Laminating adhesives, laminates and packaging materials
The laminating adhesive with a polyol composition and aminosilane compound addresses tunneling and transparency issues in laminating adhesives, ensuring fast curing and enhanced biomass content.
Patent Information
- Application Number
- JP2020218510
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-28
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-12-28
AI Technical Summary
Existing laminating adhesives using castor oil-based compositions suffer from poor initial cohesive strength, leading to tunneling and reduced transparency due to wide molecular weight distribution and low molecular weight components, particularly when bonding materials with differing elongation properties.
A laminating adhesive comprising a polyol composition with 5-33% castor oil and polyether urethane polyol, combined with a silane compound, specifically an aminosilane, to enhance interfacial adhesion and suppress tunneling while maintaining transparency.
The adhesive achieves fast curing, improved biomass content, and prevents tunneling, maintaining transparency even under varying material elongation conditions.
Smart Images

Figure 0007567467000001 
Figure 0007567467000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminating adhesive suitable for laminating various plastic films and metal-deposited films, and a laminate using the same. The present invention further relates to a package using the laminate for food, medicine, cosmetics, detergent, miscellaneous goods, etc. [Background technology]
[0002] Conventionally, a laminate in which at least a base layer containing an oriented plastic or the like and a sealant layer for welding the packaging materials together has been used as a packaging material for constituting a packaged product for filling and packaging various items such as food and drink, medicines, cosmetics, sanitary products, daily necessities, etc. Usually, the laminate further includes an adhesive layer for bonding the layers of the laminate. In recent years, with the growing demand for the creation of a recycling-oriented society, there is a desire to move away from fossil fuels in the field of laminates that make up packaging materials, and the use of biomass has attracted attention. Biomass is a non-exhaustible resource that is an industrial resource originating from the constituent materials of living organisms, and is a carbon-neutral renewable energy source.
[0003] In response to such demands, for example, Patent Document 1 discloses an adhesive composition containing a polyol component that contains urethane-modified castor oil, which is a reaction product between some of the hydroxyl groups in castor oil and a diisocyanate, and a polyisocyanate component. Furthermore, Patent Document 2 discloses a laminating adhesive that contains a polyisocyanate component that includes a reaction product of a polyol containing a castor oil-containing polyol and a polyisocyanate, and a polyol component. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-030905 A [Patent Document 2] JP 2019-137712 A Summary of the Invention [Problem to be solved by the invention]
[0005] The adhesives described in Patent Documents 1 and 2 use castor oil, which improves the biomass ratio and has a fast curing rate. However, because castor oil has a wide molecular weight distribution and contains a large amount of low molecular weight components, adhesives using castor oil have poor initial cohesive strength, which causes a problem that streaky lifting (tunneling) occurs in the width direction of the laminate after bonding. The tunneling phenomenon is more likely to occur the greater the difference in stretchability between the two substrates bonded with the adhesive. For example, a laminate bonded between a biaxially oriented polypropylene (OPP) film, which is easy to stretch, and an aluminum-deposited polyethylene terephthalate (VMPET) film, which is difficult to stretch, is particularly prone to tunneling. Furthermore, the adhesive described in Patent Document 2 uses castor oil on the polyisocyanate curing agent side, and therefore has the problem that the curing agent becomes cloudy over time, impairing the transparency of the adhesive. Therefore, an object of the present invention is to provide a laminating adhesive that has an improved biomass degree, a fast curing rate, and is capable of suppressing tunneling even in configurations in which tunneling is likely to occur, and has excellent transparency, as well as a laminate and packaging body that use the adhesive and have an improved biomass degree and suppressed tunneling. [Means for solving the problem]
[0006] As a result of intensive research aimed at solving the above problems, the present inventors have found that the above problems can be solved by the embodiments described below, and have thus completed the present invention.
[0007] A laminating adhesive according to one embodiment of the present invention is a laminating adhesive containing a polyol composition, a polyisocyanate composition, and a silane compound, characterized in that the polyol composition contains a polyol containing a castor oil and a polyether polyol, and a polyether urethane polyol which is a reaction product of a polyisocyanate, the castor oil content is 5 to 33 mass% based on the solid mass of the polyol composition, and the silane compound contains an aminosilane compound.
[0008] A laminating adhesive according to one aspect of the present invention is characterized in that the aminosilane compound is an aminosilane compound having a primary amino group.
[0009] A laminating adhesive according to one aspect of the present invention is characterized in that the content of the aminosilane compound is 0.05 to 0.5 mass % based on the solid content mass of the polyol composition.
[0010] A laminating adhesive according to one aspect of the present invention is characterized in that the silane compound further contains an epoxy silane compound.
[0011] A laminating adhesive according to one aspect of the present invention is characterized in that the content of the epoxy silane compound is 0.1 to 0.5 mass % or less based on the solid content mass of the polyol composition.
[0012] A laminate according to one aspect of the present invention is characterized in that an adhesive layer made of the above-described laminating adhesive is disposed between at least two substrates.
[0013] A packaging body according to one aspect of the present invention is characterized by using the above-mentioned laminate. Effect of the Invention
[0014] The present invention can provide a laminating adhesive that has an improved biomass degree, a fast curing rate, and is capable of suppressing tunneling even in configurations in which tunneling is likely to occur, and has excellent transparency, as well as a laminate and packaging body that use the adhesive and has an improved biomass degree and suppresses tunneling. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] <Laminating adhesive> The laminating adhesive of the present invention contains a polyol composition, a polyisocyanate composition, and a silane compound, the polyol composition contains a polyol containing a castor oil and a polyether polyol, and a polyether urethane polyol which is a reaction product of a polyisocyanate, the castor oil content is 5 to 33 mass% based on the solid mass of the polyol composition, and the silane compound contains an aminosilane compound. It is common to use polyols such as castor oils to improve the biomass ratio. However, polyether urethane polyols made from castor oils tend to have a large molecular weight distribution and contain a large amount of low molecular weight components, so the adhesive finally obtained has poor cohesive strength at the initial stage of lamination and is prone to streaky lifting (tunneling) in the width direction of the laminate after bonding. In contrast to the above, the laminating adhesive of the present invention can improve the interface adhesion and suppress the occurrence of tunneling by combining a predetermined amount of polyol, which is castor oil, with an aminosilane compound. Furthermore, since the laminating adhesive of the present invention uses castor oil on the polyol composition (polyol base) side, even when an aged polyol base is mixed to make an adhesive, it has excellent transparency. The present invention will be described in detail below.
[0016] <Polyol Composition> The polyol composition used in the present invention is a composition containing a polyol compound having two or more hydroxyl groups as a main component. The polyol composition in the present invention is characterized in that it contains a polyol containing castor oils and polyether polyol, and a polyether urethane polyol which is a reaction product of polyisocyanate, and the castor oil content is in the range of 5 to 33 mass% based on the solid mass of the polyol composition. When a polyether urethane polyol obtained by urethane-modifying castor oil and polyether polyol is included, the branching ratio of the adhesive layer formed by the reaction with the polyisocyanate composition described below is lower than when only castor oil is used. This lowers the glass transition point (Tg) of the adhesive layer, resulting in excellent adhesive strength of the laminate. In addition, by setting the content of castor oils in the range of 5 to 33 mass% based on the solid content mass of the polyol composition, it is possible to achieve both an excellent curing speed and suppression of tunneling while increasing the biomass degree. The content of castor oils is preferably in the range of 5 to 25 mass%.
[0017] [Polyether urethane polyol] The polyol that is the raw material of the polyether urethane polyol contains at least castor oil and polyether polyol.
[0018] (Castor oil) The castor oils are not particularly limited, and any known castor oil or castor oil derivative containing a hydroxyl group can be used. One type may be used alone, or two or more types may be used in combination. Examples of castor oil derivatives containing hydroxyl groups include dehydrated castor oil, hydrogenated castor oil which is a hydrogenated product of castor oil, castor oil fatty acid, dehydrated castor oil fatty acid, castor oil fatty acid condensate, ethylene oxide 5 to 50 mole adduct of castor oil, and castor oil-based polyols. In particular, from the viewpoint of the production quality stability of the polyether urethane polyol, the acid value of the castor oil is preferably in the range of 0.1 to 5.0 mgKOH / g, more preferably in the range of 0.1 to less than 2.0 mgKOH / g, and even more preferably in the range of 0.1 to 1.0 mgKOH / g. The polyol that is the raw material of the polyether urethane polyol preferably contains castor oils in the range of 5 to 33% by mass based on the mass of the polyurethane polyol.
[0019] (Polyether polyol) The polyether polyol may be any compound having two or more hydroxyl groups and two or more ether bonds in the molecule, and one type may be used alone, or two or more types may be used in combination. Examples of polyether polyols include polyalkylene glycols such as polyethylene glycol, polytrimethylene glycol, polypropylene glycol, polytetramethylene glycol, and polybutylene glycol; polyethylene glycol / polypropylene glycol block copolymers; and propylene oxide / ethylene oxide random polyethers. Alternatively, an addition polymer obtained by addition polymerization of an oxirane compound such as ethylene oxide, propylene oxide, butylene oxide, or tetrahydrofuran to a low molecular weight polyol initiator such as water, ethylene glycol, propylene glycol, trimethylolpropane, glycerin, sorbitol, or sucrose may be used as the polyether polyol. Examples of the addition polymer include a propylene glycol propylene oxide adduct, a glycerin propylene oxide adduct, a sorbitol-based propylene oxide adduct, and a sucrose-based propylene oxide adduct. The polyether polyol is preferably a polyalkylene glycol.
[0020] The number average molecular weight of the polyether polyol is preferably 100 to 5,000, and more preferably 300 to 2,500. The number average molecular weight in this specification is a value calculated in terms of standard polystyrene using a GPC (gel permeation chromatography) "Shodex GPC System-21" manufactured by Showa Denko KK and tetrahydrofuran as a solvent. When the polyether polyol contains a plurality of polyether polyols, the number average molecular weight of the polyether polyol can be determined from the number average molecular weights of the individual polyether polyols and the mass ratio thereof.
[0021] (Polyisocyanate) The polyisocyanate that is the raw material of the polyether urethane polyol is not particularly limited, and any known polyisocyanate compound can be used. As specific examples of such polyisocyanate compounds, the description in the <Polyisocyanate composition> described below can be cited, and one type may be used alone, or two or more types may be used in combination. Among these, from the viewpoints of rigidity and heat resistance, aromatic diisocyanates such as diphenylmethane diisocyanate, carbodiimide-modified diphenylmethane diisocyanate, phenylene diisocyanate, tolylene diisocyanate, and naphthalene diisocyanate; and aromatic polyisocyanates such as polymethylene polyphenyl polyisocyanate are preferred.
[0022] The weight average molecular weight of the polyetherurethane polyol, which is a reaction product of a polyol containing castor oil and a polyether polyol, and a polyisocyanate, is preferably in the range of 5,000 to 45,000. The polyetherurethane polyol may be modified, or may be a polyetherurethane polyol reacted with an acid anhydride to introduce a carboxyl group. As the acid anhydride, the acid anhydrides described in the section [Other polyol compounds] described later can be used.
[0023] [Other polyol compounds] The polyol composition in the present invention may contain other polyol compounds as long as the effects of the present invention are not impaired. The other polyol compounds may be used alone or in combination of two or more. Other polyol compounds include, for example, polyester polyol, polyether polyol, polyurethane polyol, polyesteramide polyol, acrylic polyol, polycarbonate polyol, polycaprolactone polyol, polyvalerolactone polyol, polyolefin polyol, polyhydroxyalkane, castor oil, and mixtures thereof, as well as ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-5-pentanediol, 1,6-hexanediol, neopentanediol, and the like. Examples of the glycols that can be used include glycols such as diethyl glycol, methylpentane glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, bishydroxyethoxybenzene, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, and triethylene glycol; polyalkylene glycols having a number average molecular weight of 200 to 3,000; trifunctional or tetrafunctional aliphatic alcohols such as glycerin, trimethylolpropane, and pentaerythritol; and polyols in which the above-mentioned glycols or polyols are added to the above-mentioned trifunctional or tetrafunctional aliphatic alcohols.
[0024] The other polyol compounds may be acid-modified compounds in which some of the hydroxyl groups in the polyol are acid-modified, compounds in which a carboxyl group is introduced by reacting with an acid anhydride, or compounds in which a urethane bond is introduced by reacting with a diisocyanate. Examples of the acid anhydride include pyromellitic anhydride, mellitic anhydride, trimellitic anhydride, and trimellitic ester anhydride. Examples of the trimellitic ester anhydride include ester compounds obtained by esterifying an alkylene glycol or alkanetriol having 2 to 30 carbon atoms with trimellitic anhydride, and specific examples thereof include ethylene glycol bisanhydrotrimellitate, propylene glycol bisanhydrotrimellitate, and the like. Examples of the diisocyanate include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, 1,5-naphthalene diisocyanate, hexamethylene diisocyanate, and hydrogenated diphenylmethane diisocyanate.
[0025] <Polyisocyanate composition> The polyisocyanate composition used in the present invention is a composition containing a polyisocyanate compound as a main component. The polyisocyanate compound is a compound having two or more isocyanate groups, and one kind may be used alone or a plurality of kinds may be used in combination. Examples of the polyisocyanate compound include aromatic polyisocyanates, araliphatic polyisocyanates, aliphatic polyisocyanates, and alicyclic polyisocyanates, and these may be modified products.
[0026] Examples of the aromatic polyisocyanate include aromatic diisocyanates such as diphenylmethane diisocyanate, carbodiimide-modified diphenylmethane diisocyanate, phenylene diisocyanate, tolylene diisocyanate, and naphthalene diisocyanate; and aromatic polyisocyanates such as polymethylene polyphenyl polyisocyanate. Examples of the araliphatic polyisocyanate include araliphatic diisocyanates such as 1,3- or 1,4-xylylene diisocyanate or a mixture thereof, ω,ω'-diisocyanato-1,4-diethylbenzene, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene or a mixture thereof. Examples of the aliphatic polyisocyanate include aliphatic diisocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, 2,6-diisocyanate methyl caproate, lysine diisocyanate, and dimer acid diisocyanate. Examples of alicyclic polyisocyanates include alicyclic diisocyanates such as 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, isophorone diisocyanate, 4,4'-methylene bis(cyclohexyl isocyanate), methyl 2,4-cyclohexane diisocyanate, methyl 2,6-cyclohexane diisocyanate, 1,4-bis(isocyanate methyl)cyclohexane, 1,3-bis(isocyanate methyl)cyclohexane, and norbornene diisocyanate.
[0027] Examples of modified polyisocyanates include allophanate-type modified products, isocyanurate-type modified products, biuret-type modified products, adduct-type modified products, and polyurethane polyisocyanates obtained by reacting the above-mentioned polyisocyanate compounds with a polyol component under conditions of excess isocyanate groups. The polyol component that forms the modified product of the polyisocyanate is not particularly limited and can be selected from known polyols. Examples of the polyol include polyester polyols, polyester urethane polyols, polycarbonate polyols, polycaprolactone polyols, polyether polyols such as polyalkylene glycols, polyether urethane polyols, polyolefin polyols, acrylic polyols, silicone polyols, castor oil-based polyols, and fluorine-based polyols, as well as low molecular weight polyols such as ethylene glycol, propylene glycol, trimethylolpropane, glycerin, sorbitol, and sucrose.
[0028] The polyisocyanate composition preferably contains a compound having a structural unit derived from an aromatic polyisocyanate, more preferably contains a modified product of an aromatic polyisocyanate, and even more preferably contains a polyurethane polyisocyanate obtained by reacting an aromatic polyisocyanate with a polyalkylene glycol, or a trimethylolpropane adduct of an aromatic polyisocyanate. Such polyisocyanate compounds are preferred from the viewpoints of adhesive strength and economy.
[0029] <Silane compounds> The silane compound in the present invention is a compound having a hydrolyzable silyl group, and has the function of improving the adhesive strength to a metal foil or a metal vapor deposition layer. The silane compound in the present invention must contain an aminosilane compound having an amino group and a hydrolyzable silyl group. Examples of such aminosilane compounds include 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethyldimethoxysilane and other aminosilane compounds having a primary amino group; and N-phenyl-3-aminopropyltrimethoxysilane and other aminosilane compounds having a secondary amino group. Among these, from the viewpoint of reactivity, preferred are aminosilane compounds having a primary amino group, more preferred are aminosilane compounds having one primary amino group in one molecule, and even more preferred is 3-aminopropyltrimethoxysilane. The content of the aminosilane compound is preferably in the range of 0.05 to 0.5 mass %, more preferably in the range of 0.1 to 0.3 mass %, based on the solid mass of the polyol composition. The above range is preferable because it provides excellent interface adhesion without impairing solution stability.
[0030] The silane compound may contain other silane compounds other than the aminosilane compound, as long as the effect of the present invention is not impaired. Examples of other silane compounds include epoxy silane compounds such as β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, and γ-glycidoxypropyltriethoxysilane; vinyl silane compounds such as vinyltris(β-methoxyethoxy)silane, vinyltriethoxysilane, vinyltrimethoxysilane, and γ-methacryloxypropyltrimethoxysilane; hexamethyldisilazane, and γ-mercaptopropyltrimethoxysilane. From the viewpoint of solution stability, the silane compound in the present invention preferably further contains an epoxy silane compound. When the silane compound further contains an epoxysilane compound, the content of the epoxysilane compound is preferably in the range of 0.1 to 0.7 mass% based on the solid mass of the polyol composition, and more preferably in the range of 0.1 to 0.5 mass%. The above range is preferable because it provides excellent interface adhesion.
[0031] <Solvent> The laminating adhesive of the present invention can be used as a solvent-based or solventless adhesive, and may contain a solvent as necessary. Note that the "solvent" in the present invention refers to an organic solvent having high solubility and capable of dissolving the polyol compound, the polyisocyanate compound, and the silane compound. Examples of the organic solvent having high solubility include toluene, xylene, methylene chloride, tetrahydrofuran, methanol, ethanol, isopropyl alcohol, methyl acetate, ethyl acetate, n-butyl acetate, acetone, methyl ethyl ketone, cyclohexanone, toluene, xylol, n-hexane, and cyclohexane. The organic solvent is preferably inactive against polyisocyanates, and examples of the organic solvent include ester solvents such as ethyl acetate, ketone solvents such as methyl ethyl ketone, and aromatic hydrocarbon solvents such as toluene and xylene.
[0032] The viscosity of the laminating adhesive of the present invention at room temperature to 150°C is preferably 100 to 10,000 mPa·s, more preferably 100 to 5,000 mPa·s, and even more preferably 100 to 10,000 mPa·s, more preferably 100 to 5,000 mPa·s at room temperature to 100°C. When the viscosity is 100 to 5,000 mPa·s at room temperature to 100°C, it can be used as a solventless adhesive. If the viscosity of the laminating adhesive is higher than the above range, it may be diluted with the above organic solvent. The content of the organic solvent depends on the required viscosity, but it is generally desirable to include the organic solvent in the range of 50 to 70 mass % relative to the adhesive resin.
[0033] The laminating adhesive of the present invention is a reactive adhesive obtained by blending the above-mentioned polyol composition, polyisocyanate composition, silane compound, and, as necessary, other components. The silane compound may be blended when the polyol composition and the polyisocyanate composition are mixed, or may be blended in advance in the polyol composition and / or the polyisocyanate composition. The blending ratio of the polyol composition and the polyisocyanate composition is preferably such that the molar equivalent ratio [NCO / OH] of the total isocyanate groups in the polyisocyanate composition to the total hydroxyl groups in the polyol composition is in the range of 1.0 to 5.0, more preferably 1.3 to 3.0.
[0034] The acid value immediately after the lamination adhesive is blended is preferably 3.0 mgKOH / g or less, and more preferably 1.0 mgKOH / g or less.
[0035] <Other ingredients> The laminating adhesive of the present invention may further contain other components in order to satisfy various physical properties required for the adhesive or packaging material. The other components may be blended in advance with the polyol composition and / or the polyisocyanate composition, or may be blended when the polyol composition and the polyisocyanate composition are mixed. The other components may be used alone or in combination of two or more.
[0036] (Phosphoric acid or phosphoric acid derivatives) The laminating adhesive of the present invention may contain phosphoric acid or a phosphoric acid derivative from the viewpoint of improving adhesive strength to metallic materials such as metal foil. The phosphoric acid may be any phosphoric acid having at least one free oxygen acid, and examples of the phosphoric acid include phosphoric acids such as hypophosphorous acid, phosphorous acid, orthophosphoric acid, and hypophosphoric acid; and condensed phosphoric acids such as metaphosphoric acid, pyrophosphoric acid, tripolyphosphoric acid, polyphosphoric acid, and ultraphosphoric acid. Examples of phosphoric acid derivatives include those obtained by partially esterifying the above phosphoric acid with alcohols while leaving at least one free oxygen acid. Examples of the alcohols include aliphatic alcohols such as methanol, ethanol, ethylene glycol, and glycerin; and aromatic alcohols such as phenol, xylenol, hydroquinone, catechol, and phloroglucinol. The content of phosphoric acid or a derivative thereof is preferably 0.01 to 10 mass %, more preferably 0.05 to 5 mass %, and particularly preferably 0.05 to 1 mass %, based on the solid mass of the laminating adhesive.
[0037] (Leveling agent or defoamer) The laminating adhesive of the present invention may further contain a leveling agent or an antifoaming agent in order to improve the appearance of the laminate. Examples of the leveling agent include polyether-modified polydimethylsiloxane, polyester-modified polydimethylsiloxane, aralkyl-modified polymethylalkylsiloxane, polyester-modified hydroxyl-containing polydimethylsiloxane, polyetherester-modified hydroxyl-containing polydimethylsiloxane, acrylic copolymer, methacrylic copolymer, polyether-modified polymethylalkylsiloxane, acrylic acid alkyl ester copolymer, methacrylic acid alkyl ester copolymer, and lecithin. Examples of the defoaming agent include silicone resin, silicone solution, and copolymers of alkyl vinyl ether, alkyl acrylate, and alkyl methacrylate.
[0038] (Reaction accelerator) The laminating adhesive of the present invention may further contain a reaction accelerator to accelerate the curing reaction. Examples of the reaction accelerator include metal catalysts such as dibutyltin diacetate, dibutyltin dilaurate, dioctyltin dilaurate, and dibutyltin dimaleate; tertiary amines such as 1,8-diaza-bicyclo(5,4,0)undecene-7, 1,5-diazabicyclo(4,3,0)nonene-5,6-dibutylamino-1,8-diazabicyclo(5,4,0)undecene-7; and reactive tertiary amines such as triethanolamine.
[0039] (Other additives) The laminate composition of the present invention may contain various additives within the range that does not impair the effects of the present invention. Examples of additives include inorganic fillers such as silica, alumina, mica, talc, aluminum flakes, and glass flakes, layered inorganic compounds, stabilizers (antioxidants, heat stabilizers, ultraviolet absorbers, hydrolysis inhibitors, etc.), rust inhibitors, thickeners, plasticizers, antistatic agents, lubricants, antiblocking agents, colorants, fillers, crystal nucleating agents, and catalysts for adjusting the curing reaction.
[0040] <Laminate> The laminate of the present invention is one in which an adhesive layer made of the above-mentioned laminating adhesive is disposed between at least two substrates. The laminate can be formed, for example, by applying the laminating adhesive to a first substrate, optionally drying the first substrate, laminating the second substrate, and curing the adhesive layer located between the two substrates under a temperature condition of 20°C to 60°C, but is not limited to this configuration, and another layer may be laminated via an adhesive layer or the like. The amount of the lamination adhesive applied after drying is optional, but in terms of laminate appearance and adhesive performance stability, it is preferably 1 to 4 g / m in the case of a solvent-free adhesive. 2 , more preferably 1 to 2 g / m 2 In the case of a solvent-based adhesive, the adhesive strength is preferably in the range of 1 to 6 g / m 2 , more preferably 2 to 4 g / m 2 In addition, the thickness of the laminate is preferably 10 μm or more from the viewpoint of strength and durability as a packaging material.
[0041] [Base material] The substrate is not particularly limited and examples thereof include plastic films, papers, gas barrier substrates, sealants, etc., which are commonly used for packaging applications, and the two substrates may be the same or different. Examples of plastic films that can be used include polyester resin films such as polyethylene terephthalate, polyethylene naphthalate (PEN), and polylactic acid (PLA); polyolefin resin films such as polyethylene (PE) and polypropylene (PP); polystyrene resin films; polyamide resin films such as nylon 6 and poly-p-xylylene adipamide (MXD6 nylon); polycarbonate resin films; polyacrylonitrile resin films; polyimide resin films; laminates thereof (e.g., nylon 6 / MXD6 / nylon 6, nylon 6 / ethylene-vinyl alcohol copolymer / nylon 6), and mixtures thereof. Among these, those having mechanical strength and dimensional stability are preferred. The plastic film preferably has a thickness of 5 to 50 μm, more preferably 10 to 30 μm.
[0042] The paper includes natural paper and synthetic paper. As the gas barrier substrate, aluminum foil and plastic films having a vapor-deposited layer of aluminum, silica, alumina, etc. are preferable. For example, in the case of aluminum foil, a thickness in the range of 3 to 50 μm is preferable from an economical point of view.
[0043] Examples of the sealant include polyethylenes such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and high-density polyethylene (HDPE), acid-modified polyethylene, polypropylene (PP), acid-modified polypropylene, copolymerized polypropylene, ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid ester copolymer, ethylene-(meth)acrylic acid copolymer, polyolefin resins such as ionomers, etc. Among these, polypropylene-based resins are preferred from the viewpoint of heat resistance during retort, and unstretched polypropylene is particularly preferred from the viewpoint of heat sealability. The thickness of the sealant is not particularly limited, but is preferably in the range of 10 to 60 μm, more preferably 15 to 40 μm, taking into consideration processability into packaging, heat sealing properties, etc. Also, by providing the sealant with unevenness with a height difference of 5 to 20 μm, it is possible to impart slipperiness to the sealant and tearability of the packaging. Furthermore, the various sealants may have a vapor-deposited layer of aluminum, silica, alumina, or the like in addition to the aluminum foil.
[0044] [Print layer] The laminate of the present invention may further have a printed layer. The printed layer is a layer on which any desired printed pattern such as letters, numbers, pictures, figures, symbols, patterns, etc. is formed for decoration, display of contents, display of expiration date, display of manufacturer, seller, etc., or for imparting aesthetics, and includes a solid printed layer. The printed layer can be formed using a conventionally known pigment or dye, and the method for forming the printed layer is not particularly limited. Generally, the printing layer is formed on the substrate using a printing ink containing a colorant such as a pigment or dye. The method for applying the printing ink is not particularly limited, and the printing ink can be applied by a method such as gravure coating, flexo coating, roll coating, bar coating, die coating, curtain coating, spin coating, inkjet, etc. The printing layer is formed by leaving the ink alone or, if necessary, blowing air, heating, drying under reduced pressure, irradiating with ultraviolet light, etc. The thickness of the printed layer is preferably 0.1 to 10 μm, more preferably 1 to 5 μm, and further preferably 1 to 3 μm.
[0045] The structure of the laminate is not particularly limited, but is preferably a structure in which at least one plastic film or gas barrier substrate and a sealant are laminated together. Specific examples of the structure are listed below, but are not limited thereto. Biaxially oriented polypropylene (OPP) / printing layer / adhesive layer / CPP, OPP / printed layer / adhesive layer / AL vapor deposition CPP, OPP / printing layer / adhesive layer / PE, Printing layer / OPP / adhesive layer / CPP, NY / printing layer / adhesive layer / PE, Printing layer / NY / Adhesive layer / CPP NY / printing layer / adhesive layer / CPP, PET / printing layer / adhesive layer / CPP, Printing layer / PET / adhesive layer / CPP PET / printing layer / adhesive layer / NY / adhesive layer / CPP, Transparent deposition PET / printing layer / adhesive layer / NY / adhesive layer / CPP, PET / printed layer / adhesive layer / AL-deposited PET / adhesive layer / PE, PET / printing layer / adhesive layer / AL / adhesive layer / CPP, PET / printing layer / adhesive layer / AL / adhesive layer / PE, PET / printing layer / adhesive layer / NY / adhesive layer / AL / adhesive layer / CPP, PET / printing layer / adhesive layer / AL / adhesive layer / NY / adhesive layer / CPP EXAMPLES
[0046] The present invention will be described in more detail below with reference to examples and comparative examples. In the examples and comparative examples, "parts" and "%" mean "parts by mass" and "% by mass" unless otherwise specified.
[0047] <Production of polyether urethane polyol> (Polyether urethane polyol A1) 18 parts of castor oil polyol A, 40 parts of bifunctional polypropylene glycol having a number average molecular weight of about 400, 20 parts of bifunctional polypropylene glycol having a number average molecular weight of 2,000, and 22 parts of tolylene diisocyanate (hereinafter, TDI) were charged into a reaction vessel, and dioctyltin dilaurate was added as a reaction catalyst at 0.1% relative to the total mass of castor oil polyol A, bifunctional polypropylene glycol having a number average molecular weight of about 400, bifunctional polypropylene glycol having a number average molecular weight of 2,000, and tolylene diisocyanate, and the mixture was heated at 80 to 90 ° C. for 2 to 4 hours while stirring under a nitrogen gas flow to cause a urethane reaction. The disappearance of the isocyanate group was confirmed by FT-IR, and the mixture was diluted with ethyl acetate to obtain a solution of polyether urethane polyol (A1) having a solid content concentration of 70%.
[0048] (Polyether urethane polyol A2~A8) Solutions of polyether urethane polyols A2 to A8 were obtained in the same manner as A1, except that the blending compositions were changed to those shown in Table 1. The values in Table 1 represent "parts" unless otherwise specified, and blanks indicate that no blend was added.
[0049] [Table 1]
[0050] The abbreviations in Table 1 are as follows: Castor oil polyol A: Toyokuni Oil Co., Ltd. "Industrial No. 1 Castor Oil", acid value 0.5 mg KOH / g Castor oil-based polyol B: "Kaku Koichi" manufactured by Ito Oil, acid value 1.5 mg KOH / g Castor oil-based polyol C: "Koichi" manufactured by Ito Oil, acid value 3.0 mg KOH / g PPG400: Bifunctional polypropylene glycol with a number average molecular weight of approximately 400 PPG2000: Bifunctional polypropylene glycol with a number average molecular weight of 2,000 TDI: 2.4-tolylene diisocyanate 80%, 2.6-tolylene diisocyanate 20%
[0051] <Production of polyisocyanate compounds> (Polyether urethane polyisocyanate B1) 35 parts of castor oil polyol C (Ito Oil Mills "Koichi", acid value 1.5mgKOH / g), 20 parts of bifunctional polypropylene glycol with number average molecular weight of 2,000, 10 parts of bifunctional polypropylene glycol with number average molecular weight of 400, and 35 parts of 4,4'-diphenylmethane diisocyanate were charged into a reaction vessel, and the urethane reaction was carried out by heating at 70-80℃ for 4-7 hours while stirring under a nitrogen gas flow. After the reaction was completed, the mixture was diluted with ethyl acetate to 75% nonvolatile content to obtain a solution of polyether urethane polyisocyanate B1. The viscosity of the B1 solution was 3,000mPa·s / 25℃.
[0052] <Manufacture of laminating adhesives> [Example 1] A polyether urethane polyol solution and a polyisocyanate solution were mixed to obtain the solid content mass shown in Table 1, and diluted with ethyl acetate to obtain a laminating adhesive with a solid content of 30%. The biomass degree of the obtained adhesive is shown in Table 2.
[0053] [Examples 2 to 13, Comparative Examples 1 to 5] Except for changing the blending composition to that shown in Table 2, the same procedure as in Example 1 was carried out to obtain laminating adhesives each having a solid content of 30%.
[0054] <Evaluation of lamination adhesives> The obtained adhesive was used to prepare a laminate, which was then used to carry out the following evaluations. The results are shown in Table 2.
[0055] [Laminate manufacturing] [Laminate preparation: OPP / adhesive layer / VMPET, coating speed 200m / min] The adhesive obtained above was applied to a corona-treated OPP film (Toyobo P-2161, thickness 20μm) using a laminator at a coating speed of 200m / min, and the solvent was evaporated in a drying oven (60℃-70℃-80℃ triple oven, furnace length 2.5m), after which the adhesive-coated surface was bonded to a 12μm-thick VMPET film (Reiko Dialaster H27, thickness 12μm, aluminum-deposited PET) to obtain a laminate. The solid coating amount of the adhesive was 2.5g / m 2 It was decided.
[0056] [Tunneling] The laminate was stored in an atmosphere of 40° C. for 24 hours, and then visually observed to evaluate whether streaky lifting (tunneling) occurred from the edges in the width direction. 〇: No tunneling occurred (very good) ○△: Tunneling occurred less than 5 mm from the end (good) △: Tunneling occurs at a length of 5mm or more and less than 10mm from the end (usable) ×: Tunneling occurs at a length of 10 mm or more from the end (unusable)
[0057] [Curing speed] The laminate was stored in a desiccator containing silica gel at 40° C. for 24 hours, and the disappearance of isocyanate groups was confirmed every hour by FT-IR and evaluated according to the following criteria. ○: Isocyanate groups disappear within 24 hours ×: Isocyanate groups disappear within 24 hours or more
[0058] [Solution appearance, viscosity] A 70% solid content solution of polyetherurethane polyols (A1 to A8) and a 75% solid content solution of polyisocyanates (CAT-29B, CAT-16B, B2) were left to stand for one month in a room temperature (20°C) environment. The 70% solid content solutions of polyetherurethane polyols (A1 to A8) and the 75% solid content solutions of polyisocyanates (CAT-29B, CAT-16B, B2) after the aging were mixed in the same manner as in Examples 1 to 13 and Comparative Examples 1 to 5 to obtain adhesives. The solution appearance of the obtained adhesives was visually observed in a 25°C environment. In addition, the solution viscosity (seconds) of the adhesive was measured using a Zahn cup #3, and the difference in seconds was calculated when compared with the solution viscosity (seconds) of an adhesive made of polyetherurethane polyols and polyisocyanates before the aging, and the difference was evaluated according to the following criteria. 〇: The solution appearance is transparent and the difference in solution viscosity is within 2.0 seconds ×: The solution appearance is cloudy or the difference in solution viscosity exceeds 2.0 seconds.
[0059] The abbreviations in Table 2 are as follows: PPG1000: Trifunctional polypropylene glycol with a number average molecular weight of 1,000 CAT-29B: Toyo-Morton polyisocyanate (weight average molecular weight approx. 9,000, solid content 75%) CAT-16B: Toyo-Morton polyisocyanate (weight average molecular weight approx. 5,000, solid content 75%) KBM-903: 3-aminopropyltrimethoxysilane manufactured by Shin-Etsu Silicone Co., Ltd. · KBE-903: 3-aminopropyltriethoxysilane manufactured by Shin-Etsu Silicone Co., Ltd. KBM-603: Shin-Etsu Silicone Co., Ltd. N-2-(aminoethyl)-3-aminopropyltrimethoxysilane KBM-403: 3-glycidoxypropyltrimethoxysilane manufactured by Shin-Etsu Silicone Co., Ltd.
[0060] [Table 2]
[0061] According to Table 2, the adhesive of the present invention, which contains a polyether urethane polyol made using castor oil in the polyol composition and an aminosilane compound, has an improved biomass degree, does not cause tunneling after lamination, and has an excellent curing speed. Furthermore, even when aged polyol compositions and polyisocyanate compositions are used, the transparency and viscosity of the adhesive do not change, and the adhesive has excellent stability.
Claims
1. A lamination adhesive comprising a polyol composition, a polyisocyanate composition, and a silane compound, The polyol composition includes a polyether urethane polyol which is a reaction product of a polyol and a polyisocyanate, and the polyol includes castor oil and a polyether polyol; The content of the castor oil is 5 to 33 mass% based on the solid content mass of the polyol composition, A laminating adhesive, wherein the silane compound comprises an aminosilane compound.
2. The laminating adhesive according to claim 1 , wherein the aminosilane compound is an aminosilane compound having a primary amino group.
3. 3. The laminating adhesive according to claim 1, wherein the content of the aminosilane compound is 0.05 to 0.5 mass % based on the solids mass of the polyol composition.
4. The laminating adhesive according to any one of claims 1 to 3, wherein the silane compound further comprises an epoxy silane compound.
5. The laminating adhesive according to claim 4, wherein the content of the epoxysilane compound is 0.1 to 0.5 mass% or less based on the solid mass of the polyol composition.
6. A laminate comprising an adhesive layer made of the laminating adhesive according to any one of claims 1 to 5 disposed between at least two substrates.
7. A package using the laminate according to claim 6.
Citation Information
Patent Citations
Laminate adhesive and usage thereof
JP2003113359A
Adhesive composition and laminate
JP2017137426A
Adhesive composition
JP2018030905A
Adhesive for laminate
JP2019137712A
Adhesive composition
JP2020172669A