Liquid crystal elastomer composition and preparation method thereof
By introducing a semi-interpenetrating liquid crystal polymer network into the liquid crystal elastomer, the synergistic effect of liquid crystal elastomer and linear polymer is used to solve the problem of poor damping performance of liquid crystal elastomer, achieving better damping performance and wider effectiveness Temperature range.
Patent Information
- Application Number
- CN202410812116.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing liquid crystal elastomer (LCE) has poor damping performance, which limits its wide application in the field of vibration and noise reduction.
A liquid crystal elastomer composition, including linear polymer and liquid crystal elastomer, is adopted to form a semi-interpenetrating liquid crystal polymer network, and absorb and dissipate vibration energy through the synergistic action of the liquid crystal elastomer and linear polymer, and improve damping performance.
The damping performance of the liquid crystal elastomer composition is significantly improved, its effective damping temperature range is widened, and it exhibits higher shear modulus and better mechanical properties under room temperature conditions.
Smart Images

Figure CN118879072A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of liquid crystal materials, and in particular, relates to a liquid crystal elastomer composition and a preparation method thereof. Background Art
[0002] With the rapid growth of the national economy and the continuous improvement of the level of modern industrialization, the pollution of vibration and noise to social life has become increasingly prominent, endangering human physiological and mental health and interfering with the normal use of equipment and instruments. Using damping materials (vibration reduction materials) to reduce vibration and noise is one of the most common technical means. High damping alloys, ceramics, cement, polymer materials, etc. are all damping materials. Among them, polymer materials have outstanding viscoelasticity and stronger damping effect, and are widely used in engineering scenarios for vibration reduction and noise reduction.
[0003] The loss factor tanδ is a characteristic value that characterizes the damping performance of polymer materials. Usually, damping materials are used at temperature T 0 ±25℃(T 0 The loss factor tanδ in the range of the optimal operating temperature should be greater than 0.3. g ) is one of the key characteristic temperatures of polymer materials. g When the temperature is close to the maximum value, the loss factor of the polymer will reach a maximum value, which is the damping peak.
[0004] Liquid crystal elastomer (LCE) is a polymer material that has both viscoelasticity and liquid crystal properties. The liquid crystal properties of LCE give it a new phase transition temperature - liquid crystal transition temperature (T i ). i When the temperature is below T, LCE presents a liquid crystal state, and the liquid crystal units are arranged in an orderly manner in space; i When the temperature is above 200 °C, the order of the liquid crystal unit is destroyed, and the LCE changes from an anisotropic liquid crystal state to an isotropic state. When the material is near the phase transition temperature, the energy fluctuation will increase significantly, resulting in a better damping effect of the material. To this end, the phase change of the liquid crystal enables LCE to produce a new thermodynamic phase change beyond the glass transition temperature, expanding its effective damping temperature range. In addition, LCE has "soft elasticity" in the equilibrium state, that is, the orientation of the main axis of the liquid crystal unit changes under the action of external force, and the stress of the LCE is almost constant while the strain is increased. In this process, LCE can effectively absorb the applied strain and generate energy dissipation, and the damping effect increases with the increase of the external vibration frequency. With its unique liquid crystal properties and soft elasticity, LCE is expected to become a new generation of high-performance polymer damping material.
[0005] However, the existing LCEs suffer from poor damping properties, which limits their widespread application. Summary of the invention
[0006] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide a liquid crystal elastomer composition and a preparation method thereof. The liquid crystal elastomer composition provided in the present application has excellent damping performance.
[0007] In the first aspect of the present invention, the present invention provides a liquid crystal elastomer composition. According to an embodiment of the present invention, the liquid crystal elastomer composition includes a linear polymer and a liquid crystal elastomer, and the liquid crystal elastomer composition contains a semi-interpenetrating liquid crystal polymer network.
[0008] According to the liquid crystal elastomer composition of the above embodiment of the present invention, the liquid crystal elastomer composition contains a semi-interpenetrating liquid crystal polymer network, in which the liquid crystal elastomer and the linear polymer permeate each other to form an interwoven network structure, wherein the liquid crystal elastomer has a high degree of elasticity and deformability, and at the same time has the orderliness of liquid crystal, when the liquid crystal elastomer is vibrated or impacted, the direction of the liquid crystal unit changes, and the energy can be effectively absorbed and dissipated, thereby showing good damping performance. The molecular chain of the linear polymer has flexibility and ductility, and can deform when subjected to force, absorb and disperse vibration energy, and reduce the transfer of energy in the system. Therefore, through the synergistic effect of the chain movement of the linear polymer and the phase transition of the liquid crystal unit of the liquid crystal elastomer, the vibration energy can be absorbed and dissipated together, and the damping performance of the liquid crystal elastomer composition can be effectively improved. Therefore, the liquid crystal elastomer composition provided by the present application has good damping performance.
[0009] In addition, the liquid crystal elastomer composition according to the above embodiment of the present invention may also have the following additional technical features:
[0010] In some embodiments of the present invention, based on the total mass of the liquid crystal elastomer composition, the mass proportion of the linear polymer is 30%-70%, thereby improving the damping performance of the liquid crystal elastomer composition.
[0011] In some embodiments of the present invention, the liquid crystal elastomer comprises nematic liquid crystal, which is beneficial to improve the damping performance of the liquid crystal elastomer composition.
[0012] In some embodiments of the present invention, the polymerized monomer of the linear polymer includes a liquid crystal unit, thereby facilitating the improvement of the damping performance of the liquid crystal elastomer composition.
[0013] In the second aspect of the present invention, the present invention provides a method for preparing the above-mentioned liquid crystal elastomer composition. According to an embodiment of the present invention, the method comprises: mixing a linear polymer and a liquid crystal elastomer so that the linear polymer is uniformly dispersed in the liquid crystal elastomer, and curing to obtain the liquid crystal elastomer composition. Thus, a liquid crystal elastomer composition with good damping performance can be obtained.
[0014] In some embodiments of the present invention, the method for preparing the linear polymer includes: mixing a first liquid crystal unit, a first chain extender, a first catalyst, a capping agent and a solvent, and drying to obtain a linear polymer, thereby obtaining a liquid crystal elastomer composition with good damping performance.
[0015] In some embodiments of the present invention, the method for preparing the liquid crystal elastomer composition further comprises: mixing and reacting the linear polymer, the second liquid crystal unit, the second chain extender, the crosslinking agent and the second catalyst, and curing to obtain the liquid crystal elastomer composition. Thus, a liquid crystal elastomer composition with good damping performance can be obtained.
[0016] In some embodiments of the present invention, the molar ratio of the first liquid crystal unit, the first chain extender and the end-capping agent is (9-11): (11-13): 4. Thus, a liquid crystal elastomer composition with good damping performance can be obtained.
[0017] In some embodiments of the present invention, the first liquid crystal unit includes at least one of 2-methyl-1,4-phenylene bis(4-((6-(acryloyloxy)hexyl)oxy)benzoate) and 2-methyl-1,4-phenylene bis(4-(3-(acryloyloxy)propoxy)benzoate). This helps the linear polymer maintain a certain orientation and order after curing, thereby improving the damping performance of the liquid crystal elastomer composition.
[0018] In some embodiments of the present invention, the first chain extender includes at least one of propylene glycol mercaptan and 2,2'-(1,2-ethylenedioxy)diethylmercaptan, thereby being able to easily undergo addition reaction with unsaturated bonds (such as acryloxy groups) in the liquid crystal unit, thereby effectively extending the linear polymer chain.
[0019] In some embodiments of the present invention, the first catalyst includes at least one of di-n-propylamine and triethylamine, thereby activating the functional groups in the reaction system and promoting the occurrence of the chain growth reaction.
[0020] In some embodiments of the present invention, the end-capping agent includes at least one of methyl methacrylate and acrylate, thereby terminating the chain growth process and obtaining a linear polymer with a specific molecular weight.
[0021] In some embodiments of the present invention, the solvent includes at least one of dichloromethane and chloroform, thereby improving the uniformity and efficiency of the reaction and promoting the smooth progress of the chain growth and end-capping process.
[0022] In some embodiments of the present invention, the molar ratio of the second liquid crystal unit, the second chain extender and the cross-linking agent is (0.8-1.1): (0.7-1.0): 0.05. Thus, a liquid crystal elastomer composition with good damping performance can be obtained.
[0023] In some embodiments of the present invention, the second liquid crystal unit includes at least one of 2-methyl-1,4-phenylene bis(4-((6-(acryloyloxy)hexyl)oxy)benzoate) and 2-methyl-1,4-phenylene bis(4-(3-(acryloyloxy)propoxy)benzoate). This helps the liquid crystal elastomer to maintain a certain orientation and order after curing, thereby improving the damping performance of the liquid crystal elastomer composition.
[0024] In some embodiments of the present invention, the second chain extender includes at least one of hexanedithiol and 2,2'-(1,2-ethylenedioxy)bis(ethylenethiol), thereby facilitating the preparation of a liquid crystal elastomer composition having good damping performance.
[0025] In some embodiments of the present invention, the second catalyst includes triethylamine, thereby promoting the reaction and improving the catalytic efficiency.
[0026] In some embodiments of the present invention, the cross-linking agent includes at least one of [2-methyl-3-(3-thiopropionyloxy)-2-(3-thiopropionyloxymethyl)propyl] 3-mercaptopropionate and pentaerythritol tetrakis-3-mercaptopropionate. Thus, it can react with the functional groups in the linear polymer, the second liquid crystal unit and the second chain extender to form a stable chemical bond, which can enhance the connection between the polymer chains, thereby forming a three-dimensional network structure.
[0027] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0029] Figure 1 A comparison diagram of the modulus-temperature curves of the liquid crystal elastomer compositions of Example 1 and Comparative Example 1 of the present application is shown;
[0030] Figure 2shows the differential scanning calorimetry curve of the liquid crystal elastomer composition of Comparative Example 1 of the present application;
[0031] Figure 3 shows the differential scanning calorimetry curve of the linear polymer of Example 1 of the present application;
[0032] Figure 4 The differential scanning calorimetry curve of the liquid crystal elastomer composition of Example 1 of the present application is shown. DETAILED DESCRIPTION
[0033] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0034] In the first aspect of the present invention, the present invention provides a liquid crystal elastomer composition. According to an embodiment of the present invention, the liquid crystal elastomer composition includes a linear polymer and a liquid crystal elastomer, and the liquid crystal elastomer composition contains a semi-interpenetrating liquid crystal polymer network.
[0035] According to the liquid crystal elastomer composition of the above embodiment of the present invention, the liquid crystal elastomer composition contains a semi-interpenetrating liquid crystal polymer network, in which the liquid crystal elastomer and the linear polymer permeate each other to form an interwoven structure, wherein the liquid crystal elastomer has a high degree of elasticity and deformability, and at the same time has the orderliness of liquid crystal, when the liquid crystal elastomer is vibrated or impacted, the direction of the liquid crystal unit changes, and the energy can be effectively absorbed and dissipated, thereby showing good damping performance. The molecular chain of the linear polymer has flexibility and ductility, and can deform when subjected to force, absorb and disperse vibration energy, and reduce the transfer of energy in the system. Therefore, through the synergistic effect of the chain movement of the linear polymer and the phase transition of the liquid crystal unit of the liquid crystal elastomer, the vibration energy can be absorbed and dissipated together, and the damping performance of the liquid crystal elastomer composition can be effectively improved. Therefore, the liquid crystal elastomer composition provided by the present application has good damping performance.
[0036] Liquid crystal elastomers (LCEs) refer to high molecular polymers with liquid crystal phase and soft elasticity formed after appropriate cross-linking of liquid crystal polymers. Different types of LCEs are suitable for different needs. According to different stimulus responses, LCEs can be divided into thermal response LCEs, photoresponse LCEs and magnetic response LCEs; according to the type of liquid crystal unit, they can be divided into nematic LCEs, smectic LCEs and cholesteric LCEs, and the commonly used liquid crystal units are mostly nematic phases. According to the position of the liquid crystal unit in the polymer cross-linking network, it is divided into main chain LCEs and side chain LCEs. The liquid crystal unit of the main chain LCEs exists in the main chain of the polymer. Compared with the side chain LCEs, the mechanical properties, stimulus response deformation ability and driving stress of the main chain LCEs are better.
[0037] Linear polymers refer to macromolecular compounds formed by monomer molecules linked together by covalent bonds. Their molecular chains are straight, and the monomers are linked together in sequence to form a long chain structure. They are in a linear, non-cross-linked state and usually have good flexibility and ductility and are easy to process into various shapes.
[0038] According to some specific embodiments of the present invention, based on the total mass of the liquid crystal elastomer composition, the mass proportion of the linear polymer is 30%-70%. For example, it can be 30%, 50%, 70%, etc. By limiting the mass proportion of the linear polymer to the above range, the linear polymer can be evenly interspersed between the liquid crystal elastomers to form a stable and continuous semi-interpenetrating liquid crystal polymer network structure, which can increase the friction and energy dissipation mechanism inside the material. When the liquid crystal elastomer composition is subjected to external force, the interaction between the linear polymer and the liquid crystal elastomer and the deformation of the network structure will absorb and dissipate more energy, thereby improving the damping performance of the liquid crystal elastomer composition.
[0039] According to some specific embodiments of the present invention, the liquid crystal elastomer includes nematic liquid crystal. Nematic liquid crystal is a liquid crystal phase with a special arrangement, and its molecular form is usually rod-shaped, and these molecules remain parallel or nearly parallel to each other in the length direction. In the semi-interpenetrating liquid crystal polymer network structure, linear polymers are interspersed between nematic liquid crystal elastomers, which can provide more energy dissipation paths, so that the liquid crystal elastomer composition can better absorb and disperse vibration energy, which is beneficial to improve the damping performance of the liquid crystal elastomer composition.
[0040] According to some specific embodiments of the present invention, the polymerizable monomer of the linear polymer includes a liquid crystal unit. The use of the liquid crystal unit as a polymerizable monomer enables the linear polymer and the liquid crystal elastomer to interpenetrate and interweave with each other when mixed, forming a stable semi-interpenetrating liquid crystal polymer network structure, thereby facilitating the improvement of the damping performance of the liquid crystal elastomer composition.
[0041] In the second aspect of the present invention, the present invention proposes a method for preparing the above-mentioned liquid crystal elastomer composition. According to an embodiment of the present invention, the method includes: mixing a linear polymer and a liquid crystal elastomer so that the linear polymer is uniformly dispersed in the liquid crystal elastomer, and curing to obtain the liquid crystal elastomer composition.
[0042] In this step, the linear polymer and the liquid crystal elastomer are mixed so that the linear polymer can be evenly dispersed in the liquid crystal elastomer, and then the liquid crystal elastomer composition can be obtained by curing.
[0043] According to the method of the above embodiment of the present invention, during the mixing process of the linear polymer and the liquid crystal elastomer, the molecular chain of the linear polymer can be interlaced into the molecular network of the liquid crystal elastomer to form an interwoven network structure. At the same time, the liquid crystal phase behavior of the liquid crystal elastomer also provides favorable conditions for the dispersion of the linear polymer, so that the linear polymer can be evenly dispersed in the liquid crystal elastomer to form a semi-interpenetrating liquid crystal polymer network structure, in which the liquid crystal elastomer and the linear polymer penetrate each other to form an interwoven structure, wherein the liquid crystal elastomer has a high degree of elasticity and deformability, and at the same time has the orderliness of the liquid crystal. When the liquid crystal elastomer is vibrated or impacted, the liquid crystal primitive can undergo a phase transition from an ordered arrangement to a disordered state, and can effectively absorb and dissipate energy, thereby showing good damping performance. The molecular chain of the linear polymer has flexibility and ductility, and can deform when subjected to force, absorb and disperse vibration energy, and reduce the transfer of energy in the system. Therefore, through the synergistic effect of the chain movement of the linear polymer and the phase transition of the liquid crystal primitive of the liquid crystal elastomer, the vibration energy can be absorbed and dissipated together, and the damping performance of the liquid crystal elastomer composition can be effectively improved. Moreover, the voids and interfaces in the semi-IPLC polymer network can effectively absorb and dissipate vibration energy, thereby reducing the vibration amplitude and further improving the damping performance of the liquid crystal elastomer composition.
[0044] According to some specific embodiments of the present invention, the method for preparing the linear polymer comprises:
[0045] The first liquid crystal unit, the first chain extender, the first catalyst, the end-capping agent and the solvent are mixed for reaction and dried to obtain a linear polymer.
[0046] In this step, a linear polymer can be obtained by mixing and reacting the first liquid crystal unit, the first chain extender, the first catalyst, the end capping agent and the solvent, and then drying the mixture. Specifically, the first liquid crystal unit is the basic unit constituting the liquid crystal polymer, and has a special molecular structure and arrangement, so that the liquid crystal polymer has unique physical and chemical properties. The first chain extender is used to increase the chain length of the polymer during the reaction, thereby adjusting the molecular weight and performance of the polymer. The catalyst is used to accelerate the polymerization reaction and improve the reaction efficiency. The end capping agent is used to block the end of the polymer chain at the end of the polymerization reaction to prevent the chain growth reaction from continuing, thereby controlling the molecular weight distribution of the polymer. During the mixed reaction, under the action of the first catalyst, a Michael addition reaction occurs between the first liquid crystal unit and the first chain extender, resulting in the formation and growth of a linear polymer chain. With the addition of the end capping agent, the molecular weight of the linear polymer can be controlled. After the reaction is completed, the solvent and unreacted substances are removed through a drying process to obtain a pure linear polymer.
[0047] According to some specific embodiments of the present invention, the molar ratio of the first liquid crystal unit, the first chain extender and the end capping agent is (9-11): (11-13): 4. The molar ratio of the first liquid crystal unit to the first chain extender will affect the molecular weight of the liquid crystal linear polymer, and controlling the molar ratio of the two can effectively regulate the molecular weight of the liquid crystal linear polymer. The end of the linear polymer obtained by the reaction of the first liquid crystal unit and the first chain extender is a reactive thiol group, which can react with the second liquid crystal unit. For this purpose, an end capping agent is required to react with the reactive thiol group to avoid the linear liquid crystal polymer from reacting with the second liquid crystal unit. The proportion of the end capping agent should be the same as the number of thiol groups remaining in the two segments of the liquid crystal linear polymer, thereby synthesizing a linear polymer with a specific molecular weight and performance.
[0048] According to some specific embodiments of the present invention, the first liquid crystal unit is selected from at least one of 2-methyl-1,4-phenylene bis(4-((6-(acryloyloxy)hexyl)oxy)benzoate) (RM82) and 2-methyl-1,4-phenylene bis(4-(3-(acryloyloxy)propoxy)benzoate) (RM257). By selecting the above-mentioned liquid crystal unit as a raw material, an ordered liquid crystal phase can be formed within a certain temperature range, which helps the linear polymer to maintain a certain orientation and order after curing, thereby improving the damping performance of the liquid crystal elastomer composition.
[0049] According to some specific embodiments of the present invention, the first chain extender includes at least one of propylene glycol mercaptan and 2,2'-(1,2-ethylenedioxy)diethylmercaptan (EDDET). Both propylene glycol mercaptan and 2,2'-(1,2-ethylenedioxy)diethylmercaptan contain thiol groups, which have high reactivity and can easily react with unsaturated bonds (such as acryloyloxy) in liquid crystal primitives to effectively extend the linear polymer chain.
[0050] According to some specific embodiments of the present invention, the first catalyst includes at least one of di-n-propylamine (DPA) and triethylamine (TEA). DPA and TEA, as organic amine compounds, can activate functional groups in the reaction system and promote the occurrence of chain growth reactions.
[0051] According to some specific embodiments of the present invention, the end-capping agent includes at least one of methyl methacrylate (MMA) and acrylate. By selecting the above end-capping agent, the chain length of the linear polymer can be effectively controlled. When the end-capping agent reacts with the active group at the end of the polymer chain, the chain growth process can be terminated, thereby obtaining a linear polymer with a specific molecular weight.
[0052] According to some specific embodiments of the present invention, the solvent includes at least one of dichloromethane (DCM) and chloroform. The above solvent is selected to have good solubility, can effectively dissolve the first liquid crystal unit, the first chain extender, the end-capping agent and the intermediate product generated, ensure that the components in the reaction system can fully contact and react, is conducive to improving the uniformity and efficiency of the reaction, and promotes the smooth progress of the chain growth and end-capping process.
[0053] According to some specific embodiments of the present invention, the method for preparing the liquid crystal elastomer composition further comprises:
[0054] The linear polymer, the second liquid crystal primitive, the second chain extender, the cross-linking agent and the second catalyst are mixed and reacted, and then cured to obtain the liquid crystal elastomer composition.
[0055] In this step, a liquid crystal elastomer composition can be obtained by mixing a linear polymer, a second liquid crystal primitive, a second chain extender, a crosslinker and a second catalyst for reaction, and then curing. Specifically, the second liquid crystal primitive forms a liquid crystal ordered structure through specific interactions and arrangements, and the second chain extender and the crosslinker connect the second liquid crystal primitives together through chemical bonding, that is, a liquid crystal elastomer with a three-dimensional crosslinked network structure is formed by a Michael addition reaction between the second chain extender, the crosslinker and the second liquid crystal primitive. The chain segments of the linear polymer chain and the liquid crystal elastomer chain interpenetrate each other through diffusion to form a semi-interpenetrating liquid crystal polymer network structure, wherein the liquid crystal elastomer has a high degree of elasticity and deformability, and at the same time has the orderliness of liquid crystal, so that the liquid crystal elastomer can effectively dissipate energy by adjusting the internal structure when subjected to external force, thereby showing good damping performance. The molecular chain of the linear polymer has flexibility and ductility, and can deform when subjected to force, absorb and disperse vibration energy, and reduce the transmission of energy in the system. Moreover, the voids and interfaces in the semi-interpenetrating network formed by the linear polymer and the liquid crystal elastomer can effectively absorb and dissipate vibration energy, thereby reducing the vibration amplitude and further improving the damping performance of the liquid crystal elastomer composition.
[0056] According to some specific embodiments of the present invention, the molar ratio of the second liquid crystal unit, the second chain extender and the cross-linking agent is (0.8-1.1): (0.7-1.0): 0.05. By limiting the molar ratio of the second liquid crystal unit, the second chain extender and the cross-linking agent to the above range, the mercapto-Michael addition between the second liquid crystal unit, the second chain extender and the cross-linking agent is a highly selective and highly active click chemistry reaction, which is conducive to the complete reaction and the uniformity of the product, and further conducive to the formation of a stable and uniform semi-interpenetrating liquid crystal polymer network structure, which can improve the damping performance of the liquid crystal elastomer composition.
[0057] According to some specific embodiments of the present invention, the second liquid crystal unit is selected from at least one of 2-methyl-1,4-phenylene bis(4-((6-(acryloyloxy)hexyl)oxy)benzoate) (RM82) and 2-methyl-1,4-phenylene bis(4-(3-(acryloyloxy)propoxy)benzoate) (RM257). By selecting the above-mentioned types of liquid crystal units as raw materials, an ordered liquid crystal phase can be formed within a certain temperature range, which helps the liquid crystal elastomer to maintain a certain orientation and order after curing, thereby improving the damping performance of the liquid crystal elastomer composition.
[0058] According to some specific embodiments of the present invention, the second chain extender includes at least one of hexanedithiol and 2,2'-(1,2-ethylenedioxy)diethylthiol (EDDET). By selecting the above chain extender, on the one hand, the thiol group in the chain extender can effectively react with the liquid crystal unit and other polymer chains, increase the length and flexibility of the polymer chain, and help improve the elasticity, ductility and processability of the liquid crystal elastomer. On the other hand, the thiol group in the chain extender can also interact with the reaction site in the cross-linking agent to further promote the formation of the cross-linked structure. Thus, it is beneficial to obtain a liquid crystal elastomer composition with good damping performance.
[0059] According to some specific embodiments of the present invention, the second catalyst includes triethylamine (TEA). The triethylamine molecule contains three basic ethyl groups, and its nitrogen atom has a lone pair of electrons, making it a strong alkaline substance that can promote the reaction and thus improve the catalytic efficiency.
[0060] According to some specific embodiments of the present invention, the crosslinking agent includes at least one of [2-methyl-3-(3-thiopropionyloxy)-2-(3-thiopropionyloxymethyl)propyl] 3-mercaptopropionate and pentaerythritol tetrakis-3-mercaptopropionate (PETMP). The thiol (-SH) functional group in the crosslinking agent is highly reactive and can react with the functional groups in the linear polymer, the second liquid crystal unit and the second chain extender to form a stable chemical bond, which can enhance the connection between the polymer chains, thereby forming a three-dimensional network structure.
[0061] The scheme of the present disclosure will be explained below in conjunction with the examples. Those skilled in the art will appreciate that the following examples are only used to illustrate the present disclosure and should not be considered to limit the scope of the present disclosure. Where specific techniques or conditions are not indicated in the examples, the techniques or conditions described in the literature in this area or the product instructions are used. Where the manufacturers of reagents or instruments are not indicated, they are all conventional products that can be obtained commercially.
[0062] Example 1
[0063] Raw materials: The first liquid crystal unit is 2-methyl-1,4-phenylenebis(4-((6-(acryloyloxy)hexyl)oxy)benzoate), the first chain extender is propylene glycol, the first catalyst is di-n-propylamine, the end capping agent is methyl methacrylate, the solvent is dichloromethane, the second liquid crystal unit is 2-methyl-1,4-phenylenebis(4-(3-(acryloyloxy)propoxy)benzoate), the second chain extender is 2,2'-(1,2-ethylenedioxy)bisethylmercaptan, the crosslinking agent is pentaerythritol tetrakis-3-mercaptopropionate, and the second catalyst is triethylamine.
[0064] 1. Add 10 mmol of 2-methyl-1,4-phenylenebis(4-((6-(acryloyloxy)hexyl)oxy)benzoate) and 12 mmol of propylene glycol to a 250 mL flask and mix them evenly. The solvent is dichloromethane (DCM); then add 4 wt% of di-n-propylamine to the mixture and mix them evenly. After reacting at room temperature for 18 hours, add 8 mmol of methyl methacrylate to the reaction system and mix them evenly. After reacting at room temperature for 18 hours, a linear polymer is obtained. Finally, the linear polymer is precipitated with methanol for 5 times to remove unreacted monomers. After removing most of the DCM using a rotary evaporator, the linear polymer is placed in a vacuum drying oven at 40°C and dried for 48 hours to remove the remaining DCM to obtain a dried linear polymer.
[0065] 2. Take 1 mmol of 2-methyl-1,4-phenylenebis(4-(3-(acryloyloxy)propoxy)benzoate), 0.9 mmol of 2,2'-(1,2-ethylenedioxy)bis(ethyl mercaptan) (EDDET), 0.05 mmol of pentaerythritol tetrakis-3-mercaptopropionate (PETMP) and 798.12 mg of dried linear polymer, put them into a tetrafluoroethylene mold, heat and melt them on a hot plate at 110°C, and stir for 10 minutes until they are evenly mixed; after the mixed reactants are cooled, 4 wt% of triethylamine is added and mixed evenly; dry them in a vacuum drying oven at 40°C for 4 minutes to remove bubbles in the reaction sample, and then react them in an oven at 80°C for 48 hours to complete curing to obtain a liquid crystal elastomer composition, in which the mass proportion of the linear polymer is 50%.
[0066] In this embodiment, the mold is a polytetrafluoroethylene groove with a size of 40 mm × 40 mm × 4 mm. The linear polymer needs to be fully dried before use, and the monomers used are used directly without further treatment. In the process of preparing the sample, it is necessary to remove bubbles, otherwise the material properties will be affected.
[0067] Example 2
[0068] The difference between Example 2 and Example 1 is that:
[0069] 2. Take 1 mmol of 2-methyl-1,4-phenylenebis(4-(3-(acryloyloxy)propoxy)benzoate), 0.9 mmol of 2,2'-(1,2-ethylenedioxy)bisethanethiol, 0.05 mmol of pentaerythritol tetrakis-3-mercaptopropionate and 342.05 mg of dried linear polymer, put them into a tetrafluoroethylene mold, heat and melt on a hot plate at 110°C, and stir for 10 minutes until the mixture is evenly mixed; after the mixed reactants are cooled, 4 wt% of triethylamine is added and mixed evenly; dry in a vacuum drying oven at 40°C for 4 minutes to remove bubbles in the reaction sample, react in an oven at 80°C for 48 hours to complete curing, and obtain a liquid crystal elastomer composition, in which the mass proportion of the linear polymer is 30%.
[0070] Example 3
[0071] The difference between Example 2 and Example 1 is that:
[0072] 2. Take 1 mmol of 2-methyl-1,4-phenylenebis(4-(3-(acryloyloxy)propoxy)benzoate), 0.9 mmol of 2,2'-(1,2-ethylenedioxy)bisethanethiol, 0.05 mmol of pentaerythritol tetrakis-3-mercaptopropionate and 1862.28 mg of dried linear polymer, put them into a tetrafluoroethylene mold, heat and melt on a hot plate at 110°C, and stir for 10 minutes until the mixture is evenly mixed; after the mixed reactants are cooled, 4 wt% of triethylamine is added and mixed evenly; dry in a vacuum drying oven at 40°C for 4 minutes to remove bubbles in the reaction sample, react in an oven at 80°C for 48 hours to complete curing, and obtain a liquid crystal elastomer composition, in which the mass proportion of the linear polymer is 70%.
[0073] Comparative Example 1
[0074] Take 1mmol of 2-methyl-1,4-phenylenebis(4-(3-(acryloyloxy)propoxy)benzoate), 0.9mmol of 2,2'-(1,2-ethylenedioxy)bisethanethiol and 0.05mmol of pentaerythritol tetrakis-3-mercaptopropionate, put them into a tetrafluoroethylene mold, heat and melt on a hot plate at 110°C, and stir for 10 minutes until the mixture is evenly mixed; after the mixed reactants are cooled, 4wt% of triethylamine is added and mixed evenly; dry in a vacuum drying oven at 40°C for 4min to remove bubbles in the reaction sample, and then react in an oven at 80°C for 48h to complete curing to obtain a liquid crystal elastomer composition.
[0075] Testing and analysis
[0076] Under the same conditions, the damping performance and shear modulus of the liquid crystal elastomer compositions obtained in the above Examples 1-3 and Comparative Example 1 were tested. The specific test methods are as follows:
[0077] Damping performance test: ① Cut the liquid crystal elastomer into circular samples with a diameter of 8mm, and place the circular samples on the rheological test bench for testing; ② Use the temperature control system to heat the sample from room temperature to 150℃ at a heating rate of 5℃ / min, the test frequency is 1Hz, and the temperature during the test is 0.5%; ③ Obtain the loss tangent value-temperature curve of the sample.
[0078] Shear modulus test: ① Cut the liquid crystal elastomer into a circular sample with a diameter of 8 mm, and place the circular sample on the rheological test bench for testing; ② Use the temperature control system to heat the sample from room temperature to 150°C at a heating rate of 5°C / min, the test frequency is 1Hz, and the temperature during the test is 0.5%; ③ Obtain the shear modulus-temperature curve of the sample.
[0079] Figure 1 A comparison diagram of the modulus-temperature curves of the liquid crystal elastomer compositions of Example 1 of the present application and Comparative Example 1 is shown. The loss factor is closely related to the damping performance of the material, and the range of the effective loss factor tanδ (>0.3) reflects the temperature range in which the material can achieve effective damping behavior; it can be seen from the figure that compared with Comparative Example 1, the liquid crystal elastomer composition obtained in Example 1 has a wider effective temperature range (20°C-123°C, tanδ>0.3), reflecting that it has a better damping effect; at the same time, the liquid crystal elastomer composition of Example 1 has a higher shear modulus (6.6MPa, 25°C) at room temperature, reflecting that it has a higher stiffness and is more adaptable to actual usage conditions.
[0080] Figure 2 The differential scanning calorimetry curve of the liquid crystal elastomer of comparative example 1 of the present application is shown. From the figure, the T g At -5.65℃, T i At around 74.86°C, it reflects that its glass transition temperature is -5.65°C, and the liquid crystal phase-isotropic phase transition temperature is 74.86°C, that is, there are two phase transition temperatures, and there is obvious energy absorption near the two phase transition temperatures.
[0081] Figure 3 The differential scanning calorimetry curve of the linear polymer in Example 1 of the present application is shown. From the figure, the T g At around -16.16℃, T m At 57.74℃, T i Around 106.3°C, its glass transition temperature is -5.65°C, its melting point is 57.75°C, and its liquid crystal phase-isotropic phase transition temperature is 106.3°C, that is, there are three phase transition temperatures, and there is obvious energy absorption near the three phase transition temperatures.
[0082] Figure 4 The differential scanning calorimetry curve of the liquid crystal elastomer composition of Example 1 of the present application is shown. From the figure, the T g At around -11.98℃, T m At 53.52℃, T i Around 103.54°C, it can be seen that the addition of linear polymers has a huge impact on the phase transition temperature and properties of liquid crystal elastomers.
[0083] The test results are shown in Table 1.
[0084] Table 1
[0085] Effective temperature range when tanδ>0.3 Shear modulus at 25°C Example 1 20℃-123℃ 6.6MPa Example 2 20℃-59℃ 3MPa Example 3 20℃-150℃ 7.4MPa Comparative Example 1 20℃-43℃ 0.7MPa
[0086] Combined with Table 1, it can be seen that compared with Comparative Example 1, the liquid crystal elastomer compositions obtained in Examples 1-3 have a wider effective damping temperature range and a higher modulus at room temperature, showing better mechanical properties, and can be used as a high-performance new damping material.
[0087] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", "some implementation schemes" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0088] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A liquid crystal elastomer composition, It is characterized in that The liquid crystal elastomer composition comprises a linear polymer and a liquid crystal elastomer, and the liquid crystal elastomer composition contains a semi-interpenetrating liquid crystal polymer network structure.
2. The liquid crystal elastomer composition according to claim 1, It is characterized in that Based on the total mass of the liquid crystal elastomer composition, the mass proportion of the linear polymer is 30%-70%.
3. The liquid crystal elastomer composition according to claim 1, It is characterized in that The liquid crystal elastomer comprises at least one of nematic liquid crystal, smectic liquid crystal and cholesteric liquid crystal; and / or, The polymerized monomers of the linear polymer include mesogens.
4. A method for preparing the liquid crystal elastomer composition according to any one of claims 1 to 3, It is characterized in that include: The linear polymer and the liquid crystal elastomer are mixed so that the linear polymer is uniformly dispersed in the liquid crystal elastomer, and then cured to obtain the liquid crystal elastomer composition.
5. The method according to claim 4, It is characterized in that The method for preparing the linear polymer comprises: The first liquid crystal unit, the first chain extender, the first catalyst, the end-capping agent and the solvent are mixed for reaction and dried to obtain a linear polymer.
6. The method according to claim 5, It is characterized in that The method for preparing the liquid crystal elastomer composition further comprises: The linear polymer, the second liquid crystal unit, the second chain extender, the cross-linking agent and the second catalyst are mixed and reacted, and then cured to obtain the liquid crystal elastomer composition.
7. The method according to claim 5, It is characterized in that The molar ratio of the first liquid crystal unit, the first chain extender and the end-capping agent is (9-11):(11-13):
4.
8. The method according to claim 5, It is characterized in that The first liquid crystal unit includes at least one of 2-methyl-1,4-phenylene bis(4-((6-(acryloyloxy)hexyl)oxy)benzoate) and 2-methyl-1,4-phenylene bis(4-(3-(acryloyloxy)propoxy)benzoate); and / or, The first chain extender comprises at least one of propylene glycol mercaptan and 2,2'-(1,2-ethylenedioxy)bis(ethylene glycol mercaptan); and / or, The first catalyst comprises at least one of di-n-propylamine and triethylamine; and / or, The end-capping agent comprises at least one of methyl methacrylate and acrylate; and / or, The solvent includes at least one of dichloromethane and chloroform.
9. The method according to claim 6, It is characterized in that The molar ratio of the second liquid crystal unit, the second chain extender and the cross-linking agent is (0.8-1.1): (0.7-1.0): 0.
05.
10. The method according to claim 6, It is characterized in that The second liquid crystal unit includes at least one of 2-methyl-1,4-phenylene bis(4-((6-(acryloyloxy)hexyl)oxy)benzoate) and 2-methyl-1,4-phenylene bis(4-(3-(acryloyloxy)propoxy)benzoate); and / or, The second chain extender comprises at least one of hexanedithiol and 2,2'-(1,2-ethylenedioxy)bisethylmercaptan; and / or, The second catalyst comprises triethylamine; and / or, The cross-linking agent includes at least one of [2-methyl-3-(3-mercaptopropionyloxy)-2-(3-mercaptopropionyloxymethyl)propyl] 3-mercaptopropionate and pentaerythritol tetrakis-3-mercaptopropionate.
Citation Information
Patent Citations
Responsive material based on semi-interpenetrating polymer network and application thereof
CN111087818A
Liquid crystal elastomer driver and preparation method thereof
CN113980273A
Polymer electrolyte with semi-interpenetrating network structure and preparation method thereof
CN114350004A
Polarizing Article and Method of Forming a Polarizing Article
US20200103571A1
Cited By
High-strength and high-toughness lignin-based liquid crystal elastomer as well as preparation method and application thereof
CN120818111A
High-strength and high-toughness lignin-based liquid crystal elastomer, and preparation method and application thereof
CN120818111B