Crankshaft and manufacturing method thereof

The crankshaft design with a ferrite/pearlite parallel portion and martensite fillet portion, combined with localized high-frequency heating, addresses heat treatment deformation and maintains structural integrity and fatigue strength.

JP7568903B2Active Publication Date: 2024-10-17NIPPON STEEL CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020162440
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-28
Publication Date
2024-10-17
Estimated Expiration
2040-09-28

AI Technical Summary

Technical Problem

Crankshafts subjected to induction hardening suffer from heat treatment deformation (hardening bending) due to induction hardening.

Method used

A crankshaft design with a parallel portion having a constant outer diameter and a fillet portion, where the parallel portion is composed mainly of ferrite and pearlite, and the fillet portion is composed mainly of martensite, with specific volume percentages and hardness ranges, combined with a manufacturing method that heats only the vicinity of the fillet portion using high-frequency induction heating.

Benefits of technology

The design and manufacturing method suppress thermal bending while ensuring fatigue strength, reducing bending and maintaining structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568903000002
    Figure 0007568903000002
  • Figure 0007568903000003
    Figure 0007568903000003
  • Figure 0007568903000004
    Figure 0007568903000004
Patent Text Reader

Abstract

To provide a crank shaft where glow deflection is suppressed.SOLUTION: A crank shaft 10 is provided with a journal part and a pin part 12. Each of the journal part and the pin part 12 has a parallel part 121 having a constant outer diameter and a fillet part 122 formed in continuation to the parallel part 121. In at least either the journal part or the pin part 12 is, in length L1 of at least 15.0% of length L of the parallel part 121, a tissue up to at least 6.0% depth d1 of radius R of the parallel part 121 from the surface contains 87.5 volume % or more ferrite / pearlite and a tissue up to at least 6.0% depth d2 of a radius R of the parallel part 121 from the surface of the fillet part 122 contains 87.5 volume % or more martensite.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a crankshaft and a method for manufacturing the same. [Background technology]

[0002] In some cases, crankshafts are induction hardened to improve their fatigue strength. In some cases, induction hardened crankshafts may have deformation due to heat treatment (hardening bending).

[0003] Japanese Patent No. 4007033 discloses a crankshaft in which the induction hardened layer depth of the pin and the induction hardened layer depth of the journal at each of the arm critical cross-sectional portions in one throw of the crankshaft satisfy a specified relationship.

[0004] Japanese Patent Application Laid-Open No. 2006-328497 discloses a high-frequency heating method for performing high-frequency heating when high-frequency hardening a steel plate member by arranging a conductive protective plate so as to cover a part of the steel plate member. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 4007033 [Patent Document 2] JP 2006-328497 A Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a crankshaft in which quench bending is suppressed, and a method for manufacturing the same. [Means for solving the problem]

[0007] A crankshaft according to one embodiment of the present invention is a crankshaft having a journal portion and a pin portion, each of the journal portion and the pin portion having a parallel portion having a constant outer diameter and a fillet portion formed continuously with the parallel portion, and at least one of the journal portion and the pin portion has a structure that contains 87.5% by volume or more of ferrite-pearlite from the surface to a depth of at least 6.0% of the radius of the parallel portion over a length of at least 15.0% of the length of the parallel portion, and the structure of the fillet portion from the surface to a depth of at least 6.0% of the radius of the parallel portion contains 87.5% by volume or more of martensite.

[0008] A method for manufacturing a crankshaft according to one embodiment of the present invention is the method for manufacturing the above-mentioned crankshaft, further comprising the step of quenching only the vicinity of the fillet portion from a temperature of the Ac3 point or higher by a high-frequency induction heating device. Effect of the Invention

[0009] According to the present invention, a crankshaft in which bending due to quenching is suppressed can be obtained. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic diagram of a crankshaft according to one embodiment of the present invention. [Diagram 2] FIG. 2 is an enlarged cross-sectional view showing the vicinity of a pin portion of the crankshaft in FIG. [Diagram 3] FIG. 3 is a flow chart showing an example of a method for manufacturing the crankshaft of FIG. [Figure 4] FIG. 4 is a perspective view of the three-dimensional analysis model used in the simulation. [Diagram 5] FIG. 5 is a front view of the three-dimensional analysis model of FIG. [Figure 6] FIG. 6 is an enlarged view of the vicinity of the pin top of the three-dimensional analysis model of FIG. [Figure 7] FIG. 7 is a cross-sectional view showing the arrangement of induction coils in the simulation. [Figure 8] FIG. 8 is a cross-sectional view showing another arrangement of induction coils in the simulation. [Figure 9A] FIG. 9A is a contour map showing the tissue distribution of No.1. [Figure 9B] FIG. 9B is a contour map showing the tissue distribution of No.3. [Figure 9C] FIG. 9C is a contour map showing the tissue distribution of No.5. [Figure 9D] FIG. 9D is a contour map showing the tissue distribution of No. 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. In the drawings, the same or corresponding parts are designated by the same reference numerals and their description will not be repeated. The dimensional ratios between the components shown in each drawing do not necessarily represent the actual dimensional ratios.

[0012] [Crankshaft] 1 is a schematic diagram of a crankshaft 10 according to an embodiment of the present invention. The crankshaft 10 includes a journal portion 11, a pin portion 12, and an arm portion 13.

[0013] The crankshaft 10 is made of, for example, a steel material for machine construction. The crankshaft 10 may be made of, but is not limited to, carbon steel material for machine construction of JIS G 4051:2009, steel material for machine construction (H steel) with guaranteed hardenability of JIS G 4052:2008, alloy steel material for machine construction of JIS G4053:2008, etc. Among these steel materials, S45C, S50C, and S53C of JIS G 4051:2009, SMn438 of JIS G 4053:2008, and steel materials to which S has been added to improve machinability are preferable.

[0014] The chemical composition of the crankshaft 10 may include, in mass %, in addition to Fe and impurities, C: 0.30-0.60%, Si: 0.01-2.0%, Mn: 0.1-2.0%, Cr: 0.01-0.50%, Al: 0.001-0.06%, N: 0.001-0.02%, P: 0.03% or less, and S: 0.20% or less. The chemical composition of the crankshaft 10 may include elements other than those described above. The chemical composition of the crankshaft 10 may include, in mass %, Mo: 0-0.50%, Cu: 0-0.50%, Ni: 0-0.50%, Ti: 0-0.050%, Nb: 0-0.050%, Ca: 0-0.005%, Bi: 0-0.30%, and V: 0-0.20%.

[0015] The journal portion 11 is connected to a cylinder block (not shown). The pin portion 12 is connected to a connecting rod (not shown). The arm portion 13 connects the journal portion 11 and the pin portion 12.

[0016] [Pin 12 Configuration] 2 is an enlarged cross-sectional view of the pin portion 12 of the crankshaft 10 and its vicinity. The pin portion 12 has a parallel portion 121 having a constant outer diameter and a fillet portion 122 formed continuously with the parallel portion 121. The thrust wall 14 and the pin top 15 are formed on the outside of the fillet portion 122. The parallel portion 121 is a portion that slides against a bearing of the connecting rod. The fillet portion 122 is a portion that connects the parallel portion 121 and the thrust wall 14, and is formed in a smooth shape to relieve stress concentration.

[0017] In the crankshaft 10 according to this embodiment, the surface structure of the parallel portion 121 is mainly composed of ferrite-pearlite over a certain length or more, and the surface structure of the fillet portion 122 is mainly composed of martensite. The respective structure distributions of the parallel portion 121 and the fillet portion 122 will be described in detail below.

[0018] [Structure and hardness of parallel portion 121] In this embodiment, within the range of length L1 of parallel portion 121, the structure from the surface to depth d1 (the structure of region 121a in FIG. 2) is a structure containing 87.5% by volume or more of ferrite-pearlite. Here, length L1 is 15.0% or more of length L of parallel portion 121, and depth d1 is 6.0% or more of radius R of parallel portion 121. Here, "ferrite-pearlite" includes full pearlite.

[0019] According to this configuration, the transformation expansion due to martensitic transformation is reduced, and bending of the crankshaft 10 due to quenching can be suppressed.

[0020] The length L1 is 15.0% or more of the length L of the parallel portion 121. From the viewpoint of reducing bending due to quenching, the longer the length L1, the more preferable. The lower limit of the length L1 is preferably 30.0% of the length L, more preferably 50.0% of the length L, even more preferably 70.0% of the length L, and even more preferably 80.0% of the length L. On the other hand, if the length L1 is too large, it may be difficult to make the structure of the surface layer of the fillet portion 122 a structure mainly composed of martensite. The upper limit of the length L1 is preferably 95.0% of the length L.

[0021] In the range of the length L1 of the parallel portion 121, if the structure from the surface to the depth d1 contains 87.5 volume % or more of ferrite-pearlite, the effect of suppressing quench bending can be obtained. The structure at a position deeper than the depth d1 is arbitrary. The structure in the range of the length L1 of the parallel portion 121 may be a structure mainly composed of ferrite-pearlite to the core. The depth d1 is preferably 50.0% or more of the radius R, more preferably 80.0% or more of the radius R, and even more preferably 100.0% of the radius R. Here, the depth d1 being 100.0% of the radius R means that the structure in the range of the length L1 of the parallel portion 121 is a structure mainly composed of ferrite-pearlite to the core.

[0022] The hardness from the surface to the depth d1 in the range of length L1 of the parallel portion 121 (the hardness of the region 121a in FIG. 2) is preferably HV400 or less. The hardness of the region 121a is measured by taking a sample with a cross section (longitudinal cross section) parallel to the axial direction of the crankshaft 10 as the measurement surface, and measuring the measurement surface in accordance with JIS Z 2244 (2009). The test force is 300 gf (2.942 N). The hardness of the region 121a is preferably HV350 or less, and more preferably HV320 or less. The lower limit of the hardness of the region 121a is, for example, HV220.

[0023] [Structure and hardness of fillet portion 122] In this embodiment, the structure from the surface of the fillet portion 122 to a depth d2 (the structure of the region 122a in FIG. 2) contains 87.5 volume % or more of martensite. Here, the depth d2 is 6.0% or more of the radius R of the parallel portion 121. The depth d2 may be the same as or different from the depth d1.

[0024] The fillet portion 122 is the portion of the pin portion 12 to which the strongest stress is applied. Furthermore, bending fatigue, which is a problem in the crankshaft 10, is predominantly affected by the characteristics of the surface layer of the component. Therefore, by making the structure from the surface of the fillet portion 122 to a depth d2 mainly composed of martensite, a predetermined fatigue strength can be ensured.

[0025] The structure at a position deeper than the depth d2 is arbitrary. The structure of the fillet portion 122 may be a structure mainly composed of martensite up to the core. From the viewpoint of ensuring fatigue strength, the greater the depth d2, the more preferable it is. The lower limit of the depth d2 is preferably 8.0% of the radius R, more preferably 10.0% of the radius R, and even more preferably 12.0% of the radius R. On the other hand, if the hardening depth of the fillet portion 122 is too large, it may be difficult to ensure a structure mainly composed of ferrite and pearlite in the parallel portion 121. The upper limit of the depth d2 is preferably 30.0% of the radius R, more preferably 25.0% of the radius R, and even more preferably 20.0% of the radius R.

[0026] The hardness from the surface of the fillet portion 122 to a depth d2 (the hardness of the region 122a in FIG. 2) is preferably HV580 or more. The hardness of the region 122a is measured by taking a sample with a cross section (longitudinal cross section) parallel to the axial direction of the crankshaft 10 as the measurement surface, and measuring the measurement surface in accordance with JIS Z 2244 (2009). The test force is 300 gf (2.942 N). The hardness of the region 122a is preferably HV600 or more, and more preferably HV620 or more. The upper limit of the hardness of the region 122a is, for example, HV800.

[0027] [Journal Unit 11 Configuration] Although not shown, like the pin portion 12, the journal portion 11 also has a parallel portion having a constant outer diameter and a fillet portion formed continuously with the parallel portion.

[0028] In the journal portion 11, as in the case of the pin portion 12, the structure from the surface to a depth of at least 6.0% of the radius of the parallel portion over a length of at least 15.0% of the length of the parallel portion contains 87.5% or more by volume of ferrite-pearlite. Also, in the journal portion 11, as in the case of the pin portion 12, the structure from the surface of the fillet portion to a depth of at least 6.0% of the radius of the parallel portion contains 87.5% or more by volume of martensite.

[0029] According to this configuration, it is possible to reduce the bending of the crankshaft 10 while ensuring a predetermined fatigue strength, similarly to the pin portion 12. The suitable size of the region mainly composed of ferrite-pearlite in the parallel portion and the suitable range of hardness of this region, and the suitable size of the region mainly composed of martensite in the fillet portion and the suitable range of hardness of this region are the same as those of the pin portion 12.

[0030] The structure and hardness of the portion other than the journal portion 11 and the pin portion 12 (for example, the arm portion 13) are arbitrary.

[0031] [Manufacturing method of crankshaft] Next, a description will be given of an example of a method for manufacturing the crankshaft 10. The manufacturing method described below is merely an example, and is not intended to limit the method for manufacturing the crankshaft 10.

[0032] 3 is a flow diagram showing an example of a method for manufacturing the crankshaft 10. This manufacturing method includes a step of preparing a material (step S1), a hot forging step (step S2), a heat treatment step (step S3), a machining step (step S4), a quenching step (step S5), and a finish processing step (step S6). Each step will be described in detail below.

[0033] A material for the crankshaft 10 is prepared (step S1). The material is, for example, a steel bar. The material can be produced, for example, by continuous casting or blooming molten steel having a predetermined chemical composition.

[0034] The material is hot forged to form a rough shape of the crankshaft (step S2). The hot forging may be performed in two stages: rough forging and finish forging.

[0035] The crankshaft rough product produced by hot forging is subjected to heat treatment such as normalizing as necessary (step S3). The heat treatment step (step S3) is an optional step, and this step may be omitted depending on the required characteristics of the crankshaft, etc.

[0036] The crankshaft rough product is machined (step S4). The machining includes cutting, grinding, drilling, etc. Through this process, an intermediate product having a shape close to that of the final product is manufactured.

[0037] The intermediate crankshaft that has been machined is quenched (step S5). Specifically, it is heated to a predetermined heating temperature and then quenched. At this time, for example, a high-frequency induction heating device is used to heat only the vicinity of the fillet portion of the journal portion 11 and the vicinity of the fillet portion 122 of the pin portion 12, and the parallel portion of the journal portion 11 and the parallel portion 121 of the pin portion 12 are prevented from being heated as much as possible. The heating location can be adjusted by the shape of the induction coil, the distance between the induction coil and the target portion, the output frequency, etc. This quenching may be performed in multiple steps. The heating temperature is Ac3 point or higher, preferably 900°C or higher. The quenching after heating is preferably water cooling. In order to suppress quench cracking, the intermediate product after quenching may be subjected to low-temperature tempering at a temperature that does not significantly affect the structure.

[0038] The intermediate product after quenching is subjected to finishing processing as necessary (step S6). For example, the journal portion 11 and the pin portion 12 are subjected to grinding or lapping to adjust the surface shape.

[0039] The above describes the configuration of the crankshaft 10 according to one embodiment of the present invention and an example of a manufacturing method thereof. According to this embodiment, a crankshaft in which bending due to quenching is suppressed can be obtained.

[0040] In the above-described embodiment, the surface structure of the parallel portion within a certain length range in both the journal portion 11 and the pin portion 12 is mainly composed of ferrite-pearlite, and the surface structure of the fillet portion is mainly composed of martensite. However, in the crankshaft 10, only one of the journal portion 11 and the pin portion 12 may have the above-described structure distribution. If at least one of the journal portion 11 and the pin portion 12 has the above-described structure distribution, the effect of reducing quench bending can be obtained.

[0041] Comparing the journal portion 11 and the pin portion 12, the pin portion 12 is more likely to bend due to annealing. This is because the heat capacity of the pin top 15 (FIG. 2) is small. Therefore, when only one of the journal portion 11 and the pin portion 12 is to have the above-mentioned texture distribution, it is preferable that the pin portion 12 is to have the above-mentioned texture distribution. In this case, the pin top 15 can be made smaller, which also contributes to reducing the weight of the crankshaft 10. However, from the viewpoint of minimizing annealing bending, it is preferable that both the journal portion 11 and the pin portion 12 are to have the above-mentioned texture distribution. EXAMPLES

[0042] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0043] A simulation of the heat bending of the pin of a crankshaft was carried out using the finite element method. Figures 4 to 6 show the three-dimensional analysis model used in this simulation. Figure 4 is a perspective view of this model, Figure 5 is a front view, and Figure 6 is an enlarged view of the area near the pin top. As shown in Figures 5 and 6, the thrust distance was set to 21.0 mm, the parallel portion length L was set to 15.0 mm, the parallel portion radius R was set to 24.0 mm, and the fillet curvature radius was set to 3.0 mm, and only the half region on the pin top side was modeled to reduce the calculation load. The material constants of S45C were used for various calculations.

[0044] The structure and hardness distribution, as well as the amount of displacement, were calculated when this crankshaft was induction hardened. Figures 7 and 8 are cross-sectional views showing the arrangement of induction coils in this simulation. In the arrangement in Figure 7, induction coils are arranged only in the vicinity of the fillet portions. In the arrangement in Figure 8, induction coils are arranged not only in the vicinity of the fillet portions but also in the vicinity of the parallel portions. Using these induction coils, induction heating was performed with an output frequency of 10 kHz and a current flow time of 22 seconds. After heating, a heat transfer coefficient of 40 kW / (m 2 The mixture was cooled to 20°C (K). The results are shown in Table 1.

[0045] [Table 1]

[0046] In Table 1, the "Fillet section" in the "Coil arrangement" column is data simulating the case where induction hardening was performed with the coil arrangement in Fig. 7, and the "Fillet section + parallel section" in the same column is data simulating the case where induction hardening was performed with the coil arrangement in Fig. 8. The values ​​in the "Current" column are the current values ​​passed through the induction coil, and are listed as relative values ​​with the current value of No. 6 set to 100%.

[0047] The value in the "Pin top x-direction displacement" column is the amount of displacement in a direction parallel to the axial direction of the crankshaft at the position of point P2 in Figure 6, and is listed as a percentage of the parallel section length (15.0 mm). The value in the "Pin top y-direction displacement" column is the amount of displacement in a direction perpendicular to the axial direction of the crankshaft at the position of point P2 in Figure 6, and is listed as a percentage of the parallel section radius (24.0 mm). The value in the "Parallel section y-direction displacement" column is the amount of displacement in a direction perpendicular to the axial direction of the crankshaft at the position of point P1 in Figure 5, and is listed as a percentage of the parallel section radius (24.0 mm).

[0048] 9A to 9D are contour maps showing the microstructure distribution of No. 1, No. 3, No. 5, and No. 6, respectively. In these figures, "M≧87.5%" indicates the region where the volume fraction of martensite is 87.5% or more, and "α+P≧87.5%" indicates the region where the volume fraction of ferrite and pearlite is 87.5% or more.

[0049] As shown in Table 1, Nos. 1 to 4, in which L1 / L was 15.0% or more, had smaller annealing distortion, and in particular, the displacement of the pin top in the x direction was smaller, compared to Nos. 5 and 6, in which L1 / L was less than 15.0%.

[0050] Although one embodiment of the present invention has been described above, the above-described embodiment is merely an example for carrying out the present invention. Therefore, the present invention is not limited to the above-described embodiment, and the above-described embodiment can be appropriately modified and carried out without departing from the spirit of the present invention. [Explanation of symbols]

[0051] 10. Crankshaft 11 Journal Section 12 Pin section 121 Parallel section 122 Fillet 13 Arm section 14 Thrust Wall 15 Pin Top

Claims

1. A crankshaft including a journal portion and a pin portion, each of the journal portion and the pin portion has a parallel portion having a constant outer diameter and a fillet portion formed continuously with the parallel portion; The pin portion further includes a thrust wall and a pin top. In the pin portion, The parallel portion has a structure including 87.5% by volume or more of ferrite-pearlite in a length of at least 70.0% of the length of the parallel portion from the surface to a depth of at least 80.0% of the radius of the parallel portion, A crankshaft, wherein a structure from the surface of the fillet portion to a depth of at least 12.0% of the radius of the parallel portion, and a structure of the thrust wall and the pin top are structures containing 87.5 volume % or more of martensite.

2. 2. The crankshaft of claim 1, In the pin portion, the parallel portion has a hardness of HV400 or less along a length of at least 70.0% of the length of the parallel portion from a surface to a depth of at least 80.0% of the radius of the parallel portion; The hardness of the crankshaft, from the surface of the fillet portion to a depth of at least 12.0% of the radius of the parallel portion, is HV580 or more.

3. A method for manufacturing a crankshaft according to claim 1 or 2, comprising the steps of: Only the vicinity of the fillet portion is heated with Ac by a high-frequency induction heating device. 3 A method for manufacturing a crankshaft, comprising a step of quenching from a temperature above the hardening point.

Citation Information

Patent Citations

  • Crankshaft

    JP1986270517A

  • Production of crankshaft

    JP1988118079A

  • High frequency heating method

    JP2006328497A

  • Crankshaft, internal combustion engine, transportation apparatus, and manufacturing method for crankshaft

    JP2008267598A

  • Crankshaft and method of manufacturing the same

    JP4007033B2