Hot melt composition for yogurt lid material and lid material using the same

A hot melt composition combining ethylene-unsaturated ester copolymer, waxes, and tackifier resin addresses the challenge of balancing heat resistance and easy-openability in yogurt lids, ensuring effective seal integrity and ease of opening.

JP7567457B2Active Publication Date: 2024-10-16TOYO INK MFG CO LTD +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020215684
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-24
Publication Date
2024-10-16
Estimated Expiration
2040-12-24

AI Technical Summary

Technical Problem

Existing hot melt adhesives for yogurt lids struggle to balance heat resistance during post-fermentation processes with easy-openability, as increased cohesive and adhesive forces impair the ease of opening.

Method used

A hot melt composition comprising an ethylene-unsaturated ester copolymer with specific melt mass flow rate, combined with two types of waxes having different oil contents, and a tackifier resin, to achieve both heat resistance and easy-openability.

Benefits of technology

The composition provides a yogurt lid material with heat resistance that prevents seal peeling during fermentation and ensures easy opening, maintaining optimal adhesive and cohesive forces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567457000001
    Figure 0007567457000001
  • Figure 0007567457000002
    Figure 0007567457000002
Patent Text Reader

Abstract

To provide a hot-melt composition which achieves both such heat resistance as to prevent seal peeling in a post-fermentation step in yogurt production, and such easy openability as to easily open a lid in opening, and a lid material using the composition.SOLUTION: A hot-melt composition for a yogurt lid material contains 25-50 mass% of an ethylene-unsaturated ester copolymer (A) containing an ethylene-unsaturated ester copolymer (A1) having an MFR of 3-70 g / 10 minutes, 10-30 mass% of a tackifier resin (B), 5-40 mass% of a wax (C) having an oil content of less than 0.2 mass%, 5-40 mass% of a wax (D) having an oil content of 0.2 mass% or more and 4.0 mass% or less, contains 30-50 mass% of the total of the wax (C) and the wax (D), and contains 10-50 mass% of the ethylene-unsaturated ester copolymer (A1).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hot melt composition for a yogurt lid material having excellent coatability, heat resistance, and easy-opening properties, and to a lid material using the same. [Background technology]

[0002] 2. Description of the Related Art In the field of product packaging, a method of adhering a lid material to an opening of a container via a heat seal layer is used in order to protect and preserve the contents. When the content is yogurt, a method is used in which a container obtained by vacuum molding a thermoplastic resin sheet such as high-impact polystyrene, polypropylene (PP), polyethylene terephthalate (PET), etc. is sealed with a lid material made by laminating a low-melting point resin such as low-density polyethylene, low-molecular-weight polyester, ethylene-unsaturated ester copolymer, etc. on one side of a sheet of aluminum foil, polypropylene, polyvinyl chloride, polyethylene terephthalate, etc., or a lid material made by molding these, or a lid material with a hot melt adhesive applied in advance only to the sealing part.

[0003] Hot melt adhesives used for heat sealing such food containers are required to have adhesive strength to seal the contents, as well as properties such as coatability, airtightness, water resistance, oil resistance, alkali resistance, and non-toxicity, as well as ease of opening so that the container can be opened easily.

[0004] Meanwhile, the post-fermentation method, in which yogurt is sealed with heat and then fermented at 40 to 45°C, is widely used as a method for producing yogurt. Hot melt adhesives used in yogurt lid materials are required to have heat resistance that prevents deterioration of the seal due to peeling during the post-fermentation process.

[0005] As a means for improving heat resistance, for example, Patent Document 1 discloses the use of a specific tackifier resin, and Patent Document 2 discloses the use of a high melting point base polymer. However, these methods increase the cohesive strength associated with higher molecular weight, and the adhesive strength increases, increasing the opening strength and impairing the ease of opening. Patent Document 3 discloses a method for improving heat resistance by controlling the oil content of wax. However, even when refined wax with a low oil content is used, the opening strength increases due to an increase in hardness of the hot melt composition, and the ease of opening is impaired. Therefore, with the techniques described in Patent Documents 1 to 3, it is difficult to achieve both heat resistance and easy opening properties required for use as a yogurt lid material. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 2-55783 [Patent Document 2] Japanese Patent Application Publication No. 10-130436 [Patent Document 3] JP 2000-204336 A Summary of the Invention [Problem to be solved by the invention]

[0007] The object of the present invention is to provide a hot melt composition that has both heat resistance that prevents peeling of the seal during the post-fermentation process in the production of yogurt and easy opening properties that allow easy opening when opening, and a lid material made using said composition. [Means for solving the problem]

[0008] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by a hot melt composition containing an ethylene-unsaturated ester copolymer having the following composition and a wax having a specific oil content, and have thus completed the present invention.

[0009] A hot melt composition for yogurt covering material according to one embodiment of the present invention contains 25 to 50 mass% of an ethylene-unsaturated ester copolymer (A) including an ethylene-unsaturated ester copolymer (A1) having a melt mass flow rate of 3 to 70 g / 10 min, 10 to 30 mass% of a tackifier resin (B), 5 to 40 mass% of a wax (C) having an oil content of less than 0.2 mass%, and 5 to 40 mass% of a wax (D) having an oil content of 0.2 mass% or more and 4.0 mass% or less, the wax (C) and the wax (D) constitute 30 to 50 mass% in total, and the ethylene-unsaturated ester copolymer (A1) constitutes 10 to 50 mass%.

[0010] The hot melt composition for yogurt covering material according to one embodiment of the present invention is characterized in that the ethylene-unsaturated ester copolymer (A) is a polymer of ethylene and an unsaturated ester monomer, and contains structural units derived from the unsaturated ester monomer in a range of 25 to 35 mass % based on the mass of the ethylene-unsaturated ester copolymer (A).

[0011] The hot melt composition for yogurt capping material according to one embodiment of the present invention is characterized in that the wax (C) and the wax (D) each independently have a melting point of 60 to 100°C.

[0012] The hot melt composition for yogurt lid material according to one embodiment of the present invention is characterized in that the wax (C) and the wax (D) are each independently at least one wax selected from the group consisting of paraffin wax and Fischer-Tropsch wax.

[0013] The hot melt composition for yogurt covering material according to one embodiment of the present invention is characterized in that the softening point of the tackifier resin (B) is in the range of 90 to 150°C.

[0014] A covering material according to one aspect of the present invention is characterized in that it comprises a hot melt layer made of the above-mentioned hot melt composition on one surface of a substrate.

[0015] A covering material according to one embodiment of the present invention is characterized in that the substrate has at least two or more layers selected from the group consisting of a resin layer, a paper layer, and a metal layer.

[0016] The covering material according to one aspect of the present invention is characterized in that the resin layer contains at least one resin selected from the group consisting of polyethylene resin, polypropylene resin, and polyethylene terephthalate resin.

[0017] An openable set of components for a sealed container according to one aspect of the present invention is characterized by comprising a container and the above-mentioned lid member.

[0018] An openable sealed container according to one aspect of the present invention is characterized in that an opening of the container is heat-sealed with a hot melt layer provided in the above-mentioned lid material.

[0019] In the openable sealed container according to one embodiment of the present invention, the coating amount of the hot melt layer is 10 to 30 g / m 2 The range is 5 to 20 N, and the opening strength measured in accordance with JIS S 0021-2:2018 is in the range of 5 to 20 N. Effect of the Invention

[0020] The present invention provides a hot melt composition for a yogurt lid material that has both heat resistance that prevents the seal from peeling off during the post-fermentation process in the production of yogurt and easy opening properties that allow the lid to be easily opened, and a lid material made using the composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The hot melt adhesive of the present invention is used for a yogurt lid material, and is characterized in that it contains 25 to 50 mass% of an ethylene-unsaturated ester copolymer (A) including an ethylene-unsaturated ester copolymer (A1) having a melt mass flow rate of 3 to 70 g / 10 min, 10 to 30 mass% of a tackifier resin (B), 5 to 40 mass% of a wax (C) having an oil content of less than 0.2 mass%, and 5 to 40 mass% of a wax (D) having an oil content of 0.2 mass% or more and 4.0 mass% or less, containing 30 to 50 mass% of wax (C) and wax (D) in total, and containing 10 to 50 mass% of ethylene-unsaturated ester copolymer (A1). By combining such an ethylene-unsaturated ester copolymer having a specific melt mass flow rate with two types of wax having different oil contents, it is possible to obtain a hot melt composition having suitable opening strength (easy opening) for use as a lid material and the heat resistance required for the post-fermentation process. Each component constituting the hot melt composition of the present invention will be described in detail below.

[0022] <Ethylene-unsaturated ester copolymer (A)> The ethylene-unsaturated ester copolymer (A) used in the present invention is one of the main components in the hot melt composition, and plays a major role in imparting adhesive strength and cohesive strength. The ethylene-unsaturated ester copolymer is a copolymer of ethylene and an unsaturated ester monomer. Examples of the unsaturated ester monomer include (meth)acrylic acid alkyl esters such as methyl acrylate, ethyl acrylate, isobutyl acrylate, n-butyl acrylate, isooctyl acrylate, methyl methacrylate, and isobutyl methacrylate; unsaturated carboxylic acid alkyl esters such as dimethyl maleate and diethyl maleate; and carboxylic acid vinyl esters such as vinyl acetate and vinyl propionate. In the ethylene-unsaturated ester copolymer, the unsaturated ester monomer may be used alone or in combination of two or more kinds. The unsaturated ester monomer is preferably vinyl acetate or methyl methacrylate, and more preferably vinyl acetate. The ethylene-unsaturated ester copolymer (A) may be used alone or in combination of two or more kinds.

[0023] The content of the ethylene-unsaturated ester copolymer (A) in the hot melt composition of the present invention is in the range of 25 to 50% by mass. If the content is less than 25% by mass, the adhesiveness becomes insufficient, and the heat resistance and ease of opening are poor. If the content exceeds 50% by mass, the viscosity increases and the coatability decreases. The content of the ethylene-unsaturated ester copolymer (A) is preferably in the range of 30 to 45% by mass.

[0024] It is also important that the hot melt composition of the present invention contains, as one component of the ethylene-unsaturated ester copolymer (A), 10 to 50 mass % of an ethylene-unsaturated ester copolymer (A1) having a melt mass flow rate of 3 to 70 g / 10 min in the hot melt composition. The melt mass flow rate is the amount of the hot melt composition that flows out at 190° C. under a load of 2160 g for 10 minutes (g / 10 min) as measured in accordance with JIS K 7210. If the melt mass flow rate is less than 3 g / 10 min, the viscosity of the hot melt composition increases and the coating suitability decreases. If the melt mass flow rate is more than 70 g / 10 min, the heat resistance is insufficient. The melt mass flow rate of the ethylene-unsaturated ester copolymer (A1) is preferably 10 to 70 g / 10 min.

[0025] The content of the structural unit derived from the unsaturated ester monomer in the ethylene-unsaturated ester copolymer (A) is preferably in the range of 20 to 40 mass%, more preferably in the range of 25 to 35 mass%, based on the mass of the ethylene-unsaturated ester copolymer (A). By setting the content within the above range, excellent adhesive strength and coating suitability are obtained.

[0026] When multiple ethylene-unsaturated ester copolymers are used, the content of the structural units derived from the unsaturated ester monomer can be calculated from the content and blending ratio of the structural units derived from the unsaturated ester monomer of each ethylene-unsaturated ester copolymer. If the content of the structural units derived from the unsaturated ester monomer of the first ethylene-unsaturated ester copolymer is VA1 and the blending amount is W1, and the content of the structural units derived from the unsaturated ester monomer of the second ethylene-unsaturated ester copolymer is VA2 and the blending amount is W2, the overall content VA of the structural units derived from the unsaturated ester monomer can be calculated by the following formula. Formula) VA=(VA1×W1+VA2×W2) / (W1+W2)

[0027] <Tackifying resin (B)> The tackifier resin (B) used in the present invention can be appropriately selected from known ones. Examples of such tackifier resin (B) include phenolic resin, modified phenolic resin, xylene phenolic resin, xylene resin, coumarone-indene resin, alkylphenolic resin, terpene (α-pinene, β-pinene) resin, terpene phenolic resin, rosin, rosin derivative (hydrogenated rosin, disproportionated rosin, polymerized rosin, rosin ester (esterified rosin such as alcohol, glycerin, pentaerythritol)), aliphatic (C5) petroleum resin, aromatic (C9) petroleum resin, copolymer (C5 / C9) petroleum resin, alicyclic petroleum resin (hydrogenated or DCPD petroleum resin), and low molecular weight polystyrene resin. Among these, rosin-based resins such as rosin and rosin derivatives (hydrogenated rosin, disproportionated rosin, polymerized rosin, and rosin esters (esterified rosins such as alcohol, glycerin, and pentaerythritol)); petroleum-based resins such as aliphatic (C5) petroleum resins, aromatic (C9) petroleum resins, copolymer (C5 / C9) petroleum resins, and alicyclic petroleum resins (hydrogenated or DCPD petroleum resins); and styrene-based resins such as low molecular weight polystyrene resins are preferably used, and more preferably rosin-based resins and petroleum-based resins, and rosin-based resins and petroleum-based resins may be used in combination. As the petroleum-based resin, alicyclic petroleum resins are preferable. The tackifier resin may be used alone or in combination of two or more kinds.

[0028] The content of the tackifier resin (B) in the hot melt composition is 10 to 30% by mass, and preferably 15 to 25% by mass. If the content of the tackifier resin is less than 10% by mass, the heat resistance and ease of opening are reduced, and if it exceeds 30% by mass, the ease of opening is reduced.

[0029] The softening point of the tackifier resin (B) is preferably in the range of 80 to 160° C., more preferably in the range of 90 to 150° C., and even more preferably in the range of 100 to 140° C. When the softening point is within the above range, the heat resistance becomes good. The softening point of the tackifier resin (B) can be determined in accordance with JIS K 5902 and JIS K 2207. Specifically, a specified ring filled with a resin composition is left to stand for 12 hours or more, then placed in a heating medium, a specified ball is placed on the specified ring filled with the resin composition, and the temperature of the heating medium is increased at a constant rate. The softening point is the temperature at which the ball sinks due to softening of the resin composition and touches the bottom plate of the ring stand. When the tackifier resin (B) contains a plurality of tackifier resins, the softening point of the tackifier resin (B) can be determined from the softening points of the respective tackifier resins and their mass ratios.

[0030] <Wax (C) and (D)> The hot melt composition of the present invention contains a wax (C) having an oil content of less than 0.2 mass % and a wax (D) having an oil content of 0.2 to 4.0 mass %. The inclusion of wax (C) having an oil content of less than 0.2% by mass improves the heat resistance of the hot melt composition, while the inclusion of wax (D) having an oil content of 0.2 to 4.0% by mass brings the opening strength into a suitable range, resulting in excellent ease of opening. The oil content in this specification is a value determined in accordance with JIS K 2235-5.6. Specifically, 1 g of a sample is dissolved in 15 ml of methyl ethyl ketone, cooled to −32° C., and the precipitated wax is filtered to obtain a filtrate, and the solvent of the filtrate is evaporated to obtain a residual oil mass, which is expressed as mass %.

[0031] Examples of the waxes (C) and (D) that can be used in the present invention include paraffin wax, microcrystalline wax, montan wax, Fischer-Tropsch wax, carnauba wax, ethylene wax, polyethylene wax, propylene wax, polypropylene wax, ethylene-propylene wax, polyethylene-polypropylene wax, and modified waxes such as polyethylene-polypropylene copolymers grafted with styrene. Among these, paraffin wax and Fischer-Tropsch wax are preferred. These waxes may be used alone or in combination of two or more.

[0032] Examples of commercially available wax (C) having an oil content of less than 0.2% by mass include the paraffin wax "HNP series" manufactured by Nippon Seiro Co., Ltd. Examples of commercially available wax (D) having an oil content of 0.2 to 4.0% by mass include the "Sasol series" manufactured by Sasol Chemical Industries Co., Ltd. and the "FT wax series" manufactured by Qindao Bouni Chemical Co., Ltd.

[0033] The melting points of the waxes (C) and (D) are each independently preferably in the range of 60 to 100° C., more preferably in the range of 70 to 100° C. By setting the melting points within the above range, the heat resistance of the hot melt composition is improved. Note that the melting point in this specification is the peak top temperature when the temperature is increased at 10° C. / min in a differential scanning calorimeter (DSC) measurement.

[0034] The content of wax (C) in the hot melt composition of the present invention is 5 to 40% by mass, preferably 10 to 35% by mass. If it is less than 5% by mass, the heat resistance is significantly reduced, and if it exceeds 40% by mass, the easy-opening property is impaired. The content of wax (D) is 5 to 40% by mass, preferably 10 to 35% by mass. If it is less than 5% by mass, the easy-opening property is impaired, and if it exceeds 40% by mass, the heat resistance is reduced. The total content of the wax (C) and the wax (D) is 30 to 50% by mass, and preferably 35 to 45% by mass. If it is less than 30% by mass, the viscosity increases and the coatability decreases. If it exceeds 50% by mass, the heat resistance and the ease of opening decrease.

[0035] <Other ingredients> The hot melt composition of the present invention may contain, as optional components, antioxidants, silane coupling agents, antiblocking agents, hydrophobic oxide fine particles, etc. These other components may be used alone or in combination of two or more.

[0036] Examples of the antioxidant include phenol-based antioxidants and phosphorus-based antioxidants. Specific examples include pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, 4,6-bis(octylthiomethyl)-o-cresol, ethylene bis(oxyethylene) bis[3-(5-t-butyl-4-hydroxy-m-tolyl]propionate, tris(2,4-di-t-butylphenyl)phosphite, and bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite. A preferred phenol-based antioxidant is pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], and a preferred phosphorus-based antioxidant is tris(2,4-di-t-butylphenyl)phosphite.

[0037] Examples of the silane coupling agent include vinyltrimethoxysilane, vinyltriethoxysilane, methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)3-aminopropyltrimethoxysilane, N-(2-aminoethyl)3-aminopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, mercaptobutyltrimethoxysilane, and 3-mercaptopropylmethyldimethoxysilane.

[0038] Examples of the anti-blocking agent include silicones; unsaturated fatty acid amides such as erucic acid amide and oleic acid amide; and saturated fatty acid amides such as stearic acid amide and behenic acid amide.

[0039] Examples of hydrophobic oxide particles include silica (silicon dioxide), alumina, titania, calcium oxide, calcium carbonate, calcium sulfate, and calcium silicate.

[0040] From the viewpoint of suppressing bleed-out, the content of the optional components is preferably 10% by mass or less, and more preferably 8% by mass or less, based on the mass of the hot melt composition.

[0041] The hot melt composition of the present invention can be obtained by mixing the ethylene-unsaturated ester copolymer (A), the tackifier resin (B), the wax (C), the wax (D), and any optional components used as necessary by a known method. For example, a hot melt composition of the heat melt type can be obtained by heating and mixing using a melting kettle equipped with a roll, a Banbury mixer, a kneader, or a stirrer, or a single-screw or twin-screw extruder. Also, for example, a solvent-type hot melt composition can be obtained by dissolving in a known solvent and stirring and mixing. The hot melt composition of the present invention is used for yogurt lid material applications, and from the viewpoint of residual solvent, it is preferably a solvent-free heat-melting type hot melt adhesive.

[0042] The hot melt composition of the present invention preferably has a melt viscosity in the range of 500 to 5,000 mPa s at 160° C. In this specification, the melt viscosity is a value measured using a B-type viscometer in accordance with JIS K 6862 under conditions of 160° C., rotor No. 3, 12 rpm, and 30 seconds.

[0043] <Lid material> The hot melt composition of the present invention can be suitably used as a lid material for yogurt. The lid material of the present invention has a hot melt layer made of the hot melt composition of the present invention on one side of a substrate, and can be used for an openable container. The method for producing the lid material is not particularly limited, and the lid material can be produced using a known production method. The method for forming the hot melt layer is not particularly limited, and may be either a contact coating method or a non-contact coating method. The contact coating method is a coating method in which a sprayer is brought into contact with a member or a film when applying a hot melt composition, and examples of the method include slot coater coating, gravure coater coating, and roll coater coating. The non-contact coating method is a coating method in which the sprayer does not come into contact with a member or film when coating the hot melt composition. Examples of the non-contact coating method include spiral coating, which allows for spiral coating, omega coating, which allows for wave-like coating, controlled seam coating, slot spray coating, which allows for planar coating, curtain spray coating, dot coating, which allows for spot-like coating, and bead coating, which allows for linear coating. The thickness of the hot melt layer is usually in the range of 1 to 100 μm. The hot melt layer may be crosslinked by heating or by irradiating with ultraviolet light.

[0044] [Base material] The substrate usable for the lid material of the present invention is not particularly limited and can be appropriately selected from known substrates. The substrate for the yogurt lid material is preferably a substrate having at least two or more layers selected from the group consisting of a resin layer, a paper layer, and a metal layer. The resin layer preferably contains at least one resin selected from the group consisting of polyester resins such as polyethylene terephthalate resin, polyolefin resins such as polyethylene, polypropylene, and polynorbornene, polycarbonate resins, polyarylate resins, acrylic resins, polyphenylene sulfide resins, polystyrene resins, vinyl resins, vinyl chloride resins, polyimide resins, and epoxy resins, and more preferably contains at least one resin selected from the group consisting of polyethylene resins, polypropylene resins, and polyethylene terephthalate resins. The resin layer may have a metal deposition layer formed by depositing a metal such as aluminum, or a transparent deposition layer formed by depositing alumina, silicon oxide, or the like. As the metal in the metal layer, aluminum is preferably used, and examples thereof include aluminum foil and an aluminum vapor deposition layer. The substrate may further include other layers such as nonwoven fabric, woven fabric, cloth, glass, and the like.

[0045] Preferred examples of the substrate configuration include "paper / polyethylene resin", "polyethylene terephthalate resin / paper / polyethylene resin", and "polyethylene terephthalate resin / aluminum foil / polyethylene resin". Furthermore, the surface of the substrate may be subjected to adhesion enhancing treatment such as corona discharge treatment, plasma treatment, blast treatment, and chemical etching treatment, antistatic treatment, coloring treatment, and the like, as necessary. The thickness of the substrate is not particularly limited, and is usually in the range of 1 to 300 μm.

[0046] <Sealed container parts set, sealed container> The above-mentioned lid material can be suitably used together with the container as an openable sealed container member set. The above-mentioned set can also be used as an openable sealed container by heat sealing the opening of the container and the lid material with a hot melt layer. In general, it can be said that an easy-open property is good if the opening strength is in the range of 5 to 20 N. The openable sealed container of the present invention has a coating amount of the hot melt layer of 10 to 30 g / m 2 In this range, the opening strength is preferably in the range of 5 to 20N. EXAMPLES

[0047] The present invention will be described in detail below with reference to examples, but these examples are merely one embodiment of the present invention and the present invention is not limited to these examples. In the examples, "parts" and "%" refer to "parts by mass" and "% by mass", respectively.

[0048] <Method of producing hot melt composition> The wax (C) and the wax (D) were added to a stainless steel beaker equipped with a stirrer in the blending ratio (by mass) shown in Tables 1 and 2, and the mixture was heated carefully so that the contents did not reach 180° C. or higher. After confirming that the contents were melted, stirring was started, and the ethylene-unsaturated ester copolymer (A), the tackifier resin (B), and additives as necessary were added, and the mixture was stirred until completely mixed to obtain a hot melt composition.

[0049] <Evaluation method of hot melt composition> The obtained hot melt composition was subjected to the following evaluations, and the results are shown in Tables 1 and 2.

[0050] [Coatability (melt viscosity)] The melt viscosity of the obtained hot melt composition was measured in accordance with JIS K 6862. Specifically, using a B-type viscometer, the measurement was performed under the conditions of a temperature of 160° C., a rotor No. 3, a rotation speed of 12 rpm, and a time of 30 seconds, and the results were evaluated according to the following criteria. ○: Melt viscosity is 5,000 mPa s or less (usable) ×: Melt viscosity exceeds 5,000 mPa·s (not suitable for use)

[0051] [Creating the lid] Next, the obtained hot melt composition was applied to the PE surface of a substrate having PET (20 μm), Al (aluminum foil, 15 μm), and PE (polyethylene, 20 μm) laminated in this order, using a gravure coater, in an amount of 16 g / m. 2 A lid material was obtained by coating with the above composition.

[0052] [Heat resistance (corresponding to peelability evaluation during post-fermentation)] The resulting lid material was cut to a size of 70 mm x 15 mm. The end of the resulting lid material with a size of 70 mm x 15 mm was overlapped near the center of a polystyrene (PS) substrate with a size of 70 mm x 15 mm, and heat sealed under the conditions of a gauge pressure of 0.1 MPa, a sealing temperature of 140°C, a sealing time of 1.0 second, and a bonding area of ​​20 mm x 15 mm to prepare a test piece. The test piece was fixed horizontally in an oven set at 45°C with the PS substrate side facing up. A 10g weight was attached to the end of the lid, and a load was applied at a 90 degree angle to the PS substrate. The length to which the lid had peeled off after 1 hour (peel distance) was measured. The obtained peel distance was used to evaluate heat resistance according to the following criteria. This evaluation corresponds to the evaluation of peelability during post-fermentation of yogurt. ◎: Peel distance is less than 3 mm (very good) ○: Peel distance is 3mm or more and less than 5mm (good) △: Peeling distance is 5mm or more and less than 7mm (usable) ×: Peeling distance is 7mm or more (not usable)

[0053] [Easy to open] The resulting lid material was cut to a size of 70 mm x 70 mm, and heat sealed to a PS container with an opening size of 52 mm under conditions of 0.3 MPa gauge pressure, 140°C, and 1.0 second to obtain a container. The resulting container was left to stand in a constant temperature and humidity room at a temperature of 23°C and humidity of 65% for 24 hours, and then the peel strength was measured in the same room by peeling at a 45-degree angle at a speed of 200 mm / min. The measurement was performed five times, and the average value of the maximum load (N) at the time of opening was taken as the opening strength, and the ease of opening was evaluated according to the following criteria. 〇: Opening strength is 10N or more but less than 15N (good) △: Opening strength is 5N to less than 10N, or 15N to less than 20N (usable) ×: Opening strength is less than 5N or more than 20N (unusable)

[0054] [Table 1]

[0055] [Table 2]

[0056] The abbreviations listed in Tables 1 and 2 are as follows: <Ethylene-unsaturated ester copolymer (A1)> A1-1: Ultrathene 752 (Tosoh ethylene-vinyl acetate copolymer, vinyl acetate content: 32%, MFR: 60g / 10min) A1-2: Ultrathene 750 (Tosoh ethylene-vinyl acetate copolymer, vinyl acetate content: 32%, MFR: 30g / 10min) A1-3: Ultrathene 633 (Tosoh ethylene-vinyl acetate copolymer, vinyl acetate content: 20%, MFR: 20g / 10min)

[0057] <Other ethylene-unsaturated ester copolymers (A2) other than (A1)> A2-1: Ultrathene 720 (Tosoh ethylene-vinyl acetate copolymer, vinyl acetate content: 28%, MFR: 150g / 10min) A2-2: Ultrathene 722 (Tosoh ethylene-vinyl acetate copolymer, vinyl acetate content: 28%, MFR: 400g / 10min)

[0058] <Tackifying resin (B)> B1: Alcon P-140 (Arakawa Chemical Industries, alicyclic petroleum resin (hydrogenated petroleum resin), softening point: 140°C) B2: Alcon P-125 (Arakawa Chemical Industries, alicyclic petroleum resin (hydrogenated petroleum resin), softening point: 125°C) B3: Alcon P-90 (Arakawa Chemical Industries, hydrogenated petroleum resin, softening point: 90°C) B4: Haritac FK125 (Harima Chemicals, rosin ester, softening point: 125°C) B5: Haritac F85 (Harima Chemicals, rosin ester, softening point: 85°C)

[0059] <Wax (C)> C1: HNP-9 (Nippon Seiro Co., Ltd., paraffin wax, DSC melting point: 76°C, oil content: 0.1%) C2: HNP-5 (Nippon Seiro Co., Ltd., paraffin wax, DSC melting point: 63°C, oil content: 0.1%)

[0060] <Wax (D)> D1: FT WAX T-70 (Qindao Bouni Chemical Co., Ltd., Fischer-Tropsch wax, DSC melting point: 70°C, oil content: 3.0%) D2: Sasol H1 (manufactured by Sasol Chemical Industries, Fischer-Tropsch wax, DSC melting point: 98°C, oil content: 1.0%) D3: Parraffin Wax 130 (Nippon Seiro Co., Ltd., paraffin wax, DSC melting point: 56°C, oil content: 0.3%)

[0061] <Additives> Antioxidant: Irganox1010 (BASF Japan) Anti-blocking agent: Silicone oil KF-96-100cs (Shin-Etsu Silicone Co., Ltd.)

[0062] According to the evaluation results, the hot melt composition of the present application, which is made of an ethylene-unsaturated ester copolymer with a specific melt mass flow rate and two types of wax with different oil contents, has good coatability, and further has excellent heat resistance and easy-opening properties, and is shown to be useful as a hot melt adhesive for yogurt lids. In particular, in the examples using 15 mass% or more of an ethylene-unsaturated ester copolymer (A1) having a specific melt mass flow rate, 10 mass% or more of a wax (C) having a low oil content, and 10 mass% or more of a wax (D) having a high oil content, respectively, excellent heat resistance and suitable easy-openability were achieved at the same time. On the other hand, Comparative Examples 1 and 2, in which the ethylene-unsaturated ester copolymer with a specific melt mass flow rate was less than 10% by mass, were insufficient in heat resistance. Comparative Example 5, in which only a wax with a low oil content was used, showed excellent heat resistance but was insufficient in easy opening. Comparative Example 6, in which only a wax with a high oil content was used, showed suitable easy opening but was insufficient in heat resistance.

Claims

1. Ethylene-unsaturated ester copolymer (A) containing an ethylene-unsaturated ester copolymer (A1) having a melt mass flow rate of 3 to 70 g / 10 min: 25 to 50% by mass, Tackifying resin (B): 10 to 30% by mass, Wax (C) having an oil content of less than 0.2% by mass: 5 to 40% by mass, and Wax (D) having an oil content of 0.2% by mass or more and 4.0% by mass or less: Contains 5 to 40% by mass, The wax (C) and the wax (D) are contained in a total amount of 30 to 50 mass %, A hot melt composition for yogurt lid material, comprising 10 to 50 mass% of the ethylene-unsaturated ester copolymer (A1).

2. The hot melt composition for yogurt covering material according to claim 1, wherein the ethylene-unsaturated ester copolymer (A) is a polymer of ethylene and an unsaturated ester monomer, and contains a structural unit derived from the unsaturated ester monomer in a range of 25 to 35 mass% based on the mass of the ethylene-unsaturated ester copolymer (A).

3. The hot melt composition for yogurt lid material according to claim 1 or 2, wherein the wax (C) and the wax (D) are each independently a wax having a melting point of 60 to 100°C.

4. The hot melt composition for yogurt lid material according to any one of claims 1 to 3, wherein the wax (C) and the wax (D) are each independently at least one selected from the group consisting of paraffin wax and Fischer-Tropsch wax.

5. The hot melt composition for yogurt lid material according to any one of claims 1 to 4, wherein the softening point of the tackifier resin (B) is in the range of 90 to 150 ° C.

6. A yogurt lid material comprising a hot melt layer made of the hot melt composition according to any one of claims 1 to 5 on one surface of a substrate.

7. The yogurt lid material according to claim 6, wherein the base material has at least two or more layers selected from the group consisting of a resin layer, a paper layer, and a metal layer.

8. The yogurt lid material according to claim 7, wherein the resin layer contains at least one resin selected from the group consisting of polyethylene resin, polypropylene resin, and polyethylene terephthalate resin.

9. A set of components for an openable sealed yogurt container, comprising a container and the yogurt lid material according to any one of claims 6 to 8.

10. An openable sealed yogurt container, the opening of which is heat-sealed with a hot melt layer of the yogurt lid material according to any one of claims 6 to 8.

11. The coating amount of the hot melt layer is 10 to 30 g / m 2 The openable sealed yogurt container according to claim 10, wherein the opening strength measured in accordance with JIS S 0021-2:2018 is in the range of 5 to 20 N.

Citation Information

Patent Citations

  • Hot melt adhesive composition

    JP1990055783A

  • Hot-melt composition

    JP1998130436A

  • Hot-melt adhesive

    JP2000204336A

  • Hot-melt adhesive having aptitude to recycling of used paper

    JP2003213242A

  • Hot-melt adhesive for bookbinding and calendar production

    JP2004010769A