Method for rendering slag harmless and method for producing low-carbon ferrochrome
By adjusting the basicity of slag to less than 1.2 and using a gas bottom blowing device, the method effectively converts hexavalent chromium to trivalent chromium, improving chromium yield and ensuring environmental compliance in low carbon ferrochrome production.
Patent Information
- Application Number
- JP2021533032
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-12
- Filing Date
- 2020-07-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-07-10
AI Technical Summary
The conventional method for producing low carbon ferrochrome generates harmful hexavalent chromium in the rejected slag due to high basicity, which poses environmental problems and reduces chromium yield.
The method involves adjusting the basicity of the slag to less than 1.2 and using a reducing agent to convert hexavalent chromium to trivalent chromium, while maintaining high thermal efficiency and reactivity through a gas bottom blowing device.
This approach prevents the generation of harmful hexavalent chromium, enhances chromium yield, and allows for the reuse of chromium-containing metal as a reducing agent, while meeting environmental standards.
Smart Images

Figure 0007566743000012 
Figure 0007566743000013 
Figure 0007566743000014
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for rendering slag harmless and a method for producing low-carbon ferrochrome. [Background technology]
[0002] Low-carbon ferrochrome, an Fe-Cr alloy containing 60% by mass or more of Cr and 0.1% by mass or less of C, is generally produced by reducing chromium ore with silicon. The so-called Perrin process is adopted as a specific production method. As shown in FIG. 9, the basic process of the Perrin process includes a first process in which chromium ore and quicklime are melted in an electric furnace, and a second process in which the melted raw material (hereinafter referred to as primary slag) melted in the first process is poured into a ladle, and silicochrome is added as a reducing agent in the ladle and stirred to cause a reduction reaction to produce low-carbon ferrochrome and reject slag (slag to be disposed of). The stirring in the second process is usually performed by relay rings in which two ladles are prepared and the molten primary slag containing silicochrome is repeatedly transferred from one to the other (see Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 1-225743 Summary of the Invention [Problem to be solved by the invention]
[0004] In the conventional method for producing low-carbon ferrochrome, the reduction reaction between chromium oxide in chromium ore and silicon proceeds as follows: Cr2O3+3 / 2Si→2Cr+3 / 2SiO2…(1) Here, the liberated SiO2 reacts with quicklime as shown in the following equations (2) and (3), producing reject slag. CaO+SiO2→CaO·SiO2…(2) 2CaO+SiO2→2CaO·SiO2…(3) When reject slag is generated as shown in equations (2) and (3), the amount of free SiO2 in equation (1) decreases, and the reduction reaction in equation (1) proceeds from left to right.
[0005] For low carbon ferrochrome products, there is a standard for the silicon content to be less than 1.0%, for example. For this reason, it is necessary to weakly reduce the primary slag with silicon so that silicon does not migrate to the low carbon ferrochrome. In order to advance the reduction reaction of formula (1) even with weak reduction, in the conventional manufacturing method of low carbon ferrochrome, the basicity of the discarded slag was increased to 1.7-2.0. This is because the higher the basicity, the less free SiO2 there is in formulas (2) and (3), and the more the reduction reaction of formula (1) advances.
[0006] However, increasing the basicity (CaO / SiO2) poses the problem of generating harmful hexavalent chromium in the rejected slag.
[0007] The present invention has been made in consideration of the above problems, and has an object to prevent harmful hexavalent chromium from being generated in rejected slag. [Means for solving the problem]
[0008] In order to solve the above problems, one aspect of the present invention is to charge slag containing chromium oxide and a reducing agent into an electric furnace or a reaction vessel, reduce the slag with the reducing agent to generate a chromium-containing metal and a reject slag, and reduce the chromium oxide content (Cr2O3 mass%) of the reject slag by 1.0 Mass % or less, basicity (CaO / SiO2) 1.2 Adjusted to less than The slag includes solidified slag, which is buried or temporarily stored within a plant and includes secondary slag produced in the operation of a method for producing low-carbon ferrochrome. This is a method for rendering slag harmless.
[0009] Another aspect of the present invention includes a first step of melting chromium ore and quicklime in an electric furnace, a second step of charging the melted raw material (hereinafter referred to as primary slag) melted in the first step and a reducing agent into a reaction vessel and reducing the primary slag with the reducing agent to generate low-carbon ferrochromium and secondary slag, and a third step of charging the secondary slag and the reducing agent into an electric furnace or a reaction vessel and reducing the secondary slag with the reducing agent to generate chromium-containing metal and reject slag, and the chromium oxide content (Cr2O3 mass%) of the reject slag is 1.0 Mass % or less, basicity (CaO / SiO2) 1.2 This is a method for producing low carbon ferrochromium by adjusting the temperature to less than 100°C. Effect of the Invention
[0010] The present invention One aspect of According to the report, the basicity of the rejected slag (CaO / SiO2) is 1.2 The chromium oxide content (Cr2O3 mass%) of the rejected slag is adjusted to less than 0.05%. This makes it possible to convert the harmful hexavalent chromium compounds in the rejected slag into harmless trivalent chromium compounds. 1.0 This is less than % by mass, and coupled with the fact that the amount of chromium in the rejected slag is originally small, it is possible to prevent harmful hexavalent chromium from being generated in the rejected slag. In addition, solidified slag, including secondary slag produced in the operation of the low-carbon ferrochrome manufacturing method, which is buried or temporarily stored within the plant, can be rendered harmless. According to another aspect of the present invention, the basicity of the rejected slag (CaO / SiO 2 ) is adjusted to less than 1.2, so that the harmful hexavalent chromium compounds in the rejected slag can be converted to harmless trivalent chromium compounds. 2 O 3 % by mass or less, which, combined with the fact that the chromium content of the rejected slag is originally low, can prevent harmful hexavalent chromium from being generated in the rejected slag generated in the manufacturing method for low-carbon ferrochromium. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a process diagram of a method for producing low-carbon ferrochromium according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram showing equipment used in the method for producing low carbon ferrochromium according to the present embodiment. [Diagram 3] 1 is a graph showing the relationship between the basicity (CaO / SiO2) of secondary slag and the (Cr) mass% of secondary slag. [Figure 4] FIG. 4 is a vertical sectional view of a reaction vessel used in the second step. [Diagram 5]1 is a graph showing the relationship between the (Cr) mass% of rejected slag and the [Si] mass% of recovered silicochromium. [Figure 6] 1 is a graph showing the relationship between the mass % (Cr) of the rejected slag, the basicity (CaO / SiO2) of the rejected slag, and the Cr6+ concentration (mg / l) of the rejected slag. [Figure 7] FIG. 1 is a process diagram of a slag detoxification method according to a first embodiment of the present invention. [Figure 8] FIG. 4 is a process diagram of a slag detoxification method according to a second embodiment of the present invention. [Figure 9] FIG. 1 is a process diagram of a conventional method for producing low carbon ferrochromium. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, the method for rendering slag harmless and the method for producing low-carbon ferrochrome according to the embodiment of the present invention will be described in detail with reference to the accompanying drawings. However, the method for rendering slag harmless and the method for producing low-carbon ferrochrome according to the present invention can be embodied in various forms and are not limited to the embodiments described in the present specification. The present embodiment is provided with the intention of enabling those skilled in the art to fully understand the invention by fully disclosing the specification. (Method of manufacturing low carbon ferrochrome)
[0013] Fig. 1 is a process diagram of a method for producing low-carbon ferrochromium according to one embodiment of the present invention, and Fig. 2 is a diagram showing equipment used in the method for producing low-carbon ferrochromium according to the present embodiment.
[0014] As shown in FIG. 1, the manufacturing method of low carbon ferrochrome of this embodiment includes a first step (S1) of melting a mixture of chromium ore and quicklime as a flux in an electric furnace to produce a molten raw material (hereinafter referred to as primary slag). As shown in FIG. 2, the chromium ore and quicklime are stored in a hopper 4. As the electric furnace 1, a fixed type electric furnace is used in which a tapping port 1a is provided at a position higher than the bottom of the furnace to form a basin. The tapping port 1a may be provided at the bottom of the furnace. The basin is formed in order to maintain a stable amount of heat even after the primary slag is tapped. The primary slag is tapped into a reaction vessel 2 from the tapping port 1a. The tapping temperature of the primary slag is a high temperature of 1400°C or more and 2000°C or less.
[0015] Next, as shown in Fig. 1, silicochrome as a reducing agent, additional ore, and recovered silicochrome are added to the reaction vessel 2 from which the primary slag was discharged. Then, the reaction vessel 2 is stirred by bottom-blowing inert gas, and the oxide of the chromium ore is reduced by the silicochrome to produce low-carbon ferrochrome and secondary slag. This reduction process is the second process (S2).
[0016] The additional ore is a raw material of chromium ore. The recovered silicochrome is the silicochrome recovered in the third step described later. As shown in FIG. 2, the reaction vessel 2 is a reaction vessel having a bottom gas blowing device 2a that blows in an inert gas from the bottom of the furnace.
[0017] In the conventional manufacturing method of chromium ore, in order to improve the chromium yield, the amount of lime was increased and the basicity of the secondary slag was raised to about 1.7 to 2.0. This is because the higher the basicity, the more secondary slag is generated as shown in the above formulas (2) and (3), and the reduction reaction of the above formula (1) progresses.
[0018] However, when the slag has a high basicity, the slag generally undergoes a powdering phenomenon after cooling, and an environmental problem occurs in that harmful hexavalent chromium is eluted from the slag. For this reason, in this embodiment, the upper limit of the basicity of the secondary slag in the second step (S2) is adjusted to be lower than 1.65, preferably lower than 1.5, and more preferably lower than 1.4. This is to adjust the basicity of the rejected slag in the third step described below to be lower than 1.3. The lower the lower limit of the basicity of the secondary slag, the more preferable it is, but in order to ensure reactivity in the third step (S3), the lower limit of the basicity of the secondary slag is set to 1.0 or more.
[0019] In this embodiment, the reaction vessel 2 having the bottom gas blowing device 2a with high stirring capacity is used, so that the thermal efficiency and reactivity of the reduction reaction can be improved. Therefore, even if the basicity is reduced to less than 1.65, the chromium yield can be prevented from decreasing. When the amount of quicklime is reduced and the basicity is lowered, the activity coefficient of SiO2 increases, the reduction reaction of chromium in the formula (1) becomes difficult to occur, and the (Cr) mass% of the secondary slag becomes high. However, as shown in FIG. 3, the reduction reaction progresses due to gas bubbling by the bottom gas blowing device, so that the (Cr) mass% of the secondary slag can be reduced. By reducing the (Cr) mass% of the secondary slag, advantageous operation can be performed.
[0020] Fig. 4 is a vertical cross-sectional view of a reaction vessel 2 having a bottom gas blowing device 2a. As shown in Fig. 4, refractories 8, 9 are provided on the bottom 6a of the steel shell 6 of the reaction vessel 2. A plug 19 of the bottom gas blowing device 2a is placed in the center of the bottom of the reaction vessel 2. When inert gas is introduced into the pipe portion 17 of the plug 19, the inert gas is blown into the reaction vessel 2 from the plug 19, and the molten metal in the reaction vessel 2 is stirred, i.e., gas bubbling is performed.
[0021] In the operation of the second step (S2), the reaction of formula (1) proceeds from the primary slag as described above. In the early stage of the operation, the primary slag is the main component in the reaction vessel 2. As the reaction proceeds, molten ferrochrome (metal 21) is produced, and the secondary slag 22 exists on the molten ferrochrome (metal 21). Eventually, the volume ratio of the secondary slag 22 to the metal 21 becomes approximately 4:1. In order to increase the reactivity in the presence of a large amount of highly viscous secondary slag 22, it is necessary to increase the stirring capacity, and for this purpose, a bottom gas blowing device 2a is used to blow inert gas into the bottom of the reaction vessel 2.
[0022] In general, when the molten metal is the main component, it is known that in order to increase the stirring capacity, it is good to arrange the plug 19 of the bottom gas blowing device 2a at a position offset from the center of the bottom of the reaction vessel 2 (eccentric position) (see, for example, JP-A-1-177333). However, when a large amount of highly viscous secondary slag 22 exists as in this embodiment, if the plug 19 of the bottom gas blowing device 2a is arranged at an eccentric position of the bottom of the reaction vessel 2, the side opposite to the side where the plug 19 is arranged will be in a weakly stirred state, and unmelted additional chromium ore will remain on the opposite side. In contrast, as in this embodiment, by arranging the plug 19 of the bottom gas blowing device 2a at the center of the bottom of the reaction vessel 2, a flow of molten metal is formed that rises from the center of the bottom in the reaction vessel 2 and then radially moves toward the periphery. Therefore, the inside of the reaction vessel 2 can be uniformly stirred, and the additional chromium ore can be entrained and melted. A plurality of plugs may be arranged on a circle centered on the center of the bottom of the reaction vessel 2. In this way, the inside of the reaction vessel 2 can be uniformly stirred.
[0023] Although the chromium yield is reduced, a top-blowing type reaction vessel into which an inert gas is blown in from a lance may be used as the reaction vessel for the second step, or two ladles may be used and relay ring may be performed between the two ladles.
[0024] In the second step (S2), silicochrome is used as the reducing agent, but a silicon-based reducing agent such as metal silicon may be used in addition to silicochrome. Also, an aluminum-based reducing agent such as aluminum or an aluminum alloy, a magnesium-based reducing agent such as magnesium or a magnesium alloy, or a calcium-based reducing agent such as calcium or a calcium alloy may be used in addition to the silicon-based reducing agent. Furthermore, a mixture of these reducing agents may be used.
[0025] As shown in Fig. 1, the molten low-carbon ferrochrome produced by the reduction reaction is poured into a mold to become a product. The low-carbon ferrochrome product contains 60 mass% or more of Cr, 1.0 mass% or less of Si, and 0.1 mass% or less of C. Meanwhile, the secondary slag produced by the reduction reaction is separated from the molten low-carbon ferrochrome and then charged into an electric furnace 3 (tilting type electric furnace, see Fig. 2) or a reaction vessel.
[0026] Next, as shown in Figures 1 and 2, ferrosilicon is charged as a reducing agent into the electric furnace 3 or reaction vessel in which the molten secondary slag is charged, and reacted with the chromium oxide remaining in the secondary slag to generate recovered silicochrome as a chromium-containing metal and reject slag (slag to be disposed of). This reduction process is the third process (S3).
[0027] In the third step, a large amount of ferrosilicon as a reducing agent, i.e., at least one time, preferably at least two times, the reduction equivalent of chromium oxide is added to perform strong reduction, and the chromium oxide content (Cr2O3 mass%) of the rejected slag is reduced to 1.4 mass% or less, preferably to 1.0 mass% or less. This is to reduce the hexavalent chromium content of the rejected slag and to improve the chromium yield. The Si content of the recovered silicochromium is 20 mass% or more and 70 mass% or less. As described later, reducing the chromium oxide content (Cr2O3 mass%) of the rejected slag to 1.4 mass% or less as in this embodiment means reducing the chromium content ((Cr) mass%) of the rejected slag to 1.4 mass% or less.
[0028] FIG. 5 is a graph showing the relationship between the chromium content ((Cr) mass%) of the rejected slag and the silicon content ([Si] mass%) of the recovered silico-chromium. As shown in FIG. 5, if the silicon content of the recovered silico-chromium is made 30 mass% or more (i.e., if the secondary slag is strongly reduced), the chromium content of the rejected slag can be made 1.0 mass% or less. If the silicon content of the recovered silico-chromium is less than 30 mass%, the chromium content of the rejected slag becomes high. Even if the silicon content of the recovered silico-chromium exceeds 60 mass%, the effect of reducing the chromium content of the rejected slag is small.
[0029] The basicity of the rejected slag is adjusted to be lower than 1.3, preferably lower than 1.2, and more preferably lower than 1.1. When the basicity is reduced, it is thought that the slag removes CaO from the hexavalent chromium compounds (CaO CrO3) that are bonded with CaO, and converts the hexavalent chromium compounds to trivalent chromium compounds (Cr2O3), as shown in the following equation (4). 2(CaO·CrO3)+2SiO2→2(CaO·SiO2)+Cr2O3+3 / 2O2…(4)
[0030] In addition, if the rejected slag has a high basicity, 2CaO·SiO2 is likely to be produced. This crystal form transitions from α, α', β, to γ, and during this transition, the unstable α' (specific gravity 3.31) changes to γ (specific gravity 2.69), causing a rapid volume expansion of about 12%. This causes powdering over time. This powdering phenomenon is an environmental problem. For this reason, the rejected slag is made low basicity, less than 1.3.
[0031] The lower limit of the basicity of the rejected slag is the better, but in order to reduce the chromium oxide content of the rejected slag, it is set to 0.7 or more, preferably 0.8 or more, and more preferably 0.9 or more. In order to adjust the basicity to a lower level, silica (SiO2) may be charged as an auxiliary raw material into the electric furnace 3 as necessary.
[0032] The third step (S3) is carried out while maintaining the temperature of the molten metal of the recovered silicochrome and the rejected slag at 1250° C. or higher. If the temperature of the molten metal is lower than 1250° C., the third step is carried out in an electric furnace 3 or a reaction vessel equipped with a heating means.
[0033] The recovered silicochrome is charged into the reaction vessel 2 together with the silicochrome. Since a part of the silicochrome is replaced by the recovered silicochrome, the amount of silicochrome is reduced. The recovered silicochrome may be charged into the electric furnace 3 or reaction vessel in the third step (S3) and used as a partial replacement for ferrosilicon. The rejected slag is a harmless slag, and is used as roadbed material or fertilizer, or is buried in a factory. The amount (concentration) of hexavalent chromium eluted from the rejected slag is 0.05 mg / l or less.
[0034] In the third step, an electric furnace 3 or a reaction vessel may be used. A bottom gas blowing device may be provided in the electric furnace 3. The reaction vessel may be a reaction vessel having a bottom gas blowing device, or may be a top-blown reaction vessel into which an inert gas is blown from a lance. The bottom gas blowing device provided in the electric furnace 3 or reaction vessel is preferably disposed in the center of the bottom of the electric furnace 3 or reaction vessel, similar to the bottom gas blowing device 2a of the reaction vessel 2 in the second step described above. The volume ratio of slag to metal in the second step is about 4:1, whereas the volume ratio of slag to metal in the third step is about 10:1. In order to increase the stirring force of the molten metal in the third step, it is preferable to make the amount of stirring gas (l / min) per ton of molten metal in the third step larger than the amount of stirring gas (l / min) per ton of molten metal in the second step.
[0035] The secondary slag may include solidified slag that has been buried in a factory or temporarily stored in a factory and solidified. The solidified slag includes secondary slag produced in a previous operation of a low-carbon ferrochromium production method (secondary slag produced by relay ring using two conventional ladles and / or secondary slag produced by gas bubbling using the reaction vessel 2 of this embodiment), and contains chromium oxide. The chromium oxide content of the solidified slag may be 1.4 mass% or more. When the solidified slag is added to the secondary slag, the third step is performed in an electric furnace 3 or a reaction vessel equipped with a heating means, and the molten secondary slag is kept warm and the solidified slag is remelted. The solidified slag may be added to the electric furnace 1 that produces the primary slag.
[0036] In the above embodiment, ferrosilicon is used as the reducing agent in the third step, but a silicon-based reducing agent such as metal silicon may be used in addition to ferrosilicon. Also, an aluminum-based reducing agent such as aluminum or an aluminum alloy, a magnesium-based reducing agent such as magnesium or a magnesium alloy, or a calcium-based reducing agent such as calcium or a calcium alloy may be used in addition to a silicon-based reducing agent. Furthermore, a mixture of these reducing agents may be used.
[0037] A method for quantifying the chromium oxide content of the slag and a method for quantifying the basicity of the slag will be described. The chromium oxide content of the slag is the Cr content of the slag converted into oxide. Specifically, the total amount of chromium oxide is Cr2O3, and the chromium oxide content = Cr content x 152 / 104. In this embodiment, the chromium oxide content of the rejected slag is set to 1.4 mass% or less, which means that the chromium content of the rejected slag is set to 1.4 x 104 / 152 = 0.96 ≒ 1 mass% or less. The chromium content of the slag is expressed as ((Cr) mass%). The chromium oxide content of the slag is expressed as (Cr2O3 mass%). The Cr content of the slag is quantified by ICP (Inductively Coupled Plasma) emission spectroscopy. In this analysis method, the decomposition of the sample is based on "JIS G1313-1 2012 Decomposition by Alkali Fusion".
[0038] The basicity of slag (CaO / SiO2) is expressed as the CaO content of slag / SiO2 content of slag. The CaO content of slag is the Ca content of slag converted into oxide, and is calculated as CaO content = Ca content x 56 / 40. The SiO2 content of slag is the Si content of slag converted into oxide, and is calculated as SiO2 content = Si content x 60 / 28. The method for quantifying Ca and Si in slag is ICP (Inductively Coupled Plasma) emission spectrometry. In this analysis method, the sample is decomposed according to "JIS G1313-1 2012 Decomposition by alkali fusion".
[0039] Figure 6 is a graph showing the relationship between the chromium content ((Cr) mass%) of the rejected slag, the basicity (CaO / SiO2) of the rejected slag, and the concentration (mg / l) of hexavalent chromium in the rejected slag. As shown in Figure 6, by setting the chromium content ((Cr) mass%) of the rejected slag to 1 mass% or less, i.e., by setting the chromium oxide content (Cr2O3 mass%) to 1.4 mass% or less and adjusting the basicity (CaO / SiO2) to 0.9 to 1.3, the concentration of hexavalent chromium in the rejected slag can be reduced to 0.04 (mg / l) or less. This value meets the environmental standards set out in Notification No. 46 of the Environment Agency.
[0040] On the other hand, when the basicity (CaO / SiO2) is 1.4 to 1.6, the chromium content ((Cr) mass%) of the rejected slag must be maintained below 0.3 in order to reduce the concentration of hexavalent chromium to 0.04 (mg / l) or less, which makes stable operation impossible. Also, when the basicity (CaO / SiO2) is 1.7 or more, the rejected slag disintegrates after cooling.
[0041] To analyze and measure the concentration (mg / l) of hexavalent chromium, the elution test of hexavalent chromium in accordance with Notification No. 46 of the Environment Agency, August 1991, is used. Notification No. 46 stipulates that the concentration of hexavalent chromium should be 0.05 (mg / l) or less as a desirable standard ("environmental standard") to be maintained in order to protect human health and preserve the living environment. Table 1 shows the test method for the elution test stipulated in Notification No. 46 of the Environment Agency. [Table 1]
[0042] The method for rendering slag harmless and the method for producing low-carbon ferrochrome according to the present embodiment have been described above. The method for rendering slag harmless and the method for producing low-carbon ferrochrome according to the present embodiment have the following advantages.
[0043] The basicity of the rejected slag is less than 1.3, so that the harmful hexavalent chromium compounds in the rejected slag can be converted to harmless trivalent chromium compounds. The chromium oxide content of the rejected slag is 1.4 mass% or less, and this, combined with the fact that the amount of chromium in the rejected slag is originally small, can prevent the generation of harmful hexavalent chromium in the rejected slag.
[0044] In the second step, the primary slag and the reducing agent are charged into the reactor 2 equipped with a bottom gas blowing device, and the mixture is stirred by blowing in an inert gas from the bottom of the reactor 2. This improves the thermal efficiency and reactivity, and prevents a decrease in the chromium yield even if the basicity is adjusted to a low level of less than 1.65.
[0045] In the third step (S3), silica stone is charged as an auxiliary raw material into the electric furnace 3 or the reaction vessel, so that the basicity of the rejected slag can be easily adjusted to less than 1.3.
[0046] In the third step (S3), solidified slag is added to the secondary slag, so that, for example, solidified slag that has been buried or temporarily stored in a factory can be rendered harmless.
[0047] In the third step (S3), the melting of the solidified slag and the reduction of the melted solidified slag are carried out in an electric furnace, so that the reactivity of the reduction reaction can be improved.
[0048] Since the chromium-containing metal (recovered silicochromium) obtained in the third step is reused as at least a part of the reducing agent in the second step, the chromium yield can be increased.
[0049] In the third step (S3), a reducing agent is charged in an amount equal to or more than one time the reduction equivalent of the chromium oxide to perform strong reduction, so that the chromium oxide content of the rejected slag can be easily reduced to 1.4 mass% or less, and the chromium yield can be improved.
[0050] In the third step (S3), the temperature of the molten metal is kept at 1250°C or higher, so that the reactivity of the reduction reaction can be improved when reducing the secondary slag. Therefore, even if the basicity is lowered to less than 1.3, the chromium yield can be prevented from decreasing. (Method of rendering slag harmless)
[0051] FIG. 7 is a process diagram of the slag detoxification method according to the first embodiment of the present invention. Solidified slag, a reducing agent, and auxiliary materials are charged into an electric furnace. The solidified slag is as described above. The reducing agent is a silicon-based reducing agent, an aluminum-based reducing agent, a magnesium-based reducing agent, a calcium-based reducing agent, or a mixture of these reducing agents. The reducing agent is added in an amount at least one time, and preferably at least two times, the reduction equivalent of the chromium oxide and iron oxide in the solidified slag. The auxiliary materials are silica, quicklime, etc., and are used to adjust the basicity of the rejected slag.
[0052] In the electric furnace, the solidified slag, reducing agent, and auxiliary materials are melted, and the melted solidified slag is reduced by the reducing agent to produce chromium-containing metals and reject slag (S11). The chromium oxide content of the reject slag is adjusted to 1.4 mass% or less, and the basicity is adjusted to less than 1.3.
[0053] By adjusting the chromium oxide content of the rejected slag to 1.4 mass% or less and the basicity (CaO / SiO2) of the rejected slag to less than 1.3, the hexavalent chromium concentration of the rejected slag can be reduced to 0.04 (mg / l) or less, similar to S3 of the first embodiment. Therefore, for example, harmful solidified slag that is buried or temporarily stored in a factory can be converted into harmless rejected slag. In addition, the generated chromium-containing metal can be reused as a reducing agent.
[0054] As shown by the dashed line in Fig. 7, the secondary slag generated in the method for producing low carbon ferrochromium according to the present embodiment may be charged into an electric furnace. Also, a bottom gas blowing device may be provided in the electric furnace.
[0055] 8 is a process diagram of a slag detoxification method according to a second embodiment of the present invention. In the slag detoxification method according to the first embodiment, the solidified slag is melted in an electric furnace (S11) and the melted slag is reduced in a reaction vessel (S22). In contrast, in the slag detoxification method according to the second embodiment, the solidified slag is melted in an electric furnace (S21) and the melted solidified slag is reduced in a reaction vessel (S22).
[0056] The electric furnace is charged with auxiliary materials such as silica, quicklime, etc., which are used to adjust the basicity of the solidified slag and the reject slag. The electric furnace melts the solidified slag and auxiliary materials (S21). The melted solidified slag and auxiliary materials are tapped from the electric furnace into a reaction vessel. The reaction vessel may be two ladles that perform relay ring, a reaction vessel with a bottom gas blowing device, or a top-blowing reaction vessel.
[0057] In the reaction vessel, the dissolved solidified slag is reduced by a reducing agent to produce chromium-containing metals and reject slag (S22). The chromium oxide content of the reject slag is adjusted to 1.4 mass% or less and the basicity is adjusted to less than 1.3.
[0058] According to the slag detoxifying method of the second embodiment, the same effects as those of the slag detoxifying method of the first embodiment are achieved.
[0059] As shown by the dashed line in Fig. 8, the secondary slag generated in the method for producing low carbon ferrochromium according to the present embodiment may be charged into an electric furnace. After melting and reducing the slag including the solidified slag in the electric furnace, the final reduction of the molten slag may be performed in a ladle as a reaction vessel. Furthermore, the electric furnace may be provided with a bottom gas blowing device. Example 1
[0060] Low carbon ferrochrome was produced according to the production process diagram in Figure 1. Table 2 shows the composition of the chromium ore, which was the raw material used in this example.
[0061] [Table 2]
[0062] 1750kg of chromium ore and 830kg of lime were charged into a stationary electric furnace and melted to produce the primary slag. The primary slag was poured into a reaction vessel, into which 310kg of silicochrome and 260kg of recovered silicochrome were charged. Argon gas was then blown into the reaction vessel from the bottom and the mixture was stirred. The secondary slag was separated, and the resulting molten low-carbon ferrochrome (1000kg) was cast into a mold to produce the product. Table 3 shows the composition of the product low-carbon ferrochrome.
[0063] [Table 3]
[0064] Meanwhile, the separated secondary slag was tapped into an electric furnace and 230 kg of ferrosilicon was charged. The resulting rejected slag and recovered silicochrome were then separated, yielding 1930 kg of rejected slag and 260 kg of recovered silicochrome. This recovered silicochrome was added to the primary slag together with the silicochrome. Table 4 shows the composition of the rejected slag, and Table 5 shows the composition of the recovered silicochrome.
[0065] [Table 4]
[0066] [Table 5]
[0067] As shown in Table 4, the basicity of the rejected slag was 37.0 / 36.5 ≒ 1.01. The rejected slag did not naturally disintegrate after cooling, and no elution of hexavalent chromium was confirmed. As shown in Table 6, a high chromium retention rate of over 97% was obtained. [Table 6] Example 2
[0068] As in Example 1, reject slag was produced according to the manufacturing process diagram in FIG. 1. Table 7 shows the basicity (CaO / SiO2) and chromium oxide content (C r2 The figures show the amount of hexavalent chromium (mass%) and the amount of hexavalent chromium eluted (concentration (mg / l)). In runs 1 to 4, hexavalent chromium was not detected, and in run 5, it was at the detection limit. [Table 7] (Conventional example)
[0069] Low carbon ferrochrome was produced according to the production process diagram in Fig. 9. This low carbon ferrochrome production process differs from the present embodiment in that the reduction of the primary slag is performed by relay ring and that the silicochrome is not recovered from the secondary slag and added to the primary slag. Table 8 shows the composition of the chromium ore, which is the raw material used in the conventional example.
[0070] [Table 8]
[0071] 1740kg of chromium ore and 1060kg of quicklime were charged into an electric furnace and melted to produce the primary slag. The primary slag was poured into a ladle, and 600kg of silicochrome was added to it. It was then stirred with a relay ring. 2200kg of the resulting rejected slag was separated, and the resulting molten low-carbon ferrochrome (1000kg) was cast into a mold to produce the product. Table 9 shows the composition of the product low-carbon ferrochrome, and Table 10 shows the composition of the rejected slag.
[0072] [Table 9]
[0073] [Table 10]
[0074] As shown in Table 10, in the conventional example, the chromium oxide content of the rejected slag was high at 5.9%, and the basicity was also high at 1.70. As shown in Table 11, the chromium retention rate was low at 85%. Harmful hexavalent chromium was generated in the rejected slag. [Table 11]
[0075] This specification is based on Japanese Patent Application No. 2019-130323, filed on July 12, 2019, the entire contents of which are incorporated herein by reference. [Explanation of symbols]
[0076] S1…1st process S2…Second process S3…3rd process S11: Melting and reducing process of solidified slag S21: Melting process of solidified slag S22: Reduction process of molten solidified slag 3. Electric furnace
Claims
1. A slag containing chromium oxide and a reducing agent are charged into an electric furnace or a reaction vessel, and the slag is reduced with the reducing agent to produce a chromium-containing metal and a reject slag; The chromium oxide content of the rejected slag (Cr 2 O 3 mass%) is 1.0 mass% or less, and basicity (CaO / SiO 2 ) to less than 1.2, The slag comprises solidified slag; The solidified slag is buried or temporarily stored within a plant, and the method for rendering slag harmless includes secondary slag produced in the operation of a method for producing low-carbon ferrochrome.
2. 2. The method for rendering slag harmless according to claim 1, wherein the melting and reduction of the slag including the solidified slag is carried out in the electric furnace.
3. 2. The method for rendering slag harmless according to claim 1, wherein the slag including the solidified slag is melted in the electric furnace or the reaction vessel, and the melted slag is reduced in the reaction vessel.
4. The slag is added to the reject slag. 2 4. The method for rendering slag harmless according to claim 1, further comprising the step of adding an auxiliary material for adjusting the temperature of slag.
5. A first step of melting chromium ore and quicklime in an electric furnace; A second step of charging the melted raw material (hereinafter referred to as primary slag) melted in the first step and a reducing agent into a reaction vessel, and reducing the primary slag with the reducing agent to generate low carbon ferrochrome and secondary slag; and a third step of charging the secondary slag and a reducing agent into an electric furnace or a reaction vessel, and reducing the secondary slag with the reducing agent to generate a chromium-containing metal and a reject slag. The chromium oxide content of the rejected slag (Cr 2 O 3 mass%) is 1.0 mass% or less, and basicity (CaO / SiO 2) to less than 1.
2.
6. 6. The method for producing low carbon ferrochromium according to claim 5, wherein in the second step, the primary slag and the reducing agent are charged into the reaction vessel having a bottom gas blowing device, and are stirred by blowing in an inert gas from the bottom of the reaction vessel.
7. The reducing agent charged in the second step is a silicon-based, aluminum-based, magnesium-based, or calcium-based reducing agent, or a mixture thereof; 7. The method for producing low carbon ferrochromium according to claim 5, wherein the reducing agent charged in the third step is a silicon-based, aluminum-based, magnesium-based, or calcium-based reducing agent, or a mixture thereof.
8. In the third step, the secondary slag is added to the reject slag. 2 8. The method for producing low carbon ferrochromium according to claim 5, further comprising the step of adding an auxiliary material for adjusting the temperature of the ferrochromium.
9. 9. The method for producing low carbon ferrochromium according to claim 5, wherein in the third step, solidified slag is added to the secondary slag.
10. 10. The method for producing low carbon ferrochromium according to claim 9, wherein the melting and reduction of the secondary slag including the solidified slag is performed in the electric furnace.
11. 10. The method for producing low carbon ferrochromium according to claim 9, wherein the secondary slag including the solidified slag is melted in the electric furnace, and the melted secondary slag is reduced in a reaction vessel.
12. The method for producing low carbon ferrochromium according to any one of claims 5 to 11, characterized in that the chromium-containing metal obtained in the third step is reused as at least a part of the reducing agent in the second step and / or the third step.
13. 13. The method for producing low carbon ferrochromium according to claim 5, wherein the reducing agent is charged in an amount equal to or more than one time the reducing equivalent of chromium oxide in the third step.
14. 14. The method for producing low carbon ferrochromium according to claim 5, wherein in the third step, the temperature of the molten metal containing chromium and the rejected slag is 1250° C. or higher.
Citation Information
Patent Citations
Process for recovering low carbon ferroo chromium slag
JP1977010816A
Manufacture of low-nitrogen and low-carbon ferrochrome
JP1987037340A
Desulfurization of ferrochromium
JP1989215950A
Manufacture of low-carbon ferrochrome
JP1989225743A
Production of low-carbon ferrochromium