Packaging materials and packaging bags

The packaging material with a hydrocarbon wax heat seal layer, styrene-acrylic copolymer resin surface protective layer, and polyvinyl alcohol barrier layer addresses high blocking resistance and oxygen barrier issues, enhancing performance and sustainability.

JP7567949B2Active Publication Date: 2024-10-16TOYO INK MFG CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023012039
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-01-30
Publication Date
2024-10-16
Estimated Expiration
2043-01-30

AI Technical Summary

Technical Problem

Existing packaging materials face challenges with high blocking resistance, particularly at the center of winding, lack of water friction resistance, and insufficient oxygen barrier properties, while also relying heavily on petroleum-derived plastics.

Method used

A packaging material comprising a heat seal layer with hydrocarbon wax, a paper base material, and a surface protective layer containing a styrene-acrylic copolymer resin with a glass transition temperature of 12°C or higher, along with a barrier layer made of polyvinyl alcohol resin, and optionally including glycol compounds, to enhance blocking resistance, water friction resistance, and oxygen barrier properties.

Benefits of technology

The solution provides a packaging material with improved blocking resistance, water friction resistance, and oxygen barrier properties, while reducing the reliance on petroleum-derived plastics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567949000001
    Figure 0007567949000001
  • Figure 0007567949000002
    Figure 0007567949000002
  • Figure 0007567949000003
    Figure 0007567949000003
Patent Text Reader

Abstract

To provide a packaging material which has excellent oxygen barrier property, heat-sealablility, anti-blocking property and wet friction resistance.SOLUTION: A packaging material includes a heat seal layer, a paper base material and a surface protective layer in this order. The heat seal layer contains hydrocarbon system wax. Hardness (penetration degree) at 25°C of the hydrocarbon system wax specified by JISK2207 is equal to or less than 12. The surface protective layer contains styrene-acrylic copolymer resin (A) whose glass transformation temperature is equal to or higher than 12°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a packaging material, a packaging bag, and a method for producing the same. [Background technology]

[0002] In recent years, it has become common for product packages and other wrapping materials to be printed for decoration and surface protection. Furthermore, the quality of printing, such as the design, beauty, and luxury of the printed matter, can stimulate consumer purchasing motivation and is of great industrial value.

[0003] Generally, plastic films are mainly used to construct packages, and since they are transparent, there are also usage methods that allow the contents to be visually confirmed, and laminated packaging materials have been used in particular. For example, Patent Document 1 describes an invention of a laminated packaging material consisting of a base material, a printing layer, an adhesive layer, and a sealant layer, in which biomass resin is used in the printing layer and the adhesive layer. However, laminated packaging materials have the problem that they use a large amount of petroleum-derived plastic film. For this reason, there is a demand for packaging materials that are carbon neutral and can reduce the amount of plastic used, and technological developments are being made.

[0004] On the other hand, since the packaging material is stored in a rolled-up state on a paper tube, the surface protection layer and the heat seal layer are in contact with each other and are under load during storage. The load on the packaging material is particularly large toward the center of the roll, making blocking very likely to occur, and therefore high blocking resistance is required.

[0005] Patent Document 2 describes a paper packaging material having a structure of a heat seal layer / paper base material / surface protective layer, the surface protective layer containing a styrene-acrylic copolymer resin. Patent Document 3 describes a paper packaging material having a structure of a paper base material / printed layer / surface protective layer, the surface protective layer containing a styrene-acrylic copolymer resin.

[0006] However, the packaging material of Patent Document 2 is strong enough to withstand a load of 10 kgf / cm 2However, there is no mention of blocking resistance assuming a high load at the center of winding, and no mention of water friction resistance or oxygen barrier properties. In addition, since the packaging material in Patent Document 3 is intended to be folded to wrap food or the like, it does not have a heat seal layer, and there is no mention of heat sealability or blocking resistance. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2018-051796 A [Patent Document 2] International Publication No. 2022 / 071261 [Patent Document 3] Patent Publication No. 2021-38022 Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a packaging material that is excellent in oxygen barrier properties, heat sealability, blocking resistance, and water friction resistance. [Means for solving the problem]

[0009] As a result of extensive research into the above problems, the present inventors have found that the above problems can be solved by using the packaging material described below, and have thus completed the present invention.

[0010] That is, the present invention provides: A packaging material having a heat seal layer, a paper base material, and a surface protective layer in this order, The heat seal layer comprises a hydrocarbon wax, The hardness (penetration) of the hydrocarbon wax at 25°C as defined in JIS K2207 is 12 or less, The present invention relates to a packaging material, wherein the surface protective layer contains a styrene-acrylic copolymer resin (A) having a glass transition temperature of 12°C or higher.

[0011] The present invention also relates to the packaging material, wherein the heat seal layer contains an ethylene-vinyl acetate copolymer resin and / or an acrylic resin.

[0012] The present invention also relates to the packaging material, further comprising a barrier layer.

[0013] The present invention also relates to the packaging material, wherein the barrier layer contains a polyvinyl alcohol-based resin.

[0014] The present invention also relates to the packaging material, wherein the surface protective layer further contains a glycol compound.

[0015] The present invention also relates to the packaging material, wherein the glycol compound comprises at least one selected from the group consisting of butyl cellosolve, propylene glycol, and ethylene glycol.

[0016] The present invention also relates to the packaging material, wherein the content of the glycol compound in the surface protective layer is 0.01 to 15% by mass, relative to 100% by mass of the surface protective layer.

[0017] The present invention also relates to a packaging bag formed from the packaging material.

[0018] The present invention also provides a method for producing a packaging material having a heat seal layer, a paper base material, and a printing layer in this order, comprising: A step of printing a heat sealant containing a hydrocarbon wax on one side of a paper substrate to form a printed layer; A step of printing an overcoat agent containing a styrene-acrylic copolymer resin (A) having a glass transition temperature of 12°C or higher on the other side of the paper substrate to form a surface protective layer; Including, The present invention relates to a method for producing a packaging material, wherein the hydrocarbon wax has a hardness (penetration) of 12 at 25° C. as specified in JIS K2207. Effect of the Invention

[0019] The present invention makes it possible to provide a packaging material that is excellent in oxygen barrier properties, heat sealing properties, blocking resistance, and water friction resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The following describes in detail the embodiments of the present invention. However, the following description of the components is merely an example of an embodiment of the present invention, and the present invention is not limited to these contents as long as it does not deviate from the gist of the present invention.

[0021] In the following description, unless otherwise specified, "parts" refers to "parts by mass" and "%" refers to "% by mass." In addition, the packaging material may be referred to as a "laminate," but this has the same meaning. In addition, "printing ink" refers to ink containing pigments and other colorants for forming a printed layer. "Overcoat agent" refers to a coating agent that does not contain pigments or other colorants for forming a surface protective layer, but does not exclude traces of colorants that are unintentionally mixed in.

[0022] [Packaging material] The present invention relates to a packaging material having a heat seal layer, a paper base material, and a surface protective layer in this order, wherein the heat seal layer contains a hydrocarbon wax, the hydrocarbon wax has a hardness (penetration) at 25°C specified in JIS K2207 of 12 or less, and the surface protective layer contains a styrene-acrylic copolymer resin (A) having a glass transition temperature of 12°C or more.

[0023] In the present application, the hardness of the surface protective layer is increased by using a styrene-acrylic copolymer resin with a high glass transition temperature for the surface protective layer, and the adhesion between the surface protective layer and the heat seal layer is reduced by including a hard hydrocarbon wax in the heat seal layer. These synergistic effects have realized a packaging material with excellent blocking resistance during winding. Furthermore, the surface protective layer contains a styrene-acrylic copolymer resin (A) with a glass transition temperature of 12°C or higher, improving water friction resistance and oxygen barrier properties. Note that this explanation is based on speculation only and does not limit the invention in any way.

[0024] In the present application, examples of the laminated structure of the packaging material are preferably as follows, but are not intended to limit the present invention in any way. In the following examples, " / " indicates the boundary between layers. Heat seal layer / paper base material / surface protection layer Heat seal layer / paper base material / printing layer / surface protection layer Heat seal layer / paper base material / barrier layer / printing layer / surface protection layer Heat seal layer / paper base material / printing layer / barrier layer / surface protection layer Heat seal layer / barrier layer / paper base material / printing layer / surface protection layer

[0025] [Surface protective layer] In the present application, the surface protective layer contains a styrene-acrylic copolymer resin (A) having a glass transition temperature of 12° C. or higher. In addition, from the viewpoint of film-forming properties, it preferably contains a glycol-based compound. The surface protective layer is located on the opposite side of the paper substrate to the side having the heat seal layer, and can be formed from an overcoat agent containing a styrene-acrylic copolymer resin (A) having a glass transition temperature of 12° C. or higher. The formation method can be appropriately selected from known printing methods such as gravure printing and flexographic printing, and is preferably flexographic printing. The coating weight of the surface protection layer is 0.5 to 9 g / m 2 is preferably 1 to 5 g / m 2 More preferably, the thickness is 1.5 to 2.5 g / m 2 It is more preferable that the coating amount of the surface protective layer is 0.5 g / m 2 When the coating amount is 8 g / m or more, the oxygen barrier property and water friction resistance become good. 2 When it is equal to or less than this, the amount of the residual solvent in the surface protective layer is reduced, and therefore blocking resistance is improved.

[0026] <Styrene-acrylic copolymer resin (A)> The styrene-acrylic copolymer resin (A) is preferably an aqueous resin, which may be either a water-soluble resin or an aqueous emulsion resin, but is preferably an aqueous emulsion resin.

[0027] The glass transition temperature of the styrene-acrylic copolymer resin (A) is 12°C or higher, preferably 12 to 80°C, more preferably 15 to 60°C, and even more preferably 20 to 50°C. When the glass transition temperature is within the above range, the oxygen barrier property, blocking resistance, and water friction resistance are good. The acid value of the styrene-acrylic copolymer resin (A) is preferably 20 to 200 mgKOH / g, more preferably 30 to 150 mgKOH / g, and even more preferably 70 to 120 mgKOH / g. When it is within the above range, the blocking resistance is good. The weight average molecular weight of the styrene-acrylic copolymer resin (A) is preferably 10,000 to 600,000, more preferably 50,000 to 500,000, more preferably 100,000 to 400,000, and particularly preferably 200,000 to 300,000. When it is within the above range, the water friction resistance is good.

[0028] <Acid value measurement> In the present application, the acid value is the number of milligrams of potassium hydroxide required to neutralize the acidic groups contained in 1 g of resin solid content, and is measured in accordance with JIS K0070.

[0029] <<Measurement of glass transition temperature>> In the present application, the glass transition temperature was measured by simultaneous thermogravimetry and differential thermal analysis (TG-DTA) using a DTG-60A manufactured by Shimadzu Corporation. In detail, the glass transition temperature was determined as the inflection point temperature in the baseline shift under the conditions of a nitrogen atmosphere, a measurement temperature range of −100 to 200° C., and a heating rate of 1° C. / min.

[0030] <Measurement of weight average molecular weight> In this application, the weight average molecular weight can be determined as a converted molecular weight using polyethylene glycol as a standard substance, and the measuring device used was a GPC device: Shodex GPC-401 manufactured by Showa Denko K.K. The column was a Shodex OHpak LB-805 manufactured by Showa Denko K.K. The detector was an RI (differential refractometer). The eluent used was a 0.1N NaNO3 aqueous solution, the column temperature was 35°C, and the flow rate was 3 mL / min.

[0031] The styrene-acrylic copolymer resin (A) contained in the surface protective layer may be a commercially available product, for example, HE-1335, X-436, QE-1042, etc. manufactured by Seiko PMC Corporation.

[0032] The content of the styrene-acrylic copolymer resin (A) in the surface protective layer is preferably 50 to 99% by mass, more preferably 70 to 97% by mass, and even more preferably 90 to 95% by mass, based on 100% by mass of the surface protective layer. When it is within the above range, blocking resistance and water friction resistance are improved.

[0033] <Resins other than styrene-acrylic copolymer resin (A)> The surface protective layer may further contain a resin other than the styrene-acrylic copolymer resin (A), such as a urethane resin, a polylactic acid resin, a rosin-based resin, a vinyl acetate resin, a vinyl acetate resin, an acrylic resin, a urethane-acrylic resin, a styrene-maleic acid copolymer resin, a rosin-modified maleic acid resin, etc. These resins may be used alone or in combination of two or more.

[0034] <Glycol compounds> In the present invention, the surface protective layer preferably contains a glycol-based compound. As described later in <Formation of Surface Protective Layer>, the surface protective layer can be formed by applying an overcoat agent and drying it, and a part of the glycol-based compound remains in the surface protective layer upon drying, improving the film-forming properties of the surface protective layer. The boiling point of the glycol compound is preferably 240° C. or less, more preferably 130 to 240° C., and even more preferably 150 to 200° C. When it is within the above range, the surface protective layer has a good balance between film-forming property and tackiness, and has good water friction resistance and blocking resistance.

[0035] Examples of glycol compounds include ethylene glycol (boiling point 197°C), ethylene glycol monomethyl ether (boiling point 124°C), ethylene glycol monoethyl ether (boiling point 135°C), ethylene glycol monopropyl ether (boiling point 150°C), butyl cellosolve (ethylene glycol monobutyl ether (boiling point 168°C)), diethylene glycol monomethyl ether (boiling point 193°C), diethylene glycol monoethyl ether (boiling point 202°C), diethylene glycol monobutyl ether (boiling point 231°C), triethylene glycol (boiling point 177°C), propylene glycol (boiling point 188°C), and propylene glycol. Examples of the solvent include glycol monomethyl ether (boiling point 120°C), propylene glycol monoethyl ether (boiling point 132°C), propylene glycol monopropyl ether (boiling point 149°C), propylene glycol monobutyl ether (boiling point 170°C), dipropylene glycol (boiling point 230°C), dipropylene glycol monomethyl ether (boiling point 189°C), dipropylene glycol monopropyl ether (boiling point 210°C), dipropylene glycol monobutyl ether (boiling point 230°C), and the like. It is preferable to include at least one selected from the group consisting of butyl cellosolve, propylene glycol, and ethylene glycol. These may be used alone or in combination of two or more.

[0036] The content of the glycol compound in the surface protective layer is preferably 0.01 to 15% by mass, more preferably 0.1 to 10% by mass, further preferably 1 to 5% by mass, and particularly preferably 1.5 to 3.5% by mass, based on 100% by mass of the surface protective layer. When it is within the above range, the balance between film-forming property and tackiness is good, and water friction resistance and blocking resistance are good.

[0037] <Additives contained in the surface protective layer> The surface protective layer of the present invention may contain various additives as required, such as a dispersant, a wax, an extender pigment, a leveling agent, a defoaming agent, a water repellent, and a release agent. Specifically, various additives such as wax resin fine particle dispersion of hydrocarbon wax such as polyethylene wax can be added to improve blocking resistance and water friction resistance, extender pigments such as silica, barium sulfate, resin beads, calcium carbonate, and talc can be added to improve drying property and coating film hiding property, inorganic fine particles and adhesive resins (acrylic resin, vinyl acetate resin, etc.) can be added to impart anti-slip properties, leveling agents can be added to improve leveling properties, defoaming agents can be added to impart defoaming properties, and basic compounds such as ammonia, amine compounds, sodium hydroxide, and potassium hydroxide can be added to impart resolubility properties, and from the viewpoint of improving water friction resistance and blocking resistance, it is preferable to include a hydrocarbon wax such as polyethylene wax. For the hydrocarbon wax, the embodiment of <hydrocarbon wax> described in [Heat seal layer] described later can be used.

[0038] The content of the hydrocarbon wax in the surface protective layer is preferably 0.1 to 10% by mass, more preferably 0.5 to 5% by mass, and even more preferably 1 to 3% by mass, based on 100% by mass of the surface protective layer. When it is in the above range, blocking resistance is good.

[0039] <Overcoat agent> The surface protective layer is preferably formed by an overcoat agent. The overcoat agent is preferably an aqueous overcoat agent. The overcoat agent preferably contains a styrene-acrylic copolymer resin (A) and an aqueous medium, and further contains the above-mentioned glycol-based compound and hydrocarbon-based wax. In addition, the overcoat agent may contain a resin other than the styrene-acrylic copolymer resin (A) and / or the additives contained in the above-mentioned surface protective layer. The viscosity of the overcoat agent is preferably 20 to 200 mPa·s from the viewpoint of printability, etc.

[0040] The solid content of the styrene-acrylic copolymer resin (A) in the overcoat agent is preferably 10 to 70 mass% and more preferably 25 to 75 mass% based on the total mass of the overcoat agent. The glycol compound content in the overcoat agent is preferably 0.1 to 10 mass% and more preferably 1 to 8 mass% based on the total mass of the overcoat agent. The hydrocarbon wax content in the overcoat agent is preferably 0.1 to 10 mass% and more preferably 0.5 to 5 mass% based on the total mass of the overcoat agent.

[0041] (Aqueous media (excluding glycol compounds)) The overcoat agent preferably contains an aqueous medium. The main component of the aqueous medium is preferably water, but a water-soluble organic solvent can be used in addition to water. Specifically, alcohol-based organic solvents other than glycol-based compounds can be included depending on the printing conditions (speed, plate depth, design, drying temperature). The content of the aqueous medium is preferably 30% by mass or less based on the total amount of the overcoat agent. In the present invention, the term "mainly water" means that the content of water is the largest in the aqueous medium, and the term "water-soluble organic solvent" means that the solvent is liquid at 25° C. and has a solubility of 1% by mass or more in water at 25° C.

[0042] Examples of the alcohol-based organic solvent include methanol, ethanol, propanol, isopropanol, isobutanol, normal butanol, tert-butanol, hexanol, octanol, and decanol.

[0043] <Method of manufacturing the overcoat agent> The overcoat agent can be obtained by mixing and stirring a resin solution in which a resin is dissolved or dispersed in a solvent, a solvent, and additives in a stirrer equipped with stirring blades, rotors, etc. There is no particular restriction on the stirring speed, and stirring can be performed at 50 to 2000 rpm. In order to improve the handling and coating properties of the overcoat agent, an aqueous medium can also be appropriately added.

[0044] <Formation of surface protection layer> The surface protective layer can be formed, for example, by printing on a paper substrate or a printing layer described later using an overcoat agent, and then removing the aqueous medium. As the printing method, known printing methods such as flexographic printing and gravure printing can be used, and flexographic printing is preferred. For example, the overcoat agent is diluted with a diluting solvent to a viscosity suitable for flexographic printing, and is supplied to each printing unit alone or in a mixture and applied. Thereafter, the aqueous medium is removed by drying in an oven or the like to form the surface protective layer.

[0045] (Flexographic printing) Plates used in flexographic printing include photosensitive resin plates that utilize ultraviolet curing with a UV light source, and elastomer material plates that use a direct laser engraving method. Regardless of the method used to form the image area of ​​the flexographic plate, a plate with a screen line count of 30 lpi or more is used. Any sleeve or cushion tape can be used to attach the plate.

[0046] Flexographic printing machines include CI type multi-color flexographic printing machines and unit type multi-color flexographic printing machines, and methods for supplying the heat seal agent as ink include a chamber method and a two-roll method, and an appropriate printing machine can be used.

[0047] [Heat seal layer] The heat seal layer in the present application contains a hydrocarbon wax having a hardness (penetration) of 12 or less at 25°C as specified by JISK2207. The heat seal layer is located on the side of the paper substrate opposite to the surface having the surface protective layer, and can be formed by printing and drying a heat seal agent containing a hydrocarbon wax having a hardness (penetration) of 12 or less at 25°C as specified by JISK2207 on the paper substrate or on a barrier layer described below. The coating amount of the heat seal agent is 1 to 18 g / m 2 and 2 to 12 g / m 2 is preferably 3 to 8 g / m2 When it is in the above range, the heat sealability and blocking resistance are excellent.

[0048] <Hydrocarbon wax> The heat seal layer contains a hydrocarbon wax, and the hardness (penetration) of the hydrocarbon wax at 25°C as specified by JIS K2207 is 12 or less. Examples of the hydrocarbon wax include, but are not limited to, polyethylene wax, Fischer-Tropsch wax, paraffin wax, microcrystalline wax, polypropylene wax, etc. Among them, polyethylene wax and / or Fischer-Tropsch wax are preferable.

[0049] The hardness (penetration) of the hydrocarbon wax at 25°C as specified by JISK2207 is 12 or less, preferably 0.5 to 8, more preferably 1 to 5, further preferably 2 to 4, and particularly preferably 2.5 to 3.5. When it is within the above range, the heat sealability and blocking resistance are excellent. The density of the hydrocarbon wax at 23°C as specified by JISK7112 (Method B) is 900 to 990 kg / m 3 is preferably 925 to 990 kg / m 3 It is more preferable that the melting point is within the above range. When it is within the above range, the blocking resistance is good. The melting point of the hydrocarbon wax in DSC measurement is preferably 90 to 150°C, more preferably 100 to 125°C. When it is within the above range, the heat sealability and blocking resistance are good. The melting point of the hydrocarbon wax refers to the melting point of the peak top (minimum value) of the endothermic peak in the DSC temperature rise curve. The average particle size of the hydrocarbon wax is preferably 0.5 to 12 μm, more preferably 1 to 10 μm, and even more preferably 1.5 to 4 μm. The average particle size of the hydrocarbon wax refers to the D50 value measured by laser diffraction / light scattering method.

[0050] The content of the hydrocarbon wax in the heat seal layer is preferably 0.1 to 10 mass%, more preferably 0.5 to 5 mass%, and even more preferably 1 to 3 mass%, based on 100 mass% of the heat seal layer. When it is within the above range, the heat sealability and blocking resistance are good.

[0051] (Polyethylene wax) The polyethylene wax is not particularly limited, but examples thereof include high-density polymerized polyethylene, low-density polymerized polyethylene, oxidized polyethylene, acid-modified polyethylene, and special monomer-modified polyethylene. The polyethylene wax has a density of 925 to 990 kg / m at 23° C. as specified in JIS K7112 (B method). 3 and the melt viscosity at 140°C measured in accordance with JIS K6862 is preferably 50 to 8000 mPa s. The polyethylene wax may have an acid value. If it has an acid value, the acid value is preferably 0.5 to 70 mgKOH / g. The polyethylene wax preferably has a melting point in DSC measurement of 90 to 150°C, more preferably 100 to 125°C.

[0052] Fischer-Tropsch wax is a wax produced by the Fischer-Tropsch process using carbon monoxide and hydrogen as raw materials, and is composed of a nearly saturated, unbranched, linear molecular structure. Due to its linear structure, it has a high melting point, low viscosity, and is hard. Fischer-Tropsch wax hardly deteriorates even when exposed to heat for a long period of time, and shows extremely high thermal stability. The number average molecular weight of Fischer-Tropsch wax is preferably 400 to 2000. In addition, Fischer-Tropsch wax has a density of 925 to 990 kg / m at 23°C as specified in JIS K7112 (Method B). 3The Fischer-Tropsch wax may have an acid value. When the Fischer-Tropsch wax has an acid value, the acid value is preferably 0.5 to 50 mgKOH / g. The Fischer-Tropsch wax preferably has a melting point of 90 to 130°C, more preferably 100 to 120°C, as measured by DSC.

[0053] The heat seal layer preferably contains a resin, and examples of the resin that can be used include acrylic resin, ethylene-vinyl acetate copolymer resin, urethane resin, polyethylene resin, polypropylene resin, etc. From the viewpoint of achieving both blocking resistance and heat sealability, acrylic resin and ethylene-vinyl acetate copolymer resin are preferred, and ethylene-vinyl acetate copolymer resin is more preferred. These may be used alone or in combination of two or more.

[0054] <Ethylene-vinyl acetate copolymer resin> The ethylene-vinyl acetate copolymer resin is a copolymer made of ethylene and vinyl acetate. The vinyl acetate content in the ethylene-vinyl acetate copolymer resin is preferably 5 to 50 mass%, more preferably 10 to 40 mass%, and particularly preferably 20 to 30 mass%, based on 100 mass% of the ethylene-vinyl acetate copolymer resin. The minimum film-forming temperature of the ethylene-vinyl acetate copolymer resin is preferably 40 to 120°C, and more preferably 60 to 100°C. When the vinyl acetate content and the minimum film-forming temperature are within the above ranges, the heat sealability is good. The glass transition temperature of the ethylene-vinyl acetate copolymer resin is preferably -60 to 20°C, more preferably -25 to 5°C, and particularly preferably -20 to -10°C.

[0055] <Measurement of minimum film-forming temperature> In the present application, the temperature measured in accordance with JIS K 6828-1:2003 using a TP-801MFT tester manufactured by Tester Sangyo Co., Ltd. was defined as the minimum film-forming temperature.

[0056] Examples of the ethylene-vinyl acetate copolymer resin that can be used include Aquatex EC series manufactured by Japan Coating Resins Co., Ltd., and Sumikaflex S-201HQ, S-305, S-305HQ, S-328HQ, S-400HQ, S-401HQ, S-408HQE, S-410HQ, S-450HQ, S-455HQ, S-456HQ, S-460HQ, S-467HQ, S-470HQ, S-480HQ, S-510HQ, S-520HQ, S-752, and S-755 manufactured by Sumitomo Chemical Co., Ltd.

[0057] <Acrylic resin> The acrylic resin is a resin containing a structural unit derived from an acrylic monomer. The acrylic resin preferably has a carboxyl group or other acidic group. The acid value of the acrylic resin is preferably 20 to 120 mgKOH / g, more preferably 30 to 100 mgKOH / g, and particularly preferably 40 to 80 mgKOH / g. When it is within the above range, the blocking resistance is good. The glass transition temperature of the acrylic resin is preferably -40 to 10°C, more preferably -30 to 5°C, and particularly preferably -20 to 0°C. When it is within the above range, the blocking resistance and heat sealability are good.

[0058] The acrylic resin may be a commercially available product, such as JONCRYL PDX-7356, PDX-7326, or PDX-7430 manufactured by BASF, PE-1126, JE-1113, or KE1148 manufactured by Seiko PMC Corporation, or AC-3100 manufactured by Japan Coating Resins Co., Ltd.

[0059] The content of the resin in the heat seal layer is preferably 80 to 99.5% by mass, and more preferably 85 to 99% by mass, based on 100% by mass of the heat seal layer. When it is in the above range, the heat sealability is good.

[0060] <Additives other than hydrocarbon wax> The heat seal layer may further contain optional additives such as an antifoaming agent, an emulsifier, a preservative, a plasticizer, a film-forming aid, and a chelating crosslinking agent, and preferably contains an antifoaming agent.

[0061] Defoaming Agent In the present application, it is preferable to contain an antifoaming agent, and when an antifoaming agent is contained, the smoothness of the heat seal layer is improved, thereby improving the heat sealability. Examples of the antifoaming agent include a silicon-based antifoaming agent and a non-silicon-based antifoaming agent, and the content of the antifoaming agent in the heat seal layer is preferably 0.01 to 1 mass%, more preferably 0.05 to 0.5 mass%, and particularly preferably 0.1 to 0.3 mass%, based on 100 mass% of the heat seal layer.

[0062] The defoaming agent may be a commercially available product, for example, BYK-024, BYK-025, BYK-028, etc. manufactured by BYK.

[0063] <Heat sealant> The heat seal layer is preferably formed by a heat seal agent. The heat seal agent is preferably an aqueous heat seal agent. The heat seal agent contains a hydrocarbon wax having a hardness (penetration) of 12 or less at 25°C as specified by JISK2207 and an aqueous medium, and the resin contained in the heat seal agent is preferably an ethylene-vinyl acetate copolymer resin and / or an acrylic resin. In addition, the heat seal agent may contain a resin other than the ethylene-vinyl acetate copolymer resin and the acrylic resin, and / or an additive other than the hydrocarbon wax. From the viewpoint of printability and the like, the viscosity of the heat seal agent is preferably 20 to 200 mPa·s. The embodiment of the aqueous medium can be referred to (aqueous medium) described in [Surface protective layer].

[0064] <Method of manufacturing heat sealant> The method for producing the heat seal agent can be the same as the method for producing the overcoat agent described in the section [Surface protective layer].

[0065] <Formation of heat seal layer> The heat seal layer in the present invention can be formed, for example, by printing on a paper substrate or on a barrier layer described later using a heat seal agent containing a hydrocarbon wax having a hardness (penetration) at 25°C specified by JISK2207 of 12 or less, and then removing the aqueous medium. The printing method can be appropriately selected from known printing methods such as gravure printing and flexographic printing, and is preferably flexographic printing. For example, the composition is diluted with a diluting solvent to a viscosity suitable for flexographic printing, and is supplied to each printing unit alone or in a mixture and applied. Thereafter, the heat seal layer can be obtained by fixing the coating by drying in an oven or the like.

[0066] [Paper base material] The paper substrate is not particularly limited, and any known paper substrate can be used. Examples of such paper substrates include medium-quality paper, fine paper, newsprint, various coated papers, lining paper, impregnated paper, cardboard, art paper, cast paper, kraft paper, coated board, ivory paper, card paper, cup base paper, cast paper, light-shielding paper, and surface-treated paper substrates thereof. The basis weight of the paper base material is preferably 50 to 150 g / m 2 , more preferably 55 to 120 g / m 2 , and more preferably 60 to 90 g / m 2 It is.

[0067] The packaging material may further have a printing layer formed by applying a printing ink between the surface protective layer and the paper base material. In this application, the "printing ink" refers to a material containing a colorant such as a pigment. In addition, the packaging material preferably has a barrier layer between the heat seal layer and the surface protective layer.

[0068] [Print layer] The printed layer preferably contains a colorant and a styrene-acrylic copolymer resin (A'). The thickness of the printed layer is 0.1 to 10 g / m 2 is preferably 1 to 6 g / m 2 More preferably, the thickness is 1.5 to 3 g / m 2In the present invention, not only a single printed layer but also a layer in which a plurality of printed layers are overlapped is regarded as a printed layer, and printed layers having different hues can be arbitrarily combined.

[0069] (Styrene-acrylic copolymer resin (A')) The styrene-acrylic copolymer resin (A') may be a water-soluble styrene-acrylic copolymer resin (a'1) or an aqueous emulsion styrene-acrylic copolymer resin (a'2). The styrene-acrylic copolymer resin (A') may be the same as or different from the styrene-acrylic copolymer resin (A) described above in [Surface protective layer].

[0070] (Water-soluble styrene-acrylic copolymer resin (a'1)) The acid value of the styrene-acrylic copolymer resin (a'1) is preferably 150 to 350 mgKOH / g, more preferably 200 to 300 mgKOH / g. When it is within the above range, the water friction resistance is good. The weight average molecular weight of the styrene-acrylic copolymer resin (a'1) is preferably 1500 to 50000, more preferably 1500 to 30000, and even more preferably 1500 to 8000. When it is within the above range, the blocking resistance is good. The glass transition temperature of the styrene-acrylic copolymer resin (a'1) is preferably 40 to 130°C, more preferably 60 to 100°C. When it is within the above range, the blocking resistance is good.

[0071] The styrene-acrylic copolymer resin (a'1) may be a commercially available product, for example, GL-2439 or YL-1098 manufactured by Seiko PMC Corporation.

[0072] (Aqueous emulsion styrene-acrylic copolymer resin (a'2)) The acid value of the styrene-acrylic copolymer resin (a'2) is preferably 5 to 80 mgKOH / g, more preferably 20 to 60 mgKOH / g. When it is within the above range, the adhesion is good. The weight average molecular weight of the styrene-acrylic copolymer resin (a'2) is preferably 10,000 to 600,000, more preferably 50,000 to 500,000, further preferably 100,000 to 400,000, and particularly preferably 200,000 to 300,000. When it is within the above range, the water friction resistance is good. The glass transition temperature of the styrene-acrylic copolymer resin (a'2) is preferably -20 to 60°C, more preferably 0 to 40°C. When it is within the above range, the blocking resistance is good.

[0073] The styrene-acrylic copolymer resin (a'2) may be a commercially available product, for example, HE-1335, X-436, QE-1042, etc. manufactured by Seiko PMC Corporation.

[0074] The printing layer preferably contains both the styrene-acrylic copolymer resin (a'1) and the styrene-acrylic copolymer resin (a'2). The solid content ratio of a'1 to a'2 is preferably 1:99 to 75:25, more preferably 1:99 to 55:45, and even more preferably 15:85 to 35:65. With the above ratio, water friction resistance and blocking resistance are good.

[0075] <Resins other than styrene-acrylic copolymer resin (A')> The printing layer may contain a resin other than the styrene-acrylic copolymer resin (A'), such as an acrylic resin, a styrene-maleic acid copolymer resin, a urethane resin, a polylactic acid resin, a castor oil-based resin, a rosin-based resin, a vinyl acetate resin, a vinyl acetate resin, etc. Among these, it is preferable that the printing layer contains at least one resin selected from the group consisting of a styrene-maleic acid copolymer resin and an acrylic resin.

[0076] <Colorant contained in the printing layer> The printed layer contains a colorant. The content of the colorant is preferably 1 to 60% by mass, and more preferably 30 to 50% by mass, based on the total mass of the printed layer. The colorant is preferably a pigment, and either an organic pigment or an inorganic pigment can be used.

[0077] Specific examples of organic pigments are shown by their Colour Index International (CI) numbers. Preferably, CI Pigment Red 57:1, CI Pigment Red 48:1, CI Pigment Red 48:2, CI Pigment Red 48:3, CI Pigment Red 146, CI Pigment Red 242, CI Pigment Yellow 83, CI Pigment Yellow 14, CI Pigment Orange 64, CI Pigment Orange 38, CI Pigment Orange 34, CI Pigment Orange 13, CI Pigment Yellow 180, CI Pigment Yellow 139, CI Pigment Red 185, CI Pigment Red 122, CI Pigment Red 178, CI Pigment Red 149, CI Pigment Red 144, CI Pigment Red 166, CI Pigment Violet 23, CI Pigment Violet 37, CI Pigment Blue 15, CI Pigment Blue 15:1, CI Pigment Blue 15:2, CI Pigment Blue 15:3, CI Pigment Blue 15:4, CI Pigment Blue 15:6, CI Pigment Green 7, and CI Pigment Black 7. These may be used alone or in combination of two or more.

[0078] (Inorganic pigments) Examples of inorganic pigments include titanium oxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, chromium oxide, aluminum hydroxide, silica, kaolin, clay, talc, aluminum particles, mica, bronze powder, chrome vermilion, yellow lead, cadmium yellow, cadmium red, ultramarine, Prussian blue, red iron oxide, yellow iron oxide, iron black, titanium oxide, and zinc oxide. Aluminum can be either leafing or non-leafing type, with the non-leafing type being preferred.

[0079] <Additives contained in the printing layer> The printing layer of the present invention may contain various additives as necessary, such as dispersants, waxes, extender pigments, leveling agents, antifoaming agents, and film-forming assistants. Specifically, various additives can be added, such as a dispersion of wax resin microparticles such as polyethylene wax to improve water friction resistance, inorganic microparticles and adhesive resins to impart anti-slip properties, vinyl acetate resins, leveling agents to improve leveling properties, antifoaming agents to impart antifoaming properties, basic compounds such as sodium hydroxide and potassium hydroxide to impart re-solubility, and film-forming assistants such as glycol compounds.

[0080] <Printing ink> The printing ink contains the above-mentioned colorant, the above-mentioned styrene-acrylic copolymer resin (A'), and an aqueous medium. It may further contain a resin other than the above-mentioned styrene-acrylic copolymer resin (A') and / or an additive contained in the printing layer. The embodiment of the aqueous medium can be referred to as the aqueous medium described in [Surface protective layer].

[0081] <Printing ink manufacturing method> The printing ink used to form the printing layer can be produced, for example, by dispersing a pigment in an organic solvent with a resin or the like using a disperser, and then mixing the resulting pigment dispersion with a resin, various additives, an organic solvent, and the like. As the disperser, a commonly used one, for example, a roller mill, a ball mill, a pebble mill, an attritor, or a sand mill, can be used. The particle size distribution of the pigment in the pigment dispersion can be adjusted by appropriately adjusting the size of the grinding media of the disperser, the filling rate of the grinding media, the dispersion processing time, the discharge speed of the pigment dispersion, the viscosity of the pigment dispersion, and the like. The viscosity of the printing ink at 25°C is preferably in the range of 50 mPa·s or more from the viewpoint of preventing the pigment from settling and dispersing appropriately, and 300 mPa·s or less from the viewpoint of workability and efficiency during ink production and printing.

[0082] <Formation of printing layer> The printing layer can be formed, for example, by printing on the paper substrate surface opposite to the heat seal layer using a printing ink, and then removing the volatile components. As the printing method, known methods such as flexographic printing and gravure printing can be used, and flexographic printing is preferred. For example, the material is diluted with a diluting solvent to a viscosity and concentration suitable for flexographic printing, and is supplied to each printing unit alone or in a mixture and applied. Thereafter, the coating is fixed by drying in an oven or the like to obtain a printing layer.

[0083] [Barrier layer] The packaging material of the present application preferably further has a barrier layer. The barrier layer exists to control the permeation of objects to be blocked, such as light, magnetism, and various gases, through the packaging material, and contains a barrier component. The barrier component can be formed by known methods such as vapor deposition, T-die casting, or liquid printing and drying. From the viewpoint of ease of penetration into the paper substrate, it is preferable to form the barrier layer by printing and drying a barrier coating agent. In addition, penetration of the barrier component into the paper substrate improves the cohesive force of the paper substrate, thereby improving the heat seal strength. The barrier layer can be positioned other than the outermost layer of the packaging material, and is preferably positioned between the heat seal layer and the paper substrate in order to exhibit the above-mentioned effect of improving the cohesive force of the paper substrate. Examples of the barrier component include aluminum vapor deposition film, iron, silica, alumina, extender pigment, polyvinylidene chloride resin, polyamide resin, polyvinyl alcohol resin, ethylene-vinyl alcohol copolymer resin, barrier nylon resin (MXD), etc., and polyvinyl alcohol-based resin, which is easy to penetrate into the paper substrate, is preferable. The barrier layer may have a single layer structure or a multi-layer structure, and one layer may contain two or more types of compounds.

[0084] (Polyvinyl alcohol resin) The polyvinyl alcohol-based resin used as the barrier component may be any resin having a vinyl alcohol unit, and may further contain a structural unit derived from ethylene. For example, polyvinyl alcohol resin and ethylene-vinyl alcohol copolymer resin can be mentioned, and ethylene-vinyl alcohol copolymer resin is preferable.

[0085] The content of ethylene-derived structural units in the polyvinyl alcohol resin is preferably 1 to 40 mol%, more preferably 3 to 20 mol%, and even more preferably 5 to 15 mol%. When it is in the above range, the oxygen barrier property is good. The polymerization degree of the polyvinyl alcohol resin is preferably 100 to 3000, and more preferably 500 to 2400. When it is in the above range, the solubility in water is improved, and therefore the separation property is good.

[0086] The polyvinyl alcohol resin may have a modified group, and examples of the modified group include known modified groups such as carbonyl-modified and silicon-modified groups, but are not limited to these.

[0087] The polyvinyl alcohol resin may be used which has been crosslinked with a crosslinking agent. Examples of the crosslinking agent to be used include known crosslinkers such as isocyanate-based, epoxy-based, melamine-based, oxazoline-based, and silane coupling-based crosslinkers, with oxazoline-based and silane coupling-based crosslinkers being preferred.

[0088] The degree of saponification of the polyvinyl alcohol resin is represented by the following formula 1, and is preferably 80 mol% or more, more preferably 90 mol%, and more preferably 95 mol%. When it is in the above range, the oxygen barrier property is good. <Expression 1> Saponification degree: (number of hydroxyl groups) / {(number of hydroxyl groups)+(number of acetate groups)}×100 [mol %]

[0089] As the polyvinyl alcohol-based resin, Kuraray Poval R series (polyvinyl alcohol resin, manufactured by Kuraray Co., Ltd.), Kuraray Eval L104B, F104B (ethylene-vinyl alcohol copolymer resin, manufactured by Kuraray Co., Ltd.), etc. can be used.

[0090] The barrier layer preferably contains a body pigment as a barrier component, and the body pigment is more preferably an inorganic layered filler. The inorganic layered filler here refers to an inorganic filler in which unit crystal layers are overlapped to form a layered structure, and is particularly preferably one that swells and cleaves in a solvent.

[0091] Preferred examples of the inorganic layered filler include montmorillonite, beidellite, saponite, hectorite, sauconite, vermiculite, mica, paragonite, lepidolite, margarite, clintonite, annandite, chlorite, donbasite, sudoite, cookeite, clinochlore, chamosite, nimite, tetrasilylic mica, talc, pyrophyllite, nacrite, kaolinite, halloysite, chrysotile, sodium teniolite, xanthophyllite, antigorite, dickite, hydrotalcite, and the like. Kaolin, montmorillonite, and mica are preferred, and montmorillonite is more preferred.

[0092] These inorganic layered compounds may be naturally occurring, artificially synthesized or modified, or may be treated with an organic substance such as an onium salt.

[0093] The content of the inorganic layered filler in the barrier layer is preferably 1 to 40 mass %, more preferably 10 to 35 mass %, and further preferably 20 to 30 mass %, based on 100 mass % of the barrier layer.

[0094] (Additives contained in the barrier layer) The barrier layer may contain known additives such as an isocyanate compound, a silane coupling agent, a dispersant, a stabilizer, a viscosity adjuster, a colorant, etc., within the range that does not impair the barrier properties.

[0095] <Barrier coating agent> The barrier coating agent contains the above-mentioned barrier component and aqueous medium, and may contain the additives contained in the barrier layer. From the viewpoint of printability, etc., the viscosity of the barrier coating agent is preferably 20 to 200 mPa·s. The content of the solid content of the barrier agent in the barrier coating agent is preferably 5 to 50 mass% and more preferably 10 to 30 mass% of the total mass of the barrier coating agent.

[0096] <Method of manufacturing the barrier coating agent> The method for producing the barrier coating agent can be the same as the method for producing the overcoat agent described in the section [Surface protective layer].

[0097] <Barrier layer formation> The barrier layer can be formed, for example, by printing a barrier coating agent on a substrate and then removing the aqueous medium. Printing methods include conventionally known methods such as gravure printing, flexographic printing, dipping, roll coating, screen printing, and spraying, but the flexographic printing method is preferred. For example, the agent is diluted with a diluting solvent to a viscosity suitable for flexographic printing, and is supplied to each printing unit alone or in a mixture and applied. Thereafter, the aqueous medium is evaporated by drying in an oven or the like to obtain a printed layer.

[0098] <Amount of paper base material in packaging material> From the viewpoint of recyclability, the content of the paper base material in the total amount of the packaging material is preferably 50 to 99 mass %, more preferably 65 to 95 mass %, and even more preferably 80 to 90 mass %.

[0099] <Packaging bag> In the present application, the packaging material is cut to a predetermined size, and the edges are heat-sealed in a state where the heat-seal layers are joined together to form a packaging bag. The heat-sealing temperature is preferably 50 to 250°C, and more preferably 80 to 180°C. The heat-sealing pressure is 1 to 5 kg / cm. 2 The conditions are as follows. A packaging bag can be formed by folding one sheet of packaging material and heat sealing the edges, or by heat sealing two or more sheets of packaging material together. A packaging bag can also be formed by packaging the contents and then heat sealing all openings. This packaging bag can be widely used as a packaging bag for food, medicine, etc. EXAMPLES

[0100] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In this application, parts and % represent parts by mass and % by mass unless otherwise noted. In addition, "NV." represents the mass % of non-volatile content.

[0101] <Synthesis Example 1> Synthesis of urethane resin solution PU1 In a reactor equipped with a thermometer, a stirrer, a reflux condenser and a nitrogen gas inlet tube, 173.7 parts of poly(3-methyl-1,5-pentane adipate)diol (number average molecular weight 2000), 9.1 parts of polyethylene glycol (number average molecular weight 2000), 21.5 parts of 2,2-dimethylolpropionic acid and 84 parts of isophorone diisocyanate were charged with 200 parts of methyl ethyl ketone while introducing nitrogen gas, and the mixture was heated and refluxed for 6 hours while stirring. After cooling to 40°C, 100 parts of acetone were added to obtain a solution of terminal isocyanate prepolymer. Next, the obtained terminal isocyanate prepolymer solution was gradually added at room temperature to a mixture of 8.7 parts of 2-hydroxyethylethylenediamine, 2.9 parts of isophoronediamine and 400 parts of acetone, and reacted at 50°C for 3 hours to obtain a solvent-based urethane resin solution. Next, 9.8 parts of 28% aqueous ammonia and 700 parts of deionized water were gradually added to the above solvent-based urethane resin solution to neutralize and make it water-soluble. Further, all of the methyl ethyl ketone and acetone were distilled off under azeotropic conditions, and then water was added to adjust the viscosity, obtaining urethane resin PU1 with an acid value of 30 mgKOH / g, a solids content of 40% and a weight average molecular weight of 30,000.

[0102] <Production Example 1> Production of overcoat agent X1 11.5 parts of water, 85 parts of styrene-acrylic copolymer resin SAC1 (emulsion type, acid value 71 mgKOH / g, glass transition temperature: 40°C, NV.40%), 2 parts of butyl cellosolve, and 1.5 parts of polyethylene wax were added and mixed with stirring to obtain overcoat agent X1.

[0103] <Production Examples 2 to 13, Comparative Production Examples 1 and 2> Production of Overcoat Agents X2 to 15 Overcoat agents X2 to 15 were obtained in the same manner as in Production Example 1, except that the raw materials and compounding ratios shown in Table 1 were used. The properties of the raw materials used are as follows. Styrene-acrylic copolymer resin SAC2 (aqueous emulsion, acid value: 100mgKOH / g, glass transition temperature: 16℃, NV.40%) Styrene-acrylic copolymer resin SAC3 (water-based emulsion, acid value: 110 mg KOH / g, glass transition temperature: 85°C, NV.40%) Styrene-acrylic copolymer resin SAC4 (water-based emulsion, acid value: 104 mg KOH / g, glass transition temperature: 113°C, NV.40%) Styrene-acrylic copolymer resin SAC5 (water-based emulsion, acid value: 88 mg KOH / g, glass transition temperature: 10°C, NV.40%)

[0104] [Table 1]

[0105] <Production Example 14> Production of heat sealant HS1 85 parts of ethylene-vinyl acetate copolymer resin emulsion EVA1 (Aquatex MC-3800, manufactured by Japan Coating Resins, minimum film-forming temperature: 100°C, NV. = 40%), 11.9 parts of a water / isopropyl alcohol mixed solvent (mass ratio 1:1), 3.0 parts of Chemipearl W400 (polyethylene wax, manufactured by Mitsui Chemicals, penetration: 3, density: 920 kg / m3, particle size: 4 μm), and 0.1 parts of BYK-024 (antifoaming agent, manufactured by BYK) were added and mixed with stirring to obtain a heat sealing agent HS1.

[0106] <Production Examples 15 to 20, Comparative Production Examples 3 and 4> Preparation of heat sealing agents HS2 to HS9 Heat sealing agents HS2 to HS9 were obtained in the same manner as in Production Example 14, except that the raw materials and compounding ratios shown in Table 2 were used. The properties of the raw materials used are as follows. Ethylene-acrylic copolymer resin emulsion AC1 (glass transition temperature: -30℃, NV.40%) Chemipearl W100 (Mitsui Chemicals, polyethylene wax, penetration: 1, density: 970 kg / m 3 , particle size: 3μm) Chemipearl W500 (Mitsui Chemicals, polyethylene wax, penetration: 10, density: 920 kg / m 3 , particle size: 2.5μm) Paraffin Wax-130 (Nihon Seimitsu Wax Co., Ltd., paraffin wax, penetration: 13, melting point 56°C, NV 100%)

[0107] [Table 2]

[0108] <Production Example 22> Production of printing ink W1 A mixture of 31.6 parts of water, 18 parts of Pigment Black 7, 5 parts of a urea compound, and 15 parts of a styrene-acrylic copolymer resin solution SAC6 (water-soluble, acid value: 213 mg KOH / g, weight average molecular weight: 8000, glass transition temperature: 73°C, solid content: 28%) was kneaded and dispersed in a bead mill, and then 27 parts of a styrene-acrylic copolymer resin SAC7 (aqueous emulsion, acid value: 36 mg KOH / g, glass transition temperature: 14°C, solid content: 40%) and 3 parts of polyethylene wax were added, stirred and mixed to obtain printing ink W1.

[0109] <Preparation Example 23> Barrier Coat Agent V1 6 parts of polyvinyl alcohol resin PVA1 (ethylene content: 8 mol%) and 92 parts of mixed solvent (water / IPA=8 / 2) were heated with stirring, and the heating and stirring were continued at 95°C for 1 hour, after which the heating was stopped and the stirring was continued until the temperature returned to normal, to obtain an aqueous solution of polyvinyl alcohol resin PVA1. 2 parts of montmorillonite (swelling property, particle aspect ratio: 500, particle thickness: 1 μm, particle spread: 500 nm) were added to the aqueous solution of polyvinyl alcohol resin PVA1, and the mixture was mixed and stirred to obtain a barrier coating agent V1.

[0110] <Preparation Example 24> Barrier Coat Agent V2 Acrylic resin emulsion AC1 (acid value: 108 mg KOH / g, glass transition temperature: 56°C, NV. = 50%, solvent: water) 3 parts, mixed solvent (water / IPA = 8 / 2) 95 parts, montmorillonite (swelling, particle aspect ratio: 500, particle thickness: 1 μm, particle spread: 500 nm) 2 parts were added and mixed and stirred to obtain barrier coating agent V2.

[0111] The following examples show methods for producing packaging materials.

[0112] <Measuring the coating amount of each layer> Five 10 cm square pieces were cut out from the paper substrate / printed layer component of the obtained intermediate laminate, and five 10 cm square pieces were cut out from the paper substrate. The weight of each sample was measured, and the coating weight of the printed layer was calculated using Equation 2. The paper substrate was kraft paper (Nippon Paper Industries Co., Ltd., unglazed kraft K, basis weight 70 g / m 2 ) was used. <Expression 2> Coating weight of printed layer (mg) = (average weight of 5 samples of paper substrate / printed layer) - (average weight of 5 samples of paper substrate)

[0113] For layers other than the printed layer, the coating weight was calculated in the same manner as in "Measurement of Coating Weight of Printed Layer" except that the calculation formula and the location from which the sample was cut out were different. <Expression 3> Coating weight of surface protective layer (mg) = (average weight of five samples of paper substrate / printed layer / surface protective layer) - (average weight of five samples of paper substrate / printed layer) <Expression 4> Coating weight of barrier layer (mg) = (average weight of five samples of barrier layer / paper base material / printed layer / surface protective layer) - (average weight of five samples of paper base material / printed layer / surface protective layer) <Formula 5> Coating weight of heat seal layer (mg) = (average weight of five samples of heat seal layer / barrier layer / paper base material / printing layer / surface protective layer) - (average weight of five samples of barrier layer / paper base material / printing layer / surface protective layer)

[0114] <Glycol compound content in surface protective layer> Ten pieces measuring 50 mm x 10 mm were cut out from the paper base material / printing layer / surface protection layer component of the obtained intermediate laminate, placed in a headspace vial (Agilent, 75.5 mm x 23 mm), and heated at 150°C for 30 minutes in a sealed state. A certain amount of solvent vapor was then removed using a microsyringe, and the amount of glycol-based compounds was quantified by gas chromatography.

[0115] <Example 1> Production of packaging material P1 Kraft paper (Nippon Paper Industries, double-glazed Kraft K, basis weight 70 g / m 2 A flexographic printing machine equipped with a 150-line flexographic plate was used to print the printing ink W1 on the paper substrate (original width: 100 cm, original length: 500 m) at a printing speed of 200 m / min and an in-line oven temperature of 90°C to form a printed layer on the entire surface of the paper substrate, and then an overcoat agent X1 was printed on the printed layer at a printing speed of 200 m / min and an in-line oven temperature of 90°C using a flexographic printing machine equipped with a 150-line flexographic plate having a non-image area on one half of the plate to form a surface protective layer, thereby obtaining an intermediate laminate p1 (length: 500 m) having a paper substrate / printed layer / surface protective layer configuration. The intermediate laminate p1 has a paper substrate / printed layer component and a paper substrate / printed layer / surface protective layer component, and a sample for measuring the coating amount was obtained. Next, the barrier coating agent V1 was printed three times on the surface of the intermediate laminate p1 on which the printed layer was not present, using a flexographic printing machine equipped with a 150-line flexographic plate under conditions of a printing speed of 200 m / min and an in-line oven temperature of 90°C, to form a barrier layer on the entire surface of the paper substrate, and then the heat seal agent HS1 was printed twice on the entire surface of the barrier layer, using a flexographic printing machine equipped with a 150-line flexographic plate under conditions of a printing speed of 200 m / min and an in-line oven temperature of 90°C, to form a heat seal layer on the entire surface of the barrier layer, thereby obtaining a packaging material P1 having a configuration of heat seal layer / barrier layer / paper / printing / surface protection layer. Note that the last 100 m of the entire length 500 m of the intermediate laminate p1 was not printed with the heat seal agent, so that there were components of the barrier layer / paper / printing / surface protection layer and components of the heat seal layer / barrier layer / paper / printing / surface protection layer, and a sample for measuring the coating amount was obtained. The coating weight of the printed layer of the packaging material P1 is 2 g / m 2 The coating weight of the surface protection layer is 2g / m 2 , the coating weight of the barrier layer is 4g / m 2 The coating weight of the heat seal layer is also 4g / m 2 The residual amount of glycol compounds was 54.6 g / m 2 The content of the glycol compound in the surface protective layer was 2.7% by mass relative to 100% by mass of the surface protective layer.

[0116] <Examples 2 to 26 and Comparative Examples 1 to 6> Production of packaging materials P2 to 32 Packaging materials P2 to P32 having the same configuration as in Example 1 were produced in the same manner as in Example 1, except that the overcoat agent, barrier coat agent, and heat seal agent shown in Tables 3 and 4 were used.

[0117] [Table 3]

[0118] [Table 4]

[0119] [Evaluation of packaging materials] The resulting packaging materials P1 to P32 were evaluated as described below. The results are shown in Tables 3 and 4.

[0120] <Evaluation of blocking resistance> The obtained packaging material was cut into two pieces of 40 mm square, and the heat seal layer surface of one packaging material piece was completely overlapped with the surface protection layer surface of the other packaging material piece, and the two pieces were pressed at a temperature of 40°C and a load of 100 kg / cm using a small heat press machine H30-10D manufactured by AS ONE Corporation. 2 After leaving it in that state for 12 hours, the two overlapping packaging materials were peeled off, and the peeling state of the printed layer was visually observed and evaluated according to the following criteria. A, B, and C are ranges that are acceptable for practical use. Evaluation Criteria A. The amount of the printed layer transferred to the heat seal layer surface is less than 1% by area. B. The amount of the printed layer transferred to the heat seal layer surface is 1 area % or more and less than 10 area %. C. The amount of the printed layer transferred to the heat seal layer surface is 10% by area or more and less than 30% by area. D. The amount of the printed layer transferred to the heat seal layer surface is 30% or more by area.

[0121] <Water friction resistance> The obtained packaging material was cut into a size of 25 mm x 150 mm, and the water friction resistance was evaluated according to the following criteria using a Gakushin-type friction fastness tester manufactured by Tester Sangyo Co., Ltd. Note that A, B, and C are ranges that are acceptable for practical use. Test conditions: Load: 200g, number of reciprocations: 2, paper: 5 drops of water on Kanakin cloth Evaluation Criteria A. The exposed surface area of ​​the paper base material is less than 1%. B. The exposed area ratio of the paper base material is 1% or more and less than 5%. C. The exposed area ratio of the paper base material is 5% or more and less than 10%. D. The exposed surface area of ​​the paper base material is 10% or more.

[0122] <Heat sealability evaluation> The obtained packaging material was cut into a size of 15 mm x 100 mm, folded so that the heat-sealed layers overlapped each other, and heat-sealed using the following equipment and conditions. Both unsealed ends were fixed to a small tensile tester to evaluate the heat-seal strength. A, B, and C are ranges that are acceptable for practical use. <Heat sealing conditions> Equipment: Heat seal tester manufactured by Tester Sangyo Co., Ltd., Seal width: from the folded part 10mm, heater temperature: 160℃, sealing pressure: 2kg / cm 2 , Sealing time: 1sec <Heat seal strength measurement conditions> Equipment: Intesco small tensile testing machine (model: IM-20), test piece width: 15 mm, Peeling mode: 90° peeling, tensile speed: 300mm / min Evaluation Criteria A. The heat seal strength is 5.0N or more. B. The heat seal strength is greater than or equal to 3.5N and less than 5.0N. C. The heat seal strength is 1.0N or more and less than 3.5N. D. The heat seal strength is less than 1.0 N.

[0123] <Oxygen barrier property evaluation> The obtained packaging material was subjected to oxygen transmission rate measurement according to a method in accordance with JIS K 7126-2:2006 and evaluated according to the following criteria, where A, B, and C are ranges that are acceptable for practical use. Evaluation Criteria A. Oxygen permeability is 100g / m 2 Less than 24 hours. B. Oxygen permeability is 100g / m 2 ·More than 24 hours, 1000g / m 2 Less than 24 hours. C. Oxygen permeability is 1000g / m 2 ·More than 24 hours, 10000g / m 2 Less than 24 hours. D. Oxygen permeability is 10,000g / m 2 -24 hours or more.

[0124] From the above results, Comparative Example 1 had poor blocking resistance, water friction resistance, and oxygen barrier property because the styrene-acrylic copolymer resin in the surface protective layer did not satisfy the glass transition temperature and did not have a barrier layer. Comparative Example 2 also had poor blocking resistance and water friction resistance because the styrene-acrylic copolymer resin in the surface protective layer did not satisfy the glass transition temperature. Comparative Example 3 had poor blocking resistance and water friction resistance because the surface protective layer did not contain a styrene-acrylic copolymer resin. Comparative Example 4 had poor blocking resistance and heat sealability because it did not have a heat seal layer. Comparative Example 5 had poor blocking resistance because the heat seal layer did not contain a hydrocarbon-based wax. Comparative Example 6 had poor blocking resistance because the hydrocarbon-based wax contained in the heat seal layer did not satisfy the hardness (penetration) at 25°C specified by JISK2207. On the other hand, in the examples, the surface protective layer contained a styrene-acrylic copolymer resin, which satisfied the glass transition temperature of the styrene-acrylic copolymer resin, and the heat seal layer contained a hydrocarbon-based wax, which satisfied the hardness (penetration) at 25°C specified in JIS K2207, and therefore the examples had good blocking resistance, water friction resistance, heat sealability, and oxygen barrier properties. In particular, the Tg of the styrene-acrylic copolymer resin contained in the surface protective layer is 20 to 50°C, the glycol compound is at least one selected from the group consisting of butyl cellosolve, propylene glycol, and ethylene glycol, and the coating amount of the surface protective layer is 1.5 to 2.5 g / m 2 the content of the glycol compound in the surface protective layer is 1.5 to 3.5% by mass relative to 100% by mass of the surface protective layer; the heat seal layer contains an ethylene-vinyl acetate copolymer resin and a polyethylene wax, the hardness (penetration) of the polyethylene wax at 25°C as specified in JIS K2207 is 2.5 to 3.5; and the coating amount is 3 to 8 g / m 2Examples 1, 6, and 7 in which the barrier layer contained a polyvinyl alcohol-based resin and was located between the heat seal layer and the paper base material had excellent blocking resistance, water friction resistance, heat sealability, and oxygen barrier property.

Claims

1. A packaging material having a heat seal layer, a paper base material, and a surface protective layer in this order, The heat seal layer comprises a hydrocarbon wax, The hardness (penetration) of the hydrocarbon wax at 25° C. as defined in JIS K2207 is 12 or less, the surface protective layer comprises a styrene-acrylic copolymer resin (A) having a glass transition temperature of 12° C. or higher, The packaging material, wherein the content of the styrene-acrylic copolymer resin (A) in the surface protective layer is 50% by mass or more based on 100% by mass of the surface protective layer.

2. The packaging material according to claim 1 , wherein the heat seal layer comprises an ethylene-vinyl acetate copolymer resin and / or an acrylic resin.

3. The packaging material according to claim 1 or 2, further comprising a barrier layer.

4. The packaging material of claim 3 , wherein the barrier layer comprises a polyvinyl alcohol-based resin.

5. The packaging material according to claim 1 or 2, wherein the surface protective layer further comprises a glycol-based compound.

6. The packaging material according to claim 5 , wherein the glycol-based compound comprises at least one selected from the group consisting of butyl cellosolve, propylene glycol, and ethylene glycol.

7. The packaging material according to claim 5, wherein the content of the glycol-based compound in the surface protective layer is 0.01 to 15% by mass, based on 100% by mass of the surface protective layer.

8. A packaging bag formed from the packaging material according to claim 1 or 2.

9. A method for producing a packaging material having a heat seal layer, a paper base material, and a surface protective layer in this order, comprising: A step of printing a heat seal agent containing a hydrocarbon-based wax on one side of a paper substrate to form a heat seal layer; a step of printing an overcoat agent containing a styrene-acrylic copolymer resin (A) having a glass transition temperature of 12° C. or higher on the other side of the paper substrate to form a surface protective layer in which the content of the styrene-acrylic copolymer resin (A) is 50% by mass or more relative to 100% by mass of the surface protective layer; Including, The method for producing a packaging material, wherein the hydrocarbon wax has a hardness (penetration) at 25°C as specified in JIS K2207 of 12 or less.

Citation Information

Patent Citations

  • Laminate and packaging product containing the same

    JP2018051796A

  • Food packaging paper and food packaging method using the same

    JP2021038022A

  • Barrier paper

    JP2022156000A

  • Paper laminate and method for producing the same

    JP2022169426A

  • Aqueous overcoat agent, laminate for packaging material, and packaging material

    JP2023005160A