Method for producing polycarbonate copolymer and polysiloxane compound, polycarbonate copolymer, polysiloxane compound, composition, and molded body

The production of a polycarbonate copolymer with a siloxane structural unit using a transesterification catalyst under reduced pressure addresses the fluidity and impact resistance issues of conventional polycarbonate resins, enabling efficient and environmentally friendly manufacturing for optical applications.

JP7567778B2Active Publication Date: 2024-10-16MITSUBISHI GAS CHEM CO INC

Patent Information

Application Number
JP2021509353
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-22
Filing Date
2020-03-19
Publication Date
2024-10-16
Estimated Expiration
2040-03-19

AI Technical Summary

Technical Problem

Conventional polycarbonate resins face challenges with poor fluidity due to high melt viscosity, making injection molding of precision parts and thin objects difficult, and require high temperatures that lead to longer molding cycles and increased costs, while existing methods to improve fluidity often compromise impact resistance.

Method used

A method for producing a polycarbonate copolymer with a siloxane structural unit using a transesterification catalyst, involving diaryloxysilane, dialkoxysilane, and silicon compounds, under reduced pressure to remove alcohol by-products without solvents, ensuring high fluidity and impact resistance.

Benefits of technology

The method produces a polycarbonate copolymer with enhanced fluidity and impact resistance, allowing for efficient production without environmental hazards from acid by-products and solvent use, suitable for optical uses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567778000001
    Figure 0007567778000001
  • Figure 0007567778000002
    Figure 0007567778000002
  • Figure 0007567778000003
    Figure 0007567778000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing a method for efficiently producing a polycarbonate copolymer which has siloxane constituent units and exhibits excellent impact resistance and high fluidity when molten; a method for efficiently producing a polycarbonate copolymer or a polysiloxane compound, in which by-products having a high environmental load, such as acids, are not produced, and which can be carried out without using a solvent, and especially without using a solvent that causes safety concerns; and a polysiloxane compound. The abovementioned problem can be solved by means of a method for producing a polycarbonate copolymer which has siloxane constituent units represented by any of formulae (1-1) to (1-4) and prescribed polycarbonate constituent units, the method having a polymerization step for polymerizing a silane-based compound selected from among a prescribed diaryloxysilane compound, a prescribed dialkoxysilane compound and a prescribed silicon compound, a carbonate compound and a diol compound such as an aromatic diol compound or an alicyclic diol compound in the presence of a transesterification catalyst. The polymerization step is carried out in a molten state under reduced pressure while removing alcohols derived from the carbonate compound. (In the formulae, R1 to R10, R30 to R33, Z1, Z2, J1, K1, A1, A2, L1, L2 and X are as described in the description of the present application.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a polycarbonate copolymer and a polysiloxane compound, and in particular to a method for producing a polycarbonate copolymer having a siloxane structural unit, and a polycarbonate copolymer, etc. [Background technology]

[0002] Thermoplastic polycarbonate resin has excellent impact resistance and mechanical properties, and is formed into various molded products using simple, highly productive processing methods such as injection molding. It is used in a wide range of industrial fields, including electrical and electronic equipment, office automation equipment, heavy electrical machinery, precision machinery, and the automotive industry.

[0003] Conventional polycarbonate resins have the drawback of poor fluidity due to their high melt viscosity, which can make it difficult to use them in injection molding precision parts or thin objects. For this reason, it has been necessary to raise the temperature during molding, and molding at high temperatures has the problem of longer molding cycles and higher costs, or of the polycarbonate resin deteriorating during molding. Attempts have been made to improve the fluidity of polycarbonate resins (Patent Document 1, Patent Document 2), but it has not been possible to achieve sufficiently high fluidity without impairing the inherent properties of polycarbonate resins (such as impact resistance).

[0004] In addition to polycarbonate resins, aromatic polysiloxane polymers, also known as polyarylenesiloxanes, are known as materials for molded products produced by molding methods such as injection molding (see, for example, Patent Document 3). In recent years, the importance of polysiloxane compounds such as polyarylenesiloxanes has increased, and polyarylenesiloxanes are used, for example, as release layers in photocopying, photoresist materials, plasticizers for polycarbonates, and components of powder surface coating systems.

[0005] Known methods for producing polysiloxane compounds such as polyarylenesiloxanes include a method in which dimethyldichlorosilane is reacted with bisphenol A in a solvent to produce hydrochloric acid (Non-Patent Document 1) and a method in which the reaction is carried out in a solvent to which acetic acid has been added (Patent Document 4).

[0006] Moreover, polycarbonate resins, polysiloxane compounds, and the like that are particularly suitable for specific applications such as optical applications have not necessarily been realized so far. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2016-148047 A [Patent Document 2] Japanese Patent Publication No. 62-297319 [Patent Document 3] Special Publication No. 08-502537 [Patent Document 4] Special Publication No. 2015-512999 [Non-patent literature]

[0008] [Non-Patent Document 1] Journal of Polymer Science, Vol.18, 3119-3127(1980) Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention provides a polycarbonate copolymer having a siloxane structural unit, which has excellent impact resistance and high fluidity when melted, and a method for efficiently producing the polycarbonate copolymer.

[0010] The present invention also provides a method for safely and efficiently producing a polycarbonate copolymer having a siloxane structural unit, a polysiloxane compound, etc. For example, the present invention provides a method for efficiently producing a polycarbonate copolymer and a polysiloxane compound such as a polyarylenesiloxane, without generating corrosive substances such as hydrochloric acid or acetic acid, without requiring the use of a solvent, and while reducing the environmental load.

[0011] Furthermore, the present invention provides polycarbonate resins, polysiloxane compounds, etc. that are particularly suited to specific applications such as optical applications. [Means for solving the problem]

[0012] The present invention provides a polycarbonate copolymer, which contains a siloxane structural unit and has excellent impact resistance and high fluidity, and a method for producing the polycarbonate copolymer, which are described below. The present invention also provides a method for efficiently producing a polycarbonate copolymer or a polysiloxane compound, which does not produce by-products that have a high environmental load, such as acids, and can be carried out without a solvent, particularly without a solvent that requires safety considerations, and also provides a polysiloxane compound, etc.

[0013] [1] In the presence of a transesterification catalyst, a diaryloxysilane compound containing at least one of a dialkyldiaryloxysilane, a diaryldiaryloxysilane, and a monoalkylmonoaryldiaryloxysilane; a dialkoxysilane compound containing at least one of a dialkyldialkoxysilane, a diaryldialkoxysilane, and a monoalkylmonoaryldialkoxysilane; A silicon compound containing at least one of a cyclic siloxane compound and a linear siloxane compound; A silane-based compound selected from the group consisting of A carbonate compound; The method includes a polymerization step of polymerizing an aromatic diol compound or an alicyclic diol compound with a diol compound, A method for producing a polycarbonate copolymer having a siloxane constituent unit represented by any one of formulas (1-1) to (1-4) and a polycarbonate constituent unit represented by any one of formulas (3-1) to (3-4), while removing alcohol derived from the carbonate compound in a molten state under reduced pressure in a polymerization step. [ka] (In formulas (1-1) to (1-4), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 and R 30 ~R 33 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Z1 and Z2 each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, Each J1 independently represents an integer of 0 to 5, Each K1 independently represents an integer of 0 to 5, A1 and A2 each independently represent -O- or -CH-; L1 and L2 each independently represent an integer of 0 to 3, X is a single bond or any one of the structural formulas represented by the following formula (2): [ka] (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less. [ka] (In formulas (3-1) to (3-4), R 13 ~R 20 and R 40 ~R 51 each independently represents hydrogen, halogen, alkoxy, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Z3 and Z4 each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, Each J2 independently represents an integer of 0 to 5, Each K2 independently represents an integer of 0 to 5, A1 and A2 each independently represent -O- or -CH-; L1 and L2 each independently represent an integer of 0 to 3, Y is a single bond or a structural formula represented by formula (4), [ka] (In the formula, R 21 , and R 22 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 21 and R 22 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, c and d each independently represent 0 or an integer of 1 or more and 5000 or less. [2] Z1 to Z4 each independently represent an alkylene group having 1 to 3 carbon atoms which may have a substituent, J1 and J2 each independently represent an integer of 0 to 2, K1 and K2 each independently represent an integer of 0 to 2. A method for producing the polycarbonate copolymer described in [1] above. [3] The X is R 11 and R 12 and / or the Y is R 21 and R 22 The method for producing a polycarbonate copolymer according to the above [1] or [2], wherein the polycarbonate structural unit represents a fluorene ring structure formed by bonding together.

[0014] [4] In the presence of a transesterification catalyst, a diaryloxysilane compound containing at least one of a dialkyldiaryloxysilane, a diaryldiaryloxysilane, and a monoalkylmonoaryldiaryloxysilane; a dialkoxysilane compound containing at least one of a dialkyldialkoxysilane, a diaryldialkoxysilane, and a monoalkylmonoaryldialkoxysilane; A silicon compound containing at least one of a cyclic siloxane compound and a linear siloxane compound; A silane-based compound selected from the group consisting of The method includes a polymerization step of polymerizing a carbonate compound and a diol compound including an aromatic diol compound or an alicyclic diol compound, A method for producing a polycarbonate copolymer having a siloxane constituent unit represented by formula (1) and a polycarbonate constituent unit represented by formula (3), while removing alcohol derived from the carbonate compound under reduced pressure in a molten state in a polymerization step. [ka] (In formula (1), R 1 , and R 2each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, X is any one of the structural formulas represented by the following formula (2): [ka] (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less. [ka] (In the formula, R 13 ~R 20 Each independently represents hydrogen, halogen, alkoxy, or a substituent. an alkyl group having 1 to 20 carbon atoms which may have a substituent; an alkenyl group having 2 to 20 carbon atoms which may have a substituent; a group, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Y is any one of the structural formulas represented by formula (4), [ka] (In the formula, R 21 , and R 22 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R21 and R 22 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, c and d each independently represent 0 or an integer of 1 or more and 5000 or less. [5] The method for producing a polycarbonate copolymer according to any one of the above [1] to [4], wherein the transesterification catalyst contains an alkali metal compound and / or an alkaline earth metal. [6] The method for producing a polycarbonate copolymer according to the above [5], wherein the alkali metal compound and / or alkaline earth metal compound contains a carbonate. [7] The method for producing a polycarbonate copolymer according to any one of the above [1] to [6], wherein the polycarbonate copolymer has a weight average molecular weight of 10,000 to 300,000. [8] In the polymerization step, the amount of the transesterification catalyst relative to the diol compound is 1.0 × 10 in terms of molar ratio. -7 ~1.0×10 -2 The method for producing a polycarbonate copolymer according to any one of the above [1] to [7], [9] The method for producing a polycarbonate copolymer according to any one of the above [1] to [8], wherein the reaction temperature in the polymerization step is in the range of 150° C. or higher and 300° C. or lower.

[10] The method for producing a polycarbonate copolymer according to any one of the above [1] to [9], further comprising a depressurization step of gradually reducing the reaction pressure to 400 Pa or less in the polymerization step.

[11] The method for producing a polycarbonate copolymer according to any one of the above [1] to

[10] , wherein in the polymerization step, the carbonate compound and the diol compound are polymerized under a pressure of 400 Pa or less.

[12] The method for producing the polycarbonate copolymer according to any one of the above [1] to

[11] , wherein no solvent is used in the polymerization step.

[13] The method for producing a polycarbonate copolymer according to any one of the above [1] to

[12] , wherein a ratio of a total molar number of the carbonate compound and the diaryloxysilane compound used in the polymerization step to a molar number of the diol compound is 0.9 or more and 1.2 or less.

[14] The method for producing a polycarbonate copolymer according to any one of the above [1] to

[13] , wherein in the polycarbonate copolymer, the number of moles of the siloxane constituent units is 1 to 1,000, and the number of moles of the polycarbonate constituent units is 1 to 1,000.

[15] The method for producing a polycarbonate copolymer according to any one of the above [1] to

[14] , wherein a molar ratio of the siloxane constituent units to the polycarbonate constituent units is 0.01:99.99 to 99.99:0.01.

[16] The Q value of the polycarbonate copolymer measured under conditions of 280 °C and 160 kgf is 8(×10 -2 cm 3 s -1 ) or more.

[0015]

[17] A polycarbonate copolymer having a siloxane constituent unit represented by any one of formulas (1-1) to (1-4) and a polycarbonate constituent unit represented by any one of formulas (3-1) to (3-4), wherein the content of low molecular weight compounds having a weight average molecular weight of 1,000 or less is 30% by weight or less. [ka] (In formulas (1-1) to (1-4), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 and R 3 ~R 33each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Z1 and Z2 each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, Each J1 independently represents an integer of 0 to 5, Each K1 independently represents an integer of 0 to 5, A1 and A2 each independently represent -O- or -CH-; L1 and L2 each independently represent an integer of 0 to 3, X is a single bond or any one of the structural formulas represented by the following formula (2): [ka] (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less. [ka] (In formulas (3-1) to (3-4), R 13 ~R 20 and R 40 ~R 51 each independently represents hydrogen, halogen, alkoxy, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Z3 and Z4 each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, Each J2 independently represents an integer of 0 to 5, Each K2 independently represents an integer of 0 to 5, A1 and A2 each independently represent -O- or -CH-; L1 and L2 each independently represent an integer of 0 to 3, Y is a single bond or a structural formula represented by formula (4), [ka] (In the formula, R 21 , and R 22 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 21 and R 22 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, c and d each independently represent 0 or an integer of 1 or more and 5000 or less.

[18] Z1 to Z4 each independently represent an alkylene group having 1 to 3 carbon atoms which may have a substituent, J1 and J2 each independently represent an integer of 0 to 2, K1 and K2 each independently represent an integer of 0 to 2. The polycarbonate copolymer according to

[17] above.

[19] The X is R 11 and R 12 and / or the Y is R 21 and R 22 The polycarbonate copolymer according to the above

[17] or

[18] , having polycarbonate structural units representing a fluorene ring structure formed by bonding together.

[0016]

[20] A polycarbonate copolymer having a siloxane structural unit represented by formula (1) and a polycarbonate structural unit represented by formula (3), wherein the proportion of low molecular weight compounds having a weight average molecular weight of 1,000 or less, calculated from the GPC area ratio, is 30% by weight or less. [ka] (In formula (1), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, X is any one of the structural formulas represented by the following formula (2): [ka] (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less. [ka] (In the formula, R 13 ~R 20 each independently represents hydrogen, halogen, alkoxy, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Y is any one of the structural formulas represented by formula (4), [ka] (In the formula, R 21 , and R 22 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 21 and R 22 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, c and d each independently represent 0 or an integer of 1 or more and 5000 or less.

[21] The polycarbonate copolymer according to any one of the above

[17] to

[20] , wherein the number of moles of the siloxane constituent units in the polycarbonate copolymer is 1 to 1,000, and the number of moles of the polycarbonate constituent units in the polycarbonate copolymer is 1 to 1,000.

[22] The polycarbonate copolymer according to any one of the above

[17] to

[21] , wherein a molar ratio of the siloxane constituent units to the polycarbonate constituent units is 0.01:99.9 to 99.9:0.01.

[23] The polycarbonate copolymer according to the above

[22] , wherein a molar ratio of the siloxane constituent units to the polycarbonate constituent units is 30.00:70.00 to 99.9:0.01.

[24] The Q value measured under the conditions of 280°C and 160 kgf is 8(×10 -2 cm 3 s -1 ) or more.

[0017]

[25] A polycarbonate copolymer having a siloxane constituent unit represented by any one of formulas (1-1) to (1-4) and a polycarbonate constituent unit represented by any one of formulas (3-1) to (3-4), and having a total content of cyclic units represented by formulas (5-1) to (5-3) of 4.0% by weight or less. [ka] (In formulas (1-1) to (1-4), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 and R 3 ~R 33 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Z1 and Z2 each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, Each J1 independently represents an integer of 0 to 5, Each K1 independently represents an integer of 0 to 5, A1 and A2 each independently represent -O- or -CH-; L1 and L2 each independently represent an integer of 0 to 3, X is a single bond or any one of the structural formulas represented by the following formula (2): [ka] (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less. [ka] (In formulas (3-1) to (3-4), R13 ~R 20 and R 40 ~R 51 each independently represents hydrogen, halogen, alkoxy, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Z3 and Z4 each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, Each J2 independently represents an integer of 0 to 5, Each K2 independently represents an integer of 0 to 5, A1 and A2 each independently represent -O- or -CH-; L1 and L2 each independently represent an integer of 0 to 3, Y is a single bond or a structural formula represented by formula (4), [ka] (In the formula, R 21 , and R 22 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 21 and R 22 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, c and d each independently represent 0 or an integer of 1 or more and 5000 or less. [ka] (In formulas (5-1) to (5-3), m and n represent the total number of structural units containing a (-OSi(R1R2)O-) moiety and the total number of structural units containing a (-OC(=O)O-) moiety in each cyclic structure, respectively; (In formula (5-1), m represents an integer of 2 to 10, In formula (5-2), n represents an integer of 2 to 10. In formula (5-3), the total value of m is 1 to 10, and the total value of n is 1 to 10. In formula (5-3), the structural units containing a (-OSi(R1R2)O-) moiety and the structural units containing a (-OC(=O)O-) moiety may be arranged in any manner. In formulas (5-1) to (5-3), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 and R 13 ~R 20 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, X1 and X2 each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, i and ii each independently represent an integer of 0 to 5, X is a single bond or any one of the structural formulas represented by the following formula (2): [ka] (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less.

[26] The polycarbonate copolymer according to any one of the above

[17] to

[25] , wherein the total content of cyclic structures represented by the formulae (6-1) and (6-2) is 2.0% by weight or less. [ka] (In formulas (6-1) and (6-2), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 and R 30 ~R 33 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, X1 and X2 each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, i and ii each independently represent an integer of 0 to 5, n represents an integer from 2 to 10; X is a single bond or any one of the structural formulas represented by the following formula (2): [ka] (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less.

[27] The polycarbonate copolymer according to any one of the above

[17] to

[26] , having a 1% mass loss thermal decomposition temperature of 415°C or lower.

[28] A composition comprising the polycarbonate copolymer according to any one of the above

[17] to

[27] and a polycarbonate resin.

[29] The composition according to

[28] above, wherein the total amount of Si in the composition is 0.1 to 20 mass%.

[30] The composition according to any one of

[28] and

[29] above, wherein Q1, which is a Q value of the composition measured under conditions of 280°C and 160 kgf, is 120% or more of Q2, which is a Q value of only the polycarbonate resin contained in the composition measured under the same conditions.

[31] A molded article obtained by molding the polycarbonate copolymer according to any one of the above

[17] to

[27] .

[32] An optical lens comprising the polycarbonate copolymer according to any one of the above

[17] to

[27] .

[33] An optical lens obtained by molding the composition according to any one of the above items

[28] to

[30] .

[0018]

[34] An oxysilane compound including at least one of a diaryloxysilane compound which is any one of a dialkyl diaryloxy silane, a diaryl diaryloxy silane, and a monoalkyl monoaryl diaryloxy silane, and a dialkoxysilane compound which is any one of a dialkyl dialkoxy silane, a diaryl dialkoxy silane, and a monoalkyl monoaryl dialkoxy silane; The method includes a polymerization step of polymerizing an aromatic diol compound or an alicyclic diol compound with a diol compound, In the polymerization step, the oxysilane compound and the diol compound are polymerized in a molten state under reduced pressure using an ester exchange catalyst while removing the resulting aryl alcohol and / or alkyl alcohol, and the amount of the ester exchange catalyst relative to the diol compound is 0.01 μmol / mol to 16,000 μmol / mol in terms of a molar ratio; A method for producing a polysiloxane compound, which comprises producing a poly(arylene / alkylene)siloxane compound having a weight average molecular weight of 10,000 to 300,000 and containing a constituent unit represented by any one of the following formulas (1-1') to (1-4'): [ka] (In formulas (1-1') to (1-4'), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 and R 30 ~R 33 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Z1 and Z2 each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, Each J1 independently represents an integer of 0 to 5, Each K1 independently represents an integer of 0 to 5, A1 and A2 each independently represent -O- or -CH-; L1 and L2 each independently represent an integer of 0 to 3, m1 to m4 each represent the total number of structural units in each formula and are natural numbers from 10 to 1000, X is a single bond or any one of the structural formulas represented by the following formula (2): [ka] (In the formula, R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less.

[35] Z1 and Z2 each independently represent an alkylene group having 1 to 3 carbon atoms which may have a substituent, Each J1 independently represents an integer of 0 to 2, K 12 each independently represents an integer of 0 to 2, A method for producing the polysiloxane compound according to the above item

[34] .

[36] The X is R 11 and R 12 and / or the Y is R 21 and R 22 The method for producing a polysiloxane compound according to the above

[34] or

[35] , which has polycarbonate structural units that represent a fluorene ring structure formed by bonding together.

[0019]

[37] A method for producing a photocatalyst comprising the steps of: polymerizing a diaryloxysilane compound containing at least one of a dialkyl diaryloxy silane, a diaryl diaryloxy silane, and a monoalkyl monoaryl diaryloxy silane with an aromatic diol compound; In the polymerization step, the diaryloxysilane compound and the aromatic diol compound are polymerized in a molten state under reduced pressure using a transesterification catalyst while removing aryl alcohol, and the amount of the transesterification catalyst relative to the aromatic diol compound is 0.01 μmol / mol to 16,000 μmol / mol in terms of molar ratio; A method for producing a polysiloxane compound, which comprises producing a polyarylenesiloxane compound having a weight average molecular weight of 10,000 to 300,000 and containing a constituent unit represented by the following formula (1): [ka] (In the formula, R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, m is a natural number between 10 and 1000. X is any one of the structural formulas represented by the following formula (2): [ka] (In the formula, R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less.

[38] The method for producing a polysiloxane compound according to any one of the above

[34] to

[37] , wherein the reaction temperature in the polymerization step is in the range of 150° C. or higher and 300° C. or lower.

[39] The method for producing a polysiloxane compound according to any one of the above

[34] to

[38] , wherein in the polymerization step, the reaction pressure is 101,300 Pa or less.

[40] The method for producing a polysiloxane compound according to any one of the above

[34] to

[39] , further comprising a depressurization step of gradually reducing the reaction pressure to 400 Pa or less in the polymerization step.

[41] The method for producing a polysiloxane compound according to any one of the above

[34] to

[40] , wherein in the polymerization step, the amount of the transesterification catalyst relative to the aromatic diol compound is 0.1 to 100 μmol / mol in terms of molar ratio.

[42] The method for producing a polysiloxane compound according to any one of the above

[34] to

[41] , wherein the transesterification catalyst contains an alkali metal compound and / or an alkaline earth metal compound.

[43] The method for producing a polysiloxane compound according to the above

[41] , wherein the alkali metal compound and / or alkaline earth metal compound includes at least one of a carbonate, a hydroxide, an oxide, and an alkoxy compound.

[44] The method for producing a polysiloxane compound according to the above

[42] , wherein the alkali metal compound and / or alkaline earth metal compound is a carbonate.

[45] The method for producing a polysiloxane compound according to any one of the above

[34] to

[44] , wherein no solvent is used in the polymerization step.

[46] The method for producing a polysiloxane compound according to any one of the above

[34] to

[45] , wherein a molar ratio of the diaryloxysilane compound to the aromatic diol compound used in the polymerization step is 0.9 or more and 1.2 or less.

[47] The method for producing a polysiloxane compound according to any one of the above

[34] to

[46] , wherein in the polymerization step, the oxysilane compound or the diaryloxysilane compound and the diol compound or the aromatic diol compound are polymerized at a reaction temperature higher than 200° C. and / or under reduced pressure.

[0020]

[48] ​​A polysiloxane compound containing a constitutional unit represented by any one of formulas (1-1) to (1-4), having a weight average molecular weight of 5,000 to 300,000, and having a total content of cyclic units represented by formula (5-4) of 4.0 wt% or less. [ka] (In formulas (1-1) to (1-4), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 and R 30 ~R 33each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Z1 and Z2 each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, Each J1 independently represents an integer of 0 to 5, Each K1 independently represents an integer of 0 to 5, A1 and A2 each independently represent -O- or -CH-; L1 and L2 each independently represent an integer of 0 to 3, X is a single bond or any one of the structural formulas represented by the following formula (2): [ka] (In the formula, R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less. [ka] (In formula (5-4), the constitutional unit represented by formula (5-4) may be arranged arbitrarily with other constitutional units, and the total value of m is 2 to 10. R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, X1 and X2 each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, i and ii each independently represent an integer of 0 to 5, m represents an integer from 2 to 10; X is a single bond or any one of the structural formulas represented by the following formula (2): [ka] (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less.

[49] The polysiloxane compound according to the above

[48] , wherein the total content of cyclic structures represented by the formulae (6-1) and (6-2) is 4.0% by weight or less. [ka] (In formulas (6-1) and (6-2), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 and R 30 ~R 33each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, X1 and X2 each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, i and ii each independently represent an integer of 0 to 5, n represents an integer from 2 to 10; X is a single bond or any one of the structural formulas represented by the following formula (2): [ka] (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less.

[50] The polysiloxane compound according to

[48] or

[49] above, having a 1% mass loss thermal decomposition temperature of 415°C or lower.

[51] A composition comprising a polysiloxane compound produced by the production method according to any one of the above

[34] to

[46] or a polysiloxane compound according to any one of the above

[48] to

[50] , and a polycarbonate resin.

[52] The composition according to

[51] above, wherein the total amount of Si in the composition is 0.1 to 20 mass%.

[53] The composition according to any one of

[51] and

[52] above, wherein Q1, which is a Q value of the composition measured under conditions of 280°C and 160 kgf, is 120% or more of Q2, which is a Q value of only the polycarbonate resin contained in the composition measured under the same conditions.

[54] A molded article obtained by molding the polysiloxane compound produced by the production method according to any one of the above

[34] to

[46] or the polysiloxane compound according to any one of the above

[48] to

[50] .

[55] An optical lens comprising a polysiloxane compound produced by the production method according to any one of the above

[34] to

[46] or a polysiloxane compound according to any one of the above

[48] to

[50] . Effect of the Invention

[0021] According to the method for producing a polycarbonate copolymer of the present invention, a polycarbonate copolymer having a siloxane structural unit and having high fluidity when melted can be produced. Furthermore, according to the present invention, it is also possible to realize a polycarbonate copolymer having such excellent characteristics, a composition containing the polycarbonate copolymer, and a molded article obtained by molding the polycarbonate copolymer.

[0022] In addition, the method for producing a polycarbonate copolymer and the method for producing a polyarylene compound of the present invention can efficiently produce a target compound such as polyarylenesiloxane without producing by-products such as acids that have a high environmental load and without requiring a solvent. The present invention can also realize a polyarylene compound such as polyarylenesiloxane with excellent properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] [I. Polycarbonate copolymer] The method for producing the polycarbonate copolymer in the present invention includes a polymerization step of polymerizing at least one silane-based compound selected from a specified diaryloxysilane compound, a specified dialkoxysilane compound, and a specified silicon compound (siloxane compound) in the presence of a transesterification catalyst, a carbonate compound, and an aromatic diol compound, all of which will be described in detail below.

[0024] The above-mentioned polymerization reaction is outlined below. For example, when a diaryloxysilane compound (Si(CH3)2(OPh)2) having two methyl groups and a phenoxy group, which is an example of a silane compound, is reacted with diphenyl carbonate (PhO-CO-OPh), which is an example of a carbonate compound, and bisphenol A, which is an example of an aromatic diol compound, the following polycarbonate copolymer is obtained. That is, for example, it is a polycarbonate copolymer having a siloxane constituent unit formed by the reaction of the following formula (A) and a polycarbonate constituent unit formed by the reaction of the following formula (B). In this polymerization reaction, as described below, an alcohol derived from the carbonate compound is generated as a by-product, for example, an aryl alcohol such as phenol (PhOH) is generated when diaryl carbonate is used as the carbonate compound. Therefore, in the polymerization step, the mixture of the above-mentioned components is melted and the polymerization reaction is allowed to proceed under reduced pressure while removing the by-product alcohol, for example, an aryl alcohol such as phenol. [ka] [ka] The method for producing the polycarbonate copolymer according to the present invention will be described in detail below.

[0025] <1. Manufacturing method of polycarbonate copolymer> [(I) Silane-based compounds] The silane-based compound used in the polymerization step is used to form a siloxane structural unit in a polycarbonate copolymer, for example, as shown in the above formula (A). The types of silane-based compounds are described in detail below. 1 R 2There is no particular limitation as long as it is possible to form a siloxane structural unit containing an O-moiety in the main chain of a polycarbonate copolymer, and the compound is selected from a predetermined diaryloxysilane compound, a predetermined dialkoxysilane compound, and a predetermined silicon compound (siloxane compound).

[0026] That is, in the polymerization step, a silane-based compound is used that includes at least one of diaryloxysilane compounds, at least one of dialkoxysilane compounds, and at least one of silicon compounds, which will be described in detail later.As the silane-based compound, a plurality of diaryloxysilane compounds may be used in combination, a plurality of dialkoxysilane compounds may be used in combination, a plurality of silicon compounds may be used in combination, or a mixture of a diaryloxysilane compound and a silicon compound, a mixture of a dialkoxysilane compound and a silicon compound, or a mixture of a diaryloxysilane compound and a dialkoxysilane compound may be used.The diaryloxysilane compound will be described below.

[0027] (A-1) Diaryloxysilane compound Examples of diaryloxysilane compounds include dialkyldiaryloxysilane, diaryldiaryloxysilane, and monoalkylmonoaryldiaryloxysilane. In other words, any one or a combination of these may be used as the silane-based compound in the polymerization step.

[0028] The diaryloxysilane compound is represented by the general formula Si(R a R b )(OAr)2, R a and R b are each independently selected from an alkyl group and an aryl group. a and R b are preferably each independently an alkyl group having a total of 1 to 20 carbon atoms, which may have a substituent, or an aryl group having a total of 6 to 30 carbon atoms, which may have a substituent. a and R bWhen the alkyl group is an alkyl group which may have a substituent, the total number of carbon atoms is preferably 1 to 10, more preferably 1 to 6, and particularly preferably 1 or 2. Also, R a and R b When the aryl group is an aryl group which may have a substituent, the total number of carbon atoms is preferably 6 to 20, more preferably 6 to 12, and particularly preferably 6 to 8.

[0029] Examples of the substituent include a hydroxyl group, a halogen, an amino group, a vinyl group, a carboxyl group, a cyano group, a (meth)acryloxy group, a glycidyloxy group, and a mercapto group. R in formula (1) a and R b Preferred specific examples of the alkyl group include a methyl group, a phenyl group, a vinyl group, and a propyl group.

[0030] As is clear from the above formula (A), the aryloxy group (OAr group) of the silane compound is not introduced into the polymer chain of the polycarbonate copolymer, but generates by-products such as phenol (ArOH). Therefore, the type of aryloxy group is not particularly limited. However, in order to remove by-products in the polymerization process from the reaction system as easily as possible, the aryloxy group is preferably one with low polarity and molecular weight, such as a phenoxy group.

[0031] Specific examples of dialkyldiaryloxysilanes include dimethyldiphenoxysilane, methylethyldiphenoxysilane, diethyldiphenoxysilane, etc., and specific examples of diaryldiaryloxysilanes include diphenyldiphenoxysilane, etc. Specific examples of monoalkylmonoaryldiaryloxysilanes include methylphenylphenoxysilane, etc.

[0032] (A-2) Dialkoxysilane compound Examples of dialkoxysilane compounds include dialkyldialkoxysilanes, diaryldialkoxysilanes, and monoalkylmonoaryldialkoxysilanes, and any one or more of these may be used as the silane-based compound in the polymerization step.

[0033] The dialkoxysilane compound is represented by the general formula Si(R a R b )(OR C )2, R a and R b are each independently R a and R b is selected from alkyl and aryl groups, the same as As is clear from the above formula (A), the alkoxy group (OR C The alkoxy group (OR ) is not introduced into the polymer chain of the polycarbonate copolymer, and generates by-products such as methanol (MeOH). Therefore, the type of alkoxy group is not particularly limited. However, in order to remove by-products in the polymerization process from the reaction system as easily as possible, it is preferable to use an alkoxy group (OR ). C The group) is, for example, a methoxy group.

[0034] Specific examples of dialkyldialkoxysilanes include dimethyldimethoxysilane, methylethyldimethoxysilane, diethyldimethoxysilane, etc., specific examples of diaryldialkoxysilanes include diphenyldimethoxysilane, etc., and specific examples of monoalkylmonoaryldialkoxysilanes include methylphenyldimethoxysilane, etc.

[0035] (B) Silicon compounds (siloxane compounds) The silicon compound will be described below. Examples of the silicon compound include a specific cyclic siloxane compound and a linear siloxane compound. That is, in the polymerization step, any of these may be used as the silane-based compound.

[0036] (B-1) Cyclic siloxane compound The siloxane compound used in the polymerization step includes a cyclic siloxane compound represented by the following formula (5). [ka] In formula (5), R c and R d R in formula (5) each independently represents an alkyl group, an alkenyl group, or an aryl group, which may have a substituent. c and R d is preferably an alkyl group having a total of 1 to 20 carbon atoms, or an aryl group having a total of 6 to 30 carbon atoms, each of which may have a substituent. R c and R d When the alkyl group is an alkyl group which may have a substituent, the total number of carbon atoms is preferably 1 to 10, more preferably 1 to 6, and particularly preferably 1 or 2. Also, R c and R d When the aryl group is an aryl group which may have a substituent, the total number of carbon atoms is preferably 6 to 20, more preferably 6 to 12, and particularly preferably 6 to 8.

[0037] Examples of the substituent include a hydroxyl group, a halogen, an amino group, a vinyl group, a carboxyl group, a cyano group, a (meth)acryloxy group, a glycidyloxy group, and a mercapto group. R in Equation (5) c and R d Preferred specific examples of the alkyl group include a methyl group, a phenyl group, a vinyl group, and a propyl group.

[0038] The cyclic siloxane compound has a siloxane structure, and the siloxane structure is represented by the above-mentioned R c Groups and R d -OSi(R c R dIn the polymerization process, the -OSi(R c R d )O-moieties are introduced into the polycarbonate copolymers described in detail below.

[0039] In formula (5), n represents an integer of 3 or more and 30 or less. The value of n in formula (5) is preferably 3 or more and 15 or less, more preferably 3 or more and 10 or less, even more preferably 3 or more and 8 or less, and particularly preferably 3 or more and 5 or less.

[0040] The molecular weight of the cyclic siloxane compound represented by formula (5) is preferably 2,000 or less, more preferably 1,600 or less, even more preferably 1,200 or less, and particularly preferably 1,000 or less. The molecular weight of the cyclic siloxane compound represented by formula (5) is, for example, 100 or more, preferably 150 or more, and more preferably 200 or more.

[0041] (B-2) Linear siloxane compound The siloxane compound used in the polymerization step also includes a linear siloxane compound represented by the following formula (6). [ka] In formula (6), R e and R f R in formula (6) each independently represents an alkyl group or an aryl group which may have a substituent. e and R f is preferably an alkyl group having a total of 1 to 20 carbon atoms, or an aryl group having a total of 6 to 30 carbon atoms, each of which may have a substituent. R e and R f When the alkyl group is an alkyl group which may have a substituent, the total number of carbon atoms is preferably 1 to 10, more preferably 1 to 8, and particularly preferably 1 or 2. Also, R eand R f When the aryl group is an aryl group which may have a substituent, the total number of carbon atoms is preferably 6 to 20, more preferably 6 to 12, and particularly preferably 6 to 8.

[0042] Examples of the substituent include a hydroxyl group, a halogen, an amino group, a vinyl group, a carboxyl group, a cyano group, a (meth)acryloxy group, a glycidyloxy group, and a mercapto group. R in Equation (6) e and R f Preferred specific examples of the alkyl group include a methyl group, a phenyl group, a vinyl group, and a propyl group.

[0043] The linear siloxane compound also has a siloxane structure, and the siloxane structure is represented by the above-mentioned R e Groups and R f -OSi(R e R f In the polymerization process, the linear siloxane compound has a -OSi(R e R f )O-moieties are introduced into the polycarbonate copolymers described in detail below.

[0044] In formula (6), m represents an integer of 2 or more and 10,000 or less. The value of m in formula (6) is preferably 10 or more and 7,000 or less, more preferably 100 or more and 2,000 or less, and even more preferably 200 or more and 500 or less.

[0045] In formula (6), X's each independently represent a hydrogen atom, a hydroxyl group, an alkoxy group having a total of 1 to 10 carbon atoms which may have a substituent, a hydrocarbon group having a total of 1 to 10 carbon atoms which may have a substituent and may have an oxygen atom or a nitrogen atom, or an amino group which may have a substituent. Preferably, X's each independently represent a hydrogen atom, a hydroxyl group, an alkoxy group having a total of 1 to 10 carbon atoms which may have a substituent, or an alkyl group having a total of 1 to 10 carbon atoms which may have a substituent and may have an oxygen atom or a nitrogen atom, more preferably a hydroxyl group or an alkyl group having a total of 1 to 10 carbon atoms which may have a substituent, and even more preferably a hydroxyl group or an alkyl group having a total of 1 to 5 carbon atoms. Examples of the substituent for X include a hydroxyl group, a halogen, an amino group, a vinyl group, a carboxyl group, a cyano group, a (meth)acryloxy group, a glycidyloxy group, and a mercapto group.

[0046] The molecular weight of the linear siloxane compound represented by formula (6) is preferably 60,000 or less, more preferably 56,000 or less, even more preferably 50,000 or less, and particularly preferably 45,000 or less. The molecular weight of the linear siloxane compound represented by formula (6) is, for example, 1,000 or more, preferably 5,000 or more, and more preferably 10,000 or more.

[0047] Among the cyclic siloxane compound of the above formula (5) and the linear siloxane compound of the following formula (6), a single siloxane compound may be used alone, or two or more kinds of siloxane compounds may be used as a mixture. In addition, the siloxane compound of formula (5) or formula (6) may be used in combination with the above diaryloxysilane compound (A). The above-mentioned silane-based compounds can be synthesized by known methods, and commercially available compounds may also be used.

[0048] [(II) Carbonate compound] As shown in the above formula (B) regarding the outline of the polymerization reaction, the carbonate compound is used to introduce the carbonyl group (-CO- group) of the polycarbonate structural unit into the polycarbonate copolymer. That is, the two -OR groups of the carbonate compound represented by the general formula RO-CO-OR (wherein R is independently selected from an aryl group, an alkyl group, and an aralkyl group), for example, the two aryloxy groups (ArO- groups) when the carbonate compound is a diaryl carbonate represented by the general formula ArO-CO-OAr, are not introduced into the polymer chain of the polycarbonate copolymer. These -OR groups generate alcohol derived from the carbonate compound as a by-product, and for example, a carbonate compound (monoaryl carbonate or diaryl carbonate) having an aryloxy group (ArO- group) generates aryl alcohol (ArOH) as a by-product such as phenol.

[0049] Therefore, the types of aryl group, alkyl group, and aralkyl group of the carbonate compound are not particularly limited. However, in order to remove by-products in the polymerization process from the reaction system as easily as possible, it is preferable that the -OR group in the above general formula is an aryloxy group (or the -R group in the above general formula RO-CO-OR is an aryl group) in the carbonate compound, and further, it is preferable that the polarity and molecular weight of the carbonate compound are low, and the -OR group in the above general formula is, for example, a phenoxy group. From the above, in the carbonate compound, it is preferable that either or both of the above-mentioned Ar groups are aryl groups having a total of 10 or less carbon atoms, for example, a phenyl group, a benzyl group, etc. That is, preferred specific examples of the carbonate compound include diaryl carbonates such as diphenyl carbonate, dibenzyl carbonate, ditolyl carbonate, bis(chlorophenyl)carbonate, and m-cresyl carbonate, but the carbonate compound may also be a dialkyl carbonate such as dimethyl carbonate, diethyl carbonate, dibutyl carbonate, and dicyclohexyl carbonate, or a monoaryl monoalkyl carbonate. The above carbonate compounds can be synthesized by known methods, and commercially available compounds may also be used.

[0050] [(III-1) Aromatic diol compounds] The aromatic diol compound used in the polymerization step is used to constitute the main chain of the polycarbonate copolymer, as shown in the above formulas (A) and (B) regarding the outline of the polymerization reaction. Therefore, the aromatic diol compound used in the polymerization step is preferably a monomer that can be a material for a polycarbonate resin, such as bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 1,2-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, bis(4-hydroxyphenyl)phenylmethane, 1,1-bis(4-hydroxyphenyl)-1-phenylene, etc. ethane, bis(4-hydroxyphenyl)diphenylmethane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxy-3-tert-butylphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-phenylphenyl)propane, 2,2-bis(3-cyclohexyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-bromophenyl)propane, 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane, 4,4'-Dihydroxydiphenyl ether, 4,4'-Dihydroxy-3,3'-dimethylphenyl ether, 4,4'-Dihydroxyphenyl sulfide, 4,4'-Dihydroxy-3,3'-dimethyldiphenyl sulfide, 4,4'-Dihydroxydiphenyl sulfoxide, 4,4'-Dihydroxy-3,3'-dimethyldiphenyl ether, 4,4'-Dihydroxydiphenyl sulfoxide, 4,4'-Dihydroxy-3,3'-dimethyldiphenyl ether, 4,4'-Dihydroxydiphenyl sulfide ...diphenyl sulfide, 4,4'-Dihydroxy-3,3'-dimethyldiphenyl ether, 4,4'-Dihydroxydiphenyl sulfide, 4,4'-Dihydroxydiphenyl sulfide, 4,4'-Dihydroxydiphenyl sulfide, 4,4'-Dihydroxydiphenyl sulfide, 4,4'-Dihydroxydiphenyl sulfide, 4,4'-Di Phenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfone, 2,2-bis(3-t-butyl-4-hydroxyphenyl)propane, 2,2-bis(3-bromo-4-hydroxyphenyl)propane, 1,1-bis(3-cyclohexyl-4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 4,4'-dihydroxybiphenyl, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-Bis(4-hydroxy-3-methylphenyl)fluorene, 4,4'-sulfonyldiphenol, 2,2'-diphenyl-4,4'-sulfonyldiphenol, 2,2'-dimethyl-4,4'-sulfonyldiphenol, 1,3-bis{2-(4-hydroxyphenyl)propyl}benzene, 1,4-bis{2-(4-hydroxyphenyl)propyl}benzene, 1,4-bis(4-hydroxyphenyl)cyclohexane, 1,3-bis(4-hydroxyphenyl)cyclohexane, 4,8-bis(4-hydroxyphenyl)tricyclo[5. 2.1.02,6]decane, 4,4'-(1,3-adamantanediyl)diphenol, 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane, 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene (BPEF), 9,9-bis(4-(2-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-hydroxy-3-tert-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-isopropylphenyl)fluorene, 9,9 -Bis(4-hydroxy-3-cyclohexylphenyl)fluorene, 9,9-bis(4-hydroxy-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3- Examples of such fluorene include 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthalene (BNE), 9,9-bis(6-(2-hydroxyethoxy)naphthalene-2-yl)fluorene (BNEF), 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthalene, and 2,2'-bis(2-hydroxyethoxy)-6,6'-di(phenanthren-9-yl)-1,1'-binaphthalene. Among these, 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene (BPEF), 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene (BPPEF), and 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene (BPMEF) are preferred, and 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene (BPEF) and 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene (BPPEF) are more preferred.

[0051] [(III-2) Alicyclic diol compounds] Examples of the alicyclic diol compound used in the polymerization step include the following. That is, isosorbide represented by the following formula (a compound in which, in the above formula (1-3), L1 and L2 are 1, A1 and A2 are oxygen atoms, and J1, K1, J2, and K2 are 0); [ka] Spiroglycol (SPG) represented by the following formula: [ka] Decahydro-1,4:5,8-dimethanonaphthalenediol (D-NDM, where R is hydrogen) represented by the following formula, etc.; [ka] (R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Preferably, R is hydrogen.) Cyclohexanedimethanol represented by the following formula: [ka] Pentacyclopentadecanedimethanol (PCPMD) represented by the following formula: [ka] Tricyclodecane dimethanol (TCDDM) represented by the following formula: [ka] Adamantane dimethanol, such as 1,3-adamantanedimethanol, represented by the formula: [ka] etc. The main chain of the polycarbonate copolymer preferably contains structural units derived from these alicyclic diols.

[0052] The above-mentioned polycarbonate copolymer has high fluidity and is suitable for forming molded articles, and is suitably used, for example, in the molding of thin sheets, films, and the like.

[0053] [(IV) Transesterification catalyst] The transesterification catalyst used in the polymerization step is preferably a catalyst containing a basic compound. Examples of the basic compound catalyst include those containing an alkali metal compound, an alkaline earth metal compound, etc., and examples of such compounds include organic acid salts of alkali metals and alkaline earth metal compounds, inorganic salts such as carbonates, oxides, hydroxides, hydrides, or alkoxides. Alternatively, quaternary ammonium hydroxides and their salts, amines, etc. are used as the basic compound catalyst. These compounds can be used alone or in combination of multiple types. Of the above-mentioned basic compound catalysts, the transesterification catalyst more preferably contains an alkali metal carbonate or an alkali metal hydroxide.Specific examples of more preferred transesterification catalysts include those containing cesium carbonate, potassium carbonate, sodium carbonate, sodium hydrogen carbonate, cesium hydroxide, potassium hydroxide, sodium hydroxide, etc. The above-mentioned transesterification catalyst can be prepared by a known method, and commercially available products may also be used.

[0054] [(V) Polymerization process] In the polymerization step, at least the above-mentioned (I) silane compound, (II) carbonate compound, and (III) aromatic diol compound are polymerized in the presence of (IV) transesterification catalyst. In this polymerization reaction, the mixture of the above-mentioned components is melted, and in the molten state, alcohol derived from the carbonate compound as a by-product, such as aryl alcohol, is removed under reduced pressure. By setting the reaction conditions in this way, the polymerization reaction can be efficiently carried out.

[0055] In the polymerization step, it is preferable to allow the polymerization reaction to proceed under a pressure of 400 Pa or less. That is, the pressure in the polymerization reaction is preferably within a range of 400 Pa or less. In the polymerization step, it is preferable to maintain a normal pressure state without reducing the pressure or a state where the pressure is not reduced significantly for a certain period of time, and then reduce the pressure inside the system to further advance the polymerization reaction. For example, in the polymerization step, it is preferable to gradually reduce the reaction pressure from the initial atmospheric pressure to 400 Pa or less, such as 27,000 Pa, 24,000 Pa, 20,000 Pa, 16,000 Pa, 8,000 Pa, 4,000 Pa, 2,000 Pa, 400 Pa, and 400 Pa or less. In this way, the depressurization step in which the reaction system is depressurized stepwise and the degree of depressurization is increased halfway through is preferable because it is possible to efficiently remove the by-product alcohol while suppressing the distillation of the raw material.

[0056] The time for the polymerization step is appropriately determined taking into consideration the type of the target polycarbonate copolymer, pressure, temperature, and other conditions, but for example, the total time for the polymerization step is within 5 to 10 hours. More specifically, the reaction time before decompression in the reaction system is 0.5 to 3 hours, preferably 1 to 2 hours, and the reaction time after decompression is 1 to 5 hours, preferably 2 to 4 hours.

[0057] In the polymerization step, the temperature in the above-mentioned polymerization reaction is preferably within the range of 150 to 300° C. More preferably, the temperature in the polymerization reaction is 180 to 290° C., and further preferably, 200 to 280° C.

[0058] In addition, the silane compound, diaryl carbonate, and aromatic diol compound are mutually compatible with each other, and the polycarbonate copolymer can be produced without using a solvent in the polymerization process, which simplifies the polymerization process.

[0059] In the polymerization step, the ratio of the molar amount of the transesterification catalyst to the molar amount of the aromatic diol compound (molar ratio: i.e., the value of the molar amount of the transesterification catalyst / the molar amount of the aromatic diol compound) is 1.0×10 -7 ~1.0×10 -2 (mol / mol: 0.1 to 10,000 μmol / mol, or 1.0×10 -4 The molar ratio is preferably 1.0×10 to 10 mmol / mol. -7 ~2.0×10 -5 mol / mol (or 0.5 to 20 μmol / mol).

[0060] In the polymerization step, the molar ratio of the aromatic diol compound to the silane compound (i.e., the value of the number of moles of the silane compound / the number of moles of the aromatic diol compound) is, for example, 0.8 to 1.3, preferably 0.9 or more and 1.25 or less, and more preferably 0.95 or more and 1.2 or less. In addition, in the polymerization step, the molar ratio of the aromatic diol compound to the total number of moles of the diaryl carbonate and the silane compound (i.e., the value of (total number of moles of the diaryl carbonate and the silane compound) / number of moles of the aromatic diol compound) is preferably 0.9 or more and 1.2 or less, and more preferably 0.95 or more and 1.15 or less.

[0061] Next, the polycarbonate copolymer according to the present invention will be described in detail. <2. Polycarbonate copolymer> [(I) Constitutional Unit] The polycarbonate copolymer produced by the process of the present invention is a polymer having siloxane structural units as described above, and specific examples thereof include the following. That is, the polycarbonate copolymer is a polymer having at least a siloxane constituent unit represented by any one of the following formulas (1-1) to (1-4) and a polycarbonate constituent unit, the details of which will be described later. [ka] R in formulas (1-1) to (1-4) 1 and R 2 The siloxane structure containing the above is introduced from the diaryloxysilane compound, dialkyldialkoxysilane, or silicon compound (siloxane compound).

[0062] In formulas (1-1) to (1-4), R 1 and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent. R 1 and R 2 When it is an alkyl group which may have a substituent, it preferably has a total of 1 to 10 carbon atoms, more preferably has a total of 1 to 4 carbon atoms, and particularly preferably has a total of 1 or 2 carbon atoms. Also, R 1 and R 2 When the aryl group is an aryl group which may have a substituent, the total number of carbon atoms is preferably 6 to 20, more preferably 6 to 12, and particularly preferably 6 to 8.

[0063] In formulas (1-1) and (1-2), R 3 ~R 10 and R 30 ~R 33 each independently represents hydrogen, halogen, alkoxy, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent. R 3 ~R 10 and R 30 ~R 33When it is an alkyl group which may have a substituent, it preferably has a total of 1 to 10 carbon atoms, more preferably has a total of 1 to 4 carbon atoms, and particularly preferably has a total of 1 or 2 carbon atoms. R 3 ~R 10 and R 30 ~R 33 When the alkyl group is an alkenyl group which may have a substituent, the total number of carbon atoms is preferably 2 to 10, more preferably 2 to 6, and particularly preferably 2 to 4. Also, R 3 ~R 10 and R 30 ~R 33 When the aryl group is an aryl group which may have a substituent, the total number of carbon atoms is preferably 6 to 20, more preferably 6 to 12, and particularly preferably 6 to 8.

[0064] In formulas (1-1) to (1-3), Z1 and Z2 are each independently an alkylene group having 1 to 5 carbon atoms, which may have a substituent, preferably an alkylene group having 1 to 3 carbon atoms, and more preferably an alkylene group having 1 or 2 carbon atoms. In formulas (1-1) to (1-3), J1 and K1 each independently represent an integer of 0 to 5, preferably an integer of 0 to 3, more preferably an integer of 0 to 2, for example, 1 or 2. In formula (1-3), A1 and A2 each independently represent -O- or -CH-. L1 and L2 each independently represent an integer of 0 or more and 3 or less, and L1 and L2 are preferably 1 or 2. In formulas (1-1) and (1-2), X is each independently a single bond or any one of the structural formulas represented by the following formula (2). [ka] In formula (2), R 11 , and R 12each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5,000 or less. R 11 , and R 12 are preferably each independently hydrogen, an alkyl group having 1 to 10 carbon atoms which may have a substituent, or an aryl group having 6 to 16 carbon atoms which may have a substituent. In formula (2), a and b are each independently 0 or an integer of 1 or more and 5000 or less, and a and b are preferably integers of 1000 or less, more preferably integers of 500 or less, and even more preferably integers of 100 or less. In the siloxane structural unit, X is R 11 and R 12 are preferably bonded to each other to form a fluorene ring structure.

[0065] The siloxane constitutional unit preferably contains at least one represented by the following formula (1). [ka]

[0066] R in formula (1) 1 and R 2 The siloxane structure containing the above is introduced from the diaryloxysilane compound, dialkoxysilane compound, or silicon compound (siloxane compound). In formula (1), R 1 and R 2 R in formula (1) each independently represents an alkyl group, an alkenyl group, or an aryl group, which may have a substituent. 1 and R 2represents an alkyl group having a total of 1 to 20 carbon atoms, or an aryl group having a total of 6 to 30 carbon atoms, each of which may have a substituent. R 1 and R 2 Preferred options for R in the above formulas (1-1) to (1-4) are 1 and R 2 is the same as:

[0067] The above mentioned R 1 and R 2 Examples of the substituent include a hydroxyl group, a halogen, an amino group, a vinyl group, a carboxyl group, a cyano group, a (meth)acryloxy group, a glycidyloxy group, and a mercapto group. R in formula (1) 1 and R 2 Preferred specific examples of the alkyl group include a methyl group, a phenyl group, a vinyl group, and a propyl group.

[0068] In formula (1), R 3 ~R 10 Preferred options for R in the above formulas (1-1) to (1-4) are 3 ~R 10 is the same as: The above mentioned R 3 ~R 10 Examples of the substituent include a hydroxyl group, a halogen, an amino group, a vinyl group, a carboxyl group, a cyano group, a (meth)acryloxy group, a glycidyloxy group, and a mercapto group.

[0069] In formula (1), X is the same as X in the above formulae (1-1 and (1-2).

[0070] The polycarbonate constituent unit of the polycarbonate copolymer is represented by any one of the following formulas (3-1) to (3-4). [ka]

[0071] (3-1)~(3-2) Medium, R 13 ~R 20 and R40 ~R 51 each independently represents hydrogen, halogen, alkoxy, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent. R 13 ~R 20 and R 40 ~R 51 When it is an alkyl group which may have a substituent, it preferably has a total of 1 to 10 carbon atoms, more preferably has a total of 1 to 4 carbon atoms, and particularly preferably has a total of 1 or 2 carbon atoms. R 13 ~R 20 and R 40 ~R 51 When the alkyl group is an alkenyl group which may have a substituent, the total number of carbon atoms is preferably 2 to 10, more preferably 2 to 6, and particularly preferably 2 to 4. Also, R 13 ~R 20 and R 40 ~R 51 When the aryl group is an aryl group which may have a substituent, the total number of carbon atoms is preferably 6 to 20, more preferably 6 to 12, and particularly preferably 6 to 8.

[0072] In formulas (3-1) to (3-3), Z3 and Z4 are each independently an alkylene group having 1 to 5 carbon atoms, which may have a substituent, preferably an alkylene group having 1 to 3 carbon atoms, and more preferably an alkylene group having 1 or 2 carbon atoms. In formulas (3-1) to (3-3), J2 and K2 each independently represent an integer of 0 or more and 5 or less, preferably an integer of 0 or more and 3 or less, and more preferably 1 or 2. In formula (3-3), A1 and A2 each independently represent -O- or -CH-. L1 and L2 each independently represent an integer of 0 or more and 3 or less, and L1 and L2 are preferably 0 or more and 2 or less. In the formulas (3-1) and (3-2), each Y is independently a single bond or a structural formula represented by the formula (4). [ka] (In the formula, R 21 , and R 22 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 21 and R 22 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, and c and d each independently represent 0 or an integer of 1 or more and 5,000 or less. R 21 , and R 22 are preferably each independently hydrogen, an alkyl group having 1 to 10 carbon atoms which may have a substituent, or an aryl group having 6 to 16 carbon atoms which may have a substituent. In formula (4), c and d are each independently 0 or an integer of 1 or more and 5000 or less, and c and d are preferably integers of 1000 or less, more preferably integers of 500 or less, and even more preferably integers of 100 or less. In the polycarbonate structural unit, Y is R 11 and R 12 are preferably bonded to each other to form a fluorene ring structure.

[0073] The polycarbonate structural unit preferably contains at least one represented by the following formula (3). [ka]

[0074] In formula (3), R 13 ~R 20 Preferred options for R in the above formulas (3-1) to (3-2) are 3 ~R 10 is the same as: The above mentioned R 13~R 20 Examples of the substituent include a hydroxyl group, a halogen, an amino group, a vinyl group, a carboxyl group, a cyano group, a (meth)acryloxy group, a glycidyloxy group, and a mercapto group.

[0075] In the formula (3), Y is the same as Y in the above formulas (3-1) and (3-2).

[0076] [(II) Properties of polycarbonate copolymer] The weight average molecular weight of the polycarbonate copolymer is preferably 10,000 to 300,000, more preferably 10,000 to 200,000, and even more preferably 10,000 to 100,000. For example, it is more preferably 20,000 to 80,000, still more preferably 30,000 to 70,000, and particularly preferably 40,000 to 65,000.

[0077] In the polycarbonate copolymer, the number of moles of the siloxane constituent units is preferably 1 to 1000. Also, the number of moles of the polycarbonate constituent units is preferably 1 to 1000. These numbers of moles are all the number of constituent units contained in one molecule of the polycarbonate copolymer, and are more preferably 10 to 800, and further preferably 100 to 600, respectively.

[0078] In the polycarbonate copolymer, the proportion of the siloxane structural unit in the total number of moles of the siloxane structural unit and the polycarbonate structural unit is preferably 2.0% or more and 90% or less. The proportion of the above-mentioned siloxane structural unit is more preferably 3.0% or more, for example, more preferably higher than 3.1% and 90% or less, further preferably 5% or more and 90% or less, and particularly preferably 8% or more and 90% or less. In addition, when the polycarbonate copolymer is not used alone but is used as a composition mixed with other resins, it may be better to significantly increase the proportion of the above-mentioned siloxane structural unit.For example, the polycarbonate copolymer with a high Si content and a proportion of the above-mentioned siloxane structural unit of 30% or more, 50% or more, or 70% or more can be mixed with a polymer that does not contain Si or siloxane structural units, as described in detail below, to realize a resin with excellent performance, for example, high impact resistance and fluidity.In addition, when an application in which the proportion of the siloxane structural unit is increased is preferred, the upper limit of the proportion of the above-mentioned siloxane structural unit is not limited to 90%, and may be, for example, 92%, 95%, 98%, etc.

[0079] In the polycarbonate copolymer, the molar ratio of the siloxane structural unit to the polycarbonate structural unit (i.e., the ratio of the number of moles of the siloxane structural unit to the number of moles of the polycarbonate structural unit) is preferably 0.01:99.99 to 99.99:0.01. The above-mentioned molar ratio is more preferably 30:70 to 99.9:0.01, but may be in other ranges, such as 1:99 to 99:1, 10:90 to 90:10, etc.

[0080] For polycarbonate copolymers, the Q value (melt flow volume per unit time measured at 280°C and a load of 160 kg, × 10 -2 cm 3 s -1 ), but 8(×10 -2 cm 3 s -1 ) or more. The Q value is more preferably 20(×10 -2 cm 3 s -1 ) or more, and more preferably 40(×10 -2 cm 3 s -1 ) or more, and particularly preferably 60(×10 -2 cm 3 s -1 )That's all.

[0081] The polycarbonate copolymer has a glass transition temperature (Tg) according to JIS K 7121 of, for example, 40 to 200°C, preferably 45 to 180°C, and more preferably 50 to 160°C.

[0082] In the above-mentioned polycarbonate copolymer, that is, the polycarbonate copolymer having a siloxane constitutional unit represented by any one of formulas (1-1) to (1-4) and a polycarbonate constitutional unit represented by any one of formulas (3-1) to (3-4), the low molecular weight compound having a weight average molecular weight of 1,000 or less is preferably 30% by weight or less, more preferably 20% by weight or less, more preferably 10% by weight or less, more preferably 5.0% by weight or less, particularly preferably 1.5% by weight or less, and even more preferably less than 1.0% by weight. A polycarbonate copolymer containing a large amount of low molecular weight compounds having a weight average molecular weight of 1,000 or less tends to contaminate the mold (mold) with a small amount of deposit (mold deposit) at a relatively early stage when injection molding or the like is continuously performed to manufacture a disk or a complicated and thin-walled product. In this regard, if the amount of low molecular weight compounds having a weight average molecular weight of 1,000 or less in the polycarbonate copolymer is less than 1.5 mass %, contamination of the mold is effectively prevented. The lower limit of the content of the low molecular weight compound having a weight average molecular weight of 1,000 or less in the polycarbonate copolymer is about 0.7% by weight, although it is not particularly important. However, even if the low molecular weight compound is contained in an amount of 0.001% by weight, 0.01% by weight, or 0.1% by weight or more, there is no problem in the properties of the polycarbonate copolymer, particularly when used for optical purposes, and the effect of improving the fluidity has also been confirmed. Therefore, the lower limit of the content of the low molecular weight compound having a weight average molecular weight of 1,000 or less in the polycarbonate copolymer may be 0.001% by weight, 0.01% by weight, or 0.1% by weight.

[0083] The content of the above-mentioned low molecular weight compounds in the polycarbonate copolymer is a value calculated by summing the contents of several kinds of low molecular weight compounds as impurities from the peak area ratio of each component obtained by GPC analysis, as described in detail later in the Examples. That is, as described in detail later, the proportion of low molecular weight compounds having a molecular weight of 1,000 or less in the polycarbonate copolymer is a value calculated from the ratio of the area from 20.5 min to 21.5 min of retention time / the area from 0 min to 21.5 min under predetermined GPC analysis conditions.

[0084] In the above-mentioned polycarbonate copolymer, i.e., the polycarbonate copolymer having a siloxane constituent unit represented by any one of formulas (1-1) to (1-4) and a polycarbonate constituent unit represented by any one of formulas (3-1) to (3-4), the total content of cyclic units represented by the following formulas (5-1) to (5-3) is preferably 4.0 wt % or less, more preferably 3.0 wt % or less, even more preferably 2.0 wt % or less, and particularly preferably 1.0 wt % or less, based on the total weight of the polycarbonate copolymer. If the content of these cyclic dimers is within the above-mentioned range, it can be said that there is no problem in the properties of the polycarbonate copolymer, particularly when it is used for optical applications. [ka] In formulae (5-1) to (5-3), m and n represent the total number of structural units containing a (-OSi(R1R2)O-) moiety and the total number of structural units containing a (-OC(=O)O-) moiety in each cyclic product. That is, when the cyclic product of formula (5-1) contains structural units other than structural units containing a (-OSi(R1R2)O-) moiety, and when the cyclic product of formula (5-2) contains structural units other than structural units containing a (-OC(=O)O-) moiety, m and n each represent the total number of structural units in the cyclic product shown in the formula. In particular, formula (5-3) includes a mixture of structural units containing a (-OSi(R1R2)O-) moiety and structural units containing a (-OC(=O)O-) moiety, for example, a cyclic product in which these are arranged alternately, and in this case, m and n each represent the total number of structural units in the cyclic product shown in the formula. In formula (5-1), m represents an integer of 2 to 10, preferably 2 to 5, more preferably 2 or 3, and even more preferably 2. In formula (5-2), n represents an integer of 2 to 10, preferably 2 to 5, more preferably 2 or 3, and even more preferably 2. In formula (5-3), the total value of m is 1 to 10, and the total value of n is 1 to 10. Each of m and n is preferably 1 to 5, more preferably 1 or 2, and even more preferably 1. In formula (5-3), as mentioned above, in the cyclic compound of formula (5-3), the constitutional unit containing the (-OSi(R1R2)O-) moiety and the constitutional unit containing the (-OC(=O)O-) moiety may be arranged in any manner. In formulas (5-1) to (5-3), X1 and X2 each independently represent an alkylene group having 1 to 5 carbon atoms, which may have a substituent, preferably an alkylene group having 1 to 3 carbon atoms, and more preferably an alkylene group having 1 or 2 carbon atoms. i and ii each independently represent an integer of 0 or more and 5 or less, preferably an integer of 0 or more and 3 or less, and more preferably 1 or 2. In addition, in formulas (5-1) to (5-3), R 1 , R 2 , R 3~R 10 , R 13 ~R 20 and X is R in formulas (1-1) and (1-2). 1 , R 2 , R 3 ~R 10 , R 13 ~R 20 and X, respectively.

[0085] Specific examples of the compounds of formulae (5-1) to (5-3) include cyclic compounds of the following formulae (5-1') to (5-3'). [ka] In formula (5-1'), m = 2 or 3, preferably m = 2; in formula (5-2'), n = 2 or 3, preferably n = 2; and in formula (5-3'), m = any one of 1 to 3, n = any one of 1 to 3, preferably all 1 or 2, more preferably all 1.

[0086] The polycarbonate copolymer may contain a total content of cyclic compounds represented by the following formulae (6-1) and (6-2). These cyclic compounds are considered to be cyclic dimers resulting from a side reaction of the polymerization reaction for producing the polycarbonate copolymer. The total content of these cyclic dimers in the polycarbonate copolymer is preferably 2.0% by weight or less, more preferably 1.5% by weight or less, even more preferably 1.0% by weight or less, and particularly preferably 0.5% by weight or less, based on the total weight of the polycarbonate copolymer. [ka] In formulas (6-1) and (6-2), R 1 , R 2 , R 3 ~R 10 , R 30 ~R 33 and X are the same as in formulas (1-1) and (1-2). In formulas (6-1) and (6-2), X1 and X2 are each independently an alkylene group having 1 to 5 carbon atoms, which may have a substituent, preferably an alkylene group having 1 to 3 carbon atoms, and more preferably an alkylene group having 1 or 2 carbon atoms. i and ii each independently represent an integer of 0 or more and 5 or less, preferably an integer of 0 or more and 3 or less, and more preferably 1 or 2. n represents an integer of 2 to 10, preferably an integer of 2 to 5, more preferably 2 or 3, for example, 2.

[0087] The lower limit of the total content of the cyclic dimers represented by formulae (6-1) and (6-2) contained in the polycarbonate copolymer is not particularly limited, but may be, for example, 0.001% by weight, 0.01% by weight, or 0.1% by weight. The presence of a small amount of the cyclic dimer can contribute to improving the flowability of the polycarbonate copolymer during molding.

[0088] Specific examples of the compounds of formulae (6-1) and (6-2), respectively, include cyclic compounds of the following formulae (6-1') and (6-2'). [ka] In addition, in formulas (6-1') and (6-2'), R 1 and R 2 , R 3 ~R 10 and R 30 ~R 33 , Z1 and Z2, J1, K1 and X are as defined above.

[0089] In the polycarbonate copolymer, the 1% mass loss thermal decomposition temperature is preferably 415°C or less, more preferably 400°C or less, even more preferably 385°C or less, and particularly preferably 370°C or less.

[0090] In the polycarbonate copolymer, the proportion of the total weight of silicon atoms (total Si content) based on the total weight of the polycarbonate copolymer is preferably 0.1 to 20 mass%, more preferably 1.0 to 15 mass%, even more preferably 2.0 to 12 mass%, and particularly preferably 3.0 to 10 mass% (for example, 3.1 mass% or more, or more than 3.1 mass% and 9.8 mass% or less).

[0091] Next, the composition according to the present invention, that is, the composition containing the above-mentioned polycarbonate copolymer, etc. will be described in detail.

[0092] <3. Composition> The composition of the present invention contains the above-mentioned polycarbonate copolymer and a polycarbonate resin that does not fall under the above-mentioned polycarbonate copolymer. For example, the polycarbonate resin that does not fall under the above-mentioned polycarbonate copolymer is a polycarbonate resin that does not completely or substantially contain a siloxane structure.

[0093] The type of polycarbonate resin that does not fall under the above-mentioned polycarbonate copolymer is not particularly limited as long as it contains a -[OR-OCO]- unit (R contains an aliphatic group, an aromatic group, or both an aliphatic group and an aromatic group, and further has a linear structure or a branched structure) containing a carbonate bond in the molecular main chain. In addition, the polycarbonate resin that does not fall under the above-mentioned polycarbonate copolymer may contain polyester carbonate. Similarly, the polyester carbonate is not particularly limited as long as it contains a -[OR-OC]- unit (R is as described above) containing a carbonate bond in the molecular main chain.

[0094] The weight average molecular weight of the polycarbonate resin is preferably from 10,000 to 100,000, more preferably from 13,000 to 80,000, and further preferably from 15,000 to 60,000.

[0095] The composition of the present invention may contain a resin other than a polycarbonate resin, preferably a thermoplastic resin. The type of thermoplastic resin is not particularly limited, but in addition to polycarbonate resin and polyester carbonate resin, various resins such as acrylic resins such as polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), triacetyl cellulose (TAC), polyethylene naphthalate (PEN), polyimide (PI), cycloolefin copolymer (COC), norbornene-containing resin, polyethersulfone, cellophane, and aromatic polyamide can be mentioned.

[0096] In the composition, the ratio of the total weight of silicon atoms (total Si amount) based on the total weight of the composition is preferably 0.1 to 20 mass%, more preferably 0.2 to 15 mass%, and particularly preferably 0.3 to 10 mass%. The ratio of the total Si amount in the composition can be adjusted by the ratio of the siloxane structural units to all structural units in the above-mentioned polycarbonate resin, or the amount of resin mixed with the polycarbonate resin and the amount of Si. For example, Q1, which is the Q value of a composition containing a polycarbonate copolymer measured under conditions of 280°C and 160 kgf, is preferably 120% or more (20% or more higher) than Q2, which is the Q value of only the polycarbonate resin contained in the composition measured under the same conditions, and the Q1 value of the entire composition is more preferably 130% or more, even more preferably 140% or more, and particularly preferably 150% or more, for example 160% or more, of the Q2 value of only the polycarbonate. Furthermore, for example, in the case of a composition containing 5% by mass of a polycarbonate copolymer, Q1, which is the Q value measured under conditions of 280°C and 160 kgf, is preferably a value that is 140% or more (40% or more higher) than Q2, which is the Q value measured under the same conditions for only the polycarbonate resin contained in the composition, and the Q1 value of the entire composition is more preferably 150% or more, even more preferably 160% or more, and particularly preferably 170% or more, for example 180% or more, of the Q2 value of only the polycarbonate.

[0097] By using a polycarbonate copolymer having a high Si content, a composition having excellent characteristics can be produced. By mixing a polycarbonate copolymer having a Si content of, for example, 0.1 mass% or more with a resin that does not substantially contain a siloxane structural unit, preferably a polycarbonate resin, the resulting composition can have both excellent impact resistance and flowability.

[0098] In addition, in the composition containing the polycarbonate copolymer, phenolic compounds that may be generated as by-products of the polymerization reaction, and silane compounds, carbonate compounds, and diol compounds that remain unreacted may be contained. The phenolic compounds and DPC that are impurities may cause a decrease in strength when molded into a molded body and may cause odor generation, so the content of these is preferably as small as possible. For this reason, the content of the phenolic compounds, silane compounds, carbonate compounds, and diol compounds may be reduced to an undetectable level, but may be contained in the composition within a range that does not impair the effect from the viewpoint of productivity. In addition, by containing a predetermined amount of monomer residue, for example, 1 to 1000 ppm by weight, preferably 10 to 900 ppm, more preferably 20 to 800 ppm, based on the total weight of the composition, the effect of improving the fluidity during molding can be obtained, and the plasticity can be improved when the resin is melted.

[0099] Next, the molded article according to the present invention containing a polycarbonate copolymer will be described. <4. Molded body> The molded article according to the present invention is obtained by molding the above-mentioned polycarbonate copolymer or a composition containing the polycarbonate copolymer, etc. The molding method of the molded article is not particularly limited, and examples of the molded article include injection molded articles, press molded articles, blow molded articles, extrusion molded articles, vacuum molded articles, and pressure molded articles.

[0100] The optical lens according to the present invention is obtained by molding the polycarbonate copolymer of the present invention or a composition containing the polycarbonate copolymer, etc. The polycarbonate copolymer of the present invention is suitable for optical applications, and the optical lens of the present invention has a refractive index, Abbe number, etc. within ranges suitable for a lens.

[0101] [II. Polysiloxane Compounds] The method for producing a polysiloxane compound such as polyarylenesiloxane in the present invention includes a polymerization step of polymerizing an oxysilane compound such as a specific diaryloxysilane compound and a diol compound such as an aromatic diol compound in the presence of an ester exchange catalyst, the details of which will be described later. The method for producing a polysiloxane compound will be described below. In addition, in the method for producing a polysiloxane compound, the raw materials, reaction conditions, and the like described for the above-mentioned polycarbonate copolymer can also be adopted, and in the method for producing the above-mentioned polycarbonate copolymer, the raw materials, reaction conditions, and the like described for the following method for producing a polysiloxane compound can also be adopted.

[0102] The above-mentioned polymerization reaction is outlined below. For example, when a diphenoxysilane compound (Si(CH3)2(OPh)2) having two methyl groups and a phenoxy group, which is an example of a diaryloxysilane compound, is reacted with bisphenol A, which is an example of an aromatic diol compound, the following polyarylenesiloxane compound is obtained. That is, a polyarylenesiloxane compound having a siloxane structure formed by the reaction of the following formula (A) is produced. In this polymerization reaction, aryl alcohols such as phenol (PhOH) are generated as by-products, as described below. Therefore, in the polymerization step, the mixture of the above-mentioned components is melted and the polymerization reaction is allowed to proceed under reduced pressure while removing the by-product aryl alcohols such as phenol. [ka] The method for producing the polysiloxane compound according to the present invention will be described in detail below. The polysiloxane compound includes polyarylenesiloxane compounds, polyalkylenesiloxane compounds, and mixtures thereof, as well as compounds containing both a diaryloxysilane compound-derived structural unit and a dialkoxysilane compound-derived structural unit in the polymer chain, which will be described in detail later.

[0103] <1. Method for producing polysiloxane compound> [(I) Oxysilane compound] Examples of oxysilane compounds used in the production of polysiloxane compounds include diaryloxysilane compounds and dialkoxysilane compounds.

[0104] (A-1) Diaryloxysilane compound The diaryloxysilane compound used in the polymerization step is used to form siloxane building blocks in a polyarylenesiloxane compound, for example as shown in the above formula (A). Examples of diaryloxysilane compounds include dialkyldiaryloxysilane, diaryldiaryloxysilane, and monoalkylmonoaryldiaryloxysilane. In other words, any one or a combination of these may be used as the silane-based compound in the polymerization step.

[0105] The diaryloxysilane compound is represented by the general formula Si(R a R b )(OAr)2, R a and R b are each independently selected from an alkyl group and an aryl group. a and R b are preferably each independently either an alkyl group having a total of 1 to 20 carbon atoms, which may have a substituent, or an aryl group having a total of 6 to 30 carbon atoms, which may have a substituent. a and R bWhen the alkyl group is an alkyl group which may have a substituent, the total number of carbon atoms is preferably 1 to 10, more preferably 1 to 6, and particularly preferably 1 or 2. Also, R a and R b When the aryl group is an aryl group which may have a substituent, the total number of carbon atoms is preferably 6 to 20, more preferably 6 to 12, and particularly preferably 6 to 8.

[0106] Examples of the substituent include a hydroxyl group, a halogen, an amino group, a vinyl group, a carboxyl group, a cyano group, a (meth)acryloxy group, a glycidyloxy group, and a mercapto group. R in formula (1) a and R b Preferred specific examples of the alkyl group include a methyl group, a phenyl group, a vinyl group, and a propyl group.

[0107] As is clear from the above formula (A), the aryloxy group (OAr group) of the diaryloxysilane compound is not introduced into the polymer chain of the polyarylenesiloxane compound, but generates by-products (ArOH) such as phenol. Therefore, the type of aryloxy group is not particularly limited. However, in order to remove by-products in the polymerization process from the reaction system as easily as possible, the aryloxy group is preferably low in polarity and molecular weight, for example, phenoxy group.

[0108] Specific examples of dialkyldiaryloxysilanes include dimethyldiphenoxysilane, methylethyldiphenoxysilane, diethyldiphenoxysilane, etc., and specific examples of diaryldiaryloxysilanes include diphenyldiphenoxysilane, etc. Specific examples of monoalkylmonoaryldiaryloxysilanes include methylphenylphenoxysilane, etc. These diaryloxysilane compounds can be synthesized by known methods, and commercially available compounds may also be used.

[0109] (A-2) Dialkoxysilane compound Examples of dialkoxysilane compounds include dialkyldialkoxysilanes, diaryldialkoxysilanes, and monoalkylmonoaryldialkoxysilanes, and any one or more of these may be used as the silane-based compound in the polymerization step.

[0110] The dialkoxysilane compound is represented by the general formula Si(R a R b )(OR C )2, R a and R b are each independently R a and R b is selected from alkyl and aryl groups, the same as As is clear from the above formula (A), the alkoxy group (OR C The alkoxy group (OR ) is not introduced into the polymer chain of the polycarbonate copolymer, and generates by-products such as methanol (MeOH). Therefore, the type of alkoxy group is not particularly limited. However, in order to remove by-products in the polymerization process from the reaction system as easily as possible, it is preferable to use an alkoxy group (OR ). C The group) is, for example, a methoxy group.

[0111] Specific examples of dialkyldialkoxysilanes include dimethyldimethoxysilane, methylethyldimethoxysilane, diethyldimethoxysilane, etc., specific examples of diaryldialkoxysilanes include diphenyldimethoxysilane, etc., and specific examples of monoalkylmonoaryldialkoxysilanes include methylphenyldimethoxysilane, etc.

[0112] [(II) Diol compound] The diol compound used in the production of the polysiloxane compound includes an aromatic diol compound and an alicyclic diol compound. As the diol compound, a mixture of an aromatic diol compound and an alicyclic diol compound may be used.

[0113] (A-1) Aromatic diol compound The aromatic diol compound used in the polymerization step is used to constitute the main chain of a polysiloxane compound such as a polyarylenesiloxane compound, as shown in the above formula (A) which outlines the polymerization reaction. Therefore, the aromatic diol compound used in the polymerization step is preferably a monomer that can be a material for a polycarbonate resin, such as bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 1,2-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, bis(4-hydroxyphenyl)phenylmethane, 1,1-bis(4-hydroxyphenyl)-1-phenylene, etc. ethane, bis(4-hydroxyphenyl)diphenylmethane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxy-3-tert-butylphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-phenylphenyl)propane, 2,2-bis(3-cyclohexyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-bromophenyl)propane, 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane, 4,4'-Dihydroxydiphenyl ether, 4,4'-Dihydroxy-3,3'-dimethylphenyl ether, 4,4'-Dihydroxyphenyl sulfide, 4,4'-Dihydroxy-3,3'-dimethyldiphenyl sulfide, 4,4'-Dihydroxydiphenyl sulfoxide, 4,4'-Dihydroxy-3,3'-dimethyldiphenyl ether, 4,4'-Dihydroxydiphenyl sulfoxide, 4,4'-Dihydroxy-3,3'-dimethyldiphenyl ether, 4,4'-Dihydroxydiphenyl sulfide ...diphenyl sulfide, 4,4'-Dihydroxy-3,3'-dimethyldiphenyl ether, 4,4'-Dihydroxydiphenyl sulfide, 4,4'-Dihydroxydiphenyl sulfide, 4,4'-Dihydroxydiphenyl sulfide, 4,4'-Dihydroxydiphenyl sulfide, 4,4'-Dihydroxydiphenyl sulfide, 4,4'-Di Phenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfone, 2,2-bis(3-t-butyl-4-hydroxyphenyl)propane, 2,2-bis(3-bromo-4-hydroxyphenyl)propane, 1,1-bis(3-cyclohexyl-4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 4,4'-dihydroxybiphenyl, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 4,4'-sulfonyldiphenol, 2,2'-diphenyl-4,4'-sulfonyldiphenol, 2,2'-dimethyl-4,4'-sulfonyldiphenol, 1,3-bis{2-(4-hydroxyphenyl)propyl}benzene, 1,4-bis{2-(4-hydroxyphenyl)propyl}benzene, 1,4-bis(4-hydroxyphenyl)cyclohexane, 1,3-bis(4-hydroxyphenyl)cyclohexane, 4,8-bis(4-hydroxyphenyl)tricyclo[5.2.1.02,6]decane, 4,4'-(1,3-adamantanediyl)diphenol, and 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane. In addition, the aromatic diol compounds described in the above section [(III-1) Aromatic diol compounds] regarding the polycarbonate copolymer can also be used in the polymerization step for producing the polysiloxane compound.

[0114] (A-2) Alicyclic diol compound The alicyclic diol compound used in the polymerization step is also used to constitute the main chain of the polysiloxane compound. Specific examples of the alicyclic diol compound include spiroglycol, cyclohexanedimethanol, PCPDM, and TCDDM. In addition, the alicyclic diol compounds described in the above section [(III-2) Alicyclic diol compound] regarding the polycarbonate copolymer can also be used in the polymerization step for producing the polysiloxane compound.

[0115] [(III) Transesterification catalyst] The transesterification catalyst used in the polymerization step is preferably a catalyst containing a basic compound. Examples of the basic compound catalyst include those containing an alkali metal compound, an alkaline earth metal compound, etc., and examples of such compounds include organic acid salts of alkali metals and alkaline earth metal compounds, inorganic salts such as carbonates, oxides, hydroxides, hydrides, or alkoxides. Alternatively, quaternary ammonium hydroxides and their salts, amines, etc. are used as the basic compound catalyst. These compounds can be used alone or in combination of multiple types. Of the above-mentioned basic compound catalysts, the transesterification catalyst more preferably contains an alkali metal carbonate or an alkali metal hydroxide.Specific examples of more preferred transesterification catalysts include those containing cesium carbonate, potassium carbonate, sodium carbonate, sodium hydrogen carbonate, cesium hydroxide, potassium hydroxide, sodium hydroxide, etc. The transesterification catalyst can be prepared by a known method, and commercially available products may also be used.

[0116] [(IV) Polymerization step] In the polymerization step, at least the above-mentioned (I) dioxysilane compound such as diaryloxysilane compound, and (II) diol compound such as aromatic diol compound are polymerized in the presence of (III) transesterification catalyst. In this polymerization reaction, the mixture of the above components is melted, and in the molten state, the by-product aryl alcohol and / or alkyl alcohol is removed under reduced pressure. By setting the reaction conditions in this way, the polymerization reaction can be efficiently carried out.

[0117] In the polymerization step, the pressure in the above-mentioned polymerization reaction is preferably in the range of 101,300 Pa or less. More preferably, the pressure in the polymerization reaction is 27,000 Pa or less, and even more preferably, the pressure in the polymerization reaction is 400 Pa or less. In the polymerization step, it is preferable to maintain a normal pressure state without reducing the pressure or a state where the pressure is not reduced significantly for a certain period of time, and then gradually reduce the pressure in the system to further advance the polymerization reaction. In this way, by gradually increasing the degree of reduced pressure in the reaction system from the middle, the work required at the start of the reaction can be started under normal pressure, and the by-product aryl alcohol or alkyl alcohol can be easily removed from the reaction system. Specifically, it is preferable to proceed with the depressurization step at a pace of about 100 to 10,000 Pa / min, more preferably 500 to 7,000 Pa / min, and even more preferably 1,000 to 4,000 Pa / min.

[0118] As is clear from the above description, in the polymerization step, it is not necessary to always carry out the polymerization reaction under reduced pressure, and it is preferable to reduce the pressure in the reaction system after the polymerization reaction has progressed to a certain degree, preferably from a state in which the raw materials are at least in a molten state. For example, as described later, since it is preferable to gradually increase the reaction temperature in the polymerization step, it is preferable to start the depressurization step after the temperature of the reaction system has been raised to a certain degree, for example, to 150°C or higher, more preferably 180°C or higher.

[0119] In the polymerization step, the temperature in the above-mentioned polymerization reaction is preferably within a range of 150 to 300° C. More preferably, the temperature in the polymerization reaction is 180 to 290° C., and further preferably, 200 to 280° C. Thus, in the polymerization step, it is preferable to polymerize the oxysilane compound or diaryloxysilane compound and the diol compound or aromatic diol compound at a reaction temperature higher than 200° C. In addition, it is preferable to carry out the polymerization step under reduced pressure. In order to gradually generate and remove the by-product aryl alcohol or alkyl alcohol, it is preferable to gradually raise the temperature from room temperature to a reaction temperature set within the above-mentioned range. The temperature is preferably raised at a rate of about 1 to 10°C / min, more preferably 2 to 8°C / min, and even more preferably 3 to 7°C / min.

[0120] The time for the polymerization step is appropriately determined taking into consideration the type of the target polysiloxane compound, and reaction conditions such as pressure and temperature, but for example, the total time for the polymerization step is within 1 to 10 hours. More specifically, the reaction time before the above-mentioned reduction in pressure in the reaction system is 0.1 to 3 hours, preferably 0.5 to 2 hours, and the reaction time after the reduction in pressure is 0.5 to 8 hours, preferably 1 to 6 hours.

[0121] In addition, the above-mentioned oxysilane compound and diol compound have good compatibility with each other, and the polycarbonate copolymer can be produced without using a solvent in the polymerization process. In this way, since a solvent such as a halogen-based solvent is not required, it is possible to reduce the environmental load caused by the polymerization reaction and simplify the polymerization process.

[0122] Furthermore, the by-products generated in the polymerization step are the above-mentioned aryl alcohols, alkyl alcohols, etc., which can be easily removed from the reaction system and do not require special treatment in consideration of safety, etc. Therefore, the method for producing a polysiloxane compound according to the present invention can reduce the environmental load compared to conventional production methods in which, for example, an acid is produced as a by-product or an acid is used.

[0123] In the polymerization step, the ratio of the molar amount of the transesterification catalyst to the molar amount of the aromatic diol compound (molar ratio: i.e., the value of the molar amount of the transesterification catalyst / the molar amount of the aromatic diol compound) is 0.01 μmol / mol to 16,000 μmol / mol (1.0 × 10 -8 ~1.6×10 -2 The molar ratio is 0.05 to 10,000 μmol / mol (5.0 × 10 -8 ~1.0×10 -2 ), and more preferably, 0.5 to 5000 μmol / mol (5.0×10 -7 ~5.0×10 -3 ), and more preferably 0.80 to 1000 μmol / mol (8.0 × 10 -7 ~1.0×10 -3), and particularly preferably 1.0 to 100 μmol / mol (1.0×10 -6 ~1.0×10 -4 ).

[0124] In the polymerization step, the molar ratio of the diol compound, such as an aromatic diol compound, to the oxysilane compound, such as a diaryloxysilane compound (i.e., the value of the number of moles of oxysilane compound / the number of moles of diol compound) is, for example, 0.8 to 1.3, preferably 0.9 or more and 1.2 or less, more preferably 0.95 or more and 1.18 or less, and even more preferably 1.00 or more and 1.16 or less.

[0125] Next, the polysiloxane compound according to the present invention will be described in detail. [(V) Polysiloxane compound] The polysiloxane compound produced by the process of the present invention is a polymer having siloxane constituent units as described above, and specific examples thereof include the following. That is, the polyarylene siloxane compound is a polymer having at least a siloxane constituent unit represented by any one of the following formulas (1-1') to (1-4'). [ka]

[0126] In formulas (1-1') to (1-4'), R 1 and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent. R 1 and R 2 When it is an alkyl group which may have a substituent, it preferably has a total of 1 to 10 carbon atoms, more preferably has a total of 1 to 4 carbon atoms, and particularly preferably has a total of 1 or 2 carbon atoms. Also, R 1 and R 2When the aryl group is an aryl group which may have a substituent, the total number of carbon atoms is preferably 6 to 20, more preferably 6 to 12, and particularly preferably 6 to 8.

[0127] In formulas (1-1') and (1-2'), R 3 ~R 10 each independently represents hydrogen, halogen, alkoxy, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent. R 3 ~R 10 When it is an alkyl group which may have a substituent, it preferably has a total of 1 to 10 carbon atoms, more preferably has a total of 1 to 4 carbon atoms, and particularly preferably has a total of 1 or 2 carbon atoms. R 3 ~R 10 When the alkyl group is an alkenyl group which may have a substituent, the total number of carbon atoms is preferably 2 to 10, more preferably 2 to 6, and particularly preferably 2 to 4. Also, R 3 ~R 10 When the aryl group is an aryl group which may have a substituent, the total number of carbon atoms is preferably 6 to 20, more preferably 6 to 12, and particularly preferably 6 to 8.

[0128] In formulas (1-1') to (1-3'), each Z1 is independently an alkylene group having 1 to 5 carbon atoms, which may have a substituent, preferably an alkylene group having 1 to 3 carbon atoms, and more preferably an alkylene group having 1 or 2 carbon atoms. In formulas (1-1') to (1-3'), J1 and K1 each independently represent an integer of 0 or more and 5 or less, preferably an integer of 0 or more and 3 or less, and more preferably an integer of 0 or more and 2 or less, for example, 1 or 2. In formula (1-3'), A1 and A2 each independently represent -O- or -CH-. L1 and L2 each independently represent an integer of 0 or more and 3 or less, and L1 and L2 are preferably 1 or 2. In formulas (1-1′) and (1-2′), X is each independently a single bond or any one of the structural formulas represented by the following formula (2). [ka] In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5,000 or less. R 11 , and R 12 are preferably each independently hydrogen, an alkyl group having 1 to 10 carbon atoms which may have a substituent, or an aryl group having 6 to 16 carbon atoms which may have a substituent. In formula (2), a and b are each independently 0 or an integer of 1 or more and 5000 or less, and a and b are preferably integers of 1000 or less, more preferably integers of 500 or less, and even more preferably integers of 100 or less. In the siloxane structural unit, X is R 11 and R 12 are preferably bonded to each other to form a fluorene ring structure.

[0129] The siloxane constitutional unit preferably contains at least one represented by the following formula (1'). [ka]

[0130] R in formula (1') 1 and R2 The siloxane structure containing the following formula is introduced from the above-mentioned oxysilane compound. In formula (1'), R 1 and R 2 Regarding the preferred options, R 1 and R 2 is the same as:

[0131] The above mentioned R 1 and R 2 Examples of the substituent include a hydroxyl group, a halogen, an amino group, a vinyl group, a carboxyl group, a cyano group, a (meth)acryloxy group, a glycidyloxy group, and a mercapto group. R in formula (1') 1 and R 2 Preferred specific examples of the alkyl group include a methyl group, a phenyl group, a vinyl group, and a propyl group.

[0132] In formula (1'), R 3 ~R 10 Regarding the preferred options, R 1 and R 2 is the same as: The above mentioned R 3 ~R 10 Examples of the substituent include a hydroxyl group, a halogen, an amino group, a vinyl group, a carboxyl group, a cyano group, a (meth)acryloxy group, a glycidyloxy group, and a mercapto group.

[0133] In formula (1'), m represents an integer of 10 or more and 1,000 or less. The value of m in formula (1') is preferably 20 or more and 800 or less, and more preferably 30 or more and 500 or less.

[0134] In formula (1), X is R in the above formulas (1-1′) and (1-2′). 1 and R 2 is the same as:

[0135] The weight average molecular weight of the polysiloxane compound such as the polyarylenesiloxane compound is preferably 5,000 to 300,000, more preferably 10,000 to 300,000, even more preferably 10,000 to 200,000, and particularly preferably 10,000 to 100,000, for example, 20,000 to 90,000, more preferably 30,000 to 80,000, and particularly preferably 40,000 to 70,000.

[0136] In the case of a polysiloxane compound such as a polyarylenesiloxane compound, the glass transition temperature (Tg) according to JIS K 7121 is, for example, 40 to 200°C, and preferably 45 to 160°C.

[0137] In the above-mentioned polysiloxane compound, that is, the polysiloxane compound having a siloxane constituent unit represented by any one of Formulas (1-1) to (1-4) and Formulas (1-1') to (1-4'), the weight average molecular weight is 5,000 to 300,000, and the total content of cyclic units represented by the following formula (5-4) is preferably 4.0 wt % or less, more preferably 3.0 wt % or less, even more preferably 2.0 wt % or less, and particularly preferably 1.0 wt % or less, based on the total weight of the polysiloxane compound. If the total content of these low molecular weight cyclic compounds, for example cyclic dimers, is within the above-mentioned range, the properties of the polysiloxane compound are good, particularly when used in optical applications. [ka] In formula (5-4), the constitutional unit represented by formula (5-4) and other constitutional units may be arranged arbitrarily. That is, constitutional units other than the constitutional unit whose constitution is clearly indicated as formula (5-4) may be included, but in any case, the total value of m is 2 to 10, preferably 2 to 5, more preferably 2 or 3, for example 2. R 1 , R 2 , R 3 ~R10 and X are the same as those in formulas (1-1) and (1-2). In formula (5-4), X1 and X2 are each independently an alkylene group having 1 to 5 carbon atoms, which may have a substituent, preferably an alkylene group having 1 to 3 carbon atoms, and more preferably an alkylene group having 1 or 2 carbon atoms. In formula (5-4), i and ii each independently represent an integer of 0 or more and 5 or less, preferably an integer of 0 or more and 3 or less, more preferably an integer of 0 or more and 2 or less, for example, 1 or 2.

[0138] The lower limit of the low molecular weight cyclic substance in the polysiloxane compound is not particularly important, but is about 0.7% by weight, similar to the content of the low molecular weight compound in the polycarbonate copolymer having a weight average molecular weight of 1,000 or less. However, even if the low molecular weight compound is contained in an amount of 0.001% by weight, 0.01% by weight, or 0.1% by weight or more, the properties of the polysiloxane compound, especially when used for optical purposes, are not affected, and the flowability can be improved. Therefore, the lower limit of the content of the low molecular weight compound in the polysiloxane compound having a weight average molecular weight of 1,000 or less may be 0.001% by weight, 0.01% by weight, or 0.1% by weight.

[0139] The content of the low molecular weight cyclic compounds in the polysiloxane compound is a value calculated by summing up the content of several kinds of low molecular weight compounds as impurities from the peak area ratio of each component obtained by GPC analysis, as will be described in detail later in the Examples. That is, as will be described in detail later, it can be calculated from a predetermined GPC area ratio, similarly to the measurement of the proportion of low molecular weight compounds having a molecular weight of 1,000 or less in a polycarbonate copolymer.

[0140] Among the cyclic compounds represented by formula (5-4), a specific example is the cyclic dimer represented by the following formula (5-4'), and it has been confirmed that the molecular structure of the cyclic dimer represented by formula (5-4') and such a cyclic dimer can be contained in a polysiloxane compound. [ka]

[0141] The polysiloxane compound may contain a total content of cyclic compounds represented by the following formulae (6-1) and (6-2). These cyclic compounds are considered to be cyclic dimers resulting from a side reaction of the polymerization reaction for producing the polysiloxane compound. The content of these cyclic dimers in the polysiloxane compound is preferably 2.0% by weight or less, more preferably 1.5% by weight or less, even more preferably 1.0% by weight or less, and particularly preferably 0.5% by weight or less, based on the total weight of the polysiloxane compound. [ka] In formulas (6-1) and (6-2), the constitutional units represented by these formulas and other constitutional units may be arranged arbitrarily. That is, constitutional units other than the constitutional units explicitly shown as formulas (6-1) and (6-2) may be included, but in any case, the total value of n is 2 to 10, preferably 2 to 5, more preferably 2 or 3, for example 2. In formulas (6-1) and (6-2), X1 and X2 each independently represent an alkylene group having 1 to 5 carbon atoms, which may have a substituent, preferably an alkylene group having 1 to 3 carbon atoms, and more preferably an alkylene group having 1 or 2 carbon atoms. In formulas (6-1) and (6-2), i and ii each independently represent an integer of 0 to 5, preferably an integer of 0 to 3, more preferably an integer of 0 to 2, for example, 1 or 2. In addition, in the formulas (6-1) and (6-2), R 1 and R 2 , R 3 ~R 10 , Z1 and Z2, J1, K1 and X are as defined above.

[0142] The lower limit of the total content of the cyclic dimers represented by formulae (6-1) and (6-2) contained in the polysiloxane compound is not particularly limited, but may be, for example, 0.001% by weight, 0.01% by weight, or 0.1% by weight. The presence of a small amount of the cyclic dimer can contribute to improving the flowability of the polysiloxane compound during molding.

[0143] Specific examples of the compounds of formulae (6-1) and (6-2), respectively, include cyclic compounds of the following formulae (6-1') and (6-2'). [ka] In addition, in formulas (6-1') and (6-2'), R 1 and R 2 , R 3 ~R 10 and R 30 ~R 33 , Z1 and Z2, J1, K1 and X are as defined above.

[0144] In the polysiloxane compound, the 1% mass loss thermal decomposition temperature is preferably 415°C or less, more preferably 400°C or less, even more preferably 385°C or less, and particularly preferably 370°C or less.

[0145] In the polysiloxane compound, the proportion of the total weight of silicon atoms (total Si content) based on the total weight of the polysiloxane compound is preferably 0.1 to 20 mass%, more preferably 1.0 to 15 mass%, even more preferably 2.0 to 12 mass%, and particularly preferably 3.0 to 10 mass% (for example, 3.1 mass% or more, or more than 3.1 mass% and 9.8 mass% or less).

[0146] Next, the composition according to the present invention, that is, the composition containing the above-mentioned polysiloxane compound and the like, will be described in detail.

[0147] <3. Composition> The composition of the present invention contains the above-mentioned polysiloxane compound and a polycarbonate resin. The polycarbonate resin may be, for example, a polycarbonate resin that is completely or substantially free of a siloxane structure.

[0148] The type of polycarbonate resin contained in the composition together with the above-mentioned polysiloxane compound is not particularly limited as long as it contains a -[OR-OCO]- unit (R is an aliphatic group, an aromatic group, or both an aliphatic group and an aromatic group, and has a straight-chain structure or a branched structure) containing a carbonate bond in the molecular main chain. In addition, polycarbonate resins that do not fall under the above-mentioned polysiloxane compounds may contain polyester carbonate. Similarly, the polyester carbonate is not particularly limited as long as it contains a -[OR-OC]- unit (R is as described above) containing a carbonate bond in the molecular main chain.

[0149] The weight average molecular weight of the polycarbonate resin contained in the composition together with the polysiloxane compound is preferably 10,000 to 100,000, more preferably 13,000 to 80,000, and even more preferably 15,000 to 60,000.

[0150] The composition of the present invention may contain a resin other than a polycarbonate resin, preferably a thermoplastic resin. The type of thermoplastic resin is not particularly limited, but in addition to polycarbonate resin and polyester carbonate resin, various resins such as acrylic resins such as polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), triacetyl cellulose (TAC), polyethylene naphthalate (PEN), polyimide (PI), cycloolefin copolymer (COC), norbornene-containing resin, polyethersulfone, cellophane, and aromatic polyamide can be mentioned.

[0151] In the composition, the ratio of the total weight of silicon atoms (total Si amount) based on the total weight of the composition is preferably 0.1 to 20 mass%, more preferably 0.2 to 15 mass%, and particularly preferably 0.3 to 10 mass%. The ratio of the total Si amount in the composition can be adjusted by the ratio of the siloxane structural units to all structural units in the above-mentioned polycarbonate resin, or the amount of resin mixed with the polycarbonate resin and the amount of Si. For example, Q1, which is the Q value of a composition containing a polysiloxane compound measured under conditions of 280°C and 160 kgf, is preferably 120% or more (20% or more higher) than Q2, which is the Q value of only the polycarbonate resin contained in the composition measured under the same conditions, and the Q1 value of the entire composition is more preferably 130% or more, even more preferably 140% or more, and particularly preferably 150% or more, for example 160% or more, of the Q2 value of only the polycarbonate. Furthermore, for example, in the case of a composition containing 5% by mass of a polysiloxane compound, Q1, which is the Q value measured under conditions of 280°C and 160 kgf, is preferably a value that is 140% or more (40% or more higher) than Q2, which is the Q value measured under the same conditions for only the polycarbonate resin contained in the composition, and the Q1 value of the entire composition is more preferably 150% or more, even more preferably 160% or more, and particularly preferably 170% or more, for example 180% or more, of the Q2 value of only the polycarbonate.

[0152] A composition with excellent characteristics can be produced by using a polysiloxane compound with a high Si content. By mixing a polysiloxane compound with a Si content of, for example, 0.1 mass% or more with a resin that does not substantially contain a siloxane structural unit, preferably a polycarbonate resin, the resulting composition can have both excellent impact resistance and flowability.

[0153] In addition, the composition containing the polysiloxane compound may contain phenolic compounds that may be generated as by-products of the polymerization reaction, and oxysilane compounds and diol compounds that remain unreacted. The impurities of phenolic compounds and DPC may cause a decrease in strength when molded into a molded body or may cause odor generation, so the content of these is preferably as small as possible. For this reason, the content of phenolic compounds, oxysilane compounds and diol compounds may be reduced to an undetectable level, but may be contained in the composition within a range that does not impair the effect from the viewpoint of productivity. In addition, by containing a predetermined amount of monomer residue, for example, 1 to 1000 ppm by weight, preferably 10 to 900 ppm, more preferably 20 to 800 ppm, based on the total weight of the composition, the effect of improving the fluidity during molding can be obtained, and the plasticity can be improved when the resin is melted.

[0154] <4. Molded body> Next, a molded article containing a polysiloxane compound such as the polyarylenesiloxane compound described above will be described. The molded article of the present invention is obtained by molding a polysiloxane compound such as the polyarylenesiloxane compound described above. The molding method of the molded article is not particularly limited, and examples of the molded article include injection molded articles, press molded articles, blow molded articles, extrusion molded articles, vacuum molded articles, and pressure molded articles.

[0155] The optical lens according to the present invention is obtained by molding the polysiloxane compound of the present invention or a composition containing the polysiloxane compound. The polysiloxane compound of the present invention is suitable for optical applications and is suitably used for optical films, optical lenses, etc. The optical lens of the present invention has a refractive index, Abbe number, etc. within ranges suitable for a lens.

[0156] (Secondary ingredients) Quenching Agent In the polycarbonate copolymer and polysiloxane compound of the present invention, the catalyst may be removed or deactivated after the polymerization reaction is completed in order to maintain thermal stability and hydrolytic stability. A method of deactivating the catalyst by adding a known acidic substance can be preferably carried out. Specific examples of the acidic substance include esters such as butyl benzoate, aromatic sulfonic acids such as p-toluenesulfonic acid, aromatic sulfonic acid esters such as butyl p-toluenesulfonate and hexyl p-toluenesulfonate, phosphoric acids such as phosphorous acid, phosphoric acid, and phosphonic acid, phosphoric acid esters such as triphenyl phosphite, monophenyl phosphite, diphenyl phosphite, diethyl phosphite, di-n-propyl phosphite, di-n-butyl phosphite, di-n-hexyl phosphite, dioctyl phosphite, and monooctyl phosphite, and phosphate esters such as triphenyl phosphate, diphenyl phosphate, monophenyl phosphate, dibutyl phosphate, and dioctyl phosphate. Suitable examples of the deactivator include phosphate esters such as monooctyl phosphate, diphenylphosphonic acid, dioctylphosphonic acid, dibutylphosphonic acid, and the like; phosphonic acids such as diethyl phenylphosphonate, and the like; phosphines such as triphenylphosphine, bis(diphenylphosphino)ethane, and the like; boric acid, phenylboric acid, and the like; aromatic sulfonates such as tetrabutylphosphonium dodecylbenzenesulfonate, and the like; organic halides such as stearic acid chloride, benzoyl chloride, and p-toluenesulfonic acid chloride, and the like; alkyl sulfuric acid such as dimethyl sulfate, and the like; organic halides such as benzyl chloride, and the like. These deactivators may be used in an amount of, for example, 0.001 to 50 times by mole, preferably 0.01 to 30 times by mole, relative to the amount of the catalyst.

[0157] Additives <Stabilizer> A stabilizer may be added to the polycarbonate copolymer and polysiloxane compound of the present invention. Examples of the stabilizer include a heat stabilizer and an antioxidant. When blended, the addition ratio of the stabilizer is preferably 0.001 parts by mass or more, more preferably 0.01 parts by mass or more, and even more preferably 0.02 parts by mass or more, and is preferably 2 parts by mass or less, more preferably 1.4 parts by mass or less, and even more preferably 1.0 parts by mass or less, relative to 100 parts by mass of the polycarbonate copolymer or polysiloxane compound. The stabilizer may contain only one type, or may contain two or more types. When two or more types are contained, the total amount is preferably within the above range.

[0158] <<Heat stabilizer>> Examples of the heat stabilizer include phenol-based, phosphorus-based, and sulfur-based heat stabilizers.Specific examples include phosphorus oxoacids such as phosphoric acid, phosphonic acid, phosphorous acid, phosphinic acid, and polyphosphoric acid; acid pyrophosphate metal salts such as sodium acid pyrophosphate, potassium acid pyrophosphate, and calcium acid pyrophosphate; phosphates of metals in Group 1 or Group 10 such as potassium phosphate, sodium phosphate, cesium phosphate, and zinc phosphate; organic phosphate compounds, organic phosphite compounds, and organic phosphonite compounds.Furthermore, examples include at least one selected from the group consisting of phosphorous ester compounds (a) in which at least one ester in the molecule is esterified with phenol and / or phenol having at least one alkyl group having 1 to 25 carbon atoms, phosphorous acid (b), and tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene-di-phosphonite (c).Specific examples of the phosphite ester compound (a) include trioctyl phosphite, trioctadecyl phosphite, tridecyl phosphite, trilauryl phosphite, tristearyl phosphite, triphenyl phosphite, tris(mononylphenyl)phosphite, tris(mononyl / dinonyl phenyl)phosphite, trisnonylphenyl phosphite, tris(octylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, trinonyl phosphite, didecyl monophenyl phosphite, dioctyl monophenyl phosphite, diisopropyl monophenyl phosphite, monobutyl diphenyl phosphite, monodecyl diphenyl phosphite, and bis(2,4-di-tert-butylphenyl)pentaerythritol. bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol phosphite, monooctyl diphenyl phosphite, distearyl pentaerythritol diphosphite, tricyclohexyl phosphite, diphenyl pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, bis(nonylphenyl)pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-ethylphenyl)pentaerythritol diphosphite, etc. These may be used alone or in combination of two or more. Examples of the organic phosphite compound include "ADK STAB 1178 (product name, the same applies below)", "ADK STAB 2112", and "ADK STAB HP-10" manufactured by Adeka Corporation; "JP-351", "JP-360", and "JP-3CP" manufactured by Johoku Chemical Industry Co., Ltd.; and "IRGAFOS 168" manufactured by BASF. Examples of the phosphoric acid ester include trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, triphenyl phosphate, tricresyl phosphate, tris(nonylphenyl)phosphate, and 2-ethylphenyldiphenyl phosphate. When the heat stabilizer is added, the amount thereof is preferably 0.001 part by mass or more, more preferably 0.01 part by mass or more, even more preferably 0.03 part by mass or more, and is preferably 1 part by mass or less, more preferably 0.7 part by mass or less, even more preferably 0.5 part by mass or less, per 100 parts by mass of the polycarbonate copolymer or polysiloxane compound. The heat stabilizer may be contained in only one type, or in combination with two or more types. When two or more types are contained, the total amount is preferably within the above range.

[0159] <<Antioxidants>> Examples of the antioxidant include a phenol-based antioxidant, a hindered phenol-based antioxidant, a bisphenol-based antioxidant, and a polyphenol-based antioxidant.Specifically, 2,6-di-tert-butyl-4-methylphenol, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate, tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane, 4,4'-butylidenebis-(3-methyl-6-tert-butylphenol), triethylene glycol-bis[3-(3-tert t-Butyl-4-hydroxy-5-methylphenyl)propionate], 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N' -Hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)], 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl [[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, 3,3',3”,5,5',5”-hexa-tert-butyl-a,a',a”-(mesitylene-2,4,6-triyl)tri-p-cresol, 4,6-bis(octylthiomethyl)-o-cresol, ethylenebis(oxa diethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, and the like. Examples of phenol-based antioxidants include "Irganox 1010" (registered trademark, the same applies below) and "Irganox 1076" manufactured by BASF, and "ADK STAB AO-50" and "ADK STAB AO-60" manufactured by Adeka Corporation. When the antioxidant is added, the amount thereof is preferably 0.001 part by mass or more, more preferably 0.01 part by mass or more, and preferably 1 part by mass or less, more preferably 0.5 part by mass or less, per 100 parts by mass of the polycarbonate copolymer or polysiloxane compound. The antioxidant may be contained alone or in combination with two or more kinds. When two or more kinds are contained, the total amount is preferably within the above range.

[0160] The polycarbonate copolymer and polysiloxane compound of the present invention may contain various additives within the scope of the present invention. Examples of additives include at least one additive selected from a flame retardant, a flame retardant assistant, an ultraviolet absorber, a release agent, and a colorant, and it is preferable to include at least one of a flame retardant and a release agent. In addition, antistatic agents, fluorescent brighteners, antifogging agents, flow improvers, plasticizers, dispersants, antibacterial agents, etc. may be added as long as they do not significantly impair the desired physical properties.

[0161] <Flame retardants> The polycarbonate copolymer and polysiloxane compound of the present invention may contain various additives within the scope of the present invention. As a flame retardant, an organic metal salt-based flame retardant, a phosphorus-based flame retardant, a silicone-based flame retardant, etc. may be contained. Examples of flame retardants that can be used in the present invention include the flame retardants (flame retardant compositions) described in paragraphs 0085 to 0093 of JP 2016-183422 A, the contents of which are incorporated herein by reference.

[0162] <Ultraviolet absorbing agent> Examples of the ultraviolet absorbent include inorganic ultraviolet absorbents such as cerium oxide and zinc oxide, as well as organic ultraviolet absorbents such as benzotriazole compounds, benzophenone compounds, salicylate compounds, cyanoacrylate compounds, triazine compounds, oxanilide compounds, malonic acid ester compounds, hindered amine compounds, and phenyl salicylate compounds. Of these, benzotriazole- and benzophenone-based organic ultraviolet absorbents are preferred.In particular, specific examples of benzotriazole compounds include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-[2'-hydroxy-3',5'-bis(α,α-dimethylbenzyl)phenyl]-benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butyl-phenyl)-benzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butyl-phenyl)-5-chlorobenzotriazole, Chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-amyl)-benzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2N-benzotriazol-2-yl)phenol], 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol, 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl] 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylmethyl)phenol, 2-[5-chloro(2H)-benzotriazol-2-yl]-4-methyl-6-(tert-butyl)phenol, 2,2'-(1,4-phenylene)bis[4H-3,1-benzoxazin-4-one], [(4-methoxyphenyl)-methylene]-propanediol acid dimethyl ester, 2-(2H-benzotriazol-2-yl)-p-cresol, 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylmethyl)phenol, 2-[5-chloro(2H)-benzotriazol-2-yl]-4-methyl-6-(tert-butyl)phenol phenol, 2,4-di-tert-butyl-6-(5-chlorobenzotriazol-2-yl)phenol, 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetrabutyl)phenol, 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetrabutyl)phenol], [methyl-3-[3-tert-butyl-5-(2H-benzotriazol-2-yl)-4-hydroxyphenyl]propionate-polyethylene glycol] condensate, and the like can be mentioned.Among the above, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole and 2,2'-methylene-bis[4-(1,1,3,3-tetramethylbutyl)-6-(2N-benzotriazole-2-yl)phenol] are preferred. Specific examples of benzophenone-based ultraviolet absorbers include 2,4-dihydroxy-benzophenone, 2-hydroxy-4-methoxy-benzophenone, 2-hydroxy-4-n-octoxy-benzophenone, 2-hydroxy-4-dodecyloxy-benzophenone, 2-hydroxy-4-octadecyloxy-benzophenone, 2,2'-dihydroxy-4-methoxy-benzophenone, 2,2'-dihydroxy-4,4'-dimethoxy-benzophenone, and 2,2',4,4'-tetrahydroxy-benzophenone. Specific examples of phenyl salicylate-based ultraviolet absorbers include phenyl salicylate and 4-tert-butyl-phenyl salicylate. Specific examples of triazine-based ultraviolet absorbers include 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol and 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl]-5-(octyloxy)phenol. Specific examples of hindered amine-based ultraviolet absorbers include bis(2,2,6,6-tetramethylpiperidin-4-yl)sebacate. When the ultraviolet absorber is added, the amount of the ultraviolet absorber added is preferably 0.01 part by mass or more, more preferably 0.1 part by mass or more, and is preferably 3 parts by mass or less, more preferably 1 part by mass or less, per 100 parts by mass of the polycarbonate copolymer or polysiloxane compound. The ultraviolet absorbing agent may be used alone or in combination of two or more. When two or more types are used, the total amount is preferably within the above range.

[0163] <Release agent> Examples of the release agent include carboxylate esters, polysiloxane compounds, and paraffin wax (polyolefin-based). Specifically, at least one compound selected from the group consisting of aliphatic carboxylic acids, esters of aliphatic carboxylic acids and alcohols, aliphatic hydrocarbon compounds having a number average molecular weight of 200 to 15,000, and polysiloxane-based silicone oils can be mentioned. Examples of the aliphatic carboxylic acids include saturated or unsaturated aliphatic mono-, di-, or tri-carboxylic acids. Here, the aliphatic carboxylic acids also include alicyclic carboxylic acids. Among these, preferred aliphatic carboxylic acids are mono- or di-carboxylic acids having 6 to 36 carbon atoms, and more preferred are aliphatic saturated mono-carboxylic acids having 6 to 36 carbon atoms. Specific examples of aliphatic carboxylic acids include palmitic acid, stearic acid, valeric acid, caproic acid, capric acid, lauric acid, arachic acid, behenic acid, lignoceric acid, cerotic acid, melissic acid, tetrameric acid, montanic acid, glutaric acid, adipic acid, and azelaic acid. The aliphatic carboxylic acids in the esters of aliphatic carboxylic acids and alcohols can be the same as the aliphatic carboxylic acids described above. On the other hand, the alcohols can include saturated or unsaturated monohydric or polyhydric alcohols. These alcohols may have a substituent such as a fluorine atom or an aryl group. Among these, monohydric or polyhydric saturated alcohols having 30 or less carbon atoms are preferred, and aliphatic saturated monohydric or polyhydric alcohols having 30 or less carbon atoms are more preferred. Here, aliphatic compounds also include alicyclic compounds. Specific examples of the alcohol include octanol, decanol, dodecanol, stearyl alcohol, behenyl alcohol, ethylene glycol, diethylene glycol, glycerin, pentaerythritol, 2,2-dihydroxyperfluoropropanol, neopentylene glycol, ditrimethylolpropane, dipentaerythritol, etc. The above ester compounds may contain aliphatic carboxylic acids and / or alcohols as impurities, or may be a mixture of a plurality of compounds.Specific examples of esters of aliphatic carboxylic acids and alcohols include beeswax (a mixture mainly composed of myricyl palmitate), stearyl stearate, behenyl behenate, stearyl behenate, glycerin monopalmitate, glycerin monostearate, glycerin distearate, glycerin tristearate, pentaerythritol monopalmitate, pentaerythritol monostearate, pentaerythritol distearate, pentaerythritol tristearate, and pentaerythritol tetrastearate. Examples of aliphatic hydrocarbons having a number average molecular weight of 200 to 15,000 include liquid paraffin, paraffin wax, microwax, polyethylene wax, Fischer-Tropsch wax, and α-olefin oligomers having 3 to 12 carbon atoms. Here, the aliphatic hydrocarbons also include alicyclic hydrocarbons. These hydrocarbon compounds may be partially oxidized. Among these, paraffin wax, polyethylene wax, or partial oxides of polyethylene wax are preferred, and paraffin wax and polyethylene wax are more preferred. The number average molecular weight is preferably 200 to 5000. These aliphatic hydrocarbons may be a single substance or a mixture of substances with various components and molecular weights, as long as the main component is within the above range. Examples of polysiloxane-based silicone oils include dimethyl silicone oil, phenyl methyl silicone oil, diphenyl silicone oil, and fluorinated alkyl silicone. Two or more of these may be used in combination. When the release agent is added, the amount of the release agent added is preferably 0.001 part by mass or more, more preferably 0.01 part by mass or more, and preferably 2 parts by mass or less, more preferably 1 part by mass or less, per 100 parts by mass of the polycarbonate copolymer or the polysiloxane compound. The release agent may be used alone or in combination of two or more. When two or more types are used, the total amount is preferably within the above range.

[0164] <Coloring agent> The colorant may be either a dye or a pigment, and examples of the colorant include inorganic pigments, organic pigments, organic dyes, etc. Examples of inorganic pigments include sulfide pigments such as carbon black, cadmium red, and cadmium yellow; silicate pigments such as ultramarine; oxide pigments such as titanium oxide, zinc white, red iron oxide, chromium oxide, iron black, titanium yellow, zinc-iron brown, titanium-cobalt green, cobalt green, cobalt blue, copper-chromium black, and copper-iron black; chromate pigments such as yellow lead and molybdate orange; and ferrocyanide pigments such as Prussian blue. Examples of organic pigments and organic dyes as colorants include phthalocyanine-based dyes and pigments such as copper phthalocyanine blue and copper phthalocyanine green (dyes and pigments are referred to as dyes and pigments, the same applies below); azo-based dyes and pigments such as nickel azo yellow; condensed polycyclic dyes and pigments such as thioindigo-based, perinone-based, perylene-based, quinacridone-based, dioxazine-based, isoindolinone-based, and quinophthalone-based; quinoline-based, anthraquinone-based, heterocyclic, and methyl-based dyes and pigments, etc. Among these, titanium oxide, carbon black, cyanine-based, quinoline-based, anthraquinone-based, and phthalocyanine-based dyes and pigments, etc. are preferred from the viewpoint of thermal stability. Furthermore, the colorant may be used in the form of a masterbatch with a polystyrene resin, a polycarbonate resin, or an acrylic resin, for the purposes of improving handling properties during extrusion and improving dispersibility in the resin composition. The colorant is preferably added in an amount of 5 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less, and 0.1 parts by mass or more, per 100 parts by mass of the polycarbonate copolymer or polysiloxane compound. Only one colorant may be used, or two or more colorants may be used. When two or more colorants are used, the total amount is preferably within the above range.

[0165] Molded products other than lenses There is no limitation on the shape, pattern, color, dimensions, etc. of the molded body obtained by using the polycarbonate copolymer or polysiloxane compound, and it may be arbitrarily set according to the application. Specific examples of the molded body include electric and electronic devices, OA (Office Automation) devices, information terminal devices, machine parts, home appliances, vehicle parts, building materials, various containers, leisure goods and sundries, parts of lighting equipment, etc., parts of various household electrical appliances, housings, containers, covers, storage parts, cases, covers and cases of lighting equipment, etc. Examples of the electric and electronic devices include personal computers, game machines, television receivers, display devices such as liquid crystal displays and plasma displays, printers, copy machines, scanners, fax machines, electronic organizers and personal data terminals (PDAs), electronic desk calculators, electronic dictionaries, cameras, video cameras, mobile phones, battery packs, drives and readers for recording media, mice, numeric keypads, CD (Compact Disc) players, MD (MiniDisc) players, portable radios and audio players, etc. Further examples of the molded articles include illuminated signs, liquid crystal backlights, illuminated displays, traffic signs, signboards, screens, reflectors, meter parts and other automobile parts (vehicle mounted parts), toys, decorations, and the like. The polycarbonate copolymer and polysiloxane compound of the present application have excellent impact resistance, high fluidity when melted, and can be formed into a molded article having a fine structure, and therefore can be suitably used as in-vehicle electric / electronic parts, mechanical parts, and vehicle parts. Examples of such parts include automobile interior panels, automobile lamp lenses, automobile inner lenses, automobile lens protection covers, automobile light guides, etc.

[0166] Method for forming a molded body The method for producing the molded article of the present invention is not particularly limited, and any molding method generally used for resins such as polycarbonate resins can be used. Examples of such methods include injection molding, ultra-high speed injection molding, injection compression molding, two-color molding, gas-assisted and other hollow molding methods, molding methods using heat-insulating molds, molding methods using rapidly heated molds, foam molding (including supercritical fluids), insert molding, IMC (in-mold coating molding) molding, extrusion molding, sheet molding, thermoforming, rotational molding, lamination molding, press molding, etc. Also, a molding method using a hot runner system can be used.

[0167] Other resins The polycarbonate copolymer and polysiloxane compound of the present invention may contain resins other than the polycarbonate copolymer and polysiloxane compound of the present invention as necessary, as long as the desired physical properties are not significantly impaired. Examples of such other resins include polycarbonate resins other than the polycarbonate copolymer and polysiloxane compound of the present invention, thermoplastic polyester resins such as polyethylene terephthalate resin (PET resin), polytrimethylene terephthalate resin (PTT resin), and polybutylene terephthalate resin (PBT resin); styrene-based resins such as polystyrene resin (PS resin), high impact polystyrene resin (HIPS), acrylonitrile-styrene copolymer (AS resin), and methyl methacrylate-styrene copolymer (MS resin); and methyl methacrylate-acrylic rubber-styrene copolymer. Examples of such elastomers include core / shell elastomers such as copolymers (MAS), polyester-based elastomers, and other elastomers; polyolefin resins such as cyclic cycloolefin resins (COP resins) and cyclic cycloolefin (COP) copolymer resins; polyamide resins (PA resins); polyimide resins (PI resins); polyetherimide resins (PEI resins); polyurethane resins (PU resins); polyphenylene ether resins (PPE resins); polyphenylene sulfide resins (PPS resins); polysulfone resins (PSU resins); polymethacrylate resins (PMMA resins); and polycaprolactone. EXAMPLES

[0168] [Example of polycarbonate resin] <Measurement of polystyrene equivalent weight average molecular weight (Mw)> A calibration curve was created using GPC (gel permeation chromatography) with chloroform as the developing solvent and standard polystyrene (Shodex STANDARD, SM-105) of known molecular weight (molecular weight distribution = 1). The elution time and molecular weight value of each peak from the measured standard polystyrene were plotted, and a cubic approximation was performed to create a calibration curve. Then, based on the obtained calibration curve, the weight average molecular weight (Mw) was calculated in terms of polystyrene from the following formula. [Calculation formula] Mw = Σ(W i ×M i ) / Σ(W i ) (In the above formula, i is the i-th division point when dividing the molecular weight M, W i is the i-th weight, M i represents the i-th molecular weight. Also, the molecular weight M represents the molecular weight in polystyrene equivalent at the same elution time on the calibration curve.) [Measurement conditions] Equipment: Shimadzu Corporation Labsolutions Columns: Guard column (Shodex GPC KG 4A) x 1, analytical column (Shodex GPC K-805L) x 2 Solvent: Chloroform (HPLC grade) ·Injection volume: 10μL Sample concentration: 2000ppm Solvent flow rate: 1mL / min ·Measurement temperature: 40℃ Detector: RI

[0169] <Measurement of the content of low molecular weight compounds with a weight average molecular weight (Mw) of 1,000 or less> The proportion of low molecular weight compounds with Mw of 1,000 or less in the polycarbonate resin was calculated from the ratio of the area from retention time 20.5 min to 21.5 min to the area from 0 min to 21.5 min (GPC area ratio) based on the data obtained by GPC analysis under the above-mentioned conditions. That is, GPC analysis was performed under the conditions described in the column of <Measurement of polystyrene-equivalent weight average molecular weight (Mw)>, and the content ratio of low molecular weight compounds (B / A×100(%)) was measured based on the ratio of the GPC area (A) of a peak with a retention time of 21.5 minutes or less, which is considered to correspond to the amount of all compounds contained in the polycarbonate resin sample, to the GPC area (B) of a peak confirmed with a retention time between 20.5 minutes and 21.5 minutes, which is considered to correspond to the amount of low molecular weight compounds with a weight average molecular weight of 1,000 or less.

[0170] <Measurement of glass transition temperature (Tg)> A test piece weighing 5 to 12 mg was weighed into an AI autosampler sample container (RDC aluminum pan, a cylindrical container with a diameter of 6.8 mm and a height of 2.5 mm) and the top of the sample container was sealed with an AI autosampler cover to prepare the measurement sample. The measurement was performed using a differential scanning calorimeter (DSC) under a nitrogen atmosphere (nitrogen flow rate: 50 ml / min), and 10.0 mg of sapphire was used as a standard substance in the reference cell. The measurement sample adjusted to 30°C was heated to 280°C at 20°C / min, and then cooled to 30°C at 20°C / min. The temperature was then raised to 280°C at 10°C / min and the measurement was performed. Measurement equipment: Differential scanning calorimeter (DSC) (product name "DSC-7020", manufactured by Hitachi High-Tech Science Corporation)

[0171] <Measurement of low molecular weight compounds (phenol (PhOH), bisphenol A (BPA), dimethyldiphenoxysilane (DMDPS), diphenyl carbonate (DPC)> 10 g of the sample was dissolved in 60 g of dichloromethane to prepare a resin solution, and 150 g of ethanol was added dropwise to the stirred resin solution over 30 minutes. The precipitate was filtered off using NoA5 filter paper, and the filtrate was concentrated using an evaporator to obtain oligomer component a. The obtained precipitate was dissolved in 60 g of dichloromethane to prepare a resin solution, and 150 g of ethanol was added dropwise to obtain the precipitate and oligomer component b. The obtained oligomer components a and b were dissolved in dichloromethane to prepare a 1000 μg / mL solution, and analyzed and quantified by GC / FID. The quantitative values ​​were calculated in terms of 2,2-bis(4-hydroxyphenyl)propane, using a calibration curve for 2,2-bis(4-hydroxyphenyl)propane that had been prepared in advance. [GC / FID measurement conditions] Equipment: Shimadzu GC2025 Column: Capillary column DB-35, 30 mm x 0.25 mm x 0.25 μm Heating conditions: 40℃-300℃ (5min hold), 10℃ / min Injection port temperature: 300℃, injection volume: 1.0μL (split ratio 1:20) Carrier gas: He ·Air flow rate: 400mL / min ·H2 flow rate: 40mL / min Make-up gas: 30mL / min Standard substance: 2,2-bis(4-hydroxyphenyl)propane

[0172] <Measurement of cyclic dimer> The content of the above-mentioned cyclic dimer contained in the polycarbonate copolymer was measured as follows. A 20 g sample of polycarbonate copolymer was dissolved in 120 g of dichloromethane to prepare a resin solution, and 200 g of ethanol was added dropwise to the stirred resin solution over 30 minutes. The precipitate was filtered off using NoA5 filter paper, and the filtrate was concentrated using an evaporator to obtain oligomer component A and precipitate A. The precipitate A was dissolved in 120 g of dichloromethane to prepare a resin solution, and 200 g of ethanol was added dropwise to the stirred resin solution over 30 minutes. The precipitate was filtered using No. A5 filter paper, and the filtrate was concentrated using an evaporator to obtain oligomer component B and precipitate B. The precipitate B was dissolved in 120 g of dichloromethane to prepare a resin solution, and 200 g of ethanol was added dropwise to the stirred resin solution over 30 minutes. The precipitate was filtered off using NoA5 filter paper, and the filtrate was concentrated using an evaporator to obtain oligomer component C and precipitate C. The obtained oligomer components A, B, and C were dissolved in dichloromethane to prepare a 1000 μg / mL solution, and the cyclic dimer was analyzed by GC-Q-MS / FID. The quantitative value was calculated in terms of 2,2-bis(4-hydroxyphenyl)propane based on a calibration curve of 2,2-bis(4-hydroxyphenyl)propane prepared in advance. [GC-Q-MS / FID measurement conditions] Equipment: Agilent Technologies Agilent-7890B / Agilent-5975C MSD Inert XL MSD with TAD Column: DB-5MS, 15mm x 0.25mm x 0.1μm ·Restrictor(MS):0.18mm×1.44mm ·Restrictor(FID):0.18mm×0.53mm Heating conditions: 50℃ (2min hold) - 320℃ (15min hold), 20℃ / min ·Inlet temperature: 300℃ Injection volume: 1.0 μL (split ratio 1:10) Carrier gas: He FID / MS ratio: 1 / 1 ·Aux temperature: 300℃ Scan Range: m / z 33-700 Scan rate: 2.22 scan / s ·FID temperature: 300℃ ·H2 flow rate: 30mL / min ·Air flow rate: 400mL / min Make-up gas: 25mL / min Standard substance: 2,2-bis(4-hydroxyphenyl)propane -Quantitative analysis of cyclic dimer: Quantitative analysis based on peak intensity at 16.6 min

[0173] <Liquidity (Q value)> Melt flow volume (cm) per unit time measured at 280℃ and a load of 160 kg -3 / sec) (the melt flow volume was measured using a CFT-500D model (nozzle diameter 1 mm × nozzle length 10 mm) manufactured by Shimadzu Corporation, and the value per unit time was calculated from a stroke of 7.0 to 10.0 mm).

[0174] <Charpy impact test> The Charpy impact strength (kJ / m 2 ) was measured.

[0175] <Measuring method of refractive index (nd)> Refractive index (nd): A 3 mm thick right-angled piece made of the polycarbonate copolymer produced in the examples was measured using an Abbe refractometer according to the method of JIS-K-7142. <Measuring method of Abbe number (νd)> For a 3 mm thick right-angle piece made of the polycarbonate resin produced in the examples, the refractive indexes at wavelengths of 486 nm, 589 nm, and 656 nm at 23°C were measured using an Abbe refractometer, and the Abbe number was calculated using the following formula. νd=(nd-1) / (nF-nC) nd: Refractive index at a wavelength of 589 nm nC: Refractive index at a wavelength of 656 nm nF: Refractive index at a wavelength of 486 nm

[0176] (Synthesis Example 1) Synthesis of dimethyldiphenoxysilane Dimethyldiphenoxysilane was synthesized with reference to the method described in US2012 / 184702. 176.34g (1.87mol) of phenol was stirred at 50℃ under N2 atmosphere, and 113.24g (0.88mol) of dimethyldichlorosilane was added dropwise over 30min. One hour after the end of the addition, the by-products were distilled off at 170℃ under reduced pressure of 200hPa. The reaction solution was cooled to room temperature, and the product was dissolved in 300mL of dichloromethane. The product dissolved in dichloromethane was washed twice with 300mL of 10% NaOH solution, and the organic layer was extracted. The organic layer was washed twice with 300mL of water, and the organic layer after washing was extracted. Residual water was removed with anhydrous magnesium sulfate, and then dichloromethane was distilled off with an evaporator to obtain an oily component. The oily component obtained was analyzed by 1H-NMR and confirmed to be dimethyldiphenoxysilane (1H-NMR (CDCl3, 500 MHz, δ; ppm) = 0.378 (s; 6H), 6.942, 6.944 (d; 4H), 6.959, 6.961, 6.995 (t; 2H), 7.230, 7.245, 7.257 (t; 4H)). The molar yield was 66%.

[0177] (Example A-1) 104.97g (0.46mol) of 2,2-bis(4-hydroxyphenyl)propane, 4.58g (0.02mol) of dimethyldiphenoxysilane, 101.46g (0.47mol) of diphenyl carbonate, and 2.0μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 300ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 190℃ and stirred for 20 minutes. After that, the phenol distilled from the reaction system was coagulated and removed in a cooling tube over a period of 1 hour and 20 minutes while carrying out an ester exchange reaction, and the temperature in the system was set to 260°C, the degree of vacuum was set to 2 hPa or less, and the reaction was maintained for another 1 hour and 30 minutes to obtain a colorless and transparent polycarbonate copolymer having an arylenesiloxane structure. During the decompression, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 27,000 Pa, 24,000 Pa, 20,000 Pa, 17,000 Pa, 14,000 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000 Pa, 1,000 Pa, and 200 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured by GPC and found to be 44,373. The Tg of the copolymer was measured by DSC and found to be 136° C. The weight loss of the copolymer was measured by TG-DTA and found to be 411° C. for 1% weight loss.

[0178] (Example A-2) 72.85g (0.32mol) of 2,2-bis(4-hydroxyphenyl)propane, 7.9g (0.032mol) of dimethyldiphenoxysilane, 65.86g (0.31mol) of diphenyl carbonate, and 0.6μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar number to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 300ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 30 minutes. After that, the phenol distilled from the reaction system was coagulated and removed in a cooling tube over a period of 1.5 hours while carrying out an ester exchange reaction, and the temperature in the system was set to 260°C, the degree of vacuum was set to 4 hPa or less, and the system was maintained for another 1.5 hours to obtain a colorless and transparent polycarbonate copolymer having an arylenesiloxane structure. During the decompression, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 27,000 Pa, 24,000 Pa, 20,000 Pa, 16,000 Pa, 8,000 Pa, 4,000 Pa, 2,000 Pa, 400 Pa, and 400 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured by GPC and found to be 48,035. The Tg of the copolymer was measured by DSC and found to be 129°C. The Q value of the copolymer was measured and found to be 75(×10 -2 cm 3 / sec).

[0179] (Example A-3) 21.69g (0.10mol) of 2,2-bis(4-hydroxyphenyl)propane, 9.52g (0.39mol) of dimethyldiphenoxysilane, 13.5g (0.63mol) of diphenyl carbonate, and 7.0μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative number of moles to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 30 minutes. After that, the phenol distilled from the reaction system was coagulated and removed in a cooling tube over a period of 1 hour while the ester exchange reaction was carried out, and the temperature in the system was set to 260°C, the degree of vacuum was set to 4 hPa or less, and the system was maintained for another 2 hours to obtain a colorless and transparent polycarbonate copolymer having an arylenesiloxane structure. During the decompression, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 27,000 Pa, 24,000 Pa, 20,000 Pa, 16,000 Pa, 8,000 Pa, 4,000 Pa, 2,000 Pa, 400 Pa, and 400 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured by GPC and found to be 54,007. The Tg of the copolymer was measured by DSC and found to be 101°C. The Q value of the copolymer was measured and found to be 114(×10 -2 cm 3 / sec).

[0180] (Example A-4) 30.69g (0.13mol) of 2,2-bis(4-hydroxyphenyl)propane, 25.46g (0.10mol) of dimethyldiphenoxysilane, 9.96g (0.046mol) of diphenyl carbonate, and 7.0μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar number to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 30 minutes. After that, the phenol distilled from the reaction system was coagulated and removed in a cooling tube over a period of 1 hour while carrying out an ester exchange reaction, and the temperature in the system was set to 260°C, the degree of vacuum was set to 4 hPa or less, and the system was maintained for another 2 hours to obtain a colorless and transparent polycarbonate copolymer having an arylenesiloxane structure. Note that, during the decompression, the pressure was adjusted so as to change stepwise from atmospheric pressure to 27,000 Pa, 24,000 Pa, 20,000 Pa, 16,000 Pa, 8,000 Pa, 4,000 Pa, 2,000 Pa, 400 Pa, and 400 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured by GPC and found to be 63,068. The Tg of the copolymer was measured by DSC and found to be 75°C.

[0181] (Example A-5) 30.63g (0.13mol) of 2,2-bis(4-hydroxyphenyl)propane, 31.05g (0.13mol) of dimethyldiphenoxysilane, 5.04g (0.024mol) of diphenyl carbonate, and 7.0μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative number of moles to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 30 minutes. After that, the phenol distilled from the reaction system was coagulated and removed in a cooling tube over a period of 1 hour while carrying out an ester exchange reaction, and the temperature in the system was set to 260°C, the degree of vacuum was set to 4 hPa or less, and the system was maintained for another 2 hours to obtain a colorless and transparent polycarbonate copolymer having an arylenesiloxane structure. Note that, during the decompression, the pressure was adjusted so as to change stepwise from atmospheric pressure to 27,000 Pa, 24,000 Pa, 20,000 Pa, 16,000 Pa, 8,000 Pa, 4,000 Pa, 2,000 Pa, 400 Pa, and 400 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured by GPC and found to be 49,161. The Tg of the copolymer was measured by DSC and found to be 62°C.

[0182] (Examples A-6 to A-14) A copolymer was produced in the same manner as in Example A-1, except that the raw material compounds were changed as shown in the following Table 1. The properties of the obtained copolymer are shown in Table 1. [Table 1]

[0183] (Example A-15) 2,2-bis(4-hydroxyphenyl)propane 2310g (10.13mol), dimethyldiphenoxysilane 1849.26g (7.58mol), diphenyl carbonate 753.04g (3.52mol), and cesium carbonate 14.0μmol / mol (catalyst amount is the relative molar number to 2,2-bis(4-hydroxyphenyl)propane) as a catalyst were placed in a 10L reactor equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 40 minutes. After that, the phenol distilled from the reaction system was coagulated and removed in a cooling tube over a period of 1 hour and 30 minutes while carrying out an ester exchange reaction, and the temperature in the system was set to 260°C, the degree of vacuum was set to 1 hPa or less, and the reaction was maintained for another 1 hour and 15 minutes to obtain a colorless and transparent polycarbonate copolymer having an arylenesiloxane structure. During the decompression, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 27,000 Pa, 24,000 Pa, 20,000 Pa, 17,000 Pa, 14,000 Pa, 12,000 Pa, 8,000 Pa, 4,000 Pa, and 100 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured using GPC and found to be 208,939. The Tg of the copolymer was measured by DSC and found to be 74.2° C. The weight loss of the copolymer was measured by TG-DTA and found to be 337.1° C. for 1% weight loss.

[0184] (Example A-16) 2,2-bis(4-hydroxyphenyl)propane 2497g (10.95mol), dimethyldiphenoxysilane 1997.20g (8.19mol), diphenyl carbonate 813.00g (3.80mol), and cesium carbonate 3.0μmol / mol (catalyst amount is the relative molar number to 2,2-bis(4-hydroxyphenyl)propane) as a catalyst were placed in a 10L reactor equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 45 minutes. After that, the phenol distilled from the reaction system was coagulated and removed in a cooling tube over a period of 2 hours and 30 minutes while carrying out an ester exchange reaction, and the temperature in the system was set to 260°C, the degree of vacuum was set to 1 hPa or less, and the reaction was maintained for another hour and 30 minutes to obtain a colorless and transparent polycarbonate copolymer having an arylenesiloxane structure. During the decompression, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 27,000 Pa, 24,000 Pa, 20,000 Pa, 17,000 Pa, 14,000 Pa, 10,000 Pa, 6,000 Pa, 4,000 Pa, and 100 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured by GPC and found to be 81,885. The Tg of the copolymer was measured by DSC and found to be 75.1° C. The weight loss of the copolymer was measured by TG-DTA and found to be 380.6° C. for 1% weight loss. The amounts of low molecular weight compounds contained in the copolymer were quantified using GC, and the copolymer contained 415 ppm PhOH, 475 ppm BPA, 122 ppm DMDPS, and 44 ppm DPC.

[0185] (Reference example) According to the above-mentioned measurement method of the cyclic dimer, 19.99 g of the copolymer obtained in Example A-16 was dissolved in 121.22 g of dichloromethane, and 196 g of ethanol was dropped into the resin solution under stirring over 30 minutes. The precipitate was filtered off with NoA5 filter paper, and the filtrate was concentrated with an evaporator to obtain 0.652 g of oligomer component A. The precipitate was again dissolved in dichloromethane, and ethanol was dropped to separate the precipitate and oligomer component, and this operation was repeated twice (0.268 g of obtained oligomer component B, 0.177 g of obtained oligomer component C, and 18.99 g of copolymer reprecipitate, i.e., precipitate, were obtained). The obtained oligomer components A, B, and C were dissolved in dichloromethane to obtain a 1000 μg / mL solution, and analyzed by GC-Q-MS / FID. As a result, the amount of cyclic dimer in the copolymer of the reprecipitated product was 0.71 wt%. The Q value of the siloxane-containing polycarbonate copolymer obtained in Example A-16 was 117 (×10 -2 cm 3 / sec), and the Q value of the siloxane-containing polycarbonate copolymer reprecipitated product obtained in the reference example was 74 (× 10 -2 cm 3 / sec). It can be seen that the inclusion of a cyclic dimer increases the Q value, indicating high fluidity. [Table 2]

[0186] (Example A-17) 30.99g (0.07mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene, 13.01g (0.05mol) of diphenyldimethoxysilane, 5.28g (0.02mol) of diphenyl carbonate, and 15.0μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 190℃ and stirred for 30 minutes. After that, the phenol and methanol distilled from the reaction system were coagulated and removed in a cooling tube over a period of 1 hour and 10 minutes while carrying out an ester exchange reaction, and the temperature in the system was set to 260°C, the degree of vacuum was set to 2 hPa or less, and this was maintained for another 15 minutes to obtain a colorless and transparent polycarbonate copolymer having an arylenesiloxane structure. During the decompression, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 60,000 Pa, 40,000 Pa, 20,000 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000 Pa, 1,000 Pa, and 200 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured by GPC and found to be 115,683. The Tg of the copolymer was measured by DSC and found to be 110.9° C. The weight loss of the copolymer was measured by TG-DTA and found to be 351.4° C. for 1% weight loss.

[0187] (Example A-18) 24.71g (0.071mol) of 9,9-bis(4-hydroxyphenyl)fluorene, 18.00g (0.074mol) of diphenyldimethoxysilane, 0.831g (0.004mol) of diphenyl carbonate, and 15.0μmol / mol of cesium carbonate as a catalyst (catalyst amount is the relative molar amount to 9,9-bis(4-hydroxyphenyl)fluorene) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 190℃ and stirred for 15 minutes. After that, the phenol and methanol distilled from the reaction system were coagulated and removed in a cooling tube over a period of 1 hour and 20 minutes while carrying out an ester exchange reaction, and the temperature in the system was set to 260°C, the degree of vacuum was set to 2 hPa or less, and the system was maintained for another 1 hour and 30 minutes to obtain a polycarbonate copolymer having a yellowed transparent arylenesiloxane structure. During the decompression, the pressure was adjusted to change stepwise from atmospheric pressure to 80,000 Pa, 60,000 Pa, 40,000 Pa, 20,000 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000 Pa, and 200 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured by GPC and found to be 12,992. The Tg of the copolymer was measured by DSC and found to be 165.5° C. The weight loss of the copolymer was measured by TG-DTA and found to be 361.1° C. for 1% weight loss.

[0188] (Example A-19) 17.07g (0.04mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene, 12.06g (0.03mol) of 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 12.99g (0.05mol) of diphenyldimethoxysilane, 5.26g (0.02mol) of diphenyl carbonate, and 15.0μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar number to the sum of the molar numbers of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 200℃ and stirred for 30 minutes. After that, the phenol and methanol distilled from the reaction system were coagulated and removed in a cooling tube over a period of 1 hour and 20 minutes while carrying out an ester exchange reaction, and the temperature in the system was set to 260°C, the degree of vacuum was set to 2 hPa or less, and the system was maintained for another 1 hour and 20 minutes to obtain a browned transparent polycarbonate copolymer having an arylenesiloxane structure. During the decompression, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 80,000 Pa, 60,000 Pa, 40,000 Pa, 20,000 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000 Pa, 1,000 Pa, and 200 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured by GPC and found to be 23,272. The Tg of the copolymer was measured by DSC and found to be 140.4° C. The weight loss of the copolymer was measured by TG-DTA and found to be 349.4° C. for 1% weight loss.

[0189] (Example A-20) 24.71g (0.071mol) of 9,9-bis(4-hydroxyphenyl)fluorene, 1.80g (0.007mol) of dimethyldiphenoxysilane, 16.21g (0.066mol) of diphenyldimethoxysilane, 0.83g (0.004mol) of diphenyl carbonate, and 15.0μmol / mol of cesium carbonate (catalyst amount is the relative molar amount to 9,9-bis(4-hydroxyphenyl)fluorene) as a catalyst were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 210℃ and stirred for 25 minutes. After that, the phenol and methanol distilled from the reaction system were coagulated and removed in a cooling tube over a period of 1 hour and 25 minutes while carrying out an ester exchange reaction, and the temperature in the system was set to 260°C, the degree of vacuum was set to 2 hPa or less, and the reaction was maintained for another hour to obtain a polycarbonate copolymer having a yellowed transparent arylenesiloxane structure. During the decompression, the pressure was adjusted to change stepwise from atmospheric pressure to 80,000 Pa, 60,000 Pa, 40,000 Pa, 20,000 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000 Pa, and 200 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured by GPC and found to be 28,050. The Tg of the copolymer was measured by DSC and found to be 171.4° C. The weight loss of the copolymer was measured by TG-DTA and found to be 339.1° C. for 1% weight loss.

[0190] (Example A-21) 10.22g (0.07mol) of isosorbide, 17.60g (0.07mol) of diphenyldimethoxysilane, and 15.0μmol / mol of cesium carbonate (catalyst amount is the relative molar amount to isosorbide) as a catalyst were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 100℃ and stirred for 10 minutes. After that, over a period of 1 hour and 55 minutes, the methanol distilled from the reaction system was coagulated and removed using a cooling tube while the transesterification reaction was carried out, and the temperature inside the system was set to 200°C, the degree of vacuum was set to 2 hPa or less, and this was maintained for another 1 hour and 30 minutes to obtain a yellowed transparent arylenesiloxane. Note that during the vacuum reduction, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 90,000 Pa, 80,000 Pa, 70,000 Pa, 60,000 Pa, 50,000 Pa, 30,000 Pa, 10,000 Pa, 6,000 Pa, 2,000 Pa, and 200 Pa or less. The Mw of the arylene siloxane was measured using GPC and found to be 9,125. The Tg of the copolymer was measured using DSC and found to be 71.1° C. The weight loss of the arylene siloxane was measured using TG-DTA and found to be 256.2° C. for 1% weight loss.

[0191] (Example A-22) 17.50g (0.07mol) of bis(4-hydroxyphenyl)sulfone, 17.42g (0.07mol) of diphenyldimethoxysilane, and 30.0μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to bis(4-hydroxyphenyl)sulfone) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 220℃ and stirred for 25 minutes. After that, over a period of 1 hour and 15 minutes, the methanol distilled from the reaction system was coagulated and removed using a cooling tube while the ester exchange reaction was carried out, the temperature inside the system was set to 260°C, the degree of vacuum was set to 2 hPa or less, and this was maintained for a further 1 hour and 30 minutes to obtain a transparent arylenesiloxane that had turned slightly red. Note that during the vacuum reduction, the pressure was adjusted to change stepwise from atmospheric pressure to 80,000 Pa, 60,000 Pa, 40,000 Pa, 20,000 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000 Pa, 1,000 Pa, and 200 Pa or less. The Mw of the arylene siloxane was measured using GPC and found to be 12,806. The Tg of the arylene siloxane was measured using DSC and found to be 123.6° C. The weight loss of the arylene siloxane was measured using TG-DTA and found to be 384.7° C. for 1% weight loss.

[0192] (Example A-23) 31.00g (0.07mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene, 18.98g (0.08mol) of diphenyldimethoxysilane, and 15.0μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 190℃ and stirred for 30 minutes. After that, over a period of 1 hour and 10 minutes, the methanol distilled from the reaction system was coagulated and removed using a cooling tube while an ester exchange reaction was carried out, and the temperature inside the system was set to 260°C, the degree of vacuum was set to 2 hPa or less, and this was maintained for another 1 hour and 30 minutes to obtain a colorless and transparent arylenesiloxane. Note that during the vacuum reduction, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 60,000 Pa, 40,000 Pa, 20,000 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 3,000 Pa, 2,000 Pa, 1,000 Pa, and 200 Pa or less. The Mw of the arylene siloxane was measured using GPC and found to be 46,225. The Tg of the arylene siloxane was measured using DSC and found to be 97.4° C. The weight loss of the arylene siloxane was measured using TG-DTA and found to be 350.6° C. for 1% weight loss.

[0193] (Example A-24) 24.71g (0.07mol) of 9,9-bis(4-hydroxyphenyl)fluorene, 18.95g (0.08mol) of diphenyldimethoxysilane, and 15.0μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 9,9-bis(4-hydroxyphenyl)fluorene) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 190℃ and stirred for 15 minutes. After that, over a period of 1 hour and 30 minutes, the methanol distilled from the reaction system was coagulated and removed using a cooling tube while an ester exchange reaction was carried out, and the temperature inside the system was set to 260°C, the degree of vacuum was set to 2 hPa or less, and this was maintained for another 1 hour and 30 minutes to obtain a yellowed transparent arylenesiloxane. Note that during the vacuum reduction, the pressure was adjusted to change stepwise from atmospheric pressure to 80,000 Pa, 60,000 Pa, 40,000 Pa, 20,000 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 3,000 Pa, 2,000 Pa, and 200 Pa or less. The Mw of the arylene siloxane was measured using GPC and found to be 27,028. The Tg of the arylene siloxane was measured using DSC and found to be 169.7° C. The weight loss of the arylene siloxane was measured using TG-DTA and found to be 364.8° C. for 1% weight loss.

[0194] (Example A-25) 15.26g (0.07mol) of bis(4-hydroxyphenyl)sulfide, 17.42g (0.07mol) of diphenyldimethoxysilane, and 30.0μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to bis(4-hydroxyphenyl)sulfide) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 190℃ and stirred for 15 minutes. After that, over a period of 2 hours and 15 minutes, the methanol distilled from the reaction system was coagulated and removed using a cooling tube while an ester exchange reaction was carried out, and the temperature in the system was set to 260°C, the degree of vacuum was set to 2 hPa or less, and this was maintained for another hour and 20 minutes to obtain a colorless and transparent arylenesiloxane. Note that during the vacuum reduction, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 90,000 Pa, 80,000 Pa, 70,000 Pa, 60,000 Pa, 50,000 Pa, 40,000 Pa, 20,000 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000 Pa, and 200 Pa or less. The Mw of the arylene siloxane was measured using GPC and found to be 56,797. The Tg of the arylene siloxane was measured using DSC and found to be 73.2° C. The weight loss of the arylene siloxane was measured using TG-DTA and found to be 391.6° C. for 1% weight loss.

[0195] The results of the above-mentioned Examples A-15 to A-25 and Reference Example are shown in Table 3. [Table 3]

[0196] (Example A-26) 37.73g (0.07mol) of 9,9-bis[6-(2-hydroxyethoxy)naphthalene-2-yl]fluorene, 19.47g (0.07mol) of dimethyldiphenoxysilane, and 30.0μmol / mol of sodium hydrogen carbonate as a catalyst (the amount of catalyst is the relative molar amount to 9,9-bis(6-hydroxynaphthyl)fluorene) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 210℃ and stirred for 30 minutes. After that, over a period of 1 hour and 30 minutes, the phenol distilled from the reaction system was coagulated and removed using a cooling tube while an ester exchange reaction was carried out, the temperature in the system was set to 280°C, the degree of vacuum was set to 2 hPa or less, and the system was maintained for another 1 hour and 50 minutes to obtain a yellowed transparent arylenesiloxane. Note that during the vacuum reduction, the pressure was adjusted to change stepwise from atmospheric pressure to 30,000 Pa, 27,500 Pa, 25,000 Pa, 22,500 Pa, 20,000 Pa, 17,500 Pa, 15,000 Pa, 12,500 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000, 1,000, and 200 Pa or less. The Mw of the arylene siloxane was measured using GPC and found to be 39,353. The Tg of the arylene siloxane was measured using DSC and found to be 138° C. The weight loss of the arylene siloxane was measured using TG-DTA and found to be 369.3° C. for 1% weight loss.

[0197] (Example A-27) 61.04g (0.33mol) of 4,4'-dihydroxy-biphenyl, 89.64g (0.37mol) of dimethyldiphenoxysilane, and 3.0μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 4,4'-dihydroxy-biphenyl) were placed in a 200ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 220℃ and stirred for 60 minutes. After that, the phenol distilled from the reaction system was condensed and removed in a cooling tube for 1 hour. The transesterification reaction was carried out, the system was kept at 260°C, the degree of vacuum was 1 hPa or less, and the reaction was maintained for another 2 hours to obtain a colorless and transparent arylenesiloxane. Note that the pressure was adjusted so that it changed stepwise from atmospheric pressure to 27,000 Pa, 24,000 Pa, 20,000 Pa, 17,000 Pa, 14,000 Pa, 10,000 Pa, 6,000 Pa, 4,000 Pa, and 100 Pa or less. The Mw of the arylene siloxane was measured using GPC and found to be 46,000. The Tg of the arylene siloxane was measured using DSC and found to be 70.4° C. The weight loss of the arylene siloxane was measured using TG-DTA and found to be 378° C. for 1% weight loss.

[0198] (Example A-28) 79.71g (0.43mol) of 4,4'-dihydroxy-biphenyl, 107.42g (0.44mol) of diphenyldimethoxysilane, and 3.0μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 4,4'-dihydroxy-biphenyl) were placed in a 200ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 220℃ and stirred for 30 minutes. After that, over a period of 2 hours, the methanol distilled from the reaction system was coagulated and removed using a cooling tube while the transesterification reaction was carried out, and the temperature inside the system was set to 260°C, the degree of vacuum was set to 1 hPa or less, and this was maintained for another 2 hours to obtain a colorless and transparent arylenesiloxane. Note that during the decompression, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 90,000 Pa, 80,000 Pa, 70,000 Pa, 60,000 Pa, 50,000 Pa, 40,000 Pa, 20,000 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000 Pa, and 200 Pa or less. The Mw of the arylene siloxane was measured using GPC and found to be 17,000. The Tg of the arylene siloxane was measured using DSC and found to be 110° C. The weight loss of the arylene siloxane was measured using TG-DTA and found to be 345° C. for 1% weight loss.

[0199] (Example A-29) 39.06g (0.21mol) of 4,4'-dihydroxy-biphenyl, 38.58g (0.16mol) of dimethyldiphenoxysilane, 15.60g (0.07mol) of diphenyl carbonate, and 15.0μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 4,4'-dihydroxy-biphenyl) were placed in a 300ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 220℃ and stirred for 20 minutes. After that, the phenol distilled from the reaction system was coagulated and removed in a cooling tube over a period of 1 hour and 30 minutes while carrying out an ester exchange reaction, and the temperature in the system was set to 260°C, the degree of vacuum was set to 1 hPa or less, and the reaction was held for another 10 minutes to obtain a colorless and transparent polycarbonate copolymer having an arylenesiloxane structure. During the decompression, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 30,000 Pa, 25,000 Pa, 20,000 Pa, 15,000 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000 Pa, 1,000 Pa, and 100 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured using GPC and found to be 33,710. The Tg of the copolymer was measured by DSC and found to be 78.8° C. The weight loss of the copolymer was measured by TG-DTA and found to be 357° C. for 1% weight loss.

[0200] (Example A-30) 39.06g (0.21mol) of 4,4'-dihydroxy-biphenyl, 35.00g (0.14mol) of diphenyldimethoxysilane, 15.60g (0.07mol) of diphenyl carbonate, and 15.0μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 4,4'-dihydroxy-biphenyl) were placed in a 300ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 220℃ and stirred for 20 minutes. After that, over 1 hour and 30 minutes, the methanol distilled from the reaction system was condensed and removed using a cooling tube while the ester exchange reaction was carried out, the temperature in the system was set to 260°C, the degree of vacuum was set to 1 hPa or less, and the system was maintained for another 10 minutes to obtain a colorless and transparent polycarbonate copolymer having an arylenesiloxane structure. During the decompression, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 30,000 Pa, 25,000 Pa, 20,000 Pa, 15,000 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000 Pa, 1,000 Pa, and 100 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured using GPC and found to be 11,845. The Tg of the copolymer was measured by DSC and found to be 120° C. The weight loss of the copolymer was measured by TG-DTA and found to be 363° C. for 1% weight loss.

[0201] (Example A-31) 26.18g (0.07mol) of 2,2'-bishydroxyethoxy-1,1'-binaphthyl, 19.82g (0.08mol) of dimethyldiphenoxysilane, and 30μmol / mol of sodium hydrogen carbonate as a catalyst (the amount of catalyst is the relative molar amount to 2,2'-bishydroxyethoxy-1,1'-binaphthyl) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 210℃ and stirred for 35 minutes. After that, over the course of 1 hour and 30 minutes, the phenol distilled from the reaction system was coagulated and removed using a cooling tube while an ester exchange reaction was carried out, the temperature inside the system was set to 260°C, the degree of vacuum was set to 1 hPa or less, and this was maintained for another 1 hour and 30 minutes to obtain a colorless and transparent arylenesiloxane. Note that during the decompression, the pressure was adjusted to change stepwise from atmospheric pressure to 27,500 Pa, 25,000 Pa, 22,500 Pa, 20,000 Pa, 17,500 Pa, 15,000 Pa, 12,500 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000 Pa, 1,000 Pa, and 100 Pa or less. The Mw of the arylenesiloxane was measured using GPC and found to be 19,975. The Tg of the arylene siloxane was measured using DSC and found to be 54° C. The weight loss of the arylene siloxane was measured using TG-DTA and found to be 296° C. for 1% weight loss.

[0202] (Example A-32) 26.18g (0.07mol) of 2,2'-bishydroxyethoxy-1,1'-binaphthyl, 5.40g (0.03mol) of diphenyl carbonate, 12.65g (0.05mol) of dimethyldiphenoxysilane, and 30μmol / mol of sodium hydrogen carbonate as a catalyst (the amount of catalyst is the relative molar number to 2,2'-bishydroxyethoxy-1,1'-binaphthyl) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 220℃ and stirred for 1 hour. After that, the phenol distilled from the reaction system was coagulated and removed in a cooling tube over a period of 1 hour and 10 minutes while carrying out an ester exchange reaction, and the temperature in the system was set to 260°C, the degree of vacuum was set to 1 hPa or less, and the reaction was maintained for another 1 hour and 20 minutes to obtain a colorless and transparent polycarbonate copolymer having an arylenesiloxane structure. During the decompression, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 27,500 Pa, 25,000 Pa, 22,500 Pa, 20,000 Pa, 17,500 Pa, 15,000 Pa, 12,500 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000 Pa, 1,000 Pa, and 100 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured using GPC and found to be 32,178. The Tg of the copolymer was measured by DSC and found to be 74° C. The weight loss of the copolymer was measured by TG-DTA and found to be 317° C. for 1% weight loss.

[0203] (Example A-33) 10.22g (0.07mol) of isosorbide, 5.20g (0.02mol) of diphenyl carbonate, 12.86g (0.05mol) of dimethyldiphenoxysilane, and 15.0μmol / mol of cesium carbonate (catalyst amount is the relative molar amount to isosorbide) as a catalyst were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 200℃ and stirred for 30 minutes. After that, the phenol distilled from the reaction system was coagulated and removed in a cooling tube over a period of 1 hour and 20 minutes while carrying out an ester exchange reaction, and the temperature in the system was set to 260°C, the degree of vacuum was set to 2 hPa or less, and the reaction was maintained for another 1 hour and 30 minutes to obtain a polycarbonate copolymer having a yellowed transparent arylenesiloxane structure. During the decompression, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 30,000 Pa, 25,000 Pa, 20,000 Pa, 15,000 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000 Pa, 1,000 Pa, and 200 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured by GPC and found to be 39,378. The Tg of the copolymer was measured by DSC and found to be 55° C. The weight loss of the copolymer was measured by TG-DTA and found to be 242° C. for 1% weight loss.

[0204] (Example A-34) 21.28g (0.07mol) of 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, 19.82g (0.08mol) of dimethyldiphenoxysilane, and 30.0μmol / mol of sodium hydrogen carbonate as a catalyst (the amount of catalyst is the relative molar amount to 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 210℃ and stirred for 30 minutes. After that, over a period of 1 hour and 50 minutes, the phenol distilled from the reaction system was coagulated and removed using a cooling tube while an ester exchange reaction was carried out, and the temperature inside the system was set to 260°C, the degree of vacuum was set to 2 hPa or less, and this was maintained for another hour to obtain a colorless and transparent arylenesiloxane. Note that during the vacuum reduction, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 30,000 Pa, 25,000 Pa, 20,000 Pa, 17,500 Pa, 15,000 Pa, 12,500 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000 Pa, 1,000 Pa, and 200 Pa or less. The Mw of the arylene siloxane was measured using GPC and found to be 15,708. The Tg of the arylene siloxane was measured using DSC and found to be 51° C. The weight loss of the arylene siloxane was measured using TG-DTA and found to be 236° C. for 1% weight loss.

[0205] (Example A-35) 21.28g (0.07mol) of 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, 5.20g (0.02mol) of diphenyl carbonate, 12.86g (0.05mol) of dimethyldiphenoxysilane, and 30.0μmol / mol of sodium hydrogen carbonate as a catalyst (the amount of catalyst is the relative molar number to 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 210℃ and stirred for 30 minutes. After that, the phenol distilled from the reaction system was coagulated and removed in a cooling tube over a period of 1 hour and 30 minutes while carrying out an ester exchange reaction, and the temperature in the system was set to 260°C, the degree of vacuum was set to 2 hPa or less, and the reaction was maintained for another hour to obtain a polycarbonate copolymer having a transparent arylenesiloxane structure. During the decompression, the pressure was adjusted so that it changed stepwise from atmospheric pressure to 30,000 Pa, 25,000 Pa, 20,000 Pa, 17,500 Pa, 15,000 Pa, 12,500 Pa, 10,000 Pa, 8,000 Pa, 6,000 Pa, 4,000 Pa, 2,000 Pa, 1,000 Pa, and 200 Pa or less. The Mw of the siloxane-containing polycarbonate copolymer was measured by GPC and found to be 68,693. The Tg of the copolymer was measured by DSC and found to be 63° C. The weight loss of the copolymer was measured by TG-DTA and found to be 252° C. for 1% weight loss.

[0206] (Comparative example A-1) 17.51g (0.08mmol) of 2,2-bis(4-hydroxyphenyl)propane, 20.93g (0.09mol) of dimethyldiphenoxysilane, and 7μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 30 minutes. Thereafter, an ester exchange reaction was carried out over a period of one hour while condensing and removing the phenol distilling out of the reaction system using a cooling tube. The temperature inside the system was then adjusted to 260°C and the reduced pressure to 4 hPa or less, and this was maintained for a further two hours to obtain a colorless and transparent polyarylenesiloxane. The Mw of the polyarylenesiloxane was measured using GPC and found to be 63,257. The Tg of the copolymer was measured by DSC and found to be 54°C.

[0207] (Comparative example A-2) The Mw of polycarbonate (Mitsubishi Gas Chemical Company, Iupilon S-3000) was measured by GPC and found to be 51,252. The Tg of the polycarbonate was measured using DSC and found to be 149°C.

[0208] (Comparative example A-3) Comparative Example A-3 was a polycarbonate resin using Mitsubishi Gas Chemical's Iupizeta EP6000, i.e., BPEF (9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene) as a diol compound. The polycarbonate resin of Comparative Example A-3 had an Mw of 30,000, a Q value of 97×10-2cm3 / sec, a Tg of 142°C, a refractive index (nd) of 1.638, and an Abbe number (vd) of 23.5. Compared with Comparative Example A-3, it was confirmed that Examples A-17, 19, and 23, which used the same diol compound, were able to improve the fluidity (enlarge the Q value) without significantly changing the optical properties.

[0209] The results of the above-mentioned Examples A-26 to A-35 and Comparative Examples A-1 and A-2 are shown in Table 4. [Table 4]

[0210] (Example A-36) 10 g of the polycarbonate copolymer obtained in Example A-3 and 190 g of polycarbonate (manufactured by Mitsubishi Gas Chemical Company, Iupilon S-3000) were kneaded and extruded at 280° C. using a kneading extruder (manufactured by Toyo Seiki Seisakusho, Labo Plastomill 4C150). The Q value of the obtained composition was 11.9 (×10 -2 cm 3 The composition was dried in a dryer at 110°C for 12 hours, and then a test piece for the Charpy impact test was molded in an injection molding machine ("C-Mobile" manufactured by Shinko Selvic) at a resin temperature of 300°C and a mold temperature of 90°C. A notched Charpy impact test was carried out in accordance with JIS-K7111, resulting in a value of 60.9 kJ / m 2 It was.

[0211] (Example A-37) 10 g of the polycarbonate copolymer obtained in Example A-4 and 190 g of polycarbonate (manufactured by Mitsubishi Gas Chemical Company, Iupilon S-3000) were kneaded and extruded at 280° C. using a kneading extruder (manufactured by Toyo Seiki Seisakusho, Labo Plastomill 4C150). The Q value of the obtained composition was 14.1 (×10 -2 cm 3 The composition was dried in a dryer at 110°C for 12 hours, and then a test piece for the Charpy impact test was molded in an injection molding machine ("C-Mobile" manufactured by Shinko Selvic) at a resin temperature of 300°C and a mold temperature of 90°C. A notched Charpy impact test was carried out in accordance with JIS-K7111, resulting in a value of 65.8 kJ / m 2 It was.

[0212] (Example A-38) 150g of the polycarbonate copolymer obtained in Example A-16 and 1850g of polycarbonate (Mitsubishi Gas Chemical, Iupilon E-2000) were mixed at a resin temperature of 280°C using a kneading extrusion injection molding machine (high-speed injection molding machine Sodick TR100EH), and then injection molded under conditions of a mold temperature of 80°C and a holding pressure of 90MPa to form a test piece for Charpy impact testing. A notched Charpy impact test was carried out in accordance with JIS-K7111, and the result was 70.1kJ / m 2The Q value of the obtained composition was 5.5 (× 10 -2 cm 3 / sec). (Example A-39) 300g of the polycarbonate copolymer obtained in Example A-16 and 1700g of polycarbonate (Mitsubishi Gas Chemical, Iupilon E-2000) were mixed at a resin temperature of 280°C using a kneading extrusion injection molding machine (high-speed injection molding machine Sodick TR100EH), and then injection molded under conditions of a mold temperature of 80°C and a holding pressure of 90MPa to form a test piece for Charpy impact testing. A notched Charpy impact test was carried out in accordance with JIS-K7111, and the result was 76.7kJ / m 2 The Q value of the obtained composition was 8.1 (× 10 -2 cm 3 / sec). (Example A-40) 600 g of the polycarbonate copolymer obtained in Example A-16 and 1,400 g of polycarbonate (Mitsubishi Gas Chemical, Iupilon E-2000) were mixed at a resin temperature of 280°C using a kneading extrusion injection molding machine (high-speed injection molding machine Sodick TR100EH), and then injection molded under conditions of a mold temperature of 80°C and a holding pressure of 90 MPa to form a test piece for Charpy impact testing. A notched Charpy impact test was carried out in accordance with JIS-K7111, and the result was 6.9 kJ / m 2 The Q value of the obtained composition was 17.2 (× 10 -2 cm 3 / sec).

[0213] (Comparative example A-4) The Q value of polycarbonate (Mitsubishi Gas Chemical, Iupilon S-3000) is 8.0 (× 10 -2 cm 3 In addition, the polycarbonate was dried in a dryer at 110°C for 12 hours, and then a test piece for the Charpy impact test was molded using an injection molding machine ("C-Mobile" manufactured by Shinko Selvic) at a resin temperature of 300°C and a mold temperature of 90°C. A notched Charpy impact test was then carried out in accordance with JIS-K7111, resulting in a value of 62.9kJ / m. 2It was.

[0214] (Comparative example A-5) 2000g of polycarbonate (Mitsubishi Gas Chemical, Iupilon E-2000) was mixed at a resin temperature of 300°C using a mixing extrusion injection molding machine (high-speed injection molding machine Sodick TR100EH), and then injection molded at a mold temperature of 80°C and a holding pressure of 90MPa to form test pieces for the Charpy impact test. A notched Charpy impact test was performed in accordance with JIS-K7111, resulting in an impact strength of 72.7kJ / m 2 The Q value of the obtained composition was 2.8 (× 10 -2 cm 3 / sec).

[0215] The results of Examples A-36 to A-40 and Comparative Examples A-4 and A-5 are shown in Table 5 below. [Table 5]

[0216] [Examples of polysiloxane compounds] Examples of polysiloxane compounds will now be described. <Polystyrene equivalent weight average molecular weight (Mw)> A calibration curve was prepared using GPC (gel permeation chromatography) with chloroform as the developing solvent and standard polystyrene of known molecular weight (molecular weight distribution = 1). Calculations were made from the GPC retention time based on this calibration curve. <Glass transition temperature (Tg)> It was measured by a differential scanning calorimeter (DSC). It was determined from the intersection of a straight line extending from the low-temperature baseline to the high-temperature side of the DSC curve and a tangent drawn at the point where the gradient of the curve of the step-like change in the glass transition is maximum.

[0217] (Synthesis Example 2) Synthesis of dimethyldiphenoxysilane 7.5 g (20.2 mmol, Si molar amount: 101.0 mmol) of decamethylcyclopentasiloxane, 21.6 g (101.0 mmol) of diphenyl carbonate, and 33 mg (0.1 mmol) of cesium carbonate as a catalyst were stirred at 200° C. for 60 minutes under a nitrogen atmosphere. Subsequently, the reaction mixture was cooled to 40° C., and then vacuum distilled at a reduced pressure of 4 hPa and 150° C. to obtain 23.7 g of a colorless oily component. The obtained oily component 1 Analysis by H-NMR confirmed that it was dimethyldiphenoxysilane. ( 1 H-NMR (CDCl3, 500 MHz, δ; ppm) = 0.378 (s; 6H), 6.942, 6.944 (d; 4H), 6.959, 6.961, 6.995 (t; 2H), 7.230, 7.245, 7.257 (t; 4H)). The molar yield was 96.0%.

[0218] (Example B-1) 30.03g (0.13mol) of 2,2-bis(4-hydroxyphenyl)propane, 33.50g (0.14mol) of dimethyldiphenoxysilane, and 11μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 30 minutes. Thereafter, over a period of 1.5 hours, an ester exchange reaction was carried out while condensing and removing the phenol distilling out of the reaction system using a cooling tube. The temperature inside the system was then adjusted to 240°C and the reduced pressure to 4 hPa or less, and this was maintained for a further 1.5 hours to obtain a colorless and transparent polyarylenesiloxane. The Mw of the polyarylenesiloxane was measured using GPC and found to be 26,699.

[0219] (Example B-2) 30.03g (0.13mol) of 2,2-bis(4-hydroxyphenyl)propane, 34.40g (0.14mol) of dimethyldiphenoxysilane, and 11μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 30 minutes. Thereafter, over a period of 1.5 hours, an ester exchange reaction was carried out while condensing and removing the phenol distilling out of the reaction system using a cooling tube. The temperature inside the system was then adjusted to 240°C and the reduced pressure to 4 hPa or less, and this was maintained for a further 1.5 hours to obtain a colorless and transparent polyarylenesiloxane. The Mw of the polyarylenesiloxane was measured using GPC and found to be 33,521.

[0220] (Example B-3) 30.05g (0.13mol) of 2,2-bis(4-hydroxyphenyl)propane, 34.69g (0.14mol) of dimethyldiphenoxysilane, and 11μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 30 minutes. Thereafter, over a period of 1.5 hours, an ester exchange reaction was carried out while condensing and removing the phenol distilling out of the reaction system using a cooling tube. The temperature inside the system was then adjusted to 240°C and the reduced pressure to 4 hPa or less, and this was maintained for a further 1.5 hours to obtain a colorless and transparent polyarylenesiloxane. The Mw of the polyarylenesiloxane was measured using GPC and found to be 30,603.

[0221] (Example B-4) 30.03g (0.13mol) of 2,2-bis(4-hydroxyphenyl)propane, 35.10g (0.14mol) of dimethyldiphenoxysilane, and 11μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 30 minutes. Thereafter, over a period of 1.5 hours, an ester exchange reaction was carried out while condensing and removing the phenol distilling out of the reaction system using a cooling tube. The temperature inside the system was then adjusted to 240°C and the reduced pressure to 4 hPa or less, and this was maintained for a further 1.5 hours to obtain a colorless and transparent polyarylenesiloxane. The Mw of the polyarylenesiloxane was measured using GPC and found to be 36,940.

[0222] (Example B-5) 30.08g (0.13mol) of 2,2-bis(4-hydroxyphenyl)propane, 36.00g (0.15mol) of dimethyldiphenoxysilane, and 11μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 30 minutes. Thereafter, over a period of 1.5 hours, an ester exchange reaction was carried out while condensing and removing the phenol distilling out of the reaction system using a cooling tube. The temperature inside the system was then adjusted to 240°C and the reduced pressure to 4 hPa or less, and this was maintained for a further 1.5 hours to obtain a colorless and transparent polyarylenesiloxane. The Mw of the polyarylenesiloxane was measured using GPC and found to be 39,994. The Tg of the polyarylenesiloxane was measured using DSC and found to be 49°C.

[0223] (Example B-6) 30.03g (0.13mol) of 2,2-bis(4-hydroxyphenyl)propane, 37.38g (0.15mol) of dimethyldiphenoxysilane, and 11μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 30 minutes. Thereafter, over a period of 1.5 hours, an ester exchange reaction was carried out while condensing and removing the phenol distilling out of the reaction system using a cooling tube. The temperature inside the system was then adjusted to 240°C and the reduced pressure to 4 hPa or less, and this was maintained for a further 1.5 hours to obtain a colorless and transparent polyarylenesiloxane. The Mw of the polyarylenesiloxane was measured using GPC and found to be 34,196.

[0224] (Example B-7) 17.51g (0.077mol) of 2,2-bis(4-hydroxyphenyl)propane, 20.93g (0.086mol) of dimethyldiphenoxysilane, and 7μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 30 minutes. Thereafter, an ester exchange reaction was carried out over a period of 1 hour while condensing and removing the phenol distilling out of the reaction system using a cooling tube. The temperature inside the system was then adjusted to 260°C and the reduced pressure to 4 hPa or less, and this was maintained for a further 1.5 hours to obtain a colorless and transparent polyarylenesiloxane. The Mw of the polyarylenesiloxane was measured using GPC and found to be 63,257. The Tg of the polyarylenesiloxane was measured using DSC and found to be 54°C.

[0225] (Synthesis Example 3) 14.9g (0.19mol) of octaphenylcyclotetrasiloxane represented by the following formula (3), 16.1g (0.08mol) of diphenyl carbonate, and 33mg (0.1mmol) of cesium carbonate as a catalyst were stirred at 200°C for 10 minutes under a nitrogen atmosphere. After cooling to room temperature, 20g of heptane was added to the solidified reaction mixture, and the mixture was heated to 90°C and filtered while hot. The obtained filtrate was left at room temperature for 3 days to precipitate white crystals. The mixture was filtered by adding 10g of heptane cooled to 5°C, and the crystals on the filter paper obtained by filtration were taken out and dried at 40°C and a reduced pressure of 1hPa for 45 hours, yielding 24.1g of white powder. The obtained powder was 1 Analysis by H-NMR confirmed that it was diphenyldiphenoxysilane. 1 H-NMR (CDCl3, 500 MHz, δ; ppm) = 6.915, 6.927, 6.939, 6.952, 6.965 (p; 6H), 7.142, 7.155, 7.169 (t; 4H), 7.354, 7.366, 7.379 (t; 4H), 7.425, 7.437, 7.449 (t; 2H), 7.750, 7.762 (d; 4H). The molar yield was 81.1%. [ka]

[0226] (Example B-8) 11.75g ​​(0.052mol) of 2,2-bis(4-hydroxyphenyl)propane, 20.25g (0.055mol) of diphenyldiphenoxysilane, and 20μmol / mol of cesium carbonate as a catalyst (the amount of catalyst is the relative molar amount to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 30 minutes. Thereafter, an ester exchange reaction was carried out over a period of 1 hour while condensing and removing the phenol distilling out of the reaction system using a cooling tube. The temperature inside the system was then adjusted to 260°C and the reduced pressure to 4 hPa or less, and this was maintained for a further 1.5 hours to obtain a colorless and transparent polyarylenesiloxane. The Mw of the polyarylenesiloxane was measured using GPC and found to be 24,482. The Tg of the polyarylenesiloxane was measured using DSC and found to be 89°C.

[0227] (Comparative example B-1) 20.00g (0.088mol) of 2,2-bis(4-hydroxyphenyl)propane and 23.62g (0.097mol) of dimethyldiphenoxysilane were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180°C and stirred for 30 minutes. Thereafter, the temperature inside the system was set to 240°C and the degree of vacuum was set to 4 hPa (400 Pa) or less to attempt an ester exchange reaction, but the raw materials were distilled off and the reaction did not proceed.

[0228] (Comparative example B-2) 21.28g (0.093mol) of 2,2-bis(4-hydroxyphenyl)propane, 25.12g (0.10mol) of dimethyldiphenoxysilane, and 11μmol / mol of cesium carbonate as a catalyst (catalyst amount is the relative molar amount to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 30 minutes. Thereafter, the temperature inside the system was raised to 240° C. under normal pressure over a period of 1.5 hours, and maintained at that temperature for an additional 1.5 hours to obtain a colorless and transparent polyarylenesiloxane. The Mw of the polyarylenesiloxane was measured using GPC and found to be 1,547.

[0229] (Comparative example B-3) 29.96g (0.13mol) of 2,2-bis(4-hydroxyphenyl)propane, 36.10g (0.15mol) of dimethyldiphenoxysilane, and 16600μmol / mol of cesium carbonate as a catalyst (or 16.6mmol / mol: the amount of catalyst is the relative molar amount to 2,2-bis(4-hydroxyphenyl)propane) were placed in a 100ml four-neck flask equipped with a stirrer, and the system was replaced with a nitrogen atmosphere. The raw materials were heated and melted at 180℃ and stirred for 30 minutes. Thereafter, an ester exchange reaction was carried out over a period of 1 hour while condensing and removing the phenol distilling out of the reaction system using a cooling tube. The temperature inside the system was then adjusted to 240°C and the reduced pressure to 4 hPa or less, and this was maintained for a further 1.5 hours to obtain a colorless and transparent polyarylenesiloxane. The Mw of the colorless, transparent polyarylenesiloxane was measured by GPC and found to be 886.

[0230] (Comparative example B-4) 30.75 g (0.14 mol) of 2,2-bis(4-hydroxyphenyl)propane and 36.90 g (0.15 mol) of dimethyldiphenoxysilane were placed in a 100 ml four-neck flask equipped with a stirrer. Immediately afterwards, the temperature inside the system was reduced to 240°C and the pressure reduced to 4 hPa (400 Pa) or less to attempt an ester exchange reaction, but the raw materials were distilled off and the reaction did not proceed.

[0231] The results of each of the examples and comparative examples are shown in Table 6 below. [Table 6]

Claims

1. In the presence of a transesterification catalyst, a diaryloxysilane compound containing at least one of a dialkyldiaryloxysilane, a diaryldiaryloxysilane, and a monoalkylmonoaryldiaryloxysilane; a dialkoxysilane compound containing at least one of a dialkyldialkoxysilane, a diaryldialkoxysilane, and a monoalkylmonoaryldialkoxysilane; A silicon compound containing at least one of a cyclic siloxane compound and a linear siloxane compound; A silane-based compound selected from the group consisting of A carbonate compound; The method includes a polymerization step of polymerizing an aromatic diol compound or an alicyclic diol compound with a diol compound, A method for producing a polycarbonate copolymer having a siloxane structural unit represented by any one of formulas (1-1) to (1-4) and a polycarbonate structural unit represented by any one of formulas (3-1) to (3-4), comprising the steps of: (a) removing alcohol derived from the carbonate compound under reduced pressure in a molten state in a polymerization step; 【Chemistry 1】 (In formulas (1-1) to (1-4), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 and R 30 ~R 33 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Z 1 and Z 2 each independently represents an alkylene group having 1 to 5 carbon atoms which may have a substituent, J 1 each independently represents an integer of 0 to 5, K 1 each independently represents an integer of 0 to 5, A 1 and A 2 each independently represents -O- or -CH-; L 1 and L 2 each independently represents an integer of 0 to 3, X is a single bond or any one of the structural formulas represented by the following formula (2): 【Chemistry 2】 (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less. 【Chemistry 3】 (In formulas (3-1) to (3-4), R 13 ~R 20 and R 40 ~R 51 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Z 3 and Z 4 each independently represents an alkylene group having 1 to 5 carbon atoms which may have a substituent, J 2 each independently represents an integer of 0 to 5, K 2 each independently represents an integer of 0 to 5, A 1 and A 2 each independently represents -O- or -CH-; L 1 and L 2 each independently represents an integer of 0 to 3, Y is a single bond or any one of the structural formulas represented by formula (4), 【Chemistry 4】 (In the formula, R 21 , and R 22 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 21 and R 22 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, c and d each independently represent 0 or an integer of 1 to 5000. The polycarbonate copolymer comprises at least The X represents a siloxane structural unit that represents a fluorene ring structure formed by R 11 and R 12 bonding to each other, or Y has a polycarbonate structural unit that represents a fluorene ring structure formed by R 21 and R 22 bonding to each other; A method for producing a polycarbonate copolymer.

2. Z 1 ~Z 4 each independently represents an alkylene group having 1 to 3 carbon atoms which may have a substituent, J 1 and J. 2 each independently represents an integer of 0 to 2, K 1 and K. 2 each independently represents an integer of 0 to 2, A method for producing the polycarbonate copolymer according to claim 1.

3. The X is R 11 and R 12 a siloxane constitutional unit which represents a fluorene ring structure formed by bonding together, and 21 and R 22 3. The method for producing a polycarbonate copolymer according to claim 1 or 2, comprising a polycarbonate structural unit having a fluorene ring structure formed by bonding together.

4. In the presence of a transesterification catalyst, a diaryloxysilane compound containing at least one of a dialkyldiaryloxysilane, a diaryldiaryloxysilane, and a monoalkylmonoaryldiaryloxysilane; a dialkoxysilane compound containing at least one of a dialkyldialkoxysilane, a diaryldialkoxysilane, and a monoalkylmonoaryldialkoxysilane; A silicon compound containing at least one of a cyclic siloxane compound and a linear siloxane compound; A silane-based compound selected from the group consisting of The method includes a polymerization step of polymerizing a carbonate compound and a diol compound including an aromatic diol compound or an alicyclic diol compound, A method for producing a polycarbonate copolymer having a siloxane structural unit represented by formula (1) and a polycarbonate structural unit represented by formula (3), comprising the steps of: in a polymerization step, removing alcohol derived from the carbonate compound under reduced pressure in a molten state; 【Chemistry 5】 (In formula (1), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, X is any one of the structural formulas represented by the following formula (2): 【Chemistry 6】 (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less. 【Chemistry 7】 (In the formula, R 13 ~R 20 Each independently represents hydrogen, halogen, alkoxy, or a substituent. an alkyl group having 1 to 20 carbon atoms which may have a substituent; an alkenyl group having 2 to 20 carbon atoms which may have a substituent; a group, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Y is any one of the structural formulas represented by formula (4), 【Chemistry 8】 (In the formula, R 21 , and R 22 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 21 and R 22 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, c and d each independently represent 0 or an integer of 1 to 5000. The polycarbonate copolymer comprises at least The X represents a siloxane structural unit that represents a fluorene ring structure formed by R 11 and R 12 bonding to each other, or A method for producing a polycarbonate copolymer, wherein Y has a polycarbonate structural unit that represents a fluorene ring structure formed by R 21 and R 22 being bonded to each other.

5. The method for producing a polycarbonate copolymer according to any one of claims 1 to 4, wherein the transesterification catalyst contains an alkali metal compound and / or an alkaline earth metal.

6. The method for producing a polycarbonate copolymer according to claim 5 , wherein the alkali metal compound and / or alkaline earth metal compound includes a carbonate.

7. The method for producing a polycarbonate copolymer according to any one of claims 1 to 6, wherein the weight average molecular weight of the polycarbonate copolymer is 10,000 to 300,000.

8. In the polymerization step, the amount of the transesterification catalyst relative to the diol compound is 1.0×10 in molar ratio. -7 ~1.0 x 10 -2 The method for producing the polycarbonate copolymer according to any one of claims 1 to 7,

9. The method for producing a polycarbonate copolymer according to any one of claims 1 to 8, wherein the reaction temperature in the polymerization step is in the range of 150°C or higher and 300°C or lower.

10. The method for producing a polycarbonate copolymer according to any one of claims 1 to 9, further comprising a depressurization step of gradually reducing the reaction pressure to 400 Pa or less in the polymerization step.

11. The method for producing a polycarbonate copolymer according to any one of claims 1 to 10, wherein in the polymerization step, the carbonate compound and the diol compound are polymerized under a pressure of 400 Pa or less.

12. The method for producing a polycarbonate copolymer according to any one of claims 1 to 11, wherein no solvent is used in the polymerization step.

13. The method for producing a polycarbonate copolymer according to any one of claims 1 to 12, wherein a ratio of a total mole number of the carbonate compound and the diaryloxysilane compound to a mole number of the diol compound used in the polymerization step is 0.9 or more and 1.2 or less.

14. The method for producing a polycarbonate copolymer according to any one of claims 1 to 13, wherein the number of moles of the siloxane constituent unit in the polycarbonate copolymer is 1 to 1000, and the number of moles of the polycarbonate constituent unit is 1 to 1000.

15. The method for producing a polycarbonate copolymer according to any one of claims 1 to 14, wherein a molar ratio of the siloxane constituent units to the polycarbonate constituent units is 0.01:99.99 to 99.99:0.

01.

16. The Q value of the polycarbonate copolymer measured under conditions of 280° C. and 160 kgf is 8 (×10 -2 cm 3 s -1 16. The method for producing a polycarbonate copolymer according to any one of claims 1 to 15, wherein the copolymer is at least 100% by weight.

17. A polycarbonate copolymer having a siloxane constituent unit represented by any one of formulas (1-1) to (1-4) and a polycarbonate constituent unit represented by any one of formulas (3-1) to (3-4), and containing 30% by weight or less of a low molecular weight compound having a weight average molecular weight of 1,000 or less, 【Chemistry 9】 (In formulas (1-1) to (1-4), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 and R 3 ~R 33 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Z 1 and Z 2 each independently represents an alkylene group having 1 to 5 carbon atoms which may have a substituent, J 1 each independently represents an integer of 0 to 5, K 1 each independently represents an integer of 0 to 5, A 1 and A 2 each independently represents -O- or -CH-; L 1 and L 2 each independently represents an integer of 0 to 3, X is a single bond or any one of the structural formulas represented by the following formula (2): 【Chemistry 10】 (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less. 【Chemistry 11】 (In formulas (3-1) to (3-4), R 13 ~R 20 and R 40 ~R 51 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Z 3 and Z 4 each independently represents an alkylene group having 1 to 5 carbon atoms which may have a substituent, J 2 each independently represents an integer of 0 to 5, K 2 each independently represents an integer of 0 to 5, A 1 and A 2 each independently represents -O- or -CH-; L 1 and L 2 each independently represents an integer of 0 to 3, Y is a single bond or any one of the structural formulas represented by formula (4), 【Chemistry 12】 (In the formula, R 21 , and R 22 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 21 and R 22 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, c and d each independently represent 0 or an integer of 1 to 5000. The polycarbonate copolymer comprises at least the X has a siloxane structural unit that represents a fluorene ring structure formed by R 11 and R 12 bonding to each other, or the Y has a polycarbonate structural unit that represents a fluorene ring structure formed by R 21 and R 22 bonding to each other; Polycarbonate copolymer.

18. Z 1 ~Z 4 each independently represents an alkylene group having 1 to 3 carbon atoms which may have a substituent, J 1 and J. 2 each independently represents an integer of 0 to 2, K 1 and K. 2 each independently represents an integer of 0 to 2, The polycarbonate copolymer of claim 17.

19. The X is R 11 and R 12 a siloxane constitutional unit which represents a fluorene ring structure formed by bonding together, and 21 and R 22 The polycarbonate copolymer according to claim 17 or 18, comprising polycarbonate structural units each of which represents a fluorene ring structure formed by bonding together.

20. A polycarbonate copolymer having a siloxane structural unit represented by formula (1) and a polycarbonate structural unit represented by formula (3), wherein the proportion of low molecular weight compounds having a weight average molecular weight of 1,000 or less calculated from a GPC area ratio is 30% by weight or less, 【Chemistry 13】 (In formula (1), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, X is any one of the structural formulas represented by the following formula (2): 【Chemistry 14】 (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less. 【Chemistry 15】 (In the formula, R 13 ~R 20 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Y is any one of the structural formulas represented by formula (4), 【Chemistry 16】 (In the formula, R 21 , and R 22 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 21 and R 22 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, c and d each independently represent 0 or an integer of 1 to 5000. The polycarbonate copolymer comprises at least the X has a siloxane structural unit that represents a fluorene ring structure formed by R 11 and R 12 bonding to each other, or the Y has a polycarbonate structural unit that represents a fluorene ring structure formed by R 21 and R 22 bonding to each other; Polycarbonate copolymer.

21. The polycarbonate copolymer according to any one of claims 17 to 20, wherein the number of moles of the siloxane constituent unit in the polycarbonate copolymer is 1 to 1000, and the number of moles of the polycarbonate constituent unit in the polycarbonate copolymer is 1 to 1000.

22. The polycarbonate copolymer according to any one of claims 17 to 21, wherein the molar ratio of the siloxane constituent units to the polycarbonate constituent units is 0.01:99.9 to 99.9:0.

01.

23. The polycarbonate copolymer according to claim 22, wherein the molar ratio of the siloxane constituent units to the polycarbonate constituent units is 30.00:70.00 to 99.9:0.

01.

24. The Q value measured under the conditions of 280°C and 160 kgf is 8 (x10 -2 cm 3 s -1 The polycarbonate copolymer according to any one of claims 17 to 23, wherein the copolymer has a molecular weight of 100 or more.

25. A polycarbonate copolymer having a siloxane structural unit represented by any one of formulas (1-1) to (1-4) and a polycarbonate structural unit represented by any one of formulas (3-1) to (3-4), and having a total content of cyclic units represented by formulas (5-1) to (5-3) of 4.0% by weight or less, 【Chemistry 17】 (In formulas (1-1) to (1-4), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 and R 3 ~R 33 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Z 1 and Z 2 each independently represents an alkylene group having 1 to 5 carbon atoms which may have a substituent, J 1 each independently represents an integer of 0 to 5, K 1 each independently represents an integer of 0 to 5, A 1 and A 2 each independently represents -O- or -CH-; L 1 and L 2 each independently represents an integer of 0 to 3, X is a single bond or any one of the structural formulas represented by the following formula (2): 【Chemistry 18】 (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less. 【Chemistry 19】 (In formulas (3-1) to (3-4), R 13 ~R 20 and R 40 ~R 51 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, Z 3 and Z 4 each independently represents an alkylene group having 1 to 5 carbon atoms which may have a substituent, J 2 each independently represents an integer of 0 to 5, K 2 each independently represents an integer of 0 to 5, A 1 and A 2 each independently represents -O- or -CH-; L 1 and L 2 each independently represents an integer of 0 to 3, Y is a single bond or any one of the structural formulas represented by formula (4), 【Chemistry 20】 (In the formula, R 21 , and R 22 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 21 and R 22 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, c and d each independently represent 0 or an integer of 1 to 5000. 【Chemistry 21】 In the formulas (5-1) to (5-3), m and n represent the (—OSi(R 1 R 2 represents the total number of structural units containing a (-OC(=O)O-) moiety, and the total number of structural units containing a (-OC(=O)O-) moiety, (In formula (5-1), m represents an integer of 2 to 10, In formula (5-2), n represents an integer of 2 to 10. In formula (5-3), the sum of the values ​​of m is 1 to 10, and the sum of the values ​​of n is 1 to 10. In formula (5-3), (—OSi(R 1 R 2 The structural unit containing the (—OC(═O)O—) moiety and the structural unit containing the (—OC(═O)O—) moiety may be arranged in any manner; In formulas (5-1) to (5-3), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 and R 13 ~R 20 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, X 1 and X 2 each independently represents an alkylene group having 1 to 5 carbon atoms which may have a substituent, i and ii each independently represent an integer of 0 to 5, X is a single bond or any one of the structural formulas represented by the following formula (2): 【Chemical 22】 (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 to 5000. The polycarbonate copolymer comprises at least the X has a siloxane structural unit that represents a fluorene ring structure formed by R 11 and R 12 bonding to each other, or the Y has a polycarbonate structural unit that represents a fluorene ring structure formed by R 21 and R 22 bonding to each other; Polycarbonate copolymer.

26. The polycarbonate copolymer according to any one of claims 17 to 25, wherein the total content of the cyclic structures of the formulas (6-1) to (6-2) is 2.0% by weight or less. 【Chemistry 23】 (In formulas (6-1) and (6-2), R 1 , and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, R 3 ~R 10 and R 30 ~R 33 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkenyl group having 2 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, X 1 and X 2 each independently represents an alkylene group having 1 to 5 carbon atoms which may have a substituent, i and ii each independently represent an integer of 0 to 5, n represents an integer from 2 to 10; X is a single bond or any one of the structural formulas represented by the following formula (2): 【Chemistry 24】 (In formula (2), R 11 , and R 12 each independently represents hydrogen, halogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 11 and R 12 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent, a and b each independently represent 0 or an integer of 1 or more and 5000 or less.

27. The polycarbonate copolymer according to any one of claims 17 to 26, having a 1% mass loss thermal decomposition temperature of 415°C or less.

28. A composition comprising the polycarbonate copolymer according to any one of claims 17 to 27 and a polycarbonate resin.

29. The composition according to claim 28, wherein the total amount of Si in the composition is 0.1 to 20 mass%.

30. The Q value of the composition measured under conditions of 280° C. and 160 kgf is Q 1 is the Q value measured under the same conditions for only the polycarbonate resin contained in the composition, 2 30. The composition of claim 28, wherein the viscosity is 120% or more.

31. A molded article obtained by molding the polycarbonate copolymer according to any one of claims 17 to 27.

32. An optical lens comprising the polycarbonate copolymer of any one of claims 17 to 27.

33. An optical lens obtained by molding the composition according to any one of claims 28 to 30.

Citation Information

Patent Citations

  • Production of polycarbonate resin

    JP1987297319A

  • Production of aromatic polycarbonate

    JP1995097439A

  • Novel polymers based on polyarylene siloxanes and free-radical polymerizable monomers

    JP1996502537A

  • Production of siloxane copolymer

    JP1997235375A

  • Process for producing functional siloxanes with controlled structures

    JP2015512999A

Cited By

  • Methods for producing polycarbonate copolymer and polysiloxane compound, polycarbonate copolymer, polysiloxane compound, composition and molded body

    JP2024113011A

  • Thermoplastic resin, composition, molded article, optical lens, and method for producing thermoplastic resin

    JPWO2022065329A1

  • Methods for producing polycarbonate copolymer and polysiloxane compound, polycarbonate copolymer, polysiloxane compound, composition, and molded body

    US12325796B2