Solid electrolyte, solid electrolyte battery and its manufacturing method

The laminated structure of plate-like particles in the solid electrolyte battery addresses dendrite formation and cracking issues, enhancing safety and performance by creating a labyrinth effect and improving structural integrity.

JP7567108B2Active Publication Date: 2024-10-16SHINSHU UNIVERSITY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020176758
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-25
Filing Date
2020-10-21
Publication Date
2024-10-16
Estimated Expiration
2040-10-21

AI Technical Summary

Technical Problem

Conventional solid electrolyte batteries face issues with dendrite formation and cracking due to mechanical shocks, leading to potential short circuits and reduced reliability, especially in applications requiring high performance and safety.

Method used

A solid electrolyte is designed with a laminated structure of plate-like particles having specific length-to-width and width-to-thickness ratios, arranged to form a sintered masonry body, which suppresses dendrite growth and crack propagation by creating a labyrinth effect and enhancing structural integrity.

Benefits of technology

The laminated structure effectively prevents internal short circuits and enhances the mechanical robustness of the solid electrolyte battery, improving safety and performance by reducing dendrite growth and crack propagation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567108000002
    Figure 0007567108000002
  • Figure 0007567108000003
    Figure 0007567108000003
  • Figure 0007567108000004
    Figure 0007567108000004
Patent Text Reader

Abstract

To provide a solid electrolyte and a solid electrolyte battery which are hardly damaged, and a method for manufacturing such a solid electrolyte battery.SOLUTION: A solid electrolyte of the present invention comprises a sintered product of a masonry material formed by a plurality of plate-like particles of a material having an ion conductivity, which are stacked in a plate-thickness direction of the plate-like particles and which are arrayed along a direction in which the plate-like particles extend. The plate-like particle has a ratio of vertical and horizontal length of 1-3:1, and a ratio of the horizontal length and plate thickness of 1.3-4:1. A solid electrolyte battery of the present invention is formed by use of the solid electrolyte of the invention. A manufacturing method of the present invention comprises: dispersing powder of the plate-like particles in a dispersion medium to prepare a paste; coating a coating face with the paste while applying a shear stress thereto; and sintering a coated body.SELECTED DRAWING: Figure 22
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solid electrolyte, a solid electrolyte battery, and a method for producing the same. [Background technology]

[0002] Lithium ion secondary batteries are increasingly being used as power sources for small devices such as mobile phones and laptops. Lithium ion secondary batteries have a positive electrode and a negative electrode that have active materials capable of reversibly inserting and removing lithium ions, and a non-aqueous electrolyte in which a supporting salt is dissolved in an organic solvent.

[0003] Lithium-ion secondary batteries are being considered for use as medium- to large-scale power sources for automobiles, power storage, etc. As the range of applications for lithium-ion secondary batteries expands to medium- to large-scale power sources, there is a demand for even higher performance.

[0004] Conventional lithium-ion secondary batteries have had safety and reliability concerns due to leakage of non-aqueous electrolytes, etc. In response to these concerns, development of solid electrolyte batteries (also called all-solid-state batteries) that use solid electrolytes made of solid materials instead of non-aqueous electrolytes is underway.

[0005] In conventional solid electrolyte batteries, the solid electrolyte between the positive and negative electrodes is manufactured by molding and sintering material powder. The solid electrolyte is a sintered body, and has dense and high strength properties. However, in conventional solid electrolyte batteries, as in the case of lithium ion secondary batteries using non-aqueous electrolytes, there is a risk of dendrites forming in the negative electrode. When dendrites form and grow, a conductive path is formed inside the solid electrolyte between the positive and negative electrodes, causing a problem of a short circuit between the two electrodes.

[0006] Furthermore, conventional solid electrolyte batteries have a problem in that, depending on the environment in which they are used, the solid electrolyte can be damaged by shocks such as vibrations, and as the damage progresses, cracks can form in the solid electrolyte.

[0007] As described above, conventional solid electrolytes have the problem of damage such as dendrites and cracks. Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a solid electrolyte, a solid electrolyte battery, and a method for manufacturing a solid electrolyte battery that are less susceptible to damage. [Means for solving the problem]

[0009] In order to solve the above problems, the present inventors have conducted extensive research into the structure of solid electrolytes and have completed the present invention.

[0010] The solid electrolyte of the present invention is comprised of a sintered laminate formed by stacking a plurality of plate-like particles made of an ion-conductive material in the thickness direction of the plate-like particles and arranging the plate-like particles along the direction in which the plates extend, and is characterized in that the plate-like particles have a length:width ratio of 1 to 3:1 and a width:thickness ratio of 1.3 to 4:1.

[0011] The solid electrolyte battery of the present invention is characterized by comprising: the solid electrolyte according to any one of claims 1 to 5; a positive electrode provided in close contact with one surface of the solid electrolyte in the thickness direction; and a negative electrode provided in close contact with the other surface of the solid electrolyte in the thickness direction.

[0012] The method for producing a solid electrolyte of the present invention is characterized by comprising a preparation step of preparing a paste by dispersing a powder of plate-like particles made of an ionically conductive material in a dispersion medium, a coating step of coating the paste onto a coated surface while applying a shear stress along the coated surface, and a sintering step of sintering the coated body.

[0013] The solid electrolyte of the present invention is a sintered body of a stack of plate-like particles. The sintered body has a partially different crystal structure, and the structure related to the difference cannot be generally specified. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a schematic diagram showing the peripheral shape of a plate-like particle. [Diagram 2] FIG. 2 is a schematic diagram showing a method for approximating the shape of a plate-like particle. [Diagram 3] FIG. 2 is a schematic diagram showing a method for approximating the shape of a plate-like particle. [Figure 4] FIG. 2 is a schematic diagram showing a method for approximating the shape of a plate-like particle. [Diagram 5] FIG. 2 is a schematic cross-sectional view showing the arrangement of plate-like particles in a masonry body. [Figure 6] FIG. 2 is a side view showing the overlap of plate-like particles in a masonry structure. [Figure 7] FIG. 2 is a side view showing the overlap of plate-like particles in a masonry structure. [Figure 8] FIG. 2 is a side view showing the overlap of plate-like particles in a masonry structure. [Figure 9] 2 is a cross-sectional view showing the growth of dendrites in the solid electrolyte of the first embodiment. FIG. [Figure 10] FIG. 1 is a cross-sectional schematic diagram showing the growth of dendrites in a conventional solid electrolyte. [Figure 11] FIG. 1 is a schematic diagram showing the configuration of a lithium ion secondary battery according to a first embodiment. [Figure 12] 1 is a process diagram showing a method for producing a lithium ion secondary battery according to a first embodiment. [Figure 13] 1 is an enlarged photograph of K4Nb6O17, an intermediate product in the production of embodiment 1. [Figure 14] 1 is an enlarged photograph of K4Nb6O17, an intermediate product in the production of embodiment 1. [Figure 15] 1 is an enlarged photograph of H4Nb6O17, an intermediate product in the production of embodiment 1. [Figure 16] 1 is an enlarged photograph of H4Nb6O17, an intermediate product in the production of embodiment 1. [Figure 17] 1 is an enlarged photograph of LiNbO3 of the first embodiment. [Figure 18] 1 is an enlarged photograph of LiNbO3 of the first embodiment. [Figure 19] FIG. 2 is a process diagram showing the configuration of a bar coater. [Figure 20] 1 is an enlarged photograph of the LiNbO3 laminate of the first embodiment before compression. [Figure 21] 1 is an enlarged photograph of a cross section of a compressed masonry body of embodiment 1. [Figure 22] 1 is an enlarged photograph of a cross section of the solid electrolyte of embodiment 1. [Diagram 23] 5 is a process diagram showing a method for producing a lithium ion secondary battery according to a second embodiment. FIG. [Figure 24] FIG. 11 is a cross-sectional view showing the configuration of a lithium-ion secondary battery according to a third embodiment. [Diagram 25] 10 is a process diagram showing a method for producing a lithium ion secondary battery according to a third embodiment. FIG. [Figure 26] FIG. 11 is a process diagram showing a method for producing a lithium ion secondary battery according to a fourth embodiment. [Figure 27] FIG. 11 is a cross-sectional view showing the configuration of a positive electrode of a lithium-ion secondary battery according to a fifth embodiment. [Figure 28] This is an enlarged photograph of a plate-like particle composed of Li3xLa(2 / 3)-x□(1 / 3)-2xTiO3. [Figure 29] 1 is an enlarged photograph of a plate-like particle made of Li2TiO3. [Diagram 30] 1 is an enlarged photograph of a plate-like particle made of Na2Ti3O7. [Diagram 31] 1 is an enlarged photograph of a plate-like particle made of K4Nb6O17. [Diagram 32] 1 is an enlarged photograph of a plate-like particle made of KTiNbO5. [Diagram 33] 1 is an enlarged photograph of a plate-like particle made of LaOCl. [Diagram 34] 4 is a cross-sectional view showing the effect of suppressing the propagation of a crack in a solid electrolyte according to an embodiment. FIG. [Diagram 35] FIG. 1 is a schematic cross-sectional view showing the propagation of a crack in a conventional solid electrolyte. [Diagram 36]1 is an enlarged photograph of a cross section of the compressed masonry body of Example 1. [Figure 37] 1 is an enlarged photograph of a cross section of the compressed masonry body of Comparative Example 1. [Figure 38] FIG. 2 is a diagram showing the results of measuring the impedance of the solid electrolyte of Example 1. [Figure 39] FIG. 2 is a circuit diagram showing an equivalent circuit in measuring the impedance of a solid electrolyte. [Diagram 40] FIG. 4 is a diagram showing test results of a constant current cycle test of the battery cell of Example 1. [Diagram 41] FIG. 13 is a diagram showing test results of a constant current cycle test of the battery cell of Comparative Example 1. [Diagram 42] FIG. 13 is a diagram showing test results of a constant current cycle test on the battery cell of Comparative Example 2. [Diagram 43] 1 is an enlarged photograph of a cross section of the compressed masonry of Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will be specifically described below using the embodiments. Note that each embodiment shows a specific embodiment of the present invention, and the present invention is not limited to only these embodiments. In other words, the present invention includes embodiments in which the matters described in these embodiments are appropriately combined.

[0016] [Embodiment 1] The present embodiment relates to a solid electrolyte made of LiNbO3, a lithium ion secondary battery using the same, and a method for manufacturing the same.

[0017] [Solid electrolyte] The solid electrolyte of this embodiment is made of a sintered laminate formed by arranging a plurality of plate-like particles in a predetermined state, and the plate-like particles have a length:width ratio of 1 to 3:1 and a width:plate thickness ratio of 1.3 to 4:1. The plate-like particles are made of a material having ion conductivity. The laminate is formed by stacking a plurality of plate-like particles in the plate thickness direction and arranging (or oriented) along the direction in which the plates extend.

[0018] When the multiple plate-like particles are formed into a laminate, adjacent plate-like particles are arranged in close proximity to each other so as to be sinterable, and it is preferable that adjacent plate-like particles are arranged in abutting contact with each other.

[0019] The plate-like particles are made of LiNbO3. LiNbO3 is a material with ionic conductivity. LiNbO3 is a material that is electrically conductive by Li ions (Li + ) is conducted.

[0020] The plate-like particles are preferably single crystal primary particles. The plate-like particles are preferably primary particles of crystals that have developed into a planar plate shape. When the plate-like particles are single crystal primary particles, a laminate arranged in a predetermined state can be formed.

[0021] The solid electrolyte of this embodiment is a sintered body formed by sintering a stack of plate-like particles made of LiNbO3, and is composed of LiNbO3 as a whole. The solid electrolyte (sintered body) of this embodiment has ionic conductivity to Li ions. Specifically, the sintered body is formed by causing a sintering reaction in the stack of plate-like particles. The sintering reaction is a reaction in which adjacent plate-like particles are bonded to each other by causing atomic diffusion. In the sintering reaction, there is no reaction in which the plate-like particles react with other components to produce a new compound, and no decomposition reaction in which the compound of the plate-like particles is thermally decomposed. In other words, even after the sintering reaction, the composition of the material of the plate-like particles of the stack and the characteristic of having ionic conductivity are maintained. As a result, the solid electrolyte (sintered body) of this embodiment is composed of LiNbO3 as a whole and has ionic conductivity.

[0022] In this embodiment, the plate-like particle is a particle having a plate-like shape when observing the particle shape (shape of a primary particle) using an apparatus such as an SEM. The plate-like shape has one surface (hereinafter also referred to as the upper surface), the other surface (hereinafter also referred to as the lower surface) facing away from the one surface (upper surface), and an outer peripheral surface (hereinafter also referred to as the side surface) connecting the one surface (upper surface) and the other surface (lower surface). As shown in FIG. 1, the plate-like particle has a shape in which the plate thickness is the smallest (thinnest) among the lengths of the vertical (a), horizontal (b), and plate thickness (c), and has a relationship of plate thickness (c)<horizontal (b)≦vertical (a).

[0023] The plate-like particles have a length ratio of length (a):width (b) of 1 to 3:1, and a length ratio of width (b):plate thickness (c) of 1.3 to 4:1. The length ratios of the length, width, and plate thickness of the particle shape of the plate-like particles are the length ratios of the peripheral shape of a rectangular parallelepiped plate-like particle. When the plate-like particles have this length ratio, a masonry body can be easily manufactured, for example, using the steps of the manufacturing method described below.

[0024] As shown in FIG. 1, the plate-like particles preferably have a rectangular parallelepiped outer periphery.

[0025] When the peripheral shape of the plate-like particle is not a rectangular parallelepiped shape, the above-mentioned ratio of length:width:plate thickness can be substituted with the ratio of the external length of an approximate rectangular parallelepiped shape. The approximate rectangular parallelepiped shape can be selected from a rectangular parallelepiped circumscribing the plate-like particle (exemplified in a top view in FIG. 2), a rectangular parallelepiped inscribing the plate-like particle (exemplified in a top view in FIG. 3), and a rectangular parallelepiped formed by averaging the longest and shortest parts of the length, width, and plate thickness of the plate-like particle (exemplified in a top view in FIG. 4). Furthermore, the approximate rectangular parallelepiped shape may be approximated by the above-mentioned separate conditions for each of the length, width, and plate thickness of the plate-like particle. The length ratio of the length, width, and plate thickness in this embodiment is the length ratio approximated by a rectangular parallelepiped circumscribing the plate-like particle (FIG. 2).

[0026] When the plate-like particles have a peripheral shape other than a rectangular parallelepiped shape, any shape having the above ratio may be used, and examples of the peripheral shape include film-like, sheet-like, and flake-like shapes.

[0027] The plate-like particles preferably have an average particle size (D50) of 2.0 μm to 8.0 μm. When the average particle size (D50) of the plate-like particles falls within this range, a laminate in which a plurality of plate-like particles are arranged in a predetermined state can be easily formed.

[0028] The average particle size of the plate-like particles can be measured using a conventional particle size distribution measuring device (e.g., a measuring device for a measuring method such as a dynamic light scattering method, a laser diffraction method, an image imaging method, a gravitational sedimentation method, etc.). In this embodiment, the values ​​of D50, D25, D75, etc. when measuring the particle size distribution of the plate-like particles correspond to the length of the longest side (i.e., the length of the length (a)) among the lengths of the length (a), width (b), and plate thickness (c) of the rectangular parallelepiped shape of the plate-like particles.

[0029] When the particle size distribution of the plate-like particles is measured, the length between the 25% cumulative value (D25) and the 75% cumulative value (D75) from the small diameter is preferably 34 to 230% of the length of the average particle diameter (D50). When the length between D25 and D75 is within this range, the plate-like particles are arranged in such a way that the maze effect described below can be more reliably exhibited in the masonry body.

[0030] Specifically, when the length between D25 and D75 is within this range, the plate-like particles (powder of plate-like particles) for forming the masonry body will have a variation in particle size. In other words, the powder of plate-like particles will show a broad peak in the particle size distribution measurement result. As shown in the schematic diagram of Figure 5, a masonry body formed from plate-like particles having a variation in particle size is more reliably formed in a state where the plate-like particles are alternately overlapped in the thickness direction in the stacking direction of the plate-like particles in the masonry body.

[0031] Specifically, the masonry body in this embodiment has a configuration in which a plurality of plate-like particles are arranged in a layer along the spreading direction of the plate, and a plurality of the formed layers are stacked. Each layer of the masonry body has a different arrangement of the plate-like particles due to variations in the shape of the plate-like particles (particularly variations in the vertical (a) and horizontal (b) lengths). In particular, in each layer, the positions of the abutment parts where two adjacent plate-like particles abut on their side faces are different. In a masonry body formed by stacking such layers, overlapping of the abutment parts is unlikely to occur in the two stacked layers. Even if the abutment parts partially overlap in the stacking direction, other parts of the abutment parts overlap with the upper or lower surfaces of the plate-like particles, and other parts of the abutment parts do not overlap.

[0032] More specifically, when the plate-like particles are stacked to form a first layer and a second layer, when the plate-like particles of one layer are projected onto the other layer, the outer periphery of the projected plate-like particle is arranged to be located inside the outer periphery of the plate-like particle of the other layer (schematically illustrated in FIG. 6), or the outer periphery of the plate-like particle of one layer is arranged to be overlapped with a plurality of plate-like particles of the other layer (schematically illustrated in FIG. 7). If there is no variation in the particle size of the plate-like particles, there is a risk that two plate-like particles in the stacking direction will completely overlap each other, as shown in the schematic diagram of FIG. 8. In this case, the contact portions will overlap all around, and the solid electrolyte will not exhibit the labyrinth effect described below.

[0033] The number of layers in the thickness direction of the masonry body should be 2 or more, and 3 or more is more preferable. The more layers there are, the less the amount of overlap between the abutting sides of the plate-like particles in each layer. In other words, the overlap of the abutting parts of all layers is more suppressed. It is most preferable that the masonry body has no overlap between the abutting sides of the plate-like particles in each layer. With this configuration, the maze effect described below can be most reliably achieved.

[0034] The solid electrolyte of the present embodiment is a sintered body of the laminated body having the above-mentioned structure. By being a sintered body, the solid electrolyte of the present embodiment has an integrated structure. Furthermore, when a solid electrolyte battery is formed, the solid electrolyte of the present embodiment exhibits an effect of suppressing the growth of generated dendrites, i.e., an effect of suppressing damage caused by dendrites.

[0035] Specifically, the sintered body forming the solid electrolyte of this embodiment is prepared by heat-treating a stack of plate-like particles and sintering the plate-like particles. In general, the sintering reaction proceeds such that the abutting portions of the particles join together to form necks, and the necks grow. The sintered body has a portion derived from the particles of the raw material (hereinafter referred to as the particle-derived portion) and a portion derived from the necks (hereinafter referred to as the neck-derived portion). The particle-derived portion and the neck-derived portion have the same composition, but have different crystal structures. The particle-derived portion has a higher hardness than the neck-derived portion.

[0036] In a solid electrolyte battery (for example, a lithium ion secondary battery 1) using the solid electrolyte 3, dendrites are generated on the surface facing one electrode (negative electrode 4) and grow toward the other electrode (positive electrode 2), and the dendrites grow along the neck-derived portion 31 (or the periphery of the raw material particle-derived portion 30). In the solid electrolyte 3 of this embodiment, the neck-derived portion 31 has a complicated structure, and as shown in the schematic diagram of FIG. 9, the dendrites that grow penetrating the solid electrolyte 3 are bent many times before reaching the other electrode (positive electrode 2) from one electrode (negative electrode 4). The length required for the dendrites to grow and short-circuit (the length of the dendrites required for short-circuiting) becomes long. In contrast, when the solid electrolyte 3 is made of a sintered body of a powder of conventional spherical particles, the length required for the dendrites to grow penetrating the solid electrolyte 3 to short-circuit is approximately the same as the thickness of the solid electrolyte 3, as shown in the schematic diagram of FIG. 10. As a result, the solid electrolyte battery using the solid electrolyte of this embodiment exhibits the effect of suppressing the occurrence of internal short circuits due to the growth of dendrites.

[0037] In the solid electrolyte of this embodiment, the laminate may be formed by arranging plate-like particles in a predetermined state, and it is most preferable that the plate-like particles are arranged in the same direction throughout the laminate. In addition, a laminate part formed by arranging a plurality of plate-like particles in a predetermined state may be formed, and the laminate part may be assembled into an assembly (for example, a configuration shown in FIG. 21 described later). When the laminate is an assembly of laminate parts, the arrangement direction of the plate-like particles may be random.

[0038] The thickness of the solid electrolyte of this embodiment is not limited. The thickness of the solid electrolyte is preferably longer (thicker) than the length of the longest side (i.e., the length of the length (a)) among the lengths of the vertical (a), horizontal (b), and plate thickness (c) sides of the plate-like particle. With this configuration, when the masonry body is composed of a plurality of masonry body parts, even if the upper and lower surfaces of the plate-like particles included in the masonry body part are arranged in a state of spreading along the stacking direction (thickness direction of the solid electrolyte), the side surface of the plate-like particle abuts against the plate-like particle of another masonry body part. Then, the interface between the plate-like particles is linear and does not penetrate the masonry body, and the masonry body has a complicated configuration. In other words, the solid electrolyte (sintered body of the masonry body) has a complicated configuration of the neck-derived portion 31.

[0039] Specifically, the thickness of the solid electrolyte is preferably 1.3 times or more, more preferably 1.5 times or more, and even more preferably 2 times or more, of the longest side (i.e., the length of the length (a)) of the plate-like particle when the lengths of the sides (length (a), width (b) and plate thickness (c) are taken. Furthermore, the solid electrolyte of this embodiment has a plate shape that spreads as a whole along the spreading direction of the plate-like particles, and the thickness is preferably 0.5 μm or more.

[0040] The shape of the masonry body can be a shape corresponding to the solid electrolyte of the present embodiment. The corresponding shape is a shape that takes into account volume changes such as shrinkage that occur during sintering, since the solid electrolyte of the present embodiment is a sintered masonry body.

[0041] The solid electrolyte of the present embodiment is preferably a dense body. That is, the smaller the porosity of the solid electrolyte of the present embodiment, the better. The porosity is preferably 20% or less, and more preferably 1% or less.

[0042] The solid electrolyte may be a sintered body shaped by cutting, grinding, etc. For example, the surface facing the positive electrode and / or negative electrode is preferably a ground surface.

[0043] The shape of the solid electrolyte of the present embodiment is not limited, and may be the shape at the time of use (i.e., the shape of the solid electrolyte when the battery is formed).

[0044] [Lithium-ion secondary battery] The lithium ion secondary battery of this embodiment is a battery that uses the solid electrolyte of this embodiment as an electrolyte, and is a solid electrolyte battery. As shown in Fig. 11, the lithium ion secondary battery 1 of this embodiment has a positive electrode 2, a solid electrolyte 3, a negative electrode 4, and a case 5. The positive electrode 2, the solid electrolyte 3, and the negative electrode 4 each have a disk shape of the same diameter, and are formed in a stacked state with their axes aligned.

[0045] (solid electrolyte) The solid electrolyte 3 is the solid electrolyte of this embodiment described above.

[0046] (positive electrode) The positive electrode 2 is a plate-like member having a positive electrode active material capable of absorbing and releasing Li ions (ie, ion species conducted by the solid electrolyte 3), and provided in close contact with one surface of the solid electrolyte 3 in the plate thickness direction.

[0047] The positive electrode 2 of this embodiment has a positive electrode current collector 20 and a positive electrode active material layer 21 formed on the surface thereof. The positive electrode active material layer 21 is formed by applying a positive electrode mixture, which is made by mixing a positive electrode active material with a binder and a conductive material, to the surface of the positive electrode current collector 20 and drying the mixture. The positive electrode active material layer 21 may be compressed after drying.

[0048] (Cathode active material) The positive electrode active material is not limited to a specific compound as long as it is a material capable of absorbing and releasing Li ions (ion species conducted by the solid electrolyte 3).

[0049] Examples of the positive electrode active material include Li-Mn composite oxide, Li-Ni composite oxide, Li-Co-Al composite oxide, Li-Ni-Co-Mn composite oxide, spinel-type Li-Mn-Ni composite oxide, Li-Mn-Co composite oxide, Li iron phosphate (LiFePO4) and Li manganese phosphate (LiMnPO4) having an olivine structure, etc. One selected from these compounds may be used alone, or two or more may be used in combination.

[0050] The positive electrode active material is, for example, Li x Mn2O4 or Li x Li-Mn composite oxides such as MnO2, Li x Ni 1-y Al y Li-Ni-Al composite oxides such as O2, Li x Li-Co composite oxides such as CoO2, Li x Ni 1-y-z Co y Mn z Li-Ni-Co composite oxides such as O2, Li x Mn y Co 1-y Li-Mn-Co composite oxides such as LiO2, e.g. x Mn 2-y Ni y Spinel-type Li-Mn-Ni composite oxides such as LiO4, e.g. x FePO4,Li x Fe 1-y Mn y PO4,Li x Lithium phosphate oxides with an olivine structure such as CoPO4, e.g. Li x Examples include fluorinated iron sulfate such as FeSO4F, and Li-VP composite oxides such as Li3V2(PO4)3. In the above general formulas, x and y are preferably in the range of 0 to 1 (including boundary values) unless otherwise specified.

[0051] As the positive electrode active material, further, Li-M-based compounds (M: at least one selected from K, Na, Mg, Al, H; the compound is an oxide, a phosphate, an oxychloride, an oxyfluoride, an oxynitride, a hydride, or a composite oxide containing two or more of these) can be mentioned.

[0052] Using a compound selected from these as the positive electrode active material is preferable because a high positive electrode voltage can be obtained. In particular, Li-Ni-Al composite oxide, Li-Ni-Co-Mn composite oxide, and Li-Mn-Co composite oxide can significantly improve the battery life. Especially Li x Ni 1-y-z Co y Mn z A Li-Ni-Co-Mn composite oxide represented by O2 (0 < x < 1.1, 0 < y < 0.5, 0 < z < 0.5) is preferable. By using the Li-Ni-Co-Mn composite oxide, a higher high-temperature durability life can be obtained.

[0053] (Conductive material) The conductive material ensures the electrical conductivity of the positive electrode 2. As the conductive material, carbon blacks such as fine particles of graphite, acetylene black, ketjen black, carbon nanofibers, and fine particles of amorphous carbon such as needle coke can be used, but are not limited thereto.

[0054] (Binder) The binder binds the positive electrode active material particles and the conductive material. As the binder, for example, PVDF, EPDM, SBR, NBR, fluororubber, etc. can be used, but are not limited thereto.

[0055] (Positive electrode composite material) The positive electrode mixture is dispersed in a solvent and applied to the positive electrode current collector 20. As the solvent, an organic solvent that dissolves the binder is usually used. Examples of the solvent include, but are not limited to, NMP, dimethylformamide, dimethylacetamide, methyl ethyl ketone, cyclohexanone, methyl acetate, methyl acrylate, diethyltriamine, N-dimethylaminopropylamine, ethylene oxide, and tetrahydrofuran. In addition, a dispersant, a thickener, and the like may be added to water to make a slurry of the positive electrode active material using PTFE or the like.

[0056] (Positive electrode current collector) The positive electrode current collector 20 may be, for example, a processed metal such as aluminum or stainless steel, for example, a foil processed into a plate shape, a net, a punched metal, or a foam metal, but is not limited to these.

[0057] (Negative electrode) The negative electrode 4 is a plate-like member having a negative electrode active material capable of absorbing and releasing Li ions (that is, ion species conducted by the solid electrolyte 3) and provided in close contact with the other surface of the solid electrolyte 3 in the plate thickness direction.

[0058] The negative electrode 4 of this embodiment has a negative electrode current collector 40 and a negative electrode active material layer 41 formed on the surface thereof, similar to the positive electrode 2. The negative electrode active material layer 41 may be formed only from the negative electrode active material, or may be formed by applying and drying a negative electrode mixture obtained by mixing the negative electrode active material with a binder and a conductive material onto the surface of the negative electrode current collector 40. The negative electrode active material layer 41 formed from the negative electrode mixture may be compressed after drying.

[0059] (Negative electrode active material) The negative electrode active material is not limited as long as it is a material capable of absorbing and releasing Li ions, and examples thereof include metallic Li, Li alloys, metal oxides, metal sulfides, metal nitrides, carbon materials, silicon materials, and the like.

[0060] Examples of the carbon material include graphite-based materials or carbon-based materials such as graphite, coke, carbon fiber, spherical carbon, and granular carbon. The carbon material may be a graphite-based material or carbon-based material obtained by heat treatment of a thermosetting resin, isotropic pitch, mesophase pitch, mesophase pitch-based carbon fiber, vapor-grown carbon fiber, mesophase globules, etc. Examples of the silicon material include amorphous silicon, microcrystalline silicon, and polycrystalline silicon, and two or more of these may be used in combination. It is known that the electrical conductivity of silicon materials increases as the crystallinity increases.

[0061] (Conductive material) The conductive material ensures the electrical conductivity of the negative electrode 4. As the conductive material, graphite particles, carbon black such as acetylene black, ketjen black, and carbon nanofiber, and amorphous carbon particles such as needle coke can be used, as in the conductive material of the positive electrode 2, but are not limited thereto. Furthermore, conductive plastics such as conductive polymer polyaniline, polypyrrole, polythiophene, polyacetylene, and polyacene may be used.

[0062] (Binding agent) The binder binds the negative electrode active material particles and the conductive material. As with the binder of the positive electrode 2, for example, PVDF, EPDM, SBR, NBR, fluororubber, etc. can be used as the binder, but is not limited to these.

[0063] (Negative electrode composite material) The negative electrode mixture is dispersed in a solvent and applied to the negative electrode current collector 40. As the solvent, a solvent such as water or NMP that dissolves the binder is usually used. In some cases, a dispersant, a thickener, or the like is added to water to make a slurry of the negative electrode active material using PTFE or the like.

[0064] (Negative electrode current collector) The negative electrode current collector 40 may be a conventional current collector, such as a processed metal such as copper, stainless steel, titanium, or nickel, for example, a foil processed into a plate shape, a mesh, a punched metal, or a foam metal, but is not limited to these.

[0065] (case) The case 5 accommodates therein charge / discharge elements including the positive electrode 2, the solid electrolyte 3, and the negative electrode 4. The case 5 forms the outer peripheral shape of the lithium ion secondary battery 1.

[0066] The case 5 can be formed in a shape and made of a material that can accommodate the charging and discharging elements therein. For example, the case can be made of a metal or resin and have a rectangular parallelepiped or cylindrical shape.

[0067] The case 5 has a positive electrode terminal electrically connected to the positive electrode 2 (specifically, the positive electrode current collector 20) and a negative electrode terminal electrically connected to the negative electrode 4 (specifically, the negative electrode current collector 40).

[0068] [Method of manufacturing lithium-ion secondary batteries] The lithium ion secondary battery 1 of this embodiment is manufactured by a manufacturing method including the following steps: Each step of the manufacturing method of this embodiment is shown in FIG.

[0069] (Plate-shaped particle preparation step; S1) This step S1 is a step of preparing plate-like particles.

[0070] The plate-like particles are particles that constitute the composite body. This step S1 may be either a step of manufacturing plate-like particles of LiNbO3 (a material having ion conductivity) or a step of preparing commercially available plate-like particles. This step S1 includes a step of weighing out a predetermined amount of the plate-like particles.

[0071] In this embodiment, plate-like particles were produced via the reactions of the following formulas (1) to (3).

[0072] [ka]

[0073] Equation (1) is K4Nb6O in the flux. 17 The reaction that produces K4Nb6O in the reaction of formula (1) 17 As shown in the enlarged photographs (SEM photographs) of FIGS. 13 and 14, the primary particles have a plate-like particle shape.

[0074] Formula (2) is KNbO 17 Proton exchange to H4Nb6O 17 This is a reaction that produces H4Nb6O 17 As shown in the enlarged photographs (SEM photographs) of FIGS. 15 and 16, the shape of the plate-like particles before proton exchange is maintained.

[0075] Equation (3) is expressed as H4Nb6O in the flux. 17 This reaction is a reaction in which LiNbO3 is produced by reacting with a Li compound. The produced LiNbO3 is formed of primary particles of plate-like particles, as shown in the enlarged photographs (SEM photographs) in Figures 17 and 18. From these enlarged photographs, it can be confirmed that the reaction of formula (3) is a topotactic reaction.

[0076] According to the production method using the reactions of the above formulas (1) to (3), as shown in FIGS. 13 to 18, plate-like particles can be produced in the form of plate-like primary particles.

[0077] As described above, in the platelet particle preparation step S1 of this embodiment, the platelet particles of LiNbO3 are prepared in the state of primary particles.

[0078] (Paste preparation process; S2) This step S2 is a step of preparing a paste in which plate-like particles are dispersed.

[0079] The paste prepared in this step S2 is a paste (or suspension) with fluidity, in which plate-like particles are dispersed in a dispersion medium. In the paste, the movement (displacement) of the dispersed plate-like particles is not restricted, and the plate-like particles can flow together with the dispersion medium. The dispersion medium is not limited as long as it is a dispersion medium (solvent) capable of dispersing plate-like particles. Examples of the dispersion medium (solvent) include polymeric dispersants such as polypropylene carbonate (PPC), polyvinyl alcohol (PVA), polyimide (PI), and at least one organic solvent selected from 1,4-dioxane (DO), N-methylpyrrolidone (NMP), dimethylformamide (DMF), and solvents such as water and aqueous solutions. In this embodiment, a mixed solvent in which PC:DO is mixed at a mass ratio of 1:3 is used.

[0080] The paste prepared in step S2 may contain additives that are well known in the art. Examples of additives include binders, pH adjusters, dispersants, flocculants, and viscosity adjusters. It is preferable that the additives disappear (or volatilize or burn off) when heated in the subsequent sintering step S6 or other steps.

[0081] (Coating process; S3) This step S3 is a step of applying the prepared paste.

[0082] In this step S3, the paste is applied to the coating surface while applying shear stress along the coating surface.

[0083] The coated surface is the surface onto which the paste is applied. The coated surface has a surface from which the paste-coated body can be peeled off in a later process. In this embodiment, the coated surface is formed by a release film (a silicone-based light release film manufactured by Toyobo Co., Ltd., product name: E7002-100 μm).

[0084] In this step S3, the paste is applied to the coating surface while applying a shear stress along the coating surface. That is, the paste is applied to the coating surface (or the paste is dripped or attached to the coating surface), and a predetermined shear stress is applied to the applied paste. When the paste is applied in this manner, the paste-coated body has multiple plate-like particles in the paste arranged in a predetermined state.

[0085] This step S3 can be performed using a coating device. In this embodiment, a bar coater 60, the schematic configuration of which is shown in FIG. 19, was used as the coating device 6. The bar coater 60 is arranged with a predetermined gap between it and the coating surface 61. The bar coater 60 moves at a constant speed parallel to the coating surface 61 on which the paste 62 has been applied. When the bar coater 60 moves and passes over the paste 62, a paste-coated body 63 of uniform thickness, which is the gap between the coating surface 61 and the bar coater 60, is obtained. In this embodiment, a paste-coated body 63 of 254 μm (10 mil) thickness was obtained.

[0086] In the coater 6 of this embodiment, when the bar coater 60 moves, the bar coater 60 comes into contact with the paste 62. When the bar coater 60 moves while in contact with the paste 62, a shear stress is applied near the surface of the paste 62. This shear stress is a stress in a direction along the spreading direction of the coated surface 61. When this stress is applied, the plate-like particles in the paste 62 are arranged in a state in which the spreading direction of the plate-like particles is parallel to the direction of the shear stress (i.e., parallel to the coated surface 61). As a result, the paste-coated body 63 is one in which the plate-like particles in the paste 62 are arranged in a predetermined state. As described above, in this embodiment, a paste-coated body 63 of uniform thickness in which a plurality of plate-like particles are arranged in a predetermined state was obtained.

[0087] In this embodiment, the bar coater 60 having the coating surface 61 which is flat is used, but a roll coater having a curved coating surface may also be used.

[0088] (Drying process; S4) This step S4 is a step of drying the paste coating applied to the coating surface.

[0089] The paste-coated body is dried by volatilizing the dispersion medium (solvent) from the paste-coated body. By drying the paste-coated body, a composite body in which the plate-like particles are arranged in a predetermined state is formed. This step S4 includes a step of removing the composite body from the coated surface.

[0090] The drying method of the paste-coated body is not limited to a specific method as long as the dispersion medium (solvent) can be volatilized from the paste-coated body. For example, the dispersion medium may be held at room temperature, or heated at a temperature lower than the sintering temperature of the plate-like particles. The dispersion medium (solvent) may be volatilized not only under normal pressure but also under reduced pressure. In this embodiment, the paste-coated body was held at room temperature to volatilize the dispersion medium.

[0091] (Compression process; S5) This step S5 is a step of compressing the dried paste coating.

[0092] By compressing the paste-coated body (i.e., the masonry body), the paste-coated body (dense masonry body) becomes one in which adjacent plate-like particles are in close contact with each other.

[0093] The specific method for compressing the paste-coated body is not limited, and examples thereof include pressing using a mold, cold isostatic pressing (CIP), hot isostatic pressing (HIP), and the like. The compression conditions for compressing the paste-coated body are also not limited. Appropriately select conditions (pressure, pressing time) that can obtain a molded body (masonry) of the desired density. In this embodiment, the masonry was compressed by cold isostatic pressing (CIP) under conditions of 300 MPa and 10 minutes.

[0094] (Sintering process; S6) This step S6 is a step of sintering the compressed paste-coated body (masonry body).

[0095] The paste-coated body (i.e., the masonry body) is sintered to sinter the plate-like particles forming the masonry body together, thereby producing the solid electrolyte 3 of this embodiment. This step S6 includes a debinding step of heating the plate-like particles together at a temperature equal to or lower than the sintering temperature before heating them together at the sintering temperature.

[0096] The specific heating conditions for sintering the composite body are not limited. The conditions (heating temperature, heating time, heating atmosphere, heating pressure) that can obtain the desired solid electrolyte (sintered body) are appropriately selected. In this embodiment, the body was heated at 300°C for 1 hour in an air atmosphere at normal pressure, and then heated to 1000°C and held there for 10 hours.

[0097] (Positive electrode manufacturing process; S7) This step S7 is a step for producing a positive electrode 2 having a positive electrode active material.

[0098] In this embodiment, a positive electrode mixture obtained by mixing a positive electrode active material powder with a binder and a conductive material is applied to the surface of a positive electrode current collector 20, dried, and compressed to produce a positive electrode 2.

[0099] (Negative electrode manufacturing process; S8) This step S8 is a step of producing a negative electrode 4 having a negative electrode active material.

[0100] In this embodiment, the negative electrode 4 is manufactured by applying a negative electrode mixture obtained by mixing the negative electrode active material powder with a binder and a conductive material onto the surface of the negative electrode current collector 40, drying the mixture, and compressing it.

[0101] (Assembly process; S9) This step S9 is a step of assembling the lithium ion secondary battery 1 from the positive electrode 2, the solid electrolyte 3, and the negative electrode 4.

[0102] In this embodiment, the positive electrode 2 has a surface facing (in close contact with) one surface of the solid electrolyte 3, and the negative electrode 4 has a surface facing (in close contact with) the other surface of the solid electrolyte 3. The laminate is then sealed in a case 5 to assemble the lithium ion secondary battery 1.

[0103] In this step S9, the laminate of the positive electrode 2, the solid electrolyte 3, and the negative electrode 4 may be compressed in the stacking direction to be tightly attached. Furthermore, the process of enclosing the laminate in the case 5 includes a step of connecting the positive electrode current collector 20 to a positive electrode terminal, and a step of connecting the negative electrode current collector 40 to a negative electrode terminal, and a step of sealing the case 5.

[0104] In this manner, the lithium ion secondary battery 1 (solid electrolyte battery) of this embodiment was manufactured. In the manufacturing method of this embodiment, the coating step S3 corresponds to the coating step in the claims, the sintering step S6 corresponds to the sintering step in the claims, and the positive electrode manufacturing step S7 to the assembly step S9 correspond to the electrode forming step in the claims, respectively.

[0105] [effect] The solid electrolyte of this embodiment is a sintered laminate formed by arranging plate-like particles of LiNbO3 as an ion-conductive material in a predetermined state.

[0106] Generally, a sintered body is formed by joining the abutting portions of particles to form a neck, and a sintering reaction proceeds so that the neck grows. In a sintered body, the particle-derived portion of the raw material and the neck-derived portion have the same composition, but the crystal structures of the two portions are different. The particle-derived portion has a higher hardness than the neck-derived portion.

[0107] When the lithium ion secondary battery 1 (solid electrolyte battery) using the solid electrolyte 3 of this embodiment is charged under severer conditions than the prescribed charging conditions (overcharging or rapid charging), dendrites are generated on the surface of the negative electrode 4 (the interface between the solid electrolyte 3 and the negative electrode 4). As this charging continues, the dendrites grow toward the positive electrode 2. The grown dendrites grow along the neck-derived portions in the solid electrolyte 3 (or the peripheral portions of the portions derived from the raw material particles). Here, if pores derived from the gaps between the plate-like particles are present in the solid electrolyte 3, the dendrites grow so as to connect the pores.

[0108] The solid electrolyte 3 of this embodiment is sintered while maintaining the arrangement of the plate-like particles of the laminate, and has a complicated structure with neck-derived portions. As shown in the schematic diagram of FIG. 7, the dendrites that grow penetrating the solid electrolyte 3 of this embodiment bend their growth direction many times as they grow from the negative electrode 4 toward the positive electrode 2. In other words, a maze effect is exhibited in which the growth direction bends. As a result, it becomes difficult for the dendrites to reach the positive electrode 2 from the negative electrode 4, and the occurrence of an internal short circuit in the lithium-ion secondary battery 1 is suppressed.

[0109] In contrast, in the case of a conventional solid electrolyte 3 made of a sintered body of powder particles, as shown in the schematic diagram of Fig. 8, the neck-derived portion is approximately the same length as the thickness direction of the solid electrolyte 3. In a lithium-ion secondary battery 1 using this conventional solid electrolyte 3, dendrites growing from the negative electrode 4 toward the positive electrode 2 immediately cause a short circuit because the maze effect is not exerted.

[0110] As described above in detail, the solid electrolyte 3 of this embodiment and the lithium ion secondary battery 1 using the same exhibit the effect of suppressing the occurrence of internal short circuits due to the growth of dendrites. In other words, damage due to the generation and growth of dendrites is suppressed.

[0111] In the solid electrolyte 3 of this embodiment, the plate-like particles forming the laminate have a vertical:horizontal length ratio of 1 to 3:1 and a horizontal:plate thickness ratio of 1.3 to 4:1. When the plate-like particles have an outer periphery shape having these ratios, a laminate (and a sintered body) in which the plate-like particles are arranged in a predetermined state can be formed.

[0112] In the solid electrolyte 3 of this embodiment, the plate-like particles have an average particle size (D50) of 2.0 μm to 8.0 μm. When the average particle size of the plate-like particles is in this range, a laminate (and a sintered body) is formed in which the plate-like particles are arranged in a predetermined state.

[0113] In the solid electrolyte 3 of this embodiment, the length between the 25% cumulative value (D25) and the 75% cumulative value (D75) from the smallest diameter in the particle size distribution of the plate-like particles is 34 to 230% of the length of the average particle size (D50). When the plate-like particles have this particle size distribution, when a laminate (and a sintered body) is formed, the contact portions (neck-derived portions) between the particles have a complicated configuration.

[0114] The solid electrolyte 3 of this embodiment has a plate shape extending in the direction in which the plate-like particles extend, and has a thickness of 0.5 μm or more. With this configuration, the neck-derived portion has a complicated configuration, and the above-mentioned effects are more reliably exhibited.

[0115] In the solid electrolyte 3 of this embodiment, the material having ion conductivity is LiNbO3. Since the material having ion conductivity is LiNbO3, the solid electrolyte 3 conducts Li ions.

[0116] The lithium ion secondary battery 1 (solid electrolyte battery) of this embodiment uses the solid electrolyte 3 that exerts the above-mentioned effects, and exerts the same effects.

[0117] The manufacturing method of the lithium ion secondary battery 1 of this embodiment (manufacturing method of the solid electrolyte battery) includes a step of preparing a paste and applying the paste to a coating surface while applying a shear stress, so that it is possible to manufacture a laminate in which plate-like particles are arranged in a predetermined state and a sintered body thereof, and as a result, it is possible to manufacture the lithium ion secondary battery 1 that exhibits the above-mentioned effects.

[0118] In the method for producing the lithium ion secondary battery 1 of this embodiment, the coating step S3 is a step of applying the paste to the coating surface with a bar coater. This step S3 makes it possible to produce a laminate in which the plate-like particles are arranged in a predetermined state.

[0119] In the manufacturing method of this embodiment, plate-like particles are produced by generating a plate-like intermediate product by a flux method, and then the intermediate product is used to produce a final product by an ion exchange method. By utilizing this reaction path, even LiNbO3, which is difficult to form plate-like particles, can be used to form primary particles of plate-like particles. As a result, a solid electrolyte 3 and a lithium-ion secondary battery 1 made of LiNbO3 with excellent ion conductivity can be manufactured.

[0120] More specifically, when LiNbO3 is manufactured by a manufacturing method that does not use the flux method (for example, a manufacturing method by sintering), it becomes a substantially spherical primary particle. The solid electrolyte 3 made of a sintered body of substantially spherical primary particles has a structure shown in the schematic diagram of FIG. 8 described above. In other words, the above-mentioned labyrinth effect cannot be exhibited. In contrast, in this embodiment, LiNbO3 having a plate-shaped particle shape can be manufactured by generating a plate-shaped intermediate product by the flux method. In this way, by using the flux method, primary particles of plate-shaped particles can be manufactured even if materials have different crystal growth directions.

[0121] In the manufacturing method of the present embodiment, a laminate of plate-like particles is formed (steps S1 to S4), compressed into a dense laminate (step S5), and sintered (step S6) to produce a dense solid electrolyte 3. The dense solid electrolyte 3 can better exhibit the effect of suppressing the growth of dendrites.

[0122] FIG. 20 is an enlarged photograph of a cut section of the masonry body after step S4 of the manufacturing method of this embodiment, FIG. 21 is an enlarged photograph of a cut section of the masonry body (compressed masonry body) after step S5, and FIG. 22 is an enlarged photograph of a cut section of the solid electrolyte 3 of this embodiment (sintered body after step S6).

[0123] In the manufacturing method of this embodiment, a coating step S3 is performed in which a paste 62 is applied to a coating surface 61 by a bar coater 60. By performing this step, a laminate in which plate-like particles (primary particles) are arranged in a predetermined state can be formed, as shown in Figs.

[0124] As shown in FIG. 20, in the masonry body after step S4, the plate-like particles (primary particles) are arranged in a predetermined state. As shown in FIG. 21, in the compressed masonry body after step S5, the plate-like particles (primary particles) are arranged in a state where adjacent plate-like particles are in contact with each other (specifically, the upper and lower surfaces of the plate-like particles are in surface contact with each other). Furthermore, when comparing the surface vicinity and the inside of the compressed masonry body, the surface vicinity that is in contact with the CIP mold is dense, and the inside is sparse with many gaps, and the plurality of plate-like particles are arranged. As shown in FIG. 22, the sintered body after step S6 is a sintered compressed masonry body, and like the compressed masonry body, there is a difference in partial density between the surface vicinity and the inside. Furthermore, in the sparse parts, as shown in FIG. 22, the particle shape of the plate-like particles remains, and pores along the surface of the plate-like particles remain.

[0125] [Variations] The lithium ion secondary battery 1 of this embodiment has the same configuration as that of the first embodiment, except that the manufacturing method is different. In this embodiment, configurations that are not specifically mentioned are the same as those of the first embodiment. [Method of manufacturing lithium-ion secondary batteries] The lithium ion secondary battery 1 of this embodiment is manufactured by the same manufacturing method as that of the first embodiment, except that the sintering step S6 is different.

[0126] (Sintering process; S6) The sintering step S6 in the manufacturing method of this embodiment is a step of sintering the compressed paste-coated body (masonry body) in an infrared heating furnace. An infrared heating furnace is a heating furnace that heats the object (masonry) by focusing infrared rays emitted from an infrared lamp on it. Infrared heating furnaces can quickly raise the temperature to the sintering temperature (rapid heating is possible). In addition, infrared heating furnaces start cooling (natural cooling) by stopping heating (rapid cooling is possible).

[0127] The specific heating conditions for sintering the laminate in the infrared heating furnace are not limited to those in the first embodiment. Conditions (heating temperature, heating time, heating atmosphere, heating pressure) that can obtain a desired solid electrolyte (sintered body) are appropriately selected. In this embodiment, the material was heated at 300°C for 1 hour in an air atmosphere at normal pressure, then heated to 1000°C and held for 0.08 hours (4 minutes and 48 seconds). After holding at 1000°C, the power supply to the heating furnace was immediately stopped and the material was cooled (cooled naturally).

[0128] [effect] The solid electrolyte 3, the lithium ion secondary battery 1 and the method for producing the same of this embodiment have the same effects as those of the first embodiment. In the manufacturing method of this embodiment, the heating in the sintering step S6 is performed in an infrared heating furnace. The infrared heating furnace is a heating furnace capable of rapid heating and rapid cooling (sintering treatment). In the manufacturing method of this embodiment, the sintering time (time held at 1000°C) is shorter than in the first embodiment, but a solid electrolyte 3 having a similar structure to the solid electrolyte 3 of the first embodiment can be manufactured. In other words, the manufacturing method of this embodiment allows the solid electrolyte 3 and the lithium ion secondary battery 1 to be manufactured in a short time.

[0129] The solid electrolyte 3 of this embodiment has a structure in which plate-like particles (matrix) are sintered while maintaining the particle shape of the plate-like particles. In general, when a powder is heated to a sintering temperature, a reaction occurs in which a neck is formed at the contact point between adjacent powder particles, and a reaction occurs in which the powder particles become rounded due to diffusion and grain growth on the solid surface. The longer the time held at the sintering temperature, the more these two reactions progress. In the manufacturing method of this embodiment, the time held at the sintering temperature is shortened, but the reaction of forming necks between the plate-like particles progresses. In addition, by shortening the time held at the sintering temperature, the reaction of rounding the plate-like particles is prevented from progressing excessively. Furthermore, in the manufacturing method of this embodiment, cooling is started immediately after the holding at the sintering temperature is completed, and the temperature of the matrix (sintered body) decreases to a temperature lower than the sintering temperature (a temperature at which the sintering reaction is unlikely to occur), and the sintering reaction stops. As a result, in this embodiment, the sintering step S6 (sintering treatment, heat treatment) is completed before the plate-like particles become rounded due to grain growth, and the plate-like particles remain aligned, resulting in a solid electrolyte 3 having a sintered structure in which grain growth is suppressed. The solid electrolyte 3 of this embodiment exhibits the effect of having a more complicated structure of the neck-derived portions.

[0130] The solid electrolyte 3 of this embodiment has a structure in which plate-like particles (lamination body) are sintered in a state in which grain growth is suppressed as described above. In the sintered body, it is preferable that the shape of the portion derived from the plate-like particles (i.e., the shape of the portion excluding the portion derived from the neck) is within the above-mentioned range of the length:width:plate thickness ratio.

[0131] In this embodiment, sintering is performed using an infrared heating furnace, but the same effect can be achieved by using a heating device (sintering furnace) capable of rapid heating and rapid cooling instead of an infrared heating furnace. Examples of such a heating device include a microwave heating device, a plasma heating device, a tunnel furnace, and an induction heating device.

[0132] [Embodiment 2] This embodiment is a lithium ion secondary battery 1 having the same configuration as that of the first embodiment, except that the configuration of the negative electrode 4 is different. The solid electrolyte 3 of this embodiment is the same as that of the first embodiment. In this embodiment, configurations that are not particularly mentioned are the same as those of the first embodiment.

[0133] [Lithium-ion secondary battery] The lithium ion secondary battery of this embodiment has a positive electrode 2 , a solid electrolyte 3 , a negative electrode 4 , and a case 5 .

[0134] (Negative electrode) The negative electrode 4 is made of metallic Li deposited on the solid electrolyte 3. That is, the negative electrode 4 is made of only metallic Li as a negative electrode active material.

[0135] [Method of manufacturing lithium-ion secondary batteries] The lithium ion secondary battery 1 of this embodiment is manufactured by a manufacturing method including the steps shown in FIG.

[0136] In the manufacturing method of this embodiment, the steps from the plate-like particle preparation step S1 to the positive electrode manufacturing step S7 are the same as those in the first embodiment.

[0137] (Negative electrode welding process; S8) This step S8 is a step of depositing a negative electrode active material (metal Li) onto the other surface of the solid electrolyte 3 to form them integrally.

[0138] In this embodiment, metallic Li, which is the negative electrode active material, is placed on the other surface of the solid electrolyte 3, heated and melted, and then cooled, so that the negative electrode active material (metallic Li) is integrally welded to a predetermined thickness on the other surface of the solid electrolyte 3. Note that, in this embodiment, metallic Li is integrally welded by heating, melting, and cooling, but this is not limited to this method. For example, the negative electrode 4 may be integrally formed using a method such as CVD or PVD.

[0139] (Assembly process; S9) This step S9 is a step of assembling the lithium ion secondary battery 1 from the positive electrode 2 and the solid electrolyte 3 to which the negative electrode 4 is welded.

[0140] In this embodiment, the positive electrode 2 is sealed in the case 5 with the surface of the positive electrode active material layer 21 facing (in close contact with) one surface of the solid electrolyte 3 .

[0141] In this manner, the lithium ion secondary battery 1 (solid electrolyte battery) of this embodiment was manufactured. In the manufacturing method of this embodiment, the coating step S3 corresponds to the coating step in the claims, the sintering step S6 corresponds to the sintering step in the claims, and the positive electrode manufacturing step S7 to the assembly step S9 correspond to the electrode forming step in the claims, respectively.

[0142] [effect] The solid electrolyte 3, the lithium ion secondary battery 1 and the method for producing the same of this embodiment have the same effects as those of the first embodiment.

[0143] Furthermore, in the lithium ion secondary battery 1 of this embodiment, the negative electrode 4 is integrally formed with the solid electrolyte 3 by welding. With this configuration, the metallic Li of the negative electrode 4 penetrates even into the fine irregularities on the other surface of the solid electrolyte 3. In other words, the negative electrode 4 forms a strong bond with the solid electrolyte 3, which exerts an anchor effect. As a result, peeling does not occur at the interface between the negative electrode 4 and the solid electrolyte 3.

[0144] Furthermore, Li ions can move across the entire interface between the solid electrolyte 3 and the negative electrode 4 (i.e., the entire surface including the finely uneven surface on the other surface of the solid electrolyte 3) (i.e., Li ions can be inserted into and removed from the negative electrode active material), allowing a large amount of Li ions to move at once. In other words, high battery performance can be achieved.

[0145] The manufacturing method of this embodiment includes a step of forming the negative electrode 4 by depositing the material of the negative electrode 4 (negative electrode active material, metallic Li) on the other surface of the solid electrolyte 3 (sintered body). By including this step, it is possible to manufacture the lithium ion secondary battery 1 that exhibits the above-mentioned effects.

[0146] [Embodiment 3] This embodiment is a lithium ion secondary battery 1 having the same configuration as that of the first embodiment, except that the configurations of the positive electrode 2 and the negative electrode 4 are different. The solid electrolyte 3 of this embodiment is the same as that of the first embodiment. In this embodiment, configurations that are not particularly mentioned are the same as those of the first embodiment.

[0147] [Lithium-ion secondary battery] The lithium ion secondary battery of this embodiment has a positive electrode 2, a solid electrolyte 3, a negative electrode 4, and a case 5, all of which are integrated together, as shown in the cross-sectional view of FIG.

[0148] (positive electrode) The positive electrode 2 is a sintered body of the positive electrode active material of embodiment 1. That is, the positive electrode 2 is composed only of the positive electrode active material. The positive electrode 2 may contain a conventionally known additive such as a conductive material.

[0149] (Negative electrode) The negative electrode 4 is a sintered body of the negative electrode active material of the first embodiment. That is, the negative electrode 4 is composed of only the negative electrode active material. Since the negative electrode 4 is a sintered body, the negative electrode active material is selected from sinterable materials (i.e., materials other than metallic Li). The negative electrode 4 may contain a conventionally known additive such as a conductive material.

[0150] [Method of manufacturing lithium-ion secondary batteries] The lithium ion secondary battery 1 of this embodiment is manufactured by a manufacturing method including the steps shown in FIG.

[0151] In the method for producing the lithium ion secondary battery 1 of this embodiment, the plate-like particle preparation step S1 to the sintering step S6 are the same as the respective steps in the first embodiment.

[0152] (Positive electrode manufacturing process; S7) This step S7 is a step for producing the positive electrode 2.

[0153] In this embodiment, the positive electrode 2 is manufactured by compression molding a powder of a positive electrode active material into a predetermined shape, and sintering the molded body.

[0154] The powder of the positive electrode active material is not limited with respect to its particle size characteristics (eg, particle size distribution characteristics such as D50, D25, D75, etc.).

[0155] There are no limitations on the method and conditions of compression molding, but the conditions are preferably such that the molded body can be compressed to have a predetermined density.

[0156] The sintering of the molded body is carried out under conditions that allow the positive electrode active material of the molded body to be sintered, that is, the conditions are appropriately determined depending on the material of the positive electrode active material and the shape of the molded body.

[0157] (Negative electrode manufacturing process; S8) This step S8 is a step of producing a negative electrode 4 having a negative electrode active material.

[0158] In this embodiment, the negative electrode 4 is manufactured by compression molding a powder of the negative electrode active material into a predetermined shape, and sintering the molded body.

[0159] The powder of the negative electrode active material is not limited with respect to its particle size characteristics (eg, particle size distribution characteristics such as D50, D25, D75, etc.).

[0160] There are no limitations on the method and conditions of compression molding, but the conditions are preferably such that the molded body can be compressed to have a predetermined density.

[0161] The sintering of the molded body is carried out under conditions that allow the negative electrode active material of the molded body to be sintered, that is, the conditions are appropriately determined depending on the material of the negative electrode active material and the shape of the molded body.

[0162] (Assembly and sintering process; S9) This step S9 is a step of assembling the positive electrode 2, the solid electrolyte 3, and the negative electrode 4 in a laminated state, and sintering the positive electrode 2, the solid electrolyte 3, and the negative electrode 4 to integrate them.

[0163] In this step, the positive electrode 2 (sintered body) faces one surface of the solid electrolyte 3, and the negative electrode 4 (sintered body) faces the other surface of the solid electrolyte 3, and they are laminated in a state of being in close contact with each other. Then, this laminate is sintered.

[0164] In the laminate, the positive electrode 2, the solid electrolyte 3, and the negative electrode 4 are preferably in contact with each other over the entire surface of each interface, and the contact surfaces are more preferably formed into flat surfaces. When the contact surfaces are in contact with each other over the entire surface of the interfaces, the contact surfaces are bonded over the entire surface of the interfaces when sintered, resulting in a strong bonded body (sintered body). In addition, when the contact surfaces are bonded over the entire surface, Li ions are desorbed and inserted over the entire surface of the interface between the positive electrode 2 and the negative electrode 4, and the desorbed and inserted Li ions are not concentrated in parts.

[0165] There are no limitations on the sintering conditions when sintering the laminate, and any sintering temperature, sintering time, and sintering atmosphere may be used that allow the positive electrode 2, solid electrolyte 3, and negative electrode 4 to be sintered together.

[0166] In this embodiment, the positive electrode 2, the solid electrolyte 3, and the negative electrode 4 are joined together by a single sintering process. However, the sintering of the positive electrode 2 and the solid electrolyte 3 and the sintering of the negative electrode 4 and the solid electrolyte 3 may be performed in separate processes.

[0167] In this step S9, the positive electrode 2, the solid electrolyte 3, and the negative electrode 4 are sintered together and then enclosed in a case 5. The positive electrode 2 and the negative electrode 4 are enclosed in the case 5 in a state where the positive electrode terminal and the negative electrode terminal, respectively, are joined by welding. In this case, the positive electrode terminal welded to the positive electrode 2 and the negative electrode terminal welded to the negative electrode 4 also function as current collectors.

[0168] In this manner, the lithium ion secondary battery 1 (solid electrolyte battery) of this embodiment was manufactured. In the manufacturing method of this embodiment, the coating step S3 corresponds to the coating step in the claims, the sintering step S6 corresponds to the sintering step in the claims, and the positive electrode manufacturing step S7 to the assembly / sintering step S9 correspond to the electrode formation step in the claims, respectively.

[0169] [effect] The solid electrolyte 3, the lithium ion secondary battery 1 and the method for producing the same of this embodiment have the same effects as those of the first embodiment.

[0170] In the lithium ion secondary battery 1 of this embodiment, the solid electrolyte 3, the positive electrode 2, and the negative electrode 4 are integrally formed by sintering. With this configuration, the solid electrolyte 3, the positive electrode 2, and the negative electrode 4 are firmly bonded together, improving the strength. In addition, the amount of the interface (an interface with a clear boundary) between the solid electrolyte 3 and the positive electrode 2 or the negative electrode 4 is reduced by sintering, reducing the interface resistance when Li ions move. As a result, the internal resistance of the lithium ion secondary battery 1 is reduced.

[0171] The manufacturing method of this embodiment includes a step of disposing the positive electrode 2 (material of the positive electrode 2) on one surface of the solid electrolyte 3 (sintered body) and the negative electrode 4 (material of the negative electrode 4) on the other surface, and sintering the laminate. By including this step, the solid electrolyte 3, the positive electrode 2, and the negative electrode 4 are sintered together, and the above-mentioned effects can be achieved.

[0172] [Embodiment 4] This embodiment is a lithium ion secondary battery 1 having the same configuration as that of the third embodiment, except that the configuration of the positive electrode 2 is different. The solid electrolyte 3 and the negative electrode 4 of this embodiment are the same as those of the second embodiment. In this embodiment, configurations that are not particularly mentioned are the same as those of the second embodiment.

[0173] [Lithium-ion secondary battery] The lithium ion secondary battery 1 of this embodiment has a positive electrode 2 , a solid electrolyte 3 , a negative electrode 4 , and a case 5 .

[0174] (positive electrode) The positive electrode 2 is a sintered body in which the positive electrode active material of the second embodiment and LiNbO3 are uniformly mixed. The positive electrode 2 may contain a conventionally known additive such as a conductive material.

[0175] In the positive electrode 2 of this embodiment, the mass ratio of the positive electrode active material to LiNbO3 is not limited, but it is preferable that the mass of the positive electrode active material is larger. When the total mass of the positive electrode active material and LiNbO3 is taken as 100%, the positive electrode active material is preferably 50% or more, more preferably 70% or more, and even more preferably 80% or more.

[0176] In the present embodiment, the positive electrode active material and LiNbO3 are uniformly mixed in the positive electrode 2. LiNbO3 has ion conductivity to Li ions.

[0177] [Method of manufacturing lithium-ion secondary batteries] The lithium ion secondary battery 1 of this embodiment is manufactured by a manufacturing method including the steps shown in FIG.

[0178] In the method for producing the lithium ion secondary battery 1 of this embodiment, the plate-like particle preparation step S1 to the compression step S5 are the same as the respective steps in the third embodiment.

[0179] (Positive electrode green sheet manufacturing process; S6) This step S6 is a step of producing a green sheet for the positive electrode 2.

[0180] In this embodiment, a mixed powder of the positive electrode active material and LiNbO3 is compression molded into a predetermined shape to produce a molded body (positive electrode green sheet of the positive electrode 2).

[0181] The particle shape of the LiNbO3 powder is not limited. In other words, it may be either the plate-like particles used in the production of the solid electrolyte 3 or the spherical particles. The particle size characteristics of the LiNbO3 powder (e.g., particle size distribution characteristics such as D50, D25, D75, etc.) are also not limited. However, it is preferable that the particle size characteristics are such that the powder can be uniformly mixed with the particles of the positive electrode active material.

[0182] The mixed powder of the positive electrode active material and LiNbO3 may be in a state where the positive electrode active material powder and the LiNbO3 powder are uniformly mixed, and may be in a state where they are dispersed in a dispersion medium. In addition, the mixed powder may contain a conventionally known additive.

[0183] There are no limitations on the method and conditions of compression molding, but the conditions are preferably such that the molded body can be compressed to have a predetermined density.

[0184] The green body (positive electrode green sheet) produced in this step S6 is preferably dry. That is, the green body (positive electrode green sheet) is preferably dried by carrying out a step similar to that of the drying step S4. By drying the green body (positive electrode green sheet), the occurrence of sintering defects due to uneven drying can be suppressed when sintering is carried out in the assembling and sintering step S8.

[0185] (Negative electrode green sheet manufacturing process; S7) This step S7 is a step of producing a green sheet for the negative electrode 4.

[0186] In this embodiment, a powder of the negative electrode active material is compression molded into a predetermined shape to produce a molded body (a green sheet of the negative electrode 4).

[0187] In this step S7, as in the positive electrode green sheet manufacturing step S6, the molded body (green sheet) may contain an additive or a dispersion medium.

[0188] The green compact (negative electrode green sheet) produced in this step S7 is preferably dry. That is, the green compact (negative electrode green sheet) is preferably dried by a step similar to that of the drying step S4. By drying the green compact (negative electrode green sheet), the occurrence of sintering defects due to uneven drying can be suppressed when sintering is performed in the assembling and sintering step S8.

[0189] (Assembly and sintering process; S8) This step S8 is a step of laminating a green compact of the positive electrode 2 (positive electrode green sheet), a green compact of the solid electrolyte 3, and a green compact of the negative electrode 4 (negative electrode green sheet), and sintering this laminate to produce an integrated sintered body.

[0190] In this embodiment, the green compact of the positive electrode 2 (positive electrode green sheet) faces one surface of the green compact of the solid electrolyte 3, and the green compact of the negative electrode 4 (negative electrode green sheet) faces the other surface of the green compact of the solid electrolyte 3. At this time, the laminate is preferably compressed in the lamination direction so that the interfaces are in close contact with each other. Then, the laminate is sintered.

[0191] There are no limitations on the sintering conditions when sintering the laminate, and any sintering temperature, sintering time, and sintering atmosphere may be used that allow the positive electrode 2, solid electrolyte 3, and negative electrode 4 to be sintered together.

[0192] In this step S8, after the sintered bodies of the positive electrode 2, the solid electrolyte 3, and the negative electrode 4 are manufactured, they are sealed in the case 5.

[0193] In this manner, the lithium ion secondary battery 1 (solid electrolyte battery) of this embodiment is manufactured. In the manufacturing method of this embodiment, the coating step S3 corresponds to the coating step in the claims, and the assembly / sintering step S8 corresponds to the sintering step in the claims.

[0194] [effect] This embodiment has the same effects as the third embodiment.

[0195] In the lithium ion secondary battery 1 of this embodiment, the positive electrode 2 contains a material (LiNbO3) that forms the solid electrolyte 3. This material has ion conductivity.

[0196] According to this configuration, LiNbO3 with ion conductivity is present inside the positive electrode 2. This makes it easier for Li ions to be conducted to the inside of the positive electrode 2, and the reaction of insertion and desorption into and from the positive electrode active material also proceeds inside the positive electrode 2. In other words, the reaction of insertion and desorption of Li ions into and from the positive electrode active material proceeds throughout the positive electrode 2, increasing the amount of reacting Li ions. As a result, the battery performance of the lithium-ion secondary battery 1 is improved.

[0197] Furthermore, since the LiNbO3 in the positive electrode 2 is made of the same material as the solid electrolyte 3, the LiNbO3 bonds together when sintered in step S8, and the positive electrode 2 and the solid electrolyte 3 are more strongly bonded together. With this configuration, the positive electrode 2, solid electrolyte 3, and negative electrode 4 are strongly bonded together, improving the overall strength.

[0198] [Embodiment 5] This embodiment is a lithium ion secondary battery 1 having the same configuration as that of the fourth embodiment, except that the configuration of the positive electrode 2 is different. The solid electrolyte 3 and the negative electrode 4 of this embodiment are the same as those of the fourth embodiment. In this embodiment, configurations that are not particularly mentioned are the same as those of the fourth embodiment.

[0199] [Lithium-ion secondary battery] (positive electrode) The positive electrode 2 is a sintered body in which the positive electrode active material of the second embodiment and LiNbO3 are mixed in a predetermined state. The positive electrode 2 may contain a conventionally known additive such as a conductive material.

[0200] As shown in the cross-sectional view of FIG. 27, the positive electrode 2 of this embodiment has a mixture of the positive electrode active material and LiNbO3 with the content of LiNbO3 decreasing from the surface facing the solid electrolyte 3 to the back surface. Specifically, the positive electrode 2 of this embodiment has a structure in which three layers with different content ratios of the positive electrode active material and LiNbO3 are integrally bonded. From the surface facing the solid electrolyte 3 to the back surface, the bonding layer 22 with the highest content ratio of LiNbO3, the intermediate layer 23 with a lower content ratio of LiNbO3 than the bonding layer 22, and the active material layer 24 with a lower content ratio of LiNbO3 than the intermediate layer 23 are laminated in this order. The content ratios of LiNbO3 are bonding layer 22>intermediate layer 23>active material layer 24. The content ratios of the positive electrode active material are active material layer 24>intermediate layer 23>bonding layer 22.

[0201] The positive electrode 2 of this embodiment is in a state where a large amount of LiNbO3 is present at the bonding interface between the positive electrode active material and LiNbO3 and the solid electrolyte 3. The positive electrode 2 of this embodiment is formed by stacking three layers having different mixture ratios of the positive electrode active material and LiNbO3, but the number of layers is not limited as long as it is two or more layers in which the content ratio gradually changes. In addition, the positive electrode 2 of this embodiment has a content ratio that changes stepwise, but the content ratio may change smoothly.

[0202] [Method of manufacturing lithium-ion secondary batteries] The lithium ion secondary battery 1 of this embodiment is manufactured by the same manufacturing method as in the fourth embodiment, except for the positive electrode green sheet manufacturing step S6.

[0203] (Positive electrode green sheet manufacturing process; S6) This step S6 is a step of producing a green sheet for the positive electrode 2.

[0204] In step S6, a mixed powder of the positive electrode active material and LiNbO3 is prepared so as to contain a predetermined ratio, each mixed powder is compression molded, and each molded body is stacked in a state having a concentration gradient to produce a molded body (positive electrode green sheet).

[0205] In this embodiment, a three-layer compact (a compact of the raw material powder for each of the bonding layer 22, intermediate layer 23, and active material layer 24) having different content ratios of the positive electrode active material and LiNbO3 is manufactured in the same manner as in the third embodiment.

[0206] The produced compacts of the three layers are then laminated in this order to form the bonding layer 22, the intermediate layer 23, and the active material layer 24. The laminate is compressed in the lamination direction to bring the layers into close contact with each other.

[0207] In this manner, a positive electrode green sheet was produced.

[0208] The molded body (positive electrode green sheet) produced in step S6 is preferably dried in the same manner as in the fourth embodiment, and is preferably dried by subjecting it to a similar process.

[0209] [effect] This embodiment has the same effects as the fourth embodiment.

[0210] In the lithium ion secondary battery 1 of this embodiment, the positive electrode 2 contains a material (LiNbO3) that forms the solid electrolyte 3. The positive electrode 2 has the bonding layer 22, the intermediate layer 23, and the active material layer 24 formed such that the content of LiNbO3 decreases from the surface facing the solid electrolyte 3 toward the back surface.

[0211] According to this structure, a large amount of LiNbO3 exists at the interface between the positive electrode 2 and the solid electrolyte 3. Since LiNbO3 is the same material as the solid electrolyte 3, this sintered body is more strongly bonded together when sintered. In addition, a large amount of positive electrode active material exists on the surface of the positive electrode 2 facing the interface with the solid electrolyte 3, and a high battery capacity is achieved.

[0212] [Embodiment 6] This embodiment is a solid electrolyte in which the material having ion conductivity is different from that of each of the above embodiments. That is, the solid electrolyte of each of the above embodiments uses LiNbO3 as the material having ion conductivity, but the solid electrolyte may be formed using a material other than LiNbO3 as long as it has ion conductivity.

[0213] In materials having ion conductivity, the ion species that are conducted are not limited. In other words, the ion species that are conducted to the solid electrolyte are not limited. The ion species that are conducted can be ion species that can be conducted in conventional solid electrolytes. Li ions (Li + ) other than Na ion (Na + ), Mg ions (Mg 2+ ), K ion (K + ), Ca ions (Ca 2+ ), Al ions (Al 3+ ), O ion (O 2- ), H ions (H + ),OH ion (OH - ), F ions (F - ), Cl ions (Cl - ), hydride ion (H - ) and other ions. Among these ions, Li ion (Li + ) is more preferable.

[0214] The specific composition of the plate-like particle ion-conductive material is not limited as long as it is a material that can conduct ions. Examples include previously known solid electrolyte materials. The compounds exemplified below include those partially substituted (or solid-dissolved) with other elements (e.g., transition metal elements, etc.) and those made of crystals with lattice defects.

[0215] Examples of materials capable of conducting Li ions include inorganic solid electrolyte materials such as oxide-based solid electrolyte materials, sulfide-based solid electrolyte materials, nitride-based solid electrolyte materials, halide-based solid electrolyte materials, and anti-perovskite structure electrolyte materials.

[0216] Examples of sulfide-based solid electrolyte materials include Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-LiCl, Li2S-P2S5-LiBr, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, and Li2S-P2S5-Z. m S n (where m and n are positive numbers. Z is Ge, Zn, or Ga.), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li x MO y (where x and y are positive numbers. M is P, Si, Ge, B, Al, Ga, or In.),Li 10 GeP2S 12 etc. can be mentioned.

[0217] Examples of oxide-based solid electrolyte materials include Li2O-B2O3-P2O5, Li2O-SiO2, and LiLaTaO (e.g., Li5La3Ta2O 12 ), LiLaZrO (e.g., Li7La3Zr2O 12 . So-called LLZ. ), LiBaLaTaO (for example, Li6BaLa2Ta2O 12 ), Li 1+x S x P 1-x O4(0≦x<1, for example, Li 3.6 S 0.6 P 0.4 O4), Li 1+x Al x Ge 2-x (PO4)3(0≦x≦2),Li 1+x Al x Ti 2-x (PO4)3(0≦x≦2),Li3PO (4-3 / 2x) N x (0≦x<1) etc.

[0218] Examples of nitride-based solid electrolyte materials include Li3N and Li3PO 4-x Nx Examples of the halide-based solid electrolyte material include LiI.

[0219] Antiperovskite-type electrolyte material (general formula: LiO X ) for example, Li3OCl x Br y (x+y=1),Li2OHCl x Br y (x+y=1), Li2(OH) 0.9 F 0.1 Cl x Br y Examples include (x+y=1).

[0220] Lithium ion conductive ceramics can be cited as an example of a material that can conduct Li ions. Lithium ion conductive ceramics can be, for example, Li-La-Ti-O ceramics (LLTO). 3x La (2 / 3)-x □ (1 / 3)-2x An example is TiO3 (in the composition formula, squares indicate lattice defects).

[0221] Lithium titanate is an example of a material capable of conducting Li ions. Examples of lithium titanate include Li-Ti-O compounds, specifically Li2TiO3.

[0222] Examples of materials that can conduct sodium ions (sodium ion conducting solid electrolytes) include Na2Ti3O7, Na3PS4, Na3PO4, Na3PS4-Na3PO4-Al2O3, Na3Zr2Si2PO 12 Compounds such as the above can be mentioned.

[0223] Examples of materials that can conduct K ions (K ion conductive solid electrolytes) include K4Nb6O 17 , KTiNbO5 and other compounds.

[0224] Examples of materials capable of conducting Cl ions (Cl ion conductive solid electrolytes) include compounds such as LaOCl.

[0225] The plate-like particles of the above-mentioned ion-conductive material are shown in enlarged photographs in Figs. 28 to 33. 3x La (2 / 3)-x □ (1 / 3)-2x In Fig. 29, plate-shaped particles of Li2TiO3 are shown. In Fig. 30, plate-shaped particles of Na2Ti3O7 are shown. In Fig. 31, plate-shaped particles of K4Nb6O 17 Fig. 32 shows platelet particles of KTiNbO5. Fig. 33 shows platelet particles of LaOCl.

[0226] As shown in the enlarged photographs of Figs. 28 to 33, even if materials other than LiNbO3 are used, plate-like particles can be formed from each material.

[0227] The plate-like particles of these materials can form a masonry body in the same manner as in the first embodiment. Furthermore, since these materials are inorganic oxides, the plate-like particles can be bonded by sintering in the same manner as LiNbO3. That is, even if these materials are used, a masonry body can be formed in the same manner as in each of the above embodiments, and the masonry body can be sintered to form a sintered body (i.e., a solid electrolyte). The sintered body (solid electrolyte) has a neck-derived portion 31 and a particle-derived portion 30 in the same manner as the solid electrolyte 3 in each of the above embodiments. That is, the solid electrolyte of this embodiment has a crystal structure similar to that of the solid electrolyte 3 in each of the above embodiments.

[0228] In addition, when a material other than LiNbO3 is used as the ion-conductive material of the solid electrolyte 3, that is, when the ion species to be conducted is an ion other than Li ion, the solid electrolyte battery of the present invention becomes a battery in which the ion is conducted. 2- ) is an ion species in fuel cells (specifically, solid oxide fuel cells, SOFCs), hydroxide ions (OH - ) is the ion species in the air battery, sodium ion (Na +) is the ion species in sodium-ion batteries, and potassium ions (K + ) is the ion species in potassium ion batteries, magnesium (Mg 2+ ) and aluminum ions (Al 3+ ) and other multivalent cations such as hydride ions (H - ) and chloride ions (Cl - ), fluoride ion (F - ) is the ion species in an anion-ion battery, whereas hydrogen ions (H + ) can be used to form a battery such as a redox flow battery in which the ionic species is

[0229] Furthermore, the solid electrolyte of this embodiment has a crystal structure similar to that of the solid electrolyte 3 of each of the above embodiments, and can form a lithium ion secondary battery 1 similar to each embodiment (or a solid electrolyte battery that differs depending on the type of ions conducted).

[0230] Furthermore, a solid electrolyte battery can be manufactured using the manufacturing method of each of the above embodiments.

[0231] [effect] The solid electrolyte of this embodiment exerts the same effects as the solid electrolytes of embodiments 1 to 5. That is, even if the ion-conductive material of the solid electrolyte 3 is a material other than LiNbO3, it can exert the same effects as the above embodiments.

[0232] In particular, even if a material other than LiNbO3 is difficult to form plate-like particles from, the plate-like particles can be produced by the manufacturing method of the present invention. As a result, a solid electrolyte 3 and a solid electrolyte battery having excellent ion conductivity and suppressing damage (and short circuit occurrence) caused by the generation and growth of dendrites can be manufactured.

[0233] [Other effects of each form] The solid electrolyte of each of the above forms is made of a sintered laminate in which plate-like particles are arranged in a predetermined state.

[0234] As described above, this solid electrolyte 3 (sintered body) includes the particle-derived portions 30 and the neck-derived portions 31. The particle-derived portions 30 have a higher hardness than the neck-derived portions 31.

[0235] When the solid electrolyte (sintered body) is subjected to a physical shock or a thermal shock, a crack may occur. The crack occurs in the neck-derived portion 31, which has a relatively low hardness, in the solid electrolyte 3 (sintered body). When the crack propagates, it propagates along the neck-derived portion 31 (or the peripheral portion of the raw material particle-derived portion 30).

[0236] Each form of solid electrolyte has an intricate structure of neck-derived portions 31, and as shown in the schematic diagram of Figure 34, even if a crack propagates so as to penetrate the solid electrolyte 3, the direction of crack propagation hits the upper surface of the particle-derived portion 30, which has a higher hardness than the neck-derived portion 31, in a direction approximately perpendicular to the direction of crack propagation, and further propagation of the crack is suppressed by the particle-derived portion 30.

[0237] In this way, the occurrence and propagation of cracks is suppressed in the solid electrolyte 3 of each of the above embodiments, which results in an effect of suppressing cracking of the solid electrolyte 3 caused by the propagation of cracks, i.e., an effect of providing excellent crack resistance.

[0238] In contrast, when the solid electrolyte 3 is made of a sintered body of conventional spherical particle powder, a crack that propagates through the solid electrolyte 3 does not strike the upper surface of the particle-derived portion 30 substantially perpendicularly, but propagates along the neck-derived portion 31 (or the peripheral portion of the raw material particle-derived portion 30), as shown in the schematic diagram of Fig. 35. In other words, when the solid electrolyte 3 is made of a sintered body of conventional spherical particle powder, the effect of suppressing the occurrence and propagation of cracks is not achieved.

[0239] As described above in detail, the solid electrolyte of each of the above forms (the solid electrolyte of the present invention) can be used not only in solid electrolyte batteries but also in applications requiring high strength and resistance to damage. For example, it can be used as an electrolyte for batteries in which inorganic ions, not metal ions, serve as conductive ions, or as an electrolyte for sensor elements of gas sensors. EXAMPLES

[0240] The present invention will now be described more specifically with reference to examples. As examples of the present invention, a solid electrolyte and a solid electrolyte battery according to the first embodiment or a modified embodiment thereof were produced.

[0241] The solid electrolytes of the respective Examples and Comparative Examples were produced using the following plate-like particles. The compression step S5 and the sintering step S6 in the manufacturing methods of Example 1 and each of the comparative examples were carried out under the processing conditions described above.

[0242] Example 1 Starting from Nb2O5 and K2CO3, plate-shaped K4Nb6O was used as a sacrificial template. 17 The crystals were used to carry out the reaction in KCl flux. Next, a sacrificial template was immersed in hydrochloric acid to carry out proton exchange of the resulting compound (intermediate product). After the proton exchange, the resulting compound was mixed with LiNO3 and plate-shaped LiNbO3 crystals were grown in KNO3 flux to produce the plate-shaped particles of this example. The details of the reaction are shown below.

[0243] (1) 3Nb2O5+2K2CO3 → K4Nb6O 17 +2CO2 The reaction raw materials used were niobium oxide (Nb2O5, special grade, manufactured by Wako Pure Chemical Industries, Ltd.), potassium carbonate (K2CO3, manufactured by Wako Pure Chemical Industries, Ltd.), potassium nitrate (KNO3, special grade, manufactured by Wako Pure Chemical Industries, Ltd.), and potassium chloride (KCl, special grade, manufactured by Wako Pure Chemical Industries, Ltd.).

[0244] After adjusting the solute concentration to 20 mol%, the mixture was filled into an alumina crucible and covered with an alumina plate. The covered crucible was placed in an electric furnace (product name: FO100, manufactured by Yamato Scientific Co., Ltd.) and heated to obtain K4Nb6O 17 Plate-shaped crystals were synthesized at a heating rate of 45°C h -1 , holding time 5h, cooling rate 300℃·h -1 Heating, holding and cooling were performed under the following temperature conditions: By increasing the holding time in the heated state, the crystal grains that were generated grow, and plate-like particles can be generated.

[0245] (2) K4Nb6O 17 +4HCl → H4Nb6O 17 +4KCl K4Nb6O 17 The plate-like crystals (10 g) were placed in 1 M HCl solution (1 L) and immersed and stirred for 120 h. The HCl solution was replaced every 24 h.

[0246] After the reaction was completed, the mixture was repeatedly washed with distilled water until the pH of the washing solution became neutral. The crystals were then separated by suction filtration and collected. The separated crystals were vacuum dried overnight at 60°C to remove residual moisture and dry.

[0247] (3) H4Nb6O 17 +6LiNO3 → 6LiNbO3+2H2O+6NO x K4Nb6O after proton exchange 17 (H4Nb6O 17 The ) crystals, lithium nitrate (LiNO3, manufactured by Wako Pure Chemical Industries, Ltd.), and potassium nitrate (KNO3, purity 99+%, manufactured by Wako Pure Chemical Industries, Ltd.) were weighed and dry mixed. The mixture was then placed in a B2 type alumina crucible (SSA-S). The alumina crucible was covered with an alumina plate and heated for a specified time using an electric furnace (product name: FO100, manufactured by Yamato Scientific Co., Ltd.). The heating rate was 500°C·h -1 , holding time 5min, cooling rate 200℃・h -1 The heating, holding and cooling were carried out under the temperature conditions.

[0248] In this manner, plate-like particles (primary particles) made of LiNbO3 of this example were produced.

[0249] The plate-like particles in this example are made of LiNbO3, with a length (a):width (b) ratio of 2.2:1 and a length (b):plate thickness (c) ratio of 3.1:1. The average particle size (D50) is 8.0 μm, and in the particle size distribution, the length between D25 and D75 is 11.5 μm, which is 144% of the length of D50.

[0250] FIG. 36 is an enlarged photograph of a cut surface of the compressed laminate produced in the production of the solid electrolyte of this example.

[0251] Comparative Example 1 Except for changing the potassium source of the starting material from K2CO3 to KNO3, plate-like LiNbO3 crystals were synthesized in the same manner as in Example 1. The plate-like particles (primary particles) of this example have a different particle shape from the plate-like particles of Example 1.

[0252] The plate-like particles in this example are made of LiNbO3, with a length (a):width (b) ratio of 1.6:1, and a length (b):plate thickness (c) ratio of 1.2:1, and an average particle size (D50) of 3.8 μm, and in the particle size distribution, the length between D25 and D75 is 7.3 μm, which is 192% of the length of D50.

[0253] FIG. 37 shows an enlarged photograph of a cut surface of the laminate in the production of the solid electrolyte of this example.

[0254] Comparative Example 2 Except for the difference in the shape of the plate-like particles (primary particles), plate-like LiNbO3 crystals were synthesized in the same manner as in Comparative Example 1. The plate-like particles (primary particles) of this example have a different particle shape from the plate-like particles of Example 1.

[0255] The plate-like particles in this example are made of LiNbO3, with a length (a):width (b) ratio of 1.0:1, and a length (b):plate thickness (c) ratio of 2.7:1, an average particle size (D50) of 3.8 μm, and a length between D25 and D75 in the particle size distribution of 7.3 μm, which is 192% of the length of D50.

[0256] [evaluation] Solid electrolyte battery cells (test cells) having the solid electrolytes of Example 1 and Comparative Examples 1 and 2 were manufactured and evaluated.

[0257] (Battery cell manufacturing) Steps S1 to S6 of the manufacturing method of the first embodiment are used to manufacture a disk-shaped solid electrolyte having a thickness of 45 μm.

[0258] Electrodes made of metal Li were welded to both sides of the disk-shaped solid electrolyte in the same manner as in the negative electrode welding step S8 in embodiment 3. The electrodes produced by welding were disk-shaped with a diameter of φ: 8 mm and a thickness of 500 nm.

[0259] In this manner, the solid electrolyte battery cells (test cells) of Example 1 and Comparative Examples 1 and 2 were manufactured.

[0260] (Ionic Conductivity) The ionic conductivity of the solid electrolyte 3 was determined for the battery cells of Example 1 and Comparative Examples 1 and 2 using an AC impedance method. The impedance measurement results obtained by the AC impedance method are shown in Fig. 38. In Fig. 38, the actually measured impedance values ​​are shown as points (·), and the simulation values ​​obtained by fitting to the equivalent circuit in Fig. 39 are also shown as solid lines.

[0261] The ionic conductivity of the solid electrolyte 3 of the battery cells of Example 1 and each of the comparative examples calculated from the measurement results of FIG. 38 and FIG. 39 is 1.5×10 -7 (S cm -1 ) was.

[0262] That is, the solid electrolyte of embodiment 1 has high Li ion conductivity.

[0263] (Constant current cycle characteristics) A constant current cycle test was performed on the battery cells of Example 1 and Comparative Examples 1 and 2. The test results of the battery cell of Example 1 are shown in Fig. 40, the test results of the battery cell of Comparative Example 1 in Fig. 41, and the test results of the battery cell of Comparative Example 2 in Fig. 42.

[0264] The constant current cycle test was carried out using a galvanometer stud (product name: SP-50, manufactured by Bio-Logic) as follows.

[0265] A plate-shaped LiNbO3 sheet was produced by the green sheet method. After punching out the sheet to φ12 mm, it was pressurized at 20 MPa using a uniaxial pressurizing machine (product name: 100kN Newton Press, manufactured by NPa Systems Co., Ltd.). After that, it was pressurized at 300 MPa for 10 minutes using a cold isostatic pressurizing machine (product name: Press-CIP, manufactured by NPa Systems Co., Ltd.).

[0266] A resistance heating vacuum deposition apparatus (product name: SVC-700TMSG, manufactured by Sanyu Electronics Co., Ltd.) was used, and the back pressure was 5.0 × 10 -3 A lithium electrode was fabricated on the surface of the composite at a temperature of 1000 Pa and a current of 15 to 25 A. The area of ​​the electrode was 0.50 cm 2 The experimental conditions were adjusted so that the electrode thickness was about 500 nm. A symmetric cell was prepared using a two-electrode dry measurement cell (product name: HS Flat Cell, manufactured by Hosen Co., Ltd.).

[0267] A galvanometer stud (product name: SP-50, manufactured by Bio-Logic) was used for the constant current cycle. The measurement temperature was 25°C, and the current value was 0.02 to 0.9 mA cm. -2 The cycle was repeated every hour at a current value of 0.02 to 1.5 mA cm for each comparative example. -2 The cycle was repeated.

[0268] As shown in FIG. 40, the battery cell of the embodiment has a current density of 0.9 mA cm -2It can be seen that no short circuit due to dendrites occurs even when the current density increases to 0.9 mA cm. In contrast, in the battery cell of the comparative example, as shown in Figure 41, the voltage excessively increases at 10 (s) and the current density also increases. In other words, it can be seen that a short circuit due to dendrites occurs in the battery cell of Comparative Example 1. As shown in Figure 42, when the current density is 0.9 mA cm -2 When the potential of the battery cell increases to 10V, the voltage excessively increases and the current density increases. In other words, it can be confirmed that a short circuit (micro-short circuit) due to dendrites occurred in the battery cell of Comparative Example 2.

[0269] As described above, the solid electrolyte of Example 1 exhibits the effect of suppressing damage caused by the occurrence of short circuits due to the occurrence and growth of dendrites in a battery using the solid electrolyte of Example 1.

[0270] Example 2 A solid electrolyte was produced and evaluated using the modified embodiment of the first embodiment. The configuration of this example that is not specifically mentioned is the same as that of the first embodiment. The solid electrolyte of this example can be used to produce a solid electrolyte battery in the same manner as that of the first embodiment.

[0271] Specifically, a solid electrolyte having a thickness of 45 μm was manufactured using steps S1 to S5 of the manufacturing method of embodiment 1. The solid electrolyte was then punched into a disk shape having a diameter of 12 mm using a punching machine (manufactured by Hosen Co., Ltd.), and then pressure molded at 20 MPa using a uniaxial pressing machine (product name: 100 kN Newton Press, manufactured by NPa Systems Co., Ltd.). After that, the solid electrolyte was further pressure molded at 300 MPa for 10 minutes using a cold isostatic pressing machine (product name: Press-CIP, manufactured by NPa Systems Co., Ltd.). The compact was then sintered in an infrared heating furnace (product name: HP-2-6S, manufactured by Yonekura Seisakusho Co., Ltd.). The infrared heating furnace was operated at 6000°C·h -1 The temperature is raised to 300°C at a rate of 100°C and held for 1 hour. After that, the sample is heated to 6000°C·h -1 The temperature is raised to 1000°C at a rate of 100°C and maintained at that temperature for 0.08 hours (4 minutes and 48 seconds). After maintaining the temperature, the heating is stopped (power to the heater is turned off) and the material is immediately allowed to cool. In this manner, the solid electrolyte of this example was produced.

[0272] [evaluation] (Relative Density) The solid electrolyte of this example had a film thickness of 39 μm and a relative density of 63%. The relative density was calculated by (measured density) / (true density)×100(%). The true density is the density of LiNbO3. On the other hand, the relative density of the solid electrolyte of Example 1 was 45%, and the solid electrolyte of this example had a higher relative density (i.e., was dense). A dense solid electrolyte has high strength, and the film thickness of the solid electrolyte can be made thin. This allows the lithium secondary battery using the solid electrolyte (solid electrolyte secondary battery) to be miniaturized, and a battery with high energy density can be obtained.

[0273] (SEM) The cross section of the produced solid electrolyte was observed using a FIB-SEM (product name: JIB-4610F, manufactured by JEOL Ltd.) at an acceleration voltage of 15 kV. An enlarged photograph of the cross section of the solid electrolyte taken is shown in FIG. As shown in FIG. 43, the solid electrolyte of this example has a structure in which plate-like particles (masonry) are sintered while maintaining the particle shape of the masonry (plate-like particles). More specifically, it can be seen that adjacent plate-like particles are sintered with necks formed between them. Meanwhile, it can be seen that even after sintering, the shape of the plate-like particles before sintering is almost maintained, and there is almost no grain growth of the plate-like particles themselves. In other words, the solid electrolyte of this example has a more complicated structure in the neck-derived portions. As described above, the solid electrolyte of this example has a complex crystal structure similar to that of Example 1, and therefore can exert the same effect as the solid electrolyte of Example 1. That is, the battery using the solid electrolyte of this example exerts the effect of suppressing the generation and growth of dendrites, as well as the occurrence of short circuits due to dendrites. When the constant current cycle characteristics are measured in the same manner as in Example 1, the effect of preventing short circuits due to dendrites is exerted. Moreover, the solid electrolyte of this embodiment is a dense solid electrolyte, which provides the effect of enabling a battery with a high energy density to be obtained. That is, according to this embodiment, it is possible to obtain an effect that a battery having a high energy density and in which damage caused by dendrites is suppressed can be obtained. [Explanation of symbols]

[0274] 1: Lithium-ion secondary battery, 2: Positive electrode, 3: Solid electrolyte, 4: Negative electrode, 5: Case

Claims

1. The present invention comprises a sintered laminate formed by stacking a plurality of plate-like particles made of an ion-conductive material in a thickness direction of the plate-like particles and arranging the plate-like particles in a direction in which the plates extend, The plate-like particles have a length:width ratio of 2.2 to 3:1 and a width:plate thickness ratio of 3.1 to 4:

1.

2. The solid electrolyte according to claim 1, wherein the plate-like particles have an average particle size (D50) of 2.0 μm to 8.0 μm.

3. The solid electrolyte according to claim 2, wherein the length between the 25% cumulative value (D25) and the 75% cumulative value (D75) from the smallest diameter in the particle size distribution is 34 to 230% of the length of the average particle diameter (D50).

4. The solid electrolyte according to any one of claims 1 to 3, wherein the solid electrolyte has a plate shape extending in a direction in which the plate-like particles extend, and has a thickness of 0.5 µm or more.

5. The ion-conductive material is LiNbO 3 The solid electrolyte according to any one of claims 1 to 4,

6. The solid electrolyte according to any one of claims 1 to 5, a positive electrode provided in close contact with one surface of the solid electrolyte in the thickness direction; a negative electrode provided in close contact with the other surface of the solid electrolyte in the thickness direction; A solid electrolyte battery comprising:

7. the positive electrode has a positive electrode active material capable of absorbing and releasing ionic species conducted by the solid electrolyte, 7. The solid electrolyte battery in accordance with claim 6, wherein the negative electrode comprises a negative electrode active material capable of absorbing and releasing ionic species conducted by the solid electrolyte.

8. 8. The solid electrolyte battery in accordance with claim 7, wherein at least one of the positive electrode and the negative electrode further contains a material having ion conductivity.

9. 9. The solid electrolyte battery in accordance with claim 8, wherein the material having ion conductivity is the same as the material of the solid electrolyte.

10. 10. The solid electrolyte battery according to claim 6, wherein the solid electrolyte, the positive electrode and the negative electrode are integrally formed.

11. The solid electrolyte is LiNbO 3 It consists of The positive electrode has a positive electrode active material that is a material capable of absorbing and releasing Li ions, 11. The solid electrolyte battery according to claim 6, wherein the negative electrode has a negative electrode active material that is capable of absorbing and releasing Li ions.

12. A method for producing a solid electrolyte battery having the solid electrolyte according to any one of claims 1 to 5, comprising the steps of: A preparation step of preparing a paste by dispersing a powder of plate-like particles made of an ion-conductive material in a dispersion medium; a coating step of applying the paste to the coating surface while applying a shear stress along the coating surface; a sintering step of sintering the coating body; 2. A method for producing a solid electrolyte battery comprising the steps of:

13. The method for producing a solid electrolyte battery according to claim 12, wherein the coating step is a step of coating the paste onto the coating surface with a bar coater.

14. The method for producing a solid electrolyte battery according to any one of claims 12 to 13, further comprising an electrode forming step of forming a positive electrode on one surface of the sintered body in the thickness direction and a negative electrode on the other surface.

15. The electrode forming step includes:

15. The method for producing a solid electrolyte battery according to claim 14, further comprising the step of forming the negative electrode by welding a material for the negative electrode to the other surface of the sintered body.

16. The electrode forming step includes: a step of disposing a positive electrode material on one surface of the sintered body and a negative electrode material on the other surface of the sintered body; sintering the laminate; The method for producing a solid electrolyte battery according to claim 14, comprising:

17. The method for producing a solid electrolyte battery according to any one of claims 12 to 13, wherein the sintering step is a step of disposing a positive electrode material and a negative electrode material on both sides of the coated body in a thickness direction, and then sintering the materials.

18. The method for producing a solid electrolyte battery according to any one of claims 12 to 17, wherein the plate-like particles are produced by producing a plate-like intermediate product by a flux method, and then producing a final product from the intermediate product by an ion exchange method.

19. A method for producing the solid electrolyte according to any one of claims 1 to 5, comprising the steps of: A preparation step of preparing a paste by dispersing a powder of plate-like particles made of an ion-conductive material in a dispersion medium; a coating step of applying the paste to the coating surface while applying a shear stress along the coating surface; a sintering step of sintering the coating body; 2. A method for producing a solid electrolyte comprising the steps of:

20. A method for producing a solid electrolyte as described in claim 19, wherein the coating process is a process of applying the paste to the coating surface using a bar coater.

Citation Information

Patent Citations

  • Method of manufacturing crystal oriented ceramic

    JP2009114037A

  • Solid electrolyte particle, solid electrolyte membrane and method for producing solid electrolyte particle

    JP2013058376A

  • Method for manufacturing electrode body, and battery including electrode body manufactured thereby

    JP2015109199A

  • Solid electrolyte slurry, method for manufacturing solid electrolyte sheet, solid electrolyte slurry inclusion body, electrode slurry, method for manufacturing electrode sheet, electrode slurry inclusion body, and method for manufacturing all-solid type lithium ion battery

    JP2016062709A

  • Ion conductive ceramic and manufacturing method therefor

    JP2017061390A