Articles and structures with high heat, reflectivity and laser direct structuring capabilities

A thermoplastic composition with PCT, glass fibers, and titanium compounds addresses the LED industry's need for a reflective, stable surface by enhancing heat resistance and dielectric properties, suitable for LED and 5G networks.

JP7568732B2Active Publication Date: 2024-10-16SHPP GLOBAL TECH BV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022549197
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-20
Filing Date
2021-02-11
Publication Date
2024-10-16
Estimated Expiration
2041-02-11

AI Technical Summary

Technical Problem

The LED industry faces challenges in adopting laser direct structuring (LDS) technology due to the lack of a white, highly reflective surface that is easy to assemble and economically feasible for circuit integration, with existing polymers like LCP, PPS, and PPA having high costs, water absorption issues, and unsuitable dielectric performance for 5G networks, and PCT being affected by crystallization with fillers.

Method used

A thermoplastic composition comprising poly(cyclohexylene dimethylene terephthalate) (PCT) or its copolymers, reinforced with glass fibers, and incorporating tin oxide, antimony oxide, or titanium compounds as LDS additives, maintaining a weight ratio of total titanium to LDS additive at 0.7:1 or less, to achieve high thermal performance, reflectance, and dielectric properties.

Benefits of technology

The composition achieves high heat distortion temperatures, excellent dielectric properties, and high reflectance, making it suitable for LED circuits and 5G network applications, while maintaining stability and reducing water absorption issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568732000017
    Figure 0007568732000017
  • Figure 0007568732000018
    Figure 0007568732000018
  • Figure 0007568732000019
    Figure 0007568732000019
Patent Text Reader

Abstract

The thermoplastic composition includes (a) poly(cyclohexylene dimethylene terephthalate) (PCT) or a copolymer thereof, (b) at least 10 wt. % of a reinforcing filler including glass fiber, (c) a laser direct structuring (LDS) additive including tin oxide, antimony oxide, or a combination thereof, and (d) a reflective additive including a titanium compound, wherein the weight ratio of the total titanium in the composition to the LDS additive in the composition is at least 0.7:1, or the weight ratio of the total titanium in the composition to the PCT is no greater than 1.1:1.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THE DISCLOSURE This disclosure relates to laser plateable thermoplastic compositions, and in particular to compositions that include titanium compounds to provide high reflectance properties. [Background technology]

[0002] In the trend towards miniaturization and integration of circuits, there is a demand to miniaturize circuits and make them combinable with other functional components in different industries. Laser direct structuring (LDS) technology is favored compared to traditional circuit manufacturing techniques such as printed circuit board (PCB) technology, mainly due to its design flexibility. LDS polymer compositions can be combined with additives to provide additional properties (e.g., stiffness, color, etc.) and formed into pellets that can be processed by traditional compounding techniques. LDS polymers are widely accepted and used in the consumer electronics industry, such as mobile communication devices. In particular, LDS polymers have been used in antennas for such devices.

[0003] However, technological barriers have slowed the adoption of LDS technology in some electronics industries. For example, the LED industry has yet to identify a white, highly reflective surface that is solderable for circuit integration, easy to assemble, and economically feasible. An LDS solution for such LED applications would be desirable.

[0004] Among the traditional polymers that can be considered for such applications, liquid crystal polymer (LCP) and polyphenylene sulfide (PPS) have been discounted due to their high cost. Polyphthalamide (PPA) is a semi-crystalline aromatic polyamide that shows great promise, but also has some properties that make it undesirable for LDS applications, including water absorption, dimensional stability, and color (yellowing) issues. In particular, the water absorption properties of PPA make the dielectric performance of compositions containing PPA unstable, making them unsuitable for use in 5G network applications.

[0005] Poly(cyclohexylene dimethylene terephthalate) (PCT) can provide a high heat white platform. However, the crystallization of PCT and other high heat base resins can be adversely affected by fillers and other additives, and as a result, they have not been widely adopted in LDS applications.

[0006] These and other shortcomings are addressed by aspects of the present disclosure. Summary of the Invention

[0007] An embodiment of the present disclosure relates to a thermoplastic composition comprising: (a) poly(cyclohexylene dimethylene terephthalate) (PCT) or a copolymer thereof; (b) at least 10 weight percent of a reinforcing filler comprising glass fiber; (c) a laser direct structuring (LDS) additive comprising tin oxide, antimony oxide, or a combination thereof; and (d) a reflective additive comprising a titanium compound. The weight ratio of the total titanium in the composition to the LDS additive in the composition is at least 0.7:1, or the weight ratio of the total titanium in the composition to the PCT is no greater than 1.1:1. [Brief description of the drawings]

[0008] In the drawings, which are not necessarily drawn to scale, like numerals may indicate like components in different views. Like numerals with different letter suffixes may represent different instances of like components. The drawings illustrate generally, by way of example, but not by way of limitation, various aspects discussed in the present document.

[0009] [Figure 1] 1 is a graph showing reflectance as a function of wavelength for control and example compositions formed in accordance with aspects of the present disclosure. [Diagram 2] 4 provides photographs of LDS plated plaques of the comparative and exemplary compositions of Example 2. [Diagram 3] 4 provides photographs of LDS plated plaques of the comparative and exemplary compositions of Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present disclosure may be more readily understood by reference to the following detailed description of the disclosure and the examples included therein. In various embodiments, the present disclosure relates to a laser plateable thermoplastic composition comprising: (a) at least one high heat base resin having a melting temperature (Tm) of at least 250° C.; at least 20% by weight of a reinforcing filler; (c) an LDS additive comprising tin oxide, antimony oxide, or a combination thereof; and (d) a reflective additive comprising a titanium compound. The composition, in some embodiments, has a reflectance of about 50% to about 95% at wavelengths of 400 nanometers (nm) to 750 nm.

[0011] Before the present compounds, compositions, articles, systems, devices, and / or methods are disclosed and described, it is to be understood that they are not limited to specific synthetic methods, or to particular reagents, unless otherwise specified, which can, of course, vary. It is also to be understood that the terminology used herein is for the purpose of describing particular embodiments only, and is not intended to be limiting.

[0012] Various combinations of elements of the present disclosure are encompassed by the present disclosure, including combinations of elements from dependent claims that are dependent on the same independent claim.

[0013] Furthermore, it should be understood that unless expressly stated otherwise, the methods described herein are in no way intended to be construed as requiring that the steps be performed in a particular order. Thus, where a method claim does not actually recite the order in which its steps should be followed, or where the claims or description do not specifically state that the steps are limited to a particular order, no order is intended to be inferred in any respect. This applies to any possible non-express basis for interpretation, including questions of logic regarding the arrangement of steps or operational flow, the apparent meaning derived from grammatical construction or punctuation, and the number or type of aspects described herein.

[0014] All publications mentioned herein are incorporated herein by reference to disclose and describe the methods and / or materials in connection with which the publications are cited.

[0015] definition It is also to be understood that the terms used herein are for the purpose of describing particular embodiments only and are not intended to be limiting. As used in this specification and claims, the term "comprising" can include the embodiments "consisting of" and "consisting essentially of". Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs. In this specification and the following claims, reference is made to several terms that must be defined herein.

[0016] As used in the specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a reinforcing filler" includes a mixture of two or more reinforcing fillers.

[0017] As used herein, the term "combination" is inclusive of blends, mixtures, alloys, reaction products, and the like.

[0018] Ranges may be expressed herein as from one value (first value) to another value (second value). When such a range is expressed, the range includes, in some embodiments, one or both of the first and second values. Similarly, when values ​​are expressed as approximations, by using the antecedent "about," it is understood that the particular value forms another embodiment. Moreover, it is further understood that each endpoint of a range is significant in relation to the other endpoint, and independently of the other endpoint. There are a number of values ​​disclosed herein, and each value is also understood to be disclosed herein as "about" that particular value, in addition to the value itself. For example, if the value "10" is disclosed, then "about 10" is also disclosed. It is also understood that each unit between two particular units is also disclosed. For example, if 10 and 15 are disclosed, then 11, 12, 13, and 14 are also disclosed.

[0019] As used herein, the terms "about" and "at or about" mean that the quantity or value in question can be at, approximately, or approximately the same as the specified value. As used herein, it is generally understood to be a nominal value, indicating a variation of ±10%, unless otherwise indicated or inferred. The term is intended to convey that similar values ​​promote the same results or effects as detailed in the claims. That is, it is understood that the amount, size, formulation, parameter, and other quantities and characteristics need not be exact, but may be approximately and / or larger or smaller, as appropriate, to reflect tolerances, conversion factors, rounding, measurement errors, and the like, and other factors known to those skilled in the art. In general, the amount, size, formulation, parameter, or other quantity or characteristic is "about" or "approximate", whether or not it is so stated. When "about" is used before a quantitative value, it is understood that the parameter also includes the specific quantitative value itself, unless otherwise stated.

[0020] Disclosed are the components used to prepare the compositions of the present disclosure, as well as the compositions themselves used within the methods disclosed herein. When these and other materials are disclosed herein, and when combinations, subsets, interactions, groups, etc. of these materials are disclosed, it is understood that specific references to the various individual and collective combinations and permutations of each of these compounds may not be explicitly disclosed, but each is specifically contemplated and described herein. For example, when a particular compound is disclosed and discussed, and several modifications that can be made to many molecules that include that compound are discussed, what is specifically contemplated is any and all combinations and permutations of the compounds, as well as possible modifications, unless specifically indicated to the contrary. Thus, when a class of molecules A, B, and C, and a class of molecules D, E, and F, and examples of combination molecules are disclosed, it means that A-D are disclosed, and then each is individually and collectively contemplated, even if each is not individually detailed, and combinations A-E, A-F, B-D, B-E, B-F, C-D, C-E, and C-F are considered to be disclosed. Likewise, any subset or combination thereof is also disclosed. Thus, for example, subgroups A-E, B-F, and C-E are considered to be disclosed. This concept applies to all aspects of this application, including but not limited to steps in the methods of making and using the disclosed compositions. Thus, when there are various additional steps that can be performed, it is understood that each of these additional steps can be performed in any specific aspect or combination of aspects of the disclosed method.

[0021] References in the specification and concluding claims to parts by weight of a particular element or component in a composition or article indicate the weight relationship between the element or component and any other elements or components in the composition or article for which the parts by weight are expressed. Thus, in a compound containing 2 parts by weight of component X and 5 parts by weight of component Y, X and Y are present in a weight ratio of 2:5, and are present in such ratio regardless of whether additional components are contained in the compound.

[0022] Weight percentages of components are based on the total weight of the formulation or composition in which the component is included, unless specifically stated to the contrary.

[0023] As used herein, "number average molecular weight" or "M n The terms "molecular weight" and "molecular weight average" may be used interchangeably and refer to the statistical average molecular weight of all polymer chains in a sample and are defined by the formula:

number

[0024] As used herein, "weight average molecular weight" or "M w The terms " may be used interchangeably and are defined by the formula:

number

[0025] As used herein, the terms "polydispersity index" or "PDI" may be used interchangeably and are defined by the following formula:

number

[0026] As used herein, the terms “BisA,” “BPA,” or “bisphenol A,” which may be used interchangeably, refer to a compound having a structure represented by the following formula: [ka] BisA may also be referred to by the names 4,4'-(propane-2,2-diyl)diphenol, p,p'-isopropylidenebisphenol, or 2,2-bis(4-hydroxyphenyl)propane. BisA has the CAS number 80-05-7.

[0027] As used herein, "polycarbonate" refers to an oligomer or polymer that contains the residues of one or more dihydroxy compounds, e.g., dihydroxy aromatic compounds, linked through carbonate linkages, and is inclusive of homopolycarbonates, copolycarbonates, and (co)polyestercarbonates.

[0028] The terms "residue" and "structural unit" as used in reference to polymeric constituents are synonymous throughout this specification.

[0029] As used herein, the terms "weight percent," "weight % (wt%)," and "weight % (wt.%)," which may be used interchangeably, refer to the weight percent of a given component relative to the total weight of the composition, unless otherwise specified. That is, all weight % values ​​are based on the total weight of the composition, unless otherwise specified. It is to be understood that the sum of the weight % values ​​of all components in the disclosed compositions or formulations equals 100.

[0030] Unless stated to the contrary herein, all test specifications are the latest specifications in effect at the time of filing this application.

[0031] Each of the materials disclosed herein is either commercially available and / or methods for its production are known to those of skill in the art.

[0032] It is understood that the compositions disclosed herein have specific functions. Disclosed herein are specific structural requirements for performing the disclosed functions, and it is understood that there are various structures that can perform the same functions associated with the disclosed structures, and that these structures typically achieve the same results.

[0033] thermoplastic composition The present disclosure relates to high heat base resin LDS compositions that have high thermal performance (as identified by heat distortion temperature, HDT), good dielectric properties, and good color (reflectance or whiteness) properties. The thermoplastic compositions of the present disclosure can be used in a wide range of circuit applications, including LED circuits. In addition, they have good dielectric properties, including high dielectric constant or relative permittivity (Dk) and low dissipation factor (Df), making them valuable for use in communications applications, particularly 5G network applications.

[0034] Thermoplastic compositions according to embodiments of the present disclosure combine poly(cyclohexylene dimethylene terephthalate) (PCT) or other high heat base resins, reinforcing fillers such as glass fibers, and LDS additives. These compositions are high heat solderable, laser plateable, and have good color (reflectance) properties.

[0035] In particular, thermoplastic compositions according to embodiments of the present disclosure may include titanium, which may help maintain the high thermal performance of the composition (HDT of greater than 200° C. at 1.8 megapascals (MPa)). By comparison, a similar composition without titanium has an HDT of about 100° C. Titanium may be present in a variety of forms, such as, but not limited to, titanium oxide or titanium oxide coated with an LDS additive. Additionally, the inclusion of titanium oxide may result in a composition having a higher Dk (e.g., 3.5-5) while maintaining a low Df (about 0.007).

[0036] Certain embodiments of the present disclosure relate to a thermoplastic composition comprising: (a) at least one high heat base resin having a melting temperature (Tm) of at least 250 degrees Celsius (°C); (b) at least 20% by weight of a reinforcing filler; (c) a laser direct structuring (LDS) additive comprising tin oxide, antimony oxide, or a combination thereof; and (d) a reflective additive comprising a titanium compound. The composition, in some embodiments, has a reflectance of about 50% to about 95% at wavelengths of 400 nanometers (nm) to 750 nm. The reflectance may, in some embodiments, be determined according to ASTM D6290-98. Reflectance and Color L * / a * / b * can be measured using a ColorEye 7000A available from GretagMacbeth, which measures reflectance in the wavelength interval from 360 nm to 750 nm and has the capability to take both specular and total transmission readings.

[0037] The high heat base resin has a melting temperature (Tm) of at least 250° C. In some embodiments, the high heat base resin has a Tm of 250° C. to 350° C. Any polymeric resin having this Tm characteristic can be used in the composition. In some embodiments, the at least one high heat resin includes, but is not limited to, poly(cyclohexylene dimethylene terephthalate) (PCT), polyphthalamide (PPA), copolymers thereof, or combinations thereof.

[0038] PCT is a high performance semi-crystalline thermoplastic polyester produced by the polycondensation of cyclohexanedimethanol (CHDM) and terephthalic acid (TPA). It generally has comparable mechanical properties compared to polyethylene terephthalate (PET), including but not limited to flexural strength, impact strength, and tensile strength (30% GF). Its resistance to hydrolysis and heat is superior. In addition, pure PCT has a higher melting point (about 285°C) than PET (about 245°C). The PCT monomer is represented by the following formula and has CAS Reg. No. 25135-20-0: [ka]

[0039] Exemplary PCT copolymers suitable for use in embodiments of the present disclosure include, but are not limited to, polyethylene terephthalate glycol (PETG), polycyclohexylene dimethylene terephthalate glycol (PCTG), and polycyclohexylene dimethylene terephthalate acid (PCTA). PETG and PCTG are copolyesters formed by including ethylene glycol (EG) in the polymerization reaction. When less than 50% of the diol content in the copolyester is CHDM, PETG is formed, and when more than 50% of the diol content in the copolyester is CHDM, PCTG is formed. PCTA is formed by including an additional diacid such as isophthalic acid (IPA).

[0040] PPA is a semi-aromatic engineering thermoplastic containing primary building blocks of terephthalic acid or isophthalic acid (or a combination thereof) and at least one aliphatic diamine, such as hexamethylenediamine. The PPA monomer is represented by the following formula: [ka]

[0041] The aromatic acid moiety accounts for at least 55 mole percent of the repeating units in the polymer chain, and the PPA resin is only partially aromatic. The PPA resin is characterized by having a melting point, rigidity, thermal stability, and chemical resistance, as well as low moisture absorption. Exemplary PPA compositions are disclosed, for example, in U.S. Patent No. 5,387,645, the disclosure of which is incorporated herein by reference in its entirety.

[0042] The Tm of the high heat resistant base resin can be measured by differential scanning calorimetry (DSC). Suitable instruments for DSC measurements include the Shimadzu DSC-60A. The measurement temperature range is about 80°C to 400°C with a heating or cooling rate of ±10 to 20°C / min. The sample can be in the form of a powder, pellet, or part. A typical sample size is 20 mg.

[0043] In some embodiments, the tin oxide or antimony oxide is in the form of a coating on the additional LDS additive. The additional LDS additive may be a titanium compound in some embodiments. The titanium compound included in the additional LDS additive joins with the titanium compound in element (d) of the composition.

[0044] In some embodiments, the composition comprises from about 2% to about 20% by weight of the LDS additive, hi certain embodiments, the composition comprises from about 5% to about 10% by weight of the LDS additive.

[0045] In further embodiments, the composition comprises from about 5% to about 50% by weight of the reflective additive comprising a titanium compound. In certain embodiments, the composition comprises from about 10% to about 20% by weight of the reflective additive comprising a titanium compound.

[0046] In certain embodiments, the titanium compound of element (d) of the composition is a titanium oxide, such as, but not limited to, titanium dioxide. Similarly, when included in the further LDS additive (element (c)), the titanium compound can include a titanium oxide, such as, but not limited to, titanium dioxide.

[0047] Exemplary reinforcing fillers suitable for use in the thermoplastic compositions according to embodiments of the present disclosure include, but are not limited to, glass fibers, ceramic fibers, carbon fibers, inorganic fillers, or combinations thereof. In certain embodiments, the reinforcing filler comprises glass fibers. The composition, in certain embodiments, comprises at least 20 wt.% reinforcing filler or 20 wt.% to 70 wt.% reinforcing filler.

[0048] In some embodiments, the thermoplastic composition may include one or more additional additives.The one or more additional additives may include, but are not limited to, impact modifiers, acid scavengers, anti-drip agents, antioxidants, antistatic agents, chain extenders, colorants, demolding agents, flow promoters, lubricants, release agents, plasticizers, quenching agents, flame retardants, UV reflecting additives, or combinations thereof.The one or more additional additives may be included in the thermoplastic composition in any amount that does not significantly adversely affect the desired properties of the composition.

[0049] Thermoplastic compositions according to embodiments of the present disclosure have improved properties compared to comparative compositions that do not contain either a laser direct structuring (LDS) additive comprising tin oxide, antimony oxide, or a combination thereof (element (c)), or a reflective additive comprising a titanium compound (element (d)).

[0050] In particular, thermoplastic compositions according to embodiments of the present disclosure have high heat distortion temperatures (HDT). HDT can be evaluated according to ASTM D648, for example, using a sample thickness of 3.2 mm and a load of 0.45 or 1.82 megapascals (MPa). In certain embodiments, the compositions have an HDT of at least 200°C at 1.82 MPa, or at least 250°C in further embodiments. In other embodiments, the compositions have an HDT of at least 200°C at 0.45 MPa, or at least 250°C in further embodiments, or 270°C in even further embodiments.

[0051] In some embodiments, the composition has a dissipation factor (Df) of less than 0.01. Df can be determined using an Agilent Split Post Dielectric Resonator at 1.1 gigahertz (GHz), 1.9 GHz, 5 GHz, 10 GHz, and / or 20 GHz. This method is referred to herein as the "SABIC method."

[0052] The composition may, in some embodiments, have good color properties. In particular, the composition may be * a * b * At least 50 L, as determined according to color space standards * In a further embodiment, the composition may have the CIE L * a * b * L of at least 70 as determined according to color space standards * or in still further embodiments, CIE L * a * b * L of at least 80-95 as determined according to color space standards * has.

[0053] In certain embodiments, the composition has a reflectance of about 50% to about 95% at a wavelength of 400 nm to 550 nm. In certain embodiments, the composition has a reflectance of about 50% to about 95% at a wavelength of 450 nm. The reflectance can be evaluated according to the process described in the Examples herein.

[0054] Method for making a thermoplastic composition One or any of the above-mentioned components described herein may be first dry blended with each other or with any combination of the above-mentioned components, and then fed into the extruder through one or more feeders, or may be fed into the extruder separately through one or more feeders.Additional components, such as additives or fillers, may also be first processed into a master batch and then fed into the extruder.The components may be fed into the extruder through a throat hopper or any side feeder.

[0055] Extruders used in this disclosure may have a single screw, multiple screws, intermeshing co-rotating or counter-rotating screws, non-intermeshing co-rotating or counter-rotating screws, reciprocating screws, screws with pins, screws with screens, barrels with pins, rolls, rams, helical rotors, co-kneaders, disc pack processors, various other types of extrusion equipment, or combinations comprising at least one of the foregoing.

[0056] The components may also be mixed together and then melt blended to form the thermoplastic composition. Melt blending of the components involves the use of shear forces, extensional forces, compression forces, ultrasonic energy, electromagnetic energy, thermal energy, or a combination comprising at least one of the foregoing forces or forms of energy.

[0057] The barrel temperature of the extruder during compounding can be set at a temperature at which at least a portion of the polymer has reached a temperature equal to or greater than about the melting temperature if the resin is a semi-crystalline organic polymer, or at the pour point (e.g., glass transition temperature) if the resin is an amorphous resin.

[0058] The mixture containing the aforementioned components may be subjected to multiple blending and forming steps, if necessary. For example, the thermoplastic composition may be first extruded and formed into pellets. The pellets may then be fed to a forming machine where they may be formed into any desired shape or product. Alternatively, the thermoplastic composition emerging from a single melt blender may be formed into sheets or strands and subjected to post-extrusion processes such as annealing, uniaxial or biaxial stretching, etc.

[0059] The temperature of the melt in this process may be kept as low as possible in some embodiments to avoid excessive thermal decomposition of the components. In some embodiments, the melt processed composition exits the processing device, such as an extruder, through small exit holes in a die. The resulting strands of molten resin may be cooled by passing the strands through a water bath. The cooled strands may be chopped into pellets for packaging and further processing. Exemplary conditions for making thermoplastic compositions according to embodiments of the present disclosure are described in the examples below.

[0060] Manufactured product In certain embodiments, the present disclosure relates to shaped, formed, or molded articles comprising the thermoplastic composition.The thermoplastic composition can be molded into useful shaped articles by various means, such as injection molding, extrusion, rotational molding, blow molding, and thermoforming, to form articles and structural components of personal or commercial electronic devices, including, but not limited to, mobile phones, tablet computers, personal computers, notebook and portable computers, and other such devices, medical applications, RFID applications, automotive applications, and the like.In further embodiments, the article is extruded.In even further embodiments, the article is injection molded.

[0061] In certain embodiments, the article is a component of a light emitting diode (LED) or a component of a 5G network communication device.

[0062] Various combinations of elements of the present disclosure are encompassed by the present disclosure, including combinations of elements from dependent claims that are dependent on the same independent claim.

[0063] Aspects of the Disclosure In various aspects, the present disclosure relates to and includes at least the following aspects:

[0064] Aspect 1: (a) at least one high heat base resin having a melting temperature (Tm) of at least 250 degrees Celsius (°C), or between 250°C and 350°C; (b) at least 20% by weight of a reinforcing filler; (c) a laser direct structuring (LDS) additive comprising tin oxide, antimony oxide, or a combination thereof; (d) a reflective additive comprising a titanium compound. A thermoplastic composition comprising, consisting of, or consisting essentially of. Embodiment 2. The thermoplastic composition of embodiment 1, wherein the tin oxide or antimony oxide is in the form of a coating on the additional LDS additive. Example 3. The thermoplastic composition of example 2, wherein the additional LDS additive is a titanium compound. Embodiment 4. The thermoplastic composition of embodiment 3, wherein the titanium compound comprises titanium oxide. Embodiment 5. The thermoplastic composition of any one of embodiments 1-4, wherein the at least one high heat resin comprises poly(cyclohexylene dimethylene terephthalate) (PCT), polyphthalamide (PPA), copolymers thereof, or combinations thereof. Aspect 6. The thermoplastic composition of any one of Aspects 1-5, wherein the composition comprises about 2% by weight to about 20% by weight of the LDS additive. Aspect 7. The thermoplastic composition of any one of Aspects 1-6, wherein the composition comprises about 5% to about 50% by weight of the reflective additive comprising a titanium compound. Aspect 8. The thermoplastic composition of aspect 7, wherein the composition comprises about 10% to about 20% by weight of the reflective additive comprising a titanium compound. Example 9. The thermoplastic composition of any one of Examples 1-8, wherein the reinforcing filler comprises glass fiber, ceramic fiber, carbon fiber, an inorganic filler, or a combination thereof. Example 10. The thermoplastic composition of example 9, wherein the reinforcing filler comprises glass fibers. Embodiment 11. The thermoplastic composition of any one of embodiments 1-10, wherein the composition has a heat distortion temperature (HDT) of at least 200° C. at 1.82 megapascals (MPa). Example 12. The thermoplastic composition of any one of Examples 1-11, wherein the composition has a heat distortion temperature (HDT) of at least 250° C. at 1.82 megapascals (MPa). Embodiment 13. The thermoplastic composition of any one of embodiments 1-12, having an HDT of at least 200° C. at 0.45 MPa. Embodiment 14. The thermoplastic composition of any one of embodiments 1-13, having a HDT of at least 250° C. at 0.45 MPa. Aspect 15. The thermoplastic composition of any one of aspects 1-13, having an HDT of at least 270° C. at 0.45 MPa. Embodiment 16. The thermoplastic composition of any one of embodiments 1-15, wherein the composition has a dissipation factor (Df) of less than 0.01. Embodiment 17. The composition comprises CIE L * a * b * At least 50 L, as determined according to color space standards * 17. The thermoplastic composition of any one of aspects 1 to 16, having the following structure: Embodiment 18. The composition comprises CIE L * a * b * L of at least 70, as determined according to color space standards * 18. The thermoplastic composition of any one of embodiments 1 to 17, having the following structure: Embodiment 19. The composition comprises CIE L * a * b * An L of at least 80-95 as determined according to color space standards * 19. The thermoplastic composition of any one of aspects 1 to 18, having the following structure: Aspect 20. The thermoplastic composition of any one of aspects 1 to 19, wherein the composition has a reflectance of about 50% to about 95% at wavelengths from 400 nanometers (nm) to 750 nm. Aspect 21. The thermoplastic composition of any one of aspects 1 to 20, wherein the composition has a reflectance of about 50% to about 95% at wavelengths between 400 nm and 550 nm. Embodiment 22. The thermoplastic composition of any one of embodiments 1 to 21, wherein the composition has a reflectance of about 50% to about 95% at a wavelength of 450 nm. Embodiment 23. The thermoplastic composition of any one of embodiments 1-22, wherein the composition further comprises one or more additional additives. Embodiment 24. The thermoplastic composition of embodiment 23, wherein the one or more additional additives comprise an impact modifier, an acid scavenger, an anti-drip agent, an antioxidant, an antistatic agent, a chain extender, a colorant, a demolding agent, a flow promoter, a lubricant, a release agent, a plasticizer, a quenching agent, a flame retardant, a UV reflecting additive, or a combination thereof. Example 25. An article comprising the thermoplastic composition of any one of Examples 1-24. Embodiment 26. The article of embodiment 25, wherein the article is a component of a light emitting diode (LED) or a component of a 5G network communication device. Aspect 27. (a) poly(cyclohexylene dimethylene terephthalate) (PCT) or a copolymer thereof; (b) at least 10% by weight of a reinforcing filler comprising glass fibers; (c) a laser direct structuring (LDS) additive comprising tin oxide, antimony oxide, or a combination thereof; (d) a reflective additive comprising a titanium compound, (1) the weight ratio of the total titanium in the composition to the LDS additive in the composition is at least 0.7:1; or (2) A thermoplastic composition, wherein the weight ratio of total titanium in the composition to PCT is 1.1:1 or less. In some embodiments, the ratio of titanium to the LDS additive is at least 1:1, at least 2:1, at least 4:1, at least 6:1, or greater than 6:1. Example 28. The thermoplastic composition of example 27, wherein the tin oxide or antimony oxide is in the form of a coating on the further LDS additive. Example 29. The thermoplastic composition of example 28, wherein the further LDS additive comprises titanium oxide. Embodiment 30. The thermoplastic composition of any one of embodiments 27-29, wherein the composition further comprises a thermally conductive filler different from the reinforcing filler in element (b). Example 31. The thermoplastic composition of example 30, wherein the thermally conductive filler comprises boron nitride. Embodiment 32. The thermoplastic composition of any one of embodiments 27 to 31, wherein the composition comprises about 2% by weight to about 20% by weight of the LDS additive. Embodiment 33. The thermoplastic composition of any one of embodiments 27 to 32, wherein the composition comprises about 5% by weight to about 50% by weight of the reflective additive comprising a titanium compound. Aspect 34. The thermoplastic composition of aspect 33, wherein the composition comprises about 10% by weight to about 20% by weight of the reflective additive comprising a titanium compound. Example 35. The thermoplastic composition of any one of Examples 27-34, wherein the reinforcing filler comprises glass fibers, ceramic fibers, carbon fibers, inorganic fillers, or combinations thereof. Embodiment 36. The thermoplastic composition of any one of embodiments 27-35, wherein the composition has a heat distortion temperature (HDT) of at least 200° C. at 1.82 megapascals (MPa) and a sample thickness of 3.2 millimeters (mm), or a HDT of at least 200° C. at 0.45 MPa and a sample thickness of 3.2 mm. In a further embodiment, the composition has a heat distortion temperature (HDT) of at least 220° C. at 1.82 megapascals (MPa) and a sample thickness of 3.2 millimeters (mm). Embodiment 37. The thermoplastic composition of any one of embodiments 27-36, wherein the composition has a dissipation factor (Df) of less than 0.01. Embodiment 38. The composition comprises CIE L * a * b * L of at least 70, as determined according to color space standards * In a further embodiment, the composition has a CIE L * a * b * An L of at least 75, or at least 80, or at least 85, as determined according to a color space standard * has. Embodiment 39. The thermoplastic composition of any one of embodiments 27 to 38, wherein the composition has a reflectance of about 50% to about 95% at wavelengths from 400 nanometers (nm) to 750 nm. In further embodiments, the composition has a reflectance of about 60% to about 95%, or about 70% to about 95%, or about 80% to about 95%, or greater than 50%, or greater than 60%, or greater than 70%, or greater than 80% at wavelengths from 400 nanometers (nm) to 750 nm. Embodiment 40. The thermoplastic composition of any one of embodiments 27-39, wherein the composition has an in-plane thermal conductivity of at least 0.5 Watts per meter Kelvin (W / (m·K)) or a through-plane thermal conductivity of at least 0.5 W / (m·K). In a further embodiment, the composition has an in-plane thermal conductivity of at least 1.0 W / (m·K). Embodiment 41. The thermoplastic composition of any one of embodiments 27 to 40, wherein the composition further comprises one or more additional additives. Embodiment 42. The thermoplastic composition according to embodiment 41, wherein the one or more additional additives comprise an impact modifier, an acid scavenger, an anti-drip agent, an antioxidant, an antistatic agent, a chain extender, a colorant, a demolding agent, a flow promoter, a lubricant, a release agent, a plasticizer, a quenching agent, a flame retardant, a UV reflecting additive, or a combination thereof. Example 43. An article comprising the thermoplastic composition of any one of examples 27-42, wherein the article is a component of a light emitting diode (LED) or a component of a 5G network communication device. EXAMPLES

[0065] The following examples are presented to provide those skilled in the art with a complete disclosure and description of how the compounds, compositions, articles, devices, and / or methods claimed herein are made and evaluated, and are intended to be purely illustrative and are not intended to limit the disclosure. Efforts have been made to ensure accuracy with respect to numbers (e.g., amounts, temperature, etc.), but some errors and deviations must be accounted for. Unless otherwise indicated, parts are parts by weight, temperature is in ° C. or is at ambient temperature, and pressure is at or near atmospheric pressure. Percentages relating to compositions are expressed as % by weight, unless otherwise indicated.

[0066] There are many variations and combinations of reaction conditions, such as component concentrations, desired solvents, solvent mixtures, temperatures, pressures, and other reaction ranges and conditions, that can be used to optimize the purity and yield of the products obtained from the described processes. Optimization of such process conditions will require only reasonable and routine experimentation.

[0067] Example 1 Control and example compositions were prepared according to Tables 1A and 1B: [Table 1] [Table 2]

[0068] The properties of the compositions in Tables 1A and 1B were determined as follows and are reported in Tables 1C and 1D, respectively. [Table 3] [Table 4]

[0069] The reflectance data for the compositions at 450 nanometers (nm) is presented above. The % reflectance vs. wavelength curves for the samples are provided in Figure 1. From the data, it is observed that the reflectance of the compositions varied with wavelength. Overall, the control compositions (C1.1, C1.2, C2, and C3) were unable to exceed 50% reflectance at any wavelength. Control composition C1.1 achieved the highest reflectance, approaching but not reaching 50% at higher wavelengths from 650-700 nm.

[0070] Furthermore, adding an LDS additive to the composition was observed to decrease the reflectance across all wavelengths (see, e.g., C1.2 and C2), illustrating the problems and challenges in producing LDS compounds combined with high reflectance properties. Compositions with certain LDS additives (e.g., coated TiO2, control composition C3) can mitigate the decrease in reflectance, but the reflectance is still relatively low.

[0071] By increasing the titanium content even further (see example compositions Ex1, Ex2.1, Ex2.2, Ex3), the reflectance increased to over 50% across most wavelengths. Moreover, at wavelengths between 400 nm and 550 nm (including the conventional LED industry requirement of 450 nm), the reflectance of the example compositions was very high.

[0072] Reflectance can be determined according to conventional methods and using conventional equipment. The reflectance data described herein and shown in Figure 1 was measured using a GretagMacbeth Color-Eye® 7000A at wavelength intervals of 360-750 nm. Reflectance can also be measured using a Shimadzu UV-3150 spectrophotometer at wavelengths of 200-800 nm.

[0073] Example 2 Control and example compositions were prepared according to Table 2A. Composition properties are shown in Table 2B. [Table 5] [Table 6]

[0074] The data of Example 2 shows that the tin-antimony based LDS additive is very effective on the LDS plating properties (see FIG. 2). However, PCT is a crystalline polymer and its crystallinity is difficult to maintain. By introducing a metal additive such as the tin-antimony LDS additive into the glass-filled PCT system, the crystallinity and therefore the HDT was significantly reduced (compared to C2.1-C2.2), especially at higher pressures such as 1.8 MPa, which was reduced to about 100°C.

[0075] It has been found that by incorporating titanium oxide according to embodiments of the present disclosure, the HDT can be maintained at high levels (Ex2.1), perhaps above 200° C. at high pressure, and above 250° C. at low pressure. Such compositions are suitable for use in soldering applications.

[0076] The combination of LDS additive and titanium oxide can be used in various amounts and types (Ex2.1, Ex2.2, Ex2.3). Suitable combinations include tin or tin-antimony oxide and titanium oxide as in Ex2.1. The combination can also be pre-synthesized or pre-blended chemicals such as titanium oxide coated tin or tin-antimony oxide (Ex2.2). The combination can also be a combination of these (Ex2.3).

[0077] Example 3 Control and example compositions were prepared according to Table 3A. Composition properties are shown in Table 3B. [Table 7] [Table 8]

[0078] Images of plaques of some of these LDS plating compositions are shown in Figure 3. The data of Example 3 combined with some of the data from Example 2 demonstrate the effect of the ratio of titanium to LDS additive on the heat resistance properties of the PCT compositions. Ex2.1 contains 10 wt% titanium oxide and 10 wt% LDS (i.e., a 1:1 titanium:LDS ratio) and has good heat resistance properties, demonstrating that this ratio is preferred.

[0079] Ex2.2 includes an LDS additive that includes TiO2 coated with (Sn / Sb)O2. The additive includes about 45-65% titanium and about 35-55% (Sn / Sb)O2, with a titanium to LDS additive ratio of about 0.8-1.9. This range of titanium:LDS additive ratio also provides the composition with good heat resistance properties. Based on these examples, a lower limit of titanium:LDS additive of 0.7:1 is preferred.

[0080] Ex3.1, Ex3.2, and Ex3.3 demonstrate that there is no upper limit to the ratio of titanium to LDS additive. The titanium oxide content can be as high as 30 wt%, but is not necessarily limited to 30 wt%. The LDS additive content can be as low as 5 wt% or as high as 20 wt%, but is not necessarily limited to 20 wt%. Thus, the ratio of titanium to LDS additive can be 1:1, 2:1, 4:1, 6:1, or higher. In each composition, the heat resistant properties of the PCT composition are maintained.

[0081] Furthermore, there is no necessarily upper limit on the glass fiber content. Examples are provided where the glass fiber content is greater than 20%. Furthermore, the type of PCT does not affect the properties of the composition. See Ex3.3, Ex3.4, and Ex3.5.

[0082] Example 4 Control and example compositions were prepared according to Table 4A. Composition properties are shown in Table 4B. [Table 9] [Table 10]

[0083] The data of Example 4 further demonstrates the effect of the titanium to PCT ratio on the properties of the composition. In Comparative Example C4, the titanium oxide is 40 wt % and the PCT is 34.3 wt %. Thus, the titanium:PCT ratio is 1.2:1. The heat resistance of this composition is very low, especially at high pressure of 1.8 MPa, where the HDT drops by 100°C. Although this composition has a high whiteness (L value), this composition is no longer suitable for soldering applications. Compared to Example 3 (Ex3.3 and Ex3.4), the heat resistance properties of the PCT composition are maintained by keeping the titanium to PCT ratio below 1.2.

[0084] This ratio is also acceptable when adding further components such as thermally conductive fillers (Ex4). Minimizing the ratio of titanium to PCT below 1:1 and replacing 10% by weight of titanium with 10% of a thermally conductive filler (e.g., boron nitride) minimizes the loss of whiteness and reflectance, maintains heat resistance properties, and improves the thermal conductivity of the composition. The combination of whiteness, reflectance, heat resistance, thermal conductivity, and LDS plating properties provides a composition that is valuable for use in solder ignition applications. Such properties are achieved by compositions according to embodiments of the present disclosure that include the use of PCT, glass fiber, LDS additive, titanium, and optionally a thermally conductive filler.

[0085] For the thermal conductivity (TC) data reported herein, pellets extruded from the extruder were injection molded into 80 mm x 10 mm x 3 mm bars and cut into 10 mm x 10 mm x 3 mm square samples for through-plane TC measurements, and 100 mm diameter x 0.4 mm thick sheets were cut into 25 mm diameter x 0.4 mm thick circular samples for in-plane TC measurements.

[0086] Thermal conductivity, (κ, W / mK), is measured by Nanoflash LFA447 using a Pyroceram reference of similar thickness. This measurement determines the thermal diffusivity (α, cm2 / s) and specific heat (Cp, J / gK) of the sample, along with the density (ρ, g / cm3), measured using the water immersion method (ASTM D792). The product of the three values ​​gives the through-plane and in-plane thermal conductivity according to κ=α(T)Cp(T)ρ(T). Each point was repeated three times to ensure that the exact TC was measured.

[0087] As described herein, the compositions according to the embodiments of the present disclosure have good heat resistance properties resulting from the crystallization of crystalline polymers. Conventional polymers such as polyamides have a strong ability to maintain crystallization without being easily destroyed by additives or ingredients. The inclusion of LDS additives in polyamide resin systems does not adversely affect the heat resistance properties of crystalline polyamides. However, in PCT resin systems, the inclusion of LDS additives adversely affects the heat resistance properties of crystalline PCT. However, PCT-based compositions according to the embodiments of the present disclosure have improved heat resistance properties even with the inclusion of LDS additives. It was found that the combination of titanium and LDS in PCT adequately maintains the heat resistance of PCT. This was a surprising and novel discovery.

[0088] The data in Example 2 (Tables 2A and 2B) demonstrated the adverse effect of the addition of the LDS additive on the crystallization and heat resistance properties of PCT, and further demonstrated that the inclusion of titanium allowed the composition to maintain its crystallization and heat resistance properties.

[0089] The data of Example 3 (Tables 3A and 3B) demonstrated the effect of the ratio of titanium to LDS additive. The discovery of maintaining the heat resistance properties of PCT does not necessarily apply to open or free ratios of titanium and LDS additive. However, by maintaining the ratio of titanium to LDS additive within the ratios described herein, additional novel and inventive performance results are provided.

[0090] The data of Example 4 (Tables 4A and 4B) demonstrated the effect of the ratio of titanium to PCT in the disclosed compositions. The discovery of maintaining the heat resistance properties of PCT does not necessarily apply to the free ratio of titanium and PCT. However, by maintaining the ratio of titanium to PCT within the ratios described herein, additional novel and inventive performance results are provided.

[0091] The above description is intended to be illustrative, not limiting. For example, the above examples (or one or more aspects thereof) may be used in combination with each other. Other aspects may be used by one of ordinary skill in the art, etc., upon review of the preceding description. The Abstract is provided to comply with 37 CFR §1.72(b) to enable the reader to quickly ascertain the nature of the technical disclosure. It is submitted with the understanding that it will not be used to interpret or limit the scope or meaning of the claims. Also, in the above Detailed Description, various features may be grouped together to streamline the disclosure. This should not be construed as intending that an unclaimed disclosed feature is essential to the claim. Rather, the subject matter of the invention may comprise less than all features of a particular disclosed aspect. Accordingly, the following claims are hereby incorporated into the Detailed Description as an example or aspect, with each claim standing by itself as a separate aspect, and it is contemplated that such aspects may be combined with each other in various combinations or permutations. The scope of the present disclosure should be determined with reference to the appended claims, along with the full scope of equivalents to which such claims are entitled.

Claims

1. (a) about 34.3% to about 54.3% by weight of poly(cyclohexylene dimethylene terephthalate) (PCT) or a copolymer thereof; (b) about 20% to about 53.7% by weight of a reinforcing filler comprising glass fibers; (c) about 2% to about 20% by weight of a laser direct structuring (LDS) additive comprising tin oxide, antimony oxide, or a combination thereof; (d) about 10% to about 20% by weight of a reflective additive comprising a titanium compound, (1) the weight ratio of the total titanium in the composition to the LDS additive in the composition is at least 0.7 / 1; or (2) the weight ratio of the total titanium in the composition to the PCT is 1.1 / 1 or less; the tin oxide or antimony oxide is present as the LDS additive or as a coating on a further LDS additive; A thermoplastic composition, wherein all weight percent values ​​are based on the total weight of the composition and the sum of all component weight percent values ​​is 100.

2. 10. The thermoplastic composition of claim 1, wherein the tin oxide or the antimony oxide is in the form of a coating on a further LDS additive.

3. 3. The thermoplastic composition of claim 2, wherein the further LDS additive comprises titanium oxide.

4. The thermoplastic composition of claim 1, wherein the composition further comprises a thermally conductive filler different from the reinforcing filler in element (b).

5. The thermoplastic composition of claim 4 , wherein the thermally conductive filler comprises boron nitride.

6. The thermoplastic composition of claim 1 , wherein the reinforcing filler further comprises ceramic fiber, carbon fiber, inorganic filler, or a combination thereof.

7. 7. The thermoplastic composition of any one of claims 1 to 6, wherein the composition has a heat distortion temperature (HDT) of at least 220°C at 1.82 megapascals (MPa) and a sample thickness of 3.2 millimeters (mm), or a HDT of at least 200°C at 0.45 MPa and a sample thickness of 3.2 mm.

8. The composition is CIE L * a * b * An L of at least 70 as determined according to a color space standard * The thermoplastic composition according to any one of claims 1 to 6, having the formula:

9. The thermoplastic composition of any one of claims 1 to 6, wherein the composition has a reflectance of about 50% to about 95% at wavelengths from 400 nanometers (nm) to 750 nm.

10. 7. The thermoplastic composition of any one of claims 1 to 6, wherein the composition has an in-plane thermal conductivity of at least 0.5 Watts per meter Kelvin (W / (mK)) or a through-plane thermal conductivity of at least 0.5 W / (mK).

11. The thermoplastic composition according to any one of claims 1 to 6, wherein the composition further comprises one or more additional additives.

12. 12. The thermoplastic composition of claim 11, wherein the one or more further additives comprise an impact modifier, an acid scavenger, an anti-drip agent, an antioxidant, an antistatic agent, a chain extender, a colorant, a demolding agent, a flow promoter, a lubricant, a release agent, a plasticizer, a quenching agent, a flame retardant, a UV reflective additive, or a combination thereof.

13. 7. An article comprising the thermoplastic composition according to any one of claims 1 to 6, wherein the article is a component of a light emitting diode (LED) or a component of a 5G network communication device.

Citation Information

Patent Citations

  • NMT polyester composition with LDS function

    CN105623206A

  • Highly heat-resistant resin composition having high reflectance

    JP1992142362A

  • Thermoplastic resin composition, resin molding product, and method for producing resin molding product having plating layer

    WO2013141157A1

  • Thermoplastic resin composition, resin molded article, and method for producing plating-layer-equipped resin molded article

    WO2015033955A1