tire
A tire with a sulfur concentration gradient across multiple rubber layers enhances steering stability and wear resistance by maintaining consistent tread surface hardness and rigidity, addressing issues of rigidity and wear in existing designs.
Patent Information
- Application Number
- JP2022531674
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-06-25
- Filing Date
- 2021-06-04
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-06-04
AI Technical Summary
Tires with relatively rigid cap rubber lose road-following ability and generate insufficient reaction force due to low base rubber rigidity, leading to poor handling stability on wet roads and rapid wear resistance deterioration.
A tire design with three or more rubber layers, featuring a sulfur concentration gradient from the radially inner to outer layers, where the second layer has higher free sulfur content than the first, maintaining consistent crosslinking and rigidity across the tread surface.
Improves steering stability and total wear resistance on wet roads by maintaining consistent tread surface hardness and rigidity, preventing sudden wear resistance drops.
Smart Images

Figure 0007567911000007 
Figure 0007567911000008 
Figure 0007567911000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a tire. [Background technology]
[0002] Patent Document 1 describes a tire having a tread portion having a cap rubber that comes into contact with the road surface and a base rubber that is positioned radially inward of the cap rubber, in which the cap rubber is made a rubber layer with relatively high rigidity and the base rubber is made a rubber layer with relatively low rigidity, and the thickness of the base rubber is inclined in the tire width direction, thereby reducing the difference in ground contact pressure and improving braking performance. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-162242 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the tire described in Patent Document 1 is prone to losing road surface conformity due to the relatively high rigidity of the cap rubber, and is unable to generate sufficient reaction force due to the low rigidity of the base rubber, so there is room for improvement in steering stability on wet roads. Furthermore, there is concern that wear resistance will rapidly deteriorate when the base rubber is exposed, and there is also room for improvement in overall wear resistance up to the end of the running period.
[0005] An object of the present invention is to provide a tire which has improved overall performance including steering stability on wet road surfaces and total wear resistance up to the end of the running period. [Means for solving the problem]
[0006] As a result of extensive research, the inventors have found that the above-mentioned problems can be solved by providing three or more rubber layers in the tread portion and providing a free sulfur concentration gradient from the rubber layer on the radially inner side of the tire to the rubber layer on the radially outer side of the tire, and have thus completed the present invention.
[0007] That is, the present invention provides [1] A tire having a tread including at least a first layer constituting a tread surface, a second layer adjacent to the radially inner side of the first layer, and a third layer adjacent to the radially inner side of the second layer, wherein the first layer, the second layer, and the third layer are made of a rubber composition containing a rubber component, the free sulfur content of the rubber composition constituting the third layer is greater than the free sulfur content of the rubber composition constituting the second layer, and the free sulfur content of the rubber composition constituting the second layer is greater than the free sulfur content of the rubber composition constituting the first layer; [2] The mass change rate X of the rubber composition constituting the first layer before and after immersion in toluene at 23 ° C. for 24 hours, measured in accordance with JIS K 6258:2016 1 (%), and the mass change rate X of the rubber composition constituting the second layer before and after immersion in toluene at 23 ° C. for 24 hours, measured in accordance with JIS K 6258:2016 2 (%) difference (X 1 -X 2 The tire according to [1], wherein the ratio of the surface roughness to the surface roughness is 50% or less. [3] The tire according to [1] or [2], wherein the rubber composition constituting the first layer and the rubber composition constituting the second layer have a tan δ of 0.45 or more at 0 ° C.; [4] The tire according to any one of [1] to [3], wherein the difference between the hardness of the rubber composition constituting the second layer and the hardness of the rubber composition constituting the first layer is 5 or less. [5] The tire according to any one of [1] to [4], wherein the specific gravity of the rubber composition constituting the first layer and the rubber composition constituting the second layer is 1.25 or less, [6] The tire according to any one of [1] to [5], wherein the specific gravity of the rubber composition constituting the second layer is less than 1.20. [7] Acetone extractable amount AE of the rubber composition constituting the second layer 2 The acetone extractable amount AE of the rubber composition constituting the first layer is 1 The tire according to any one of [1] to [6], [8] The tire according to any one of [1] to [7], wherein the modulus of the rubber composition constituting the second layer at 100% elongation at 23 ° C. is greater than the modulus of the rubber composition constituting the first layer at 100% elongation at 23 ° C.; [9] The tire according to any one of [1] to [8], wherein the rubber component constituting the first layer and the rubber component constituting the second layer each contain butadiene rubber.
[10] The tire according to any one of [1] to [9], wherein the rubber composition constituting the first layer and the rubber composition constituting the second layer each contain a reinforcing filler and a silane coupling agent, and the content of silica in the reinforcing filler in the rubber composition constituting the first layer and the content of silica in the reinforcing filler in the rubber composition constituting the second layer are 80 mass% or more.
[11] The tire according to
[10] , wherein the silane coupling agent contained in the rubber composition constituting the first layer and the rubber composition constituting the second layer are each a mercapto-based silane coupling agent.
[12] The tire according to any one of [1] to
[11] , wherein the rubber composition constituting the second layer contains a resin component.
[13] The tire according to any one of [1] to
[12] , wherein the third layer has a thickness smaller than each of the first layer and the second layer.
[14] The tire according to any one of [1] to
[13] , wherein the tread has a land portion partitioned by a plurality of circumferential grooves, and the deepest portion of the groove bottom of at least one of the circumferential grooves is formed to be located radially inward of the outermost portion of the second layer.
[15] The tire according to
[14] , wherein the land portion has a sipe, both ends of which do not open into the circumferential groove. Effect of the Invention
[0008] According to the present invention, there is provided a tire which has improved overall performance including steering stability on wet road surfaces and total wear resistance up to the end of the running period. [Brief description of the drawings]
[0009] [Figure 1] 1 is an enlarged cross-sectional view of a portion of a tread of a tire according to an embodiment of the present disclosure. [Diagram 2] 1 is a schematic diagram of a tire contact surface when the tread is pressed against a flat surface. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] A tire which is one embodiment of the present disclosure is a tire having a tread including at least a first layer constituting a tread surface, a second layer adjacent to the radially inward side of the first layer, and a third layer adjacent to the radially inward side of the second layer, wherein the first layer, the second layer, and the third layer are composed of a rubber composition containing a rubber component, the free sulfur content of the rubber composition constituting the third layer is greater than the free sulfur content of the rubber composition constituting the second layer, and the free sulfur content of the rubber composition constituting the second layer is greater than the free sulfur content of the rubber composition constituting the first layer.
[0011] In a vulcanized rubber composition vulcanized with sulfur, unreacted sulfur that is not chemically bonded to a rubber component and does not contribute to a crosslinking reaction of the rubber component, i.e., free sulfur, is contained. In this disclosure, "free sulfur" means free sulfur that is not chemically bonded to a rubber component and does not contribute to a crosslinking reaction, and "amount of free sulfur" means the amount of free sulfur contained in a vulcanized rubber composition.
[0012] Without intending to be bound by theory, in the present disclosure, the following is believed to be the mechanism by which steering stability performance and wear resistance performance on wet road surfaces can be improved in a balanced manner.
[0013] The free sulfur, which is not chemically bonded to the rubber component and does not contribute to the crosslinking reaction, reacts with the rubber component on the outermost surface (tread surface) that is in contact with the road surface due to heat generated during driving. This improves the abrasion resistance of the tread surface, and enables the rubber composition constituting the first layer to maintain the same hardness as immediately after vulcanization.
[0014] In this way, the sulfur in the rubber composition constituting the first layer is consumed by heat generation during running, but the sulfur in the rubber composition can move between the rubber layers due to the concentration gradient. Therefore, by providing a concentration gradient of the free sulfur amount from the rubber layer on the inner side of the tire radial direction to the rubber layer on the outer side of the tire radial direction, a constant amount of sulfur can be constantly delivered to the first layer, and the free sulfur and the rubber component are easily bonded to the tread surface due to friction between the tread surface and the road surface, making it possible to increase the rigidity, and therefore making it easier to generate a reaction force. In addition, since the entire rubber layer does not undergo a large change in rigidity and the ability to follow the road surface is not impaired, it is possible to improve the steering stability performance on wet road surfaces. In addition, it is thought that the wear resistance performance of the tread surface can also be improved at this time. Furthermore, when the second layer is exposed, the same degree of crosslinking as the first layer is ensured, and a sudden decrease in wear resistance performance can be prevented, so it is thought that it is possible to maintain and improve the total wear resistance until the end of the run without causing a sudden deterioration in wear resistance performance.
[0015] On the other hand, if a concentration gradient of free sulfur is applied from the rubber layer on the radially outer side of the tire to the rubber layer on the radially inner side of the tire, the amount of free sulfur consumed in the first layer will increase, and the crosslink density of the first layer will become too high, which is thought to deteriorate the steering stability on wet roads. It is also thought that the wear resistance will decrease significantly after the first layer has worn away.
[0016] The mass change rate X of the rubber composition constituting the first layer before and after immersion in toluene at 23°C for 24 hours, measured in accordance with JIS K 6258:2016 1(%), and the mass change rate X of the rubber composition constituting the second layer before and after immersion in toluene at 23 ° C. for 24 hours, measured in accordance with JIS K 6258:2016 2 (%) difference (X 1 -X 2 ) is preferably 50% or less.
[0017] The rubber composition constituting the first layer and the rubber composition constituting the second layer preferably have a tan δ at 0° C. of 0.45 or more.
[0018] The difference in hardness between the rubber composition constituting the second layer and the rubber composition constituting the first layer is preferably 5 or less.
[0019] The specific gravity of the rubber composition constituting the first layer and the rubber composition constituting the second layer is preferably 1.25 or less. The specific gravity of the rubber composition constituting the first layer is more preferably 1.24 or less, even more preferably 1.23 or less, and particularly preferably 1.22 or less. The specific gravity of the rubber composition constituting the second layer is more preferably 1.23 or less, even more preferably 1.21 or less, and particularly preferably less than 1.20. It is believed that by setting the specific gravity within the above range, the energy applied to the tread when the tire rolls can be reduced, consumption of free sulfur inside the rubber layer can be prevented, and the steering stability on wet road surfaces and the total wear resistance performance up to the end of the driving period can be improved.
[0020] The acetone extractable amount AE of the rubber composition constituting the second layer 2 is the acetone extractable amount AE of the rubber composition constituting the first layer. 1 More than that is preferred.
[0021] The modulus of the rubber composition constituting the second layer at 23°C when stretched 100% is preferably greater than the modulus of the rubber composition constituting the first layer at 23°C when stretched 100%.
[0022] The rubber component constituting the first layer and the rubber component constituting the second layer each preferably contain butadiene rubber.
[0023] It is preferable that the rubber composition constituting the first layer and the rubber composition constituting the second layer each contain a reinforcing filler and a silane coupling agent, and that the silica content in the reinforcing filler in the rubber composition constituting the first layer and the silica content in the reinforcing filler in the rubber composition constituting the second layer are 80 mass% or more.
[0024] The silane coupling agents contained in the rubber composition constituting the first layer and the rubber composition constituting the second layer are preferably mercapto-based silane coupling agents.
[0025] The rubber composition constituting the second layer preferably contains a resin component.
[0026] The thickness of the third layer is preferably less than the thickness of each of the first and second layers.
[0027] It is preferable that the tread has a land portion partitioned by a plurality of circumferential grooves, and is formed so that the deepest part of the groove bottom of at least one of the circumferential grooves is located radially inward of the outermost part of the second layer.
[0028] The land portion preferably has a sipe having both ends not opening into the circumferential groove.
[0029] A procedure for producing a tire according to an embodiment of the present disclosure will be described in detail below. However, the following description is merely an example for explaining the present disclosure, and is not intended to limit the technical scope of the present invention to the described range. In this specification, when a numerical range is indicated using "to" it is intended to include both ends of the numerical range.
[0030] Fig. 1 is an enlarged cross-sectional view showing a portion of a tire tread, in which the up-down direction is the tire radial direction, the left-right direction is the tire width direction, and the direction perpendicular to the paper surface is the tire circumferential direction.
[0031] As shown in the figure, the tread portion of the tire of the present disclosure includes a first layer 6, a second layer 7, and a third layer 8, with the outer surface of the first layer 6 constituting the tread surface 3, the second layer 7 adjacent to the radially inner side of the first layer 6, and the third layer 8 adjacent to the radially inner side of the second layer 7. The first layer 6 typically corresponds to a cap tread. The second layer 7 and the third layer 8 typically correspond to a base tread or an undertread. In addition, one or more rubber layers may be further provided between the third layer 8 and the belt layer, as long as the object of the present disclosure is achieved.
[0032] In Fig. 1, double arrow t1 indicates the thickness of the first layer 6, double arrow t2 indicates the thickness of the second layer 7, and double arrow t3 indicates the thickness of the third layer 8. In Fig. 1, an arbitrary point on the tread surface where no grooves are formed is indicated by the symbol P. The straight line indicated by the symbol N is a straight line (normal line) that passes through point P and is perpendicular to the tangent plane at point P. In this specification, thicknesses t1, t2, and t3 are measured along the normal line N drawn from point P on the tread surface at a position where no grooves exist in the cross section of Fig. 1.
[0033] In the present disclosure, the thickness t1 of the first layer 6 is not particularly limited, but from the viewpoint of wet grip performance, it is preferably 1.0 mm or more, more preferably 1.5 mm or more, and even more preferably 2.0 mm or more. On the other hand, from the viewpoint of heat generation, the thickness t1 of the first layer 6 is preferably 10.0 mm or less, more preferably 9.0 mm or less, and even more preferably 8.0 mm or less.
[0034] In the present disclosure, the thickness t2 of the second layer 7 is not particularly limited, but is preferably 1.5 mm or more, more preferably 2.0 mm or more, and even more preferably 2.5 mm or more. The thickness t2 of the second layer 7 is preferably 10.0 mm or less, more preferably 9.0 mm or less, and even more preferably 8.0 mm or less.
[0035] In the present disclosure, the thickness t3 of the third layer 8 is not particularly limited, but is preferably 1.0 mm or more, more preferably 1.5 mm or more. Also, the thickness t3 of the third layer 8 is preferably 10.0 mm or less, more preferably 9.0 mm or less, and even more preferably 8.0 mm or less.
[0036] The tread of the present disclosure has a plurality of circumferential grooves 1 that extend continuously in the tire circumferential direction. The circumferential grooves 1 extend linearly along the circumferential direction, but are not limited to this form, and may extend, for example, in a wavy, sinusoidal, or zigzag shape along the circumferential direction.
[0037] The tread of the present disclosure has land portions 2 partitioned by circumferential grooves 1 in the tire width direction.
[0038] The groove depth H of the circumferential groove 1 is determined by the distance between the extension line 4 of the land portion 2 and the extension line 5 of the deepest part of the groove bottom of the circumferential groove 1. Note that, for example, when there are multiple circumferential grooves 1, the groove depth H is the distance between the extension line 4 of the land portion 2 and the extension line 5 of the deepest part of the groove bottom of the circumferential groove 1 having the deepest groove depth among the multiple circumferential grooves 1 (the circumferential groove 1 on the left side in FIG. 1 ).
[0039] In the present disclosure, the circumferential groove 1 is formed such that the deepest portion of the groove bottom of the circumferential groove 1 is located radially inward of the outermost portion of the second layer 7 of the land portion 2. Specifically, directly below the circumferential groove 1 (inner in the tire radial direction), the second layer 7 has a recess that is recessed radially inward from its outermost portion, and a part of the first layer 6 is formed with a predetermined thickness within the recess of the second layer 7. The circumferential groove 1 is formed so as to extend beyond the outermost portion of the second layer 7 and into the inside of the recess of the second layer 7.
[0040] A schematic diagram of the contact surface when the tread is pressed against a flat surface is shown in Fig. 2. The tread 10 constituting the tire according to the present disclosure has a circumferential groove 1 that extends continuously in the tire circumferential direction C (extending linearly along the tire circumferential direction in the example of Fig. 2), and lateral grooves 21 and sipes 22, 23 that extend in the width direction, as shown in Figs. 1 and 2.
[0041] The tread 10 has a plurality of circumferential grooves 1 that extend continuously in the circumferential direction C. In Fig. 2, three circumferential grooves 1 are provided, but the number of circumferential grooves is not particularly limited and may be, for example, two to five. In addition, in the present disclosure, the circumferential grooves 1 extend linearly along the circumferential direction, but are not limited to such an embodiment and may extend, for example, in a wavy, sinusoidal, or zigzag shape along the circumferential direction.
[0042] The tread 10 has land portions 2 separated by a plurality of circumferential grooves 1 in the tire width direction W. The shoulder land portions 11 are a pair of land portions formed between the circumferential groove 1 and the tread end Te. The center land portion 12 is a land portion formed between the pair of shoulder land portions 11. In FIG. 2, two center land portions 12 are provided, but the number of center land portions is not particularly limited and may be, for example, one to five.
[0043] The land portion 2 is preferably provided with lateral grooves and / or sipes crossing the land portion 2. It is more preferable that the land portion 2 has sipes whose both ends do not open into the circumferential groove 1. In FIG. 2, the shoulder land portion 11 is provided with a plurality of shoulder lateral grooves 21 whose ends open into the circumferential groove 1 and a plurality of shoulder sipes 22 whose both ends do not open into the circumferential groove 1, and the center land portion 12 is provided with a plurality of center sipes 23 whose one end opens into the circumferential groove 1, but the present invention is not limited to such an embodiment.
[0044] In this specification, the term "groove", including circumferential grooves and lateral grooves, refers to a recess having a width of at least 2.0 mm, whereas the term "sipe" refers to a thin cut having a width of 2.0 mm or less, preferably 0.5 to 2.0 mm.
[0045] In this disclosure, unless otherwise specified, the dimensions and angles of each component of the tire are measured when the tire is mounted on a standard rim and inflated to a standard internal pressure. No load is applied to the tire during measurement. In this specification, the term "standard rim" refers to a rim that is determined for each tire by a standard system that includes the standard on which the tire is based, such as a standard rim for JATMA, a "Design Rim" for TRA, and a "Measuring Rim" for ETRTO. In this specification, the term "standard internal pressure" refers to the air pressure determined for each tire by the standard, such as the maximum air pressure for JATMA, the maximum value listed in the table "TIRE LOAD LIMITS AT VARIOUS COLD INFLATION PRESSURES" for TRA, and "INFLATION PRESSURE" for ETRTO.
[0046] The "free sulfur content" in the present disclosure can be determined as follows. The sulfur content Ts (mass%) in the rubber test piece after vulcanization is calculated by the oxygen combustion flask method in accordance with JIS K 6233:2016 "Rubber - Determination of total sulfur by ion chromatography (quantitative)". Next, the test piece is immersed in acetone for 24 hours to extract the soluble components in accordance with JIS K 6229:2015 "Rubber - Determination of solvent extract (quantitative)". The test piece after the soluble components are extracted is heated and dried to remove the solvent in the test piece, and then the sulfur content As (mass%) in the test piece is calculated by the oxygen combustion flask method in accordance with JIS K 6233:2016. The free sulfur content can be determined by calculating the difference (Ts-As) between the sulfur content Ts and the sulfur content As. The free sulfur content in the rubber composition can be appropriately adjusted by the amount of sulfur and the type and amount of vulcanization accelerator.
[0047] In the present disclosure, the free sulfur content of the rubber composition constituting the third layer 8 is greater than the free sulfur content of the rubber composition constituting the second layer 7, and the free sulfur content of the rubber composition constituting the second layer 7 is greater than the free sulfur content of the rubber composition constituting the first layer 6. The difference between the free sulfur content of the rubber composition constituting the third layer 8 and the free sulfur content of the rubber composition constituting the second layer 7 is preferably 0.1% or more, more preferably 0.2% or more, and even more preferably 0.3% or more. The difference between the free sulfur content of the rubber composition constituting the second layer 7 and the free sulfur content of the rubber composition constituting the first layer 6 is preferably 0.1% or more, more preferably 0.2% or more, and even more preferably 0.3% or more.
[0048] The "acetone extractable amount" in the present disclosure can be calculated according to JIS K 6229:2015 by immersing each vulcanized rubber test piece in acetone for 24 hours to extract the soluble components, measuring the mass of each test piece before and after extraction, and using the following formula. The acetone extractable amount is an index of the concentration of organic low molecular weight compounds in the plasticizer contained in the vulcanized rubber composition. In the present disclosure, unless otherwise specified, the acetone extractable amount is a value measured by cutting a sample from a tire. Acetone extractable amount (mass%)={(mass of rubber test piece before extraction-mass of rubber test piece after extraction) / (mass of rubber test piece before extraction)}×100
[0049] Acetone extractable amount AE of the rubber composition constituting the second layer 7 2 is the acetone extractable amount AE of the rubber composition constituting the first layer 6 1 The acetone extractable amount AE of the rubber composition constituting the second layer 7 is preferably greater than 1. 2 and the acetone extractable amount AE of the rubber composition constituting the first layer 6 2 Difference from (AE 2 -AE 1) is preferably 1 to 20 mass%, more preferably 2 to 15 mass%, and even more preferably 3 to 10 mass%. By setting the difference in acetone extractable amount within the above range, it is considered that free sulfur can easily move into the plasticizer component in the second layer 7, and as a result, free sulfur can easily migrate from the second layer 7 to the first layer 6 during running.
[0050] Acetone extractable amount AE of the rubber composition constituting the first layer 6 1 The acetone extractable amount AE of the rubber composition constituting the second layer 7 2 Ratio of (AE 2 / AE 1 ) is preferably 1.05 to 2.00, more preferably 1.10 to 1.80, even more preferably 1.15 to 1.60, and particularly preferably 1.20 to 1.40. By setting the ratio of the acetone extractable amounts in the above ranges and the difference in the acetone extractable amounts in the above ranges, it is believed that free sulfur becomes more likely to move into the plasticizer component in the second layer 7, and as a result, free sulfur becomes more likely to migrate from the second layer 7 to the first layer 6 during running.
[0051] In this disclosure, the mass change rate before and after toluene swelling is used as a measure reflecting the crosslink density of the rubber composition. In this disclosure, the mass change rate before and after toluene swelling can be determined in accordance with JIS K 6258:2016 "Vulcanized rubber and thermoplastic rubber - Determination of liquid resistance" by measuring the mass change rate (%) before and after immersing each test rubber composition after vulcanization in toluene at 23°C for 24 hours. A smaller value indicates a higher crosslink density. In addition, in this disclosure, unless otherwise specified, the mass change rate before and after toluene swelling is a value measured by cutting a sample from a tire.
[0052] In the present disclosure, the mass change rate X of the rubber composition constituting the first layer 6 before and after immersion in toluene at 23° C. for 24 hours, measured in accordance with JIS K 6258:2016, is 1 (%), and the mass change rate X of the rubber composition constituting the second layer 7 before and after immersion in toluene at 23 ° C. for 24 hours measured in accordance with JIS K 6258:2016 2(%) difference (X 1 -X 2 ) is preferably 50% or less, more preferably 40% or less, even more preferably 35% or less, and particularly preferably 30% or less. By setting the difference in the mass change rate within the above range, the crosslink density of the first layer 6 is low and the difference with the crosslink density of the second layer 7 is small, so that a constant amount of free sulfur can be constantly delivered to the first layer 6, and good steering stability and wear resistance on wet roads are maintained.
[0053] The modulus at 100% stretch in the present disclosure refers to the tensile stress at 100% stretch in the grain direction measured under conditions of a tensile speed of 3.3 mm / sec in an atmosphere of 23°C in accordance with JIS K 6251:2017 "Vulcanized rubber and thermoplastic rubber - Determination of tensile test properties". The sample may be, for example, a dumbbell-shaped No. 7. The modulus at 100% stretch of the rubber composition constituting the first layer 6 is preferably 1.6 MPa or more, more preferably 1.8 MPa or more, and even more preferably 2.0 MPa or more. The modulus at 100% stretch of the rubber composition constituting the second layer 7 is preferably 1.8 MPa or more, more preferably 2.0 MPa or more, and even more preferably 2.2 MPa or more. The upper limit of the modulus at 100% stretch of the rubber compositions constituting the first layer 6, the second layer 7, and the third layer 8 is not particularly limited. From the viewpoint of the effects of the present disclosure, the modulus of the rubber composition constituting the second layer 7 at 100% elongation at 23° C. is preferably greater than the modulus of the rubber composition constituting the first layer 6 at 100% elongation at 23° C. In this specification, the term "grain direction" refers to the rolling direction when a rubber sheet is formed by extrusion or shearing treatment, and coincides with the circumferential direction of the tire.
[0054] In the present disclosure, "0°C tan δ" refers to the loss tangent tan δ under the conditions of temperature 0°C, initial strain 10%, dynamic strain 1%, and frequency 10Hz. When preparing a test rubber composition (for example, it can be 20mm long x 4mm wide x 1mm thick) by cutting it out from a tire, it is cut out from the tread part of the tire so that the tire circumferential direction is the long side and the tire radial direction is the thickness direction. The 0°C tan δ of the rubber composition constituting the first layer 6 is preferably 0.45 or more, more preferably 0.50 or more, even more preferably 0.55 or more, and particularly preferably 0.60 or more. The 0°C tan δ of the rubber composition constituting the second layer 7 is preferably 0.45 or more, more preferably 0.50 or more, and even more preferably 0.55 or more. By setting the 0°C tan δ in the above range, not only can good wet grip performance be obtained due to hysteresis loss, but also when running on a wet road surface or a low-temperature road surface, it is possible to generate heat on the tread surface 3, which can further improve the wear resistance. On the other hand, from the viewpoint of fuel economy performance, the 0°C tan δ of the rubber compositions constituting the first layer 6, the second layer 7, and the third layer 8 is preferably 1.60 or less, more preferably 1.40 or less, even more preferably 1.20 or less, and particularly preferably 1.00 or less. The 0°C tan δ value of the rubber composition constituting the first layer 6 is preferably greater than the 0°C tan δ value of the rubber composition constituting the second layer 7.
[0055] In the present disclosure, the rubber hardness means the Shore hardness (Hs) measured using a type A durometer in an atmosphere at 23°C in accordance with JIS K 6253-3:2012 "Vulcanized rubber and thermoplastic rubber - Determination of hardness". Specifically, the tire is cut in the radial direction at a width of 20 mm, the cut surface is smoothed, and then a type A durometer is pressed against the cut surface from the cross-sectional direction to measure the Shore hardness (Hs) of each rubber layer after vulcanization at 23°C. In the present disclosure, the difference between the rubber hardness of the rubber composition constituting the first layer 6 and the rubber hardness of the rubber composition constituting the second layer 7 is preferably 6 or less, more preferably 5 or less, even more preferably 4 or less, and particularly preferably 3 or less. It is believed that by setting the difference in rubber hardness within the above range, excessive performance changes when the second layer 7 becomes the outermost surface due to wear can be suppressed.
[0056] <Rubber component> The rubber composition constituting each rubber layer of the tread according to the present disclosure (rubber composition for tread) preferably contains at least one rubber component selected from the group consisting of isoprene-based rubber, styrene butadiene rubber (SBR) and butadiene rubber (BR). The rubber components constituting the first layer 6 and the second layer 7 preferably contain SBR, more preferably contain SBR and BR, or may be rubber components consisting of only SBR and BR. The rubber component constituting the third layer 8 preferably contains isoprene-based rubber, more preferably contains isoprene-based rubber and BR, or may be rubber components consisting of only isoprene-based rubber and BR.
[0057] (Isoprene rubber) Examples of isoprene-based rubbers include natural rubber (NR), isoprene rubber (IR), modified NR, modified NR, modified IR, etc. As NR, for example, SIR20, RSS♯3, TSR20, etc., which are common in the tire industry, can be used. As IR, there is no particular limitation, and for example, IR2200, etc., which are common in the tire industry, can be used. Examples of modified NR include deproteinized natural rubber (DPNR), high-purity natural rubber, etc., as modified NR, epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), grafted natural rubber, etc., as modified IR, epoxidized isoprene rubber, hydrogenated isoprene rubber, grafted isoprene rubber, etc. can be used. These isoprene-based rubbers may be used alone or in combination of two or more.
[0058] In the rubber component constituting the first layer 6 and the second layer 7, when an isoprene-based rubber (preferably NR) is contained, the content in 100% by mass of the rubber component is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 20% by mass or less, from the viewpoint of wet grip performance. In addition, when an isoprene-based rubber is contained, the lower limit of the content is not particularly limited, but can be, for example, 1% by mass or more, 3% by mass or more, 5% by mass or more, 10% by mass or more, or 15% by mass or more.
[0059] When the rubber component constituting the third layer 8 contains an isoprene-based rubber (preferably NR), the content thereof in 100% by mass of the rubber component is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more. The upper limit of the content of the isoprene-based rubber in the rubber component is not particularly limited, and may be 100% by mass.
[0060] (SBR) The SBR is not particularly limited, and examples thereof include solution-polymerized SBR (S-SBR), emulsion-polymerized SBR (E-SBR), and modified SBRs thereof (modified S-SBR, modified E-SBR). Modified SBRs include SBRs whose ends and / or main chains are modified, and modified SBRs coupled with tin, silicon compounds, etc. (condensates, those having a branched structure, etc.). Furthermore, hydrogenated products of these SBRs (hydrogenated SBR) can also be used. Among these, S-SBR is preferred, and modified S-SBR is more preferred.
[0061] The modified SBR may be modified SBR into which a functional group that is usually used in this field has been introduced. Examples of the functional group include an amino group (preferably an amino group in which a hydrogen atom of the amino group is substituted with an alkyl group having 1 to 6 carbon atoms), an amide group, a silyl group, an alkoxysilyl group (preferably an alkoxysilyl group having 1 to 6 carbon atoms), an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imido group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group (preferably an alkoxy group having 1 to 6 carbon atoms), a hydroxyl group, an oxy group, an epoxy group, and the like. These functional groups may have a substituent. Examples of the substituent include functional groups such as an amino group, an amide group, an alkoxysilyl group, a carboxyl group, and a hydroxyl group. Examples of modified SBR include hydrogenated SBR, epoxidized SBR, and tin-modified SBR.
[0062] As the SBR, oil-extended SBR or non-oil-extended SBR can be used. When oil-extended SBR is used, the amount of oil extension of SBR, i.e., the content of oil extension oil contained in SBR, is preferably 10 to 50 parts by mass per 100 parts by mass of rubber solid content of SBR.
[0063] The SBRs listed above may be used alone or in combination of two or more. As the SBRs listed above, for example, SBRs manufactured and sold by Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Zeon Corporation, ZS Elastomers Co., Ltd., etc. may be used.
[0064] The styrene content of SBR is preferably 15% by mass or more, more preferably 20% by mass or more, from the viewpoints of ensuring damping properties in the tread portion and wet grip performance. Also, from the viewpoints of temperature dependency of grip performance and wear resistance, it is preferably 60% by mass or less, more preferably 50% by mass or less. In this specification, the styrene content of SBR is 1 This value is calculated by H-NMR measurement.
[0065] The vinyl content of SBR is preferably 10 mol% or more, more preferably 13 mol% or more, and even more preferably 16 mol% or more, from the viewpoints of ensuring reactivity with silica, rubber strength, and abrasion resistance. Also, the vinyl content of SBR is preferably 70 mol% or less, more preferably 65 mol% or less, and even more preferably 60 mol% or less, from the viewpoints of preventing an increase in temperature dependency, wet grip performance, elongation at break, and abrasion resistance. In this specification, the vinyl content of SBR (amount of 1,2-bonded butadiene units) is measured by infrared absorption spectroscopy.
[0066] The weight average molecular weight (Mw) of SBR is preferably 150,000 or more, more preferably 200,000 or more, and even more preferably 250,000 or more, from the viewpoint of abrasion resistance. Moreover, from the viewpoint of crosslinking uniformity, etc., Mw is preferably 2.5 million or less, more preferably 2 million or less. Note that Mw can be determined by standard polystyrene conversion based on the measured value by gel permeation chromatography (GPC) (for example, GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMALTPORE HZ-M manufactured by Tosoh Corporation).
[0067] In the rubber components constituting the first layer 6 and the second layer 7, when SBR is contained, the content in 100% by mass of the rubber component is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 65% by mass or more, and particularly preferably 70% by mass or more, from the viewpoint of wet grip performance. The upper limit of the content of SBR in the rubber component is not particularly limited, and may be 100% by mass. When the rubber composition constituting the third layer 8 contains SBR, the content in 100% by mass of the rubber component is not particularly limited.
[0068] (BR) The BR is not particularly limited, and can be one that is commonly used in the tire industry, such as BR with a cis content of less than 50 mol% (low cis BR), BR with a cis content of 90 mol% or more (high cis BR), rare earth butadiene rubber (rare earth BR) synthesized using a rare earth catalyst, BR containing syndiotactic polybutadiene crystals (SPB-containing BR), and modified BR (high cis modified BR, low cis modified BR). Modified BR can be BR modified with the same functional groups as those described above for SBR. These BRs can be used alone or in combination of two or more.
[0069] As the high cis BR, for example, those commercially available from Zeon Corporation, Ube Industries, Ltd., JSR Corporation, etc. can be used. By containing high cis BR, it is possible to improve the abrasion resistance performance. The cis content is preferably 95 mol% or more, more preferably 96 mol% or more, further preferably 97 mol% or more, and particularly preferably 98 mol% or more. In this specification, the cis content (amount of cis-1,4-bonded butadiene units) is a value calculated by infrared absorption spectrum analysis.
[0070] The rare earth BR is synthesized using a rare earth catalyst, and has a vinyl content of preferably 1.8 mol% or less, more preferably 1.0 mol% or less, and even more preferably 0.8% or less, and a cis content of preferably 95 mol% or more, more preferably 96 mol% or more, even more preferably 97 mol% or more, and particularly preferably 98 mol% or more. As the rare earth BR, for example, commercially available products from LANXESS Co., Ltd. can be used.
[0071] The SPB-containing BR is not one in which 1,2-syndiotactic polybutadiene crystals are simply dispersed in the BR, but one in which the 1,2-syndiotactic polybutadiene crystals are dispersed after being chemically bonded to the BR. As such an SPB-containing BR, commercially available products from Ube Industries, Ltd. can be used.
[0072] As the modified BR, a modified butadiene rubber (modified BR) in which the terminals and / or the main chain are modified with a functional group containing at least one element selected from the group consisting of silicon, nitrogen and oxygen is preferably used.
[0073] Other modified BRs include those obtained by polymerizing 1,3-butadiene with a lithium initiator and then adding a tin compound, and further having the terminals of the modified BR molecule bonded with tin-carbon bonds (tin-modified BR), etc. The modified BR may be either non-hydrogenated or hydrogenated.
[0074] The BRs listed above may be used alone or in combination of two or more.
[0075] From the viewpoint of preventing low-temperature brittleness, the glass transition temperature (Tg) of BR is preferably -14°C or lower, more preferably -17°C or lower, and even more preferably -20°C or lower. On the other hand, the lower limit of the Tg is not particularly limited, but from the viewpoint of abrasion resistance, it is preferably -150°C or higher, more preferably -120°C or higher, and even more preferably -110°C or higher. The glass transition temperature of BR is a value measured by differential scanning calorimetry (DSC) at a heating rate of 10°C / min according to JIS K 7121.
[0076] The weight average molecular weight (Mw) of BR is preferably 300,000 or more, more preferably 350,000 or more, and even more preferably 400,000 or more from the viewpoint of abrasion resistance. From the viewpoint of crosslinking uniformity, etc., it is preferably 2,000,000 or less, and more preferably 1,000,000 or less. Mw can be determined by standard polystyrene conversion based on the measured value by gel permeation chromatography (GPC) (for example, GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMALTPORE HZ-M manufactured by Tosoh Corporation).
[0077] In the rubber components constituting the first layer 6 and the second layer 7, when BR is contained, the content in 100% by mass of the rubber component is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 20% by mass or less, from the viewpoint of wet grip performance. When BR is contained, the lower limit of the content is not particularly limited, and can be, for example, 1% by mass or more, 3% by mass or more, 5% by mass or more, 10% by mass or more, or 15% by mass or more. When the rubber composition constituting the third layer 8 contains BR, the content in 100% by mass of the rubber component is not particularly limited.
[0078] (Other rubber components) The rubber component according to the present disclosure may contain rubber components other than the isoprene-based rubber, SBR, and BR. As the other rubber components, crosslinkable rubber components generally used in the tire industry can be used, such as styrene-isoprene-butadiene copolymer rubber (SIBR), styrene-isobutylene-styrene block copolymer (SIBS), chloroprene rubber (CR), acrylonitrile-butadiene rubber (NBR), hydrogenated nitrile rubber (HNBR), butyl rubber (IIR), ethylene propylene rubber, polynorbornene rubber, silicone rubber, chlorinated polyethylene rubber, fluororubber (FKM), acrylic rubber (ACM), hydrin rubber, etc. These other rubber components may be used alone or in combination of two or more.
[0079] <Reinforcing filler> The rubber composition for tread according to the present disclosure preferably contains a reinforcing filler containing carbon black and / or silica. The reinforcing filler may be a reinforcing filler consisting of only carbon black and silica. The rubber composition constituting the first layer 6 and the second layer 7 preferably contains silica as a reinforcing filler, more preferably carbon black and silica. The rubber composition constituting the third layer 8 preferably contains carbon black as a reinforcing filler.
[0080] (Carbon Black) The carbon black is not particularly limited, and GPF, FEF, HAF, ISAF, SAF, and other carbon blacks commonly used in the tire industry can be used. Specifically, N110, N115, N120, N125, N134, N135, N219, N220, N231, N234, N293, N299, N326, N330, N339, N343, N347, N351, N356, N358, N375, N539, N550, N582, N630, N642, N650, N660, N683, N754, N762, N765, N772, N774, N787, N907, N908, N990, N991, and the like can be suitably used. In addition to these, in-house synthesized products and the like can also be suitably used. These carbon blacks may be used alone or in combination of two or more.
[0081] The nitrogen adsorption specific surface area of carbon black (N 2 SA) is a 50m 2 / g or more is preferable, and 80m 2 / g or more is more preferable, and 100m 2 From the viewpoints of dispersibility, fuel efficiency, breakage characteristics and pinch cut resistance, it is more preferable that the pore size is 250 m / g or more. 2 / g or less is preferable, and 220m 2 In this specification, the N 2 SA is a value measured in accordance with Method A of JIS K 6217-2 "Basic properties of carbon black for rubber - Part 2: Determination of specific surface area - Nitrogen adsorption method - Single point method".
[0082] When the rubber composition constituting the first layer 6 and the second layer 7 contains carbon black, the content thereof per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, from the viewpoint of weather resistance and reinforcement. Also, from the viewpoint of improving chipping resistance performance by suppressing heat generation in the tread portion, the content thereof is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 10 parts by mass or less. When the rubber composition constituting the third layer 8 contains carbon black, the content thereof per 100 parts by mass of the rubber component is preferably 20 to 100 parts by mass, more preferably 25 to 80 parts by mass, and even more preferably 30 to 60 parts by mass.
[0083] (silica) The silica is not particularly limited, and can be, for example, silica prepared by a dry method (anhydrous silica), silica prepared by a wet method (hydrated silica), or other silica commonly used in the tire industry. Among them, hydrated silica prepared by a wet method is preferred because it contains a large number of silanol groups. These silicas can be used alone or in combination of two or more.
[0084] The nitrogen adsorption specific surface area of silica (N 2 SA) is 140mm in order to ensure reinforcement and damping properties in the tread area. 2 / g or more is preferable, and 150m 2 / g or more is more preferable, and 160m 2 / g or more is more preferable, and 170m 2 From the viewpoint of heat generation and processability, it is particularly preferable that the tensile strength is 350 m 2 / g or less is preferable, and 300m 2 / g or less is more preferable, and 250m 2 / g or less is more preferable. 2 SA is a value measured by the BET method in accordance with ASTM D3037-93.
[0085] The average primary particle size of silica is preferably 20 nm or less, more preferably 18 nm or less. The lower limit of the average primary particle size is not particularly limited, but is preferably 1 nm or more, more preferably 3 nm or more, and even more preferably 5 nm or more. By having the average primary particle size of silica in the above range, the dispersibility of silica can be further improved, and the reinforcing properties, fracture properties, and abrasion resistance can be further improved. The average primary particle size of silica can be obtained by observing with a transmission or scanning electron microscope, measuring 400 or more primary particles of silica observed in the field of view, and averaging the results.
[0086] The content of silica per 100 parts by mass of the rubber component in the rubber composition constituting the first layer 6 and the second layer 7 is preferably 50 parts by mass or more, more preferably 60 parts by mass or more, even more preferably 70 parts by mass or more, and particularly preferably 80 parts by mass or more, from the viewpoint of ensuring damping properties in the tread portion and wet grip performance. Also, from the viewpoint of reducing the specific gravity of the rubber to reduce weight, and from the viewpoint of improving pinch cut resistance performance by suppressing heat generation in the tread portion, it is preferably 120 parts by mass or less, more preferably 110 parts by mass or less, even more preferably 105 parts by mass or less, and particularly preferably 100 parts by mass or less. The content of silica per 100 parts by mass of the rubber component in the rubber composition constituting the third layer 8 is not particularly limited.
[0087] (Other reinforcing fillers) As reinforcing fillers other than silica and carbon black, those which have been generally used in the tire industry, such as aluminum hydroxide, calcium carbonate, alumina, clay, and talc, can be used.
[0088] The silica content in the rubber composition constituting the first layer 6 and the second layer 7, based on the total of silica and carbon black (100 mass%), is preferably 60 mass% or more, more preferably 70 mass% or more, even more preferably 80 mass% or more, and particularly preferably 85 mass% or more. The silica content is preferably 99 mass% or less, more preferably 97 mass% or less, and even more preferably 95 mass% or less. It is believed that by setting the silica content in the above range, the interaction between the reinforcing filler and the free sulfur is reduced, and the free sulfur is more easily transferred to the first layer 6.
[0089] The rubber composition constituting the third layer 8 has a carbon black content of preferably 50 mass% or more, more preferably 75 mass% or more, even more preferably 90 mass% or more, and particularly preferably 100 mass% based on the total of silica and carbon black (100 mass%).
[0090] The total content of the reinforcing filler per 100 parts by mass of the rubber component is preferably 130 parts by mass or less, more preferably 120 parts by mass or less, even more preferably 110 parts by mass or less, and particularly preferably 105 parts by mass or less, from the viewpoint of reducing the specific gravity of the rubber and reducing the weight. Also, from the viewpoint of ensuring reinforcement and damping properties in the tread portion, the total content is preferably 55 parts by mass or more, more preferably 65 parts by mass or more, even more preferably 75 parts by mass or more, and particularly preferably 85 parts by mass or more.
[0091] (Silane coupling agent) Silica is preferably used in combination with a silane coupling agent. The silane coupling agent is not particularly limited, and any silane coupling agent that has been used in combination with silica in the tire industry can be used, for example, the following mercapto-based silane coupling agents; sulfide-based silane coupling agents such as bis(3-triethoxysilylpropyl) disulfide and bis(3-triethoxysilylpropyl) tetrasulfide; thioester-based silane coupling agents such as 3-octanoylthio-1-propyltriethoxysilane, 3-hexanoylthio-1-propyltriethoxysilane, and 3-octanoylthio-1-propyltrimethoxysilane; vinyltriethoxysilane, ... Examples of the silane coupling agent include vinyl-based silane coupling agents such as methoxysilane; amino-based silane coupling agents such as 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, and 3-(2-aminoethyl)aminopropyltriethoxysilane; glycidoxy-based silane coupling agents such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based silane coupling agents such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; chloro-based silane coupling agents such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane; and the like. Among these, it is preferable to contain a sulfide-based silane coupling agent and / or a mercapto-based silane coupling agent. These silane coupling agents may be used alone or in combination of two or more.
[0092] The mercapto-based silane coupling agent is preferably a compound represented by the following formula (1) and / or a compound containing a bonding unit A represented by the following formula (2) and a bonding unit B represented by the following formula (3). [ka] (In the formula, R 101 , R 102 , and R 103 are each independently an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or -O-(R111 -O) z -R 112 (z R 111 each independently represents a divalent hydrocarbon group having 1 to 30 carbon atoms; R 112 represents an alkyl group having 1 to 30 carbon atoms, an alkenyl group having 2 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an aralkyl group having 7 to 30 carbon atoms; z represents an integer of 1 to 30; 104 represents an alkylene having 1 to 6 carbon atoms. [ka] [ka] (wherein x represents an integer of 0 or more; y represents an integer of 1 or more; R 201 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 30 carbon atoms, an alkenyl group having 2 to 30 carbon atoms, or an alkynyl group having 2 to 30 carbon atoms, which may be substituted by a hydroxyl or carboxyl group; R 202 represents an alkylene having 1 to 30 carbon atoms, an alkenylene having 2 to 30 carbon atoms, or an alkynylene having 2 to 30 carbon atoms; 201 and R 202 may form a ring structure.)
[0093] Examples of the compound represented by formula (1) include 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and the compound represented by the following formula (4) (Si363 manufactured by Evonik Degussa), and the compound represented by the following formula (4) can be preferably used. These may be used alone or in combination of two or more. [ka]
[0094] Examples of compounds containing a bond unit A represented by formula (2) and a bond unit B represented by formula (3) include those manufactured and sold by Momentive, Inc. These may be used alone or in combination of two or more.
[0095] When containing silane coupling agent, the content relative to 100 parts by mass of silica is preferably 1.0 parts by mass or more, more preferably 3.0 parts by mass or more, and even more preferably 5.0 parts by mass or more, from the viewpoint of improving the dispersibility of silica. Also, from the viewpoint of preventing the deterioration of abrasion resistance, it is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less.
[0096] <Plasticizer> The rubber composition for a tread according to the present disclosure preferably contains a plasticizer. Examples of the plasticizer include a resin component, oil, and liquid rubber.
[0097] The rubber composition constituting the second layer 7 preferably contains a resin component. The resin component is not particularly limited, but may be a petroleum resin, a terpene resin, a rosin resin, a phenol resin, or the like commonly used in the tire industry, or may be a hydrogenated version of these. These resin components may be used alone or in combination of two or more.
[0098] In this specification, the term "C5 petroleum resin" refers to a resin obtained by polymerizing a C5 fraction. Examples of C5 fractions include petroleum fractions having 4 to 5 carbon atoms, such as cyclopentadiene, pentene, pentadiene, and isoprene. As the C5 petroleum resin, a cyclopentadiene resin is preferably used. Examples of the cyclopentadiene resin include dicyclopentadiene resin (DCPD resin), cyclopentadiene resin, methylcyclopentadiene resin (non-hydrogenated cyclopentadiene resin), and these cyclopentadiene resins that have been subjected to hydrogenation treatment (hydrogenated cyclopentadiene resin). As the cyclopentadiene resin, for example, commercially available products from ExxonMobil Chemical Corporation and the like can be used.
[0099] In this specification, the term "aromatic petroleum resin" refers to a resin obtained by polymerizing a C9 fraction, and may be a hydrogenated or modified resin. Examples of C9 fractions include petroleum fractions having 8 to 10 carbon atoms, such as vinyl toluene, alkyl styrene, indene, and methyl indene. Specific examples of aromatic petroleum resins include, for example, Coumarone-indene resin, coumaron resin, indene resin, and aromatic vinyl resin are preferably used. As the aromatic vinyl resin, a homopolymer of α-methylstyrene or styrene, or a copolymer of α-methylstyrene and styrene is preferred, and a copolymer of α-methylstyrene and styrene is more preferred, because they are economical, easy to process, and have excellent heat generation properties. As the aromatic vinyl resin, for example, commercially available products from Kraton, Eastman Chemical, etc. can be used.
[0100] In this specification, the term "C5C9 petroleum resin" refers to a resin obtained by copolymerizing the C5 fraction and the C9 fraction, and may be a hydrogenated or modified resin. Examples of the C5 fraction and the C9 fraction include the petroleum fractions described above. As the C5C9 petroleum resin, for example, those commercially available from Tosoh Corporation, LUHUA, etc. can be used.
[0101] Examples of the terpene resin include polyterpene resins consisting of at least one selected from terpene compounds such as α-pinene, β-pinene, limonene, and dipentene; aromatic modified terpene resins made from the terpene compounds and aromatic compounds; terpene phenolic resins made from terpene compounds and phenolic compounds; and terpene resins obtained by subjecting these terpene resins to hydrogenation treatment (hydrogenated terpene resins). Examples of aromatic compounds that are raw materials for aromatic modified terpene resins include styrene, α-methylstyrene, vinyltoluene, and divinyltoluene. Examples of phenolic compounds that are raw materials for terpene phenolic resins include phenol, bisphenol A, cresol, and xylenol. Examples of the terpene resins that can be used include those commercially available from Yasuhara Chemical Co., Ltd.
[0102] The rosin-based resin is not particularly limited, but examples thereof include natural rosin resin, modified rosin resin, etc. As the rosin-based resin, for example, those commercially available from Arakawa Chemical Industries, Ltd., Harima Chemical Industries, Ltd., etc. can be used.
[0103] The phenol-based resin is not particularly limited, but examples thereof include phenol formaldehyde resin, alkylphenol formaldehyde resin, alkylphenol acetylene resin, and oil-modified phenol formaldehyde resin.
[0104] From the viewpoint of wet grip performance, the softening point of the resin component is preferably 60° C. or higher, and more preferably 65° C. or higher. From the viewpoint of processability and improving the dispersibility of the rubber component and the filler, the softening point is preferably 150° C. or lower, more preferably 140° C. or lower, and even more preferably 130° C. or lower. In this specification, the softening point may be defined as the temperature at which the ball drops when the softening point specified in JIS K 6220-1:2001 is measured using a ring and ball softening point tester.
[0105] When a resin component is contained, the content per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 5 parts by mass or more, even more preferably 10 parts by mass or more, and particularly preferably 12 parts by mass or more, from the viewpoint of wet grip performance, and is preferably 60 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 40 parts by mass or less, and particularly preferably 30 parts by mass or less, from the viewpoint of suppressing heat buildup.
[0106] Examples of the oil include process oil, vegetable oil, and animal oil. Examples of the process oil include paraffin-based process oil, naphthenic process oil, and aromatic process oil. In addition, as an environmental measure, process oil with a low content of polycyclic aromatic compound (PCA) compounds can be used. Examples of the low PCA content process oil include light extract solvate (MES), treated distillate aromatic extract (TDAE), and heavy naphthenic oil.
[0107] When oil is contained, the content per 100 parts by mass of the rubber component is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more from the viewpoint of processability. Also, from the viewpoint of abrasion resistance, the content is preferably 100 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 60 parts by mass or less. In this specification, the content of oil includes the amount of oil contained in the oil-extended rubber.
[0108] The liquid rubber is not particularly limited as long as it is a polymer that is in a liquid state at room temperature (25° C.), and examples thereof include liquid butadiene rubber (liquid BR), liquid styrene butadiene rubber (liquid SBR), liquid isoprene rubber (liquid IR), liquid styrene isoprene rubber (liquid SIR), liquid farnesene rubber, etc. These liquid rubbers may be used alone or in combination of two or more kinds.
[0109] When the liquid rubber is contained, the content per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 2 parts by mass or more, even more preferably 3 parts by mass or more, and particularly preferably 5 parts by mass or more. The content of the liquid rubber is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 20 parts by mass or less.
[0110] When a plasticizer is contained, the content per 100 parts by mass of the rubber component (the total amount when multiple plasticizers are used in combination) is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and even more preferably 25 parts by mass or more from the viewpoint of wet grip performance, and is preferably 130 parts by mass or less, more preferably 120 parts by mass or less, even more preferably 110 parts by mass or less, even more preferably 70 parts by mass or less, and particularly preferably 50 parts by mass or less from the viewpoint of processability.
[0111] <Other compounding agents> In addition to the above-mentioned components, the rubber composition for tread according to the present disclosure may appropriately contain compounding agents generally used in the tire industry, such as wax, processing aid, stearic acid, zinc oxide, antioxidant, vulcanizing agent, vulcanization accelerator, etc.
[0112] When the wax is contained, the content thereof per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, and more preferably 1 part by mass or more, from the viewpoint of weather resistance of the rubber, and is preferably 10 parts by mass or less, and more preferably 5 parts by mass or less, from the viewpoint of preventing whitening of the tire due to bloom.
[0113] Examples of the processing aid include fatty acid metal salts, fatty acid amides, amide esters, silica surfactants, fatty acid esters, mixtures of fatty acid metal salts and amide esters, mixtures of fatty acid metal salts and fatty acid amides, etc. These processing aids may be used alone or in combination of two or more. Examples of the processing aids that can be used include those commercially available from Schill+Seilacher, Performance Additives, etc.
[0114] When a processing aid is contained, the content thereof per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, from the viewpoint of improving processability, and is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, from the viewpoints of abrasion resistance and breaking strength.
[0115] The antiaging agent is not particularly limited, but examples thereof include amine-based, quinoline-based, quinone-based, phenol-based, and imidazole-based compounds, and carbamic acid metal salts, and the like. Phenylenediamine-based antiaging agents such as N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, and N-cyclohexyl-N'-phenyl-p-phenylenediamine, and quinoline-based antiaging agents such as 2,2,4-trimethyl-1,2-dihydroquinoline polymer and 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline are preferred. These antiaging agents may be used alone or in combination of two or more.
[0116] When an antioxidant is contained, the content per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, from the viewpoint of ozone crack resistance of the rubber, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, from the viewpoint of abrasion resistance and wet grip performance.
[0117] When stearic acid is contained, the content thereof per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, from the viewpoint of processability, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, from the viewpoint of vulcanization speed.
[0118] When zinc oxide is contained, the content per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, from the viewpoint of processability, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, from the viewpoint of abrasion resistance.
[0119] As the vulcanizing agent, sulfur is preferably used, and examples of the sulfur that can be used include powdered sulfur, oil-treated sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, and highly dispersible sulfur.
[0120] When sulfur is contained as a vulcanizing agent, the content per 100 parts by mass of the rubber component is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, from the viewpoint of ensuring sufficient vulcanization reaction. From the viewpoint of preventing deterioration, the content is preferably 5.0 parts by mass or less, more preferably 4.0 parts by mass or less, and even more preferably 3.0 parts by mass or less. Note that, when oil-containing sulfur is used as a vulcanizing agent, the content of the vulcanizing agent is the total content of pure sulfur contained in the oil-containing sulfur.
[0121] Examples of vulcanizing agents other than sulfur include alkylphenol-sulfur chloride condensates, sodium 1,6-hexamethylene-dithiosulfate dihydrate, 1,6-bis(N,N'-dibenzylthiocarbamoyldithio)hexane, etc. As these vulcanizing agents other than sulfur, commercially available products from Taoka Chemical Co., Ltd., Lanxess Co., Ltd., Flexis, etc. can be used.
[0122] Examples of the vulcanization accelerator include sulfenamide-based, thiazole-based, thiuram-based, thiourea-based, guanidine-based, dithiocarbamic acid-based, aldehyde-amine-based or aldehyde-ammonia-based, imidazoline-based, and xanthate-based vulcanization accelerators. These vulcanization accelerators may be used alone or in combination of two or more. Among them, sulfenamide-based, guanidine-based, and thiazole-based vulcanization accelerators are preferred, and it is more preferred to use a sulfenamide-based vulcanization accelerator and a guanidine-based vulcanization accelerator in combination.
[0123] Examples of sulfenamide vulcanization accelerators include N-tert-butyl-2-benzothiazolylsulfenamide (TBBS), N-cyclohexyl-2-benzothiazolylsulfenamide (CBS), N,N-dicyclohexyl-2-benzothiazolylsulfenamide (DCBS), etc. Among them, N-cyclohexyl-2-benzothiazolylsulfenamide (CBS) is preferred.
[0124] Examples of the guanidine vulcanization accelerator include 1,3-diphenylguanidine (DPG), 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, di-o-tolylguanidine salt of dicatechol borate, 1,3-di-o-cumenylguanidine, 1,3-di-o-biphenylguanidine, 1,3-di-o-cumenyl-2-propionylguanidine, etc. Among them, 1,3-diphenylguanidine (DPG) is preferable.
[0125] Examples of the thiazole-based vulcanization accelerator include 2-mercaptobenzothiazole, cyclohexylamine salt of 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, etc. Among these, 2-mercaptobenzothiazole is preferred.
[0126] When a vulcanization accelerator is contained, the content per 100 parts by mass of the rubber component is preferably 1.0 part by mass or more, more preferably 1.5 parts by mass or more. The content per 100 parts by mass of the rubber component is preferably 8 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 6 parts by mass or less. By setting the content of the vulcanization accelerator within the above range, breaking strength and elongation tend to be secured.
[0127] The rubber composition according to the present disclosure can be produced by a known method, for example, by kneading the above-mentioned components using a rubber kneading device such as an open roll or an internal kneader (such as a Banbury mixer or kneader).
[0128] The kneading step includes, for example, a base kneading step in which compounding ingredients and additives other than the vulcanizing agent and the vulcanization accelerator are kneaded, and a final kneading (F kneading) step in which the vulcanizing agent and the vulcanization accelerator are added to the kneaded product obtained in the base kneading step and kneaded. Furthermore, the base kneading step can be divided into a plurality of steps as desired.
[0129] The kneading conditions are not particularly limited, but examples thereof include a method in which in the base kneading step, kneading is performed for 3 to 10 minutes at a discharge temperature of 150 to 170° C., and in the final kneading step, kneading is performed for 1 to 5 minutes at 70 to 110° C. The vulcanization conditions are not particularly limited, but examples thereof include a method in which vulcanization is performed for 10 to 30 minutes at 150 to 200° C.
[0130] [tire] The tire according to the present disclosure has a tread including a first layer 6, a second layer 7, and a third layer 8, and may be a pneumatic tire or a non-pneumatic tire. Examples of pneumatic tires include passenger car tires, truck and bus tires, motorcycle tires, and high performance tires. In this specification, the high performance tire is a tire that is particularly excellent in grip performance, and is a concept that includes racing tires used on racing vehicles.
[0131] A tire having a tread including the first layer 6, the second layer 7, and the third layer 8 can be manufactured by a normal method using the above rubber composition. That is, an unvulcanized rubber composition in which the above components are blended with the rubber component as necessary is extruded into the shapes of the first layer 6, the second layer 7, and the third layer 8 using an extruder equipped with a die of a predetermined shape, and then laminated together with other tire components on a tire building machine and molded by a normal method to form an unvulcanized tire, and the unvulcanized tire is heated and pressurized in a vulcanizer to manufacture a tire.
[0132] The tire of the present disclosure may be provided with a sealant, a noise damper, a sensor or tag for tire monitoring, and mounting members therefor in the tire cavity.
[0133] As the sealant, a sealant generally used on the inner peripheral surface of the tire tread portion for puncture prevention can be suitably used. Specific examples of such a sealant layer include those described in JP 2020-23152 A. The thickness of the sealant is usually preferably 1 to 10 mm. The width of the sealant is usually preferably 85 to 115% of the maximum width of the belt layer, and preferably 95 to 105%.
[0134] Any sound-damping body can be suitably used as long as it can exert a sound-damping effect in the tire cavity. Specific examples of such sound-damping bodies include those described in JP 2019-142503 A. The sound-damping body is, for example, made of a porous sponge material. The sponge material is a spongy porous structure, and includes, for example, a so-called sponge having continuous bubbles formed by foaming rubber or synthetic resin, as well as a web-like structure in which animal fibers, plant fibers, synthetic fibers, etc. are intertwined and connected together. In addition, the "porous structure" includes those having not only continuous bubbles but also closed bubbles. An example of the sound-damping body is a sponge material having continuous bubbles made of polyurethane. Suitable sponge materials include synthetic resin sponges such as ether-based polyurethane sponge, ester-based polyurethane sponge and polyethylene sponge, and rubber sponges such as chloroprene rubber sponge (CR sponge), ethylene propylene rubber sponge (EDPM sponge) and nitrile rubber sponge (NBR sponge). In particular, polyurethane-based or polyethylene-based sponges including ether-based polyurethane sponge are preferred from the standpoints of sound-damping properties, light weight, foaming adjustability, durability, and the like.
[0135] The sound-damping body is in the form of a long strip having a bottom surface fixed to the inner surface of the tread portion and extends in the circumferential direction of the tire. In this case, the outer ends in the circumferential direction may be butted against each other to form a substantially annular shape, or the outer ends may be spaced apart from each other in the circumferential direction. EXAMPLES
[0136] The present disclosure will be described based on examples, but the present disclosure is not limited to only the examples.
[0137] The various chemicals used in the examples and comparative examples are listed below. NR:TSR20 SBR1: Modified S-SBR produced in Production Example 1 described later (styrene content: 30 mass%, vinyl content: 52 mol%, Mw: 250,000, non-oil extended product) SBR2: Modified S-SBR (styrene content: 40% by mass, vinyl content: 25% by mole, Mw: 1.1 million, non-oil extended) BR: UBEPOL BR (registered trademark) 150B manufactured by Ube Industries, Ltd. (vinyl content: 1.5 mol%, cis content: 97 mol%, Tg: -108°C, Mw: 440,000) Carbon black: Diablack N220 (Mitsubishi Chemical Corporation) 2 SA:115m 2 / g) Silica: Ultrasil VN3 (N) manufactured by Evonik Degussa 2 SA: 175m 2 / g, average primary particle size: 18nm) Silane coupling agent 1: Si266 (bis(3-triethoxysilylpropyl) disulfide) manufactured by Evonik Degussa Silane coupling agent 2: NXT-Z45 (mercapto-based silane coupling agent) manufactured by Momentive Oil: VivaTec500 (TDAE oil) manufactured by H&R Corporation Resin component: Petrotac 100V manufactured by Tosoh Corporation (C5C9 petroleum resin, softening point: 96°C) Anti-aging agent: Antigen 6C (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine) manufactured by Sumitomo Chemical Co., Ltd. Wax: Sannock N manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Stearic acid: Beads of stearic acid camellia manufactured by NOF Corporation Zinc oxide: Two types of zinc oxide manufactured by Mitsui Mining & Smelting Co., Ltd. Sulfur: Powdered sulfur manufactured by Karuizawa Sulfur Co., Ltd. Vulcanization accelerator 1: Noccela CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide (CBS)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator 2: Noccelaer D (1,3-diphenylguanidine (DPG)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.
[0138] Preparation Example 1: Synthesis of SBR1 Cyclohexane, tetrahydrofuran, styrene, and 1,3-butadiene were charged into a nitrogen-substituted autoclave reactor. The temperature of the reactor contents was adjusted to 20°C, and n-butyllithium was added to initiate polymerization. Polymerization was carried out under adiabatic conditions, with the maximum temperature reaching 85°C. When the polymerization conversion rate reached 99%, 1,3-butadiene was added, and polymerization was continued for another 5 minutes, after which N,N-bis(trimethylsilyl)-3-aminopropyltrimethoxysilane was added as a modifier to carry out the reaction. After the polymerization reaction was completed, 2,6-di-tert-butyl-p-cresol was added. Next, the solvent was removed by steam stripping, and the mixture was dried with a heated roll adjusted to 110°C to obtain SBR1.
[0139] Examples and Comparative Examples According to the compounding recipe shown in Table 1, chemicals other than sulfur and vulcanization accelerator were kneaded for 1 to 10 minutes using a 1.7 L closed type Banbury mixer until the discharge temperature reached 150 to 160 ° C., and a kneaded product was obtained. Next, sulfur and vulcanization accelerator were added to the kneaded product obtained using a two-axis open roll, and the mixture was kneaded for 4 minutes until the temperature reached 105 ° C., and an unvulcanized rubber composition was obtained. The unvulcanized rubber composition obtained was extruded and molded into the shapes of the first layer (thickness: 3 mm), second layer (thickness: 3 mm), and third layer (thickness: 1 mm) of the tread using an extruder equipped with a die of a predetermined shape, and the extruded rubber composition was laminated together with other tire components to prepare an unvulcanized tire, and press-vulcanized for 12 minutes under the condition of 170 ° C. to obtain each test tire (size: 205 / 65R15, rim: 15 × 6JJ, internal pressure: 230 kPa) described in Table 2. The groove depth of the circumferential groove was set to 6 mm.
[0140] <Measurement of free sulfur content in the first, second and third layers> The sulfur content Ts (mass%) in each rubber test piece after vulcanization was calculated by the oxygen combustion flask method according to JIS K 6233:2016. Next, the test piece was immersed in acetone for 24 hours according to JIS K 6229-3:2015 to extract the soluble components. The test piece after the soluble components were extracted was placed in an oven and heated at 100°C for 30 minutes to remove the solvent in the test piece, and then the sulfur content As (mass%) in the test piece was calculated by the oxygen combustion flask method according to JIS K 6233:2016. The free sulfur content was calculated by calculating the difference (Ts-As) between the sulfur content Ts and the sulfur content As. The rubber test pieces of the first layer, second layer, and third layer were cut out from the tread portion of each test tire.
[0141] <Measurement of acetone extractables (AE amount) from the first, second and third layers> In accordance with JIS K 6229:2015, each vulcanized rubber test piece was immersed in acetone for 24 hours to extract the soluble components. The mass of each test piece was measured before and after extraction, and the amount of acetone extracted was calculated using the following formula. The rubber test pieces for the first, second and third layers were cut out from the tread portion of each test tire. Acetone extractable amount (mass%)={(mass of rubber test piece before extraction-mass of rubber test piece after extraction) / (mass of rubber test piece before extraction)}×100
[0142] <Measurement of toluene swelling index and mass change rate> In accordance with JIS K 6258:2016, the mass of each vulcanized rubber test piece was measured before and after immersion in toluene at 23°C for 24 hours, and the toluene swelling index was calculated using the following formula. The results are shown in Table 1. The mass change rate (%) is calculated by subtracting 100 from the calculated toluene swelling index. The smaller the toluene swelling index and mass change rate, the higher the crosslink density. (Toluene swelling index) = (weight after immersion) / (weight before immersion) x 100
[0143] <Tensile test> A dumbbell-shaped No. 7 test piece was prepared by cutting out each rubber layer of the tread portion of each test tire so that the tire circumferential direction was the tensile direction. In accordance with JIS K 6251:2017 "Vulcanized rubber and thermoplastic rubber - Determination of tensile test properties", a tensile test was carried out on the dumbbell-shaped No. 7 test piece in an atmosphere of 23°C at a tensile speed of 3.3 mm / sec, and the modulus (MPa) at 100% elongation was measured.
[0144] <Measurement of loss tangent tanδ> Each rubber test piece after vulcanization was cut from each rubber layer of the tread of each test tire with a length of 20 mm, width of 4 mm, and thickness of 1 mm, with the long side in the tire circumferential direction. The loss tangent tanδ of each rubber test piece was measured using a GABO Iplexer series under the conditions of temperature 0°C, initial strain 10%, dynamic strain 1%, and frequency 10 Hz. The thickness direction of the sample was the tire radial direction.
[0145] <Rubber hardness measurement> The tire was cut in the radial direction to a width of 20 mm, and the cut surfaces were smoothed. A type A durometer was then pressed against the surfaces in the cross-sectional direction to measure the Shore hardness (Hs) at 23° C. of each rubber layer after vulcanization.
[0146] <Wet driving stability> Each test tire was fitted to all wheels of a vehicle (domestic FF 2000cc), which was driven 10 laps around a test course with a wet asphalt surface, and the handling stability when entering, turning, and exiting corners was scored on a 10-point scale based on the feeling of 10 test drivers, a total score was calculated, and the score of Comparative Example 1 was indexed to 100. A higher value indicates better handling stability on wet roads.
[0147] <Total wear resistance> Each test tire was mounted on all wheels of a vehicle (domestic FF 2000cc), and the distance traveled until the wear indicator became exposed was measured and indexed with the distance traveled for Comparative Example 1 being set at 100. A higher index indicates better overall wear resistance up to the end of the run.
[0148] [Table 1]
[0149] [Table 2]
[0150] The results in Tables 1 and 2 show that tires of the present disclosure, which have three or more rubber layers in the tread portion and a gradient in the concentration of free sulfur from the rubber layer on the radially inner side of the tire to the rubber layer on the radially outer side of the tire, have improved steering stability on wet roads and overall wear resistance up to the end of the journey (the sum of the wet steering stability performance index and the total wear resistance performance index). [Explanation of symbols]
[0151] 1...Circumferential groove 2... land department 3. Tread surface 4. Land extension 5. Extension line of the deepest part of the bottom of the circumferential groove 6...First layer 7...Second layer 8...Third layer 9. The outermost extension of the second layer 11. Shoulder land section 12. Center Land Section 21. Shoulder groove 22. Shoulder sipes 23. Center sipe
Claims
1. A tire having a tread including at least a first layer constituting a tread surface, a second layer adjacent to the radially inner side of the first layer, and a third layer adjacent to the radially inner side of the second layer, the first layer, the second layer and the third layer are made of a rubber composition containing a rubber component, the free sulfur content of the rubber composition constituting the third layer is greater than the free sulfur content of the rubber composition constituting the second layer, The tire in which the free sulfur content of the rubber composition constituting the second layer is greater than the free sulfur content of the rubber composition constituting the first layer.
2. The mass change rate X of the rubber composition constituting the first layer before and after immersion in toluene at 23 ° C. for 24 hours measured in accordance with JIS K 6258: 2016 1 (%), and the mass change rate X of the rubber composition constituting the second layer before and after immersion in toluene at 23 ° C. for 24 hours, measured in accordance with JIS K 6258: 2016 2 (%) and the difference (X 1 -X 2 2. The tire of claim 1, wherein the axial length of the tire is 50% or less.
3. 3. The tire according to claim 1, wherein the rubber composition constituting the first layer and the rubber composition constituting the second layer have a tan δ at 0° C. of 0.45 or more.
4. The tire according to any one of claims 1 to 3, wherein a difference in hardness between the rubber composition constituting the second layer and the rubber composition constituting the first layer is 5 or less.
5. The tire according to any one of claims 1 to 4, wherein the specific gravity of the rubber composition constituting the first layer and the rubber composition constituting the second layer is each 1.25 or less.
6. The tire according to any one of claims 1 to 5, wherein the rubber composition constituting the second layer has a specific gravity of less than 1.
20.
7. The acetone extractable amount AE of the rubber composition constituting the second layer 2 The acetone extractable amount AE of the rubber composition constituting the first layer is 1 A tire according to any one of claims 1 to 6, wherein the tread width is greater than 100 mm.
8. The tire according to any one of claims 1 to 7, wherein a modulus of the rubber composition constituting the second layer at 100% elongation at 23°C is greater than a modulus of the rubber composition constituting the first layer at 100% elongation at 23°C.
9. The tire according to any one of claims 1 to 8, wherein the rubber component constituting the first layer and the rubber component constituting the second layer each contain butadiene rubber.
10. The tire according to any one of claims 1 to 9, wherein the rubber composition constituting the first layer and the rubber composition constituting the second layer each contain a reinforcing filler and a silane coupling agent, and the content of silica in the reinforcing filler in the rubber composition constituting the first layer and the content of silica in the reinforcing filler in the rubber composition constituting the second layer are 80 mass% or more.
11. The tire according to claim 10, wherein the silane coupling agent contained in the rubber composition constituting the first layer and the rubber composition constituting the second layer are each a mercapto-based silane coupling agent.
12. The tire according to any one of claims 1 to 11, wherein the rubber composition constituting the second layer contains a resin component.
13. A tire according to any one of claims 1 to 12, wherein the third layer has a thickness less than the thicknesses of the first and second layers.
14. The tire according to any one of claims 1 to 13, wherein the tread has a land portion partitioned by a plurality of circumferential grooves, and a deepest portion of a groove bottom of at least one of the circumferential grooves is formed so as to be located radially inward of an outermost portion of the second layer.
15. The tire according to claim 14 , wherein the land portion has a sipe, both ends of which are not open to the circumferential groove.
Citation Information
Patent Citations
Large tire
JP1994040214A
Pneumatic tire
JP2008174638A
High silica content for heavy vehicle tires
JP2013514428A