All-solid-state battery and method for producing the same
The introduction of a resin layer with specific adhesive and conductive regions in all-solid-state batteries addresses non-uniform lithium deposition, enhancing battery characteristics by ensuring uniform lithium distribution and reducing gaps, thus improving performance without external restraints.
Patent Information
- Application Number
- JP2021130259
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-08-06
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-08-06
AI Technical Summary
In all-solid-state batteries with a precipitated metal lithium negative electrode, non-uniform deposition and gaps form between the solid electrolyte layer and the negative electrode current collector during charging and discharging, leading to potential deterioration of battery characteristics.
A resin layer with distinct first and second regions is introduced between the solid electrolyte layer and the negative electrode current collector, where the first region applies a pressure higher than the yield stress of metal lithium to adhere and flatten the deposition, while the second region has lower Young's modulus to accommodate volume changes, ensuring uniform deposition and minimizing gaps.
This configuration enhances the input and output characteristics of the battery by preventing gaps and facilitating uniform deposition and dissolution of metallic lithium, thereby improving battery performance without the need for external restraining members.
Smart Images

Figure 0007567714000001 
Figure 0007567714000002 
Figure 0007567714000003
Abstract
Description
[Technical field]
[0001] The present application discloses an all-solid-state battery and a method for manufacturing an all-solid-state battery. [Background technology]
[0002] Patent Document 1 discloses a technique for applying a constraining pressure in the thickness direction by a constraining member to an all-solid-state battery having metallic lithium as a negative electrode active material that is precipitated between a solid electrolyte layer and a negative electrode current collector by charging. Patent Document 2 discloses a technique for preventing short circuits caused by thermal contraction of a separator by filling the peripheral portion of an electrode with resin. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2015 / 098551 [Patent Document 2] JP 2007-257859 A Summary of the Invention [Problem to be solved by the invention]
[0004] According to the findings of the present inventor, in an all-solid-state battery having a deposition-type metallic lithium anode as disclosed in Patent Document 1, metallic lithium is deposited non-uniformly and columnarly between the solid electrolyte layer and the anode current collector during charging, and a metallic lithium layer with many gaps is likely to be formed between the solid electrolyte layer and the anode current collector. Alternatively, in an all-solid-state battery having a deposition-type metallic lithium anode, metallic lithium deposited between the solid electrolyte layer and the anode current collector dissolves (ionizes) during discharging and returns to the positive electrode, causing shrinkage in the thickness direction, so that a gap is likely to be formed between the solid electrolyte layer and the anode current collector. Thus, in an all-solid-state battery having a deposition-type metallic lithium anode, a gap is likely to be formed between the solid electrolyte layer and the anode current collector during both charging and discharging. Therefore, there is a risk that the input or output characteristics of the battery may be reduced. [Means for solving the problem]
[0005] As one of the means for solving the above problems, the present application provides: An all-solid-state battery comprising: a positive electrode; a solid electrolyte layer; a negative electrode current collector; and metallic lithium as a negative electrode active material that is deposited between the solid electrolyte layer and the negative electrode current collector upon charging; a resin layer is disposed between the solid electrolyte layer and the negative electrode current collector; The resin layer has a first region and a second region in a planar direction, the first region bonds the solid electrolyte layer and the negative electrode current collector together such that a pressure higher than a yield stress of the metallic lithium is applied to the metallic lithium; The second region has electronic conductivity and a Young's modulus lower than that of the metallic lithium. All-solid-state battery. Disclose.
[0006] In the all-solid-state battery of the present disclosure, the first regions and the second regions may be regularly arranged in a planar direction.
[0007] In the all-solid-state battery of the present disclosure, the second region may be surrounded by the first region in a planar direction.
[0008] In the all-solid-state battery of the present disclosure, the first region may contain at least one resin selected from the group consisting of an acrylic resin, an epoxy resin, and an EVA resin.
[0009] In the all-solid-state battery of the present disclosure, the first region may contain a thermoplastic resin.
[0010] In the all-solid-state battery of the present disclosure, the second region may contain a conductive filler and a resin.
[0011] As one of the means for solving the above problems, the present application provides: forming a resin layer having a first region and a second region in a planar direction on at least one of a surface of a negative electrode current collector and a surface of a solid electrolyte layer; obtaining a laminate having a positive electrode, the solid electrolyte layer, the resin layer, and the negative electrode current collector in this order, by using the negative electrode current collector or the solid electrolyte layer on which the resin layer is formed; and charging the laminate to deposit metallic lithium between the solid electrolyte layer and the negative electrode current collector; Including, a first material is used as a material constituting the first region, the first material being capable of bonding the solid electrolyte layer and the negative electrode current collector together such that a pressure higher than a yield stress of the metallic lithium is applied to the metallic lithium; A second material having electronic conductivity and a Young's modulus lower than that of the metallic lithium is used as a material constituting the second region. Manufacturing method for all-solid-state batteries Disclose.
[0012] The manufacturing method of the present disclosure includes: the first region and the second region are regularly arranged in a planar direction on at least one of a surface of the negative electrode current collector and a surface of the solid electrolyte layer; may also include
[0013] The manufacturing method of the present disclosure includes: forming at least one of the first region and the second region by printing on at least one of a surface of the negative electrode current collector and a surface of the solid electrolyte layer; may also include Effect of the Invention
[0014] According to the technique of the present disclosure, the input or output characteristics of an all-solid-state battery having a deposition-type metallic lithium negative electrode are likely to be improved. [Brief description of the drawings]
[0015] [Figure 1]The configurations of the all-solid-state battery 100 after charging and after discharging are shown generally. [Diagram 2] 1 shows an example of the arrangement of first regions 41 and second regions 42 in a resin layer 40. [Diagram 3] 1 shows an example of a flow of a manufacturing method for an all-solid-state battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] 1.All-solid-state battery As shown in FIG. 1, an all-solid-state battery 100 according to an embodiment includes a positive electrode 10, a solid electrolyte layer 20, a negative electrode current collector 31, and metallic lithium 32 as a negative electrode active material that is deposited between the solid electrolyte layer 20 and the negative electrode current collector 31 by charging. As shown in FIG. 1, a resin layer 40 is disposed between the solid electrolyte layer 20 and the negative electrode current collector 31. The resin layer 40 has a first region 41 and a second region 42 in a planar direction. The first region 41 bonds the solid electrolyte layer 20 and the negative electrode current collector 31 such that a pressure higher than the yield stress of the metallic lithium 32 is applied to the metallic lithium 32. The second region 42 has electronic conductivity and a Young's modulus lower than that of the metallic lithium 32.
[0017] 1.1 Positive electrode The positive electrode 10 includes at least a positive electrode active material. When the all-solid-state battery 100 is charged, lithium ions released from the positive electrode active material reach between the solid electrolyte layer 20 and the negative electrode current collector 31 through the solid electrolyte layer 20, receive electrons, and are precipitated as metallic lithium. When the battery is discharged, the metallic lithium 32 between the solid electrolyte layer 20 and the negative electrode current collector 31 is dissolved (ionized) and returned to the positive electrode 10. The form of the positive electrode 10 may be any form known as a positive electrode for an all-solid-state battery. For example, as shown in FIG. 1, the positive electrode 10 may include a positive electrode current collector 11 and a positive electrode active material layer 12.
[0018] 1.1.1 Positive electrode current collector The positive electrode collector 11 may be any of those generally used as positive electrode collectors for all-solid-state batteries. The positive electrode collector 11 may be a metal foil or a metal mesh. In particular, metal foil is excellent in terms of ease of handling. The positive electrode collector 11 may be made of a plurality of metal foils. Examples of metals constituting the positive electrode collector 11 include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, and stainless steel. In particular, from the viewpoint of ensuring oxidation resistance, the positive electrode collector 11 may contain Al. The positive electrode collector 11 may have some kind of coating layer on its surface for the purpose of adjusting resistance, etc. In addition, when the positive electrode collector 11 is made of a plurality of metal foils, some kind of layer may be present between the plurality of metal foils. The thickness of the positive electrode collector 11 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.
[0019] 1.1.2 Cathode active material layer The positive electrode active material layer 12 contains at least a positive electrode active material. In addition to the positive electrode active material, the positive electrode active material layer 12 may further contain any of a solid electrolyte, a binder, a conductive assistant, and the like.
[0020] The positive electrode active material may be any known positive electrode active material for solid-state batteries that can supply lithium to the negative electrode side during charging. For example, lithium cobalt oxide, lithium nickel oxide, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 Various lithium-containing composite oxides such as O2, lithium manganate, and spinel-based lithium compounds can be used. In order to suppress a reaction caused by contact between the positive electrode active material and the solid electrolyte, a coating layer such as a lithium niobate layer, a lithium titanate layer, or a lithium phosphate layer may be provided on the surface of the positive electrode active material. The positive electrode active material may be, for example, in the form of particles, and the size is not particularly limited. Only one type of positive electrode active material may be used alone, or two or more types may be mixed and used.
[0021] The solid electrolyte may be either an organic solid electrolyte (organic polymer electrolyte) or an inorganic solid electrolyte. In particular, the inorganic solid electrolyte has higher ionic conductivity than the organic polymer electrolyte and is more heat resistant than the organic polymer electrolyte. Furthermore, it has higher rigidity than the organic polymer electrolyte. Examples of the inorganic solid electrolyte include lithium lanthanum zirconate, LiPON, Li 1+X Al X Ge 2-X Examples of the oxide solid electrolyte include (PO4)3, Li-SiO-based glass, and Li-Al-SO-based glass; and sulfide solid electrolytes such as Li2S-P2S5, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Si2S-P2S5, Li2S-P2S5-LiI-LiBr, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, and Li2S-P2S5-GeS2. Among them, sulfide solid electrolytes, particularly sulfide solid electrolytes containing Li2S-P2S5, have high performance. The solid electrolyte may be, for example, particulate, and its size is not particularly limited. Only one type of solid electrolyte may be used alone, or two or more types may be mixed and used.
[0022] Examples of the binder include butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, etc. Only one type of binder may be used alone, or two or more types may be mixed and used.
[0023] Examples of the conductive assistant include carbon materials such as acetylene black and ketjen black, and metal materials such as nickel, aluminum, and stainless steel. The conductive assistant may be, for example, particulate or fibrous, and the size is not particularly limited. Only one type of conductive assistant may be used alone, or two or more types may be mixed and used.
[0024] The content of each component in the positive electrode active material layer 12 may be the same as in the past. The shape of the positive electrode active material layer 12 may also be the same as in the past. From the viewpoint of making it easier to configure the all-solid-state battery 100, the positive electrode active material layer 12 may be in a sheet form. The thickness of the positive electrode active material layer 12 is not particularly limited. For example, it may be 0.1 μm or more and 2 mm or less. The lower limit may be 1 μm or more, and the upper limit may be 1 mm or less.
[0025] 1.2 Solid electrolyte layer The solid electrolyte layer 20 may include at least a solid electrolyte. The solid electrolyte layer 20 may optionally include a binder and the like in addition to the solid electrolyte.
[0026] The solid electrolyte is as described above. In particular, when the solid electrolyte layer 20 contains an inorganic solid electrolyte, the rigidity of the solid electrolyte layer 20 is increased, the metallic lithium 32 is less likely to penetrate the solid electrolyte layer, and the solid electrolyte layer 20 and the negative electrode current collector 31 are more likely to apply a restraining pressure to the metallic lithium 32. The binder can be appropriately selected from those exemplified as the binders used in the positive electrode active material layer 12.
[0027] The content of each component in the solid electrolyte layer 20 may be the same as in the conventional case. The shape of the solid electrolyte layer 20 may also be the same as in the conventional case. From the viewpoint of making it easier to configure the all-solid-state battery 100, the solid electrolyte layer 20 may be in a sheet form. The thickness of the solid electrolyte layer 20 may be, for example, 0.1 μm or more and 2 mm or less. The lower limit may be 1 μm or more, and the upper limit may be 1 mm or less.
[0028] 1.3 Negative electrode current collector The negative electrode current collector 31 may be any of those generally used as negative electrode current collectors for all-solid-state batteries. The negative electrode current collector 31 may be a metal foil or metal mesh, or may be a carbon sheet. In particular, metal foil is excellent in terms of ease of handling. The negative electrode current collector 31 may be made of a plurality of metal foils or sheets. Examples of metals constituting the negative electrode current collector 31 include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, and the like. In particular, from the viewpoint of ensuring reduction resistance and being difficult to alloy with lithium, the negative electrode current collector 31 may contain at least one metal selected from Cu, Ni, and stainless steel. The negative electrode current collector 31 may have some kind of coating layer on its surface for the purpose of adjusting resistance, etc. In addition, when the negative electrode current collector 31 is made of a plurality of metal foils, some kind of layer may be present between the plurality of metal foils. The thickness of the negative electrode current collector 31 is not particularly limited. For example, it may be 0.1 μm or more, or 1 μm or more, and may be 1 mm or less, or 100 μm or less.
[0029] 1.4 Metallic lithium as a negative electrode active material In the all-solid-state battery 100, metallic lithium 32 is precipitated as a negative electrode active material between the solid electrolyte layer 20 and the negative electrode current collector 31 by charging. More specifically, as shown in Fig. 1, metallic lithium 32 is likely to precipitate between the solid electrolyte layer 20 and the second region 42. Also, as shown in Fig. 1, metallic lithium 32 precipitated between the solid electrolyte layer 20 and the negative electrode current collector 31 dissolves (ionizes) with discharge and is returned to the positive electrode 10. In this way, when charging and discharging of the all-solid-state battery 100 are repeated, deposition and dissolution of metallic lithium 32 are repeated on the negative electrode side.
[0030] In the all-solid-state battery 100 according to this embodiment, as described later, a pressure higher than the yield stress of the metallic lithium 32 is applied to the metallic lithium 32 deposited between the solid electrolyte layer 20 and the negative electrode current collector 31 by the adhesive force of the first region 41. As a result, the metallic lithium 32 is easily buckled and stretched between the solid electrolyte layer 20 and the negative electrode current collector 31, and is easily plastically deformed in the planar direction and leveled. As described later, the Young's modulus of the second region 42 is lower than that of the metallic lithium 32, so that the second region 42 may deform as the metallic lithium 32 deposits or dissolves. For example, as shown in FIG. 1, the second region 42 is compressed in the thickness direction by the deposition of the metallic lithium 32, and the metallic lithium 32 may fill the space defined by the solid electrolyte layer 20, the first region 41, and the second region 42. Furthermore, the dissolution of metallic lithium 32 causes second region 42 to expand in the thickness direction, and the generation of a gap between solid electrolyte layer 20 and negative electrode current collector 31 is easily suppressed.
[0031] The amount of metallic lithium 32 precipitated between the solid electrolyte layer 20 and the negative electrode current collector 31 is not particularly limited. It may be adjusted appropriately according to the desired battery performance. For example, it is considered that the higher the SOC, the greater the amount of metallic lithium 32 precipitated, and the metallic lithium 32 is more likely to be uniform between the solid electrolyte layer 20 and the negative electrode current collector 31. However, if the amount of metallic lithium 32 precipitated is too large, there is a concern that pressure may be concentrated. In this regard, as a guideline for the amount of metallic lithium 32 precipitated, it is considered that the charge capacity of the all-solid-state battery 100 is, for example, 1 mAh / cm 2 More than 3mAh / cm 2 The amount may be such that:
[0032] 1.5 Resin layer As shown in FIG. 1, the resin layer 40 has a first region 41 and a second region 42 in the planar direction. The "planar direction" means a direction along the interface between the solid electrolyte layer 20 and the resin layer 40, or a direction along the interface between the resin layer 40 and the negative electrode current collector 31, as shown in FIG. 1. The planar direction may be at least one direction. As shown in FIG. 1, the resin layer 40 may have a plurality of the first regions 41 and the second regions 42 in the planar direction, or may have the first regions 41 and the second regions 42 repeatedly. The thickness of the resin layer 40 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 10 mm or less, 5 mm or less, 1 mm or less, or 100 μm or less.
[0033] 1.5.1 First area The first region 41 bonds the solid electrolyte layer 20 and the negative electrode current collector 31 such that a pressure higher than the yield stress of the metallic lithium 32 is applied to the metallic lithium 32. That is, as described above, a constraining pressure higher than the yield stress of the metallic lithium 32 is generated between the solid electrolyte layer 20 and the negative electrode current collector 31 due to the adhesive force of the first region 41. As a result, when the metallic lithium 32 is precipitated between the solid electrolyte layer 20 and the negative electrode current collector 31, the metallic lithium 32 is easily buckled and stretched by the constraining pressure and plastically deformed in the planar direction to be leveled.
[0034] The adhesive force of the first region 41 may be such that the pressure applied to the metallic lithium 32 deposited between the solid electrolyte layer 20 and the negative electrode current collector 31 is higher than the yield stress of the metallic lithium 32. In other words, the adhesive force may be such that a restraining pressure is applied to the metallic lithium 32 so as to be sandwiched between the solid electrolyte layer 20 and the negative electrode current collector 31, causing the metallic lithium 32 to buckle, extend, and plastically deform in the planar direction. The pressure applied to the metallic lithium 32 by the adhesive force may be, for example, 0.4 MPa or more, or 1.0 MPa or more, based on the area of the second region 42. On the other hand, if the pressure applied to the metallic lithium 32 by the adhesive force is too high, the metallic lithium 32 may excessively enter the gaps in the solid electrolyte layer 20, and in some cases, may pass through the solid electrolyte layer 20 and reach the positive electrode 10 side. In this regard, the pressure due to the adhesive force may be, for example, 100 MPa or less, 50 MPa or less, 10 MPa or less, or 5 MPa or less, based on the area of the second region.
[0035] The first region 41 may be made of a resin material (first material) capable of exhibiting the above-mentioned adhesive force. For example, the first region 41 may contain at least one resin selected from the group consisting of acrylic resin, epoxy resin, and EVA resin. Alternatively, the first region 41 may contain a thermoplastic resin. In particular, a thermoplastic resin such as an EVA resin can recover its adhesive force by reheating. Alternatively, the resin constituting the first region 41 may be selected from those exemplified as binders that can be contained in the above-mentioned active material layer and solid electrolyte layer.
[0036] 1.5.2 Second area The second region 42 has electronic conductivity and has a Young's modulus lower than that of metallic lithium 32. Lithium ions that reach between the solid electrolyte layer 20 and the negative electrode current collector 31 from the positive electrode 10 can receive electrons via the second region 42 having electronic conductivity and precipitate as metallic lithium 32. That is, metallic lithium 32 is likely to precipitate between the solid electrolyte layer 20 and the second region 42 during charging.
[0037] The second region 42 only needs to have electronic conductivity to the extent that it can cause a precipitation reaction or dissolution reaction of the metallic lithium 32 as a battery reaction during charging and discharging. The electronic conductivity and Young's modulus of the second region 42 can be easily changed by adjusting the types and ratios of the materials constituting the second region 42.
[0038] The second region 42 has a Young's modulus lower than that of the metallic lithium 32. For example, the Young's modulus of the second region 42 may be less than 4.9 GPa. Since the second region 42 has a Young's modulus lower than that of the metallic lithium 32, the second region 42 can deform so as to follow the deposition or dissolution of the metallic lithium 32. As a result, even if the metallic lithium 32 is deposited or dissolved between the solid electrolyte layer 20 and the negative electrode current collector 31, a gap is unlikely to occur between the solid electrolyte layer 20 and the negative electrode current collector 31. In addition, a volume change on the negative electrode side due to the deposition or dissolution of the metallic lithium 32 is unlikely to occur, which is considered to facilitate the design of a battery pack or stack.
[0039] The second region 42 may have a yield stress higher than the yield stress of the metallic lithium 32. The second region 42 may have a yield stress of, for example, 0.4 MPa or more or 1.0 MPa or more. This is thought to enable the metallic lithium 32 to be more appropriately buckled and extended between the solid electrolyte layer 20 and the second region 42 during charging. Also, contact between the solid electrolyte layer 20 and the second region 42 is more likely to be ensured during discharging.
[0040] The second region 42 may be made of a material (second material) capable of exhibiting the above-mentioned electronic conductivity and Young's modulus. For example, the second region 42 may include a conductive filler and a resin. Examples of the resin constituting the second region 42 include thermoplastic resins and various cured resins (thermosetting resins, ultraviolet curing resins, photocuring resins, etc.). The resin may be selected from among the binders exemplified as those that may be contained in the above-mentioned active material layer and solid electrolyte layer. Specific examples of the resin include polyvinylidene fluoride (PVdF) resins, vinyl resins, polyolefin resins, etc. As the conductive filler, any of fillers made of various conductive materials such as metals, metal compounds, and carbon may be used, and the material, shape, size, and content may be adjusted according to the required electronic conductivity.
[0041] 1.5.3 Positional relationship and size of the first and second areas The positional relationship between the first region 41 and the second region 42 in the surface direction is not particularly limited. For example, the first region 41 and the second region 42 may be regularly arranged in the surface direction. Specifically, as shown in FIG. 2, the first region 41 and the second region 42 may be arranged in a lattice shape in the surface direction, or in a stripe shape, or may be arranged in any other regular surface shape. By regularly arranging the first region 41 and the second region 42 in the surface direction, uneven deposition of the metallic lithium 32 between the solid electrolyte layer 20 and the negative electrode current collector 31 is more likely to be suppressed.
[0042] 2, the second region 42 may be surrounded by the first region 41 in the planar direction. The size (diameter of a circle having an area equivalent to that of the second region 42) in the planar direction may be smaller than the thickness of the negative electrode current collector 31. This makes it possible to easily make the deformation (bending) of the negative electrode current collector 31 caused by the surface pressure generated when the metallic lithium 32 is precipitated small enough to be negligible.
[0043] 1.6 Other materials The all-solid-state battery 100 may have at least the above-described configurations, and may have other components in addition to the above. The components described below are examples of other components that the all-solid-state battery 100 may have.
[0044] 1.6.1 Enclosure The all-solid-state battery 100 may be one in which each of the above-mentioned components is housed inside an exterior body. More specifically, a portion excluding a tab or terminal for extracting power from the all-solid-state battery 100 to the outside may be housed inside the exterior body. Any known exterior body for a battery may be adopted as the exterior body. For example, a laminate film may be used as the exterior body. In addition, a plurality of all-solid-state batteries 100 may be electrically connected and arbitrarily stacked to form an assembled battery. In this case, the assembled battery may be housed inside a known battery case.
[0045] 1.6.2 Sealing resin In the all-solid-state battery 100, each of the above components may be sealed with a resin. For example, at least the side surface (surface along the stacking direction) of the laminate 50 described below may be sealed with a resin. This makes it easier to prevent moisture from entering the inside of each layer. As the sealing resin, a known curable resin or thermoplastic resin may be used.
[0046] 1.6.3 Restraining members The all-solid-state battery 100 may or may not have a restraining member for restraining each of the above components in the thickness direction. The internal resistance of the battery is likely to be reduced by applying a restraining pressure by the restraining member. However, as described above, in this embodiment, a predetermined restraining pressure is ensured between the solid electrolyte layer 20 and the negative electrode current collector 31 by the adhesive force of the first region 41 of the resin layer 40, so that a restraining member such as an external jig is not necessarily required.
[0047] 2. Manufacturing method of all-solid-state batteries The above-mentioned all-solid-state battery 100 can be manufactured, for example, as follows. That is, as shown in Figs. 3(A) to (C), the manufacturing method of the all-solid-state battery 100 according to this embodiment includes the following steps: Forming a resin layer 40 having a first region 41 and a second region 42 in a planar direction on at least one of a surface of a negative electrode current collector 31 and a surface of a solid electrolyte layer 20 ( FIG. 3(A) ); Obtaining a laminate 50 having a positive electrode 10, the solid electrolyte layer 20, the resin layer 40, and the negative electrode current collector 31 in this order by using the negative electrode current collector 31 or the solid electrolyte layer 20 on which the resin layer 40 is formed ( FIG. 3(B) ); and The laminate 50 is charged to deposit metallic lithium 32 between the solid electrolyte layer 20 and the negative electrode current collector 31 (FIG. 3(C)). Including, a first material is used as a material for forming the first region 41, the first material being capable of bonding the solid electrolyte layer 20 and the negative electrode current collector 31 together such that a pressure higher than the yield stress of the metallic lithium 32 is applied to the metallic lithium 32; As a material constituting the second region 42, a second material having electronic conductivity and a Young's modulus lower than that of the metallic lithium 32 is used.
[0048] 2.1 Formation of resin layer In the manufacturing method according to the present embodiment, a resin layer 40 having a first region 41 and a second region 42 arranged in a planar direction is formed on at least one of the surfaces of the negative electrode current collector 31 and the solid electrolyte layer 20. From the viewpoint of excellent handling properties, the resin layer 40 may be formed on the surface of the negative electrode current collector 31 as shown in FIG. 3(A). The arrangement of the first region 41 and the second region 42 in the resin layer 40 is not particularly limited. For example, the first region 41 and the second region 42 may be arranged regularly in a planar direction on at least one of the surfaces of the negative electrode current collector 31 and the solid electrolyte layer 20.
[0049] The method of forming the resin layer 40 on at least one of the surface of the negative electrode current collector 31 and the surface of the solid electrolyte layer 20 is not particularly limited. For example, the first material and the second material may be laminated, coated, or printed on the surface. In particular, at least one of the first region 41 and the second region 42 may be formed on the surface by printing. The printing method is not particularly limited, and for example, inkjet printing or the like may be adopted. On the surface, one of the first region 41 and the second region 42 may be formed first, or the first region 41 and the second region 42 may be formed simultaneously.
[0050] The first material constituting the first region 41 and the second material constituting the second region 42 are as described above, and detailed description thereof will be omitted here. In forming the resin layer 40, a heat treatment, a curing treatment, or the like may be performed depending on the type of the first material and the second material.
[0051] 2.2 Preparation of the laminate As shown in FIG. 3(B), in the manufacturing method according to the present embodiment, a laminate 50 having a positive electrode 10, a solid electrolyte layer 20, a resin layer 40, and a negative electrode collector 31 in this order is obtained using a negative electrode collector 31 or a solid electrolyte layer 20 on which a resin layer 40 is formed as described above. The laminate 50 can be easily obtained, for example, by forming and laminating the above-mentioned materials by coating or transferring them so that the above-mentioned positive electrode collector 11, the positive electrode active material layer 12, the solid electrolyte layer 20, the resin layer 40, and the negative electrode collector 31 are laminated in this order. The laminate 50 may include at least one each of the positive electrode collector 11, the positive electrode active material layer 12, the solid electrolyte layer 20, the resin layer 40, and the negative electrode collector 31. That is, the laminate 50 may have at least one laminate unit of the above-mentioned positive electrode current collector 11, positive electrode active material layer 12, solid electrolyte layer 20, resin layer 40, and negative electrode current collector 31, and may have a plurality of such laminate units. In this case, the plurality of laminate units may be electrically connected to each other in series, in parallel, or not electrically connected.
[0052] After obtaining the laminate 50, pressure may be applied to the laminate 50 in the thickness direction (stacking direction). For example, the layers constituting the laminate 50 may be pressed to be integrated, or the gaps between the layers constituting the laminate 50 may be eliminated to reduce the interface resistance. The laminate 50 may be pressed by a known means. For example, the laminate 50 may be pressed in the stacking direction by various pressing methods such as CIP, HIP, roll press, uniaxial press, and die press. In particular, when the laminate 50 is pressed by a uniaxial press such as CIP or HIP, it is considered that the stacking surface of the laminate 50 is more uniformly pressed. The magnitude of the pressure applied to the laminate 50 in the stacking direction may be appropriately determined according to the performance of the target battery. For example, from the viewpoint of easily performing the above-mentioned integration and elimination of the gaps by plastically deforming the solid electrolyte contained in the laminate 50, the pressure may be 100 MPa or more, 150 MPa or more, 200 MPa or more, 250 MPa or more, 300 MPa or more, or 350 MPa or more. The pressing time and pressing temperature of the laminate 50 are not particularly limited.
[0053] 2.3 Charging 3(C), in the manufacturing method according to the present embodiment, the laminate 50 obtained as described above is charged, and metallic lithium 32 is precipitated between the solid electrolyte layer 20 and the negative electrode current collector 31. In the all-solid-state battery 100, the metallic lithium 32 can function as a negative electrode active material. The charging may be the first charging after the preparation of the laminate 50, or may be the second or subsequent charging.
[0054] The laminate 50 may be charged in the same manner as a general battery. That is, charging may be performed by connecting an external power source to the positive electrode current collector 11 and the negative electrode current collector 31 of the laminate 50. By charging the laminate 50, lithium ions are conducted from the positive electrode active material contained in the positive electrode active material layer 12 to the negative electrode current collector 31 side through the solid electrolyte layer 20, and the lithium ions receive electrons between the solid electrolyte layer 20 and the negative electrode current collector 31 (particularly between the solid electrolyte layer 20 and the second region 42), and are precipitated as metallic lithium 32. At this time, the metallic lithium 32 buckles and stretches between the solid electrolyte layer 20 and the negative electrode current collector 31 due to the restraining pressure caused by the adhesive force of the first region 41, and is plastically deformed in the planar direction. That is, even if the metallic lithium 32 is precipitated in an uneven and columnar shape, the metallic lithium 32 is easily leveled in the planar direction.
[0055] 2.4 Other processes The manufacturing method according to the present embodiment may include general steps for manufacturing an all-solid-state battery in addition to the above-mentioned steps. For example, the steps include a step of housing the laminate 50 inside an exterior body such as a laminate film, a step of connecting a current collecting tab to the laminate 50, and the like. Specifically, for example, after connecting a current collecting tab to the current collectors 11 and 31 of the laminate 50 (parts of the current collectors 11 and 31 may be protruded and used as tabs), the laminate 50 may be housed in a laminate film as an exterior body, while the laminate film may be sealed with the tab pulled out to the outside of the laminate film, and then the laminate 50 may be charged via the tab outside the laminate film.
[0056] 3. Supplementary Information As described above, in an all-solid-state battery including a precipitation-type metallic lithium negative electrode, by disposing a resin layer having a first region and a second region between a solid electrolyte layer and a negative electrode current collector, metallic lithium can be precipitated between the solid electrolyte layer and the negative electrode current collector (particularly between the solid electrolyte layer and the second region) during charging of the battery. In addition, since a predetermined restraining pressure is secured between the solid electrolyte layer and the negative electrode current collector by the adhesive force of the first region, metallic lithium precipitated between the solid electrolyte layer and the negative electrode current collector can be buckled and extended, and plastically deformed in the planar direction to be uniform. In addition, during discharging of the battery, the second region is easily deformed to follow the dissolution of metallic lithium between the solid electrolyte layer and the negative electrode current collector. Thus, according to the technology of the present disclosure, in an all-solid-state battery including a precipitation-type metallic lithium negative electrode, a gap is unlikely to occur between the solid electrolyte layer and the negative electrode current collector during both charging and discharging, and therefore the input or output characteristics of the battery can be easily improved.
[0057] In addition, when a fixed size constraint is applied to an all-solid-state battery using a constraint member such as an external jig, it is difficult to eliminate the gap caused by the volumetric shrinkage between the solid electrolyte layer and the negative electrode current collector. On the other hand, when a constant pressure constraint is applied to an all-solid-state battery using a constraint member such as an external jig, if the constraint pressure is greater than the yield stress of metallic lithium, the metallic lithium deposited between the solid electrolyte layer and the negative electrode current collector during charging can be buckled and extended to cause plastic deformation in the surface direction, and it is considered that the metallic lithium can be uniformed between the solid electrolyte layer and the negative electrode current collector. In addition, it is considered that the gap between the solid electrolyte layer and the negative electrode current collector during discharge can also be eliminated. However, in this case, the volumetric energy density of the all-solid-state battery is reduced by the amount of the constraint member required. In contrast, according to the technology disclosed herein, even if the constraint member such as an external jig is miniaturized or omitted, the above-mentioned effect is exerted, so that the volumetric energy density of the all-solid-state battery is easily increased. [Explanation of symbols]
[0058] 10 positive electrode 11 Positive electrode current collector 12 Cathode active material layer 20 Solid electrolyte layer 31 Negative electrode current collector 32 Metallic lithium 40 Resin layer 41 First area 42 Second area 50 Laminate 100 solid state battery
Claims
1. An all-solid-state battery comprising: a positive electrode; a solid electrolyte layer; a negative electrode current collector; and metallic lithium as a negative electrode active material that is deposited between the solid electrolyte layer and the negative electrode current collector upon charging; a resin layer is disposed between the solid electrolyte layer and the negative electrode current collector; The resin layer has a first region and a second region in a planar direction, the first region bonds the solid electrolyte layer and the negative electrode current collector together such that a pressure higher than a yield stress of the metallic lithium is applied to the metallic lithium; The second region has electronic conductivity and a Young's modulus lower than that of the metallic lithium. All-solid-state battery.
2. The first region and the second region are regularly arranged in the surface direction. The all-solid-state battery according to claim 1 .
3. The second region is surrounded by the first region in a surface direction. The all-solid-state battery according to claim 1 or 2.
4. The first region contains at least one resin selected from the group consisting of an acrylic resin, an epoxy resin, and an EVA resin. The all-solid-state battery according to any one of claims 1 to 3.
5. The first region comprises a thermoplastic resin. The all-solid-state battery according to any one of claims 1 to 4.
6. The second region includes a conductive filler and a resin. The all-solid-state battery according to any one of claims 1 to 5.
7. forming a resin layer having a first region and a second region in a planar direction on at least one of a surface of a negative electrode current collector and a surface of a solid electrolyte layer; obtaining a laminate having a positive electrode, the solid electrolyte layer, the resin layer, and the negative electrode current collector in this order, by using the negative electrode current collector or the solid electrolyte layer on which the resin layer is formed; and charging the laminate to deposit metallic lithium between the solid electrolyte layer and the negative electrode current collector; Including, a first material is used as a material constituting the first region, the first material being capable of bonding the solid electrolyte layer and the negative electrode current collector together such that a pressure higher than a yield stress of the metallic lithium is applied to the metallic lithium; A second material having electronic conductivity and a Young's modulus lower than that of the metallic lithium is used as a material constituting the second region. How solid-state batteries are manufactured.
8. the first region and the second region are regularly arranged in a planar direction on at least one of a surface of the negative electrode current collector and a surface of the solid electrolyte layer; The method of claim 7, comprising:
9. forming at least one of the first region and the second region by printing on at least one of a surface of the negative electrode current collector and a surface of the solid electrolyte layer; The method of claim 7 or 8, comprising: