Packaging bags
A laminate structure with polybutylene terephthalate resin and metal foil layers addresses flexibility and gas barrier issues in packaging bags for hair coloring agents, ensuring durability and suitability for filling processes.
Patent Information
- Application Number
- JP2020090460
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-25
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-05-25
AI Technical Summary
Existing packaging bags for hair coloring agents with strong odors and basic substances like monoethanolamine lack flexibility, gas barrier properties, and durability, leading to issues such as pinhole formation, increased stiffness, and poor suitability for filling processes.
A laminate structure comprising a base film layer of polybutylene terephthalate resin, a gas barrier layer of metal foil, a surface modification layer with Zr or Cr salts, an extruded resin layer, and a sealant layer, with specific thickness and material properties to ensure flexibility and gas barrier properties.
The laminate structure provides a packaging bag that is resistant to strong bases, maintains gas barrier properties, and is flexible enough for filling machines, reducing pinhole formation and improving sealing performance.
Smart Images

Figure 0007567203000002 
Figure 0007567203000003 
Figure 0007567203000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a packaging bag, particularly to a packaging bag capable of storing contents containing monoethanolamine, such as a hair coloring agent, which can withstand use under high temperature conditions of 50°C or higher, can prevent the contents from penetrating into the base layer, does not affect the appearance due to pinholes or deterioration of the barrier layer, and has flexibility and suitability for use in a filling machine. [Background technology]
[0002] Many types of packaging bags have been put to practical use, depending on their convenience and design, as well as the contents and the environment in which they are used. In particular, in recent years, packaging bags that are formed from a laminate having a sealant layer and a plastic film as a base film and can fulfill required functions have been commercialized in various fields.
[0003] Generally, the role of packaging bags is to protect the contents from the external environment and external forces. They are used in a variety of environments, including cases where the packaging bag itself is heated, and so suitability is required for each case. Naturally, it is required to prevent the contents from leaking out, but for contents with particularly strong odors, there are also cases where it is most important to prevent the odor from seeping out and leaking out.
[0004] For example, hair colorants used to dye hair contain strong basic substances such as monoethanolamine and ammonia in the dye-containing solution, which gives them a strong odor, so they often require gas barrier properties as well as resistance to the contents.
[0005] That is, when a metal foil such as aluminum foil is used as a gas barrier layer in a packaging bag for storing a hair coloring agent, since the contents are strongly alkaline, it is necessary to prevent corrosion of the metal foil due to seepage of the contents, the resulting appearance defects, and a decrease in the peel strength between the layers of the laminate. Furthermore, it is also necessary to ensure the durability and peel strength of the components of the laminate that make up the packaging bag, such as preventing deterioration of the plastic film itself.
[0006] As a method for achieving both gas barrier properties and strong base resistance, Patent Document 1 proposes a packaging bag in which aluminum foil is subjected to a chemical conversion treatment to suppress corrosion of the aluminum foil. Prior Art Document 2 proposes a packaging bag made of a laminate using aluminum foil as a gas barrier layer, and proposes to solve the problem by providing an extrusion layer of a thermoplastic resin to improve the peel strength of the laminate.
[0007] However, in either case, a hard aluminum foil layer and a thermoplastic resin layer are laminated adjacent to each other in the laminate, and an intermediate base material layer is provided, so that the thickness of the laminate becomes thick, and accordingly, the stiffness of the laminate becomes strong and the flexibility is poor.
[0008] As a result, for example, resistance increases when folding in half during the filling process, or heat is not easily transmitted to the sealant layer during heat sealing, resulting in a high sealing temperature that approaches the melting point of the material, making the package unsuitable for the process of filling the contents, and further causing problems such as meandering of the laminate or poor appearance. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Patent No. 5584970 [Patent Document 2] JP 2003-81285 A Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been made in consideration of such circumstances, and an objective of the present invention is to provide a packaging bag capable of storing a hair color agent as a content, which has gas barrier properties, resistance to strong base-resistant contents, and flexibility as a packaging bag. [Means for solving the problem]
[0011] As a means for solving the above problem, the invention described in claim 1 is: A packaging bag capable of storing a hair color agent containing monoethanolamine as a content, The packaging bag is formed by making a laminate using a plastic film as a base material, The laminate is constructed by laminating, from the outside of the packaging bag, a base film layer, a gas barrier layer, a surface modification layer, an extrusion resin layer, and a sealant layer in this order, The base film layer is made of polybutylene terephthalate resin, The gas barrier layer is made of a metal foil, The packaging bag is characterized in that the loop stiffness strength of the laminate is 100 mN or less.
[0012] The invention described in claim 2 is as follows: 2. The packaging bag according to claim 1, wherein the surface modification layer comprises an inorganic coating containing Zr, Cr or a salt thereof, and an organic polymer coating covering the inorganic coating.
[0013] The invention described in claim 3 is a packaging bag described in claim 1 or claim 2, characterized in that the base film layer is made of biaxially stretched polybutylene terephthalate resin having a thickness of 15 μm or more and 25 μm or less.
[0014] The invention described in claim 4 is as follows: The packaging bag according to any one of claims 1 to 3, wherein the gas barrier layer is a foil made of aluminum or an aluminum alloy and has a thickness of 5 μm or more and 50 μm or less.
[0015] The invention described in claim 5 is as follows: The packaging bag according to any one of claims 1 to 4, characterized in that the extruded resin layer is formed by extruding low-density polyethylene or maleic anhydride-grafted polyethylene having a thickness of 10 μm or more and 35 μm or less, or by co-extrusion of low-density polyethylene and maleic anhydride-grafted polyethylene.
[0016] The invention described in claim 6 is as follows: The packaging bag according to any one of claims 1 to 4, wherein the extruded resin layer is made of a thermoplastic polyethylene resin having a thickness of 15 μm or more and 30 μm or less.
[0017] The invention described in claim 7 is as follows: The packaging bag according to any one of claims 1 to 6, wherein the sealant layer has a thickness of 20 μm or more and 100 μm or less. Effect of the Invention
[0018] According to the present invention, it is possible to provide a packaging bag capable of storing a hair color agent as a content, which has gas barrier properties, and combines resistance to strong base-resistant contents with the flexibility required for a packaging bag.
[0019] That is, the packaging bag is formed by manufacturing a laminate using a plastic film as a base material. The laminate is composed of a base film layer, a gas barrier layer, a surface modification layer, an extruded resin layer, and a sealant layer laminated in that order from the outside of the packaging bag. Therefore, it is possible to seal the contents after filling them, and filling by an automatic filling machine, for example, is also possible.
[0020] By using polybutylene terephthalate resin, which has a SP value different from that of the contents, for the base film layer, it is possible to reduce the thickness of the laminate and to achieve both excellent resistance and filling suitability. In addition, since polybutylene terephthalate film has excellent pinhole resistance, it is also effective in improving storage suitability after filling.
[0021] The gas barrier layer is made of a metal foil, so that it is possible to maintain a high level of gas barrier properties.
[0022] Furthermore, the laminate according to the present invention can have a loop stiffness strength of 100 mN or less, which gives the packaging bag sufficient flexibility and satisfies suitability for use with filling machines.
[0023] In particular, according to the invention described in claim 2, the surface modification layer is composed of an inorganic coating containing Zr, Cr or a salt thereof and an organic polymer coating covering the inorganic coating, and is therefore effective in improving the adhesion of the gas barrier layer made of metal foil to the resin layer, and is effective in improving the interlayer strength of the laminate.
[0024] In particular, according to the invention described in claim 3, the base film layer is made of biaxially oriented polybutylene terephthalate resin having a thickness of 15 μm or more and 25 μm or less, thereby ensuring the flexibility of the laminate (10), and is more effective in achieving both resistance to the contents and suitability for filling machines without adversely affecting suitability for filling machines, and in improving storage suitability after filling.
[0025] In particular, according to the invention described in claim 4, the gas barrier layer is a foil made of aluminum or an aluminum alloy having a thickness of 5 μm or more and 50 μm or less, thereby ensuring a high level of sufficient gas barrier properties while also achieving flexibility as a laminate, and making it possible to achieve a loop stiffness strength of 100 mN or less.
[0026] Furthermore, aluminum and aluminum alloys are generally materials that are stable in price and easy to obtain, and have sufficient flexibility in the foil state and can be easily laminated, making them suitable for use as packaging bags.
[0027] Furthermore, according to the invention described in claim 5 in particular, the extruded resin layer is formed by extruding low-density polyethylene or maleic anhydride-grafted polyethylene having a thickness of 10 μm or more and 35 μm or less, or by co-extrusion of low-density polyethylene and maleic anhydride-grafted polyethylene, thereby making it possible to directly form a laminate without providing an adhesive layer on the surface modification layer of the gas barrier layer.
[0028] In particular, according to the invention described in claim 6, the extruded resin layer is made of a thermoplastic polyethylene resin having a thickness of 15 μm or more and 30 μm or less, which is effective in improving adhesion when laminating the adhesive layer and the sealant layer using this extruded resin layer.
[0029] In particular, according to the invention described in claim 7, the sealant layer has a thickness of 20 μm or more and 100 μm or less, which makes it possible to ensure sufficient sealing properties, ensures sealing properties during bag manufacturing, and is effective in improving the sealing of the contents after they are filled. [Brief description of the drawings]
[0030] [Figure 1] FIG. 1 is a partial schematic cross-sectional view illustrating one embodiment of a laminate forming a packaging bag according to the present invention. [Diagram 2] FIG. 2 is a partial schematic cross-sectional view illustrating Example 1, which shows another embodiment of the laminate forming the packaging bag according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] The invention will now be described in more detail with reference to the drawings, in which: The invention is not limited to the examples shown, but is defined by the claims.
[0032] FIG. 1 is a partial schematic cross-sectional view illustrating one embodiment of a laminate forming a packaging bag according to the present invention.
[0033] The packaging bag according to the present invention is a packaging bag capable of storing, as its contents, a hair coloring agent that contains, in particular, monoethanolamine.
[0034] This packaging bag is made by making a laminate (10) using a plastic film as a base material. Generally, hair coloring agents discolor when exposed to oxygen, and metals are corroded by strong alkali, which can cause pinholes and the associated discoloration and poor appearance, so the laminate (10) is required to have special resistance and material composition that is suited to the contents.
[0035] In the present invention, the laminate (10) is configured by sequentially laminating a base film layer (1), a gas barrier layer (2), a surface modification layer (3), an extruded resin layer (4), and a sealant layer (5) from the outside of the packaging bag, characterized in that the base film layer (1) is made of polybutylene terephthalate resin, and the gas barrier layer (2) is made of metal foil.
[0036] The present invention is also characterized in that the loop stiffness strength of the laminate (10) is 100 mN or less. In other words, the laminate (10) has resistance to the contents and at the same time has flexibility, making it possible to provide a packaging bag that is suitable for use with a filling machine.
[0037] By using polybutylene terephthalate for the base film layer (1), which has an SP value different from that of monoethanolamine, the main component of the contents, and which has excellent mechanical strength and resistance to the occurrence of pinholes, it is possible to reduce the thickness of the laminate (10) without compromising the resistance to the contents, thereby improving the flexibility of the packaging bag and improving its suitability for filling machines.
[0038] In particular, the base film layer can be a biaxially oriented polybutylene terephthalate resin having a thickness of 15 μm or more and 25 μm or less. In this case, the flexibility of the laminate (10) can be ensured, and it is possible to achieve both resistance to the contents and suitability for filling machines without adversely affecting suitability for filling machines, and to further improve storage suitability after filling.
[0039] The base film layer (1) and the gas barrier layer (2) can be laminated together, for example, via an adhesive layer.
[0040] In addition, since the gas barrier layer (2) is made of metal foil, a high level of gas barrier properties can be ensured, while by using polybutylene terephthalate for the base film layer (1) as described above, it is possible to achieve both the prevention of pinholes and suitability for filling machines.
[0041] In particular, the gas barrier layer (2) can be a foil made of aluminum or an aluminum alloy having a thickness of 5 μm or more and 50 μm or less. In this case, it is more effective to achieve both flexibility and gas barrier properties of the laminate (10).
[0042] In the present invention, the surface modification layer (3) is composed of an inorganic coating containing Zr, Cr or a salt thereof and an organic polymer coating covering the inorganic coating. The gas barrier layer (2) is made of a metal foil, and the surface modification layer (3) is provided on the surface of the metal foil of the gas barrier layer (2) to improve adhesion with the extruded resin layer (4) and the sealant layer (5) and at the same time to improve the interlayer strength of the laminate (10).
[0043] The extruded resin layer (4) may be a thermoplastic polyethylene resin having a thickness of 15 μm or more and 30 μm or less, and this extruded resin layer (4) is effective for improving adhesion when laminating the sealant layer (5). In this case, an adhesive layer can be provided between the surface modification layer (3) of the gas barrier layer (2) and the extruded resin layer (4), which is effective for improving the interlayer strength of the entire laminate (10).
[0044] The extruded resin layer (4) may be formed by extruding low-density polyethylene or maleic anhydride-grafted polyethylene, or by co-extrusion of low-density polyethylene and maleic anhydride-grafted polyethylene, with a thickness of 10 μm or more and 35 μm or less. In this case, it is possible to form the extruded resin layer (4) and configure the laminate (10) for forming the packaging bag without providing an adhesive layer on the surface modification layer (3) of the gas barrier layer (2).
[0045] The sealant layer (5) may have a thickness of 20 μm or more and 100 μm or less. In this case, it is effective in achieving both the flexibility and filling suitability of the laminate (10) while ensuring sufficient sealing properties.
[0046] The sealant layer (5) enables two laminates (10) to be laminated together with the sealant layers (5) facing each other, and then bonded together by applying heat and pressure to heat seal, thereby forming a packaging bag.
[0047] As the material for the sealant layer (5), polyolefin-based resins, which are thermoplastic resins, are generally used. Specifically, ethylene-based resins such as low-density polyethylene resin (LDPE), medium-density polyethylene resin (MDPE), linear low-density polyethylene resin (LLDPE), ethylene-vinyl acetate copolymer (EVA), ethylene-α-olefin copolymer, and ethylene-methacrylic acid resin copolymer; blend resins of polyethylene and polybutene; and polypropylene-based resins such as homopolypropylene resin (PP), propylene-ethylene random copolymer, propylene-ethylene block copolymer, and propylene-α-olefin copolymer can be used.
[0048] The sealant layer 10 can be formed by forming a film of molten resin using an extruder or the like to form a layer on the laminate 10. Alternatively, a sealant layer can be formed on the surface of the laminate 10 by laminating a material that has already been formed into a film state.
[0049] If necessary, in order to improve the image of the product, to display necessary information about the contents, and to improve the design, a printed layer can be provided on a layer that is visible from the outside of the packaging bag in the laminate (10) based on a plastic film. The printed layer may be provided on the outermost layer of the packaging bag.
[0050] There are no particular restrictions on the printing method and printing ink, and any suitable method may be selected from known printing methods taking into consideration printability on plastic films, design such as color tone, adhesion, safety, and the like.
[0051] For example, a printing method can be selected from known printing methods such as gravure printing, offset printing, gravure offset printing, flexographic printing, silk screen printing, inkjet printing, etc. Among them, gravure printing is preferably used in terms of productivity, printability on plastic films, and high definition of patterns.
[0052] If necessary, the laminate (10) may be provided with a printed layer, and a substrate having a light-shielding layer may be laminated thereto.
[0053] In this way, according to the present invention, it is possible to provide a packaging bag capable of storing a hair color agent as the content, which has gas barrier properties, resistance to strong base-resistant contents, and flexibility as a packaging bag. EXAMPLES
[0054] The present invention will be described in more detail below with reference to Examples 1 and 2 and Comparative Examples 1 to 3. However, the present invention is not limited to the examples shown here. The present invention is defined by the claims.
[0055] A laminate having a barrier property was prepared, and a substrate having a light-shielding layer was laminated with a urethane adhesive to be evaluated as a sample. Also, a packaging bag was prepared using this, and the contents were filled and evaluated.
[0056] The evaluation items are as follows: Pinhole resistance evaluation Loop stiffness strength evaluation · Content resistance evaluation The evaluation methods for each evaluation item are as follows.
[0057] Pinhole resistance evaluation The test was performed using a Gelbo Flex Tester (manufactured by Tester Sangyo Co., Ltd.) at room temperature, 1000 times, and the number of pinholes that occurred was counted.
[0058] Loop Stiffness Strength Evaluation Using a loop stiffness tester (manufactured by Toyo Seiki Seisakusho Co., Ltd.), the strength was confirmed under the conditions of width 15 mm, circumference 50 mm, and push-in depth 10 mm.
[0059] Content resistance evaluation Two rectangular samples were stacked with the sealant facing each other, and three sides were sealed to make a three-sided bag. The contents were filled with hair color agent 1 (main ingredient: monoethanolamine, SP value 16.3) with a pH of 9 to 10, and the bag was sealed. This sample was bent 100 times in a room temperature environment, then stored in a thermostatic chamber at 50°C, and after two weeks it was taken out and its appearance was observed.
[0060] <Example 1> FIG. 2 is a partial schematic cross-sectional view illustrating Example 1, which shows another embodiment of the laminate forming the packaging bag according to the present invention.
[0061] The laminate (10) having barrier properties has the following structure. Starting from the outside of the packaging bag, Base film layer (1) Polybutylene terephthalate film (Boblet (registered trademark) ST, thickness 15 μm, manufactured by Kohjin Film & Chemicals Co., Ltd.) Adhesive layer (7) Urethane adhesive (main agent: Takelac (registered trademark) A525 manufactured by Mitsui Chemicals, Inc., hardener: Takenate (registered trademark) A50 manufactured by Mitsui Chemicals, Inc.) Gas barrier layer (2) Aluminum foil (Toyo Aluminum Co., Ltd., 8079 material, thickness 9 μm) Surface modification layer (3) Zr-based coating agent (Surfcoat (registered trademark) EC1000A / B manufactured by Nippon Paint Surf Chemicals Co., Ltd.) Adhesive layer (6) Adhesive mainly composed of biuret type hexamethylene diisocyanate / Extrusion resin layer (4) Low density polyethylene (LC600A manufactured by Japan Polyethylene Co., Ltd.) · Sealant layer (5) Linear low-density polyethylene resin (LL-MTNST manufactured by Futamura Chemical Co., Ltd.) A laminate having the following layer structure was prepared. Furthermore, a substrate having a light-shielding layer was attached to this laminate using a urethane adhesive.
[0062] <Example 2> In comparison with Example 1, instead of the adhesive layer (6) and the extrusion resin layer (4), maleic anhydride grafted polyethylene (manufactured by Mitsubishi Chemical Corporation, melting point peak: 98°C, density 0.88 g / cm 3 The same procedure as in Example 1 was repeated, except that a co-extrusion layer of polyethylene (MFR: 10 g / 10 min) and low-density polyethylene resin (LC600A manufactured by Japan Polyethylene Corporation) was formed, and after extrusion lamination, the laminated film was heated at 140° C. for 15 seconds with a heater roll to produce a laminated film.
[0063] <Comparative Example 1> The procedure was the same as in Example 1, except that a polyethylene terephthalate film (FE2001, manufactured by Futamura Chemical Co., Ltd., thickness 12 μm) was used as the base film layer (1).
[0064] <Comparative Example 2> The procedure was the same as in Example 1, except that a stretched polyamide film (Bonyl (registered trademark) RX, thickness 15 μm, manufactured by Kojin Film & Chemicals Co., Ltd.) was used as the base film layer (1).
[0065] <Comparative Example 3> The same procedure as in Example 1 was repeated except that a polyethylene terephthalate film (FE2001, 12 μm thick, manufactured by Futamura Chemical Co., Ltd.) was used as the base film layer (1) and a stretched polyamide film (Bonyl (registered trademark) W, 15 μm thick, manufactured by Kojin Film & Chemicals Co., Ltd.) was laminated as an intermediate base layer between the base film layer (1) and the gas barrier layer (2).
[0066] The evaluation results are shown in Table 1.
[0067] [Table 1]
[0068] As can be seen from Table 1, both Example 1 and Example 2 according to the present invention showed a smaller number of pinholes than Comparative Examples 1 to 3 in the pinhole resistance evaluation.
[0069] In addition, in the loop stiffness evaluation, the values satisfied the limit of 100 mN or less specified in the present invention in both Example 1 and Example 2. This provides the laminate with flexibility and makes it suitable for use in a filling machine.
[0070] These are considered to be due to the effect of using the polybutylene terephthalate film (Boblet (registered trademark) ST, thickness 15 μm, manufactured by Kohjin Film & Chemicals Co., Ltd.) specified in the present invention as the base film layer (1).
[0071] In Comparative Example 1, a polyethylene terephthalate film (FE2001, 12 μm thick, manufactured by Futamura Chemical Co., Ltd.) was used for the base film layer (1), which is outside the range specified in the present invention, and as a result, the pinhole resistance was poor.
[0072] In Comparative Example 2, a stretched polyamide film (Bonyl (registered trademark) RX, thickness 15 μm, manufactured by Kojin Film & Chemicals Co., Ltd.) was used for the base film layer (1), exceeding the range specified in the present invention. Since the SP value was close to monoethanolamine, which is the main component of the contents, partial discoloration (brown spots) was observed after storage at 50°C in the content resistance evaluation, which is problematic in practical use as a packaging bag.
[0073] In Comparative Example 3, a polyethylene terephthalate film (FE2001, thickness 12 μm, manufactured by Futamura Chemical Co., Ltd.) was used as the base film layer (1), and a stretched polyamide film (Bonyl (registered trademark) W, thickness 15 μm, manufactured by Kojin Film & Chemicals Co., Ltd.) was laminated as an intermediate base layer between the base film layer (1) and the gas barrier layer (2). As a result, the thickness of the entire laminate increased and the loop stiffness strength was larger than the 100 mN or less specified in the present invention, resulting in poor flexibility and a risk of not being suitable for use in filling machines, etc. as a packaging bag.
[0074] In this way, it has been verified that the present invention makes it possible to provide a packaging bag capable of storing a hair color agent as a content, which has gas barrier properties, resistance to strong base-resistant contents, and flexibility as a packaging bag. [Explanation of symbols]
[0075] 1. Base film layer 2. Gas barrier layer 3. Surface modification layer 4. Extrusion resin layer 5. Sealant layer 6...Adhesive layer 7...Adhesive layer 10...Laminate
Claims
1. A packaging bag capable of storing a hair color agent containing monoethanolamine as a content, The packaging bag is formed by making a laminate using a plastic film as a base material, The laminate is configured by laminating, from the outside of the packaging bag, a base film layer, a first adhesive layer, a gas barrier layer, a surface modification layer, a second adhesive layer, an extrusion resin layer, and a sealant layer in this order, The base film layer is a single layer made of a biaxially oriented polybutylene terephthalate resin having a thickness of 15 μm or more and 25 μm or less, The gas barrier layer is made of a metal foil, The loop stiffness strength of the laminate is 100 mN or less, the first adhesive layer is a layer formed of a urethane adhesive and bonds the base film layer and the gas barrier layer; The second adhesive layer is a layer formed of an adhesive containing hexamethylene diisocyanate, and adheres the surface modification layer and the extrusion resin layer to each other; The packaging bag is characterized in that the extruded resin layer has a thickness of 10 μm or more and 35 μm or less and is formed by extrusion of maleic anhydride grafted polyethylene or by co-extrusion of low-density polyethylene and maleic anhydride grafted polyethylene.
2. 2. The packaging bag according to claim 1, wherein the surface modification layer comprises an inorganic coating containing Zr, Cr or a salt thereof, and an organic polymer coating covering the inorganic coating.
3. 3. The packaging bag according to claim 1, wherein the gas barrier layer is a foil made of aluminum or an aluminum alloy having a thickness of 5 μm or more and 50 μm or less.
4. The packaging bag according to any one of claims 1 to 3, wherein the sealant layer has a thickness of 20 µm or more and 100 µm or less.
Citation Information
Patent Citations
JP1980084970A
Packaging bag
JP2001240085A
Hair dye packaging bag
JP2003081285A
Laminated packaging bag having superior pinhole resistance
JP2005096791A
Packing bag
JP2015048142A