Laminate for tube container and tube container

The laminate structure for tube containers, with a paper base, barrier, and sealant layers, and an adhesive coat, addresses the issue of lacking paper texture by ensuring high peel strength and barrier properties, improving the overall feel and functionality.

JP7567329B2Active Publication Date: 2024-10-16DAI NIPPON PRINTING CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020164565
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-30
Publication Date
2024-10-16
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

Conventional tube containers with plastic-based laminates fail to adequately express the texture of paper due to thermoplastic resin sealant layers on the outermost surface, which compromises the paper feel.

Method used

A laminate structure for tube containers is designed with a paper base layer, barrier layer, and sealant layer, featuring an easily adhesive coat layer on the outer surface, and a joining tape on both inner and outer surfaces to enhance adhesion and maintain paper texture.

Benefits of technology

The laminate structure effectively expresses the paper texture while ensuring high peel strength and side seam strength, maintaining oxygen barrier properties and adhesion, thus enhancing the overall feel and functionality of the tube container.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567329000002
    Figure 0007567329000002
  • Figure 0007567329000003
    Figure 0007567329000003
  • Figure 0007567329000004
    Figure 0007567329000004
Patent Text Reader

Abstract

To provide a laminate for a tube container in which feeling of paper is expressed sufficiently; and to provide a tube container using such a laminate.SOLUTION: In a laminate 10 used for a trunk 31 of a tube container 30 by laminating at least a paper base material layer 13, a barrier layer 14 and a sealant layer 15 in due order from the outer surface side, and by butting the end faces, an easy adhesive coat layer 12 is formed on at least a part on the outer surface side of the paper base material layer 13.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a laminate for a tube container and a tube container, and in particular to a laminate and a tube container that make use of the texture and feel of paper. [Background technology]

[0002] Conventionally, laminates used in tube containers have a structure in which a base layer is provided between sealant layers used on the outer and inner surfaces. A resin film is used as the base layer because it satisfies mechanical, physical, chemical and other suitability requirements (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2005-178851 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, it has been recommended to reduce the amount of plastic (synthetic resin) used in consideration of the environment. In order to reduce the amount of plastic used, paper base materials are being used in the laminated body of tube containers as well. Meanwhile, in tube containers, in order to prevent the contents from seeping out and to maintain the strength of the cylindrical body, a sealant layer is provided on the outermost and innermost surfaces of the laminate, and both ends of the laminate are overlapped and heat sealed to form the body. The body formed in this way does not fully express the texture of paper because a sealant layer, which is a thermoplastic resin, is present on the outermost surface.

[0005] Therefore, an object of the present disclosure is to provide a laminate for a tube container that fully expresses the texture of paper, and a tube container using such a laminate. [Means for solving the problem]

[0006] In order to solve the above problems, the present disclosure provides: A laminate in which at least a paper base layer, a barrier layer, and a sealant layer are laminated in this order from the outer surface side, and the end faces are butted together to be used for the body part of a tube container, The present invention provides a laminate in which an easy-adhesion coating layer is formed on at least a part of the outer surface side of the paper base layer.

[0007] In addition, the laminate of the present disclosure is A printed portion may be formed on the outer surface of the paper base layer, and the easy-adhesion coating layer may be formed at a position that does not overlap the printed portion.

[0008] In addition, the laminate of the present disclosure is The easy-adhesion coating layer may contain polyethyleneimine.

[0009] The present disclosure also provides The tube container has a body portion in which both ends of the laminate are butted together and joined on both the inner and outer surfaces of the laminate with joining tape so as to cover the both ends.

[0010] In addition, the tube container of the present disclosure is The tube container may have a side seam strength of 80N / 15mm or more.

[0011] In addition, the tube container of the present disclosure is The easy-adhesion coating layer may be formed at a position including an area overlapping with the bonding tape.

[0012] In addition, the tube container of the present disclosure is The peel strength between the body and the shoulder joined to the body may be 40N / 15mm or more. Effect of the Invention

[0013] According to the present disclosure, it is possible to provide a laminate for a tube container that fully expresses the texture of paper, and a tube container using such a laminate. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a front view (partial cross-sectional view) of the tube container with the cap attached. [Diagram 2] This is a partial cross-sectional view of a packaged product of a tube container containing a content. [Diagram 3] FIG. 2 is a diagram showing a cylindrical body portion of a tube container according to an embodiment of the present disclosure. [Figure 4] 1 is a partial cross-sectional view of a portion where both ends 33A, 33B of cylindrical body 31 are butted together, as viewed from the axial direction of cylindrical body 31. FIG. [Diagram 5] FIG. 2 is a cross-sectional view of a laminate of a body portion of a tube container according to one embodiment of the present disclosure. [Figure 6] FIG. 2 is a cross-sectional view of a joining tape used in a tube container according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, preferred embodiments of the present disclosure will be described in detail with reference to the drawings. However, the present disclosure is not limited to these specifically exemplified forms or various specifically described structures. In each drawing, the size and ratio of the members may be changed or exaggerated for ease of understanding. In addition, for ease of viewing, unnecessary parts for explanation and repeated reference symbols may be omitted.

[0016] In this specification, the terms "outer surface" and "inner surface" refer to the "outer surface" and "inner surface" when a tube container 30 is produced using the laminate 10. Additionally, the terms "upper side" and "lower side" refer to the side of the mouth 36 when the tube container 30 is held with the mouth 36 and the cap 20 facing upward, and the terms "lower side" refer to the opposite side of the mouth 36 (the 34B side in FIG. 1 and the 39 side in FIG. 2).

[0017] Fig. 1 is a partial cross-sectional view of a tube container according to this embodiment with a cap attached. Fig. 2 is a partial cross-sectional view of a packaged product of a tube container containing a content. As shown in Fig. 1, a tube container 30 according to this embodiment includes a body 31 formed of a laminate 10, and a head molded body 37 produced by providing a synthetic resin to the body 31 by a method such as compression molding or injection molding. The head molded body 37 further includes a shoulder portion 35 and a mouth portion 36. A cap 20 is attached to the mouth portion 36 of the tube container 30.

[0018] The tube container 30 has a head molded body 37 composed of a cylindrical mouth 36 including an opening for discharge, and a truncated cylindrical shoulder 35 connected to the mouth 36 and expanding in circumference toward the lower side. In FIG. 1, the right half shows the front of the head molded body 37, and the left half shows a cross section parallel to the front through the radial center. The hatched portion in the left half of FIG. 1 shows the actual body of the head molded body 37, and the blank portion is a cavity. The shoulder 35 is configured, for example, in a truncated cone shape that expands radially outward of the tube container 30 as it moves away from the mouth 36. For example, the shoulder 35 has an inclination of 30 degrees with respect to the horizontal. The shoulder 35 is connected to the body 31 on the lower side.

[0019] The generally cylindrical mouth 36 has a helical convex portion on its outer surface that functions as a screw thread. The inner circumferential surface of the mouth 36 defines an opening. The opening of the mouth 36 serves as a discharge port for discharging the contents 38. The contents contained in the body 31 are discharged from the tube container 30 by passing through the opening. The head molded body 37 has the above-described structure, and can be detached by screwing it onto the cap 20 having a screw groove on the inside.

[0020] The body 31 is a film-like laminate formed into a cylindrical shape. One end of the body 31 extending cylindrically is joined to a shoulder 35. Meanwhile, the other end of the body 31 is sealed by a bottom seal 39 formed by overlapping and joining the inner surfaces of the cylindrical body 31 (see FIG. 2). The bottom seal 39 may be joined after the body 31 is filled with the contents 38. The body 31 of the tube container 30, in particular, may be configured to have flexibility (softness, squeezability) that allows a desired amount of contents to be easily pushed out even if the contents have some viscosity. The dimensions of the body 31 may be appropriately designed depending on the type of contents, and may be, for example, 40 mm in diameter.

[0021] The tube container 30 having the above-mentioned configuration is obtained through the following manufacturing process. First, as shown in FIG. 3, a pair of ends 33A, 33B of the laminate 10 are butted together using the laminate 10. Then, a joining tape 60 is heat-sealed and joined to the outer and inner surfaces of the butted parts to form a body-attached part 32 (also called a side seam part). In this manner, a cylindrical body part 31 is manufactured. The part joined by the joining tape 60 becomes the body-attached part 32 of the body part 31. The heat sealing method can be a conventionally known method such as bar sealing, rotary roll sealing, belt sealing, impulse sealing, high-frequency sealing, ultrasonic sealing, and flame sealing.

[0022] 4 is a view of the portion where both ends 33A and 33B in FIG. 3 are butted together, as viewed from the axial direction of the cylindrical body 31. FIG. 4(a) shows a case where both ends 33A and 33B of the laminate 10 are formed perpendicular to the surface of the laminate 10, and FIG. 4(b) shows a case where both ends 33A and 33B of the laminate 10 are formed obliquely to the surface of the laminate 10. In FIG. 4, for convenience of explanation, the laminate 10 constituting the body 31 is shown as a four-layer structure of an easy-adhesion coating layer 12, a paper base layer 13, a barrier layer 14, and a sealant layer 15. As shown in FIG. 4(a) and (b), the joining mode differs depending on the mode of both ends 33A and 33B, but in either case, a joining tape 60 is arranged so as to cover the portion where both ends 33A and 33B of the laminate 10 are in contact, and heat-sealed, thereby joining both ends 33A and 33B. At this time, the outer surface side (the paper base layer 13 side) is heat sealed via the easy-adhesion coating layer 12.

[0023] Next, the cylindrical body 31 shown in Fig. 3 is placed in a mold (not shown), and a head molded body 37 (shoulder part 35, mouth part 36) is formed at one opening (upper side) 34A of the body 31 by a method such as compression molding or injection molding. In this way, the head molded body 37 (shoulder part 35, mouth part 36) is integrally molded at one opening (upper side) 34A of the body 31, and the tube container 30 is produced. Then, as shown in Fig. 1, the cap 20 is attached to the mouth part 36 side of the tube container 30.

[0024] Next, an appropriate amount of contents 38, such as hand cream, sunscreen, toothpaste, or other contents, is filled into the tube container 30 from the other opening (lower side) 34B of the cylindrical body 31 shown in Fig. 1. The opening (lower side) 34B is then welded to form a bottom seal 39. As a result, a packaged product 30A including the tube container 30 filled and packaged with the contents 38 is obtained, as shown in Fig. 2.

[0025] The details of the head molded body 37 will be further described. The head molded body 37 is made of a material that can be molded so that the mouth portion 36 and the shoulder portion 35 have appropriate hardness, has high adhesion to the material of the body portion 31, does not affect the quality of the contents, and does not cause hygienic problems even if it comes into contact with the contents. As such a material, a thermoplastic resin is used for the head molded body 37, and more specifically, high density polyethylene (HDPE) is used.

[0026] Furthermore, the head molding 37 may be made of polyolefin resins such as low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, polypropylene (homopolypropylene, block polypropylene, random polypropylene), copolymers of olefins with copolymerizable monomers such as vinyl monomers, acrylic monomers, unsaturated carboxylic acids, or blends thereof, or resins in which the above-mentioned resins are blended with high-density polyethylene. Furthermore, from the viewpoint of heat resistance and thermal adhesion to the body 31, it is preferable to use a resin in which high-density polyethylene is blended with linear low-density polyethylene for the head molding 37. Furthermore, a truncated cone-shaped cylinder may be laminated as a barrier material to prevent the permeation of gases such as oxygen, particularly on the shoulder 35 of the head molding 37. The shoulder 35 may contain a plant-derived resin.

[0027] The high density polyethylene used to form the shoulder 35 of the head molded body 37 may be derived from fossil raw materials, but biomass-derived high density polyethylene, known as a carbon neutral material, may be used to reduce the environmental impact. Since the head and cap account for a large mass ratio of the tube container, by molding the head molded body 37 using biomass-derived high density polyethylene, the amount of fossil raw materials used for the entire tube container can be reduced, thereby reducing the environmental impact. In addition, the head molded body 37 of the tube container 30 is comparable in terms of physical properties such as mechanical properties to heads manufactured from conventional raw materials obtained from fossil raw materials, so it can replace conventional heads.

[0028] From the viewpoint of reducing the environmental load, it is preferable to use only biomass-derived polyethylene, but a blend of fossil-derived polyethylene and biomass-derived polyethylene may be used in consideration of production costs, etc. Here, biomass-derived polyethylene is a monomer polymer containing biomass-derived ethylene. Since biomass-derived ethylene is used as the raw material monomer, the polymerized polyethylene is derived from biomass. The content of biomass-derived ethylene in the raw material monomer does not need to be 100% by mass, and is, for example, preferably 10% by mass or more, more preferably 30% by mass or more.

[0029] The raw material monomer may contain ethylene derived from fossil raw materials, or may contain α-olefin monomers such as butylene, hexene, and octene. Even in such a case, the obtained polymer is called biomass polyethylene. When using biomass-derived polyethylene, it may contain two or more polyolefins with different biomass degrees. When blending fossil-derived polyethylene and biomass-derived polyethylene, the mixing method is not particularly limited, and dry blending or melt blending may be used. When mixing the two, the mixing ratio of fossil-derived polyethylene and biomass-derived polyethylene is preferably 1:9 to 9:1 in mass ratio, more preferably 2:8 to 8:2.

[0030] For example, biomass-derived ethylene can be produced using biomass-derived ethanol as a raw material. In particular, it is preferable to use biomass-derived fermented ethanol obtained from a plant raw material. In other words, it is preferable to use a plant-derived resin. The plant raw material is not particularly limited, and any conventionally known plant can be used. Examples include corn, sugarcane, beet, and manioc.

[0031] In the present disclosure, fermented ethanol derived from biomass refers to ethanol produced by contacting a culture solution containing a carbon source obtained from a plant raw material with an ethanol-producing microorganism or a product derived from its crushed material, and then purifying the ethanol. Conventionally known methods such as distillation, membrane separation, and extraction can be applied to purify ethanol from the culture solution. For example, methods include adding benzene, cyclohexane, etc., and removing water by azeotropy or membrane separation, etc.

[0032] The thickness of the head molded body 37 using such resins is preferably 0.5 mm or more and 2.0 mm or less. In this embodiment, the head molded body 37 is produced by compression molding. Therefore, in the head molded body 37, which is a compression molded product, it is possible to prevent the occurrence of depressions, so-called sink marks, caused by shrinkage during molding, even in thick parts such as the top surface. Furthermore, it is possible to reduce waste of material such as in the gate portion. The head molded body 37 may also be produced by injection molding.

[0033] Next, the laminate 10 forming the cylindrical body 31 will be described with reference to Fig. 5. The laminate 10 forming the body 31 of the tube container 30 is a laminate having an easy-adhesion coating layer 12, a paper base layer 13, an adhesive layer 16, a barrier layer 14, and a sealant layer 15, which are arranged in this order from the outer surface to the inner surface, as shown in Fig. 5. The thicknesses of the paper base layer 13, the adhesive layer 16, the barrier layer 14, and the sealant layer 15 are different in reality, but are shown as the same thickness in Fig. 5 for convenience. In addition, each layer can also be bonded by dry lamination using an adhesive, but the adhesive layer formed during bonding by dry lamination is thinner than the other layers and is therefore not shown.

[0034] The easy-adhesion coating layer 12 is formed on a part or the entire surface of the paper base layer. The easy-adhesion coating layer 12 may be formed on the entire surface, but it is sufficient that it is formed only in the range corresponding to the bonding tape 60. In this embodiment, the easy-adhesion coating layer 12 is formed at a position including the range overlapping with the bonding tape 60. Specifically, the easy-adhesion coating layer 12 is formed only in the range of WE (mm) from both ends 33A, 33B. When the width of the bonding tape 60 is WT (mm), it is preferable that WE≧WT / 2. By WE≧WT / 2, the easy-adhesion coating layer 12 is present on the entire surface of the bonding tape 60, and the adhesion at the body attachment portion 32 is improved. In this embodiment, WE=(WT / 2+1). As a result, when the bonding tape 60 is attached at an accurate position, the entire bonding tape 60 is included in the formation position of the easy-adhesion coating layer 12, and the easy-adhesion coating layer 12 remains at 1 mm on both sides of the bonding tape 60. The range in which the easy-adhesion coating layer 12 is formed from both ends 33A, 33B may be different between both ends 33A, 33B. In order to further increase the adhesion with the bonding tape, it is preferable that the easy-adhesion coating layer 12 is formed at a position that does not overlap with the outer surface printed portion 13A.

[0035] On the outer surface of the paper base layer 13, an outer surface printed portion 13A including a desired pattern is formed using printing ink. The easy-adhesion coating layer 12 is formed by applying an easy-adhesion coating agent to the outer surface of the paper base layer 13 and drying it. The easy-adhesion coating layer 12 is formed by applying the easy-adhesion coating agent to the paper base layer 13 by, for example, roll coating, gravure coating, knife coating, dip coating, spray coating, or other coating methods, and drying the coating film. Alternatively, it may be formed in the same process as the outer surface printed portion 13A. The easy-adhesion coating layer 12 can also be applied by flexographic printing when the smoothness of the paper used for the paper base layer 13 is insufficient.

[0036] The paper base layer 13 and the barrier layer 14 are joined by an adhesive layer 16 formed by extrusion lamination. The barrier layer 14 and the sealant layer 15 are joined by extrusion lamination (adhesive layer 16: not shown) or dry lamination. When the barrier layer 14 and the sealant layer 15 are laminated by extrusion lamination, the barrier layer 14 and the sealant layer 15 are made compatible with the extruded resin, thereby maintaining the resistance to contents.

[0037] When overlapping both ends 33A, 33B and joining the first sealant layer on the outermost surface and the second sealant layer on the innermost surface by heat sealing, the first sealant layer on the outermost surface is required, but when butting both ends 33A, 33B together and covering them with joining tape 60, the first sealant layer on the outermost surface is not required and only the sealant layer on the innermost surface is sufficient.

[0038] When two layers are bonded by dry lamination, an adhesive layer can be formed by applying an adhesive to the surface of the layer to be laminated and drying it. As the adhesive, for example, one-component or two-component curing or non-curing type vinyl, (meth)acrylic, polyamide, polyester, polyether, polyurethane, epoxy, rubber, and other solvent-based, water-based, or emulsion-based adhesives can be used. As a two-component curing type adhesive, a cured product of polyol and an isocyanate compound can be used. As a coating method of the above-mentioned adhesive for lamination, for example, it can be applied to the coating surface of the layer constituting the laminate by a direct gravure roll coating method, a gravure roll coating method, a kiss coating method, a reverse roll coating method, a Fountain method, a transfer roll coating method, or other methods.

[0039] Thermoplastic resins used for extrusion lamination include polyethylene resins, polypropylene resins, cyclic polyolefin resins, copolymer resins, modified resins, or mixtures (including alloys) that mainly contain these resins. Examples of polyolefin resins include the above-mentioned polyethylene, polypropylene (PP), ethylene-α-olefin copolymers polymerized using a metallocene catalyst, random or block copolymers of ethylene and polypropylene, ethylene-vinyl acetate copolymers (EVA), ethylene-acrylic acid copolymers (EAA), ethylene-ethyl acrylate copolymers (EEA), ethylene-methacrylic acid copolymers (EMAA), ethylene-methyl methacrylate copolymers (EMMA), ethylene-maleic acid copolymers, ionomer resins, and acid-modified polyolefin resins obtained by modifying the above-mentioned polyolefin resins with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, fumaric acid, and itaconic acid to improve adhesion between layers.

[0040] In addition, resins obtained by graft-polymerizing or copolymerizing unsaturated carboxylic acids, unsaturated carboxylic anhydrides, and ester monomers can be used as polyolefin resins. These materials can be used alone or in combination of two or more. As cyclic polyolefin-based resins, for example, cyclic polyolefins such as ethylene-propylene copolymers, polymethylpentene, polybutene, and polynorbornene can be used. These resins can be used alone or in combination of two or more. In addition, as the above-mentioned polyethylene-based resins, those using the above-mentioned biomass-derived ethylene as a monomer unit can be used to further improve the biomass degree.

[0041] When the adhesive layer 16, which is an adhesive resin layer, is laminated by extrusion lamination, an anchor coat (AC) layer formed by applying and drying an anchor coat agent on the surface of the layer to be laminated may be provided. The anchor coat agent may be any resin having a heat resistance temperature of 135° C. or higher, such as an anchor coat agent made of vinyl modified resin, epoxy resin, urethane resin, polyester resin, polyethyleneimine, etc. In particular, an anchor coat agent which is a cured product of a polyacrylic or polymethacrylic resin (polyol) having two or more hydroxyl groups in its structure and an isocyanate compound as a curing agent can be preferably used. A silane coupling agent may be used in combination with this as an additive. Nitrocellulose may also be used in combination to improve heat resistance. For example, "EL-510" manufactured by Toyo-Morton Co., Ltd. may be used as the anchor coat agent. For example, "RT-80" manufactured by Toyo-Morton Co., Ltd. may be used as the curing agent.

[0042] The anchor coat layer after drying has a thickness of 0.1 μm to 1 μm, preferably 0.3 μm to 0.5 μm. The adhesive layer after drying has a thickness of preferably 1 μm to 10 μm, preferably 2 μm to 5 μm. The adhesive resin layer has a thickness of preferably 5 μm to 50 μm, preferably 10 μm to 30 μm.

[0043] Next, the materials of each part constituting the laminate 10 of the cylindrical body portion 31 will be described. The easy-adhesion coating layer 12 may be any material that facilitates adhesion between the bonding tape 60 and the paper base layer 13, and may be, for example, an adhesive based on polyethyleneimine, vinyl acetate resin, ethylene-vinyl acetate copolymer resin, or an aqueous dispersion of modified polyolefin resin. An example of an adhesive based on ethylene-vinyl acetate copolymer resin is "Seikadyne" manufactured by Dainichiseika Chemicals Mfg. Co., Ltd. An example of an aqueous dispersion of modified polyolefin resin is Arrowbase (registered trademark) manufactured by Unitika Ltd.

[0044] Moreover, unbleached kraft paper, bleached kraft paper, cup base paper, parchment paper, or coated paper can be used as the paper base layer 13, and an outer surface printed portion 13A made of printing ink can be provided on the paper base layer 13 by printing on the paper base layer 13. The paper base layer 13 also maintains the rigidity and light-blocking properties of the tube container.

[0045] As the barrier layer 14, an appropriate one is selected according to the required functions, such as the barrier property against water vapor and other gases, and an ethylene-vinyl alcohol copolymer film, a vapor deposition film, or a metal foil can be used. When a metal foil is used as the barrier layer 14, various metal foils having barrier properties, such as copper and tin, can be used, but it is preferable to use an aluminum foil.

[0046] When a vapor-deposited film is used as the barrier layer 14, the base film of the vapor-deposited film may be polyethylene terephthalate (PET), nylon, or the like. As the metal to be vapor-deposited on the base film, various materials generally used for metal vapor deposition, such as copper and tin, may be used. Also, a vapor-deposited film of a metal oxide such as aluminum oxide or an inorganic oxide such as silicon oxide may be provided.

[0047] When a vapor-deposited film is used as the barrier layer 14, a PET layer having a metal vapor-deposited film on at least one side and gas barrier properties may be used, or a nylon layer having a metal vapor-deposited film on at least one side and gas barrier properties may be used.

[0048] Also, a PET layer having a vapor-deposited silica film on at least one surface thereof and thus having gas barrier properties may be used, or a nylon layer having a vapor-deposited silica film on at least one surface thereof and thus having gas barrier properties may be used.

[0049] Also, a PET layer having an aluminum oxide vapor deposition film on at least one surface thereof and thus having gas barrier properties may be used, or a nylon layer having an aluminum oxide vapor deposition film on at least one surface thereof and thus having gas barrier properties may be used.

[0050] When a nylon layer is used, the mechanical strength is often superior to that of a PET layer. In addition, a film provided with various deposition films has superior gas barrier properties to a film serving as a base material. Furthermore, a gas barrier coating film may be provided on the deposition film. This suppresses the permeation of oxygen and water vapor, and by providing the coating film adjacent to the deposition film, the occurrence of cracks in the deposition film can be effectively prevented. The gas barrier coating film is a gas barrier coating film containing at least one resin composition such as a hydrolyzate of a metal alkoxide or a hydrolyzed condensate of a metal alkoxide obtained by polycondensing a mixture of a metal alkoxide and a water-soluble polymer by a sol-gel method in the presence of a sol-gel catalyst, water, an organic solvent, and the like.

[0051] The sealant layer 15 may contain, for example, polyethylene (PE). Specifically, the sealant layer 15 may be made of the following materials. The sealant layer 15 may be made of any material that can be melted by heat and mutually fused with the bonding layer of the bonding tape 60. For example, low-density polyethylene (LDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), linear low-density polyethylene (LLDPE), polypropylene (PP), ethylene-vinyl acetate copolymer, ionomer resin, ethylene-ethyl acrylate copolymer, ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, ethylene-propylene copolymer, methylpentene polymer, acid-modified polyolefin resins obtained by modifying polyolefin resins such as polyethylene or polypropylene with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, fumaric acid, itaconic acid, and others, polyvinyl acetate resins, polyester resins, polystyrene resins, and others may be used.

[0052] The resins described above as materials used for the sealant layer 15 may be not only those derived from fossil raw materials, but also biomass-derived resins. For example, in addition to the biomass-derived polyethylene resin described above, biomass polyesters using biomass-derived ethylene glycol as a diol component as described in JP 2012-116082 A, polylactic acid resins, cellophane, starch, cellulose, etc. can be used. As the biomass-derived resin, it is preferable to use a plant-derived resin.

[0053] The outer printed portion 13A provided on the outer surface of the paper base layer 13 is formed by gravure printing, offset printing, or flexographic printing on the paper base layer 13, and therefore allows printing with excellent cosmetic properties. In addition, the surface of the outer printed portion 13A may be coated with OP varnish or the like to prevent scratches.

[0054] Next, a bonding tape 60 for covering and bonding both ends 33A, 33B of the laminate 10 will be described with reference to FIG. 6. The bonding tape 60 is a laminate in which a first bonding layer 61 and a second bonding layer 62 are laminated on both sides of a tape substrate 63, as shown in FIG. 6. The first bonding layer 61, the second bonding layer 62, and the tape substrate 63 have different thicknesses in reality, but in FIG. 6, they are shown as having the same thickness for convenience. In addition, each layer can be bonded by dry lamination using an adhesive, but the adhesive layer formed during bonding by dry lamination is thinner than the other layers and is therefore not shown. Alternatively, the first bonding layer 61 and the second bonding layer 62 are formed on the tape substrate 63 by extrusion lamination.

[0055] Next, the materials of each part constituting the bonding tape 60 will be described. The first bonding layer 61 and the second bonding layer 62 may include, for example, polyethylene (PE). Specifically, the first bonding layer 61 and the second bonding layer 62 may be made of the following materials, similar to the sealant layer 15 of the laminate 10:

[0056] The first bonding layer 61 and the second bonding layer 62 of the bonding tape 60 may be any material that can be melted by heat and fused to the sealant layer 15 of the laminate 10. For example, low-density polyethylene (LDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), linear low-density polyethylene (LLDPE), polypropylene (PP), ethylene-vinyl acetate copolymer, ionomer resin, ethylene-ethyl acrylate copolymer, ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, ethylene-propylene copolymer, methylpentene polymer, acid-modified polyolefin resins such as polyethylene or polypropylene modified with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, fumaric acid, itaconic acid, and others, polyvinyl acetate resins, polyester resins, polystyrene resins, and others may be used.

[0057] Paper or resin can be used as the tape base material 63 of the bonding tape 60. For example, unbleached kraft paper, bleached kraft paper, cup base paper, and parchment paper can be used as paper. However, when using a paper-based tape, it is preferable not to use it on the inner surface because the paper edge surface may be exposed and the contents may penetrate.

[0058] When a resin is used as the tape substrate 63, a polyolefin film such as polyethylene (PE) or polypropylene (PP) can be used. As the polyethylene (PE), low density polyethylene (LDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), linear low density polyethylene (LLDPE), etc. can be used. The same polyolefin film as that used as the sealant layer 15 of the laminate 10 may be used. Furthermore, the tape substrate 63 may be a polyethylene terephthalate (PET) layer or a nylon layer.

[0059] The bonding tape 60 may be a double-sided bonding type having a first bonding layer 61 and a second bonding layer 62, or a single-sided bonding type having only the first bonding layer 61.

[0060] Next, a method for manufacturing the laminate 10 of the cylindrical body portion 31 will be described with reference to FIG. First, printing is applied to the outer surface of the paper base layer 13 to provide an outer surface printed portion 13A made of printing ink on the outer surface of the paper base layer 13.

[0061] Next, an adhesive layer 16 is extruded onto the inner surface of the paper base layer 13, and the barrier layer 14 is laminated by extrusion lamination. This prepares a laminate in which the paper base layer 13 and the barrier layer 14 are laminated. Next, a sealant layer 15 is bonded to the inner surface of the laminate of the paper base layer 13 and the barrier layer 14 prepared above by extrusion lamination or dry lamination. Then, an easy-adhesion coating agent is applied to the outer surface of the paper base layer 13 and dried to form an easy-adhesion coating layer 12.

[0062] In the manner described above, the laminate 10 of the body portion 31 is obtained. However, as long as the desired laminate 10 can be obtained, the manufacturing method is not limited to the above method.

[0063] The laminate 10 of the trunk 31 thus obtained is wound into a cylindrical shape, and the end faces of both ends 33A and 33B are butted together as described above. Then, the bonding tape 60 is heat-sealed in a state in which it is in contact with the outer and inner surfaces of the laminate 10 at both ends 33A and 33B to form the trunk attachment part 32, and the tubular trunk 31 is produced. In this case, the easy-adhesion coating layer 12 provided on the outer surface side of the laminate 10 and the first bonding layer 61 (or the second bonding layer 62) of the bonding tape 60 superimposed on the easy-adhesion coating layer 12 side are melted and bonded, and the sealant layer 15 provided on the inner surface side and the first bonding layer 61 (or the second bonding layer 62) of the bonding tape 60 superimposed on the sealant layer 15 side are melted and bonded, and the tubular trunk 31 is obtained.

[0064] Next, the opening (upper side) 34A of the cylindrical body 31 shown in FIG. 3 is inserted into a mold (not shown), and a shoulder 35 and a mouth 36 are formed at the opening (upper side) 34A of the cylindrical body 31 using a method such as compression molding or injection molding, thereby obtaining the tube container 30 (see FIG. 1).

[0065] Next, the cap 20 is attached to the mouth 36 of the tube container 30 manufactured as described above, and a plurality of the tube containers 30 with the cap 20 attached are stored together in a cardboard box. After that, the plurality of tube containers 30 with the cap 20 attached are transported together in a cardboard box. After that, at the transport destination, an appropriate amount of hand cream, sunscreen, toothpaste, or other contents 38 is filled in the tube containers 30, and the opening (lower side) 34B is welded to form a bottom seal portion 39. This results in a packaged product 30A in which the contents 38 are filled and packaged in the tube container 30.

[0066] <Example 1> The adhesive coating layer 12 was made of polyethyleneimine having a thickness of 1.0 μm, and the paper base layer 13 was made of paper having a thickness of 70 μm ("Single Gloss Kraft" manufactured by Taiko Paper Co., Ltd. (basis weight 50 g / m 2 )"), a 20 μm thick ethylene-methacrylic acid copolymer resin layer (EMAA) was used as the adhesive layer 16, a 12 μm thick transparent vapor-deposited PET film was used as the barrier layer 14, and a 100 μm thick PE film was used as the central substrate of the sealant layer 15.

[0067] Specifically, first, the outer surface printed portion 13A was formed on the outer surface side of a 70 μm-thick paper that would become the paper base layer 13. Next, on the inner surface of the paper base layer 13, a 120 μm-thick unbleached kraft paper (80 g / m) was laminated with a 15 μm-thick adhesive layer of polyethylene (PE), which is a thermoplastic resin, by extrusion lamination. 2 ) was further attached.

[0068] Next, a 12 μm thick transparent vapor-deposited PET film that would become the barrier layer 14 was bonded by extrusion lamination with EMAA, a thermoplastic resin, as a 20 μm thick adhesive layer 16. Furthermore, an anchor coat layer was formed on the inner surface side of the 12 μm thick transparent vapor-deposited PET film that would become the barrier layer 14, and a 100 μm thick PE film that would become the central substrate of the sealant layer 15 was bonded by extrusion lamination with polyethylene (PE), a thermoplastic resin, as a 20 μm thick adhesive layer.

[0069] As a result, a laminate 10 was obtained having a structure of polyethyleneimine / printing layer (ink) / paper 70 μm / PE 15 μm / paper 120 μm / EMAA 20 μm / transparent vapor-deposited PET film 12 μm / PE 20 μm / PE film 100 μm.

[0070] A bonding tape 60 was prepared using a 25 μm thick PET film as the tape base material 63, and a 30 μm thick PE resin as the first bonding layer 61 and the second bonding layer 62. The bonding tape 60 has a bonding layer of PE resin on both sides.

[0071] Furthermore, the laminate 10 was wound into a cylindrical shape, and the end faces of both ends 33A, 33B were butted together as described above, and the joining tape 60 was heat sealed to the outer and inner faces of the laminate 10 so as to cover both ends 33A, 33B, forming the body attachment part 32. In this manner, the cylindrical body part 31 was produced.

[0072] The inner diameter of the cylindrical body 31, which specifies the tube shape, was 40 mm. Next, the opening 34A of the cylindrical body 31 was inserted into a mold, and a shoulder 35 and a mouth 36 were formed at the opening 34A of the cylindrical body 31 by compression molding. The shoulder 35 and the mouth 36 were made of high density polyethylene (HDPE).

[0073] 1 and the opening 34B was 120 mm. Then, 80 ml of water was filled into the cylindrical body 31 from the other opening 34B. After that, the opening 34B was welded to form the bottom seal 39, and the sealed packaged product 30A was produced.

[0074] <Example 2> The adhesive coating layer 12 was an ethylene-vinyl acetate copolymer adhesive with a thickness of 1.0 μm, and the paper base layer 13 was paper ("FibreForm" manufactured by BillerudKorsnas, Sweden, with a basis weight of 150 g / m 2 )"), a 20 μm thick ethylene-methacrylic acid copolymer resin layer (EMAA) was used as the adhesive layer 16, a 9 μm thick aluminum foil (ALM) was used as the barrier layer 14, and a 120 μm thick PE film was used as the central substrate of the sealant layer 15.

[0075] Specifically, first, an outer surface printed portion 13A was formed on the outer surface side of a 200 μm-thick paper that would become the paper base layer 13. Next, a film that would become the barrier layer 14, made of an aluminum foil with a thickness of 9 μm and a PET film with a thickness of 12 μm bonded together with an adhesive, was bonded to the inner surface of the paper base layer 13 by extrusion lamination, with an adhesive layer 16 of 20 μm-thick EMAA, a thermoplastic resin.

[0076] Next, an anchor coat layer was formed on the inner surface of a 12 μm thick PET film, and a 120 μm thick PE film, which serves as the central substrate of sealant layer 15, was bonded to the inner surface of the 12 μm thick PET film by extrusion lamination using a 20 μm thick adhesive layer made of polyethylene (PE), a thermoplastic resin.

[0077] As a result, a laminate 10 was obtained having a structure of ethylene-vinyl acetate copolymer adhesive / printing layer (ink) / paper 200 μm / EMAA 20 μm / ALM 9 μm / adhesive / PET film 12 μm / PE 20 μm / PE film 120 μm.

[0078] A bonding tape 60 was prepared using a PET film having a thickness of 25 μm as the tape base material 63 and a PE resin having a thickness of 50 μm as the first bonding layer 61. The bonding tape 60 has a bonding layer of PE resin on only one side.

[0079] Furthermore, in the same manner as in Example 1, a cylindrical body 31 was produced on the outer and inner surfaces of the laminate 10 using joining tape 60. Then, in the same manner as in Example 1, a sealed packaged product 30A filled with 80 ml of water was produced.

[0080] <Comparative Example 1> In Comparative Example 1, at both ends 33A, 33B, the outermost sealant layer and the innermost sealant layer are overlapped and joined by heat sealing, so two sealant layers are provided, with the outermost sealant layer being the first sealant layer and the innermost sealant layer being the second sealant layer. Also, no easy-adhesion coating layer is formed on the outer surface of the paper base layer. In Comparative Example 1, PE resin with a thickness of 60 μm was used as the first sealant layer, and paper with a thickness of 120 μm ("Nagoya Sarashi Ryuo" manufactured by Daio Paper Co., Ltd. (basis weight 100 g / m)) was used as the paper base layer. 2 )"), a 20 μm-thick ethylene-methacrylic acid copolymer resin layer (EMAA) was used as the adhesive layer, a 12 μm-thick transparent vapor-deposited PET film was used as the barrier layer, and a 100 μm-thick PE film was used as the central substrate of the second sealant layer.

[0081] Specifically, first, an outer surface printed portion was formed on the outer surface side of the paper having a thickness of 120 μm that would become the paper base layer. Next, a first sealant layer was laminated by extrusion lamination on the outer surface of the paper having a thickness of 120 μm that would become the paper base layer. Specifically, on the outer surface of the paper base layer, PE, which is a thermoplastic resin, was laminated by extrusion lamination as a first sealant layer having a thickness of 60 μm on the paper base layer.

[0082] Next, a transparent vapor-deposited PET film having a thickness of 12 μm, which serves as a barrier layer, was attached to the inner surface of the paper base layer 13 by extrusion lamination, with an adhesive layer of EMAA, which is a thermoplastic resin, having a thickness of 20 μm.

[0083] Next, an anchor coat layer was formed on the inner surface of a 12 μm-thick transparent vapor-deposited PET film that would serve as a barrier layer, and a 100 μm-thick PE film that would serve as the central substrate for the second sealant layer was bonded to the film by extrusion lamination using a 20 μm-thick adhesive layer made of polyethylene (PE), a thermoplastic resin.

[0084] As a result, a laminate was obtained with a structure of PE 60 μm / printing layer (ink) / paper 120 μm / EMAA 20 μm / transparent vapor-deposited PET 12 μm / PE 20 μm / PE film 100 μm.

[0085] Furthermore, the laminate 10 was wound into a cylindrical shape, and both ends 33A, 33B were overlapped, and the outer surface and inner surface of the laminate 10 were heat-sealed at both ends 33A, 33B to produce a cylindrical body 31. Since both ends 33A, 33B were overlapped and the first sealant layer and the second sealant layer were joined by heat sealing, no joining tape was used.

[0086] Thereafter, in the same manner as in Example 1, a sealed packaged product 30A filled with 80 ml of water was prepared.

[0087] <Comparative Example 2> The first sealant layer was made of PE resin with a thickness of 20 μm, PE film with a thickness of 80 μm, and PE resin with a thickness of 20 μm. The paper base layer was made of paper with a thickness of 200 μm (FibreForm manufactured by Billerud Korsnas, Sweden, with a basis weight of 150 g / m). 2 )"), a 20 μm-thick ethylene-methacrylic acid copolymer resin layer (EMAA) was used as the adhesive layer, an aluminum foil (ALM) with a thickness of 9 μm was used as the barrier layer, and a 100 μm-thick PE film was used as the central substrate of the second sealant layer. Then, in the same manner as in Comparative Example 1, each layer was appropriately laminated to form a laminate.

[0088] As a result, a laminate was obtained with a structure of printing layer (ink) / PE 20 μm / PE film 80 μm / PE 20 μm / paper 200 μm / EMAA 20 μm / aluminum foil 9 μm / adhesive / PET 12 μm / PE 20 μm / PE film 100 μm.

[0089] Then, similarly to Comparative Example 1, the laminate 10 was wound into a cylindrical shape, both end portions 33A, 33B were overlapped as described above, and the outer and inner surfaces of the laminate 10 at both end portions 33A, 33B were heat-sealed to produce a cylindrical body portion 31. Since both end portions 33A, 33B were overlapped and the first sealant layer and the second sealant layer were joined by heat sealing, no joining tape was used.

[0090] Thereafter, in the same manner as in Example 1, a sealed packaged product 30A filled with 80 ml of water was prepared.

[0091] <Evaluation> The laminates and tube containers of Examples 1 and 2 and Comparative Examples 1 and 2 were evaluated using four indices: paper-likeness, shoulder adhesive strength, side seam strength, and oxygen barrier property of the side seam.

[0092] Regarding paper-likeness, subjects subjectively evaluated the appearance and feel of the body of the tube container containing 80 ml of water produced in Examples 1 and 2 and Comparative Examples 1 and 2. If it was paper-like, it was rated ◯, if it was not paper-like, it was rated ×, and if it was in between (lacking in paper-likeness), it was rated △.

[0093] For the shoulder adhesive strength, a tensile test was conducted to measure the peel strength between the body and the shoulder, using a test specimen in which the body was cut into a 15 mm wide strip in the direction of the bottom seal from the adhesive point between the body and the shoulder. The 15 mm wide strip of the body of the test specimen was taken from the body attachment part and the part of the body that was 180° opposite from the body attachment part. The body and shoulder of the test specimen were then pulled with a pair of chucks using a tensile tester. Specifically, one chuck clamped the shoulder 35, and the other chuck clamped the lower end side of the body 31 (the opening 34B, the bottom seal part 39 side) and pulled. A tensile load was applied until the body and the shoulder were separated, and the maximum load during that time was taken as the shoulder adhesive strength. The average value was then calculated for the test specimen in which the strip was attached to the body and the test specimen in which the strip was attached to the body part and the part of the body that was 180° opposite from the body attachment part. The tensile tester used was the "Tensilon Universal Testing Machine RTF" manufactured by Orientec Co., Ltd. The tensile test speed was 300 mm / min. The shoulder adhesive strength (peel strength) was measured three times for each example and comparative example, and the average value was recorded. A value of 40 N / 15 mm or more was marked with ◯, and a value of less than 40 N / 15 mm was marked with ×. In addition, in Figs. 1 and 2, the joint between the body 31 and the shoulder 35 is shown as a relatively simple structure as an example. However, in reality, the resin of the shoulder 35 is melted and joined to the body 31 by a method such as compression molding or injection molding, so that the shape of the shoulder 35 may be different from that shown in Figs. 1 and 2. Therefore, the shape of the shoulder 35 may be different from that shown in Figs. 1 and 2. In addition, the end of the body 31 may be covered with the resin of the shoulder 35.

[0094] For the side seam strength, a tensile test was performed to measure the breaking strength when the test piece breaks, using a test piece cut into a strip shape with a width of 15 mm so as to include the body attachment portion and extend in the circumferential direction. Specifically, a pair of chucks was used to pull two opposing points of the test piece using a tensile tester, and a tensile load was applied until the test piece broke, and the maximum load during that time was taken as the side seam strength. Here, "the test piece breaks" does not mean peeling of the bonding tape 60 or breakage of the bonding tape 60, but breakage of the laminate 10 itself constituting the body 31. The tensile tester used was "Tensilon Universal Testing Machine RTF" manufactured by Orientec Co., Ltd. The tensile test speed was 300 mm / min. For the side seam strength, measurements were taken three times for each of the examples and comparative examples, and the average value was recorded. A value of 80 N / 15 mm or more was marked as "○", and a value of less than 80 N / 15 mm was marked as "×".

[0095] To check the oxygen barrier properties of the side seam, a leucomethylene blue agar solution was prepared as follows, filled and sealed in a tube container so as to prevent a head space, and left at room temperature of 23°C for one week, after which the contents were removed and the dyeing condition was visually confirmed. A mark of ◯ was given when there was almost no linear blue dyeing in the side seam (body attachment portion 32 and its vicinity), and a mark of × was given when the blue dyeing was clearly visible.

[0096] The leucomethylene blue agar solution was prepared as follows: First, 20 g of agar was dissolved in 1 L of water by heating, cooled to 70-75°C, and 0.2 g of methylene blue was added and stirred. The solution was further cooled to 65-70°C, and 0.8 g of sodium hydrosulfite was added and stirred to prepare the solution.

[0097] The evaluation results for the above four indicators are shown in Table 1.

[0098] [Table 1]

[0099] As shown in Table 1, Examples 1 and 2, in which the sealant layer was only one layer on the innermost surface and the portions where both ends 33A and 33B contacted were joined with joining tape on both the outer and inner surfaces, showed good results in all four indices. In contrast, Comparative Examples 1 and 2, in which the first sealant layer on the outermost surface and the second sealant layer on the innermost surface were overlapped and joined at both ends 33A and 33B, did not show good results in the indices of paper-likeness and oxygen barrier property of the side seam portion.

[0100] From the evaluation results shown in Table 1, it became clear that a laminate in which at least a paper base layer 13, a barrier layer 14, and a sealant layer 15 are laminated in that order from the outer surface side and used for the body of a tube container by butting the end faces together, in which an easy-adhesion coating layer 12 is formed on at least a portion of the outer surface side of the paper base layer 13, can express a paper-like appearance (paper texture) and maintain the oxygen barrier properties of the body attachment portion 32 (also called the side seam portion).

[0101] Although the preferred embodiment of the present disclosure has been described above, the present disclosure is not limited to the above embodiment and various modifications are possible. For example, in the above embodiment, a screw-type cap is used in which a thread is provided on the outer peripheral surface of the mouth and a thread groove is provided on the inner surface of the cap to screw into the thread, but other types of caps may be used, such as a type that is connected by a so-called one-touch fitting in which the cap is attached to and detached from the container only by a linear movement in the up and down direction. [Explanation of symbols]

[0102] 10.... (of body 31 of tube container 30) laminate 12. Easy-adhesion coating layer 13...Paper base layer 14. Barrier layer 15. Sealant layer 16...adhesive layer 20 Cap 30...Tube container 30A·Packaging products 31... Body 32... Body attachment section 33A...End 33B...End 34A...Opening (upper side) 34B...Opening (lower side) 35...Shoulder 36...Mouth 37... Head molding 38...Contents 39 Bottom seal 60.... Joint tape 61...1st bonding layer 62...Second bonding layer 63 Tape base material

Claims

1. A laminate in which at least an outermost paper base layer, a barrier layer, and a sealant layer are laminated in this order from the outer surface side, A laminate for a tube container used for a tube container having a body part in which end faces of the laminate are butted together and joined with a joining tape, An easy-adhesion coating layer is formed on at least a part of the outer surface side of the paper base layer, The easy-adhesion coating layer is formed at a position including an area overlapping with the bonding tape, and when the width of the easy-adhesion coating layer at both ends of the body is WE (mm) and the width of the bonding tape is WT (mm), WE≧WT / 2.

2. 2. The laminate for a tube container according to claim 1, wherein a printed portion is formed on an outer surface of the paper base layer, and the easy-adhesion coating layer is formed at a position not overlapping with the printed portion.

3. The tube container laminate according to claim 1 or 2, wherein the easy-adhesion coating layer contains polyethyleneimine.

4. A tube container comprising a body portion in which both ends of the laminate for a tube container according to any one of claims 1 to 3 are butted together and joined on both inner and outer surfaces of the laminate with joining tape so as to cover both ends.

5. 5. The tube container according to claim 4, wherein the tube container has a side seam strength of 80 N / 15 mm or more.

6. The peel strength between the body and the shoulder joined to the body is 40 N / 15 mm or more. The tube container according to claim 4 or 5.

Citation Information

Patent Citations

  • Barrel part of tubular vessel

    JP1994166107A

  • Body of tubular container

    JP1995041020A

  • Tubular container

    JP1995137753A

  • Laminate tube

    JP1996324599A

  • Laminate tube container

    JP2005178851A