Cured film-forming composition, alignment material and retardation material
The cured film-forming composition with specific photoalignment components and polymers addresses solvent resistance and alignment sensitivity issues, enabling efficient and uniform retardation material formation on thin films for 3D displays.
Patent Information
- Application Number
- JP2021522786
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-27
- Filing Date
- 2020-05-26
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-05-26
AI Technical Summary
Existing alignment materials for retardation materials in 3D displays lack sufficient solvent resistance and alignment sensitivity, requiring excessive polarized UV exposure, which reduces orientation sensitivity and efficiency.
A cured film-forming composition containing a low-molecular photoalignment component with specific functional groups and polymers derived from N-alkoxymethyl (meth)acrylamide and N-hydroxyalkyl (meth)acrylamide compounds, along with a crosslinking catalyst, to enhance alignment sensitivity and solvent resistance.
The composition achieves high alignment sensitivity and uniformity with solvent resistance, enabling efficient formation of retardation materials on thin films, protecting film substrates and maintaining adhesion under high-temperature conditions.
Smart Images

Figure 0007569016000001 
Figure 0007569016000002 
Figure 0007569016000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a cured film-forming composition, an alignment material, and a retardation material. [Background technology]
[0002] In the case of a circularly polarized glasses type 3D display, a retardation material is usually arranged on a display element that forms an image, such as a liquid crystal panel. This retardation material has two types of retardation regions with different retardation characteristics arranged regularly, forming a patterned retardation material. In the following, in this specification, such a patterned retardation material that arranges multiple retardation regions with different retardation characteristics is referred to as a patterned retardation material.
[0003] The patterned retardation material can be produced by optically patterning a retardation material made of polymerizable liquid crystal, as disclosed in Patent Document 1, for example. The optical patterning of the retardation material made of polymerizable liquid crystal utilizes a photo-alignment technique known for forming alignment materials for liquid crystal panels. That is, a coating film made of a photo-alignable material is provided on a substrate, and two types of polarized light with different polarization directions are irradiated onto the coating film. Then, a photo-alignment film is obtained as an alignment material in which two types of liquid crystal alignment regions with different liquid crystal alignment control directions are formed. A solution-like retardation material containing polymerizable liquid crystal is applied onto the photo-alignment film to realize the alignment of the polymerizable liquid crystal. Then, the aligned polymerizable liquid crystal is cured to form a patterned retardation material.
[0004] The anti-reflection film of an organic EL display is composed of a linear polarizer and a quarter-wave retardation plate, and converts external light toward the panel surface of the image display panel into linearly polarized light by the linear polarizer, and then into circularly polarized light by the subsequent quarter-wave retardation plate. Here, this circularly polarized external light is reflected by the surface of the image display panel, but the rotation direction of the polarization plane is reversed during this reflection. As a result, this reflected light is converted by the quarter-wave retardation plate into linearly polarized light in the direction that is blocked by the linear polarizer, in the opposite direction to when it arrived, and then is blocked by the subsequent linear polarizer, resulting in significant suppression of emission to the outside.
[0005] Regarding this quarter-wave retardation plate, Patent Document 2 proposes a method of constructing this optical film with reverse dispersion characteristics by combining a half-wave plate and a quarter-wave plate to construct a quarter-wave retardation plate. In this method, an optical film with reverse dispersion characteristics can be constructed using a liquid crystal material with positive dispersion characteristics in a wide wavelength band used for displaying color images.
[0006] Recently, liquid crystal materials having reverse dispersion characteristics have been proposed as liquid crystal materials applicable to the retardation layer (Patent Documents 3 and 4). With such liquid crystal materials having reverse dispersion characteristics, instead of forming a quarter-wave retardation plate from two retardation layers by combining a half-wave plate and a quarter-wave plate, the retardation layer can be formed from a single layer to ensure reverse dispersion characteristics, and thus an optical film capable of ensuring a desired retardation in a wide wavelength band can be realized with a simple configuration.
[0007] An alignment layer is used to align liquid crystals. Methods for forming an alignment layer include, for example, a rubbing method and a photoalignment method. The photoalignment method is useful in that it does not generate static electricity or dust, which are problems with the rubbing method, and it allows quantitative control of the alignment process.
[0008] In forming an alignment material using a photoalignment method, acrylic resins and polyimide resins having photodimerization sites such as cinnamoyl groups and chalcone groups in the side chains are known as photoalignment materials that can be used. It has been reported that these resins exhibit the ability to control the alignment of liquid crystals (hereinafter, also referred to as liquid crystal alignment) by irradiating them with polarized UV light (see Patent Documents 5 to 7).
[0009] In addition to the liquid crystal alignment ability, the alignment layer is required to have solvent resistance. For example, the alignment layer may be exposed to heat or a solvent during the manufacturing process of the retardation material. If the alignment layer is exposed to a solvent, the liquid crystal alignment ability may be significantly reduced.
[0010] Therefore, for example, Patent Document 8 proposes a liquid crystal aligning agent containing a polymer component having a structure capable of undergoing a crosslinking reaction by light and a structure that crosslinks by heat, in order to obtain stable liquid crystal aligning ability, and a liquid crystal aligning agent containing a polymer component having a structure capable of undergoing a crosslinking reaction by light and a compound having a structure that crosslinks by heat. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2005-49865 A [Patent Document 2] Japanese Patent Application Publication No. 10-68816 [Patent Document 3] U.S. Patent No. 8,119,026 [Patent Document 4] JP 2009-179563 A [Patent Document 5] Patent No. 3611342 [Patent Document 6] JP 2009-058584 A [Patent Document 7] Special Publication No. 2001-517719 [Patent Document 8] Patent No. 4207430 Summary of the Invention [Problem to be solved by the invention]
[0012] As described above, the retardation material is formed by laminating a layer of hardened polymerizable liquid crystal on a photo-alignment film, which is an alignment material. Therefore, there is a need to develop an alignment material that can achieve both excellent liquid crystal alignment properties and solvent resistance.
[0013] However, according to the study by the present inventors, it has been found that acrylic resins having photodimerization sites such as cinnamoyl groups or chalcone groups in the side chains do not provide sufficient characteristics when used to form retardation materials. In particular, in order to form an alignment material by irradiating these resins with polarized UV light and then use the alignment material to produce a retardation material made of polymerizable liquid crystal, a large amount of polarized UV exposure is required. The amount of polarized UV exposure is sufficient to align liquid crystals for normal liquid crystal panels (for example, 30 mJ / cm2). 2 degree.) will be significantly more.
[0014] The reason for the large amount of polarized UV exposure is that, unlike liquid crystals for liquid crystal panels, when forming retardation materials, polymerizable liquid crystals are used in the form of a solution and are applied onto the alignment material.
[0015] When an alignment material is formed using an acrylic resin or the like having a photodimerization site such as a cinnamoyl group in the side chain to align a polymerizable liquid crystal, the acrylic resin or the like is photocrosslinked by a photodimerization reaction. Then, it is necessary to perform polarized light irradiation with a large amount of exposure until resistance to the polymerizable liquid crystal solution is developed. In order to align the liquid crystal of a liquid crystal panel, it is usually sufficient to perform a dimerization reaction only on the surface of the photoalignment material. However, when using a conventional material such as the above-mentioned acrylic resin to develop solvent resistance in an alignment material, it is necessary to cause the reaction to extend to the inside of the alignment material, which requires a larger amount of exposure. As a result, there is a problem that the alignment sensitivity of the conventional material becomes very small.
[0016] In addition, a technique of adding a crosslinking agent to the resin, which is the conventional material, is known to impart such solvent resistance. However, it is known that after the thermal curing reaction using the crosslinking agent, a three-dimensional structure is formed inside the formed coating film, and the photoreactivity decreases. In other words, the orientation sensitivity is greatly reduced, and the desired effect cannot be obtained even if a crosslinking agent is added to the conventional material.
[0017] Furthermore, various organic solvents are used in liquid crystal inks, and films with low resistance to organic solvents may be used as substrates, so alignment films with high solvent resistance are required to protect the films.
[0018] In view of the above, there is a demand for a photo-alignment technique that can improve the alignment sensitivity of an alignment material and reduce the amount of polarized UV exposure, and a cured film-forming composition that can be used as a liquid crystal alignment agent for photo-alignment used in forming the alignment material. Also, there is a demand for a technique that can provide a retardation material with high efficiency.
[0019] The object of the present invention has been achieved based on the above findings and study results. That is, the object of the present invention is to provide a cured film-forming composition that can be used as a liquid crystal alignment agent for photo-alignment to provide an alignment material that has excellent alignment sensitivity, excellent alignment uniformity, and resistance to a solvent in a liquid crystal solution even in a thin film, and can also function as a protective layer to protect a film substrate.
[0020] Other objects and advantages of the present invention will become apparent from the following description. [Means for solving the problem]
[0021] The first aspect of the present invention is (A) a compound having a photoalignable group and a substituent selected from the group consisting of a hydroxyl group, a carboxyl group, and an amino group; (B) a polymer obtained by polymerizing a monomer containing at least an N-alkoxymethyl(meth)acrylamide compound, and (C) The present invention relates to a cured film-forming composition comprising a polymer obtained by polymerizing a monomer containing at least an N-hydroxyalkyl (meth)acrylamide compound.
[0022] In the first aspect of the present invention, the photoalignable group of the component (A) is preferably a functional group having a structure that undergoes photodimerization or photoisomerization. In the first aspect of the present invention, the photoalignable group of the component (A) is preferably a cinnamoyl group. In the first aspect of the present invention, the photoalignable group of the component (A) is preferably a group having an azobenzene structure. In the first aspect of the present invention, it is preferable to further contain a crosslinking catalyst as the component (D). In the first aspect of the present invention, it is preferable to further contain an adhesion improving component as the component (E). In the first embodiment of the present invention, the total amount of the components (B) and (C) is preferably 100 to 3,000 parts by mass based on 100 parts by mass of the component (A). In the first embodiment of the present invention, the mass ratio of the component (B) to the component (C) is preferably 1:99 to 99:1. In the first embodiment of the present invention, it is preferable to contain 0.01 to 10 parts by mass of the component (D) based on 100 parts by mass of the total amount of the components (B) and (C).
[0023] A second aspect of the present invention relates to an alignment material obtained by using the cured film-forming composition according to the first aspect of the present invention.
[0024] A third aspect of the present invention relates to a retardation material which is formed using a cured film obtained from the cured film-forming composition according to the first aspect of the present invention. Effect of the Invention
[0025] According to a first aspect of the present invention, it is possible to provide a cured film-forming composition for providing an alignment material that has excellent alignment sensitivity, excellent alignment uniformity, and even when it is a thin film, has resistance to a solvent in a liquid crystal solution, and can also function as a protective layer for protecting a film substrate.
[0026] According to the second aspect of the present invention, an alignment material can be provided which has excellent alignment sensitivity, excellent alignment uniformity, and even when thin, is resistant to the solvent in the liquid crystal solution and can also function as a protective layer to protect the film substrate.
[0027] According to the third aspect of the present invention, it is possible to provide a retardation material which can be formed with high efficiency even on a film substrate and which allows optical patterning. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] <Cured film forming composition> The cured film-forming composition of the present invention contains a compound having a photo-alignable group and one substituent selected from the group consisting of a hydroxyl group, a carboxyl group, and an amino group (hereinafter also referred to as a "low-molecular photo-alignment component") as component (A), a polymer obtained by polymerizing a monomer containing at least an N-alkoxymethyl(meth)acrylamide compound as component (B), and a polymer obtained by polymerizing a monomer containing at least an N-hydroxyalkyl(meth)acrylamide compound as component (C). In addition to components (A), (B), and (C), the cured film-forming composition of the present invention may further contain a crosslinking catalyst as component (D) and a component that improves the adhesion of the cured film as component (E). Other additives may be contained as long as they do not impair the effects of the present invention.
[0029] Each component will be described in detail below. <Component (A)> The component (A) contained in the cured film-forming composition of the present invention is the above-mentioned low molecular weight photoalignment component.
[0030] The low molecular weight photo-alignment component (A) is a compound having a photo-alignment group and one substituent selected from the group consisting of a hydroxyl group, a carboxyl group, and an amino group. In the compound having a photo-alignment group and one substituent selected from the group consisting of a hydroxyl group, a carboxyl group, and an amino group, as described above, the photo-alignment group reacts with light to form a hydrophobic photo-alignment portion, and the hydroxyl group or the like forms a hydrophilic heat-reactive portion. In the present invention, the photoalignable group refers to a functional group at a structural site that is photodimerized or photoisomerized.
[0031] The structural portion that undergoes photodimerization is a portion that forms a dimer by irradiation with light, and specific examples thereof include a cinnamoyl group, a chalcone group, a coumarin group, and an anthracene group. Of these, a cinnamoyl group is preferred, which has high transparency in the visible light region and photodimerization reactivity. The structural portion that undergoes photoisomerization refers to a structural portion that changes into a cis form and a trans form by irradiation with light, and specific examples thereof include a portion consisting of an azobenzene structure, a stilbene structure, and the like. Of these, an azobenzene structure is preferred because of its high reactivity. The compound having a photoalignment group and a hydroxyl group is represented by the following formula, for example.
[0032] [ka]
[0033] In the formulas [A1] to [A5], A 1 and A 2 each independently represents a hydrogen atom or a methyl group; X 1 represents a divalent group formed by bonding, via one or more bonds selected from a single bond, an ether bond, an ester bond, an amide bond, a urethane bond, an amino bond, or a combination thereof, one to three groups selected from an alkylene group having 1 to 18 carbon atoms, a phenylene group, a biphenylene group, or a combination thereof. X 2 represents a hydrogen atom, a halogen atom, a cyano group, an alkyl group having 1 to 18 carbon atoms, a phenyl group, a biphenyl group, or a cyclohexyl group. In this case, the alkyl group having 1 to 18 carbon atoms, the phenyl group, the biphenyl group, and the cyclohexyl group may be bonded to the benzene ring via a covalent bond, an ether bond, an ester bond, an amide bond, or a urea bond. 5 represents a hydroxyl group, a carboxyl group, an amino group, or an alkoxysilyl group. X represents a single bond, an oxygen atom, or a sulfur atom. X 6 represents a hydroxy group, a mercapto group, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, a phenyl group, a phenoxy group, or a biphenoxy group. 7represents a single bond, an alkylene group having 1 to 20 carbon atoms, a divalent group obtained by removing two hydrogen atoms from an aromatic ring, or a divalent group obtained by removing two hydrogen atoms from an aliphatic ring, where the alkylene group having 1 to 20 carbon atoms may be branched or linear.
[0034] In these substituents, the phenylene group, the phenyl group, the biphenylene group, the biphenyl group, the phenoxy group and the biphenoxy group may be substituted with one or more identical or different substituents selected from an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a halogen atom, a trifluoromethyl group and a cyano group.
[0035] In the above formula, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 and R 8 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a halogen atom, a trifluoromethyl group, or a cyano group.
[0036] Examples of the alkyl group having 1 to 18 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl-n-propyl group, an n-hexyl group, a 1-methyl-n-pentyl group, a 2- Methyl-n-pentyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1 -ethyl-2-methyl-n-propyl, n-heptyl, 1-methyl-n-hexyl, 2-methyl-n-hexyl, 3-methyl-n-hexyl, 1,1-dimethyl-n-pentyl, 1,2-dimethyl-n-pentyl, 1,3-dimethyl-n-pentyl, 2,2-dimethyl-n-pentyl, 2,3-dimethyl-n-pentyl, 3,3-dimethyl-n-pentyl, 1-ethyl-n-pentyl, 2-ethyl-n-pentyl, 3-ethyl-n-pentyl, 1-methyl-1-ethyl n-butyl, 1-methyl-2-ethyl-n-butyl, 1-ethyl-2-methyl-n-butyl, 2-methyl-2-ethyl-n-butyl, 2-ethyl-3-methyl-n-butyl, n-octyl, 1-methyl-n-heptyl, 2-methyl-n-heptyl, 3-methyl-n-heptyl, 1,1-dimethyl-n-hexyl, 1,2-dimethyl-n-hexyl, 1,3-dimethyl-n-hexyl, 2,2-dimethyl-n-hexyl, 2,3-dimethyl-n-hexyl, 3,Examples of the alkyl group include 3-dimethyl-n-hexyl group, 1-ethyl-n-hexyl group, 2-ethyl-n-hexyl group, 3-ethyl-n-hexyl group, 1-methyl-1-ethyl-n-pentyl group, 1-methyl-2-ethyl-n-pentyl group, 1-methyl-3-ethyl-n-pentyl group, 2-methyl-2-ethyl-n-pentyl group, 2-methyl-3-ethyl-n-pentyl group, 3-methyl-3-ethyl-n-pentyl group, n-nonyl group, n-decyl group, n-undecyl group, n-dodecyl group, n-tridecyl group, n-tetradecyl group, n-pentadecyl group, n-hexadecyl group, n-heptadecyl group, and n-octadecyl group. Examples of the alkylene group having 1 to 18 carbon atoms include divalent groups obtained by removing one hydrogen atom from the alkyl groups listed above. Examples of the alkyl group having 1 to 4 carbon atoms include groups having the corresponding number of carbon atoms among the groups listed above. The alkoxy group having 1 to 10 carbon atoms, the alkoxy group having 1 to 4 carbon atoms, and the alkylthio group having 1 to 10 carbon atoms include groups having the corresponding number of carbon atoms among the above-mentioned alkyl groups which have been oxylated or thiolated. Examples of the alkylene group having 1 to 20 carbon atoms include the above alkyl groups as well as divalent groups obtained by removing one hydrogen atom from an alkyl group having 1 to 20 carbon atoms, such as an n-nonadecyl group or an n-eicosyl group.
[0037] Specific examples of the compound having a photoalignable group and a hydroxy group, which is the component (A), include, for example, 4-(8-hydroxyoctyloxy)cinnamic acid methyl ester, 4-(6-hydroxyhexyloxy)cinnamic acid methyl ester, 4-(4-hydroxybutyloxy)cinnamic acid methyl ester, 4-(3-hydroxypropyloxy)cinnamic acid methyl ester, 4-(2-hydroxyethyloxy)cinnamic acid methyl ester, 4-hydroxymethyloxycinnamic acid methyl ester, 4-hydroxycinnamic acid methyl ester, 4-(8-hydroxyoctyloxy)cinnamic acid methyl ester, 4-hydroxycinnamic acid methyl ester, 4-hydroxyoctyloxy ... 4-(6-hydroxyhexyloxy)cinnamic acid ethyl ester, 4-(4-hydroxybutyloxy)cinnamic acid ethyl ester, 4-(3-hydroxypropyloxy)cinnamic acid ethyl ester, 4-(2-hydroxyethyloxy)cinnamic acid ethyl ester, 4-hydroxymethyloxycinnamic acid ethyl ester, 4-hydroxycinnamic acid ethyl ester, 4-(8-hydroxyoctyloxy)cinnamic acid phenyl ester, 4-(6-hydroxyhexyloxy)cinnamic acid phenyl ester, 4-(4-hydroxy butyloxy)cinnamic acid phenyl ester, 4-(3-hydroxypropyloxy)cinnamic acid phenyl ester, 4-(2-hydroxyethyloxy)cinnamic acid phenyl ester, 4-hydroxymethyloxycinnamic acid phenyl ester, 4-hydroxycinnamic acid phenyl ester, 4-(8-hydroxyoctyloxy)cinnamic acid biphenyl ester, 4-(6-hydroxyhexyloxy)cinnamic acid biphenyl ester, 4-(4-hydroxybutyloxy)cinnamic acid biphenyl ester, 4-(3-hydroxypropyloxy)cinnamic acid biphenyl ester ester, 4-(2-hydroxyethyloxy)cinnamic acid biphenyl ester, 4-hydroxymethyloxycinnamic acid biphenyl ester, 4-hydroxycinnamic acid biphenyl ester, cinnamic acid 8-hydroxyoctyl ester, cinnamic acid 6-hydroxyhexyl ester, cinnamic acid 4-hydroxybutyl ester, cinnamic acid 3-hydroxypropyl ester, cinnamic acid 2-hydroxyethyl ester, cinnamic acid hydroxymethyl ester, 4-(8-hydroxyoctyloxy)azobenzene, 4-(6-hydroxyhexyloxy)azobenzene,4-(4-hydroxybutyloxy)azobenzene, 4-(3-hydroxypropyloxy)azobenzene, 4-(2-hydroxyethyloxy)azobenzene, 4-hydroxymethyloxyazobenzene, 4-hydroxyazobenzene, 4-(8-hydroxyoctyloxy)chalcone, 4-(6-hydroxyhexyloxy)chalcone, 4-(4-hydroxybutyloxy)chalcone, 4-(3-hydroxypropyloxy)chalcone, 4-(2-hydroxyethyloxy)chalcone, 4-hydroxymethyloxychalcone, 4-hydroxychalcone, 4'-(8-hydroxyoctyloxy)chalcone, 4'-(6-hydroxyhexyloxy)chalcone, 4'-(4-hydroxybutyloxy)chalcone, 4'-(3-hydroxypropyloxy)chalcone coumarin, 4'-(2-hydroxyethyloxy) chalcone, 4'-hydroxymethyloxy chalcone, 4'-hydroxychalcone, 7-(8-hydroxyoctyloxy) coumarin, 7-(6-hydroxyhexyloxy) coumarin, 7-(4-hydroxybutyloxy) coumarin, 7-(3-hydroxypropyloxy) coumarin, 7-(2-hydroxyethyloxy) coumarin, 7-hydroxymethyloxy coumarin, 7-hydroxycoumarin, 6-hydroxyoctyloxy coumarin, 6-hydroxyhexyloxy coumarin, 6-(4-hydroxybutyloxy) coumarin, 6-(3-hydroxypropyloxy) coumarin, 6-(2-hydroxyethyloxy) coumarin, 6-hydroxymethyloxy coumarin, and 6-hydroxycoumarin.
[0038] Specific examples of compounds having a photoalignable group and a carboxyl group include cinnamic acid, ferulic acid, 4-nitrocinnamic acid, 4-methoxycinnamic acid, 3,4-dimethoxycinnamic acid, coumarin-3-carboxylic acid, and 4-(dimethylamino)cinnamic acid. Specific examples of the compound having a photoalignable group and an amino group include methyl 4-aminocinnamate, ethyl 4-aminocinnamate, methyl 3-aminocinnamate, and ethyl 3-aminocinnamate. The low molecular weight photoalignment component (A) may be specifically exemplified by those mentioned above, but is not limited thereto.
[0039] In addition, when the low molecular weight photo-alignment component (A) is a compound having a photo-alignment group and a hydroxyl group, it is possible to use a compound having two or more photo-alignment groups and / or two or more hydroxyl groups in the molecule as the component (A). Specifically, it is possible to use a compound having one hydroxyl group and two or more photo-alignment groups in the molecule, a compound having one photo-alignment group and two or more hydroxyl groups in the molecule, or a compound having two or more photo-alignment groups and two or more hydroxyl groups in the molecule as the component (A). For example, as an example of a compound having two or more photo-alignment groups and two or more hydroxyl groups in the molecule, a compound represented by the following formula can be used. [ka]
[0040] By appropriately selecting such a compound, it is possible to control the molecular weight of the low molecular weight photo-alignment component (A) to be increased. As a result, as described below, when the low molecular weight photo-alignment component (A) and the polymer (B) and the polymer (C) undergo a thermal reaction, the low molecular weight photo-alignment component (A) can be suppressed from sublimating. And, the cured film-forming composition of the present invention can form an alignment material with high photoreaction efficiency as a cured film.
[0041] The compound of component (A) in the cured film-forming composition of the present invention may be a mixture of multiple compounds having a photoalignable group and one substituent selected from the group consisting of a hydroxy group, a carboxyl group, and an amino group.
[0042] <(B) component> The component (B) contained in the cured film-forming composition of the present invention is a polymer obtained by polymerizing a monomer containing at least an N-alkoxymethyl(meth)acrylamide compound. Note that N-alkoxymethyl(meth)acrylamide means both N-alkoxymethylacrylamide and N-alkoxymethylmethacrylamide.
[0043] Such polymers include polymers obtained by polymerizing N-alkoxymethyl(meth)acrylamide compounds alone or with copolymerizable monomers. Examples of such polymers include poly(N-butoxymethylacrylamide), poly(N-ethoxymethylacrylamide), poly(N-methoxymethylacrylamide), copolymers of N-butoxymethylacrylamide and styrene, copolymers of N-butoxymethylacrylamide and methyl methacrylate, copolymers of N-ethoxymethylmethacrylamide and benzyl methacrylate, and copolymers of N-butoxymethylacrylamide, benzyl methacrylate, and 2-hydroxypropyl methacrylate.
[0044] The method for obtaining the polymer, which is the component (B) used in the present invention, is not particularly limited, but for example, it can be obtained by carrying out a polymerization reaction at a temperature of 50 to 110° C. in a solvent in which an N-alkoxymethyl(meth)acrylamide compound, a copolymerizable monomer if desired, and a polymerization initiator are coexisting. The solvent used in this case is not particularly limited as long as it dissolves the N-alkoxymethyl(meth)acrylamide compound, a copolymerizable monomer if desired, and a polymerization initiator. Specific examples are described in the section <Solvent> below. The polymer obtained by the above method is usually in the form of a solution dissolved in a solvent.
[0045] Alternatively, the polymer solution obtained by the above method may be poured into stirred diethyl ether or water to cause precipitation, and the resulting precipitate may be filtered and washed, and then dried at room temperature or by heating under normal or reduced pressure to obtain a polymer powder. By the above operation, the polymerization initiator and unreacted monomers coexisting with the polymer may be removed, and as a result, a purified polymer powder may be obtained. If the polymer cannot be sufficiently purified by one operation, the obtained powder may be redissolved in a solvent and the above operation may be repeated.
[0046] In the present invention, the polymer (B) may be used in the form of a powder, or in the form of a solution obtained by redissolving a purified powder in a solvent described below.
[0047] In the present invention, the polymer that is the component (B) may be a mixture of multiple types of polymers.
[0048] In the present invention, when the above-mentioned copolymerizable monomer is used in producing the polymer of component (B), the amount of the copolymerizable monomer used is preferably 1 mol % to 200 mol %, more preferably 10 mol % to 100 mol %, based on the total moles of the monomers used in producing the polymer of component (B).
[0049] The weight average molecular weight of the polymer that is component (B) is from 1,000 to 500,000, preferably from 2,000 to 200,000, more preferably from 3,000 to 150,000, and further preferably from 3,000 to 50,000. The weight average molecular weight is a value obtained by gel permeation chromatography (GPC) using polystyrene as a standard sample.
[0050] These polymers of component (B) can be used alone or in combination of two or more kinds.
[0051] <(C) component> The component (C) is a polymer obtained by polymerizing a monomer containing at least an N-hydroxyalkyl(meth)acrylamide compound. Note that N-hydroxyalkyl(meth)acrylamide refers to both N-hydroxyalkylacrylamide and N-hydroxyalkylmethacrylamide.
[0052] When the composition of the present invention is formed into a coating film and then heat cured, the N-alkoxymethyl groups of component (B) react with the hydroxyl groups of component (C) to form bonds, which strengthens the coating film and provides it with solvent resistance.
[0053] Examples of the N-hydroxyalkyl(meth)acrylamide compound include N-(2-hydroxyethyl)acrylamide, N-(2-hydroxyethyl)methacrylamide, N-(2-hydroxypropyl)acrylamide, N-(2-hydroxypropyl)methacrylamide, N-(4-hydroxybutyl)acrylamide, N-(4-hydroxybutyl)methacrylamide, N-(2,3-dihydroxypropyl)acrylamide, and N-(2,3-dihydroxypropyl)methacrylamide.
[0054] In the present invention, when producing the polymer of component (C), monomers other than the above-mentioned N-hydroxyalkyl(meth)acrylamide compounds (hereinafter also referred to as "other monomers") may be copolymerized. In the present invention, when other monomers are used in producing the polymer of component (C), the amount of the other monomers used is preferably 30 mol % to 90 mol %, more preferably 30 mol % to 70 mol %, based on the total number of moles of the monomers used in producing the polymer of component (C).
[0055] Examples of the other monomers include industrially available monomers capable of undergoing radical polymerization reaction.
[0056] Specific examples of the other monomers include unsaturated carboxylic acids, acrylic acid ester compounds, methacrylic acid ester compounds, amide group-containing monomers, maleimide compounds, acrylonitrile, maleic anhydride, styrene compounds, and vinyl compounds.
[0057] Specific examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, itaconic acid, maleic acid, and fumaric acid.
[0058] Examples of the acrylic acid ester compound include methyl acrylate, ethyl acrylate, isopropyl acrylate, benzyl acrylate, naphthyl acrylate, anthryl acrylate, anthryl methyl acrylate, phenyl acrylate, 2,2,2-trifluoroethyl acrylate, tert-butyl acrylate, cyclohexyl acrylate, isobornyl acrylate, 2-methoxyethyl acrylate, methoxytriethylene glycol acrylate, 2-ethoxyethyl acrylate, tetrahydrofurfuryl acrylate, 3-methoxybutyl acrylate, 2-methyl-2-adamantyl acrylate, 2-propanol, 2-methyl- ... Examples of the acryloyloxy-2-adamantyl acrylate include 8-methyl-8-tricyclodecyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 2,3-dihydroxypropyl acrylate, diethylene glycol monoacrylate, caprolactone 2-(acryloyloxy)ethyl ester, poly(ethylene glycol) ethyl ether acrylate, 5-acryloyloxy-6-hydroxynorbornene-2-carboxylic-6-lactone, acryloylethyl isocyanate, 8-ethyl-8-tricyclodecyl acrylate, and glycidyl acrylate.
[0059] Examples of the methacrylic acid ester compound include methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, benzyl methacrylate, naphthyl methacrylate, anthryl methacrylate, anthryl methyl methacrylate, phenyl methacrylate, 2,2,2-trifluoroethyl methacrylate, tert-butyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, 2-methoxyethyl methacrylate, methoxytriethylene glycol methacrylate, 2-ethoxyethyl methacrylate, tetrahydrofurfuryl methacrylate, 3-methoxybutyl methacrylate, 2-methyl-2-adamantyl methacrylate, γ-butyrolactone ... methacryloyloxy, 2-propyl-2-adamantyl methacrylate, 8-methyl-8-tricyclodecyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 4-hydroxybutyl methacrylate, 2,3-dihydroxypropyl methacrylate, diethylene glycol monomethacrylate, caprolactone 2-(methacryloyloxy)ethyl ester, poly(ethylene glycol) ethyl ether methacrylate, 5-methacryloyloxy-6-hydroxynorbornene-2-carboxylic-6-lactone, methacryloylethyl isocyanate, 8-ethyl-8-tricyclodecyl methacrylate, and glycidyl methacrylate.
[0060] Examples of the amide group-containing monomer include N-vinylpyrrolidone, N-vinylformamide, N-vinylacetamide, N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-butyl(meth)acrylamide, N-isobutyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-octyl(meth)acrylamide, N-(methoxymethyl)(meth)acrylamide, N-(methoxybutyl)(meth)acrylamide, N-(ethoxymethyl)(meth)acrylamide, N-(butoxymethyl)(meth)acrylamide, N-(isobutoxymethyl)(meth)acrylamide, N-(isobutoxyethyl)(meth)acrylamide, N-vinylphthalimide, and N-vinylsuccinimide.
[0061] Examples of the vinyl compound include vinyl ether, methyl vinyl ether, benzyl vinyl ether, vinyl naphthalene, vinyl anthracene, vinyl biphenyl, vinyl carbazole, 2-hydroxyethyl vinyl ether, phenyl vinyl ether, and propyl vinyl ether.
[0062] Examples of the styrene compound include styrene, methylstyrene, chlorostyrene, and bromostyrene.
[0063] Examples of the maleimide compound include maleimide, N-methylmaleimide, N-phenylmaleimide, and N-cyclohexylmaleimide.
[0064] The acrylonitrile compound includes, for example, acrylonitrile.
[0065] The method for obtaining the polymer, component (C) used in the present invention, is not particularly limited. However, in the method for producing the polymer, component (B), an N-hydroxyalkyl(meth)acrylamide compound may be used instead of an N-alkoxymethyl(meth)acrylamide compound.
[0066] The weight average molecular weight of the polymer that is component (C) is from 1,000 to 500,000, preferably from 2,000 to 200,000, more preferably from 3,000 to 150,000, and further preferably from 3,000 to 100,000. The weight average molecular weight is a value obtained by gel permeation chromatography (GPC) using polystyrene as a standard sample.
[0067] These polymers of component (C) can be used alone or in combination of two or more kinds.
[0068] The content of the polymer as component (B) and the polymer as component (C) in the cured film-forming composition of the present invention is preferably 100 to 3,000 parts by mass, more preferably 200 to 2,500 parts by mass, and particularly preferably 300 to 2,000 parts by mass in total, based on 100 parts by mass of component (A).
[0069] Furthermore, the mass ratio of the component (B) to the component (C) is preferably from 1:99 to 99:1, more preferably from 5:95 to 95:5, and particularly preferably from 10:90 to 90:10.
[0070] <(D) component> The cured film-forming composition of the present invention may further contain a crosslinking catalyst as a component (D) in addition to the components (A), (B) and (C). The crosslinking catalyst (D) may be, for example, an acid or a thermal acid generator. This component (D) is effective in accelerating the thermal curing reaction of the cured film-forming composition of the present invention.
[0071] The acid may be a sulfonic acid group-containing compound, hydrochloric acid or a salt thereof, etc. The thermal acid generator is not particularly limited as long as it is a compound that is thermally decomposed during pre-baking or post-baking to generate an acid, i.e., a compound that is thermally decomposed at a temperature of 80° C. to 250° C. to generate an acid. Examples of the acid include hydrochloric acid or a salt thereof; sulfonic acids such as methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, pentanesulfonic acid, octane sulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, camphorsulfonic acid, trifluoromethanesulfonic acid, p-phenolsulfonic acid, 2-naphthalenesulfonic acid, mesitylenesulfonic acid, p-xylene-2-sulfonic acid, m-xylene-2-sulfonic acid, 4-ethylbenzenesulfonic acid, 1H,1H,2H,2H-perfluorooctane sulfonic acid, perfluoro(2-ethoxyethane)sulfonic acid, pentafluoroethanesulfonic acid, nonafluorobutane-1-sulfonic acid, and dodecylbenzenesulfonic acid, or hydrates or salts thereof. Examples of the compound that generates an acid by heat include bis(tosyloxy)ethane, bis(tosyloxy)propane, bis(tosyloxy)butane, p-nitrobenzyl tosylate, o-nitrobenzyl tosylate, 1,2,3-phenylene tris(methylsulfonate), p-toluenesulfonic acid pyridinium salt, p-toluenesulfonic acid morphonium salt, p-toluenesulfonic acid ethyl ester, p-toluenesulfonic acid propyl ester, p-toluenesulfonic acid butyl ester, p-toluenesulfonic acid isobutyl ester, p-toluenesulfonic acid methyl ester, p-toluenesulfonic acid phenethyl ester, cyanomethyl p-toluenesulfonate, 2,2,2-trifluoroethyl p-toluenesulfonate, 2-hydroxybutyl p-toluenesulfonate, N-ethyl-p-toluenesulfonamide, and compounds represented by the following formula:
[0072] [ka]
[0073] [ka]
[0074] [ka]
[0075] [ka]
[0076] [ka]
[0077] [ka]
[0078] The content of the (D) component in the cured film-forming composition of the present invention is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 6 parts by mass, and even more preferably 0.5 to 5 parts by mass, based on 100 parts by mass of the total amount of the polymer of the (B) component and the polymer of the (C) component. By making the content of the (D) component 0.01 parts by mass or more, sufficient thermosetting properties and solvent resistance can be imparted, and further, high sensitivity to light irradiation can be imparted. However, if it is more than 10 parts by mass, the storage stability of the composition may decrease.
[0079] <(E) component> The cured film-forming composition of the present invention may also contain, as the component (E), a component that improves the adhesion of the cured film to be formed (hereinafter also referred to as an adhesion improving component).
[0080] The adhesion improving component (E) can link the polymerizable functional group of the polymerizable liquid crystal and the crosslinking reaction site of the alignment material by a covalent bond so that the adhesion between the alignment material obtained from the cured film-forming composition of the present invention and the polymerizable liquid crystal layer is improved. As a result, the retardation material of the present embodiment, which is obtained by laminating the cured polymerizable liquid crystal on the alignment material of the present embodiment, can maintain strong adhesion even under high temperature and high temperature conditions, and can show high durability against peeling, etc.
[0081] The component (E) is preferably a monomer or polymer having a group selected from a hydroxy group and an N-alkoxymethyl group, and a polymerizable group. Examples of such component (E) include a compound having a hydroxy group and a (meth)acrylic group, a compound having an N-alkoxymethyl group and a (meth)acrylic group, a polymer having an N-alkoxymethyl group and a (meth)acrylic group, etc. Specific examples of each are shown below.
[0082] An example of the component (E) is a polyfunctional acrylate containing a hydroxy group (hereinafter, also referred to as a hydroxy group-containing polyfunctional acrylate). Examples of the hydroxyl group-containing polyfunctional acrylate that is the component (E) include pentaerythritol triacrylate and dipentaerythritol pentaacrylate.
[0083] An example of the component (E) is a compound having one (meth)acryl group and one or more hydroxy groups.
[0084] Furthermore, examples of the compound of component (E) include compounds having at least one polymerizable group containing a C═C double bond and at least one N-alkoxymethyl group in one molecule.
[0085] Examples of the polymerizable group containing a C=C double bond include an acrylic group, a methacrylic group, a vinyl group, an allyl group, and a maleimide group.
[0086] A preferred example of the compound having at least one polymerizable group containing a C═C double bond and at least one N-alkoxymethyl group in one molecule is a compound represented by the following formula (X1). [ka] (In the formula, R 31 represents a hydrogen atom or a methyl group, R 32 represents a hydrogen atom or a linear or branched alkyl group having 1 to 10 carbon atoms.
[0087] Examples of the alkyl group having 1 to 10 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl-n-propyl group, an n-hexyl group, a 1-methyl-n-pentyl group, a 2- Methyl-n-pentyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1 -ethyl-2-methyl-n-propyl, n-heptyl, 1-methyl-n-hexyl, 2-methyl-n-hexyl, 3-methyl-n-hexyl, 1,1-dimethyl-n-pentyl, 1,2-dimethyl-n-pentyl, 1,3-dimethyl-n-pentyl, 2,2-dimethyl-n-pentyl, 2,3-dimethyl-n-pentyl, 3,3-dimethyl-n-pentyl, 1-ethyl-n-pentyl, 2-ethyl-n-pentyl, 3-ethyl-n-pentyl, 1-methyl-1-ethyl n-butyl, 1-methyl-2-ethyl-n-butyl, 1-ethyl-2-methyl-n-butyl, 2-methyl-2-ethyl-n-butyl, 2-ethyl-3-methyl-n-butyl, n-octyl, 1-methyl-n-heptyl, 2-methyl-n-heptyl, 3-methyl-n-heptyl, 1,1-dimethyl-n-hexyl, 1,2-dimethyl-n-hexyl, 1,3-dimethyl-n-hexyl, 2,2-dimethyl-n-hexyl, 2,3-dimethyl-n-hexyl, 3,Examples of the alkyl group include 3-dimethyl-n-hexyl group, 1-ethyl-n-hexyl group, 2-ethyl-n-hexyl group, 3-ethyl-n-hexyl group, 1-methyl-1-ethyl-n-pentyl group, 1-methyl-2-ethyl-n-pentyl group, 1-methyl-3-ethyl-n-pentyl group, 2-methyl-2-ethyl-n-pentyl group, 2-methyl-3-ethyl-n-pentyl group, 3-methyl-3-ethyl-n-pentyl group, n-nonyl group, and n-decyl group.
[0088] Specific examples of the compound represented by the above formula (X1) include acrylamide compounds or methacrylamide compounds substituted with a hydroxymethyl group or an alkoxymethyl group, such as N-hydroxymethyl(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-ethoxymethyl(meth)acrylamide, and N-butoxymethyl(meth)acrylamide, where (meth)acrylamide means both methacrylamide and acrylamide.
[0089] Preferred examples of the compound having a polymerizable group containing a C═C double bond and an N-alkoxymethyl group as the component (E) include the following compounds. [ka]
[0090] The content of the component (E) in the cured film-forming composition of the present invention is preferably 1 part by mass to 100 parts by mass, and more preferably 5 parts by mass to 70 parts by mass, based on 100 parts by mass of the low molecular weight photoalignment component which is the component (A).
[0091] <Solvent> The cured film-forming composition of the present invention is mainly used in a state of solution dissolved in a solvent. The solvent used in this case is not particularly limited in type and structure, as long as it can dissolve the components (A), (B) and (C), and optionally the components (D) and (E) and / or other additives described below.
[0092] Specific examples of the solvent include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-butanone, 3-methyl-2-pentanone, 2 ... Examples of the solvent include pentanone, 2-heptanone, γ-butyrolactone, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone. These solvents can be used alone or in combination of two or more.
[0093] <Other additives> Furthermore, the cured film-forming composition of the present invention may contain, as necessary, a sensitizer, a silane coupling agent, a surfactant, a rheology modifier, a pigment, a dye, a storage stabilizer, an antifoaming agent, an antioxidant, and the like, as long as the effects of the present invention are not impaired.
[0094] For example, the sensitizer is effective in promoting the photoreaction after a thermally cured film is formed using the cured film-forming composition of the present invention.
[0095] Examples of sensitizers, which are other additives, include benzophenone, anthracene, anthraquinone, thioxanthone, and derivatives thereof, as well as nitrophenyl compounds. Of these, benzophenone derivatives and nitrophenyl compounds are preferred. Specific examples of preferred compounds include N,N-diethylaminobenzophenone, 2-nitrofluorene, 2-nitrofluorenone, 5-nitroacenaphthene, 4-nitrobiphenyl, 4-nitrocinnamic acid, 4-nitrostilbene, 4-nitrobenzophenone, and 5-nitroindole. In particular, N,N-diethylaminobenzophenone, a derivative of benzophenone, is preferred.
[0096] These sensitizers are not limited to those mentioned above. The sensitizers can be used alone or in combination of two or more compounds.
[0097] The proportion of the sensitizer used in the cured film-forming composition of the present invention is preferably 0.1 to 20 parts by mass, and more preferably 0.2 to 10 parts by mass, based on 100 parts by mass of the low-molecular-weight photoalignment component (A). If this proportion is too small, the effect as a sensitizer may not be fully obtained, whereas if it is too large, a decrease in transmittance and roughness of the coating film may occur.
[0098] <Preparation of Cured Film-Forming Composition> The cured film-forming composition of the present embodiment contains a low molecular weight photoalignment component (A), a polymer obtained by polymerizing a monomer containing at least an N-alkoxymethyl(meth)acrylamide compound (B), and a polymer obtained by polymerizing a monomer containing at least an N-hydroxyalkyl(meth)acrylamide compound (C). If necessary, the composition may contain a crosslinking catalyst (D), an adhesion improving component (E), and / or other additives.
[0099] The blending ratio, preparation method, etc. when the cured film-forming composition of the present invention is used in the form of a solution will be described in detail below. The solid content in the cured film-forming composition of the present invention is not particularly limited as long as each component is uniformly dissolved in the solvent, but is 1 to 80% by mass, preferably 3 to 60% by mass, and more preferably 5 to 40% by mass. Here, the solid content refers to all the components of the cured film-forming composition excluding the solvent.
[0100] The method for preparing the cured film-forming composition of the present invention is not particularly limited. For example, the method for preparing the composition includes a method in which the solution of the component (B) dissolved in a solvent is mixed with the component (A), the component (C), and if necessary, the component (D) and the component (E) in a predetermined ratio to prepare a homogeneous solution, or a method in which other additives are further added and mixed at an appropriate stage of the preparation method, if necessary.
[0101] In preparing the cured film-forming composition of the present invention, the polymer solution obtained by the polymerization reaction in the solvent can be used as it is. In this case, for example, the (A) component, the (B) component, and if necessary, the (D) component and the (E) component are added to the (C) component solution to prepare a homogeneous solution. In this case, a solvent may be added for the purpose of adjusting the concentration. In this case, the solvent used in the process of producing the (C) component and the solvent used to adjust the concentration of the cured film-forming composition may be the same or different.
[0102] The prepared solution of the cured film-forming composition is preferably filtered using a filter having a pore size of about 0.2 μm before use.
[0103] <Curing film, alignment material and retardation material> A solution of the cured film-forming composition of the present invention can be applied onto a substrate (e.g., a silicon / silicon dioxide-coated substrate, a silicon nitride substrate, a substrate coated with a metal, for example, aluminum, molybdenum, chromium, or the like, a glass substrate, a quartz substrate, an ITO substrate, or the like) or a film (e.g., a resin film such as a triacetyl cellulose (TAC) film, a cycloolefin polymer film, a polyethylene terephthalate film, or an acrylic film) by bar coating, spin coating, flow coating, roll coating, slit coating, spin coating followed by slit coating, inkjet coating, printing, or the like to form a coating film, and then the coating is heated and dried on a hot plate or in an oven, or the like to form a cured film.
[0104] The conditions for the heat drying are such that the crosslinking reaction by the crosslinking agent proceeds to such an extent that the components of the alignment material formed from the cured film are not dissolved in the polymerizable liquid crystal solution applied thereon, and for example, a heating temperature and a heating time appropriately selected from the ranges of 60° C. to 200° C. and 0.4 to 60 minutes are adopted. The heating temperature and heating time are preferably 70° C. to 160° C. and 0.5 to 10 minutes.
[0105] The thickness of the cured film formed using the cured film forming composition of the present invention is, for example, 0.05 μm to 5 μm, and can be appropriately selected taking into consideration the step height and optical and electrical properties of the substrate used.
[0106] The cured film thus formed can be made to function as an alignment material, that is, a member that aligns a compound having liquid crystallinity such as liquid crystal, by irradiating it with polarized UV light.
[0107] The polarized UV irradiation method generally uses ultraviolet light or visible light with a wavelength of 150 nm to 450 nm, and is performed by irradiating linearly polarized light from a vertical or oblique direction at room temperature or in a heated state.
[0108] Since the alignment material formed from the cured film-forming composition of the present invention has solvent resistance and heat resistance, a retardation material made of a polymerizable liquid crystal solution is applied onto the alignment material, and then the retardation material is heated to a phase transition temperature of the liquid crystal to make the retardation material in a liquid crystal state and aligned on the alignment material. The aligned retardation material is then cured as it is to form a retardation material as a layer having optical anisotropy.
[0109] As the retardation material, for example, a liquid crystal monomer having a polymerizable group and a composition containing the same are used.And, when the substrate on which the alignment material is formed is a film, the film having the retardation material of the present invention is useful as a retardation film.The retardation material forming such a retardation material is in a liquid crystal state, and on the alignment material, there are some that take the alignment state such as horizontal alignment, cholesteric alignment, vertical alignment, hybrid alignment, etc., and can be used according to the retardation required.
[0110] In addition, when manufacturing a patterned retardation material used in a 3D display, the cured film formed by the above-mentioned method from the cured film-forming composition of the present invention is exposed to polarized UV light at, for example, +45 degrees from a predetermined reference through a mask with a line and space pattern, and then exposed to polarized UV light at -45 degrees from the mask is removed to obtain an alignment material in which two types of liquid crystal alignment regions with different liquid crystal alignment control directions are formed. Thereafter, a retardation material made of a polymerizable liquid crystal solution is applied, and then heated to the phase transition temperature of the liquid crystal to make the retardation material in a liquid crystal state and oriented on the alignment material. Then, the retardation material in the oriented state is cured as it is, and a patterned retardation material in which two types of retardation regions with different retardation characteristics are regularly arranged in multiples can be obtained.
[0111] In addition, two substrates having the alignment material of the present invention formed as described above can be used, bonded together via a spacer so that the alignment materials on both substrates face each other, and then liquid crystal can be injected between the substrates to create a liquid crystal display element in which the liquid crystal is aligned. Thus, the curable film-forming composition of the present invention can be suitably used in the production of various retardation materials (retardation films), liquid crystal display elements, and the like.
Examples
[0112] Hereinafter, the present invention will be specifically described with reference to examples of the present invention, but the present invention is not construed as being limited thereto.
[0113] [Abbreviations used in the examples] The meanings of the abbreviations used in the following examples are as follows. <Raw materials> BMAA: N-butoxymethylacrylamide AIBN: α,α'-azobisisobutyronitrile MMA: Methyl methacrylate HEAA: N-(2-hydroxyethyl)acrylamide MAIB: Dimethyl 2,2-azobisisobutyrate
[0114] <Component A> MCA: 4-Methoxycinnamic acid
Chemical formula
[0115] <Component B> PB-1: Represented by the following structural formula.
Chemical formula
[0116] <Component C> PC-1: Represented by the following structural formula.
Chemical formula
Chemical formula
[0117] <Component D> PTSA: p-Toluenesulfonic acid monohydrate
[0118] <Component E> E-1: A compound having an N-alkoxymethyl group and an acrylic group represented by the following structural formula
Chemical formula
[0119] <Solvent> Each resin composition of the examples and comparative examples contained a solvent, and as the solvent, propylene glycol monomethyl ether (PM) and butyl acetate (BA) were used.
[0120] <Measurement of the molecular weight of the polymer> The molecular weight of the acrylic copolymer in the polymerization example was measured as follows using a gel permeation chromatography (GPC) apparatus (HLC-8320) manufactured by Tosoh Corporation and columns (TSKgel ALPHA4000, TSKgel ALPHA3000) manufactured by Tosoh Corporation. The following number average molecular weight (hereinafter referred to as Mn) and weight average molecular weight (hereinafter referred to as Mw) were expressed in terms of polystyrene conversion values. Column temperature: 40 °C Eluent: Tetrahydrofuran Flow rate: 1.0 mL / min Standard sample for calibration curve preparation: Standard polystyrene (molecular weights 427,000, 190,000, 37,900, 18,100, 5,970, 2,420, 1,010) manufactured by Tosoh Corporation
[0121] <Synthesis of Component B> <Polymerization Example - 1> 100.0 g of BMAA and 1.0 g of AIBN as a polymerization initiator were dissolved in 193.5 g of PM, and reacted at 80 °C for 20 hours to obtain an acrylic polymer solution. The Mn of the obtained acrylic polymer was 10,000 and the Mw was 23,000. The acrylic polymer solution was gradually dropped into 2000.0 g of hexane to precipitate a solid, which was then filtered and dried under reduced pressure to obtain a polymer (PB-1).
[0122] <Synthesis of Component C> <Polymerization Example - 2> 7.0 g of MMA, 5.8 g of HEAA, and 0.23 g of MAIB as a polymerization initiator were dissolved in 13.0 g of PM. A solution dissolved in a dropping tank, which had been heated to 85 °C by previously adding 6.50 g of PM to a four-necked flask, was dropped over 3 hours and reacted under reflux for 3 hours to obtain an acrylic polymer solution. The Mn of the obtained acrylic polymer was 12,600 and the Mw was 43,100. A 40% PM solution of the target polymer (PC-1) was obtained.
[0123] <Synthesis of Component C> <Polymerization Example - 3> 47.10 g of BMAA, 34.5 g of HEAA, and 0.829 g of MAIB as a polymerization initiator were dissolved in 82.50 g of PM. A solution dissolved in a dropping tank, which had been heated to 85 °C by previously adding 41.25 g of PM to a four-necked flask, was dropped over 3 hours and reacted for 5 hours after dropping to obtain an acrylic polymer solution. The Mn of the obtained acrylic polymer was 6,500 and the Mw was 17,000. A 40% PM solution of the target polymer (PC-2) was obtained.
[0124] <Preparation of Liquid Crystal Alignment Agent (Curing Film-Forming Composition)> <Preparation Example 1> As the (A) component, 0.079g of MCA, as the (B) component, 0.66g of PB-1 obtained in polymerization example-1, as the (C) component, 0.26g of 40% PM solution of the polymer (PC-1) obtained in polymerization example-2, as the (C) component, 0.056g of E-1 (94.6% BA solution manufactured by Junsei Chemical Co., Ltd.), as the (D) component, 0.021g of PTSA were mixed, and 6.65g of PM and 1.62g of BA were added as solvents and stirred for 1 hour, and the solution was confirmed to have dissolved visually to obtain a solution. Next, the obtained solution was filtered through a filter with a pore size of 0.2 μm to prepare a liquid crystal alignment agent (A-1).
[0125] <Preparation Examples 2 to 6> Except for using the components of the types and amounts shown in Table 1 below, the same procedure as in Preparation Example 1 was performed to prepare liquid crystal alignment agents (A-2) to (A-4), (B-1), and (B-2).
[0126] [Table 1] APEPO-1: RFK-505 (Kawasaki Chemical Industries, Ltd.) PEPO-1: Polylite 8651 (DIC Corporation)
[0127] <Preparation of polymerizable liquid crystal solution for horizontal alignment> <Production Example 1> 1.57 g of LC-242 (BASF), a polymerizable liquid crystal for horizontal alignment, 0.047 g of Irgacure907 (BASF), a photoradical initiator, and 0.008 g of BYK-361N, a leveling material, were added, and then 6.55 g of N-methylpyrrolidone (NMP) and 9.83 g of cyclopentanone were added as solvents. The mixture was stirred for 2 hours and visually confirmed to be dissolved, yielding a 9% by mass polymerizable liquid crystal solution LC-1.
[0128] <Formation of liquid crystal alignment film and preparation of retardation film> <Example 1> The liquid crystal alignment agent (A-1) prepared in Preparation Example 1 was applied to a triacetyl cellulose (TAC) film substrate with a wet film thickness of 6 μm using a bar coater. Heat drying was carried out at 130° C. for 2 minutes in a heat circulation oven to form a cured film on the film. Next, linearly polarized light of 313 nm was applied at 10 mJ / cm on the surface of this cured film. 2 The film was then irradiated vertically with an exposure dose of 100 mJ / cm2 to form a liquid crystal alignment film. A polymerizable liquid crystal solution LC-1 for horizontal alignment was applied to the liquid crystal alignment film with a wet thickness of 34 μm using a bar coater. The film was then dried by heating at 120° C. for 2 minutes in an oven, and then irradiated with 365 nm non-polarized light at 300 mJ / cm2 under nitrogen. 2 The polymerizable liquid crystal was cured by vertical irradiation with an exposure amount of 10 ...
[0129] <Examples 2 to 4> Retardation films were produced in the same manner as in Example 1, except that (A-2) to (A-4) were used as liquid crystal aligning agents.
[0130] <Comparative Example 1> The liquid crystal alignment agent (B-1) prepared in Preparation Example 1 was applied to a TAC film as a substrate with a bar coater to a wet film thickness of 4 μm. The film was dried by heating at 130° C. for 2 minutes in a heat circulation oven to form a cured film on the film. Next, the surface of the cured film was exposed to linearly polarized light of 313 nm at 10 mJ / cm. 2 The film was then irradiated vertically with an exposure dose of 100 mJ / cm2 to form a liquid crystal alignment film. A polymerizable liquid crystal solution LC-1 for horizontal alignment was applied to the liquid crystal alignment film with a wet thickness of 34 μm using a bar coater. The film was then dried by heating at 120° C. for 2 minutes in an oven, and then irradiated with 365 nm non-polarized light at 300 mJ / cm2 under nitrogen. 2 The polymerizable liquid crystal was cured by vertical irradiation with an exposure amount of 10 ...
[0131] <Comparative Example 2> A retardation film was produced in the same manner as in Comparative Example 1, except that (B-1) was used as a liquid crystal aligning agent.
[0132] The retardation films prepared above were evaluated by the following method. The evaluation results are shown in Table 2.
[0133] <Evaluation of orientation> The retardation film on the prepared substrate was sandwiched between a pair of polarizing plates, and the occurrence state of the retardation characteristics under crossed Nicols was visually observed. Those with retardation expressed without defects were marked as ○, and those without expressed retardation were marked as × and described in the column of "orientation".
[0134] <TAC protectiveness> For the retardation film containing the prepared TAC film, those without curling were marked as 〇, and those with curling were marked as × and described in the column of "protectiveness".
[0135]
Table 2
[0136] From the results in Table 2, it is clear that by using a polymer obtained by polymerizing a monomer containing an N-hydroxyalkyl (meth) acrylamide compound as the (C) component, the orientation with respect to the liquid crystal solution containing NMP can be obtained, and the damage to the TAC film by NMP can also be protected.
Industrial applicability
[0137] The cured film-forming composition according to the present invention is very useful as an alignment material for forming a liquid crystal alignment film of a liquid crystal display element or an optically anisotropic film provided inside or outside the liquid crystal display element. In particular, it is suitable as a material for forming a patterned retardation material of a 3D display. Furthermore, it is suitable as a material for forming cured films such as protective films, planarization films, and insulating films in various displays such as thin-film transistor (TFT) type liquid crystal display elements and organic EL elements. In particular, it is suitable as a material for forming an interlayer insulating film of a TFT type liquid crystal element, a protective film of a color filter, or an insulating film of an organic EL element.
Claims
1. (A) a compound having a photoalignable group and one substituent selected from the group consisting of a hydroxyl group, a carboxyl group, and an amino group; (B) a polymer obtained by polymerizing a monomer containing at least an N-alkoxymethyl(meth)acrylamide compound, and (C) A cured film-forming composition comprising a polymer obtained by polymerizing a monomer containing at least an N-hydroxyalkyl(meth)acrylamide compound.
2. 2. The cured film-forming composition according to claim 1, wherein the photoalignable group of the component (A) is a functional group having a structure that undergoes photodimerization or photoisomerization.
3. 3. The cured film-forming composition according to claim 1, wherein the photoalignable group of the component (A) is a cinnamoyl group.
4. 3. The cured film-forming composition according to claim 1, wherein the photoalignable group of the component (A) is a group having an azobenzene structure.
5. The cured film-forming composition according to claim 1 , further comprising a crosslinking catalyst as component (D).
6. The cured film-forming composition according to claim 1 , further comprising an adhesion improving component as the component (E).
7. 7. The cured film-forming composition according to claim 1, wherein a total amount of the components (B) and (C) is 100 to 3,000 parts by mass based on 100 parts by mass of the component (A).
8. The mass ratio of the component (B) to the component (C) is 1:99 to 99:
1. The cured film-forming composition according to claim 1 .
9. The cured film-forming composition according to claim 5 , comprising 0.01 to 10 parts by mass of the component (D) based on 100 parts by mass of the total amount of the components (B) and (C).
10. An alignment material obtained by using the cured film-forming composition according to any one of claims 1 to 9.
11. A retardation material, which is formed by using a cured film obtained from the cured film-forming composition according to any one of claims 1 to 9.
Citation Information
Patent Citations
Phase difference plate and circularly polarizing plate
JP1998068816A
Photocrosslinkable polyimides
JP2001517719A
Manufacturing method of optical phase difference element
JP2005049865A
Liquid crystal aligning agent and method of forming liquid crystal alignment layer
JP2009058584A
Compound, liquid crystal composition and anisotropic material
JP2009179563A