Improved microlayer membranes, improved battery separators, and related methods
Multilayer microporous membranes produced by coextrusion and lamination of polymer mixtures address the strength and performance issues in battery separators, resulting in safer and more durable lithium ion batteries with enhanced dielectric breakdown and puncture resistance.
Patent Information
- Application Number
- JP2022119795
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-05-18
- Filing Date
- 2022-07-27
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2037-11-10
AI Technical Summary
Existing methods for producing battery separators, such as laminating or coextruding multiple layers, fail to optimize the balance of strength and performance properties, particularly in thinner and stronger lithium ion rechargeable batteries, leading to reduced safety and durability.
The development of multilayer microporous membranes with improved properties, achieved through coextrusion of multiple polymer mixtures to form bilayer, trilayer, or multilayer films, which are then stacked and laminated to create a microporous battery separator with enhanced strength, dielectric breakdown, and reduced tearing tendency.
The resulting microporous multilayer battery separators exhibit increased dielectric breakdown, shutdown speed, puncture strength, and tortuosity, indicating improved safety and durability compared to traditional bilayer or trilayer separators, enhancing the performance of lithium ion batteries.
Smart Images

Figure 0007568681000003 
Figure 0007568681000004 
Figure 0007568681000005
Abstract
Description
[Technical field]
[0001] Priority claim This application claims the benefit of and priority under 35 U.S.C. §119(e)(1) to U.S. Provisional Patent Application No. 62 / 508,360, filed May 18, 2017, and U.S. Provisional Patent Application No. 62 / 420,781, filed November 11, 2016. Each of these provisional patent applications is incorporated herein by reference in its entirety.
[0002] According to at least selected embodiments, the present application, disclosure and inventions relate to new or improved membranes, separator films, separators, battery separators, lithium secondary battery separators, multilayer membranes, multilayer separator films, multilayer separators, multilayer battery separators, multilayer lithium secondary battery separators, and / or multilayer battery separators, new or improved batteries, capacitors, fuel cells, lithium batteries, lithium ion batteries, lithium secondary batteries, and / or lithium ion secondary batteries, and / or methods of making and / or using such membranes, separator films, separators, battery separators, lithium secondary battery separators, batteries, capacitors, fuel cells, lithium batteries, lithium ion batteries, lithium secondary batteries, and / or lithium ion secondary batteries, and / or devices, vehicles or products comprising same. According to at least certain embodiments, the present disclosure or inventions relate to new or improved membrane layers, membranes or separator films, battery separators comprising such membranes, and / or related methods. According to at least certain selected embodiments, the disclosure or invention relates to new or improved porous polymeric or separator membranes, battery separators including such membranes, and / or related methods. According to at least certain embodiments, the disclosure or invention relates to new or improved microporous polyolefin or separator membranes, microlayer membranes, multilayer membranes including one or more microlayers or nanolayer membranes, battery separators including such membranes, and / or related methods. According to at least certain embodiments, the disclosure or invention relates to new, optimized, or improved microporous stretched polymeric or separator membranes having one or more new or improved outer and / or inner layers, microlayer membranes, multilayered microporous or separator membranes having outer and inner layers, some of such layers or sublayers being produced by coextrusion and then laminated together to form said new, optimized, or improved membrane or separator membrane.In some embodiments, a layer, microlayer, or nanolayer may comprise a homopolymer, copolymer, block copolymer, elastomer, and / or polymer blend. In selected embodiments, at least a layer, microlayer, or nanolayer may comprise a different or distinct polymer, homopolymer, copolymer, block copolymer, elastomer, and / or polymer blend. The present disclosure or invention also relates to new or improved methods of making such membranes, separator membranes, or separators, and / or new or improved methods of using such membranes, separator membranes, or separators, for example, as lithium battery separators. According to at least selected embodiments, the present application or invention is directed to new or improved multilayer and / or microlayer porous or microporous membranes, separator membranes, separators, composites, electrochemical devices, and / or batteries, and / or methods of making and / or using such membranes, separators, composites, devices, and / or batteries. According to at least certain selected embodiments, the present application or invention is directed to new or improved separator membranes that are multi-layered, where one or more layers of the multi-layer structure are produced in a multi-layer or micro-layer co-extrusion die having multiple extruders. The new or improved membranes, separator membranes, or separators may preferably demonstrate improved shutdown, improved strength, improved dielectric breakdown strength, and / or reduced tendency to tear. [Background technology]
[0003] Known methods for making microporous bi- or tri-layer membranes for use as battery separator membranes include laminating or gluing two or more monolayer precursors together, or co-extruding more than one membrane layer simultaneously using a co-extrusion die. Such methods are described, for example, in U.S. Pat. No. 5,952,120, U.S. Pat. No. 2014 / 0079980, U.S. Pat. No. 5,223,032, U.S. Pat. No. 5,240,655, and U.S. Pat. No. 2005 / 031943.
[0004] The above methods cannot fully optimize the balance of strength and / or performance properties for use in certain primary and / or secondary battery applications, such as lithium-ion rechargeable batteries. This is especially true as battery separator requirements become more demanding as consumers desire thinner and stronger battery separators. For example, a microporous trilayer membrane formed by co-extrusion of three layers may have reduced strength. Separators formed by stacking single layers also ultimately cannot meet the ever-increasing demands. Summary of the Invention [Problem to be solved by the invention]
[0005] Thus, there is a need for new and improved multi-layer microporous membranes, base films, or battery separators that have various improvements, such as improved tensile strength and improved dielectric breakdown strength. [Means for solving the problem]
[0006] According to at least selected embodiments, the present application, disclosure and inventions may address the above needs, challenges or problems and / or provide new or improved membranes, separator films, separators, battery separators, lithium secondary battery separators, multilayer membranes, multilayer separator films, multilayer separators, multilayer battery separators, multilayer lithium secondary battery separators, and / or multilayer battery separators, new or improved batteries, capacitors, fuel cells, lithium batteries, lithium ion batteries, lithium secondary batteries, and / or lithium ion secondary batteries, and / or methods of making and / or using such membranes, separator films, separators, battery separators, lithium secondary battery separators, batteries, capacitors, fuel cells, lithium batteries, lithium ion batteries, lithium secondary batteries, and / or lithium ion secondary batteries, and / or devices, vehicles or products including same, according to at least certain embodiments, the present disclosure or inventions relate to new or improved membrane layers, membranes or separator films, battery separators including such membranes, and / or related methods. According to at least certain selected embodiments, the disclosure or invention relates to new or improved porous polymeric or separator membranes, battery separators including such membranes, and / or related methods. According to at least certain embodiments, the disclosure or invention relates to new or improved microporous polyolefin or separator membranes, microlayer membranes, multilayer membranes including one or more microlayers or nanolayer membranes, battery separators including such membranes, and / or related methods. According to at least certain embodiments, the disclosure or invention relates to new, optimized, or improved microporous stretched polymeric or separator membranes having one or more new or improved outer and / or inner layers, microlayer membranes, multilayered microporous or separator membranes having outer and inner layers, some of such layers or sublayers being produced by coextrusion and then laminated together to form said new, optimized, or improved membrane or separator membrane.In some embodiments, a layer, microlayer, or nanolayer may comprise a homopolymer, copolymer, random copolymer, PP and / or PE copolymer, block copolymer, elastomer, and / or polymer blend. In selected embodiments, at least a layer, microlayer, or nanolayer may comprise a different or distinct polymer, homopolymer, copolymer, block copolymer, elastomer, and / or polymer blend. The present disclosure or invention also relates to new or improved methods of making such membranes, separator membranes, or separators, and / or new or improved methods of using such membranes, separator membranes, or separators, for example, as lithium battery separators. According to at least selected embodiments, the present application or invention is directed to new or improved multi-layer and / or micro-layer porous or microporous membranes, separator membranes, separators, composites, electrochemical devices, and / or batteries, and / or methods of making and / or using such membranes, separators, composites, devices, and / or batteries. According to at least certain selected embodiments, the present application or invention is directed to new or improved separator membranes that are multi-layered, where one or more layers of the multi-layer structure are produced in a multi-layer or micro-layer co-extrusion die having multiple extruders. The new or improved membranes, separator membranes, or separators may preferably demonstrate improved shutdown, improved strength, improved dielectric breakdown strength, and / or reduced tendency to tear.
[0007] The microporous multi-layer battery separators described herein, in some embodiments, exhibit improved safety, strength, and durability compared to previous bi-layer, tri-layer, or multi-layer battery separators. For example, the separators may exhibit increased average dielectric breakdown (DB), increased minimum DB, increased shutdown speed, and increased flexure, all of which are indicative of a safer battery separator. The separators may also exhibit increased puncture strength and increased mixed penetration values, indicative of a stronger, more durable battery.
[0008] These properties of the microporous multi-layer battery separators described herein are at least partially a result of the method by which they are made. The method, in some embodiments, includes at least co-extruding two or more polymer mixtures to form a first co-extruded bi-, tri-, or multi-layer film, co-extruding two or more other polymer mixtures to form a second co-extruded bi-, tri-, or multi-layer film, and co-extruding two or more additional polymer mixtures to form a third co-extruded bi-, tri-, or multi-layer film. Co-extrusion typically includes using a co-extrusion die with one or more extruders (typically one extruder per layer of the bi-, tri-, or multi-layer film) feeding the die. The polymer mixtures used to form each layer of the first, second, and third bi-, tri-, or multi-layer films can be the same or different. The mixtures may include one polymer or more than one polymer, such as a polymer blend. Also, more than three bi-, tri-, or multi-layer films may be formed. After the first, second, and third bilayer, trilayer, or multilayer thin films are formed, the thin films are laminated together with two of the thin films formed on opposing sides of one of the thin films to form the optionally preferred microporous battery separator described herein.
[0009] The microporous multilayer battery separators described herein can be used in lithium ion batteries, including lithium secondary batteries, resulting in batteries with improved safety and durability.
[0010] The battery separators herein can be described in several different ways.
[0011] In a first aspect, a battery separator for a lithium battery is described herein. In some embodiments, the battery separator comprises at least one microporous separator membrane or sub-membrane comprising a plurality of porous or microporous polymeric micro- or nano-layers, where at least one of the individual micro- or nano-layers comprises a different or distinct polymer, molecular weight polymer, homopolymer, copolymer, and / or polymer blend, comprises a different or distinct additive, agent, material, and / or filler, or comprises a combination of different or distinct polymer, molecular weight polymer, homopolymer, copolymer, random copolymer of ethylene and / or propylene, polymer blend, additive, agent, material, elastomer, SEPS, SEBS, PVDF, EVOH, PMP, filler, particle, ceramic particle, bead, fiber, scavenger, crosslinker, adhesion promoter, surface modifier, and / or combination thereof, compared to adjacent individual micro- or nano-layers. In some embodiments, the above separator membranes or sub-membranes of the polymeric micro- or nano-layers are laminated to each other or to the microporous polymeric membrane. In some embodiments, at least one of the separator membranes or sub-membranes of the polymeric microlayers or nanolayers has at least three microlayers or nanolayers. Optionally, at least one of the separator membranes or sub-membranes of the polymeric microlayers or nanolayers is made from one or more polyolefins. Optionally, at least one of the separator membranes or sub-membranes of the polymeric microlayers or nanolayers is made from a coextruded dry-process polyolefin microlayer or nanolayer. In some embodiments, at least two of the separator membranes or sub-membranes of the polymeric microlayers or nanolayers. In some embodiments, at least three of the separator membranes or sub-membranes of the polymeric microlayers or nanolayers.
[0012] In another aspect, described herein is a lithium battery including any of the battery separators described immediately above. In another aspect, an improved separator, membrane or base film is described herein.
[0013] In some embodiments, the separator is a multilayer separator, membrane, or base film comprising one or more microporous coextruded micro- or nano-multilayer polymeric membranes or sub-membranes adapted to be laminated or adhered to another polymeric membrane, wherein at least one of the individual micro- or nano-layers comprises a different or distinct polymer, molecular weight polymer, homopolymer, copolymer, and / or polymer blend, comprises a different or distinct additive, drug, material, and / or filler, or comprises a combination of different or distinct polymers, molecular weight polymers, homopolymers, copolymers, polymer blends, additives, drugs, materials, and / or fillers, as compared to an adjacent individual micro- or nano-layer.
[0014] In another aspect, described herein is a battery that includes at least one battery separator as described in the preceding paragraph.
[0015] In one other aspect, a battery separator or separator film is described herein.In some embodiments, the battery separator or separator film comprises one or more coextruded micro-multilayer films laminated or bonded to another polymeric film, and the separator or separator film can provide improved strength, such as improved puncture strength, and can also exhibit improved shutdown and / or reduced tear tendency, particularly at a certain thickness, and at least one of the individual microlayers comprises a different or separate polymer, molecular weight polymer, homopolymer, copolymer, and / or polymer blend, comprises a different or separate additive, drug, material, and / or filler, or comprises a combination of different or separate polymer, molecular weight polymer, homopolymer, copolymer, polymer blend, additive, drug, material, and / or filler, compared to adjacent individual microlayers.
[0016] In another aspect, described herein are batteries, particularly lithium ion batteries, that include at least one separator as described in the preceding paragraph. In another aspect, a battery separator or separator membrane is described herein.
[0017] The battery separator or separator film, in some embodiments, comprises one or more coextruded micro- or nano-multilayer films optionally laminated or bonded to another polymeric film. The separator or separator film may exhibit improved strength, improved puncture strength, and / or improved shutdown and / or reduced tear tendency at a certain thickness. In some embodiments, at least one of the individual micro- or nano-layers comprises a different or distinct polymer, molecular weight polymer, homopolymer, copolymer, and / or polymer blend, comprises a different or distinct additive, drug, material, and / or filler, or comprises a combination of different or distinct polymers, molecular weight polymers, homopolymers, copolymers, polymer blends, additives, drugs, materials, and / or fillers, as compared to adjacent individual micro- or nano-layers.
[0018] In another aspect, described herein are batteries, particularly lithium ion batteries, that include at least one separator as described in the preceding paragraph.
[0019] In another aspect, an improved battery separator is described herein that includes a multi-layered microporous membrane. In some embodiments, the multi-layered microporous membrane includes 9 or more layers, 12 or more layers, 15 or more layers, 18 or more layers, 21 or more layers, 24 or more layers, 27 or more layers, 30 or more layers. In some embodiments, at least three consecutive layers of the microporous membrane have a thickness of 0.1 to 5 microns, 0.1 to 3 microns, 0.1 to 2.5 microns, or 0.1 to 2.0 microns. In some embodiments, the battery separator itself has a thickness of 1 micron to 30 microns, 2 microns to 20 microns, 3 microns to 15 microns, or 4 microns to 10 microns.
[0020] In some embodiments, at least three consecutive layers each individually comprise a polyolefin or polyolefin blend, and in some embodiments, these layers each comprise polyethylene, and in some embodiments, each comprise polypropylene.
[0021] In some cases, the at least three consecutive layers are coextruded layers. In some embodiments, the at least three consecutive layers are laminated with at least one other layer to form a microporous polymeric thin film. In some embodiments, the at least one other layer is also a coextruded layer, coextruded with at least one other layer. In the battery separator of claim 28, the at least one other layer is a coextruded layer. The battery separator described has a puncture strength of 290 gf or more, 300 gf or more, or 310 gf or more in some embodiments.
[0022] In another aspect, described herein are batteries, including lithium ion batteries, particularly lithium ion secondary batteries, that include one or more of the battery separators described in the preceding paragraphs. The batteries are at least more durable, particularly in embodiments where the battery separator has a puncture strength of 290 gf or greater, 300 gf or greater, or 310 gf or greater.
[0023] In yet another aspect, a microporous multi-layer battery separator is described herein. The battery separator includes a first region that includes two or more layers and includes a majority of discontinuous amorphous regions when viewed in the z-direction of the film using SEM; and a second region that includes at least one layer. In some embodiments, 50% or more, 60% or more, 70% or more, 80% or more, or 90% or more of the amorphous regions in the first region are discontinuous. In some embodiments, the second region includes two or more layers, preferably three or more layers, and an amorphous region having a maximum width of 0.8 microns, a maximum width of 0.7 microns, or a maximum width of 0.6 microns. In some of the embodiments described herein, at least one of the first and second regions includes one or more layers that include a polyolefin. In some embodiments, the first region includes at least one layer that includes polyethylene, and the second region includes at least one layer that includes polypropylene. Optionally, at least one of the first and second regions includes a coextruded bi-layer, tri-layer, or multi-layer film. Optionally, the first region comprises a coextruded bi-, tri- or multi-layer thin film. Optionally, the first region and the second region comprise a coextruded bi-, tri- or multi-layer thin film. Optionally, the first region, the second region, and the third region of the microporous multi-layer battery separator each comprise a coextruded bi-, tri- or multi-layer thin film. Optionally, at least one of the second and third regions of the microporous multi-layer battery separator comprises a coextruded bi-, tri- or multi-layer thin film. Optionally, the second region comprises a coextruded bi-, tri- or multi-layer thin film. Optionally, the third region comprises a coextruded bi-, tri- or multi-layer thin film.
[0024] In another aspect, described herein are batteries, particularly lithium ion batteries, that include at least one separator as described in the preceding paragraph.
[0025] In another aspect, a battery separator comprising a multi-layer microporous thin film having an average dielectric breakdown (DB) value higher than that of a typical tri-layer microporous thin film having at least one of the same thickness, Gurley, and porosity as the multi-layer microporous thin film. For example, the average DB value may be 1-35% higher, 5-35% higher, 10-35% higher, 15-35% higher, or 20-35% higher. In some embodiments, the DB minimum value of the microporous multi-layer thin film of the battery separator described herein may be higher than that of a typical or conventional tri-layer microporous thin film having the same thickness, Gurley, and / or porosity as the multi-layer microporous thin film. For example, the DB minimum value may be 3-20% higher, 5-15% higher, or 10-15% higher than that of a tri-layer microporous thin film having the same thickness, Gurley, and / or porosity as the multi-layer microporous thin film. In some cases, the multilayer microporous thin film includes 9 or more layers, 12 or more layers, 15 or more layers, 18 or more layers, 21 or more layers, 24 or more layers, 27 or more layers, or 30 or more layers. In some embodiments, at least one of such layers includes a polyolefin or polyolefin blend. The polyolefin blend may be a polyethylene or polyethylene blend or a polypropylene or polypropylene blend. In some other embodiments, the multilayer microporous thin film having the dielectric breakdown values herein may include a first region including two or more layers and a second region including at least one layer. The first region may include polypropylene and a largely discontinuous amorphous region when viewed in the z-direction of the thin film using SEM. In some embodiments, the multilayer microporous thin film of the battery separator having the dielectric breakdown improvement described herein may include the following: (1) a first region including two or more layers, a second region including at least one layer, and a third region including at least one layer. The first region may include polypropylene and mostly discontinuous amorphous regions when viewed in the z-direction (or thickness direction) of the film using an SEM.
[0026] In another aspect, described herein are batteries, particularly lithium ion batteries, that include at least one separator as described in the preceding paragraph.
[0027] In another aspect herein, a battery separator comprising a multilayer microporous thin film that exhibits a mercury intrusion value of 5 mL / g or less, 4.5 mL / g or less, 4 mL / g or less, or 3.5 mL / g or less, at a pressure sufficient to cause mercury to fill the pores, as measured using mercury intrusion porosimetry. In another aspect, described herein is a battery, particularly a lithium ion battery, that includes at least one separator as described in the preceding paragraph.
[0028] In another aspect, described herein is a battery separator comprising a multilayer microporous thin film having a McMillan number greater than 5, greater than 5.5, greater than 6, greater than 6.5, greater than 7, greater than 8, greater than 9, or greater than 10. In another aspect, described herein is a battery, particularly a lithium ion battery, that includes at least one separator as described in the preceding paragraph.
[0029] In another aspect herein, a battery separator is described herein, comprising a multi-layered microporous thin film having a tortuosity value of 1.6 or more, 1.8 or more, or 2.0 or more.In some embodiments, the battery separator herein is a microporous battery separator.In some embodiments, the battery separator is a microporous multi-layered battery separator.
[0030] In another aspect, described herein are batteries, particularly lithium ion batteries, that include at least one separator as described in the preceding paragraph.
[0031] In another embodiment, a battery separator comprising a multilayer microporous thin film exhibiting a pin removal force of less than 50 Newtons, 40 Newtons, 30 Newtons, 20 Newtons, 15 Newtons, or 10 Newtons.
[0032] In another aspect, a battery, particularly a lithium-ion battery, is described herein, which comprises at least one membrane or separator described in the preceding paragraph.The battery may preferably be a dry-process or dry-stretch process polyolefin-based membrane, particularly blown or bubble extrusion MD-stretch or MD+TD-stretch membrane, although other membranes, such as slot-die extrusion or casting, wet process, BNBOPP, BOPP, particle stretch, and / or equivalent membranes, may be used.For example, a dry-process multilayer PO membrane may be laminated to a BNBOPP membrane.
[0033] In another embodiment, a battery separator is described herein. The battery separator includes a microporous multi-layered thin film including: (1) a first region including two or more layers; (2) a second region including two or more layers on a first surface of the first region; and (3) a third region including two or more layers on a surface opposite the first surface of the first region, wherein at least one of the first, second, or third regions includes PE and has a lower crystallinity as measured by DSC than the PE-containing layer of the tri-layered microporous thin film, wherein the tri-layered microporous thin film has the same thickness as the multi-layered microporous thin film. For example, the crystallinity may be 1-20% lower, 1-15% lower, 1-10% lower, or 1-5% lower.
[0034] In another aspect, described herein are batteries, particularly lithium ion batteries, that include at least one separator as described in the preceding paragraph.
[0035] In another aspect, described herein is a battery separator comprising a multilayer microporous thin film having a mixed penetration (N) value of greater than 380N, greater than 400N, greater than 450N, greater than 500N, greater than 550N, greater than 600N, greater than 650N, or greater than 700N.
[0036] In another aspect, described herein are batteries, particularly lithium ion batteries, that include at least one separator as described in the preceding paragraph.
[0037] In another aspect, a battery separator is described herein, the battery separator comprising a microporous thin film having an electrical resistance value of 2 or less, in some embodiments 1.7 or less, in some embodiments 1.6 or less, in some embodiments 1.5 or less, in some embodiments 1.4 or less, in some embodiments 1.3 or less, in some embodiments 1.2 or less, and in some embodiments 1.0 or less.
[0038] In another aspect, described herein are batteries, particularly lithium ion batteries, that include at least one separator as described in the preceding paragraph.
[0039] In another embodiment, a battery separator is described that includes a multilayer microporous thin film having a mixed penetration value of 380N or greater, 400N or greater, 450N or greater, 500N or greater, 550N or greater, 600N or greater, 650N or greater, or 700N or greater.
[0040] In another aspect, described herein are batteries, particularly lithium ion batteries, that include at least one separator as described in the preceding paragraph.
[0041] In another aspect, a battery separator is described that includes a multilayer microporous thin film having an electrical resistivity of 2.0 or less, 1.7 or less, 1.6 or less, 1.5 or less, 1.4 or less, 1.3 or less, 1.2 or less, 1.1 or less, or 1.0 or less.
[0042] In another aspect, described herein are batteries, particularly lithium ion batteries, that include at least one separator as described in the preceding paragraph.
[0043] In another embodiment, a battery separator comprising a multilayer microporous thin film comprising two or more layers or microlayers and a region comprising polyethylene in one or more of the layers or microlayers, wherein at least one of the following is satisfied when the region is tested according to the machine learning test described herein: T x' ≥ -4, W T x' ≧ -2.654, W T x' ≥ 1.3, and W T x' ≥ 2, W T It is most preferred that x'≧2.
[0044] In another aspect, described herein are batteries, particularly lithium ion batteries, that include at least one separator as described in the preceding paragraph.
[0045] In another embodiment, a battery separator comprising a multilayer microporous thin film comprising two or more layers or microlayers and a region comprising polypropylene in one or more of the layers or microlayers, wherein the region, when tested according to the machine learning tests described herein, satisfies at least one of the following: W T x' ≥ -5, W T x' ≥ -3, W T x' ≥ 0, W T x' ≥ 3, W T It is most preferred that x'≧3.
[0046] In another aspect, described herein are batteries, particularly lithium ion batteries, that include at least one separator as described in the preceding paragraph.
[0047] In another embodiment, a battery separator comprising a multilayer or microporous thin film having the same thickness, porosity and dielectric breakdown uniformity that is better than Gurley's typical separator.
[0048] In another aspect, described herein are batteries, particularly lithium ion batteries, that include at least one separator as described in the preceding paragraph.
[0049] In another embodiment, a battery separator is described, the battery separator comprising at least one multi-layer microporous membrane or thin film having at least two regions or sub-layers, each region or sub-layer comprising at least two microlayers, the multi-layer membrane having or exhibiting at least one of the following: (a) a mixed penetration (N) value of greater than 380 N; (b) a mixed penetration (N) value of greater than 600 N; (c) a tortuosity of 1.8 or greater; (d) an average dielectric breakdown value (V) that is 1-35% higher than that of a tri-layer microporous thin film having the same thickness, Gurley, and / or porosity as the multi-layer microporous thin film; (e) a minimum dielectric breakdown value (V) that is 3-20% higher than that of a tri-layer microporous thin film having the same thickness, Gurley, and / or porosity as the multi-layer microporous thin film; (f) a dielectric breakdown uniformity of 0.01 to 0.01; (g) passes a nail penetration test; (h) has at least one microlayer comprising PO, PP and / or PE and an elastomer; (i) has at least one microlayer comprising a siloxane; (j) has at least one microlayer comprising PP and an elastomer; (k) has at least one microlayer comprising a copolymer; (l) has at least one microlayer comprising PP and a copolymer; (m) has at least two microlayers comprising different resins or resin blends; (n) when one of the above regions comprises polypropylene in one or more of the microlayers, at least one of the following is met when the region is tested according to the machine learning test described herein: W T x' ≥ -5 or W Tx'≧-3; (o) when one of the above regions comprises polypropylene in one or more of the microlayers, when the region is tested according to the dimensional reduction technique known as PCA described herein, at least one of the following is satisfied: W T x' ≥ 0, and W T x'≧3; (p) when one of the regions above comprises polyethylene in one or more of the microlayers, when the region is tested according to the machine learning tests described herein, at least one of the following is satisfied: W T x' ≥ -4 and W T x'≧-2.654; (q) when one of the regions above comprises polyethylene in one or more of the microlayers, when the region is tested according to the machine learning tests described herein, at least one of the following is satisfied: W T x' ≥ 1.3, and W Tx'≧2; (r) one of the regions comprises PE and has 1-20% less crystallinity, as measured by DSC, than that of a PE-containing layer of a tri-layer microporous membrane or thin film having the same thickness, Gurley, and / or porosity as the multilayer microporous thin film; (s) the microporous multilayer or thin film has 30-100 microlayers or more; (t) at least one of the microlayers comprises lithium stearate; (u) the multilayer microporous thin film exhibits reduced MD or TD tearing; (v) at least one of the microlayers comprises PE beads; (w) has a pin removal of less than 50 N; (x) exhibits reduced contact with pins; (y) has reduced MD or TD tearing; (z) may be a precursor for at least one of transverse (TD) stretching, calendaring, and pore filling. In some embodiments, the microporous multilayer membrane exhibits 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, 9 or more, 10 or more, 11 or more, 12 or more, 13 or more, 14 or more, 15 or more, 16 or more, 17 or more, 18 or more, 19 or more, 20 or more, 21 or more, 22 or more, 23 or more, 24 or more, 25 or more, or 26 of the 26 options. The separator may include other properties. In some embodiments, the battery separator is coated on one or more surfaces thereof, and in some embodiments, is uncoated. In some embodiments, the coating is a ceramic coating.
[0050] In another aspect, described herein are batteries, particularly lithium ion batteries, that include at least one separator as described in the preceding paragraph.
[0051] In another aspect, a method of forming an improved battery separator comprising a multi-layer microporous membrane or thin film is described herein. The method includes at least the steps of co-extruding at least two layers and laminating at least two co-extruded layers to one other layer, or in some embodiments, two other layers to form a multi-layer microporous membrane. In some embodiments, at least 2, 3, 4, 5, 6, 7, 8, 9, or 10 layers are co-extruded. In some embodiments, at least one other layer, or at least one of the at least two other layers, is a co-extruded layer. In some embodiments, at least one of the other layers is a mono-extruded layer. In embodiments where at least two co-extruded layers are laminated to two other layers, optionally one of the other two layers is laminated to a first surface of the at least two co-extruded layers, and a second of the other two layers is laminated to a surface of the at least two co-extruded layers that is opposite to the first surface. At least one of the other two layers may be a co-extruded layer. In some embodiments, both of the other two layers are co-extruded layers. In some embodiments, at least one of the at least two coextruded layers and the other layer comprises a polyolefin or a polyolefin blend. For example, they may comprise polyethylene or a polyethylene blend or polypropylene or a polypropylene blend. In some embodiments, at least one of the at least two coextruded layers comprises polyethylene and at least one or both of the other layers comprise polypropylene or a polyethylene blend. In some embodiments, at least one of the at least two coextruded layers comprises polyethylene and at least one or both of the other layers comprise polypropylene or a polypropylene blend. In some embodiments, each of the other two layers comprises polyethylene or a polyethylene blend. In some embodiments, each of the other two layers comprises polypropylene or a polypropylene blend.In some embodiments, one or both of the other two layers is a coextruded layer, coextruded with 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, or 9 or more other layers. When a layer is coextruded with 9 other layers, the total number of coextruded layers is 10.
[0052] In another embodiment, a battery separator made by the method described in the preceding paragraph. [Brief description of the drawings]
[0053] [Figure 1] FIG. 1 is a partial cross-sectional scanning electron micrograph (SEM) at 2,500x magnification of an exemplary laminated trilayer or triple trilayer microporous membrane of the present invention, trilayer / trilayer / trilayer (with nine coextruded microlayers for each trilayer and three microlayers for each PP or PE sublayer in each trilayer) (at least the outer PP layer of each layer is microporous). [Diagram 2] FIG. 2 is a partial cross-sectional scanning electron micrograph (SEM) at 15,000x magnification of a portion of the polypropylene surface sublayer (three microlayers of PP) of the surface tri-layer component or sub-membrane of the composite laminate membrane of FIG. 1 (the PP sublayer is magnified and is actually three coextruded PP microlayers where it is difficult to discern the interfaces). [Diagram 3] FIG. 3 is a partial cross-sectional scanning electron micrograph (SEM) at 15,000× magnification of the polyethylene sublayer (three microlayers of PE) of the nine microlayer trilayers of the three-layer membrane of FIG. 1 (the PE sublayer is enlarged). [Figure 4] FIG. 4 is a graph demonstrating the improved cycling behavior of an exemplary inventive construct compared to COM EX1. [Diagram 5] FIG. 5 is a graph demonstrating the compressive elasticity results of certain structures compared to COM EX1. [Figure 6] FIG. 6 is a graph demonstrating Mix P penetration test results of a structure compared to COM EX1. [Figure 7]FIG. 7 is a schematic diagram of how microlayers can be created in a feedblock by layer augmentation in a coextrusion process. [Figure 8] FIG. 8 is a schematic diagram of how microlayers can be created by delamination in a coextrusion process. [Figure 9] FIG. 9 is a cross-sectional scanning electron micrograph (SEM) at 5,000x magnification of an exemplary three layer or trilayer (nine microlayers total with three triple-microlayer sublayers laminated together) PP / PE / PP microporous membrane of the present invention (at least the outer PP sublayer is microporous). [Figure 10] Figure 10 is a surface scanning electron micrograph (SEM) at 3,000x magnification of the surface of the polypropylene surface sublayer (surface PP microlayer) of the 9-microlayer layer, 3-layer membrane of Figure 9. This 9-microlayer membrane could be used as one layer of a 3-layer (9 sublayer, 27 microlayer) membrane, for example, as shown in Figure 1. [Figure 11] FIG. 11 is a surface scanning electron micrograph (SEM) at 10,000x magnification of a portion of the surface of the polypropylene surface sub-layer (surface PP microlayer) of the 9-microlayer layer, 3-layer membrane of FIG. [Figure 12] FIG. 12 is a surface scanning electron micrograph (SEM) at 30,000x magnification of a portion of the surface of the polypropylene surface sub-layer (surface PP microlayer) of the nine-microlayer layer, three-layer membrane of FIG. [Figure 13]FIG. 13 is a cross-sectional scanning electron micrograph (SEM) at 5,000x magnification of an exemplary three "microlayer" coextruded sublayer (PO1 / PO2 / PO1) microporous membrane of the present invention, with microlayer PO2 made of a different resin or resin blend than microlayer PO1, more clearly showing the interfaces (interface zones) of adjacent coextruded microlayers (at least the outer PO1 microlayer is microporous). The multiple coextruded microlayer interfaces and lamination interfaces between adjacent sublayers are believed to impart the unique characteristics, properties and / or performance of the multilayer structure of the present invention. The sublayers in the example of FIG. 13 are made of three PP layers with a central PP layer of a different PP resin than the two outer layers, which had to be made with a thicker precursor due to the lower viscosity of the central PP layer (typically the microlayers were less than 4um, preferably less than 3um, more preferably less than 2um, respectively). [Figure 14] FIG. 14 is a markup of a portion of the SEM of FIG. 13, showing the interface zone with red and green horizontal lines. [Figure 15] FIG. 15 is an enlarged version of FIG. 13, showing the unique pore and membrane structures. [Figure 16] Figure 16 is a schematic representation of an exemplary 12um tri-layer according to at least one embodiment of the present invention (PP / PE / PP sublayers or microlayers laminated together, the sublayers are each different, the top PP sublayer has three coextruded PP microlayers, the middle PE sublayer has three PE microlayers that may be the same or different from each other, and the bottom PP sublayer has two PP blend microlayers and one PP microlayer). Figure 16 shows that many different embodiments are possible in one, 9-microlayer membrane, and that variations in the sublayers and individual microlayers are possible and sometimes desirable. For example, some PP may have to be added in the outermost PP microlayer to increase adhesion, wettability, lamination bond strength, and / or the like. [Figure 17]Figure 17 is a schematic representation of an exemplary 3, 9, 18, or 21 microlayer embodiment or example of the present invention (blue represents PP microlayers, yellow represents PE microlayers, and numbered black lines indicate interfaces). Figure 17 illustrates that many different embodiments are possible, and that variations in the use of PP or PE sublayers are possible and sometimes desirable. For example, one might add some PE in the outer or center sublayers to increase adhesion, wettability, lamination bond strength, or to provide center shutdown functionality, and / or the like. [Figure 18] FIG. 18 shows improved DB uniformity data in several examples of multi-layer products (EX1, EX3, EX6) compared to other more conventional three-layer products. [Figure 19] FIG. 19 is a graph demonstrating the improved cycling behavior of an exemplary inventive structure (EX1) compared to a conventional 12um trilayer product. The comparative film shown here is a 12um trilayer (PP / PE / PP) (no microlayer). This was done at a C-rate of C / 3 with a cutoff of 4.3V at 523NCM versus the graphite system. The data shown represents an average of 5 cells for each sample (or a total of 10 cells). We can see a repeatable improvement in cycle life in EX1 over the conventional trilayer, possibly due to improved electrolyte uptake due to increased interfacial area and pore structure complexity. [Figure 20] FIG. 20 lists a number of non-limiting, exemplary embodiments, features, advantages, or configurations of the present multi-layer products and concepts. [Figure 21]Figure 21 is a 10,000X cross-sectional SEM showing a 9 microlayer (each sublayer has 3 microlayers) PP / PE / PP sublayer that is about 14 um film with a central PE sublayer that is about 3.11 um thick (each PE microlayer is only about 1.037 um thick). Using the present invention, microlayer structures can be created from polyolefin resins with microlayers each 2 um or less thick, microlayers each 1.5 um or less thick, microlayers each 1.3 um or less thick, microlayers each 1.15 um or less thick, microlayers each 1.05 um or less thick, and / or the like that perform better than other PO films. [Figure 22A] Figure 22A shows data for several examples of multi-layer products (EX1, EX3, EX2, EX4, and EX6) compared to other more conventional three-layer products (COM EX1, COM EX3, COM EX2, COM EX4). Normalization of thickness and porosity helps to show some of the benefits of the new multi-layer structure. [Figure 22B] Figure 22B shows data for several examples of multi-layer products (EX1, EX3, EX2, EX4, and EX6) compared to other more conventional three-layer products (COM EX1, COM EX3, COM EX2, COM EX4). Normalization of thickness and porosity helps to show some of the benefits of the new multi-layer structure. [Figure 23] FIG. 23 shows further data for several examples of multi-layer products (EX1, EX3, EX4, and EX6) compared to other more conventional three-layer products (COM EX1, COM EX3, COM EX2, COM EX4). Normalization of thickness and porosity helps to show some of the benefits of the new multi-layer structure. Tortuosity was calculated by Nm=T2 / P, where Nm is the McMullin number, T is the tortuosity, and P is the porosity. [Figure 24] FIG. 24 includes an SEM image of a polypropylene layer of a multi-layer product according to some embodiments described herein. [Diagram 25] FIG. 25 contains an SEM image of the polypropylene layer of a more conventional three-layer product described herein. [Figure 26] FIG. 26 includes an SEM image of a polyethylene layer of a multi-layer product according to some embodiments described herein. [Figure 27] FIG. 27 contains an SEM image of the polyethylene layer of a more conventional tri-layer product described herein. [Figure 28] FIG. 28 includes SEM images showing a side-by-side comparison of the polypropylene layers of the tri-layer and multi-layer products described herein. [Figure 29] FIG. 29 contains SEM images showing a side-by-side comparison of the polyethylene layers of the tri-layer and multi-layer products described herein. [Diagram 30] FIG. 30 includes SEM images showing a side-by-side comparison of the three-layer or multi-layer products described herein. [Diagram 31] FIG. 31 is a table of DSC data for the polyethylene layers of the tri-layer and multi-layer products described herein. [Diagram 32] FIG. 32 is a table of DSC data for the polypropylene layers of the tri-layer and multi-layer products described herein. [Diagram 33] FIG. 33 is a graph showing a quantitative assessment of pore diameter distribution (using mercury intrusion porosimetry) of the tri-layer and multi-layer products described herein. [Diagram 34] FIG. 34 shows the normalization of x to x′ (in PP) according to the machine learning tests described herein. [Diagram 35] FIG. 35 shows the coefficients and boundary parameters (PP) from the machine learning studies described herein. [Diagram 36] FIG. 36 shows the normalization of x to x′ (in PE) according to the machine learning tests described herein. [Figure 37] FIG. 37 shows the coefficients and boundary parameters (PE) from the machine learning studies described herein. [Figure 38] FIG. 38 is a representative schematic representation of a coextruded multilayer precursor, membrane or separator according to some further embodiments described herein. [Figure 39] FIG. 39 is a representative schematic representation of a coextruded multilayer precursor, membrane or separator according to some further embodiments described herein. [Diagram 40] FIG. 40 is a representative schematic representation of a coextruded multilayer precursor, membrane or separator according to some further embodiments described herein. [Diagram 41] FIG. 41 is a representative schematic representation of a coextruded multilayer precursor, membrane or separator according to some further embodiments described herein. [Diagram 42] FIG. 42 is a representative schematic representation of a coextruded multilayer precursor, membrane or separator according to some further embodiments described herein. [Diagram 43] FIG. 43 is a representative schematic representation of a coextruded multilayer precursor, membrane or separator according to some further embodiments described herein. [Diagram 44] FIG. 44 is a representative schematic representation of a coextruded multilayer precursor, membrane or separator according to some further embodiments described herein. [Diagram 45] FIG. 45 is a representative schematic representation of a coextruded multilayer precursor, membrane or separator according to some further embodiments described herein. [Diagram 46] FIG. 46 is a representative schematic representation of a coextruded multilayer precursor, membrane or separator according to some further embodiments described herein. [Figure 47] FIG. 47 is a representative schematic representation of a coextruded multilayer precursor, membrane or separator according to some further embodiments described herein. [Figure 48] FIG. 48 is a representative schematic representation of a coextruded multilayer precursor, membrane or separator according to some further embodiments described herein. [Figure 49]FIG. 49 is a representative schematic representation of a coextruded multilayer precursor, membrane or separator according to some further embodiments described herein. [Figure 50] FIG. 50 is a representative schematic representation of a coextruded multilayer precursor, membrane or separator according to some further embodiments described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0054] The embodiments described herein may be more readily understood by reference to the following detailed description, examples, and figures. However, the elements, devices, and methods described herein are not limited to the specific embodiments presented in the detailed description, examples, and figures. It should be recognized that these embodiments are merely illustrative of the principles of the invention. Many changes and modifications will be readily apparent to those skilled in the art without departing from the spirit and scope of the invention.
[0055] Additionally, all ranges disclosed herein should be understood to encompass any and all subranges contained therein. For example, a range stated as "1.0 to 10.0" should be considered to include any and all subranges beginning with a minimum value equal to or greater than 1.0 and ending with a maximum value equal to or less than 10.0, such as 1.0 to 5.3, or 4.7 to 10.0, or 3.6 to 7.9.
[0056] All ranges disclosed herein should also be considered to include both ends of the range, unless expressly stated otherwise. For example, the range "between 5 and 10," "from 5 to 10," or "5-10" should generally be considered to include the ends 5 and 10.
[0057] Additionally, when the phrase "up to" is used in conjunction with an amount or quantity, it should be understood that the amount is at least a detectable amount or quantity. For example, a material present in an amount "up to" a specified amount may be present from a detectable amount up to and including the specified amount.
[0058] Described herein are: microporous multilayer films or membranes; battery separators comprising at least one of the microporous multilayer films or membranes; batteries, particularly lithium ion batteries, comprising at least one of the battery separators described herein, devices comprising the batteries described herein, and methods of making the microporous multilayer films or membranes.
[0059] The multilayer microporous films or membranes exhibit improved properties, particularly when compared to previous tri-layer and multi-layer microporous films of the same thickness, Gurley, and / or porosity. Improved film or membrane properties include, but are not limited to, improved puncture strength (gf) compared to previous tri-layer and multi-layer products, improved mixed penetration average (N) compared to previous tri-layer and multi-layer products, improved elongation (kgf / cm) compared to previous tri-layer and multi-layer products, and improved tensile strength (kgf / cm) compared to previous tri-layer and multi-layer products. 2 ), faster shutdown rates (Ω-cm) compared to previous tri-layer and multi-layer products 2 ), higher average dielectric breakdown (DB) values (V) compared to prior tri-layer and multi-layer products, lower DB standard deviation (V) compared to prior tri-layer and multi-layer products, higher minimum DB values (V) compared to prior tri-layer and multi-layer products, passing industrial nail penetration tests that prior tri-layer and multi-layer microporous thin films did not, and improved cycle life compared to past tri-layer and multi-layer products. The multi-layer microporous thin films herein have also been found to have a unique structure. The unique structure of these thin films explains many of the improved properties observed.
[0060] Battery separator The battery separator herein comprises, consists of, or consists essentially of a (i.e., one or more) multi-layered membrane or multi-layered microporous thin membrane, and optionally a coating layer on one or both sides of the membrane. The thin membrane itself, i.e., without the coating or any other additional components, exhibits the improved properties described above. The performance of the thin membrane can be improved by the addition of a coating or other additional components.
[0061] (1) Multilayer microporous thin film or membrane In some embodiments, the multilayer or multilayer microporous thin film comprises 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, 9 or more, 11 or more, 12 or more, 13 or more, 14 or more, 15 or more, 15 or more, 16 or more, 17 or more, 18 or more, 19 or more, 20 or more, 21 or more, 22 or more, 23 or more, 24 or more, 25 or more, 26 or more, 27 or more, 28 or more, 29 or more, 30 or more, 40 or more, 50 or more, 60 or more, 70 or more, 80 or more, 90 or more, or 100 or more layers. What is meant by the term "layer" is a monoextruded layer having a thickness of 2 to 20 microns. As will be understood by those skilled in the art, a monoextruded layer is a layer that is extruded by itself without any other layers. Also, each layer of a coextruded bilayer, trilayer, or multilayer thin film is considered to be a "layer" for purposes of determining whether a given battery separator is a multilayer battery separator. The number of layers in a coextruded bilayer is two, the number of layers in a coextruded trilayer is three, and the number of layers in a coextruded multilayer film is two or more, preferably three or more. The exact number of layers in a bilayer, trilayer, or multilayer coextruded film is determined by the die design, not necessarily the materials that are coextruded to form the coextruded film. For example, a coextruded bilayer, trilayer, or multilayer film may be formed using the same material to form each of the two, three, or four or more layers, and these layers are still considered to be separate layers even though each is made of the same material. The exact number is likewise determined by the die design. The layers of the coextruded bi-, tri- or multi-layered thin film each have a thickness of 0.01 to 20 microns, preferably 0.1 to 5 microns, and most preferably 0.1 to 3 microns, 0.1 to 2 microns, 0.1 to 1 micron, 0.01 to 0.9 microns, 0.01 to 0.8 microns, 0.01 to 0.7 microns, 0.01 to 0.6 microns, 0.01 to 0.5 microns, 0.01 to 0.4 microns, 0.01 to 0.3 microns, or 0.01 to 0.2 microns. These layers are microlayers.
[0062] In some embodiments, the multilayer microporous thin film or membrane disclosed herein comprises two or more, or preferably three or more coextruded layers. A coextruded layer is a layer formed by a coextrusion process. At least two, preferably at least three, consecutive coextruded layers may be formed by the same or separate coextrusion processes. For example, at least two or at least three consecutive layers may be formed by the same coextrusion process, two or more layers may be coextruded by one process, two or more layers may be coextruded by separate processes, and two or more layers formed by one process may be laminated to two or more layers formed by separate processes so that four or more consecutive coextruded layers are combined. In some preferred embodiments, two or more, or preferably three or more coextruded layers are formed by the same coextrusion process. For example, 2 or more, or preferably 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, 9 or more, 10 or more, 15 or more, 20 or more, 25 or more, 30 or more, 35 or more, 40 or more, 45 or more, 50 or more, 55 or more, or 60 or more coextruded layers may be formed by the same coextrusion process. In a further preferred embodiment, the extrusion process is carried out by extruding two or more polymer mixtures, which may be the same or different, without the use of a solvent. A preferred coextrusion process is a dry process, such as the Celgard® dry process.
[0063] In some embodiments, the multi-layer microporous film or multi-layer film described herein is made by forming a coextruded bi-layer (2 coextruded layers), tri-layer (3 coextruded layers), or multi-layer (2 or more, preferably 3 or more coextruded layers) film and then laminating the bi-layer, tri-layer, or multi-layer film to at least one, but preferably two, other films. The at least one, but preferably two, other films can be nonwoven films, mono-extruded films, or coextruded films. In a preferred embodiment, the other film is a coextruded film having the same number of coextruded layers as the coextruded bi-layer, tri-layer, or multi-layer film. For example, when a coextruded tri-layer film is formed, the other is also a coextruded tri-layer.
[0064] Lamination of a bi-layer, tri-layer, or multi-layer coextruded thin film with at least one other monoextruded mono-layer thin film or bi-layer, tri-layer, or multi-layer thin film may involve the use of heat, pressure, or preferably heat and pressure.
[0065] Polymers or copolymers that can be used in current battery separators are those that are extrudable. Such polymers are typically referred to as thermoplastic polymers.
[0066] In some embodiments, one or more of the layers of the multilayer microporous thin film or multilayer film comprises a polymer or copolymer, or a polymer or copolymer blend, preferably a polyolefin or a polyolefin blend.Polyolefin blends may comprise two or more different types of polyolefins, such as a mixture of polyethylene and polypropylene, a blend of two or more of the same type of polyolefins, each polyolefin having different properties, such as an ultra-high molecular weight polyolefin and a low or ultra-low molecular weight polyolefin, or a mixture of polyolefins with another type of polymer or copolymer, or any additive, as understood by those skilled in the art.
[0067] Polyolefins include, but are not limited to: polyethylene, polypropylene, polybutylene, polymethylpentene, copolymers thereof, and blends thereof. In some embodiments, the polyolefin can be an ultra-low molecular weight, low molecular weight, medium molecular weight, high molecular weight, or ultra-high molecular weight polyolefin, such as medium or high molecular weight polyethylene (PE) or polypropylene (PP). For example, ultra-high molecular weight polyolefins can have a molecular weight of 450,000 (450k) or more, such as 500k or more, 650k or more, 700k or more, 800k or more, 1000000 or more, 2000000 or more, 3000000 or more, 4000000 or more, 5000000 or more, 6000000 or more, etc. High molecular weight polyolefins can have a molecular weight in the range of 250k to 450k, such as 250k to 400k, 250k to 350k, or 250k to 300k. The medium molecular weight polyolefin may have a molecular weight of 150-250k, for example, 100k, 125k, 130k, 140k, 150k-225k, 150k-200k, 150k-200k, etc. The low molecular weight polyolefin may have a molecular weight in the range of 100k-150k, for example, 100k-125k. The ultra-low molecular weight polyolefin may have a molecular weight of less than 100k. The above values are weight average molecular weights. In some embodiments, higher molecular weight polyolefins may be used to increase the strength or other properties of the microporous multilayer membrane or battery, including those described herein. In some embodiments, lower molecular weight polymers, for example, medium, low, or ultra-low molecular weight polymers, may be beneficial. For example, without wishing to be bound by any particular theory, it is believed that the crystallization behavior of lower molecular weight polyolefins may result in microporous multilayer thin films having smaller pores resulting from at least the MD stretching process that forms the pores.
[0068] Exemplary thermoplastic polymers, blends, mixtures or copolymers other than polyolefin polymers, blends or mixtures include, but are not limited to: polyacetal (or polyoxymethylene), polyamides, polyesters, polysulfides, polyvinyl alcohol, polyvinyl esters, and polyvinylidene (PVDF, PVDF:HFP, PTFE, PEO, PVA, PAN, etc.). Polyamides (nylons) include, but are not limited to: polyamide 6, polyamide 66, nylon 10, 10, polyphthalamide (PPA), copolymers thereof, and blends thereof. Polyesters include, but are not limited to: polyester terephthalate, polybutyl terephthalate, copolymers thereof, and blends thereof. Polysulfides include, but are not limited to: polyphenyl sulfide, copolymers thereof, and blends thereof. Polyvinyl alcohols include, but are not limited to: ethylene-vinyl alcohol, copolymers thereof, and blends thereof. Polyvinyl esters include, but are not limited to: polyvinyl acetate, ethylene vinyl acetate, copolymers thereof, and blends thereof. Polyvinylidenes include, but are not limited to: fluorinated polyvinylidenes (e.g., polyvinylidene chloride, polyvinylidene fluoride), copolymers thereof, and blends thereof. Various materials may be added to the polymer. These materials are added to modify or improve the performance or properties of individual layers or the separator as a whole. Such materials include, but are not limited to: materials that may be added to lower the melting point of the polymer. Typically, multi-layer separators contain layers designed to close pores at a certain temperature that blocks the flow of ions between the electrodes of the battery. This function is commonly referred to as shutdown.
[0069] In some embodiments, each layer of a multilayer microporous film or multilayer film comprises, consists of, or consists essentially of a different polymer or copolymer or polymer or copolymer blend. In some embodiments, each layer comprises, consists of, or consists essentially of the same polymer or copolymer or polymer or copolymer blend. In some embodiments, alternating layers of a multilayer microporous film or multilayer film comprise, consist of, or consist essentially of the same polymer or copolymer or polymer or copolymer blend. In other embodiments, some of the layers of a multilayer film or microporous multilayer film comprise, consist of, or consist essentially of the same polymer or polymer blend, and some do not.
[0070] Although it may be preferred that each of the layers or microlayers comprises, consists of, or consists essentially of a polyolefin (PO), e.g., PP or PE, or PE+PP blends, mixtures, copolymers, and the like, it is contemplated that other polymers (PY), additives, agents, materials, fillers, and / or particles (M), and / or the like may be added or used and may form a layer or microlayer, e.g., PP+PY, PE+PY, PP+M, PE+M, PP+PE+PY, PE+PP+M, PP+PY+M, PE+PY+M, PP+PE+PY+M, or blends, mixtures, copolymers, and / or the like.
[0071] Also, the same, similar, different, or different PP or PE or PE+PP polymers, homopolymers, copolymers, molecular weights, blends, mixtures, copolymers, etc. may be used. For example, the same, similar, different, or different molecular weight PP, PE, and / or PP+PE polymers, homopolymers, copolymers, multipolymers, blends, mixtures, and / or the like may be used in each layer. Thus, the structure may include various combinations and subcombinations of PP, PE, PP+PE, PP1, PP2, PP3, PE1, PE2, PE3, PP1+PP2, PE1+PE2, PP1+PP2+PP3, PE1+PE2+PE3, PP1+PP2+PE, PP+PE1+PE2, PP1 / PP2, PP1 / PP2 / PP1, PE1 / PE2, PE1 / PE2 / PP1, PE1 / PE2 / PE3, PP1+PE / PP2, or other combinations or structures.
[0072] In some embodiments, one or more additives can be added to the outermost layer of the multilayer microporous thin film or multilayer film to improve its properties or the properties of the battery separator or battery containing it. The outermost layer can include PE, PP, or PE+PP in addition to the additive. For example, additives such as lithium stearate, calcium stearate PE beads, siloxanes, and polysiloxanes can be added to improve pin removal (i.e., to reduce the coefficient of friction of the thin film or film).
[0073] In addition, certain polymers, copolymers, or polymer or copolymer blends can be used in the outermost layer of a multilayer microporous thin film or membrane to improve its properties or the properties of the battery separator or battery containing it. For example, the addition of a high molecular weight polymer or copolymer in the outermost layer can improve puncture strength.
[0074] In a further embodiment, additives to improve oxidation resistance may be added to the outermost layer of the multilayer microporous thin film or membrane. The additives may be organic or inorganic, or polymeric or non-polymeric additives.
[0075] In some embodiments, the outermost layer of the multilayer film or membrane may comprise, consist of, or consist essentially of polyethylene, polypropylene, or mixtures thereof.
[0076] In some embodiments, the microporous multilayer film or membrane may include three or more distinct regions or sub-membrane areas. In preferred embodiments, one or more of the regions or sub-membrane areas may comprise, consist of, or consist essentially of two or more layers that may or may not be coextruded layers. In some preferred embodiments, two or more layers are coextruded layers. In some embodiments, there is a laminate barrier between a region or sub-membrane area and an adjacent region or sub-membrane area. A laminate barrier is formed when two surfaces, for example two surfaces of different films or layers, are laminated together using heat, pressure, but preferably heat and pressure. In some embodiments, the sub-membrane area has the following non-limiting structures: PP, PE, PP / PP, PP / PE, PE / PP, PE / PE, PP / PP / PP, PP / PP / PE, PP / PE / PE, PP / PE / PP, PE / PP / PE, PE / PE / PP, PP / PP / PP / PP, PP / PE / PE / PP, PE / PP / PP / PE, PP / PE / PP / PP. , PE / PE / PP / PP, PE / PP / PE / PP, PP / PE / PE / PE / PP, PE / PP / PP / PP / PE, PP / PP / PE / PP / PP, PE / PE / PP / PP / PE / PE, PP / PE / PP / PE / PP, PP / PP / PE / PE / PP / PP, PE / PE / PP / PP / PE / PE, PE / PP / PE / PP / PE / PP, PP / PE / PP / PE / PP / PE, PP / PP / PP / PE / PP / PP / PP, PE / PE / PE / PP / PE / PE / PE, PP / PE / PP / PE / PP / PE / PP, PE / PP / PE / PP / PE / PP / PE, PE / PP / PE / PP / PE / PP / PE / PP, PP / PE / PP / PE / PP / PE / PP / PE, PP / PP / PE / PE / PP / PP / PE / PE, PP / PE / P E / PE / PE / PE / PE / PP, PE / PP / PP / PP / PP / PP / PP / PE, PP / PP / PE / PE / PEPE / PP / PP, PP / PP / PP / PP / PE / PE / PE / PE, PP / PP / PP / PP / PE / PP / PP / PP / PP, PE / PE / PE / PE / PP / PE / PE / PE / PE, PP / PE / PP / PE / PP / PE / PP / PE / PP,PE / PP / PE / PP / PE / PP / PE / PP / PE, PE / PE / PE / PE / PE / PP / PP / PP / PP, PP / PP / PP / PP / PP / PE / PE / PE / PE, PP / PP / PP / PP / PP / P E / PE / PE / PE / PE, PE / PE / PE / PE / PE / PP / PP / PP / PP / PP, PP / PE / PP / PE / PP / PE / PP / PE / PP / PE, PE / PP / PE / PP / PE / PP / PE / PP / PE / PP, PE / PP / PP / PP / PP / PP / PP / PP / PP / PP / PP / PE, PP / PE / PE / PE / PE / PE / PE / PE / PE / PE / PE / PP, PP / PP / PE / PE / PP / PP / PP / PP / PE / PP / PP / PE / PP / PP, PE / PE / PP / PP / PP / PP / PP / PP / PP / PP / PP / PP / PE / PE, PP / PP / PP / PP / PP / PP / PP / PP / PP / PP / PE / PE / PP / PE / PE / PP / PP. Herein, PE stands for a layer or microlayer of a region or sub-membrane area that comprises, consists of, or essentially consists of PE, e.g., a coextruded layer or microlayer. Herein, PP stands for a layer or microlayer of a region or sub-membrane area that comprises, consists of, or essentially consists of PP, e.g., a coextruded layer or microlayer. The PE or PP of different layers or microlayers may be the same or different. Similar variations, including up to 50 layers or microlayers per region or sub-film area, particularly coextruded layers or microlayers, can be formed by suitable extrusion dies.
[0077] In one preferred embodiment, the coextruded precursor may have the structure (PP1 / PP2 / PP3) (PP3 / PP2 / PP1), (PP3 / PP3 / PP2 / PP1 / PP1), (PP3 / PP3 / PP2 / PP2 / PP1 / PP1), (PP3 / PP3 / PP3 / PP2 / PP2 / PP2 / PP1 / PP1 / PP1), etc.
[0078] PP1 is made of homopolymer PP and additives, including optional anti-slip or anti-block additives, such as polysiloxanes or siloxanes, to modify the surface friction coefficient. PP2 may be made of the same or different PP homopolymer as PP1, and copolymers of PP. The PP copolymers may be any propylene-ethylene or ethylene-propylene random copolymers, block copolymers, or elastomers. PP3 may be made of the same or different homopolymer PP as PP1 and PP2, and also includes additives to modify the surface friction coefficient, which may be the same or different from those used in PP1.
[0079] In other preferred embodiments, the coextruded precursor may have the structure (PP1 / PP2 / PP3)(PP3 / PP2 / PP1), (PP3 / PP3 / PP2 / PP1 / PP1), (PP3 / PP3 / PP2 / PP2 / PP1 / PP1), (PP3 / PP3 / PP3 / PP2 / PP2 / PP2 / PP1 / PP1 / PP1), etc. PP1 may be any polypropylene blend. PP2 may be made of any PP block copolymer, including those described herein. PP3 may be made of the same or different PP-block copolymer used in PP2.
[0080] The regions or sub-membrane areas may be arranged in any order to form a microporous multilayer membrane or a microporous multilayer thin film. For example, the microporous multilayer membrane or the microporous multilayer thin film may have the following non-limiting structures: (PP / PP)(PE / PE) / (PP / PP); (PE / PE)(PP / PP)(PE / PE); (PP / PE)(PP / PE)(PP / PE); (PP / PE)(PE / PP)(PE / PP); (PP / PP / PP)(PE / PE / PE)(PP / PP / PP); (PE / PE / PE)(PP / PP / PP)(PE / PE / PE); (PP / PE / PP)(PE / PP / PE)(PP / PE / PP); (PP / PP / PE)(PE / PE / PE)(PE / PP / PP); (PE / PE / PP)(PP / PP / PP)(PP / PE / PE); (PE / PP / PE) / (PP / PE / PP)(PE / PP / PE); (PP / PE / PP)(PE / PP / PE)(PP / PE / PP); (PP / PE / PP)(PP / PE / PP)(PP / PE / PP); (PP / PP / PP)(PP / PP / PP)(PP / PP / PP); (PE / PE / PE)(PE / PE / PE)(PE / PE / PE); (PE / PE / PE)(PP)(PE / PE / PE); (PP / PP / PP)(PE)(PP / PP / PP); (PE / PE / PE)(PP / PP)(PE / PE / PE); (PP / PP / PP)(PE / PE)(PP / PP / PP); (PE / PP / PE)(PP)(PE / PP / PE); (PP / PE / PP)(PE)(PP / PE / PP); (PE / PP / PE)(PP / PP)(PE / PP / PE); (PP / PE / PP)(PE / PE)(PP / PE / PP); (PP / PP / PP / PP)(PE)(PP / PP / PP / PP); (PE / PE / PE / PE)(PP)(PE / PE / PE / PE); (PP / PP / PP / PP / PP)(PE)(PP / PP / PP / PP / PP); (PE / PE / PE / PE / PE)(PP / PP)(PE / PE / PE / PE / PE); (PP / PP / PP / PP / PP)(PE / PE / PE / PE / PE)(PP / PP / PP / PP / PP); (PE / PE / PE / PE / PE / PE)(PP / PP / PP / PP / PP)(PE / PE / PE / PE / PE);(PP / PE / PP / PE / PP) (PE / PP / PE / PP / PE) (PP / PE / PP / PE / PP); (PE / PP / PE / PP / PE) (PP / PE / PP / PE / PP) (PE / PP / PE / PP / PE). Variations of the above may be used to form microporous multilayer thin films or membranes having up to 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, or 200 layers or microlayers;
[0081] The thickness of the microporous multilayer film or membrane is not particularly limited, but is preferably less than 50 microns, less than 40 microns, less than 30 microns, less than 25 microns, less than 20 microns, less than 19 microns, less than 18 microns, less than 17 microns, less than 16 microns, less than 15 microns, less than 14 microns, less than 13 microns, less than 12 microns, less than 11 microns, less than 10 microns, less than 9 microns, less than 8 microns, less than 7 microns, less than 6 microns, or less than 5 microns. This is the thickness of the multilayer film or membrane before any coatings or treatments are applied.
[0082] Microporous, as used herein, means that the average pore size of the thin film, membrane, or coating is 2 microns or less, preferably 1 micron or less, 0.9 microns or less, 0.8 microns or less, 0.7 microns or less, 0.6 microns or less, 0.5 microns or less, 0.4 microns or less, 0.3 microns or less, 0.2 microns or less, preferably 0.1 microns or less, 0.09 microns or less, 0.08 microns or less, 0.07 microns or less, 0.06 microns or less, 0.05 microns or less, 0.04 microns or less, 0.03 microns or less, 0.02 microns or less, or 0.01 microns or less. In a preferred embodiment, the pores may be formed, for example, by performing a stretching process on the precursor thin film, such as is done in the Celgard® dry process.
[0083] In some preferred embodiments, the multilayer microporous thin film or membrane includes sub-membranes or regions that comprise, consist of, or consist essentially of PE, which are microporous and have an average pore size between 0.03 and 0.1, preferably between 0.05-0.09, 0.05-0.08, 0.05-0.07, or 0.05-0.06.
[0084] In another preferred embodiment, the multilayer microporous thin film or membrane PP comprises sub-membranes or regions that consist of or consist essentially of, which are microporous and have an average pore size between 0.02 and 0.06, preferably between 0.03 and 0.05, more preferably between 0.04 and 0.05 or 0.03 and 0.04.
[0085] In some other preferred embodiments, the multilayer microporous thin film or membrane comprises sub-membranes or regions that comprise, consist of, or consist essentially of PP, or comprises sub-membranes or regions that comprise, consist of, or consist essentially of PE, and the average pore size of the PP sub-membrane or region is smaller than that of the PE sub-membrane or region.
[0086] The Gurley of the microporous multilayer film or membrane is not so limited and may have any Gurley that makes it acceptable for use as a battery separator. In some embodiments, the microporous multilayer film or membrane described herein has a JIS Gurley (s / 100cc) of 150 or more, 160 or more, 170 or more, 180 or more, 190 or more, 200 or more, 210 or more, 220 or more, 230 or more, 240 or more, 250 or more, 260 or more, 270 or more, 280 or more, 290 or more, 300 or more, 310 or more, 320 or more, 330 or more, 340 or more, or 350 or more.
[0087] The porosity of the microporous multilayer thin film is not critical. For example, any porosity that can form an acceptable battery separator is acceptable. In some embodiments, the porosity of the thin film or membrane can be 10-60%, 20-60%, 30-60%, or 40-60%.
[0088] The microporous multilayer film or membrane may have a high uncoated puncture strength of 290 gf or more, 300 gf or more, 310 gf or more, 320 gf or more, 330 gf or more, 340 gf or more, 350 gf or more, or 400 gf or more.
[0089] The microporous multilayer thin film or membrane may have any average dielectric breakdown consistent with the goals described herein. In some embodiments, the average dielectric breakdown value is improved or higher than that of a tri-layer microporous thin film having at least one of the same thickness, Gurley, and porosity. For example, it may be 1-35% higher, 5-35% higher, 10-35% higher, 15-35% higher, 20-35% higher, 25-35% higher, or 30-35% higher than that of a tri-layer microporous thin film having the same thickness, Gurley, and / or porosity.
[0090] The minimum dielectric breakdown value of a microporous multilayer film or membrane is not particularly limited. In some embodiments, the minimum value may be improved (or higher) than that of a three-layer microporous membrane having the same thickness, Gurley, and / or porosity. For example, the minimum dielectric breakdown value may be 3-20% higher, 5-15% higher, 10-15% higher, 5-10% higher, 3-10% higher, 3-15% higher, 15-20% higher, 10-20% higher, or 5-20% higher than that of a three-layer microporous membrane having the same thickness, Gurley, and / or porosity.
[0091] The standard deviation of the dielectric breakdown values is also not so limited. In some embodiments, the standard deviation is improved (or lower) compared to a three-layer microporous thin film having the same thickness, Gurley, and / or porosity. For example, the standard deviation may be 10-55% lower, 10-50% lower, 10-45% lower, 10-40% lower, 10-35% lower, 10-30% lower, 10-25% lower, 10-20% lower, or 10-15% lower.
[0092] The higher average DB value, minimum DB value, and lower DB standard deviation indicate that the thin films can be used to provide safer battery separators and batteries. Dielectric breakdown is the voltage value at which current begins to flow across the insulator. Higher values clearly indicate a separator that can withstand higher voltages. The higher minimum value is also important because a battery separator is only as safe as its weakest point. A higher average value is not good if one point in the film breaks down at a lower value. The lower standard deviation of DB values for the multilayer microporous thin films described herein indicates consistency in the safety of the microporous multilayer thin films described herein.
[0093] The mixed intrusion average (N) of the microporous multilayer thin films or membranes described herein is also not so limited. For example, the mixed intrusion value can be 380N or more, 390N or more, 400N or more, 410N or more, 420N or more, 440N or more, 450N or more, 460N or more, 470N or more, 480N or more, 500N or more, 510N or more, 520N or more, 550N or more, 560N or more, 580N or more, 600N or more, 620N or more, 640N or more, 660N or more, 680N or more, 690N or more, 700N or more, 710N or more, 720N or more, 740N or more, 750N or more, or 760N or more.
[0094] The MD shrinkage of the multilayer microporous thin films or membranes described herein is not particularly limited, but is preferably lower than that of the conventional three-layer microporous thin films, for example, the MD shrinkage (%) at 105° C. is less than 3%, preferably less than 2.5%, more preferably less than 2% or less than 1.5%, and most preferably less than 1%.
[0095] The MD tensile strength of the microporous multilayer thin film is not particularly limited, but is preferably high. For example, 1800 kgf / cm 2 Super, 2000kgf / cm 2 Super, 2100kgf / cm 2 Super, 2200kgf / cm 2 Super, 2250kgf / cm 2 Super, 2300kgf / cm 2 Super, 2400kgf / cm 2 or over 2500kgf / cm 2 It's super.
[0096] The MD elongation of the microporous multilayer thin film is not particularly limited, for example, in some embodiments, it is greater than 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, or 60%.
[0097] The TD tensile strength of the microporous multilayer thin film is not particularly limited. For example, in some embodiments, the TD tensile strength is 120 kgf / cm 2 Above, 125kgf / cm 2 Above, 130kgf / cm 2 Above, 135kgf / cm 2 Over 140kgf / cm 2 Above, 145kgf / cm 2 Above, 150kgf / cm 2 Above, 155kgf / cm 2 Above, 160kgf / cm 2 Above, 165kgf / cm 2 Above, 170kgf / cm 2 Above, 175kgf / cm 2Above, 180kgf / cm 2 Above, 185kgf / cm 2 or more, or 190kgf / cm 2 or more, or 195kgf / cm 2 That's all.
[0098] The TD elongation of the microporous multilayer thin film is not particularly limited, and may be, for example, greater than 500%, greater than 550%, greater than 600%, greater than 650%, greater than 700%, greater than 750%, greater than 800%, greater than 850%, greater than 900%, greater than 950%, or greater than 1000%.
[0099] The shutdown temperature of the microporous multilayer thin film is not particularly limited, but is preferably 120°C or higher, 130°C or higher, 140°C or higher, 150°C or higher, 160°C or higher, 170°C or higher, 180°C or higher, 190°C or higher, or 200°C or higher.
[0100] The shutdown speed of the microporous multilayer thin film is not particularly limited, but is preferably 6,000 Ω-cm 2 More than 7,000Ω-cm 2 More than 8,000Ω-cm 2 More than 9,000Ω-cm 2 More than 10,000Ω-cm 2 More than 11,000Ω-cm 2 More than 12,000Ω-cm 2 More than 13,000Ω-cm 2 More than 14,000Ω-cm 2 More than 15,000Ω-cm 2 More than 16,000Ω-cm 2 More than 17,000Ω-cm 2 More than 18,000Ω-cm 2 More than 19,000Ω-cm 2 or more than 20,000 Ω-cm 2 That's all.
[0101] A higher shutdown speed also indicates a safer battery separator: the faster a battery can be shut down, the greater its ability to prevent thermal runaway.
[0102] In some embodiments, the microporous multilayer or thin films described herein may surprisingly exhibit increased strength performance, as defined by reduced tear or reduced tendency to tear, when compared to known battery separators of the same (or greater) thickness, particularly when compared to known dry process battery separators of the same (or greater) thickness. The improved tear or tear may be quantified by the test method disclosed herein as Composite Tear Index (CSI), and new or improved separators formed from the films or thin films described herein may have an improved CSI.
[0103] Regarding the structural features of the microporous multilayer thin films and membranes described herein, in some embodiments, the tortuosity of the thin films is greater than 1.6, greater than 1.7, greater than 1.8, greater than 1.9, greater than 2.0, greater than 2.1, or greater than 2.2. Without wishing to be bound by any particular theory, it is believed that the observed tortuosity values, particularly values greater than 2.0, 2.1, or 2.2, may be responsible for the increased puncture strength and mixed penetration average values disclosed herein. The more tortuosity thin films are also believed to be safer when used as battery separators for lithium ion batteries.
[0104] The McMullin numbers of the microporous multilayer films or membranes described herein are greater than 5.0, greater than 5.5, greater than 6.0, greater than 6.5, greater than 7.0, greater than 7.5, greater than 8.0, greater than 8.5, greater than 9.0, greater than 9.5, greater than 10.0, or greater than 10.5.
[0105] In some embodiments, the electrical resistivity of the microporous multilayer film or membrane is greater than 0.9, greater than 1.0, greater than 1.1, greater than 1.2, greater than 1.3, greater than 1.4, greater than 1.5, greater than 1.6, or greater than 1.7.
[0106] The crystallinity of the microporous multilayer thin film described herein has been found to be different from that of previous multilayer and trilayer thin films. For example, in some embodiments where a microporous multilayer thin film includes: (1) a first region including two or more layers; (2) a second region including two or more layers on a first surface of the first region; and (3) a third region including two or more layers on a surface opposite to the first surface of the first region, at least one of the first, second, or third regions includes PE and has a lower crystallinity as measured by DSC than the PE-containing layer of the trilayer microporous thin film when the trilayer microporous thin film has the same thickness as the multilayer microporous thin film. For example, the crystallinity may be 1-20% lower, 1-19%, 1-18%, 1-17%, 1-16%, 1-15% lower, 1-14%, 1-13%, 1-12%, 1-11%, 1-10%, 1-9%, 1-8%, 1-7%, 1-6%, 1-5%, 1-4%, 1-3%, or 1-2% lower than the PE-containing layer of the tri-layer microporous thin film when the tri-layer microporous thin film has the same thickness as the multi-layer microporous thin film.
[0107] Another structural difference between the multilayer microporous thin films described herein and previous tri-layer and multilayer thin films can be seen using a scanning electron microscope. See, for example, Figures 25-31. For example, as shown in Figures 25-31, a multilayer microporous thin film or membrane can include at least a first region including two or more layers and a second region including at least one layer. The first region can include a largely discontinuous amorphous region when viewed in the z-direction of the film using an SEM. By "mostly" it is meant that most, but not necessarily all, of the amorphous region in the first layer is discontinuous. This can mean that at least 50%, more than 50%, more than 60%, more than 70%, more than 80%, more than 90%, more than 95%, more than 99%, or 100% of the amorphous region in the first layer is continuous. "Discontinuous amorphous regions" means that when a sample of the first layer is analyzed, for example by SEM, the path of the amorphous regions is interrupted or blocked by crystalline (lamellar) regions along the entire thickness of the first layer. Discontinuous means that the path of the amorphous regions is interrupted or blocked by crystalline (lamellar) regions along the entire thickness of the first layer. The path of the amorphous regions does not orbit the crystalline (lamellar) regions. Instead, the crystalline (lamellar) regions completely interrupt the path of the amorphous regions along the entire thickness of the first layer. The path of the amorphous regions may be linear or circuitous. An example of the difference between discontinuous and continuous amorphous regions can be seen by comparing the SEM of the polyethylene layer of COM EX4 with the SEM of polyethylene layer RO397 in FIG. 29. Discontinuous can also mean that the amorphous regions are non-columnar, non-vertically continuous, or non-pillar-like along the thickness of the layer. In some preferred embodiments, the first region, which is a predominantly discontinuous amorphous region, may comprise, consist of, or consist essentially of polypropylene in some or all of the layers in that region. In some other embodiments, the second region comprises two or more layers and the amorphous area of that region of the film or membrane has a maximum width of 0.85 microns, 0.8 microns, 0.75 microns, 0.70 microns, 0.65 microns, or 0.6 microns.For example, this can be seen by comparing COM EX4 with R037 in Figure 30. In some preferred embodiments, the second region may comprise, consist of, or consist essentially of polyethylene in some or all of the layers in the region.
[0108] (2) Optional Coating In some embodiments, one or more coating layers may be applied to one or two sides of a microporous membrane or thin film to form a battery separator. In some embodiments, one or more of the coatings may be a ceramic coating that includes, consists of, or consists essentially of a polymeric binder and organic and / or inorganic particles. In some embodiments, only a ceramic coating is applied to one or both sides of a microporous membrane or thin film. In other embodiments, a different coating may be applied to the microporous membrane or thin film before or after application of the ceramic coating. A different additional coating may also be applied to one or both sides of the membrane or thin film. In some embodiments, the different polymeric coating layers may include, consist of, or consist essentially of at least one of polyvinylidene difluoride (PVdF) or polycarbonate (PC).
[0109] In some embodiments, the thickness of the coating layer is less than about 12 μm, optionally less than 10 μm, optionally less than 9 μm, optionally less than 8 μm, optionally less than 7 μm, optionally less than 5 μm. In at least certain selected embodiments, the coating layer is less than 4 μm, less than 2 μm, or less than 1 μm.
[0110] The coating method is not particularly limited, and the coating layer described herein can be coated onto the porous structure by at least one of the following coating methods: extrusion coating, roll coating, gravure coating, printing, knife coating, air knife coating, spray coating, dip coating, or curtain coating. The coating process can be carried out at room temperature or at an elevated temperature.
[0111] The coating layer may be one of non-porous, nanoporous, microporous, mesoporous, or macroporous. The coating layer may have a JIS Gurley of 700 or less, optionally 600 or less, 500 or less, 400 or less, 300 or less, 200 or less, or 100 or less.
[0112] One or more layers, treatments, materials, or coatings (CT) and / or nets, meshes, mats, wovens or nonwovens (NW) may be added to one or both surfaces or within a multilayer film or membrane (M) described herein, which may include CT / M, CT / M / CT, NW / M, NW / M / NW, CT / M / NW, CT / NW / M / NW / CT, CT / M / NW / CT, etc.
[0113] method The method of forming the multilayer microporous thin film or membrane described herein is not so limited and may be a dry process, preferably the CELGARD® dry-stretch process, a dry process such as BNOPP, or a wet process utilizing a solvent or oil.
[0114] The method of forming a multilayer microporous film or membrane described herein includes at least the following steps: (1) coextrusion of two or more polymer mixtures, which may be the same or different, to form a coextruded film having two or more layers or microlayers, as described herein above; (2) laminating the coextruded film to at least one other monoextruded film, coextruded film, or nonwoven, in some preferred embodiments, the coextruded film is laminated to two other coextruded films having two or more microlayers; and (3) optionally, one or more further steps.
[0115] (1) Co-extrusion process Coextrusion is not so limited. An exemplary coextrusion process is shown in FIG. 7, and a coextrusion die is shown in FIG. 8. In some embodiments, a coextrusion die is used with one or more extruders feeding the die. Typically, there is one extruder for each desired layer or microlayer of the final coextruded thin film. For example, when the desired coextruded thin film has three microlayers, three extruders are used with the coextrusion die. In at least one embodiment, the film of the present invention can be composed of many microlayers or nanolayers, with the final product containing 50 or more layers of individual microlayers or nanolayers. In at least some embodiments, the microlayer or nanolayer technique can be triggered by a pre-encapsulation feedblock before entering a cast film or blown film die.
[0116] In some preferred embodiments, the coextrusion is a bubble coextrusion process, and the blow ratio can vary from 0.5 to 2.0, preferably from 0.7 to 1.8, and most preferably from 0.9 to 1.5. After coextrusion using this blow ratio, the film can be MD stretched, MD and then TD stretched (with or without MD relaxation), or simultaneously MD and TD stretched. The film can be optionally calendered to further control the porosity.
[0117] Benefits of coextrusion include, but are not limited to, an increase in the number of layers (interfaces), which is said to improve puncture strength, without wishing to be bound by any particular theory. Coextrusion is also said to result in an observed improvement in DB, without wishing to be bound by any particular theory. Specifically, the improvement in DB may be related to the reduced PP pore size observed when a coextrusion process is used. Coextrusion also allows for a wider range of material options by incorporating blends in the microlayers. Coextrusion also allows for the formation of thin tri-layer or multi-layer films (coextrusion films). For example, tri-layer coextrusion films with thicknesses of 8 or 10 microns or less can be formed. Coextrusion allows for higher MD elongation, different pore structures (less PP, more PE). Coextrusion can be combined with lamination to create the desired multi-layer structures of the present invention. For example, structures are as formed in the examples.
[0118] The minimum achievable thickness is determined by the extrusion process. In some examples, the thinnest PP microlayer may be about 0.19 mil (sublayer of about 4.83 um), and the PE is about 0.17 mil (sublayer is about 4.32 um), with 0.19 mil or 0.17 mil for each of the three microlayer layers of PP and PE, respectively. For one example 21-layer structure, the inventors have found that it can have about 1.14 mil of PP (or 0.57 mil on each side) and 0.17 mil of PE, with a total extrusion thickness of 1.31 mil (33 um). The inventors may be able to make a 21-layer product of only 30 um or less with this configuration.
[0119] (2) Lamination is not so limited and includes bringing a surface of a coextruded thin film together with a surface of at least one other thin film and using heat, pressure, and / or heat and pressure to secure such two surfaces together. Heat can be used, for example, to increase the viscosity of either or both surfaces of the coextruded thin film and at least one other thin film making lamination easier, thereby making the two surfaces tacky and better able to adhere together.
[0120] In some preferred embodiments, the laminate formed by laminating the coextruded thin film to at least one other thin film is a precursor for a subsequent MD and / or TD stretching step, with or without relaxation. In some embodiments, the coextruded thin film is stretched before lamination.
[0121] (3) Further processing The further steps may include, consist of, or consist essentially of MD, TD, or sequential or simultaneous MD and TD stretching steps. The stretching step may occur before or after the lamination step. The stretching may be performed with or without MD and / or TD relaxation. Co-pending and commonly owned U.S. Patent Application Publication No. US2017 / 0084898A1, published March 23, 2017, is hereby incorporated by reference in its entirety.
[0122] Other additional steps may include calendaring. For example, in some embodiments, a calendaring step may be performed as a means to reduce pore size and / or porosity, and / or reduce thickness as a means to further improve the transverse direction (TD) tensile strength and / or puncture strength of the porous biaxially stretched membrane precursor. Calendaring may also improve strength, wettability, and / or uniformity, and may also reduce surface layer defects that may be introduced during the manufacturing process, for example, during the MD and TD stretching process. Calendared thin films or membranes may have improved coatability (using smooth calendar rolls). In addition, the use of textured calendaring rolls may help improve coating adhesion to the thin film or membrane.
[0123] Calendering may be cold (below room temperature), ambient (room temperature), or hot (e.g., 90° C.) and may involve the application of pressure or the application of heat and pressure to controllably reduce the thickness of the film or thin film. Calendering may be in one or more steps, such as low pressure calendering followed by calendering at higher pressure, cold calendering followed by hot calendering, and / or the like. Additionally, the calendering process may use at least one of heat, pressure, and speed to densify the heat-sensitive material. Additionally, the calendaring process can use uniform or non-uniform heat, pressure, and / or speed to selectively densify the thermally sensitive material, impart uniform or non-uniform calendaring conditions (e.g., use of smooth rolls, rough rolls, patterned rolls, micropatterned rolls, nanopatterned rolls, speed changes, temperature changes, pressure changes, humidity changes, double roll processes, multiple roll processes, or combinations thereof) to produce improved, desired or unique structure, characteristics, and / or performance, and to produce or control the resulting structure, characteristics, and / or performance, and / or the like.
[0124] Another further step may include pore filling. The pore filling step is not so limited and may be performed in any manner consistent with the goals described herein. For example, in some embodiments, the pores may be partially or completely coated, treated, or filled with a pore filling composition, material, polymer, gel polymer, layer, or deposition (PVD). Preferably, the pore filling composition covers 50% or more, 60% or more, 70% or more, 80% or more, 90% or more, 95% or more, etc. of the surface area of the pores. The pore filling composition may comprise, consist of, or consist essentially of a polymer and a solvent. The solvent may be any suitable solvent useful for forming a composition for coating or filling pores, including an organic solvent such as octane, water, or a mixture of an organic solvent and water. The polymer may be any suitable polymer, including an acrylate polymer, or a polyolefin, including low molecular weight polyolefins. The concentration of the polymer in the pore-filling composition is not particularly limited as long as the viscosity of the pore-filling composition is such that the composition is capable of coating the walls of the pores of any of the porous biaxially stretched precursor membranes disclosed herein, but may be between 1% and 30%, between 2% and 25%, between 3% and 20%, between 4% and 15%, between 5% and 10%, etc. Pore-filling increases either or both of the machine direction (MD) and transverse direction (TD) tension.
[0125] Composites, vehicles, or devices A composite material comprising the battery separator described hereinabove and one or more electrodes, such as an anode, a cathode, or an anode and a cathode, disposed in direct contact therewith. The type of electrode is not particularly limited. For example, the electrode may be suitable for use in a lithium ion secondary battery.
[0126] Suitable anodes may have an energy capacity of 372 mAh / g or more, preferably ≧700 mAh / g, and most preferably ≧1000 mAH / g. The anodes are composed of lithium metal or lithium alloy foils (e.g., lithium aluminum alloys), or mixtures of lithium metal and / or lithium alloys with materials such as carbon (e.g., coke, graphite), nickel, copper. The anodes are not simply made of lithium-containing intercalation compounds or lithium-containing insertion compounds.
[0127] Suitable cathodes may be any cathode compatible with the anode and may include intercalation compounds, insertion compounds, or electrochemically active polymers. Suitable intercalation materials include, for example, MoS2, FeS2, MnO2, TiS2, NbSe3, LiCoO2, LiNiO2, LiMn2O4, VO 13 , V2O5, and CuCl2. Suitable polymers include, for example, polyacetylene, polypyrrole, polyaniline, and polythiophene.
[0128] Any of the separators described herein above may be incorporated into any vehicle, such as an electric vehicle, or device that is fully or partially battery powered, such as a cell phone or laptop computer.
[0129] Various embodiments of the present invention have been described in order to achieve various objectives of the present invention. It should be recognized that these embodiments are merely illustrative of the principles of the present invention. Many changes and modifications will be readily apparent to those skilled in the art without departing from the spirit and scope of the invention. EXAMPLES
[0130] Preparation of Examples Inventive (multi-layer) products were prepared and compared to comparative (tri-layer) products. The multi-layer products were formed by the methods described herein, which include co-extruding three separate films comprising three coextruded layers, and laminating the three films together. The tri-layer products were formed by forming three separate extruded monolayer films and laminating the monolayers together.
[0131] The microlayer composition of the product of the invention prepared is as follows:
[0132] Example 1 (EX1) - (PP / PP / PP) (PE / PE / PE) (PP / PP / PP) - all PP layers are made of homopolymer PP, density = 0.90 g / cm 3 All PE layers have a melt index between 0.25 and 0.5 g / 10 min at 2.16 kg and 190 °C, and a viscosity of 0.955 to 0.966 g / cm 3 It is made of a blend of 95% high density polyethylene with a density range of 100 / 100 / 200 / 100 and 5% mLLDPE.
[0133] Example 2 (EX2) - (PP1 / PP2 / PP1) (PE1 / PE2 / PE3) (PP1 / PP2 / PP1) - PP1 is homopolymer PP. PP2 is homopolymer polypropylene with higher MFR than PP1. PE1 is high density polyethylene with melt index between 0.25-0.5 g / 10 min at 2.16 kg and 190°C. PE2 is ultra high density polyethylene. PE3 is high density polyethylene with melt index between 0.25-0.5 g / 10 min at 2.16 kg and 190°C and 0.955-0.966 g / cm 3 The blend is 95% high density polyethylene having a density range of 100 / 100 / 200 / 100 / 250 / 200 / 100 / 250 / 200 / 100 / 250 / 100 / 150 / 250 / 100 / 250 / 1 ...250 / 150 / 150 / 250
[0134] Example 3 (EX3) - (PP / PP / PP) (PE1 / PE2 / PE1) (PP / PP / PP) - PP layer is made of homopolymer PP, density = 0.90 g / cm 3, with MFR ranging from 0.5MFR to 2MFR. PE1 is made of high density polyethylene with melt index between 0.25 to 0.5g / 10min at 2.16kg and 190℃. PE2 is made of ultra-high molecular weight polyethylene.
[0135] Example 4 (EX4) - (PP / PP / PP) (PE / PE / PE) (PP / PP / PP) - all PP layers are made of homopolymer PP, density = 0.90 g / cm 3 All PE layers have a melt index between 0.25 and 0.5 g / 10 min at 2.16 kg and 190 °C, and a density of 0.955 to 0.966 g / cm 3 It is made of a blend of 95% high density polyethylene and 5% mLLDPE, with densities ranging from 0.01 to 0.05.
[0136] Example 5 (EX5) - PP / PP / PP) (PE / PE / PE) (PP / PP / PP) - all PP layers are made of homopolymer PP, density = 0.90 g / cm 3 All PE layers have a melt index between 0.25 and 0.5 g / 10 min at 2.16 kg and 190 °C, and a density of 0.955 to 0.966 g / cm 3 It is made of a blend of 95% high density polyethylene and 5% mLLDPE, with densities ranging from 0.01 to 0.05.
[0137] Example 6 (EX6) - (PP / PP / PP) (PE / PE / PE) (PP / PP / PP) - PP is made of homopolymer PP, density = 0.90 g / cm 3 , with an MFR ranging from 0.5MFR to 2MFR. PE is made of high density polyethylene with a melt index between 0.25 to 0.5g / 10min at 2.16kg and 190℃.
[0138] Example 7 - (EX7) - (PP / PP / PP) (PE / PE / PE) (PP / PP / PP) - all PP layers are made of homopolymer PP, density = 0.90 g / cm3 All PE layers have a melt index between 0.25 and 0.5 g / 10 min at 2.16 kg and 190 °C, and a density of 0.955 to 0.966 g / cm 3 It is made of a blend of 95% high density polyethylene and 5% mLLDPE, with densities ranging from 0.01 to 0.05.
[0139] Example 8 (EX8) - (PP1 / PP2 / PP1) (PE1 / PE2 / PE1) (PP1 / PP2 / PP1) PP1 is homopolymer PP, density = 0.90 g / cm 3 , with an MFR ranging from 0.5 MFR to 2 MFR. PP2 is made of homopolymer PP, with an MFR of 0.25 and a density of 0.9. PE1 is a high density polyethylene with a melt index between 0.25 and 0.5 g / 10 min at 2.16 kg and 190°C. PE2 is an ultra-high molecular weight polyethylene.
[0140] Example 9 (EX9) - (PP1 / PP2 / PP1) (PE / PE / PE) (PP1 / PP2 / PP1) - PP1 is made of homopolymer PP, density = 0.90 g / cm 3 , MFR in the range of 0.5MFR to 2MFR. PP2 has a density of 0.90g / cm 3 , is a blend of 95% homopolymer PP with MFR ranging from 0.5 MFR to 2 MFR and 5% propylene-ethylene copolymer. PE is a blend of 92% high density polyethylene with melt index between 0.25-0.5 g / 10 min at 2.16 kg and 190°C and 8% olefin block copolymer.
[0141] Example 10 (EX10) - (PP / PP / PP) (PE / PE / PE) (PP / PP / PP) - all PP layers are made of homopolymer PP, density = 0.90 g / cm 3 All PE layers have a melt index between 0.25 and 0.5 g / 10 min at 2.16 kg and 190 °C, and a density of 0.955 to 0.966 g / cm3 It is made of a blend of 95% high density polyethylene and 5% mLLDPE, with densities ranging from 0.01 to 0.05. Referring primarily to Figures 38-50 and further multi-layer embodiments, further Examples 11-38 are as follows:
[0142] Example 11 - Each PP and PE layer of the three-layer structure is itself made of multiple layers, preferably coextruded and then laminated - (PP / PP / PP) (PE / PE / PE) (PP / PP / PP) - all PP layers are made of homopolymer PP, density = 0.90 g / cm 3 All PE layers have a melt index between 0.25 and 0.5 g / 10 min at 2.16 kg and 190 °C, and a density of 0.955 to 0.966 g / cm 3 It is made of a blend of 95% high density polyethylene and 5% mLLDPE, with densities ranging from 0.01 to 0.05.
[0143] Example 12 - (PP1 / PP2 / PP3) - PP1 is a polypropylene blend, PP2 is a PP block copolymer, and PP3 is the same as PP1, PP2 or a different blend or block copolymer.
[0144] Example 13 - (PP1 / PP1) or (PP2 / PP2) or (PP1 / PP2) - PP1 is a polypropylene blend and PP2 is a PP block copolymer.
[0145] Example 14 - (PP1 / PP1 / PP1) or (PP2 / PP2 / PP2) - PP1 is a polypropylene blend and PP2 is a PP block copolymer.
[0146] Example 15 - (PP1 / PP2 / PP3) - PP1 is a polypropylene blend, PP2 is a PP block copolymer, and PP3 is the same or a different PP block copolymer.
[0147] Example 16 - (PP3 / PP2 / PP1) / (PP3 / PP2 / PP1) - PP1 is a polypropylene blend, PP2 is a PP block copolymer, and PP3 is the same or a different PP block copolymer.
[0148] Example 17 - (PP1 / PP2 / PP3) / (PP3 / PP2 / PP1) - PP1 is a polypropylene blend, PP2 is a PP block copolymer, and PP3 is the same or a different PP block copolymer.
[0149] Example 18 - (PP1 / PP2) / (PP3 / PP1) - PP1 is a polypropylene blend, PP2 is a PP block copolymer, and PP3 is the same or a different PP block copolymer.
[0150] Example 19 - (PP1 / PP2 / PP3 / PP1) - PP1 is a polypropylene blend, PP2 is a PP block copolymer, and PP3 is the same or a different PP block copolymer.
[0151] Example 20 - (PP1 / PP2 / PP3) - PP1 is a polypropylene blend, PP2 is a PP block copolymer, and PP3 contains an adhesion promoter.
[0152] Example 21 - (PO3 / PP2 / PP1) - PP1 is a polypropylene blend, PP2 is a PP block copolymer, and PO3 is a polyolefin blend (eg PP+PE).
[0153] Example 22 - (PP1 / PP2 / PP3) - PP1 is a homopolymer PP + additives as described herein that may include any slip or block additives such as siloxanes that modify the coefficient of friction. PP2 is the same or different homopolymer PP as used in PP1, including a copolymer PP that may be any propylene ethylene or ethylene-propylene random copolymer, block copolymer, or elastomer. PP3 is the same or different homopolymer PP as in PP1 and PP2 + additives that modify the surface coefficient of friction (COF), the same or different as used in PP1.
[0154] Example 23 - (PP3 / PP2 / PP1) - PP1 is a homopolymer PP + additives as described herein that may include any slip or block additives such as siloxanes that modify the coefficient of friction (COF). PP2 is the same or different homopolymer PP as used in PP1 and PP3, and includes a copolymer PP that may be any propylene ethylene or ethylene-propylene random copolymer, block copolymer, or elastomer. PP3 includes the same or different homopolymer PP as in PP1 and PP2 + additives that modify the surface coefficient of friction, the same or different from those used in PP1.
[0155] Example 24 - (PP3 / PP2 / PP1) or (PP1 / PP2 / PP3) - PP1 is homopolymer PP + additives described herein that may include any slip or block additives such as siloxanes that modify the coefficient of friction (COF). PP2 is the same or different homopolymer PP used in PP1 and PP3 + copolymer PP that may be any propylene ethylene or ethylene-propylene random copolymer, block copolymer or elastomer. PP3 is the same or different homopolymer PP used in PP1 and PP2 + copolymer PP that may be any propylene ethylene or ethylene-propylene random copolymer, block copolymer or elastomer.
[0156] The composition of the layers of the comparative product may be as follows: Comparison – Typical mono-ply PP (e.g. Celgard 2500) Comparison – Typical three-ply laminate (PP / PE / PP) Comparison - Typical monolayer PP or typical three-layer (PP / PE / PP) in a typical ceramic coated version
[0157] Example 25: A coextruded PP precursor is proposed with the following structure: Homopolymer PP + additives to modify surface COF ---------------------- Homopolymer PP + Copolymer PP ---------------------- Homopolymer PP + additives to modify surface COF
[0158] The additives for surface modification may include any slip or anti-block additive such as siloxane. The copolymer may be any propylene-ethylene or ethylene-propylene random copolymer, block copolymer or elastomer.
[0159] The coextruded PP precursor can be extruded at a blow ratio (BUR) anywhere between 0.9 and 1.5 to control the porosity. The coextruded PP precursor is then either sequentially MD-then TD-oriented or simultaneously biaxially oriented. The biaxially oriented film can be further calendered to control the porosity.
[0160] Example 26: A second proposed structure can be made for battery separator or textile applications as follows:
[0161] PP Blend -------------- PP Block Copolymer -------------- PP Block Copolymer
[0162] This structure allows the design of a higher tortuosity surface layer for water barrier in high velocity water tests.
[0163] The types of copolymers that can be incorporated into the structure include, but are not limited to, propylene-ethylene or ethylene-propylene random copolymers, block copolymers or elastomers.
[0164] By extruding PP in a coextrusion format, the surface characteristics of the PP layer can be modified while incorporating a lower melting copolymer resin interlayer to reduce the shutdown temperature. Different copolymer resins can also be incorporated anywhere in the structure to control the porosity of the TD stretched film.
[0165] The incorporation of BUR into the precursor film allows for further control of the porosity required for various applications.
[0166] Example 27 - (PP1 / PP2 / PP3) (PP1 / PP2 / PP3) (PP1 / PP2 / PP3) - PP1 is a polypropylene blend, PP2 is a PP block copolymer, and PP3 is the same or a different PP block copolymer.
[0167] Example 28 - (PP3 / PP2 / PP1) / (PP3 / PP2 / PP1) / (PP3 / PP2 / PP1) - PP1 is a polypropylene blend, PP2 is a PP block copolymer, and PP3 is the same or a different PP block copolymer.
[0168] Example 29 - (PP3 / PP2 / PP1) (PP1 / PP2 / PP3) (PP3 / PP2 / PP1) PP1 is a polypropylene blend, PP2 is a PP block copolymer, and PP3 is the same or a different PP block copolymer.
[0169] Example 30 - (PP1 / PP2 / PP3) (PP3 / PP2 / PP1) (PP1 / PP2 / PP3) PP1 is a polypropylene blend, PP2 is a PP block copolymer, and PP3 is the same or a different PP block copolymer.
[0170] Example 31 - (PP1 / PP2 / PP3) (PP3 / PP2 / PP1) (PP3 / PP2 / PP1) PP1 is a polypropylene blend, PP2 is a PP block copolymer, and PP3 is the same or a different PP block copolymer.
[0171] Example 32 - (PP3 / PP2 / PP1) (PP1 / PP2 / PP3) (PP1 / PP2 / PP3) PP1 is a polypropylene blend, PP2 is a PP block copolymer, and PP3 is the same or a different PP block copolymer.
[0172] Example 33 - (PP1 / PP2 / PP3) (PP1 / PP2 / PP3) (PP1 / PP2 / PP3) - PP1 is homopolymer PP + additives as described herein that may include any slip or block additives such as siloxanes that modify the coefficient of friction. PP2 is the same or different homopolymer PP as used in PP1 and PP3 + copolymer PP that may be any propylene ethylene or ethylene-propylene random copolymer, block copolymer or elastomer. PP3 is the same or different homopolymer PP as used in PP1 and PP2 + additives that modify the surface coefficient of friction that may be the same or different as used in PP1.
[0173] Example 34 - (PP3 / PP2 / PP1) / (PP3 / PP2 / PP1) / (PP3 / PP2 / PP1) - PP1 is homopolymer PP + additives as described herein that may include any slip or block additives such as siloxanes that modify the coefficient of friction. PP2 is the same or different homopolymer PP as used in PP1 and PP3 + copolymer PP that may be any propylene ethylene or ethylene-propylene random copolymer, block copolymer or elastomer. PP3 is the same or different homopolymer PP as used in PP1 and PP2 + additives that modify the surface coefficient of friction that may be the same or different as used in PP1.
[0174] Example 35 - (PP3 / PP2 / PP1) (PP1 / PP2 / PP3) (PP3 / PP2 / PP1) PP1 is a homopolymer PP + additives as described herein that may include any slip or block additives such as siloxanes that modify the coefficient of friction. PP2 is the same or different homopolymer PP as used in PP1 and PP3 + copolymer PP that may be any propylene ethylene or ethylene-propylene random copolymer, block copolymer or elastomer. PP3 is the same or different homopolymer PP as used in PP1 and PP2 + additives that modify the surface coefficient of friction, the same or different from those used in PP1.
[0175] Example 36 - (PP1 / PP2 / PP3) (PP3 / PP2 / PP1) (PP1 / PP2 / PP3) PP1 is a homopolymer PP + additives as described herein that may include any slip or block additives such as siloxanes that modify the coefficient of friction. PP2 is the same or different homopolymer PP as used in PP1 and PP3 + copolymer PP that may be any propylene ethylene or ethylene-propylene random copolymer, block copolymer or elastomer. PP3 is the same or different homopolymer PP as used in PP1 and PP2 + additives that modify the surface coefficient of friction that may be the same or different as used in PP1.
[0176] Example 37 - (PP1 / PP2 / PP3) (PP3 / PP2 / PP1) (PP3 / PP2 / PP1) PP1 is homopolymer PP + additives as described herein that may include any slip or block additives such as siloxanes that modify the coefficient of friction. PP2 is the same or different homopolymer PP as used in PP1 and PP3 + copolymer PP that may be any propylene ethylene or ethylene-propylene random copolymer, block copolymer or elastomer. PP3 is the same or different homopolymer PP as used in PP1 and PP2 + additives that modify the surface coefficient of friction that may be the same or different as used in PP1.
[0177] Example 38 - (PP3 / PP2 / PP1) (PP1 / PP2 / PP3) (PP1 / PP2 / PP3) PP1 is a homopolymer PP + additives as described herein that may include any slip or block additives such as siloxanes that modify the coefficient of friction. PP2 is the same or different homopolymer PP as used in PP1 and PP3 + copolymer PP that may be any propylene ethylene or ethylene-propylene random copolymer, block copolymer or elastomer. PP3 is the same or different homopolymer PP as used in PP1 and PP2 + additives that modify the surface coefficient of friction that may be the same or different as used in PP1.
[0178] The layer composition of one comparative product was prepared as follows:
[0179] Comparative Example 1 (COM EX1) - (PP) (PE) (PP) - All PP layers are made of homopolymer PP, density = 0.90 g / cm 3 All PE layers have a melt index between 0.25 and 0.5 g / 10 min at 2.16 kg and 190 °C, and a viscosity of 0.955 to 0.966 g / cm 3 It is made of a blend of 95% high density polyethylene with a density range of 100 / 100 / 200 / 100 and 5% mLLDPE.
[0180] Comparative Example 2 (COM EX2) - (PP) (PE) (PP) - All PP layers are made of homopolymer PP, density = 0.90 g / cm 3 All PE layers have a melt index between 0.25 and 0.5 g / 10 min at 2.16 kg and 190 °C, and a viscosity of 0.955 to 0.966 g / cm 3 It is made of a blend of 95% high density polyethylene with a density range of 100 / 100 / 200 / 100 and 5% mLLDPE.
[0181] Comparative Example 3 (COM EX3) - (PP)(PE)(PP) - All PP layers are made of homopolymer PP, density = 0.90 g / cm 3 All PE layers have a melt index between 0.25 and 0.5 g / 10 min at 2.16 kg and 190 °C, and a viscosity of 0.955 to 0.966 g / cm 3 It is made of a blend of 95% high density polyethylene with a density range of 100 / 100 / 200 / 100 and 5% mLLDPE.
[0182] Comparative Example 4 (COM EX4) - (PP)(PE)(PP) - All PP layers are made of homopolymer PP, density = 0.90 g / cm 3 All PE layers have a melt index between 0.25 and 0.5 g / 10 min at 2.16 kg and 190 °C, and a viscosity of 0.955 to 0.966 g / cm 3 It is made of a blend of 95% high density polyethylene with a density range of 100 / 100 / 200 / 100 and 5% mLLDPE.
[0183] Comparative Example 5 (COM EX5) - (PP) (PE) (PP) - All PP layers are made of homopolymer PP, density = 0.90 g / cm 3 All PE layers have a melt index between 0.25 and 0.5 g / 10 min at 2.16 kg and 190 °C, and a viscosity of 0.955 to 0.966 g / cm3 It is made of a blend of 95% high density polyethylene with a density range of 100 / 100 / 200 / 100 and 5% mLLDPE.
[0184] Characterization of the Examples - Separator Properties and Battery Performance Thickness (μm) The thickness is measured in micrometers μm using an Emveco Microgage 210-A micrometer thickness tester and test procedure ASTM D374. The thicknesses of Examples 1-6 and Comparative Examples 1-4 were determined and are reported in the tables in Figures 22 and 23. Comparative Examples with thicknesses comparable to the Examples were prepared so that the separators could be meaningfully compared.
[0185] Basic weight (mg / cm 2 ) The basis weights of Examples 1-6 and Comparative Examples 1-4 were determined and are reported in the table in FIG.
[0186] JIS Gurley (s / 100cc) Gurley is defined herein as in Japanese Industrial Standard (JIS Gurley) and is measured herein using an OHKEN Permeability Tester. JIS Gurley is defined as the time in seconds required for 100 cc of air to pass through a 1 square inch membrane at a constant pressure of 4.9 inches of water. The JIS Gurley of Examples 1-6 and Comparative Examples 1-4 was measured and reported in the table in FIG. 22.
[0187] MD shrinkage rate (%) at 105℃ / 1 hour Shrinkage is measured by placing a test sample between two pieces of paper, which are then clamped together to hold the sample between the papers and suspend in an oven. For the "105°C for 1 hour" test, the sample is placed in an oven at 105°C for 1 hour. After the indicated heating time in the oven, each sample is removed and taped to a flat opposing surface using double-sided adhesive tape, the sample is flattened and smooth, and the exact length and width are measured. Shrinkage is measured in both machine direction (MD) and transverse direction (TD) and is expressed as MD shrinkage (%) and TD shrinkage (%).
[0188] The MD shrinkage rates of Examples 1 to 6 and Comparative Examples 1 to 4 were measured and are reported in the table in FIG.
[0189] MD tensile strength (kgf / cm 2 ) The machine direction (MD) tensile strength is measured using an Instron Model 4201 according to the ASTM-882 procedure. The MD tensile strengths of Examples 1-6 and Comparative Examples 1-4 were measured and are reported in the table in FIG.
[0190] MD elongation (%) MD elongation at break (%) is the percentage of the elongation of the test sample along the machine direction of the test sample measured at the maximum tensile strength required to break the sample. The MD elongation of Examples 1-6 and Comparative Examples 1-4 was measured and is reported in the table in FIG.
[0191] TD tensile strength (kgf / cm 2 ) The transverse direction (TD) tensile strength is measured according to the ASTM-882 procedure using an Instron Model 4201. The TD tensile strengths of Examples 1-6 and Comparative Examples 1-4 were measured and are reported in the table in FIG.
[0192] TD Elongation (%) TD elongation at break (%) is the percentage of the elongation of the test sample along the transverse direction of the test sample measured at the maximum tensile strength required to break the sample. The TD elongation of Examples 1-6 and Comparative Examples 1-4 was measured and is reported in the table in FIG.
[0193] Puncture strength (gf) The puncture strength is measured using an Instron Model 4442 based on ASTM D3763. The measurement is performed across the width of the microporous membrane, and the puncture strength is defined as the force required to puncture the test sample. The puncture strength of Examples 1-6 and Comparative Examples 1-4 was measured and reported in the table in FIG. 22.
[0194] One idea is to use UHMW polymers to increase puncture strength. However, these polymers, which may have molecular weights greater than 1,000,000, cause processing difficulties, especially when the process is a dry process, such as the CELGARD® dry process. By utilizing these techniques, the need to use polymers with molecular weights greater than 1M, which can be very difficult to process, especially in dry process membranes, can be alleviated.
[0195] DB average (V) A voltage is applied to the separator film until dielectric breakdown of the sample is observed. A strong separator exhibits a high DB. Any non-uniformity in the separator film will cause a lower DB value. A battery separator with a higher average DB, especially a higher minimum DB value, will make the battery safer when used in a battery. The average DB of Examples 1-6 and Comparative Examples 1-4 were measured and are reported in the table in FIG. 22.
[0196] DB minimum value (V) A voltage is applied to the separator film until the dielectric breakdown of the sample is observed. A strong separator shows a high DB. Any non-uniformity in the separator film will cause a lower DB value. A battery separator with a higher average DB, and especially a higher minimum DB value, will make the battery safer when used in a battery. The minimum DB for Examples 1-6 and Comparative Examples 1-4 were measured and are reported in the table in FIG. 22.
[0197] DB uniformity The DB values of Examples 1, 4, and 5 were compared to Comparative Examples 1, 2, and 4. The results are shown in Figure 18. The DB standard deviations were calculated and are reported.
[0198] Mixed penetration average (N) Mixed penetration is the force required to cause a short circuit through a separator when placed between a cathode material and an anode material. This test is used to indicate the tendency of a separator to cause a short circuit during assembly of a battery. Details of this method are described in US2010 / 209758, which is incorporated herein in its entirety. Mixed penetration values for Examples 1-6 and Comparative Examples 1-4 were calculated and are reported in the table in FIG. 22.
[0199] Nail penetration test Examples 1-9 and Comparative Examples 1-5 were tested and Examples 1 and 6 passed the nail penetration test. None of the Comparative Examples passed the nail penetration test. Nail penetration tests at velocities of 1 cm / sec and 10 cm / sec are described in U.S. Patent No. 9,065,152, the entirety of which is incorporated herein by reference.
[0200] Shutdown Temperature (℃) Shutdown start temperature is 100W×cm 2 Resistance readings were recorded and reported in ° C. Shutdown temperatures for Examples 1-6 and Comparative Examples 1-4 were measured and are reported in the table in FIG.
[0201] Shutdown Speed (Ω-cm 2 ) The example thin film is sandwiched between two nickel disks and wetted with PC solvent. The wetted separator stack is then subjected to a temperature ramp of 60°C / min. The resistance between the two nickel disks is monitored by a multimeter for the duration of the test. The definition of shutdown in this test is a resistance of 100 W×cm 2 ~10,000W×cm 2 The shutdown rate should increase by two orders of magnitude from 100 W x cm and is normalized by the time required for this resistance increase. 2 The shutdown speeds are reported in units of / second. The shutdown speeds of Examples 1 to 6 and Comparative Examples 1 to 4 were measured and are reported in the table in FIG.
[0202] ER(Ω-cm 2 ) The ER method uses an electrolyte solution composed of a solvent mixture of DI water and 2-propanol. Electrical resistance is assessed by sequentially adding four circular separator disks (38 mm diameter) between two metal electrodes. The resistance of the separator is measured in Ω using an LCR meter and then multiplied by the area of the electrodes to obtain Ω-cm 2 The resistivity of the electrolyte is measured using a YSI meter.
[0203] calculation: 1) The average separator resistance of successive separator layers, (Ω) = (R 層4 Ω-R 層3 Ω+R 層3 Ω-R 層2 Ω / 2 2) Electrical resistance, Ω-cm 2 = average resistance of successive separator layers Ω * Nickel plating electrode area cm 2 The QC-ER was determined for Examples 1 to 6 and Comparative Examples 1 to 4. The results are reported in the table in FIG.
[0204] McMullin number The electrical resistivity (ER) measurements are used to calculate the McMullen number, which is calculated as follows: McMullen number = (electrical resistivity, Ω-cm 2 / separator thickness, cm) / electrolyte resistivity (Ω-cm).
[0205] The McMullin numbers were determined for Examples 1 to 6 and Comparative Examples 1 to 4. They are reported in the table in FIG.
[0206] Cycle Life All cycling was performed in constant current (CC) mode. The cathode used was 523NMC. The anode used was superior graphite. The electrolyte was 1M LiPF6 salt in EC:EMC solvent 3:7 v:v. The voltage window was 3.0-4.3V. Cycles 1-5 had charge and discharge rates of C / 10. Cycles 6-10 had charge and discharge rates of C / 5. Cycles 11-15 had charge rates of C / 5 and C / 2. Cycles 16-20 had charge rates of C / 5 and 1C (charge / discharge rate capacity; 1C is the full charge or discharge rate in 60 minutes). Cycles 21-25 had charge rates of C / 5 and 5C. Cycles 26-30 had charge rates of C / 5 and 10C. Cycles 31-35 had charge and discharge rates of C / 10.
[0207] The cycle life of Example 1 and Comparative Example 1 was compared. This was done at a C rate of C / 3 with a cutoff of 4.3 V at 523 NCM for the graphite system. The data shown presents an average of 5 cells for each sample (or a total of 10 cells). The results are shown in FIG. 19. Without wishing to be bound by any particular theory, this is likely due to improved electrolyte uptake due to increased interfaces, e.g., lamination interfaces, and the complexity of the pore structure. Repeatable improvements in cycle life for the multilayer product compared to the conventional trilayer are shown by this test.
[0208] Compression Elasticity Compressive modulus was evaluated using a TMA Q400 and a hemispherical probe. A 5mm x 5mm sample was compressed at a constant rate up to 1N (568N / cm2) and then released with the pressure returning at a constant rate to 0N at ambient temperature. The percentage of dimensional change during compression and recovery is estimated based on the initial thickness of the sample. Example 1 and Comparative Example 1 were tested for compressive elasticity. The results are reported in Figure 5 and Table 1 below.
[0209] [Table 1]
[0210] The microlayer structure imparts higher compression recovery than comparable wet process membranes. In certain applications, less squeeze and / or better compression recovery may be desirable.
[0211] Pin Removal Pin removal data for the installation was collected using a pin removal winding machine. The machine is equipped with a 45 mm slit roll and a separator roll is placed on the machine onto a split pin mandrel (4 mm diameter). The separator is wound onto the mandrel and the pins are pulled apart. The maximum removal force is recorded and reported in Newtons. For each test sample, the outer diameter is held constant and the film tension and length are varied based on the film thickness. It is best to compare films of the same or nearly the same thickness.
[0212] Characterization of the Examples - Structural Properties AQ porosity (%) The porosity of the microporous thin film samples was measured using ASTM method D-2873 and is defined as the void percentage in the microporous membrane measured in both the machine direction (MD) and the transverse direction (TD). The AQ porosity for Examples 1-6 and Comparative Examples 1-4 was calculated and is reported in the table in Figure 22. Some additional porosity data for Example 1 was determined and is reported in Table 2 below:
[0213] [Table 2]
[0214] Aquaporeporosity(%) The Aquapore (AQ) porosity for Examples 1-6 and Comparative Examples 1-4 was measured and is reported in the table in FIG.
[0215] AQ PP pore diameter (μm) Pore size is measured using an Aquapore available through Porous Materials Inc. (PMI). Pore size is expressed in μm. AQ PP pore size for Examples 1-6 and Comparative Examples 1-4 was calculated and is reported in the table in FIG. 22. Further data for Examples 1, 9, and 10 was obtained and is reported in Table 2.
[0216] AQ PE pore diameter (μm) Pore size is measured using an Aquapore available through Porous Materials Inc. (PMI). Pore size is expressed in μm. AQ PE pore sizes for Examples 1-6 and Comparative Examples 1-4 were determined and are reported in the table in FIG. 22. Further data for Examples 1, 9, and 10 were determined and are reported in Table 2.
[0217] AQ surface area (m 2 / g) Aquapore is a water intrusion measurement technique and is only available for testing base membranes. In this measurement, a large area of the membrane is immersed in water and pressurized to 3,000 psi. The results of the test are the overall porosity of the membrane (reported in %), the PP and / or PE pore size (reported in μm), and the inner and outer surface areas of the pores (m 2 The aquapore surface area was determined for Examples 1-6 and Comparative Examples 1-4 and is reported in the table in FIG. 22. Further data was determined for Examples 1, 9, and 10 and is reported in Table 2.
[0218] Pore diameter distribution The pore diameter distributions of Examples 6 and 11 and Comparative Example 4 were measured using mercury intrusion porosimetry, and the results are shown in Figure 33. The pore diameters in Comparative Example 4 were larger and had a narrower distribution than in the inventive example.
[0219] Calculated bending degree. The degree of bending was calculated according to the following formula (1): N m =T 2 / P(1), In the formula, N m is the McMullin number, T is the tortuosity, and P is the porosity. Without wishing to be bound by any particular theory, it is believed that battery separators with higher tortuosity are safer. The reason for this is believed to be that it is more difficult for dendrites to grow between the electrodes due to the more tortuous path that the growing dendrites must take to travel from the anode to the cathode. The calculated tortuosity for Examples 1-6 and Comparative Examples 1-4 are given in the table in FIG. 23.
[0220] SEM image 1. Processing conditions Procedure for cross-sectional observation using a scanning electron microscope (SEM). a.) Cut the sample to an appropriate size (a few mm square). b.) A flat cross section is produced by ion milling (MD-ND plane). Ion milling equipment: E-3500 (Hitachi High-Technologies Corporation.) Ion source: Ar+ Accelerating voltage: 3.5 kV Discharge voltage: 2.0kV Stage control: 5 (set value) Processing time: 4 hours Temperature: 20~25℃ c.) The sample is attached to a stub using double-sided carbon conductive tape and carbon paste. d.) An osmium plasma coating is applied to render the sample conductive. 2. SEM Observation Conditions a.) Equipment: S-4800 (Hitachi High-Technologies Corporation.) Acceleration voltage: 1kV Working distance: Approx. 5 mm
[0221] SEM images were taken of Examples 1, 2, 4, and 6 and Comparative Examples 1, 4, and 5. Some of these images are shown in Figures 24-30. It was found that there were distinct structural differences between the multi-layered products in the Examples and the three-layered products in the Comparative Examples. For example, the amorphous regions of the multi-layered PP region (having three layers of PP in the Examples) were mostly discontinuous and non-columnar, while the PP layers of the three-layered products contained more cylindrical or vertically continuous amorphous regions. The side-by-side comparisons in Figures 28-30 show these differences between the multi-layered and three-layered products.
[0222] Machine Learning Test DETAILED STEPS 1: Image feature extraction to obtain vectors for machine learning · Read image by OpenCV python module cv2 Obtain 50 240x160 pixel^2 subimages at uniformly random positions from either the PP or PE regions and normalize the images by using cv2.normalize with α=0, β=255 and norm_type=cv2.NORM_MINMAX. For each subimage, use the SIFT feature detector cv2.x features 2d.SIFT_create with default settings to obtain features with angle and size. Convert each angle a of the obtained features to a'=90-|a mod 180-90|. For i from 1 to 9, called the bin count, [10 * (i-1), 10 * Count the number of angles a' transformed in the range [i] Concatenate the bin count, the average feature size (a scalar) and the number of features (a scalar) to obtain the feature vector x k (11 dimensions) (kth image) Take the median values of 11 features from the 50 subimages and use them as the feature vector x of the input image.
[0223] Conventions for the OpenCV python module cv2 include Python Machine Learning by Raschka (ISBN1783555130) and OpenCV by Python Blueprints by Michael Beyeler (1785282697), both of which are incorporated herein by reference in their entirety. More information on OpenCV can be found at https: / / en.wikipedia.org / wiki / OpenCV.
[0224] Example of PP layer: After obtaining the feature vector x from the PP layer by step 1 described below, each value in x is transformed into the following average vector m=[0.121252742025, 0.0932702969461, 0.0637613832138, 0.0471628522627, 0.0410994787666, 0.0455612990903, 0.0663893557564, 0.143913936237, 0.373695714612, 3.470413863, 569.8305 08475] and standardize as x'=(xm) / s using standard deviation vector s=[0.0177890460233, 0.0126226741459, 0.0109280746046, 0.00952236047605, 0.00919810029221, 0.00802167410741, 0.00965575771023, 0.0135729399588, 0.0556357096109, 0.181326979354, 52.6681415756] · Let w be [-2.29884147179, -0.120953660963, 0.609748975014, -0.354807579078, 0.0742943451505, -0.0596756155513, 0.679531409197, 1.18484320645, 0.639551068782, -0.123277373445, 0.495565514875], and the dot product is w T x' Calculate ·w T If x'>-1.27465281948, classify the image as 9 layers.
[0225] Example of PE layer: After obtaining the feature vector x from the PE layer by step 1 described below, each value in x is transformed into the following average vector m=[0.0753659021681, 0.0647442404474, 0.052445934828, 0.0441842705626, 0.0424971059836, 0.0495261454071 , 0.0745156791392, 0.15315494777, 0.434028151238, 3.51412063686, 480.02173913] and standard deviation vector s = [0.0212709138539, 0.0156303526361, 0.0100887199823, 0.00610554172426, 0.00588628646619, 0.00509466227247, 0.00868424601387, 0.0177249443105, 0.0499726205047, 0.217925555283, 60.5317430669] and standardize w as [0.0026717153, -0 .2072501509, -0.4883326802, 0.0172248418, -0.5467527574, -0.3892225728, 0.7356477088, 1.1574408691, -1.1992044378, -1.920101147, 0.1068808983, 0.6542173447] and take the inner product as w T x' Calculate ·w TIf x'>-0.6542173447, classify the image as 9 layers. Examples 1, 2, 4, 7, 8, and 10, and Comparative Examples 1, 4, and 5 were subjected to a machine learning test to determine whether the comparative (three-layer) examples and the inventive (multi-layer) examples could be distinguished by the test. The results are shown in Figures 34 to 37. The comparative (three-layer) examples and the inventive (multi-layer) examples could be distinguished.
[0226] DSC DSC analysis was performed to determine the melting point (T m ) and to determine the onset of crystallization. A Netzsch DSC200F3 model is used with a sealed aluminum sample holder with a perforated lid. Nitrogen is used as carrier gas at 40 ml / min to prevent oxidation of the samples. The mass of the analyzed samples varies between 5 and 6 mg. T m The sample is first subjected to a heat treatment to erase the thermal history in order to determine the onset of crystallization and crystallization. The instrument then performs another heating and cooling cycle at 10°C / min starting from 25°C to 300°C. Data acquisition and handling is performed by Proteus Analysis software. Examples 1, 3, 5, and 6 and Comparative Examples 1, 2, 3, and 4 were evaluated by DSC. The PE and PP layers were evaluated separately. The results are shown in Figures 31 and 32.
[0227] According to at least selected embodiments, the present application, disclosure and inventions relate to new or improved membranes, separator films, separators, battery separators, lithium secondary battery separators, multilayer membranes, multilayer separator films, multilayer separators, multilayer battery separators, multilayer lithium secondary battery separators, and / or multilayer battery separators, new or improved batteries, capacitors, fuel cells, lithium batteries, lithium ion batteries, lithium secondary batteries, and / or lithium ion secondary batteries, and / or methods of making and / or using such membranes, separator films, separators, battery separators, lithium secondary battery separators, batteries, capacitors, fuel cells, lithium batteries, lithium ion batteries, lithium secondary batteries, and / or lithium ion secondary batteries, and / or devices, vehicles or products comprising same. According to at least certain embodiments, the present disclosure or inventions relate to new or improved membrane layers, membranes or separator films, battery separators comprising such membranes, and / or related methods. According to at least certain selected embodiments, the disclosure or invention relates to new or improved porous polymeric or separator membranes, battery separators including such membranes, and / or related methods. According to at least certain embodiments, the disclosure or invention relates to new or improved microporous polyolefin or separator membranes, microlayer membranes, multilayer membranes including one or more microlayers or nanolayer membranes, battery separators including such membranes, and / or related methods. According to at least certain embodiments, the disclosure or invention relates to new, optimized, or improved microporous stretched polymeric or separator membranes having one or more new or improved outer and / or inner layers, microlayer membranes, multilayered microporous or separator membranes having outer and inner layers, some of such layers or sublayers being produced by coextrusion and then laminated together to form said new, optimized, or improved membrane or separator membrane.In some embodiments, a layer, microlayer, or nanolayer may comprise a homopolymer, copolymer, block copolymer, elastomer, and / or polymer blend. In selected embodiments, at least a layer, microlayer, or nanolayer may comprise a different or distinct polymer, homopolymer, copolymer, block copolymer, elastomer, and / or polymer blend. The present disclosure or invention also relates to new or improved methods of making such membranes, separator membranes, or separators, and / or new or improved methods of using such membranes, separator membranes, or separators, for example, as lithium battery separators. According to at least selected embodiments, the present application or invention is directed to new or improved multilayer and / or microlayer porous or microporous membranes, separator membranes, separators, composites, electrochemical devices, and / or batteries, and / or methods of making and / or using such membranes, separators, composites, devices, and / or batteries. According to at least certain selected embodiments, the present application or invention is directed to new or improved separator membranes that are multi-layered, where one or more layers of the multi-layer structure are produced in a multi-layer or micro-layer co-extrusion die having multiple extruders. The new or improved membranes, separator membranes, or separators may preferably demonstrate improved shutdown, improved strength, improved dielectric breakdown strength, and / or reduced tendency to tear.
[0228] According to at least selected embodiments, the application or invention is directed to additives for improved battery performance, improved additive-containing membranes, improved battery separators, and / or improved batteries, and / or related improved methods of making and / or using the same. According to at least certain embodiments, the application or invention is directed to additive-containing membranes, separator membranes, and / or battery separators, and / or methods of making and / or using such membranes, separator membranes, and / or battery separators. According to at least certain embodiments, the application or invention is directed to the incorporation of additives into microporous or separator membranes for use in lithium secondary batteries, e.g., lithium ion secondary batteries, improved battery separators, and / or related methods. In some embodiments, the membranes may contain additives that improve performance in battery chemistries, e.g., in lithium ion batteries. In other selected embodiments, the membranes may contain additives that improve pin removal performance, such as siloxanes or lithium stearate. In certain other embodiments, the present invention may also relate to methods of making such membranes or separator membranes, and methods of using such membranes or separator membranes, for example, as lithium battery separators. According to at least selected embodiments, the present application or invention is directed to new or improved porous membranes, separator membranes, separators, dry process separators, composites, electrochemical devices, batteries, methods of making such membranes, separators, composites, devices, and / or batteries. According to at least certain selected embodiments, the present invention is directed to new or improved separator membranes containing additives or elastomers. The improved membranes may preferably demonstrate improved shutdown, improved strength, improved dielectric breakdown strength, and / or reduced tendency to tear.According to at least certain selected embodiments, the application or invention is directed to a battery separator having a microporous polymeric thin film or membrane and an optional coating layer on at least one side of the microporous polymeric thin film, wherein at least one of the microporous polymeric thin film and the optional coating comprises an additive. The additive may be selected from the group of lubricants, plasticizers, nucleating agents, shrinkage reducing agents, surfactants, SEI modifiers, cathodic protection agents, flame retardant additives, LiPF6 salt stabilizers, overcharge inhibitors, aluminum corrosion inhibitors, lithium deposition agents or deposition modifiers, or solvation promoters, aluminum corrosion inhibitors, wetting agents, viscosity modifiers, friction reducers, COF reducers, pin removal force reducers, copolymers, block copolymers, and / or combinations thereof. Also described herein are batteries, including lithium ion primary or secondary batteries, comprising one or more of the above thin films, membranes, coatings, and / or separators. Methods of making the above thin films, membranes, coatings, and / or battery separators are also described.According to at least certain embodiments, this application or invention provides an improved or novel battery separator having at least one of increased puncture strength, reduced pin removal force, improved electrolyte wettability, and increased pore size; a microporous polymeric thin film having an optional coating layer on at least one surface thereof; a battery separator having at least one of an optional coating and a microporous polymeric thin film therein and / or thereon; an additive selected from the group of a lubricant, a surfactant, a nucleating agent, a shrinkage reducing agent, and / or a plasticizer; a microporous polymeric thin film having at least one surface of the film; The present invention is directed to the above microporous polymeric thin films having additives present primarily in a face region or in a single surface region of the film, in a first surface region of the film and in a second surface region of the film opposite the first surface region, or throughout the film, coatings applied to the surface of the microporous polymeric thin film, which coating may be applied to only one surface of the microporous polymeric thin film, or may be applied to a first surface of the microporous polymeric thin film and a separate coating may be applied to a second surface of the microporous polymeric thin film opposite the first surface, and / or combinations thereof. According to at least a possibly preferred embodiment, the microporous polymeric thin film or membrane is a microporous polyolefin membrane, such as a dry stretch process membrane, such as a single layer dry process film, a bilayer dry process film, or a multilayer dry process film. Also, according to at least possibly preferred embodiments, one, two, three, four, or all five of the different types of additives may be added, or a single additive that acts as one, two, three, four, or all five of the different types of additives may be added to the film, coating, or separator, such as an additive that is both a lubricant and a surfactant may be added in or on it.
[0229] The microporous multi-layer battery separators described herein, in some embodiments, exhibit improved safety, strength, and durability compared to previous bi-layer, tri-layer, or multi-layer battery separators. For example, the separators may exhibit increased average dielectric breakdown (DB), increased minimum DB, increased shutdown speed, and increased flexure, all of which are indicative of a safer battery separator. The separators may also exhibit increased puncture strength and increased mixed penetration values, indicative of a stronger, more durable battery.
[0230] These properties of the microporous multi-layer battery separators described herein are at least partially a result of the method by which they are made. The method, in some embodiments, includes at least co-extruding two or more polymer mixtures to form a first co-extruded bi-, tri-, or multi-layer film, co-extruding two or more other polymer mixtures to form a second co-extruded bi-, tri-, or multi-layer film, and co-extruding two or more additional polymer mixtures to form a third co-extruded bi-, tri-, or multi-layer film. Co-extrusion typically includes using a co-extrusion die with one or more extruders (typically one extruder per layer of the bi-, tri-, or multi-layer film) feeding the die. The polymer mixtures used to form each layer of the first, second, and third bi-, tri-, or multi-layer films can be the same or different. The mixtures may include one polymer or more than one polymer, such as a polymer blend. Also, more than three bi-, tri-, or multi-layer films may be formed. After the first, second, and third bilayer, trilayer, or multilayer thin films are formed, the thin films are laminated together with two of the thin films formed on opposing sides of one of the thin films to form the microporous battery separator described herein.
[0231] The microporous multilayer battery separators described herein can be used in lithium ion batteries, including lithium secondary batteries, resulting in batteries with improved safety and durability.
[0232] The battery separators herein can be described in several different ways.
[0233] In a first aspect, a battery separator for a lithium battery is described herein. In some embodiments, the battery separator comprises at least one microporous separator membrane or sub-membrane comprising a plurality of porous or microporous polymeric micro- or nano-layers, where at least one of the individual micro- or nano-layers comprises a different or distinct polymer, molecular weight polymer, homopolymer, copolymer, and / or polymer blend, comprises a different or distinct additive, drug, material, and / or filler, or comprises a combination of different or distinct polymer, molecular weight polymer, homopolymer, copolymer, polymer blend, additive, drug, material, and / or filler, compared to an adjacent individual micro- or nano-layer. In some embodiments, a plurality of the separator membranes or sub-membranes of the polymeric micro- or nano-layers are laminated to each other or to a microporous polymeric membrane. In some embodiments, at least one of the separator membranes or sub-membranes of the polymeric micro- or nano-layers has at least three micro- or nano-layers. Optionally, at least one of the separator membranes or sub-membranes of the polymeric micro- or nano-layers is made of one or more polyolefins. Optionally, at least one of the separator membranes or sub-membranes of the polymeric microlayers or nanolayers is made from a coextruded dry-process polyolefin microlayer or nanolayer. In some embodiments, at least two of the separator membranes or sub-membranes of the polymeric microlayers or nanolayers. In some embodiments, at least three of the separator membranes or sub-membranes of the polymeric microlayers or nanolayers.
[0234] Described herein are multi-layered microporous thin films or membranes that may exhibit improved properties, including improved dielectric breakdown and strength, compared to previous single-layered or triple-layered microporous membranes of the same thickness. A preferred multi-layered microporous membrane comprises a microlayer and one or more laminated barriers. Also disclosed are battery separators or batteries that comprise one or more of the multi-layered microporous thin films or membranes. The batteries and battery separators of the present invention are preferably safer and more robust than batteries and battery separators that use previous single-layered and triple-layered microporous membranes. Also described herein are methods for making the multi-layered microporous separators, membranes or thin films described herein.
[0235] Various embodiments of the present invention have been described in order to achieve various objectives of the present invention. It should be recognized that these embodiments are merely illustrative of the principles of the present invention. Many changes and modifications will be readily apparent to those skilled in the art without departing from the spirit and scope of the invention.
[0236] The present invention may be embodied without departing from its spirit and essential characteristics, and therefore, reference should be made to the appended claims, rather than the above specification, as indicating the scope of the present invention. Components that can be used to implement the disclosed methods and systems are disclosed. These and other components are disclosed herein, and it is understood that combinations, subsets, interactions, groups, etc. of these components are specifically contemplated and described herein for all methods and systems when disclosed, even though each of their various individual and collective combinations and permutations may not be expressly disclosed. This applies to all aspects of this application, including, but not limited to, steps in the disclosed methods. Thus, when there are various additional steps that can be implemented, it is understood that these additional steps can each be implemented by any specific embodiment or combination of embodiments of the disclosed methods.
[0237] The above detailed description of the structures and methods are presented for illustrative purposes only. The examples are used to disclose exemplary embodiments, including the best mode, and to enable any person skilled in the art to practice the invention, including making and using any device or system, and performing any incorporated methods. These examples are not intended to be exhaustive or to limit the invention to the precise steps and / or forms disclosed, many modifications and variations are possible in light of the above teachings. The features described herein may be combined in any combination. The steps of the methods described herein may be performed in any order that is physically possible. The patentable scope of the invention is defined by the appended claims, and may include other examples that occur to those skilled in the art. Such other examples are intended to be within the scope of the claims when they have structural elements that do not differ from the literal language of the claims, or when they include equivalent structural elements that do not differ substantially from the literal language of the claims.
[0238] The compositions and methods of the appended claims are not limited in scope by the specific compositions and methods described herein. In addition to those shown and described herein, various modifications of the compositions and methods are intended to be within the scope of the appended claims. Furthermore, although only certain representative compositions and method steps disclosed herein are specifically described, other combinations of such compositions and method steps are also intended to be within the scope of the appended claims even if not specifically recited. Thus, although combinations of steps, elements, components, or ingredients may be explicitly referred to herein or below, other combinations of steps, elements, components, or ingredients are encompassed even if not explicitly described.
[0239] As used in the specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. Ranges may be expressed herein as from "about" or "approximately" one particular value and / or to "about" or "approximately" another particular value. When such a range is expressed, another embodiment includes from the one particular value and / or to the other particular value. Similarly, when values are expressed as approximations, by use of the antecedent "about," it is understood that the particular value forms another embodiment. It is further understood that each of the endpoints of a range is significant both in relation to the other endpoint, and independently of the other endpoint. "Optional" or "optionally" means that the subsequently described event or circumstance may or may not occur, and that the description includes instances when the event or circumstance occurs and instances when the event or circumstance does not occur.
[0240] Throughout the detailed description and claims of this specification, the word "comprise" and variations of the word, such as "comprising" and "comprises," mean "including but not limited to," and are not intended to exclude, for example, other additives, components, integers, or steps. The terms "consisting essentially of" and "consisting of" may be used in place of "comprising" and "including" to provide more specific embodiments of the present invention and are disclosed. "Exemplary" or "for example" means "an example of" and is not intended to convey an indication of a preferred or ideal embodiment. Similarly, "such as" is used in a descriptive or illustrative sense, rather than in a restrictive sense.
[0241] Unless otherwise noted, all numbers expressing geometric shapes, dimensions, and the like used in the specification and claims should be understood to be at least as and should be construed in light of the number of significant digits and ordinary rounding approaches, and not as an attempt to limit the application of the doctrine of equivalents to the scope of the claims.
[0242] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the disclosed invention belongs. All publications and materials cited herein are specifically incorporated by reference.
[0243] In addition, the invention illustratively disclosed herein may suitably be practiced in the absence of any element not specifically disclosed herein.
Claims
1. 1. An improved battery separator comprising a multi-layered microporous membrane, at least two successive layers of said multi-layered microporous membrane having a thickness of 0.1 to 3 microns; The at least two continuous layers are coextruded layers, and the at least two continuous layers are laminated with at least one other layer to form a microporous polymeric thin film, and the at least two continuous layers are microlayers or nanolayers laminated by a dry process; A battery separator for a lithium battery, wherein the multilayer microporous thin film is a three-layer film and has a puncture strength of 290 gf or more.
2. 10. The battery separator of claim 1, wherein said multi-layer microporous membrane has a thickness of 1 to 30 microns.
3. 10. The battery separator of claim 1 wherein said at least one other layer is a coextruded layer.
4. 10. The battery separator of claim 1, wherein said at least two continuous layers comprise a polyolefin or a blend of polyolefins.
5. 10. The battery separator of claim 1, wherein said multi-layer microporous membrane comprises 9 or more layers.
6. 1. A method for forming an improved battery separator comprising a multi-layer microporous thin film, comprising: The method includes co-extruding at least two layers; laminating the at least two coextruded layers with at least one other layer to form the multilayer microporous membrane; 1. A method of forming a battery separator comprising:
7. 7. The method of forming a battery separator according to claim 6, wherein said at least one other layer is a coextruded layer.
8. 7. The method of forming a battery separator according to claim 6, wherein said at least one other layer is a single extruded layer.
9. 7. The method of forming a battery separator according to claim 6, wherein said at least two layers that are coextruded are laminated to two other layers.
10. 10. The method of forming a battery separator according to claim 9, wherein each of said two other layers is a coextruded layer.
11. 10. The method of forming a battery separator according to claim 9, wherein each of said two other layers is a single extruded layer.
12. 10. The method of forming a battery separator according to claim 9, wherein each of said two other layers is independent of one another and is a monoextruded layer or a coextruded layer.
13. 7. A battery separator made by the method of forming a battery separator according to claim 6.
Citation Information
Patent Citations
Multilayer microporous membrane and method for manufacturing and using such membrane.
JP2012506792A