Rubber Compositions Combining Bagasse-Containing Guayule Rubber and Silanes and Related Methods
A tire rubber composition using guayule rubber, a silica-free filler, and silanes enhances rolling resistance by addressing the detrimental effects of bagasse, offering significant performance improvements.
Patent Information
- Application Number
- JP2023537121
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-18
- Filing Date
- 2021-12-16
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-12-16
AI Technical Summary
The presence of bagasse in guayule rubber compositions can detrimentally affect the properties of tire rubber, particularly in tread compositions, and existing technologies do not effectively address this issue.
A tire rubber composition is developed using guayule rubber as the majority component, combined with a silica-free filler and at least one silane, such as mercaptosilanes, blocked mercaptosilanes, or alkoxysilanes, to improve rolling resistance.
The composition achieves improved rolling resistance compared to control compositions without silica and silane, with potential improvements ranging from 3% to 20% or more.
Smart Images

Figure 0007568861000001 
Figure 0007568861000002 
Figure 0007568861000003
Abstract
Description
[Technical field]
[0001] This application is directed to a tire rubber composition that combines bagasse-containing guayule rubber and a silane in the absence of silica filler, and an associated method of reducing the rolling resistance of the tire rubber composition. Summary of the Invention [Problem to be solved by the invention]
[0002] The guayule plant (Parthenium argentatum) is a woody, shrub-like plant that contains rubber within the plant's cells. The process aimed at isolating rubber from the guayule plant requires isolating it from woody material (called bagasse). The presence of bagasse in guayule rubber can be detrimental to the properties of the rubber composition, especially when the rubber composition is used in tires (e.g., in tread rubber compositions).
[0003] Disclosed herein is a rubber composition comprising a majority by weight of guayule rubber as a rubber component comprising a bagasse component, a silica-free filler component, and at least one silane. Also disclosed is a method of improving the rolling resistance of a tire rubber composition by providing a rubber composition comprising a majority by weight of guayule rubber as a rubber component comprising a bagasse component, a silica-free filler component, and at least one silane.
[0004] In a first embodiment, a method of improving the rolling resistance of a tire rubber composition is provided, the method comprising providing a rubber composition comprising a rubber component comprising a majority by weight of guayule rubber, the rubber component comprising a bagasse component, and a silica-free filler component, by including at least one silane in the rubber composition, the at least one silane being selected from the group consisting of mercaptosilanes, blocked mercaptosilanes, and alkoxysilanes.
[0005] In a second embodiment, a tire rubber composition is provided that includes: (a) 100 parts of a rubber component including a majority by weight of guayule rubber that includes a bagasse component, (b) a silica-free filler component, and (c) at least one silane selected from the group consisting of mercaptosilanes, blocked mercaptosilanes, and alkoxysilanes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0006] Disclosed herein is a rubber composition comprising a majority by weight of guayule rubber as a rubber component comprising a bagasse component, a silica-free filler component, and at least one silane. Also disclosed is a method of improving the rolling resistance of a tire rubber composition by providing a rubber composition comprising a majority by weight of guayule rubber as a rubber component comprising a bagasse component, a silica-free filler component, and at least one silane.
[0007] In a first embodiment, a method of improving the rolling resistance of a tire rubber composition is provided, the method comprising providing a rubber composition comprising a rubber component comprising a majority by weight of guayule rubber, the rubber component comprising a bagasse component, and a silica-free filler component, by including at least one silane in the rubber composition, the at least one silane being selected from the group consisting of mercaptosilanes, blocked mercaptosilanes, and alkoxysilanes.
[0008] In a second embodiment, a tire rubber composition is provided that includes: (a) 100 parts of a rubber component including a majority by weight of guayule rubber that includes a bagasse component, (b) a silica-free filler component, and (c) at least one silane selected from the group consisting of mercaptosilanes, blocked mercaptosilanes, and alkoxysilanes.
[0009] definition The terminology used herein is for the purpose of describing the embodiments only and is not to be construed as limiting the invention as a whole.
[0010] As used herein, the term "BR" or "polybutadiene" refers to a homopolymer of 1,3-butadiene.
[0011] As used herein, the term "major amount" refers to more than 50% (e.g., at least 50.1%, at least 50.5%, at least 51%, etc.).
[0012] As used herein, the term "less than half" refers to less than 50% (eg, 49.5% or less, 49% or less, etc.).
[0013] As used herein, the abbreviation Mn is used for number average molecular weight.
[0014] As used herein, the abbreviation Mp is used for peak molecular weight.
[0015] As used herein, the abbreviation Mw is used for weight average molecular weight.
[0016] Unless otherwise specified herein, the term "Mooney viscosity" refers to Mooney viscosity, ML 1+4 Those skilled in the art will appreciate that the Mooney viscosity of a rubber composition is measured prior to vulcanization or curing.
[0017] As used herein, the term "natural rubber" refers to naturally occurring rubber such as that which can be harvested from sources such as the Hevea rubber tree and from non-Hevea sources (e.g., the guayule plant and dandelion such as TKS). In other words, the term "natural rubber" should be interpreted to exclude synthetic polyisoprene.
[0018] As used herein, the term "guayule rubber" is a subclass of natural rubber harvested from the guayule plant. In contrast, natural rubber not harvested from the guayule plant is referred to herein as "non-guayule natural rubber" and can include hevea rubber as well as other sources such as dandelion.
[0019] As used herein, the term "phr" means parts per hundred of rubber. 100 parts of rubber is also referred to herein as 100 parts of the rubber component.
[0020] As used herein, the term "polyisoprene" refers to synthetic polyisoprene. In other words, the term is used to indicate a polymer made from isoprene monomers, and should not be construed to include naturally occurring rubbers (e.g., Hevea rubber, guayule rubber, or dandelion rubber). However, the term "polyisoprene" should be construed to include polyisoprene made from natural sources of isoprene monomers.
[0021] As used herein, the term "SBR" means styrene-butadiene copolymer rubber.
[0022] As used herein, the term "tread" refers to that portion of the tire that contacts the road under normal inflation and load, and the term "subtread" refers to that portion below the tread that generally does not contact the road.
[0023] Rubber component As noted above, in accordance with the first and second embodiments, the tire rubber composition includes a rubber component that includes a majority by weight (e.g., 51%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, or 100%) of guayule rubber, which includes a bagasse component. In certain embodiments of the first and second embodiments, the rubber component includes at least 60% by weight (e.g., 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, 60-100%, 60-90%, 60-80%, 60-70%, etc.) of guayule rubber. In certain embodiments of the first and second embodiments, the rubber component comprises at least 70% by weight (e.g., 70%, 75%, 80%, 85%, 90%, 95%, 100%, 70-100%, 70-90%, 70-80%, etc.) guayule rubber. In yet other embodiments of the first and second embodiments, the entirety (i.e., 100% by weight) of the rubber component is guayule rubber.
[0024] According to the first and second embodiments disclosed herein, the Mw and Mn of the guayule rubber used in the rubber composition can vary. In preferred embodiments of the first and second embodiments, the guayule rubber has a Mw and Mn of at least 1 million grams / mole (e.g., 1 million, 1.1 million, 1.2 million, 1.3 million, 1.4 million, 1.5 million, 1.6 million, 1.7 million, 1.8 million, 1.9 million, 2 million, or more) or between 1 million and 2 million grams / mole (e.g., 1 million, 1.1 million, 1.2 million, 1.3 million, 1.4 million, 1.5 million, 1.6 million, 1.7 million, 1.8 million, 1.9 million, 2 million, or more). The Mw of the copolymer is preferably from 1.3 million to 2 million grams / mole (e.g., 1.3 million, 1.4 million, 1.5 million, 1.6 million, 1.7 million, 1.8 million, 1.9 million, or 2 million), more preferably from 1.5 million to 2 million grams / mole (e.g., 1 million, 1.5 million, 1.6 million, 1.7 million, 1.8 million, 1.9 million, or 2 million). In preferred embodiments of the first and second embodiments, the guayule rubber has a viscosity of at least 200,000 grams / mole (e.g., 200,000; 250,000; 300,000; 350,000; 400,000; 450,000; 500,000; 550,000; or more), or between 200,000 and 500,000 grams / mole (e.g., 200,000; 250,000; 300,000; 350,000; 40 In certain embodiments of the first and second embodiments, the guayule rubber has a Mw and Mn each within one of the ranges set forth above, preferably a Mw and Mn each within one of the preferred ranges set forth above, more preferably a Mw and Mn each within one of the more preferred ranges set forth above.
[0025] In certain embodiments of the first and second embodiments disclosed herein, the amount of guayule resin present in the guayule rubber is limited. In preferred embodiments of the first and second embodiments, the guayule rubber comprises 5% by weight or less of guayule resin (e.g., 5%, 4.5%, 4%, 3.5%, 3%, 2.5%, 2%, 1.5%, 1%, 0.5% or less), preferably 4% by weight or less of guayule resin (e.g., 4%, 3.5%, 3%, 2.5%, 2%, 1.5%, 1%, 0.5% or less), more preferably less than 4% guayule resin (e.g., 3.9%, 3.5%, 3%, 2.5%, 2%, 1.5%, 1%, 0.5% or less), even more preferably less than 1% guayule resin (e.g., 0.9%, 0.8%, 0.7%, 0.6%, 0.5%, 0.4%, 0.3%, 0.2%, 0.1% or 0%).
[0026] According to the first and second embodiments disclosed herein, the amount of bagasse present in the guayule rubber (i.e., the bagasse component) can vary. In preferred embodiments of the first and second embodiments, the bagasse component comprises 1-20% by weight (e.g., 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%) guayule rubber. In the above specific embodiment, the bagasse component more preferably comprises 1-10% by weight (e.g., 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, or 10%) guayule rubber, or less than 5% by weight (e.g., 4.9%, 4.5%, 4%, 3.5%, 3%, 2.5%, 2%, 1.5%, 1%, 0.5%, 0.4%, 0.3%, 0.2%, 0.1%, or less than 0.1%) guayule rubber. Generally, according to current technology methods, guayule rubber containing 0.00% by weight bagasse is not available. Thus, amounts less than or equal to 0.1% or less than 0.1% should be understood as including trace amounts of bagasse. In other embodiments of the first and second embodiments, the bagasse component constitutes 5-20% by weight (e.g., 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%), preferably 10-20% by weight (e.g., 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%), based on the weight of the guayule rubber. The embodiments of the first and second embodiments in which relatively more bagasse is present in the guayule rubber (e.g., 5-20% by weight or 10-20% by weight) may present advantages with respect to the isolation of guayule rubber from guayule plants, since by allowing more bagasse to be present, the processing costs and time associated with isolating guayule rubber from guayule plants may be reduced.
[0027] Overall, according to the first and second embodiments, the total amount of rubber present in the rubber component of the rubber composition should be understood to be 100 parts. Thus, in certain embodiments of the first and second embodiments, the rubber component can be understood as comprising less than half by weight of at least one additional rubber. The specific amount that constitutes less than half by weight of the at least one additional rubber varies depending on the amount of guayule rubber used. As a non-limiting example, if the rubber component comprises 60% by weight of guayule rubber (or 60 parts of guayule rubber), 40% by weight of the rubber component is comprised of at least one additional rubber. Thus, generally, if at least one additional rubber is present, it constitutes an amount of 49-1%, 49-5%, 49-10%, 40-1%, 40-5%, 40-10%, 30-1%, 30-5%, 30-10% (all amounts by weight based on the total weight of the rubber component), etc. The specific additional rubber or rubbers used may vary. In preferred embodiments of the first and second embodiments, the rubber component comprises less than half by weight of at least one rubber selected from the group consisting of non-guayule natural rubber (e.g., hevea natural rubber or natural rubber from non-hevea and non-guayule sources such as dandelion), polyisoprene, polybutadiene having at least 90% cis-1,4-bond content, functionalized polybutadiene having at least 90% cis-1,4-bond content, styrene-butadiene rubber, and functionalized styrene-butadiene rubber.
[0028] In the first and second embodiments in which the rubber component comprises a functionalized rubber (e.g., a functionalized polybutadiene having a cis-1,4-bond content of at least 90% and / or a functionalized SBR), the functional groups present may vary. According to the preferred embodiment described above, the functional groups used are carbon black reactive, and in a more preferred embodiment, the functional groups comprise polar groups. Non-limiting examples of suitable functional groups (for BR and SBR) include, but are not limited to, hydroxyl, carbonyl, ether, ester, halide, amine, imine, amide, nitrile, and oxirane (e.g., epoxy ring) groups. When a functionalized polymer is used, the functional groups may be incorporated into the head and / or tail of the polymer and / or may be added along the polymer backbone. Non-limiting examples of functionalized initiators include organoalkali metal compounds (e.g., organolithium compounds) containing one or more heteroatoms (e.g., nitrogen, oxygen, boron, silicon, sulfur, tin, and phosphorus atoms) or heterocyclic groups containing such atoms, often further containing one or more nitrogen atoms (e.g., substituted aldimines, ketimines, secondary amines, etc.), optionally pre-reacted with compounds such as diisopropenylbenzene. Many functional initiators are known in the art. Exemplary ones are disclosed in U.S. Pat. Nos. 5,153,159, 5,332,810, 5,329,005, 5,578,542, 5,393,721, 5,698,464, 5,491,230, 5,521,309, 5,496,940, 5,567,815, 5,574,109, 5,786,441, 7,153,919, 7,868,110, and U.S. Patent Application Publication No. 2011-0112263, which are incorporated herein by reference. In certain embodiments of the first and second embodiments, when a functional initiator is used, a functional nitrogen-containing initiator is utilized, non-limiting examples of which include cyclic amines, particularly cyclic secondary amines such as azetidine; pyrrolidine; piperidine; morpholine; N-alkyl piperazines; hexamethyleneimine; heptamethyleneimine, and dodecamethyleneimine.
[0029] Styrene-butadiene rubber According to the first and second embodiments disclosed herein, when at least one SBR is present in the rubber component of the rubber composition, the Mw, Mn, and polydispersity (Mw / Mn) of the styrene-butadiene rubber can vary. In certain embodiments of the first and second embodiments, the SBR has a Mw of 300,000 to 600,000 grams / mole (e.g., 300,000; 325,000; 350,000; 375,000; 400,000; 425,000; 450,000; 475,000; 500,000; 525,000; 550,000; 575,000; or 600,000 grams / mole). In certain embodiments of the first and second embodiments, the SBR has a Mw of 350,000 to 550,000, or 400,000 to 500,000 grams / mole. The Mw values referred to herein are weight average molecular weights, which can be determined by using gel permeation chromatography (GPC) calibrated with styrene-butadiene standards and the Mark-Hawin constant for the polymer of interest. In certain embodiments of the first and second embodiments, the SBR has a Mn of 200,000 to 400,000 grams / mole (e.g., 200,000; 225,000; 250,000; 275,000; 300,000; 325,000; 350,000; 375,000; or 400,000 grams / mole). In certain embodiments of the first and second embodiments, the SBR has an Mn of 200,000 to 300,000. The Mn values referred to herein are number average molecular weights, which can be determined by using gel permeation chromatography (GPC) calibrated with styrene-butadiene standards and the Mark-Hawin constant for the polymer of interest. In certain embodiments of the first and second embodiments disclosed herein, the SBR has an Mw / Mn (polydispersity) of 1.2 to 2.5 (e.g., 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, or 2.5, preferably 1.3 to 2).In certain embodiments of the first and second embodiments, the Mw, Mn, and Mw / Mn of the SBR all fall within one of the ranges set forth above, and in certain such embodiments, the Mw, Mn, and Mw / Mn each fall within one of the preferred ranges set forth above. In other embodiments of the first and second embodiments, the SBR utilized is (a) an SBR having a Mw of 350,000 to 600,000 grams / mole (e.g., 350,000; 400,000; 450,000; 500,000; 550,000; or 600,000 grams / mole), or an SBR having a Mw of 400,000 to 550,000 grams / mole (e.g., 400,000; 425,000; 450,000; 475,000; 500,000; 525,000; or 550,000 grams / mole) within one of the aforementioned ranges. , Mn, and / or Mw / Mn, or (b) only one or more SBRs having a Mw of 350,000 to 600,000 grams / mole (e.g., 350,000; 400,000; 450,000; 500,000; 550,000; or 600,000 grams / mole), or 400,000 to 550,000 grams / mole (e.g., 400,000; 425,000; 450,000; 475,000; 500,000; 525,000; or 550,000 grams / mole).
[0030] According to the first and second embodiments, the Tg of any SBR used in the rubber component can vary. In certain preferred embodiments in the first and second embodiments, the SBR has a Tg of about -75 to about -50°C, -75 to -50°C (e.g., -75, -70, -65, -60, -55, or -50°C), preferably -70 to -55°C (e.g., -70, -65, -60, or -55°C), or more preferably -65 to -55°C (e.g., -65, -60, or -55°C). In other embodiments in the first and second embodiments, the SBR used may be an SBR having a Tg of about -10 to about -70°C, -10 to -70°C (e.g., -10, -15, -20, -25, -30, -35, -40, -45, -50, -55, -60, -65, or -70°C), preferably about -10 to about -49°C or -10 to -49°C (e.g., -10, -12, -14, -15, -16, -18, -20, -22, -24, -26, -28, -30, -32, -34, -36, -35, -38, -40, -42, -44, -45, -46, -48, or -49°C). SBR may have a Tg in one of the aforementioned ranges, optionally in combination with one or more of the above Mw, Mn, and / or Mw / Mn ranges, and in certain embodiments, optionally in combination with one of the styrene monomer contents described below. The Tg values mentioned herein for elastomers represent Tg measurements made on elastomers without any oil extension. In other words, for oil-extended elastomers, the above Tg values refer to the Tg before oil extension, or to the unextended version of the same elastomer. Elastomer or polymer Tg values may be measured using a differential scanning calorimetry (DSC) instrument, such as that manufactured by TA Instruments (New Castle, Delaware), with measurements performed using a 10°C / min temperature increase after cooling at -120°C. A tangent is then drawn to the baseline before and after the jump in the DSC curve. The temperature on the DSC curve (read at the point corresponding to the middle of the two tangent points) can be used as the Tg.
[0031] According to the first and second embodiments, the styrene monomer content (i.e., the weight percent of polymer chains that contain styrene units as opposed to butadiene units) of any SBR used in the rubber component can vary. In certain embodiments of the first and second embodiments, the styrene monomer content of the SBR is about 10 to about 40% by weight, 10 to 40% by weight (e.g., 10%, 15%, 20%, 25%, 30%, 35%, or 40%), 10 to 30% by weight (e.g., 10%, 15%, 20%, 25%, or 30%), or 10 to 20% by weight (e.g., 10%, 12%, 14%, 16%, 18%, or 20%). In certain embodiments of the first and second embodiments, the SBR can have a styrene monomer content in one of the ranges previously described, optionally in combination with one or more of the Mw, Mn, and / or Mw / Mn ranges described below, and in certain embodiments, optionally in combination with the Tg ranges above and / or one of the following vinyl bond contents:
[0032] According to the first and second embodiments, the vinyl bond content (i.e., 1,2-microstructure) of any SBR used in the elastomer component can vary. In certain embodiments of the first and second embodiments, the vinyl bond content of the SBR is about 10 to about 50%, 10 to 50% (e.g., 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, or 50%), about 10 to about 40%, 10 to 40% (e.g., 10%, 15%, 20%, 25%, 30%, 35%, or 40%), about 20 to about 40%, or 20 to 40% (e.g., 20%, 25%, 30%, 35%, or 40%). In certain embodiments of the first and second embodiments, the SBR may have a vinyl bond content in one of the aforementioned ranges, optionally in combination with one or more of the above Mw, Mn, Mw / Mn, Tg, and / or styrene monomer content ranges. The vinyl bond content referred to herein should be understood as referring to the total vinyl bond content in the SBR polymer chain, not the vinyl bond content in the butadiene portion of the SBR polymer chain, and H 1 -NMR and C13 - NMR (for example, using a 300 MHz Gemini 300 NMR spectrometer system (Varian)).
[0033] Polybutadiene According to the first and second embodiments, the rubber component of the rubber composition may include a polybutadiene rubber. The particular type of polybutadiene rubber utilized may vary. Preferably, according to the first and second embodiments, any polybutadiene rubber present in the rubber component has a cis bond content of at least 90% (e.g., 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, or more), preferably at least 92% (e.g., 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, or more), more preferably at least 95% (e.g., 95%, 96%, 97%, 98%, 99%, or more), and a Tg of less than -101°C (e.g., -102, -103, -104, -105, -106, -107, -108, -109°C, or less). In certain such embodiments, the Tg of the polybutadiene rubber is -101 to -110°C. Cis bond content refers to cis 1,4-bond content. Cis 1,4-bond content referred to herein is determined by FTIR (Fourier Transform Infrared Spectroscopy), where a polymer sample is dissolved in CS2 and then subjected to FTIR. In certain embodiments of the first and second embodiments, the polybutadiene rubber present in the rubber component may have a cis 1,4-bond content of at least 98% (e.g., 98%, 99%, or more), or at least 99% (e.g., 99%, 99.5%, or more). In certain embodiments of the first and second embodiments, any polybutadiene rubber present in the rubber component has a Tg of -105°C or less (e.g., -105, -106, -107, -108, -109°C or less), such as -105 to -110°C or -105 to -108°C. In certain embodiments of the first and second embodiments, any polybutadiene rubber present in the rubber component contains less than 3% by weight (e.g., 3%, 2%, 1%, 0.5%, or less), preferably less than 1% by weight (e.g., 1%, 0.5%, or less) or 0% by weight of syndiotactic 1,2-polybutadiene.Generally, according to the first and second embodiments, one or more polybutadiene rubbers having a cis bond content of at least 92% and a Tg of less than -101°C can be used in the rubber component. In certain embodiments of the first to third embodiments, the only polybutadiene rubber used has a cis bond content of at least 92% (e.g., 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, or more) and a Tg of less than -101°C. As mentioned above, when polybutadiene is present in the rubber component, it may be optionally functionalized with one or more of the functional groups described above.
[0034] According to the first and second embodiments, when polybutadiene rubber is used in the rubber composition, the amount used may vary. Since guayule rubber is present in a majority amount, the total amount of any polybutadiene rubber present in the rubber component will be less than half by weight, i.e., less than 50 wt.%. In such embodiments of the first and second embodiments, the total amount of polybutadiene rubber present in the rubber component is less than 50 phr, less than 40 phr, less than 30 phr, less than 20 phr, or less than 10 phr. In certain embodiments of the first and second embodiments, the total amount of polybutadiene rubber present in the rubber component is 5-49 phr, 5-40 phr, 5-30 phr, 5-20 phr, 5-10 phr, 10-49 phr, 10-40 phr, 10-30 phr, 10-20 phr, 20-49 phr, 20-40 phr, or 20-30 phr.
[0035] Non-guayule natural rubber or polyisoprene According to the first and second embodiments, the rubber component may include non-guayule natural rubber, polyisoprene, or a combination thereof. In certain embodiments of the first and second embodiments, the rubber component includes non-guayule natural rubber but does not include polyisoprene. In other embodiments of the first and second embodiments, the rubber component includes only polyisoprene and does not include natural rubber. According to the first and second embodiments, if natural rubber is present in the rubber component, it is preferably Hevea natural rubber. When non-guayule natural rubber is used in the rubber composition of the first and second embodiments, the natural rubber preferably has a Mw of 1,000,000 to 2,000,000 grams / mole (e.g., 1,000,000, 1,100,000, 1,200,000, 1,300,000, 1,400,000, 1,500,000, 1,700,000, 1,800,000, 1,900,000, 2,000,000 grams / mole), 1,250,000 to 2,000,000 grams / mole, or 1,500,000 to 2,000,000 grams / mole (measured by GPC using polystyrene standards). When non-guayule natural rubber is used in the rubber composition of the first and second embodiments, the Tg of the natural rubber may vary. Preferably, according to the first and second embodiments, when non-guayule natural rubber is utilized, it has a Tg of −65 to −80° C. (e.g., −65, −66, −67, −68, −69, −70, −71, −72, −73, −74, −75, −76, −77, −78, −79, or −80° C.), more preferably a Tg of −67 to −77° C. (e.g., −67, −68, −69, −70, −71, −72, −73, −74, −75, −76, or −77° C.). When polyisoprene is utilized in the rubber compositions of the first and second embodiments, the Tg of the polyisoprene can vary.Preferably, according to the first and second embodiments, when polyisoprene is utilized, it has a Tg of −55 to −75° C. (e.g., −55, −56, −57, −58, −59, −60, −61, −62, −63, −64, −65, −66, −67, −68, −69, −70, −71, −72, −73, −74, or −75° C.), more preferably −58 to −74° C. (e.g., −58, −59, −60, −61, −62, −63, −64, −65, −66, −67, −68, −69, −70, −71, −72, −73, or −74° C.).
[0036] According to the first and second embodiments, when non-guayule natural rubber and / or polyisoprene is used in the rubber composition, the amount utilized may vary. Generally, according to the first and second embodiments, guayule rubber is used in a majority amount, so that the total amount of any non-guayule natural rubber and / or polyisoprene present in the rubber component is less than half by weight, i.e., less than 50 wt. %. In certain embodiments of the first and second embodiments, the total amount of non-guayule natural rubber and / or polyisoprene present in the rubber component is less than 50 phr, less than 40 phr, less than 30 phr, less than 20 phr, or less than 10 phr. In certain embodiments of the first and second embodiments, the total amount of non-guayule natural rubber and / or polyisoprene present in the rubber component is 5-49 phr, 5-40 phr, 5-30 phr, 5-20 phr, 5-10 phr, 10-49 phr, 10-40 phr, 10-30 phr, 10-20 phr, 20-49 phr, 20-40 phr, or 20-30 phr. In certain embodiments of the first and second embodiments, the rubber component comprises non-guayule natural rubber but no polyisoprene, and the amount of natural rubber is within one of the aforementioned ranges.
[0037] Filler Ingredients As mentioned above, according to the first and second embodiments, the rubber composition includes a filler component that does not include silica. By silica-free, it is meant that the filler component (and thus the entire rubber composition) contains 0 phr of silica. Without being bound by theory, the exclusion of silica from the filler component allows for the binding of at least one silane to the bagasse component (rather than the binding of at least one silane to the silica). According to the first and second embodiments disclosed herein, the amount and type of filler present in the filler component of the rubber composition can vary.
[0038] In certain preferred embodiments of the first and second embodiments disclosed herein, the filler component is present in an amount of 30 to 200 phr (e.g., 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, or 200 phr), more preferably 30 to 150 phr (e.g., 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, or 150 phr), or 40 to 120 phr (e.g., 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, or 140 phr). In certain preferred embodiments of the first and second embodiments disclosed herein, the filler component is present in one of the amounts described above and comprises a majority by weight of reinforcing carbon black (e.g., at least 60% by weight reinforcing carbon black, at least 70% by weight reinforcing carbon black, at least 80% by weight reinforcing carbon black, and at least 90% by weight reinforcing carbon black). In certain of the foregoing embodiments, the filler component is entirely reinforcing carbon black, i.e., 100% by weight of the filler component is reinforcing carbon black.
[0039] According to the first and second embodiments, the particular type of carbon black used may vary. In general, suitable carbon blacks for use as reinforcing fillers in the rubber compositions of the first and second embodiments have a carbon black content of at least about 20% by weight. 2 / g (at least 20m 2 / g), and more preferably at least about 35m 2 / g ~ Maximum approx. 200m 2 / g or higher (35m 2 / g~200m 2The carbon blacks include any of the commonly available commercially produced carbon blacks, including those having a surface area of 1000 nm to 1000 nm / g. Surface area values used herein for carbon blacks are determined by ASTM D-1765 using the cetyltrimethyl-ammonium bromide (CTAB) technique. Among the useful carbon blacks are furnace blacks, channel blacks, and lamp blacks. More specifically, examples of useful carbon blacks include super abrasion furnace (SAF) blacks, high abrasion furnace (HAF) blacks, fast extrusion furnace (FEF) blacks, fine furnace (FF) blacks, intermediate super abrasion furnace (ISAF) blacks, semi-reinforcing furnace (SRF) blacks, medium processable channel blacks, hard processable channel blacks, and conductive channel blacks. Other carbon blacks that can be utilized include acetylene blacks. In certain embodiments of the first and second embodiments, the rubber composition comprises a mixture of two or more of the above blacks. Preferably, according to the first and second embodiments, the carbon black filler, if present, consists of only one type (or grade) of reinforcing carbon black. Typical carbon blacks suitable for use in certain embodiments of the first and second embodiments are N-110, N-220, N-339, N-330, N-351, N-550 and N-660, as designated by ASTM D-1765-82a. The carbon black used can be in pelletized form or in non-pelletized flocculent form. Preferably, non-pelletized carbon black is preferred, as it provides a more homogeneous mixture.
[0040] In certain embodiments of the first and second embodiments, the tread rubber composition includes a reinforcing filler other than carbon black (i.e., additional reinforcing fillers). One or more additional reinforcing fillers may be utilized, but their total amount is preferably limited to 10 phr or less (e.g., 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, or 0 phr), or 5 phr or less (e.g., 5, 4, 3, 2, 1, or 0 phr). In certain preferred embodiments of the first and second embodiments, the rubber composition of the tread does not contain additional reinforcing fillers (i.e., 0 phr). In other words, in such embodiments, there are no reinforcing fillers other than carbon black.
[0041] In those embodiments in the first and second embodiments in which additional reinforcing fillers are utilized, the additional reinforcing fillers can vary. Non-limiting examples of suitable additional reinforcing fillers for use in the rubber compositions of certain embodiments in the first and second embodiments include, but are not limited to, alumina, aluminum hydroxide, clay (reinforcing grades), magnesium hydroxide, boron nitride, aluminum nitride, titanium dioxide, reinforcing zinc oxide, and combinations thereof.
[0042] In certain embodiments of the first and second embodiments, the rubber composition includes at least one non-reinforcing filler that is a non-carbon black non-reinforcing filler. In other preferred embodiments of the first and second embodiments, the rubber composition does not include a non-carbon black non-reinforcing filler (i.e., 0 phr). In yet other embodiments of the first and second embodiments, the rubber composition does not include a non-reinforcing filler (in such embodiments, the carbon black filler of the filler component is a reinforcing carbon black filler). In embodiments of the first and second embodiments in which at least one non-reinforcing filler is utilized, the at least one non-carbon black non-reinforcing filler may be selected from clay (non-reinforcing grades), graphite, magnesium dioxide, aluminum oxide, starch, boron nitride (non-reinforcing grades), silicon nitride, aluminum nitride (non-reinforcing grades), calcium silicate, silicon carbide, ground rubber, and combinations thereof. In certain preferred embodiments of the first and second embodiments, the rubber composition comprises 1 to 20 phr (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20 phr) of ground rubber, preferably 1 to 5 phr (e.g., 1, 2, 3, 4, or 5 phr) of ground rubber. 2 / g or less (20m 2 In certain embodiments, the solubility is about 10 m / g, 2 / g or less (10m 2The term "non-reinforcing filler" is used to mean a particulate material having a nitrogen adsorption specific surface area (N2SA) of less than 1000 nm / g (including less than 1000 nm). The N2SA surface area of a particulate material may be determined according to various standard methods, including ASTM D6556. In certain embodiments, the term "non-reinforcing filler" alternatively or additionally refers to a particulate material having a particle size greater than about 1000 nm (including greater than 1000 nm). In those embodiments in the first and second embodiments, non-carbon black non-reinforcing fillers are present in the rubber composition, and the total amount of non-carbon black non-reinforcing fillers can vary, but is preferably 20 phr or less (e.g., 20, 19, 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, 2, or 1 phr), and in certain embodiments, 1 to 10 phr, 10 phr or less, 5 phr or less (e.g., 5, 4, 3, 2, or 1 phr), 1 to 5 phr, or 1 phr or less.
[0043] At least one silane As described above, according to the first and second embodiments, the rubber composition includes at least one silane selected from the group consisting of mercaptosilane, blocked mercaptosilane, and alkoxysilane. As will be discussed in more detail below, alkoxysilane should be understood to include both sulfur-containing alkoxysilanes and non-sulfur-containing alkoxysilanes.
[0044] According to the first and second embodiments, the amount of the at least one silane used in the rubber composition may vary. Generally, the amount of silane used may be adjusted depending on the total amount of bagasse present in the rubber composition (bagasse is generally present as a component of guayule rubber). The amount of bagasse may vary depending on its concentration in the guayule rubber (generally 1-20% by weight) and depending on the amount of guayule rubber used in the rubber composition. In a preferred embodiment of the first and second embodiments, the at least one silane is present in a total amount of 0.1-5 phr (e.g., 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, or 5 phr), more preferably in a total amount of 0.2-1 phr (e.g., 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or 1 phr). In preferred embodiments of the first and second embodiments, the at least one silane is present in a total amount of 5 to 20 wt. % (e.g., 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20 wt. %) based on the amount of bagasse present in the rubber composition. As a non-limiting example, if the rubber component of the rubber composition comprises 70 wt. % guayule rubber (i.e., 70 wt. % of the rubber component is guayule rubber) and the guayule rubber contains 10 wt. % bagasse, the amount of bagasse in the rubber composition will be 7 phr. When the amount of 5 to 20 wt. % is applied to 7 phr of bagasse, the amount of silane will be in the range of 0.35 phr (i.e., 5%) to 1.4 phr (i.e., 20%). In certain embodiments of the first and second embodiments, the at least one silane is present in a total amount of 0.1 to 5 phr, preferably 0.2 to 1 phr, and is present in a total amount of 5 to 20 wt. % based on the amount of bagasse in the rubber composition.
[0045] According to the first and second embodiments disclosed herein, one or more silanes (as described above) can be used in the rubber composition. In preferred embodiments of the first and second embodiments, the rubber composition includes only one silane selected from the group consisting of mercaptosilanes, blocked mercaptosilanes, and alkoxysilanes. In other embodiments of the first and second embodiments, the rubber composition includes two silanes selected from the group consisting of mercaptosilanes, blocked mercaptosilanes, and alkoxysilanes. In embodiments where two (or more) silanes are used in the rubber composition, the total amount of all silanes is as described above.
[0046] In certain embodiments of the first and second embodiments disclosed herein, at least one silane is a non-sulfur-containing alkoxysilane. Preferably, according to such embodiments, the non-sulfur-containing alkoxysilane has the formula (I): [ka] (wherein n=2, 3, or 4; each R 1 are independently selected from hydrocarbyl groups having 1 to 20 carbons, preferably 2 to 18 carbons; R 2 is an alkyl group having 1 to 10 carbons, preferably 1 to 6, more preferably 1 to 3 carbons, or an aromatic group having 6 to 18 carbons, preferably 6 to 12 carbons). When n=2, the non-sulfur-containing alkoxysilane can be understood to be a dialkoxysilane. When n=3, the non-sulfur-containing alkoxysilane can be understood to be a trialkoxysilane. When n=4, the non-sulfur-containing alkoxysilane can be understood to be a tetraalkoxysilane.
[0047] In certain embodiments of the first and second embodiments, at least one silane is a non-sulfur-containing alkoxysilane having formula (I) where n=2, ie, a dialkoxysilane. Non-limiting examples of non-sulfur-containing alkoxysilanes that are dialkoxysilanes include dimethyldimethoxysilane, dimethyldiethoxysilane, dimethyldipropoxysilane, dimethyldiisopropoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, diethyldipropoxysilane, diethyldiisopropoxysilane, dipropyldimethoxysilane, dipropyldiethoxysilane, dibutyldimethoxysilane, dibutyldiethoxysilane, dipentyldimethoxysilane, dipentyldiethoxysilane, dihexyldimethoxysilane, dihexyldiethoxysilane, diheptyldimethoxysilane, diheptyldiethoxysilane, dioctyldimethoxysilane, dioctyldiethoxysilane, dinonyldimethoxysilane, dinonyldiethoxysilane, didecyldimethoxysilane, didecyldiethoxysilane, diundecyldimethoxysilane, diethyl silane, diundecyl diethoxysilane, didodecyl dimethoxysilane, didodecyl diethoxysilane, ditridecyl dimethoxysilane, ditridecyl diethoxysilane, ditetradecyl dimethoxysilane, dipentadecyl dimethoxysilane, ditetradecyl diethoxysilane, dipentadecyl diethoxysilane, dihexadecyl dimethoxysilane, dihexadecyl diethoxysilane, diheptadecyl dimethoxy Silanes include, but are not limited to, diheptadecyldiethoxysilane, dioctadecyldimethoxysilane, dioctadecyldiethoxysilane, dinonadecyldimethoxysilane, dinonadecyldiethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, diphenyldipropoxysilane, diphenyldiisopropoxysilane, dibenzyldimethoxysilane, and dibenzyldiethoxysilane.
[0048] In certain embodiments of the first and second embodiments, at least one silane is a non-sulfur-containing alkoxysilane having formula (I) where n=3, ie, a trialkoxysilane. Non-limiting examples of non-sulfur-containing alkoxysilanes that are trialkoxysilanes include methyltrimethoxysilane, methyltriethoxysilane, methyltripoxysilane, methyltriisopropoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltripoxysilane, ethyltriisopropoxysilane, propyltrimethoxysilane, propyltriethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, pentyltrimethoxysilane, pentyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, heptyltrimethoxysilane, heptyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, nonyltrimethoxysilane, nonyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, undec ... Examples of suitable silanes include, but are not limited to, butylsilane, undecyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, tridecyltrimethoxysilane, tridecyltriethoxysilane, tetradecyltrimethoxysilane, tetradecyltriethoxysilane, pentadecyltrimethoxysilane, pentadecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, heptadecyltrimethoxysilane, heptadecyltriethoxysilane, octadecyltrimethoxysilane, octadecyltriethoxysilane, nonadecyltrimethoxysilane, nonadecyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, phenyltripoxysilane, phenyltriisopropoxysilane, benzyltrimethoxysilane, and benzyltriethoxysilane.
[0049] In certain embodiments of the first and second embodiments, at least one silane is a non-sulfur-containing alkoxysilane having formula (I) where n=4, i.e., a tetraalkoxysilane. Non-limiting examples of non-sulfur-containing alkoxysilanes that are tetraalkoxysilanes include, but are not limited to, tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetraisopropoxysilane, tetrabutoxysilane, and tetraisobutoxysilane.
[0050] In certain embodiments of the first and second embodiments disclosed herein, at least one silane is a non-sulfur-containing bisalkoxysilane. The non-sulfur-containing bisalkoxysilane preferably contains two silicon atoms separated by a divalent hydrocarbyl group, and each silicon atom can be understood to have two or three alkoxy groups. In certain embodiments of the first and second embodiments, the non-sulfur-containing bisalkoxysilane has the formula (Y)G(Z), where G is a C1-C 50 Straight chain and branched alkylene, C2-C 50 Linear and branched alkenylene, C6-C 50 aromatic, each optionally containing a heteroatom selected from the group consisting of one or more O or one or more N, and combinations thereof; Y and Z may be the same or different and each independently represent a group of the formula Si(R 7 ) p (OR 8 ) 3-p (In the formula, each R 7 are independent, C1~C 20 aliphatic, alicyclic, or aromatic, R 8 is a C1-C6 aliphatic or alicyclic group, and p is an integer of 0 or 1. In a preferred embodiment of the first and second embodiments, when the non-sulfur-containing bisalkoxysilane has the above formula, G of the non-elastomeric reactive filler reinforcing agent is a C2-C6 aliphatic or alicyclic group. 20 Alkylene, alkenylene, and C6-C 20aromatic, each optionally containing a heteroatom selected from the group consisting of one or more O or one or more N, and combinations thereof. In certain embodiments of the first and second embodiments, the non-sulfur-containing bisalkoxysilane has the formula (Y)G(Z), where G is a C6-C 20 alkylene and alkenylene; 8 is selected from the group consisting of C1-C6 straight chain and branched aliphatics. In certain embodiments of the first and second embodiments, the non-sulfur-containing bisalkoxysilane has the formula (Y)G(Z), where G is a C4-C 20 Linear and branched alkylene, and C4-C 20It is selected from the group consisting of linear and branched alkenylenes, both of which optionally contain additional carbon atoms in the form of one or more aromatic rings. In certain embodiments, the non-sulfur-containing bisalkoxysilane is a bis(trialkoxy)silane having an alkoxy carbon portion selected from the group consisting of C1-C6 (i.e., methyl-hexyl), preferably C1-C3, and even more preferably C1-C2. Specific examples of such bis(trialkoxy)silanes include bis(trimethoxysilyl)ethane, bis(triethoxysilyl)ethane, bis(tributoxysilyl)ethane, bis(triethoxysilyl)propane, bis(trimethoxysilyl)propane, bis(tributoxysilyl)propane, bis(triethoxysilyl)butane, bis(trimethoxysilyl)butane, bis(tributoxysilyl)butane, bis(triethoxysilyl)isobutane, bis(trimethoxysilyl)isobutane, bis(tributoxysilyl)isobutane, bis(triethoxysilyl)hexane, bis(trimethoxysilyl)hexane, bis(tributoxysilyl)hexane, bis(triethoxysilyl)cyclohexane, bis(trimethoxysilyl)cyclohexane, bis(tributoxysilyl)cyclohexane, bis(trimethoxysilyl)heptane, bis(triethoxysilyl), silyl)heptane, bis(tributoxysilyl)heptane, bis(triethoxysilyl)octane, bis(trimethoxysilyl)octane, bis(tributoxysilyl)octane, bis(triethoxysilyl)nonane, bis(trimethoxysilyl)nonane, bis(tributoxysilyl)nonane, bis(triethoxysilyl)decane, bis(trimethoxysilyl)decane, bis(tributoxysilyl)decane, bis(triethoxy silyl)dodecane, bis(trimethoxysilyl)dodecane, bis(tributoxysilyl)dodecane, bis(triethoxysilyl)tetradecane, bis(trimethoxysilyl)tetradecane, bis(tributoxysilyl)tetradecane, bis(triethoxysilyl)octadecane, bis(trimethoxysilyl)octadecane, bis(tributoxysilyl)octadecane, and mixtures thereof.
[0051] In certain embodiments of the first and second embodiments disclosed herein, at least one silane is a sulfur-containing alkoxysilane having 2 to 6 alkoxysilane groups. Preferably, according to such embodiments, the sulfur-containing alkoxysilane is selected from disulfide alkoxysilanes or tetrasulfide alkoxysilanes. Disulfide alkoxysilanes can be understood as having two sulfur atoms (single-bonded to each other), each of which is bonded to a separate alkylene group bonded to a silicon atom, the silicon atom having two or three alkoxy groups. Tetrasulfide alkoxysilanes can be understood as having four sulfur atoms (single-bonded to each other), each of which is bonded to a separate alkylene group bonded to a silicon atom, the silicon atom having two or three alkoxy groups. In certain embodiments of the first and second embodiments, the disulfide alkoxysilane is represented by the formula (alkoxy) a (Alkyl) 3-a Si-(CH2) b -SS-(CH2) b -Si(alkyl) 3-a (alkoxy) a where a is 2 or 3; b is an integer from 1 to 10, preferably 2 to 8, more preferably 2 or 3; and the alkyl in the alkoxy group is selected from alkyl of 1 to 10 carbons, preferably 1 to 6 carbons, more preferably 1 to 4 carbons. In certain embodiments of the first and second embodiments, the tetrasulfide alkoxysilane has the formula (alkoxy) d (Alkyl) 3-d Si-(CH2) e SSSS-(CH2) e -Si(alkyl) 3-d (alkoxy) dwhere d is 2 or 3; e is an integer from 1 to 10, preferably 2 to 8, more preferably 2 or 3; and the alkyl in the alkoxy group is selected from alkyl of 1 to 10 carbons, preferably 1 to 6 carbons, more preferably 1 to 4 carbons. Alternatively, in other embodiments, the tetrasulfide alkoxysilane has an alkoxysilane alkylene moiety at only one end of the sulfur chain (e.g., the first sulfur) and another moiety is present at the other end of the sulfur chain (e.g., the fourth sulfur) (e.g., thiocarbamoyl, benzothiazole).
[0052] In certain embodiments of the first and second embodiments disclosed herein, when at least one silane is a disulfide alkoxysilane, it is selected from the group consisting of 3,3'-bis(triethoxysilylpropyl) disulfide, 3,3'-bis(trimethoxysilylpropyl) disulfide, 3,3'-bis(tributoxysilyl-propyl) disulfide, 3,3'-bis(tri-m-butoxysilyl-propyl) disulfide, 3,3'-bis(tripropoxypropyl) disulfide, 3,3'-bis(trihexoxysilylpropyl) disulfide, 2,2'-bis 12,12'-bis(triisopropoxysilylpropyl) disulfide, 3,3'-bis(dimethoxyphenylsilyl-2-methylpropyl) disulfide, and mixtures thereof.
[0053] In certain embodiments of the first and second embodiments disclosed herein, when the at least one silane is a tetrasulfide alkoxysilane, it is selected from the group consisting of bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-triethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-trimethoxysilylpropyl-benzotriazole tetrasulfide, 3-triethoxysilylpropyl benzotriazole tetrasulfide, and mixtures thereof.
[0054] In certain embodiments of the first and second embodiments disclosed herein, the at least one silane is a mercaptosilane compound. In certain such embodiments, the at least one silane comprises a mercaptosilane. In other words, an additional silane selected from the group consisting of blocked mercaptosilanes and alkoxysilanes may be used in combination with the mercaptosilane. In other embodiments, the at least one silane comprises a mercaptosilane. In other words, the only type of silane used is a mercaptosilane, and blocked mercaptosilanes and alkoxysilanes are not present in the rubber composition. The mercaptosilane compound may be represented by the general formula HS-R 3 -Si(X n )(R 4 3-n wherein each X is independently selected from a halogen or an alkoxy group, which in the case of an alkoxy group has the formula OR 5 (In the formula, R 5 is a C1 to C6 aliphatic, alicyclic, or aromatic group); R 3 is selected from C1 to C4 alkylene; each R 4 are independent, C1~C 30 Alkyl, C7-C 30 Alkaryl, C5~C 30 Alicyclic or C6~C20 aromatic; n is an integer from 1 to 4. When X is a halogen, it may be selected from the group consisting of chlorine, bromine, iodine and fluorine, and preferably chlorine. In certain preferred embodiments of the first and second embodiments disclosed herein, at least one silane is a mercaptosilane having the formula above, where R 3 is selected from C1-C3 alkylene, X is an alkoxy group (having a carbon portion of C1-C6), and n is 3. 1-mercaptomethyltriethoxysilane, 2-mercaptoethyltriethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldiethoxysilane, 2-mercaptoethyltriproxysilane, 18-mercaptooctadecyldiethoxychlorosilane
[0055] In certain embodiments of the first and second embodiments disclosed herein, the at least one silane is a blocked mercaptosilane. In certain such embodiments, the at least one silane comprises a blocked mercaptosilane. In other words, an additional silane selected from the group consisting of mercaptosilanes and alkoxysilanes can be used in combination with the blocked mercaptosilane. In other embodiments, the at least one silane consists of a blocked mercaptosilane. In other words, the only type of silane used is the blocked mercaptosilane, and mercaptosilanes and alkoxysilanes are not present in the rubber composition. The blocked mercaptosilane can be represented by the general formula BSR 6 -Si-X3, with a blocking group B replacing the mercapto hydrogen atom to "block" the sulfur atom from reacting with the polymer. In certain embodiments of the first and second embodiments, when the blocked mercaptosilane has the above general formula, B is a blocking group which may be in the form of an unsaturated heteroatom or carbon bonded directly to the sulfur through a single bond; R 6is selected from a C1-C6 straight or branched alkyl chain, and each X is independently selected from the group consisting of C1-C6 alkyl, C1-C6 alkoxy, halogen, halogen-containing C1-C6 alkyl, and halogen-containing C1-C6 alkoxy. Blocked mercaptosilanes suitable for use in certain embodiments of the first and second embodiments disclosed herein include, but are not limited to, those described in U.S. Patent Nos. 6,127,468, 6,204,339, 6,528,673, 6,635,700, 6,649,684, 6,683,135, and 7,256,231. In certain embodiments of the first and second embodiments disclosed herein, when at least one silane is a blocked mercaptosilane, it is selected from the group consisting of 2-triethoxysilyl-1-ethylthioacetate, 2-trimethoxysilyl-1-ethylthioacetate, 2-(methyldimethoxy-silyl)-1-ethylthioacetate, 3-trimethoxysilyl-1-propylthioacetate, triethoxysilylmethyl-thioacetate, trimethoxysilylmethylthioacetate, triisopropoxysilylmethylthioacetate, methyldiethoxysilylmethylthioacetate, methyldimethoxysilylmethylthioacetate, methyldiisopropoxysilylmethylthioacetate, dimethylethoxysilylmethylthioacetate, dimethylmethoxysilylmethylthioacetate, dimethylethoxysilylmethylthioacetate, dimethylmethoxysilylmethylthioacetate, methyldiisopropoxy ... , dimethylisopropoxysilylmethylthioacetate, 2-triisopropoxysilyl-1-ethylthioacetate, 2-(methyldiethoxysilyl)-1-ethylthioacetate, 2-(methyldiisopropoxysilyl)-1-ethylthioacetate, 2-(dimethylethoxysilyl-1-ethylthioacetate, 2-(dimethylmethoxysilyl)-1-ethylthioacetate, 2-(dimethylisopropoxysilyl)-1-ethylthioacetate, 3-triethoxysilyl-1-propylthioacetate, 3-triisopropoxysilyl-1-propylthioacetate, 3-methyldiethoxysilyl-1-propylthioacetate, 3-methyldimethoxysilyl-1-propylthioacetate, 3-methyldiisopropoxysilyl-1-propylthioacetate,1-(2-triethoxysilyl-1-ethyl)-4-thioacetylcyclohexane, 1-(2-triethoxysilyl-1-ethyl)-3-thioacetylcyclohexane, 2-triethoxysilyl-5-thioacetylnorbornene, 2-triethoxysilyl-4-thioacetylnorbornene, 2-(2-triethoxysilyl-1-ethyl)-5-thioacetylnorbornene, 2-(2-triethoxy-silyl-1-ethyl)-4-thioacetylnorbornene, 1-(1-oxo-2-thia-5-triethoxysilylphenyl)benzoic acid, 6-triethoxysilyl silyl-1-hexylthioacetate, 1-triethoxysilyl-5-hexylthioacetate, 8-triethoxysilyl-1-octylthioacetate, 1-triethoxysilyl-7-octylthioacetate, 6-triethoxysilyl-1-hexylthioacetate, 1-triethoxysilyl-5-octylthioacetate, 8-trimethoxysilyl-1-octylthioacetate, 1-trimethoxysilyl-7-octylthioacetate, 10-triethoxysilyl-1-decylthioacetate, 1-triethoxysilyl-9-decylthioacetate, 1-triethoxysilyl-2-butylthioacetate, 1-triethoxysilyl-3-butylthioacetate, 1-triethoxysilyl-3-methyl-2-butylthioacetate, 1-triethoxysilyl-3-methyl-3-butylthioacetate, 3-trimethoxysilyl-1-propylthiooctanoate, 3-triethoxysilyl-1-propyl-1-propylthiopalmitate, 3-triethoxysilyl-1-propylthiooctanoate, 3-triethoxysilyl-1-propylthiobenzoate, 3-triethoxysilyl-1-propylthio -2-ethylhexanoate, 3-methyldiacetoxysilyl-1-propyl thioacetate, 3-triacetoxysilyl-1-propyl thioacetate, 2-methyldiacetoxysilyl-1-ethyl thioacetate, 2-triacetoxysilyl-1-ethyl thioacetate, 1-methyldiacetoxysilyl-1-ethyl thioacetate, 1-triacetoxysilyl-1-ethyl thioacetate, tris-(3-triethoxysilyl-1-propyl)trithiophosphate, bis-(3-triethoxysilyl-1-propyl)methyldithiophosphonate,Bis-(3-triethoxysilyl-1-propyl)ethyl dithiophosphonate, 3-triethoxysilyl-1-propyl dimethylthiophosphinate, 3-triethoxysilyl-1-propyl diethylthiophosphinate, tris-(3-triethoxysilyl-1-propyl)tetrathiophosphate, bis-(3-triethoxysilyl-1-propyl)methyl trithiophosphonate, bis-(3-triethoxysilyl-1-propyl)ethyl trithiophosphonate, 3-triethoxysilyl-1-propyl dimethylthiophosphinate, tris-(3-triethoxysilyl-1-propyl)tetrathiophosphate, bis-(3-triethoxysilyl-1-propyl)methyl trithiophosphonate, bis-(3-triethoxysilyl-1-propyl)ethyl trithiophosphonate, 3-Triethoxysilyl-1-propyl diethyl dithiophosphinate, tris-(3-methyldimethoxysilyl-1-propyl) trithiophosphate, bis-(3-methyldimethoxysilyl-1-propyl) methyl dithiophosphonate, bis-(3-methyldimethoxysilyl-1-propyl)-ethyl dithiophosphonate, 3-methyldimethoxysilyl-1-propyl dimethyl thiophosphinate, 3-methyldi Methoxysilyl-1-propyl diethyl thiophosphinate, 3-triethoxysilyl-1-propyl methyl thiosulfate, 3-triethoxysilyl-1-propyl methane thiosulfonate, 3-triethoxysilyl-1-propyl ethane thiosulfonate, 3-triethoxysilyl-1-propyl benzene thiosulfonate, 3-triethoxysilyl-1-propyl toluene thiosulfonate, 3-triethoxysilyl-1-propyl naphthalene thiosulfonate, 3- The group consisting of triethoxysilyl-1-propylxylenethiosulfonate, triethoxysilylmethylmethylthiosulfate, triethoxysilylmethylmethanethiosulfonate, triethoxysilylmethylethanethiosulfonate, triethoxysilylmethylbenzenethiosulfonate, triethoxysilylmethyltoluenethiosulfonate, triethoxysilylmethylnaphthalenethiosulfonate, triethoxysilylmethylxylenethiosulfonate, etc.
[0056] In certain embodiments of the method of the first embodiment, the at least one silane is premixed with the guayule rubber prior to any mixing of the guayule rubber with the filler component. In certain such embodiments, the guayule rubber is dissolved in a solvent or is present in latex form when premixed with the at least one silane. In other embodiments, the guayule rubber is present in solid form when premixed with the at least one silane. Without wishing to be bound by theory, it is believed that premixing the guayule rubber may aid in the bonding of the silane to the bagasse particles within the guayule rubber.
[0057] resin In certain embodiments of the first and second embodiments disclosed herein, the amount of guayule resin present in the rubber composition is limited. In general, the guayule resin may be added to the rubber composition as a component of the guayule rubber used, but it is also possible to add the guayule resin separately (as a "free" resin). In a preferred embodiment of the first and second embodiments, the rubber composition comprises 4 phr or less of guayule resin, e.g., 4, 3.5, 3, 2.5, 2, 1.5, 1, 0.5 phr or less, more preferably less than 4 phr of guayule resin (e.g., 3.9, 3.5, 3, 2.5, 2, 1.5, 1, 0.5 phr or less), even more preferably less than 1 phr of guayule resin (e.g., 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1, or 0 phr or less).
[0058] Although the amount of guayule resin present in the rubber compositions of the first and second embodiments is preferably limited, in certain embodiments, other hydrocarbon (non-guayule) resins may be utilized in the rubber compositions. When non-guayule hydrocarbon resins are used in the rubber compositions of the first and second embodiments disclosed herein, the type and amount of resin used may vary.
[0059] In the first and second embodiments in which a non-guayule hydrocarbon resin is used, the amount present in the rubber composition is generally between 5 and 50 phr (e.g., 5, 10, 15, 20, 25, 30, 35, 40, 45, or 50 phr). Various types of non-guayule hydrocarbon resins, including plasticizing resins, can be utilized. As used herein, the term plasticizing resin refers to a compound that is solid at room temperature (23° C.) and is miscible in the rubber composition in the amount used, typically at least 5 phr. Generally, plasticizing resins act as diluents, which can be contrasted with tackifying resins, which are generally immiscible, and can migrate to the surface of the rubber composition to provide tack. In certain embodiments of the first and second embodiments, when a non-guayule hydrocarbon resin (in the form of a plasticizing resin) is utilized, it is selected from aliphatic, aromatic, or aliphatic / aromatic types, depending on the monomers contained therein. Examples of plasticizing resins (non-guayule hydrocarbon resins) suitable for use in the rubber compositions of the first and second embodiments include, but are not limited to, cyclopentadiene (abbreviated as CPD) or dicyclopentadiene (abbreviated as DCPD) homopolymer or copolymer resins, terpene homopolymer or copolymer resins, and C5 fraction homopolymer or copolymer resins. Such resins can be used, for example, individually or in combination. In a particular embodiment of the first and second embodiments, a plasticizing resin (non-guayule hydrocarbon resin) is used that satisfies at least one of the following: Tg above 30°C (preferably above 40°C and / or 120°C or less or 100°C or less), number average molecular weight (Mn) of 400 to 2000 grams / mol (preferably 500 to 2000 grams / mol), and polydispersity index (PI) of less than 3 (preferably less than 2) (PI=Mvv / Mn, where Mvv is the weight average molecular weight of the resin). The Tg of a resin can be measured by DSC (differential scanning calorimetry) in accordance with ASTM D3418 (1999).The Mw, Mn, and PI of the resins can be determined by size exclusion chromatography (SEC) using THF, 35° C., a concentration of 1 g / 1, a flow rate of 1 milliliter / min, the solution filtered through a filter with a porosity of 0.45 μm before injection, Moore calibration with polystyrene standards, a set of three “Waters” columns in series ("Styragel" HR4E, HR1, and HR0.5), and detection with a differential refractometer ("Waters 2410") and its associated operating software ("Waters Empower").
[0060] Other (optional) components of the rubber composition According to the first and second embodiments, additional components may be present in the rubber composition. These additional components include, but are not limited to, liquid plasticizers, curing packages, waxes (which may be antioxidants), processing aids, reinforcing resins, peptizers, and antioxidants / antidegradants. In a preferred embodiment of the first and second embodiments, a curing package is included in the rubber composition.
[0061] In certain embodiments of the first and second embodiments, the rubber composition comprises 1-30 phr of liquid plasticizer. The term liquid plasticizer should be understood to refer to plasticizers that are liquid at 25°C, including but not limited to oil and ester-based plasticizers. Generally, according to the first and second embodiments, when liquid plasticizers are used, one or more liquid plasticizers may be utilized. The total amount of liquid plasticizer may be considered as the amount of plasticizer component. In certain embodiments of the first and second embodiments, the rubber composition comprises a liquid plasticizer in an amount within the aforementioned ranges, such as 1-30 phr (e.g., 1, 2, 4, 6, 8, 10, 12, 14, 15, 16, 18, 20, 22, 24, 25, 26, 28, or 30 phr), or 1-20 phr or 5-20 phr, preferably 10-30 phr (e.g., 10, 12, 14, 15, 16, 18, 20, 22, 24, 25, 26, 28, or 30 phr), or 10-25 phr or 10-20 phr, etc. The term "oil" is meant to include both free oil (usually added during the compounding process) and extending oil (used to extend the rubber). As a non-limiting example, by stating that a rubber composition comprises 20 phr of oil, it should be understood that the total amount of any free oil and any extending oil is 20 phr. Similarly, by stating that a rubber composition comprises 20 phr of liquid plasticizer, it should be understood that the total amount of any liquid plasticizer (including free oil, extending oil, and ester plasticizer) is 20 phr. In certain embodiments of the first and second embodiments, when the rubber composition contains oil, the only oil is free oil in one of the amounts previously mentioned (e.g., 1-30 phr, 10-30 phr, 5-20 phr, etc.). In other embodiments of the first and second embodiments, when the rubber composition contains oil, the only oil is extending oil in one of the amounts previously mentioned (e.g., 1-30 phr, 10-30 phr, 5-20 phr, etc.). In those embodiments in the first and second embodiments in which oil-extended rubber is used, the amount of oil used in the preparation of the oil-extended rubber may vary.In certain such embodiments, the amount of extending oil present in the oil-extended rubber (polymer) is 10 to 50 parts of oil per 100 parts of rubber (e.g., 10, 15, 20, 25, 30, 35, 40, 45, or 50 parts of oil per 100 parts of rubber), preferably 10 to 40 parts of oil per 100 parts of rubber or 20 to 40 parts of oil per 100 parts of rubber. When oil-extended rubber is used in the rubber component of the rubber composition disclosed herein, as described above, the amount specified for the rubber of the rubber component should be understood to refer only to the amount of rubber, not the amount of oil-extended rubber. As a non-limiting example, extending oil can be used in an amount of 40 parts of oil per 100 parts of rubber for SBR used in an amount of 15 parts in the overall rubber composition, and therefore the amount of oil contributed by the oil-extended SBR to the rubber composition can be described as 6 phr.
[0062] As used herein, oil refers to both petroleum-based oils (e.g., aromatic oils, naphthenic oils, and low PCA oils) and vegetable oils (such as those that may be obtained from vegetables, nuts, and seeds). Vegetable oils generally include triglycerides, and this term should be understood to include synthetic triglycerides and those that are actually sourced from plants.
[0063] According to the first and second embodiments, when one or more oils are present in the rubber composition, various types of processing oils and extending oils can be utilized, including but not limited to aromatic oils, naphthenic oils, and low PCA oils (petroleum-derived or vegetable-derived). Suitable low PCA oils include those having a polycyclic aromatic content of less than 3 wt.% as measured by IP346 method. The procedure of IP346 method can be found in Standard Methods for Analysis & Testing of Petroleum and Related Products and British Standard 2000 Parts, 2003, 62nd Edition, published by the Institute of Petroleum (UK). Exemplary petroleum-derived low PCA oils include mild extraction solvate (MES), treated distillate aromatic extract (TDAE), TRAE, and heavy naphthenic. Exemplary MES oils are commercially available as CATENEX SNR (from SHELL), PROREX 15 and FLEXON 683 (from EXXONMOBIL), VIVATEC 200 (from BP), PLAXOLENE MS (from TOTAL FINA ELF), TUDALEN 4160 / 4225 (from DAHLEKE), MES-H (from REPSOL), MES (from Z8), and OLIO MES S201 (from AGIP). Exemplary TDAE oils are available as TYREX 20 (from EXXONMOBIL), VIVATEC 500, VIVATEC 180, and ENERTHENE 1849 (from BP), and EXTENSOIL 1996 (from REPSOL). Exemplary heavy naphthenic oils are available as SHELLFLEX 794, ERGON BLACK OIL, ERGON H2000, CROSS C2000, CROSS C2400, and SAN JOAQUIN 2000 L. Exemplary low PCA oils also include various plant-derived oils, such as those that can be obtained from vegetables, nuts, and seeds.Non-limiting examples include soybean oil, sunflower oil (including high oleic sunflower oil), safflower oil, corn oil, linseed oil, cottonseed oil, rapeseed oil, cashew oil, sesame oil, camellia oil, jojoba oil, hemp oil, macadamia nut oil, coconut oil, and palm oil. The above-mentioned processed oils can also be used as extending oils, i.e., for the preparation of oil-extended polymers or copolymers, or as processed oils or free oils.
[0064] In those embodiments in the first and second embodiments in which one or more oils are present in the rubber composition, the Tg of the one or more oils used may vary. In certain embodiments of the first and second embodiments, any oil utilized may have a Tg of about -40 to about -100°C, -40 to -100°C (e.g., -40, -45, -50, -55, -60, -65, -70, -75, -80, -85, -90, -95, or -100°C), about -40 to about -90°C, -40 to -90°C (e.g., -40, -45, -50, -55, -60, The polymer has a Tg of about -65, -70, -75, -80, -85, or -90°C), about -45 to about -85°C, -45 to -85°C (e.g., -45, -50, -55, -60, -65, -70, -75, -80, or -85°C), about -50 to about -80°C, or -50 to -80°C (e.g., -50, -55, -60, -65, -70, -75, or -80°C).
[0065] In certain embodiments of the first and second embodiments, the rubber composition contains less than 5 phr (e.g., 4.5, 4, 3, 2, 1, or 0 phr) of MES or TDAE oil, and preferably contains neither MES oil nor TDAE oil (i.e., 0 phr). In certain embodiments of the first and second embodiments, the rubber composition does not contain petroleum-based oil (i.e., 0 phr), and instead, any oil utilized is a vegetable oil. In certain embodiments of the first and second embodiments, the rubber composition contains soybean oil in one of the amounts described above, and in certain such embodiments, the only oil included is soybean oil. In certain embodiments of the first and second embodiments, the rubber composition does not contain sunflower oil (i.e., 0 phr). In other embodiments of the first and second embodiments, the only oil included is sunflower oil.
[0066] In certain embodiments of the first and second embodiments, the rubber composition includes one or more ester plasticizers, which are generally a class of plasticizers that are liquid at room temperature. Suitable ester plasticizers are known to those skilled in the art and include, but are not limited to, phosphate esters, phthalate esters, adipate esters, and oleate esters (i.e., derived from oleic acid). Considering that esters are chemical compounds derived from acids in which at least one -OH is replaced with an -O-alkyl group, they generally range from C1 to C6. 20 (For example, C1, C2, C3, C4, C5, C6, C7, C8, C9, C 10 , C 11 , C 12 , C 13 , C 14 , C 15 , C 16 , C 17 , C 18 , C 19 , C 20 ) or C6~C 12A variety of alkyl groups, including linear or branched alkyl groups of the formula (I) may be used in ester plasticizers suitable for use in tread rubber compositions. Certain of the aforementioned esters are based on acids having more than one -OH group and therefore may accommodate one or more O-alkyl groups (e.g., trialkyl phosphates, dialkyl phthalates, dialkyl adipates). Non-limiting examples of suitable ester plasticizers include trioctyl phosphate, dioctyl phthalate, dioctyl adipate, nonyl oleate, octyl oleate, and combinations thereof. The use of ester plasticizers, such as one or more of the foregoing, may be beneficial to the snow or ice performance of tires made from tread rubber compositions containing such ester plasticizers, due at least in part to the relatively low Tg of the ester plasticizers. In certain embodiments of the first and second embodiments, the tread rubber composition comprises one or more ester plasticizers having a Tg of −40° C. to −70° C. (e.g., −40, −45, −50, −55, −60, −65, or −70° C.) or −50° C. to −65° C. (e.g., −50, −51, −52, −53, −54, −55, −56, −57, −58, −59, −60, −61, −62, −63, −64, or −65° C.). In those embodiments in the first and second embodiments where one or more ester plasticizers are utilized, the amount utilized may vary. In certain embodiments of the first and second embodiments, the one or more ester plasticizers are present in an amount of 1 to 25 phr (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, or 25 phr), 1 to 20 phr (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, or 25 phr),
[0046] In some embodiments, the total amount of ethanol may be from 1 to 20 phr (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 phr), from 1 to 10 phr (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 phr), from 2 to 6 phr (e.g., 2, 3, 4, 5, or 6 phr), or from 2 to 5 phr (e.g., 2, 3, 4, or 5 phr).In certain preferred embodiments of the first and second embodiments, the amount of ester plasticizer is 15 phr or less, or 12 phr or less. In certain embodiments of the first and second embodiments, one or more ester plasticizers are used in combination with oil (in one of the amounts mentioned above) when the oil is present in an amount of 1 to less than 10 phr, or 1 to 5 phr. In other embodiments of the first and second embodiments, one or more ester plasticizers are used in the complete absence of oil in the tread rubber composition (i.e., 0 phr of oil).
[0067] As mentioned above, in certain embodiments of the first and second embodiments disclosed herein, the rubber composition comprises (constitutes) a curing package. The contents of the curing package may vary, but generally, the curing package comprises at least one of a vulcanizing agent, a vulcanization accelerator, a vulcanization activator (e.g., zinc oxide, stearic acid, etc.), a vulcanization inhibitor, and a scorch inhibitor. In certain embodiments of the first and second embodiments, the curing package comprises at least one vulcanizing agent, at least one vulcanization accelerator, at least one vulcanization activator, and optionally a vulcanization inhibitor and / or a scorch inhibitor. The vulcanization accelerator and the vulcanization activator act as catalysts for the vulcanizing agent. Various vulcanization inhibitors and scorch inhibitors are known in the art and can be selected by those skilled in the art based on the desired vulcanization properties.
[0068] Examples of types of vulcanizing agents suitable for use in certain embodiments of the first and second embodiments include, but are not limited to, sulfur or peroxide-based curing components. Thus, in certain such embodiments, the curing package includes a sulfur-based curing agent or a peroxide-based curing agent. In preferred embodiments of the first and second embodiments, the vulcanizing agent is a sulfur-based curing agent, and in certain such embodiments, the vulcanizing agent consists (only) of a sulfur-based curing agent. Examples of certain suitable sulfur vulcanizing agents include "rubbermaker's" soluble sulfur, sulfur donor curing agents such as amine disulfide, polymeric polysulfide, or sulfur olefin adducts, and insoluble polymeric sulfur. Preferably, the sulfur vulcanizing agent is soluble sulfur or a mixture of soluble and insoluble sulfur polymers. For a general disclosure of suitable curing agents and other components (e.g., vulcanization inhibitors and scorch inhibitors) used in curing, see Kirk-Othmer, Encyclopedia of Chemical Technology, 3rd ed., Wiley Interscience, NY 1982, Vol. 20, pp. 365-468, especially Vulcanization Agents and Auxiliary Materials, pp. 390-402, or Vulcanization by AY Coran (Encyclopedia of Polymer Science and Engineering, Second Edition (1989 John Wiley & Sons, Inc.)), both of which are incorporated herein by reference. The vulcanizing agents may be used alone or in combination. Generally, in certain embodiments of the first and second embodiments, the vulcanizing agent may be used in an amount ranging from 0.1 to 10 phr (e.g., 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 phr), such as 1 to 7.5 phr, such as 1 to 5 phr, preferably 1 to 3.5 phr (e.g., 1, 1.5, 2, 2.5, 3, or 3.5 phr).
[0069] Vulcanization accelerators are used to control the time and / or temperature required for vulcanization and improve the properties of the vulcanizate. Examples of vulcanization accelerators suitable for use in certain embodiments of the first and second embodiments disclosed herein include, but are not limited to, thiazole vulcanization accelerators, such as 2-mercaptobenzothiazole, 2,2'-dithiobis(benzothiazole) (MBTS), N-cyclohexyl-2-benzothiazole-sulfenamide (CBS), N-tert-butyl-2-benzothiazole-sulfenamide (TBBS), guanidine vulcanization accelerators, such as diphenyl guanidine (DPG), thiuram vulcanization accelerators, carbamic acid vulcanization accelerators, and the like. Generally, the amount of vulcanization accelerator used ranges from 0.1 to 10 phr (e.g., 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 phr), preferably from 0.5 to 5 phr (e.g., 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, or 5 phr).Preferably, the optional vulcanization accelerator used in the rubber composition in the first and second embodiments excludes any thiuram, such as thiuram monosulfide and thiuram polysulfide (examples of which include TMTM (tetramethyl thiuram monosulfide), TMTD (tetramethyl thiuram disulfide), DPTT (dipentamethylene thiuram tetrasulfide), TETD (tetraethyl thiuram disulfide), TiBTD (tetraisobutyl thiuram disulfide), and TBzTD (tetrabenzyl thiuram disulfide)). In other words, the rubber composition in the first and second embodiments preferably does not contain a thiuram accelerator (i.e., 0 phr).
[0070] Vulcanization activators are additives used to aid in vulcanization. Generally, vulcanization activators include both inorganic and organic components. Zinc oxide is the most widely used inorganic vulcanization activator. A variety of organic vulcanization activators are commonly used, including stearic acid, palmitic acid, lauric acid, and zinc salts of each of the foregoing. Generally, in certain embodiments of the first and second embodiments, the amount of vulcanization activator used ranges from 0.1 to 6 phr (e.g., 0.1, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, or 6 phr), preferably 0.5 to 4 phr (e.g., 0.5, 1, 1.5, 2, 2.5, 3, 3.5, or 4 phr). In certain embodiments of the first and second embodiments, both zinc oxide and stearic acid are used as vulcanization activators, and the total amount utilized falls within one of the ranges described above. In certain such embodiments, the only vulcanization activators used are zinc oxide and stearic acid. In certain embodiments of the first and second embodiments, one or more vulcanization activators are used, including one or more thiourea compounds (used in the amounts described above), optionally in combination with one or more of the vulcanization activators described above. In general, the thiourea compounds have the structure (R 1 )(R 2 )NS(=C)N(R 3 )(R 4 ) in which R 1 , R 2 , R 3 , and R 4 Each of is independently selected from H, alkyl, aryl, and N-containing substituents (e.g., guanyl). Optionally, two of the foregoing structures can be linked together through N (removing one of the R groups) in a dithiobiurea compound. In certain embodiments, R 1 or R 2 One of the two, and R 3 or R 4 can be linked together with one or more methylene groups (-CH-) between them. In certain embodiments of the first and second embodiments, the thiourea has R selected from one of the aforementioned groups.1 , R 2 , R 3 , and R 4 and the remaining R group is hydrogen. Exemplary alkyls include C1-C6 straight chain, branched, or cyclic groups such as methyl, ethyl, propyl, iso-propyl, butyl, iso-butyl, pentyl, hexyl, and cyclohexyl. Exemplary aryls include C6-C12 aromatic groups such as phenyl, tolyl, and naphthyl. Exemplary thiourea compounds include, but are not limited to, dihydrocarbyl thioureas, such as dialkyl thioureas and diaryl thioureas. Non-limiting examples of specific thiourea compounds include one or more of thiourea, N,N'-diphenylthiourea, trimethylthiourea, N,N'-diethylthiourea (DEU), N,N'-dimethylthiourea, N,N'-dibutylthiourea, ethylenethiourea, N,N'-diisopropylthiourea, N,N'-dicyclohexylthiourea, 1,3-di(o-tolyl)thiourea, 1,3-di(p-tolyl)thiourea, 1,1-diphenyl-2-thiourea, 2,5-dithiobiurea, guanylthiourea, 1-(1-naphthyl)-2-thiourea, 1-phenyl-2-thiourea, p-tolylthiourea, and o-tolylthiourea. In certain embodiments of the first and second embodiments, the activator comprises at least one thiourea compound selected from thiourea, N,N'-diethylthiourea, trimethylthiourea, N,N'-diphenylthiourea, and N-N'-dimethylthiourea.
[0071] Vulcanization inhibitors are used to control the vulcanization process, generally to slow or inhibit vulcanization until a desired time and / or temperature is reached. Common vulcanization inhibitors include, but are not limited to, PVI (cyclohexylthiophthalmide) from Santogard. Generally, in certain embodiments of the first and second embodiments, the amount of vulcanization inhibitor is 0.1-3 phr (e.g., 0.1, 0.5, 1, 1.5, 2, 2.5, or 3 phr), preferably 0.5-2 phr (e.g., 0.5, 1, 1.5, or 2 phr).
[0072] Various other components that may be optionally added to the rubber compositions of the first and second embodiments disclosed herein include waxes (which may be antioxidants), processing aids, reinforcing resins, mastication accelerators, and antioxidants / antidegradants. The antioxidant components may be classified as antiozonants or antioxidants, such as those selected from N,N'-disubstituted-p-phenylenediamines, such as N-1,3-dimethylbutyl-N'phenyl-p-phenylenediamine (6PPD), N,N'-bis(1,4-dimethylpentyl)-p-phenylenediamine (77PD), N-phenyl-N-isopropyl-p-phenylenediamine (IPPD), and N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (HPPD). Other examples of antidegradants include acetone diphenylamine condensation products, 2,4-trimethyl-1,2-dihydroquinoline, octylated diphenylamine, 2,6-di-t-butyl-4-methylphenol, and certain waxes. In certain other embodiments of the first and second embodiments, the composition may be free or essentially free of antidegradants, such as antioxidants or antiozonants.
[0073] How to improve rolling resistance As mentioned above, the first embodiment disclosed herein is directed to a method for improving the rolling resistance of a rubber composition. The improvement in rolling resistance is compared to a control rubber composition containing the same ingredients except that it does not contain any silica and silane. It should be understood that the tire rubber composition according to the second embodiment disclosed herein also shows an improvement in rolling resistance (when compared to a control rubber composition containing the same ingredients except that it does not contain any silica and silane).
[0074] According to the first and second embodiments disclosed herein, the amount of improvement in rolling resistance achieved by using at least one silane in combination with bagasse-containing guayule rubber can vary. The improvement in rolling resistance can be measured by a variety of methods, including but not limited to those provided in the examples. In certain embodiments of the first and second embodiments, the improvement in rolling resistance is at least 3% (e.g., 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 25%, or more) or from 3 to 20% (e.g., 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%) when compared to a control rubber composition containing the same ingredients except that it does not contain any silica or silane. In preferred embodiments of the first and second embodiments, the improvement in rolling resistance is at least 5% (e.g., 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 25%, or more) or from 5 to 20% (e.g., 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%) when compared to a control rubber composition containing the same ingredients except that it does not contain any silica and silane. %), more preferably at least 10% (e.g., 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 25% or more) or 10-20% (e.g., 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%), or even at least 15% (e.g., 15%, 16%, 17%, 18%, 19%, 20%, 25% or more) or 15-20% (e.g., 15%, 16%, 17%, 18%, 19%, or 20%).
[0075] In certain embodiments of the first and second embodiments, the improvement in rolling resistance is combined with an improvement in M300. According to such embodiments, the amount of improvement in M300 can vary. In certain embodiments of the first and second embodiments, the improvement in M300 is at least 3% (e.g., 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, or more) or 3 to 10% (e.g., 3%, 4%, 5%, 6%, 7%, 8%, 9%, or 10%) when compared to a control rubber composition containing the same ingredients except that it does not contain any silica and silane. In preferred embodiments of the first and second embodiments, the improvement in M300 is at least 5% (e.g., 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, or more) or 5-10% (e.g., 5%, 6%, 7%, 8%, 9%, or 10%) when compared to a control rubber composition containing the same ingredients except that it does not contain any silica or silane.
[0076] tire The rubber composition according to the first embodiment (or the rubber composition made according to the method of the first embodiment) can be used to prepare a tire having at least one component made of the rubber composition, the component being selected from a tire tread, a tire sidewall, a tire belt skim, or a tire carcass. In a preferred embodiment, the component is a tire tread. Also disclosed herein is a heavy-duty or commercial truck or bus tire having a tread made from the rubber composition according to the first embodiment (or the rubber composition made according to the method of the first embodiment). EXAMPLES
[0077] The following examples are illustrative of certain exemplary embodiments and / or features of the embodiments of the present disclosure. The examples are provided for illustrative purposes only and should not be construed as limiting the present disclosure. Many variations to these specific examples are possible without departing from the spirit and scope of the embodiments of the present disclosure. It is specifically understood that the rubber compositions can be prepared using different amounts of guayule rubber (containing different amounts of bagasse, as described above), using different amounts or types of silanes, as described above, or using different amounts or types of fillers, as described above. It should also be understood that the bagasse component and guayule rubber containing silanes can be utilized in rubber compositions with components (e.g., additional rubbers, fillers, curing package components) that are different in relative amounts, compositions, or both from those used in the examples (i.e., completely different, as disclosed in the previous paragraph).
[0078] Examples 1-6: Rubber compositions were prepared using one of two types of guayule rubber (containing different amounts of bagasse). As shown in Table 1 below, some rubber compositions contained silica but no silane (Examples 1 and 4), others contained both silica and silane (Examples 3 and 5), and others contained silane but no silica (Examples 2 and 6). Examples 2 and 6 can be considered examples of the present invention, while the other examples are presented for comparison purposes. The overall rubber composition used was a tread rubber composition, and the relative amounts of rubber, carbon black filler, silica filler, silane, and resin are shown in Table 1 (amounts are provided in phr or amounts per 100 parts of rubber), while the other ingredients remained the same in all of Examples 1-6. In particular, the amount of guayule rubber-2 is listed as 110 parts or phr (indicating the presence of 100 parts rubber and 10 parts bagasse). [Table 1]
[0079] The ingredients for each example were mixed in a Brabender mixer using the procedure set forth below in Table 2. The resulting rubber compositions were cured at 145°C for 15 minutes.
[0080] For each of the rubber compositions of Examples 1-6, the properties listed in Table 3 were determined as follows: tan δ values were measured by strain sweep tests performed on an Advanced Rheometric Expansion System (ARES) manufactured by TA Instruments. The specimens had a cylindrical shape with a length of 14.4 mm and a diameter of 7.8 mm. The tests were performed using a frequency of 10 rad / s. The strain was swept from 0.1% to 16% and the temperature was increased to 60°C starting at 22°C and held at 60°C. The measurements at 60°C and 10% strain are listed in Table 3 for each rubber composition. The index tan δ at 60°C of a rubber composition is an index of its rolling resistance when incorporated into a tire tread. The tan δ values are presented as an index (calculated by comparing the value of a given example with that of a comparative control rubber composition) with a number greater than 100 being considered an improvement. At 60° C., lower tan δ values are considered improvements, so the index was calculated as (control / value)×100. Example 1 is used as a control for Examples 2 and 3, and Example 4 is used as a control for Examples 5 and 6.
[0081] The mechanical tensile properties of the samples were measured using dumbbell-shaped samples with a cross-sectional dimension of 4 mm in width and a center thickness of 1.9 mm according to standard procedures described in, but not limited to, ASTM D-412. The specimens were strained at a constant rate and the resulting force was recorded as a function of elongation (strain). The samples were cured at 150°C for 40 minutes and then analyzed for tensile properties at 25°C. The abbreviation M300 is used for the tensile stress measured at 300% elongation. The M300 value is presented as an index (calculated by comparing the value of a given example with that of a comparative control rubber composition), with a number greater than 100 considered an improvement. The index was calculated as (value / control) x 100, since a higher M300 value is considered an improvement. Example 1 is used as a control for Examples 2 and 3, and Example 4 is used as a control for Examples 5 and 6. [Table 2] [Table 3]
[0082] As can be seen from the data in Table 3, among Examples 1 to 3, Example 2 of the present invention (containing silane but not silica) has the best tan δ at 60° C., which indicates that the rubber composition will have the lowest (best) rolling resistance when used in a tire tread. Among Examples 4 to 6, Example 6 of the present invention (containing silane but not silica) has the best tan δ at 60° C., which indicates that the rubber composition will have the lowest (best) rolling resistance when used in a tire tread.
[0083] Examples 7-10: A rubber composition was prepared using 90 phr of a third type of guayule rubber (guayule rubber-3) in combination with 10 phr of high cis polybutadiene (having a cis 1,4-bond content of 96% and a Tg of -108°C). The ingredients are shown in Table 4 below. Examples 8 and 9 (containing silane but no silica) can be considered examples of the present invention, while the other examples are presented for comparative purposes. The overall rubber composition used was a tread rubber composition (albeit slightly different from the base tread rubber composition of Examples 1-6), with the relative amounts of rubber, carbon black filler, silica filler, silane, and resin shown in Table 4 (amounts are provided in phr or per hundred parts of rubber), and the other (not listed) ingredients remained the same in all of Examples 7-10. [Table 4]
[0084] The ingredients of each of Examples 7-10 were mixed in a Brabender mixer using the procedure set forth above in Table 2. The resulting rubber compositions were cured at 160° C. for 12 minutes.
[0085] For each of the rubber compositions of Examples 7-10, the properties listed in Table 5 were determined using the procedures described above for Examples 1-6. Example 7 is considered the control for each of Examples 8-10, and the index values are calculated as above. [Table 5]
[0086] As can be seen from the data in Table 5, among Examples 7-10, the one with the best tan δ at 60°C is Example 8 of the present invention, indicating that this rubber composition will have the lowest (best) rolling resistance when utilized in a tire tread. The tan δ at 60°C of Example 9 of the present invention is only slightly worse than Comparative Example 7, indicating that the rolling resistance is essentially the same for the two. Notably, Example 9 of the present invention has a significantly higher (i.e., improved) M300 when compared to Comparative Example 7, indicating that Example 9 of the present invention has better properties overall than Comparative Example 7.
[0087] Examples 11-13: Rubber compositions were prepared using 90 phr of guayule rubber-1 in combination with 10 phr of high cis polybutadiene. The ingredients are shown in Table 6 below. The silane used is the same as in Examples 1-10. Examples 11 and 12 (containing silane but no silica) can be considered examples of the present invention, the other examples are presented for comparison purposes. The overall rubber composition used was the tread rubber composition (the same base tread rubber composition from Examples 7-10), with the relative amounts of rubber, carbon black filler, silica filler, silane, and resin shown in Table 6 (amounts are provided in phr or per hundred parts of rubber), and the other (not listed) ingredients remained the same in all of Examples 11-13. [Table 6]
[0088] The ingredients of each of Examples 11-13 were mixed in a Brabender mixer using the same procedure set forth above in Table 2. The resulting rubber compositions were cured at 160° C. for 12 minutes.
[0089] For each of the rubber compositions of Examples 11-13, the properties listed in Table 7 were determined using the procedures described above for Examples 1-6. Example 13 is considered the control for Examples 11 and 12, and the index values are calculated as above. [Table 7]
[0090] As can be seen from the data in Table 7, among Examples 11 to 13, the Examples of the present invention (Examples 11 and 12) all have better tan δ at 60° C. than Comparative Example 13, which indicates that these rubber compositions exhibit lower (better) rolling resistance when used in tire treads. Also, all of the Examples of the present invention have better (higher) M300 compared to Comparative Example 13.
[0091] Examples 14-18: Rubber compositions were prepared using natural rubber instead of guayule rubber. Natural rubber (obtained from the Hevea tree) does not contain any bagasse. The ingredients are shown in Table 8 below. The silane used is the same as in Examples 1-13. None of these examples are considered to be the present invention. The overall rubber composition used was the tread rubber composition (same base tread rubber composition as Examples 7-13), with the relative amounts of rubber, carbon black filler, silica filler, silane, and resin shown in Table 8 (amounts are provided in phr or per hundred parts of rubber), and the other (not listed) ingredients remained the same in all of Examples 14-18. The resin used in Examples 15 and 18 was guayule resin (polar fraction). [Table 8]
[0092] The ingredients of each of the examples were mixed in a Brabender mixer using the same procedure set forth above in Table 2. The resulting rubber compositions were cured at 160° C. for 12 minutes.
[0093] For each of the rubber compositions of Examples 14-18, the properties listed in Table 9 were determined using the procedures described above for Examples 1-6. Example 14 is considered the control for each of Examples 15-18, and the index values are calculated as above. [Table 9]
[0094] As can be seen from the data in Table 9, the rubber composition with the best (lowest) tan δ at 60°C among Examples 14-18 is Example 14, which does not contain silica, silane, or resin. In other words, the rubber compositions of Examples 16 and 17, which contain silane in the absence of silica and resin, do not show a better tan δ at 60°C than Example 14. This data using natural rubber (instead of bagasse-containing guayule rubber) shows that there is no effect of using silane in the absence of silica (i.e., improvement in tan δ at 60°C), which supports the conclusion that a reaction occurs between the bagasse in the guayule rubber and the silane (in the absence of silica). Similarly, the rubber compositions of Examples 15 and 18, which contain silane in the absence of silica but also contain 2 phr of guayule resin, also do not show a better tan δ at 60°C than Example 14, which supports the conclusion that the improvement in rolling resistance is due to bagasse-silane interactions rather than guayule resin-silane interactions.
[0095] The present application discloses several numerical range limits that support any range within the disclosed numerical ranges, even if no explicit range limit is literally stated in the specification, since the compositions and methods disclosed herein can be practiced throughout the disclosed numerical ranges. With respect to the use of virtually any plural or singular term herein, one of ordinary skill in the art can substitute plural for singular or singular for plural as appropriate to the situation or application. Various singular or plural substitutions may be explicitly stated herein for the sake of brevity.
[0096] In general, those skilled in the art will understand that the terms used in this specification, and particularly in the appended claims, are generally intended to be "open" terms. For example, the term "including" should be interpreted as "including but not limited to," the term "having" should be interpreted as "having at least," and the term "including" should be interpreted as "including but not limited to." Furthermore, those skilled in the art will understand that if a specific number is intended in a prefaced claim recitation, such intent shall be expressly recited in the claim, and in the absence of such recitation, no such intent exists. For example, as an aid to understanding, the following appended claims may include the use of the preface phrases "at least one" and "one or more" to preface the claim recitation. However, the use of such phrases should not be construed as meaning that the preface of a claim recitation with the indefinite article "a" or "an" limits any particular claim that includes the claim recitation so prefaced to an invention that contains only one such recitation, even if the same claim includes the prefaced phrase "one or more" or "at least one" and an indefinite article such as "a" or "an" (e.g., "a" or "an" should typically be construed to mean "at least one" or "one or more"), and the same is true for the use of definite articles used to preface a claim recitation. In addition, even if a particular number is explicitly recited in a prefaced claim recitation, those skilled in the art will understand that such a recitation should typically be construed to mean at least the recited number (e.g., the explicit recitation "two recitations" without any other modifier typically means at least two recitations, or more than two recitations).Furthermore, when a conventional expression similar to "at least one of A, B, and C, etc." is used, such a configuration is generally intended in the sense that one of ordinary skill in the art would understand the conventional expression (e.g., "a system having at least one of A, B, and C" may include, but is not limited to, a system having only A, only B, only C, A and B together, A and C together, B and C together, and / or A, B, and C together, etc.). Furthermore, one of ordinary skill in the art will understand that virtually any disjunctive word or phrase indicating two or more alternative terms, whether in the specification, claims, or drawings, should be understood to contemplate the possibility of including one of those terms, either of those terms, or both of those terms. For example, the phrase "A or B" will be understood to include the possibilities of "A" or "B" or "A and B." All references, including but not limited to patents, patent applications, and non-patent literature, are incorporated herein by reference in their entirety. While various aspects and embodiments of the compositions and methods have been disclosed herein, other aspects and embodiments will be apparent to those of ordinary skill in the art. The various aspects and embodiments disclosed herein are for illustrative purposes only and are not intended to limit the true scope and spirit of the invention, as set forth in the appended claims.
Claims
1. A tire rubber composition for use in a tire tread, comprising: a. 100 parts of a rubber component comprising a majority by weight of guayule rubber, which comprises a bagasse component; b. a silica-free filler component; c. at least one silane selected from the group consisting of mercaptosilane, blocked mercaptosilane, and alkoxysilane; A tire rubber composition comprising:
2. 2. The tire rubber composition of claim 1, wherein the bagasse component of the guayule rubber is present in an amount of 1 to 20 weight percent based on the weight of the guayule rubber.
3. 3. The tire rubber composition of claim 1 or claim 2, comprising less than 4 phr of guayule resin.
4. A tire having a tire tread comprising the tire rubber composition according to any one of claims 1 to 3.
5. A method for improving the rolling resistance of a tire rubber composition, comprising providing a tire rubber composition according to any one of claims 1 to 3.
Citation Information
Patent Citations
Preparation method for bagasse nano-crystalline cellulose and rubber composite material of bagasse nano-crystalline cellulose
CN105419002A
Fine cellulose fiber composite, and method for producing the same
JP2015044948A
Fiber material and method for producing fiber material, and composite material and method for producing composite material
JP2018111768A
Natural rubber compound containing silica and its use in tires
JP2018502980A
Natural rubber compounds with silica and use with tires
US20180265601A1