Composite particles

Composite particles of zirconium nitride and aluminum with specific aluminum content enhance transmittance in ultraviolet and near-infrared regions while maintaining high light-shielding in the visible region, addressing the limitations of existing zirconium nitride particles.

JP7566606B2Active Publication Date: 2024-10-15NISSHIN ENG
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020204809
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-10
Publication Date
2024-10-15
Estimated Expiration
2040-12-10

AI Technical Summary

Technical Problem

Current zirconium nitride particles lack high transmittance in the ultraviolet and near-infrared light regions while maintaining high light-shielding properties in the visible light region, and there is a demand for expanding their uses and adding other functions.

Method used

Composite particles of zirconium nitride and aluminum are formed with an aluminum content of 9.5 to 43% by mass, resulting in high transmittance in the ultraviolet and near-infrared regions while maintaining high light-shielding properties in the visible region.

Benefits of technology

The composite particles achieve high transmittance in the ultraviolet and near-infrared regions while maintaining low transmittance in the visible region, with a narrow particle size distribution and uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566606000001
    Figure 0007566606000001
  • Figure 0007566606000002
    Figure 0007566606000002
  • Figure 0007566606000003
    Figure 0007566606000003
Patent Text Reader

Abstract

To provide a composite particle having optical characteristics in which transmittance in an ultraviolet light range and a near-infrared light range is higher than that in a visible light range while maintaining high light shielding property in the visible light range.SOLUTION: A composite particle is a composite of ZrN and Al, and a content of Al is 9.5-43 mass%. The content of Al is preferably 14-38 mass%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite particle of zirconium nitride and aluminum, and in particular to a composite particle of zirconium nitride and aluminum which has characteristic optical properties. [Background technology]

[0002] Currently, various types of fine particles are used for various purposes. For example, fine particles such as metal fine particles, oxide fine particles, nitride fine particles, and carbide fine particles are used in electrical insulating materials such as various electrical insulating parts, cutting tools, machining materials, functional materials such as sensors, sintered materials, electrode materials for fuel cells, and catalysts. Patent Document 1 describes black composite particles having high light-shielding properties suitable as a black component for the black matrix of a color filter, etc. The black composite particles are composed of titanium nitride particles and metal particles, and are represented by the composition formula: TiNxOy·zX (in the composition formula, Ti represents a titanium atom, N represents a nitrogen atom, O represents an oxygen atom, and X represents a metal atom. x represents a number greater than 0 and less than 2, y represents a number equal to or greater than 0 and less than 2, and z represents a number greater than 0 and less than 10).

[0003] Non-Patent Document 1 describes the growth of ultrafine particles of transition metal nitride by a reactive gas evaporation method using electron beam heating, and describes ZrN fine particles of 2 to 10 nm. Patent Document 2 describes a ZrN nanoparticle having a peak of low-order zirconium oxide and a peak of zirconium nitride in an X-ray diffraction profile, and a specific surface area of ​​10 to 60 m 2 A particulate low-order zirconium oxide-zirconium nitride composite with a particle size of 1 / g is described. Patent Document 3 describes a method for producing a sintered body having a specific surface area of ​​20 to 90 m2 measured by the BET method. 2 / g, and a powder for forming a black light-shielding film containing zirconium nitride as a main component and magnesium and / or aluminum, wherein when magnesium is contained, the content ratio of magnesium is 0.01 to 1.0 mass% relative to 100 mass% of the powder for forming the black light-shielding film, and when aluminum is contained, the content ratio of aluminum is 0.01 to 1.0 mass% relative to 100 mass% of the powder for forming the black light-shielding film. The powder for forming a black light-shielding film of Patent Document 3 has an oxide coating layer or nitride coating layer of aluminum or magnesium generated on the extreme surface layer of nanoparticulated zirconium nitride particles. Non-Patent Document 2 describes ZrN powder synthesized from ZrO2 by Mg reduction in a temperature range of 500° C. to 1100° C. under a nitrogen gas flow (150 to 200 ml / min). Non-Patent Document 2 also confirms that the ZrN powder is a single phase ZrN by an X-ray diffraction test. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-227282 A [Patent Document 2] Patent No. 4931011 [Patent Document 3] JP 2019-112275 A [Non-patent literature]

[0005] [Non-Patent Document 1] Saburo IWAMA, Kenji HAYAKAWA and Tetsuya ARIZUMI, GROWTH OF ULTRAFINE PARTICLES OF TRANSITION METAL NITRIDES BY THE REACTIVE GAS EVAPORATION TECHNIQUE WITH ELECTRON BEAM HEATING, Journal of Crystal Growth 66 (1984) 189-194 [Non-Patent Document 2] Tsutomu Ikeda, Toshiyuki Mori, Fumio Noguchi, Takeaki Iida, Takashi Mitamura, Synthesis of ultrafine zirconium nitride powder from zirconia by reduction with magnesium, Journal of the Japan Ceramic Association 93 [9] 1985 505 Summary of the Invention [Problem to be solved by the invention]

[0006] As described above, various types of fine particles are used for various purposes, and as in the above-mentioned Patent Document 1, black composite fine particles consisting of titanium nitride particles and metal fine particles have been proposed. As described in the above Non-Patent Document 1 and Non-Patent Document 2, ZrN fine particles are known. It is known that the properties of these ZrN (zirconium nitride) fine particles are high transmittance in the ultraviolet light region and low transmittance in the visible light region with a wavelength of 400 to 800 nm. However, in the industrial field, the current situation is that single-phase zirconium nitride as described in Patent Document 2 has not been obtained. Furthermore, the powder for forming a black light-shielding film in Patent Document 3 has an aluminum or magnesium oxide coating layer or nitride coating layer formed on the extreme surface layer of nanoparticulated zirconium nitride particles, but it is described that if the aluminum content exceeds 1.0 mass %, the light-shielding performance of the black light-shielding film decreases. Furthermore, there is a demand for further expansion of applications of the fine particles and addition of other functions. Currently, compared to the optical properties of single-phase zirconium nitride, there is a demand for higher transmittance in the ultraviolet light region while maintaining high light-shielding properties in the visible light region. Furthermore, compared to the visible light region, there is a demand for high transmittance in the near-infrared light region with a wavelength of 1000 nm or more.

[0007] An object of the present invention is to provide composite particles having optical properties such as higher transmittance in the ultraviolet and near-infrared regions compared to the visible light region, while maintaining high light-shielding properties in the visible light region. [Means for solving the problem]

[0008] In order to achieve the above object, the present invention provides composite particles characterized in that ZrN and Al are composited together, and the Al content is 9.5 to 43 mass %. The Al content is preferably 14 to 38 mass %. The particle size is preferably 1 to 200 nm. Effect of the Invention

[0009] According to the present invention, there are provided composite particles having optical properties such as high transmittance in the ultraviolet light region and high transmittance in the near-infrared light region while maintaining high light-shielding properties in the visible light region. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic diagram showing an example of a fine particle production apparatus used for producing composite particles according to an embodiment of the present invention. [Diagram 2] 1 is a graph showing the transmittance of composite particles in which zirconium nitride and aluminum are combined. [Diagram 3] 1 is a graph showing the transmittance of composite particles of zirconium nitride and aluminum, and mixed particles of zirconium nitride and aluminum nitride. [Figure 4] 1 is a graph showing the transmittance ratio at a wavelength of 365 nm and the transmittance ratio at a wavelength of 1100 nm, with respect to a wavelength of 600 nm as the reference, for composite particles in which zirconium nitride and aluminum are composited, and mixed particles of zirconium nitride and aluminum nitride. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the composite particles of the present invention will be described in detail based on preferred embodiments shown in the accompanying drawings. It should be noted that the drawings described below are illustrative for explaining the present invention, and the present invention is not limited to the drawings shown below.

[0012] [Composite particles] The composite particles are particles containing zirconium nitride (ZrN) particles in which zirconium nitride (ZrN) and aluminum (Al) are composited together, and the aluminum (Al) content is 9.5 to 43 mass %. The above-mentioned composite of ZrN and Al means that ZrN and Al are contained in a single particle, and in this case, the form of Al is not particularly limited, and it may be in the form of a compound such as a nitride, oxide, oxynitride, non-stoichiometric oxide, and non-stoichiometric nitride as well as a simple metal, and may be dissolved in the ZrN particle or may not be dissolved in the ZrN particle. Also, the composite particle is a particle containing the above-mentioned composite particle. In addition, particles containing composite particles of zirconium nitride (ZrN) and aluminum (Al) are also referred to as composite particles of zirconium nitride (ZrN) and aluminum (Al).

[0013] The composite particles are called nanoparticles. The particle size of the composite particles is 1 to 200 nm, preferably 10 to 150 nm, and particularly preferably 25 to 40 nm. The particle size is an average particle size measured using a BET method. The composite particles are produced, for example, by a production method described later, and are obtained in a particle state, not in a state dispersed in a solvent, and exist as composite particles alone. Therefore, the combination with a solvent is not particularly limited, and the degree of freedom in selecting a solvent is high.

[0014] The composite particles of ZrN and Al, so long as the Al content is within the range of 9.5 to 43 mass %, have optical properties in which the particles maintain high light blocking properties in the visible light region, i.e., maintain low transmittance in the visible light region, have higher transmittance in the ultraviolet light region, and further have high transmittance in the near-infrared light region, as described below. The above-mentioned Al (aluminum) content (mass%) can be determined by measurement using XRF (X-ray fluorescence analysis), but the Al content (mass%) is obtained excluding impurities. Specifically, the Al content is the mass% Al when the contents (mass%) of elements other than Zr and Al are excluded from the contents (mass%) of each element obtained by measuring with XRF (X-ray fluorescence analysis) so that the total mass% of Zr and Al is 100.

[0015] [Composite particle manufacturing equipment] Next, an example of a composite particle manufacturing apparatus will be described, which is not limited to the one shown in FIG. FIG. 1 is a schematic diagram showing an example of a fine particle production apparatus used for producing composite particles according to an embodiment of the present invention. A fine particle production apparatus 10 shown in FIG. 1 (hereinafter simply referred to as production apparatus 10) produces composite particles of zirconium nitride (ZrN) and aluminum (Al). The manufacturing equipment 10 includes a plasma torch 12 that generates thermal plasma, a material supply device 14 that supplies raw material powder of the composite particles into the plasma torch 12, a chamber 16 that functions as a cooling tank for generating primary particles 15 of the composite particles, a cyclone 19 that removes coarse particles having a particle size equal to or larger than an arbitrarily specified particle size from the primary particles 15 of the composite particles, and a recovery section 20 that recovers secondary particles 18 of the composite particles having a desired particle size classified by the cyclone 19. For example, various devices disclosed in JP 2007-138287 A can be used for the material supply device 14, chamber 16, cyclone 19, and recovery section 20. The primary fine particles 15 of the composite particles are also simply referred to as primary fine particles 15.

[0016] In the present embodiment, for example, zirconium nitride (ZrN) powder and aluminum (Al) powder are used as raw material powders to manufacture the composite particles. For example, nano-sized zirconium nitride (ZrN) and aluminum (Al) composite particles having a particle size of 1 to 100 nm are obtained from the above-mentioned raw material powders. The zirconium nitride (ZrN) powder and aluminum (Al) powder used as the raw material powder are each appropriately set in average particle size so that they can be easily evaporated in a thermal plasma flame. The average particle size is, for example, 100 μm or less, preferably 10 μm or less, and more preferably 5 μm or less.

[0017] The plasma torch 12 is composed of a quartz tube 12a and a high-frequency oscillation coil 12b surrounding the outside of the quartz tube 12a. A supply tube 14a (described later) is provided in the center of the upper part of the plasma torch 12 for supplying raw material powder of composite particles into the plasma torch 12. A plasma gas supply port 12c is formed in the peripheral part (on the same circumference) of the supply tube 14a, and the plasma gas supply port 12c is ring-shaped.

[0018] The plasma gas supply source 22 supplies plasma gas into the plasma torch 12, and has, for example, a gas supply unit 22a. The gas supply unit 22a is connected to the plasma gas supply port 12c via a pipe 22b. The gas supply unit 22a is provided with a supply amount adjustment unit such as a valve for adjusting the supply amount, although not shown. The plasma gas is supplied into the plasma torch 12 from the plasma gas supply source 22 through the ring-shaped plasma gas supply port 12c in the directions indicated by the arrows P and S.

[0019] The plasma gas may be, for example, a mixture of argon gas and nitrogen gas, and the thermal plasma flame is derived from at least one of argon gas and nitrogen gas. At least one of argon gas and nitrogen gas is stored in gas supply unit 22a. At least one of argon gas and nitrogen gas is supplied from gas supply unit 22a of plasma gas supply source 22 through piping 22b and plasma gas supply port 12c into plasma torch 12 in the directions indicated by arrows P and S. At least one of argon gas and nitrogen gas may be supplied in the direction indicated by arrow P. When a high-frequency voltage is applied to the high-frequency oscillation coil 12 b , a thermal plasma flame 24 is generated in the plasma torch 12 .

[0020] The temperature of the thermal plasma flame 24 must be higher than the boiling point of the raw material powder. On the other hand, the higher the temperature of the thermal plasma flame 24, the easier it is for the raw material powder to become in a gaseous state, so this is preferable, but the temperature is not particularly limited. For example, the temperature of the thermal plasma flame 24 can be set to 6000°C, and theoretically it is thought to reach about 10000°C. The pressure atmosphere in the plasma torch 12 is preferably equal to or lower than atmospheric pressure. Here, the pressure atmosphere equal to or lower than atmospheric pressure is not particularly limited, but is, for example, 0.5 to 100 kPa. In addition, for example, at least one of argon gas and nitrogen gas is used as the plasma gas, but this is not limited to this, and it is also possible to use a combination of at least one of argon gas and nitrogen gas with helium gas, or a combination of at least one of argon gas and nitrogen gas with hydrogen gas.

[0021] The outside of the quartz tube 12a is surrounded by a concentric tube (not shown), and cooling water is circulated between this tube and the quartz tube 12a to water-cool the quartz tube 12a and prevent the quartz tube 12a from becoming too hot due to the thermal plasma flame 24 generated in the plasma torch 12.

[0022] The material supply device 14 is connected to the upper part of the plasma torch 12 via a supply pipe 14a. The material supply device 14 supplies raw material powder, for example, in the form of powder, into a thermal plasma flame 24 in the plasma torch 12.

[0023] As the material supplying device 14 that supplies the raw material powder, for example, the one disclosed in JP 2007-138287 A can be used. In this case, the material supplying device 14 has, for example, a storage tank (not shown) that stores the raw material powder, a screw feeder (not shown) that transports a fixed amount of the raw material powder, a dispersing section (not shown) that disperses the raw material powder transported by the screw feeder into a state of primary particles before it is finally spread, and a carrier gas supply source (not shown).

[0024] The raw material powder is supplied together with carrier gas under extrusion pressure from a carrier gas supply source through a supply pipe 14a into a thermal plasma flame 24 in the plasma torch 12. The configuration of the material supply device 14 is not particularly limited as long as it can prevent the raw material powder from agglomerating and can disperse the raw material powder into the plasma torch 12 while maintaining the raw material powder in a dispersed state. For example, an inert gas such as argon gas is used as the carrier gas. The flow rate of the carrier gas can be controlled using a flow meter such as a float type flow meter. The flow rate value of the carrier gas refers to the scale value of the flow meter.

[0025] The chamber 16 is provided adjacent to and below the plasma torch 12, and is connected to a gas supply device 28. Primary fine particles 15 of composite particles are generated in the chamber 16. The chamber 16 also functions as a cooling tank.

[0026] The gas supply device 28 supplies a cooling gas and a nitriding gas into the chamber 16. The gas supply device 28 has a gas supply source 28a, a pipe 28b, and a pipe 28d. The pipe 28b is for supplying the cooling gas into the chamber 16. The pipe 28b is provided with a pressure control valve 28c that controls the amount of gas supplied from the gas supply source 28a. The pipe 28d is for supplying the nitriding gas into the chamber 16. The pipe 28d is provided with a pressure control valve 28e that controls the amount of gas supplied from the gas supply source 28a. The cooling gas is also called a cooling gas. Gas supply device 28 further has pressure applying means (not shown) such as a compressor or a blower that applies extrusion pressure to the cooling gas to be supplied into chamber 16. Cooling gas is supplied from gas supply source 28a by the pressure applying means through pipe 28b, and nitriding gas is supplied through pipe 28d. For example, at least one of argon gas and nitrogen gas is stored in the gas supply source 28a, the cooling gas is at least one of argon gas and nitrogen gas, and the nitriding gas is nitrogen gas.

[0027] The gas supply device 28 supplies at least one of argon gas and nitrogen gas as a cooling gas in the direction of arrow Q at an angle of, for example, 45° toward the tail of the thermal plasma flame 24, i.e., the end of the thermal plasma flame 24 opposite the plasma gas supply port 12c, i.e., the terminal end of the thermal plasma flame 24, and also supplies the above-mentioned cooling gas from above to below along the inner wall 16a of the chamber 16, i.e., in the direction of arrow R shown in FIG. 1.

[0028] The raw powder that has been put into a gaseous state by the thermal plasma flame 24 is quenched by the cooling gas supplied from the gas supply device 28 into the chamber 16, and primary fine particles 15 of the composite particles are obtained. In addition to this, the above-mentioned cooling gas has an additional effect of contributing to the classification of the primary fine particles 15 in the cyclone 19. If the primary particles 15 of the composite particles collide with each other immediately after generation and form aggregates, resulting in non-uniform particle size, this will cause a decrease in quality. However, the cooling gas supplied in the direction of arrow Q toward the tail (end) of the thermal plasma flame dilutes the primary particles 15, preventing the particles from colliding with each other and agglomerating. Furthermore, the cooling gas in the direction of arrow R prevents the primary particles 15 from adhering to the inner wall 16a of the chamber 16 during the recovery of the primary particles 15, improving the yield of the generated primary particles 15.

[0029] Furthermore, nitrogen gas is supplied as the nitriding gas in the direction of the arrow G shown in Fig. 1. This further supplies nitrogen to the primary fine particles 15, enabling stable nitriding. Note that nitrogen gas is used as the cooling gas, and sufficient nitriding can be achieved with the cooling gas, so if composite particles can be obtained, nitriding gas is not necessarily required. The cooling gas and the nitriding gas may be the same or different. When the cooling gas and the nitriding gas are different, a gas supply source 28a is provided for each of the cooling gas and the nitriding gas.

[0030] 1, the chamber 16 is provided with a cyclone 19 for classifying the primary fine particles 15 of the composite particles into particles of a desired particle size. The cyclone 19 includes an inlet pipe 19a for supplying the primary fine particles 15 from the chamber 16, a cylindrical outer cylinder 19b connected to the inlet pipe 19a and located at the top of the cyclone 19, a truncated cone section 19c that continues downward from the bottom of the outer cylinder 19b and has a gradually decreasing diameter, a coarse particle recovery chamber 19d connected to the bottom of the truncated cone section 19c for recovering coarse particles having a particle size equal to or larger than the desired particle size, and an inner pipe 19e connected to a recovery section 20 described later and protruding from the outer cylinder 19b.

[0031] An airflow containing primary fine particles 15 is blown from the inlet pipe 19a of the cyclone 19 along the inner circumferential wall of the outer cylinder 19b, and as a result, this airflow flows from the inner circumferential wall of the outer cylinder 19b toward the truncated cone portion 19c as shown by the arrow T in Figure 1, forming a downward swirling flow. When the descending swirling flow reverses and becomes an ascending flow, the coarse particles cannot join the ascending flow due to the balance between centrifugal force and drag, and so they descend along the side surface of the truncated cone portion 19c and are collected in the coarse particle collection chamber 19d. Fine particles that are more affected by drag than centrifugal force are discharged from the inner pipe 19e to the outside of the system together with the ascending flow on the inner wall of the truncated cone portion 19c.

[0032] Also, a negative pressure (suction force) is generated through the inner pipe 19e from the collecting section 20, which will be described later in detail. The composite particles separated from the above-mentioned swirling air current are sucked in by this negative pressure (suction force) as indicated by the symbol U, and are sent to the collecting section 20 through the inner pipe 19e.

[0033] A collection section 20 for collecting secondary fine particles 18 (composite particles) having a desired nanometer-order particle size is provided on the extension of inner pipe 19e, which is the outlet of the airflow in cyclone 19. Collection section 20 includes collection chamber 20a, filter 20b provided in collection chamber 20a, and vacuum pump 30 connected via a pipe provided below collection chamber 20a. Fine particles sent from cyclone 19 are sucked by vacuum pump 30 and drawn into collection chamber 20a, where they are collected while remaining on the surface of filter 20b. In addition, the number of cyclones used in the above-mentioned manufacturing apparatus 10 is not limited to one, and may be two or more.

[0034] [Method of manufacturing composite particles] Next, an example of a method for producing composite particles will be described using the above-mentioned production apparatus 10. First, zirconium nitride (ZrN) powder and aluminum (Al) powder are prepared as raw material powders for the composite particles. The raw material powders are fed into the material supply device 14. The raw material powder is appropriately determined depending on the Al content in the composite particle to be produced. For example, the amount of ZrN powder and the amount of Al powder are appropriately adjusted depending on the Al content. In the raw material powders, the sizes of the ZrN powder and the Al powder are both appropriately determined depending on the production method, etc., but when a thermal plasma flame is used as described above, the ZrN powder and the Al powder each have an average particle size of, for example, 100 μm or less, preferably 10 μm or less, and more preferably 5 μm or less, so that they are easily evaporated in the thermal plasma flame.

[0035] For example, at least one of argon gas and nitrogen gas is used as the plasma gas, and a high-frequency voltage is applied to the high-frequency oscillation coil 12 b to generate a thermal plasma flame 24 in the plasma torch 12 . Furthermore, at least one of argon gas and nitrogen gas is supplied as a cooling gas from the gas supply device 28 to the tail of the thermal plasma flame 24, i.e., the end of the thermal plasma flame 24, in the direction of the arrow Q. At this time, at least one of argon gas and nitrogen gas is also supplied as a cooling gas in the direction of the arrow R. Furthermore, nitrogen gas is supplied in the direction of the arrow G as a nitriding gas.

[0036] Next, the raw material powder is gas-transported using, for example, argon gas as a carrier gas, and is supplied into the thermal plasma flame 24 in the plasma torch 12 via the supply pipe 14a. The supplied raw material powder evaporates in the thermal plasma flame 24 and becomes a gas phase state, reacts with nitrogen and is nitrided, and is rapidly cooled by a cooling gas (gas for cooling), thereby obtaining primary fine particles 15 of composite particles of zirconium nitride and aluminum. Furthermore, a sufficient amount of nitrogen is supplied to the primary fine particles 15 by the nitriding gas, stabilizing the nitriding, and composite particles of zirconium nitride and aluminum can be obtained stably. As described above, a method for producing composite particles having a step of supplying a carrier gas in which raw material powder is dispersed into a thermal plasma flame and a step of supplying a cooling gas to the end of the thermal plasma flame to produce composite particles is called a thermal plasma method.

[0037] The primary fine particles 15 of the composite particles obtained in the chamber 16 are blown together with the airflow from the inlet pipe 19a of the cyclone 19 along the inner peripheral wall of the outer cylinder 19b, and as a result, this airflow flows along the inner peripheral wall of the outer cylinder 19b as shown by the arrow T in Fig. 1, forming a swirling flow and descending. When the descending swirling flow reverses and becomes an ascending flow, the balance between the centrifugal force and the drag force prevents the coarse particles from joining the ascending flow, and they descend along the side of the truncated cone section 19c and are collected in the coarse particle collection chamber 19d. The fine particles, which are more affected by the drag force than the centrifugal force, are discharged from the inner pipe 19e to the outside of the system together with the ascending flow on the inner wall of the truncated cone section 19c.

[0038] The discharged secondary fine particles 18 (composite particles) of zirconium nitride (ZrN) and aluminum (Al) are sucked in the direction indicated by the symbol U in FIG. 1 by the negative pressure (suction force) from the collection section 20 by the vacuum pump 30, sent to the collection section 20 through the inner pipe 19e, and collected by the filter 20b of the collection section 20. At this time, the internal pressure in the cyclone 19 is preferably equal to or lower than atmospheric pressure. In addition, the particle size of the secondary fine particles 18 (composite particles) is specified to any particle size on the order of nanometers depending on the purpose. In this way, composite particles of zirconium nitride (ZrN) and aluminum (Al) (ZrN+Al composite particles) can be easily and reliably obtained simply by subjecting zirconium nitride (ZrN) powder and Al powder to plasma treatment. Moreover, the composite particles produced by the method for producing composite particles of this embodiment have a narrow particle size distribution, that is, they have a uniform particle size and are almost free of coarse particles of 1 μm or more.

[0039] The ratio of ZrN powder and Al powder used in the raw powder is appropriately determined according to the composition of the composite particles to be finally obtained. For the above ratio, for example, the composition to be finally obtained and the ratio of ZrN powder and Al powder are determined in advance. Using the determined ratio, composite particles of a predetermined composition can be obtained.

[0040] Although the primary fine particles of the composite particles are formed by a thermal plasma method using a thermal plasma flame, the primary fine particles of the composite particles can be formed by a gas phase method. Therefore, as long as the gas phase method is used, it is not limited to the thermal plasma method using a thermal plasma flame, and a manufacturing method for forming the primary fine particles of the composite particles by a flame method, an arc plasma method, a microwave heating method, or a pulse wire method may be used.

[0041] The flame method is a method for synthesizing composite particles by passing a gaseous or liquid raw material powder through a flame using a flame as a heat source. In the flame method, the raw material powder is supplied to the flame in a gaseous or liquid state, and a cooling gas is supplied to the flame to lower the temperature of the flame, thereby obtaining primary fine particles 15 of the composite particles. The raw material powder in a gas phase state refers to a state in which the raw material powder is dispersed in the above-mentioned carrier gas, and the raw material powder in a liquid phase state refers to a state in which the raw material powder is dispersed in a solvent. The cooling gas can be the same as that of the thermal plasma method described above. The raw material powder can be the same as that of the thermal plasma flame described above. As the raw material powder, ZrN powder and Al powder are used as described above.

[0042] <Optical properties of composite particles> Next, the optical properties of the zirconium nitride and aluminum composite particles will be described. FIG. 2 is a graph showing the transmittance of composite particles in which zirconium nitride and aluminum are combined. The horizontal axis of FIG. 2 is wavelength (nm), and the vertical axis is transmittance (%). The transmittances shown by measurement lines 50 and 52 in FIG. 2 are each normalized by the transmittance value at a wavelength of 600 nm. Also, reference numeral 53 in FIG. 2 is a line showing a wavelength of 365 nm (i-line). The wavelength of 365 nm is a wavelength in the ultraviolet light region called the i-line. The wavelength of 1100 nm is a wavelength in the near-infrared light region.

[0043] [Transmittance measurement method] The method for measuring the transmittance will be described below. First, 0.005 g of the powder of the composite particles of zirconium nitride and aluminum (ZrN+Al composite particles) to be measured is weighed out, ethanol is added so that the total amount becomes 50 g, and a dispersion process is performed for 5 minutes using an ultrasonic device (Tetora 150, manufactured by Nikkaki Bios Co., Ltd.). Next, 10 g is taken from the obtained solution, ethanol is added so that the total amount becomes 50 g, and a dispersion process is performed for 1 minute using an ultrasonic device to obtain a solution with a mass concentration of 20 ppm. The transmittance of the obtained solution is then measured using an ultraviolet-visible-near infrared spectrophotometer (V-670, manufactured by JASCO Corporation).

[0044] 2 shows the transmittance of a composite particle of zirconium nitride and aluminum with an Al content of 32.7 mass %. The composite particle of measurement line 50 has an Al content within the range of the present invention. The particle diameter of the composite particle of measurement line 50 is 28.1 nm. Measurement line 52 shows the transmittance of a composite particle of zirconium nitride and aluminum with an Al content of 3.5 mass %. The Al content of the composite particle of measurement line 52 is outside the range of the present invention. The particle diameter of the composite particle of measurement line 52 is 29.8 nm. The particle size of the composite particle indicated by measurement line 50 and the particle size of the composite particle indicated by measurement line 52 in FIG. 2 are both average particle sizes measured by the BET method.

[0045] As shown in FIG. 2, the transmittance of the zirconium nitride and aluminum composite particle of the present invention (measurement line 50) and the transmittance of the zirconium nitride and aluminum composite particle outside the scope of the present invention (measurement line 52) are such that while maintaining high light-shielding properties in the visible light region, the transmittance is higher in the short wavelength region of 300 to 400 nm compared to the visible light region, and a large amount of light in the vicinity of the i-line with a wavelength of 365 nm (ultraviolet light region) can be transmitted. When measuring line 50 and measuring line 52 are compared, the zirconium nitride and aluminum composite particle of the present invention shown by measuring line 50 has optical properties such as a higher transmittance in the ultraviolet light region and also a higher transmittance in the near-infrared light region compared to the composite particle (measuring line 52) outside the scope of the present invention. In this way, the zirconium nitride and aluminum composite particles of the present invention are particles having optical properties such as a high light-shielding property in the visible light region, i.e., a low transmittance in the visible light region, a higher transmittance in the ultraviolet light region compared to the visible light region, and a high transmittance in the near-infrared light region.

[0046] [Transmittance of composite particles] Fig. 3 is a graph showing the transmittance of a composite particle of zirconium nitride and aluminum, and a mixed particle of zirconium nitride and aluminum nitride. The horizontal axis of Fig. 3 is wavelength (nm), and the vertical axis is transmittance (%). The transmittance shown by each measurement line in Fig. 3 is normalized by the transmittance value at a wavelength of 600 nm for each measurement line. Reference numeral 53 in Fig. 3 is a line showing a wavelength of 365 nm (i-line). 3, measurement line 60 indicates the transmittance of a composite particle of zirconium nitride (ZrN) and aluminum (Al) with an Al content of 9.7 mass%, measurement line 62 indicates the transmittance of a composite particle of zirconium nitride and aluminum with an Al content of 12.4 mass%, and measurement line 64 indicates the transmittance of a composite particle of zirconium nitride and aluminum with an Al content of 14.3 mass%. The composite particle of measurement line 60 has a particle size of 33.8 nm, the composite particle of measurement line 62 has a particle size of 35.1 nm, and the composite particle of measurement line 64 has a particle size of 31.1 nm. Measurement line 66 shows the transmittance of a composite particle of zirconium nitride and aluminum with an Al content of 17.9% by mass. Measurement line 68 shows the transmittance of a composite particle of zirconium nitride and aluminum with an Al content of 22.3% by mass. Measurement line 70 shows the transmittance of a composite particle of zirconium nitride and aluminum with an Al content of 27.3% by mass. Measurement line 72 shows the transmittance of a composite particle of zirconium nitride and aluminum with an Al content of 32.7% by mass. Measurement line 72 is measurement line 50 shown in FIG. 2. Measurement line 74 shows the transmittance of a composite particle of zirconium nitride and aluminum with an Al content of 42.2% by mass. The composite particle of measurement line 66 has a particle size of 33.0 nm, the composite particle of measurement line 68 has a particle size of 26.8 nm, the composite particle of measurement line 70 has a particle size of 29.4 nm, the composite particle of measurement line 72 has a particle size of 28.1 nm, and the composite particle of measurement line 74 has a particle size of 28.8 nm.

[0047] Measurement line 100 shown in Figure 3 indicates the transmittance of a composite particle of zirconium nitride and aluminum with an Al content of 3.5 mass%. Measurement line 100 is measurement line 52 shown in Figure 2. Measurement line 102 indicates the transmittance of a composite particle of zirconium nitride and aluminum with an Al content of 8.4 mass%. The particle size of the composite particle of measurement line 100 is 29.8 nm. The particle size of the composite particle of measurement line 102 is 36.9 nm. Measurement line 104 indicates the transmittance of a mixed particle of zirconium nitride and aluminum nitride. The mixed particle has an aluminum content of 37 mass %. The mixed particles are obtained by mixing zirconium nitride particles and aluminum nitride particles so that the aluminum content is 37 mass%. In the mixed particles, the zirconium nitride particles have an Al content of 3.5 mass% and a particle size of 29.8 nm. The aluminum nitride particles have a particle size of 30.9 nm. Measurement line 106 shows the transmittance of a composite particle of zirconium nitride and aluminum with an Al content of 44 mass%. Measurement line 108 shows the transmittance of a composite particle of zirconium nitride and aluminum with an Al content of 56.1 mass%. The particle size of the composite particle of measurement line 106 is 29.2 nm. The particle size of the composite particle of measurement line 108 is 31.5 nm. The particle size of the composite particles and the particle size of the mixed particles shown in FIG. 3 are both average particle sizes measured by the BET method.

[0048] Regarding the transmittance, 0.005 g of the powder of the composite particles of zirconium nitride and aluminum (ZrN+Al composite particles) to be measured as described above was weighed out, ethanol was added to make the total amount 50 g, and dispersion treatment was performed for 5 minutes using an ultrasonic device (Tetora150, manufactured by Nikkaki Bios Co., Ltd.). Next, 10 g was taken from the obtained solution, ethanol was added to make the total amount 50 g, and dispersion treatment was performed for 1 minute using an ultrasonic device to obtain a solution with a mass concentration of 20 ppm. The transmittance of the obtained solution was then measured using an ultraviolet-visible-near infrared spectrophotometer (V-670, manufactured by JASCO Corporation). The transmittance of mixed particles of zirconium nitride and aluminum nitride was also measured in the same manner as in the case of composite particles of zirconium nitride and aluminum.

[0049] The transmittances shown by the measurement lines 60, 62, 64, 66, 68, 70, 72, and 74 are those of composite particles within the scope of the present invention. The transmittances shown by the measurement lines 100, 102, 106, and 108 are those of composite particles outside the scope of the present invention. The transmittances shown by the measurement line 104 are those of mixed particles outside the scope of the present invention. The measurement lines 60, 62, 64, 66, 68, 70, 72, and 74 within the scope of the present invention have higher transmittance in the ultraviolet and near-infrared regions than the measurement lines 100, 102, 104, 106, and 108 outside the scope of the present invention. In addition, by changing the Al content in the range of 9.5 to 43 mass%, the transmittance can be changed while maintaining a high transmittance in the ultraviolet and near-infrared regions compared to the measurement lines 100, 102, 104, 106, and 108.

[0050] Next, the transmittance in the ultraviolet light region and the near infrared light region will be described. Figure 4 shows the transmittance ratio T at a wavelength of 365 nm relative to a wavelength of 600 nm for a composite particle of zirconium nitride and aluminum, and a mixed particle of zirconium nitride and aluminum nitride. UV , and the transmittance ratio T at a wavelength of 1100 nm IR Graph showing the above. In Fig. 4, ▲ indicates the transmittance ratio T UV indicates the transmittance ratio T IR The horizontal axis of FIG. 4 is the Al content (mass%), and the vertical axis is the transmittance ratio. The transmittance ratio is calculated based on the above-mentioned T UV and T IR It is. The transmittance ratio T UV and the transmittance ratio T IR is a value obtained by the following formula: Transmittance ratio T UV = (Transmittance at 365 nm wavelength) / (Transmittance at 600 nm wavelength) Transmittance ratio T IR = (Transmittance at wavelength 1100 nm) / (Transmittance at wavelength 600 nm)

[0051] As shown in FIG. 4, when the Al content is 9.5 to 43 mass %, the transmittance ratio T UV and the transmittance ratio T IR All of these values ​​exceed 1.40, and the film has high transmittance in the ultraviolet and near-infrared regions while maintaining high light-shielding properties in the visible light region. In addition, if the Al content is 14 to 38 mass %, the above-mentioned transmittance ratio T UV and the transmittance ratio T IR All of these values ​​exceed 1.60, and the transmittance in the ultraviolet and near infrared regions is further increased, so the Al content is preferably 14 to 38 mass %. Furthermore, if the Al content is 14 to 20 mass %, the above-mentioned transmittance ratio T UV is 1.90 or more, and the transmittance ratio T UV Therefore, the Al content is more preferably 14 to 20 mass %.

[0052] <Applications of composite particles> The applications of the composite particles will be described below. The composite particles can be used in applications requiring light shielding in the visible light region, such as black matrices for liquid crystal displays and organic electroluminescence displays. In such applications, some patterns are created on a substrate using photolithography technology, and photoresist resins that generate patterns using i-lines, which are one of the emission lines of high-pressure mercury lamps, are in widespread use. When the composite particles are dispersed in the photoresist resin, the composite particles do not absorb i-lines, so that the photochemical reaction of the photoresist resin is not hindered, and a pattern with good light shielding performance in the visible light region can be obtained on the substrate. In addition to the above, the composite particles can also be used in printing inks, inkjet inks, materials for producing photomasks, materials for producing printing proofs, etching resists, and solder resists.

[0053] In addition to the above, the composite particles can be used, for example, as a catalyst carrier. In this case, the particle size can be made small, thereby improving the performance of the catalyst. The present invention can also be used in photoelectric conversion elements and photothermal conversion elements. It can also be used as a pigment to adjust color tone by mixing with metals, oxides, plastics, etc. Other applications include electrical insulating materials such as semiconductor substrates, printed circuit boards, and various electrical insulating parts; high-hardness, high-precision machining materials such as cutting tools, dies, and bearings; functional materials such as grain boundary capacitors and humidity sensors; the manufacture of sintered bodies such as precision sintered molding materials; the manufacture of sprayed parts such as engine valves and other materials that require high-temperature abrasion resistance; and electrodes, electrolyte materials, and various catalysts for fuel cells. In this embodiment, since the particle size of the nitride fine particles can be made nano-sized, for example, when used for a sintered body, the sinterability can be improved and a sintered body with high strength can be obtained. As a result, for example, a tool with good cutting performance can be obtained.

[0054] The present invention is basically configured as described above. Although the composite particles of the present invention have been described in detail above, the present invention is not limited to the above-mentioned embodiment, and various improvements or modifications may be made without departing from the spirit and scope of the present invention. [Explanation of symbols]

[0055] 10 Fine particle manufacturing equipment (manufacturing equipment) 12 Plasma Torch 14 Material supply device 15 Primary fine particles 16 Chamber 18 Secondary fine particles 19. Cyclone 20 Collection Department 22 Plasma gas supply source 24 Hot Plasma Flame 28 Gas supply device 30 Vacuum Pump 50, 52, 60, 62, 64, 66, 68, 70, 72, 74 measurement lines 100, 102, 104, 106, 108 measurement lines

Claims

1. ZrN and Al are composited within a single particle, The particle size is 1 to 200 nm, The composite particles have an Al content of 22.3 to 43 mass %.

2. The composite particle according to claim 1, wherein the Al content is 22.3 to 38 mass %.

Citation Information

Patent Citations

  • JP1974031011A

  • Encapsulated nanoparticles for electromagnetic energy absorption

    JP2006523593A

  • Black color composite fine particle, black color resin composition, color filter substrate and liquid crystal display device

    JP2015227282A

  • Powder for forming black light-shielding film and manufacturing method therefor

    JP2019112275A

  • Zirconium nitride powder coated with alumina, and production method thereof

    JP2020158377A