Manufacturing method of image display device and laminate for polarizer transfer
The polarizer transfer laminate with coating and retardation layers addresses thickness reduction and protection challenges in image display devices, resulting in more durable and thinner devices.
Patent Information
- Application Number
- JP2021522825
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-28
- Filing Date
- 2020-05-27
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-05-27
AI Technical Summary
Existing image display devices face challenges in reducing thickness while protecting polarizers from scratches and deterioration due to environmental factors and handling issues.
A method involving a polarizer transfer laminate with a coating layer and polarizer on a releasable film, where the laminate is laminated on the image display cell, incorporating retardation layers and protective coatings to enhance durability and reduce thickness.
The method enables the production of thinner image display devices with improved protection against scratches and deterioration of polarizers, enhancing durability and performance.
Smart Images

Figure 0007567785000001 
Figure 0007567785000002 
Figure 0007567785000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an image display device and a laminate for transferring a polarizer. [Background technology]
[0002] For example, in a liquid crystal display device, a polarizing plate is attached to both the visible side and the light source side of a liquid crystal cell, and in an organic EL display device, a circular polarizing plate is attached to the visible side of an organic EL cell. Conventionally, these polarizing plates are made by attaching a polarizer protective film to a polarizer, and a rigid film of 40 to 100 μm such as triacetyl cellulose (TAC), acrylic resin, cyclic polyolefin (COP), polyethylene terephthalate (PET) has been used as the polarizing protective film. Furthermore, an optical compensation film is usually laminated between the polarizing plate and the image display cell in the case of a liquid crystal display device, and a λ / 4 retardation film is usually laminated in the case of an organic EL display device.
[0003] In line with the recent trend toward thinner image display devices, a method has been proposed in which an adhesive layer is provided on the polarizer surface of a polarizing plate having a polarizer protective film on only one side of the polarizer, and the polarizer and the image display cell are directly attached to each other (for example, Patent Document 1). However, the polarizer protective film itself is essential in terms of ease of handling the polarizer, prevention of scratches on the polarizer surface due to contact with other objects, prevention of deterioration of the polarizer surface due to moisture, detergent, harmful gas components in the environment, etc., and since the polarizer protective film itself has a thickness of several tens of μm, it has not been adequately suited to thin image display devices. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2010-277018 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made in view of the problems with the conventional techniques. That is, an object of the present invention is to provide a method for manufacturing an image display device that can suppress scratches, deterioration, etc. of a polarizer while responding to further thinning. [Means for solving the problem]
[0006] The present inventors have conducted extensive research to achieve the above object, and as a result have completed the present invention. Section 1. A method for manufacturing an image display device, comprising the step of laminating a polarizer transfer laminate LP1 onto at least one side of an image display cell, so that the polarizer of the polarizer transfer laminate LP1, which is composed of a coating layer and a polarizer laminated in this order on a release film, is positioned on the image display cell side. Section 2. (A) a step of laminating a laminate for polarizer transfer LP1 on one surface of an image display cell such that a polarizer of the laminate for polarizer transfer LP1, which is formed by laminating a coating layer and a polarizer in this order on a release film, is disposed on the image display cell side; and (B) A step of laminating a laminate for polarizer transfer LP2 on the other surface of the image display cell so that the polarizer of the laminate for polarizer transfer LP2, in which a polarizer is laminated on a release film, is disposed on the image display cell side. A method for manufacturing an image display device comprising the steps of: Section 3. Item 3. The method for producing an image display device according to item 1 or 2, wherein the polarizer transfer laminate LP1 has a retardation layer on the opposite side of the polarizer to the coating layer. Section 4. Item 4. The method for producing an image display device according to Item 2 or 3, wherein the polarizer transfer laminate LP2 has a retardation layer on the side of the polarizer opposite to the release film. Section 5. Item 5. The method for producing an image display device according to any one of items 2 to 4, wherein the polarizer transfer laminate LP2 has a coating layer between the release film and the polarizer. Section 6. 6. The method for producing an image display device according to any one of items 1 to 5, wherein the coating layer includes any one of a hard coating layer, a reflection reducing layer, and an antistatic layer. Section 7. 7. The method for producing an image display device according to any one of Items 1 to 6, wherein the image display cell is a liquid crystal display cell. Section 8. 7. The method for producing an image display device according to claim 1, 3, or 6, wherein the image display cell is an organic EL display cell. Section 9. A laminate for polarizer transfer, in which a coating layer and a polarizer are laminated in this order on a release film. Section 10. Item 10. The laminate for polarizer transfer according to item 9, further comprising a retardation layer on the opposite side of the coating layer of the polarizer. Effect of the Invention
[0007] According to the present invention, it is possible to manufacture an image display device which can be made thinner and which can suppress scratches and deterioration of the polarizer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] In one embodiment of the present invention, a manufacturing method for an image display device preferably includes a step of laminating a polarizer transfer laminate LP1 onto at least one side of an image display cell so that the polarizer of the polarizer transfer laminate LP1, which is composed of a coating layer and a polarizer laminated in this order on a release film, is positioned on the image display cell side.
[0009] In one embodiment of the present invention, a method for producing an image display device includes the steps of: (A) a step of laminating a laminate for polarizer transfer LP1 on one surface of an image display cell such that a polarizer of the laminate for polarizer transfer LP1, which is formed by laminating a coating layer and a polarizer in this order on a release film, is disposed on the image display cell side; and (B) A step of laminating a laminate for polarizer transfer LP2 on the other surface of the image display cell so that the polarizer of the laminate for polarizer transfer LP2, in which a polarizer is laminated on a release film, is disposed on the image display cell side. It is preferred that the compound contains
[0010] (Polarizer transfer laminate LP1) The LP1 preferably has a coating layer and a polarizer in this order on a release film.
[0011] (Release film) As the release film of LP1, a film widely used as a release film can be appropriately used. The release film is composed of a single layer or multiple layers, and includes at least a base film. The base film is preferably a resin film. The resin of the resin film is not particularly limited, and any resin film can be used without limitation, such as polyester, polycarbonate, polyamide, polyimide, polyamideimide, polystyrene, triacetyl cellulose, polypropylene, and cyclic polyolefin. Among these, polyester is preferable from the viewpoint of mechanical strength, heat resistance, supply stability, and the like, and polyethylene terephthalate is more preferable. In addition, the base film may be an unstretched film or a stretched film. When it is a stretched film, it may be a uniaxially stretched film or a biaxially stretched film. Among them, a biaxially stretched polyethylene terephthalate film is preferable.
[0012] When the substrate film itself has releasability, the substrate film can be used as it is as a releasable film. In order to adjust the releasability of the substrate film, the substrate film may be subjected to a surface treatment such as a corona treatment, a plasma treatment, or a flame treatment.
[0013] The release film may have a release layer on the base film. Examples of the release layer include silicone-based, amino resin-based, alkyd resin-based, long-chain acrylic resin-based, etc., and the composition and type can be appropriately selected according to the required release force.
[0014] The release film may have an easy-adhesion layer between the base film and the release layer. As the easy-adhesion layer, those conventionally used in each base film such as polyester-based, acrylic-based, and polyurethane-based can be used, and can be selected according to the base film and / or release layer to be used.
[0015] (Coat layer) The coating layer of LP1 may be of any type, as long as it is composed of a single layer or multiple layers, and the constituent layers (in the case of multiple layers, each layer) are formed by coating. The coating layer is preferably provided on the release surface of the release film. The upper limit of the thickness of the coating layer is preferably 50 μm, more preferably 30 μm, and even more preferably 20 μm. The lower limit of the thickness of the coating layer is not particularly limited, but is preferably 0.1 μm, more preferably 0.5 μm, and even more preferably 1 μm. When the coating layer is composed of multiple layers, it is preferable that the total thickness of the multiple layers satisfies the above. By reducing the thickness of the coating layer, the image display device can be made even thinner.
[0016] The coating layer may be made of a resin. Examples of the resin include, but are not limited to, polyester resin, acrylic resin, polyurethane resin, polyvinyl alcohol, epoxy resin, polyvinyl alcohol, polyvinyl acetate, etc. Only one type of resin may be used, or two or more types may be used in combination.
[0017] The resin may be crosslinked. Examples of the crosslinking agent include an isocyanate compound, an epoxy resin, a melamine resin, an oxazoline compound, and a carbodiimide compound. Only one type of crosslinking agent may be used, or two or more types may be used in combination.
[0018] The coating layer may be formed by curing (thermally curing or photocuring) an acrylic monomer and / or oligomer.
[0019] Examples of the coating layer include a reflection reducing layer, a hard coat layer, and an antistatic layer. The coating layer may have a function of protecting the polarizer, separately from or in addition to the reflection reducing function, the hard coat function, and the antistatic function. Examples of the protective function of the polarizer include a function of protecting the polarizer from scratches and damage before assembly into an image display device, a function of protecting the polarizer from scratches and damage caused by contact with other members or the outside when the image display device is used, and a function of protecting the polarizer from harmful substances (liquids such as water, detergents, and alcohols, harmful gases such as SOx and NOx, etc.) to which the image display device is exposed in the environment in which the image display device is used.
[0020] (Reflection reduction layer) The reflection-reducing layer may be of any type as long as it can reduce the reflectance at the interface with air. The reflection-reducing layer can suppress reflection from external light, making images easier to see.
[0021] The upper limit of the reflectance of the reflection-reduction layer is preferably 5%, more preferably 4%, even more preferably 3%, particularly preferably 2%, and most preferably 1.5%. By keeping the reflectance below the above range, the display screen becomes easier to see. The lower limit of the reflectance is not particularly specified, but is preferably 0.01%, and more preferably 0.1%. The reflectance is measured by the following method: A polarizer transfer laminate is attached to a black acrylic plate using HCP highly transparent adhesive transfer sheet 9483PL. The surfaces to be attached are the surface of the polarizer transfer laminate opposite to the release film (the polarizer surface, or the surface of the other layer if another layer is laminated on the polarizer) and the surface of the black acrylic plate. After attachment, the release film is peeled off from the sample, and the 5-degree reflectance at a wavelength of 550 nm is measured using a spectrophotometer (Shimadzu Corporation, UV-3150). The 5-degree reflectance is the reflectance when the incident angle is 5 degrees with respect to the transmission axis direction of the polarizer of the sample.
[0022] The reflection reducing layer may be of various types, such as a low reflection layer, an anti-reflection layer, or an anti-glare layer.
[0023] (Low reflective layer) The low reflection layer is not particularly limited as long as it is a layer that can reduce the refractive index difference with air, and can be, for example, a low refractive index layer.In the case of the low reflection layer, the upper limit of the reflectance is preferably 5%, more preferably 4%, and even more preferably 3%.The lower limit of the reflectance is preferably 0.8%, and more preferably 1%.
[0024] (Anti-reflection layer) The antireflection layer is not particularly limited as long as it is a layer that can prevent reflection by interfering between reflected light at the interface on the viewing side and reflected light at the interface on the image display cell side. For example, the antireflection layer may be a low refractive index layer having a thickness of about the wavelength of visible light (400 to 700 nm) / (refractive index of the low refractive index layer×4).
[0025] The antireflection layer may be a combination of a low refractive index layer and a high refractive index layer, and in such a combination, the low refractive index layer is preferably disposed on the viewing side (or the release film side). The antireflection layer may have two or more low refractive index layers and / or high refractive index layers. Such an antireflection layer can further enhance the antireflection effect by multiple interference.
[0026] In the case of the anti-reflection layer, the upper limit of the reflectance is preferably 2%, more preferably 1.5%, further preferably 1.2%, and particularly preferably 1%. The lower limit of the reflectance is preferably 0.01%, more preferably 0.1%.
[0027] (Low refractive index layer) The refractive index of the low refractive index layer is preferably 1.45 or less, more preferably 1.42 or less. The refractive index of the low refractive index layer is preferably 1.20 or more, more preferably 1.25 or more. The refractive index of the low refractive index layer is a value measured under the condition of a wavelength of 589 nm.
[0028] The thickness of the low refractive index layer is not limited, but may be appropriately set within the range of about 30 nm to 1 μm. In order to reduce the reflectance by offsetting the reflection at the interface of the low refractive index layer on the viewing side and the reflection at the interface of the low refractive index layer on the image display cell side, the thickness of the low refractive index layer is preferably 70 to 120 nm, more preferably 75 to 110 nm.
[0029] Preferred examples of the low refractive index layer include (1) a layer made of a resin composition containing a binder resin and low refractive index particles, (2) a layer made of a fluororesin which is a low refractive index resin, (3) a layer made of a fluororesin composition containing silica or magnesium fluoride, and (4) a thin film of a low refractive index material such as silica or magnesium fluoride.
[0030] The binder resin contained in the resin composition (1) can be any of polyester, polyurethane, polyamide, polycarbonate, acrylic, etc., without any particular limitation. Among them, acrylic is preferable, and it is preferable that the binder resin is obtained by polymerizing (crosslinking) a photopolymerizable compound by irradiation with light.
[0031] Examples of the photopolymerizable compound include a photopolymerizable monomer, a photopolymerizable oligomer, and a photopolymerizable polymer, which can be appropriately adjusted for use. As the photopolymerizable compound, a combination of a photopolymerizable monomer and a photopolymerizable oligomer or a photopolymerizable polymer is preferred.
[0032] (Photopolymerizable monomer) The photopolymerizable monomer preferably has a molecular weight of less than 1000. Moreover, the photopolymerizable monomer is preferably a polyfunctional monomer having two or more photopolymerizable functional groups (that is, bifunctional).
[0033] Examples of polyfunctional monomers include tripropylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, acrylate, tripentaerythritol octa(meth)acrylate, tetrapentaerythritol deca(meth)acrylate, isocyanuric acid tri(meth)acrylate, isocyanuric acid di(meth)acrylate, polyester tri(meth)acrylate, polyester di(meth)acrylate, bisphenol di(meth)acrylate, diglycerin tetra(meth)acrylate, adamantyl di(meth)acrylate, isobornyl di(meth)acrylate, dicyclopentane di(meth)acrylate, tricyclodecane di(meth)acrylate, and those modified with PO, EO, etc.
[0034] Among these, from the viewpoint of obtaining a layer having high hardness, pentaerythritol triacrylate (PETA), dipentaerythritol hexaacrylate (DPHA), pentaerythritol tetraacrylate (PETTA), dipentaerythritol pentaacrylate (DPPA), etc. are preferable. Only one type of photopolymerizable monomer may be used, or two or more types may be used in combination.
[0035] (Photopolymerizable oligomer) The photopolymerizable oligomer preferably has a weight average molecular weight of 1000 or more and less than 10000. In this specification, the "weight average molecular weight" is a value obtained by dissolving in a solvent such as THF and converting the weight average molecular weight into polystyrene equivalent by a conventionally known gel permeation chromatography (GPC) method. The photopolymerizable oligomer is preferably a polyfunctional oligomer having two or more functionalities. Examples of the polyfunctional oligomer include polyester (meth)acrylate, urethane (meth)acrylate, polyester-urethane (meth)acrylate, polyether (meth)acrylate, polyol (meth)acrylate, melamine (meth)acrylate, isocyanurate (meth)acrylate, and epoxy (meth)acrylate. Only one type of photopolymerizable oligomer may be used, or two or more types may be used in combination.
[0036] (Photopolymerizable polymer) The photopolymerizable polymer preferably has a weight average molecular weight of 10,000 or more, and more preferably 10,000 to 80,000, and even more preferably 10,000 to 40,000, in terms of coating suitability and the appearance of the resulting layer. The photopolymerizable polymer is preferably a multifunctional polymer having two or more functional groups. Examples of the multifunctional polymer include urethane (meth)acrylate, isocyanurate (meth)acrylate, polyester-urethane (meth)acrylate, and epoxy (meth)acrylate. Only one type of photopolymerizable polymer may be used, or two or more types may be used in combination.
[0037] The low refractive index particles contained in the resin composition (1) include silica particles (e.g., hollow silica particles), magnesium fluoride particles, etc., and among them, hollow silica particles are preferred. Such hollow silica particles can be produced, for example, by the production method described in the examples of JP-A-2005-099778.
[0038] The average particle size of the primary particles of the low refractive index particles is preferably from 5 to 200 nm, more preferably from 5 to 100 nm, and even more preferably from 10 to 80 nm.
[0039] The low refractive index particles are more preferably surface-treated with a silane coupling agent, and more preferably surface-treated with a silane coupling agent having a (meth)acryloyl group. Only one type of low refractive index particles may be used, or two or more types may be used in combination.
[0040] The resin composition (1) may contain, in addition to the above components, a polymerization initiator, a crosslinking agent catalyst, a polymerization inhibitor, an antioxidant, an ultraviolet absorber, a leveling agent, a surfactant, and the like.
[0041] The content of the low refractive index particles in the low refractive index layer (or the resin composition (1)) is preferably 10 to 250 parts by mass, more preferably 50 to 200 parts by mass, and further preferably 100 to 180 parts by mass, per 100 parts by mass of the binder resin.
[0042] As the fluorine-based resin (2), a polymerizable compound containing at least a fluorine atom in the molecule or a polymer thereof can be used. The polymerizable compound is not particularly limited, but is preferably, for example, a compound having a curing reactive group such as a photopolymerizable functional group or a thermosetting polar group, or may be a compound having a plurality of these curing reactive groups at the same time.
[0043] As the compound having a photopolymerizable functional group, for example, a wide variety of fluorine-containing monomers having an ethylenically unsaturated bond can be used.
[0044] It is also preferable to appropriately add a known polysiloxane-based or fluorine-based antifouling agent to the low refractive index layer in order to improve fingerprint resistance. Preferred examples of polysiloxane-based antifouling agents include, for example, polyether-modified polydimethylsiloxane having an acrylic group, polyether-modified dimethylsiloxane, polyester-modified dimethylsiloxane having an acrylic group, polyether-modified polydimethylsiloxane, polyester-modified polydimethylsiloxane, and aralkyl-modified polymethylalkylsiloxane. It is preferable that the fluorine-based antifouling agent has a substituent that contributes to the formation of the low refractive index layer or compatibility with the low refractive index layer. The substituent may be one or more, and the multiple substituents may be the same or different from each other. Preferred examples of the substituent include an acryloyl group, a methacryloyl group, a vinyl group, an aryl group, a cinnamoyl group, an epoxy group, an oxetanyl group, a hydroxyl group, a polyoxyalkylene group, a carboxyl group, and an amino group.
[0045] (High refractive index layer) The refractive index of the high refractive index layer is preferably 1.55 to 1.85, and more preferably 1.56 to 1.70. The refractive index of the high refractive index layer is a value measured under the condition of a wavelength of 589 nm.
[0046] The thickness of the high refractive index layer is preferably 30 to 200 nm, more preferably 50 to 180 nm. The high refractive index layer may be a multi-layered structure, but is preferably two or less layers, more preferably a single layer. When the high refractive index layer is composed of a multi-layered structure, the total thickness of the multi-layered structure is preferably within the above range.
[0047] When the high refractive index layer has two layers, it is preferable that the refractive index of the high refractive index layer on the low refractive index layer side is higher. Specifically, the refractive index of the high refractive index layer on the low refractive index layer side is preferably 1.60 to 1.85, and the refractive index of the other high refractive index layer is preferably 1.55 to 1.70.
[0048] The high refractive index layer is preferably made of a resin composition containing high refractive index particles and a resin. As high refractive index particles, antimony pentoxide particles (1.79), zinc oxide particles (1.90), titanium oxide particles (2.3 to 2.7), cerium oxide particles (1.95), tin-doped indium oxide particles (1.95 to 2.00), antimony-doped tin oxide particles (1.75 to 1.85), yttrium oxide particles (1.87), zirconium oxide particles (2.10), etc. are preferred. The above parentheses indicate the refractive index of the material of each particle. Among these, titanium oxide particles and / or zirconium oxide particles are preferred.
[0049] The high refractive index particles may be used alone or in combination of two or more kinds. In particular, it is preferable to combine a first high refractive index particle with a second high refractive index particle having a smaller surface charge amount than the first high refractive index particle in order to prevent aggregation. In addition, it is also preferable that the high refractive index particles are surface-treated in terms of dispersibility.
[0050] The preferred average particle size of the primary particles of the high refractive index particles is the same as that of the low refractive index particles.
[0051] The content of the high refractive index particles is preferably 30 to 400 parts by mass, more preferably 50 to 200 parts by mass, and further preferably 80 to 150 parts by mass, relative to 100 parts by mass of the resin.
[0052] Resins used in the high refractive index layer include the same resins as those listed for the low refractive index layer, except for fluorine-based resins.
[0053] The high refractive index layer and the low refractive index layer can be formed, for example, by applying a resin composition containing a photopolymerizable compound to a release film, drying the resin composition, and then irradiating the coating-like resin composition with light such as ultraviolet light to polymerize (crosslink) the photopolymerizable compound. When the high refractive index layer and the low refractive index layer are provided on the release film, it is preferable that the release film side is the low refractive index layer.
[0054] The high refractive index layer and the low refractive index layer (or the resin composition (paint) constituting them) may contain, as necessary, a thermoplastic resin, a thermosetting resin, a solvent, a polymerization initiator, a dispersant, a surfactant, an antistatic agent, a silane coupling agent, a thickener, a coloring inhibitor, a colorant (pigment, dye), a defoamer, a leveling agent, a flame retardant, an ultraviolet absorbing agent, an adhesion promoter, a polymerization inhibitor, an antioxidant, a surface modifier, a lubricant, and the like.
[0055] (Anti-glare layer) The antiglare layer is not particularly limited as long as it is a layer capable of causing diffuse reflection by the unevenness of the surface. The antiglare layer can prevent the shape of the light source from being reflected when external light is reflected on the surface and can reduce glare.
[0056] On the surface of the antiglare layer, the area where the inclination angle (surface angle) of the antiglare surface is 0.05° or more is preferably 50% or more, more preferably 55% or more, and even more preferably 60% or more. The upper limit of the ratio of the area where the surface angle is 0.05° or more is preferably 95%, more preferably 90%. When the surface angle is in the above range, rainbow spots due to interference of the antiglare surface itself can be reduced.
[0057] The root mean square slope (RΔq) of the surface of the antiglare layer is preferably 0.004 or less.
[0058] The kurtosis (Rku) of the surface of the antiglare layer is preferably 5 or less, more preferably 4 or less, and further preferably 3 or less. Rku is preferably 2 or more.
[0059] The surface skewness (RSk) of the antiglare layer is preferably from −1.0 to 1.0, more preferably from −0.5 to 0.5, and further preferably from −0.3 to 0.3.
[0060] The average inclination angle (θa) of the irregularities on the surface of the antiglare layer is preferably 0.01 to 1.5°, more preferably 0.04 to 1.2°, and further preferably 0.1 to 0.5°.
[0061] The arithmetic mean roughness (Ra) of the unevenness on the surface of the antiglare layer is preferably 0.02 to 0.25 μm, more preferably 0.02 to 0.15 μm, and further preferably 0.02 to 0.12 μm.
[0062] The ten-point average roughness (Rzjis) of the unevenness on the surface of the antiglare layer is preferably 0.15 to 2.00 μm, more preferably 0.20 to 1.20 μm, and further preferably 0.30 to 0.80 μm.
[0063] When the values of RΔq, Rku, RSk, θa, Ra, and Rzjis are equal to or greater than the lower limits, the reflection of external light can be more effectively suppressed.When the values of RΔq, Rku, RSk, θa, Ra, and Rzjis are equal to or less than the upper limits, the brightness and contrast are excellent.
[0064] The average spacing (RSm) of the irregularities on the antiglare surface is preferably 50 to 600 μm, more preferably 100 to 400 μm, further preferably 120 to 300 μm, and particularly preferably 150 to 280 μm. When the RSm value is equal to or greater than the lower limit, it is easy to control aggregation. When the RSm value is equal to or less than the upper limit, it is possible to reproduce the fineness of the image.
[0065] RΔq, Rku, RSk, θa, Ra, Rzjis, and RSm are calculated from a roughness curve measured using a contact type roughness meter in accordance with JIS B0601-1994 or JIS B0601-2001.
[0066] Examples of the method for providing unevenness on the surface of the antiglare layer (the surface on the release film side) include a method for providing unevenness corresponding to the release surface of the release film, and specifically include a method of (1) providing unevenness on the base film of the release film, and (2) providing a layer having unevenness on the base film by coating (or application), etc. In this specification, coating includes not only a wet process in which a coating material is applied and solidified, but also dry processes such as deposition, sputtering, and CVD.
[0067] Method (1) includes, for example, sandblasting, chemical etching, contacting a release film with a mold having a concave-convex structure, and adding particles to a release film.
[0068] Method (2) includes a method in which a base film contains a filler such as particles and a layer having a thickness thinner than the particle diameter of the filler is provided; a coating material for transferring unevenness (a curable composition, preferably a photocurable composition) is applied to a base film and then brought into contact with a mold having unevenness to cure; and a method in which a coating material for transferring unevenness (a curable composition, preferably a photocurable composition) is applied to a mold having unevenness and then overlaid on the base film and cured.
[0069] The lower limit of the thickness of the antiglare layer is preferably 0.1 μm, more preferably 0.5 μm, and the upper limit of the thickness of the antiglare layer is preferably 100 μm, more preferably 50 μm, and further preferably 20 μm.
[0070] The refractive index of the antiglare layer is preferably 1.20 to 1.80, more preferably 1.40 to 1.70. When a low reflection effect is desired by lowering the refractive index of the antiglare layer itself, the refractive index of the antiglare layer is preferably 1.20 to 1.45, more preferably 1.25 to 1.40. When a low refractive index layer and an antiglare layer are combined, particularly when the low refractive index layer and the antiglare layer are laminated in this order on a release film, the refractive index of the antiglare layer is preferably 1.50 to 1.80, more preferably 1.55 to 1.70. The refractive index of the antiglare layer is a value measured under conditions of a wavelength of 589 nm.
[0071] (Hard coat layer) The hard coat (HC) layer may be appropriately selected from those that are widely used as hard coat layers. The pencil hardness of the hard coat layer is preferably H or more, more preferably 2H or more. The hard coat layer may be provided, for example, by applying and curing a composition (paint for hard coat layer) containing a thermosetting resin or a radiation curable resin.
[0072] Examples of the thermosetting resin include acrylic resin, urethane resin, phenol resin, urea melamine resin, epoxy resin, unsaturated polyester resin, silicone resin, etc. The thermosetting resin may be used alone or in combination of two or more. In the composition, a curing agent is added to the curable resin as necessary.
[0073] The radiation curable resin is preferably a compound having a radiation curable functional group, and examples of the radiation curable functional group include ethylenically unsaturated bond groups such as (meth)acryloyl group, vinyl group, and allyl group, epoxy group, and oxetanyl group. Among these, a compound having an ethylenically unsaturated bond group is preferred, a compound having two or more ethylenically unsaturated bond groups is more preferred, and among these, a polyfunctional (meth)acrylate compound having two or more ethylenically unsaturated bond groups is even more preferred. The polyfunctional (meth)acrylate compound may be a monomer, an oligomer, or a polymer.
[0074] Specific examples of the radiation curable resin include those exemplified as the binder resin in the low refractive index layer. The radiation curable resin may be used alone or in combination of two or more kinds.
[0075] In order to achieve the hardness required for a hard coat, the compound having a radiation-curable functional group preferably contains 50% by mass or more of difunctional or higher functional monomers, more preferably 70% by mass or more, and further preferably contains 50% by mass or more of trifunctional or higher functional monomers, more preferably 70% by mass or more, in the compound having a radiation-curable functional group.
[0076] The thickness of the hard coat layer is preferably in the range of 0.1 to 100 μm, more preferably in the range of 0.8 to 20 μm.
[0077] The refractive index of the hard coat layer is more preferably 1.45 to 1.70, and further preferably 1.50 to 1.60. The refractive index of the hard coat layer is a value measured under the condition of a wavelength of 589 nm.
[0078] Methods for adjusting the refractive index of the hard coat layer include a method for adjusting the refractive index of a resin, a method for adjusting the refractive index of particles when particles are added, etc. Specific examples of particles include those exemplified as particles for the antiglare layer.
[0079] The hard coat layer may be a single layer, and it is also preferable to combine it with a reflection reducing layer or the like. When the hard coat layer and the reflection reducing layer are combined, it is preferable to laminate the reflection reducing layer and the hard coat layer in this order on the release film. In this specification, the hard coat layer and the reflection reducing layer are regarded as one member, and the member may be referred to as the reflection reducing layer.
[0080] (Antistatic layer) The antistatic layer is not particularly limited as long as it is a layer containing an antistatic agent. Examples of the antistatic agent include cationic antistatic agents such as quaternary ammonium salts; conductive polymers such as polyaniline and polythiophene; needle-shaped metal fillers; and conductive high refractive index fine particles such as tin-doped indium oxide fine particles and antimony-doped tin oxide fine particles. The antistatic agent may be used alone or in combination of two or more.
[0081] The antistatic layer preferably contains a binder resin in addition to the antistatic agent. The binder resin may be polyester, polyurethane, polyamide, acrylic, etc. Only one type of binder resin may be used, or two or more types may be used in combination.
[0082] In addition, an antistatic agent may be added to the hard coat layer so that the hard coat layer functions as an antistatic layer. The antistatic agent to be added to the hard coat layer may be any of the above-mentioned components, such as cationic antistatic agents such as quaternary ammonium salts, fine particles such as tin-doped indium oxide (ITO), conductive polymers, etc.
[0083] The content of the antistatic agent is preferably 1 to 30% by mass based on the total mass of all solids in the antistatic layer (or the hard coat layer when the hard coat layer has an antistatic function).
[0084] (Polarizer) Examples of polarizers (also called polarizing plates, polarizing films, polarizing layers, etc.) that can be used include those in which iodine or an organic dichroic dye is adsorbed onto uniaxially stretched polyvinyl alcohol (PVA) (PVA polarizers), those in which a composition consisting of a liquid crystal compound and a dichroic dye is coated and oriented (liquid crystal polarizers), and wire grid polarizers.
[0085] As examples of methods for providing a polarizer on the coating layer, in the case of a PVA polarizer, methods (a) and (b) can be mentioned. (a) A method of bonding individual PVA polarizers. (b) A method for transferring a PVA polarizer onto a releasable substrate.
[0086] The method (a) includes a method of laminating a PVA polarizer alone using an adhesive or pressure-sensitive adhesive, and a method of laminating a PVA polarizer to a coating layer on a release film using an adhesive or pressure-sensitive adhesive is preferred. The thickness of this type of polarizer is preferably 5 to 50 μm, more preferably 10 to 30 μm, and particularly preferably 12 to 25 μm. The thickness of the adhesive or pressure-sensitive adhesive is preferably 1 to 10 μm, and more preferably 2 to 5 μm.
[0087] In the method (b), the releasable substrate may be any of those listed as the releasable film, and preferably is an unstretched or uniaxially stretched film such as PET or polypropylene. A method for laminating a PVA polarizer on a releasable substrate may include a method in which PVA is coated on the releasable substrate, and the substrate is stretched together with the releasable substrate to allow iodine or an organic dichroic dye to be adsorbed on the PVA, and then the orientation is fixed with a boron compound. In this specification, a laminate of a releasable substrate and a PVA polarizer may be referred to as a "PVA polarizer transfer laminate".
[0088] Further, as a transfer method, a method of bonding the polarizer surface (the surface on which the releasable substrate is not laminated) of the PVA polarizer transfer laminate to the coating layer surface of the laminate of the release film and the coating layer with an adhesive or pressure-sensitive adhesive, and peeling off the releasable substrate as necessary, can be mentioned. The thickness of this type of polarizer is preferably 1 to 10 μm, more preferably 2 to 8 μm, and particularly preferably 3 to 6 μm. The thickness of the adhesive or pressure-sensitive adhesive is preferably 1 to 10 μm, more preferably 2 to 5 μm.
[0089] The adhesive used for lamination is preferably a polyvinyl alcohol adhesive, an ultraviolet-curing adhesive such as acrylic or epoxy, or a heat-curing adhesive such as epoxy or isocyanate (urethane). The adhesive may also be a hot melt adhesive. Examples of the pressure-sensitive adhesive include acrylic, urethane, and rubber-based adhesives. It is also preferable to use an acrylic substrate-less optical transparent pressure-sensitive adhesive sheet as the pressure-sensitive adhesive.
[0090] Examples of the method for providing a polarizer on the coating layer include methods (c) and (d) in the case of a liquid crystal polarizer. (c) A method for applying paint for liquid crystal polarizers. (d) A method of transferring a liquid crystal polarizer on a releasable substrate.
[0091] As the method (c), a method of coating a liquid crystal polarizer coating material containing a liquid crystal compound on the coating layer, and orienting and fixing the liquid crystal compound can be mentioned. As a method of orienting and fixing the liquid crystal compound, a method of rubbing the coating layer, coating the liquid crystal polarizer coating material on the coating layer, heating to align it, and then curing and fixing it with ultraviolet light can be mentioned; a method of irradiating polarized ultraviolet light after coating the liquid crystal polarizer coating material to align and fix the liquid crystal compound, and the like can be mentioned. In addition, a method of providing an orientation control layer on the coating layer before coating the liquid crystal polarizer coating material, that is, laminating a liquid crystal polarizer on the coating layer via an orientation control layer, is also preferred.
[0092] The method (d) includes a method of laminating a liquid crystal polarizer on a releasable substrate in accordance with the above method (c), laminating a coating layer on the liquid crystal polarizer surface using an adhesive or pressure-sensitive adhesive, and peeling off the releasable substrate as necessary. The adhesive and pressure-sensitive adhesive used in lamination include those mentioned above. The releasable substrate may be one of those listed as the releasable substrate for the PVA polarizer transfer laminate, a metal belt, or the like. In this specification, the laminate of the releasable substrate and the liquid crystal polarizer may be referred to as the "liquid crystal polarizer transfer laminate".
[0093] The thickness of the liquid crystal polarizer is preferably from 0.1 to 7 μm, more preferably from 0.3 to 5 μm, and particularly preferably from 0.5 to 3 μm. The thickness of the adhesive or pressure-sensitive adhesive is preferably from 1 to 10 μm, and more preferably from 2 to 5 μm.
[0094] Furthermore, the alignment control layer and the liquid crystal polarizer will be described in detail. (Orientation control layer) The liquid crystal polarizer coating material may be directly applied to a coating layer or a releasable substrate, but it is also preferable to provide an orientation control layer in advance and then apply the coating material onto the orientation control layer. In this specification, the orientation control layer and the liquid crystal polarizer are regarded as a single member, and the member may be called a liquid crystal polarizer. The liquid crystal polarizer combined with the orientation control layer may be called a liquid crystal polarizing layer to clearly distinguish it from the general term liquid crystal polarizer.
[0095] The alignment control layer may be any layer that can cause the liquid crystal compound to be aligned in a desired state. Suitable examples of the alignment control layer include a rubbed alignment control layer having a rubbing treatment on the surface and a photoalignment control layer that aligns the molecules by irradiating them with polarized light to produce an alignment function.
[0096] (Rubbing treatment alignment control layer) The material of the rubbing treatment alignment control layer is usually a polymer. As the polymer, polyvinyl alcohol and its derivatives, polyimide and its derivatives, acrylic resin, polysiloxane derivatives, etc. are preferably used. Only one type of polymer may be used, or two or more types may be used in combination.
[0097] The method for forming the rubbing treatment alignment control layer preferably includes a step of rubbing the surface of the coating film obtained by applying a coating material for the rubbing treatment alignment control layer containing the above-mentioned polymer and solvent onto a coating layer or the release surface of a releasable substrate. The coating material for the rubbing treatment alignment control layer may contain a crosslinking agent.
[0098] The solvent for the coating material for the rubbing treatment alignment control layer can be used without any restrictions as long as it dissolves the polymer material. Specific examples include alcohols such as water, methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, and cellosolve; ester solvents such as ethyl acetate, butyl acetate, and gamma-butyrolactone; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, and cyclohexanone; aromatic hydrocarbon solvents such as toluene and xylene; and ether solvents such as tetrahydrofuran and dimethoxyethane. Only one type of solvent may be used, or two or more types may be used in combination.
[0099] The concentration of the polymer in the coating material for the rubbing treatment alignment control layer can be adjusted appropriately depending on the type of polymer and the thickness of the alignment control layer to be produced, but it is preferable that the solid content concentration be 0.2 to 20 mass %, and a range of 0.3 to 10 mass % is particularly preferable.
[0100] As the coating method, a known method can be used, such as a coating method such as a gravure coating method, a die coating method, a bar coating method, or an applicator method, or a printing method such as a flexography method.
[0101] After application, it is preferable to dry (for example, heat drying). The drying temperature depends on the material of the release film, but in the case of PET, it is preferably 30°C to 170°C, more preferably 50°C to 150°C, and even more preferably 70°C to 130°C. If the drying temperature is in this range, there is no need to take a long drying time, and productivity is excellent, there is no thermal elongation or thermal shrinkage of the transfer orientation film, the optical function as designed can be achieved, and the flatness is also excellent. The drying time is, for example, 0.5 to 30 minutes, more preferably 1 to 20 minutes, and even more preferably 2 to 10 minutes.
[0102] The thickness of the rubbing treatment alignment control layer is preferably 0.01 to 10 μm, more preferably 0.05 to 5 μm, and particularly preferably 0.1 to 1 μm.
[0103] The rubbing treatment can generally be carried out by rubbing the surface with paper or cloth in a certain direction. The rubbing treatment is preferably carried out using a rubbing roller made of raised cloth made of fibers such as nylon, polyester, and acrylic. When an orientation control layer is provided that is oriented in a specific direction oblique to the longitudinal direction of a long film, the rubbing direction is preferably set at an angle that matches the direction. The angle can be adjusted by adjusting the angle between the rubbing roller and the film, the film transport speed, and the number of rotations of the roller, etc.
[0104] (Photo alignment control layer) The photo-alignment control layer is preferably an alignment film in which a coating material for a photo-alignment control layer containing a polymer and / or monomer having a photoreactive group and a solvent is applied to a coat layer or a releasable substrate, and then polarized light, preferably polarized ultraviolet light, is applied to the coating material to impart an alignment control force. The photoreactive group is preferably a group that generates a liquid crystal alignment ability upon light irradiation, and specifically, it is preferably a group that generates a photoreaction that is the origin of the liquid crystal alignment ability, such as molecular orientation induction or isomerization reaction, dimerization reaction, photocrosslinking reaction, or photodecomposition reaction, which occurs upon light irradiation. Among the photoreactive groups, those that cause a dimerization reaction or a photocrosslinking reaction are preferred in terms of excellent alignment and maintaining the smectic liquid crystal state. The photoreactive group that can cause the above-mentioned reaction is preferably an unsaturated bond, particularly a double bond, and particularly preferably a group having at least one selected from the group consisting of a C=C bond, a C=N bond, an N=N bond, and a C=O bond.
[0105] Examples of photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazolyl groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. Examples of photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, formazan groups, and groups having azoxybenzene as a basic structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have substituents such as alkyl groups, alkoxy groups, aryl groups, allyloxy groups, cyano groups, alkoxycarbonyl groups, hydroxyl groups, sulfonic acid groups, and halogenated alkyl groups. The number of substituents is not particularly limited, and may be, for example, 1, 2, 3, or 4.
[0106] Among them, photoreactive groups capable of photodimerization are preferred, and cinnamoyl and chalcone groups are preferred because the amount of polarized light irradiation required for photoalignment is relatively small, and a photoalignment control layer having excellent thermal stability and stability over time is easily obtained. Furthermore, as the polymer having a photoreactive group, one having a cinnamoyl group such that the terminal of the polymer side chain has a cinnamic acid structure is particularly preferred. Examples of the main chain structure include polyimide, polyamide, (meth)acrylic, and polyester.
[0107] Specific examples of the orientation control layer include those described in JP-A-2006-285197, JP-A-2007-76839, JP-A-2007-138138, JP-A-2007-94071, JP-A-2007-121721, JP-A-2007-140465, JP-A-2007-156439, JP-A-2007-133184, and JP-A-2009 Examples of the orientation control layers include those described in JP-A-109831, JP-A-2002-229039, JP-A-2002-265541, JP-A-2002-317013, JP-T-2003-520878, JP-T-2004-529220, JP-A-2013-33248, JP-A-2015-7702, and JP-A-2015-129210.
[0108] The solvent for the coating material for the photo-alignment control layer can be any solvent that dissolves the polymer and monomer having a photoreactive group. Specific examples include those mentioned in the method for forming the alignment control layer by rubbing treatment. It is also preferable to add a photopolymerization initiator, a polymerization inhibitor, and various stabilizers to the coating material for the photo-alignment control layer. In addition, the coating material for the photo-alignment control layer may contain polymers other than the polymer and monomer having a photoreactive group, and monomers that do not have a photoreactive group and are copolymerizable with the monomer having a photoreactive group.
[0109] The concentration of the polymer or monomer of the coating material for the photo-alignment control layer, the coating method, and the drying conditions can be the same as those mentioned in the formation method of the rubbing treatment alignment control layer. The preferred thickness is also the same as that of the rubbing treatment alignment control layer.
[0110] It is preferable that the polarized light is irradiated from the direction of the surface of the photo-alignment control layer before alignment.
[0111] The wavelength of the polarized light is preferably in a wavelength range where the photoreactive group of the polymer or monomer having the photoreactive group can absorb light energy. Specifically, ultraviolet light having a wavelength of 250 to 400 nm is preferable. Examples of the light source of the polarized light include a xenon lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, and an ultraviolet laser such as KrF or ArF, and the high-pressure mercury lamp, the ultra-high-pressure mercury lamp, and the metal halide lamp are preferable.
[0112] Polarized light can be obtained, for example, by passing the light from the light source through a polarizer. The direction of polarization can be adjusted by adjusting the polarization angle of the polarizer. Examples of polarizers include polarizing filters, polarizing prisms such as Glan-Thompson and Glan-Taylor, and wire grid type polarizers. It is preferable that the polarized light is substantially parallel light.
[0113] By adjusting the angle of the irradiated polarized light, the direction of the alignment regulating force of the photoalignment layer can be adjusted as desired.
[0114] The irradiation intensity varies depending on the type and amount of polymerization initiator and resin (monomer), but for example, it is 10 to 10,000 mJ / cm at 365 nm. 2 is preferable, and more preferably 20 to 5000 mJ / cm 2 is preferred.
[0115] (Liquid crystal polarizer) The liquid crystal polarizer functions as a polarizer that transmits light in only one direction, and preferably contains a dichroic dye.
[0116] <Dichroic dye> The dichroic dye is preferably an organic dye having different absorbance in the long axis direction and in the short axis direction of the molecule.
[0117] The dichroic dye preferably has a maximum absorption wavelength (λMAX) in the range of 300 to 700 nm. Examples of such dichroic dyes include acridine dyes, oxazine dyes, cyanine dyes, naphthalene dyes, azo dyes, and anthraquinone dyes, and among these, azo dyes are preferred. Examples of azo dyes include monoazo dyes, bisazo dyes, trisazo dyes, tetrakisazo dyes, and stilbene azo dyes, and are preferably bisazo dyes and / or trisazo dyes. The dichroic dyes may be used alone or in combination of two or more kinds, but in order to adjust the color tone (achromatic color), it is preferable to combine two or more kinds. In particular, it is preferable to combine three or more kinds. In particular, it is preferable to combine three or more kinds of azo compounds.
[0118] Preferred azo compounds include dyes described in JP-A-2007-126628, JP-A-2010-168570, JP-A-2013-101328, and JP-A-2013-210624.
[0119] The dichroic dye is preferably a dichroic dye polymer introduced into the side chain of a polymer such as an acrylic polymer. Examples of the dichroic dye polymer include the polymers described in JP-A-2016-4055 and the polymers obtained by polymerizing the compounds of [Chemical formula 6] to [Chemical formula 12] in JP-A-2014-206682.
[0120] From the viewpoint of obtaining good alignment of the dichroic dye, the content of the dichroic dye in the liquid crystal polarizer is preferably from 0.1 to 30 mass %, more preferably from 0.5 to 20 mass %, further preferably from 1.0 to 15 mass %, and particularly preferably from 2.0 to 10 mass %.
[0121] The liquid crystal polarizer preferably further contains a polymerizable liquid crystal compound in order to improve the film strength, polarization degree, and film uniformity. The polymerizable liquid crystal compound also includes a polymerized film.
[0122] <Polymerizable liquid crystal compound> The polymerizable liquid crystal compound is preferably a compound having a polymerizable group and exhibiting liquid crystallinity. The polymerizable group means a group involved in a polymerization reaction, and is preferably a photopolymerizable group. Here, the photopolymerizable group means a group capable of undergoing a polymerization reaction by an active radical generated from a photopolymerization initiator described later, an acid, or the like. Examples of the polymerizable group include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among these, an acryloyloxy group, a methacryloyloxy group, a vinyloxy group, an oxiranyl group, and an oxetanyl group are preferred, and an acryloyloxy group is more preferred. The compound exhibiting liquid crystallinity may be a thermotropic liquid crystal or a lyotropic liquid crystal. The thermotropic liquid crystal may be a nematic liquid crystal or a smectic liquid crystal.
[0123] The polymerizable liquid crystal compound is preferably a smectic liquid crystal compound, and more preferably a high-order smectic liquid crystal compound, in that higher polarization properties can be obtained. When the liquid crystal phase formed by the polymerizable liquid crystal compound is a high-order smectic phase, a liquid crystal polarizer with a higher degree of orientation order can be produced.
[0124] Specific preferred polymerizable liquid crystal compounds include those described in, for example, JP2002-308832A, JP2007-16207A, JP2015-163596A, JP2007-510946A, JP2013-114131A, WO2005 / 045485A, Lub et al. Recl. Trav. Chim. Pays-Bas, 115, 321-328(1996), and the like.
[0125] From the viewpoint of increasing the alignment property of the polymerizable liquid crystal compound, the content of the polymerizable liquid crystal compound in the liquid crystal polarizer is preferably 70 to 99.5 mass %, more preferably 75 to 99 mass %, even more preferably 80 to 97 mass %, and particularly preferably 83 to 95 mass %.
[0126] The liquid crystal polarizer can be provided by applying a coating material for liquid crystal polarizers. The coating material for liquid crystal polarizers may contain additives such as a solvent, a polymerization initiator, a sensitizer, a polymerization inhibitor, a leveling agent, a polymerizable non-liquid crystal compound, a crosslinking agent, etc. The additives may be used alone or in combination of two or more kinds.
[0127] As the solvent, those exemplified as the solvent for the coating material for the alignment control layer are preferably used.
[0128] The polymerization initiator is not limited as long as it polymerizes the polymerizable liquid crystal compound, but a photopolymerization initiator that generates active radicals by light is preferable. Examples of the polymerization initiator include benzoin compounds, benzophenone compounds, alkylphenone compounds, acylphosphine oxide compounds, triazine compounds, iodonium salts, and sulfonium salts.
[0129] The sensitizer is preferably a photosensitizer, and examples thereof include a xanthone compound, an anthracene compound, phenothiazine, and rubrene.
[0130] Examples of the polymerization inhibitor include hydroquinones, catechols, and thiophenols.
[0131] The polymerizable non-liquid crystal compound is preferably one that copolymerizes with the polymerizable liquid crystal compound, and for example, when the polymerizable liquid crystal compound has a (meth)acryloyloxy group, (meth)acrylates can be mentioned. The (meth)acrylates may be monofunctional or polyfunctional. By using polyfunctional (meth)acrylates, the strength of the polarizer can be improved. When a polymerizable non-liquid crystal compound is used, the content thereof in the liquid crystal polarizer is preferably 1 to 15% by mass, more preferably 2 to 10% by mass, and particularly preferably 3 to 7% by mass, in order to suppress a decrease in the degree of polarization.
[0132] Examples of the crosslinking agent include compounds capable of reacting with functional groups of the polymerizable liquid crystal compound and the polymerizable non-liquid crystal compound, such as isocyanate compounds, melamine, epoxy resins, and oxazoline compounds.
[0133] The liquid crystal polarizer coating material is applied onto the coating layer, onto the releasable substrate, or onto the alignment control layer, and then, if necessary, dried, heated, and cured, whereby a liquid crystal polarizer can be produced.
[0134] As the coating method, known methods such as coating methods such as gravure coating, die coating, bar coating and applicator methods, and printing methods such as flexography can be used.
[0135] Drying is preferably carried out in a dryer (such as a hot air dryer or an infrared dryer) at a temperature of 30 to 170° C. The drying temperature is more preferably 50 to 150° C., and even more preferably 70 to 130° C., and the drying time is preferably 0.5 to 30 minutes, more preferably 1 to 20 minutes, and even more preferably 2 to 10 minutes.
[0136] In order to more firmly align the dichroic dye and the polymerizable liquid crystal compound in the liquid crystal polarizer, heating can be performed. The heating temperature is preferably set to a temperature range in which the polymerizable liquid crystal compound forms a liquid crystal phase.
[0137] When the liquid crystal polarizer coating material contains a polymerizable liquid crystal compound, it is preferable to cure it. Examples of the curing method include heating and light irradiation, and light irradiation is preferable. The dichroic dye can be fixed in an oriented state by curing. Curing is preferably performed in a state in which a liquid crystal phase is formed in the polymerizable liquid crystal compound, and may be cured by light irradiation at a temperature at which the liquid crystal phase is exhibited. Examples of light for light irradiation include visible light, ultraviolet light, and laser light. In terms of ease of handling, ultraviolet light is preferable.
[0138] The irradiation intensity varies depending on the type and amount of polymerization initiator and resin (monomer), but for example, it is 100 to 10,000 mJ / cm at 365 nm. 2 is preferable, and more preferably 200 to 5000 mJ / cm2 is preferred.
[0139] When a liquid crystal polarizer paint is applied onto an orientation control layer, the pigment is oriented along the orientation direction of the orientation layer, resulting in a liquid crystal polarizer having a polarization transmission axis in a predetermined direction. However, if an orientation control layer is not provided, the liquid crystal polarizer can also be oriented by irradiating it with polarized light to harden the liquid crystal polarizer paint.
[0140] Any method may be used for providing the polarizer, but methods (b), (c) and (d) are particularly preferred.
[0141] (phase contrast layer) It is also a preferred embodiment that LP1 has a retardation layer on the opposite side of the coating layer of the polarizer. Representative examples of the retardation layer include those provided between the polarizer and the image display cell for optical compensation in the case of a liquid crystal display device, and those (λ / 4 retardation layer, λ / 2 retardation layer, etc.) provided for anti-reflection in the case of an organic EL display device, a micro LED display device, etc.
[0142] The retardation layer is preferably a layer provided by coating a retardation paint, more preferably a layer provided by coating a paint containing a liquid crystal compound or a polymer compound. The retardation layer can be appropriately selected from positive or negative A plates, positive or negative C plates, O plates, etc. according to the purpose. As the C plate, a plate in which a discotic liquid crystal compound is horizontally aligned (JP Patent Publication 2008-40309 A), a plate in which a chiral agent is added to a rod-shaped liquid crystal compound to form a twisted helical structure alignment, and a polymer compound layer are preferred, and a plate in which a discotic liquid crystal compound is horizontally aligned is particularly preferred. As the A plate, a plate in which a rod-shaped liquid crystal compound is horizontally aligned can be mentioned, and the alignment direction (slow axis direction) is preferably parallel to the transmission axis of the polarizer.
[0143] Examples of the polymeric compound include polymers having at least one aromatic ring in the repeating unit, such as polyimide, polyamideimide, polyester, polyetherketone, polyaryletherketone, and polyesterimide.
[0144] The liquid crystal compound is preferably a polymerizable liquid crystal compound having a polymerizable group such as a double bond, in terms of being able to fix the alignment state. Also, the liquid crystal compound may be a rod-shaped liquid crystal compound, a discotic liquid crystal compound, or the like.
[0145] Examples of the rod-shaped liquid crystal compound include rod-shaped liquid crystal compounds having a polymerizable group described in JP-A-2002-030042, JP-A-2004-204190, JP-A-2005-263789, JP-A-2007-119415, JP-A-2007-186430, and JP-A-11-513360.
[0146] Specific examples of rod-shaped liquid crystal compounds include: CH2=CHCOO-(CH2) m -O-Ph1-COO-Ph2-OCO-Ph1-O-(CH2) n -OCO-CH=CH2 CH2=CHCOO-(CH2) m -O-Ph1-COO-NPh-OCO-Ph1-O-(CH2) n -OCO-CH=CH2 CH2=CHCOO-(CH2) m -O-Ph1-COO-Ph2-OCH3 CH2=CHCOO-(CH2) m -O-Ph1-COO-Ph1-Ph1-CH2CH(CH3)C2H5 (In the formula, m and n are integers from 2 to 6; Ph1 and Ph2 are 1,4-phenylene groups (Ph2 may be substituted with a methyl group at the 2-position), NPh is the 2,6-naphthylene group. Examples include:
[0147] These rod-shaped liquid crystal compounds are commercially available as LC242 manufactured by BASF, and these compounds can be used.
[0148] These rod-shaped liquid crystal compounds may be used in combination of two or more kinds in any ratio.
[0149] Examples of discotic liquid crystal compounds include benzene derivatives, truxene derivatives, cyclohexane derivatives, azacrowns, phenylacetylene macrocycles, etc. Various discotic liquid crystal compounds are described in JP-A-2001-155866, and these are preferably used.
[0150] Among them, as the discotic liquid crystal compound, a compound having a triphenylene ring represented by the following general formula (1) is preferably used. [ka] In the formula, R1 to R6 are each independently hydrogen, halogen, an alkyl group, or a group represented by -OX (wherein X is an alkyl group, an acyl group, an alkoxybenzyl group, an epoxy-modified alkoxybenzyl group, an acryloyloxy-modified alkoxybenzyl group, or an acryloyloxy-modified alkyl group). R1 to R6 are preferably an acryloyloxy-modified alkoxybenzyl group represented by the following general formula (2) (m is an integer of 4 to 10).
[0151] [ka]
[0152] When used as an optical compensation for a liquid crystal display device, the degree of retardation is appropriately set according to the type of liquid crystal cell and the properties of the liquid crystal compound used in the liquid crystal cell. For example, in the case of a TN type, a tilted alignment is preferably used in which the tilt angle is changed in the thickness direction using a discotic liquid crystal. In the case of a VA type or an IPS type, a C plate layer or an A plate layer using a rod-shaped liquid crystal compound or a discotic liquid crystal compound is preferably used. In addition, in the case of a λ / 4 retardation layer and a λ / 2 retardation layer, it is preferable to use a rod-shaped compound to form an A plate layer. These retardation layers may be used as a single layer, or multiple retardation layers may be used in combination.
[0153] The method for forming the retardation layer may be a method of applying a paint for the retardation layer onto a polarizer, or a method of transferring the retardation layer (a laminate for transferring the retardation layer) on a releasable substrate to a polarizer. In addition, the polarizer (e.g., PVA polarizer, liquid crystal polarizer) and the retardation layer (a laminate for transferring the polarizer and the retardation layer) on the releasable substrate may be transferred to a coat layer. The laminate for transferring the retardation layer and the releasable substrate for the laminate for transferring the polarizer and the retardation layer may be the releasable substrate for the laminate for transferring the PVA polarizer.
[0154] The coating material for the retardation layer may contain a solvent, a polymerization initiator, a sensitizer, a polymerization inhibitor, a leveling agent, a polymerizable non-liquid crystal compound, a crosslinking agent, etc. These can be those described in the alignment control layer or the liquid crystal polarizer.
[0155] The method of orienting the liquid crystal compound of the retardation layer can be the same as the method of orienting the liquid crystal polarizer described above. That is, the method of directly applying the coating material for the retardation layer to the polarizer or the releasable substrate and irradiating it with polarized ultraviolet light, the method of rubbing the polarizer or the releasable substrate, the method of providing an orientation control layer between the polarizer and the retardation layer, etc. are included. Among these conditions, the conditions described for the orientation control layer or the liquid crystal polarizer are preferably used.
[0156] A plurality of retardation layers may be provided. In this case, a laminate having a plurality of retardation layers on one releasable substrate may be used to transfer a plurality of retardation layers to a polarizer. Alternatively, a plurality of laminates having one retardation layer on one releasable substrate may be used to transfer the retardation layers one by one to a polarizer. The coating method and the transfer method may be combined.
[0157] The retardation layer can be appropriately selected depending on the type of image display cell. Retardation layers used in typical liquid crystal cells will be described below.
[0158] (Retardation layer for TN type liquid crystal cells) In a TN type liquid crystal cell, the retardation layer is preferably a layer formed of a discotic liquid crystal compound, and particularly preferably a layer in which the discotic planes of the discotic structural units of the discotic liquid crystal compound are oriented with gradually changing inclination angles in the thickness direction of the retardation layer.
[0159] The lower limit of the angle between the disc plane of the discotic structural unit of the discotic liquid crystal compound and the plane of the retardation layer is preferably 5 degrees, more preferably 10 degrees, and the upper limit of this angle is preferably 85 degrees, more preferably 80 degrees.
[0160] The lower limit of the difference between the minimum and maximum angles between the disc plane of the discotic structural unit of the discotic liquid crystal compound and the plane of the retardation layer is preferably 10 degrees, more preferably 15 degrees, and the upper limit of this difference is preferably 60 degrees, more preferably 55 degrees.
[0161] The alignment direction of the discotic liquid crystal compound in the planar direction of the retardation layer is preferably adjusted so that the disc surface of the discotic structure of the discotic liquid crystal compound is parallel to the absorption axis of the polarizer when the disc surface is upright.
[0162] The lower limit of the retardation Rth (((nx+ny) / 2-nz)×d) in the thickness direction of the retardation layer is preferably 20 nm, more preferably 50 nm, and even more preferably 100 nm. The upper limit of Rth is preferably 400 nm, more preferably 380 nm, and even more preferably 350 nm.
[0163] The retardation layer does not have a specific optical axis, and preferably has a minimum absolute value of retardation in a direction inclined from the normal direction. The lower limit of the angle between the direction in which the absolute value of retardation is minimum and the normal direction is preferably 5 degrees, more preferably 10 degrees. The upper limit of this angle is preferably 50 degrees, more preferably 40 degrees.
[0164] By providing the retardation layer with the above characteristics, it is possible to effectively prevent light leakage and color change when the image display device is viewed obliquely, and to widen the viewing angle.
[0165] In general, it is preferable that the absorption axis of the polarizer used in a TN type liquid crystal cell is set at 45 degrees to the side of the liquid crystal cell. When the polarizer transfer laminate is wound into a roll, it is preferable that the direction of the absorption axis of the polarizer is set at 45 degrees to the longitudinal direction (e.g., the film flow direction or the roll winding direction) of the rolled polarizer transfer laminate in terms of convenience of bonding to the liquid crystal cell. In this case, it is preferable that the retardation layer is laminated on the rolled polarizer transfer laminate in accordance with the absorption axis direction of the polarizer.
[0166] In such a roll-shaped laminate for polarizer transfer having an inclined absorption axis, the polarizer is preferably a liquid crystal polarizer from the viewpoint of ease of production.
[0167] The polarizer transfer laminate may be prepared by cutting a roll of the polarizer transfer laminate obliquely to the longitudinal direction so that the absorption axis of the polarizer is parallel or perpendicular to the longitudinal direction, and using this to transfer the laminate to a liquid crystal cell.
[0168] When the retardation layers are provided on the viewing side and the light source side of the liquid crystal cell, the viewing side retardation layer and the light source side retardation layer are not particularly limited as long as they are optically compensated as a whole, and the retardation layers on the viewing side and the light source side may not be the same. For example, when the viewing side retardation layer is an inclined alignment layer of discotic liquid crystal, it is also a preferred embodiment that the light source side retardation layer is not provided, or is an A plate layer or a C plate layer, or a composite layer thereof. It is also a preferred embodiment that the viewing side retardation layer and the light source side retardation layer are the same retardation layer.
[0169] (Retardation layer for VA type liquid crystal cells) In a VA type liquid crystal cell, the index ellipsoid of the retardation layer is preferably in the shape of a thick disk (eg, anpan-shaped) to an elliptical plate (eg, hamburger-shaped).
[0170] The in-plane retardation (Re) of the retardation layer is preferably from 0 to 200 nm, the retardation in the thickness direction (Rth) is preferably from 70 to 400 nm, and it is preferable to satisfy Re < Rth.
[0171] The lower limit of Re is more preferably 10 nm, and even more preferably 20 nm. The upper limit of Re is more preferably 100 nm, and even more preferably 70 nm.
[0172] The lower limit of Rth is more preferably 100 nm, and even more preferably 120 nm. The upper limit of Rth is more preferably 350 nm, and even more preferably 300 nm, and particularly preferably 250 nm.
[0173] The lower limit of Rth - Re is preferably 20 nm, more preferably 40 nm, and even more preferably 50 nm. The upper limit is preferably 300 nm, more preferably 250 nm, and even more preferably 200 nm.
[0174] By setting Re, Rth, and the difference (Rth - Re) within the above ranges, it is possible to effectively reduce the occurrence of light leakage due to the angle, the reduction of gradation, and the deviation of color tone.
[0175] The retardation layer is preferably a retardation layer formed of a discotic liquid crystal compound or a rod-like liquid crystal compound. Further, specific examples of the retardation layer include only a C-plate layer (for example, a negative C-plate layer), only an A-plate layer (for example, a positive A-plate layer), a combination of a C-plate layer and an A-plate layer, and an orthogonal combination of A-plate layers.
[0176] When the retardation layer is provided on the viewing side and the light source side of the liquid crystal cell, the viewing side retardation layer and the light source side retardation layer are not particularly limited as long as they are optically compensated as a whole, and the retardation layer on the viewing side and the light source side may not be the same. For example, when the optical compensation is performed by a combination of the A plate layer and the C plate layer, the viewing side retardation layer may be a combination of the A plate layer and the C plate layer, and the light source side retardation layer may not be provided, or the viewing side retardation layer may be the A plate and the light source side retardation layer may be the C plate layer, or the viewing side retardation layer may be the C plate and the light source side retardation layer may be the A plate layer. It is also a preferred embodiment that the viewing side retardation layer and the light source side retardation layer are the same retardation layer.
[0177] The absorption axis of a polarizer (for example, an absorptive polarizer in the case of a composite polarizer) is preferably parallel or perpendicular to the side of a liquid crystal cell, and the absorption axis of a polarizer (for example, a roll film) is preferably parallel or perpendicular to the longitudinal direction (for example, the film flow direction or the roll winding direction).
[0178] (Retardation layer for IPS type liquid crystal cells) In the case of an IPS type liquid crystal cell, it is preferable not to provide a retardation layer, but a retardation layer may be provided. In an IPS type liquid crystal cell, the influence of the liquid crystal compound of the liquid crystal cell is small, but when the display is viewed from an oblique direction, the absorption axis of the light source side polarizer and the absorption axis of the viewing side polarizer are shifted from 90 degrees, causing light leakage. Therefore, when a retardation layer is used, it is preferable that the retardation layer is one that corrects this angle shift.
[0179] It is preferable that the absolute value of Re of the retardation layer is selected from the range of 0 to 360 nm, and the absolute value of Rth of the retardation layer is selected from the range of 0 to 360 nm according to the design concept. The retardation layer is preferably a combination of a positive C plate and a positive A plate, in which a plurality of index ellipsoids (e.g., hamburger-shaped ones) are arranged horizontally. It is preferable that nx>nz≧ny or nz>nx>ny in each plate.
[0180] It is also preferable to combine a plurality of retardation layers and stack them in the vertical direction. The retardation layer preferably has at least a positive C plate layer. The Re of the positive C plate layer is preferably -10 to 10 nm, more preferably -5 to 5 nm. The Rth of the positive C plate layer is preferably -220 to -50 nm, more preferably -200 to -60 nm. The positive C plate layer is preferably one in which a rod-shaped liquid crystal compound is vertically aligned.
[0181] The positive C plate layer is preferably combined with a positive A plate layer. The Re of the positive A plate layer is preferably 50 to 230 nm, more preferably 80 to 220 nm. The Rth of the positive A plate layer is preferably 30 to 150 nm, more preferably 60 to 130 nm. The nz ((nx-nz) / (nx-ny)) of the positive A plate layer is preferably 0.8 to 1.2, more preferably 0.9 to 1.1. The positive A plate layer is preferably one in which rod-shaped liquid crystal compounds are horizontally aligned, and the alignment direction (slow axis direction) is preferably parallel to the transmission axis of the polarizer.
[0182] The order of lamination of the positive C plate layer and the positive A plate layer is not limited, but it is preferable that the positive C plate layer is on the liquid crystal cell side. It is also preferable that the combination of the positive C plate layer and the positive A plate layer is used as a retardation layer on the viewing side of the liquid crystal cell, and no retardation layer is provided on the light source side of the liquid crystal cell, but a separate retardation layer may be provided. The positive C plate layer may be used on either the light source side or the viewing side, and the positive A plate layer may be used on the other side. In this case, the optical characteristics can be adjusted appropriately.
[0183] In the case of an IPS type liquid crystal cell, as in the case of a VA type liquid crystal cell, it is preferable that the absorption axis of the polarizer (e.g., a roll film) is oriented parallel or perpendicular to the longitudinal direction (e.g., the film flow direction or the winding direction of the roll).
[0184] In the above description of the retardation layers for each type of liquid crystal cell, the angles (45 degrees, parallel, perpendicular) preferably include an error of 5 degrees, more preferably 3 degrees, and further preferably 2 degrees.
[0185] (Organic EL display device) For the purpose of preventing reflection, the organic EL display device preferably has a circular polarizing plate on the viewing side of the organic EL cell. The retardation layer in the circular polarizing plate is preferably a λ / 4 retardation layer. The λ / 4 retardation layer will be described in detail below.
[0186] (λ / 4 retardation layer) The λ / 4 retardation layer can convert linearly polarized light that has passed through a polarizer into circularly polarized light, and can convert circularly polarized light reflected by wiring in an organic EL cell, a glass substrate, etc., into linearly polarized light that is shifted by 90 degrees from the incident linearly polarized light. The λ / 4 retardation layer may be a single-layer λ / 4 retardation layer, or a composite λ / 4 retardation layer of a λ / 4 retardation layer and a λ / 2 retardation layer. The λ / 4 retardation layer may be provided with a C-plate layer or the like. In this specification, the single-layer retardation layer and the composite λ / 4 retardation layer may be collectively referred to as a λ / 4 retardation layer.
[0187] The in-plane retardation of the λ / 4 retardation layer is preferably 100 to 180 nm, more preferably 120 to 150 nm, and the in-plane retardation of the λ / 2 retardation layer is preferably 200 to 360 nm, more preferably 240 to 300 nm.
[0188] (angle of slow axis of λ / 4 retardation layer) In the case of a single λ / 4 retardation layer, the angle between the alignment axis (slow axis) of the λ / 4 retardation layer and the transmission axis of the polarizer is preferably 35 to 55 degrees, more preferably 40 to 50 degrees, and further preferably 42 to 48 degrees.
[0189] In the case of a composite λ / 4 retardation layer in which a λ / 4 retardation layer and a λ / 2 retardation layer are combined, it is preferable that the alignment axis (slow axis) of each retardation layer is arranged at an angle such that both layers have a retardation of λ / 4. Specifically, the angle (θ) between the alignment axis (slow axis) of the λ / 2 retardation layer and the transmission axis of the polarizer is preferably 5 to 20 degrees, more preferably 7 to 17 degrees. The angle between the alignment axis (slow axis) of the λ / 2 retardation layer and the alignment axis (slow axis) of the λ / 4 retardation layer is preferably in the range of 2θ+45 degrees±10 degrees, more preferably in the range of 2θ+45 degrees±5 degrees, and even more preferably in the range of 2θ+45 degrees±3 degrees.
[0190] Examples of the λ / 4 retardation layer can be found in JP2008-149577A, JP2002-303722A, WO2006 / 100830A, JP2015-64418A, JP2018-10086A, and the like.
[0191] Furthermore, in order to reduce the change in color when viewed from an oblique angle, it is also a preferred embodiment to provide a C plate layer on the λ / 4 retardation layer. As the C plate layer, a positive or negative C plate layer is selected according to the characteristics of the λ / 4 retardation layer and the λ / 2 retardation layer.
[0192] In the composite λ / 4 retardation layer, the lamination method of the λ / 4 retardation layer and the λ / 2 retardation layer can be, for example, A method in which a λ / 2 retardation layer is formed on a polarizer by transfer, and then a λ / 4 retardation layer is formed on top of that by transfer. A method in which a λ / 2 retardation layer is formed on a polarizer by transfer, and then a λ / 4 retardation layer is formed on top of that by coating. A method in which a λ / 2 retardation layer is formed on a polarizer by coating, and a λ / 4 retardation layer is then formed on top of the layer by transfer. A method of providing a λ / 2 retardation layer and a λ / 4 retardation layer on a polarizer by coating A method in which a λ / 4 retardation layer and a λ / 2 retardation layer are provided in this order on a release substrate, and then these are transferred onto a polarizer. Examples include:
[0193] As a method for laminating a C plate layer on a λ / 4 retardation layer, various methods can be used, such as a method of providing a C plate layer on a λ / 4 retardation layer on a polarizer by transfer, a method of providing a C plate layer on a releasable substrate, and further providing a single-layer λ / 4 retardation layer or a composite λ / 4 retardation layer (λ / 2 retardation layer and λ / 4 retardation layer) on the C plate layer, and then transferring them to a polarizer.
[0194] The retardation of the retardation layer can be measured, for example, by using an automatic birefringence meter (KOBRA series, Oji Measurement Co., Ltd., etc.) to tilt the surface of the retardation layer from a position of 0 degrees relative to the normal direction to an in-plane optical axis direction at 10 degree intervals up to 50 degrees, and then inputting the film thickness and the average refractive index na into the accompanying software to perform calculations.
[0195] As another method, for example, the retardation (R0=Re) is measured from the normal direction using the above-mentioned automatic birefringence meter, and the retardation (R40) is measured by tilting the surface of the retardation layer 40 degrees from the normal direction toward the in-plane optical axis direction. From these retardation values, the thickness d of the retardation layer, and the average refractive index na of the retardation layer, nx, ny, and nz are calculated using the following formulas (2), (3), and (4), and Rth can be calculated by substituting these values into formula (1). Rth = [(nx + ny) / 2 - nz] × d (1) R0 = (nx-ny) × d (2) R40 = (nx-ny') × d / cos(φ) (3) (nx+ny+nz) / 3=na (4) In addition, φ=sin -1 [sin(40°) / na] ny'=ny×nz / 〔ny 2 ×sin 2 (φ)+nz 2 ×cos 2 (φ) 1 / 2
[0196] The average refractive index na may be, for example, a value obtained by the following method. After removing the solvent from the retardation layer paint, a thin film slice was obtained by irradiating it with ultraviolet light in an amorphous state, and the value was measured with an Abbe refractometer. Values of retardation layers made of similar compositions or their average values The value calculated when the film is oriented so that the optical axis is in the plane, Re is measured, nx and ny are calculated from the film thickness, and nz is set to the same value as nx (negative A plate) or ny (positive A plate).
[0197] Examples of samples for measuring the retardation of the retardation layer include a glass film having a retardation layer formed thereon under the same conditions, and a releasable substrate having a retardation layer formed thereon under the same conditions, which is then transferred onto a glass plate.
[0198] (interlayer protective layer) LP1 may have an interlayer protective layer between any two layers (for example, between the polarizer and the retardation layer, the surface of the retardation layer where the polarizer is not laminated, between a plurality of retardation layers, between an adhesive or pressure-sensitive adhesive and a polarizer or retardation layer). The interlayer protective layer can prevent the components of each layer or the solvent used from migrating to the adjacent layers, causing a decrease in the degree of polarization or a change in the retardation. The interlayer protective layer may be provided on a releasable substrate together with the retardation layer and / or the polarizer, and then transferred to an object.
[0199] Examples of the interlayer protective layer include a transparent resin layer. Examples of the transparent resin include, but are not limited to, polyvinyl alcohol, ethylene vinyl alcohol copolymer, polyester, polyurethane, polyamide, polystyrene, acrylic resin, and epoxy resin. The transparent resin may be crosslinked with a crosslinking agent to form a crosslinked structure. The transparent resin may also be a hard coat obtained by curing (for example, photocuring) a curable (for example, photocurable) composition such as acrylic. The interlayer protective layer may be provided on an alignment film, and then the interlayer protective layer may be subjected to a rubbing treatment, and a liquid crystal compound alignment layer (such as a liquid crystal polarizer or a retardation layer) may be provided thereon without providing an alignment control layer.
[0200] It is preferable that the retardation layer is provided directly on the polarizer or via an interlayer protective layer. The retardation layer is provided directly on the polarizer, which includes not only that the polarizer and the retardation layer are in contact with each other, but also that the polarizer and the retardation layer are bonded together with an adhesive or pressure-sensitive adhesive. The adhesive or pressure-sensitive adhesive used for bonding is one mentioned above.
[0201] (Polarizer transfer laminate LP2) LP2 preferably has a polarizer on a release film. Also, LP2 preferably has a retardation layer on the side of the polarizer opposite to the release film, and preferably has a coating layer between the release film and the polarizer.
[0202] The release film used in LP2 is the same as that described for LP1. The release film used in LP2 may be the same as or different from the release film used in LP1.
[0203] The coating layer used in LP2 is similar to that described for LP1. The coating layer used in LP2 may be the same as or different from the coating layer used in LP1.
[0204] The polarizer used in LP2 is similar to that described for LP1. The polarizer used in LP2 may be the same as or different from the polarizer used in LP1.
[0205] In addition, when LP2 does not have a coating layer between the release film and the polarizer, in the explanation of the method of providing a polarizer and an orientation control layer described in LP1, the "coating layer" can be read as the "release film" and the "coating layer surface of the laminate of the release film and the coating layer" can be read as the "release surface of the release film."
[0206] The retardation layer used in LP2 is the same as that described for LP1. The retardation layer used in LP2 may be the same as or different from the retardation layer used in LP1.
[0207] LP1 and LP2 may have a masking film attached to the surface (polarizer surface or retardation layer surface, etc.) on which the image display cell is laminated in order to protect the surface. As the masking film, a film having an acrylic, rubber, polyolefin, or other adhesive layer provided on a substrate such as polyethylene, polypropylene, or polyester is preferably used. Instead of the masking film, a releasable substrate used when transferring the polarizer or retardation layer, etc., may remain. The masking film and the releasable substrate are preferably peeled off immediately before bonding to the image display cell or immediately before providing the pressure-sensitive adhesive layer or adhesive layer. LP1 and LP2 may be provided with an adhesive layer or pressure-sensitive adhesive layer for bonding an image display cell to the polarizer surface or retardation layer surface, or may be provided with a separator laminated on the adhesive layer or pressure-sensitive adhesive layer. The separator may be any of those listed as examples of the releasable substrate for the PVA polarizer transfer laminate.
[0208] It is preferable that LP1 and LP2 do not have a self-supporting film other than the film for manufacturing process as a constituent layer. Here, the self-supporting film is a film that is independently manufactured. For example, a polarizer protective film can be mentioned as a self-supporting film. The film for manufacturing process is a member that is used for manufacturing a laminate for polarizer transfer but is finally removed in the image display device, and examples thereof include a release film, a release substrate, a masking film, a separator, etc.
[0209] Each layer constituting LP1 and LP2 is preferably provided by coating or transfer, which allows further reduction in thickness and weight.
[0210] (Image display cell and image display device) Generally, a liquid crystal cell is a liquid crystal display device in which a liquid crystal compound is sealed in a glass plate having electrodes, and an organic EL cell is an organic EL display device in which an organic light-emitting body is sealed in a glass plate having electrodes, etc. In the present invention, such a state before the provision of a polarizing plate is referred to as an image display cell.
[0211] Generally, an image display cell having a polarizing plate provided thereon and capable of displaying an image when a signal is input thereto, and a member such as a touch panel laminated thereon, are called an image display panel, and an image display panel incorporating a controller for signals for displaying an image and a housing or the like are sometimes called an image display device. The image display device of the present invention preferably includes an image display panel, i.e., an image display device capable of displaying an image when a signal is input thereto.
[0212] (Liquid crystal display device) The liquid crystal display device is preferably provided with polarizers on both sides of the liquid crystal cell. The polarizer on at least one side of the liquid crystal display panel is preferably the above-mentioned polarizer, and the polarizers on both sides are preferably the above-mentioned polarizer. The order of providing the polarizers on the liquid crystal cell may be the viewing side first or the light source side first, or they may be provided simultaneously.
[0213] (LP1 pasting) The liquid crystal display device preferably has LP1 on the viewing side of the liquid crystal cell. A method of bonding LP1 to the viewing side of the liquid crystal cell includes bonding the viewing side of the liquid crystal cell to the surface of LP1 opposite to the release film (the polarizer surface, or the surface of the other layer if another layer is laminated on the polarizer) using an adhesive or pressure-sensitive adhesive. As the adhesive or pressure-sensitive adhesive, an adhesive or pressure-sensitive adhesive that bonds each layer of LP1 is preferably used. The adhesive or pressure-sensitive adhesive may be provided on LP1 in advance, or may be applied to LP1 or the liquid crystal cell immediately before bonding.
[0214] When an adhesive is used for bonding, it is preferable to cure the adhesive by heating or irradiating it with radiation, depending on the type of adhesive.
[0215] When laminating, LP1 may be a sheet cut to the required length. In addition, when LP1 is a roll film, LP1 may be cut to the required length while unwinding, immediately before laminating to the liquid crystal cell or while laminating. For example, when LP1 is a roll film in which a substrate-less optical transparent adhesive sheet is laminated on a retardation layer, the release layer of the optical transparent adhesive sheet may be peeled off while unwinding LP1, and the end of the sheet may be laminated to the liquid crystal cell, or the sheet may be cut to the required length and then laminated to the entire surface, or the sheet may be laminated to the entire surface and then cut to the required length. Cutting may be performed using a blade or a laser.
[0216] When the liquid crystal display device is a stationary VA or IPA type, it is preferable to attach the LP1 so that the absorption axis of the polarizer is in the horizontal direction.
[0217] After laminating the LP1, the release film may be peeled off. The release film may be peeled off immediately after lamination, or may be peeled off immediately before or after assembly into a final form to prevent scratches during transportation in the next step or thereafter. Also, the release film may be peeled off by the final consumer after the image display device is delivered to the final consumer.
[0218] (LP2 pasting) The liquid crystal display device preferably has LP2 on the light source side of the liquid crystal cell. The method of bonding LP2 may be the same as or different from the method of bonding LP1. However, when the liquid crystal display device is a stationary VA type or IPA type, LP2 is preferably bonded so that the absorption axis of the polarizer is in the vertical direction.
[0219] When LP2 has the same layer structure as LP1, a laminate for polarizer transfer of LP1 may be used as LP2. However, since a liquid crystal display device is generally provided such that the absorption axis direction of the polarizer on the viewing side and the absorption axis direction of the polarizer on the light source side are perpendicular to each other, it is preferable to change the width and length of LP1 and LP2 according to the size of the liquid crystal display cell.
[0220] The release film of LP2 may be peeled off in the same manner as LP1, but it is preferable that it is peeled off before assembling into the final form.
[0221] The liquid crystal display device preferably has a reflective polarizing plate between the light source side polarizer and the light source unit. An example of the reflective polarizing plate is the brightness enhancement film DBEF series sold by 3M. The reflective polarizing plate may be attached to the polarizer surface or the coated surface using an adhesive or pressure sensitive adhesive after peeling off the release film.
[0222] (Organic EL display device) The organic EL display device preferably has LP1 on the viewing side of the organic EL cell.
[0223] After laminating the LP1, the release film may be peeled off. The release film may be peeled off immediately after lamination, during an intermediate stage before assembling into a final form, or after assembling into a final form. In addition, the release film may be peeled off by the final consumer after the image display device is delivered to the final consumer. The organic EL display device may be of a foldable type (foldable type) or a rollable type (rollable type). The organic EL display device of the present invention can be made thin and has good foldability and rollability. EXAMPLES
[0224] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples, and can be practiced by making appropriate modifications within the scope of the present invention. All of these modifications are included in the technical scope of the present invention.
[0225] The retardation of the retardation layer in the laminate of the example was measured as follows.
[0226] (Retardation measurement of phase difference layer) An orientation control layer and a retardation layer were provided on the non-adhesive layer surface of a 50 μm thick polyester film (Cosmoshine (TM) A4100 manufactured by Toyobo Co., Ltd.) under the same conditions as in the examples described below, and this was transferred onto a glass plate (35 mm × 35 mm) to prepare a measurement sample. A UV-curable adhesive was used for the transfer. The retardation value (Re) of the sample was measured from the vertical direction using an automatic birefringence meter (KOBRA-WR, Oji Measurement Co., Ltd.) at a wavelength of 590 nm. Furthermore, in the case of the retardation layer using the retardation layer paint B, the slow axis in the film plane was used as the tilt axis (rotation axis), and in the case of the retardation layers using the retardation layer paints A and C, an arbitrary direction in the film plane was used as the tilt axis. The retardation values were similarly measured at angles from 0 degrees to 50 degrees in 10 degree increments with respect to the film normal direction, and Rth was calculated from this value, the thickness, and the average refractive index. The thickness was determined by embedding the film in epoxy resin, cutting out a cross-sectional piece, and observing it under a polarizing microscope. The average refractive index was 1.60 in the retardation layers using the paints B and C for the retardation layer, and 1.66 in the retardation layer using the paint A for the retardation layer.
[0227] Each layer in the laminate of the examples is described below.
[0228] (Release film) The release film was a 50 μm thick polyester film (Cosmoshine (TM) A4100 manufactured by Toyobo Co., Ltd.), with the non-easy adhesion layer side serving as the release side. The non-release side was previously subjected to corona treatment to adjust the peel strength.
[0229] TIFF0007567785000003.tif228155
[0230] TIFF0007567785000004.tif139154
[0231] (Polarizer) (1) PVA polarizer transfer laminate As a thermoplastic resin substrate, polyethylene terephthalate with an intrinsic viscosity of 0.62 dl / d was melted and kneaded in an extruder, then extruded into a sheet on a cooling roll to produce an unstretched film with a thickness of 100 μm. An aqueous solution of polyvinyl alcohol with a degree of polymerization of 2400 and a degree of saponification of 99.9 mol% was applied to one side of this unstretched film and dried to form a PVA layer. The obtained laminate was stretched twice in the longitudinal direction between rolls with different peripheral speeds at 120° C. and taken up. Next, the obtained laminate was treated with a 4% boric acid aqueous solution for 30 seconds, and then immersed in a mixed aqueous solution of iodine (0.2%) and potassium iodide (1%) for 60 seconds to dye it, and subsequently treated with a mixed aqueous solution of potassium iodide (3%) and boric acid (3%) for 30 seconds. Furthermore, this laminate was uniaxially stretched in the longitudinal direction in a mixed aqueous solution of boric acid (4%) and potassium iodide (5%) at 72°C, subsequently washed with a 4% aqueous solution of potassium iodide, the aqueous solution was removed with an air knife, and then dried in an oven at 80°C. Both ends were slit and wound up to obtain a laminate for PVA polarizer transfer with a width of 50 cm and a length of 1000 m. The total stretching ratio was 6.5 times, and the thickness of the PVA polarizer was 5 μm. The thickness was measured by embedding the laminate for PVA polarizer transfer in epoxy resin, cutting out a slice, and observing it with an optical microscope. This PVA polarizer is labeled as PVA (transfer) in Table 1.
[0232] (2) Liquid crystal polarizer The following compounds (d) and (e) were synthesized according to the description in paragraph
[0134] of JP-A 2007-510946 and Lub et al. Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996). [ka] [ka] The following dye (f) was synthesized according to Example 1 of JP-A-63-301850. [ka] The following dye (g) was synthesized according to Example 2 of JP-B-5-49710. [ka] The following dye (h) was synthesized according to the method for producing the compound of formula (1) described in JP-B-63-1357. [ka]
[0233] 75 parts by mass of (d), 25 parts by mass of (e), 2.5 parts by mass of (f), 2.5 parts by mass of (g), 2.5 parts by mass of (h), 6 parts by mass of IRGACURE (trademark) 369E (manufactured by BASF), and 250 parts by mass of ortho-xylene were mixed and dissolved to prepare a coating material for liquid crystal polarizers. The liquid crystal polarizer obtained by coating this coating material is indicated as liquid crystal coating in Table 1.
[0234] Example 1 A coating material for a low refractive index layer was applied to the corona-treated surface of a 50 cm wide release film, and the coating material was dried in an oven at 90°C to evaporate the solvent, followed by irradiation with ultraviolet light to form a low refractive index layer with a thickness of 0.5 μm. A coating material for a hard coat layer was further applied on the low refractive index layer, and the coating material was dried in an oven at 90°C to evaporate the solvent, followed by irradiation with ultraviolet light to form a hard coat layer with a thickness of 3 μm. An acrylic ultraviolet-curing adhesive was then applied to the hard coat layer surface, which was then superimposed on the polarizer surface (PVA surface) of a PVA polarizer transfer laminate, and ultraviolet light was irradiated from the release film surface to cure the adhesive, to obtain a polarizer transfer laminate (LPPVA0). The film was wound into a roll film with a length of 1000 m.
[0235] Example 2 The laminate for polarizer transfer (LPPVA0) obtained in Example 1 was cut to a length of 70 cm, the thermoplastic resin substrate was peeled off, and the coating material for the orientation control layer was applied to this surface and dried at 100°C to provide an orientation control layer with a thickness of 0.5 μm. The orientation control layer was then treated with a rubbing roll wrapped with a nylon napped cloth. The rubbing direction was in the flow direction of the film. Subsequently, the coating material A for the retardation layer was applied to the rubbed surface, and the solvent was evaporated by heating at 125°C for 3 minutes to align the discotic liquid crystal compound. Subsequently, the laminate for polarizer transfer (LPPVA1) was obtained by irradiating ultraviolet light for 30 seconds in an environment of 80°C.
[0236] Example 3 An alignment control layer was provided in the same manner as in Example 2, and the alignment control layer was treated with a rubbing roll wrapped with a nylon napped cloth. The rubbing direction was perpendicular to the flow direction of the film. Subsequently, the retardation layer coating material B was applied, and the film was heated at 110°C for 3 minutes to evaporate the solvent and align the rod-shaped liquid crystal compound. Furthermore, the film was irradiated with ultraviolet light for 30 seconds in an environment of 110°C to obtain a laminate for polarizer transfer (LPPVA2).
[0237] Example 4 A laminate for polarizer transfer (LPPVA3) was obtained in the same manner as in Example 3, except that the rubbing direction for the orientation control layer was set at 45 degrees to the flow direction of the film.
[0238] Example 5 (Preparation of laminate for transferring retardation layer) A polyester film (Cosmoshine (TM) A4100 manufactured by Toyobo Co., Ltd.) with a width of 50 cm and a thickness of 38 μm was used as a release substrate. The coating material for the orientation control layer was applied to the non-adhesive layer surface of the release substrate, and dried at 100 ° C to provide an orientation control layer with a thickness of 0.5 μm. The orientation control layer was then treated with a rubbing roll wrapped with a nylon napped cloth. The film was slanted on the rubbing roll, and the direction of the rubbing roll, the running speed of the film, and the number of revolutions of the rubbing roll were adjusted so that the rubbing direction was 45 degrees to the flow direction of the film. Subsequently, the coating material B for the retardation layer was applied, and the film was heated at 110 ° C for 3 minutes to evaporate the solvent and align the rod-shaped liquid crystal compound. The film was then irradiated with ultraviolet light for 30 seconds in an environment of 110 ° C to obtain a retardation layer transfer laminate with a length of 200 m.
[0239] The polarizer transfer laminate (LPPVA0) obtained in Example 1 and the above-mentioned retardation layer transfer laminate were unwound, and the polarizer surface of LPPVA0 and the retardation layer surface of the retardation layer transfer laminate were bonded together using a UV-curable adhesive, and then the laminate was wound up to obtain a polarizer transfer laminate (LPPVA4) having a length of 200 m.
[0240] Example 6 A coating material for a low refractive index layer was applied to the corona-treated surface of the release film, and the coating material was dried in an oven at 90°C to evaporate the solvent, followed by irradiation with ultraviolet light to form a low refractive index layer having a thickness of 86 nm. A coating material for a high refractive index layer was applied on the low refractive index layer, and the coating material was dried in an oven at 90°C to evaporate the solvent, followed by irradiation with ultraviolet light to form a high refractive index layer having a thickness of 130 nm. The thickness was measured using an ellipsometer (manufactured by Horiba, Ltd., automatic thin film measuring device Smart SE). Subsequently, a hard coat layer and a polarizer were provided in the same manner as in Example 1 to obtain a laminate for polarizer transfer. Furthermore, a retardation layer was provided in the same manner as in Example 4 to obtain a laminate for polarizer transfer (LPPVA5).
[0241] Example 7 One side of a 50 cm wide polyester film (Cosmoshine(TM) A4300 manufactured by Toyobo Co., Ltd.) was coated with the uneven transfer paint, and the film was heated and cured at 160°C for 3 minutes to obtain a coating weight of 1.0 g / m 2 The cured film had an uneven surface structure (Ra 0.7 μm) derived from the particles.
[0242] A low refractive index layer, a hard coat layer, and a polarizer were provided on the cured film surface in the same manner as in Example 1, except that the film having this obtained cured film was used as a release film, to obtain a laminate for polarizer transfer (LPPVA6).
[0243] Example 8 On the retardation layer of the polarizer transfer laminate (LPPVA2) obtained in Example 3, a coating material for an interlayer protective coating layer was applied and dried, and then an interlayer protective coating layer having a dry thickness of 0.5 μm was provided by irradiating with ultraviolet light. Subsequently, a coating material C for a retardation layer was applied and dried, and then irradiated with ultraviolet light at 38° C. for 80 seconds to obtain a retardation layer in which the liquid crystal compound was vertically aligned.
[0244] Example 9 The film having the low refractive index layer and the hard coat layer laminated thereon produced in Example 1 was cut to a length of 70 cm, the hard coat layer surface was rubbed in the long side direction, and the paint for liquid crystal polarizing film was applied to the rubbed surface. It was then dried at 110°C for 3 minutes to form a film with a thickness of 2 μm, and subsequently irradiated with ultraviolet light to obtain a laminate for polarizer transfer (LPLC0).
[0245] Example 10 A polarizer transfer laminate (LPLC1) was obtained in the same manner as in Example 3, except that the polarizer transfer laminate (LPLC0) obtained in Example 9 was used instead of the polarizer transfer laminate (LPPVA0) and the rubbing direction of the orientation control layer was set at 45 degrees to the flow direction of the film.
[0246] Example 11 An orientation control layer was provided in the same manner as in Example 10, and the liquid crystal retardation layer coating solution D was applied onto the orientation control layer that had been subjected to rubbing treatment, and after drying at 120°C, the coating solution was further heated for 3 minutes to mature the liquid crystal and align the discotic compound. Subsequently, the coating layer was cured by irradiating ultraviolet light, and a retardation layer having a thickness of 1.8 μm was produced, thereby obtaining a laminate for polarizer transfer (LPLC2).
[0247] Example 12 A polarizer transfer laminate (LPLC3) was obtained in the same manner as in Example 10, except that the film having a low refractive index layer, a high refractive index layer, and a hard coat layer prepared in Example 6 was used instead of the film having a low refractive index layer and a hard coat layer prepared in Example 1.
[0248] The layer structures of Examples 1 to 12 are shown in Table 1. [Table 1]
[0249] (Evaluation on a liquid crystal display device) The viewing side polarizing plate and the light source side polarizing plate of each type (IPS, VA, TN) of commercially available liquid crystal display cell were peeled off, and instead, the laminate for polarizer transfer was cut to the size of the liquid crystal display cell and laminated using an optical adhesive, and then the release film of the laminate for polarizer transfer was peeled off. The lamination was performed so that the absorption axis of the polarizing plate of the original liquid crystal display device and the absorption axis of the laminate for polarizer transfer were in the same direction. In addition, the release substrate of the laminate for retardation layer transfer of LPPVA4 was peeled off immediately before lamination with the liquid crystal cell.
[0250] (Image displayability) When landscape pictures were displayed on the liquid crystal display device and the display state of the image was observed from the front, all images displayed were of the same quality as those on the original display device.
[0251] (Viewing angle characteristics) The image was observed by moving from the front in each direction: up and down, left and right, upper right and lower right. For IPS and VA type liquid crystal cells, the viewing angle was improved when compared with the case where LPPVA0 was used on both the viewing side and the light source side, and for TN type liquid crystal cells, the viewing angle was improved when compared with the case where LPPVA0 was used on both the viewing side and the light source side, and the viewing angle was improved when compared with the case where LPPVA0 was used on both the viewing side and the light source side.
[0252] (Reflected) The liquid crystal display device was tilted at an angle of about 45 degrees from the normal direction so that the fluorescent lights in the room were reflected. A 50 μm thick polyester film (Cosmoshine(TM) A4100 manufactured by Toyobo Co., Ltd.) was placed on the liquid crystal display device with the non-easy adhesion layer side facing up, and all reflections were less than those of the polyester film side.
[0253] (Scratch resistance) The liquid crystal display screen was rubbed back and forth with steel wool 50 times, and then peeling of the polarizer was observed. However, no peeling of the polarizer was observed, and the screen was also excellent in terms of scratch resistance.
[0254] Table 2 shows a summary of the evaluation results for the liquid crystal display device. [Table 2]
[0255] (Evaluation on an organic EL display device) The circular polarizer of a commercially available organic EL display device was peeled off, and instead, a laminate for polarizer transfer was cut to the size of a liquid crystal display cell, and laminated using an optical pressure-sensitive adhesive, and then the release film of the laminate for polarizer transfer was peeled off. The lamination was performed so that the absorption axis of the circular polarizer of the original display device and the absorption axis of the laminate for polarizer transfer were in the same direction.
[0256] (Anti-reflective property) When the screens were observed indoors with fluorescent lights behind them to check the anti-reflection effect, it was found that all of the screens had the same anti-reflection effect as the original organic EL display device.
[0257] (Reflection) The organic EL display device was tilted at an angle of about 45 degrees from the normal direction so that the indoor fluorescent lights were reflected. A 50 μm thick polyester film (Cosmoshine(TM) A4100 manufactured by Toyobo Co., Ltd.) was placed on top of the organic EL display device with the non-easy adhesion layer side facing up, and all reflections were less than those of the polyester film side.
[0258] (Scratch resistance) The organic EL display screen was rubbed back and forth with steel wool 50 times, and then peeling of the polarizer was observed. However, no peeling of the polarizer was observed, and the screen had excellent scratch resistance.
[0259] Table 3 shows a summary of the evaluation results for the organic EL display device. [Table 3]
Claims
1. A method for producing an image display device, comprising: laminating a polarizer transfer laminate LP1, which is a laminate including a coating layer and a polarizer laminated in this order on a release film, on at least one surface of an image display cell such that the polarizer of the polarizer transfer laminate LP1 is disposed on the image display cell side, The coating layer is applied to the release surface of the release film, the polarizer is a PVA polarizer or a liquid crystal polarizer, In the case where the polarizer is a PVA polarizer, the polarizer is provided on the coating layer by either of the following (a) and (b): In the method for producing an image display device as described above, when the polarizer is a liquid crystal polarizer, the polarizer is provided on the coating layer by either of the following (c) and (d): (a) A method in which the PVA polarizer itself is attached to the coating layer on the release film using an adhesive or pressure-sensitive adhesive. (b) A method in which the PVA polarizer on a releasable substrate and the coating layer surface of a laminate of the releasable film and the coating layer are bonded to each other with an adhesive or a pressure-sensitive adhesive, and then the releasable substrate is peeled off to transfer the PVA polarizer. (c) A method of applying a coating material for liquid crystal polarizers containing a liquid crystal compound onto the coating layer on the release film, and aligning and fixing the liquid crystal compound. (d) A method in which the coating layer surface of a laminate of the release film and the coating layer is bonded to the liquid crystal polarizer surface on a releasable substrate using an adhesive or pressure-sensitive adhesive, and then the releasable substrate is peeled off to transfer the liquid crystal polarizer.
2. (A) a step of laminating a polarizer transfer laminate LP1 on one surface of an image display cell such that the polarizer of the polarizer transfer laminate LP1, which is formed by laminating a coating layer and a polarizer in this order on a release film, is disposed on the image display cell side; and (B) A step of laminating the polarizer transfer laminate LP2 on the other surface of the image display cell so that the polarizer of the polarizer transfer laminate LP2, in which a polarizer is laminated on a release film, is disposed on the image display cell side. A method for manufacturing an image display device, comprising: The coating layer of the polarizer transfer laminate LP1 is provided by coating on the release surface of the release film, The polarizer of the polarizer transfer laminate LP1 is a PVA polarizer or a liquid crystal polarizer, In the case where the polarizer of the polarizer transfer laminate LP1 is the PVA polarizer, the polarizer is provided on the coating layer by either of the following (a) and (b): The method for manufacturing an image display device, wherein, when the polarizer of the polarizer transfer laminate LP1 is a liquid crystal polarizer, the polarizer is provided on the coating layer by either (c) or (d) below. (a) A method in which the PVA polarizer itself is attached to the coating layer on the release film using an adhesive or pressure-sensitive adhesive. (b) A method in which the PVA polarizer on a releasable substrate and the coating layer surface of a laminate of the releasable film and the coating layer are bonded to each other with an adhesive or a pressure-sensitive adhesive, and then the releasable substrate is peeled off to transfer the PVA polarizer. (c) A method of applying a coating material for liquid crystal polarizers containing a liquid crystal compound onto the coating layer on the release film, and aligning and fixing the liquid crystal compound. (d) A method in which the coating layer surface of a laminate of the release film and the coating layer is bonded to the liquid crystal polarizer surface on a releasable substrate using an adhesive or pressure-sensitive adhesive, and then the releasable substrate is peeled off to transfer the liquid crystal polarizer.
3. A method for manufacturing an image display device as described in claim 1 or 2, wherein the polarizer transfer laminate LP1 has a phase difference layer on the opposite side to the coating layer of the polarizer.
4. A method for manufacturing an image display device as described in claim 2 or 3, wherein the polarizer transfer laminate LP2 has a retardation layer on the opposite side of the polarizer to the release film.
5. A method for manufacturing an image display device described in any one of claims 2 to 4, wherein the polarizer transfer laminate LP2 has a coating layer between the release film and the polarizer.
6. A method for manufacturing an image display device described in any one of claims 1 to 5, wherein the coating layer of the polarizer transfer laminate LP1 includes any one of a hard coating layer, a reflection reduction layer, and an antistatic layer.
7. The method for producing an image display device according to any one of claims 1 to 6, wherein the polarizer transfer laminate LP1 does not have a self-supporting polarizer protective film.
8. A method for manufacturing an image display device according to claim 1, wherein the image display cell is a liquid crystal display cell.
9. A method for manufacturing an image display device described in any one of claims 1, 3, 6, and 7, wherein the image display cell is an organic EL display cell.
Citation Information
Patent Citations
Load module preparing system
JP1989070829A
Polarizing plate excellent in durability, method of manufacturing the same, and image display device using the same
JP2010277018A
Polarizing sheet laminate
JP2012027260A
Polarizing plate with protection film and laminate including the same
JP2016118776A