Rubber resin material and metal substrate using same
A rubber resin composition with specific liquid rubber, polyphenylene ether resin, and surface-modified inorganic fillers addresses the challenge of high thermal conductivity and low dielectricity in high-frequency substrates, enhancing thermal and dielectric properties for 5G applications.
Patent Information
- Application Number
- JP2022163798
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-06-16
- Filing Date
- 2022-10-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-10-12
AI Technical Summary
Existing rubber resin materials face challenges in achieving high thermal conductivity and low dielectricity, particularly when used in high-frequency substrates for 5G applications, due to issues with liquid rubber content affecting glass transition temperature and peel strength, and thermally conductive fillers impacting heat resistance.
A rubber resin composition comprising 30% to 60% liquid rubber with a molecular weight of 2500g/mol to 6000g/mol, 10% to 40% polyphenylene ether resin, 10% to 40% crosslinking agent, and surface-modified inorganic fillers such as magnesium oxide, aluminum oxide, silicon oxide, zinc oxide, aluminum nitride, boron nitride, silicon carbide, or aluminum silicate, with specific functional groups, is used to enhance thermal conductivity and reduce dielectric properties.
The rubber resin material achieves thermal conductivity of 1.2 W/m·K or more, dielectric constant of 3.2 to 4.0, and dielectric loss tangent less than 0.0030, with improved peel strength and heat resistance, making it suitable for high-frequency substrates.
Smart Images

Figure 0007565989000002 
Figure 0007565989000003 
Figure 0007565989000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber-resin material and its application, and in particular to a rubber-resin material having high thermal conductivity and low dielectric constant and a metal substrate (for example, a copper clad laminate (CCL)) using the same. [Background technology]
[0002] 5th generation mobile communication system (5 th With the development of 5G (first generation wireless system), high frequency transmission has become the current mainstream of development in order to meet the 5G wireless communication standard. Therefore, the industry is working on developing high frequency board materials (e.g., in the frequency range of 6-77 GHz) suitable for high frequency transmission, so that the high frequency board can be applied to base station antennas, satellite radars, automotive radars, wireless communication antennas, or power amplifiers.
[0003] The dielectric constant (Dk) and dielectric dissipation factor (Df) directly affect the speed and quality of the transmission signal, so when applied to 5G, it is necessary to use materials with low dielectric constant and extremely low dielectric dissipation factor to improve signal delay and reduce signal transmission loss. In addition, when applied to 5G, thermal conductivity and heat resistance are also required. Hereinafter, the dielectric constant and dielectric dissipation factor of the high frequency board are collectively referred to as the dielectric properties of the high frequency board.
[0004] Currently available rubber resin materials contain a certain ratio of liquid rubber, which has the characteristics of high solubility and reactive functional groups. Thus, the rubber resin material is suitable for use as a high-frequency circuit board material. However, the amount of liquid rubber added must not be too high. If the liquid rubber content is too high (over 25% by weight), the glass transition temperature (Tg) of the rubber resin material will be relatively low, and the peel strength of the circuit board will be poor.
[0005] In addition, commercially available high thermal conductive resin materials contain a specific ratio of thermal conductive filler to improve the thermal conductivity of the resin material. The amount of thermal conductive filler added is more than 45 parts by weight and not more than 60 parts by weight per 100 parts by weight of resin, but an excessive amount of thermal conductive filler adversely affects the interfacial compatibility between the rubber resin material and the thermal conductive filler, affecting the heat resistance of the board and being disadvantageous for application as a high frequency board material. Summary of the Invention [Problem to be solved by the invention]
[0006] The technical problem that the present invention aims to solve is to provide a rubber-resin material having high thermal conductivity and low dielectric constant, and a metal substrate using the same, in response to the shortcomings of the conventional techniques. [Means for solving the problem]
[0007] In order to solve the above technical problems, one technical means adopted by the present invention provides a rubber resin material having high thermal conductivity and low dielectric constant. The rubber resin material includes a rubber resin composition and a surface-modified inorganic filler. The rubber resin composition includes 30% to 60% by weight of a liquid rubber having a molecular weight of 2500 g / mol to 6000 g / mol, 10% to 40% by weight of a polyphenylene ether resin, and 10% to 40% by weight of a crosslinking agent. The modifying functional group of the surface-modified inorganic filler is selected from the group consisting of an acrylic group, a functional group having nitrogen in the main chain or side chain, a functional group containing a double bond, and an epoxy group.
[0008] In one embodiment of the invention, the surface-modified inorganic filler is selected from the group consisting of magnesium oxide, aluminum oxide, silicon oxide, zinc oxide, aluminum nitride, boron nitride, silicon carbide and aluminum silicate and comprises said modifying functional group.
[0009] In one embodiment of the present invention, the monomers constituting the liquid rubber are selected from the group consisting of styrene monomers, butadiene monomers, divinylbenzene monomers and maleic anhydride monomers.
[0010] In one embodiment of the present invention, the proportion of vinyl groups in all the end groups of the liquid rubber is 30 mol% to 90 mol%, and the proportion of styrene groups in all the end groups of the liquid rubber is 10 mol% to 50 mol%.
[0011] In one embodiment of the present invention, 30% by weight to 90% by weight of the butadiene monomers is a butadiene monomer having a side chain containing a vinyl group, with the total weight of the butadiene monomers being 100% by weight.
[0012] In one embodiment of the present invention, the modifying functional group of the surface-modified inorganic filler comprises an acrylic group and a functional group having nitrogen in the main chain or side chain.
[0013] In one embodiment of the present invention, the amount of the surface-modified inorganic filler added is 20 parts by weight to 300 parts by weight based on 100 parts by weight of the rubber resin composition.
[0014] In one embodiment of the present invention, the surface-modified inorganic filler is present as particles, and the median diameter (D50) of the surface-modified inorganic filler is 0.3 μm to 0.6 μm.
[0015] In one embodiment of the present invention, the surface-modified inorganic filler further comprises a siloxane coupling agent having an acrylic and / or vinyl group.
[0016] In one embodiment of the present invention, the content of the siloxane coupling agent is 0.1 parts by weight to 5 parts by weight based on 100 parts by weight of the rubber resin composition.
[0017] In order to solve the above technical problem, another technical means adopted by the present invention provides a metal substrate. The metal substrate includes a base layer and a metal layer disposed on the base layer. The material of the base layer includes a rubber resin material having high thermal conductivity and low dielectric properties, which includes the above composition.
[0018] In one embodiment of the present invention, the thermal conductivity of the metal substrate is 1.2 W / m·K or more.
[0019] In one embodiment, the metal substrate has a relative dielectric constant of 3.2 to 4.0 at 10 GHz, and a dielectric loss tangent of the metal substrate at 10 GHz of less than 0.0030.
[0020] In one embodiment of the present invention, the peel strength of the metal substrate is 4.5 lb / in to 7.0 lb / in. Effect of the Invention
[0021] As an advantageous effect of the present invention, the rubber resin material and metal substrate having high thermal conductivity and low dielectric properties according to the present invention can achieve desired physical properties (e.g., thermal conductivity, dielectric properties, peel strength, heat resistance, etc.) when actually applied due to the technical features that "the rubber resin composition contains 30% by weight to 60% by weight of liquid rubber having a molecular weight of 2500 g / mol to 6000 g / mol, 10% by weight to 40% by weight of polyphenylene ether resin, and 10% by weight to 40% by weight of a crosslinking agent" and "the modifying functional group of the surface-modified inorganic filler is selected from the group consisting of an acrylic group, a functional group having nitrogen in the main chain or side chain, a functional group containing a double bond, and an epoxy group." [Brief description of the drawings]
[0022] [Figure 1] 1 is a schematic diagram showing a structure of a metal substrate according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing another structure of a metal substrate according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] In order to better understand the features and technical contents of the present invention, please refer to the following detailed description of the present invention and the accompanying drawings, which are provided for reference and explanation only and are not intended to limit the scope of the present invention.
[0024] Hereinafter, the embodiment of the "rubber resin material and metal substrate using the same" according to the present invention will be described by way of certain specific embodiments, and those skilled in the art can understand the advantages and effects of the present invention based on the contents disclosed in this specification. The present invention can be implemented or applied by other different specific embodiments, and various modifications and changes can be made to each detail in this specification based on different viewpoints and applications without departing from the concept of the present invention. In addition, as described in advance, the accompanying drawings of the present invention are simple schematic illustrations and are not drawn based on actual size. The technical contents of the present invention will be described in more detail based on the following embodiments, but the disclosed contents do not limit the scope of protection of the present invention. In addition, the term "or" used in this specification may include any one or more combinations of the items listed in relation to each other according to the actual situation.
[0025] [Rubber resin material with high thermal conductivity and low dielectric properties] The present invention provides a rubber-resin material with high thermal conductivity and low dielectric constant. The rubber-resin material is obtained by introducing a surface-modified inorganic filler into a rubber-resin system. As a result, the physical properties of the rubber-resin system (thermal conductivity, dielectric properties, etc.) meet the requirements for high frequency and high speed, and it can be used as a high frequency and high speed substrate material compared to conventional materials.
[0026] Specifically, the rubber resin material of the present invention includes a rubber resin composition and a surface-modified inorganic filler that is uniformly dispersed in the rubber resin composition. The rubber resin composition and the surface-modified inorganic filler will be described in detail later.
[0027] [Rubber resin composition] In the present invention, the rubber resin composition mainly contains 30 wt % to 60 wt % of liquid rubber, 10 wt % to 40 wt % of polyphenylene ether resin, and 10 wt % to 40 wt % of a crosslinking agent.
[0028] It is worth noting that when the molecular weight of the liquid rubber is 2500 g / mol to 6000 g / mol, the fluidity of the rubber resin composition is improved, and the effect of improving the filling property of the low dielectric substrate material can be achieved. The molecular weight of the liquid rubber is preferably 3000 g / mol to 5500 g / mol, and more preferably 3000 g / mol to 5000 g / mol. Since the liquid rubber has a high solubility property, it can improve the compatibility between each component, and since the liquid rubber has a reactive functional group, it can improve the degree of crosslinking after the rubber resin material is hardened.
[0029] In addition, since the liquid rubber has a specific molecular weight and a specific structure and constitutional units, it can be added in a larger amount to the rubber resin composition, that is, the content ratio of the liquid rubber in the rubber resin composition can be significantly increased. Specifically, the content of the liquid rubber can exceed 40% by weight, assuming the total weight of the rubber resin composition to be 100% by weight, which clearly exceeds the content of the liquid rubber in the rubber resin composition of the conventional technology (25% by weight). Preferably, the content of the liquid rubber in the rubber resin composition is 30% by weight to 60% by weight.
[0030] In one embodiment, the liquid rubber comprises a liquid diene-based rubber. More specifically, the liquid diene-based rubber comprises a polybutadiene resin. A polybutadiene resin is a polymer polymerized using butadiene monomer, such as a butadiene homopolymer or a copolymer of butadiene and other monomers.
[0031] In one preferred embodiment, the liquid diene rubber is a copolymer composed of butadiene and styrene. That is, the monomers constituting the liquid rubber include styrene and butadiene. The styrene monomer and the butadiene monomer can be arranged randomly to form a random copolymer, or they can be arranged regularly to form an alternating copolymer or a block copolymer.
[0032] The content of the styrene monomer is 10% to 50% by weight, with the total weight of the liquid rubber being 100% by weight. When the content of the styrene monomer in the liquid rubber is 10% to 50% by weight, the structure of the liquid rubber resembles the molecular geometric structure of the liquid crystal molecular arrangement, and the heat resistance and system compatibility can be improved. Preferably, the content of the styrene monomer in the liquid rubber is 15% to 50% by weight. When the content of the styrene monomer exceeds 50% by weight, the viscosity of the rubber resin material becomes disadvantageous for the production of a high thermal conductive metal substrate.
[0033] To explain further, butadiene itself has two double bonds, and therefore when polymerized, different structures are obtained depending on the polymerization method. That is, polybutadiene may be composed of any one or more structures among cis-1,4-polybutadiene, trans-1,4-polybutadiene, and 1,2-polybutadiene. To be more specific, when butadiene undergoes a 1,4-addition polymerization reaction, a cis-1,4-polybutadiene or trans-1,4-polybutadiene structure is produced. In the cis-1,4-polybutadiene or trans-1,4-polybutadiene structure, polybutadiene does not have an unsaturated side chain. When butadiene undergoes a 1,2-addition polymerization reaction, a 1,2-polybutadiene structure is produced. In the 1,2-polybutadiene structure, polybutadiene has an unsaturated side chain (vinyl group).
[0034] Preferably, 30 to 90% by weight of the butadiene monomer (after polymerization), based on 100% by weight of the total weight of the butadiene monomer, has a side chain containing a vinyl group. Preferably, 30 to 80% by weight of the butadiene monomer (after polymerization), based on 100% by weight of the total weight of the butadiene monomer, has a side chain containing a vinyl group.
[0035] When the liquid rubber has at least one side chain (or vinyl group) containing a vinyl group, the crosslink density and heat resistance of the crosslinked highly thermally conductive rubber-resin composition are improved. In the present invention, the unsaturated side chain (or vinyl group) containing a vinyl group in the liquid rubber can be quantified by the iodine value in chemical analysis. The higher the iodine value of the liquid rubber, the higher the content of the unsaturated side chain (or vinyl group) containing a vinyl group in the liquid rubber. The unsaturated side chain (or vinyl group) containing a vinyl group can improve the physical properties of the crosslinked rubber-resin composition. In the present invention, the iodine value of the liquid rubber is 30g / 100g to 60g / 100g.
[0036] The iodine value is measured by first taking 0.3mg to 1mg of liquid rubber, adding chloroform to completely dissolve the liquid rubber, adding Wijs solution and leaving it in the dark for 30 minutes. Next, add 20mL of potassium iodide (100g / L) and 100mL of water, then titrate with 0.1mol / L sodium thiosulfate solution. When the solution turns light yellow, add a few drops of starch solution (10g / L) and continue titrating until the blue color disappears.
[0037] In one embodiment of the present invention, the liquid diene rubber is a copolymer formed of butadiene monomer, styrene monomer, divinylbenzene monomer and maleic anhydride monomer. That is, the monomers constituting the liquid rubber include styrene monomer, butadiene monomer, divinylbenzene monomer and maleic anhydride monomer. The styrene monomer, butadiene monomer, divinylbenzene monomer and maleic anhydride monomer may be arranged regularly or randomly. The total amount of the butadiene monomer, the styrene monomer, the divinylbenzene monomer and the maleic anhydride monomer is taken as 100 mol%, and the content of the butadiene monomer may be 30 mol% to 90 mol%, the content of the styrene monomer may be 10 mol% to 50 mol%, the content of the divinylbenzene monomer may be 10 mol% to 40 mol%, and the content of the maleic anhydride monomer may be 2 mol% to 20 mol%.
[0038] The molecular weight of the polyphenylene ether resin is 1000 g / mol to 20000 g / mol, preferably 2000 g / mol to 10000 g / mol, and more preferably 2000 g / mol to 2200 g / mol. It is noteworthy that when the molecular weight of the polyphenylene ether resin is less than 20000 g / mol, it has better solubility, which is advantageous for producing a rubber resin composition.
[0039] Preferably, the polyphenylene ether resin may have at least one modifying group. The modifying group may be selected from the group consisting of hydroxyl, amino, vinyl, styrene, methacrylate and epoxy groups. The modifying group in the polyphenylene ether resin provides an unsaturated bond, which favors the progress of the crosslinking reaction, thereby forming a material with a high glass transition temperature and good heat resistance. In this embodiment, the two ends of the molecular structure of the polyphenylene ether each have a modifying group, and the two modifying groups are the same.
[0040] Preferably, the polyphenylene ether resin may contain a single type of polyphenylene ether, or may contain multiple types of polyphenylene ethers simultaneously.
[0041] For example, the polyphenylene ether resin may be a polyphenylene ether resin having product numbers SA90 (the modifying groups at the two ends are hydroxyl groups) or SA9000 (the modifying groups at the two ends are methacrylate groups) manufactured by SABIC, or a polyphenylene ether resin having product numbers OPE-2St (the modifying groups at the two ends are styrene groups), OPE-2EA (the modifying groups at the two ends are methacrylate groups), or OPE-2Gly (the modifying groups at the two ends are epoxy groups) manufactured by Mitsubishi Gas Chemical Company, Inc. (MGC), but the present invention is not limited thereto.
[0042] For example, the polyphenylene ether may be a polyphenylene ether in which the modifying groups at the two ends are hydroxyl groups, a polyphenylene ether in which the modifying groups at the two ends are methacrylate groups, a polyphenylene ether in which the modifying groups at the two ends are styrene groups, or a polyphenylene ether in which the modifying groups at the two ends are epoxy groups, but the present invention is not limited thereto.
[0043] In one embodiment, the polyphenylene ether resin may include a first polyphenylene ether and a second polyphenylene ether. The first polyphenylene ether and the second polyphenylene ether each have at least one modifying group at a molecular end thereof, the modifying group being selected from the group consisting of a hydroxyl group, an amino group, a vinyl group, a styrene group, a methacrylate group, and an epoxy group, and the modifying group of the first polyphenylene ether is different from the modifying group of the second polyphenylene ether. Specifically, the weight ratio of the first polyphenylene ether to the second polyphenylene ether is 0.5 to 1.5, preferably 0.75 to 1.25, and more preferably 1.
[0044] For example, the first polyphenylene ether and the second polyphenylene ether may independently be a polyphenylene ether having hydroxyl groups as modifying groups at the two ends, a polyphenylene ether having methacrylate groups as modifying groups at the two ends, a polyphenylene ether having styrene groups as modifying groups at the two ends, or a polyphenylene ether having epoxy groups as modifying groups at the two ends, but the invention is not limited thereto.
[0045] For example, the first polyphenylene ether resin and the second polyphenylene ether resin may independently be a polyphenylene ether resin having product numbers SA90 (the modifying groups at the two ends are hydroxyl groups) or SA9000 (the modifying groups at the two ends are methacrylate groups) manufactured by SABIC, or a polyphenylene ether resin having product numbers OPE-2St (the modifying groups at the two ends are styrene groups), OPE-2EA (the modifying groups at the two ends are methacrylate groups), or OPE-2Gly (the modifying groups at the two ends are epoxy groups) manufactured by Mitsubishi Gas Chemical Company, Inc. (MGC), but the present invention is not limited thereto.
[0046] The crosslinking agent of the present invention can improve the crosslinking degree between the polyphenylene ether resin and the liquid rubber. In this embodiment, the crosslinking agent may include an allyl group. For example, the crosslinking agent may be triallyl cyanurate (TAC), triallyl isocyanurate (TAIC), diallyl phthalate, divinylbenzene, triallyl trimellitate, or a combination thereof. Preferably, the crosslinking agent is triallyl isocyanurate, but the present invention is not limited thereto.
[0047] [Surface-modified inorganic filler] The addition of the surface-modified inorganic filler can improve the thermal conductivity of the rubber-resin material, and can maintain the relative dielectric constant and dielectric loss tangent of the rubber-resin material at a low level when actually applied. The above content is for explaining the function of the surface-modified inorganic filler, and the present invention is not limited thereto. When actually applied, the surface-modified inorganic filler has better bonding and compatibility with the copper foil and the resin. In addition, the surface-modified inorganic filler can achieve other advantageous effects, such as improving the heat resistance of the rubber-resin material, reducing the viscosity of the rubber-resin material, and improving the peeling strength of the copper foil substrate.
[0048] In the present invention, the surface-modified inorganic filler is selected from the group consisting of magnesium oxide (MgO), aluminum oxide (Al2O3), silicon oxide (SiO2), zinc oxide (ZnO), aluminum nitride (AlN), boron nitride (BN), silicon carbide (SiC) and aluminum silicate (Al2O3·SiO2). The surface-modified inorganic filler has a modifying functional group, that is, the surface is covered with a sufficient amount of the modifying functional group, but the present invention is not limited thereto. In one preferred embodiment, the surface-modified inorganic filler is composed of silicon oxide having a modifying functional group on its surface and boron nitride having a modifying functional group on its surface.
[0049] To explain further, the modifying functional group of the surface-modified inorganic filler is selected from the group consisting of an acrylic group, a functional group having nitrogen in the main chain or side chain, a functional group containing a double bond, and an epoxy group. Preferably, the modifying functional group of the surface-modified inorganic filler is an acrylic group, a functional group having nitrogen in the main chain or side chain, or a combination thereof. As a result, the surface-modified inorganic filler reacts with the liquid rubber to give good compatibility to the rubber resin composition and does not adversely affect the heat resistance of the high thermal conductive metal substrate. In addition, the surface-modified inorganic filler is added in a larger amount to the rubber resin composition, which can improve the upper limit of the inorganic filler added in the rubber resin composition of the conventional technology. Thus, the rubber resin material of the present invention is more suitable as a high-frequency substrate material.
[0050] In one embodiment, the surface-modified inorganic filler has a nitrogen-containing functional group in the main chain or side chain by being modified with a nitrogen-containing silane compound having a structure represented by the following formula (1). [ka]
[0051] It is worth noting that the surface-modified inorganic filler may be a single inorganic powder or a mixture of multiple inorganic powders. The surface-modified inorganic filler may be entirely or partially surface-treated. In a specific example where the surface-modified inorganic filler includes aluminum oxide and boron nitride, the aluminum oxide is surface-modified to have acrylic and / or vinyl groups, and the boron nitride is not surface-modified. The above are possible embodiments, but the present invention is not limited thereto.
[0052] In one preferred embodiment, the surface-modified inorganic filler simultaneously contains aluminum oxide, silicon oxide, and boron nitride, and the amount of aluminum oxide added is 50 to 120 parts by weight, the amount of silicon oxide added is 10 to 100 parts by weight, and the amount of boron nitride added is 30 to 80 parts by weight, relative to 100 parts by weight of the rubber resin composition.
[0053] In practical application, the surface modification method of inorganic fillers may be to impregnate them with silanes having specific functionality (e.g., silanes having vinyl groups or silanes having acrylic groups) to provide the inorganic fillers with acrylic and / or vinyl groups.
[0054] The amount of the surface-modified inorganic filler added can be adjusted according to the product specifications. In one embodiment, the content of the surface-modified inorganic filler may be 20 parts by weight to 250 parts by weight, preferably 100 parts by weight to 150 parts by weight, and more preferably 120 parts by weight to 130 parts by weight, relative to 100 parts by weight of the rubber resin composition. However, the above example is merely one embodiment, and the present invention is not limited thereto.
[0055] The surface-modified inorganic filler may have a particle or sheet-like appearance, and is preferably sheet-like. The median diameter (D50) of the surface-modified inorganic filler is 0.3 μm to 3 μm, and preferably 0.3 μm to 0.6 μm. This allows the surface-modified inorganic filler to be uniformly dispersed in the rubber resin composition, and the advantageous effects (particularly, thermal conductivity and low dielectric properties) are significantly improved. It should be noted that when the median diameter is within the above range, the inorganic filler has a large specific surface area, the effect of surface modification is significant, and the drilling ability of the metal substrate is improved.
[0056] [Siloxane coupling agents] The rubber-resin material of the present invention may further include a siloxane coupling agent. One end of the siloxane coupling agent is a silane end capable of bonding with inorganic matter, and the other end of the siloxane coupling agent has a functional group capable of bonding with rubber / resin. Thus, the addition of the siloxane coupling agent can improve the reactivity and compatibility between the fiber cloth, the high thermal conductive rubber-resin composition and the inorganic filler, and improve the peel strength and heat resistance of the metal substrate.
[0057] In one preferred embodiment, the siloxane coupling agent contains an acrylic group and / or a vinyl group, and the molecular weight of the siloxane coupling agent is 100 g / mol to 500 g / mol, preferably 110 g / mol to 250 g / mol, and more preferably 120 g / mol to 200 g / mol.
[0058] The content of the siloxane coupling agent is 0.1 to 5 parts by weight, and preferably 0.5 to 3 parts by weight, based on 100 parts by weight of the rubber resin composition.
[0059] [Flame retardant] The rubber resin material of the present invention may further include a flame retardant. The addition of the flame retardant can improve the flame retardancy of the high frequency substrate. For example, the flame retardant may be a phosphorus-based flame retardant or a bromine-based flame retardant. Preferably, the flame retardant is a halogen-free flame retardant, i.e., does not contain bromine.
[0060] The brominated flame retardant may be ethylene bis(tetrabromophthalimide), tetradecabromodiphenoxy benzene, decabromo diphenoxy oxide, or a combination thereof, but the present invention is not limited thereto.
[0061] The phosphorus-based flame retardant may be a sulphosuccinic acid ester, a phosphazene, an ammonium polyphosphate, a melamine polyphosphate, or a melamine cyanurate. Examples of the phosphorus-based flame retardant include triphenyl phosphate (TPP), tetraphenyl resorcinol bis(diphenylphosphate), RDP, bisphenol A bis(diphenyl phosphate), BPAPP, bisphenol A bis(dimethyl)phosphate (BBC), resorcinol diphosphate (e.g., CR-733S, manufactured by Daihachi Chemical Industry Co., Ltd.), and resorcinol bis(2,6-dimethylphenyl phosphate) (e.g., PX-200, manufactured by Daihachi Chemical Industry Co., Ltd.), but the present invention is not limited thereto.
[0062] The amount of the flame retardant added can be adjusted according to the product specifications. In one embodiment, the amount of the flame retardant added is 0.1 to 5 parts by weight based on 100 parts by weight of the rubber resin composition.
[0063] [Metal substrate] As shown in FIG. 1 and FIG. 2, the present invention further provides a metal substrate Z including a base layer 1 and at least one metal layer 2 disposed on the base layer 1. The material of the base layer 1 includes a rubber resin material having the above-mentioned composition ratio and having high thermal conductivity and low dielectric property. Specifically, the metal substrate Z may be a copper clad laminate (CCL). The metal layer 2 (copper foil layer) may be formed on one side (e.g., the upper surface) of the base layer 1 (the number of the metal layer 2 is only one). Alternatively, the metal layer 2 may be formed on both surfaces (e.g., the upper surface and the lower surface) of the base layer 1 (the number of the metal layers 2 is two).
[0064] Specifically, the relative dielectric constant (10 GHz) of the metal substrate Z is 3.2 to 4, preferably 3.3 to 3.9, and more preferably 3.4 to 3.8. The dielectric tangent (10 GHz) of the metal substrate Z is less than 0.0030, preferably less than 0.0025, and more preferably less than 0.0020. The thermal conductivity of the metal substrate Z is 1.2 W / m·K or more, preferably 1.3 W / m·K or more, and more preferably 1.4 W / m·K or more. The peel strength of the metal substrate Z is preferably 4.5 lb / in to 7.0 lb / in, and more preferably 5 lb / in to 7.0 lb / in.
[0065] The method for evaluating the characteristics of the metal substrate Z is as follows. (1) Dielectric constant (10 GHz): The dielectric constant at a frequency of 10 GHz is measured using a dielectric analyzer (product number: HP Agilent E5071C). (2) Dielectric loss tangent (10 GHz): The dielectric loss tangent at a frequency of 10 GHz is measured using a dielectric analyzer (product number: HP Agilent E5071C). (3) Peel strength: The peel strength of the copper foil substrate is measured based on the test method IPC-TM-650-2.4.8. (4) Thermal conductivity: The thermal conductivity of the copper foil substrate is measured based on the measurement method ASTM D5470.
[0066] [Advantageous Effects of the Embodiments] As an advantageous effect of the present invention, the rubber resin material and metal substrate having high thermal conductivity and low dielectric properties according to the present invention can achieve desired physical properties (e.g., thermal conductivity, dielectric properties, peel strength, heat resistance, etc.) when actually applied due to the technical features that "the rubber resin composition contains 30% by weight to 60% by weight of liquid rubber having a molecular weight of 2500 g / mol to 6000 g / mol, 10% by weight to 40% by weight of polyphenylene ether resin, and 10% by weight to 40% by weight of a crosslinking agent" and "the modifying functional group of the surface-modified inorganic filler is selected from the group consisting of an acrylic group, a functional group having nitrogen in the main chain or side chain, a functional group containing a double bond, and an epoxy group."
[0067] To further explain, the modified functional group of the surface-modified inorganic filler is selected from the group consisting of an acrylic group, a functional group having nitrogen in the main chain or side chain, a functional group containing a double bond, and an epoxy group. Preferably, the modified functional group of the surface-modified inorganic filler is an acrylic group, a functional group having nitrogen in the main chain or side chain, or a combination thereof. In this way, the addition of the surface-modified inorganic filler can improve the thermal conductivity of the rubber-resin material, and can maintain the relative dielectric constant and dielectric loss tangent of the rubber-resin material at a low level in practical application. In addition, the surface-modified inorganic filler has better bonding and compatibility with the copper foil and resin. In addition, the surface-modified inorganic filler can achieve other advantageous effects. For example, it can improve the heat resistance of the rubber-resin material, reduce the viscosity of the rubber-resin material, and improve the peeling strength of the copper foil substrate.
[0068] The above disclosure is merely a preferred embodiment of the present invention, and the scope of the claims of the present invention is not limited thereto. Therefore, all equivalent technical modifications made by utilizing the specification and drawings of the present invention are included in the scope of the claims of the present invention. [Explanation of symbols]
[0069] Z: Metal substrate 1...Base material layer 2…Metal layer
Claims
1. A rubber resin material comprising a rubber resin composition and a surface-modified inorganic filler, The amount of the surface-modified inorganic filler added is 20 parts by weight to 300 parts by weight based on 100 parts by weight of the rubber resin composition; The rubber resin composition comprises, where the total weight of the rubber resin composition is 100% by weight, 30% to 60% by weight of a liquid rubber having a molecular weight of 2500 g / mol to 6000 g / mol; 10% to 40% by weight of a polyphenylene ether resin; and 10% to 40% by weight of a crosslinking agent; The monomer constituting the liquid rubber is selected from the group consisting of styrene monomers, butadiene monomers, divinylbenzene monomers and maleic anhydride monomers; a ratio of vinyl groups to all end groups of the liquid rubber is 30 mol % to 90 mol %, a ratio of styrene groups to all end groups of the liquid rubber is 10 mol % to 50 mol %, The crosslinking agent comprises an allyl group, the polyphenylene ether resin has at least one modifying group selected from the group consisting of hydroxyl, amino, vinyl, styrene, methacrylate and epoxy groups; A rubber resin material, wherein the modifying functional group of the surface-modified inorganic filler is composed of an acrylic group and a functional group having nitrogen in the main chain or side chain.
2. 2. The rubber resin material according to claim 1, wherein the surface-modified inorganic filler is selected from the group consisting of magnesium oxide, aluminum oxide, silicon oxide, zinc oxide, aluminum nitride, boron nitride, silicon carbide and aluminum silicate and contains the modifying functional group.
3. 2. The rubber resin material according to claim 1, wherein 30% by weight to 90% by weight of the butadiene monomers is a butadiene monomer having a side chain containing a vinyl group, with the total weight of the butadiene monomers being 100% by weight.
4. The rubber resin material according to claim 1, wherein the surface-modified inorganic filler is present as particles, and the median diameter (D50) of the surface-modified inorganic filler is 0.3 μm to 0.6 μm.
5. The rubber resin material according to claim 1 , wherein the surface-modified inorganic filler further comprises a siloxane coupling agent having an acrylic group and / or a vinyl group.
6. The rubber resin material according to claim 5, wherein the content of the siloxane coupling agent is 0.1 to 5 parts by weight based on 100 parts by weight of the rubber resin composition.
7. A metal substrate comprising a base layer and a metal layer disposed on the base layer, The metal substrate, wherein the material of the base layer contains the rubber resin material according to claim 1.
8. The metal substrate according to claim 7 , having a thermal conductivity of 1.2 W / m·K or more.
9. The metal substrate according to claim 7, wherein the metal substrate has a relative dielectric constant of 3.2 to 4.0 at 10 GHz and a dielectric loss tangent of less than 0.0030 at 10 GHz.
10. 8. The metal substrate of claim 7, wherein the peel strength is from 0.51 N·m to 0.8 N·m (4.5 lb / in to 7.0 lb / in).
Citation Information
Patent Citations
New semi-IPN type composite material-containing thermosetting resin composition and varnish, prepreg and metal clad laminate using the same
JP2008133414A
Resin composition, resin layer-attached support, prepreg, laminate, multilayer printed board and printed wiring board for millimeter wave radar
JP2018012772A
Powder dispersion and laminate manufacturing method
JP2022011017A
Resin composition for high-frequency substrates, and metal laminate board
JP2022022090A
High frequency resin composition and use thereof
JP2022508173A