Method for manufacturing a resistance spot welded joint and resistance spot welding device
By controlling the pressurizing force change rate during resistance spot welding, the method effectively prevents expulsion, ensuring consistent nugget diameter and joint strength.
Patent Information
- Application Number
- JP2021000107
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-04
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2041-01-04
AI Technical Summary
Existing resistance spot welding techniques fail to effectively predict and suppress the occurrence of expulsion, leading to variations in nugget size and reduced weld strength, with debris scattering posing quality issues.
A method and device that control the pressurizing force change rate during resistance spot welding by setting a threshold value, using feedback control to adjust welding current and pressure to prevent expulsion, ensuring a stable nugget diameter and strength.
Stably forms a spot weld of desired size while suppressing expulsion, maintaining joint strength and preventing debris scattering.
Smart Images

Figure 0007568921000003 
Figure 0007568921000004 
Figure 0007568921000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a resistance spot welded joint and a resistance spot welding apparatus. [Background technology]
[0002] In automobile assembly, spot welding is used to join components. In spot welding, the occurrence of expulsion is a problem. Explosion refers to the phenomenon in which the base material is locally overheated and melts and splashes in lap resistance welding, or the metal involved. Explosion that occurs on the outer surface of the electrode tip and the contacting base material is called surface expulsion, expulsion that occurs between the base materials is called internal expulsion, and the phenomenon in which metal in the nugget splashes out to the surface, or the splashed metal, is called surface expulsion (JIS-Z 3001-6:2013).
[0003] Explosion can cause variations in the size of the nugget and reduce the strength of the weld. In addition, there is a problem that the expulsion remains as a protrusion on the surface of the weld or scatters and adheres to other components. Therefore, a technology is required that can stably ensure the nugget diameter required by the design of the component while suppressing expulsion.
[0004] Patent Document 1 discloses an adaptive control method for resistance welding, which is characterized by detecting the resistance between electrodes sandwiching a material to be welded while a welding current is flowing, comparing the detected resistance value with a resistance value according to a preset reference resistance curve from moment to moment or at a predetermined specific point in time, and controlling the pressure applied between the electrodes in accordance with the difference in resistance values to change the resistance between the electrodes so that it coincides with the resistance value according to the reference resistance curve, thereby ensuring the desired quality of the weld.
[0005] Patent Document 2 discloses a spot welding method in which pressure is applied to the workpiece by moving an electrode tip with the rotation of a servo motor, and a control method for suppressing the occurrence of expulsion in spot welding is disclosed in which the motor current of the servo motor is detected at short time intervals during welding, the pressing force based on the motor current is compared with a preset reference pressing force, and if it is determined that the pressing force based on the motor current has decreased below the reference pressing force, a correction is made to increase the pressing force or decrease the welding current.
[0006] Patent Document 3 describes a resistance spot welding method in which a workpiece consisting of overlapping metal plates is sandwiched between a pair of electrodes and joined by applying pressure and passing current through the workpiece, in which a main welding step and a test welding step prior to the main welding step are performed, and the test welding step is performed under two or more welding conditions. In the test welding step, for each of the welding conditions, a time change curve of the instantaneous heat generation per unit volume and a time change curve of the instantaneous heat generation per unit volume are calculated from a pressure parameter from when pressure is started to be applied to the workpiece before the start of current flow until a set pressure is reached, and an electrical characteristic between the electrodes when a current is passed under constant current control to form an appropriate nugget. and storing a cumulative heat generation amount and a time-varying curve for the instantaneous heat generation amount per unit volume in the test welding, and further, in the main welding, before the start of current application, pressurization of the welded material is performed under the same conditions as in the test welding, and a pressing force parameter from the start of pressurization until a set pressing force is reached is compared with the pressing force parameter stored in the test welding, for each welding condition of the test welding. The time-varying curve for the instantaneous heat generation amount per unit volume and the cumulative heat generation amount per unit volume in the test welding, which are stored under the welding conditions for which the difference is smallest, are set as target values for the main welding, and adaptive control welding is performed in which the current application amount is controlled in accordance with the target values.
[0007] Patent Document 4 discloses a method for controlling current flow time in resistance welding, characterized in that after a predetermined current flow time has elapsed in lap resistance welding, a sudden drop in electrode pressure due to the expulsion phenomenon occurring from the material to be welded is detected and the welding current is stopped. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Unexamined Patent Publication No. 56-148481 [Patent Document 2] Japanese Patent Application Publication No. 7-96376 [Patent Document 3] International Publication No. 2019 / 160141 [Patent Document 4] Japanese Patent Publication No. 58-47579 Summary of the Invention [Problem to be solved by the invention]
[0009] However, none of the techniques described in the above patent documents have a sufficient expulsion suppression effect to ensure the product quality required in recent years, because none of the above patent documents have a means for effectively predicting the occurrence of expulsion during resistance spot welding.
[0010] In consideration of the above circumstances, an object of the present invention is to provide a method for manufacturing a resistance spot welded joint and a resistance spot welding apparatus that are capable of stably forming a spot weld of a desired size while suppressing the occurrence of expulsion. [Means for solving the problem]
[0011] (1) A method for manufacturing a resistance spot welded joint according to one embodiment of the present invention is a method for manufacturing a resistance spot welded joint comprising a step of resistance spot welding two or more overlapping steel sheets, wherein, during the resistance spot welding, a rate of change of welding force α (kN / sec) calculated by the following equation 1 is controlled to be equal to or greater than a predetermined threshold value during the period from T1 to the end of current flow. α = (P-P1) / (T-T1): Equation 1 Here, in Equation 1, T is the elapsed time (sec) from the start of the resistance spot welding, P is the pressing force (kN) at a point when T has elapsed from the start of the resistance spot welding, T1 is the elapsed time (sec) between the point when the value obtained by differentiating P with respect to T becomes 0 the second time counting from the start of current flow in the resistance spot welding and the start of the resistance spot welding, and P1 is the pressing force (kN) at a point when T1 has elapsed from the start of the resistance spot welding. (2) In the method for manufacturing a resistance spot welded joint described in (1) above, the method for manufacturing a resistance spot welded joint may further include a step of stacking steel plates of the same material as the two or more steel plates and performing preliminary resistance spot welding prior to the resistance spot welding, and the threshold value may be identified by performing the preliminary resistance spot welding multiple times while changing the welding current, and comparing the rate of change α of pressing force in the preliminary resistance spot welding that caused expulsion with the rate of change α of pressing force in the preliminary resistance spot welding that did not cause expulsion. (3) In the manufacturing method of the resistance spot welded joint described above in (1), the tensile strength of the two or more steel plates may be 270 to 2000 MPa, the total thickness of the two or more steel plates may be 1.6 to 5.0 mm, and the threshold value may be -3.5 kN / sec. (4) In the method for producing a resistance spot welded joint according to (1) or (3) above, the tensile strength of one or more of the steel plates may be set to 980 to 2000 MPa, and the threshold value may be set to -3.0 kN / sec. (5) In the method for manufacturing a resistance spot welded joint according to any one of (1) to (4) above, when the rate of change of pressing force α falls below half of the threshold value, the passage of current may be stopped for a period of 20 to 160 msec. (6) In the method for manufacturing a resistance spot welded joint described in any one of (1) to (4) above, when the rate of change of welding force α falls below half of the threshold value, the welding current value may be reduced and / or the set welding force may be increased. (7) In the method for manufacturing a resistance spot welded joint described in (6) above, when the rate of change of welding force α falls below half of the threshold value, the current reduction rate Ri of the welding current may be set within a range that satisfies the following formula 2. 1.2×(20×α+30)≦Ri≦0.8×(20×α+30): Formula 2 Here, in the above formula 2, Ri is the current reduction rate (%) (Ri≦0%) based on the welding current at the start of the energization, and α is the above welding pressure change rate. (8) In the method for manufacturing a resistance spot welded joint described in (6) above, when the rate of change of pressing force α falls below ½ of the threshold value, the set pressing force increase rate Rf may be set to be within a range that satisfies the following formula 3. 0.8×(-33×α-50)≦Rf≦1.2×(-33×α-50): Formula 3 Here, in the formula 3, Rf is the rate of increase (%) of the set pressure based on the set pressure at the start of pressure application (0%≦Rf), and α is the rate of change of the pressure. (9) In the method for manufacturing a resistance spot welded joint described in (6) above, when the rate of change of welding force α falls below ½ of the threshold value, the welding current reduction rate Ri and the set welding force increase rate Rf may be set within ranges that satisfy the following equations 4 and 5. 1.2×β×(20×α+30)≦Ri≦0.8×β×(20×α+30): Formula 4 0.8×(1-β)×(-33×α-50)≦Rf≦1.2×(1-β)×(-33×α-50): Formula 5 Here, in the above-mentioned formula 4 and formula 5, Ri is the current reduction rate (%) (Ri≦0%) based on the welding current at the start of the current flow, β is a constant between 0 and 1, α is the rate of change of the pressing force, and Rf is the set pressing force increase rate (%) (0%≦Rf) based on the set pressing force at the start of the current flow. (10) In the method for manufacturing a resistance spot welded joint described in any one of (1) to (4) and (6) to (9) above, the welding current may be 8 kA or more from the start of the resistance spot welding to the end of the current flow. (11) A resistance spot welding apparatus according to another aspect of the present invention is a resistance spot welding apparatus for carrying out the method of manufacturing a resistance spot welded joint according to any one of (1) to (10) above, comprising: a pair of electrodes; a pressurizing unit configured to apply a pressurizing force between the pair of electrodes; a welding current control unit configured to pass a welding current between the pair of electrodes; a pressurizing force measuring unit configured to measure the pressurizing force between the pair of electrodes; and a pressurizing force measuring unit configured to monitor a change in pressurizing force over time based on a measurement result of the pressurizing force measuring unit and to control the pressurizing force measuring unit and the welding current control unit. Department and a pressing force change rate control unit configured to be able to control the pressing force change rate α to a predetermined threshold value or higher by controlling one or both of the above. Effect of the Invention
[0012] According to the present invention, it is possible to provide a method for manufacturing a resistance spot welded joint and a resistance spot welding apparatus that are capable of stably forming a spot weld of a desired size while suppressing the occurrence of expulsion. [Brief description of the drawings]
[0013] [Figure 1] 4 is a graph showing a schematic change in applied pressure over time during resistance spot welding. [Diagram 2] 1 is a schematic diagram of a resistance spot welding device according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] As described above, expulsion can be classified into three types: surface expulsion, intermediate expulsion, and surface expulsion. The method for manufacturing a welded joint according to this embodiment is primarily intended to suppress intermediate expulsion.
[0015] Resistance spot welding (spot welding) is a type of resistance welding in which overlapping base materials are sandwiched between the tips of electrodes with properly shaped tips, current is concentrated in a relatively small area to heat it locally, and pressure is applied with the electrodes at the same time. Explosion refers to the phenomenon in which the base materials are locally overheated and melted and scattered in resistance lap welding, or the metal involved, and expulsion that occurs between base materials is called intermediate expulsion.
[0016] Explosion is a phenomenon in which the molten metal, compressed by pressure applied by the electrode during resistance spot welding, breaks the surrounding pressure weld and splashes out of the weld between the base materials. A pressure weld is a solid-phase welded ring-shaped part that occurs around the nugget in lap resistance welding, and is also called a corona bond. If the pressure weld grows in accordance with the growth of the molten metal and has an area (i.e., strength) that can withstand the pressure of the molten metal, expulsion will not occur.
[0017] Increasing the welding current to increase the nugget diameter and ensure joint strength increases the risk of expulsion. This is because the growth rate of the molten metal is greater than the growth rate of the pressure welded portion. This causes the area of the pressure welded portion to be insufficient during resistance spot welding, and the pressure welded portion cannot withstand the pressure from the molten metal. As a result, the pressure welded portion is destroyed and the molten metal splashes out. Therefore, a simple method of suppressing expulsion is to reduce the welding current. However, the smaller the welding current, the smaller the nugget diameter and the lower the joint strength. Therefore, in the manufacture of spot welded joints that require high strength, suppressing the welding current cannot be a practical solution for suppressing expulsion.
[0018] The inventors have repeatedly investigated and examined the relationship between the change over time in the welding current value and the welding pressure and the occurrence of expulsion. As a result, the inventors have found that a unique fluctuation in the welding pressure occurs when expulsion occurs. Furthermore, the inventors have found that the occurrence of expulsion can be suppressed by suppressing the fluctuation in the welding pressure to a predetermined threshold value or less.
[0019] During spot welding, the resistance-heated base material undergoes thermal expansion and strength loss as the temperature rises. The thermal expansion and strength loss cause minute displacements in the electrodes that press the base material, and in mechanisms such as the shank and holder that hold the electrodes (hereinafter, the electrodes and the mechanisms that hold them are collectively referred to as "electrodes"). Specifically, when the base material thermally expands, the electrodes that clamp the base material are subjected to a force in a direction away from the base material. This increases the actual pressure force (hereinafter, referred to as "actual pressure force" or simply "pressure force") measured by a load cell or the like of the resistance spot welding machine. On the other hand, when the base material softens, the electrodes that clamp the base material are displaced so as to be pushed into the base material. This reduces the pressure force.
[0020] FIG. 1 shows a schematic diagram of the change in the pressing force over time during resistance spot welding. The inventors found that in the initial stage of resistance heating, the pressing force was greater than the pressing force (hereinafter referred to as the "set pressing force") that was set in advance in the control device of the resistance spot welding machine. It was presumed that this is because, when the temperature of the base material is low, the thermal expansion of the base material is dominant with respect to the pressing force of the electrode, and the thermal expansion of the base material displaces the electrode so as to move away from the center of the base material. On the other hand, when resistance heating progresses, the pressing force decreased. Currently, servo motor type pressing mechanisms are mainstream for welding machines. The torque acting on the drive system is measured by a torque sensor arranged near the servo motor. Since there is a correlation between this torque and the pressing force, the pressing force is controlled through the control of the torque. It was presumed that the decrease after the increase in the pressing force was also the result of the control of the torque and the pressing force. The present invention is directed to a welding machine using a servo motor pressing method.
[0021] Such an increase or decrease in the pressing force was confirmed regardless of the occurrence of expulsion. On the other hand, the present inventors also found that a significant decrease in the pressing force occurs in resistance spot welding in which expulsion has occurred. It is believed that such a significant decrease occurs because it is difficult to restore the pressing force with the above-mentioned normal torque control. Then, by measuring the rate at which the pressing force decreases during resistance spot welding, the present inventors were able to predict the occurrence of expulsion. Specifically, the present inventors found that expulsion occurs frequently when the rate at which the pressing force decreases exceeds a threshold value according to the characteristics of the base material. Note that there have been no reports so far on the specific relationship between the rate at which the pressing force decreases in resistance spot welding and the occurrence of expulsion. Therefore, no technology has been reported so far that attempts to predict the occurrence of expulsion based on the rate at which the pressing force decreases.
[0022] In addition, the inventors were able to suppress expulsion extremely effectively by performing feedback control to reduce the welding current when the rate of decrease in the welding pressure exceeds a threshold value, and even with such feedback control, a nugget having a sufficient diameter to ensure joint strength was formed.
[0023] The manufacturing method (resistance spot welding method) of a resistance spot welded joint according to this embodiment, obtained based on the above findings, includes a process of resistance spot welding two or more overlapping steel sheets, and during the resistance spot welding, the rate of change of welding force α (unit: kN / sec) calculated by the following equation 1 is controlled to be equal to or greater than a predetermined threshold value in the period from T1 to the end of current flow. α=(P-P1) / (T-T1): Equation 1 The meaning of the letters in formula 1 will be explained below with reference to the graph of the change in applied pressure over time shown in FIG. T is the elapsed time (unit: sec) from the start of resistance spot welding. The start of resistance spot welding means the start of pressure application. In the graph shown in FIG. 1, the start of pressure application is earlier than the left end of the graph. P is the applied pressure (unit: kN) at the point T has elapsed since the start of resistance spot welding. The applied pressure is the actual applied pressure measured by a load cell or the like. T1 is the elapsed time (unit: sec) between the time when the value obtained by differentiating P with respect to T becomes 0 the second time counting from the time when current started in resistance spot welding, and the start of resistance spot welding. In Fig. 1, the time when current started is located at the left foot of the first peak of the applied pressure shown on the left side of the graph, the time when the value obtained by differentiating P with respect to T becomes 0 the first time counting from the time when current started in resistance spot welding is located at the top of the first peak of the applied pressure, and the time when the value obtained by differentiating P with respect to T becomes 0 the second time counting from the time when current started in resistance spot welding is located at the right foot of the first peak of the applied pressure. P1 is the applied pressure (unit: kN) at the time T1 has elapsed from the start of resistance spot welding. If it is known that P1 is equal to the applied pressure set at the start of resistance spot welding, the applied pressure set at the start of resistance spot welding may be regarded as P1.
[0024] The rate of change of the pressing force α is an index indicating the rate of decrease of the pressing force described above. The rate of decrease of the pressing force is the change in the pressing force P at a point in time T after the start of resistance spot welding, i.e., the value obtained by differentiating the pressing force with respect to time, and this value changes over time. However, from the viewpoint of the control accuracy of the resistance spot welding device, it is not easy to control the welding conditions while instantly calculating the time-differential value of the pressing force. Therefore, the inventors decided to use the rate of change of the pressing force α defined by Equation 1 as an index for predicting the occurrence of expulsion.
[0025] Specifically, the pressure force change rate α means an average change rate of the pressure force during the period from time T1 to time T. For example, the pressure force change rate α calculated for point X in the dashed line graph in FIG. X is the angle α X is equivalent to.
[0026] The present inventors conducted a detailed study of the pressure history of resistance spot welding in which expulsion occurred and found that a reduction in the pressure was observed before expulsion occurred.
[0027] The solid line graph in Figure 1 is a graph that shows a schematic representation of the change in pressure over time in resistance spot welding where expulsion does not occur. The dashed line graph in Figure 1 is a graph that shows a schematic representation of the change in pressure over time in resistance spot welding where expulsion does occur. In these graphs, the pressure first increases as soon as current begins to flow. This is presumably a phenomenon caused by thermal expansion of the steel sheet. Next, the pressure decreases. This is presumably a result of pressure control. This phenomenon is observed regardless of whether expulsion occurs or not.
[0028] Thereafter, in resistance spot welding where no expulsion occurred, the pressing force generally decreases steadily, but in resistance spot welding where expulsion occurred, the pressing force decreases and then suddenly decreases. It is presumed that the sudden decrease in pressing force is a phenomenon that occurs when the amount of molten metal in the weld is greatly reduced (expulsion occurs) due to the occurrence of expulsion, and the electrode moves as if being pushed into the steel sheet. It is presumed that the decrease in pressing force that occurs before the occurrence of expulsion is caused by softening due to the temperature rise of the steel sheet. However, the decrease in pressing force that occurs prior to the occurrence of expulsion is a phenomenon commonly observed in resistance spot welding where expulsion occurred. It was also confirmed that expulsion occurrence can be suppressed by controlling the pressing force change rate α to a predetermined value or more by some means. For the above reasons, in the manufacturing method of a resistance spot welded joint according to this embodiment, the pressing force change rate α is controlled to a predetermined threshold value or more that is determined according to various characteristics such as the material and thickness of the steel sheet that is the base material.
[0029] In the method for manufacturing resistance spot welding according to this embodiment, the steel plate serving as the base material, the method for determining the threshold value, and the method for controlling the rate of change of pressure α to be equal to or greater than the threshold value are not particularly limited, but a suitable example will be described below.
[0030] (Method of determining the threshold) The threshold value can be specified by performing preliminary resistance spot welding on two or more steel plates of the same material as the base material in the resistance spot welding before the resistance spot welding. The steel plates of the same material are, for example, steel plates whose steel type and thickness are substantially the same as those of the steel plates to be actually welded. However, it is presumed that the steel type and thickness do not need to be strictly the same. Here, the preliminary resistance spot welding is performed multiple times while changing at least the welding current, and thus, preliminary resistance spot welding that causes expulsion and preliminary resistance spot welding that does not cause expulsion are performed at least once each. Furthermore, the pressing force change rate α in these preliminary resistance spot weldings is calculated. Then, the pressing force change rate α in the preliminary resistance spot welding that causes expulsion is compared with the pressing force change rate α in the preliminary resistance spot welding that does not cause expulsion. However, this α may differ if the welding equipment is different even if the steel plates are the same, and it is necessary to determine it according to the welding equipment.
[0031] This allows the threshold value in the plate assembly subjected to the preliminary resistance spot welding to be specified. By performing the above-mentioned resistance spot welding using this threshold value, it is possible to ensure joint strength while suppressing the occurrence of expulsion. However, the method of determining the threshold value is not limited to this, and it is permissible to determine the threshold value by performing various experiments based on the above-mentioned technical concept. According to the results of experiments conducted by the present inventors, it was estimated that the absolute value of the threshold value tends to increase as the strength of the steel plate decreases.
[0032] Furthermore, when two or more steel plates are automotive steel plates, for example, having a tensile strength of 270 to 2000 MPa and a total thickness of 1.6 to 5.0 mm, the threshold value was approximately -3.5 kN / sec. When at least one of the two or more steel plates is a high-strength steel plate, for example, having a tensile strength of 980 to 2000 MPa and a total thickness of 1.6 to 5.0 mm, the threshold value was approximately -3.0 kN / sec. Therefore, when the strength of the steel plate and the total thickness of the overlapped steel plates are within the ranges exemplified above, the above threshold value may be used instead of performing preliminary resistance spot welding.
[0033] For example, in the technology described in the above-mentioned Patent Document 2, it is necessary to find and set a reference pressure for each steel sheet, and it is also necessary to find the reference pressure whenever there is a disturbance such as a sheet gap or an impact angle, which is cumbersome, whereas the threshold value according to this embodiment changes relatively little in response to disturbances. According to this embodiment, even if there is a disturbance, it is possible to effectively predict the occurrence of expulsion by applying the above-mentioned threshold value to the pressure force change rate α.
[0034] (Method for controlling the pressure change rate α to be equal to or greater than a threshold value) The pressure varies depending on the welding current value. Specifically, when the welding current value in resistance spot welding is reduced or the welding current value is stopped to be 0, the temperature of the steel sheet decreases due to heat transfer from the steel sheet to the electrode and heat conduction to the periphery of the welded part, and the pressure increases. Therefore, for example, when the pressure change rate α falls below 1 / 2 of the threshold, the current may be stopped for 20 to 160 msec. This makes it possible to increase the pressure and prevent the pressure change rate α from falling below the threshold. In addition, by restarting the current, the growth of the molten metal can be restarted and a sufficient nugget diameter can be secured to ensure the joint strength. Since the expulsion occurs with the reduction in the pressure, the threshold value of the pressure change rate α for preventing the expulsion is a negative value. Therefore, "1 / 2 of the threshold" is used as a trigger for executing the stop of the current. Specifically, the increase in the pressure is realized by increasing the motor current of the servo motor. Since there is a correlation between the motor current, torque, and pressure, the degree of increase in the pressure can be achieved by controlling the motor current.
[0035] However, the method of controlling the pressing force change rate α to be equal to or greater than the threshold value is not limited to the above. For example, instead of stopping the energization, the decrease in the pressing force can also be suppressed by reducing the welding current value. Also, the decrease in the pressing force (i.e., the actual pressing force) can also be suppressed by increasing the set pressing force of the electrodes. Therefore, for example, when the pressing force change rate α falls below half the threshold value, the welding current value may be reduced and / or the set pressing force may be increased. This makes it possible to increase the pressing force and prevent the pressing force change rate α from falling below the threshold value. Also, by continuing the energization, a nugget diameter sufficient to ensure joint strength can be secured.
[0036] Specifically, when the welding force change rate α falls below half the threshold value, the current decrease rate Ri of the welding current may be set within a range that satisfies Equation 2. 1.2×(20×α+30)≦Ri≦0.8×(20×α+30): Formula 2 Here, the meanings of the letters in formula 2 are as follows: Ri is the current reduction rate (%) (Ri≦0%) based on the welding current at the start of current flow. Specifically, the current value at the start of current flow is defined as I1, and the current value at time T is defined as I T When this is defined, Ri at time T can be calculated by the following formula. Ri = {(I T -I1) / I1}×100 α is the above-mentioned rate of change of welding pressure. When α is within the range of 1 / 2 of the threshold value to the threshold value, control of Ri is performed. For example, when the threshold value is -3.0, control of Ri is performed when -3.0≦α≦-1.5. More specifically, control of Ri is started from the point in time when it is detected that α has fallen below -1.5 during welding.
[0037] According to formula 2, the target control range of Ri is determined according to the degree of fluctuation in the rate of change of pressing force α. By controlling the welding current value so that Ri satisfies formula 2, it is possible to prevent the rate of change of pressing force α from falling below a threshold value. Furthermore, by controlling the welding current value so that Ri satisfies formula 2, it is possible to continue the passage of current while maintaining the rate of change of pressing force α at or above the threshold value, thereby ensuring joint strength.
[0038] Furthermore, when the pressure change rate α falls below half the threshold value, the set pressure increase rate Rf may be set within a range that satisfies the following formula 3. 0.8×(-33×α-50)≦Rf≦1.2×(-33×α-50): Formula 3 Here, the meanings of the letters in formula 3 are as follows: Rf is the rate of increase in the set pressure (%) (0%≦Rf) based on the set pressure at the start of pressurization. Specifically, the set pressure at the start of pressurization is defined as F1, and the set pressure at time T is defined as F2. T When this is defined, Rf at time T can be calculated using the following formula: Rf = {(F T -F1) / F1}×100 α is the above-mentioned rate of change of welding pressure. When α is within a range of 1 / 2 the threshold value to the threshold value, Rf is controlled. For example, when the threshold value is -3.0, Rf is controlled when -3.0≦α≦-1.5. More specifically, Rf control is started when it is detected that α has fallen below -1.5 during welding.
[0039] According to formula 3, the target control range of Rf is determined according to the degree of fluctuation in the rate of change of press force α. By controlling the set press force so that Rf satisfies formula 3, it is possible to prevent the rate of change of press force α from falling below a threshold value. In addition, by controlling the press force so that Rf satisfies formula 3, it is possible to continue energization while maintaining the rate of change of press force α at or above the threshold value, thereby ensuring joint strength.
[0040] Although specific control guidelines for the welding current value or the set pressure have been described above, the welding current value and the set pressure may be controlled simultaneously. In this case, when the pressure change rate α falls below half the threshold, the welding current decrease rate Ri and the set pressure increase rate Rf may be set within ranges that satisfy the following formulas 4 and 5. 1.2×β×(20×α+30)≦Ri≦0.8×β×(20×α+30): Formula 4 0.8×(1-β)×(-33×α-50)≦Rf≦1.2×(1-β)×(-33×α-50): Formula 5 Here, the meanings of the letters in formulas 4 and 5 are as follows: Ri is the current reduction rate (%) (Ri≦0%) based on the welding current at the start of energization, and is the same as Ri included in formula 2. β is a constant that can be set to any value between 0 and 1. α is the rate of change of applied pressure. Rf is the rate of increase (%) of the set pressure based on the set pressure at the start of pressure application (0%≦Rf), and is the same as Rf included in Equation 3.
[0041] Equation 4 is similar to equation 2, and the two coincide when β is 1. Equation 5 is similar to equation 3, and the two coincide when β is 0. β is a value used to distribute the influence of the set pressure force and the influence of the welding current value. The smaller β is, the stronger the influence of the set pressure force and the smaller the influence of the welding current value. This makes it possible to avoid overlapping between the influence of the welding current value and the influence of the welding current value, further stabilizing resistance spot welding.
[0042] The manufacturing method of the resistance spot welded joint according to the present embodiment can employ various conditions other than the above-exemplified conditions. For example, the welding current may be 8 kA or more from the start of energization to the end of energization. This makes it possible to more reliably form a nugget having a sufficient diameter to ensure joint strength. Normally, increasing the welding current increases the risk of splashing, but in the manufacturing method of the resistance spot welded joint according to the present embodiment, the occurrence of splashing can be effectively suppressed by controlling the pressing force change rate α within a predetermined range. Even when a current stop period is provided to increase the pressing force change rate α, the welding current may be 8 kA or more from the start of energization to the end of energization, excluding the current stop period. The welding current may be 9 kA or more from the start of energization to the end of energization, or 10 kA or more.
[0043] Next, a resistance spot welding device according to another embodiment of the present invention will be described. As illustrated in Fig. 2, the resistance spot welding device 1 according to this embodiment is a resistance spot welding device for implementing the above-mentioned manufacturing method of the resistance spot welded joint, and includes a pair of electrodes 11, a pressure unit 12 configured to be able to apply a pressure force between the pair of electrodes 11, a welding current control unit 13 configured to be able to pass a welding current between the pair of electrodes 11, a pressure force measuring unit 14 configured to be able to measure the pressure force between the pair of electrodes 11, and a pressure force change rate control unit 15 configured to monitor the time change in the pressure force based on the measurement result of the pressure force measuring unit 14 and control one or both of the pressure unit 12 and the welding current control unit 13 to control the pressure force change rate α to a predetermined threshold value or more. The pressure force may be measured by arranging a load cell or the like above the upper electrode or below the lower electrode.
[0044] There are no particular limitations on the pair of electrodes 11, the pressure unit 12, and the welding current control unit 13, and various ordinary configurations suitable for resistance spot welding of two or more steel sheets A can be applied to these. The welding current control unit 13 may be one built into the resistance spot welding apparatus 1, or may be a control device connected to an external power source.
[0045] The pressure measuring unit 14 is a mechanism capable of measuring the actual pressure applied to the steel sheet A by the pair of electrodes 11, and is, for example, a load cell disposed on the pair of electrodes.
[0046] The pressing force change rate control unit 15 controls the pressing force based on the measurement result of the pressing force measurement unit 14. The means for controlling the pressing force is not particularly limited, and may be configured to be capable of controlling the welding current value and / or the set pressing force, as exemplified above. In this case, the pressing force change rate control unit 15 controls one or both of the pressing unit 12 and the welding current control unit 13. The welding current control unit 13 and the pressing force change rate control unit 15 may be integrated.
[0047] By having the pressing force measuring unit 14 and the pressing force change rate control unit 15, the resistance spot welding apparatus 1 of this embodiment can efficiently carry out a manufacturing method for a resistance spot welded joint that can stably form a spot weld of a predetermined size while suppressing the occurrence of expulsion. EXAMPLES
[0048] The effects of one embodiment of the present invention will be explained more specifically with reference to an example. However, the conditions in the example are merely an example of conditions adopted to confirm the feasibility and effects of the present invention. The present invention is not limited to this example of conditions. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.
[0049] Various resistance spot welded joints were produced by stacking two or more steel plates and resistance spot welding them. The steel plates and welding conditions were as shown in Table 1.
[0050] [Table 1]
[0051] The details of Table 1 are supplemented as follows: Number of steel plates: 2 (both as specified in Table 1) Set pressure: The set pressure at the start of pressure application was as shown in Table 1. Unless otherwise specified in the "Controlled or Uncontrolled" column, the set pressure was kept constant. Welding current value: The welding current value at the start of energization was set to the "set current" shown in Table 1. Unless otherwise specified in the "Controlled or Uncontrolled" column, the welding current value was kept constant. · Control of welding conditions: In some cases, when the rate of change of applied pressure α fell below 1 / 2 of the threshold value (i.e., −1.5 kN / sec), the welding conditions were controlled as described in Table 1. - Rate of change of applied pressure α: In resistance spot welding, the rate of change of applied pressure α varies, but the minimum value of this is defined as the "minimum measured rate of change of applied pressure α min " are listed in Table 1. It should be noted that no particular preliminary resistance spot welding was performed before performing the resistance spot welding under the conditions shown in Table 1. However, as a result of experiments conducted by the present inventors so far, it has already been found that when the tensile strength of the two or more steel sheets is 270 to 2000 MPa and the total thickness of the two or more steel sheets is 1.6 to 5.0 mm, the threshold value of the pressing force change rate α should be -3 kN / sec. Therefore, when performing the resistance spot welding under the conditions shown in Table 1, the threshold value was set to -3 kN / sec. The results of resistance spot welding performed under the conditions shown in Table 1 are shown in Table 2.
[0052] [Table 2]
[0053] The nugget diameters shown in Table 2 are the smallest values among the five nugget diameters obtained by performing five tests under the conditions shown in Table 1. In addition, the welding conditions under which no expulsion occurred after five tests are shown in Table 2 as "Expulsion: None."
[0054] In welding condition No. 1 and welding condition No. 6, no particular control was performed during resistance spot welding, so the rate of change in welding pressure α was below the threshold. In these examples, expulsion occurred. On the other hand, under welding conditions that satisfy the requirements of the present invention, the occurrence of expulsion could be suppressed while maintaining the nugget diameter.
[0055] Welding condition No. 2 and welding condition No. 7 are examples in which the welding current was reduced when it was detected that the rate of change of the applied pressure α fell below 1 / 2 of the threshold value (i.e., -1.5 kN / sec). Ri for welding condition No. 2 was -20%, and Ri for welding condition No. 2 was -18%. Ri and α for these welding conditions min satisfied Equation 2. In welding conditions No. 2 and No. 7, the welding force change rate α was prevented from falling below the threshold value, and the occurrence of expulsion was suppressed.
[0056] Welding condition No. 3 and welding condition No. 8 are examples in which the set pressure is increased when it is detected that the pressure change rate α falls below half the threshold value. The Rf of welding condition No. 3 is 15%, and the Rf of welding condition No. 8 is 36%. The Rf and α in these welding conditions are min satisfied Equation 3. In welding conditions No. 3 and No. 8, the welding force change rate α was prevented from falling below the threshold value, and the occurrence of expulsion was suppressed.
[0057] Welding condition No. 4 and welding condition No. 9 are examples in which, when it was detected that the rate of change in the applied pressure α fell below half the threshold value, the welding current value was decreased and the set applied pressure was increased. The Ri of welding condition No. 4 was -10%, and the Ri of welding condition No. 9 was -9%. The Rf of welding condition No. 4 was 18%, and the Rf of welding condition No. 9 was 14%. The Rf, Ri, and α under these welding conditions min , and β satisfied formulas 4 and 5. Under welding conditions No. 4 and No. 9, the rate of change of pressure α was prevented from falling below the threshold value, and the occurrence of expulsion was suppressed.
[0058] In welding condition No. 5, when it was detected that the rate of change of the welding force α fell below half the threshold, the passage of current was stopped for 60 msec. In welding condition No. 5, it was possible to prevent the rate of change of the welding force α from falling below the threshold, and suppress the occurrence of expulsion. [Explanation of symbols]
[0059] 1 Resistance spot welding equipment 11 Pair of electrodes 12 Pressurizing section 13 Welding current control unit 14 Pressure measurement section 15 Pressure force change rate control section A steel plate
Claims
1. A method for manufacturing a resistance spot welded joint comprising a step of stacking two or more steel plates and resistance spot welding the plates, During the resistance spot welding, a pressing force change rate α (kN / sec) calculated by the following formula 1 is controlled to be equal to or greater than a predetermined threshold value during a period from T1 to the end of current application, The threshold is a negative value. A method for manufacturing resistance spot welded joints. α=(P-P1) / (T-T1): Formula 1 Here, in the formula 1, T is the elapsed time (sec) from the start of the resistance spot welding, P is the welding force (kN) at the time T has elapsed since the start of the resistance spot welding, T1 is the elapsed time (sec) between the point at which the value obtained by differentiating P with respect to T becomes 0 for the second time counted from the point at which current is started in the resistance spot welding, and the start of the resistance spot welding, P1 is the applied pressure (kN) at the time when the time T1 has elapsed from the start of the resistance spot welding.
2. The method for manufacturing the resistance spot welded joint further includes a step of stacking steel plates of the same material as the two or more steel plates and performing preliminary resistance spot welding before the resistance spot welding, The preliminary resistance spot welding is performed a plurality of times while changing the welding current; The threshold value is determined by comparing the pressing force change rate α in the preliminary resistance spot welding in which expulsion occurred with the pressing force change rate α in the preliminary resistance spot welding in which expulsion did not occur. The method for manufacturing a resistance spot welded joint according to claim 1 .
3. The tensile strength of the two or more steel plates is 270 to 2000 MPa, The total thickness of two or more of the steel plates is 1.6 to 5.0 mm, The threshold value is set to -3.5 kN / sec. The method for manufacturing a resistance spot welded joint according to claim 1 .
4. The tensile strength of one or more of the steel plates is 980 to 2000 MPa, The threshold value is set to −3.0 kN / sec.
4. The method for manufacturing a resistance spot welded joint according to claim 1 or 3.
5. When the pressure change rate α falls below half the threshold value, the current flow is stopped for 20 to 160 msec. The method for manufacturing a resistance spot welded joint according to any one of claims 1 to 4.
6. When the pressure change rate α falls below half the threshold value, the welding current value is decreased and / or the set pressure is increased. The method for manufacturing a resistance spot welded joint according to any one of claims 1 to 4.
7. 7. The method for producing a resistance spot welded joint according to claim 6, wherein when the rate of change in welding force α falls below ½ of the threshold value, a current reduction rate Ri of the welding current is set within a range that satisfies the following formula 2. 1.2×(20×α+30)≦Ri≦0.8×(20×α+30): Formula 2 Here, in the formula 2, Ri is a current reduction rate (%) (Ri≦0%) based on the welding current at the start of the current application, α is the rate of change of the pressure.
8. 7. The method for producing a resistance spot welded joint according to claim 6, wherein when the rate of change in pressing force α falls below ½ of the threshold value, a set pressing force increase rate Rf is set within a range that satisfies the following formula 3. 0.8×(-33×α-50)≦Rf≦1.2×(-33×α-50): Formula 3 Here, in the formula 3, Rf is the rate of increase in the set pressure (%) based on the set pressure at the start of pressure application (0%≦Rf), α is the rate of change of the pressure.
9. 7. The method for manufacturing a resistance spot welded joint according to claim 6, wherein when the rate of change of pressing force α falls below ½ of the threshold value, the current reduction rate Ri of the welding current and the set pressing force increase rate Rf are set within ranges that satisfy the following equations 4 and 5. 1.2×β×(20×α+30)≦Ri≦0.8×β×(20×α+30): Formula 4 0.8×(1-β)×(-33×α-50)≦Rf≦1.2×(1-β)×(-33×α-50): Formula 5 Here, in the formula 4 and the formula 5, Ri is a current reduction rate (%) (Ri≦0%) based on the welding current at the start of the current application, β is a constant between 0 and 1, α is the pressure force change rate, Rf is the rate (%) of increase in the set pressure based on the set pressure at the start of pressure application (0%≦Rf).
10. The method for manufacturing a resistance spot welded joint according to any one of claims 1 to 4 and 6 to 9, characterized in that the welding current is 8 kA or more from the start of the resistance spot welding to the end of the current flow.
11. A pair of electrodes; A pressure unit configured to apply a pressure force between the pair of electrodes; a welding current control unit configured to be able to pass a welding current between the pair of electrodes; a pressure measuring unit configured to be able to measure the pressure between the pair of electrodes; a pressing force change rate control unit configured to monitor a change in pressing force over time based on a measurement result of the pressing force measurement unit and to control one or both of the pressing unit and the welding current control unit to control a pressing force change rate α to a predetermined threshold value or more; A resistance spot welding apparatus for carrying out the method for producing a resistance spot welded joint according to any one of claims 1 to 10, comprising:
Citation Information
Patent Citations
Adaptation controlling method in resistance welding
JP1981148481A
Method and device for controlling weld time in resistance welding
JP1983047579A
Method for control and suppression of expulsion and surface flash generation of spot welding
JP1995096376A
Spot weld method
JP2014180699A
Method and apparatus for monitoring and controlling resistance spot welding
US4694135A