Magnetic recording medium and magnetic recording / reproducing device

The magnetic recording medium with an aromatic polyester support and controlled spacing difference addresses stability issues under environmental changes, ensuring consistent performance by minimizing moisture absorption and surface component changes.

JP7566184B2Active Publication Date: 2024-10-11FUJIFILM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024004346
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-01-16
Publication Date
2024-10-11
Estimated Expiration
2039-05-15

AI Technical Summary

Technical Problem

Magnetic recording media experience decreased running stability due to environmental changes, particularly when transitioning from high temperature to low temperature under low humidity, leading to instability in the contact state between the backcoat layer and drive components.

Method used

A magnetic recording medium with an aromatic polyester support having a moisture absorption rate of 0.3% or less, and a spacing difference between the backcoat layer before and after ethanol cleaning of greater than 0 nm and less than 15.0 nm, is designed to stabilize the running stability under such environmental changes.

Benefits of technology

The magnetic recording medium maintains stable running performance even after temperature and humidity changes, reducing the negative impact on contact stability with drive components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566184000001
    Figure 0007566184000001
  • Figure 0007566184000002
    Figure 0007566184000002
  • Figure 0007566184000003
    Figure 0007566184000003
Patent Text Reader

Abstract

To prevent a deterioration in running stability of a magnetic recording medium including an aromatic polyester support after a temperature change from a high temperature to a low temperature at a low humidity and further after being stored in a low-temperature and low-humidity environment.SOLUTION: The magnetic recording medium has a magnetic layer including a ferromagnetic powder on one surface of a non-magnetic support, and has a back coating layer including a non-magnetic powder on the other surface, in which a difference (Safter-Sbefore) between a spacing Safter measured by optical interferometry regarding a surface of the back coating layer after ethanol cleaning and a spacing Sbefore measured by the optical interferometry before the ethanol cleaning is greater than 0 nm and equal to or less than 15.0 nm, and the non-magnetic support is an aromatic polyester support having a moisture absorption of 0.3% or less. A magnetic recording and reproducing device comprises the magnetic recording medium.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a magnetic recording medium and a magnetic recording / reproducing device. [Background technology]

[0002] 2. Description of the Related Art Magnetic recording media (see, for example, Patent Document 1) are useful as data storage media for storing large amounts of data (information) for long periods of time. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 9-227883 Summary of the Invention [Problem to be solved by the invention]

[0004] Recording data on a magnetic recording medium and reproducing the recorded data are generally performed by mounting the magnetic recording medium in a magnetic recording and reproducing device (called a drive) and running the magnetic recording medium within the drive. In order to suppress the occurrence of errors during recording and reproducing, it is desirable to stabilize the running of the magnetic recording medium within the drive (improve running stability).

[0005] On the other hand, magnetic recording media used for data storage purposes may be used in data centers where temperature and humidity are controlled. On the other hand, data centers are required to save power in order to reduce costs. In order to save power, it is desirable to be able to relax the temperature and humidity management conditions in data centers from the current level, or to make management unnecessary. However, if the temperature and humidity management conditions are relaxed or not managed, it is expected that the magnetic recording media will be exposed to environmental changes due to weather changes, seasonal changes, and the like, or will be stored under various temperature and humidity environments. An example of the environmental change is a temperature change from high to low in low humidity. Also, an example of a temperature and humidity environment is a low temperature and low humidity environment. Therefore, it is desirable to be able to stabilize the running of the magnetic recording media in the drive even after such an environmental change and after storage in such a temperature and humidity environment.

[0006] Incidentally, magnetic recording media generally have a structure including a non-magnetic support and a magnetic layer containing ferromagnetic powder. Also, as described in claim 2 of JP-A-9-227883 (Patent Document 1), a backcoat layer is provided on the surface of the non-magnetic support of the magnetic recording medium opposite to the surface having the magnetic layer. Regarding the non-magnetic support, for example, paragraph 0062 of JP-A-9-227883 (Patent Document 1) lists various films that can be used as the non-magnetic support.

[0007] As a result of investigations by the present inventors regarding the above points, it has become clear that a phenomenon occurs in which the running stability of a magnetic recording medium that includes an aromatic polyester support as a non-magnetic support is reduced when the temperature is changed from high to low in a low-humidity environment and then the medium is stored in a low-temperature, low-humidity environment.

[0008] One aspect of the present invention aims to suppress a decrease in running stability in a magnetic recording medium including an aromatic polyester support after a temperature change from a high temperature to a low temperature under low humidity conditions and after storage in a low temperature and low humidity environment. [Means for solving the problem]

[0009] One aspect of the present invention is A magnetic recording medium having a magnetic layer containing ferromagnetic powder on one surface side of a non-magnetic support and a backcoat layer containing non-magnetic powder on the other surface side, The spacing S on the surface of the backcoat layer is measured by optical interferometry after washing with ethanol. after and the spacing S measured by optical interferometry on the surface of the backcoat layer before washing with ethanol. before Difference from (S after -S before ) (hereinafter, "the spacing difference before and after ethanol washing (S after -S before )" or simply "Diff(S after -S before ) is more than 0 nm and 15.0 nm or less, and the non-magnetic support is an aromatic polyester support having a moisture absorption rate of 0.3% or less; Regarding.

[0010] In one embodiment, the difference (S after -S before ) can be 1.0 nm or more and 15.0 nm or less.

[0011] In one embodiment, the difference (S after -S before ) can be 2.0 nm or more and 13.0 nm or less.

[0012] In one embodiment, the moisture absorption rate of the aromatic polyester support can be 0.1% or more and 0.3% or less.

[0013] In one embodiment, the magnetic recording medium can have a non-magnetic layer containing non-magnetic powder between the non-magnetic support and the magnetic layer.

[0014] In one embodiment, the magnetic recording medium can be a magnetic tape.

[0015] One aspect of the present invention relates to a magnetic recording and reproducing device including the above magnetic recording medium and a magnetic head. Effect of the Invention

[0016] According to one aspect of the present invention, it is possible to provide a magnetic recording medium which includes an aromatic polyester support and which exhibits little deterioration in running stability even when stored in a low-temperature, low-humidity environment after a temperature change from high to low temperature under low humidity conditions, and a magnetic recording and reproducing device which includes this magnetic recording medium. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] One aspect of the present invention is a magnetic recording medium having a magnetic layer containing ferromagnetic powder on one surface side of a non-magnetic support and a backcoat layer containing non-magnetic powder on the other surface side, after and the spacing S measured by optical interferometry on the surface of the backcoat layer before washing with ethanol. before Difference from (S after -S before ) is greater than 0 nm and not greater than 15.0 nm, and the non-magnetic support is an aromatic polyester support having a moisture absorption rate of 0.3% or less.

[0018] In the present invention and this specification, "ethanol cleaning" refers to immersing a sample piece cut out from a magnetic recording medium in ethanol (200 g) at a liquid temperature of 20 to 25°C and ultrasonically cleaning (ultrasonic output: 40 kHz) for 100 seconds. When the magnetic recording medium to be cleaned is a magnetic tape, a sample piece having a length of 5 cm is cut out and subjected to ethanol cleaning. The width of the magnetic tape and the width of the sample piece cut out from the magnetic tape are usually 1 / 2 inch. 1 inch = 0.0254 meters. For magnetic tapes with a width other than 1 / 2 inch, a sample piece having a length of 5 cm may be cut out and subjected to ethanol cleaning. When the magnetic recording medium to be cleaned is a magnetic disk, a sample piece having a size of 5 cm x 1.27 cm is cut out and subjected to ethanol cleaning. The measurement of the spacing after ethanol cleaning, which will be described in detail below, is performed after leaving the sample piece after ethanol cleaning in an environment at a temperature of 23°C and a relative humidity of 50% for 24 hours.

[0019] In the present invention and this specification, the "surface of the backcoat layer" of a magnetic recording medium is synonymous with the surface of the magnetic recording medium on the backcoat layer side.

[0020] In the present invention and this specification, the spacing measured by optical interference method on the surface of the backcoat layer of a magnetic recording medium is a value measured by the following method. A magnetic recording medium (more specifically, the sample piece described above; the same applies below) and a transparent plate-like member (e.g., a glass plate, etc.) are superimposed so that the backcoat layer surface of the magnetic recording medium faces the transparent plate-like member, and a pressing member is pressed from the side opposite the backcoat layer side of the magnetic recording medium with a pressure of 0.5 atm (1 atm = 101325 Pa (pascal)). In this state, light is irradiated onto the backcoat layer surface of the magnetic recording medium through the transparent plate-like member (irradiation area: 150,000 to 200,000 μm 2), the spacing (distance) between the backcoat layer surface of the magnetic recording medium and the magnetic recording medium side surface of the transparent plate-like member is obtained based on the intensity of the interference light (for example, the contrast of the interference fringe image) generated by the optical path difference between the reflected light from the backcoat layer surface of the magnetic recording medium and the reflected light from the magnetic recording medium side surface of the transparent plate-like member. The light irradiated here is not particularly limited. In the case where the irradiated light has an emission wavelength over a relatively wide wavelength range, such as white light containing light of multiple wavelengths, a member having a function of selectively cutting light of a specific wavelength or light other than a specific wavelength range, such as an interference filter, is disposed between the transparent plate-like member and the light receiving unit that receives the reflected light, and light of a part of the wavelengths or light of a part of the wavelength range of the reflected light is selectively made to enter the light receiving unit. In the case where the irradiated light is light having a single emission peak (so-called monochromatic light), the above member may not be used. The wavelength of the light incident on the light receiving unit can be, for example, in the range of 500 to 700 nm. However, the wavelength of the light incident on the light receiving unit is not limited to the above range. The transparent plate-like member may be any member having transparency that allows the light to pass therethrough to such an extent that interference light can be obtained by irradiating the magnetic recording medium with light through the member. The interference fringe image obtained by the above spacing measurement is divided into 300,000 points, and the spacing (the distance between the backcoat layer surface of the magnetic recording medium and the surface of the transparent plate-like member facing the magnetic recording medium) of each point is obtained and plotted as a histogram. The most frequent value in this histogram is taken as the spacing. after -S before ) refers to the value obtained by subtracting the most frequent value before ethanol washing from the most frequent value after ethanol washing at the above 300,000 points. Two sample pieces were cut out from the same magnetic recording medium, and one of them was cut at the spacing value S without being washed with ethanol. before The other one is washed with ethanol and the spacing value S after By calculating the difference (S after -S beforeAlternatively, the sample piece for which the spacing value was determined before the ethanol washing may be subjected to ethanol washing and then the spacing value may be determined, thereby obtaining the difference (S after -S before ) may be obtained. The above measurements can be performed using a commercially available tape spacing analyzer (TSA), such as the Tape Spacing Analyzer manufactured by Micro Physics Corp. The spacing measurements in the examples were performed using the Tape Spacing Analyzer manufactured by Micro Physics Corp.

[0021] In the present invention and this specification, "aromatic polyester" means a resin containing an aromatic skeleton and a plurality of ester bonds, and "aromatic polyester support" means a support containing at least one layer of aromatic polyester film. "Aromatic polyester film" means a film in which the component that constitutes this film in the largest proportion by mass is an aromatic polyester. The "aromatic polyester support" in the present invention and this specification includes a support in which all the resin films contained in this support are aromatic polyester films, and a support containing an aromatic polyester film and another resin film. Specific embodiments of the aromatic polyester support include a single-layer aromatic polyester film, a laminated film of two or more layers of aromatic polyester films having the same constituent components, a laminated film of two or more layers of aromatic polyester films having different constituent components, a laminated film containing one or more layers of aromatic polyester films and one or more layers of resin films other than aromatic polyesters, and the like. An adhesive layer or the like may be optionally included between two adjacent layers in the laminated film. In addition, the aromatic polyester support may optionally include a metal film and / or a metal oxide film formed by deposition or the like on one or both surfaces.

[0022] In the present invention and this specification, the moisture absorption rate of the aromatic polyester support is a value determined by the following method. A sample piece (e.g., a sample piece having a mass of several grams) cut out from an aromatic polyester support to be measured for moisture absorption is dried until it reaches a constant weight in a vacuum dryer at a temperature of 180°C and a pressure of 100 Pa or less. The mass of the sample piece thus dried is designated as W1. W1 is a value measured in a measurement environment at a temperature of 23°C and a relative humidity of 50% within 30 seconds after removal from the vacuum dryer. Next, the mass of the sample piece after being placed in an environment at a temperature of 25°C and a relative humidity of 75% for 48 hours is designated as W2. W2 is a value measured in a measurement environment at a temperature of 23°C and a relative humidity of 50% within 30 seconds after removal from the environment. The moisture absorption rate is calculated by the following formula. Moisture absorption rate (%)=[(W2-W1) / W1]×100 For example, after removing the portions other than the aromatic polyester support, such as the magnetic layer, from the magnetic recording medium by a known method (e.g., removal of the film using an organic solvent), the moisture absorption rate of the aromatic polyester support can be determined by the above method.

[0023] Below, the inventors' speculations will be described as to why the above-mentioned magnetic recording medium makes it possible to suppress the deterioration of running stability (hereinafter also referred to simply as "decrease in running stability") after a temperature change from high to low temperature under low humidity conditions and then after storage in a low temperature and low humidity environment.

[0024] Recording data on a magnetic tape and reproducing the recorded data are generally performed by running the magnetic recording medium in a drive. Usually, during such running, the surface of the backcoat layer comes into contact with drive components in the drive. If the contact state between the surface of the backcoat layer and the drive components becomes unstable, it is considered that the running stability of the magnetic recording medium in the drive will decrease. On the other hand, it is considered that organic components are easily exuded to the surface of the backcoat layer under low humidity and high temperature. It is also considered that when the temperature changes from high to low under low humidity, the organic components exuded to the surface of the backcoat layer solidify or become highly viscous. It is considered that such solidified or highly viscous organic components make the contact state between the surface of the backcoat layer and the drive components unstable when they come into contact with each other. Therefore, if the amount of organic components that solidify or become highly viscous when the temperature changes from high to low under low humidity can be reduced, it is considered that this leads to suppression of the deterioration of running stability. Meanwhile, the surface of the backcoat layer usually has a portion (protrusion) that is in main contact (so-called true contact) with the drive component when the backcoat layer surface comes into contact with the drive component, and a portion that is lower than this portion (hereinafter referred to as the "base portion"). The spacing described above is considered to be a value that serves as an index of the distance between the drive component and the base portion when the backcoat layer surface comes into contact with the drive component. However, if any component is present on the surface of the backcoat layer, the spacing is considered to become narrower the greater the amount of the above component present between the base portion and the drive component. On the other hand, when this component is removed by washing with ethanol, the spacing widens, so that the spacing S after ethanol washing is considered to be 100%. after The value of S before ethanol washing is before Therefore, the difference in the spacing before and after ethanol washing (S after -S before ) can be considered as an indicator of the amount of the above-mentioned components present between the substrate portion and the drive component. Regarding the above, the present inventor believes that the components removed by ethanol washing are organic components that solidify or become highly viscous on the surface of the backcoat layer due to the temperature change from high to low temperature under low humidity as described above. Therefore, the difference in the spacing before and after ethanol washing (S after -S beforeIt is believed that reducing the amount of the above-mentioned components leads to suppression of the deterioration of running stability caused by the temperature change from high to low temperature under low humidity conditions. In contrast, according to the inventor's investigation, no correlation was found between the difference in spacing before and after cleaning with a solvent other than ethanol, such as n-hexane, and the difference in spacing before and after cleaning with ethanol. This is presumably because the above-mentioned components cannot be removed or cannot be removed sufficiently by cleaning with n-hexane. The details of the above components are not clear. The inventors speculate that the above components are organic components and / or binder-derived components that are usually added to the backcoat layer as additives (e.g., lubricants). The inventors speculate that the binder-derived components are likely to be relatively low molecular weight components of the resin (which usually has a molecular weight distribution) used as the binder, which are likely to seep out to the backcoat layer surface under low humidity and high temperature conditions.

[0025] In addition, if the aromatic polyester support absorbs a large amount of moisture during storage in a low-temperature, low-humidity environment after the temperature change, the friction coefficient of the backcoat layer surface of the magnetic recording medium containing this support when it comes into contact with the drive components is thought to increase. This is thought to be one of the reasons for the deterioration of running stability after further storage in a low-temperature, low-humidity environment after the temperature change. In contrast, since the moisture absorption rate of the aromatic polyester support of the magnetic recording medium is 0.3% or less, the amount of moisture absorbed by the aromatic polyester support during storage is thought to be small. This is also thought to contribute to suppressing the deterioration of running stability.

[0026] However, the above is merely speculation and does not limit the present invention in any way. The above magnetic recording medium will be described in more detail below.

[0027] <Nonmagnetic support> The magnetic recording medium includes an aromatic polyester support having a moisture absorption rate of 0.3% or less as a non-magnetic support. From the viewpoint of suppressing a decrease in running stability, the moisture absorption rate of the aromatic polyester support is 0.3% or less, preferably 0.2% or less, and more preferably 0.1% or less. The moisture absorption rate of the aromatic polyester support can be, for example, 0% or more, more than 0%, or 0.1% or more. From the viewpoint of suppressing a decrease in running stability, it is preferable that the moisture absorption rate of the aromatic polyester support is low, so the moisture absorption rate can be 0%. In addition, using an aromatic polyester support having a low moisture absorption rate as a non-magnetic support of a magnetic recording medium is also preferable from the viewpoint of suppressing deformation of the magnetic recording medium after long-term storage. For example, it is preferable that a tape-shaped magnetic recording medium (magnetic tape) includes an aromatic polyester support having a low moisture absorption rate from the viewpoint of suppressing deformation of the magnetic tape in the tape width direction after long-term storage. In addition, in the magnetic tape, the Young's modulus of the aromatic polyester support in the longitudinal direction is 3000 N / mm 2 It is preferable that the resistance is 4000N / mm 2 From the viewpoint of increasing the capacity of the magnetic recording medium, the surface roughness of one or both surfaces of the aromatic polyester support is preferably 10 nm or less in terms of center line average roughness Ra.

[0028] The aromatic ring contained in the aromatic skeleton of the aromatic polyester is not particularly limited, but specific examples of the aromatic ring include a benzene ring and a naphthalene ring. For example, polyethylene terephthalate (PET) is a polyester containing a benzene ring, and is a resin obtained by polycondensation of ethylene glycol with terephthalic acid and / or dimethyl terephthalate. In the present invention and this specification, "polyethylene terephthalate" also includes structures having one or more other components (e.g., copolymerized components, components introduced into the terminal or side chain, etc.) in addition to the above components. Hereinafter, an aromatic polyester film containing polyethylene terephthalate as an aromatic polyester may be referred to as a polyethylene terephthalate film. Polyethylene naphthalate (PEN) is a polyester containing a naphthalene ring, and is a resin obtained by esterification of dimethyl 2,6-naphthalenedicarboxylate with ethylene glycol, followed by transesterification and polycondensation. In the present invention and this specification, "polyethylene naphthalate" also includes structures having one or more other components (e.g., copolymer components, components introduced into the terminal or side chain, etc.) in addition to the above components. Hereinafter, an aromatic polyester film containing polyethylene naphthalate as an aromatic polyester may be referred to as a polyethylene naphthalate film. The moisture absorption rate of the aromatic polyester support can be controlled, for example, by the type and ratio of the components constituting the aromatic polyester. For example, aromatic polyesters such as polyethylene terephthalate and polyethylene naphthalate can be resins synthesized using a hydrophobic component as a copolymerization component, and can also be those having a hydrophobic component introduced into the side chain and / or end. Examples of the hydrophobic component include a long-chain alkyl group-containing component and a fluorine-containing component. By containing a hydrophobic component in the aromatic polyester, the moisture absorption rate of the aromatic polyester film can be reduced, and by increasing the proportion of the hydrophobic component, the moisture absorption rate can be further reduced. As a means for reducing the moisture absorption rate of the aromatic polyester support, it is possible to reduce the moisture absorption rate of the aromatic polyester film in this way. In addition, when the aromatic polyester support is a laminated film of one or more layers of aromatic polyester film and one or more layers of other resin film, the moisture absorption rate of the aromatic polyester support can also be reduced by using a resin film with a low moisture absorption rate as the other resin film. As such an aromatic polyester support, for example, a laminated film described in JP-A-2011-84036 can be mentioned. For details of such a laminated film, reference can be made to paragraphs 0014 to 0061 of the publication and the description of the examples of the publication, etc. The aromatic polyester support may be a biaxially stretched film, or may be a film that has been subjected to corona discharge, plasma treatment, easy-adhesion treatment, heat treatment, etc.

[0029] <Magnetic layer> (Spacing difference before and after ethanol washing (S after -S before )) The spacing difference (S after -S before ) is greater than 0 nm and less than 15.0 nm. The difference (S after -S before ) of 15.0 nm or less can contribute to suppressing a decrease in the running stability of the magnetic recording medium. after -S before ) is 15.0 nm or less, preferably 14.0 nm or less, more preferably 13.0 nm or less, even more preferably 12.0 nm or less, even more preferably 11.0 nm or less, and even more preferably 10.0 nm or less. As will be described in detail later, the difference (S after -S before ) can be controlled by surface treatment of the backcoat layer during the manufacturing process of the magnetic recording medium. In addition, the spacing difference (S after -S before It is presumed that if the surface treatment of the backcoat layer is performed to such an extent that the spacing difference (S after -S before ) is greater than 0 nm, preferably 1.0 nm or more, and more preferably 2.0 nm or more.

[0030] (Ferromagnetic powder) As the ferromagnetic powder contained in the magnetic layer, one or more of the ferromagnetic powders known as ferromagnetic powders used in the magnetic layers of various magnetic recording media can be used in combination. It is preferable to use a ferromagnetic powder with a small average particle size from the viewpoint of improving recording density. From this viewpoint, the average particle size of the ferromagnetic powder is preferably 50 nm or less, more preferably 45 nm or less, even more preferably 40 nm or less, even more preferably 35 nm or less, even more preferably 30 nm or less, even more preferably 25 nm or less, and even more preferably 20 nm or less. On the other hand, from the viewpoint of magnetization stability, the average particle size of the ferromagnetic powder is preferably 5 nm or more, more preferably 8 nm or more, even more preferably 10 nm or more, even more preferably 15 nm or more, and even more preferably 20 nm or more.

[0031] Hexagonal Ferrite Powder A preferred specific example of the ferromagnetic powder is hexagonal ferrite powder. For details of the hexagonal ferrite powder, see, for example, JP2011-225417A, paragraphs 0012-0030, JP2011-216149A, paragraphs 0134-0136, JP2012-204726A, paragraphs 0013-0030, and JP2015-127985A, paragraphs 0029-0084.

[0032] In the present invention and this specification, the term "hexagonal ferrite powder" refers to a ferromagnetic powder in which a hexagonal ferrite type crystal structure is detected as the main phase by X-ray diffraction analysis. The main phase refers to a structure to which the most intense diffraction peak belongs in the X-ray diffraction spectrum obtained by X-ray diffraction analysis. For example, when the most intense diffraction peak in the X-ray diffraction spectrum obtained by X-ray diffraction analysis is assigned to a hexagonal ferrite type crystal structure, it is determined that the hexagonal ferrite type crystal structure has been detected as the main phase. When only a single structure is detected by X-ray diffraction analysis, the detected structure is regarded as the main phase. The hexagonal ferrite type crystal structure contains at least an iron atom, a divalent metal atom, and an oxygen atom as constituent atoms. The divalent metal atom is a metal atom that can become a divalent cation as an ion, and examples of such include alkaline earth metal atoms such as strontium atoms, barium atoms, and calcium atoms, and lead atoms. In the present invention and this specification, the hexagonal strontium ferrite powder refers to a powder in which the main divalent metal atom contained therein is a strontium atom, and the hexagonal barium ferrite powder refers to a powder in which the main divalent metal atom contained therein is a barium atom. The main divalent metal atom refers to the divalent metal atom that is the most abundant of the divalent metal atoms contained in the powder on an atomic % basis. However, the above divalent metal atoms do not include rare earth atoms. In the present invention and this specification, the "rare earth atom" is selected from the group consisting of scandium atoms (Sc), yttrium atoms (Y), and lanthanoid atoms. The lanthanide atom is selected from the group consisting of a lanthanum atom (La), a cerium atom (Ce), a praseodymium atom (Pr), a neodymium atom (Nd), a promethium atom (Pm), a samarium atom (Sm), a europium atom (Eu), a gadolinium atom (Gd), a terbium atom (Tb), a dysprosium atom (Dy), a holmium atom (Ho), an erbium atom (Er), a thulium atom (Tm), a ytterbium atom (Yb), and a lutetium atom (Lu).

[0033] Hereinafter, the hexagonal strontium ferrite powder, which is one embodiment of the hexagonal ferrite powder, will be described in further detail.

[0034] The activation volume of the hexagonal strontium ferrite powder is preferably 800 to 1600 nm 3 The finely divided hexagonal strontium ferrite powder exhibiting an activation volume in the above range is suitable for producing a magnetic recording medium exhibiting excellent electromagnetic conversion characteristics. The activation volume of the hexagonal strontium ferrite powder is preferably 800 nm 3 For example, 850 nm or more. 3 From the viewpoint of further improving the electromagnetic conversion characteristics, the activation volume of the hexagonal strontium ferrite powder can be 1500 nm or more. 3 More preferably, it is 1400 nm or less. 3 More preferably, it is 1300 nm or less. 3 More preferably, it is 1200 nm or less. 3 More preferably, it is equal to or less than 1100 nm. 3 It is even more preferable that the activation volume of the hexagonal barium ferrite powder is equal to or less than 1000 nm. The same is true for the activation volume of the hexagonal barium ferrite powder.

[0035] "Activation volume" is a unit of magnetization reversal and is an index showing the magnetic size of a particle. The activation volume and the anisotropy constant Ku described in the present invention and this specification are values ​​obtained by measuring the coercive force Hc measurement section at magnetic field sweep speeds of 3 minutes and 30 minutes (measurement temperature: 23°C ± 1°C) using a vibrating sample magnetometer, and calculating from the following relationship between Hc and activation volume V. The unit of the anisotropy constant Ku is 1 erg / cc = 1.0 x 10 -1 J / m 3 It is. Hc=2Ku / Ms{1-[(kT / KuV)ln(At / 0.693)] 1 / 2} [In the above formula, Ku: anisotropy constant (unit: J / m 3 ), Ms: saturation magnetization (unit: kA / m), k: Boltzmann constant, T: absolute temperature (unit: K), V: activation volume (unit: cm 3), A: spin precession frequency (unit: s -1 ), t: magnetic field reversal time (unit: s)]

[0036] The anisotropy constant Ku can be used as an index of reduction in thermal fluctuation, in other words, improvement in thermal stability. The hexagonal strontium ferrite powder is preferably 1.8×10 5 J / m 3 More preferably, the Ku is 2.0×10 or more. 5 J / m 3 The Ku of the hexagonal strontium ferrite powder can be, for example, 2.5×10 5 J / m 3 However, since a higher Ku value means higher thermal stability and is preferable, the Ku value is not limited to the above-mentioned values.

[0037] The hexagonal strontium ferrite powder may or may not contain rare earth atoms. When the hexagonal strontium ferrite powder contains rare earth atoms, it is preferable that the rare earth atoms are contained at a content (bulk content) of 0.5 to 5.0 atomic % relative to 100 atomic % of iron atoms. In one embodiment, the hexagonal strontium ferrite powder containing rare earth atoms can have uneven distribution of rare earth atoms in the surface layer portion. In the present invention and this specification, the term "surface distribution of rare earth atoms" refers to the rare earth atom content relative to 100 atomic % of iron atoms in a solution obtained by partially dissolving a hexagonal strontium ferrite powder in an acid (hereinafter referred to as "surface content of rare earth atoms" or simply "surface content" for rare earth atoms), which is greater than the rare earth atom content relative to 100 atomic % of iron atoms in a solution obtained by completely dissolving a hexagonal strontium ferrite powder in an acid (hereinafter referred to as "bulk content of rare earth atoms" or simply "bulk content" for rare earth atoms), Rare earth atom surface content / rare earth atom bulk content>1.0 The rare earth atom content of the hexagonal strontium ferrite powder described later is synonymous with the rare earth atom bulk content. In contrast, partial dissolution using an acid dissolves the surface layer of the particles constituting the hexagonal strontium ferrite powder, so the rare earth atom content in the solution obtained by partial dissolution is the rare earth atom content in the surface layer of the particles constituting the hexagonal strontium ferrite powder. The rare earth atom surface layer content satisfying the ratio of "rare earth atom surface layer content / rare earth atom bulk content>1.0" means that the rare earth atoms are unevenly distributed (i.e., more present in the surface layer) in the particles constituting the hexagonal strontium ferrite powder. In the present invention and this specification, the surface layer refers to a portion of the region extending from the surface of the particles constituting the hexagonal strontium ferrite powder toward the inside.

[0038] When the hexagonal strontium ferrite powder contains rare earth atoms, the rare earth atom content (bulk content) is preferably in the range of 0.5 to 5.0 atomic % relative to 100 atomic % of iron atoms. It is considered that the rare earth atoms contained in the bulk content in the above range and the rare earth atoms unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder contribute to suppressing the decrease in the reproduction output during repeated reproduction. This is presumed to be because the hexagonal strontium ferrite powder contains rare earth atoms in the bulk content in the above range and the rare earth atoms unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder can increase the anisotropy constant Ku. The higher the value of the anisotropy constant Ku, the more the occurrence of a phenomenon called thermal fluctuation can be suppressed (in other words, the thermal stability can be improved). By suppressing the occurrence of thermal fluctuation, the decrease in the reproduction output during repeated reproduction can be suppressed. It is speculated that the uneven distribution of rare earth atoms in the surface layer of hexagonal strontium ferrite powder particles contributes to stabilizing the spin of the iron (Fe) sites in the crystal lattice of the surface layer, thereby increasing the anisotropy constant Ku. In addition, it is presumed that using the hexagonal strontium ferrite powder having rare earth atom uneven distribution on the surface as the ferromagnetic powder of the magnetic layer also contributes to suppressing the wear of the magnetic layer surface due to sliding with the magnetic head. That is, it is presumed that the hexagonal strontium ferrite powder having rare earth atom uneven distribution on the surface can also contribute to improving the running durability of the magnetic recording medium. This is presumed to be because the uneven distribution of rare earth atoms on the surface of the particles constituting the hexagonal strontium ferrite powder contributes to improving the interaction between the particle surface and the organic substance (e.g., binder and / or additive) contained in the magnetic layer, and as a result, the strength of the magnetic layer is improved. From the viewpoint of further suppressing the decrease in regeneration output during repeated regeneration and / or further improving running durability, the rare earth atom content (bulk content) is more preferably in the range of 0.5 to 4.5 atomic %, even more preferably in the range of 1.0 to 4.5 atomic %, and even more preferably in the range of 1.5 to 4.5 atomic %.

[0039] The bulk content is the content obtained by completely dissolving the hexagonal strontium ferrite powder. In the present invention and this specification, unless otherwise specified, the content of an atom refers to the bulk content obtained by completely dissolving the hexagonal strontium ferrite powder. The hexagonal strontium ferrite powder containing rare earth atoms may contain only one rare earth atom as a rare earth atom, or may contain two or more rare earth atoms. The bulk content when containing two or more rare earth atoms is obtained for the total of two or more rare earth atoms. This point is the same for other components in the present invention and this specification. That is, unless otherwise specified, a certain component may be used in only one type or in two or more types. When two or more types are used, the content or content refers to the total of two or more types.

[0040] When the hexagonal strontium ferrite powder contains rare earth atoms, the rare earth atoms contained therein may be any one or more of rare earth atoms. From the viewpoint of further suppressing the decrease in the reproduction output during repeated reproduction, preferred rare earth atoms include neodymium atoms, samarium atoms, yttrium atoms and dysprosium atoms, more preferred are neodymium atoms, samarium atoms and yttrium atoms, and even more preferred are neodymium atoms.

[0041] In the hexagonal strontium ferrite powder having rare earth atom uneven distribution in the surface layer, the rare earth atoms may be unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder, and the degree of uneven distribution is not limited. For example, for the hexagonal strontium ferrite powder having rare earth atom uneven distribution in the surface layer, the ratio of the surface content of rare earth atoms obtained by partial dissolution under the dissolution conditions described below to the bulk content of rare earth atoms obtained by complete dissolution under the dissolution conditions described below, "surface content / bulk content", is more than 1.0 and can be 1.5 or more. The "surface content / bulk content" being greater than 1.0 means that the rare earth atoms are unevenly distributed in the surface layer (i.e., more than in the interior) in the particles constituting the hexagonal strontium ferrite powder. In addition, the ratio of the surface layer content of rare earth atoms obtained by partial dissolution under the dissolution conditions described later to the bulk content of rare earth atoms obtained by total dissolution under the dissolution conditions described later, "surface layer content / bulk content", can be, for example, 10.0 or less, 9.0 or less, 8.0 or less, 7.0 or less, 6.0 or less, 5.0 or less, or 4.0 or less. However, in a hexagonal strontium ferrite powder having rare earth atom surface layer uneven distribution, it is sufficient that the rare earth atoms are unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder, and the above "surface layer content / bulk content" is not limited to the upper or lower limit exemplified.

[0042] The partial and total dissolution of hexagonal strontium ferrite powder will be described below. For hexagonal strontium ferrite powder present as powder, the sample powders to be partially and completely dissolved are taken from the same lot of powder. On the other hand, for hexagonal strontium ferrite powder contained in the magnetic layer of a magnetic recording medium, a part of the hexagonal strontium ferrite powder taken out of the magnetic layer is subjected to partial dissolution, and the other part is subjected to total dissolution. The hexagonal strontium ferrite powder can be taken out of the magnetic layer by, for example, the method described in paragraph 0032 of JP 2015-91747 A. The above-mentioned partial dissolution means that the hexagonal strontium ferrite powder is dissolved to such an extent that the remaining powder can be visually confirmed in the liquid at the end of dissolution. For example, the partial dissolution can dissolve a region of 10 to 20 mass% of the particles constituting the hexagonal strontium ferrite powder, with the whole particles being 100 mass%. On the other hand, the above-mentioned complete dissolution means that the hexagonal strontium ferrite powder is dissolved to such an extent that the remaining powder cannot be visually confirmed in the liquid at the end of dissolution. The partial dissolution and the surface layer content are measured, for example, by the following method. Note that the dissolution conditions such as the amount of sample powder are merely examples, and any dissolution conditions that allow partial or complete dissolution can be used. A container (e.g., a beaker) containing 12 mg of sample powder and 10 mL of 1 mol / L hydrochloric acid is placed on a hot plate set at 70°C for 1 hour. The resulting solution is filtered through a 0.1 μm membrane filter. Elemental analysis of the filtrate thus obtained is performed using an inductively coupled plasma (ICP) analyzer. In this way, the surface layer content of rare earth atoms relative to 100 atomic % of iron atoms can be determined. When multiple types of rare earth atoms are detected by elemental analysis, the total content of all rare earth atoms is taken as the surface layer content. This is also true for the measurement of bulk content. On the other hand, the total dissolved and bulk contents are measured, for example, by the following method. A container (e.g., a beaker) containing 12 mg of sample powder and 10 mL of 4 mol / L hydrochloric acid is placed on a hot plate set at 80° C. for 3 hours. After that, the bulk content relative to 100 atomic % of iron atoms can be calculated by carrying out the same procedure as the partial dissolution and surface layer content measurement described above.

[0043] From the viewpoint of increasing the reproduction output when reproducing data recorded on a magnetic recording medium, it is desirable that the mass magnetization σs of the ferromagnetic powder contained in the magnetic recording medium is high. In this regard, hexagonal strontium ferrite powder that contains rare earth atoms but does not have uneven distribution of rare earth atoms in the surface layer tends to have a significantly lower σs than hexagonal strontium ferrite powder that does not contain rare earth atoms. In contrast, hexagonal strontium ferrite powder that has uneven distribution of rare earth atoms in the surface layer is considered preferable in terms of suppressing such a large decrease in σs. In one embodiment, the σs of the hexagonal strontium ferrite powder is 45 A·m 2 / kg or more, and 47A·m 2 / kg or more. On the other hand, from the viewpoint of noise reduction, σs is 80A·m 2 / kg or less, and 60A·m 2 / kg or less. σs can be measured using a known measuring device capable of measuring magnetic properties, such as a vibrating sample magnetometer. In the present invention and this specification, unless otherwise specified, the mass magnetization σs is a value measured at a magnetic field strength of 15 kOe. 1 kOe=(10 6 / 4π) A / m.

[0044] Regarding the content (bulk content) of the constituent atoms of the hexagonal strontium ferrite powder, the strontium atom content can be, for example, in the range of 2.0 to 15.0 atomic % relative to 100 atomic % of iron atoms. In one embodiment, the divalent metal atoms contained in the hexagonal strontium ferrite powder can be only strontium atoms. In another embodiment, the hexagonal strontium ferrite powder can also contain one or more other divalent metal atoms in addition to strontium atoms. For example, it can contain barium atoms and / or calcium atoms. When divalent metal atoms other than strontium atoms are contained, the barium atom content and calcium atom content in the hexagonal strontium ferrite powder can each be, for example, in the range of 0.05 to 5.0 atomic % relative to 100 atomic % of iron atoms.

[0045] Known crystal structures of hexagonal ferrite include magnetoplumbite type (also called "M type"), W type, Y type, and Z type. The hexagonal strontium ferrite powder may have any of the crystal structures. The crystal structure can be confirmed by X-ray diffraction analysis. The hexagonal strontium ferrite powder may be one in which a single crystal structure or two or more types of crystal structures are detected by X-ray diffraction analysis. For example, in one embodiment, the hexagonal strontium ferrite powder may be one in which only the M-type crystal structure is detected by X-ray diffraction analysis. For example, the M-type hexagonal ferrite is AFe 12 O 19Here, A represents a divalent metal atom, and when the hexagonal strontium ferrite powder is of the M type, A is only a strontium atom (Sr), or when A contains a plurality of divalent metal atoms, the strontium atom (Sr) accounts for the largest proportion on an atomic % basis as described above. The divalent metal atom content of the hexagonal strontium ferrite powder is usually determined by the type of crystal structure of the hexagonal ferrite, and is not particularly limited. The same applies to the iron atom content and the oxygen atom content. The hexagonal strontium ferrite powder contains at least an iron atom, a strontium atom, and an oxygen atom, and may further contain a rare earth atom. Furthermore, the hexagonal strontium ferrite powder may or may not contain atoms other than these atoms. As an example, the hexagonal strontium ferrite powder may contain an aluminum atom (Al). The content of aluminum atoms can be, for example, 0.5 to 10.0 atomic % relative to 100 atomic % of iron atoms. From the viewpoint of further suppressing the decrease in the reproduction output during repeated reproduction, the hexagonal strontium ferrite powder contains iron atoms, strontium atoms, oxygen atoms, and rare earth atoms, and the content of atoms other than these atoms is preferably 10.0 atomic % or less, more preferably in the range of 0 to 5.0 atomic %, relative to 100 atomic % of iron atoms, and may be 0 atomic %. That is, in one embodiment, the hexagonal strontium ferrite powder may not contain atoms other than iron atoms, strontium atoms, oxygen atoms, and rare earth atoms. The content expressed in atomic % above is obtained by converting the content (unit: mass %) of each atom obtained by completely dissolving the hexagonal strontium ferrite powder into a value expressed in atomic % using the atomic weight of each atom. In addition, in the present invention and this specification, "not containing" a certain atom means that the content measured by an ICP analyzer after completely dissolving is 0 mass %. The detection limit of an ICP analyzer is usually 0.01 ppm (parts per million) or less on a mass basis. The above term "free" is used to mean that the content is below the detection limit of the ICP analyzer.In one embodiment, the hexagonal strontium ferrite powder may be free of bismuth atoms (Bi).

[0046] metal powder A specific preferred example of the ferromagnetic powder is a ferromagnetic metal powder. For details of the ferromagnetic metal powder, reference can be made to, for example, paragraphs 0137 to 0141 of JP 2011-216149 A and paragraphs 0009 to 0023 of JP 2005-251351 A.

[0047] ε-iron oxide powder A preferred specific example of the ferromagnetic powder is ε-iron oxide powder. In the present invention and this specification, the term "ε-iron oxide powder" refers to a ferromagnetic powder in which an ε-iron oxide type crystal structure is detected as the main phase by X-ray diffraction analysis. For example, when the highest intensity diffraction peak in the X-ray diffraction spectrum obtained by X-ray diffraction analysis is attributed to an ε-iron oxide type crystal structure, it is determined that the ε-iron oxide type crystal structure is detected as the main phase. Known methods for producing ε-iron oxide powder include a method of producing it from goethite and a reverse micelle method. All of the above production methods are publicly known. In addition, for a method for producing ε-iron oxide powder in which a part of Fe is replaced by a substitution atom such as Ga, Co, Ti, Al, or Rh, reference can be made to, for example, J. Jpn. Soc. Powder Metallurgy Vol. 61 Supplement, No. S1, pp. S280-S284, J. Mater. Chem. C, 2013, 1, pp.5200-5206, etc. However, the method for producing the ε-iron oxide powder that can be used as the ferromagnetic powder in the magnetic layer of the magnetic recording medium is not limited to the method given here.

[0048] The activation volume of the ε-iron oxide powder is preferably 300 to 1500 nm 3 The finely divided ε-iron oxide powder exhibiting an activation volume in the above range is suitable for producing a magnetic recording medium exhibiting excellent electromagnetic conversion characteristics. The activation volume of the ε-iron oxide powder is preferably 300 nm 3For example, 500 nm or more. 3 From the viewpoint of further improving the electromagnetic conversion characteristics, the activation volume of the ε-iron oxide powder can be 1400 nm or more. 3 More preferably, it is 1300 nm or less. 3 More preferably, it is 1200 nm or less. 3 More preferably, it is equal to or less than 1100 nm. 3 It is even more preferred that:

[0049] The anisotropy constant Ku can be used as an index of the reduction in thermal fluctuation, in other words, the improvement in thermal stability. The ε-iron oxide powder is preferably 3.0×10 4 J / m 3 More preferably, the Ku is 8.0×10 or more. 4 J / m 3 The Ku of the ε-iron oxide powder can be, for example, 3.0×10 5 J / m 3 However, since a higher Ku value means higher thermal stability and is preferable, the Ku value is not limited to the above-mentioned values.

[0050] From the viewpoint of increasing the reproduction output when reproducing data recorded on the magnetic recording medium, it is desirable that the mass magnetization σs of the ferromagnetic powder contained in the magnetic recording medium is high. In this regard, in one embodiment, the σs of the ε-iron oxide powder is 8 A m 2 / kg or more, and can be 12 A m 2 On the other hand, the σs of ε-iron oxide powder is 40 A m 2 / kg or less, and 35A·m 2 It is more preferable that the amount is not more than 1 / kg.

[0051] In the present invention and this specification, unless otherwise specified, the average particle size of various powders such as ferromagnetic powders is a value measured by the following method using a transmission electron microscope. The powder is photographed at a magnification of 100,000 times using a transmission electron microscope, and a photograph of the particles that make up the powder is obtained by printing it on photographic paper or displaying it on a display so that the total magnification is 500,000 times. From the obtained particle photograph, the target particle is selected, and the particle outline is traced with a digitizer to measure the particle (primary particle) size. Primary particles are independent particles that are not aggregated. The above measurements are carried out for 500 randomly selected particles. The arithmetic mean of the particle sizes of the 500 particles thus obtained is the average particle size of the powder. As the transmission electron microscope, for example, a Hitachi transmission electron microscope H-9000 type can be used. The particle size can be measured using a known image analysis software, for example, Carl Zeiss image analysis software KS-400. The average particle size shown in the examples described below is a value measured using a Hitachi transmission electron microscope H-9000 type as the transmission electron microscope and Carl Zeiss image analysis software KS-400 as the image analysis software, unless otherwise specified. In the present invention and this specification, powder means a collection of multiple particles. For example, ferromagnetic powder means a collection of multiple ferromagnetic particles. In addition, the collection of multiple particles is not limited to a form in which the particles constituting the collection are in direct contact with each other, and also includes a form in which a binder, additive, etc., described later, are interposed between the particles. The term particle is sometimes used to refer to powder.

[0052] As a method for collecting a sample powder from a magnetic recording medium for particle size measurement, for example, the method described in paragraph 0015 of JP 2011-048878 A can be used.

[0053] In the present invention and this specification, unless otherwise specified, the size of the particles constituting the powder (particle size) is determined by the shape of the particles observed in the particle photograph. (1) In the case of needle-shaped, spindle-shaped, columnar (where the height is greater than the maximum major axis of the base), etc., it is expressed by the length of the major axis that constitutes the particle, i.e., the major axis length. (2) In the case of a plate or columnar shape (where the thickness or height is smaller than the maximum long diameter of the plate or base), it shall be expressed by the maximum long diameter of the plate or base. (3) In the case of a particle having a spherical, polyhedral, or unspecified shape, and the major axis of the particle cannot be specified from its shape, the particle is expressed as the equivalent circle diameter, which is determined by the circle projection method.

[0054] The average acicular ratio of a powder refers to the arithmetic average of the short axis length of the particles, i.e., the short axis length, the (long axis length / short axis length) value of each particle, and the values ​​obtained for the 500 particles. Here, unless otherwise specified, the short axis length refers to the length of the short axis constituting the particle in the above definition of particle size (1), and to the thickness or height in the above definition of particle size (2), and in the above definition of particle size (3), since there is no distinction between the long axis and the short axis, (long axis length / short axis length) is considered to be 1 for the sake of convenience. Unless otherwise specified, when the particle shape is specific, for example, in the case of the above definition of particle size (1), the average particle size is the average major axis length, in the case of definition (2), the average particle size is the average plate diameter, and in the case of definition (3), the average particle size is the average diameter (also called the average particle diameter or average particle size).

[0055] The content (filling rate) of the ferromagnetic powder in the magnetic layer is preferably in the range of 50 to 90 mass %, and more preferably in the range of 60 to 90 mass %. A high filling rate of the ferromagnetic powder in the magnetic layer is preferable from the viewpoint of improving recording density.

[0056] (Binding agent, hardener) The magnetic recording medium may be a coating type magnetic recording medium, and may contain a binder in the magnetic layer. The binder is one or more kinds of resin. As the binder, various resins that are usually used as binders for coating type magnetic recording media may be used. For example, as the binder, a resin selected from polyurethane resin, polyester resin, polyamide resin, vinyl chloride resin, acrylic resin copolymerized with styrene, acrylonitrile, methyl methacrylate, etc., cellulose resin such as nitrocellulose, epoxy resin, phenoxy resin, polyvinyl acetal, polyvinyl butyral, etc. may be used alone or in combination of a plurality of resins. Among these, polyurethane resin, acrylic resin, cellulose resin, and vinyl chloride resin are preferred. These resins may be homopolymers or copolymers. These resins may also be used as binders in the backcoat layer and / or the non-magnetic layer described later. For the above binders, for example, paragraphs 0028 to 0031 of JP-A-2010-24113 can be referred to. The content of the binder in the magnetic layer can be, for example, 1.0 to 30.0 parts by mass with respect to 100.0 parts by mass of the ferromagnetic powder. The average molecular weight of the resin used as the binder can be, for example, 10,000 to 200,000 in weight average molecular weight. The weight average molecular weight in the present invention and this specification is a value obtained by converting a value measured by gel permeation chromatography (GPC) under the following measurement conditions into a polystyrene equivalent. The weight average molecular weight of the binder shown in the examples described later is a value obtained by converting a value measured under the following measurement conditions into a polystyrene equivalent. GPC equipment: HLC-8120 (Tosoh Corporation) Column: TSK gel Multipore HXL-M (Tosoh Corporation, 7.8 mm ID (inner diameter) × 30.0 cm) Eluent: tetrahydrofuran (THF)

[0057] A curing agent can also be used together with the resin usable as a binder. In one embodiment, the curing agent can be a thermosetting compound that undergoes a curing reaction (crosslinking reaction) by heating, and in another embodiment, the curing agent can be a photocuring compound that undergoes a curing reaction (crosslinking reaction) by irradiation with light. The curing agent can be included in the magnetic layer in a state where at least a part of the curing agent reacts (crosslinks) with other components such as the binder as the curing reaction proceeds during the magnetic layer forming process. This point is also true for layers formed using a composition used to form other layers that contains a curing agent. A preferred curing agent is a thermosetting compound, and polyisocyanate is suitable. For details about polyisocyanate, refer to paragraphs 0124 to 0125 of JP 2011-216149 A. The curing agent can be used in an amount of, for example, 0 to 80.0 parts by mass relative to 100.0 parts by mass of the binder, and preferably 50.0 to 80.0 parts by mass from the viewpoint of improving the strength of the magnetic layer.

[0058] The above description of the binder and hardener can also be applied to the backcoat layer and / or the non-magnetic layer. In that case, the above description of the content can be applied by replacing the ferromagnetic powder with the non-magnetic powder. Spacing difference (S after -S before From the viewpoint of reducing the spacing difference (S) between before and after ethanol washing, it is preferable to reduce the amount of components derived from the binder that seep out to the surface of the backcoat layer under low humidity and high temperature conditions. after -S before ) can be cited as one way to reduce

[0059] (Additives) The magnetic layer may contain one or more additives as necessary. An example of the additive is the curing agent. Examples of the additives contained in the magnetic layer include non-magnetic powders (e.g., inorganic powders, carbon black, etc.), lubricants, dispersants, dispersion aids, antifungal agents, antistatic agents, antioxidants, etc. Examples of the non-magnetic powders include non-magnetic powders that can function as abrasives, and non-magnetic powders (e.g., non-magnetic colloidal particles, etc.) that can function as protrusion-forming agents that form protrusions that protrude appropriately on the magnetic layer surface. The average particle size of colloidal silica (silica colloidal particles) shown in the examples described below is a value obtained by the method described as the method for measuring the average particle size in paragraph 0015 of JP-A-2011-048878. The additives can be appropriately selected from commercially available products according to the desired properties, or can be manufactured by a known method, and can be used in any amount. As an example of an additive that can be used in the magnetic layer containing an abrasive, the dispersant described in paragraphs 0012 to 0022 of JP 2013-131285 A can be mentioned as a dispersant for improving the dispersibility of the abrasive. For example, for the lubricant, refer to paragraphs 0030 to 0033, 0035 and 0036 of JP 2016-126817 A. The non-magnetic layer may contain a lubricant. For the lubricant that can be contained in the non-magnetic layer, refer to paragraphs 0030, 0031, 0034, 0035 and 0036 of JP 2016-126817 A. For the dispersant, refer to paragraphs 0061 and 0071 of JP 2012-133837 A. For details about dispersants, see paragraphs 0061 and 0071 of JP2012-133837A and paragraph 0035 of JP2017-016721A. For details about additives in the magnetic layer, see paragraphs 0035 to 0077 of JP2016-51493A. The dispersant may be contained in the non-magnetic layer. For details about dispersants that may be contained in the non-magnetic layer, see paragraph 0061 of JP2012-133837A. The various additives can be appropriately selected from commercially available products according to the desired properties, or can be produced by known methods and used in any amount.

[0060] The magnetic layer described above can be provided directly on the surface of the non-magnetic support, or indirectly via a non-magnetic layer.

[0061] <Nonmagnetic layer> Next, the non-magnetic layer will be described. The magnetic recording medium may have a magnetic layer directly on the non-magnetic support, or may have a non-magnetic layer containing a non-magnetic powder between the non-magnetic support and the magnetic layer. The non-magnetic powder used in the non-magnetic layer may be a powder of an inorganic substance or a powder of an organic substance. Carbon black and the like can also be used. Examples of inorganic substances include metals, metal oxides, metal carbonates, metal sulfates, metal nitrides, metal carbides, and metal sulfides. These non-magnetic powders are commercially available, and can also be produced by known methods. For details, refer to paragraphs 0146 to 0150 of JP-A-2011-216149. For carbon black usable in the non-magnetic layer, refer to paragraphs 0040 to 0041 of JP-A-2010-24113. The content (filling rate) of the non-magnetic powder in the non-magnetic layer is preferably in the range of 50 to 90% by mass, more preferably in the range of 60 to 90% by mass.

[0062] The non-magnetic layer may contain a binder and may also contain an additive. For other details of the binder, additive, etc. of the non-magnetic layer, known techniques related to non-magnetic layers can be applied. In addition, for example, for the type and content of the binder, the type and content of the additive, known techniques related to magnetic layers can also be applied.

[0063] In the present invention and this specification, the nonmagnetic layer also includes a substantially nonmagnetic layer that contains a small amount of ferromagnetic powder, for example as an impurity or intentionally, together with the nonmagnetic powder. Here, the substantially nonmagnetic layer refers to a layer having a residual magnetic flux density of 10 mT or less, a coercive force of 100 Oe or less, or a layer having a residual magnetic flux density of 10 mT or less and a coercive force of 100 Oe or less. It is preferable that the nonmagnetic layer has no residual magnetic flux density or coercive force.

[0064] <Backcoat layer> The magnetic recording medium has a backcoat layer containing a nonmagnetic powder on the surface side opposite to the surface side having the magnetic layer of the nonmagnetic support. For the type of nonmagnetic powder contained in the backcoat layer, the description regarding the nonmagnetic powder contained in the nonmagnetic layer can be referred to. The nonmagnetic powder contained in the backcoat layer can be one or more types of nonmagnetic powder selected from the group consisting of inorganic powder and carbon black. The magnetic recording medium can contain, for example, an inorganic powder as the main powder of the nonmagnetic powder of the backcoat layer (the nonmagnetic powder contained in the largest amount by mass among the nonmagnetic powders). When the nonmagnetic powder contained in the backcoat layer is one or more types of nonmagnetic powder selected from the group consisting of inorganic powder and carbon black, the proportion of the inorganic powder relative to the total amount of the nonmagnetic powder (100.0 parts by mass) can be, for example, in the range of more than 50.0 parts by mass to 100.0 parts by mass, and is preferably in the range of 60.0 parts by mass to 100.0 parts by mass. When the proportion of the inorganic powder in the nonmagnetic powder is increased, the difference ( after -S before ) tends to become smaller.

[0065] The average particle size of the nonmagnetic powder may be, for example, in the range of 10 to 200 nm. The average particle size of the inorganic powder is preferably in the range of 50 to 200 nm, more preferably in the range of 80 to 150 nm. On the other hand, the average particle size of the carbon black is preferably in the range of 10 to 50 nm, more preferably in the range of 15 to 30 nm.

[0066] The backcoat layer may contain a binder and may also contain additives, such as known dispersants that can contribute to improving the dispersibility of non-magnetic powder.

[0067] Another example of the additive is a lubricant. For example, the lubricant may include fatty acids, fatty acid esters, and fatty acid amides, and the magnetic layer may be formed using one or more selected from the group consisting of fatty acids, fatty acid esters, and fatty acid amides. Examples of fatty acids include lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, behenic acid, erucic acid, elaidic acid, etc., with stearic acid, myristic acid, and palmitic acid being preferred, and stearic acid being more preferred. The fatty acid may be contained in the magnetic layer in the form of a salt such as a metal salt. Examples of fatty acid esters include esters of lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, behenic acid, erucic acid, elaidic acid, etc. Specific examples include butyl myristate, butyl palmitate, butyl stearate, neopentyl glycol dioleate, sorbitan monostearate, sorbitan distearate, sorbitan tristearate, oleyl oleate, isocetyl stearate, isotridecyl stearate, octyl stearate, isooctyl stearate, amyl stearate, butoxyethyl stearate, etc. Examples of the fatty acid amide include amides of the above-mentioned various fatty acids, such as lauric acid amide, myristic acid amide, palmitic acid amide, and stearic acid amide. The fatty acid content of the backcoat layer is, for example, 0 to 10.0 parts by mass, preferably 0.1 to 10.0 parts by mass, and more preferably 1.0 to 7.0 parts by mass per 100.0 parts by mass of the nonmagnetic powder contained in the backcoat layer. The fatty acid ester content of the backcoat layer is, for example, 0.1 to 10.0 parts by mass, and preferably 1.0 to 5.0 parts by mass per 100.0 parts by mass of the nonmagnetic powder contained in the backcoat layer. The fatty acid amide content of the backcoat layer is, for example, 0 to 3.0 parts by mass, preferably 0 to 2.0 parts by mass, and more preferably 0 to 1.0 parts by mass per 100.0 parts by mass of the nonmagnetic powder contained in the backcoat layer. In the present invention and this specification, unless otherwise specified, a certain component may be used alone or in combination of two or more. When two or more components are used, the content refers to the total content of these two or more components.

[0068] For the binder, additives, etc. of the backcoat layer, known techniques related to the backcoat layer can be applied, and known techniques related to the formulation of the magnetic layer and / or nonmagnetic layer can also be applied. For example, the descriptions of the backcoat layer can be found in paragraphs 0018 to 0020 of JP2006-331625A and in column 4, line 65 to column 5, line 38 of US7029774.

[0069] <Various thicknesses> The thickness of the non-magnetic support of the magnetic recording medium is, for example, 3.0 to 80.0 μm, preferably 3.0 to 50.0 μm, and more preferably 3.0 to 10.0 μm. The thickness of the non-magnetic support means the thickness of this film when the non-magnetic support is made of only a single-layer aromatic polyester film, and means the total thickness of the non-magnetic support in other cases.

[0070] The thickness of the magnetic layer can be optimized depending on the saturation magnetization amount and head gap length of the magnetic head used, and the band of the recording signal, and is, for example, 10 nm to 100 nm, and from the viewpoint of high density recording, is preferably in the range of 20 to 90 nm, and more preferably in the range of 30 to 70 nm. At least one magnetic layer is sufficient, and the magnetic layer may be separated into two or more layers having different magnetic properties, and a known configuration related to a multilayer magnetic layer can be applied. When the magnetic layer is separated into two or more layers, the thickness of the magnetic layer is the total thickness of these layers.

[0071] The thickness of the nonmagnetic layer is, for example, 50 nm or more, preferably 70 nm or more, and more preferably 100 nm or more, while the thickness of the nonmagnetic layer is preferably 800 nm or less, and more preferably 500 nm or less.

[0072] The thickness of the backcoat layer is preferably 0.9 μm or less, and more preferably in the range of 0.1 to 0.7 μm.

[0073] The thickness of each layer of the magnetic recording medium and the non-magnetic support can be determined by a known film thickness measurement method. For example, the cross section of the magnetic recording medium in the thickness direction is exposed by a known method such as ion beam or microtome, and then the exposed cross section is observed by a scanning electron microscope. Various thicknesses can be determined as the thickness determined at any one point in the cross section observation, or the arithmetic average of the thicknesses determined at two or more randomly selected points, for example, two points. Alternatively, the thickness of each layer may be determined as a design thickness calculated from the manufacturing conditions.

[0074] <Manufacturing method> (Preparation of compositions for forming each layer) The compositions for forming the magnetic layer, backcoat layer, and non-magnetic layer usually contain a solvent in addition to the various components described above. As the solvent, various organic solvents generally used for manufacturing coating-type magnetic recording media can be used. The amount of solvent in each layer-forming composition is not particularly limited, and can be the same as that of each layer-forming composition of a normal coating-type magnetic recording medium. The process for preparing the composition for forming each layer usually includes at least a kneading process, a dispersing process, and a mixing process provided before or after these processes as necessary. Each individual process may be divided into two or more stages. The various components used for forming each layer may be added at the beginning or during any process. Also, each component may be added in two or more steps in separate steps.

[0075] In order to prepare each layer-forming composition, a known technique can be used. In the kneading step, it is preferable to use a kneader having a strong kneading force, such as an open kneader, a continuous kneader, a pressure kneader, or an extruder. Details of these kneading processes are described in JP-A-1-106338 and JP-A-1-79274. In addition, in order to disperse each layer-forming composition, one or more types of dispersion beads selected from the group consisting of glass beads and other dispersion beads can be used as a dispersion medium. As such dispersion beads, zirconia beads, titania beads, and steel beads, which are dispersion beads with high specific gravity, are suitable. The particle size (bead diameter) and packing rate of these dispersion beads can be optimized for use. A known dispersing machine can be used. Each layer-forming composition may be filtered by a known method before being subjected to the coating step. Filtration can be performed, for example, by filter filtration. As the filter used for filtration, for example, a filter with a pore size of 0.01 to 3 μm (for example, a glass fiber filter, a polypropylene filter, etc.) can be used.

[0076] (coating process) The magnetic layer can be formed, for example, by directly applying the magnetic layer-forming composition onto the non-magnetic support, or by successively or simultaneously applying the magnetic layer-forming composition and the non-magnetic layer-forming composition in a multilayer manner. The backcoat layer can be formed by applying the backcoat layer-forming composition to the side of the non-magnetic support opposite to the side having the magnetic layer (or the side on which the magnetic layer will be provided later). For details of the coating for forming each layer, refer to paragraph 0051 of JP2010-24113A.

[0077] (Other processes) After the coating step, various treatments such as drying, orientation of the magnetic layer, and surface smoothing (calendering) can be performed. For the various steps, refer to paragraphs 0052 to 0057 of JP 2010-24113 A. For example, vertical orientation can be performed by a known method such as a method using magnets with different poles facing each other. In the orientation zone, the drying speed of the coating layer can be controlled by the temperature and volume of the drying air and / or the transport speed in the orientation zone. In addition, the coating layer may be pre-dried before being transported to the orientation zone.

[0078] At any stage after the coating process of the backcoat layer forming composition, it is preferable to perform a heat treatment of the coating layer formed by coating the backcoat layer forming composition. As an example, this heat treatment can be performed before and / or after the calendar treatment. For example, the heat treatment can be performed by placing the support on which the coating layer of the backcoat layer forming composition is formed in a heated atmosphere. The heated atmosphere can be an atmosphere with an atmosphere temperature of 65 to 90°C, and more preferably an atmosphere with an atmosphere temperature of 65 to 75°C. This atmosphere can be, for example, an air atmosphere. The heat treatment in the heated atmosphere can be performed for, for example, 20 to 50 hours. In one embodiment, this heat treatment can promote the curing reaction of the curable functional group of the curing agent.

[0079] (One aspect of the manufacturing method) As an embodiment of the method for producing the magnetic recording medium, a production method including wiping the surface of the backcoat layer with a wiping material soaked with alcohol, preferably after the heat treatment (hereinafter also referred to as "alcohol wiping treatment"). The components that can be removed by this alcohol wiping treatment seep out onto the surface of the backcoat layer under low humidity and high temperature conditions, and solidify or become highly viscous on the surface of the backcoat layer due to a temperature change from high temperature to low temperature, as described above, is considered to be the cause of the decrease in running stability caused by a temperature change from high temperature to low temperature under low humidity. The alcohol used in the alcohol wiping treatment is preferably an alcohol having 2 to 4 carbon atoms, more preferably ethanol, 1-propanol and 2-propanol, and even more preferably ethanol. The alcohol wiping treatment can be carried out using a wiping material soaked with alcohol instead of the wiping material used in the dry wiping treatment, in accordance with the dry wiping treatment generally carried out in the manufacturing process of the magnetic recording medium. For example, for a tape-shaped magnetic recording medium (magnetic tape), after or before slitting the magnetic tape to a width to be housed in a magnetic tape cartridge, the magnetic tape is run between a feed roller and a take-up roller, and a wiping material (e.g., cloth (e.g., nonwoven fabric) or paper (e.g., tissue paper)) soaked with alcohol is pressed against the surface of the backcoat layer of the running magnetic tape, thereby performing an alcohol wiping process on the surface of the backcoat layer. The running speed of the magnetic tape during the above running and the tension applied in the longitudinal direction of the backcoat layer surface (hereinafter simply referred to as "tension") can be the same as the processing conditions generally adopted in the dry wiping process generally carried out in the manufacturing process of the magnetic recording medium. For example, the running speed of the magnetic tape in the alcohol wiping process can be about 60 to 600 m / min, and the tension can be about 0.196 to 3.920 N (Newtons). The alcohol wiping process can be carried out at least once. The spacing difference (S after -S beforeIt is preferable to set the treatment conditions and the number of treatments for the alcohol wiping treatment so that the average particle size distribution is more than 0 nm and 15.0 nm or less. In addition, before and / or after the alcohol wiping treatment, the surface of the backcoat layer may be subjected to one or more polishing treatments and / or dry wiping treatments (hereinafter, these will be referred to as "dry surface treatments") that are generally performed in the manufacturing process of coating-type magnetic recording media. The dry surface treatment can remove foreign matter that is generated during the manufacturing process and adheres to the surface of the backcoat layer, such as cutting chips generated by slits. The above description has been given taking a tape-shaped magnetic recording medium (magnetic tape) as an example, but the various processes can also be carried out for a disk-shaped magnetic recording medium (magnetic disk) by referring to the above description.

[0080] The magnetic recording medium according to one embodiment of the present invention described above is a magnetic recording medium including an aromatic polyester support, and can be a magnetic recording medium in which the running stability is less deteriorated even when stored in a low-temperature, low-humidity environment after a temperature change from high to low in a low-humidity environment. The temperature change from high to low in a low-humidity environment can be, for example, a temperature change from a high temperature of 30°C to 50°C in an environment with a relative humidity of 0% to 30% to a low temperature of more than 0°C to 15°C. Storage in a low-temperature, low-humidity environment can be, for example, storage in an environment with a temperature of more than 0°C to 15°C and a relative humidity of 0 to 30%.

[0081] The magnetic recording medium may be, for example, a tape-shaped magnetic recording medium (magnetic tape). Magnetic tapes are usually distributed and used in a magnetic tape cartridge. The magnetic tape cartridge is mounted on a magnetic recording and reproducing device, and the magnetic tape is run in the magnetic recording and reproducing device to bring the magnetic tape surface (magnetic layer surface) into contact with and slide against a magnetic head, thereby recording and reproducing data on the magnetic tape. However, the magnetic recording medium according to one embodiment of the present invention is not limited to a magnetic tape. The magnetic recording medium according to one embodiment of the present invention is suitable as various magnetic recording media (magnetic tape, disk-shaped magnetic recording medium (magnetic disk), etc.) used in a sliding type magnetic recording and reproducing device. The sliding type device refers to a device in which the magnetic layer surface and the head come into contact and slide when recording data on the magnetic recording medium and / or reproducing the recorded data.

[0082] In the magnetic recording medium manufactured as described above, a servo pattern can be formed by a known method in order to enable tracking control of a magnetic head in a magnetic recording and reproducing device, control of the running speed of the magnetic recording medium, and the like. "Formation of a servo pattern" can also be called "recording of a servo signal." The magnetic recording medium may be a tape-shaped magnetic recording medium (magnetic tape) or a disk-shaped magnetic recording medium (magnetic disk). The formation of a servo pattern will be described below using a magnetic tape as an example.

[0083] The servo pattern is usually formed along the longitudinal direction of the magnetic tape. Control methods that use servo signals (servo control) include timing-based servo (TBS), amplitude servo, and frequency servo.

[0084] As shown in ECMA (European Computer Manufacturers Association)-319, magnetic tapes (generally called "LTO tapes") conforming to the LTO (Linear Tape-Open) standard employ a timing-based servo system. In this timing-based servo system, a servo pattern is formed by a pair of non-parallel magnetic stripes (also called "servo stripes") arranged continuously in the longitudinal direction of the magnetic tape. As described above, the reason why the servo pattern is formed by a pair of non-parallel magnetic stripes is to inform the servo signal reading element passing over the servo pattern of its passing position. Specifically, the pair of magnetic stripes is formed so that the interval between them changes continuously along the width direction of the magnetic tape, and the servo signal reading element can know the relative position between the servo pattern and the servo signal reading element by reading the interval. This relative position information enables tracking of the data track. For this purpose, a plurality of servo tracks are usually set on the servo pattern along the width direction of the magnetic tape.

[0085] A servo band is made up of a series of servo signals along the length of the magnetic tape. Usually, multiple servo bands are provided on a magnetic tape. For example, there are five servo bands on an LTO tape. The area between two adjacent servo bands is called a data band. A data band is made up of multiple data tracks, and each data track corresponds to one servo track.

[0086] Also, in one embodiment, as shown in JP 2004-318983 A, information indicating the number of the servo band (also called "servo band ID (identification)" or "UDIM (Unique Data Band Identification Method) information") is embedded in each servo band. This servo band ID is recorded by shifting a specific one of a plurality of pairs of servo stripes in the servo band so that its position is displaced relatively in the longitudinal direction of the magnetic tape. Specifically, the way in which a specific one of a plurality of pairs of servo stripes is shifted is changed for each servo band. As a result, the recorded servo band ID is unique for each servo band, so that the servo band can be uniquely identified simply by reading one servo band with a servo signal reading element.

[0087] As a method for uniquely identifying servo bands, there is also a method using the staggered method as specified in ECMA-319. In this staggered method, a group of pairs of non-parallel magnetic stripes (servo stripes) arranged continuously in the longitudinal direction of the magnetic tape are recorded so that they are shifted in the longitudinal direction of the magnetic tape for each servo band. Since the combination of the shift between adjacent servo bands is unique across the entire magnetic tape, it is possible to uniquely identify the servo bands when reading the servo pattern with two servo signal reading elements.

[0088] Also, as specified in ECMA-319, information indicating the longitudinal position of the magnetic tape (also called "LPOS (Longitudinal Position) information") is usually embedded in each servo band. Like UDIM information, this LPOS information is also recorded by shifting the positions of a pair of servo stripes in the longitudinal direction of the magnetic tape. However, unlike UDIM information, the same signal is recorded in each servo band with this LPOS information.

[0089] It is also possible to embed information other than the above UDIM information and LPOS information in the servo bands. In this case, the embedded information may be different for each servo band, such as UDIM information, or may be common to all servo bands, such as LPOS information. Also, methods other than those described above can be used to embed information in the servo bands. For example, a predetermined code may be recorded by thinning out a predetermined pair from a group of pairs of servo stripes.

[0090] The head for forming a servo pattern is called a servo write head. The servo write head has a pair of gaps corresponding to the pair of magnetic stripes, the number of which is equal to the number of servo bands. Usually, a core and a coil are connected to each pair of gaps, and a magnetic field generated in the core can generate a leakage magnetic field in the pair of gaps by supplying a current pulse to the coil. When forming a servo pattern, a magnetic pattern corresponding to the pair of gaps can be transferred to the magnetic tape by inputting a current pulse while running the magnetic tape on the servo write head, thereby forming the servo pattern. The width of each gap can be appropriately set according to the density of the servo pattern to be formed. The width of each gap can be set, for example, to 1 μm or less, 1 to 10 μm, or 10 μm or more.

[0091] Before forming a servo pattern on the magnetic tape, the magnetic tape is usually subjected to a demagnetization (erase) process. This erase process can be performed by applying a uniform magnetic field to the magnetic tape using a direct current magnet or an alternating current magnet. There are two types of erase processes: DC (Direct Current) erase and AC (Alternating Current) erase. AC erase is performed by gradually lowering the strength of the magnetic field applied to the magnetic tape while reversing the direction of the magnetic field. On the other hand, DC erase is performed by applying a unidirectional magnetic field to the magnetic tape. There are two more methods of DC erase. The first method is horizontal DC erase, which applies a unidirectional magnetic field along the longitudinal direction of the magnetic tape. The second method is vertical DC erase, which applies a unidirectional magnetic field along the thickness direction of the magnetic tape. The erase process may be performed on the entire magnetic tape, or may be performed for each servo band of the magnetic tape.

[0092] The direction of the magnetic field of the formed servo pattern is determined according to the direction of erasure. For example, when the magnetic tape is subjected to horizontal DC erasure, the servo pattern is formed so that the direction of the magnetic field is opposite to the direction of erasure. This makes it possible to increase the output of the servo signal obtained by reading the servo pattern. As shown in JP2012-53940A, when the magnetic pattern is transferred to the magnetic tape that has been vertically DC erased using the above gap, the servo signal obtained by reading the formed servo pattern has a unipolar pulse shape. On the other hand, when the magnetic pattern is transferred to the magnetic tape that has been horizontally DC erased using the above gap, the servo signal obtained by reading the formed servo pattern has a bipolar pulse shape.

[0093] [Magnetic recording and playback device] One aspect of the present invention relates to a magnetic recording and reproducing device including the above magnetic recording medium and a magnetic head.

[0094] In the present invention and this specification, the term "magnetic recording and reproducing device" refers to a device capable of at least one of recording data to a magnetic recording medium and reproducing data recorded on the magnetic recording medium. Such a device is generally called a drive. The magnetic recording and reproducing device may be a sliding type magnetic recording and reproducing device. The magnetic head included in the magnetic recording and reproducing device may be a recording head capable of recording data to a magnetic recording medium, and may be a reproducing head capable of reproducing data recorded on the magnetic recording medium. In one aspect, the magnetic recording and reproducing device may include both a recording head and a reproducing head as separate magnetic heads. In another aspect, the magnetic head included in the magnetic recording and reproducing device may have a configuration in which both a recording element and a reproducing element are provided in one magnetic head. As the reproducing head, a magnetic head (MR head) including a magnetoresistive (MR) element capable of reading data recorded on a magnetic recording medium with good sensitivity as a reproducing element is preferable. As the MR head, various known MR heads can be used. In addition, the magnetic head that records and / or reproduces data may include a servo pattern reading element. Alternatively, the magnetic recording and reproducing device may include a magnetic head (servo head) equipped with a servo pattern reading element as a separate head from the magnetic head that records and / or reproduces data.

[0095] In the magnetic recording and reproducing device, data can be recorded on the magnetic recording medium and data recorded on the magnetic recording medium can be reproduced by contacting and sliding the magnetic head against the magnetic layer surface of the magnetic recording medium. The magnetic recording and reproducing device may include the magnetic recording medium according to one aspect of the present invention, and other known techniques may be applied. EXAMPLES

[0096] The present invention will be described below based on examples. However, the present invention is not limited to the embodiments shown in the examples. In addition, the indications of "parts" and "%" in the following mean "parts by mass" and "% by mass" unless otherwise specified. eq is an equivalent weight, and is a unit that cannot be converted into SI units. In addition, the steps and evaluations described below were carried out in an environment with an atmospheric temperature of 23°C ± 1°C unless otherwise specified.

[0097] [Example 1] The formulation of each layer-forming composition is shown below.

[0098] <Formulation of the composition for forming the magnetic layer> (Magnetic liquid) Ferromagnetic powder (see Table 1): 100.0 parts Oleic acid: 2.0 parts Vinyl chloride copolymer (Kaneka MR-104): 10.0 parts SO3Na group-containing polyurethane resin: 4.0 parts (Weight average molecular weight: 70000, SO3Na group: 0.07meq / g) Polyalkyleneimine polymer (a synthetic product obtained by the method described in paragraphs 0115 to 0123 of JP 2016-51493 A): 6.0 parts Methyl ethyl ketone: 150.0 parts Cyclohexanone: 150.0 parts (abrasive liquid) α-alumina (BET (Brunauer-Emmett-Teller) specific surface area 19m 2 / g):6.0 copies SO3Na group-containing polyurethane resin: 0.6 parts (Weight average molecular weight: 70000, SO3Na group: 0.1meq / g) 2,3-dihydroxynaphthalene: 0.6 parts Cyclohexanone: 23.0 parts (Protrusion forming agent liquid) Colloidal silica (average particle size: 120 nm): 2.0 parts Methyl ethyl ketone: 8.0 parts (Other Ingredients) Stearic acid: 3.0 parts Stearic acid amide: 0.3 parts Butyl stearate: 6.0 parts Methyl ethyl ketone: 110.0 parts Cyclohexanone: 110.0 parts Polyisocyanate (Tosoh Corporation, Coronate (registered trademark) L): 3.0 parts

[0099] <Formulation of the composition for forming the nonmagnetic layer> Non-magnetic inorganic powder (type: α-iron oxide, average particle size: 10 nm, BET specific surface area: 75 m 2 / g):100.0 copies Carbon black (average particle size: 20 nm): 25.0 parts SO3Na group-containing polyurethane resin (weight average molecular weight: 70000, SO3Na group: 0.2 meq / g): 18.0 parts Stearic acid: 1.0 parts Cyclohexanone: 300.0 parts Methyl ethyl ketone: 300.0 parts

[0100] <Formulation of the composition for forming the backcoat layer> Non-magnetic powder: 100.0 parts α-Iron oxide: See Table 1 for mixing ratio (mass ratio) Average particle size (average major axis length): 150nm Average acicular ratio: 7 BET specific surface area: 52m 2 / g Carbon black: See Table 1 for mixing ratio (mass ratio) Average particle size: 20nm Vinyl chloride copolymer (Kaneka MR-104): See Table 1 SO3Na group-containing polyurethane resin: 6.0 parts Phenylphosphonic acid: 3.0 parts Cyclohexanone: 155.0 parts Methyl ethyl ketone: 155.0 parts Stearic acid: 3.0 parts Butyl stearate: 3.0 parts Polyisocyanate: 5.0 parts Cyclohexanone: 200.0 parts

[0101] <Preparation of Magnetic Layer-Forming Composition> A magnetic layer forming composition was prepared by the following method. The magnetic liquid was prepared by dispersing the various components of the magnetic liquid for 24 hours (bead dispersion) using a batch-type vertical sand mill. Zirconia beads with a bead diameter of 0.5 mm were used as the dispersion beads. The polishing agent liquid was prepared by mixing the various components of the polishing agent liquid described above and putting them into a horizontal bead mill disperser together with zirconia beads having a bead diameter of 0.3 mm, adjusting the ratio of [bead volume / (abrasive liquid volume+bead volume)]×100 to 80%, and dispersing the mixture in the bead mill for 120 minutes. The liquid after the treatment was taken out and subjected to ultrasonic dispersion filtration using a flow-type ultrasonic dispersion filtration device. Thus, the polishing agent liquid was prepared. The prepared magnetic liquid and abrasive liquid, as well as the above-mentioned protrusion-forming agent liquid and other components were introduced into a dissolver stirrer and stirred for 30 minutes at a peripheral speed of 10 m / sec., then subjected to three passes at a flow rate of 7.5 kg / min using a flow-type ultrasonic disperser, and then filtered through a filter with a pore size of 1 μm to prepare a composition for forming a magnetic layer.

[0102] <Preparation of composition for forming nonmagnetic layer> The various components of the nonmagnetic layer forming composition described above were dispersed for 24 hours using a batch-type vertical sand mill with zirconia beads having a bead diameter of 0.1 mm, and then filtered through a filter with a pore diameter of 0.5 μm to prepare the nonmagnetic layer forming composition.

[0103] <Preparation of Composition for Forming Backcoat Layer> The above-mentioned various components of the composition for forming backcoat layer are kneaded and diluted by open kneader except lubricant (stearic acid and butyl stearate), polyisocyanate and 200.0 parts of cyclohexanone, and then, by horizontal bead mill disperser, use zirconia beads with a bead diameter of 1 mm, bead filling rate of 80 volume%, rotor tip peripheral speed of 10 m / sec, 1 pass residence time of 2 minutes, and 12 passes of dispersion treatment.Then, add the above-mentioned remaining components and stir with dissolver, and obtain dispersion liquid is filtered with a filter with a pore diameter of 1 μm to prepare the composition for forming backcoat layer.

[0104] <Magnetic tape production> The non-magnetic layer-forming composition prepared above was applied and dried on the surface of an aromatic polyester support (see Table 1) so that the thickness after drying was 400 nm to form a non-magnetic layer, and then the magnetic layer-forming composition prepared above was applied on the surface of the non-magnetic layer so that the thickness after drying was 70 nm to form a coating layer. While the coating layer of the magnetic layer-forming composition was in a wet (undried) state, a vertical orientation treatment was performed in which a magnetic field with a magnetic field strength of 0.3 T was applied perpendicularly to the surface of the coating layer, and the coating was dried. Thereafter, the backcoat layer-forming composition prepared above was applied to the opposite side of the support so that the thickness after drying was 0.4 μm, and then dried. In this way, a magnetic tape raw sheet was produced. The magnetic tape raw material thus produced was subjected to a calendering process (surface smoothing process) using a calender consisting of only metal rolls at a speed of 100 m / min, a linear pressure of 294 kN / m, and a surface temperature of the calender roll of 100° C., and then heat treatment was performed for 36 hours in an environment with an atmospheric temperature of 70° C. After the heat treatment, the magnetic tape raw material was slit using a cutter to obtain a magnetic tape having a width of 1 / 2 inch. While this magnetic tape was run between a feed roller and a take-up roller (running speed 120 m / min, tension: see Table 1), the backcoat layer surface was subjected to blade polishing, dry wiping, and alcohol wiping with ethanol in that order. Specifically, a sapphire blade, a dry wiping material (Toray Industries, Inc.'s Toraysee (registered trademark)) and a wiping material soaked with ethanol (Toray Industries, Inc.'s Toraysee (registered trademark)) were placed between the two rollers, the sapphire blade was pressed against the backcoat layer surface of the magnetic tape running between the two rollers to perform blade polishing, then the backcoat layer surface was dry wiped with the dry wiping material, and then the backcoat layer surface was ethanol wiped with the ethanol-soaked wiping material. As a result, the blade polishing, dry wiping and ethanol wiping were each performed once on the backcoat layer surface. In a demagnetized state of the magnetic layer of the produced magnetic tape, a servo pattern with a layout and shape conforming to the LTO (Linear Tape-Open) Ultrium format was formed on the magnetic layer by a servo write head mounted on a servo writer. In this way, a magnetic tape was obtained in which the magnetic layer had a data band, a servo band, and a guide band in a layout conforming to the LTO Ultrium format, and the servo pattern on the servo band had a layout and shape conforming to the LTO Ultrium format. In this way, the magnetic tape of Example 1 was obtained.

[0105] [Examples 2 to 11, Comparative Examples 1 to 9] A magnetic tape was produced in the same manner as in Example 1, except that various conditions were changed as shown in Table 1. Regarding the surface treatment of the backcoat layer after slitting, the following surface treatment was carried out in Examples 2 to 11 and Comparative Examples 1 to 9. In Examples 2 to 4, 7, 9 to 11 and Comparative Examples 4 and 5, blade polishing, dry wiping treatment and ethanol wiping treatment were carried out in the same manner as in Example 1. In Examples 5, 6, and 8 and Comparative Examples 6 and 9, the blade grinding, dry wiping treatment, and ethanol wiping treatment were carried out in the same manner as in Example 1, except that the tension was changed. In Comparative Examples 1 to 3, 7 and 8, the blade polishing and dry wiping treatment were carried out in the same manner as in Example 1, but the ethanol wiping treatment was not carried out.

[0106] In Table 1, "BaFe" is a hexagonal barium ferrite powder with an average particle size (average plate diameter) of 21 nm.

[0107] In Table 1, "SrFe1" is a hexagonal strontium ferrite powder produced by the following method. 1707 g of SrCO3, 687 g of H3BO3, 1120 g of Fe2O3, 45 g of Al(OH)3, 24 g of BaCO3, 13 g of CaCO3, and 235 g of Nd2O3 were weighed out and mixed in a mixer to obtain a raw material mixture. The obtained raw material mixture was melted in a platinum crucible at a melting temperature of 1390°C, and the melt was poured into a rod shape at about 6 g / sec by heating the tapping hole at the bottom of the platinum crucible while stirring the melt. The tapped liquid was rolled and quenched with a water-cooled twin roller to produce an amorphous body. 280 g of the produced amorphous body was placed in an electric furnace, heated to 635°C (crystallization temperature) at a heating rate of 3.5°C / min, and held at that temperature for 5 hours to precipitate (crystallize) hexagonal strontium ferrite particles. Next, the crystallized material obtained above containing hexagonal strontium ferrite particles was coarsely crushed in a mortar, and 1000 g of zirconia beads with a particle size of 1 mm and 800 ml of 1% aqueous acetic acid solution were added to a glass bottle and dispersed for 3 hours using a paint shaker. The resulting dispersion was then separated from the beads and placed in a stainless steel beaker. The dispersion was left to stand at a liquid temperature of 100°C for 3 hours to dissolve the glass components, and then precipitated in a centrifuge and washed by repeated decantation, and dried for 6 hours in a heating furnace at a furnace temperature of 110°C to obtain hexagonal strontium ferrite powder. The average particle size of the hexagonal strontium ferrite powder obtained above is 18 nm, and the activation volume is 902 nm. 3 , the anisotropy constant Ku is 2.2×10 5 J / m 3 , mass magnetization σs is 49A m 2 / kg. A 12 mg sample powder was taken from the hexagonal strontium ferrite powder obtained above, and this sample powder was partially dissolved under the dissolution conditions exemplified above. The elemental analysis of the filtrate obtained was performed using an ICP analyzer to determine the surface layer content of neodymium atoms. Separately, 12 mg of sample powder was taken from the hexagonal strontium ferrite powder obtained above, and this sample powder was completely dissolved under the dissolution conditions exemplified above. The elemental analysis of the filtrate obtained was performed using an ICP analyzer to determine the bulk content of neodymium atoms. The neodymium atom content (bulk content) relative to 100 atomic % of iron atoms in the hexagonal strontium ferrite powder obtained above was 2.9 atomic %. The surface layer content of neodymium atoms was 8.0 atomic %. The ratio of the surface layer content to the bulk content, "surface layer content / bulk content," was 2.8, confirming that neodymium atoms were unevenly distributed in the surface layers of the particles. It was confirmed that the powder obtained above exhibited a hexagonal ferrite crystal structure by scanning with CuKα radiation at a voltage of 45 kV and an intensity of 40 mA and measuring the X-ray diffraction pattern under the following conditions (X-ray diffraction analysis). The powder obtained above exhibited a magnetoplumbite-type (M-type) hexagonal ferrite crystal structure. The crystal phase detected by the X-ray diffraction analysis was a single phase of magnetoplumbite type. PANalytical X'Pert Pro diffractometer, PIXcel detector Soller slits for incident and diffracted beams: 0.017 radians Dispersion slit fixed angle: 1 / 4 degree Mask: 10mm Anti-scatter slit: 1 / 4 degree Measurement mode: Continuous Measurement time per step: 3 seconds Measurement speed: 0.017 degrees per second Measurement step: 0.05 degrees

[0108] In Table 1, "SrFe2" is a hexagonal strontium ferrite powder produced by the following method. 1725 g of SrCO3, 666 g of H3BO3, 1332 g of Fe2O3, 52 g of Al(OH)3, 34 g of CaCO3, and 141 g of BaCO3 were weighed out and mixed in a mixer to obtain a raw material mixture. The obtained raw material mixture was melted in a platinum crucible at a melting temperature of 1380°C, and the melt was poured into a rod shape at about 6 g / sec by heating the tapping hole at the bottom of the platinum crucible while stirring the melt. The tapped liquid was quenched and rolled with a water-cooled twin roll to produce an amorphous body. 280 g of the obtained amorphous body was placed in an electric furnace, heated to 645° C. (crystallization temperature), and held at that temperature for 5 hours to precipitate (crystallize) hexagonal strontium ferrite particles. Next, the crystallized material obtained above containing hexagonal strontium ferrite particles was coarsely crushed in a mortar, and 1000 g of zirconia beads with a particle size of 1 mm and 800 ml of 1% aqueous acetic acid solution were added to a glass bottle and dispersed for 3 hours using a paint shaker. The resulting dispersion was then separated from the beads and placed in a stainless steel beaker. The dispersion was left to stand at a liquid temperature of 100°C for 3 hours to dissolve the glass components, and then precipitated in a centrifuge and washed by repeated decantation, and dried for 6 hours in a heating furnace at a furnace temperature of 110°C to obtain hexagonal strontium ferrite powder. The average particle size of the obtained hexagonal strontium ferrite powder was 19 nm, and the activation volume was 1102 nm. 3 , the anisotropy constant Ku is 2.0×10 5 J / m 3 , mass magnetization σs is 50A m 2 / kg.

[0109] In Table 1, "ε-iron oxide" is ε-iron oxide powder prepared by the following method. 8.3g of iron (III) nitrate nonahydrate, 1.3g of gallium (III) nitrate octahydrate, 190mg of cobalt (II) nitrate hexahydrate, 150mg of titanium (IV) sulfate, and 1.5g of polyvinylpyrrolidone (PVP) were dissolved in 90g of pure water, and 4.0g of ammonia solution with a concentration of 25% was added under the condition of an atmospheric temperature of 25°C while stirring with a magnetic stirrer in the air atmosphere, and the mixture was stirred for 2 hours at an atmospheric temperature of 25°C. A citric acid solution obtained by dissolving 1g of citric acid in 9g of pure water was added to the obtained solution, and the mixture was stirred for 1 hour. The powder precipitated after stirring was collected by centrifugation, washed with pure water, and dried in a heating furnace at an internal temperature of 80°C. 800g of pure water was added to the dried powder, and the powder was dispersed in water again to obtain a dispersion. The obtained dispersion was heated to 50°C, and 40g of 25% ammonia aqueous solution was added dropwise while stirring. After stirring for 1 hour while maintaining the temperature at 50°C, 14mL of tetraethoxysilane (TEOS) was added dropwise and stirred for 24 hours. 50g of ammonium sulfate was added to the obtained reaction solution, and the precipitated powder was collected by centrifugation, washed with pure water, and dried for 24 hours in a heating furnace with an internal temperature of 80°C to obtain a precursor of ferromagnetic powder. The obtained precursor of the ferromagnetic powder was placed in a heating furnace at an internal temperature of 1000° C. in an air atmosphere and subjected to a heat treatment for 4 hours. The heat-treated ferromagnetic powder precursor was placed in a 4 mol / L aqueous solution of sodium hydroxide (NaOH), and the liquid temperature was maintained at 70°C while stirring for 24 hours, thereby removing the impurity silicate compound from the heat-treated ferromagnetic powder precursor. Thereafter, the silicic acid compound was removed by centrifugation, and the ferromagnetic powder was collected and washed with pure water to obtain a ferromagnetic powder. The composition of the obtained ferromagnetic powder was confirmed by inductively coupled plasma-optical emission spectrometry (ICP-OES). The results showed that the powder was composed of Ga, Co, and Ti substituted ε-iron oxide (ε-Ga 0.28 Co 0.05 Ti 0.05 Fe 1.62 In addition, X-ray diffraction analysis was performed under the same conditions as those described above for SrFe1, and it was confirmed from the peaks in the X-ray diffraction pattern that the obtained ferromagnetic powder had a single-phase ε-phase crystal structure (ε-iron oxide type crystal structure) that did not contain α-phase or γ-phase crystal structures. The average particle size of the obtained ε-iron oxide powder was 12 nm, and the activation volume was 746 nm. 3 , the anisotropy constant Ku is 1.2×10 5 J / m 3 , mass magnetization σs is 16A m 2 / kg.

[0110] The activation volume and anisotropy constant Ku of the above hexagonal strontium ferrite powder and ε-iron oxide powder were determined for each ferromagnetic powder by the method described above using a vibrating sample magnetometer (manufactured by Toei Kogyo Co., Ltd.). Moreover, the mass magnetization σs is a value measured at a magnetic field strength of 15 kOe using a vibrating sample magnetometer (manufactured by Toei Kogyo Co., Ltd.).

[0111] In Table 1, "Support 1" is an aromatic polyester film produced by the method described in Example 2 of JP 2011-84036 A. Support 1 is a laminated film containing a polyethylene naphthalate film, and the thickness of the support is 4.2 μm. "Support 2" is an aromatic polyester film produced by the method described in Example 1 of JP 2011-84036 A. Support 2 is a laminated film including a polyethylene terephthalate film, and the thickness of the support is 5.0 μm. "Support 3" is an aromatic polyester film produced by the method described in Example 6 of JP 2011-84036 A. Support 3 is a laminated film including a polyethylene naphthalate film, and the thickness of the support is 4.2 μm. "Support 4" is a laminated film containing a polyethylene naphthalate film, and the thickness of the support is 4.2 μm. "Support 5" is a laminated film containing a polyethylene terephthalate film, and the thickness of the support is 4.2 μm. A sample piece weighing several grams was cut out from each aromatic polyester support, and the moisture absorption rate was determined by the method described above, with the values ​​shown in Table 1.

[0112] [Evaluation method] (1) Spacing difference before and after ethanol washing (S after -S before ) Using a TSA (Tape Spacing Analyzer (Micro Physics)), the spacing difference (S after -S before) was sought. Two sample pieces each having a length of 5 cm were cut out from each of the magnetic tapes of the Examples and Comparative Examples. One of the sample pieces was not washed with ethanol, and the spacing (S before The other sample piece was washed with ethanol as described above, and the spacing (S after ) was sought. A glass plate (a glass plate manufactured by Thorlabs, Inc. (model number: WG10530)) provided in the TSA was placed on the surface of the backcoat layer of the magnetic tape (specifically, the above sample piece), and a urethane hemisphere provided in the TSA as a pressing member was used to press the hemisphere against the magnetic layer surface of the magnetic tape at a pressure of 0.5 atm. In this state, white light was projected from a stroboscope provided in the TSA through the glass plate onto a certain area (150,000 to 200,000 μm) of the backcoat layer surface of the magnetic tape. 2 ) and the resulting reflected light was received by a CCD (Charge-Coupled Device) through an interference filter (a filter that selectively transmits light with a wavelength of 633 nm), obtaining an image of the interference fringes caused by the unevenness of this area. This image was divided into 300,000 points, and the distance (spacing) from the surface of the glass plate facing the magnetic tape to the surface of the backcoat layer of the magnetic tape was calculated for each point, and this was used as a histogram. The most frequent value S of the histogram obtained for the sample piece after washing with ethanol was after From the above, the most frequent value S of the histogram obtained for the specimen without ethanol washing is before Subtract the difference (S after -S before ) was sought.

[0113] (2) Spacing difference before and after n-hexane washing (S reference -S before ) (Reference value) A sample piece having a length of 5 cm was cut out from each of the magnetic tapes of the Examples and Comparative Examples, and washed in the same manner as above except that n-hexane was used instead of ethanol. The spacing after washing with n-hexane was then measured in the same manner as above. As a reference value, the spacing S measured here was reference and the spacing S obtained for the uncleaned specimen obtained in (1) above. before Difference (S reference -S before ) was sought.

[0114] (3) Evaluation of deterioration of driving stability Each magnetic tape of the Examples and Comparative Examples was stored for 3 hours in a thermobox whose inside temperature was kept at 32° C. and relative humidity at 20%. After that, the magnetic tape was taken out of the thermobox (outside air temperature was 23° C. and relative humidity was 50%) and within 1 minute was transferred to a thermoroom whose inside temperature was kept at 10° C. and relative humidity at 20% and stored for 1 week. After that, the PES (Position Error Signal) was obtained in this thermoroom by the following method. For each magnetic tape of the examples and comparative examples, the servo pattern was read by a verify head on the servo writer used to form the servo pattern. The verify head is a reading magnetic head for confirming the quality of the servo pattern formed on the magnetic tape, and a reading element is arranged at a position corresponding to the position of the servo pattern (position in the width direction of the magnetic tape) like the magnetic head of a known magnetic tape device (drive). The verify head is connected to a known PES calculation circuit that calculates the head positioning accuracy in the servo system as PES from the electric signal obtained by reading the servo pattern with the verify head. The PES calculation circuit calculates the displacement in the width direction of the magnetic tape from the input electric signal (pulse signal) at any time, and calculates the value obtained by applying a high-pass filter (cutoff: 500 cycles / m) to the time change information (signal) of this displacement as PES. The PES can be used as an index of running stability, and if the value of the PES calculated above is 15 nm or less, it can be evaluated that the decrease in running stability after storage in a low-temperature and low-humidity environment after a temperature change from high to low temperature under low humidity conditions is suppressed.

[0115] The above results are shown in Table 1 (Table 1-1 to Table 1-4).

[0116] [Table 1-1]

[0117] [Table 1-2]

[0118] [Table 1-3]

[0119] [Table 1-4]

[0120] The magnetic tape of the embodiment is a magnetic tape having an aromatic polyester support. From the PES values ​​in Table 1, it can be confirmed that the magnetic tape of the embodiment is prevented from decreasing in running stability after being stored in a low-temperature and low-humidity environment after being subjected to a temperature change from high to low temperature under low humidity. As shown in Table 1, the spacing difference (S reference -S before) and the spacing difference (S after -S before ) values, no correlation was observed. [Industrial Applicability]

[0121] One aspect of the present invention is useful in the technical field of magnetic recording media for various data storage.

Claims

1. A magnetic recording medium having a magnetic layer containing ferromagnetic powder on one surface side of a non-magnetic support and a backcoat layer containing non-magnetic powder on the other surface side, The thickness of the magnetic layer is 30 nm or more and 70 nm or less, The spacing S on the surface of the backcoat layer is measured by optical interferometry after washing with ethanol. after and a spacing S measured by optical interferometry on the surface of the backcoat layer before washing with ethanol. before The difference between after -S before , is more than 0 nm and 15.0 nm or less, and The non-magnetic support is an aromatic polyester support having a moisture absorption rate of 0.3% or less.

2. Said difference, S after -S before , is 1.0 nm or more and 15.0 nm or less; 2. The magnetic recording medium according to claim 1.

3. Said difference, S after -S before , is 2.0 nm or more and 13.0 nm or less; 3. The magnetic recording medium according to claim 1 or 2.

4. 4. The magnetic recording medium according to claim 1, wherein the moisture absorption rate of the aromatic polyester support is 0.1% or more and 0.3% or less.

5. 5. The magnetic recording medium according to claim 1, further comprising a non-magnetic layer containing non-magnetic powder between the non-magnetic support and the magnetic layer.

6. 6. The magnetic recording medium according to claim 1, which is a magnetic tape.

7. A magnetic recording medium according to any one of claims 1 to 6, A magnetic head; A magnetic recording and reproducing apparatus comprising:

Citation Information

Patent Citations

  • Lubricant and magnetic recording medium made by using the same

    JP1997227883A

  • Method for quantitative analysis of surface lubricant on magnetic recording medium

    JP2001229529A

  • Magnetic recording medium

    JP2012043495A

  • Magnetic tape and magnetic tape apparatus

    JP2017174476A

  • Magnetic recording medium for high recording density and recording and reproducing mechanism thereof

    JP2018181396A