Vinyl chloride resin composition for powder molding, vinyl chloride resin molded body for powder molding, and laminate
A vinyl chloride resin composition with a plasticizer and polyglycerin fatty acid ester addresses odor issues in molded bodies, enhancing their suitability for automobile interiors by reducing odor and improving tensile properties.
Patent Information
- Application Number
- JP2020034155
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-02-28
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-02-28
AI Technical Summary
Vinyl chloride resin molded bodies used in automobile interiors emit odors that cause discomfort to occupants, necessitating the development of a composition that suppresses odor generation.
A vinyl chloride resin composition for powder molding containing a vinyl chloride resin, a plasticizer, and a polyglycerin fatty acid ester, formulated to minimize odor generation and enhance low-temperature tensile elongation.
The composition effectively reduces odor emission and improves low-temperature tensile elongation in molded articles, making them suitable for automobile interior materials.
Smart Images

Figure 0007567173000001 
Figure 0007567173000002 
Figure 0007567173000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a vinyl chloride resin composition for powder molding, a vinyl chloride resin molded article, and a laminate. [Background technology]
[0002] Polyvinyl chloride resins are generally used in a variety of applications due to their excellent properties such as cold resistance, heat resistance, and oil resistance. Specifically, for example, automobile interior parts such as automobile instrument panels and door trims are formed using automobile interior materials such as a skin made of a polyvinyl chloride resin molded product and a laminate in which a skin made of a polyvinyl chloride resin molded product is backed with a foam such as polyurethane foam.
[0003] Polyvinyl chloride resin molded articles constituting the skin of automobile interior parts such as automobile instrument panels are produced, for example, by powder molding a vinyl chloride resin composition containing vinyl chloride resin, a plasticizer, and additives such as pigments using a known molding method such as powder slush molding (see, for example, Patent Document 1).
[0004] Specifically, for example, in Patent Document 1, a vinyl chloride resin composition containing vinyl chloride resin particles, a trimellitic acid ester plasticizer, and additives such as a pigment made of a mixture of phthalocyanine blue, titanium oxide, and carbon is powder slush molded to produce a skin made of a vinyl chloride resin molded body. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 8-291243 Summary of the Invention [Problem to be solved by the invention]
[0006] When a vinyl chloride resin molded article is used as an automobile interior material such as the skin of an automobile interior part, the vinyl chloride resin molded article generates an odor, which may cause discomfort to automobile occupants. Therefore, there is a need to suppress the generation of odor from the vinyl chloride resin molded article.
[0007] Therefore, an object of the present invention is to provide a vinyl chloride resin composition for powder molding which is capable of forming vinyl chloride resin molded articles with suppressed odor generation. Another object of the present invention is to provide a vinyl chloride resin molded article that is suppressed in generating odor. A further object of the present invention is to provide a laminate which includes the vinyl chloride resin molded article and which is suppressed in generating odor. [Means for solving the problem]
[0008] The present inventors have conducted extensive research with the aim of solving the above problems, and have found that a vinyl chloride resin composition containing a vinyl chloride resin, a plasticizer, and a polyglycerol fatty acid ester can be powder molded to obtain a vinyl chloride resin molded article that suppresses odor generation, thereby completing the present invention.
[0009] That is, the present invention aims to advantageously solve the above problems, and the vinyl chloride resin composition for powder molding of the present invention is characterized by containing a vinyl chloride resin, a plasticizer, and a polyglycerin fatty acid ester. In this way, by using the vinyl chloride resin composition for powder molding containing a vinyl chloride resin, a plasticizer, and a polyglycerin fatty acid ester, it is possible to form a vinyl chloride resin molded body in which odor generation is suppressed.
[0010] Here, in the vinyl chloride resin composition for powder molding of the present invention, the polyglycerol fatty acid ester is represented by the following formula (I): [ka] [In formula (I), n represents an integer between 2 and 20, R represents hydrogen or a fatty acid residue; At least one of the R's represents a fatty acid residue; The multiple R's may be the same or different. When the polyglycerol fatty acid ester is represented by formula (I) in which the number of repeats n of structural units derived from glycerol falls within the above-mentioned range, odor generation from the vinyl chloride resin molded article formed can be further suppressed, and the low-temperature tensile elongation of the vinyl chloride resin molded article after heating can be increased.
[0011] In addition, in the vinyl chloride resin composition for powder molding of the present invention, the number of fatty acid residues among the plurality of R is preferably n+1 or less. If the number of fatty acid residues among the plurality of R is the above-mentioned predetermined value or less, the emission of odor from the vinyl chloride resin molded article formed can be further suppressed, and the low-temperature tensile elongation after heating of the vinyl chloride resin molded article can be increased.
[0012] Furthermore, in the vinyl chloride resin composition for powder molding of the present invention, the number of carbon atoms in the fatty acid residue is preferably from 2 to 30. When the number of carbon atoms in the fatty acid residue is within the above-mentioned range, odor generation from the vinyl chloride resin molded article formed can be further suppressed, and the low-temperature tensile elongation after heating of the vinyl chloride resin molded article can be increased.
[0013] In the vinyl chloride resin composition for powder molding of the present invention, it is preferable that at least one of the plurality of R represents a saturated fatty acid residue. When at least one of the plurality of R represents a saturated fatty acid residue, the low-temperature tensile elongation after heating of the resulting vinyl chloride resin molding can be increased.
[0014] Furthermore, in the vinyl chloride resin composition for powder molding of the present invention, the content of the polyglycerol fatty acid ester is preferably 0.1 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the vinyl chloride resin. If the content of the polyglycerol fatty acid ester is within the above-mentioned range, the generation of odor from the vinyl chloride resin molded article formed can be further suppressed, and the low-temperature tensile elongation of the vinyl chloride resin molded article after heating can be increased.
[0015] In addition, the vinyl chloride resin composition for powder molding of the present invention preferably contains the plasticizer in an amount of 30 parts by mass or more per 100 parts by mass of the vinyl chloride resin. If the plasticizer content in the vinyl chloride resin composition for powder molding is equal to or more than the above-mentioned predetermined value, the low-temperature tensile elongation after heating of the resulting vinyl chloride resin molded article can be increased.
[0016] Furthermore, in the vinyl chloride resin composition for powder molding of the present invention, it is preferable that the plasticizer contains at least one of a trimellitate ester and a polyester, and the total content of the trimellitate ester and the polyester is 30 parts by mass or more and 200 parts by mass or less per 100 parts by mass of the vinyl chloride resin. When the vinyl chloride resin composition for powder molding contains the trimellitate ester and / or polyester in the above-mentioned predetermined amount in total, the low-temperature tensile elongation after heating of the formed vinyl chloride resin molded article can be increased.
[0017] In addition, in the vinyl chloride resin composition for powder molding of the present invention, it is preferable that the plasticizer contains a trimellitate ester and a polyester, and the mass ratio of the trimellitate ester to the polyester (trimellitate ester / polyester) is 1 / 9 or more and 9 / 1 or less. If the plasticizer contains the trimellitate ester and the polyester in the above-mentioned predetermined mass ratio, the generation of odor from the vinyl chloride resin molded article formed can be further suppressed.
[0018] The vinyl chloride resin composition for powder molding of the present invention is preferably used for powder slush molding. By using the vinyl chloride resin composition for powder molding for powder slush molding, it is possible to more easily obtain a vinyl chloride resin molded article that can be favorably used as an automobile interior material such as the skin for an automobile instrument panel.
[0019] Furthermore, the present invention has an object to advantageously solve the above problems, and the vinyl chloride resin molded article of the present invention is characterized in that it is obtained by molding any one of the vinyl chloride resin compositions for powder molding described above. In this way, the vinyl chloride resin molded article obtained by molding the vinyl chloride resin composition for powder molding described above is suppressed in generating odors.
[0020] The vinyl chloride resin molded article of the present invention is preferably used for the surface of an automobile instrument panel. The vinyl chloride resin molded article of the present invention can be suitably used as the surface of an automobile instrument panel in which odor generation is suppressed.
[0021] Furthermore, the present invention has an object to advantageously solve the above problems, and the laminate of the present invention is characterized by having a polyurethane foam molded product and any one of the vinyl chloride resin molded products described above. The laminate having the polyurethane foam molded product and the vinyl chloride resin molded product described above is suppressed in the generation of odor.
[0022] The laminate of the present invention is preferably used for an automobile instrument panel. In this manner, by using the laminate of the present invention in an automobile instrument panel, it is possible to produce an automobile instrument panel in which odor generation from the surface layer is suppressed. Effect of the Invention
[0023] According to the present invention, it is possible to provide a vinyl chloride resin composition for powder molding which is capable of forming vinyl chloride resin molded articles with suppressed odor generation. Moreover, according to the present invention, it is possible to provide a vinyl chloride resin molded article in which odor generation is suppressed. Furthermore, according to the present invention, it is possible to provide a laminate which includes the vinyl chloride resin molded article and which is suppressed in generating odor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, an embodiment of the present invention will be described in detail. The vinyl chloride resin composition for powder molding of the present invention can be used, for example, when forming the vinyl chloride resin molded article of the present invention. The vinyl chloride resin molded article formed using the vinyl chloride resin composition for powder molding of the present invention can be suitably used, for example, as an automobile interior material such as the skin of automobile interior parts such as automobile instrument panels and door trims. The vinyl chloride resin molded article of the present invention can be used, for example, when forming the laminate of the present invention. The laminate formed using the vinyl chloride resin molded article of the present invention can be suitably used, for example, as an automobile interior material used when producing automobile interior parts such as automobile instrument panels and door trims.
[0025] (Vinyl chloride resin composition for powder molding) The vinyl chloride resin composition for powder molding of the present invention is characterized by containing (a) a vinyl chloride resin, (b) a plasticizer, and (c) a polyglycerol fatty acid ester. The vinyl chloride resin composition for powder molding of the present invention may optionally further contain additives other than the above-mentioned (a) vinyl chloride resin, (b) plasticizer, and (c) polyglycerol fatty acid ester. And, since the vinyl chloride resin composition for powder molding of the present invention contains at least the above-mentioned (a) vinyl chloride resin, (b) plasticizer, and (c) polyglycerin fatty acid ester, it is possible to form a vinyl chloride resin molding in which odor generation is suppressed. Also, since the vinyl chloride resin composition for powder molding of the present invention contains at least the above-mentioned (a) vinyl chloride resin, (b) plasticizer, and (c) polyglycerin fatty acid ester, the vinyl chloride resin molding formed using the vinyl chloride resin composition for powder molding of the present invention is also excellent in tensile elongation when evaluated at low temperature after heating (hereinafter, sometimes referred to as "low-temperature tensile elongation after heating"). Therefore, by using the vinyl chloride resin composition for powder molding of the present invention, it is possible to obtain vinyl chloride resin molded articles suitable for automobile interior materials, such as skins for automobile instrument panels and door trim skins, which are suppressed in generating odors. From the viewpoint of easily obtaining vinyl chloride resin molded articles that can be favorably used as automobile interior materials, for example, using the vinyl chloride resin composition for powder molding of the present invention, it is preferable that the vinyl chloride resin composition for powder molding of the present invention is used for powder slush molding.
[0026] <(a) Polyvinyl chloride resin> As the (a) vinyl chloride resin, a particulate vinyl chloride resin is usually used. And, as the (a) vinyl chloride resin, for example, one or more kinds of vinyl chloride resin particles can be contained, and optionally, one or more kinds of vinyl chloride resin microparticles can be further contained. Among them, the (a) vinyl chloride resin preferably contains at least vinyl chloride resin particles, and more preferably contains vinyl chloride resin particles and vinyl chloride resin microparticles. The (a) vinyl chloride resin can be produced by any of the conventionally known production methods, such as suspension polymerization, emulsion polymerization, solution polymerization, and bulk polymerization. In this specification, the term "resin particles" refers to particles having a particle diameter of 30 μm or more, and the term "resin fine particles" refers to particles having a particle diameter of less than 30 μm.
[0027] In addition, the vinyl chloride resin (a) may be a homopolymer made of vinyl chloride monomer units, or a vinyl chloride copolymer containing preferably 50% by mass or more, more preferably 70% by mass or more, of vinyl chloride monomer units. Specific examples of monomers (comonomers) that can be copolymerized with vinyl chloride monomers and that can constitute vinyl chloride copolymers include those described in International Publication No. 2016 / 098344. These components may be used alone or in combination of two or more at any ratio.
[0028] <<Vinyl chloride resin particles>> In the vinyl chloride resin composition, the vinyl chloride resin particles usually function as a matrix resin (substrate). The vinyl chloride resin particles are preferably produced by a suspension polymerization method.
[0029] [Average degree of polymerization] The average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin particles is preferably 800 or more, more preferably 1000 or more, more preferably 5000 or less, more preferably 3000 or less, and even more preferably 2800 or less. If the average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin particles is the above lower limit or more, the physical strength of the vinyl chloride resin molded body formed using the vinyl chloride resin composition for powder molding can be sufficiently ensured, while, for example, the tensile properties, particularly the tensile elongation, can be made better. And, a vinyl chloride resin molded body having good tensile elongation can be suitably used as an automobile interior material such as the skin of an automobile instrument panel having excellent ductility, which breaks as designed without scattering fragments when an airbag is inflated and deployed. Also, if the average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin particles is the above upper limit or less, the meltability of the vinyl chloride resin composition for powder molding can be improved. In the present invention, the "average degree of polymerization" can be measured in accordance with JIS K6720-2.
[0030] [Average particle size] Also, the average particle size of the vinyl chloride resin particles is usually 30 μm or more, preferably 50 μm or more, more preferably 100 μm or more, and preferably 500 μm or less, more preferably 200 μm or less. If the average particle size of the vinyl chloride resin particles is the above lower limit or more, the powder flowability of the vinyl chloride resin composition for powder molding is further improved. If the average particle size of the vinyl chloride resin particles is the above upper limit or less, the meltability of the vinyl chloride resin composition for powder molding is further improved, and the surface smoothness of the vinyl chloride resin molded body formed using the composition can be improved. In the present invention, the "average particle size" can be measured as a volume average particle size by a laser diffraction method in accordance with JIS Z8825.
[0031] [Content ratio] The content of vinyl chloride resin particles in (a) vinyl chloride resin is preferably 70% by mass or more, more preferably 80% by mass or more, and can be 100% by mass, and is preferably 95% by mass or less, and more preferably 90% by mass or less. If the content of vinyl chloride resin particles in (a) vinyl chloride resin is the above lower limit or more, the vinyl chloride resin molding formed using the vinyl chloride resin composition for powder molding can have good tensile elongation while sufficiently ensuring the physical strength. Also, if the content of vinyl chloride resin particles in (a) vinyl chloride resin is the above upper limit or less, the powder flowability of the vinyl chloride resin composition for powder molding is improved.
[0032] <<Polyvinyl chloride resin particles>> In the vinyl chloride resin composition for powder molding, the vinyl chloride resin fine particles usually function as a dusting agent (powder flow improver). The vinyl chloride resin fine particles are preferably produced by an emulsion polymerization method.
[0033] [Average degree of polymerization] The average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin microparticles is preferably 500 or more, more preferably 700 or more, and more preferably 2600 or less, more preferably 2400 or less. If the average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin microparticles as a dusting agent is above the above lower limit, the powder flowability of the vinyl chloride resin composition for powder molding is improved, and the tensile elongation of the molded body obtained using the composition is improved. If the average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin microparticles is below the above upper limit, the meltability of the vinyl chloride resin composition for powder molding is improved, and the surface smoothness of the vinyl chloride resin molded body formed using the composition is improved.
[0034] [Average particle size] Also, the average particle diameter of the vinyl chloride resin fine particles is usually less than 30 μm, preferably 10 μm or less, more preferably 5 μm or less, preferably 0.1 μm or more, more preferably 1 μm or more. If the average particle diameter of the vinyl chloride resin fine particles is the above lower limit or more, for example, the powder flowability of the vinyl chloride resin composition for powder molding can be further improved without excessively reducing the size as a dusting agent. Also, if the average particle diameter of the vinyl chloride resin fine particles is the above upper limit or less, the meltability of the vinyl chloride resin composition for powder molding can be further improved, and the surface smoothness of the vinyl chloride resin molded body formed can be further improved.
[0035] [Content ratio] The content of vinyl chloride resin fine particles in (a) vinyl chloride resin may be 0% by mass, but is preferably 5% by mass or more, more preferably 10% by mass or more, and preferably 30% by mass or less, and more preferably 20% by mass or less. If the content of vinyl chloride resin fine particles in (a) vinyl chloride resin is equal to or more than the above lower limit, the powder flowability of the vinyl chloride resin composition for powder molding is further improved. Also, if the content of vinyl chloride resin fine particles in (a) vinyl chloride resin is equal to or less than the above upper limit, the physical strength of the vinyl chloride resin molded body formed using the vinyl chloride resin composition for powder molding can be further increased.
[0036] <(b) Plasticizer> The (b) plasticizer is not particularly limited, but preferably contains at least one of (b1) trimellitic acid ester and (b2) polyester. If the (b) plasticizer used in the vinyl chloride resin composition for powder molding of the present invention contains at least one of (b1) trimellitic acid ester and (b2) polyester, it is possible to form a vinyl chloride resin molded product having even better low-temperature tensile elongation after heating. The (b) plasticizer may contain plasticizers other than the (b1) trimellitic acid ester and the (b2) polyester.
[0037] <<(b1) Trimellitic acid ester>> The (b1) trimellitic acid ester contained in the (b) plasticizer is preferably an ester compound of trimellitic acid and a monohydric alcohol.
[0038] Specific examples of the monohydric alcohol include, but are not limited to, aliphatic alcohols such as 1-hexanol, 1-heptanol, 1-octanol, 2-ethylhexanol, 1-nonanol, 1-decanol, 1-undecanol, 1-dodecanol, etc. Among them, as the monohydric alcohol, aliphatic alcohols having 6 to 18 carbon atoms are preferred, and linear aliphatic alcohols having 6 to 18 carbon atoms are more preferred.
[0039] Among them, the trimellitic acid ester (b1) is preferably a triester product in which substantially all of the carboxy groups of trimellitic acid are esterified with the above-mentioned monohydric alcohol. The alcohol residue portions in the triester product may be derived from the same alcohol or from different alcohols. The trimellitic acid ester (b1) may consist of a single compound, or may be a mixture of different compounds.
[0040] Specific examples of suitable (b1) trimellitic acid esters include tri-n-hexyl trimellitate, tri-n-heptyl trimellitate, tri-n-octyl trimellitate, tri-(2-ethylhexyl) trimellitate, tri-n-nonyl trimellitate, tri-n-decyl trimellitate, triisodecyl trimellitate, tri-n-undecyl trimellitate, tri-n-dodecyl trimellitate, trialkyl trimellitate (esters having two or more types of alkyl groups with different carbon numbers [however, the number of carbon atoms is 6 to 18] in the molecule), tri-n-alkyl trimellitate (esters having two or more types of alkyl groups with different carbon numbers [however, the number of carbon atoms is 6 to 18] in the molecule), and mixtures thereof. More preferred specific examples of (b1) trimellitic acid esters include tri-n-octyl trimellitate, tri-(2-ethylhexyl) trimellitate, tri-n-nonyl trimellitate, tri-n-decyl trimellitate, tri-n-alkyl trimellitate (esters having two or more alkyl groups with different carbon numbers [however, the number of carbon atoms is 6 to 18] in the molecule), and mixtures thereof.
[0041] The content of the (b1) trimellitic acid ester in the (b) plasticizer can be 0% by mass or more, preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, and can be 100% by mass or less, preferably 70% by mass or less, and more preferably 50% by mass or less. If the content of the (b1) trimellitic acid ester in the (b) plasticizer is within the above-mentioned range, the low-temperature tensile elongation after heating of the resulting vinyl chloride resin molded article can be further increased.
[0042] The content of the (b1) trimellitic acid ester in the vinyl chloride resin composition for powder molding can be 0 parts by mass or more, preferably 10 parts by mass or more, more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, preferably 100 parts by mass or less, more preferably 70 parts by mass or less, and even more preferably 50 parts by mass or less, relative to 100 parts by mass of the (a) vinyl chloride resin composition for powder molding. If the content of the (b) trimellitic acid ester in the vinyl chloride resin composition for powder molding is within the above-mentioned predetermined range, the low-temperature tensile elongation after heating of the vinyl chloride resin molded article formed can be further increased.
[0043] <<(b2) Polyester>> The (b2) polyester contained in the (b) plasticizer is not particularly limited, and examples of polyesters that can be used include polyesters containing structural units derived from adipic acid (adipic acid-based polyesters), polyesters containing structural units derived from sebacic acid (sebacic acid-based polyesters), and polyesters containing structural units derived from phthalic acid (phthalic acid-based polyesters). These polyesters may be used alone or in combination of two or more at any ratio. The (b2) polyester contained in the (b) plasticizer is not particularly limited, and for example, a polyester containing a structural unit derived from a diol compound such as 3-methyl-1,5-pentanediol or 1,3-butanediol can be used.
[0044] From the viewpoint of further increasing the low-temperature tensile elongation after heating of the resulting vinyl chloride resin molded article, it is preferable to use, as the (b2) polyester, a polyester containing a structural unit derived from adipic acid, it is more preferable to use a polyester containing a structural unit derived from adipic acid and a structural unit derived from a diol compound, and it is particularly preferable to use a polyester containing a structural unit derived from adipic acid and a structural unit derived from 3-methyl-1,5-pentanediol.
[0045] For ease of explanation, the polyester containing structural units derived from adipic acid and structural units derived from 3-methyl-1,5-pentanediol will be referred to as "polyester A" hereinafter. Here, the polyester A containing the above-mentioned specific structural units may have structural units other than the structural units derived from adipic acid and the structural units derived from 3-methyl-1,5-pentanediol, but the total of the structural units derived from adipic acid and the structural units derived from 3-methyl-1,5-pentanediol is preferably 50% by mass or more, more preferably 80% by mass or more, of the total structural units.In addition, the polyester A containing the above-mentioned specific structural units preferably has only the structural units derived from adipic acid and the structural units derived from 3-methyl-1,5-pentanediol as repeating units.
[0046] The polyester A containing the above-mentioned predetermined structural unit can be obtained by condensation polymerization of adipic acid and 3-methyl-1,5-pentanediol without any particular limitation. The above-mentioned condensation polymerization can be carried out in the presence of a catalyst. The above-mentioned condensation polymerization can be carried out using an alcohol and / or a monobasic acid as a terminal termination component. The condensation polymerization of adipic acid and 3-methyl-1,5-pentanediol and the termination reaction of the obtained condensation polymer with the above-mentioned terminal termination component may be carried out together or separately. The product obtained through the condensation polymerization and the termination reaction may be subjected to post-treatment such as distillation. The reaction conditions of the condensation polymerization, such as the amounts of the above-mentioned monomers, catalysts and terminal termination components, can be known. As the polyester A containing the above-mentioned predetermined structural unit, a commercially available product may be used.
[0047] The catalyst used in the condensation polymerization reaction is not particularly limited, and examples thereof include dibutyltin oxide and tetraalkyl titanate.
[0048] Examples of alcohols that can be used as the end-stopping component include methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, hexanol, isohexanol, heptanol, isoheptanol, octanol, isooctanol, 2-ethylhexanol, nonanol, isononanol, decanol, isodecanol, undecanol, isoundecanol, dodecanol, tridecanol, isotridecanol, tetradecanol, pentadecanol, hexadecanol, heptadecanol, octadecanol, cellosolve, carbitol, phenol, nonylphenol, benzyl alcohol, and mixtures thereof. Additionally, monobasic acids which may be used as end-stopping components include, for example, acetic acid, propionic acid, butyric acid, isobutyric acid, valeric acid, pivalic acid, caproic acid, heptanoic acid, caprylic acid, 2-ethylhexyl acid, pelargonic acid, capric acid, undecanoic acid, lauric acid, tridecanoic acid, myristic acid, pentadecanoic acid, palmitic acid, heptadecanoic acid, stearic acid, benzoic acid, and mixtures thereof. Among these, 2-ethylhexanol is preferred as the end-terminator component.
[0049] The polyester A containing the above-mentioned predetermined structural unit preferably has a number average molecular weight of 1,000 or more, more preferably 2,000 or more, and preferably 10,000 or less, more preferably 7,000 or less. The "number average molecular weight" can be measured by a VPO (vapor pressure osmosis) method. Moreover, the polyester A containing the above-mentioned specific structural units preferably has an acid value of 1 or less. Furthermore, the polyester A containing the above-mentioned specific structural units preferably has a hydroxyl value of 30 or less.
[0050] Furthermore, the polyester A containing the above-mentioned specified structural unit preferably has a viscosity of 500 mPa·s or more, more preferably 1000 mPa·s or more, and preferably 8000 mPa·s or less, more preferably 5000 mPa·s or less. The "viscosity" can be measured at a temperature of 23°C in accordance with JIS Z8803.
[0051] The content of the (b2) polyester in the (b) plasticizer can be 0% by mass or more, preferably 20% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more, and can be 100% by mass or less, preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less. If the content of the (b2) polyester in the (b) plasticizer is within the above-mentioned range, the low-temperature tensile elongation after heating of the resulting vinyl chloride resin molded article can be further increased.
[0052] The content of the (b2) polyester in the vinyl chloride resin composition for powder molding can be 0 parts by mass or more, preferably 20 parts by mass or more, more preferably 40 parts by mass or more, even more preferably 50 parts by mass or more, and preferably 100 parts by mass or less, more preferably 90 parts by mass or less, even more preferably 80 parts by mass or less, and even more preferably 70 parts by mass or less, relative to 100 parts by mass of the (a) vinyl chloride resin. If the content of the (b2) polyester in the vinyl chloride resin composition for powder molding is within the above-mentioned predetermined range, the low-temperature tensile elongation after heating of the vinyl chloride resin molded article can be further increased.
[0053] Furthermore, the total content of the (b1) trimellitic acid ester and (b2) polyester in the vinyl chloride resin composition for powder molding is preferably 30 parts by mass or more, more preferably 50 parts by mass or more, even more preferably 70 parts by mass or more, even more preferably 90 parts by mass or more, and preferably 200 parts by mass or less, more preferably 180 parts by mass or less, even more preferably 150 parts by mass or less, and even more preferably 110 parts by mass or less, relative to 100 parts by mass of the (a) vinyl chloride resin. If the total content of the (b1) trimellitic acid ester and (b2) polyester in the vinyl chloride resin composition for powder molding is within the above-mentioned predetermined range, the low-temperature tensile elongation after heating of the vinyl chloride resin molded body formed can be further increased.
[0054] In addition, the mass ratio of (b1) trimellitic acid ester to (b2) polyester (trimellitic acid ester / polyester) in the vinyl chloride resin composition for powder molding is preferably 1 / 9 or more, more preferably 2 / 8 or more, and even more preferably 3 / 7 or more, and is preferably 9 / 1 or less, more preferably 8 / 2 or less, and even more preferably 7 / 3 or less. If the mass ratio of (b1) trimellitic acid ester to (b2) polyester (trimellitic acid ester / polyester) in the vinyl chloride resin composition for powder molding is within the above-mentioned predetermined range, the generation of odor from the vinyl chloride resin molded article formed can be further suppressed.
[0055] The (b2) polyester contained in the (b) plasticizer is a component different from the polyglycerol fatty acid ester described below.
[0056] The weight average molecular weight of the (b2) polyester is preferably 4,200 or more, more preferably 4,500 or more, even more preferably 5,000 or more, and even more preferably 5,500 or more, and is preferably 10,000 or less. The weight average molecular weight of the polyester can be measured by the method described in the Examples of this specification.
[0057] <<(b3) Other plasticizers>> The (b) plasticizer contained in the vinyl chloride resin composition for powder molding may optionally contain a plasticizer other than the above-mentioned (b1) trimellitic acid ester and (b2) polyester (sometimes referred to as "(b3) other plasticizer").
[0058] Specific examples of the (b3) other plasticizer include the above-mentioned (b1) trimellitic acid ester and (b2) plasticizers other than polyester among the plasticizers described in International Publication No. 2016 / 098344. Among them, it is preferable to use epoxidized soybean oil from the viewpoint of further increasing the flexibility of the vinyl chloride resin molded body at low temperatures.
[0059] The content of the (b3) other plasticizer in the (b) plasticizer is not particularly limited, but is preferably 0% by mass or more and 5% by mass or less. If the content of the (b3) other plasticizer in the (b) plasticizer is within the above range, the low-temperature tensile elongation after heating of the resulting vinyl chloride resin molded article can be further increased.
[0060] In addition, the content of the above-mentioned (b3) other plasticizer in the vinyl chloride resin composition for powder molding is not particularly limited, but can be from 0 to 5 parts by mass per 100 parts by mass of the above-mentioned (a) vinyl chloride resin.
[0061] The total content of the (b1) trimellitic acid ester, (b2) polyester, and (b3) other plasticizer in the vinyl chloride resin composition for powder molding (i.e., the content of the (b) plasticizer) is preferably 30 parts by mass or more, more preferably 50 parts by mass or more, even more preferably 70 parts by mass or more, even more preferably 90 parts by mass or more, and preferably 205 parts by mass or less, more preferably 185 parts by mass or less, even more preferably 155 parts by mass or less, and even more preferably 115 parts by mass or less, relative to 100 parts by mass of vinyl chloride resin. If the content of the (b) plasticizer in the vinyl chloride resin composition for powder molding is within the above-mentioned predetermined range, the low-temperature tensile elongation after heating of the vinyl chloride resin molded body formed can be further increased.
[0062] <(c) Polyglycerol fatty acid ester> The (c) polyglycerol fatty acid ester contained in the vinyl chloride resin composition for powder molding of the present invention is an ester compound of a fatty acid and polyglycerol formed by condensation polymerization of multiple glycerol molecules.
[0063] Furthermore, since the vinyl chloride resin composition for powder molding of the present invention contains (c) a polyglycerol fatty acid ester, odor generation from the vinyl chloride resin molded article formed can be effectively suppressed. Also, since the vinyl chloride resin composition for powder molding of the present invention contains (c) a polyglycerol fatty acid ester, the low-temperature tensile elongation after heating of the vinyl chloride resin molded article formed can be improved.
[0064] Here, the (c) polyglycerol fatty acid ester contained in the vinyl chloride resin composition for powder molding of the present invention is represented by the following formula (I): [ka] [In formula (I), n represents an integer of 2 or more, R represents hydrogen or a fatty acid residue; At least one of the R's represents a fatty acid residue; The multiple R's may be the same or different. It can be expressed as:
[0065] In the above formula (I), n represents the repeat number of the structural unit derived from glycerin. The repeat number n of the structural unit derived from glycerin is preferably 20 or less, more preferably 15 or less, even more preferably 10 or less, preferably 3 or more, more preferably 4 or more, and particularly preferably 4. When the repeat number n of the structural unit derived from glycerin is within the above-mentioned range, the generation of odor from the vinyl chloride resin molded article formed can be further suppressed, and the low-temperature tensile elongation after heating of the vinyl chloride resin molded article can be further increased.
[0066] The polyglycerin fatty acid ester represented by (I) has a plurality of R (n+2). The lower limit of the number of fatty acid residues (alkylcarbonyl groups) among the plurality of Rs in the polyglycerin fatty acid ester represented by (I) is not particularly limited as long as it is 1 or more. The upper limit of the number of fatty acid residues (alkylcarbonyl groups) among the plurality of Rs in the polyglycerin fatty acid ester represented by (I) is not particularly limited as long as it is n+2 or less, but is preferably n+1 or less. If the number of fatty acid residues in the polyglycerin fatty acid ester is n+1 or less, the generation of odor from the vinyl chloride resin molded body formed can be further suppressed, and the low-temperature tensile elongation after heating of the vinyl chloride resin molded body can be further increased. The number of fatty acid residues in the polyglycerin fatty acid ester may be, for example, n or less, or n-1 or less. Among the multiple R's contained in the polyglycerol fatty acid ester represented by (I) above, it is particularly preferable that the number of fatty acid residues (alkylcarbonyl groups) is 1. If the number of fatty acid residues contained in the polyglycerol fatty acid ester is 1, the generation of odor from the vinyl chloride resin molded article formed can be further suppressed, and the low-temperature tensile elongation after heating of the vinyl chloride resin molded article can be further increased.
[0067] When R represents a fatty acid residue (alkylcarbonyl group), the fatty acid residue is not particularly limited and may be, for example, a saturated fatty acid residue such as a caprylic acid residue, a lauric acid residue, a myristic acid residue, a stearic acid residue, a behenic acid residue, or the like, or an unsaturated fatty acid residue such as an oleic acid residue, an erucic acid residue, or the like. However, from the viewpoint of further increasing the low-temperature tensile elongation after heating of the resulting vinyl chloride resin molded article, it is preferable that the fatty acid residue be a saturated fatty acid.
[0068] Furthermore, when R represents a fatty acid residue (alkylcarbonyl group), the number of carbon atoms in the fatty acid residue (alkylcarbonyl group) is preferably 2 or more, more preferably 5 or more, and even more preferably 10 or more, and is preferably 30 or less, more preferably 25 or less, and even more preferably 20 or less. When the number of carbon atoms in the fatty acid residue is within the above-mentioned range, odor generation from the formed vinyl chloride resin molded article can be further suppressed, and the low-temperature tensile elongation after heating of the vinyl chloride resin molded article can be further increased.
[0069] Specific examples of the polyglycerol fatty acid ester represented by the above formula (I) include polyglycerol stearic acid esters such as decaglycerol monostearate, decaglycerol tristearate, decaglycerol deca stearate, hexaglycerol monostearate, hexaglycerol tristearate, hexaglycerol pentastearate, tetraglycerol monostearate, tetraglycerol tristearate, and tetraglycerol pentastearate; decaglycerol monooleate, decaglycerol decaoleate, hexaglycerol monooleate, hexaglycerol pentaoleate, tetraglycerol monooleate, tetraglycerol monooleate, and tetraglycerol monooleate. Examples of suitable polyglycerol oleate esters include polyglycerol pentaoleate; polyglycerol caprylate esters, such as decaglycerol monocaprylate and diglycerol monocaprylate; polyglycerol laurate esters, such as decaglycerol monolaurate, hexaglycerol monolaurate and tetraglycerol monolaurate; polyglycerol myristate esters, such as decaglycerol monomyristate; polyglycerol behenate esters, such as decaglycerol heptabehenate and decaglycerol dodecabehenate; polyglycerol erucate esters, such as decaglycerol octaerucate; and polyglycerol condensed ricinoleate esters.
[0070] As the (c) polyglycerol fatty acid ester contained in the vinyl chloride resin composition for powder molding of the present invention, only one type of polyglycerol fatty acid ester represented by the above formula (I) may be used alone, or two or more types may be mixed in any ratio and used. Furthermore, when the (c) polyglycerol fatty acid ester contained in the vinyl chloride resin composition for powder molding of the present invention is a mixture containing two or more polyglycerol fatty acid esters represented by the above formula (I), the preferred ranges of the average values of the number of repeats n of the glycerol-derived structural unit, the number of fatty acid residues (alkylcarbonyl groups), and the number of carbon atoms of the fatty acid residues of the polyglycerol fatty acid esters in the mixture can be the same as the preferred ranges of the number of repeats n of the glycerol-derived structural unit, the number of fatty acid residues (alkylcarbonyl groups), and the number of carbon atoms of the fatty acid residues described above.
[0071] The weight-average molecular weight of the (c) polyglycerol fatty acid ester is preferably at least 600, more preferably at least 800, and even more preferably at least 1000, and is preferably at most 4000, more preferably at most 3000, and even more preferably at most 2000. When the weight-average molecular weight of the (c) polyglycerol fatty acid ester is within the above-mentioned range, odor generation from the formed vinyl chloride resin molded article can be further suppressed, and the low-temperature tensile elongation of the vinyl chloride resin molded article after heating can be further increased. The weight average molecular weight of the polyglycerol fatty acid ester can be measured by the method described in the Examples of this specification.
[0072] The HLB value of the (c) polyglycerol fatty acid ester is preferably, for example, 1 or more and 15 or less. The HLB value of (c) polyglycerol fatty acid ester can be calculated by the formula 20(1-S / A), where S is the saponification value of the polyglycerol fatty acid ester and A is the acid value of the fatty acid constituting the polyglycerol fatty acid ester.
[0073] (c) As the polyglycerol fatty acid ester, commercially available products can be used, for example, products with the names "DAS-7S", "PS-5S", "MS-3S", "PS-3S", "PO-5S", and "PO-3S" (all manufactured by Sakamoto Pharmaceutical Co., Ltd.), etc.
[0074] The content of (c) polyglycerol fatty acid ester in the vinyl chloride resin composition for powder molding is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.5 parts by mass or more, and preferably 10 parts by mass or less, more preferably 6 parts by mass or less, and even more preferably 3 parts by mass or less, relative to 100 parts by mass of vinyl chloride resin. If the content of (c) polyglycerol fatty acid ester in the vinyl chloride resin composition for powder molding is within the above-mentioned predetermined range, the generation of odor from the vinyl chloride resin molded article formed can be further suppressed, and the low-temperature tensile elongation after heating of the vinyl chloride resin molded article can be further increased.
[0075] <Additives> The vinyl chloride resin composition for powder molding of the present invention may further contain various additives in addition to the above-mentioned components. The additives are not particularly limited, and include lubricants, stabilizers such as perchloric acid-treated hydrotalcite, zeolite, β-diketone, and fatty acid metal salts, release agents, dusting agents other than the above-mentioned vinyl chloride resin fine particles, impact resistance improvers, perchloric acid compounds other than perchloric acid-treated hydrotalcite (sodium perchlorate, potassium perchlorate, etc.), antioxidants, antifungal agents, flame retardants, antistatic agents, fillers, light stabilizers, foaming agents, and pigments.
[0076] As the above-mentioned additives that may be contained in the vinyl chloride resin composition for powder molding of the present invention, for example, those described in WO 2016 / 098344 can be used, and the preferred content thereof can also be the same as that described in WO 2016 / 098344.
[0077] <Method for preparing vinyl chloride resin composition for powder molding> The vinyl chloride resin composition for powder molding of the present invention can be prepared by mixing the above-mentioned components. Here, the method of mixing the (a) vinyl chloride resin, (b) plasticizer, (c) polyglycerol fatty acid ester, and various additives further blended as necessary is not particularly limited, and for example, the components other than the dusting agent (including the vinyl chloride resin fine particles) are mixed by dry blending, and then the dusting agent is added and mixed. Here, it is preferable to use a Henschel mixer for dry blending. In addition, the temperature during dry blending is not particularly limited, and is preferably 50°C or higher, more preferably 70°C or higher, and preferably 200°C or lower.
[0078] <Applications of polyvinyl chloride resin compositions for powder molding> The obtained vinyl chloride resin composition for powder molding can be used for powder molding, and can be suitably used for powder slush molding.
[0079] (Vinyl chloride resin molding) The vinyl chloride resin molded body of the present invention is characterized in that it is obtained by molding the above-mentioned vinyl chloride resin composition for powder molding by any method. Since the vinyl chloride resin molded body of the present invention is formed using the above-mentioned vinyl chloride resin composition for powder molding, it usually contains at least (a) vinyl chloride resin, (b) plasticizer, and (c) polyglycerin fatty acid ester, and odor generation is suppressed. Furthermore, since the vinyl chloride resin molded body of the present invention is formed using the above-mentioned vinyl chloride resin composition for powder molding, it is also excellent in low-temperature tensile elongation after heating. Therefore, the laminate formed by backing a foamed polyurethane molding with the vinyl chloride resin molding of the present invention has reduced odor generation and can be suitably used as an automobile interior material such as the surface of an automobile instrument panel.
[0080] <Method of forming polyvinyl chloride resin molded article> Here, when forming a vinyl chloride resin molded article by powder slush molding, the mold temperature during powder slush molding is not particularly limited, but is preferably 200°C or higher, more preferably 220°C or higher, and is preferably 300°C or lower, and more preferably 280°C or lower.
[0081] When producing a vinyl chloride resin molded article, the following method can be used, without any particular limitation. That is, the vinyl chloride resin composition for powder molding of the present invention is sprinkled on a mold having a temperature in the above range, and the mold is left for 5 to 30 seconds, after which the excess vinyl chloride resin composition for powder molding is shaken off, and the mold is further left for 30 seconds to 3 minutes at an arbitrary temperature. Thereafter, the mold is cooled to 10°C to 60°C, and the obtained vinyl chloride resin molded article of the present invention is demolded from the mold. Then, a sheet-shaped molded article having the shape of the mold is obtained.
[0082] (Laminate) The laminate of the present invention comprises a polyurethane foam molded article and the vinyl chloride resin molded article described above. The vinyl chloride resin molded article usually constitutes one surface of the laminate. The laminate of the present invention has, for example, a vinyl chloride resin molded article formed using the vinyl chloride resin composition for powder molding of the present invention, and thus odor generation is suppressed. Therefore, the laminate of the present invention is suitably used as an automobile interior part, particularly an automobile interior material for forming an automobile instrument panel.
[0083] Here, the lamination method of the polyurethane foam molded body and the vinyl chloride resin molded body is not particularly limited, and the following methods can be used, for example. That is, (1) a method of separately preparing a polyurethane foam molded body and a vinyl chloride resin molded body, and then bonding them together by heat fusion, heat adhesion, or using a known adhesive, etc.; (2) a method of directly forming a polyurethane foam molded body on a vinyl chloride resin molded body by reacting isocyanates and polyols, etc., which are raw materials for the polyurethane foam molded body, on the vinyl chloride resin molded body to polymerize them, and foaming the polyurethane by a known method; etc. Among them, the latter method (2) is preferable because the process is simple and it is easy to firmly bond the vinyl chloride resin molded body and the polyurethane foam molded body even when laminates of various shapes are obtained. EXAMPLES
[0084] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following description, the units "%" and "parts" expressing amounts are by mass unless otherwise specified. The weight average molecular weights of Polyester A and polyglycerol fatty acid ester, as well as the low-temperature tensile elongation and odor intensity of the polyvinyl chloride resin molded sheet, were measured and evaluated by the following methods.
[0085] <Weight average molecular weight> The weight average molecular weight (Mw) of polyester A and polyglycerol fatty acid ester was determined as a polystyrene equivalent value by gel permeation chromatography (GPC) using THF as a solvent.
[0086] <Low temperature tensile elongation> <<Before heating (initial stage)>> The obtained polyvinyl chloride resin molded sheet was punched out with a No. 1 dumbbell as specified in JIS K6251, and the tensile elongation at break (%) was measured at a low temperature of -10°C at a pulling speed of 200 mm / min in accordance with JIS K7113. The larger the tensile elongation at break value, the better the polyvinyl chloride resin molded sheet is in tensile elongation at low temperatures before heating (initial stage) (low-temperature tensile elongation). <<After heating (thermal aging test)>> A laminate backed by a polyurethane foam was used as a sample. The sample was placed in an oven and heated for 1200 hours in an environment at a temperature of 120°C. Next, the polyurethane foam was peeled off from the heated laminate to prepare only a vinyl chloride resin molded sheet. Then, under the same conditions as in the initial case, the tensile elongation at break (%) of the vinyl chloride resin molded sheet after heating at 120°C for 1200 hours was measured. The larger the tensile elongation at break, the better the vinyl chloride resin molded sheet is in low-temperature tensile elongation after heating.
[0087] <Odor Intensity> The obtained vinyl chloride resin molded sheet was cut into a size of 5 cm x 5 cm, and the obtained test piece was placed in a 6 L polyethylene terephthalate bag and closed by heat sealing. 4 L of nitrogen gas was charged into the bag from the inlet, and then the bag was heated in a thermostatic chamber at 100 ° C for 1 hour. After heating, the bag was taken out and cooled to room temperature, and then opened, and the odor in the bag was evaluated by five panelists on the following five-level scale. The average value of the evaluations by the five panelists was taken as the odor intensity. The smaller the odor intensity value, the more the odor generation from the vinyl chloride resin molded sheet was suppressed. 4. Very strong odor 3. Detectable odors 2. A weak smell that makes it easy to identify what it is. 1. A smell that can barely be detected 0 Odorless
[0088] (Production example) The polyesters used in the examples and comparative examples were prepared as follows. <Polyester A> Adipic acid as a polyvalent carboxylic acid, 3-methyl-1,5-pentanediol as a polyhydric alcohol, and 2-ethylhexanol as a stopper (terminal termination component) were charged into a reaction vessel, tetraisopropyl titanate was added as a catalyst, a solvent was added appropriately, and the temperature was raised while stirring. The by-product water was removed under normal pressure and reduced pressure, and the temperature was finally raised to 220-230°C to complete the dehydration condensation reaction. The obtained product was subjected to thin-film distillation under conditions of a pressure of 4-80 Pa and an outer jacket temperature of 250°C to obtain polyester A (viscosity: 3600 mPa·s, number average molecular weight: 5300, acid value: 0.32, hydroxyl value: 12.7) consisting of 2-ethylhexoxy groups at the ends. When measured according to the method described above, the weight average molecular weight of polyester A was 6227.
[0089] Example 1 <Preparation of vinyl chloride resin composition for powder molding> Of the ingredients shown in Table 1, the ingredients other than the plasticizer (trimellitic acid ester, polyester A, and epoxidized soybean oil) and the vinyl chloride resin fine particles as a dusting agent were mixed in a Henschel mixer. Then, when the temperature of the mixture rose to 80°C, all of the plasticizer was added and the mixture was allowed to dry up (referring to a state in which the plasticizer is absorbed into the vinyl chloride resin particles as the vinyl chloride resin and the mixture becomes smooth). Thereafter, when the dried-up mixture was cooled to a temperature of 70°C or less, the vinyl chloride resin fine particles as a dusting agent were added to prepare a vinyl chloride resin composition for powder molding. The weight-average molecular weight of the polyglycerol fatty acid ester used as a blending component was measured according to the method described above. The results are shown in Table 1. <Formation of polyvinyl chloride resin molded body> A vinyl chloride resin molded sheet having dimensions of 200 mm×300 mm×1 mm was prepared as follows. Specifically, the vinyl chloride resin composition for powder molding obtained above was sprinkled onto a textured mold heated to a temperature of 250°C, and after leaving it for an arbitrary time to melt, the excess vinyl chloride resin composition for powder molding was shaken off. The textured mold onto which the vinyl chloride resin composition for powder molding had been sprinkled was then placed in an oven set at a temperature of 200°C, and after 60 seconds had elapsed since being placed still, the textured mold was cooled with cooling water. When the mold temperature was cooled to 40°C, a vinyl chloride resin molded sheet as a vinyl chloride resin molded body was removed from the mold. The obtained polyvinyl chloride resin molded sheet (dimensions: 200 mm × 300 mm × 1 mm) was then measured and evaluated for odor intensity and low-temperature tensile elongation before heating (initial stage) according to the above-mentioned method. The results are shown in Table 1. <Formation of Laminate> The obtained polyvinyl chloride resin molded sheet (dimensions: 200 mm×300 mm×1 mm) was placed in a mold of 200 mm×300 mm×10 mm with the textured surface facing down. Separately, 50 parts of propylene glycol PO (propylene oxide) · EO (ethylene oxide) block adduct (hydroxyl value 28, content of terminal EO units = 10%, content of internal EO units 4%), 50 parts of glycerin PO · EO block adduct (hydroxyl value 21, content of terminal EO units = 14%), 2.5 parts of water, 0.2 parts of ethylene glycol solution of triethylenediamine (manufactured by Tosoh Corporation, product name "TEDA-L33"), 1.2 parts of triethanolamine, 0.5 parts of triethylamine, and 0.5 parts of foam stabilizer (manufactured by Shin-Etsu Chemical Co., Ltd., product name "F-122") were mixed to obtain a polyol mixture. In addition, a mixed liquid was prepared by mixing the obtained polyol mixture with polymethylene polyphenylene polyisocyanate (Polymeric MDI) in a ratio such that the index was 98. The prepared mixed liquid was then poured onto the polyvinyl chloride resin molding sheet laid in the mold as described above. Thereafter, the mold was covered with an aluminum plate measuring 348 mm × 255 mm × 10 mm to seal the mold. The mold was left for 5 minutes after sealing, and a polyurethane foam molded body (thickness: 9 mm, density: 0.2 g / cm) was formed on a polyvinyl chloride resin molded sheet (thickness: 1 mm) as a skin. 3) backed laminate was formed. The formed laminate was then removed from the mold, and the low-temperature tensile elongation of the vinyl chloride resin molded sheet after heating (thermal aging test) was measured and evaluated according to the method described above. The results are shown in Table 1.
[0090] (Examples 2 to 6) A vinyl chloride resin composition for powder molding, a vinyl chloride resin molded body, and a laminate were prepared in the same manner as in Example 1, except that the type of polyglycerol fatty acid ester was changed as shown in Table 1. Measurements and evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 1.
[0091] Comparative Example 1 A vinyl chloride resin composition for powder molding, a vinyl chloride resin molded body, and a laminate were produced in the same manner as in Example 1, except that no polyglycerol fatty acid ester was added. Measurements and evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 1.
[0092] Example 7 As shown in Table 1, a vinyl chloride resin composition for powder molding and a vinyl chloride resin molded body were produced in the same manner as in Example 3, except that the amount of trimellitic acid ester added was increased to compensate for the absence of polyester A. Then, measurements and evaluations were performed in the same manner as in Example 1, except that evaluation of low-temperature tensile elongation was not performed. The results are shown in Table 1.
[0093] Comparative Example 2 A vinyl chloride resin composition for powder molding and a vinyl chloride resin molded body were produced in the same manner as in Example 7, except that no polyglycerol fatty acid ester was added. Measurements and evaluations were then carried out in the same manner as in Example 1, except that evaluation of low-temperature tensile elongation was not carried out. The results are shown in Table 1.
[0094] Example 8 As shown in Table 1, a vinyl chloride resin composition for powder molding and a vinyl chloride resin molded body were produced in the same manner as in Example 3, except that the amount of polyester A added was increased to compensate for the absence of trimellitic ester. Measurements and evaluations were then carried out in the same manner as in Example 1, except that evaluation of low-temperature tensile elongation was not performed. The results are shown in Table 1.
[0095] Comparative Example 3 A vinyl chloride resin composition for powder molding and a vinyl chloride resin molded body were produced in the same manner as in Example 8, except that no polyglycerol fatty acid ester was added. Measurements and evaluations were then carried out in the same manner as in Example 1, except that evaluation of low-temperature tensile elongation was not carried out. The results are shown in Table 1.
[0096] Example 9 As shown in Table 1, a vinyl chloride resin composition for powder molding and a vinyl chloride resin molded body were produced in the same manner as in Example 3, except that the amounts of both the trimellitic acid ester and polyester A added were reduced. Then, measurements and evaluations were performed in the same manner as in Example 1, except that evaluation of low-temperature tensile elongation was not performed. The results are shown in Table 1.
[0097] Comparative Example 4 A vinyl chloride resin composition for powder molding and a vinyl chloride resin molded body were produced in the same manner as in Example 9, except that no polyglycerol fatty acid ester was added. Measurements and evaluations were then carried out in the same manner as in Example 1, except that evaluation of low-temperature tensile elongation was not carried out. The results are shown in Table 1.
[0098] [Table 1]
[0099] 1) Shin-Daiichi Vinyl Corporation, product name "ZEST (registered trademark) 1700ZI" (prepared by suspension polymerization method, average polymerization degree: 1700, average particle size: 129 μm) 2) Shin-Daiichi Vinyl Corporation, product name "ZEST PQLTX" (prepared by emulsion polymerization method, average polymerization degree: 800, average particle size: 1.8 μm) 3) Tosoh Corporation, product name "Ryuron Paste 761" (prepared by emulsion polymerization method, average polymerization degree: 2100, average particle size: 1.7 μm) 4) Kao Corporation, product name "Trimex N-08" 5) ADEKA, product name: Adeka Cizer O-130S 6) Kyowa Chemical Industry Co., Ltd., product name "Alcamizer (registered trademark) 5" 7) Mizusawa Chemical Industry Co., Ltd., product name "MIZUKALIZER DS" 8) Showa Denko Co., Ltd., product name "Karens DK-1" 9) ADEKA Corporation, product name "ADEKA STAB SC-131" 10) Sakai Chemical Industry Co., Ltd., product name "SAKAI SZ2000" 11) ADEKA, product name "ADEKA STAB LS-12" 12) Sakamoto Pharmaceutical Co., Ltd., product name "DAS-7S" (HLB value: 3.8) 13) Sakamoto Pharmaceutical Co., Ltd., product name "PS-5S" (HLB value: 4.5) 14) Sakamoto Pharmaceutical Co., Ltd., product name "MS-3S" (HLB value: 8.4) 15) Sakamoto Pharmaceutical Co., Ltd., product name "PS-3S" (HLB value: 2.6) 16) Sakamoto Pharmaceutical Co., Ltd., product name "PO-5S" (HLB value: 4.7) 17) Sakamoto Pharmaceutical Co., Ltd., product name "PO-3S" (HLB value: 2.9) 18) Shin-Etsu Silicone Co., Ltd., product name "KF-96H-300,000cs" (unmodified silicone oil (polydimethylsiloxane), viscosity: 30 x 10 4 cs) 19) Dainichi Seika Chemicals Co., Ltd., product name "DA PX 1720(A) Black"
[0100] From Table 1, it can be seen that the vinyl chloride resin molded sheets formed using the vinyl chloride resin compositions for powder molding of Examples 1 to 6, which contain vinyl chloride resin, plasticizer, and polyglycerin fatty acid ester, are able to suppress the generation of odors compared to the vinyl chloride resin molded sheets formed using the vinyl chloride resin composition for powder molding of Comparative Example 1, which has the same formulation except that it does not contain polyglycerin fatty acid ester. Similarly, it can be seen that the vinyl chloride resin molded sheets formed using the vinyl chloride resin compositions for powder molding of Examples 7 to 9, which contain vinyl chloride resin, a plasticizer, and polyglycerol fatty acid ester, are able to suppress the generation of odors, compared to the vinyl chloride resin molded sheets formed using the vinyl chloride resin compositions for powder molding of Comparative Examples 2 to 4, which have the same formulations as Examples 7 to 9 above, except that they do not contain polyglycerol fatty acid ester. [Industrial Applicability]
[0101] According to the present invention, it is possible to provide a vinyl chloride resin composition for powder molding which is capable of forming vinyl chloride resin molded articles with suppressed odor generation. Moreover, according to the present invention, it is possible to provide a vinyl chloride resin molded article in which odor generation is suppressed. Furthermore, according to the present invention, it is possible to provide a laminate which includes the vinyl chloride resin molded article and which is suppressed in generating odor.
Claims
1. A vinyl chloride resin composition for powder molding comprising a vinyl chloride resin, a plasticizer, and a polyglycerin fatty acid ester, the plasticizer includes at least one of a trimellitic acid ester and a polyester, A polyvinyl chloride resin composition for powder molding, wherein the total content of the trimellitate ester and the polyester is 90 parts by mass or more and 200 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
2. The polyglycerol fatty acid ester has the following formula (I): [Formula 1] [In formula (I), n represents an integer of 2 or more and 20 or less; R represents hydrogen or a fatty acid residue; At least one of the R's represents a fatty acid residue; The multiple R's may be the same or different. The vinyl chloride resin composition for powder molding according to claim 1, wherein the vinyl chloride resin composition is represented by the formula:
3. 3. The vinyl chloride resin composition for powder molding according to claim 2, wherein the number of fatty acid residues among the plurality of R is n+1 or less.
4. 4. The vinyl chloride resin composition for powder molding according to claim 2 or 3, wherein the fatty acid residue has 2 or more and 30 or less carbon atoms.
5. The vinyl chloride resin composition for powder molding according to any one of claims 2 to 4, wherein at least one of the plurality of R represents a saturated fatty acid residue.
6. The polyglycerol fatty acid ester content is 0.1 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the vinyl chloride resin.
7. the plasticizer comprises a trimellitic ester and a polyester; The polyvinyl chloride resin composition for powder molding according to any one of claims 1 to 6, wherein the mass ratio of the trimellitate ester to the polyester (trimellitate ester / polyester) is 1 / 9 or more and 9 / 1 or less.
8. The vinyl chloride resin composition for powder molding according to any one of claims 1 to 7, which is used for powder slush molding.
9. A vinyl chloride resin molded article obtained by powder molding the vinyl chloride resin composition for powder molding according to any one of claims 1 to 8.
10. 10. The vinyl chloride resin molded article according to claim 9, which is for use as a surface layer of an instrument panel of an automobile.
11. A laminate comprising a polyurethane foam molded article and the vinyl chloride resin molded article according to claim 9 or 10.
12. The laminate of claim 11 for use in an automobile instrument panel.
Citation Information
Patent Citations
Vinyl chloride based resin mixture
JP1984213748A
Vinyl chloride resin composition for powder molding and laminate using the same
JP1996291243A
Vinyl chloride resin hose
JP1998082484A
Vinyl chloride resin composition for food-wrapping