Insulating aluminum alloy conductor and its manufacturing method
The insulating aluminum alloy conductor with controlled Si and Mg contents and anionic electrodeposition with polyamide-imide resin addresses surface defects by minimizing aluminum elution and hydrogen gas, achieving a smooth and defect-free insulating layer with enhanced properties.
Patent Information
- Application Number
- JP2021138898
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-08-27
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-08-27
AI Technical Summary
Anionic electrodeposition of polyamide-imide resin on aluminum alloys results in proton generation, leading to acidic electrodeposition solutions, aluminum elution, and hydrogen gas formation, causing surface defects and unevenness in the insulating layer.
The insulating aluminum alloy conductor is manufactured with a specific Si content (0.3% to 13.5% by mass) and Mg content (1.8% by mass or less) to minimize aluminum elution, using anionic electrodeposition with polyamide-imide resin containing carboxyl groups, reducing hydrogen gas generation and surface irregularities.
The method produces a smooth and uniform insulating layer with reduced defects, maintaining high heat resistance and flexibility, while improving the conductor's hardness and workability.
Smart Images

Figure 0007567720000002 
Figure 0007567720000003 
Figure 0007567720000004
Abstract
Description
[Technical field]
[0001] The present invention relates to an insulating aluminum alloy conductor and a method for producing the same. [Background technology]
[0002] Insulating aluminum alloy conductors, which are made of aluminum alloys and coated with an insulating layer, are widely used as conductive materials and heat sink materials for various electrical devices that require insulation. Examples of aluminum alloys used include Al-Cu alloys, Al-Mn alloys, Al-Si alloys, and Al-Mg-Si alloys. Resins such as polyimide and polyamide-imide resins are used as materials for the insulating layer of insulating aluminum alloy conductors.
[0003] Electrodeposition is a known method for covering the surface of an aluminum alloy conductor with an insulating layer. The electrodeposition method includes an electrodeposition step and a baking step. In the electrodeposition step, the conductor body and a counter electrode are immersed in an electrodeposition solution in which charged resin particles are dispersed, and a voltage is applied between the conductor body and the counter electrode to electrodeposit the resin particles onto the surface of the conductor body, forming an electrodeposition layer. In the baking step, the electrodeposition layer is heated to bake the electrodeposition layer onto the conductor body, forming an insulating layer.
[0004] There are two types of electrodeposition: anionic electrodeposition, which uses resin particles made of a resin having an anionic group, and cationic electrodeposition, which uses resin particles made of a resin having a cationic group. In anionic electrodeposition, a voltage is applied to the conductor body as the anode and the counter electrode as the cathode. In cationic electrodeposition, a voltage is applied to the conductor body as the cathode and the counter electrode as the anode. For example, Patent Document 1 discloses an electrodeposition liquid (electrodeposition coating composition) using a block copolymer polyimide having a siloxane bond in the molecular skeleton and an anionic group in the molecule as a material for the insulating layer. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-156378 A Summary of the Invention [Problem to be solved by the invention]
[0006] An insulating layer formed by anionic electrodeposition of a polyamide-imide resin having carboxyl groups has high heat resistance and high flexibility, and is therefore used for highly heat-resistant enameled wires. However, anionic electrodeposition has a problem in that protons are generated on the surface of the conductor body, which is the anode, during electrodeposition, and the pH of the electrodeposition solution around the conductor body may decrease. If the pH of the electrodeposition solution decreases and the electrodeposition solution becomes acidic, aluminum from the conductor body may dissolve into the electrodeposition solution and hydrogen gas may be generated. If hydrogen gas is generated during electrodeposition, the hydrogen gas may be mixed into the electrodeposition layer, and bubbles may be mixed into the film, which may cause poor appearance. If an aluminum substrate is coated with this polyamide-imide resin by anionic electrodeposition, the electrodeposition layer immediately after electrodeposition may have abnormal appearance, which is thought to be caused by the bubbles, and the insulating layer may have unevenness or bubbles after baking.
[0007] The present invention has been made in consideration of the above circumstances, and aims to provide an insulating aluminum alloy conductor that can be produced by anionic electrodeposition and is coated with an insulating layer having a smooth surface with minimal irregularities, and a method for producing the same. [Means for solving the problem]
[0008] In order to solve the above problems, the insulating aluminum alloy conductor of the present invention is an insulating aluminum alloy conductor comprising a conductor body made of an aluminum alloy and an insulating layer covering the conductor body, characterized in that the Si content of the conductor body is in the range of 0.3 mass% or more and 13.5 mass% or less, the Mg content is 1.8 mass% or less, and the insulating layer contains a polyamideimide resin having a carboxyl group.
[0009] According to the insulating aluminum alloy conductor having such a configuration, the insulating layer contains a polyamide-imide resin having a carboxyl group, and therefore can be manufactured by anionic electrodeposition. The Si content of the conductor body is set to be within a range of 0.3 mass% to 13.5 mass%, so that in the electrodeposition process when manufacturing the insulating aluminum alloy conductor by anionic electrodeposition, even when the pH of the electrodeposition solution around the conductor body is lowered and the electrodeposition solution becomes acidic, aluminum is less likely to be eluted from the conductor body. This reduces the amount of hydrogen gas generated by the elution of aluminum, thereby reducing the appearance defects of the electrodeposition layer. Furthermore, the Mg content of the conductor body is set to be 1.8 mass% or less, and the content of Mg, which has a higher ionization tendency than aluminum, is low, so that aluminum is less likely to be eluted from the conductor body even when the electrodeposition solution becomes acidic. Therefore, the insulating aluminum alloy conductor having the above configuration has a smooth surface of the insulating layer with few irregularities.
[0010] In the insulating aluminum alloy conductor of the present invention, the conductor body may have a Si content in the range of 0.5 mass % to 11.0 mass %. In this case, since the Si content of the conductor body is within the range of 0.5 mass% or more and 11.0 mass% or less, aluminum is less likely to dissolve from the conductor body even when the electrodeposition solution becomes acidic during the electrodeposition process when producing an insulating aluminum alloy conductor by anionic electrodeposition.
[0011] In the insulative aluminum alloy conductor of the present invention, the conductor body may have a Mg content in the range of 0.8% by mass to 1.3% by mass. In this case, since the Mg content of the conductor body is 0.8 mass% or more, the conductor body has high hardness and improves workability, and since the Mg content of the conductor body is 1.3 mass% or less, aluminum is further prevented from eluting from the conductor body even when the electrodeposition solution becomes acidic.
[0012] The method for producing an insulating aluminum alloy conductor of the present invention includes an electrodeposition step in which resin particles are electrodeposited onto the surface of a conductor body made of an aluminum alloy by anionic electrodeposition to obtain a conductor body with an electrodeposition layer, and a baking step in which the conductor body with the electrodeposition layer is heated and the electrodeposition layer is baked onto the conductor body to form an insulating layer and obtain an insulating aluminum alloy conductor, wherein the conductor body has a Si content in the range of 0.3 mass% or more and 13.5 mass% or less and a Mg content of 1.8 mass% or less, and in the electrodeposition step, the conductor body is immersed in an electrodeposition liquid containing resin particles that contain polyamideimide resin having carboxyl groups.
[0013] According to the manufacturing method of the insulating aluminum alloy conductor having such a configuration, since the electrodeposition liquid contains resin particles containing polyamideimide resin having a carboxyl group, the electrodeposition layer can be formed by anionic electrodeposition. Since the Si content of the conductor body is set to be within a range of 0.3 mass% to 13.5 mass%, in the electrodeposition process, even when the pH of the electrodeposition liquid around the conductor body is lowered and the electrodeposition liquid becomes acidic, aluminum is less likely to be eluted from the conductor body. This reduces the amount of hydrogen gas generated by the elution of aluminum, thereby reducing the appearance defects of the electrodeposition layer. Furthermore, since the Mg content of the conductor body is set to be 1.8 mass% or less, and the content of metals having a higher ionization tendency than aluminum is low, aluminum is less likely to be eluted from the conductor body even when the electrodeposition liquid becomes acidic. Therefore, the manufacturing method having the above configuration makes it possible to manufacture an insulating aluminum alloy conductor having a smooth surface of the insulating layer with few irregularities. Effect of the Invention
[0014] According to the present invention, it is possible to provide an insulated aluminum alloy conductor that can be produced by anionic electrodeposition and is coated with an insulating layer having a smooth surface with minimal irregularities, and a method for producing the same. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a cross-sectional view of an insulative aluminum alloy conductor according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a flow diagram showing a method for producing an insulated aluminum alloy conductor according to an embodiment of the present invention. [Diagram 3] FIG. 1 is a diagram showing the configuration of an electrodeposition apparatus that can be used in a method for producing an insulated aluminum alloy conductor according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an insulating aluminum alloy conductor according to one embodiment of the present invention and a method for producing the same will be described with reference to the accompanying drawings.
[0017] FIG. 1 is a cross-sectional view of an insulative aluminum alloy conductor according to one embodiment of the present invention. As shown in FIG. 1, an insulated aluminum alloy conductor 10 according to this embodiment includes a conductor body 11 and an insulating layer 12 that covers the conductor body 11.
[0018] The conductor body 11 is made of an aluminum alloy. The aluminum alloy contains Si. Si has the effect of chemically stabilizing the aluminum alloy and making it less soluble in acid. Si also has the effect of improving the strength of the aluminum alloy. On the other hand, if the Si content is too high, the strength of the aluminum alloy may become too high, which may reduce the workability. For this reason, in this embodiment, the Si content of the conductor body 11 is set to a range of 0.3 mass% to 13.5 mass%. The Si content of the conductor body 11 is preferably in the range of 0.5 mass% to 11.0 mass%, and particularly preferably in the range of 0.8 mass% to 11.0 mass%.
[0019] The aluminum alloy may contain Mg. Mg has the effect of reducing the weight of the aluminum alloy and improving its hardness. On the other hand, Mg has a higher ionization tendency than aluminum. Therefore, if the Mg content is too high, the aluminum alloy becomes more likely to dissolve in acid. For this reason, in this embodiment, the Mg content of the conductor body 11 is set to 1.8 mass% or less. From the viewpoint of the solubility of the aluminum alloy in acid, the Mg content is preferably 1.3 mass% or less. Furthermore, from the viewpoint of improving the hardness of the aluminum alloy, the Mg content of the conductor body 11 is preferably 0.8 mass% or more.
[0020] The aluminum alloy preferably contains 0.1 mass% or less of each of Li, K, Ca, and Na. These metals have a higher ionization tendency than aluminum. Therefore, if the content of these metals is too high, the aluminum alloy may be easily dissolved in acid.
[0021] The aluminum alloy may be an Al-Cu alloy, an Al-Mn alloy, or an Al-Si alloy. An Al-Mg-Si alloy may be used. The Al-Cu alloy may be a 2000 series alloy such as A2024. The Al-Mn alloy may be a 3000 series alloy such as A3003. The Al-Si alloy may be a 4000 series alloy such as A4032. The Al-Mg-Si alloy may be a 6000 series alloy such as A6061. Of these alloys, the 6000 series alloy is preferred.
[0022] The insulating layer 12 contains a polyamideimide resin having a carboxyl group. The polyamideimide resin having a carboxyl group may be electrodeposited on the surface of the conductor body 11 by anionic electrodeposition. The polyamideimide resin having a carboxyl group electrodeposited by anionic electrodeposition has high adhesion to the conductor body 11. This increases the heat resistance of the insulating layer 12. In addition, the insulating layer 12 has high flexibility, so that peeling is unlikely to occur even when the conductor body 11 is deformed.
[0023] The shape of the insulating aluminum alloy conductor 10 is not particularly limited, and may be, for example, a line, a cylinder, a square prism, a coil, etc. The thickness of the insulating layer 12 is not particularly limited, and may be, for example, within the range of 5 μm to 100 μm.
[0024] Next, a method for producing the insulating aluminum alloy conductor of this embodiment will be described. FIG. 2 is a flow diagram showing a method for producing an insulative aluminum alloy conductor according to one embodiment of the present invention. As shown in FIG. 2, the method for producing an insulated aluminum alloy conductor according to this embodiment includes a degreasing step S01, an electrodeposition step S02, and a baking step S03.
[0025] The degreasing step S01 is a step of removing grease adhering to the surface of the conductor body 11. As a method for removing grease, for example, a method of immersing the conductor body 11 in a degreaser can be adopted. As the degreaser, an organic solvent or a surfactant can be used. For example, in this embodiment, the grease adhering to the surface of the substrate is dissolved and removed by immersing the substrate for 1 minute in an aqueous degreaser solution containing 10 mass % of a degreaser (Neo Sundep S, manufactured by Nippon Marcel Co., Ltd.) having a liquid temperature of about 20°C.
[0026] The conductor body 11 preferably has a surface roughness Ra of 2.0 μm or less. By using a conductor body 11 having a smooth surface with a surface roughness Ra of 2.0 μm or less, generated air bubbles are less likely to adhere to the surface of the conductor body 11 in the next electrodeposition step S02.
[0027] The electrodeposition step S02 is a step of electrodepositing resin particles onto the surface of the conductor body 11 made of an aluminum alloy by anionic electrodeposition to obtain the conductor body 11 with an electrodeposition layer. FIG. 3 is a configuration diagram of an electrodeposition apparatus that can be used in a method for producing an insulated aluminum alloy conductor according to one embodiment of the present invention. The electrodeposition apparatus 20 shown in Fig. 3 has an electrodeposition tank 21 and a power source 22. An electrodeposition liquid 30 is stored in the electrodeposition tank 21. A conductor body 11 and a counter electrode 23 are immersed in the electrodeposition liquid 30. The power source 22 is connected to the conductor body 11 and the counter electrode 23.
[0028] The electrodeposition liquid 30 contains resin particles 31 and a solvent 32 . The resin particles 31 contain a polyamideimide resin having a carboxyl group. The resin particles 31 are negatively charged. The particle diameter of the resin particles 31 is not particularly limited, but may be, for example, within a range of 50 nm to 500 nm in terms of median diameter. The content of the resin particles 31 in the electrodeposition liquid is not particularly limited, but may be, for example, within a range of 1% by mass to 10% by mass, and preferably within a range of 1.5% by mass to 5% by mass.
[0029] The solvent 32 may include an organic solvent, water, and a hydrophobic base. As the organic solvent, for example, polar solvents such as N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3 dimethylimidazolidinone, dimethyl sulfoxide (DMSO), and γ-butyrolactone (γ-BL) can be used. These solvents may be used alone or in combination of two or more. In addition, it is preferable that the hydrophobic base has affinity for the organic solvent. Examples of the hydrophobic base include tri-n-propylamine, tri-n-butylamine, dibenzylamine, decylamine, octylamine, hexylamine, diamylamine, dihexylamine, dioctylamine triamylamine, trihexylamine, trioctylamine, tribenzylamine, and aniline. These hydrophobic bases may be used alone or in combination of two or more. The content of the organic solvent relative to the total amount of the organic solvent and water is, for example, in the range of 10% by mass to 87% by mass, and the content of the hydrophobic base is, for example, in the range of 0.02% by mass to 0.1% by mass with respect to the electrodeposition solution 30.
[0030] The electrodeposition liquid 30 can be obtained, for example, by adding water, which is a poor solvent for the polyamideimide solution, to a polyamideimide resin solution prepared by mixing a polyamideimide resin having a carboxyl group, an organic solvent capable of dissolving the polyamideimide resin, and a hydrophobic base.
[0031] The electrodeposition liquid 30 may further contain fluororesin particles. Examples of the fluororesin particles include polytetrafluoroethylene (PTFE), perfluoroalkoxy fluororesin (PFA) particles, and tetrafluoroethylene-hexafluoropropylene copolymer (FEP) particles. The content of the fluororesin particles in the electrodeposition liquid is not particularly limited, but is, for example, within a range of 0.5% by mass to 10% by mass with respect to the electrodeposition liquid 30, and within a range of 100% by mass to 1000% by mass with respect to the resin particles 31 (polyamideimide resin particles).
[0032] In the electrodeposition step S02, the conductor body 11 immersed in the electrodeposition liquid 30 is used as the anode, and the counter electrode 23 is used as the cathode, and a DC voltage is applied using the power source 22. The applied DC voltage is preferably within a range of 1 V to 600 V. By applying the DC voltage, the resin particles 31 in the electrodeposition liquid 30 are electrodeposited onto the surface of the conductor body 11 to form an electrodeposition layer.
[0033] The baking step S03 is a step of heating the conductor body 11 with the electrodeposition layer to bake the electrodeposition layer onto the conductor body 11 to form an insulating layer and obtain an insulating aluminum alloy conductor. The baking temperature may be within a temperature range in which the polyamideimide resin in the electrodeposition layer hardens to form an insulating layer on the substrate, and may be within a range of 200° C. to 450° C. The baking time may be within a range of, for example, 1 minute to 60 minutes.
[0034] Before baking the electrodeposition layer onto the conductor body, the electrodeposition liquid 30 adhering to the conductor body 11 with the electrodeposition layer may be removed. Methods for removing the electrodeposition liquid 30 include a method of blowing compressed air onto the conductor body 11 with the electrodeposition layer to blow off the electrodeposition liquid 30, and a method of heating the conductor body 11 with the electrodeposition layer at a temperature lower than the temperature at which the electrodeposition layer is formed to volatilize the electrodeposition liquid 30.
[0035] Through the above-mentioned steps, the insulating layer 12 containing polyamide-imide resin can be formed on the surface of the conductor body 11. If no oil or grease is attached to the surface of the conductor body 11, the degreasing step S01 may be omitted.
[0036] According to the insulating aluminum alloy conductor 10 configured as above, the insulating layer 12 contains a polyamide-imide resin having a carboxyl group, and therefore can be manufactured by anionic electrodeposition. The Si content of the conductor body 11 is set to be within a range of 0.3 mass% or more and 13.5 mass% or less, so that in the electrodeposition step S02 when manufacturing the insulating aluminum alloy conductor 10 by anionic electrodeposition, the pH of the electrodeposition liquid 30 around the conductor body 11 is lowered, and even when the electrodeposition liquid 30 becomes acidic, aluminum is less likely to be eluted from the conductor body 11. This reduces the amount of hydrogen gas generated by the elution of aluminum, thereby reducing the appearance defects of the electrodeposition layer. Furthermore, the Mg content of the conductor body 11 is set to be 1.8 mass% or less, so that aluminum is more unlikely to be eluted from the conductor body 11 even when the electrodeposition liquid 30 becomes acidic. Therefore, the insulating aluminum alloy conductor 10 configured as above has a smooth surface of the insulating layer 12 with few irregularities.
[0037] Furthermore, in the insulating aluminum alloy conductor of the present invention, when the Si content of the conductor body 11 is within the range of 0.5 mass% or more and 11.0 mass% or less, aluminum is less likely to dissolve from the conductor body 11 even when the electrodeposition solution becomes acidic during the electrodeposition process when producing the insulating aluminum alloy conductor 10 by anionic electrodeposition.
[0038] In the insulating aluminum alloy conductor 10 of the present invention, when the Mg content of the conductor body 11 is 1.3 mass% or less, even when the electrodeposition solution becomes acidic, aluminum is more unlikely to be eluted from the conductor body 11. In the insulating aluminum alloy conductor 10 of the present embodiment, when the Mg content of the conductor body 11 is 0.8 mass% or more, the hardness of the conductor body 11 is increased.
[0039] According to the manufacturing method of the insulating aluminum alloy conductor of this embodiment, the electrodeposition liquid 30 contains resin particles 31 containing polyamideimide resin having a carboxyl group, so that the electrodeposition layer can be formed by anionic electrodeposition. The Si content of the conductor body 11 is set to be within a range of 0.3 mass% or more and 13.5 mass% or less, so that in the electrodeposition step S02, even when the pH of the electrodeposition liquid 30 around the conductor body 11 decreases and the electrodeposition liquid 30 becomes acidic, aluminum is less likely to be eluted from the conductor body 11. This reduces the amount of hydrogen gas generated by the elution of aluminum, so that the appearance defect of the electrodeposition layer is reduced. Furthermore, the Mg content of the conductor body 11 is set to be 1.8 mass% or less, so that aluminum is more unlikely to be eluted from the conductor body 11 even when the electrodeposition liquid 30 becomes acidic. Therefore, the manufacturing method of this embodiment makes it possible to manufacture an insulating aluminum alloy conductor 10 in which the surface of the insulating layer 12 is smooth and has few irregularities.
[0040] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. EXAMPLES
[0041] [Example 1] (Preparation of electrodeposition solution) Carboxyl group-containing polyamideimide (PAI) was dissolved in NMP (N-methyl-2-pyrrolidone) to obtain a PAI varnish with a PAI concentration of 20% by mass. NMP, tri-n-propylamine, and water were added to the obtained PAI varnish to precipitate PAI particles, and an electrodeposition solution with PAI particles:NMP:water:tri-n-propylamine=2.0% by mass:79% by mass:18.95% by mass:0.05% by mass was prepared.
[0042] (Degreasing process) A conductor body (A2024, width: 1 cm, length: 10 cm, thickness: 0.3 cm) made of an aluminum alloy containing 0.5% by mass of Si, 1.8% by mass of Mg, and the remainder being Al, was prepared as an aluminum alloy conductor. The conductor body was machined to a surface roughness Ra of 2 μm. The machined conductor body was immersed for 1 minute in a degreaser aqueous solution containing 10% by mass of a degreaser (Neo Sandep S, manufactured by Nippon Marcel Co., Ltd.). After immersion, the conductor body was removed from the degreaser, washed with water, and then the moisture on the surface was wiped off. In this manner, the conductor body was degreased.
[0043] (electrodeposition process) The electrodeposition solution prepared in (1) above was placed in an electrodeposition tank equipped with a stirrer and a thermostat. A cylindrical counter electrode made of pure copper (diameter: 5 cm, length: 15 cm, thickness: 0.3 mm) was immersed in this electrodeposition solution. Next, the conductor body degreased in (2) above was immersed in the center of the cylindrical counter electrode. Furthermore, a stirrer and a throw-in thermostat were placed in the electrodeposition solution.
[0044] The temperature of the electrodeposition solution was adjusted to 10° C. Next, while stirring the electrodeposition solution, a voltage of 100 V was applied for 20 seconds between the conductor body as the anode and the cylindrical counter electrode as the cathode to adhere the PAI resin particles to the surface of the conductor body, thereby obtaining a conductor body with an electrodeposition layer.
[0045] (Baking process) The conductor body with the electrodeposition layer was removed from the electrodeposition tank, and the electrodeposition layer was washed with water. Next, the washed conductor body with the electrodeposition layer was heated at 100°C for 10 minutes to dry the electrodeposition layer, and then heated at 220°C for 30 minutes to bake the electrodeposition layer onto the conductor body.
[0046] Thus, an insulating aluminum alloy conductor was produced. The insulating layer of the resulting insulating aluminum alloy conductor had a thickness of 34 μm.
[0047] [Examples 2 to 6 of the present invention, Comparative Examples 1 to 3] An insulating aluminum alloy conductor was produced in the same manner as in Example 1 of the present invention, except that the conductor body used had a chemical composition shown in Table 1 below. The thickness of the insulating layer of the obtained insulating aluminum alloy conductor was 34 μm, the same as that obtained in Example 1 of the present invention.
[0048] [evaluation] The following evaluations were carried out on the insulating aluminum alloy conductors obtained in Inventive Examples 2 to 6 and Comparative Examples 1 to 3. The results are shown in Table 1 below.
[0049] (Foaming of insulation layer) The appearance of the insulating layers on both sides of the obtained insulating aluminum alloy conductor was observed using an optical microscope, and the number of bubbles in the insulating layers was counted. 2 When the number of winning bubbles was 9 or less, it was marked as "◎", when it was 10 to 29, it was marked as "◯", when it was 30 to 59, it was marked as "△", and when it was 60 or more, it was marked as "X".
[0050] (hardness) The Brinell hardness of the obtained insulating aluminum alloy conductor was evaluated. The evaluation was performed by measuring the Brinell hardness of the portion of the insulating aluminum alloy conductor where no insulating layer was formed. The Brinell hardness was measured in accordance with JIS Z 2243-1:2018 (Brinell hardness test - Part 1: Test method). A Brinell hardness of 70 or more was evaluated as "Good", a Brinell hardness of 20 or more but less than 70 was evaluated as "Good", and a Brinell hardness of less than 20 was evaluated as "Poor".
[0051] [Table 1]
[0052] The insulating aluminum alloy conductors obtained in Examples 1 to 6 of the present invention, in which the Si content and the Mg content of the conductor body are within the ranges of the present invention, all showed reduced foaming of the insulating layer. The insulating aluminum alloy conductors obtained in Examples 1, 3, and 4 of the present invention, in which the Mg content of the conductor body is 0.8 mass% or more, showed high hardness. In contrast, the insulating aluminum alloy conductor obtained in Comparative Example 1, in which the Si content of the conductor body is lower than the range of the present invention, showed a lot of foaming of the insulating layer and a low hardness. The insulating aluminum alloy conductor obtained in Comparative Example 2, in which the Si content of the conductor body is lower than the range of the present invention and the Mg content is higher than the range of the present invention, showed high hardness but showed a lot of foaming of the insulating layer. The insulating aluminum alloy conductor obtained in Comparative Example 3, in which the Si content of the conductor body is within the range of the present invention and the Mg content is higher than the range of the present invention, showed high hardness but showed a lot of foaming of the insulating layer, similar to Comparative Example 2. [Explanation of symbols]
[0053] 10 Insulated aluminum alloy conductors 11 Conductor body 12 Insulating layer 20 Electrodeposition equipment 21 Electroplating bath 22 Power supply 23 Counter electrode 30 Electrodeposition liquid 31 Resin particles 32 Solvents
Claims
1. An insulated aluminum alloy conductor comprising a conductor body made of an aluminum alloy and an insulating layer covering the conductor body, The conductor body has a Si content in the range of 0.3 mass % or more and 13.5 mass % or less, and a Mg content in the range of 1.8 mass % or less, 1. An insulating aluminum alloy conductor, wherein the insulating layer contains a polyamide-imide resin having a carboxyl group.
2. 2. The insulated aluminum alloy conductor according to claim 1, wherein the Si content of the conductor body is within a range of 0.5 mass % to 11.0 mass %.
3. 3. The insulated aluminum alloy conductor according to claim 1, wherein the Mg content of the conductor body is within the range of 0.8% by mass to 1.3% by mass.
4. an electrodeposition step of electrodepositing resin particles on a surface of a conductor body made of an aluminum alloy by anionic electrodeposition to obtain a conductor body with an electrodeposition layer; a baking step of heating the conductor body with the electrodeposition layer to bake the electrodeposition layer onto the conductor body to form an insulating layer and obtain an insulated aluminum alloy conductor, The conductor body has a Si content in the range of 0.3 mass % or more and 13.5 mass % or less, and a Mg content in the range of 1.8 mass % or less, A method for producing an insulating aluminum alloy conductor, characterized in that in the electrodeposition step, the conductor body is immersed in an electrodeposition liquid containing resin particles containing a polyamideimide resin having a carboxyl group.