Polyamide laminate film and its manufacturing method

A polyamide-based laminate film with a polyurethane resin layer addresses the challenge of achieving high slip and printability, ensuring stable processing and preventing delamination, particularly under high humidity, by employing a specific layer configuration and coating process.

JP7568294B2Active Publication Date: 2024-10-16UNITIKA LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021512041
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-29
Filing Date
2020-03-27
Publication Date
2024-10-16
Estimated Expiration
2040-03-27

AI Technical Summary

Technical Problem

Conventional polyamide films face challenges in achieving both high slip properties and good printability, particularly under varying humidity conditions, which affects their suitability for high-speed processing and high-definition printing, and they also struggle with delamination during cold forming due to frictional issues.

Method used

A polyamide-based laminate film comprising a polyamide film and a polyurethane resin layer with specific properties, including a glass transition temperature of 50°C or higher, an arithmetic mean height (Ra) of 0.010 to 0.060 μm, and a dynamic friction coefficient of 0.40 or less, is developed, with a coating process involving biaxial stretching and application of a water-based coating solution containing a polyurethane resin and organic lubricant.

Benefits of technology

The film exhibits excellent slip properties and printability, allowing for stable processing and high-definition printing, while preventing delamination during cold forming, even under high humidity conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568294000003
    Figure 0007568294000003
  • Figure 0007568294000004
    Figure 0007568294000004
  • Figure 0007568294000001
    Figure 0007568294000001
Patent Text Reader

Abstract

[Problem] To provide a polyamide-based laminated film endowed with both high slipperiness and good printability. [Solution] The present invention pertains to a laminated film including a polyamide film and a polyurethane resin layer containing a polyurethane resin and an organic lubricant on at least one surface of the polyamide film, wherein the polyamide-based laminated film is characterized in that (1) the glass transition temperature of the polyurethane resin is 50°C or higher, (2) the arithmetic mean height (Ra) of the polyurethane resin layer surface is 0.010 to 0.060 μm, and the dynamic friction coefficient of the polyurethane resin layer surface in a 20°C×90% RH environment is 0.40 or lower.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyamide-based laminate film used for packaging or covering foods, electronic parts, and the like. [Background technology]

[0002] Polyamide films have excellent toughness and are widely used in a variety of applications, from food packaging to industrial applications. Resin films, including polyamide films, are processed using printers, laminators, etc., depending on the intended use. In these processing machines, the resin film is transported by running between rolls whose surfaces are made of metal or rubber. Since the rolls and the resin film are in direct contact with each other, if the friction coefficient of the contact surface of the resin film is large, a difference occurs between the transport speed of the resin film and the rotation speed of the rolls. As a result, scratches may appear on the surface of the resin film, or the running of the resin film may become unstable. For this reason, a method has been proposed in which the resin film contains an inorganic filler and the surface of the resin film is roughened to reduce the contact surface with the rolls and reduce friction.

[0003] However, in recent years, there has been a demand for increasing the running speed of resin films in order to improve productivity, and the effect of reducing friction is not sufficient when the film surface is roughened by a conventional physical method alone, and excessive roughening may impair printability. Furthermore, roughening the film surface alone causes a problem of an increase in the coefficient of friction under high humidity.

[0004] In response to this, a method has been proposed in which inorganic particles and long-chain fatty acid bisamide are incorporated into a polyamide film (Patent Document 1). However, although the incorporation of an aliphatic amide can suppress an increase in the dynamic friction coefficient under high humidity conditions, it is difficult to control the amount of bleed-out, and this raises concerns about roll contamination and reduced printability.

[0005] On the other hand, a biaxially oriented polyamide film has been proposed in which a coating layer containing wax having a long-chain alkyl group and spherical fine particles is laminated on a polyamide film (Patent Document 2). With this film, by providing a coating layer containing slip agents and particles, a predetermined effect can be obtained with a smaller amount than when they are contained in a resin film. However, when the particle diameter of the spherical fine particles is small compared to the thickness of the coating layer, the effect of adding the spherical fine particles is small. On the other hand, when the particle diameter of the spherical fine particles is large, there is a high risk that the fine particles will slip or fall off. In addition, when high-definition printing is required, if the surface roughness is large, printing defects and the like may occur, and printing accuracy may decrease.

[0006] As described above, in conventional technology, making a film slippery sacrifices its printability, while improving printability creates the problem of making the film less slippery, making it difficult to improve both at once.

[0007] In recent years, polyamide films have been used in the industrial field as exterior materials for lithium-ion batteries, but even in such applications, the slipperiness of the film becomes an issue.

[0008] Metal can types have traditionally been the mainstream exterior materials for lithium-ion batteries. However, drawbacks of metal can types, such as low freedom of shape and difficulty in reducing weight, have been pointed out. For this reason, it has been proposed to use a laminate consisting of a base layer (polyamide film), a metal foil layer (aluminum foil layer), and a sealant layer as an exterior body. Such laminates are more flexible and have a higher degree of freedom of shape than metal cans, and can be made thinner to reduce weight and easily miniaturized, and therefore are becoming more widely used.

[0009] Then, the laminate as described above is processed into a predetermined shape by cold forming to obtain various products such as containers. One of the physical properties of the film that affects the moldability during cold forming is the slipperiness of the film. For example, when a laminate having a polyamide film as the outermost layer is cold formed, the polyamide film comes into contact with the molding die, and if the polyamide film is not slippery (i.e., has a large coefficient of friction), wrinkles may occur on the surface of the laminate when the molding die is pressed in, and the laminate may be delaminate. Moreover, it is difficult to uniformly form the entire laminate, and thickness unevenness occurs, so there is a concern about the occurrence of pinholes. In particular, when cold forming is performed under high humidity, these problems become even more pronounced. In this respect, it is also required that the slipperiness of the film does not depend on humidity. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2002-348465 A [Patent Document 2] JP 2015-168125 A Summary of the Invention [Problem to be solved by the invention]

[0011] In view of the above, there is a demand for a polyamide film that has excellent slip properties regardless of humidity, and therefore also has excellent cold formability and various processability, and that can be subjected to high-resolution printing; however, such a film has not yet been developed.

[0012] Therefore, a main object of the present invention is to provide a polyamide-based laminate film that combines high slip properties with good printability. [Means for solving the problem]

[0013] As a result of extensive research into solving the above problems, the inventors discovered that the above object can be achieved by adopting a specific layer structure including a polyamide film and a specific resin layer, and thus completed the present invention.

[0014] That is, the present invention relates to the following polyamide-based laminate film and a method for producing the same. 1. A laminated film comprising a polyamide film and a polyurethane resin layer containing a polyurethane resin and an organic lubricant laminated on at least one surface of the film, (1) The glass transition temperature of the polyurethane resin is 50° C. or higher, (2) The arithmetic mean height (Ra) of the surface of the polyurethane resin layer is 0.010 to 0.060 μm, and the dynamic friction coefficient of the surface of the polyurethane resin layer in an environment of 20° C.×90% RH is 0.40 or less. A polyamide-based laminate film characterized by: 2. The polyamide-based laminate film according to item 1, wherein the dynamic friction coefficient of the surface of the polyurethane resin layer in an environment of 23° C.×50% RH is 0.30 or less. 3. The polyamide-based laminate film according to item 1, wherein the polyurethane resin layer has a thickness of 0.005 to 0.150 μm. 4. A food packaging laminate comprising the polyamide-based laminate film according to any one of items 1 to 3. 5. A laminate for cold forming, comprising the polyamide-based laminate film according to any one of items 1 to 3. 6. A method for producing a polyamide-based laminate film comprising a polyamide film and a polyurethane resin layer containing a polyurethane resin and an organic lubricant on at least one surface of the film, comprising the steps of: (1) a sheet forming step of forming a melt-kneaded material containing a polyamide resin into a sheet to obtain an unstretched sheet; (2) a stretching step in which the unstretched sheet is stretched in the MD and TD to obtain a biaxially stretched film; and (3) A coating step of applying an aqueous coating liquid containing a polyurethane resin and an organic lubricant onto one surface of the unstretched sheet, MD-stretched film, TD-stretched film, or biaxially stretched film. A method for producing a polyamide-based laminate film, comprising: 7. The method according to item 6, wherein the aqueous coating liquid is a mixture of a dispersion of a polyurethane resin and a dispersion of an organic lubricant having a particle size of 0.010 μm to 0.500 μm. 8. The stretching step is carried out by simultaneous biaxial stretching and is represented by the following formulas (a) and (b); (a) 0.80≦X / Y≦0.95 (b) 9.8≦X×Y≦11.6 (wherein X represents the stretching ratio in the MD direction, and Y represents the stretching ratio in the TD direction). Item 7. The method according to item 6, wherein both of the above conditions are satisfied. 9. The stretching step is carried out by sequential biaxial stretching and is represented by the following formulas (a) and (b); (a) 0.85≦X / Y≦0.95 (b) 8.5≦X×Y≦9.5 (wherein X represents the stretching ratio in the MD direction, and Y represents the stretching ratio in the TD direction). Item 7. The method according to item 6, wherein both of the above conditions are satisfied. Effect of the Invention

[0015] According to the present invention, it is possible to provide a polyamide-based laminate film having both high slip properties and good printability. That is, the present invention makes it possible to simultaneously improve slip properties and printability (particularly ink transfer from a plate), which have been considered to be mutually exclusive properties in the prior art.

[0016] The polyamide laminate film of the present invention has a low arithmetic mean height (Ra) of the polyurethane resin layer, so that it can be printed with high resolution. At the same time, despite the low Ra, the dynamic friction coefficient at high humidity is small, so that it can exhibit stable slip properties regardless of humidity. As a result, the polyamide laminate film of the present invention is suitable for transport by rolls and can be suitably used in various processing.

[0017] In particular, since the polyurethane resin layer is mainly composed of an organic polyurethane resin, it has excellent ink adhesion and can exhibit excellent printability. In addition, since the polyurethane resin layer has relatively good flexibility, it can follow dimensional changes of the polyamide film, for example, during boiling or retort treatment. Therefore, when processing such as molding (particularly cold molding) is performed using the polyamide-based laminate film of the present invention, the occurrence of delamination can be effectively suppressed or prevented.

[0018] Furthermore, when the polyamide-based laminate film of the present invention is laminated with aluminum foil and subjected to cold forming, it has good conformability to the aluminum foil and has low friction with the forming die, and therefore has excellent formability, making it possible to obtain a molded product that is free of delamination or pinholes.

[0019] According to the method for producing a polyamide-based laminate film of the present invention, the polyamide-based laminate film of the present invention can be obtained more reliably and with good productivity. [Brief description of the drawings]

[0020] [Figure 1] 1 is a diagram showing an example of a layer structure of a polyamide-based laminate film of the present invention. [Diagram 2] 1 is a diagram showing an embodiment of a polyamide-based laminate film of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] 1. Polyamide laminate film The polyamide-based laminate film of the present invention (the film of the present invention) is a laminate film comprising a polyamide film and a polyurethane resin layer containing a polyurethane resin and an organic lubricant laminated on at least one surface of the film, (1) The glass transition temperature of the polyurethane resin is 50° C. or higher, (2) The arithmetic mean height (Ra) of the surface of the polyurethane resin layer is 0.010 to 0.060 μm, and the dynamic friction coefficient of the surface of the polyurethane resin layer in an environment of 20° C.×90% RH is 0.40 or less. It is characterized by:

[0022] A. Layer structure of the film of the present invention As described above, the film of the present invention is basically composed of a laminated film including a polyamide film and a polyurethane resin layer (hereinafter, simply referred to as "polyurethane resin layer") containing a polyurethane resin and an organic lubricant laminated on at least one surface of the film. That is, the film of the present invention is basically composed of a laminated structure in which a polyurethane resin layer is formed adjacent to one or both surfaces of a polyamide film without an adhesive layer therebetween.

[0023] FIG. 1 shows an example of the layer structure of the film of the present invention. FIG. 1A shows a laminate (film of the present invention) 10 in which a polyurethane resin layer 12 is laminated on one side of a polyamide film 11. FIG. 1B shows a laminate (film of the present invention) 10' in which polyurethane resin layers 12, 12 are laminated on both sides of a polyamide film 11. In both of these cases, the polyurethane resin layer is disposed as the outermost layer (outermost layer) (layer exposed to the outside). By exposing the polyurethane resin layer as the outermost layer in this way, for example, when a package (bag, etc.) is produced using the film of the present invention with the polyurethane resin layer facing outward, the contents of the package can be protected from the outside. Therefore, in the film of the present invention, it is desirable that the polyurethane resin layer is disposed as the outermost layer (outermost layer) (layer exposed to the outside) on at least one of the front and back surfaces.

[0024] In the film of the present invention, as long as the polyurethane resin layer is formed directly on the surface of the polyamide film as described above and at least one polyurethane resin layer is disposed as the outermost layer, other layers may be further laminated as necessary, such as a barrier layer (gas barrier layer, water vapor barrier layer, etc.), a printing layer, an adhesive layer, a heat fusion layer (sealant layer, heat seal layer), a primer layer (anchor coat layer), an antistatic layer, a deposition layer, an ultraviolet absorbing layer, an ultraviolet blocking layer, etc.

[0025] FIG. 2 shows an example of a layer structure of a polyamide-based laminate film in which, in addition to a polyamide film and a polyurethane resin layer, other optional layers are further laminated.

[0026] Fig. 2A shows a laminate 20 obtained by sequentially laminating a barrier layer 13 and a heat-sealing layer 14 on one side of the laminate 10 in Fig. 1A. In this laminate 20, the barrier layer 13 and the heat-sealing layer 14 are laminated on the side of the polyamide film 11 on which the polyurethane resin layer 12 is not formed, so that the polyurethane resin layer 12 is maintained in an exposed state as the outermost surface layer.

[0027] Fig. 2B shows a laminate 20' in which a barrier layer 13 and a heat-sealing layer 14 are laminated in this order on one side of the laminate 10' in Fig. 1B. In this laminate 20', the barrier layer 13 and the heat-sealing layer 14 are laminated on one of the polyurethane resin layers 12 of the polyamide film 11, and the other polyurethane resin layer 12 is maintained in an exposed state as the outermost surface layer.

[0028] 2A or 2B, when the film of the present invention has a heat-sealing layer 14, the heat-sealing layer 14 is disposed as the outermost layer. That is, when the film of the present invention has a heat-sealing layer 14, it is preferable to adopt a layer structure in which one outermost layer is the polyurethane resin layer 12 and the other outermost layer is the heat-sealing layer 14.

[0029] In the following, the polyamide film and polyurethane resin layer constituting the film of the present invention as well as the optional layers will be described.

[0030] A-1.Polyamide film The polyamide film is the substrate (core) of the film of the present invention, and is usually provided in the form of a preformed film. The polyamide film itself may be a publicly known or commercially available product. A film produced by a publicly known production method may also be used.

[0031] The polyamide film may have a single layer structure or a multilayer structure in which two or more polyamide films are laminated, and in the case of a multilayer structure, each layer may have the same composition or different compositions.

[0032] The polyamide film is mainly composed of a polyamide resin, but may contain other components within the range that does not impair the effects of the present invention. In this case, the content of the polyamide resin in the polyamide film is not limited, but is usually about 70 to 100 mass%, particularly preferably 90 to 99.5 mass%, and more preferably 95 to 99 mass%.

[0033] The polyamide resin may be any melt-moldable thermoplastic resin having an amide bond (-CONH-) in the molecule, and may be any known or commercially available one. For example, polyamides obtained by polycondensation of lactams, ω-amino acids, or dibasic acids with diamines may be used.

[0034] Examples of lactams include ε-caprolactam, enantholactam, capryllactam, and lauryllactam.

[0035] Examples of the ω-amino acids include 6-aminocaproic acid, 7-aminoheptanoic acid, 9-aminononanoic acid, and 11-aminoundecanoic acid.

[0036] Examples of dibasic acids include adipic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecadioic acid, hexadecadioic acid, eicosanedionic acid, eicosadienedioic acid, 2,2,4-trimethyladipic acid, terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, and xylylenedicarboxylic acid.

[0037] Examples of diamines include ethylenediamine, trimethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, 2,2,4 (or 2,4,4)-trimethylhexamethylenediamine, cyclohexanediamine, bis-(4,4'-aminocyclohexyl)methane, and metaxylylenediamine.

[0038] In the present invention, from the standpoint of environmental protection and the like, compounds derived from biomass can also be used as these compounds (starting materials).

[0039] As the polymer or copolymer obtained by polycondensing these monomer components, for example, nylon 6, 7, 11, 12, 6.6, 6.9, 6.11, 6.12, 6T, 9T, 10T, 6I, MXD6 (polymetaxylylene adipamide), 6 / 6.6, 6 / 12, 6 / 6T, 6 / 6I, 6 / MXD6, etc. can be used. These can be used alone or in combination of two or more. Among these, aliphatic polyamide resins such as nylon 6 and nylon 6,6 are preferred, and nylon 6 is more preferred in terms of its excellent balance between heat resistance and mechanical properties.

[0040] The relative viscosity of the polyamide resin used in the polyamide film is not limited, but is preferably about 1.5 to 5.0, and more preferably 2.0 to 4.0. If the relative viscosity is less than 1.5, the mechanical properties of the resulting film are likely to be significantly reduced. On the other hand, if the relative viscosity exceeds 5.0, the film formability of the film is likely to be impaired. The above relative viscosity is a value measured using a Ubbelohde viscometer for a sample solution (liquid temperature 25°C) in which polyamide is dissolved in 96% sulfuric acid to a concentration of 1.0 g / dl. In the present invention, the relative viscosity of the polyamide film in the finally obtained film of the present invention is also preferably within the above range.

[0041] As described above, the polyamide film may contain other components in addition to the polyamide resin, as long as the effects of the present invention are not hindered. Examples of other components include known or commercially available additives. More specifically, metals (metal ions), pigments, heat stabilizers, antioxidants, weathering agents, flame retardants, plasticizers, release agents, and reinforcing agents (fillers) are exemplified. In particular, hindered phenols, phosphorus compounds, hindered amines, sulfur compounds, copper compounds, alkali metal halides, and the like can be suitably used as heat stabilizers or antioxidants.

[0042] The polyamide film may contain a lubricant as required. Specific examples of the lubricant include inorganic lubricants such as clay, talc, calcium carbonate, zinc carbonate, wollastonite, silica, alumina, magnesium oxide, calcium silicate, sodium aluminate, calcium aluminate, magnesium aluminosilicate, glass balloons, carbon black, zinc oxide, antimony trioxide, zeolite, hydrotalcite, and layered silicate, and organic lubricants such as erucic acid amide, oleic acid amide, stearic acid amide, ethylene bisstearic acid amide, ethylene bisethylene bisoleic acid amide, hexamethylene bisstearic acid amide, and hexamethylene bisoleic acid amide methylene bisstearic acid amide. These may be used alone or in combination of two or more.

[0043] The thickness of the polyamide film is not particularly limited, but is generally preferably 4 to 35 μm, and more preferably 5 to 25 μm. If the thickness is less than 4 μm, the mechanical strength is likely to be insufficient, and the moldability is reduced. On the other hand, if the thickness exceeds 35 μm, the amount of raw material used may increase or the productivity may decrease.

[0044] Moreover, from the viewpoint of mechanical strength, the polyamide film is preferably stretched. That is, it is preferable that the polyamide film has an oriented structure. In this case, the polyamide film may be uniaxially or biaxially stretched, but it is particularly preferable that the polyamide film has an oriented structure due to biaxial stretching. The stretching ratio can be appropriately set within the range described below.

[0045] In order to improve the adhesion between the layers constituting the laminate when made into a laminate, it is preferable that the polyamide film has a surface that has been subjected to a known surface treatment such as corona treatment, plasma treatment, or ozone treatment on at least one side.

[0046] A-2. Polyurethane resin layer The polyurethane resin layer constituting the film of the present invention is a layer that is primarily intended to exhibit slip properties and printability, and contains a polyurethane resin and an organic lubricant.

[0047] The polyurethane resin is, for example, a polymer obtained by the reaction of a polyfunctional isocyanate with a hydroxyl group-containing compound. More specifically, examples of the polyurethane resin include urethane resins obtained by the reaction of a polyfunctional isocyanate such as an aromatic polyisocyanate (e.g., tolylene diisocyanate, diphenylmethane isocyanate, polymethylene polyphenylene polyisocyanate) or an aliphatic polyisocyanate (e.g., hexamethylene diisocyanate, xylene isocyanate) with a hydroxyl group-containing compound (e.g., polyether polyol, polyester polyol, polyacrylate polyol, polycarbonate polyol). These polyurethane resins themselves may be publicly known or commercially available.

[0048] In addition, various functional groups such as anionic functional groups, cationic functional groups, and nonionic functional groups may be introduced into the polyurethane resin within a range that does not impair the effects of the present invention. In particular, it is preferable that the polyurethane resin contains an anionic functional group from the viewpoint of dispersibility in the coating liquid. Examples of the anionic functional group include a carboxyl group and a sulfone group.

[0049] The method of introducing an anionic functional group into the polyurethane resin is not particularly limited, and examples thereof include a) a method of using a diol having an anionic functional group as a polyol component, and b) a method of using a diol having an anionic functional group as a chain extender. Examples of the diol having an anionic functional group include aliphatic carboxylic acids such as glyceric acid, dioxymaleic acid, dioxyfumaric acid, tartaric acid, dimethylolpropionic acid, dimethylolbutanoic acid, 2,2-dimethylolvaleric acid, 2,2-dimethylolpentanoic acid, 4,4-di(hydroxyphenyl)valeric acid, and 4,4-di(hydroxyphenyl)butyric acid, as well as aromatic carboxylic acids such as 2,6-dioxybenzoic acid.

[0050] The polyurethane resin layer preferably forms a crosslinked structure. The crosslinked structure can be formed by a) a method of forming the crosslinked structure by adding a crosslinking agent capable of reacting with the polyurethane resin to form a crosslinked structure, or b) a method of using a polyurethane resin containing a reactive group in the skeleton.

[0051] The crosslinking agent is preferably one that can react with the terminal group of the polyurethane resin. This can reduce the polar groups in the polyurethane resin molecule, thereby further improving the slipperiness. Specific examples of the crosslinking agent include isocyanate, oxazoline, carbodiimide, and melamine resin. Among these, it is preferable to use melamine resin from the viewpoints of reactivity, economy, and the like. A representative example of the melamine resin is tri(alkoxymethyl)melamine. Examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, and a butoxy group. One or more of these melamine resins can be used.

[0052] When a crosslinking agent is used, the amount added may be appropriately set depending on the type of crosslinking agent used, but can usually be set within the range of 1 to 10 parts by mass per 100 parts by mass of the polyurethane resin.

[0053] The glass transition temperature of the polyurethane resin must be 50°C or higher, particularly from the viewpoint of improving slipperiness, and is preferably 70°C or higher, and more preferably 90°C or higher. If the glass transition temperature is less than 50°C, the dynamic friction coefficient may exceed the range specified in the present invention, and the slipperiness tends to decrease, especially under high humidity. The upper limit of the glass transition temperature is not limited, but can be, for example, about 150°C.

[0054] The content of the polyurethane resin in the polyurethane resin layer is not particularly limited, but can usually be about 50 to 98% by weight (particularly 70 to 95% by weight), but is not limited thereto.

[0055] In the present invention, the organic lubricant, when present together with a polyurethane resin having a glass transition temperature of 50° C. or higher, serves to simultaneously enhance both of the mutually contradictory properties of slipperiness and printability.

[0056] The organic lubricant is not particularly limited, and examples thereof include various organic compounds such as hydrocarbons, fatty acids, aliphatic bisamides, and metal soaps, as well as resin-based organic lubricants such as phenol resins, melamine resins, and polymethyl methacrylate resins.

[0057] Among these organic lubricants, in the present invention, it is particularly preferable to use an organic lubricant having a melting point of 50 to 200°C. Such an organic lubricant is not particularly limited, but it is preferable to use at least one of polyethylene wax, silicon-acrylic copolymer, silicon-urethane copolymer, and aliphatic amide. These organic lubricants can be in a liquid state, so they do not impair the smoothness of the polyurethane resin layer surface. In addition, since they are added to the polyurethane resin layer, it is possible to obtain the effect as a lubricant with a smaller amount added, and the amount of bleed-out can be controlled more easily. These organic lubricants can also be commercially available products.

[0058] From the viewpoint of slipperiness, the polyethylene wax is preferably one that is mainly composed of highly crystalline polyethylene, and preferably has a melting point of 90°C or higher, more preferably 100°C or higher, and most preferably 120°C or higher. As long as the melting point is 90°C or higher, the wax may be polyethylene alone, a polyethylene copolymer, or a mixture of polyethylene and a polyethylene copolymer. The upper limit of the melting point may be, for example, about 150°C.

[0059] From the viewpoint of compatibility with polyurethane resins, it is preferable that the silicone-acrylic copolymer and silicone-urethane copolymer have side chains polymerized to the main chain by graft polymerization. If the main chain is a silicone component, the side chain is preferably an acrylic or urethane component, and if the main chain is an acrylic or urethane component, the side chain is preferably a silicone component.

[0060] The aliphatic amide preferably has a carbon number of C8 to C20, particularly preferably C12 to C18, and more preferably C16 to C18. If it exceeds C20, printability may be reduced. If it is less than C8, the effect of improving slippage may not be sufficient. Specific examples of such fatty acid amides include saturated fatty acids such as stearic acid (C18) and monoamides of unsaturated fatty acids such as oleic acid (C18). Among these, at least one of stearic acid amide and ethylene bisstearic acid amide is preferred because of its good compatibility with water-based coating liquid.

[0061] The organic lubricant may be contained in the polyurethane resin layer, but may be unevenly distributed on the surface of the polyurethane resin layer. When the organic lubricant is unevenly distributed on the surface of the polyurethane resin layer, slipperiness can be reliably imparted with a smaller amount of the organic lubricant.

[0062] From the viewpoint of improving slipperiness and printability, the content (solid content ratio) of the organic lubricant is preferably 5 to 30 parts by mass, more preferably 10 to 30 parts by mass, and most preferably 15 to 30 parts by mass, relative to 100 parts by mass of the polyurethane resin. If the organic lubricant exceeds 0 parts by mass, not only will the printability deteriorate, but the effect of lowering the dynamic friction coefficient will also be reduced. If the organic lubricant is less than 5 parts by mass, the printability will be good, but it will be difficult to lower the dynamic friction coefficient.

[0063] The polyurethane resin layer may contain additives other than the organic lubricant as necessary, so long as the properties of the layer are not significantly impaired. For example, additives such as surfactants, defoamers, heat stabilizers, antioxidants, reinforcing materials, pigments, deterioration inhibitors, weather resistance agents, flame retardants, plasticizers, and mold release agents may be contained.

[0064] The thickness of the polyurethane resin layer is not particularly limited, but is usually preferably 0.005 to 0.150 μm, more preferably 0.010 to 0.150 μm, and most preferably 0.020 to 0.100 μm. If the thickness of the polyurethane resin layer is less than 0.005 μm, it is difficult to form a polyurethane resin layer with a uniform thickness on the polyamide film, making it difficult to obtain sufficient slippage. On the other hand, if the thickness of the polyurethane resin layer exceeds 0.150 μm, the slippage improvement effect of the polyurethane resin layer becomes saturated, which is economically disadvantageous.

[0065] A-3. Other layers As described above, the film of the present invention can be laminated with various layers as necessary in addition to the polyamide film and polyurethane resin layer. That is, the polyamide-based laminate film of the present invention includes a basic structure of a polyamide film and a polyurethane resin layer, and also includes a laminate in which other layers are laminated. Therefore, in this specification, a laminate in which other layers are laminated in addition to the basic structure (the laminate film) is also called a "laminate".

[0066] Such a laminate can be suitably used as a packaging laminate, for example, for food packaging, battery packaging (exterior material), etc. In addition, the film of the present invention is also suitable for cold forming (for example, at a forming temperature of 50° C. or less) as a laminate for cold forming, and therefore can also be applied to a manufacturing method of a molded product including a step of cold forming the film of the present invention. Thus, the present invention includes a polyamide-based laminate film particularly used for food packaging or cold forming.

[0067] As layers other than the above basic configuration, layers similar to those employed in known packaging materials, etc., can be used. For example, a barrier layer, a primer layer, a heat-sealing layer, an adhesive layer, a clear layer, a printed layer, etc. can be mentioned. These can be similar to those in known laminates, but among these, it is desirable to set the barrier layer and the heat-sealing layer as follows.

[0068] The barrier layer has excellent barrier properties (gas barrier properties, particularly oxygen barrier properties, etc.), and examples thereof include various barrier films such as inorganic barrier layers such as known metal foils, metal vapor deposition films, transparent vapor deposition films, and organic coating layers such as polyvinyl alcohol and ethylene-vinyl alcohol copolymers. Among these, metal foils such as aluminum foil and copper foil are preferred in terms of versatility, and aluminum foil is particularly more preferred.

[0069] When a metal foil is used as the barrier layer, the thickness of the metal foil is not particularly limited, but is usually about 5 to 200 μm, more preferably 5 to 150 μm, and most preferably 7 to 50 μm.

[0070] In addition, one or both surfaces of the metal foil may be subjected to a surface treatment to improve adhesion, corrosion resistance, etc. Examples of the surface treatment include chemical conversion treatment, chromate treatment, etc. In particular, it is preferable that such a surface treatment is performed on the surface that contacts the heat-sealing layer.

[0071] The heat-sealable layer is not particularly limited as long as it is a heat-sealable layer, and known ones can be used, for example, polyvinyl chloride film, polyolefin film, etc. Examples of polyolefins include polyethylene, polypropylene, polyethylene, copolymers mainly composed of polypropylene, and acid-modified products thereof. The heat-sealable layer can be either a stretched film or a non-stretched film, and the molten resin can be directly laminated.

[0072] The thickness of the heat-sealing layer is not particularly limited, but is usually preferably 20 to 200 μm, and more preferably 30 to 100 μm.

[0073] In addition, when laminating these, for example, a known adhesive or the like can be used for lamination, but the invention is not limited to this.

[0074] In the present invention, the method of bonding the polyamide film and the metal foil can be suitably implemented by dry lamination, heat lamination, or the like using a two-liquid type urethane adhesive, for example.

[0075] As a method for bonding the metal foil and the heat-sealing layer, for example, dry lamination, heat lamination, extrusion lamination, sandwich lamination, etc. can be suitably used.

[0076] The surface of the film, metal foil or heat-sealing layer on which the adhesive layer is formed may be previously provided with an anchor coat layer, a primer layer or the like as required, so long as the effect of the present invention is not impaired.

[0077] In the present invention, when other layers are laminated, particularly by disposing a polyurethane resin layer as the outermost layer, excellent slip properties and printability are obtained, and therefore the film can be suitably used for various industrial applications, including packaging applications for food, electronic and electrical parts, etc.

[0078] As the film of the present invention, for example, a laminate including a polyurethane resin layer 12 / a polyamide film 11 / a metal foil 13 / a heat-sealing layer 14 as shown in FIG. 2A or FIG. 2B, or a laminate including a polyurethane resin layer 12 / a polyamide film 11 / a polyurethane resin layer 12 / a metal foil 13 / a heat-sealing layer 14, are effective as packaging materials including, for example, exterior materials for batteries.

[0079] B. Properties of the Film of the Invention The thickness of the film of the present invention is not particularly limited and can be appropriately set depending on, for example, the application, the method of use, etc. For example, when the film of the present invention is used as an exterior material for a battery, the thickness of the laminate 10 or 10' in Fig. 1 can be, for example, in the range of about 10 to 25 µm, and can also be, for example, in the range of 15 to 25 µm, but is not limited thereto.

[0080] In the film of the present invention, the dynamic friction coefficient of the polyurethane resin layer surface in a 20°C x 90% RH environment is usually 0.40 or less, preferably 0.35 or less, and more preferably 0.30 or less. In the film of the present invention, the lower limit of the dynamic friction coefficient in a 20°C x 90% RH environment is not particularly limited, but is usually about 0.20. If the dynamic friction coefficient in a 20°C x 90% RH environment is 0.40 or less, excellent processability and printability can be more reliably obtained even under high humidity.

[0081] Furthermore, in terms of improving formability, printability, etc., the film of the present invention has a kinetic friction coefficient of the polyurethane resin layer surface in an environment of 23°C x 50% RH of usually 0.30 or less, preferably 0.25 or less, and more preferably 0.20 or less. The lower limit of the kinetic friction coefficient in an environment of 23°C x 50% RH is not particularly limited, but is usually about 0.10.

[0082] In addition, the arithmetic average height (Ra) of the polyurethane resin layer surface of the film of the present invention calculated from two-dimensional surface roughness measurement is usually required to be 0.010 to 0.060 μm, particularly preferably 0.010 to 0.055 μm, more preferably 0.020 to 0.050 μm, and most preferably 0.010 to 0.040 μm. If the Ra exceeds 0.060 μm, the unevenness of the resin layer surface becomes large, so that printing defects may occur, making it difficult to perform high-definition printing.

[0083] Furthermore, the contact angle of water on the surface of the polyurethane resin layer of the film of the present invention is preferably 82° to 98° from the viewpoint of improving slipperiness or printability, more preferably 86° to 98°, and most preferably 90° to 98°. If the contact angle is less than 82°, frictional resistance increases, and slipperiness may decrease. If the contact angle exceeds 98°, ink adhesion may decrease, and printability may decrease. Furthermore, since the surface of the polyurethane resin layer of the film of the present invention has few irregularities, the variation in the contact angle measurement value can be suppressed.

[0084] 2. Manufacturing of polyamide laminated film The film of the present invention is, for example, a method for producing a polyamide-based laminate film comprising a polyamide film and a polyurethane resin layer containing a polyurethane resin and an organic lubricant laminated on at least one surface of the film, the method comprising the steps of: (1) a sheet forming step of forming a melt-kneaded material containing a polyamide resin into a sheet to obtain an unstretched sheet; (2) a stretching step in which the unstretched sheet is stretched in the MD and TD to obtain a biaxially stretched film; and (3) A coating step of applying an aqueous coating liquid containing a polyurethane resin and an organic lubricant onto one surface of the unstretched sheet, MD-stretched film, TD-stretched film, or biaxially stretched film. The polyamide-based laminate film can be suitably produced by a method for producing the polyamide-based laminate film, which comprises the steps of:

[0085] Sheet forming process In the sheet forming step, a melt-kneaded material containing a polyamide resin is formed into a sheet to obtain an unstretched sheet.

[0086] The unstretched sheet can be obtained by forming a melt-kneaded material containing a polyamide resin into a film shape. The preparation of the melt-kneaded material itself may be carried out according to a known method. For example, the melt-kneaded material obtained by melting a resin composition containing a polyamide resin can be formed into a film (sheet). This can be carried out by using a known or commercially available device. For example, a melt extruder having a T-die can be used. That is, first, a starting material (e.g., a pellet-shaped raw material) is supplied to a hopper, plasticized and melted in a melt extruder, and the melt-kneaded material is extruded into a sheet shape from a T-die attached to the tip of the extruder, and cooled and solidified by a cast roll. At this time, the melt-kneaded material can be pressed against a cast roll by air to obtain an unstretched sheet.

[0087] In addition to the polyamide resin, the resin composition may contain various additives as required. Examples of the additives include those that are added to polyamide films.

[0088] In this case, the average thickness of the unstretched sheet is not particularly limited, but is generally about 15 to 250 μm, and preferably 50 to 235 μm. By setting the thickness within such a range, the stretching step can be carried out more efficiently.

[0089] Stretching process In the stretching step, the unstretched sheet is stretched in the MD and TD to obtain a biaxially stretched film.

[0090] Prior to the stretching step, it is preferable to preheat the unstretched sheet or uniaxially stretched film. The preheating temperature is not limited, but is preferably set within ±50°C of the stretching temperature. Preheating can more reliably obtain a biaxially stretched film with good physical properties. The preheating time depends on the preheating temperature, etc., but is usually preferably about 0.5 to 5 seconds.

[0091] The method for preheating is not particularly limited. For example, a method in which the temperature of hot air blown onto the film traveling in the preheating zone of the stretching machine is set to within the above-mentioned temperature range can be suitably adopted.

[0092] The method for adjusting the stretching temperature to the above range is not limited, but it is preferable to set the temperature of hot air blown onto the film traveling in the stretching zone of the stretching machine to the above range. In this case, the time for which the polyamide film travels in the stretching zone is usually preferably about 0.5 to 5 seconds.

[0093] As the stretching method, when a biaxially stretched film of the present invention is finally obtained, a simultaneous biaxial stretching method or a sequential biaxial stretching method can be adopted. In addition, the stretching method can be classified according to the stretching device, for example, a tubular method, a tenter method, etc., and any of them can be applied. In the present invention, the stretching method by the tenter method is preferable in terms of quality stability and dimensional stability. Therefore, a tenter type simultaneous biaxial stretching method or a tenter type sequential biaxial stretching method can be suitably adopted. Examples of the tenter type biaxial stretching method include a pantograph type tenter, a screw type tenter, and a linear motor type tenter.

[0094] In addition, when a simultaneous biaxial stretching method is adopted as the stretching method, an aqueous coating liquid containing a urethane resin and an organic lubricant is applied to an unstretched sheet, and then the sheet is simultaneously biaxially stretched in the MD and TD directions to obtain the film of the present invention in which a urethane resin layer is formed on a predetermined biaxially stretched polyamide film.

[0095] Furthermore, when the sequential biaxial stretching method is adopted, an aqueous coating liquid containing a urethane resin and an organic lubricant is applied to a film that has been uniaxially stretched in advance in the MD direction or the TD direction, and then the film is stretched in a direction (TD direction or MD direction) approximately perpendicular to the uniaxial stretching direction to obtain the film of the present invention in which a urethane resin layer is formed on a specified biaxially stretched polyamide film.

[0096] The stretching ratio is not particularly limited, but usually it is sufficient to stretch the film in the MD direction and the TD direction to about 2.0 to 4.5 times. In this case, the stretching ratios in the MD direction and the TD direction may be the same or different. By stretching in this manner, a stretched film having good physical properties such as tensile strength and tensile elongation can be obtained.

[0097] In order to set the arithmetic mean height (Ra) of the polyurethane resin layer within the range specified in the present invention, the polyamide laminate film of the present invention must simultaneously satisfy the following conditions (a) and (b). In the following formulas (a) and (b), X represents the stretching ratio in the MD direction, and Y represents the stretching ratio in the TD direction. Furthermore, X / Y represents the stretching ratio ratio between the MD stretching ratio (X) and the TD stretching ratio (Y). X×Y represents the areal stretching ratio.

[0098] When simultaneous biaxial stretching is performed, (a) 0.80≦X / Y≦0.94 (b) 9.8≦X×Y≦11.6 It is preferable that the following is satisfied.

[0099] When sequential biaxial stretching is performed, (a) 0.85≦X / Y≦0.95 (b) 8.5≦X×Y≦9.5 It is preferable that the following is satisfied.

[0100] The stretching temperature is not limited, and can be appropriately set within a range of 225° C. or less (preferably 40 to 220° C.) depending on, for example, the stretching method, the application of the film of the present invention, and the form of use.

[0101] The film stretched in the stretching step is preferably further heat-treated. The heat treatment temperature is not particularly limited, but is usually preferably about 190 to 220°C, and more preferably 195 to 215°C. If the heat treatment temperature is less than 190°C, the film will have a large shrinkage rate, which is not preferable for packaging polyamide films. In addition, when an organic lubricant, a crosslinking agent, etc. are added, the former does not bleed out sufficiently, and the latter does not progress in the crosslinking reaction sufficiently, so that the effect of the addition may not be fully obtained. On the other hand, if the heat treatment temperature exceeds 220°C, the strength of the polyamide film decreases. In addition, if the bleed out of the organic lubricant or the progress of the crosslinking reaction of the crosslinking agent is insufficient in the above heat treatment, an aging treatment may be performed after the completion of stretching. In addition, the heat treatment time can be appropriately set depending on the heat treatment temperature, etc., but it is usually preferable to set it to about 1 to 15 seconds.

[0102] The heat treatment method is not particularly limited, and may be, for example, a method of blowing hot air, a method of irradiating infrared rays, a method of irradiating microwaves, etc. Among these, a method of blowing hot air is preferred from the viewpoint of uniform and accurate heating. For example, the heat setting treatment can be performed by blowing hot air set to the above-mentioned temperature range onto the film traveling in the heat setting zone of the stretching machine.

[0103] Coating process In the coating step, an aqueous coating liquid containing a polyurethane resin and an organic lubricant is applied onto one surface of the unstretched sheet, MD-stretched film, TD-stretched film, or biaxially stretched film.

[0104] The aqueous coating liquid can be prepared by dissolving or dispersing the polyurethane resin and the organic lubricant in an aqueous medium. By using an aqueous coating liquid, the desired film of the present invention can be efficiently obtained, and it is also advantageous in terms of workability, environmental friendliness, etc.

[0105] In the present invention, the aqueous medium is water or a mixed solvent mainly composed of water (usually a liquid containing 50% by mass or more of water). As the mixed solvent, a mixed solvent of water and a water-soluble organic solvent can be used. The water-soluble organic solvent is not limited, and examples thereof include alcohols such as methanol, ethanol, and isopropanol, and ketones such as acetone and methyl ethyl ketone (MEK). One or more kinds of water-soluble organic solvents can be used. By mixing a water-soluble organic solvent, effects such as increasing the wettability of the polyamide film and shortening the drying process can be obtained. In this respect, even when additives such as a crosslinking agent are used in addition to polyurethane resins, it is preferable that these additives are aqueous (aqueous solution or aqueous dispersion (emulsion)).

[0106] In preparing the water-based coating fluid, the order of mixing the components such as the polyurethane resin, the organic lubricant, and the water-based medium is not limited, and the water-based coating fluid can be suitably prepared, for example, by adding the organic lubricant to a previously prepared aqueous dispersion or solution of the polyurethane resin. This method will be described below as a representative example.

[0107] The polyurethane resin used in the water-based coating liquid is not particularly limited, but as described above, it is preferable to use a polyurethane resin having an anionic functional group introduced therein (anionic polyurethane resin). By using an anionic polyurethane resin, it is possible to disperse the polyurethane resin more uniformly and stably in water. Thus, in the present invention, it is preferable to prepare the coating liquid by using the polyurethane resin in the form of an aqueous dispersion.

[0108] Furthermore, when dispersing an anionic polyurethane resin in an aqueous medium, it is generally preferred to use a volatile base. The volatile base is not particularly limited, and any known base can be used. More specifically, ammonia, methylamine, ethylamine, dimethylamine, diethylamine, triethylamine, morpholine, ethanolamine, etc. are exemplified. Among these, triethylamine is more preferred in that the liquid stability of the water-dispersible polyurethane resin is good, and furthermore, the boiling point is relatively low, so that the amount of residue in the primer layer is small.

[0109] The aqueous dispersion of such polyurethane resin may be a known or commercially available one. Examples of commercially available anionic water-dispersible polyurethane resins include "Takelac W-5030", "Takelac WS-4000", and "Takelac WS-4022" manufactured by Mitsui Chemicals Polyurethanes, Inc., and "Hydran AP40F" manufactured by DIC Corporation.

[0110] Next, an organic lubricant is added and mixed into the aqueous dispersion of polyurethane resin. The type and amount of the organic lubricant may be the same as those described above. In this case, the organic lubricant may be dispersed in a solvent (water or solvent) or may be used alone (powder). In particular, in the present invention, it is preferable to use the organic lubricant in the form of a dispersion (e.g., aqueous dispersion) obtained by dispersing the organic lubricant in a solvent. Therefore, it is desirable that the aqueous coating liquid is a mixture of a dispersion of polyurethane resin and a dispersion of organic lubricant.

[0111] In this case, the particle size of the organic lubricant in the dispersion is not particularly limited, but is usually preferably about 0.010 μm to 0.500 μm, more preferably 0.010 μm to 0.400 μm, and even more preferably 0.010 μm to 0.200 μm, and most preferably 0.010 μm to 0.100 μm. If the particle size is smaller than 0.010 μm, the organic lubricant is very finely dispersed in the polyurethane resin layer, improving printability, but reducing the effect of reducing the dynamic friction coefficient. On the other hand, if the particle size exceeds 0.500 μm, the organic lubricant is likely to aggregate, reducing printability, although it can achieve the effect of reducing the dynamic friction coefficient.

[0112] The particle size of the organic lubricant in the dispersion liquid indicates the median size obtained by a laser diffraction / scattering method (dispersion medium: water) based on the Mie theory using a laser diffraction particle size distribution measuring device (product name "Mastersizer 3000" manufactured by MalVern Instruments LTD). In this case, the refractive index of the dispersion medium (water) was set to 1.330. The refractive index of the organic lubricant was set to 1.500 for polyethylene wax, 1.59 for silicone-acrylic copolymer, 1.49 for silicone-urethane copolymer, and 1.46 for fatty acid amide.

[0113] The mixing of the polyurethane resin and the organic lubricant is not particularly limited as long as the organic lubricant can be uniformly dispersed, and can be carried out using a known or commercially available mixing device such as a mixer or kneader. In particular, in the present invention, heating can be appropriately performed, and the mixing can be suitably carried out using a dissolving kettle equipped with a stirrer. The mixing temperature is not particularly limited, and can be, for example, about 5 to 40°C.

[0114] In addition to the polyurethane resin and the organic lubricant, the water-based coating liquid may contain other components within the range that does not impair the effects of the present invention. For example, the various additives exemplified above can be blended.

[0115] As the additive, in the present invention, a surfactant can be added for the purpose of improving the coatability to the polyamide film. The surfactant is not particularly limited, but examples thereof include anionic surfactants such as polyethylene alkyl phenyl ether, polyoxyethylene fatty acid ester, glycerin fatty acid ester, fatty acid metal soap, alkyl sulfate, alkyl sulfonate, and alkyl sulfosuccinate, as well as nonionic surfactants such as acetylene glycol.

[0116] The content of the surfactant is not particularly limited, but it is generally preferred that the surfactant be contained in the aqueous coating liquid in an amount of 0.01 to 1% by mass, and it is also preferred that the surfactant be one that volatilizes during heat treatment in the production process of the polyamide-based laminate film.

[0117] The solid content concentration of the aqueous coating liquid can be appropriately adjusted, for example, depending on the specifications of the coating device and drying / heat treatment device used. However, a coating liquid that is too dilute is likely to cause problems such as a long drying time and an increase in the risk of defects due to the coating thickness being too thin after drying, making it difficult to form a uniform coating. On the other hand, an aqueous coating liquid that is too concentrated is likely to cause problems in coatability, with the coated surface being difficult to achieve uniformity. Therefore, from this perspective, the solid content concentration of the aqueous coating liquid is generally preferably about 5 to 70 mass%.

[0118] The method of applying the aqueous coating liquid to the polyamide film is not particularly limited, and any known method can be appropriately adopted, such as gravure roll coating, reverse roll coating, wire bar coating, air knife coating, curtain coating, doctor knife coating, die coating, dip coating, bar coating, or a combination of these methods.

[0119] The drying step after coating is not particularly limited, and can be performed using a known method, such as drying in a dry atmosphere such as an oven, drying by contact with a heated roll, drying in a stretching machine, etc. The drying temperature is not limited, but can usually be set within a range of about 30 to 200° C. The drying time can be appropriately set depending on the drying temperature, etc., but can generally be set within a range of 0.5 to 60 seconds.

[0120] The timing of coating the aqueous coating liquid may be any timing as long as the aqueous coating liquid can be coated on one surface of the unstretched sheet, MD stretched film, TD stretched film, or biaxially stretched film. In other words, any method such as in-line coating method or post-coating method (off-line coating method) can be adopted.

[0121] In particular, in the present invention, by adopting the in-line coating method, the film thickness can be made thinner and more uniform than in the offline coating method, and the productivity is improved, so that it is possible to manufacture high-quality products at low cost. In particular, when the in-line coating method is adopted, both the slipperiness and printability can be improved. Although the reason is not clear, it is considered that the slipperiness and printability are improved by performing heat treatment simultaneously with stretching in the in-line coating method, which orients the molecular chains of the polyurethane resin, promotes the crosslinking reaction, or promotes the bleeding out of the organic lubricant. In particular, it is possible to unevenly distribute the organic lubricant on the surface of the stretched film by bleeding out the organic lubricant, and it is presumed that even a relatively small amount of the organic lubricant can modify the stretched film to have a slippery property.

[0122] The in-line coating method is not particularly limited as long as the formation of a coating film with an aqueous coating liquid and the stretching of the film can be carried out substantially simultaneously, and examples thereof include a) a method in which an aqueous coating liquid is applied to an unstretched sheet, followed by sequential or simultaneous biaxial stretching, b) a method in which an aqueous coating liquid is applied to an MD-stretched uniaxially stretched film, followed by TD stretching, and c) a method in which an aqueous coating liquid is applied to a TD-stretched uniaxially stretched film, followed by MD stretching, etc. In contrast, the post-coating method is a method in which a coating film with an aqueous coating liquid is formed on a film after biaxial stretching.

[0123] A preferred embodiment of the in-line coating method in the case of simultaneous biaxial stretching is a method including a step of forming a polyamide resin into a sheet and applying an aqueous coating liquid after a sheet forming step of obtaining an unstretched polyamide sheet. The unstretched polyamide sheet coated with the aqueous coating liquid is preferably dried at 50 to 220°C, preferably 80 to 180°C, more preferably 120 to 160°C in a drying step, and then simultaneously biaxially stretched at a stretching temperature of 215°C or less (preferably 190 to 215°C) and at a stretching ratio of 2.5 to 3.8 times in both MD and TD directions. The method of simultaneously biaxially stretching the unstretched polyamide sheet can be performed by a known stretching method. Among them, it is preferable to perform the simultaneous biaxial stretching by tenter type simultaneous biaxial stretching or Lisim simultaneous biaxial stretching method from the viewpoint of economic efficiency such as productivity.

[0124] A preferred embodiment of the in-line coating method in the case of sequential biaxial stretching includes a method including the following steps. After a sheet forming step in which a polyamide resin is formed into a sheet to obtain an unstretched sheet, the unstretched sheet is stretched 2.5 to 3.5 times in the machine direction of the sheet at a stretching temperature of 40 to 80°C (preferably 50 to 65°C) (MD stretching), and then an aqueous coating liquid is applied to the uniaxially stretched polyamide film. The uniaxially stretched film coated with the aqueous coating liquid is stretched 2.5 to 3.5 times in the width direction at a preheating and stretching temperature of 50 to 220°C (preferably 60 to 130°C) in a stretching step that also serves as a drying step, thereby making it possible to produce the film of the present invention. When performing sequential biaxial stretching, it is preferable to use a combination of a roll stretching method and a tenter type stretching method. More specifically, successive biaxial stretching can be suitably performed by carrying out MD stretching by roll stretching and then carrying out TD stretching by tenter stretching.

[0125] Other processes The method for laminating each layer is not particularly limited, and any of a) a method for forming a coating film using a coating liquid, b) a method for laminating a preformed film, and c) a method for forming a vapor deposition film by a PVD method, a CVD method, etc. can be used. In the case of b), any of a method for laminating via an adhesive and a method for laminating by coextrusion molding can be used. In particular, when the film of the present invention is used as an exterior material for a battery such as a lithium ion secondary battery, a known method for manufacturing an exterior material can also be used. In this case, it is also possible to laminate using a known adhesive.

[0126] For example, when laminating with a barrier layer, a method such as dry lamination or heat lamination can be used in which a laminate including a urethane resin layer / polyamide film or a laminate including a urethane resin layer / polyamide film / urethane resin layer is bonded to a metal foil or the like for forming a barrier layer via a two-liquid urethane-based adhesive or the like.

[0127] The barrier layer and the heat-sealing layer can be joined together by known methods (dry lamination, heat lamination, extrusion lamination, sandwich lamination, etc.).

[0128] An anchor coat layer, a primer layer, a printed layer, a clear layer, etc. may be provided on the surface of the polyamide film, the barrier layer, or the heat-sealing layer on which the adhesive layer is formed, as necessary, as long as the effects of the present invention are not impaired.

[0129] 3. Use of polyamide laminate film The film (or laminate) of the present invention can be used for various purposes, but is particularly suitable for use as a packaging material. That is, it can be used as a packaging material for packaging contents. The contents are not limited, and can include, for example, foods and beverages, electronic parts, chemical products, cosmetics, medical products (medical devices), and the like.

[0130] The form of the packaging material is not particularly limited, and the material can be used, for example, as a packaging bag or a packaging container. As the packaging bag, the material can be used in various bag shapes such as a pillow bag, a gusset bag, a stand bag, etc. The bag shape can be formed according to a known method.

[0131] Furthermore, the present invention also includes a product (packaged product) in which the contents are packaged in the above-mentioned packaging material or packaging bag. In this case, the packaged state may be, for example, a state in which the contents are sealed from the outside by the packaging material or packaging bag. EXAMPLES

[0132] The features of the present invention will be described in more detail below with reference to examples and comparative examples. However, the scope of the present invention is not limited to the examples. In addition, "%" regarding weight or concentration described below means "% by mass".

[0133] 1. Materials used (1) Polyurethane resin As the polyurethane resin, the following polyurethane water dispersions (a) to (d) were used. (a) Product name: Hydran AP40F (DIC Corporation, glass transition temperature: 55°C, solid content: 25%) (b) Product name: "Takelac W-5030" (manufactured by Mitsui Chemicals, Inc., glass transition temperature 85°C, solid content 30%) (c) Product name: "Takelac WS-4022" (manufactured by Mitsui Chemicals, Inc., glass transition temperature 115°C, solid content 30%) (d) Product name: Hydran AP-201 (manufactured by DIC, glass transition temperature 7°C, solid content 25%)

[0134] (2) Organic lubricants The following organic lubricants (a) to (g) were used, all of which were in the form of a dispersion liquid. (a) Product name: "AQUACER517" (BYK, polyethylene wax, solid content 35%, particle size 0.150 μm, melting point 120°C) (b) Product name: "Hi-Tech E6400" (manufactured by Toho Chemical Industry Co., Ltd., polyethylene wax, solid content concentration 35%, particle size 0.050 μm, melting point 120°C) (c) Product name: "Chaline E E-370" (manufactured by Nissin Chemical Industry Co., Ltd., silicone-acrylic copolymer, solid content concentration 50%, particle size 0.450 μm) (d) Product name: "Simac US-450" (manufactured by Toagosei Co., Ltd., silicone-acrylic copolymer, solid content concentration 30%, particle size 0.350 μm) (e) Product name: "Chaline E RU-911" (manufactured by Nissin Chemical Industry Co., Ltd., silicone-urethane copolymer, solid content concentration 40%, particle size 0.330 μm) (f) Product name: "Alflow H-50ES" (manufactured by NOF Corporation, fatty acid amide, solid content concentration 42%, particle size 0.450 μm, melting points 113°C, 147°C) (g) Product name: "Slipax E SA-20" (manufactured by Mitsubishi Chemical Corporation, fatty acid amide, solid content concentration 22%, particle size 0.460 μm, melting point 113°C, 147°C)

[0135] (3) Other additives As other additives, the following (a) and (b) were used. (a) Product name: Aerosil 200 (manufactured by Nippon Aerosil Co., Ltd., silica particles, primary particle diameter 12 nm) (b) Product name "MX100W" (manufactured by Nippon Shokubai, acrylic particles, average particle diameter 150 nm)

[0136] 2. Examples and Comparative Examples Example 1 (1) Preparation of coating solution The polyurethane water dispersion "HYDRAN AP40F" and the organic lubricant "AQUACER 515" were mixed in this order into water so that the solid content concentration was 9% by mass, and stirred to obtain a water-based coating solution A. The "HYDRAN AP40F" and "AQUACER 515" were weighed so that the solid content mass ratio was HYDRAN AP40F / AQUACER 515=100 / 20. (2) Manufacturing of polyamide laminated film (sequential biaxial stretching) Using an extruder equipped with a T-die, nylon 6 (Unitika, A1030BRF, relative viscosity 3.1) was extruded into a sheet from the T-die, and then brought into close contact with a casting roll whose surface temperature was adjusted to 18°C ​​and quenched to obtain an unstretched sheet. Next, this unstretched sheet was passed through a stretching roll heated to a preheat temperature of 58°C and a stretching temperature of 61°C, and stretched in the MD direction to a stretch ratio of 2.85 times to obtain an MD stretched film. Next, an aqueous coating solution A with a solid content concentration of 9% by mass was applied to the MD stretched film so that the thickness after drying and stretching was 0.10 μm, and then stretched in the TD direction at a stretch ratio of 3.20 times under conditions of a preheat temperature of 80°C and a stretching temperature of 120°C. Furthermore, after heat treatment was performed under conditions of a heat treatment temperature of 210°C and a heat treatment time of 3 seconds, a 3% relaxation treatment was performed in the TD direction. The polyamide film surface of the obtained laminated film was subjected to a corona treatment to obtain a polyamide-based laminated film (thickness 15 μm) on which a polyurethane resin layer having a thickness of 0.10 μm was laminated. (3) Preparation of the laminate A two-component polyurethane adhesive (TM-K55 / CAT-10L, manufactured by Toyo-Morton Co., Ltd.) was applied at a rate of 5 g / m to the corona-treated surface of the obtained polyamide laminate film. 2 and dried for 10 seconds at 80° C. An aluminum foil (thickness: 50 μm) was attached to the adhesive-coated surface. Next, the above adhesive was applied to the aluminum foil surface under the same conditions and dried, and an unstretched polypropylene film (Mitsui Chemicals Tocello, GHC, thickness 50 μm) was laminated as a heat-sealing layer, and aging treatment was carried out for 7 days in an atmosphere of 60°C to obtain a laminate laminated in the following order: polyurethane resin layer / polyamide film / adhesive layer / aluminum foil / heat-sealing layer.

[0137] Examples 2, 5 to 17 and Comparative Examples 1 to 2, 4, 7 A polyamide-based laminate film was produced in the same manner as in Example 1, except that the conditions shown in Table 1 were used. A coating liquid was prepared in the same manner as in Example 1, except that the types and blending ratios of the polyurethane water dispersion and the organic lubricant were changed as shown in Table 1. Note that the order of addition of the organic lubricants in a coating liquid containing two types of organic lubricants is not limited and can be selected arbitrarily. Furthermore, a laminate was produced in the same manner as in Example 1 using the obtained polyamide-based laminate film.

[0138] Example 3 A polyamide-based laminate film was produced in the same manner as in Example 1, except that the stretching method was changed as follows. Using an extruder equipped with a T-die, nylon 6 (Unitika, A1030BRF, relative viscosity 3.1) was extruded into a sheet from the T-die, and then brought into close contact with a casting roll whose surface temperature was adjusted to 18°C ​​and quenched to obtain an unstretched sheet. Next, this unstretched sheet was coated with aqueous coating solution B having a solid content concentration of 9% by mass using a gravure coater so that the thickness after drying and stretching would be 0.10 μm, and after drying with a hot air dryer, it was introduced into a pantograph-type tenter simultaneous biaxial stretching machine and simultaneously biaxially stretched at a stretch ratio of 3.0 times in the MD direction and 3.3 times in the TD direction under conditions of a preheating stretching temperature of 200° C. Further, it was subjected to a heat treatment under conditions of a heat treatment temperature of 215° C. and a heat treatment time of 3 seconds, and then subjected to a 3% relaxation treatment in the TD direction. The polyamide film surface of the obtained laminate film was subjected to corona treatment to obtain a 15 μm thick polyamide laminate film on which a 0.10 μm thick polyurethane resin layer was laminated. Further, a laminate was produced in the same manner as in Example 1 using the obtained polyamide laminate film.

[0139] Example 4 A polyamide-based laminate film was obtained in the same manner as in Example 3, except that the simultaneous biaxial stretching machine was changed from a pantograph-type tenter to a linear motor-type tenter and a 1% relaxation treatment was also performed in the MD direction. Furthermore, a laminate was produced in the same manner as in Example 1 using the obtained polyamide-based laminate film.

[0140] Comparative Example 3 A polyamide-based laminate film was produced in the same manner as in Example 1, except that the aqueous coating liquid contained 2.0% by mass of silica relative to 100% by mass of the solid content of the polyurethane aqueous dispersion. Furthermore, a laminate was produced in the same manner as in Example 1 using the obtained polyamide-based laminate film.

[0141] Comparative Example 5 A polyamide-based laminate film was obtained in the same manner as in Example 1, except that the coating process of the aqueous coating liquid was changed from during the stretching process to after the stretching process. In the coating process, the stretched polyamide film was introduced into a gravure coater, and the aqueous coating liquid R was applied to the film so that the coating thickness was 0.5 μm. The film was then dried through a drying furnace consisting of five zones: Zone 1 (80°C) → Zone 2 (100°C) → Zone 3 (120°C) → Zone 4 (110°C) → Zone 5 (80°C). A polyamide-based laminate film was obtained by drying the film through the drying furnace. Furthermore, a laminate was produced in the same manner as in Example 1 using the obtained polyamide-based laminate film.

[0142] Comparative Example 6 A polyamide-based laminate film was produced in the same manner as in Example 1, except that the aqueous coating liquid contained 2.0% by mass of acrylic particles relative to 100% by mass of the solid content of the polyurethane aqueous dispersion. Furthermore, a laminate was produced in the same manner as in Example 1 using the obtained polyamide-based laminate film.

[0143] [Table 1]

[0144] Test Example 1 The polyamide-based laminate films or laminates obtained in the respective Examples and Comparative Examples were measured for the following properties, and the results are shown in Table 2.

[0145] (1) Coefficient of kinetic friction The dynamic friction coefficient of the polyurethane resin layer surface in the present invention was measured according to the Japanese Industrial Standard "JIS K7125". The measuring device used was a tabletop material testing machine "STB-1225S" manufactured by A&D Co., Ltd., and a data processing system "TACT", and the measurement environment was 23°C x 50% RH and 20°C x 90% RH. Specifically, the polyamide laminate film sample was humidified at 23°C x 50% RH or 20°C x 90% RH for 2 hours, and then the polyurethane resin layers of the polyamide laminate film were overlapped and measured under the same temperature and humidity as above. In the case of a laminate including the film of the present invention as the outermost layer, the surface of the polyurethane resin layer that is the outermost layer was used as the measurement surface, and the measurement was performed in the same manner as above. In practical terms, the dynamic friction coefficient is required to be 0.30 or less at 23°C x 50% RH and 0.40 or less at 20°C x 90% RH. The measurement was performed with n=5, and the average value was taken as the measured value.

[0146] (2) Arithmetic mean height (Ra) The arithmetic mean height measurement (Ra) in the present invention was performed in accordance with the Japanese Industrial Standard "JIS B 0601" using a contact surface roughness measuring instrument "Surfcorder SE500A" manufactured by Kosaka Laboratory Co., Ltd. Specifically, a sample of a polyamide laminated film was conditioned at 23°C x 50% RH for 2 hours, and then the surface of the polyurethane resin layer was measured under the same temperature and humidity as above. In the case of a laminate including the film of the present invention as the outermost layer, the surface of the polyurethane resin layer that is the outermost layer was used as the measurement surface. The measurement was performed with n=5, and the average value was used as the measured value.

[0147] (3) Contact angle The contact angle was measured using water with a KRUSS automatic contact angle meter, model DSA30S. Specifically, the polyamide laminate film sample was conditioned at 23°C x 50% RH for 2 hours, and then the measurement was carried out under the same temperature and humidity as above. The measurement was carried out with n=5, and the average value was taken as the measured value.

[0148] (4) Printability (ink transfer from the plate) The printability in the present invention was measured under the same temperature and humidity conditions after conditioning a polyamide laminate film sample at 23°C x 50% RH for 2 hours. A dot pattern was printed on the polyurethane resin layer of the polyamide laminate film using a gravure printing method so that there were 100 dots within a 1 cm x 1 cm area, and the number of defects in the dot pattern within a 1 cm x 1 cm area was counted, and the average value of three locations was calculated to evaluate the printability. As the ink, a commercially available ink (Rio Alpha R39 Indigo, manufactured by Toyo Ink Co., Ltd.) was used. With regard to printability, in practical terms, it is preferable that the number of defects in the dot pattern is 7.0 or less, more preferably 3.5 or less, and most preferably 1.0 or less.

[0149] (5) Formability of laminate (Erichsen test) Based on the Japanese Industrial Standard "JIS Z 2247," a laminate sample that had been conditioned at 23°C x 50% RH for 2 hours was measured at the same temperature and humidity as above using an Erichsen tester (Yasuda Seiki Seisakusho No. 5755). A steel ball punch was pressed into the polyurethane resin layer surface of the laminate sample to a specified depth to obtain the Erichsen value, and the moldability was evaluated according to the following evaluation criteria. The Erichsen value was measured every 0.5 mm. For practical purposes, the Erichsen value is preferably 5.0 mm or more, more preferably 8.0 mm or more, and most preferably 9.0 mm or more. The measurement was performed with n=5, and the average value was taken as the measured value.

[0150] [Table 2]

[0151] As is clear from the results in Table 2, the polyamide-based laminate films of each example have a small dynamic friction coefficient on the polyurethane resin layer surface in an environment of 20°C x 90% RH, and are therefore equipped with good printability and formability. In the polyamide laminate films described in Comparative Examples 1 to 3, the glass transition temperature of the polyurethane water dispersion was less than 50°C, so the dynamic friction coefficient of the polyurethane resin layer surface was large. In addition, the polyamide laminate film described in Comparative Example 4 did not contain an organic lubricant, and Comparative Example 5 adopted a post-coating method, so sufficient slipperiness was not obtained. In Comparative Example 6, the dynamic friction coefficient of the polyurethane resin layer surface was small by adding acrylic particles, but the arithmetic mean height Ra exceeded the range specified in the present invention, and the printability and moldability were poor. In Comparative Example 7, although the glass transition temperature was 50°C or higher, the dynamic friction coefficient of the polyurethane resin layer surface was high because no organic lubricant was added.

Claims

1. A laminated film comprising a polyamide film and a polyurethane resin layer laminated on at least one surface of the film, the polyurethane resin layer containing 5 to 30 parts by mass of an organic lubricant per 100 parts by mass of a polyurethane resin, (1) The glass transition temperature of the polyurethane resin is 90° C. or higher, (2) The arithmetic mean height (Ra) of the surface of the polyurethane resin layer is 0.010 to 0.022 μm, and the dynamic friction coefficient of the surface of the polyurethane resin layer in an environment of 20° C.×90% RH is 0.27 or less. A polyamide-based laminate film characterized by:

2. 2. The polyamide-based laminate film according to claim 1, wherein the dynamic friction coefficient of the surface of the polyurethane resin layer in an environment of 23° C.×50% RH is 0.30 or less.

3. 2. The polyamide-based laminate film according to claim 1, wherein the polyurethane resin layer has a thickness of 0.005 to 0.150 μm.

4. A food packaging laminate comprising the polyamide laminate film according to any one of claims 1 to 3.

5. A laminate for cold forming comprising the polyamide-based laminate film according to any one of claims 1 to 3.

6. A method for producing a polyamide-based laminate film comprising: a polyamide film; and a polyurethane resin layer on at least one surface of the film, the polyurethane resin layer comprising 5 to 30 parts by mass of an organic lubricant per 100 parts by mass of a polyurethane resin having a glass transition temperature of 90° C. or higher; the polyurethane resin layer has a surface arithmetic mean height (Ra) of 0.010 to 0.022 μm; and the polyurethane resin layer has a surface dynamic friction coefficient of 0.27 or less in an environment of 20° C. and 90% RH, (1) a sheet forming step of forming a melt-kneaded material containing a polyamide resin into a sheet shape to obtain an unstretched sheet; (2) a stretching step in which the unstretched sheet is stretched in the MD and TD to obtain a biaxially stretched film; and (3) A coating step of applying an aqueous coating liquid containing a polyurethane resin and an organic lubricant onto one surface of the unstretched sheet, the MD stretched film, or the TD stretched film. A method for producing a polyamide-based laminate film, comprising:

7. 7. The method according to claim 6, wherein the water-based coating liquid is a mixture of a dispersion of a polyurethane resin and a dispersion of an organic lubricant having a particle size of 0.010 μm to 0.500 μm.

8. The stretching step is carried out by simultaneous biaxial stretching and is represented by the following formulas (a) and (b): (a) 0.80≦X / Y≦0.95 (b) 9.8≦X×Y≦11.6 (wherein X represents the stretch ratio in the MD direction, and Y represents the stretch ratio in the TD direction.) The method according to claim 6, which satisfies both of the above.

9. The stretching step is carried out by sequential biaxial stretching and is represented by the following formulas (a) and (b): (a) 0.85≦X / Y≦0.95 (b) 8.5≦X×Y≦9.5 (wherein X represents the stretch ratio in the MD direction, and Y represents the stretch ratio in the TD direction.) The method according to claim 6, which satisfies both of the above.

Citation Information

Patent Citations

  • Laminated polyamide film and its manufacture

    JP1997248886A

  • Laminated polyamide film and its manufacture

    JP1997248887A

  • Biaxially oriented polyamide film

    JP2002348465A

  • Laminated polyamide film

    JP2006123465A

  • Battery case packaging material for cold molding