magnetic stripes, the number of which is equal to the number of servo bands. Usually, a core and a coil are connected to each pair of gaps, and a magnetic field generated in the core can generate a leakage magnetic field in the pair of gaps by supplying a current pulse to the coil. When forming a servo pattern, a magnetic pattern corresponding to the pair of gaps can be transferred to the magnetic tape by inputting a current pulse while running the magnetic tape on the servo write head, thereby forming the servo pattern. The width of each gap can be appropriately set according to the density of the servo pattern to be formed. The width of each gap can be set, for example, to 1 μm or less, 1 to 10 μm, or 10 μm or more.
[0132] Before forming a servo pattern on the magnetic tape, the magnetic tape is usually subjected to a demagnetization (erase) process. This erase process can be performed by applying a uniform magnetic field to the magnetic tape using a direct current magnet or an alternating current magnet. There are two types of erase processes: DC (Direct Current) erase and AC (Alternating Current) erase. AC erase is performed by gradually lowering the strength of the magnetic field applied to the magnetic tape while reversing the direction of the magnetic field. On the other hand, DC erase is performed by applying a unidirectional magnetic field to the magnetic tape. There are two more methods of DC erase. The first method is horizontal DC erase, which applies a unidirectional magnetic field along the longitudinal direction of the magnetic tape. The second method is vertical DC erase, which applies a unidirectional magnetic field along the thickness direction of the magnetic tape. The erase process may be performed on the entire magnetic tape, or may be performed for each servo band of the magnetic tape.
[0133] The direction of the magnetic field of the formed servo pattern is determined according to the direction of erasure. For example, when the magnetic tape is subjected to horizontal DC erasure, the servo pattern is formed so that the direction of the magnetic field is opposite to the direction of erasure. This can increase the output of the servo signal obtained by reading the servo pattern. As shown in JP2012-53940A, when the magnetic pattern is transferred to the magnetic tape that has been vertically DC erased using the above gap, the servo signal obtained by reading the formed servo pattern has a unipolar pulse shape. On the other hand, when the magnetic pattern is transferred to the magnetic tape that has been horizontally DC erased using the above gap, the servo signal obtained by reading the formed servo pattern has a bipolar pulse shape.
[0134] <Magnetic head> In the present invention and this specification, the term "magnetic tape device" refers to a device capable of at least one of recording data on a magnetic tape and reproducing data recorded on the magnetic tape. Such a device is generally called a drive. The magnetic head included in the magnetic tape device can be a recording head capable of recording data on a magnetic tape, and can also be a reproducing head capable of reproducing data recorded on the magnetic tape. In one embodiment, the magnetic tape device can include both a recording head and a reproducing head as separate magnetic heads. In another embodiment, the magnetic head included in the magnetic tape device can have a configuration in which both a recording element and a reproducing element are provided in one magnetic head. As the reproducing head, a magnetic head (MR head) including a magnetoresistive (MR) element capable of reading information recorded on a magnetic tape with good sensitivity as a reproducing element is preferable. As the MR head, various known MR heads (for example, a GMR (Giant Magnetoresistive) head, a TMR (Tunnel Magnetoresistive) head, etc.) can be used. In addition, the magnetic head that records and / or reproduces data may include a servo pattern reading element. Alternatively, the magnetic tape device may include a magnetic head (servo head) equipped with a servo pattern reading element as a head separate from the magnetic head that records and / or reproduces data. For example, a magnetic head that records and / or reproduces recorded data (hereinafter also referred to as a "recording and reproducing head") may include two servo signal reading elements, and each of the two servo signal reading elements may simultaneously read two adjacent servo bands sandwiching a data band. One or more data elements may be disposed between the two servo signal reading elements. The element for recording data (recording element) and the element for reproducing data (reproducing element) are collectively referred to as the "data element."
[0135] By using a reproducing element with a narrow reproducing element width as the reproducing element to reproduce data, data recorded at a high density can be reproduced with high sensitivity. From this viewpoint, the reproducing element width of the reproducing element is preferably 0.8 μm or less. The reproducing element width of the reproducing element can be, for example, 0.3 μm or more. However, from the above viewpoint, it is also preferable that the reproducing element width is less than this value. On the other hand, the narrower the reproducing element width, the more likely it is that phenomena such as poor reproduction caused by off-track will occur. In order to suppress the occurrence of such phenomena, a magnetic tape device is preferred that controls the dimension of the magnetic tape in the width direction by adjusting and changing the tension applied to the magnetic tape in the longitudinal direction while it is running. Here, the "reading element width" refers to the physical dimension of the width of the reading element. Such physical dimension can be measured using an optical microscope, a scanning electron microscope, or the like.
[0136] When recording data and / or reproducing recorded data, head tracking using servo signals can be performed first. That is, by making the servo signal reading element follow a specific servo track, the data element can be controlled to pass over the target data track. The data track is moved by changing the servo track read by the servo signal reading element in the tape width direction. The recording / reproducing head can also record and / or reproduce data on other data bands by using the UDIM information described above to move the servo signal reading element to a specific servo band and start tracking on that servo band.
[0137] FIG. 2 shows an example of the arrangement of data bands and servo bands. In FIG. 2, a plurality of servo bands 1 are arranged on the magnetic layer of the magnetic tape MT, sandwiched between guide bands 3. A plurality of regions 2 sandwiched between two servo bands are data bands. A servo pattern is a magnetized region, and is formed by magnetizing a specific region of the magnetic layer with a servo write head. The region magnetized by the servo write head (the position where the servo pattern is formed) is determined by a standard. For example, in an LTO Ultrium format tape, which is an industry standard, a plurality of servo patterns inclined with respect to the tape width direction are formed on the servo band during the manufacturing of the magnetic tape, as shown in FIG. 3. More specifically, in FIG. 3, a servo frame SF on the servo band 1 is composed of a servo subframe 1 (SSF1) and a servo subframe 2 (SSF2). The servo subframe 1 is composed of an A burst (symbol A in FIG. 3) and a B burst (symbol B in FIG. 3). The A burst is composed of servo patterns A1 to A5, and the B burst is composed of servo patterns B1 to B5. On the other hand, the servo subframe 2 is composed of a C burst (symbol C in FIG. 3) and a D burst (symbol D in FIG. 3). The C burst is composed of servo patterns C1 to C4, and the D burst is composed of servo patterns D1 to D4. Such 18 servo patterns are arranged in a subframe arranged in a 5, 5, 4, 4 arrangement in a set of 5 and 4, and are used to identify a servo frame. For the sake of explanation, one servo frame is shown in FIG. 3. However, in reality, a plurality of servo frames are arranged in the running direction in each servo band on the magnetic layer of a magnetic tape where head tracking of the timing-based servo method is performed. In FIG. 3, the arrow indicates the running direction. For example, an LTO Ultrium format tape usually has 5,000 or more servo frames per meter of tape length in each servo band on the magnetic layer. EXAMPLES
[0138] An embodiment of the present invention will be described below based on an example. However, the present invention is not limited to the embodiment shown in the example. The indications of "parts" and "%" below mean "parts by mass" and "% by mass" unless otherwise specified. "eq" is an equivalent, and is a unit that cannot be converted to SI units. In addition, the following various steps and operations were carried out in an environment with a temperature of 20 to 25° C. and a relative humidity of 40 to 60%, unless otherwise specified.
[0139] [Non-magnetic support] In Table 1 below, "PEN" indicates a polyethylene naphthalate support and "PET" indicates a polyethylene terephthalate support.
[0140] [Ferromagnetic powder] In Table 1, "BaFe" in the column for type of ferromagnetic powder indicates hexagonal barium ferrite powder with an average particle size (average plate diameter) of 21 nm.
[0141] In Table 1, "SrFe1" in the column for type of ferromagnetic powder indicates a hexagonal strontium ferrite powder prepared as follows. SrCO 3 1707g, H 3 BO 3 687g, Fe 2 O 3 1120g, Al(OH) 3 45g, BaCO 3 24g, CaCO 3 13g, and Nd 2 O 3 The above was weighed out in an amount of 235 g and mixed in a mixer to obtain a raw material mixture. The obtained raw material mixture was melted in a platinum crucible at a melting temperature of 1390°C, and the melt was poured into a rod shape at about 6 g / sec by heating the tapping hole at the bottom of the platinum crucible while stirring the melt. The tapped liquid was rolled and quenched with a water-cooled twin roller to produce an amorphous body. 280 g of the produced amorphous body was placed in an electric furnace, heated to 635°C (crystallization temperature) at a heating rate of 3.5°C / min, and held at that temperature for 5 hours to precipitate (crystallize) hexagonal strontium ferrite particles. Next, the crystallized material obtained above containing hexagonal strontium ferrite particles was coarsely crushed in a mortar, and 1000 g of zirconia beads with a particle size of 1 mm and 800 mL of 1% aqueous acetic acid solution were added to a glass bottle and dispersed for 3 hours using a paint shaker. The resulting dispersion was then separated from the beads and placed in a stainless steel beaker. The dispersion was left to stand at a liquid temperature of 100°C for 3 hours to dissolve the glass components, and then precipitated in a centrifuge and washed by repeated decantation, and dried for 6 hours in a heating furnace at a furnace temperature of 110°C to obtain hexagonal strontium ferrite powder. The average particle size of the hexagonal strontium ferrite powder obtained above is 18 nm, and the activation volume is 902 nm. 3 , the anisotropy constant Ku is 2.2×10 5 J / m 3 , mass magnetization σs is 49A m 2 / kg. A 12 mg sample powder was taken from the hexagonal strontium ferrite powder obtained above, and this sample powder was partially dissolved under the dissolution conditions exemplified above. The elemental analysis of the filtrate obtained was performed using an ICP analyzer to determine the surface layer content of neodymium atoms. Separately, 12 mg of sample powder was taken from the hexagonal strontium ferrite powder obtained above, and this sample powder was completely dissolved under the dissolution conditions exemplified above. The elemental analysis of the filtrate obtained was performed using an ICP analyzer to determine the bulk content of neodymium atoms. The neodymium atom content (bulk content) relative to 100 atomic % of iron atoms in the hexagonal strontium ferrite powder obtained above was 2.9 atomic %. The surface layer content of neodymium atoms was 8.0 atomic %. The ratio of the surface layer content to the bulk content, "surface layer content / bulk content," was 2.8, confirming that neodymium atoms were unevenly distributed in the surface layers of the particles.
[0142] It was confirmed that the powder obtained above exhibited a hexagonal ferrite crystal structure by scanning with CuKα radiation at a voltage of 45 kV and an intensity of 40 mA and measuring the X-ray diffraction pattern under the following conditions (X-ray diffraction analysis). The powder obtained above exhibited a magnetoplumbite-type (M-type) hexagonal ferrite crystal structure. The crystal phase detected by the X-ray diffraction analysis was a single phase of magnetoplumbite type. PANalytical X'Pert Pro diffractometer, PIXcel detector Soller slits for incident and diffracted beams: 0.017 radians Dispersion slit fixed angle: 1 / 4 degree Mask: 10mm Anti-scatter slit: 1 / 4 degree Measurement mode: Continuous Measurement time per step: 3 seconds Measurement speed: 0.017 degrees per second Measurement step: 0.05 degrees
[0143] In Table 1, "SrFe2" in the column for type of ferromagnetic powder indicates hexagonal strontium ferrite powder prepared as follows. SrCO 3 1725g, H 3 BO 3 666g, Fe 2 O 3 1332g, Al(OH) 3 52g, CaCO 3 34g, BaCO 3 The above was weighed out in an amount of 141 g and mixed in a mixer to obtain a raw material mixture. The obtained raw material mixture was melted in a platinum crucible at a melting temperature of 1380°C, and the melt was poured into a rod shape at about 6 g / sec by heating the tapping hole at the bottom of the platinum crucible while stirring the melt. The tapped liquid was rolled and quenched with a water-cooled twin roll to produce an amorphous body. 280 g of the obtained amorphous body was placed in an electric furnace, heated to 645° C. (crystallization temperature), and held at that temperature for 5 hours to precipitate (crystallize) hexagonal strontium ferrite particles. Next, the crystallized material obtained above containing hexagonal strontium ferrite particles was coarsely crushed in a mortar, and 1000 g of zirconia beads with a particle size of 1 mm and 800 mL of 1% aqueous acetic acid solution were added to a glass bottle and dispersed for 3 hours using a paint shaker. The resulting dispersion was then separated from the beads and placed in a stainless steel beaker. The dispersion was left to stand at a liquid temperature of 100°C for 3 hours to dissolve the glass components, and then precipitated in a centrifuge and washed by repeated decantation, and dried for 6 hours in a heating furnace at a furnace temperature of 110°C to obtain hexagonal strontium ferrite powder. The average particle size of the obtained hexagonal strontium ferrite powder was 19 nm, and the activation volume was 1102 nm. 3 , the anisotropy constant Ku is 2.0×10 5 J / m 3 , mass magnetization σs is 50A m 2 / kg.
[0144] In Table 1, "ε-iron oxide" refers to ε-iron oxide powder prepared as follows. 8.3g of iron (III) nitrate nonahydrate, 1.3g of gallium (III) nitrate octahydrate, 190mg of cobalt (II) nitrate hexahydrate, 150mg of titanium (IV) sulfate, and 1.5g of polyvinylpyrrolidone (PVP) were dissolved in 90g of pure water, and 4.0g of ammonia solution with a concentration of 25% was added under the condition of an atmospheric temperature of 25°C while stirring with a magnetic stirrer in the air, and the mixture was stirred for 2 hours at an atmospheric temperature of 25°C. A citric acid solution obtained by dissolving 1g of citric acid in 9g of pure water was added to the obtained solution, and the mixture was stirred for 1 hour. The powder precipitated after stirring was collected by centrifugation, washed with pure water, and dried in a heating furnace at an internal temperature of 80°C. 800g of pure water was added to the dried powder, and the powder was dispersed in water again to obtain a dispersion. The obtained dispersion was heated to 50°C, and 40g of 25% ammonia aqueous solution was added dropwise while stirring. After stirring for 1 hour while maintaining the temperature at 50°C, 14mL of tetraethoxysilane (TEOS) was added dropwise and stirred for 24 hours. 50g of ammonium sulfate was added to the obtained reaction solution, and the precipitated powder was collected by centrifugation, washed with pure water, and dried for 24 hours in a heating furnace with an internal temperature of 80°C to obtain a precursor of ferromagnetic powder. The obtained precursor of the ferromagnetic powder was placed in a heating furnace at an internal temperature of 1000° C. in an air atmosphere and subjected to a heat treatment for 4 hours. The heat-treated ferromagnetic powder precursor was placed in a 4 mol / L aqueous solution of sodium hydroxide (NaOH), and the liquid temperature was maintained at 70°C while stirring for 24 hours, thereby removing impurities such as silicate compounds from the heat-treated ferromagnetic powder precursor. Thereafter, the silicic acid compound was removed by centrifugation, and the ferromagnetic powder was collected and washed with pure water to obtain a ferromagnetic powder. The composition of the obtained ferromagnetic powder was confirmed by inductively coupled plasma-optical emission spectrometry (ICP-OES). The results showed that the powder was composed of Ga, Co, and Ti substituted ε-iron oxide (ε-Ga 0.28 Co 0.05 Ti 0.05 Fe 1.62 O 3 In addition, X-ray diffraction analysis was performed under the same conditions as those described above for the hexagonal strontium ferrite powder SrFe1, and it was confirmed from the peaks in the X-ray diffraction pattern that the obtained ferromagnetic powder had a single-phase ε-phase crystal structure (ε-iron oxide type crystal structure) that did not contain α-phase or γ-phase crystal structures. The average particle size of the obtained ε-iron oxide powder was 12 nm, and the activation volume was 746 nm. 3 , the anisotropy constant Ku is 1.2×10 5 J / m 3 , mass magnetization σs is 16A m 2 / kg.
[0145] The activation volume and anisotropy constant Ku of the above hexagonal strontium ferrite powder and ε-iron oxide powder were determined for each ferromagnetic powder by the method described above using a vibrating sample magnetometer (manufactured by Toei Kogyo Co., Ltd.). The mass magnetization σs is a value measured using a vibrating sample magnetometer (manufactured by Toei Industry Co., Ltd.) at a magnetic field strength of 1194 kA / m (15 kOe).
[0146] [Example 1] <Magnetic tape cartridge production> (1) Preparation of alumina dispersion Alpha conversion rate approximately 65%, BET (Brunauer-Emmett-Teller) specific surface area 20m 2 100.0 parts of alumina powder (HIT-80 manufactured by Sumitomo Chemical Co., Ltd.) with a molecular weight of 1.0 g / g was mixed with 3.0 parts of 2,3-dihydroxynaphthalene (manufactured by Tokyo Chemical Industry Co., Ltd.) and SO 3 31.3 parts of a 32% solution (solvent is a mixed solvent of methyl ethyl ketone and toluene) of polyester polyurethane resin having a Na group (UR-4800 (polar group amount: 80 meq / kg) manufactured by Toyobo Co., Ltd.) was mixed with 570.0 parts of a mixed solution of methyl ethyl ketone and cyclohexanone at a 1:1 (mass ratio) as a solvent, and dispersed for 5 hours in the presence of zirconia beads using a paint shaker. After dispersion, the dispersion liquid and the beads were separated using a mesh to obtain an alumina dispersion.
[0147] (2) Magnetic layer forming composition formulation (Magnetic liquid) Ferromagnetic powder 100.0 parts Hexagonal barium ferrite powder with an average particle size (average plate diameter) of 21 nm ("BaFe" in Table 1) Magnetic layer dispersant See Table 1 SO 3 Sodium-containing polyurethane resin 14.0 parts Weight average molecular weight: 70,000, SO 3 Sodium group: 0.2 meq / g Cyclohexanone 150.0 parts Methyl ethyl ketone 150.0 parts (abrasive liquid) 6.0 parts of the alumina dispersion prepared in (1) above (Silica sol (protrusion forming liquid)) Colloidal silica (average particle size: 120 nm) 2.0 parts Methyl ethyl ketone 1.4 parts (Other Ingredients) Stearic acid 2.0 parts Stearic acid amide 0.2 parts Butyl stearate 2.0 parts Polyisocyanate (Tosoh Corporation, Coronate (registered trademark) L) 2.5 parts (Finishing solvent) Cyclohexanone 200.0 parts Methyl ethyl ketone 200.0 parts
[0148] The dispersant is a compound (a compound having a polyalkyleneimine chain and a vinyl polymer chain) described as a component of the magnetic layer forming composition of Example 1 in JP 2019-169225 A. The reaction solution obtained after the synthesis of the above compound was used as a component of the magnetic layer forming composition. The content of the dispersant in the magnetic layer shown in Table 1 below is the amount of the above compound in the reaction solution.
[0149] (3) Formulation of composition for forming nonmagnetic layer Non-magnetic inorganic powder: α-iron oxide 100.0 parts Average particle size (average major axis length): 0.15μm Average acicular ratio: 7 BET specific surface area: 52m 2 / g Carbon black 20.0 parts Average particle size: 20nm SO 3 Sodium-containing polyurethane resin 18.0 parts Weight average molecular weight: 70,000, SO 3 Sodium group: 0.2 meq / g Stearic acid 2.0 parts Stearic acid amide 0.2 parts Butyl stearate 2.0 parts Cyclohexanone 300.0 parts Methyl ethyl ketone 300.0 parts
[0150] (4) Formulation of composition for forming backcoat layer Carbon black 100.0 parts DBP (Dibutyl phthalate) oil absorption 74cm 3 / 100g Nitrocellulose 27.0 parts Polyester polyurethane resin containing sulfonic acid groups and / or their salts 62.0 copies Polyester resin 4.0 parts Polyethyleneimine (manufactured by Nippon Shokubai, number average molecular weight 600) See Table 1 Stearic acid See Table 1 Alumina powder (BET specific surface area: 17m 2 / g) 0.6 parts Methyl ethyl ketone 600.0 parts Toluene 600.0 parts Polyisocyanate (Tosoh Coronate L) 15.0 parts
[0151] (5) Preparation of compositions for forming each layer The magnetic layer forming composition was prepared by the following method. The magnetic liquid was prepared by dispersing the components of the magnetic liquid for 24 hours (bead dispersion) using a batch-type vertical sand mill. Zirconia beads with a bead diameter of 0.5 mm were used as the dispersion beads. The prepared magnetic liquid, the abrasive liquid, and other components (silica sol, other components, and finishing additive solvent) were mixed using the sand mill and dispersed with beads for 5 minutes, and then treated with a batch-type ultrasonic device (20 kHz, 300 W) for 0.5 minutes (ultrasonic dispersion). After that, filtration was performed using a filter with a pore size of 0.5 μm to prepare the magnetic layer forming composition. The composition for forming the nonmagnetic layer was prepared by the following method. The above components, except for the lubricants (stearic acid, stearic acid amide, and butyl stearate), were kneaded and diluted using an open kneader, and then dispersed using a horizontal bead mill disperser. The lubricants (stearic acid, stearic acid amide, and butyl stearate) were then added, and the mixture was stirred and mixed using a dissolver stirrer to prepare the composition for forming the nonmagnetic layer. The composition for forming a backcoat layer was prepared by the following method. The above components except for the polyisocyanate were introduced into a dissolver mixer, stirred at a peripheral speed of 10 m / sec for 30 minutes, and then dispersed using a horizontal bead mill disperser. Then, the polyisocyanate was added, and the mixture was stirred and mixed using the dissolver mixer to prepare the composition for forming a backcoat layer.
[0152] (6) Methods for manufacturing magnetic tapes and magnetic tape cartridges On the surface of a biaxially stretched support of the type and thickness shown in Table 1, the nonmagnetic layer-forming composition prepared in (5) above was applied and dried to form a nonmagnetic layer so that the thickness after drying was the value shown in Table 1. Next, the magnetic layer-forming composition prepared in (5) above was applied on the nonmagnetic layer so that the thickness after drying was the value shown in Table 1 to form a coating layer. Thereafter, while the coating layer of the magnetic layer-forming composition was in a wet state, a magnetic field with a magnetic field strength of 0.3 T was applied perpendicularly to the surface of the coating layer to perform a vertical orientation treatment, and then the coating layer was dried to form a magnetic layer. Thereafter, the backcoat layer-forming composition prepared in (5) above was applied and dried on the surface of the support opposite to the surface on which the nonmagnetic layer and magnetic layer were formed so that the thickness after drying was the thickness shown in Table 1 to form a backcoat layer. Thereafter, a surface smoothing treatment (calendering) was performed using a calender roll consisting only of a metal roll at a speed of 100 m / min, a linear pressure of 300 kg / cm, and a calender temperature (surface temperature of the calender roll) of 90°C. Thereafter, the long magnetic tape was heat-treated by storing it in a heat treatment furnace at an atmospheric temperature of 70°C (heat treatment time: 36 hours). After the heat treatment, the magnetic tape was slit into 1 / 2 inch width to obtain a magnetic tape. A servo signal was recorded on the magnetic layer of the obtained magnetic tape by a commercially available servo writer to obtain a magnetic tape having a data band, a servo band, and a guide band in an arrangement according to the LTO (Linear Tape-Open) Ultrium format, and having a servo pattern (timing-based servo pattern) on the servo band with an arrangement and shape according to the LTO Ultrium format. The servo pattern thus formed is a servo pattern according to the descriptions of JIS (Japanese Industrial Standards) X6175:2006 and Standard ECMA-319 (June 2001). The magnetic tape (length 960 m) after the servo signal recording was wound around a core for heat treatment, and heat treatment was performed while the tape was wound around the core. A solid core-shaped member (outer diameter: 50 mm) made of resin with a flexural modulus of 0.8 GPa was used as the core for heat treatment, and the tension during winding was 0.6 N. The heat treatment was performed for 5 hours at a heat treatment temperature of 55°C. The weight absolute humidity of the atmosphere in which the heat treatment was performed was 10 g / kg dry air. After the above heat treatment, the magnetic tape and the core for heat treatment were sufficiently cooled, and then the magnetic tape was removed from the core for heat treatment and wound onto the core for temporary winding, and then the magnetic tape was wound from the core for temporary winding onto a reel (reel outer diameter: 44 mm) of a magnetic tape cartridge (LTO Ultrium 7 data cartridge) by the final product length (950 m), and the remaining 10 m was cut off, and a leader tape was spliced to the end of the cut-off side using a commercially available splicing tape in accordance with item 9 of Section 3 of Standard ECMA (European Computer Manufacturers Association)-319 (June 2001). As the core for temporary winding, a solid core member made of the same material and having the same outer diameter as the core for heat treatment was used, and the tension during winding was 0.6 N. As a result of the above, a single-reel type magnetic tape cartridge of Example 1 was produced, in which a magnetic tape of 950 m length was wound around a reel.
[0153] The above steps were repeated to prepare three magnetic tape cartridges. Of the three magnetic tape cartridges, one was used for (7) to (9) below, another was used for (10) below, and the remaining magnetic tape cartridge was used for (11) below.
[0154] Whether the backcoat layer of a magnetic tape contains a compound containing an ammonium salt structure of an alkyl ester anion represented by formula 1, which is formed from polyethyleneimine and stearic acid, can be confirmed by the following method. A sample is cut out from the magnetic tape, and the surface of the backcoat layer (measurement area: 300 μm × 700 μm) is subjected to X-ray photoelectron spectroscopy using an ESCA device. In detail, a wide scan measurement is performed using the ESCA device under the following measurement conditions. In the measurement results, peaks are confirmed at the position of the binding energy of the ester anion and the position of the binding energy of the ammonium cation. Equipment: Shimadzu AXIS-ULTRA Excitation X-ray source: Monochromated Al-Kα radiation Scan range: 0~1200eV Pass energy: 160 eV Energy resolution: 1eV / step Acquisition time: 100ms / step Number of times: 5 In addition, a sample piece of 3 cm in length was cut out from the magnetic tape, and the surface of the backcoat layer was measured with an ATR-FT-IR (Attenuated total reflection-Fourier transform-infrared spectrometer) (reflection method). - The wave number corresponding to the absorption of -1 or 1430cm -1 ), and the wavenumber corresponding to the absorption of the ammonium cation (2400 cm-1 ) absorption is confirmed.
[0155] (7) Recording of data on magnetic tapes before storage and playback of recorded data Recording and playback before storage were performed using a magnetic tape device with the configuration shown in Figure 1. The recording and playback head mounted on the recording and playback head unit has 32 or more channels of playback elements (playback element width: 0.8 μm) and recording elements, with servo signal reading and playback elements on both sides. To acclimate the magnetic tape cartridge to the recording and playback environment, the cartridge was placed in an environment with an ambient temperature of 23° C. and a relative humidity of 50% for five days. After that, recording and playback were performed in the same environment as described below. A magnetic tape cartridge is set in a magnetic tape device and the magnetic tape is loaded. Next, while performing servo tracking, pseudo-random data with a specific data pattern is recorded on the magnetic tape by the recording / playback head unit. A constant tension of 0.50 N is applied to the tape in the longitudinal direction during this process. At the same time as the data is recorded, the servo band intervals over the entire length of the tape are measured every 1 m along the longitudinal direction and recorded in the cartridge memory. Next, the data recorded on the magnetic tape is reproduced by the recording / reproducing head unit while performing servo tracking. At the same time as reproduction, the value of the servo band interval is measured, and based on the information recorded in the cartridge memory, the tension applied in the longitudinal direction of the tape is changed so that the absolute value of the difference from the servo band interval at the time of recording at the same longitudinal position approaches 0. During reproduction, the measurement of the servo band interval and the tension control based on the measurement are performed continuously in real time. During such reproduction, the tension applied in the longitudinal direction of the magnetic tape is changed in the range of 0.50N to 0.85N by the control device of the magnetic tape device. Therefore, during the above reproduction, the maximum value of the tension applied in the longitudinal direction of the magnetic tape is 0.85N. At the end of the playback, the entire length of the magnetic tape has been wound onto the cartridge reel of the magnetic tape cartridge.
[0156] (8) Rewinding the cartridge reel (rewinding before storage) and storage The magnetic tape was then run in the magnetic tape device under the above-mentioned environment until the entire length of the magnetic tape was wound onto the take-up reel of the magnetic tape device. The tension applied to the magnetic tape in the longitudinal direction during the winding was set to a constant value of 0.50 N. Thereafter, a constant tension of 0.30 N was applied to the magnetic tape in the longitudinal direction, and the entire length of the magnetic tape was wound onto a cartridge reel (also referred to as "rewinding before storage"). After the above pre-storage rewinding, the magnetic tape cartridge containing the magnetic tape was stored in an environment having an atmospheric temperature of 60° C. and a relative humidity of 20% for 72 hours.
[0157] (9) Evaluation of recording and playback quality after storage After the above storage, the magnetic tape cartridge was placed in an environment with an ambient temperature of 23°C and a relative humidity of 50% for 5 days to allow it to acclimate to the environment in which it would be played back. Thereafter, in the same environment, playback was performed in the same manner as in the playback before storage in (7) above. That is, playback was performed while changing the tension applied to the magnetic tape in the longitudinal direction as described above. The number of channels in the above playback was 32. When the data for all 32 channels was read correctly during playback after storage, the recording and playback quality was rated as "3." When the data for channels 31 to 28 was read correctly, the recording and playback quality was rated as "2." In all other cases, the recording and playback quality was rated as "1."
[0158] (10) Minimum load for winding slippage The minimum load required for the magnetic tape to slip was determined using the method described above. An ultrasonic cutter was used to remove the upper and lower flanges. The load was applied by pressing the plate with a pressing device so that a uniform load was applied to the entire surface of the plate.
[0159] (11) Tape thickness Ten tape samples (5 cm long) were cut from any part of the magnetic tape removed from the magnetic tape cartridge, and these tape samples were stacked and the thickness was measured. The thickness was measured using a digital thickness meter with a Millimar 1240 compact amplifier and a Millimar 1301 inductive probe manufactured by MARH. The measured thickness was divided by 10 to obtain the value (thickness per tape sample), which was taken as the tape thickness.
[0160] [Examples 2 to 24, Comparative Examples 1 to 18] A magnetic tape cartridge was produced and various evaluations were carried out in the same manner as in Example 1, except that the items in Table 1 were changed as shown in Table 1.
[0161] In the examples and comparative examples in Table 1 where the "Tension change during running" column is marked "Yes," playback before storage was performed by changing the tension applied to the magnetic tape in the longitudinal direction within the same minimum to maximum range as in Example 1. In the examples in Table 1 where "none" is listed in the "tension change during running" column, playback before storage was performed with a constant tension of 0.50 N applied in the longitudinal direction of the magnetic tape.
[0162] For the embodiments and comparative examples in which the tension values are listed in the "Rewinding tension before storage" column in Table 1, the tension applied in the longitudinal direction of the magnetic tape when rewinding it onto the cartridge reel (rewinding it before storage) in (8) above was the value shown in Table 1. For the comparative examples in Table 1 where "No rewinding" is written in the "Rewinding tension before storage" column, after playback as described above in (7), the magnetic tape cartridge containing the magnetic tape was stored for 72 hours in an environment with an ambient temperature of 60°C and a relative humidity of 20% without rewinding.
[0163] In the examples and comparative examples, the playback after storage was performed in the same manner as the playback before storage. That is, the tension applied in the longitudinal direction of the magnetic tape during playback after storage and the presence or absence of change in the tension were the same as those before storage.
[0164] The above results are shown in Table 1 (Table 1-1 to Table 1-4).
[0165] [Table 1-1]
[0166] [Table 1-2]
[0167] [Table 1-3]
[0168] [Table 1-4]
[0169] From the results shown in Table 1, it can be confirmed that good recording and reproduction quality was obtained after storage in the examples.
[0170] A magnetic tape cartridge was produced in the same manner as in Example 1, except that no vertical orientation treatment was performed during the production of the magnetic tape. A sample piece was cut out from the magnetic tape removed from the magnetic tape cartridge. The squareness in the vertical direction of the sample piece was measured by the above-mentioned method using a vibrating sample magnetometer, TM-TRVSM5050-SMSL model manufactured by Tamagawa Seisakusho, and was found to be 0.55. The magnetic tape was also removed from the magnetic tape cartridge of Example 1, and a sample piece was cut out from this magnetic tape. The squareness ratio in the vertical direction was similarly determined to be 0.60.
[0171] The magnetic tapes taken out of the two magnetic tape cartridges were each attached to a 1 / 2 inch reel tester, and the electromagnetic conversion characteristics (SNR; Signal-to-Noise Ratio) were evaluated by the following method. As a result, the magnetic tape taken out of the magnetic tape cartridge of Example 1 had an SNR value 2 dB higher than that of the magnetic tape produced without the vertical orientation treatment. In an environment with a temperature of 23°C and a relative humidity of 50%, 10 passes of recording and reproduction were performed with a tension of 0.7 N applied in the longitudinal direction of the magnetic tape. The relative speed between the magnetic tape and the magnetic head was 6 m / sec. Recording was performed using a MIG (Metal-in-gap) head (gap length 0.15 μm, track width 1.0 μm) as the recording head, and the recording current was set to the optimal recording current for each magnetic tape. Reproduction was performed using a GMR (Giant-magnetoresistive) head (element thickness 15 nm, shield spacing 0.1 μm, reproduction element width 0.8 μm) as the reproduction head. A signal with a linear recording density of 300 kfci was recorded, and the reproduction signal was measured with a spectrum analyzer manufactured by Shibasoku. The unit kfci is the unit of linear recording density (not convertible to SI units). The signal was used at a portion where the signal was sufficiently stable after the magnetic tape started running. [Industrial Applicability]
[0172] One aspect of the present invention is useful in the technical fields of various data storage such as archives.
Claims
1. A magnetic tape cartridge including a magnetic tape and a cartridge reel, The magnetic tape has a non-magnetic support and a magnetic layer containing a ferromagnetic powder, and further has a backcoat layer containing a non-magnetic powder on a surface side of the non-magnetic support opposite to the surface side having the magnetic layer, The backcoat layer contains a compound having an ammonium salt structure of an alkyl ester anion represented by the following formula 1: 【Chemistry 1】 In formula 1, R represents an alkyl group having 7 or more carbon atoms or a fluorinated alkyl group having 7 or more carbon atoms, Z + represents an ammonium cation, the magnetic tape has a minimum load for causing a slippage of 250 N or less, measured after being rewound onto the cartridge reel with a tension of 0.30 N applied in the longitudinal direction of the magnetic tape; The minimum load at which a winding slippage occurs is measured by the following method for measuring a magnetic tape cartridge. (a) It is determined by the following method in an environment with an ambient temperature of 23° C. and a relative humidity of 50%. (b) The magnetic tape cartridge to be measured is an unused magnetic tape cartridge that is not installed in a magnetic tape device. (c) The magnetic tape wound around the cartridge reel in the magnetic tape cartridge is temporarily taken out of the magnetic tape cartridge by winding it onto a temporary take-up reel. The magnetic tape is taken out by applying a tension of 0.30 N in the longitudinal direction of the magnetic tape. (d) After that, the magnetic tape wound on the temporary winding reel is rewound onto the cartridge reel with a tension of 0.30 N applied in the longitudinal direction of the magnetic tape, so that the entire length of the magnetic tape is wound again onto the cartridge reel and housed in the magnetic tape cartridge. (e) Thereafter, the cartridge reel on which the entire length of the magnetic tape is wound is removed from the magnetic tape cartridge. (f) For cartridge reels having flanges, the flanges are removed by cutting means to expose both tape winding surfaces on which the magnetic tape is wound. (g) The reel hub is then placed on the receiving platform. (h) Place an aluminum ring with an outer diameter of 90 mm and an inner diameter of 80 mm on the tape winding surface of the wound magnetic tape placed on the receiving table so that the center of rotation of the reel hub and the center of the aluminum ring are aligned. The "alignment" here is not limited to a perfect alignment, and a deviation of 3 mm or less is permitted. (i) On top of this aluminum ring, an aluminum plate having a square shape of 100 mm x 100 mm in plan view and a thickness of 3 mm is placed. (j) A load is applied from above the plate and maintained for 10 minutes, after which the load is removed. (k) The vertical position of the top surface of the plate before the load is applied is A, and the vertical position of the top surface of the plate after the load is removed is B. If "A-B ≧ 1 mm", it is determined that a miswinding has occurred in the wound magnetic tape. (l) For the same magnetic tape, the load is started from 5 N and increased in increments of 5 N while carrying out the above measurements, and the minimum load at which a winding slippage occurs is defined as the "minimum load at which a winding slippage occurs."
2. A magnetic tape cartridge as described in claim 1, wherein the non-magnetic support is a polyester support.
3. 3. The magnetic tape cartridge according to claim 2, wherein the magnetic tape further comprises a non-magnetic layer containing a non-magnetic powder between the non-magnetic support and the magnetic layer.
4. 4. The magnetic tape cartridge according to claim 1, wherein the magnetic tape has a thickness of 5.6 μm or less.
5. 5. The magnetic tape cartridge according to claim 1, wherein the magnetic tape has a thickness of 5.3 μm or less.
6. 6. The magnetic tape cartridge according to claim 1, wherein the minimum load required for generating a winding shear is 10N or more and 250N or less.
7. 7. The magnetic tape cartridge according to claim 1, wherein the squareness of the magnetic tape in the perpendicular direction is 0.60 or more.
8. The magnetic tape is run between the take-up reel and the cartridge reel of the magnetic tape cartridge under tension in the longitudinal direction of the magnetic tape, the maximum value of the tension being 0.50 N or more, and The magnetic tape cartridge according to any one of claims 1 to 7, which is used in a magnetic tape device that applies a tension of 0.30 N or less in the longitudinal direction of the magnetic tape to wind the magnetic tape, after it has been run under the tension, onto the cartridge reel.
9. A magnetic tape device comprising the magnetic tape cartridge according to any one of claims 1 to 8.
10. the magnetic tape cartridge; A take-up reel; Including, The magnetic tape is run between the take-up reel and the cartridge reel of the magnetic tape cartridge under tension in the longitudinal direction of the magnetic tape, the maximum value of the tension being 0.50 N or more; and 10. The magnetic tape device according to claim 9, wherein the magnetic tape after being run under said tension is wound around a cartridge reel of said magnetic tape cartridge under a tension of 0.30 N or less in the longitudinal direction of said magnetic tape.
11. 11. The magnetic tape device according to claim 10, wherein tension applied to the magnetic tape in the longitudinal direction is changed during the running.
Citation Information
Patent Citations
Magnetic recording medium
JP2002050030A
Tape cassette
JP2002133817A
Linear tape drive apparatus
JP2005285268A
Magnetic tape, magnetic tape cartridge, and magnetic record reproducer
JP2020140757A