Electrochromic sheet and electrochromic device
The electrochromic sheet addresses the issue of light resistance by using a low-transmittance support layer with ultraviolet absorbers and protective resins, enhancing durability against harmful light rays.
Patent Information
- Application Number
- JP2023183711
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-10-26
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2042-11-04
AI Technical Summary
Conventional electrochromic elements and optical lenses lack sufficient light resistance, particularly against harmful blue light and ultraviolet rays, which can harm human eye health.
The electrochromic sheet is designed with a support layer having a light transmittance of 10% or less at a wavelength of 380 nm, incorporating ultraviolet absorbers and specific transparent resins like polycarbonate, and a sealing part to protect the layers from external factors.
The design significantly improves the light resistance of the electrochromic sheet, effectively reducing ultraviolet rays and enhancing the durability of the electrochromic elements.
Smart Images

Figure 0007568032000005 
Figure 0007568032000006 
Figure 0007568032000007
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrochromic sheet and an electrochromic device. [Background technology]
[0002] Electrochromic elements are known as elements that utilize electrochromism, a phenomenon in which a reversible redox reaction occurs when a voltage is applied, causing a reversible change in transmittance. For example, a color can be produced by applying a positive voltage to an electrochromic element, and the color can be removed by applying a negative voltage to make the element transparent. Therefore, by providing a switch that can switch between applying a positive voltage and a negative voltage, the electrochromic element can be made to color and remove color at any time.
[0003] Such electrochromic elements can be broadly divided into two types of layer configurations. One is a layer configuration in which an electrochromic material and an electrolyte material are mixed, and the other is a multi-layer configuration in which an electrochromic material and an electrolyte material are formed as separate layers. In the latter multi-layer electrochromic element, the electrochromic material is fixed in a layered form, so the charge injected into the electrochromic material undergoes a reverse reaction through an external circuit. This has the advantage that once a color is generated, the colored state can be maintained until the decoloring drive is performed, reducing power consumption.
[0004] For example, there is a device described in Patent Document 1. Patent Document 1 discloses that the device includes an electrode layer arranged on a substrate for applying a voltage current, an electrochromic element containing an electrochromic material, and a sealing seal that covers the periphery of the electrochromic element. Patent Document 1 also discloses that the electrode layer and the substrate are "transparent" and can transmit light.
[0005] In the field of optical lenses, light rays with wavelengths of 420 to 450 nm, known as blue light, are known to be harmful to human eye health, and therefore the development of optical lenses capable of blocking light rays with wavelengths of 420 to 450 nm has been attracting attention (Patent Document 2). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2020-106786 A [Patent Document 2] International Publication No. 2017 / 077359 Summary of the Invention [Problem to be solved by the invention]
[0007] The present inventor has newly focused on the light resistance of electrochromic sheets when they are used outdoors. However, the electrochromic element described in Patent Document 1 focuses on transmitting light, and is insufficient in terms of light resistance. In addition, as disclosed in Patent Document 2, the conventional optical lens focuses on cutting blue light, and is insufficient in terms of light resistance. [Means for solving the problem]
[0008] The present inventors have conducted research into improving the light resistance of electrochromic sheets, and have found that it is effective to set the light transmittance of the support layer at a wavelength of 380 nm to 10% or less, thereby completing the present invention. This effectively reduces ultraviolet rays with wavelengths shorter than blue light, and improves the light resistance of the electrochromic sheet.
[0009] According to the present invention, the following electrochromic sheet and related techniques are provided.
[0010] [1] A support layer; an electrolyte layer provided on the support layer; an electrochromic layer provided on at least one surface of the electrolyte layer; a sealing portion provided so as to cover at least a side surface of the electrolyte layer; An electrochromic sheet comprising: The support layer is an electrochromic sheet having a light transmittance of 10% or less at a wavelength of 380 nm. [2] The electrochromic sheet according to [1], The support layer has a light transmittance of 80% or more at a wavelength of 430 nm. [3] The electrochromic sheet according to [1] or [2], The electrochromic sheet, wherein the support layer contains an ultraviolet absorbing agent. [4] [1] to [3] An electrochromic sheet according to any one of the above, The support layer is an electrochromic sheet containing one or more resins selected from episulfide-based resins, thiourethane-based resins, acrylic-based resins, polycarbonate-based resins, urethane-based resins, polyamide-based resins, polyester-based resins, cellulose-based resins, cycloolefin polymers (COP), cycloolefin copolymers (COC), norbornene-based resins, and silicone-based resins. [5] An electrochromic sheet according to any one of [1] to [4], The sealing portion is formed using a sealing material including a thermosetting resin. [6] [5] An electrochromic sheet according to the present invention, The electrochromic sheet, wherein the thermosetting resin includes one or more resins selected from the group consisting of epoxy resins, acrylic resins, phenolic resins, maleimide resins, silicone resins, urethane resins, cyanate resins, melamine resins, urea resins, and unsaturated polyester resins. [7] An electrochromic sheet according to any one of [1] to [6], An electrochromic sheet, wherein the electrolyte layer of the electrochromic sheet is a solid or a gel. [8] An electrochromic sheet according to any one of [1] to [7], An electrochromic sheet, the electrochromic layer being provided on the upper and lower surfaces of the electrolyte layer of the electrochromic sheet. [9] An electrochromic sheet according to any one of [1] to [8], The electrochromic sheet further comprises an electrode layer between the support layer and the electrochromic layer.
[10] An electrochromic device using the electrochromic sheet described in any one of [1] to [9]. Effect of the Invention
[0011] The present invention provides an electrochromic sheet with improved light resistance. [Brief description of the drawings]
[0012] [Figure 1] 1 is a cross-sectional view showing a schematic diagram of an electrochromic sheet according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing the light transmission spectrum of the support layer in Example 1. [Diagram 3] FIG. 2 is a diagram showing the light transmission spectrum of the support layer in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In order to avoid complexity, when there are multiple identical components in the same drawing, only one of them may be marked with a symbol, and not all of them may be marked with a symbol. All drawings are for illustrative purposes only. The shape and dimensional ratio of each component in the drawings do not necessarily correspond to the actual product.
[0014] In this specification, the expression "a to b" in the description of a numerical range means a or more and b or less, unless otherwise specified. For example, "1 to 5 mass%" means "1 mass% or more and 5 mass% or less." In addition, the lower limit and upper limit of a numerical range can be arbitrarily combined with the lower limit and upper limit of another numerical range.
[0015] Unless otherwise specified, each of the components and materials exemplified in this specification may be used alone or in combination of two or more kinds.
[0016] In this embodiment, "covering" is not limited to being continuous, but may include some discontinuous portions.
[0017] <Electrochromic sheet> FIG. 1 is a schematic cross-sectional view showing an example of an embodiment of an electrochromic sheet 100. As shown in FIG. As shown in FIG. 1, the electrochromic sheet 100 comprises a laminate (hereinafter also referred to as "electrochromic element 10") in which an electrolyte layer 4, a first electrochromic layer 3, and a second electrochromic layer 5 are stacked in order, a sealing portion 8 covering the side surfaces of the electrochromic element 10, and a pair of support layers (a first support layer 1 and a second support layer 7) sandwiching the top and bottom surfaces of the electrochromic element 10 and the sealing portion 8 therebetween. In other words, the electrochromic sheet 100 comprises a first electrochromic layer 3, an electrolyte layer 4, a second electrochromic layer 5, and a second support layer 7 stacked in sequence on a first support layer 1, and the sides of the first electrochromic layer 3, the electrolyte layer 4, and the second electrochromic layer 5 are each covered by a sealing portion 8.
[0018] In this embodiment, the electrochromic sheet 100 further includes a first electrode 2 between the first support layer 1 and the first electrochromic layer 3, and a second electrode 6 between the second support layer 7 and the second electrochromic layer 5.
[0019] In this embodiment, the electrochromic sheet 100 will be described taking as an example a case in which a first electrochromic layer 3 and a second electrochromic layer 5 are laminated on both sides of an electrolyte layer 4, but only one of the electrochromic layers may be provided.
[0020] In the present embodiment, the electrochromic sheet 100 will be described taking an example in which both the first support layer 1 and the second support layer 7 have a light transmittance of 10% or less at a wavelength of 380 nm, but only one of the first support layer 1 and the second support layer 7 may have a light transmittance of 10% or less at a wavelength of 380 nm, and the other may not. In this case, for example, the sealing material may be photocured by irradiating ultraviolet light from the support layer side that does not have a light transmittance of 10% or less at a wavelength of 380 nm.
[0021] Each component will be described below.
[0022] [Support layer] The first support layer 1 and the second support layer 7 have the function of supporting the first electrode 2, the first electrochromic layer 3, the electrolyte layer 4, the second electrochromic layer 5, the second electrode 6, and the sealing portion 8. They also serve as the outermost layers of the electrochromic sheet 100.
[0023] Moreover, the first support layer 1 and the second support layer 7 constitute the outermost layers of the electrochromic sheet 100. That is, at least the first electrochromic layer 3, the electrolyte layer 4, and the second electrochromic layer 5 are not exposed to the outside. Therefore, the first electrochromic layer 3, the electrolyte layer 4, and the second electrochromic layer 5 can be protected from moisture and oxygen gas from the outside, physical impacts, friction, and the like.
[0024] In this embodiment, the first support layer 1 and the second support layer 7 have a light transmittance of 10% or less at a wavelength of 380 nm, preferably 5% or less, and more preferably 1% or less, which can effectively reduce ultraviolet rays and improve the light resistance of the electrochromic. In this embodiment, the first support layer 1 and the second support layer 7 have a maximum light transmittance of 10% or less, preferably 5% or less, and more preferably 1% or less at a wavelength of 300 to 380 nm, which can effectively reduce ultraviolet rays and improve the light resistance of the electrochromic. Moreover, the first support layer 1 and the second support layer 7 preferably have a light transmittance of 80% or more at a wavelength of 430 nm.
[0025] The first support layer 1 and the second support layer 7 are not particularly limited as long as they are composed primarily of a transparent resin material, but it is preferable that they contain a transparent resin (base resin) having thermoplastic properties as their primary material.
[0026] The transparent resin is not particularly limited, but examples thereof include one or more types selected from episulfide-based resins, thiourethane-based resins, acrylic-based resins, polycarbonate-based resins, urethane-based resins, polyamide-based resins, polyester-based resins, cellulose-based resins, cycloolefin polymers (COP), cycloolefin copolymers (COC), norbornene-based resins, and silicone-based resins.
[0027] Among these, polycarbonate-based resins or polyamide-based resins are preferred, and polycarbonate-based resins are particularly preferred. Polycarbonate-based resins are rich in transparency (light transmissivity) and mechanical strength such as rigidity, and also have high heat resistance, so that the transparency, impact resistance, and heat resistance of the first support layer 1 and the second support layer 7 can be improved by using a polycarbonate-based resin as the transparent resin.
[0028] As the polycarbonate resin, various resins can be used, among which aromatic polycarbonate resins are preferable. Aromatic polycarbonate resins have aromatic rings in their main chains, which allows the first support layer 1 and the second support layer 7 to have superior strength.
[0029] The aromatic polycarbonate resin is synthesized, for example, by an interfacial polycondensation reaction between bisphenol and phosgene, or an ester exchange reaction between bisphenol and diphenyl carbonate.
[0030] Examples of bisphenols include bisphenol A and bisphenol (modified bisphenol) which is the source of the repeating unit of polycarbonate represented by the following formula (1A).
[0031] [ka]
[0032] (In formula (1A), X is an alkyl group having 1 to 18 carbon atoms, an aromatic group, or a cyclic aliphatic group; Ra and Rb are each independently an alkyl group having 1 to 12 carbon atoms; m and n are each an integer of 0 to 4; and p is the number of repeating units.)
[0033] Specific examples of bisphenols that are the source of the repeating units of the polycarbonate represented by formula (1A) include 4,4'-(pentane-2,2-diyl)diphenol, 4,4'-(pentane-3,3-diyl)diphenol, 4,4'-(butane-2,2-diyl)diphenol, 1,1'-(cyclohexanediyl)diphenol, 2-cyclohexyl-1,4-bis(4-hydroxyphenyl)benzene, 2,3-biscyclohexyl-1,4-bis(4-hydroxyphenyl)benzene, 1,1'-bis(4-hydroxy-3-methylphenyl)cyclohexane, and 2,2'-bis(4-hydroxy-3-methylphenyl)propane, and any of these may be used alone or in combination of two or more.
[0034] Among them, the polycarbonate resin is preferably a bisphenol-type polycarbonate resin having a skeleton derived from bisphenol as the main component. By using such a bisphenol-type polycarbonate resin, the first support layer 1 and the second support layer 7 can exhibit even better strength and can easily improve light resistance when a later-described ultraviolet absorbing agent is applied.
[0035] ·UV absorber The first support layer 1 and the second support layer 7 preferably further contain an ultraviolet absorbing agent, which makes it easier to improve the light resistance of the electrochromic sheet 100. In this case, the ultraviolet absorbent may be mixed with the resin material constituting the first support layer 1 and the second support layer 7, and the resin material containing the ultraviolet absorbent may be molded to form the first support layer 1 and the second support layer 7, or the first support layer 1 and the second support layer 7 may each have a multilayer structure having a layer containing an ultraviolet absorbent. When a multilayer structure is used, for example, the first support layer 1 may be formed by coating an ultraviolet absorbent on a polycarbonate substrate to form a multilayer structure.
[0036] The ultraviolet absorber is not particularly limited, and any known compound can be used. Examples of the ultraviolet absorber include triazine-based compounds, benzophenone-based compounds, benzotriazole-based compounds, and cyanoacrylate-based compounds. One or a combination of two or more of these compounds can be used.
[0037] Examples of triazine compounds include 2-mono(hydroxyphenyl)-1,3,5-triazine compounds, 2,4-bis(hydroxyphenyl)-1,3,5-triazine compounds, and 2,4,6-tris(hydroxyphenyl)-1,3,5-triazine compounds. Specific examples of such compounds include 2,4-diphenyl-6-(2-hydroxy-4-methoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-ethoxyphenyl)-1,3,5-triazine, and 2,4-diphenyl-(2-hydroxy-4-propoxyphenyl)-1,3,5-triazine. ,3,5-triazine, 2,4-diphenyl-(2-hydroxy-4-butoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-butoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-hexyloxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-octyloxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-dodecyloxyphenyl)-1,3,5-triazine, 2,4-diphenyl phenyl-6-(2-hydroxy-4-benzyloxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-butoxyethoxy)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-dibutoxyphenyl)-1,3-5-triazine, 2,4,6-tris(2-hydroxy-4-methoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-ethoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4- propoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-butoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-hexyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-octyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-dodecyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-benzyloxyphenyl)-1,3,5-triazine, 2,4,6-Tris(2-hydroxy-4-ethoxyethoxyphenyl)-1,3,5-triazine, 2,4,6-Tris(2-hydroxy-4-butoxyethoxyphenyl)-1,3,5-triazine, 2,4,6-Tris(2-hydroxy-4-propoxyethoxyphenyl)-1,3,5-triazine, 2,4,6-Tris(2-hydroxy-4-methoxycarbonylpropyloxyphenyl)-1,3,5-triazine, 2,4,6-Tris(2-hydroxy-4-ethoxycarbonylethyloxyphenyl)-1,3,5-triazine, 2,4,6- Tris(2-hydroxy-4-(1-(2-ethoxyhexyloxy)-1-oxopropan-2-yloxy)phenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-methoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-ethoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-propoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-butoxyphenyl) -1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-hexyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-octyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-dodecyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-benzyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-ethoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-butoxyethoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-propoxyethoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-methoxycarbonylpropyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-ethoxycarbonylethyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-(1-(2-ethoxyhexyloxy)-1-oxopropan-2-yloxy)phenyl)-1,3,5-triazine and the like.
[0038] Examples of benzotriazole compounds include 2-(2-hydroxy-5-t-octylphenyl)benzotriazole, 2-(3-t-butyl-2-hydroxy-5-methylphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-t-pentyl-2-hydroxyphenyl)-2H-benzotriazole, and 2-(2H-benzotriazol-2-yl)-4-methyl-6-(3,4,5,6-tetrahydrophthalimidylmethyl). )phenol, 2-(2-hydroxy-4-octyloxyphenyl)-2H-benzotriazole, 2-(2-hydroxy-5-t-octylphenyl)-2H-benzotriazole, 2-[2'-hydroxy-3,5-di(1,1-dimethylbenzyl)phenyl]-2H-benzotriazole, 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)4-(1,1,3,3-tetramethylbutyl)phenol], and the like.
[0039] When preparing the first support layer 1 and the second support layer 7 by extrusion molding, triazine-based compounds are preferably used from the viewpoint of good heat resistance, but benzophenone-based compounds, benzotriazole-based compounds, and cyanoacrylate-based compounds can also be used without particular restrictions as long as they have sufficient heat resistance to the extrusion temperature.
[0040] Commercially available triazine-based ultraviolet absorbers include, for example, "Tinuvin 1577," "Tinuvin 460," and "Tinuvin 477" (manufactured by BASF Japan), and "Adeka STAB LA-F70" (manufactured by ADEKA). Moreover, examples of commercially available benzotriazole-based ultraviolet absorbents with high heat resistance include "ADEKA STAB LA-31G" (manufactured by ADEKA).
[0041] The content of the ultraviolet absorbent is preferably 0.05 to 8 mass %, more preferably 0.06 to 7 mass %, and even more preferably 0.07 to 6 mass %, based on the total amount of the first support layer 1. This allows the above-mentioned effects to be exhibited more reliably. By setting the content of the ultraviolet absorbent to be equal to or more than the above-mentioned lower limit, the ultraviolet absorbing effect can be sufficiently obtained. On the other hand, by setting the content of the ultraviolet absorbent to be equal to or less than the above-mentioned upper limit, aggregation of the ultraviolet absorbent can be suppressed. The content of the ultraviolet absorber is preferably 0.05 to 8 mass %, more preferably 0.06 to 7 mass %, and even more preferably 0.07 to 6 mass %, based on the total amount of the second support layer 7. This allows the above-mentioned effects to be exhibited more reliably. By setting the content of the ultraviolet absorber to be equal to or more than the above-mentioned lower limit, the ultraviolet absorbing effect can be sufficiently obtained. On the other hand, by setting the content of the ultraviolet absorber to be equal to or less than the above-mentioned upper limit, aggregation of the ultraviolet absorber can be suppressed.
[0042] Coloring agents As long as the first support layer 1 and the second support layer 7 are optically transparent, they may further contain a colorant, and the color may be any color, such as colorless, red, blue, yellow, etc.
[0043] These color choices are made possible by incorporating colorants such as dyes or pigments in the first support layer 1 and the second support layer 7 . Examples of the dye include acid dyes, direct dyes, reactive dyes, and basic dyes, and one or more selected from these may be used in combination.
[0044] Specific examples of dyes include CI Acid Yellow 17, 23, 42, 44, 79, 142, CI Acid Red 52, 80, 82, 249, 254, 289, CI Acid Blue 9, 45, 249, CI Acid Black 1, 2, 24, 94, CI Food Black 1, 2, CI Direct Yellow 1, 12, 24, 33, 50, 55, 58, 86, 132, 142, 14 4,173, CI Direct Red 1, 4, 9, 80, 81, 225, 227, CI Direct Blue 1, 2, 15, 71, 86, 87, 98, 165, 199, 202, CI Direct Black 19, 38, 51, 71, 154, 168, 171, 195, CI Reactive Red 14, 32, 55, 79, 249, CI Reactive Black 3, 4, 35, etc.
[0045] The first support layer 1 and the second support layer 7 may contain, in addition to the transparent resin, dye or pigment described above, various additives such as antioxidants, fillers, plasticizers, light stabilizers, ultraviolet absorbers, heat absorbers, and flame retardants, as necessary.
[0046] Moreover, the first support layer 1 and the second support layer 7 may be either stretched or unstretched.
[0047] Furthermore, the refractive index at a wavelength of 589 nm of the first support layer 1 and the second support layer 7 is preferably 1.3 to 1.8, more preferably 1.4 to 1.65. By setting the refractive index n1 of the first support layer 1 and the second support layer 7 within the above numerical range, the color developing and decoloring function of the electrochromic sheet 100 can be easily visually recognized.
[0048] The average thickness of the first support layer 1 and the second support layer 7 is preferably set to be 0.1 mm or more and 10.0 mm or less, and more preferably 0.3 mm or more and 5.0 mm or less. By setting the average thickness of the first support layer 1 and the second support layer 7 within this range, it is possible to accurately suppress or prevent the electrochromic sheet 100 from warping while making the electrochromic sheet 100 thinner.
[0049] The first support layer and the second support layer 7 may be made of the same or different constituent materials, and both may be stretched or only one may be unstretched.
[0050] The first support layer and the second support layer 7 may have the same refractive index or different refractive indices. The first support layer and the second support layer 7 may have the same thickness or different thicknesses.
[0051] [Sealing part] The sealing portion 8 integrally covers the side surface of the electrolyte layer 4 and the side surfaces of the first electrochromic layer 3 and the second electrochromic layer 5, and is used to prevent moisture and oxygen gas from entering the electrochromic element 10 from the outside, and to adhere to the first support layer 1 and the second support layer 7 to prevent peeling from the electrochromic element 10. In addition, if the first electrochromic layer 3 and the second electrochromic layer 5 formed between the opposing first electrode 2 and second electrode 6 are misaligned, the color development quality during operation will decrease, so the sealing portion 8 is used to prevent this.
[0052] The average thickness (length in the stacking direction) of the sealing portion 8 is adjusted according to the average thickness of the electrochromic element 10, and is set, for example, preferably to about 20 μm or more and 100 μm or less, and more preferably to about 30 μm or more and 80 μm or less.
[0053] (Sealing material) The sealing material of the present embodiment is not particularly limited as long as it is an insulating material, but preferably contains a thermosetting resin. This allows the sealing material to be cured by heat treatment, and an electrochromic sheet with improved light resistance can be obtained. In addition, in this embodiment, since both the first support layer 1 and the second support layer 7 have a light transmittance of 10% or less at a wavelength of 380 nm, the sealing material may not be photocured well even if ultraviolet light is irradiated through the first support layer 1 and the second support layer 7, but by containing a thermosetting resin, the sealing material can be thermally cured well through the first support layer 1 and the second support layer 7.
[0054] Examples of the thermosetting resin include one or more resins selected from epoxy resins, acrylic resins, phenolic resins, maleimide resins, silicone resins, urethane resins, cyanate resins, melamine resins, urea resins, and unsaturated polyester resins.
[0055] Examples of the epoxy resin include novolac type epoxy resins such as phenol novolac type epoxy resins and cresol novolac type epoxy resins, bisphenol type epoxy resins such as bisphenol A type epoxy resins and bisphenol F type epoxy resins, aromatic glycidylamine type epoxy resins such as N,N-diglycidylaniline, N,N-diglycidyltoluidine, diaminodiphenylmethane type glycidylamine, and aminophenol type glycidylamine, hydroquinone type epoxy resins, biphenyl type epoxy resins, stilbene type epoxy resins, triphenolmethane type epoxy resins, triphenolpropane type epoxy resins, and alkyl glycidylamines. Examples of the epoxy resin include one or more selected from epoxy resins such as modified triphenolmethane type epoxy resins, triazine nucleus-containing epoxy resins, dicyclopentadiene modified phenol type epoxy resins, naphthol type epoxy resins, naphthalene type epoxy resins, aralkyl type epoxy resins such as phenol aralkyl type epoxy resins having a phenylene and / or biphenylene skeleton, and naphthol aralkyl type epoxy resins having a phenylene and / or biphenylene skeleton; and aliphatic epoxy resins such as alicyclic epoxy resins such as vinylcyclohexene dioxide, dicyclopentadiene oxide, and alicyclic diepoxy adipide.
[0056] Furthermore, the sealing material of the present embodiment may contain, in addition to the thermosetting resin, a compound having an ultraviolet-reactive functional group, an ultraviolet-curable resin, or an epoxy / (meth)acrylic resin having at least one (meth)acrylic group and at least one epoxy group in one molecule.
[0057] The sealing material of the present embodiment may further contain inorganic particles.
[0058] ·Inorganic particles Examples of inorganic particles include one or more types selected from silica, talc, glass beads, asbestos, gypsum, diatomaceous earth, smectite, bentonite, montmorillonite, sericite, activated clay, alumina, zinc oxide, iron oxide, magnesium oxide, tin oxide, titanium oxide, calcium carbonate, magnesium carbonate, magnesium hydroxide, aluminum hydroxide, aluminum nitride, silicon nitride, barium sulfate, calcium silicate, and the like.
[0059] The inorganic particles may be those whose surfaces have been hydrophobically treated. For example, the inorganic particles may be surface-treated by a known method using epoxysilane, aminosilane, (meth)acrylic silane, vinylsilane, methylchlorosilane, dimethylpolysiloxane, etc. The inorganic particles may be used in combination with those that have been hydrophobically treated and those that have not.
[0060] The content of the inorganic particles is from 1 to 80 mass %, preferably from 3 to 70 mass %, and more preferably from 20 to 60 mass %, based on the total amount of the sealing material.
[0061] ·others The sealing material of the present embodiment may contain organic particles, a polymerization initiator, a thermosetting agent, and the like in addition to the above-mentioned thermosetting resin and inorganic particles.
[0062] The organic particles may be, for example, one or more types selected from polyester fine particles, polyurethane fine particles, vinyl polymer fine particles, acrylic polymer fine particles, silicone fine particles, core-shell type rubber fine particles, and the like.
[0063] Examples of the polymerization initiator include a radical polymerization initiator and a cationic polymerization initiator.
[0064] Examples of the radical polymerization initiator include a photoradical polymerization initiator which generates radicals upon irradiation with light, and a thermal radical polymerization initiator which generates radicals upon heating.
[0065] Examples of the photoradical polymerization initiator include benzophenone-based compounds, acetophenone-based compounds, acylphosphine oxide-based compounds, titanocene-based compounds, oxime ester-based compounds, benzoin ether-based compounds, and thioxanthone.
[0066] Examples of the thermal radical polymerization initiator include those made of an azo compound, an organic peroxide, etc. Among them, a polymeric azo initiator made of a polymeric azo compound is preferred.
[0067] As the cationic polymerization initiator, a photocationic polymerization initiator can be suitably used. The photocationic polymerization initiator is not particularly limited as long as it generates a protonic acid or a Lewis acid upon irradiation with light, and may be either an ionic photoacid generating type or a nonionic photoacid generating type. Examples of the photocationic polymerization initiator include onium salts such as aromatic diazonium salts, aromatic halonium salts, and aromatic sulfonium salts; and organometallic complexes such as iron-allene complexes, titanocene complexes, and arylsilanol-aluminum complexes.
[0068] The content of the polymerization initiator is preferably 0.1 to 30 parts by weight, and more preferably 1 to 10 parts by weight, based on 100 parts by weight of the curable resin. When the content of the polymerization initiator is equal to or more than the lower limit, the sealing material has better curability, whereas when the content of the polymerization initiator is equal to or less than the upper limit, the sealing material has better storage stability.
[0069] The heat curing agent is used to react and crosslink the heat-reactive functional groups in the curable resin by heating, and has the role of improving the adhesiveness and moisture resistance of the curable resin composition after curing. Examples of the heat curing agent include organic acid hydrazides, imidazole derivatives, amine compounds, polyhydric phenol compounds, acid anhydrides, etc. Among these, solid organic acid hydrazides are preferably used.
[0070] The content of the above-mentioned heat curing agent is preferably 0.1 to 50 parts by weight, and more preferably 1 to 30 parts by weight, based on 100 parts by weight of the curable resin. When the content of the polymerization initiator is equal to or more than the lower limit, the sealing material has better curability, whereas when the content of the polymerization initiator is equal to or less than the upper limit, the sealing material has better coatability.
[0071] In addition, additives such as a silane coupling agent, a light blocking agent, a reactive diluent, a spacer, a curing accelerator, an antifoaming agent, a leveling agent, a polymerization inhibitor, and other coupling agents may be contained as necessary.
[0072] (Method of manufacturing sealing materials) An example of a method for producing the sealing material of the present embodiment is a method in which a thermosetting resin and, if necessary, inorganic particles and additives such as a polymerization initiator and / or a thermosetting agent or a silane coupling agent are mixed using a mixer. Examples of the mixer include a homodisper, a homomixer, a universal mixer, a planetary mixer, a kneader, a three-roll mill, and a planetary mixer.
[0073] [Electrochromic layer] The first electrochromic layer 3 and the second electrochromic layer 5 are provided on the upper and lower surfaces of the electrolyte layer 4, respectively, and are disposed so as to sandwich the electrolyte layer 4 therebetween, and are layers containing an electrochromic material.
[0074] The electrochromic material may be either an inorganic electrochromic compound or an organic electrochromic compound, or a conductive polymer known to exhibit electrochromism. The first electrochromic layer 3 and the second electrochromic layer 5 can be made of any of these electrochromic materials. However, when one of them is made of an electrochromic material having oxidative coloring properties, it is preferable that the other is made of an electrochromic material having reductive coloring properties. As the electrochromic material having oxidative coloring properties, a polymer obtained by polymerizing an oxidative coloring electrochromic composition containing a radical polymerizable compound is preferable, and an electrochromic composition containing a radical polymerizable compound having triarylamine is particularly preferable.
[0075] (First Electrochromic Layer) The first electrochromic layer 3 contains, as a main material, a material that exhibits color through an oxidation reaction, and is thus a layer that is colored.
[0076] The average thickness of the first electrochromic layer 3 is not particularly limited, but is preferably about 0.1 μm or more and 30 μm or less, and more preferably about 0.4 μm or more and 10 μm or less.
[0077] The material contained as the main material in the first electrochromic layer 3 and which exhibits color through an oxidation reaction is not particularly limited, and examples thereof include a polymer obtained by polymerizing a composition containing a radically polymerizable compound having a triarylamine, a bisacridan compound, a Prussian blue complex, and nickel oxide, and one or more of these may be used in combination.
[0078] Examples of polymers obtained by polymerizing a composition containing a radically polymerizable compound having a triarylamine include those described in JP-A-2022-25243, JP-A-2016-45464, and JP-A-2020-138925.
[0079] Furthermore, an example of a Prussian blue-type complex is a material made of Fe(III)4[Fe(II)(CN)6]3.
[0080] Among these, a polymer obtained by polymerizing a composition containing a radically polymerizable compound having triarylamine is preferably used, since it can be operated at a constant voltage, has excellent durability during repeated use, and can provide an electrochromic element with high contrast.
[0081] In addition, the composition containing the radical polymerizable compound having a triarylamine may contain another radical polymerizable compound different from the radical polymerizable compound having a triarylamine, and the polymer obtained by polymerizing such a composition may be composed of a crosslinked product in which these radical polymerizable compounds are crosslinked.
[0082] (Second Electrochromic Layer) The second electrochromic layer 5 contains, as a main material, an electrochromic material that changes from transparent to colored by a reduction reaction, and is thus a layer that is colored.
[0083] The average thickness of the second electrochromic layer 5 is not particularly limited, but is preferably about 0.2 μm to 5.0 μm, and more preferably about 1.0 μm to 4.0 μm. If the average thickness is less than 0.2 μm, it may be difficult to obtain a desired color density depending on the type of electrochromic material, and if it exceeds 5.0 μm, the manufacturing cost may increase and visibility may decrease due to coloring depending on the type of electrochromic material.
[0084] The second electrochromic layer 5 is preferably made of an electrochromic material having the same color tone as the first electrochromic layer 3. This improves the maximum color density, and as a result, the contrast can be improved.
[0085] In contrast, when materials of different colors are used, color mixing becomes possible. In addition, by coloring the first electrode 2 and the second electrode 6 through oxidation and reduction reactions, the driving voltages in the electrochromic layer 3, the electrolyte layer 4, and the second electrochromic layer 5 can be effectively reduced, and the repeated durability of the electrochromic sheet 100 can be improved.
[0086] The material contained as the main material in the second electrochromic layer 5 and which exhibits coloration by a reduction reaction is not particularly limited, and examples thereof include inorganic electrochromic compounds, organic electrochromic compounds, conductive polymers, etc., and one or a combination of two or more of these can be used.
[0087] Examples of inorganic electrochromic compounds include tungsten oxide, molybdenum oxide, iridium oxide, titanium oxide, etc., and among these, tungsten oxide is preferred. Tungsten oxide is preferably used because it has a low color development / discoloration potential due to its low reduction potential, and is also excellent in durability because it is an inorganic material.
[0088] In addition, as the organic electrochromic compound, for example, azobenzene-based, anthraquinone-based, diarylethene-based, dihydroprene-based, dipyridine-based, styryl-based, styrylspiropyran-based, spirooxazine-based, spirothiopyran-based, thioindigo-based, tetrathiafulvalene-based, terephthalic acid-based, triphenylmethane-based, triphenylamine-based, naphthopyran-based, viologen-based, pyrazoline-based, phenazine-based, phenylenediamine-based, phenoxazine-based, phenothiazine-based, phthalocyanine-based, fluoran-based, fulgide-based, benzopyran-based, metallocene-based, and other low molecular weight organic electrochromic compounds can be mentioned, among which viologen-based compounds and dipyridine-based compounds are preferred.These compounds are preferably used because they have low color development and fading potential and show good color value.
[0089] Examples of viologen compounds include those described in JP 2022-025243 A, JP 3955641 A, JP 2007-171781 A, etc. Examples of dipyridine compounds include those described in JP 2007-171781 A, JP 2008-116718 A, etc.
[0090] Examples of the conductive polymer include polypyrrole, polythiophene, polyaniline, and derivatives thereof.
[0091] [Electrolyte layer] The electrolyte layer 4 is disposed between the first electrochromic layer 3 and the second electrochromic layer 5, and contains an electrolyte having ion conductivity.
[0092] The average thickness of the electrolyte layer 4 is not particularly limited, but is preferably set to 10 μm or more and 100 μm or less, more preferably 20 μm or more and 80 μm or less, and further preferably 30 μm or more and 70 μm or less.
[0093] The electrolyte layer includes a binder resin and an electrolyte.
[0094] The binder resin is not particularly limited and can be appropriately selected depending on the purpose, but it is preferable that the binder resin contains a urethane resin unit in terms of the phase separation temperature and film strength as a polymer membrane. Also, by containing a polyethylene oxide (PEO) chain, the compatibility with the electrolyte is improved and the phase separation temperature can be increased. Also, by containing a polymethyl methacrylate (PMMA) chain, the compatibility with the electrolyte is improved and the phase separation temperature can be increased, similarly to the case of containing a PEO chain.
[0095] The electrolyte is not particularly limited, but examples thereof include inorganic ion salts such as alkali metal salts and alkaline earth metal salts, quaternary ammonium salts, acids, and alkali supporting salts. Specific examples include LiClO4, LiBF4, LiAsF6, LiPF6, LiCF3SO3, LiCF3COO, KCl, NaClO3, NaCl, NaBF4, NaSCN, KBF4, Mg(ClO4)2, Mg(BF4)2, etc., and one or a combination of two or more of these can be used.
[0096] In addition, ionic liquids can also be used as electrolyte materials. Among these ionic liquids, organic ionic liquids are preferably used because they have a molecular structure that shows liquidity over a wide temperature range including room temperature and are easy to handle.
[0097] As the molecular structure of the organic ionic liquid, the cationic component may be, for example, an imidazole derivative such as N,N-dimethylimidazole salt, N,N-methylethylimidazole salt, or N,N-methylpropylimidazole salt; a pyridinium derivative such as N,N-dimethylpyridinium salt or N,N-methylpropylpyridinium salt; or an aliphatic quaternary ammonium derivative such as trimethylpropylammonium salt, trimethylhexylammonium salt, or triethylhexylammonium salt. In addition, it is preferable to use a fluorine-containing compound as the anionic component, taking into consideration stability in the atmosphere, such as BF4 - , CF3SO3 - , PF4 - , (CF3SO2)2N - etc.
[0098] Such an electrolyte material is preferably an ionic liquid containing any combination of cationic and anionic components.
[0099] The ionic liquid may be directly dissolved in any of the photopolymerizable monomers, oligomers, and liquid crystal materials. If the ionic liquid has poor solubility in these materials, it may be dissolved in a small amount of solvent to obtain a solution, and then this solution may be mixed with any of the photopolymerizable monomers, oligomers, and liquid crystal materials to dissolve the ionic liquid.
[0100] Examples of the solvent include propylene carbonate, acetonitrile, γ-butyrolactone, ethylene carbonate, sulfolane, dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethylsulfoxide, 1,2-dimethoxyethane, 1,2-ethoxymethoxyethane, polyethylene glycol, alcohols, and mixed solvents thereof.
[0101] The electrolyte filled as the electrolyte layer 4 may be either solid or liquid, but in addition to the electrolyte being a low-viscosity liquid, it may take various forms, such as a gel, a polymer cross-linked type, or a liquid crystal dispersion type. Of these, it is preferable that the electrolyte be formed into a gel or solid state. This can improve the element strength and reliability of the electrochromic element 10.
[0102] A preferred method for making the electrolyte layer 4 solid is, for example, a method in which a liquid containing an electrolyte and a solvent is held in a binder resin. This allows the electrolyte layer 4 to have both high ionic conductivity and solid strength. In addition, a photocurable resin is preferred as the polymer resin. This allows the electrolyte layer 4 to be solid at a lower temperature and in a shorter time than when the electrolyte layer 4 is solidified by thermal polymerization or evaporation of a solvent.
[0103] When the electrolyte layer 4 is in a gel state, it can be prepared, for example, as follows. First, a composition solution is prepared, and the prepared composition solution is sandwiched between a mold or a film and polymerized by a cast polymerization method or the like. The composition solution can be prepared by mixing an electrolyte solution obtained by mixing the ionic liquid or solid electrolyte with a solvent, a polymerizable material, a urethane acrylate monomer, and, if necessary, an acrylate monomer having a PEO chain, and, if necessary, an acrylate monomer having a PMMA chain in a desired ratio, and, if necessary, the polymerization initiator and other components can be mixed. As another preparation method, a method of applying a composition solution before polymerization onto one electrochromic layer and polymerizing it by ultraviolet irradiation or heating can be used. Also, a method of placing the supports on which the electrochromic layers have been formed facing each other with a gap of 5 μm to 150 μm maintained, filling the composition solution, and then polymerizing it by ultraviolet irradiation or heating can be used.
[0104] [electrode] The first electrode 2 and the second electrode 6 are electrodes that supply electrons between the first electrode 2 and the second electrode 6, or receive electrons from between the first electrode 2 and the second electrode 6, when a positive voltage or a negative voltage is applied to the first electrochromic layer 3, the electrolyte layer 4, and the second electrochromic layer 5, respectively. The first electrode 2 is provided on the surface of the first electrochromic layer 3 opposite to the electrolyte layer 4. The second electrode 6 is provided on the surface of the second electrochromic layer 5 opposite to the electrolyte layer 4.
[0105] The constituent material of the first electrode 2 and the second electrode 6 is not particularly limited as long as it is a transparent conductive material, and examples thereof include oxides such as ITO (indium tin oxide), FTO (F-doped tin oxide), ATO (antimony tin oxide), IZO (indium zinc oxide), In2O3, SnO2, Sb-containing SnO2, and Al-containing ZnO, Au, Pt, Ag, Cu, and alloys containing these, and one or more of these may be used in combination.
[0106] Examples of methods for producing the first electrode 2 and the second electrode 6 include vacuum deposition, sputtering, and ion plating. In addition, as long as the materials for the first electrode 2 and the second electrode 6 can be applied, various printing methods such as spin coating, casting, microgravure coating, gravure coating, bar coating, roll coating, wire bar coating, dip coating, slit coating, capillary coating, spray coating, nozzle coating, gravure printing, screen printing, flexographic printing, offset printing, reverse printing, and inkjet printing can be used.
[0107] The average thickness of the first electrode 2 and the second electrode 6 is adjusted so as to obtain the electrical resistance value required for the oxidation-reduction reaction of the first electrochromic layer 3 and the second electrochromic layer 5. For example, when ITO is used as the constituent material of the first electrode 2 and the second electrode 6, the average thickness is preferably set to about 50 nm or more and 200 nm or less, more preferably about 100 nm or more and 150 nm or less, respectively.
[0108] Between each layer between the first electrode 2 and the second electrode 6, an intermediate layer such as an insulating porous layer or a protective layer may be provided.
[0109] The total thickness of the electrochromic sheet 100 of this embodiment is not particularly limited, but is preferably 0.3 mm or more and 10.0 mm or less, and more preferably 0.5 mm or more and 5.0 mm or less. By making the total thickness of the electrochromic sheet 100 equal to or greater than the above-mentioned lower limit, strength can be maintained, while by making the layer thickness equal to or less than the above-mentioned upper limit, the electrochromic sheet 100 can be easily processed, such as by cutting or bending.
[0110] Each layer of the electrochromic sheet 100 may be replaced with any layer having a similar function, or other layers may be further provided.
[0111] [Effects] By having the above-described configuration, the electrochromic sheet 100 can, for example, cause the electrochromic element 10 to develop a predetermined color by applying a positive voltage between the first electrode 2 and the second electrode 6, while the electrochromic element 10 can be decolorized and made transparent by applying a negative voltage between the first electrode 2 and the second electrode 6.
[0112] <Manufacturing method of electrochromic sheet> The method for producing an electrochromic sheet according to the present embodiment is not limited to the case where there is one electrochromic layer, but can also be applied to the case where there are multiple electrochromic layers. An example of a method for producing the electrochromic sheet 100 will now be described.
[0113] The method for producing the electrochromic sheet 100 includes the following steps. A step of forming a first electrode 2 on a first support 1 and laminating a first electrochromic layer 3 on the first electrode 2; forming a second electrode 6 on a second support 7 and forming a second electrochromic layer 5 on the second electrode 6; applying a sealing material onto the first electrode 2 so as to surround the outer edge of the first electrochromic layer 3, or applying a sealing material onto the second electrode 6 so as to surround the outer edge of the second electrochromic layer 5; a step of preparing an electrolyte layer 4, and bonding a first support 1 and a second support 2 together with a first electrochromic layer 3 and a second electrochromic layer 5 facing each other with the electrolyte layer 4 interposed therebetween; A step of hardening the sealing material to form a sealing portion 8; having In the lamination step, the sealing material is spread out, so that the first electrochromic layer 3 and the second electrochromic layer 5 are covered with the sealing material. This results in an electrochromic sheet 100.
[0114] <Electrochromic device> The electrochromic device of this embodiment has the above-mentioned electrochromic sheet 100, and may further have other means as necessary. The other means are not particularly limited and can be appropriately selected depending on the application. Examples of the other means include a power source, a fixing means, and a control means. Examples of electrochromic devices include eyewear, photochromic glasses, binoculars, opera glasses, bicycle goggles, watches, electronic paper, electronic albums, and electronic billboards.
[0115] For example, when a so-called UV-cut lens is produced using the above electrochromic sheet 100, with the first support layer 1 being the convex side of the lens and the second support layer 7 being the concave side of the lens, the first support layer 1 may have a light transmittance of 10% or less at a wavelength of 380 nm, and the second support layer 7 may have a light transmittance different from that of the first support layer 1. In this case, a UV-cut resin layer may be further provided on the concave side of the UV-cut lens (on the second support layer 7).
[0116] Although the embodiments of the present invention have been described above with reference to the drawings, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. EXAMPLES
[0117] Next, the present invention will be described in detail with reference to examples, but the content of the present invention is not limited to the examples.
[0118] <Example 1> (1) Preparation of the support layer The following support layers were prepared and their light transmittance was measured. The results are shown in Table 1. First support layer and second support layer: 100 parts by mass of bisphenol A polycarbonate (Mitsubishi Gas Chemical's "Iupilon E2000F-N") and 0.35 parts by mass of an ultraviolet absorber (ADEKA's "Adeka STAB LA-31G") were mixed, melt-kneaded in an extruder, and extruded from a T-die to obtain a 300 μm sheet.
[0119] (2) Preparation of electrochromic sheet An electrochromic sheet as shown in FIG. 1 was produced by the following procedure. - Formation of the first electrode - An ITO film was formed by sputtering on the first support prepared in (1) above to a thickness of about 100 nm, thereby forming a first electrode. 3 g of titanium oxide (ST-21, manufactured by Ishihara Sangyo Kaisha), 0.2 g of acetylacetone, 0.3 g of a surfactant (polyoxyethylene octylphenyl ether, manufactured by Wako Pure Chemical Industries, Ltd.) were treated in a bead mill together with 5.5 g of water and 1.0 g of ethanol for 12 hours. To the resulting dispersion was added 1.2 g of polyethylene glycol (#20,000, manufactured by NOF Corporation) to prepare a paste. The obtained paste was applied onto the first electrode by screen printing to a thickness of 2 μm, dried at 80°C, and then subjected to UV ozone treatment at 90°C for 20 minutes to form an electron transport layer made of a porous titanium oxide particle film.
[0120] - Formation of the first electrochromic layer - Next, a 2,2,3,3-tetrafluoropropanol solution containing 1.5 mass % of a reductively coloring electrochromic compound I represented by the following chemical formula was applied by spin coating, and then annealed at 80°C for 10 minutes to support (adsorb) the compound on the porous titanium oxide particle film, thereby forming a first electrochromic layer.
[0121] [ka]
[0122] - Formation of the second electrode - On the second support prepared in (1) above, an ITO film was formed by sputtering to a thickness of about 100 nm to form a second electrode.
[0123] - Formation of the second electrochromic layer - On the ITO film, which is the second electrode, polyethylene glycol diacrylate (PEG400DA, manufactured by Nippon Kayaku Co., Ltd.) and a photoinitiator (IRGACURE 184, manufactured by BASF) were applied. A solution was prepared by mixing a radical polymerizable compound II having a triarylamine represented by the following formula as an oxidative coloring electrochromic material and 2-butanone in a mass ratio of (57:3:140:800). The prepared solution was then applied to an ITO glass substrate by spin coating.
[0124] [ka] (In the formula, Me represents a methyl group.)
[0125] Next, under a nitrogen atmosphere, a patterned second electrochromic layer having a thickness of 1.2 μm and containing the compound represented by the radical polymerizable compound II was selectively formed on the second electrode by UV curing via a quartz substrate having a patterned Cr layer.
[0126] -Preparation of gel electrolyte- A polymerizable material (V3877, Daido Chemical Industry Co., Ltd.) and an electrolyte (1-ethyl-3-methylimidazolium tetracyanoborate (EMIMTCB)) were mixed in a mass ratio of 20:80 on the surface of a release-treated PET film (NP75C, PANAC Corporation), and a solution in which a photopolymerization initiator (irgacure184, Nippon Kayaku Co., Ltd.) was mixed at 0.5 mass% relative to the polymerizable material was applied. The film was then bonded to a release-treated PET film (NP75A, PANAC Corporation), and cured with ultraviolet (UV) light to produce a gel electrolyte.
[0127] -Lamination process- The release film was peeled off from the prepared gel electrolyte, and the gel electrolyte was attached to the surface of the first electrochromic layer. Next, a sealing material (epoxy resin "CRM-1576AW" manufactured by Sumitomo Bakelite Co., Ltd.) was applied using a dispenser so as to surround the periphery of the side surface of the first electrochromic layer. Thereafter, the second electrochromic layer of the second support was aligned with the surface of the gel electrolyte and bonded to each other, and the sealing material was spread to cover the sides of the first electrochromic layer and the second electrochromic layer with the sealing material. A thermal curing treatment was then performed at 100°C for 1 hour to harden the sealing material and form a sealing portion, thereby producing an electrochromic sheet.
[0128] (3) Evaluation and measurement The light resistance of the resulting electrochromic sheet was evaluated. Light resistance The electrochromic sheet was colored by applying a voltage of 1.6V for 15 seconds, and the light transmittance was measured. After that, a light resistance test was performed in accordance with ISO12311:2013, in an environment of 28°C, by irradiating the sheet with a xenon lamp with a light output of 450W for 51 hours. After that, the electrochromic sheet was once put into a decolorized state, and then the color was developed again by applying a voltage of 1.6V for 15 seconds, and the light transmittance was measured again, and the difference in the color transmittance before and after the light resistance test was calculated. The smaller the difference in transmittance when colored before and after the light fastness test, the better the light fastness. The light transmittance was measured using an ultraviolet-visible-near infrared spectrophotometer (V-670, manufactured by JASCO Corporation).
[0129] -Light transmittance measurement The transmittance of each support layer was measured using an ultraviolet-visible-near infrared spectrophotometer (V-670, manufactured by JASCO Corporation), and the light transmittance was calculated. The measurement wavelength was 280 nm to 780 nm. The results are shown in FIG. 2 (Example 1) and FIG. 3 (Comparative Example 1).
[0130] <Comparative Example 1> The same procedure as in Example 1 was carried out, except that no ultraviolet absorber (ADEKA "ADEKA STAB LA-31G") was used in the first support layer and the second support layer.
[0131] [Table 1] [Explanation of symbols]
[0132] 1 First Support Layer 2 Second electrode 3 First electrochromic layer 4 Electrolyte layer 5 Second Electrochromic Layer 6 Second electrode 7 Second Support Layer 8 Sealing part 10 Electrochromic elements 100 Electrochromic Sheet
Claims
1. A support layer; an electrolyte layer provided on the support layer; an electrochromic layer provided on at least one surface of the electrolyte layer; a sealing portion provided so as to cover at least a side surface of the electrolyte layer; An electrochromic sheet comprising: the electrolyte layer comprises a photocured gel; The support layer is made of a resin material containing a transparent resin and an ultraviolet absorber, and has a light transmittance of 10% or less at a wavelength of 380 nm and a light transmittance of 80% or more at a wavelength of 430 nm.
2. 2. The electrochromic sheet according to claim 1, The support layer is an electrochromic sheet containing one or more resins selected from episulfide-based resins, thiourethane-based resins, acrylic-based resins, polycarbonate-based resins, urethane-based resins, polyamide-based resins, polyester-based resins, cycloolefin polymers (COP), cycloolefin copolymers (COC), norbornene-based resins, and silicone-based resins.
3. 3. The electrochromic sheet according to claim 1 or 2, The thickness of the electrolyte layer is 10 μm or more and 100 μm or less.
4. 3. The electrochromic sheet according to claim 1 or 2, The sealing portion is formed using a sealing material including a thermosetting resin.
5. 5. The electrochromic sheet according to claim 4, The electrochromic sheet, wherein the thermosetting resin includes one or more resins selected from the group consisting of epoxy resins, acrylic resins, phenolic resins, maleimide resins, silicone resins, urethane resins, cyanate resins, melamine resins, urea resins, and unsaturated polyester resins.
6. 3. The electrochromic sheet according to claim 1 or 2, An electrochromic sheet, the electrochromic layer being provided on the upper and lower surfaces of the electrolyte layer of the electrochromic sheet.
7. 3. The electrochromic sheet according to claim 1 or 2, The electrochromic sheet has a thickness of 0.3 mm or more and 10.0 mm or less.
Citation Information
Patent Citations
Light control film, and method of manufacturing light control film
JP2013148687A
Electrochromic device and method of manufacturing the same
JP2017111380A
Electrochemical device with plastic substrate
JP2018514799A
Electrochromic element
JP2020106786A
Electrochromic organic frameworks
US20180321565A1