Neutron shielding materials and containers for storing radioactive materials

The use of an olefin copolymer rubber-based neutron shielding material with a brominated flame retardant and optional boron-based compound enhances neutron shielding and self-extinguishing properties in storage containers for radioactive substances, addressing performance gaps in conventional materials.

JP7568602B2Active Publication Date: 2024-10-16KOBE STEEL LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021200353
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-12-09
Publication Date
2024-10-16
Estimated Expiration
2041-12-09

AI Technical Summary

Technical Problem

Conventional neutron shielding materials and storage containers for radioactive substances lack sufficient neutron shielding performance and self-extinguishing properties.

Method used

A neutron shielding material composed of olefin copolymer rubber, crosslinked with an organic peroxide and containing a brominated flame retardant, with a specific ratio of brominated flame retardant to olefin copolymer rubber, and optionally including a boron-based compound, is used in the storage container.

Benefits of technology

The material provides enhanced neutron shielding and self-extinguishing properties, reducing secondary gamma ray generation and preventing corrosion, while maintaining high hydrogen content for effective neutron shielding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568602000004
    Figure 0007568602000004
  • Figure 0007568602000005
    Figure 0007568602000005
  • Figure 0007568602000006
    Figure 0007568602000006
Patent Text Reader

Abstract

To provide a neutron shielding material having high neutron shielding performance and self-digestion performance.SOLUTION: A neutron shielding material is used in a storage container 100 for radioactive substances. A main material of the neutron shielding material is olefinic copolymer rubber. The olefinic copolymer rubber is molded using an organic peroxide as a cross-linking agent. The neutron shielding material contains a brominated flame retardant. An amount of the brominated flame retardant compounded with respect to 100 pts.wt. of the olefinic copolymer rubber is 45 pts.wt. or more and 55 pts.wt. or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a neutron shielding material and a storage container for radioactive materials. [Background technology]

[0002] Patent Documents 1 and 2 describe neutron shielding materials used in nuclear facilities and the like, and neutron shielding materials used in analytical instruments or medical instruments. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 57-173795 [Patent Document 2] Japanese Patent Application Publication No. 9-33691 Summary of the Invention [Problem to be solved by the invention]

[0004] There is a demand for improving the neutron shielding performance and self-extinguishing properties of neutron shielding materials.

[0005] An object of the present invention is to provide a neutron shielding material having higher performance such as neutron shielding performance and self-extinguishing property than conventional neutron shielding materials. Another object of the present invention is to provide a storage container for radioactive materials having higher performance such as neutron shielding performance than conventional neutron shielding materials. [Means for solving the problem]

[0006] The neutron shielding material disclosed in this specification is a neutron shielding material used in containers for storing radioactive materials, wherein the main material of the neutron shielding material is an olefin-based copolymer rubber, the olefin-based copolymer rubber is molded using an organic peroxide as a cross-linking agent, the neutron shielding material contains a bromine-based flame retardant, and the number of parts of the bromine-based flame retardant per 100 parts by weight of the olefin-based copolymer rubber is 45 parts by weight or more and 55 parts by weight or less.

[0007] The radioactive material storage container disclosed in this specification is a radioactive material storage container in which the above-mentioned neutron shielding material is installed on at least one of the side, lid, and bottom of the storage container. Effect of the Invention

[0008] It is possible to provide a neutron shielding material having higher neutron shielding performance, self-extinguishing properties, etc. than conventional neutron shielding materials. It is possible to provide a storage container for radioactive materials having higher neutron shielding performance, etc. than conventional neutron shielding materials. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a schematic diagram showing the configuration of a storage container for radioactive materials. [Diagram 2] FIG. 1 is a graph showing the relationship between boron carbide (B4C) content and dose equivalent rate. [Diagram 3] FIG. 1 is a graph showing the relationship between boron carbide (B4C) content and dose equivalent rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Preferred embodiments of the present invention will now be described.

[0011] The neutron shielding material according to the present embodiment is a neutron shielding material used in a storage container for radioactive materials. The neutron shielding material according to the present embodiment is a neutron shielding material whose main material is an olefin-based copolymer rubber. The olefin-based copolymer rubber is molded using an organic peroxide as a crosslinking agent. The neutron shielding material contains a bromine-based flame retardant.

[0012] The olefin copolymer rubber is a copolymer rubber of two or more kinds of ethylene and olefins other than ethylene. The olefin copolymer rubber may be a binary copolymer containing two different structural units, a ternary copolymer containing three different structural units, or a copolymer containing four or more different structural units. Examples of olefins include propylene, butadiene, isoprene, and dienes (diolefins). The main material of the neutron shielding material being an olefin copolymer rubber means, for example, that the content of the olefin copolymer rubber is 50% by weight or more relative to 100% by weight of the neutron shielding material.

[0013] Olefin copolymer rubber contains hydrogen. Neutrons are elastically scattered by hydrogen, slowing them down and shielding them. Because olefin copolymer rubber contains a lot of hydrogen, which slows down neutrons, using olefin copolymer rubber as the main material increases the neutron shielding effect.

[0014] The olefin copolymer rubber is not particularly limited, but examples thereof include ethylene-propylene-diene rubber (EPDM) and ethylene-propylene rubber (EPM). The density of ethylene-propylene-diene rubber (EPDM) and ethylene-propylene rubber (EPM) is 0.86 to 0.87 g / cm 3 Its density is smaller than other rubbers (natural rubber, chloroprene rubber (CR), butyl rubber (IIR), polyurethane rubber, silicone rubber, etc.). Therefore, by using ethylene-propylene-diene rubber (EPDM) or ethylene-propylene rubber (EPM) as the main material, it is possible to reduce the weight of neutron shielding materials. In addition, ethylene-propylene rubber (EPM) is expected to have a greater neutron shielding effect because it contains a large amount of hydrogen.

[0015] In this embodiment, an organic peroxide is used as a crosslinking agent for the olefin copolymer rubber. Sulfur may be used as a crosslinking agent, but when sulfur is used, unreacted sulfur that does not contribute to the crosslinking reaction may remain in the rubber. The remaining sulfur may be generated as a corrosive gas such as sulfur dioxide. Such gases may combine with a small amount of moisture generated from the neutron shielding material to produce sulfite ions (SO3 - ), which is then further oxidized to sulfate ions (SO4 2- ) may be generated and cause corrosion of surrounding metal materials. In the present embodiment, since an organic peroxide is used as the crosslinking agent instead of sulfur, corrosive gases such as sulfur dioxide are not generated. Therefore, corrosion of surrounding metal materials can be suppressed.

[0016] The organic peroxide used as the crosslinking agent is not particularly limited. For example, 1,1-di(t-hexylperoxy)cyclohexane, 1,1-di(t-butylperoxy)cyclohexane, n-butyl 4,4-di(t-butylperoxy)valerate, dicumyl peroxide, α,α'-di(t-butylperoxy)diisopropylbenzene, t-butyl cumyl peroxide, 2,5-dimethyl 2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, etc. may be used as the organic peroxide.

[0017] The neutron shielding material contains a bromine-based flame retardant in addition to the olefin copolymer. A bromine-based flame retardant is a flame retardant that contains bromine atoms. The amount of the bromine-based flame retardant is 45 to 55 parts by weight per 100 parts by weight of the olefin copolymer rubber.

[0018] By including the bromine-based flame retardant in the above-mentioned blending parts, even if the neutron shielding material burns, it does not continue to burn. In addition, since the ratio of the olefin copolymer rubber, which is the main material in the neutron shielding material, is unlikely to decrease, the ratio of hydrogen in the neutron shielding material does not decrease very much. This makes it possible to provide a neutron shielding material that has self-extinguishing properties while maintaining neutron shielding properties.

[0019] The bromine-based flame retardant is not particularly limited. Examples of the bromine-based flame retardant include 1,2-bis(2,3,4,5,6-pentabromophenyl)ethane, 1,2-bis(2,4,6-tribromophenoxy)ethane, 2,4,6-tris(2,4,6-tribromophenoxy)-1,3,5-triazine, 2,4-dibromophenol, 2,6-dibromophenol, decabromodiphenyl ether, tetrabromophthalimide, and dibromopropyl ether.

[0020] The neutron shielding material may contain one or more types of bromine-based flame retardants. When the neutron shielding material contains multiple types of bromine-based flame retardants, the total blending parts of the multiple types of bromine-based flame retardants is 45 parts by weight or more and 55 parts by weight or less.

[0021] The neutron shielding material may include other flame retardants along with the brominated flame retardant, for example, the neutron shielding material may include a brominated flame retardant and antimony trioxide.

[0022] The neutron shielding material may further contain a boron-based compound. A boron-based compound is a compound that contains boron (B). Neutrons are moderated by hydrogen, and the moderated (reduced in energy) thermal neutrons undergo a (n, γ) reaction in the neutron shielding material, generating secondary gamma rays. When a boron-based compound is added to the neutron shielding material, the moderated thermal neutrons react with boron ( 10 B) can reduce the generation of secondary gamma rays.

[0023] When a boron-based compound is added to the neutron shielding material, the content of the boron-based compound is preferably 5 wt% or less relative to 100 wt% of the neutron shielding material, more preferably 1 wt% or more, and even more preferably 1 wt% or more and 2 wt% or less.

[0024] The boron-based compound is not particularly limited. Examples of boron-based compounds include boron carbide, boron nitride, and boron oxide. Among these, boron carbide (B4C) is preferable. Since boron carbide has a high ratio of boron in the compound, even a small amount of boron carbide can absorb thermal neutrons and suppress the generation of secondary gamma rays. In addition, since only a small amount of boron carbide is added, the ratio of the olefin copolymer rubber, which is the main material, is relatively unlikely to decrease. Therefore, the ratio of hydrogen in the neutron shielding material does not decrease much. This makes it possible to suppress the generation of secondary gamma rays while maintaining the neutron shielding effect. In addition, since boron carbide is a thermally stable substance (melting point is 2000°C or higher), it is possible to obtain the effect of suppressing the generation of secondary gamma rays even in a high-temperature environment.

[0025] The neutron shielding material may contain multiple types of boron-based compounds. When the neutron shielding material contains multiple types of boron-based compounds, it is preferable that the total content of the multiple types of boron-based compounds is within the above range.

[0026] The neutron shielding material may further contain additives other than those mentioned above, such as an antioxidant, a crosslinking aid, a stabilizer, and the like.

[0027] The neutron shielding material can be obtained, for example, by mixing and / or kneading an olefin copolymer rubber, a bromine-based flame retardant, a boron-based compound, additives, etc., and then molding the mixture. The olefin copolymer rubber, the bromine-based flame retardant, the boron-based compound, and additives may all be mixed at once, or some of them may be mixed first, and then the others may be added and mixed. The molding method is not particularly limited.

[0028] As described above, according to the present embodiment, it is possible to provide a neutron shielding material having higher performance in terms of neutron shielding property, self-extinguishing property, etc. than conventional neutron shielding materials. In addition, when the neutron shielding material further contains a boron-based compound, the effect of reducing the generation of secondary gamma rays can be further obtained.

[0029] Next, an example of using the neutron shielding material according to this embodiment in a radioactive material storage container will be described with reference to Fig. 1. Note that Fig. 1 is a diagram mainly for explaining the installation location of the neutron shielding material, and hatching showing a cross section is omitted.

[0030] A radioactive material storage container 100 shown in Fig. 1 is used for storing, transporting, and storing radioactive materials such as spent fuel and radioactive waste. As shown in Fig. 1, the radioactive material storage container 100 comprises a cylindrical container body 1 with a bottom, and a primary lid 2, a secondary lid 3, and a tertiary lid 4 arranged at one end of the container body 1. The container body 1, the primary lid 2, the secondary lid 3, and the tertiary lid 4 are made of, for example, carbon steel.

[0031] A space S for storing radioactive material is formed in the container body 1. The container body 1 has a cylindrical inner cylinder 11 with a bottom and a cylindrical outer cylinder 12 arranged outside the inner cylinder 11 with a gap therebetween. A neutron shielding material 21 according to this embodiment is arranged between the inner cylinder 11 and the outer cylinder 12. A neutron shielding material 22 according to this embodiment is installed at the bottom of the container body 1.

[0032] The primary lid 2, secondary lid 3 and tertiary lid 4 are arranged in this order from the inside of the radioactive material storage container 100. The primary lid 2 is a lid that seals the opening of the container body 1. The secondary lid 3 on the outside of the primary lid 2 is a lid that maintains the pressure in the space between the primary lid 2 and the primary lid 2 together with the inner cylinder 11 of the container body 1. The neutron shielding material 23 according to this embodiment is installed on the secondary lid 3. The tertiary lid 4 on the outside of the secondary lid 3 is a lid that is attached when the radioactive material storage container 100 is transported. The tertiary lid 4 is removed after the radioactive material storage container 100 has been transported to a specified storage location, except in special cases.

[0033] As described above, the neutron shielding material according to the present embodiment is installed, for example, on the side, bottom, and lid of the radioactive material storage container 100. Note that, although the above describes an example in which the neutron shielding material according to the present embodiment is installed on the side, bottom, and lid of the radioactive material storage container 100, the neutron shielding material according to the present embodiment may be installed in one or more locations on the side, bottom, and lid of the radioactive material storage container 100.

[0034] When the neutron shielding material according to this embodiment is installed in the storage container 100 for radioactive material, the following effects are obtained.

[0035] Radioactive material is stored in the space S of the radioactive material storage container 100. The stored radioactive material generates heat due to decay heat. This heat is transferred to the inner surface of the inner cylinder 11 of the container body 1, and transferred from the outer surface to the outer cylinder 12 by heat transfer fins (not shown) installed between the neutron shielding material 21, and is dissipated from the surface of the outer cylinder 12 mainly by radiation and convection. During operation of the radioactive material storage container 100, the temperature of the members constituting the radioactive material storage container 100 increases due to the heat generated by the radioactive material stored in the space S, and the maximum temperature of the neutron shielding material (21, 22, 23) may be, for example, about 100 to 150°C according to design. Although it is not the maximum temperature mentioned above, a temperature higher than room temperature continues over the design storage period (for example, 60 years) of the radioactive material storage container 100. In addition, the neutron shielding material is used in a sealed space and is not replaced during operation of the radioactive material storage container 100. Furthermore, the container body 1, primary lid 2, secondary lid 3, and tertiary lid 4 that constitute the radioactive material storage container 100 are made not of a material with excellent rust resistance, but of carbon steel or the like that takes into consideration gamma ray shielding function and structural strength. As described above, the neutron shielding materials (21, 22, 23) used in the radioactive material storage container 100 are different from ordinary rubber products and are used in special environments and conditions.

[0036] Since the main material of the neutron shielding material (21, 22, 23) is generally rubber, gas is likely to be generated by heat in the above-mentioned special usage environment. Depending on the constituent material of the neutron shielding material, corrosive gas may be generated. Assumed corrosive gases include organic acid gases containing formic acid, acetic acid, etc., and gases containing sulfur (sulfur dioxide). For example, when sulfur is used as a crosslinking agent for the rubber, gases containing sulfur are generated. There is a risk that the corrosive gas will corrode the surrounding metal materials including the container body 1, the primary lid 2, the secondary lid 3, and the tertiary lid 4. However, in this embodiment, an organic peroxide is used as the crosslinking agent for the olefin copolymer, instead of sulfur. Therefore, gases containing sulfur are not generated. In addition, as described in the examples below, it was found that the amount of organic acid gases containing formic acid, acetic acid, etc. generated is smaller than when sulfur is used as a crosslinking agent for the rubber. Therefore, even in the above-mentioned special usage environment, the surrounding metal materials can be prevented from corroding.

[0037] In addition, the main material of the neutron shielding materials (21, 22, 23) is an olefin copolymer rubber containing a large amount of hydrogen, so that the neutron shielding effect of the radioactive material storage container 100 is high.

[0038] Furthermore, by using a low-density olefin copolymer rubber, for example, ethylene-propylene-diene rubber (EPDM) or ethylene-propylene rubber (EPM), as the main material of the neutron shielding materials (21, 22, 23), it is possible to reduce the weight of the radioactive material storage container 100. This allows the amount of radioactive material to be increased within the design weight limit of the radioactive material storage container 100, thereby improving the storage efficiency of the radioactive material.

[0039] Furthermore, since the neutron shielding material (21, 22, 23) contains a bromine-based flame retardant, even if the neutron shielding material (21, 22, 23) burns, the neutron shielding material does not continue to burn. As will be described in the experiment below, it was found that the neutron shielding material of this embodiment does not continue to burn in a fire resistance test (a test in which the material is left at a temperature of 800°C for 30 minutes) required as a design requirement for a radioactive material storage container. In addition, the blending amount of the bromine-based flame retardant is within a specified range, and the ratio of the olefin copolymer rubber, which is the main material, is unlikely to decrease. In other words, the ratio of hydrogen in the neutron shielding material does not decrease much. Therefore, the neutron shielding material exhibits self-extinguishing properties while maintaining neutron shielding properties.

[0040] Furthermore, when the neutron shielding material (21, 22, 23) further contains a boron-based compound, the generation of secondary gamma rays is reduced. In particular, when boron carbide is contained as a boron-based compound, the effect of reducing the generation of secondary gamma rays can be reliably obtained even in the high-temperature environment described above, since boron carbide is a thermally stable substance (its melting point is 2000°C or higher).

[0041] As described above, it is possible to provide a radioactive material storage container that has high performance, such as neutron shielding performance, even in special environments and conditions in which the radioactive material storage container is used. EXAMPLES

[0042] The present invention will be described in detail below with reference to examples. However, the following examples do not limit the present invention, and all modifications and variations within the scope of the present invention are included in the technical scope of the present invention.

[0043] The raw materials were mixed and / or kneaded according to the composition shown in Table 1, and then molded. The physical properties of the obtained molded body (neutron shielding material) were evaluated.

[0044] [Table 1]

[0045] In this experiment, 1,2-bis(2,3,4,5,6-pentabromophenyl)ethane was used as a flame retardant (bromine-based), 2,5-dimethyl-2,5-di(t-butyl-peroxy)hexane was used as a crosslinking agent (organic peroxide), and triallyl isocyanate was used as a crosslinking aid. In Table 1, the raw materials are shown in the number of parts per 100 parts by weight of olefin copolymer rubber. The hydrogen and boron contents shown in Table 1 were calculated based on the nominal density (1.16 g / cm3).

[0046] Based on the experience of the present inventors, the specification values ​​of the neutron shielding material used in a storage container for radioactive materials are set as follows. Oxygen Index: 24 If the oxygen index is 24 or higher, the material has self-extinguishing properties. Here, "self-extinguishing properties" means that the neutron shielding material does not continue to burn after a fire resistance test at 800°C for 30 minutes, which is a design requirement for containers for storing radioactive materials. Hydrogen content: 0.1g / cm 3 (This is converted to atomic density of 5.97×10 22 atoms / cm 3 ) Hydrogen content is 0.1g / cm 3 (converted to atomic density of 5.97×10 22 atoms / cm 3 or more), the neutron shielding performance is high.

[0047] [Evaluation of corrosive gases] The molded product of blend S shown in Table 1 is a neutron shielding material that uses sulfur as a cross-linking agent for olefin copolymer rubber. When sulfur is used as a cross-linking agent, there is a possibility that corrosive gases will be generated by unreacted sulfur when heated. To confirm this, the following test was carried out.

[0048] A sample of Blend S (diameter Φ20 mm, length 70 mm) was sealed in a glass bottle and heated at 150°C for 10 days. The components (acetate ions, formate ions, sulfate ions) contained in the corrosive gas generated during this process were analyzed by ion chromatography.

[0049] For comparison, a sample of Formula E (diameter Φ20 mm, length 70 mm) was sealed in a glass bottle and heated at 150°C for 30 days, and the components contained in the generated corrosive gas (acetate ions, formate ions, sulfate ions) were analyzed by ion chromatography. Formula E uses an organic peroxide as a crosslinking agent.

[0050] The results are shown in Table 2.

[0051] [Table 2]

[0052] From the results shown in Table 2, sulfate ions were detected in Blend S, which used sulfur as the crosslinking agent, while sulfate ions were below the quantification limit in Blend E, which used an organic peroxide as the crosslinking agent. This shows that formulation S, which used sulfur as a cross-linking agent, generated corrosive gases containing sulfur, whereas formulation E, which used an organic peroxide as a cross-linking agent, was able to suppress the generation of corrosive gases containing sulfur.

[0053] In addition, formate ions were detected in formulation S, but in formulation E, the formate ions were below the quantification limit. The amount of acetate ions in Formula S is about half that of Formula E, but the heating period for Formula S (10 days) is one-third that of Formula E (30 days). The amount of acetate ions in Formula E is greater than that in Formula S, but considering the difference in heating period, it is considered to be the same or less.

[0054] In the above test, formulation E was used for comparison, but formulations A to D shown in Table 1 also use an organic peroxide as a crosslinking agent, just like formulation E, so it is expected that similar results will be obtained.

[0055] [Autolytic] The oxygen index was evaluated by changing the amount of flame retardant added. Table 1 shows the oxygen index (actual measured values).

[0056] The oxygen index of blends A to C and E in Table 1 exceeds the specification value of 24. Blends A to C and E have self-extinguishing properties. The blended parts of the flame retardant (bromine-based) in blends A to C and E are 45 parts by weight or more and 60 parts by weight or less.

[0057] Incidentally, the oxygen index of blend D is not shown in Table 1. However, from blends A to C and blend E, when the blended number of parts of flame retardant (bromine-based) is 45 parts by weight or more, the oxygen index exceeds the specification value of 24, and the oxygen index increases as the blended number of parts of flame retardant (bromine-based) increases. From this, it is considered that the oxygen index exceeds the specification value of 24 even in blend D, where the blended number of parts of flame retardant (bromine-based) is 55 parts by weight.

[0058] Here, the hydrogen content (atomic density [atoms / cm 3 ]), the hydrogen content of blends A, B, D, and E was within the specification value (5.97 × 10 22 atoms / cm 3 ), but the hydrogen content of blend C exceeds the specified value (5.97×10 22 atoms / cm 3 ) in blend C, the amount of flame retardant (bromine-based) is 60 parts by weight, but in blends A, B, D, and E, where the amount of flame retardant (bromine-based) is 55 parts by weight or less, the hydrogen content exceeds the specification value. In blend C, the amount of flame retardant (bromine-based) is set to 60 parts by weight, which reduces the proportion of olefin copolymer rubber in the neutron shielding material, and this is thought to be why the hydrogen content fell below the specification value.

[0059] From the above, it was found that by mixing 45 parts by weight or more and 55 parts by weight or less of flame retardant (bromine-based) per 100 parts by weight of olefin-based copolymer rubber, a neutron shielding material with self-extinguishing properties can be obtained while maintaining neutron shielding properties.

[0060] In addition, in this test, ethylene-propylene-diene rubber (EPDM), which has a relatively low density, was used as the main material for the neutron shielding material, resulting in a density of 1.14 to 1.18 g / cm 3 A low density neutron shielding material was obtained.

[0061] [Shielding performance (content of boron-based compounds)] The shielding performance was evaluated by changing the amount of boron carbide (B4C) added.

[0062] The dose equivalent rate of neutrons and secondary gamma rays on the outer surface of the center of the side of the radioactive material storage container was calculated under the shielding analysis conditions shown in Table 3, assuming that a neutron shielding material was placed on the side of the radioactive material storage container, with the content of boron carbide (B4C) as a parameter. The neutron shielding material was assumed to be the composition E shown in Table 1, and the amount of boron carbide (B4C) added was changed. Note that, since the atomic number density calculated from the content of the neutron shielding material (content relative to 100 wt% of the neutron shielding material (unit: wt%)) is used to calculate the dose equivalent rate, the addition rate of boron carbide (B4C) is shown below as the addition rate relative to 100 wt% of the neutron shielding material (unit: wt%). In addition, in this shielding analysis, input data was created conservatively based on the minimum density of the neutron shielding material. The analysis results are shown in Figures 2 and 3.

[0063] [Table 3]

[0064] From Figure 2, we can see the following: Regarding secondary gamma rays, it was found that the higher the content of boron carbide (B4C), the more the secondary gamma rays were reduced, but the effect was small when the content of boron carbide (B4C) was 20wt% or more. On the other hand, for neutrons, when the content of boron carbide (B4C) is 5wt% or more, the number of neutrons increases significantly, and the total dose equivalent rate of neutrons and secondary gamma rays increases significantly. This is because the increase in the content of boron carbide (B4C) causes a relative decrease in the content of the main olefin copolymer rubber, which reduces the hydrogen atom number density, thereby reducing the neutron shielding effect.

[0065] From the above, it is considered that the maximum content of boron carbide (B4C) should be about 5wt%. Further investigation into the range of boron carbide (B4C) content of 5wt% or less was carried out based on the enlarged view shown in Figure 3, and the following was found.

[0066] The relationship between the dose equivalent rates of neutrons and secondary gamma rays changes when the boron carbide (B4C) content is in the range of 1 wt% to 2 wt%. According to the neutron shielding materials evaluated here, the total dose equivalent rates of neutrons and secondary gamma rays are almost the same when the boron carbide (B4C) content is in the range of 1 wt% to 2 wt%, so almost no difference in the total dose equivalent rate of neutrons and secondary gamma rays due to differences in the boron carbide (B4C) content was observed, but the shielding effect due to the boron carbide (B4C) content also differs depending on the radiation source conditions (energy spectrum distribution and radiation source strength) of the contents stored in the radioactive material storage container, and when considering the balance of the dose equivalent rates of both neutrons and secondary gamma rays, it can be said that an addition amount of about 1 wt% to 2 wt% is preferable.

[0067] From the above, when taking into consideration the overall shielding effect against neutrons and secondary gamma rays, it is desirable for the boron carbide (B4C) content to be between 1wt% and 2wt%. Also, since the price of boron carbide (B4C) is high, costs can be reduced by adding as little as possible while maintaining the same level of shielding effect. Even when considering costs, the above content is desirable. In addition, based on the experience of the present inventors, the atomic density of the boron content is 5.00×10 20 atoms / cm 3It has been found that when the boron carbide (B4C) content is between 1wt% and 2wt%, the secondary gamma ray suppression effect is higher. When the boron content is 5.00×10 20 atoms / cm 3 It turned out that this was the case.

[0068] In the above examples, boron carbide was used as the boron-based compound. However, boron-based compounds other than boron carbide can also reduce the generation of secondary gamma rays while maintaining neutron shielding performance, as in the above evaluation results, due to the boron contained in the compound.

[0069] Although the embodiment of the present invention has been described above based on the examples, the specific configuration should not be considered to be limited to these embodiments. The scope of the present invention is indicated by the claims rather than the above description, and includes all modifications within the meaning and scope of the claims. [Explanation of symbols]

[0070] 1 Container body 2 Primary lid 3 Secondary lid 4 Tertiary lid 11 Inner cylinder 12 Outer cylinder 21, 22, 23 Neutron shielding materials 100 Radioactive material storage container

Claims

1. A neutron shielding material used in a storage container for radioactive materials, The main material of the neutron shielding material is an olefin copolymer rubber, The olefin copolymer rubber is molded using an organic peroxide as a crosslinking agent, The neutron shielding material contains a bromine-based flame retardant, A neutron shielding material characterized in that the blending amount of the bromine-based flame retardant per 100 parts by weight of the olefin copolymer rubber is 45 parts by weight or more and 55 parts by weight or less.

2. In the neutron shielding material according to claim 1, The neutron shielding material is characterized in that the olefin copolymer rubber is an ethylene-propylene-diene rubber or an ethylene-propylene rubber.

3. In the neutron shielding material according to claim 1 or 2, Further containing a boron-based compound, A neutron shielding material, characterized in that the content of a boron-based compound is 5 wt % or less relative to 100 wt % of the neutron shielding material.

4. In the neutron shielding material according to claim 3, A neutron shielding material, characterized in that the content of a boron-based compound is 1 wt % or more and 2 wt % or less relative to 100 wt % of the neutron shielding material.

5. A container for storing radioactive material, A storage container for radioactive material, comprising a neutron shielding material according to any one of claims 1 to 4 installed on at least one of the side, lid and bottom of the storage container.

Citation Information

Patent Citations

  • Neutron shielding material

    JP1982173795A

  • Neutron shielding material

    JP1986213694A

  • Neutron shielding material

    JP1997033691A

  • Cask, composition for neutron shield, and production method for neutron shield

    JP2004028987A