A red phosphorus-carbon negative electrode material and preparation method thereof
By inlaiding low-melting point transition metal compounds and red phosphorus inside the carbon nanotube sphere, the poor conductivity and volume expansion problems of phosphorus-carbon composite anode materials are solved, the energy density and rate performance of lithium-ion batteries are improved, and the cycle life of the battery is extended .
Patent Information
- Application Number
- CN202211312036.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-10-25
AI Technical Summary
The existing phosphorus-carbon composite anode materials have problems such as poor conductivity, large volume expansion, unstable interface and poor wetting of metal lithium in lithium in lithium, which limits their application performance.
By inlaid with low melting point transition metal compounds and red phosphorus in the carbon nanotube spheres, high-performance phosphorus-carbon composite anode material is prepared by using low-temperature liquid phase method and hydrothermal reaction technology to improve its conductivity and cyclic stability.
The specific capacity and rate performance of the phosphorus-carbon composite anode material is significantly improved, the volume expansion is reduced, the wetting and electrochemical stability of metal lithium are enhanced, and the cycle life of the battery is extended.
Smart Images

Figure CN115621445B_ABST
Abstract
Description
Technical Field
[0001] The present invention specifically relates to a method for preparing a phosphorus-carbon composite negative electrode based on red phosphorus-doped carbon nanotube technology. The preparation of a phosphorus-carbon composite negative electrode with high reversible specific capacity and good rate performance is achieved by embedding a low-melting point transition metal compound inside a carbon tube ball and then compounding red phosphorus, which is conducive to further realizing a commercial lithium-ion battery system with high energy density, high rate performance and low cost. It belongs to the lithium-ion battery negative electrode direction in the field of lithium-ion new energy material technology. Background Art
[0002] Lithium-ion batteries are expected to have a larger application market in the fields of consumption, power and energy storage, but more opportunities also mean more challenges. With the vigorous development of lithium-ion batteries in new energy vehicles, mobile devices and other fields, people have also put forward higher requirements for the energy density and high-rate performance of lithium-ion battery systems. At present, conventional commercial negative electrode materials are mainly based on carbon-based negative electrodes (such as the most conventional and widely used graphite negative electrode). The layered structure of lithium insertion and delithiation has good cycle performance, but it also has a low theoretical specific capacity (372mA·h·g -1 ), poor high rate charge and discharge performance. On the contrary, among many negative electrode material systems, phosphorus-based negative electrodes have higher theoretical specific capacity (such as Li3P, 2596mA·h·g -1 ) and excellent rate performance, and relatively low cost, is one of the research directions that is expected to further achieve high energy density and high rate performance in the future. However, phosphorus-based materials have poor conductivity and large volume expansion during the cycle (volume expansion rate is as high as 300%), and the material cycle performance needs to be further optimized and improved, which largely limits the application of phosphorus-based negative electrode materials in lithium-ion batteries.
[0003] In order to solve this problem, the phosphorus-carbon composite negative electrode is expected to combine the advantages of both, and achieve higher energy density and better rate performance by means of the synergistic effect of phosphorus-based and multidimensional carbon materials. Among the many carbon-based materials, carbon nanotubes can form a three-dimensional skeleton structure, which can effectively solve the problems of volume expansion of phosphorus-based negative electrodes. In the work of CN109309199, a method for preparing a red phosphorus / carbon nanotube composite material for a negative electrode of a lithium ion battery is disclosed. The method uses a low-temperature liquid phase method to make red phosphorus uniformly adsorbed on the wall of carbon nanotubes by means of the surface electrical difference between red phosphorus and carbon nanotubes in a solvent, and obtains a uniform red phosphorus / carbon nanotube composite material. The preparation method is simple and environmentally friendly, and the obtained material significantly improves the specific capacity of lithium ion batteries and the cyclic charge and discharge stability. In the work of CN111769271, a MXene / red phosphorus composite negative electrode material with high capacity and high cycle performance is obtained by mixing and calcining large-spacing MXene with red phosphorus at high temperature. The composite material is based on the high theoretical specific capacity of red phosphorus, and makes full use of the advantages of large-spacing MXene such as high electronic conductivity, large specific surface area, strong mechanical properties, surface modifiable and unique layered structure, as an ideal carbon carrier to improve the conductivity and structural stability of red phosphorus. CN112420999 discloses a phosphorus-carbon composite material with a core-shell coating structure, including a phosphorus-based material core body and a carbon-based material coating layer, which can not only alleviate the volume expansion during the charge and discharge process, but also inhibit the dissolution of lithium phosphide during the charge and discharge cycle of the lithium battery and the side reaction between the electrode interface / electrolyte, thereby having good charge and discharge specific capacity and cycle performance. In the work of CN114122386, a tin phosphide @ carbon composite negative electrode active precursor material includes a carbon single substance skeleton, and tin phosphide nanoparticles embedded on its outer surface and distributed in a dotted manner. The material described in CN109309 has tin phosphide nanodots evenly dispersed on the outer surface of the carbon skeleton. Based on the innovative morphology and structural characteristics, combined with the rich specific surface area and good conductivity of the carbon skeleton, the local current density is effectively reduced, and more uniform lithium deposition and dissolution are achieved during the cycle. Summary of the invention
[0004] The purpose of this patent is to protect a method for preparing a high-performance composite phosphorus-carbon negative electrode by using carbon nanotube balls doped with red phosphorus and internal low-melting-point transition metal compounds through low-temperature liquid phase immersion.
[0005] The conductivity of pure phosphorus-based negative electrode materials is poor (the conductivity of red phosphorus is only 10 -14 S cm -1 ), the redox kinetics are slow during the lithium insertion / extraction process, the internal polarization of the battery is severe, the SEI film thickens, resulting in serious lithium ion loss, and the huge volume expansion during the charge and discharge cycle (the volume expansion rate is as high as 300%) easily causes the active material to pulverize, seriously affecting the coulombic efficiency and rate cycling performance of the material.
[0006] The theoretical specific capacity of pure carbon-based negative electrode materials is low (372mA·h·g -1 ), and during high current charging and discharging, the lithium ion diffusion rate and diffusion channel are limited, the lithium extraction / insertion rate is slow, and at the same time, a compound Li is formed between the graphite carbon layers during the insertion process. x C6, increases the interlayer spacing of the carbon layer, easily causes the carbon layer to fall off, and reduces the capacity, cycle performance and service life of the carbon-based negative electrode material.
[0007] The existing phosphorus-carbon composite negative electrode materials connect the carbon carrier and the phosphorus active component with a stable chemical bond. The carbon material has high conductivity, large specific surface area and flexible surface, which can easily form a conductive network, promote the uniform dispersion of the active component, and absorb the mechanical stress generated by the volume change process, prevent the phosphorus active component from breaking and pulverizing, and improve the rate performance and cycle stability. However, at present, phosphorus-carbon negative electrodes generally have problems such as unstable interface and poor wettability to metallic lithium.
[0008] Gasification condensation process: Red phosphorus is sublimated at a temperature above 450 degrees, so that the red phosphorus vapor is evenly deposited on the wall of the carbon nanotube through capillary force and pressure difference, and adsorbed and deposited on the inner surface of the carbon nanotube after cooling. Its disadvantage is that the amount of phosphorus deposited on the conductive carbon frame through the gasification condensation process is limited, and the phosphorus loading is an important factor affecting the battery capacity performance. In addition, the white phosphorus byproduct that is easily formed during the cooling process is flammable and has a certain degree of danger. The removal of white phosphorus requires the use of toxic reagents such as carbon disulfide, which poses a great safety hazard.
[0009] High-temperature pyrolysis process: With phosphorus material as the substrate, amorphous carbon produced by high-temperature pyrolysis of organic matter in an inert atmosphere is used as the carbon source to coat the phosphorus material, thereby obtaining a phosphorus-carbon composite material with a core-shell coating structure. However, phosphorus as the core in the composite material prepared by the high-temperature pyrolysis process has poor dispersion, and the carbon layer produced by the pyrolysis of organic matter is prone to uneven distribution, and the agglomeration phenomenon between particles is serious when the pyrolysis temperature is slightly higher.
[0010] Carbon thermal reduction process: At a certain temperature, inorganic carbon is used as a reducing agent to reduce phosphide to prepare a phosphorus-carbon composite material. Its disadvantages are that the reduction process is difficult to control, the phosphorus-carbon ratio requires high precision, and it is easy to produce impurities, making product quality control difficult, and the particle size is inconsistent and the dispersion is poor.
[0011] Based on the above-mentioned related technical means, with the help of the introduction of similar intermediate products such as SnS2 inside the carbon tube ball, the performance of the phosphorus-carbon composite negative electrode is improved by the method of low-temperature liquid phase immersion: First, the generation of white phosphorus byproducts can be effectively reduced by controlling the temperature and atmosphere, effectively reducing the manufacturing cost and improving the safety of the preparation process; second, by forming similar solid solutions such as lithium tin inside the carbon tube ball during the first charge and discharge, the wettability of the phosphorus-carbon composite ball to metallic lithium in the cycle is improved. At the same time, SnS2 and the like can be precisely controlled to form a nanosheet structure with highly exposed active sites, which can easily form uniformly distributed alloy sites when in contact with molten metallic lithium at high temperatures. The third aspect is that there is a potential difference of about 0.3V between the series of lithium-tin alloys formed and metallic lithium, which can be used as a driving force for lithium diffusion. At the same time, due to the low deposition overpotential of metallic lithium on tin, it is helpful for metallic lithium to penetrate into the interior of the phosphorus-carbon composite microspheres, so that the first charge specific capacity of the phosphorus-carbon negative electrode is increased by 30% or more. Fourthly, lithium-tin alloy has a relatively high chemical potential, so compared with pure metallic lithium anode or phosphorus-carbon anode, it is less likely to have side reactions with liquid electrolyte, thereby ensuring less electrolyte consumption and longer cycle life.
[0012] In view of the above technical problems, the present invention provides a red phosphorus-carbon composite negative electrode material doped with carbon nanotubes, comprising red phosphorus and composite carbon nanotube balls.
[0013] Furthermore, the mass ratio of the red phosphorus to the composite carbon nanotube sphere is 1:1-3:1.
[0014] Furthermore, in the product obtained by thermal reaction after red phosphorus and composite carbon nanotube balls are mixed in a solvent, the mass concentration of the composite carbon nanotube balls in the solution is 10%-20%.
[0015] The small-size red phosphorus of the present invention is uniformly compounded on the carbon nanotube microspheres with a three-dimensional porous skeleton, which prevents the large-scale agglomeration of red phosphorus particles, improves the conductivity of the red phosphorus material, and effectively solves the volume expansion problem during the charging and discharging process. The red phosphorus can be in a powder state of 60-100 meshes, or in a microsphere particle state of 10-20 meshes.
[0016] Furthermore, the solvent in the thermal reaction process includes at least one of deionized water, anhydrous ethanol, anhydrous methanol, and anhydrous ether.
[0017] Furthermore, the composite carbon nanotube ball is doped and embedded with a low melting point transition metal compound (≤200° C.); the mass concentration of the low melting point transition metal compound is 0.2-3%.
[0018] The low-melting-point transition metal compound intermediates embedded inside the carbon nanotubes help lithium to be evenly infiltrated into the internal channels of the carbon tube balls, significantly improving the specific capacity and rate performance of the phosphorus-carbon composite negative electrode material (the first charge specific capacity is increased by 30% or more), while avoiding the deposition of metallic lithium on the electrode surface and reacting with the electrolyte, thereby improving the cycle performance of the material.
[0019] Furthermore, the low melting point transition metal compound is obtained by reacting a metal source of tin, titanium, cadmium, iron, cobalt, chromium, manganese, germanium, or nickel with a non-metal source, and the molar ratio of the non-metal source to the metal source is 1:1-3:1.
[0020] Furthermore, the metal salts include fluorides, chlorides, nitrates, sulfates and carbonates of tin, titanium, cadmium, iron, cobalt, chromium, manganese and nickel; the non-metallic source includes any one or more of sulfides, selenides, tellurides and phosphides; the sulfides include at least one of sublimated sulfur, thioacetamide and thiourea, the selenides include at least one of elemental selenium powder and sodium selenite, the tellurides include at least one of elemental tellurium powder and sodium tellurite, and the phosphides include at least one of sodium hypophosphite, phosphoric acid, ammonium dihydrogen phosphate and diammonium hydrogen phosphate.
[0021] Further examples include Fe2S3, GeS2, SnS2, Co9S8, NiSe, SnTe2 or TiP, but are not limited to these.
[0022] Furthermore, the precursor of the three-dimensional carbon tube material can be any one of carbon nanofibers, carbon nanotubes, mesoporous carbon, porous carbon, and commonly used conductive agents such as carbon black and Super P.
[0023] The carbon nanotube spheres may also be materials with different particle sizes and skeleton structures obtained by surface modification through any one or more of amination, carboxylation, hydroxylation, phosphination, or graphitization.
[0024] The surface-modified three-dimensional porous skeleton of carbon nanotubes can enhance the composite strength with low-melting-point transition metal compounds and red phosphorus, avoid the consumption of lithium ions by the SEI film, reduce the occurrence of side reactions, and improve the reversible charge and discharge performance and cycle stability of the phosphorus-carbon composite negative electrode material.
[0025] The phosphorus-carbon composite negative electrode prepared based on red phosphorus carbon nanotube ball doping technology has good morphological and structural stability due to the strong interaction between the components. It can still maintain the basic morphological structure after multiple charge and discharge cycles at a high current density, avoiding structural collapse and causing lithium precipitation problems.
[0026] The second aspect of the present invention is a method for preparing a phosphorus-carbon composite negative electrode material doped with red phosphorus carbon nanotubes, which is based on a liquid phase method to prepare a low melting point transition metal compound intermediate, has a simple preparation process, is easy to operate, and the prepared intermediate material has a uniform morphology and a small particle size, which is conducive to the subsequent doping in the carbon tube ball. The method specifically comprises the following steps:
[0027] (1) Preparation of a low melting point transition metal compound intermediate solution: dissolving a metal source and a non-metal source in a solvent, and performing a solvent / hydrothermal reaction to obtain a low melting point transition metal compound intermediate solution;
[0028] (2) Preparation of composite carbon nanotube balls: The carbon nanotube balls are dispersed in the low-melting point transition metal compound intermediate solution, and solid-liquid separation is performed after solvent / hydrothermal reaction. The filter cake is dried to obtain a composite carbon nanotube ball powder material; the low-melting point transition metal compound intermediate is introduced into the carbon nanotube ball, which can better realize the composite of phosphorus and carbon materials on the one hand, and on the other hand, it is alloyed with metallic lithium and introduced into the internal channel of the carbon nanotube ball to prevent deposition on the outer surface of the carbon nanotube ball and reaction with the electrolyte, while improving the material specific capacity and rate performance.
[0029] (3) Preparation of red phosphorus dispersion: After ball milling, red phosphorus is subjected to hydrothermal treatment, and the dried solid matter is dispersed in a solvent to obtain a uniform red phosphorus dispersion;
[0030] (4) Preparation of composite phosphorus-carbon negative electrode material: ultrasonically disperse the composite carbon nanotube ball powder material in a solvent, add the red phosphorus dispersion, perform solvent / hydrothermal reaction after ultrasonic treatment, collect the solid matter after centrifugal washing, and freeze-dry to obtain a composite phosphorus-carbon negative electrode material.
[0031] The introduction of the liquid phase and the molten phase in the process of the present invention is conducive to better achieving uniform compounding of the phosphorus-carbon material, improving the bonding strength between the components, enhancing the structural stability of the material, and improving the cycle performance of the phosphorus-carbon composite negative electrode material.
[0032] Preferably, the metal source in step (1) comprises any one of fluorides, chlorides, nitrates, sulfates or carbonates of tin, titanium, cadmium, iron, cobalt, chromium, manganese, germanium or nickel.
[0033] Preferably, the non-metallic source includes one of a sulfide, a selenide, a telluride or a phosphide; preferably, the sulfide includes at least one of sublimated sulfur, thioacetamide and thiourea, the selenide includes at least one of elemental selenium powder and sodium selenite, the telluride includes at least one of elemental tellurium powder and sodium tellurite, and the phosphide includes at least one of sodium hypophosphite, phosphoric acid, ammonium dihydrogen phosphate and diamine hydrogen phosphate.
[0034] Preferably, it includes Fe2S3, GeS2, SnS2, Co9S8, NiSe, SnTe2 or TiP, but is not limited thereto.
[0035] Preferably, the molar ratio of the non-metal source to the metal source is 1:1-3:1.
[0036] Preferably, the solvent includes at least one of deionized water, anhydrous ethanol, anhydrous methanol or anhydrous ether.
[0037] Preferably, the mass concentration of the low melting point transition metal compound intermediate is 0.2-3%.
[0038] Preferably, during the preparation of the low melting point transition metal compound intermediate solution, the solvent / hydrothermal reaction temperature is 50-100° C., the reaction time is 5-50 mins, and magnetic stirring is used during the solvent / hydrothermal reaction at a rotation speed of 300-2000 rpm.
[0039] The carbon nanotube spheres may also be materials with different particle sizes and skeleton structures obtained by surface modification through any one or more of amination, carboxylation, hydroxylation, phosphination, or graphitization.
[0040] Preferably, the mass ratio of the carbon nanotube spheres to the low-melting-point transition metal compound intermediate is 1:1-3:1.
[0041] Preferably, in the preparation process of the composite carbon nanotube spheres in step (2), the solvent / hydrothermal reaction temperature is 40-90°C, the reaction time is 20-80 minutes, and solid-liquid separation is carried out by suction filtration and washing, and the obtained filter cake is placed in a vacuum drying oven at 50-60°C and dried overnight.
[0042] Preferably, during the red phosphorus ball milling process of step (3), red phosphorus and stainless steel balls are loaded into a stainless steel ball tank at a mass ratio of 1:10-1:50, and ball milled at a speed of 300-500 rpm for 1-5 hours under a nitrogen atmosphere. During the hydrothermal treatment, the hydrothermal reaction temperature is 150-200° C. and the reaction time is 10-20 hours.
[0043] The formation of strong and stable chemical bonds between different components during the ball milling process is crucial to achieving high rate and cycle performance of phosphorus-carbon composite materials. However, in the process of achieving phosphorus-carbon composites through mechanical ball milling, the uniformity of the material cannot be well guaranteed, the particle agglomeration phenomenon is serious, it is difficult to establish connections between components through chemical bonds, and ball milling will cause damage to the three-dimensional skeleton of carbon nanotubes, which is not conducive to suppressing the volume expansion effect during the cycle. The present invention, with the help of liquid phase and melting and other forms, can effectively achieve uniform composite materials without damaging the three-dimensional skeleton of the material.
[0044] Preferably, the mass concentration of the red phosphorus dispersion in step (4) is 10%-20%; the mass concentration of the composite carbon nanotube ball powder material in the solution is 10%-20%; and the mass ratio of red phosphorus to the composite carbon nanotube ball powder material is 1:1-3:1.
[0045] Preferably, in step (4), the solvent / hydrothermal reaction temperature is 150-500° C., and the reaction time is 20-60 minutes.
[0046] The third aspect of the present invention is to use the prepared red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material as a negative electrode for a lithium-ion battery.
[0047] The present invention uses a battery assembled from the phosphorus-carbon composite negative electrode material under the doping system.
[0048] The composite negative electrode material of the present invention is used in a high-capacity and high-rate lithium-ion battery system.
[0049] The assembly steps of the high-capacity, high-rate lithium-ion battery are as follows: the phosphorus-carbon composite negative electrode material prepared above is mixed with a binder (PVDF) and acetylene black (AB) in a mass ratio of 8:1:1, mixed evenly in an NMP solvent, coated on a copper foil, and vacuum dried at 80°C to punch out a sheet as a working electrode, a metal lithium sheet as a counter electrode, and 1.0M LiTFSI in DOL:DME (V:V=1:1) + 1.0wt.% LiNO3 as an experimental electrolyte system to assemble a button cell (half cell) and perform a charge and discharge cycle test.
[0050] The technical solution of the present invention has the following beneficial effects:
[0051] Improve safety: With the introduction of low-melting-point transition metal compound intermediates, the generation of by-product white phosphorus can be effectively reduced, the manufacturing cost can be effectively reduced, and the safety of the preparation process can be improved;
[0052] Solve the volume expansion problem: Use the three-dimensional skeleton structure of carbon nanotubes to effectively inhibit the volume expansion problem of phosphorus-based materials during the cycle; Improve the wettability of the phosphorus-carbon composite negative electrode: The process of transition metal compound intermediates, composite carbon nanotube balls, and red phosphorus doping all involve liquid or molten phases, which is conducive to the uniform compounding of materials. Good wettability maintains the granularity and electrode morphology of the composite negative electrode. Even after a high charge and discharge depth and a long number of cycles, the electrode structure remains basically unchanged, avoiding the deposition of metallic lithium on the outer wall of the carbon skeleton, resulting in the formation of inactivated lithium agglomerates or dead lithium in the electrode;
[0053] Reduce costs: The process is simple and feasible, the cost is low, the safety is high, and there is a prospect of large-scale application;
[0054] Improve specific capacity: Li+ The deposition overpotential on tin is lower than that on carbon materials. Its lithium affinity helps to evenly immerse the molten metal lithium into the internal channels of the carbon tube balls during the stirring process, obtaining fuller and denser phosphorus-carbon composite microsphere particles, which increases the first charge specific capacity of the pretreated composite material by 30% or more.
[0055] Improved electrochemical stability: The dense filling of metallic lithium inside the composite material avoids the side reaction between metallic lithium and electrolyte, effectively improving the utilization rate of electrolyte and active lithium. The half-cell assembled by the phosphorus-carbon composite material has a high conductivity at 2.5 mA cm -2 It still maintains a low overpotential under high current density, and the capacity retention rate reaches 85% after 150 cycles, achieving a double breakthrough in the cycle life and capacity retention rate of phosphorus-carbon composite materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 Schematic diagram of the preparation of phosphorus-carbon composite negative electrode materials.
[0057] Figure 2 This is the optical image of carbon tube ball / red phosphorus / phosphorus-carbon composite material.
[0058] Figure 3 These are the SEM images of the CNT and P-CNT@SnS2 materials prepared in Example 1, where A is the SEM image of the CNT material and B is the SEM image of the P-CNT@SnS2 material.
[0059] Figure 4 This is the XRD diagram of the carbon tube / red phosphorus / phosphorus-carbon composite material prepared in Example 1 before and after being doped with SnS2.
[0060] Figure 5 This is a deposition potential bar graph of the carbon tube / doped SnS2 phosphorus-carbon composite material prepared in Example 1, wherein A is the SEM image of the carbon tube / doped SnS2 phosphorus-carbon composite material, and B is the potential bar graph of the carbon tube / doped SnS2 phosphorus-carbon composite material.
[0061] Figure 6 These are the first discharge curves of the red phosphorus / carbon tube and SnS2@red phosphorus / carbon tube materials prepared in Example 1.
[0062] Figure 7 The cycling performance diagram and potential-time curve of the CNT and SnS2@CNT materials prepared in Example 1 (attached figure).
[0063] Figure 8 is the DFT simulation of Li in Example 1 + Binding energy diagram with different substrates: (a) Li + and Sn substrate; (b) Li + With C base.
[0064] Fig. 9 These are the SEM images of CNT and P-CNT@Ni3S4 materials prepared in Example 2, where A is the SEM image of CNT material and B is the SEM image of P-CNT@Ni3S4 material.
[0065] Fig.10 These are the SEM images of CNT and P-CNT@CoSe2 materials prepared in Example 3, where A is the SEM image of CNT material and B is the SEM image of P-CNT@CoSe2 material.
[0066] Fig.11 These are the SEM images of the CNT and P-CNT@GeS2 materials prepared in Example 4, where A is the SEM image of the CNT material and B is the SEM image of the P-CNT@GeS2 material.
[0067] Fig.12 These are SEM images of CNT and P-CNT@TiP materials prepared in Example 5, where A is the SEM image of CNT material and B is the SEM image of P-CNT@TiP material. DETAILED DESCRIPTION
[0068] Explanation of terms
[0069] Phosphorus-based anode: It has a high theoretical specific capacity and good rate performance, with a theoretical lithium storage capacity of 2596mA·h·g -1 (Li3P) and has a higher safety reaction electrode potential (0.8V vs Li / Li + ), but its conductivity is poor, and the volume changes greatly during the lithium insertion and extraction process, with a volume expansion rate of up to 300%, resulting in the need to improve the material's cycle stability, which greatly limits its application in lithium-ion batteries.
[0070] Carbon-based anode: Typical commercial electrodes such as graphite have low cost, simple and mature preparation process, strong conductivity, low working voltage, good reversible charge and discharge performance, and strong safety, but have low specific capacity (372mA·h·g -1 ), low Coulombic efficiency and poor high-rate charge and discharge performance.
[0071] Phosphorus-carbon composite negative electrode: It is a composite material with carbon as the dispersed matrix and phosphorus as the active material, combining the composite advantages of phosphorus negative electrode and carbon negative electrode: it has good electrical conductivity, improves the conductivity of the negative electrode, alleviates the volume expansion problem of the electrode during the cycle, and thus improves the cycle stability. However, the internal structure of the composite negative electrode has large gaps and poor internal wettability to metallic lithium, which increases the contact area between active lithium and electrolyte to a certain extent, thereby inducing side reactions and reducing the initial coulomb efficiency.
[0072] Energy density: Refers to the amount of energy stored in a certain unit of space or mass. The energy density of a battery refers to the amount of electrical energy released per unit volume or unit mass of the battery.
[0073] Rate performance: Refers to storing or releasing a certain amount of energy in the battery at a certain speed. The premise of this storage and release process is controllable and safe, and will not significantly affect the battery life and other performance indicators. Generally, we call lithium batteries with 1.0C discharge as standard batteries, 2.0C-10C discharge as small rate batteries, and more than 10C as high rate batteries.
[0074] In the present invention, the diameter of the carbon nanotubes is preferably 2 nm to 50 nm, more preferably 5 nm to 40 nm, more preferably 10 nm to 30 nm, and most preferably 15 nm to 25 nm.
[0075] In the present invention, the length of the carbon nanotube is preferably 0.1 micron to 500 microns, more preferably 1 micron to 400 microns, more preferably 10 microns to 300 microns, more preferably 50 microns to 200 microns, and most preferably 100 microns to 150 microns. The present invention has no particular limitation on the source of the carbon nanotube, and carbon nanotubes well known to those skilled in the art can be used, which can be purchased from the market.
[0076] In the present invention, the carbon nanotubes are preferably carboxylated carbon nanotubes, aminated carbon nanotubes, hydroxylated carbon nanotubes, phosphorylated carbon nanotubes, and graphitized carbon nanotubes. The present invention has no particular restrictions on the source of the modified carbon nanotubes, and the modified carbon nanotubes well known to those skilled in the art can be used, such as commercially available carbon nanotubes with carboxyl groups (purchased by Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.). Carbon nanotubes can also be surface oxidized to obtain carboxylated carbon nanotubes. As in the present invention, the oxidant for the surface oxidation preferably includes sulfuric acid and nitric acid, more preferably a mixed solution of sulfuric acid and nitric acid.
[0077] The purpose of this patent is to protect a method for preparing a high-performance composite phosphorus-carbon negative electrode by using carbon nanotube balls doped with red phosphorus and internal low-melting-point transition metal compounds through low-temperature liquid phase immersion.
[0078] The preparation method of the composite phosphorus-carbon negative electrode material comprises the following steps:
[0079] (1) Preparation of a low melting point transition metal compound intermediate solution: dissolving a metal source and a non-metal source in a solvent in a certain proportion, and performing a solvent / hydrothermal reaction to obtain a low melting point transition metal compound intermediate solution;
[0080] (2) Preparation of composite carbon nanotube spheres: dispersing carbon nanotube spheres in the low melting point transition metal compound intermediate solution, performing solid-liquid separation after solvent / hydrothermal reaction, and drying the filter cake to obtain composite carbon nanotube sphere powder material;
[0081] (3) Preparation of red phosphorus dispersion: After ball milling, red phosphorus is subjected to hydrothermal treatment, and the dried solid matter is dispersed in a solvent to obtain a uniform red phosphorus dispersion;
[0082] (4) Preparation of composite phosphorus-carbon negative electrode material: ultrasonically disperse the composite carbon nanotube ball powder material in a solvent, add the red phosphorus dispersion, perform solvent / hydrothermal reaction after ultrasonic treatment, collect the solid matter after centrifugal washing, and freeze-dry to obtain a composite phosphorus-carbon negative electrode material.
[0083] The metal source in step (1) includes any one of fluorides, chlorides, nitrates, sulfates and carbonates of tin, titanium, cadmium, iron, cobalt, chromium, manganese and nickel.
[0084] The non-metallic source includes one of sulfide, selenide, telluride and phosphide; preferably, the sulfide includes at least one of sublimated sulfur, thioacetamide and thiourea, the selenide includes at least one of elemental selenium powder and sodium selenite, the telluride includes at least one of elemental tellurium powder and sodium tellurite, and the phosphide includes at least one of sodium hypophosphite, phosphoric acid, ammonium dihydrogen phosphate and diamine hydrogen phosphate.
[0085] The molar ratio of the non-metal source to the metal source is 1:1-3:1.
[0086] The solvent includes at least one of deionized water, anhydrous ethanol, anhydrous methanol and anhydrous ether.
[0087] The mass concentration of the low melting point transition metal compound intermediate is 0.2-3%.
[0088] During the preparation of the low melting point transition metal compound intermediate solution, the solvent / hydrothermal reaction temperature is 50-100° C., the reaction time is 5-50 mins, and magnetic stirring is used during the solvent / hydrothermal reaction at a rotation speed of 300-2000 rpm.
[0089] The precursor of the carbon nanotube ball is any one of carbon nanofiber, carbon nanotube, mesoporous carbon, porous carbon, common conductive agent carbon black and Super P;
[0090] The carbon nanotube spheres may also be materials with different particle sizes and skeleton structures obtained by surface modification through any one or more of amination, carboxylation, hydroxylation, phosphination, and graphitization.
[0091] The mass ratio of the carbon nanotube ball to the low melting point transition metal compound intermediate is 1:1-3:1.
[0092] In the preparation process of the composite carbon nanotube spheres in step (2), the solvent / hydrothermal reaction temperature is 40-90°C, the reaction time is 20-80 minutes, and solid-liquid separation is carried out by suction filtration and washing. The filter cake is placed in a vacuum drying oven at 50-60°C and dried overnight.
[0093] The red phosphorus precursor of step (3) is in the form of a powder of 60-100 meshes, or in the form of microsphere particles of 10-20 meshes;
[0094] During the red phosphorus ball milling process, red phosphorus and stainless steel balls are loaded into a stainless steel ball tank at a mass ratio of 1:10-1:50, and ball milled at a speed of 300-500rpm for 1-5h in a nitrogen atmosphere. During the hydrothermal treatment process, the hydrothermal reaction temperature is 150-200°C and the reaction time is 10-20h.
[0095] The mass concentration of the red phosphorus dispersion in step (4) is 10%-20%; the mass concentration of the composite carbon nanotube ball powder material in the solution is 10%-20%; the mass ratio of red phosphorus to the composite carbon nanotube ball powder material is 1:1-3:1.
[0096] In step (4), the solvent / hydrothermal reaction temperature is 150-500° C., and the reaction time is 20-60 minutes.
[0097] The present invention uses the prepared red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material as a negative electrode for a lithium ion battery.
[0098] The assembly steps of the high-capacity, high-rate lithium-ion battery are as follows: the phosphorus-carbon composite negative electrode material prepared above is mixed with a binder (PVDF) and acetylene black (AB) in a mass ratio of 8:1:1, mixed evenly in an NMP solvent, coated on a copper foil, and vacuum dried at 80°C to punch out a sheet as a working electrode, a metal lithium sheet as a counter electrode, and 1.0M LiTFSI in DOL:DME (V:V=1:1) + 1.0wt.% LiNO3 as an experimental electrolyte system to assemble a button cell (half cell) and perform a charge and discharge cycle test.
[0099] Example 1
[0100] 1.1 Preparation of SnS2 nanosheet intermediate solution: Dissolve tin tetrachloride and thioacetamide in a molar ratio of 1:1 in a high-purity ethanol solution, stir at 300 rpm to mix thoroughly, react at 60°C for 30 min to obtain a 2 wt.% SnS2 intermediate solution for standby use;
[0101] 1.2 Preparation of SnS2@CNT composite material: Soak carbon nanotubes (CNT diameter is 15nm~25nm, tube length is 100μm~150μm) in the above SnS2 intermediate solution at a mass fraction of 2%, and continue to heat to 60℃ at 300rpm, react for 40mins, and after the sample is cooled to room temperature, use high-purity ethanol to wash and filter the obtained sample several times. Finally, place the obtained sample in a vacuum oven at 50℃ and dry overnight to obtain SnS2@CNT composite carbon tube ball powder material;
[0102] 1.3 Preparation of carbon nanotube dispersion: Weigh the above SnS2@CNT composite carbon nanotube powder at a mass fraction of 2% and disperse it in a mixed solvent of ethanol / deionized water, and ultrasonically disperse it for 50 minutes to obtain a uniform composite carbon nanotube dispersion;
[0103] 1.4 Preparation of red phosphorus dispersion: red phosphorus was dispersed in deionized water for ball milling. The red phosphorus and stainless steel balls were loaded into a stainless steel ball tank at a mass ratio of 1:30. The mixture was ball milled at a speed of 300 rpm for 1 h under a nitrogen atmosphere and then transferred to a reactor. The mixture was hydrothermally treated at 200°C for 12 h. The product was placed in a vacuum drying oven at 50°C for overnight drying. The dried red phosphorus was dispersed in a mixed solvent of ethanol / deionized water at a mass fraction of 2%, and ultrasonically dispersed for 80 mins to obtain a uniform red phosphorus dispersion.
[0104] 1.5 Dispersion mixing reaction and purification: The above red phosphorus dispersion was added to the composite carbon nanotube dispersion ball at a red phosphorus / carbon nanotube mass ratio of 2:1 and ultrasonically dispersed for 50 minutes. The obtained mixed solution was charged into a reactor for hydrothermal reaction at a reaction temperature of 200°C for 60 minutes. After cooling to room temperature, the upper clear liquid was removed, and the solid phase material deposited in the lower layer was centrifuged and washed several times to obtain a composite phosphorus-carbon negative electrode material;
[0105] 1.6 Freeze drying of the composite phosphorus-carbon negative electrode material: The composite phosphorus-carbon negative electrode material obtained above was placed in a -80°C freeze dryer and freeze-dried to obtain a doped and modified phosphorus-carbon composite negative electrode material (P-CNT@SnS2);
[0106] 1.7 Assembly of high-capacity, high-rate lithium-ion batteries: The phosphorus-carbon composite negative electrode material prepared in the above process was mixed with a binder (PVDF) and acetylene black (AB) in a mass ratio of 8:1:1, mixed in NMP solvent to form a slurry, coated on a copper foil, and vacuum dried at 80°C to punch out a sheet as a working electrode, a metal lithium sheet as a counter electrode, and 1.0M LiTFSI in DOL:DME (V:V=1:1) + 1.0wt.% LiNO3 as the experimental electrolyte system to assemble a button cell (half-cell) and perform a charge and discharge cycle test;
[0107] 1.8 Figure 1 The schematic diagram of the preparation of the phosphorus-carbon composite negative electrode material is shown in FIG. A carbon tube ball (or a modified carbon tube ball, wherein the modified carbon tube ball is subjected to surface modification by any one or more of amination, carboxylation, hydroxylation, phosphorylation, and graphitization to obtain a material with different particle sizes and skeleton structures) is placed in a transition metal nano-doping solution to obtain a transition metal nano-sheet-doped carbon tube ball, which is then placed in a small-particle red phosphorus dispersion that has been ball-milled for a constant temperature water bath reaction to obtain a phosphorus-carbon composite negative electrode material.
[0108] 1.9 Figure 2 This is an optical image of the carbon tube ball / red phosphorus / phosphorus-carbon composite material. It can be seen that the carbon tube ball / red phosphorus / phosphorus-carbon composite material is uniformly dispersed in the solvent, and no agglomeration precipitation phenomenon is observed.
[0109] 1.10 Figure 3 The SEM images of CNT and P-CNT@SnS2 materials show that CNT presents a spherical structure formed by self-assembly of nanotubes, and on P-CNT@SnS2, it can be observed that carbon nanotube microspheres and small-sized red phosphorus are evenly mixed and co-coated.
[0110] 1.11 Figure 4 The XRD diagram of carbon tube / red phosphorus / phosphorus-carbon composite material before and after SnS2 doping. The carbon tube / red phosphorus carbon tube composite material before and after doping showed a typical carbon broad peak at 26.5°. At the same time, the XRD diagram of the red phosphorus carbon tube composite material before and after doping was compared. The doped material showed two characteristic peaks belonging to SnS2 at 28.5° and 51.1°, indicating that SnS2 was successfully doped into the carbon tube.
[0111] 1.12 Figure 5 The SEM image and potential bar graph of carbon nanotube / doped SnS2 phosphorus-carbon composite material. When the doping amount increases from 0% to 10%, the uneven surface formed by the carbon nanotube gradually becomes smooth. When the doping amount increases to 15%, the surface becomes rough again. At the same time, it can be observed that the size of the carbon nanotube becomes larger, which may be due to the change in the internal structure of the carbon nanotube caused by the excessive doping amount. From the potential bar graph, it can be seen that the potential of the SnS2 intermediate doped electrode material has decreased to varying degrees, and when the doping amount is 10%, the potential is the lowest (65mV), indicating that there is a potential difference of about 0.3V between the lithium-tin alloy and the metallic lithium, so that the carbon nanotube doped SnS2 has excellent lithium affinity, which is conducive to uniformly immersing the molten metal lithium into the internal channel of the carbon nanotube during the stirring process, and obtaining fuller and denser phosphorus-carbon composite microsphere particles, with better specific capacity and rate performance, while avoiding the side reaction between the metallic lithium and the electrolyte, effectively improving the utilization rate of the electrolyte and active lithium.
[0112] 1.13 Figure 6The first discharge curves of red phosphorus / carbon tube and SnS2@red phosphorus / carbon tube materials. The first discharge capacity of the doped phosphorus-carbon negative electrode material is 1000 mA·h·g -1 Compared with the discharge capacity before doping (1300mA·h·g -1 ) significantly improved.
[0113] 1.14 Figure 7 The cycling performance diagram and potential-time curve of CNT and SnS2@CNT materials (attached picture). -2 Under high current density, the coulombic efficiency of SnS2@CNT was basically maintained at 99.6% after 200 cycles, while the coulombic efficiency of CNT showed obvious fluctuations after 100 cycles, indicating that the SnS2@CNT material has better cycle stability; and the potential-time diagram also shows that compared with CNT (-150mV), SnS2@CNT has a relatively high potential (-71mV), and is less likely to have side reactions with liquid electrolytes, which can ensure less electrolyte consumption and longer cycle life.
[0114] 1.15 Figure 8 Simulating Li for DFT + Binding energy diagrams with different substrates show that Li + It has a lower binding energy (-1.12eV) with the SnS2-doped three-dimensional conductive carbon substrate, indicating that it has better lithium affinity.
[0115] Example 2
[0116] 2.1 Preparation of Ni3S4 nanosheet intermediate solution: nickel nitrate hexahydrate and thiourea in a molar ratio of 1:2 were dissolved in anhydrous methanol solution, and stirred at a speed of 500 rpm to mix thoroughly. After reacting at 80°C for 20 minutes, a 1wt.% Ni3S4 intermediate solution was obtained for standby use. With the introduction of Ni3S4 nanosheet intermediates, the generation of by-product white phosphorus can be effectively reduced, and the safety of the preparation process can be improved;
[0117] 2.2 Preparation of Ni3S4@CNT composite material: Place carbon nanotubes (CNT diameter is 15nm~25nm, tube length is 100μm~150μm) in a concentrated H2SO4 and concentrated HNO3 solution with a volume ratio of 3:1, reflux at 80 degrees for 12 hours, wash the product to neutrality and then dry it, remove impurities on the surface of carbon nanotubes with carboxyl and hydroxyl groups, which are easier to disperse in the solvent and are also conducive to the composite with Ni3S4 intermediates and red phosphorus particles. Take the modified carbon tube ball and immerse it in the Ni3S4 intermediate solution with a mass fraction of 1%, and continue to heat to 80℃ at a speed of 500rpm, react for 40mins, wait for the sample to cool to room temperature, wash and filter it several times to collect the obtained sample. Finally, place the obtained sample in a vacuum oven at 50℃ and dry it overnight to obtain Ni3S4@CNT composite carbon tube ball powder material;
[0118] 2.3 Preparation of carbon nanotube dispersion: Disperse the above Ni3S4@CNT composite carbon nanotube powder in anhydrous methanol at a mass fraction of 1%, and perform ultrasonic dispersion for 30 minutes to obtain a uniform composite carbon nanotube dispersion;
[0119] 2.4 Preparation of red phosphorus dispersion: Red phosphorus was dispersed in deionized water and ball-milled. Red phosphorus and stainless steel balls were loaded into a stainless steel ball tank at a mass ratio of 1:20. After ball-milling at 300 rpm for 2 h under a nitrogen atmosphere, the mixture was transferred to a reactor. After hydrothermal treatment at 150 °C for 20 h, the mixture was placed in a vacuum drying oven at 50 °C for overnight drying. The dried red phosphorus was dispersed in anhydrous methanol and ultrasonically dispersed for 60 mins to obtain a uniform 1 wt.% red phosphorus dispersion.
[0120] 2.5 Dispersion mixing reaction and purification: The above red phosphorus dispersion was added to the composite carbon nanotube dispersion ball at a red phosphorus / carbon nanotube mass ratio of 3:1 and ultrasonically dispersed for 30 minutes. The obtained mixed solution was charged into a reactor for hydrothermal reaction at a reaction temperature of 150°C for 50 minutes. After cooling to room temperature, the upper clear liquid was removed, and the solid phase material deposited in the lower layer was centrifuged and washed several times to obtain a doped and modified phosphorus-carbon composite negative electrode material (P-CNT@Ni3S4);
[0121] 2.6 Freeze drying of the composite phosphorus-carbon negative electrode material: The composite phosphorus-carbon negative electrode material obtained above was placed in a -80°C freeze dryer for freeze drying to obtain a red phosphorus / carbon nanotube composite material;
[0122] 2.7 Assembly of high-capacity, high-rate lithium-ion batteries: The phosphorus-carbon composite negative electrode material prepared in the above process was mixed with a binder (PVDF) and acetylene black (AB) in a mass ratio of 8:1:1, mixed in NMP solvent to form a slurry, coated on a copper foil, and vacuum dried at 80°C to punch out a sheet as a working electrode, a metal lithium sheet as a counter electrode, and 1.0M LiTFSI in DOL:DME (V:V=1:1) + 1.0wt.% LiNO3 as the experimental electrolyte system to assemble a button cell (half-cell) and perform a charge and discharge cycle test;
[0123] 2.8 Fig. 9 The SEM images of CNT and P-CNT@Ni3S4 materials. In the SEM image of P-CNT@Ni3S4 material, it can be observed that the carbon nanotube microspheres are fully mixed with red phosphorus, which increases the conductivity of the red phosphorus material and inhibits the volume expansion during the charge and discharge process.
[0124] Example 3
[0125] 3.1 Preparation of CoSe2 nanosheet intermediate solution: Cobalt chloride and selenium powder in a molar ratio of 1:2 were dissolved in anhydrous ethanol solution, and stirred at 400 rpm to mix well. After reacting at 60°C for 50 min, a 0.5 wt.% CoSe2 intermediate solution was obtained for standby use;
[0126] 3.2 Preparation of CoSe2@CNT composite material: Disperse carbon nanotubes (CNT diameter is 15nm~25nm, tube length is 100μm~150μm) in a methanol solvent containing methylphosphoric acid, stir magnetically for 60mins to mix evenly, then place in an oil bath at 110℃ and continue stirring until the methanol is completely volatilized. The phosphorus-containing groups are modified on the surface of the carbon tubes by high-temperature reduction and oxidation. The chemical adsorption and catalytic effects are beneficial to improve the electrochemical properties of the material. The carbon tubes modified with phosphorus-containing groups are immersed in the above-mentioned CoSe2 intermediate solution at a mass fraction of 0.5%, and continuously heated to 50℃ at a speed of 400rpm. The reaction is carried out for 80mins. After the sample is cooled to room temperature, it is washed and filtered several times to collect the obtained sample. Finally, the obtained sample is placed in a vacuum oven at 50℃ and dried overnight to obtain CoSe2@CNT composite carbon tube powder material;
[0127] 3.3 Preparation of carbon nanotube dispersion: Disperse the above-mentioned CoSe2@CNT composite carbon nanotube powder in anhydrous ethanol, and ultrasonically disperse for 40 minutes to obtain a uniform 0.5wt.% composite carbon nanotube dispersion;
[0128] 3.4 Preparation of red phosphorus dispersion: Red phosphorus was dispersed in deionized water and ball-milled. Red phosphorus and stainless steel balls were loaded into a stainless steel ball tank at a mass ratio of 1:40. After ball-milling at 400 rpm for 4 h under a nitrogen atmosphere, the mixture was transferred to a reactor. After hydrothermal treatment at 170°C for 16 h, the mixture was placed in a vacuum drying oven at 50°C for overnight drying. The dried red phosphorus was dispersed in anhydrous ethanol and ultrasonically dispersed for 80 mins to obtain a uniform 0.5 wt.% red phosphorus dispersion.
[0129] 3.5 Dispersion mixing reaction and purification: The above red phosphorus dispersion was added to the composite carbon nanotube dispersion ball at a red phosphorus / carbon nanotube mass ratio of 3:1 and ultrasonically dispersed for 40 minutes. The obtained mixed solution was charged into a reactor for hydrothermal reaction at a reaction temperature of 180°C for 40 minutes. After cooling to room temperature, the upper clear liquid was removed, and the solid phase material deposited in the lower layer was centrifuged and washed several times to obtain a doped and modified phosphorus-carbon composite negative electrode material (P-CNT@CoSe2);
[0130] 3.6 Freeze drying of the composite phosphorus-carbon negative electrode material: The composite phosphorus-carbon negative electrode material obtained above was placed in a -80°C freeze dryer and freeze-dried to obtain a red phosphorus / carbon nanotube composite material;
[0131] 3.7 Assembly of high-capacity and high-rate lithium-ion batteries: The phosphorus-carbon composite negative electrode material prepared in the above process was mixed with a binder (PVDF) and acetylene black (AB) in a mass ratio of 8:1:1, mixed evenly in an NMP solvent, coated on a copper foil, and vacuum dried at 80°C. The punched sheets were used as working electrodes, and the metal lithium sheets were used as counter electrodes. 1.0M LiTFSI in DOL:DME (V:V=1:1) + 1.0wt.% LiNO3 was used as the experimental electrolyte system to assemble button cells (half cells) and perform charge and discharge cycle tests.
[0132] 3.8 Fig.10 The SEM images of CNT and P-CNT@CoSe2 materials show that after the phosphorus-carbon composite material is formed, carbon tubes are attached to the surface of the red phosphorus material, and small-sized red phosphorus is attached to the inside of the carbon tubes.
[0133] Example 4
[0134] 4.1 Preparation of GeS2 nanosheet intermediate solution: dissolve germanium fluoride and thioacetamide in anhydrous ether solution at a molar ratio of 1:3, stir at 1000 rpm to mix well, react at 100°C for 40 min to obtain a 1 wt.% GeS2 solution for standby use;
[0135] 4.2 Preparation of GeS2@CNT composite materials: Carbon nanotubes (CNT diameter is 15nm~25nm, tube length is 100μm~150μm) are placed in a tubular furnace and calcined at 600℃ for 4h under an inert atmosphere to enhance the graphitization strength of the carbon nanotubes. The three-dimensional skeleton structure of the carbon nanotubes is used to effectively inhibit the volume expansion of the phosphorus-based materials during the charge and discharge cycle. The calcined carbon nanotubes are then immersed in a GeS2 intermediate solution at a mass fraction of 1%, and continuously heated to 90℃ at a speed of 1000rpm for reaction for 60mins. After the sample is cooled to room temperature, it is washed and filtered several times to collect the obtained sample. Finally, the obtained sample was placed in a vacuum oven at 50°C and dried overnight to obtain GeS2@CNT composite carbon tube ball powder material; 4.3 Preparation of carbon nanotube ball dispersion: The above GeS2@CNT composite carbon tube ball powder was dispersed in anhydrous ether and ultrasonically dispersed for 80 minutes to obtain a uniform 1wt.% composite carbon nanotube ball dispersion;
[0136] 4.4 Preparation of red phosphorus dispersion: ball-mill red phosphorus in deionized water, load red phosphorus and stainless steel balls into a stainless steel ball tank at a mass ratio of 1:30, ball-mill at 350 rpm for 5 h under nitrogen atmosphere, transfer to a reactor, hydrothermally treat at 180 °C for 10 h, place in a 50 °C vacuum drying oven for overnight drying, disperse the dried red phosphorus in anhydrous ether at a mass fraction of 1%, and ultrasonically disperse for 40 mins to obtain a uniform red phosphorus dispersion;
[0137] 4.5 Dispersion mixing reaction and purification: The above red phosphorus dispersion was added to the composite carbon nanotube dispersion ball at a red phosphorus / carbon nanotube mass ratio of 2:1, and ultrasonic dispersion was continued for 45 minutes. The obtained mixed solution was charged into a reactor for hydrothermal reaction at a reaction temperature of 300°C for 30 minutes. After cooling to room temperature, the upper clear liquid was removed, and the solid phase material deposited in the lower layer was centrifuged and washed several times to obtain a composite phosphorus-carbon negative electrode material;
[0138] 4.6 Freeze drying of the composite phosphorus-carbon negative electrode material: The composite phosphorus-carbon negative electrode material obtained above was placed in a -80°C freeze dryer and freeze-dried to obtain a doped and modified phosphorus-carbon composite negative electrode material (P-CNT@GeS2);
[0139] 4.7 Assembly of high-capacity, high-rate lithium-ion batteries: The phosphorus-carbon composite negative electrode material prepared in the above process was mixed with a binder (PVDF) and acetylene black (AB) in a mass ratio of 8:1:1, mixed in NMP solvent to form a slurry, coated on a copper foil, and vacuum dried at 80°C to punch out a sheet as a working electrode, a metal lithium sheet as a counter electrode, and 1.0M LiTFSI in DOL:DME (V:V=1:1) + 1.0wt.% LiNO3 as the experimental electrolyte system to assemble a button cell (half-cell) and perform a charge and discharge cycle test;
[0140] 4.8 Fig.11 SEM images of CNT and P-CNT@GeS2 materials.
[0141] Example 5
[0142] 5.1 Preparation of TiP nanosheet intermediate solution: titanium sulfate and sodium hypophosphite in a molar ratio of 1:1 were dissolved in anhydrous ether solution, stirred at 1500 rpm to mix thoroughly, and reacted at 70°C for 20 min to obtain a 2 wt.% TiP intermediate solution for standby use;
[0143] 5.2 Preparation of TiP@CNT composite materials: Place carbon nanotubes (CNT diameter is 15nm~25nm, tube length is 100μm~150μm) in a tubular furnace and bake at 800℃ for 2h under an inert atmosphere to enhance the graphitization strength of the carbon tubes. Then, immerse the baked carbon tubes in a TiP intermediate solution at a mass fraction of 2%, and continue to heat to 70℃ at a speed of 1500rpm. React for 50mins. After the sample is cooled to room temperature, wash and filter the obtained sample several times. Finally, place the obtained sample in a vacuum oven at 50℃ and dry overnight to obtain a TiP@CNT composite carbon tube powder material;
[0144] 5.3 Preparation of carbon nanotube dispersion: The TiP@CNT composite carbon nanotube powder was dispersed in anhydrous ether at a mass fraction of 2%, and ultrasonically dispersed for 90 minutes to obtain a uniform composite carbon nanotube dispersion;
[0145] 5.4 Preparation of red phosphorus dispersion: red phosphorus was dispersed in deionized water and ball-milled. The red phosphorus and stainless steel balls were loaded into a stainless steel ball tank at a mass ratio of 1:30. The mixture was ball-milled at 400 rpm for 2 h under a nitrogen atmosphere and then transferred to a reactor. After hydrothermal treatment at 180 °C for 15 h, the mixture was placed in a vacuum drying oven at 50 °C for overnight drying. The dried red phosphorus was dispersed in anhydrous ether at a mass fraction of 2%, and ultrasonically dispersed for 40 mins to obtain a uniform red phosphorus dispersion.
[0146] 5.5 Dispersion mixing reaction and purification: The above red phosphorus dispersion was added to the composite carbon nanotube dispersion ball at a red phosphorus / carbon nanotube mass ratio of 1:1, and ultrasonic dispersion was continued for 30 minutes. The obtained mixed solution was charged into a reactor for hydrothermal reaction at a reaction temperature of 150°C and a reaction time of 40 minutes. After cooling to room temperature, the upper clear liquid was removed, and the solid phase material deposited in the lower layer was centrifuged and washed several times to obtain a doped and modified phosphorus-carbon composite negative electrode material (P-CNT@TiP);
[0147] 5.6 Freeze drying of the composite phosphorus-carbon negative electrode material: The composite phosphorus-carbon negative electrode material obtained above was placed in a -80°C freeze dryer for freeze drying to obtain a red phosphorus / carbon nanotube composite material;
[0148] 5.7 Assembly of high-capacity, high-rate lithium-ion batteries: The phosphorus-carbon composite negative electrode material prepared in the above process was mixed with a binder (PVDF) and acetylene black (AB) in a mass ratio of 8:1:1, mixed in NMP solvent to form a slurry, coated on a copper foil, and vacuum dried at 80°C to punch out a sheet as a working electrode, a metal lithium sheet as a counter electrode, and 1.0M LiTFSI in DOL:DME (V:V=1:1) + 1.0wt.% LiNO3 as the experimental electrolyte system to assemble a button cell (half-cell) and perform a charge-discharge cycle test;
[0149] 5.8 Fig.12 SEM images of CNT and P-CNT@TiP materials.
[0150] Example 6
[0151] The implementation steps are the same as those in Example 1, except that the non-metallic source is sodium tellurite, 2 wt.% SnTe2 is obtained in step 6.1, and the other steps are the same as those in Example 1 to obtain a doped and modified phosphorus-carbon composite negative electrode material (P-CNT@SnTe2).
[0152] Example 7
[0153] The implementation steps are the same as those in Example 1, except that the non-metal source is sodium selenite and the metal source is nickel nitrate hexahydrate. 2 wt.% NiSe is obtained in step 6.1. The other steps are the same as those in Example 1 to obtain a doped and modified phosphorus-carbon composite negative electrode material (P-CNT@NiSe).
[0154] Example 8
[0155] The implementation steps are the same as those in Example 1, and the carbon nanotubes (CNTs) are surface modified by amino to obtain amino-modified carbon nanotubes / red phosphorus / phosphorus-carbon composite materials NH3-P-CNT@SnS2.
[0156] Example 9
[0157] The implementation steps are the same as those in Example 1, and the carbon nanotube ball is surface-modified by carboxylation to obtain a graphitized modified carbon nanotube ball / red phosphorus / phosphorus-carbon composite material COOH-P-CNT@SnS2.
[0158] Example 10
[0159] The implementation steps are the same as those in Example 1, and the carbon nanotube ball is subjected to phosphorus-based surface modification to obtain a phosphorus-based modified carbon nanotube ball / red phosphorus / phosphorus-carbon composite material PP-CNT@SnS2.
[0160] The cycle stability of the materials prepared in each embodiment and comparative example was determined by testing the capacity retention rate after 150 cycles. + The lower deposition overpotential on titanium makes it easier for lithium to penetrate into the carbon tubes, forming denser and fuller phosphorus-carbon composite microspheres, improving the utilization of lithium during the first charge and discharge process, and thus improving the specific capacity and cycle performance of the phosphorus-carbon composite electrode, as shown in Table 1:
[0161] Table 1 Cyclic stability of materials prepared in various embodiments and comparative examples
[0162]
[0163]
[0164] Example 11 refers to the phosphorus-carbon negative electrode in Example 1 that is not modified with SnS2.
[0165] Example 12 refers to the phosphorus-carbon negative electrode of SnS2 in Example 8 that has not been modified by SnS2.
[0166] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material, characterized in that: The invention comprises red phosphorus and a composite carbon nanotube ball, wherein the composite carbon nanotube ball is doped and embedded with a low-melting-point transition metal compound, wherein the low-melting-point transition metal compound is obtained by reacting a metal source of tin, titanium, cadmium, iron, cobalt, chromium, manganese, germanium, or nickel with a non-metal source, wherein the metal source comprises fluoride, chloride, nitrate, sulfate, or carbonate of tin, titanium, cadmium, iron, cobalt, chromium, manganese, germanium, or nickel; and the non-metal source comprises any one or more of sulfide, selenide, telluride, or phosphide. The preparation method of the low-melting-point transition metal compound comprises dissolving the metal source and the non-metal source in a solvent, and obtaining the low-melting-point transition metal compound after solvent / hydrothermal reaction.
2. The red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 1, characterized in that: The mass ratio of red phosphorus to the composite carbon nanotube ball is 1:1-3:
1.
3. The red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 2, characterized in that: The product is obtained by mixing red phosphorus and composite carbon nanotube balls in a solvent and subjecting the mixture to a thermal reaction. The mass concentration of the composite carbon nanotube balls in the solvent is 10%-20%.
4. The red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 3, characterized in that: The solvent in the thermal reaction process includes at least one of deionized water, anhydrous ethanol, anhydrous methanol and anhydrous ether.
5. The red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 4, characterized in that: The melting point of the low-melting-point transition metal compound doped and embedded inside the composite carbon nanotube ball is ≤200°C.
6. The red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 1, characterized in that: The molar ratio of the non-metal source to the metal source is 1:1-3:
1.
7. The red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 6, characterized in that: The sulfide includes at least one of thioacetamide and thiourea; The selenide includes sodium selenite; The telluride comprises sodium tellurite; The phosphide includes at least one of sodium hypophosphite, phosphoric acid, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate.
8. The red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 7, characterized in that: The sulfide is replaced by sublimated sulfur; The selenide is replaced by elemental selenium powder; The telluride is replaced by elemental tellurium powder.
9. The red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 5, characterized in that: The carbon nanotube spheres are materials with different particle sizes and skeleton structures obtained by surface modification through any one or more of amination, carboxylation, hydroxylation, phosphination, and graphitization.
10. A method for preparing a phosphorus-carbon composite negative electrode material doped with carbon nanotubes based on red phosphorus, characterized in that: The following steps are involved: (1) Preparation of a low melting point transition metal compound intermediate solution: dissolving a metal source and a non-metal source in a solvent, and performing a solvent / hydrothermal reaction to obtain a low melting point transition metal compound intermediate solution; the low melting point transition metal compound comprises a metal source of tin, titanium, cadmium, iron, cobalt, chromium, manganese, germanium, or nickel and a non-metal source; the metal source comprises a fluoride, chloride, nitrate, sulfate, or carbonate of tin, titanium, cadmium, iron, cobalt, chromium, manganese, germanium, or nickel; the non-metal source comprises any one or more of a sulfide, a selenide, a telluride, and a phosphide; (2) Preparation of composite carbon nanotube spheres: dispersing carbon nanotube spheres in the low melting point transition metal compound intermediate solution, performing solid-liquid separation after solvent / hydrothermal reaction, and drying the filter cake to obtain composite carbon nanotube sphere powder material; (3) Preparation of red phosphorus dispersion: After ball milling, the red phosphorus is subjected to hydrothermal treatment, and the dried solid matter is dispersed in a solvent to obtain a uniform red phosphorus dispersion; (4) Preparation of composite phosphorus-carbon negative electrode material: ultrasonically disperse the composite carbon nanotube ball powder material in a solvent, add the red phosphorus dispersion, perform solvent / hydrothermal reaction after ultrasonic treatment, collect the solid matter after centrifugal washing and freeze-drying to obtain a composite phosphorus-carbon negative electrode material.
11. The method for preparing a red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 10, characterized in that: The sulfide includes at least one of thioacetamide and thiourea; The selenide includes sodium selenite; The telluride comprises sodium tellurite; The phosphide includes at least one of sodium hypophosphite, phosphoric acid, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate.
12. The method for preparing a red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 11, characterized in that: The sulfide is replaced by sublimated sulfur; The selenide is replaced by elemental selenium powder; The telluride is replaced by elemental tellurium powder.
13. The method for preparing a red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 11 or 12, characterized in that: The molar ratio of the non-metal source to the metal source is 1:1-3:
1.
14. The method for preparing a red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 13, characterized in that: The solvent includes at least one of deionized water, anhydrous ethanol, anhydrous methanol and anhydrous ether.
15. The method for preparing a red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 14, characterized in that: During the preparation of the low melting point transition metal compound intermediate solution, the solvent / hydrothermal reaction temperature is 50-100° C., the reaction time is 5-50 mins, and the solvent / hydrothermal reaction is performed with magnetic stirring at a rotation speed of 300-2000 rpm.
16. The method for preparing a red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 15, characterized in that: The precursor of the carbon nanotube ball is carbon nanotube; The carbon nanotube spheres are materials with different particle sizes and skeleton structures obtained by surface modification through any one or more of amination, carboxylation, hydroxylation, phosphination, and graphitization.
17. The method for preparing a red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 16, characterized in that: The mass ratio of the carbon nanotube ball to the low melting point transition metal compound intermediate is 1:1-3:
1.
18. The method for preparing a red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 10, characterized in that: In the preparation process of the composite carbon nanotube spheres in step (2), the solvent / hydrothermal reaction temperature is 40-90°C, the reaction time is 20-80 mins, and solid-liquid separation is carried out by suction filtration and washing. The filter cake obtained is placed in a vacuum drying oven at 50-60°C and dried overnight.
19. The method for preparing a red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 18, characterized in that: The red phosphorus precursor of step (3) is in the form of a powder of 60-100 meshes, or in the form of microsphere particles of 10-20 meshes; During the ball milling of red phosphorus, red phosphorus and stainless steel balls are loaded into a stainless steel ball tank at a mass ratio of 1:10-1:50, and ball milled at a speed of 300-500 rpm for 1-5 h in a nitrogen atmosphere. During the hydrothermal treatment, the hydrothermal reaction temperature is 150-200°C and the reaction time is 10-20 h.
20. The method for preparing a red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 10, characterized in that: In step (4), the mass concentration of the red phosphorus dispersion is 10%-20%; the mass concentration of the composite carbon nanotube ball powder material in the solvent is 10%-20%; and the mass ratio of red phosphorus to the composite carbon nanotube ball powder material is 1:1-3:
1.
21. The method for preparing a red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material according to claim 20, characterized in that: In step (4), the solvent / hydrothermal reaction temperature is 150-500°C and the reaction time is 20-60 mins.
22. Use of the red phosphorus-based carbon nanotube-doped phosphorus-carbon composite negative electrode material prepared by the preparation method according to any one of claims 10 to 21 as a negative electrode for a lithium-ion battery.
Citation Information
Patent Citations
Large-spacing MXene / red phosphorus anode material as well as preparation method and application thereof
CN111769271A
Tin phosphide and carbon composite negative electrode active precursor material of lithium-sulfur battery, negative electrode active material, negative electrode and preparation thereof
CN114122386A
Novel carbon nanotubes and production method therefor
CN103201215A
Preparation method for anode material of red phosphorous cladding carbon nano tube composite ion battery
CN105098154A
Composite cathode material for sodium battery and preparation method of composite cathode material
CN105514356A
Cited By
Low-cost and green phosphorus coal composite negative electrode material and preparation method thereof
CN121085254A