Photoelectric conversion element

By employing SnO2 and SnCl2 surface treatment for the electron transport layer, the method addresses non-uniform film formation and voltage loss issues, achieving high open-circuit voltage and efficient photoelectric conversion.

JP7569046B2Active Publication Date: 2024-10-17MITSUBISHI CHEM CORP +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020073582
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-16
Publication Date
2024-10-17
Estimated Expiration
2040-04-16

AI Technical Summary

Technical Problem

Existing methods for manufacturing inorganic metal halide perovskite films face challenges such as non-uniform film formation, high hygroscopicity of lead compounds, and insufficient voltage output in photoelectric conversion elements, leading to inefficiencies and high voltage loss.

Method used

The use of SnO2 and SnCl2 solution surface treatment for the electron transport layer, combined with specific film formation and exposure to the atmosphere, results in a high-uniformity film with amorphous SnO2, enhancing the open-circuit voltage of photoelectric conversion elements.

Benefits of technology

This approach enables the production of a photoelectric conversion element with a high open-circuit voltage and improved efficiency through a simple and effective method, utilizing SnO2 and SnCl2 surface treatment to suppress recombination and enhance film uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569046000005
    Figure 0007569046000005
  • Figure 0007569046000006
    Figure 0007569046000006
  • Figure 0007569046000007
    Figure 0007569046000007
Patent Text Reader

Abstract

To provide a photoelectric conversion element that produces a higher voltage.SOLUTION: A photoelectric conversion element 100 includes a pair of electrodes composed of an upper electrode 105 and a lower electrode 101, and an active layer 103 located between the electrodes, and further includes an electron transport layer 102 between the active layer 103 and at least one of the pair of electrodes. In the photoelectric conversion element 100, the electron transport layer 102 contains SnO2, and a Sn2+ component is not detected by X-ray photoelectron spectroscopy (XPS) on the surface of the electron transport layer 102.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photoelectric conversion element, and more preferably to a photoelectric conversion element having an active layer made of a semiconductor compound using a perovskite crystal. [Background technology]

[0002] In recent years, many proposals have been made for semiconductor devices using perovskite crystals, and many inventions have been made regarding the manufacture of perovskite crystals. In particular, there is a demand for a method for manufacturing inorganic metal halide perovskite films that are easy to use in practice and that are highly uniform and easy to manufacture.

[0003] For example, when producing an inorganic metal halide perovskite film using lead and other metals, typically a lead-containing iodine compound that supplies lead and a metal iodide that supplies the other metals are placed on the surface of a substrate on which the inorganic metal halide perovskite film is to be formed, and then fired, thereby producing an inorganic metal halide perovskite film containing lead and other metals.

[0004] As a technique for obtaining a film with better properties, for example, Patent Document 1 describes a method for producing a crystalline perovskite film, which includes disposing on a substrate a first precursor compound containing a first cation, which is a metal or semimetal cation, and a sacrificial anion containing two or more atoms, and a second precursor compound containing a second anion and a second cation capable of forming a first volatile compound together with the sacrificial anion. This document describes the use of a metal or semimetal monocation as the second cation.

[0005] Furthermore, Non-Patent Document 1 describes a method for producing a perovskite crystal film by adding lead acetate to a CsPbI2Br solution, coating and heating the solution to form a thin film.

[0006] Non-Patent Document 2 describes that an open circuit voltage Voc of 1.32 V can be obtained when manufacturing a photoelectric conversion element using a perovskite crystal obtained by adding a trace amount of CaCl2 to a CsPbI2Br precursor solution.

[0007] Non-Patent Document 3 describes that, as an intermediate layer used for a CsPbI2Br active layer, a thin film of tin oxide (SnO2) is used as an electron transport layer, and a surface treatment is further performed with an aqueous solution of tin chloride (SnCl2), thereby suppressing recombination between the electron transport layer and the active layer and obtaining an open circuit voltage of 1.31 V. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Special Publication No. 2017-530546 [Non-patent literature]

[0009] [Non-Patent Document 1] Advanced Energy Materials 2018,8,1801050 [Non-Patent Document 2] Advanced Functional Materials 2020,1909972 [Non-Patent Document 3] Journal of Materials Chemistry A,2019,7,1227. Summary of the Invention [Problem to be solved by the invention]

[0010] However, for example, in the method described in Patent Document 1, a compound synthesized from a metal or semimetal monocation and a sacrificial anion does not necessarily form a compound that is evaporated or decomposed, and the desired effect of producing a uniform perovskite film is not fully obtained. In addition, in the method described in Non-Patent Document 1, lead acetate is hygroscopic, so film formation in an inert atmosphere is necessary, and the heating temperature for removing the absorbed moisture is high, making production difficult.

[0011] Furthermore, even in the methods described in Non-Patent Documents 2 and 3, the voltage loss in the photoelectric conversion element is still large compared to the band gap of CsPbI2Br perovskite, which is 1.92 eV, and it is difficult to say that a sufficiently high voltage is obtained.

[0012] The present invention is devised to solve the above problems, and has an object to provide a photoelectric conversion element that produces a higher voltage. [Means for solving the problem]

[0013] Therefore, the present inventors have conducted extensive research to solve the above problems. In the method disclosed in Non-Patent Document 3, an electron transport layer SnO2 is used as a base for an inorganic metal halide perovskite layer CsPbI2Br, and the surface is passivated with a SnCl2 solution to suppress recombination between the electron transport layer and the perovskite layer. The inventors have developed a method for preparing a SnCl2 solution used to treat the SnO2 film, which is different from the conventional method, to obtain a highly uniform Sn 4+ The inventors discovered that a SnO2 film containing the above-mentioned component can be obtained, and that a photoelectric conversion element that produces a high open circuit voltage can be easily obtained, thereby arriving at the invention. The present invention includes the following.

[0014] [1] A photoelectric conversion element having a pair of electrodes composed of an upper electrode and a lower electrode, and an active layer located between the pair of electrodes, An electron transport layer is provided between the active layer and at least one of the pair of electrodes, the electron transport layer contains SnO2, and Sn is detected by X-ray photoelectron spectroscopy (XPS) of the surface of the electron transport layer. 2+ Photoelectric conversion element where no components are detected. [2] The photoelectric conversion element according to [1], wherein the electron transport layer is a SnO2 film that has been surface-treated with a SnCl2 solution. [3] A photoelectric conversion element having a pair of electrodes composed of an upper electrode and a lower electrode, and an active layer located between the pair of electrodes, A photoelectric conversion element comprising an electron transport layer between the active layer and at least one of the pair of electrodes, the electron transport layer including a SnO2 film that has been surface-treated with a SnCl2 solution that has been exposed to the atmosphere for 24 hours or more. [4] A photoelectric conversion element having a pair of electrodes composed of an upper electrode and a lower electrode, and an active layer located between the pair of electrodes, A photoelectric conversion element comprising an electron transport layer between the active layer and at least one of the pair of electrodes, the electron transport layer including a non-crystalline SnO2 film on a surface in contact with the active layer.[5] The photoelectric conversion element according to [4], wherein the thickness of the non-crystalline SnO2 film is 1 nm or more and 50 nm or less. [6] The photoelectric conversion element according to any one of [1] to [5], wherein the electron transport layer has a band gap of 3.9 eV or more. [7] The photoelectric conversion element according to any one of [1] to [6], wherein the active layer contains an organic-inorganic hybrid semiconductor compound. [8] The photoelectric conversion element according to [7], wherein the organic-inorganic hybrid semiconductor compound is an inorganic metal halide perovskite compound. [9] The photoelectric conversion element according to any one of [1] to [8], further comprising a hole transport layer between the active layer and the other electrode of the pair of electrodes, the hole transport layer containing a polymer compound. Effect of the Invention

[0015] According to the present invention, it is possible to provide a photoelectric conversion element which easily produces a high open circuit voltage by a simple method. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a diagram illustrating a typical example of a photoelectric conversion element according to an embodiment of the present invention. [Diagram 2] 1 shows (a) the UV-Vis spectrum and the calculated ionization potential of the electron transport layer formed in the example. [Diagram 3] 1 shows the (b) chlorine atom Cl(2p) XPS spectrum of the electron transport layer formed in the example. [Figure 4] 3 shows the valence band spectrum (XPS) of (c) tin of the electron transport layer formed in the example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention will be described in detail below. However, the description of the constituent elements described below is one example (representative example) of an embodiment of the present invention, and the present invention is not limited to these contents, and can be implemented in various modifications within the scope of the gist of the present invention.

[0018] One embodiment of the present invention is a photoelectric conversion element having a pair of electrodes composed of an upper electrode and a lower electrode, and an active layer located between the pair of electrodes, The photoelectric conversion element includes an electron transport layer between the active layer and at least one of the pair of electrodes. The electron transport layer contains SnO2, and Sn is detected by X-ray photoelectron spectroscopy (XPS) of the surface of the electron transport layer. 2+ It is a photoelectric conversion element in which no components are detected. In this embodiment, the electron transport layer contains SnO2, and X-ray photoelectron spectroscopy (XPS) of the surface of the electron transport layer shows that Sn 2+ No Sn component was detected, i.e. the electron transport layer has high uniformity. 4+ By using these as components, a photoelectric conversion element with a high open circuit voltage can be obtained. Hereinafter, an explanation will be given with reference to FIG.

[0019] Fig. 1 is a cross-sectional view showing a schematic diagram of one embodiment of a photoelectric conversion element. The photoelectric conversion element shown in Fig. 1 has a structure of a photoelectric conversion element used in a general thin-film solar cell, but the photoelectric conversion element according to this embodiment is not limited to the structure shown in Fig. 1. In the photoelectric conversion element 100 shown in Fig. 1, a photoelectric conversion layer (active layer) 103 is located between a pair of electrodes composed of a lower electrode 101 and an upper electrode 105. In the photoelectric conversion element 100, an electron transport layer 102 is disposed between the lower electrode 101 and the photoelectric conversion layer 103, and a hole transport layer 104 is disposed between the upper electrode 105 and the photoelectric conversion layer 103. Furthermore, as shown in Fig. 1, the photoelectric conversion element 100 may have a base material 106, and may have other layers such as an insulator layer and a work function tuning layer.

[0020] The photoelectric conversion layer 103 is a layer where photoelectric conversion takes place. When the photoelectric conversion element 100 receives light, the light is absorbed by the photoelectric conversion layer 103 to generate carriers. The generated carriers are extracted from the lower electrode 101 and the upper electrode 105. In this embodiment, the photoelectric conversion layer 103 is generally a layer containing a semiconductor compound. It is preferably a layer containing an inorganic hybrid semiconductor compound, and more preferably contains an inorganic metal halide perovskite compound. Hereinafter, the photoelectric conversion layer will be described as a film containing a suitably used inorganic metal halide perovskite compound.

[0021] Inorganic metal halide perovskite compounds are (MA) a D3, where M is a first cation and A is a second cation. M is not particularly limited as long as it is a metal element that can provide a perovskite crystal, but it preferably contains Pb, and more preferably is Pb. A includes one selected from Cs, Rb, Cu, Pd, Pt, Ag, Au, Rh, and Ru, preferably includes Cs or Rb, more preferably includes Cs, and even more preferably is Cs. In the formula, D is a halogen, such as fluorine, chlorine, bromine, or iodine, and preferably contains iodine, and more preferably is a mixture of iodine and bromine. In the formula, a is 1±0.3, may be 1±0.2, or may be 1±0.1.

[0022] Although the method for producing a film containing an inorganic metal halide perovskite compound is not particularly limited, a preferred example is as follows: That is, the method includes a step of disposing a halide containing the first cation (M), a halide containing the second cation (A), and an organometallic compound containing the first cation (M) on a substrate (hereinafter also referred to as a disposing step), and a step of heating the halide and the organometallic compound on the substrate (hereinafter also referred to as a heating step).

[0023] The substrate used in the disposing step is not particularly limited as long as the above-mentioned halide and organometallic compound can be disposed thereon, and can be appropriately selected according to the application of the perovskite film. For example, when the organometallic halide perovskite film is used as a photoelectric conversion layer of a photoelectric conversion element, the above-mentioned halide and organometallic compound are disposed on a substrate such as PEN on which a lower electrode and an electron transport layer are formed.

[0024] The organometallic compound is an organometallic compound containing a first cation, preferably a carboxylate of the first cation, more preferably a metal propionate. Since the first cation preferably contains lead, the organometallic compound is preferably a carboxylate of lead, most preferably a propionate of lead. The number of carbon atoms in the carboxylate is not particularly limited, but is usually 1 or more, may be 2 or more, and is usually 18 or less, may be 12 or less, or may be 6 or less.

[0025] The halide having a first cation disposed on the substrate is preferably an iodide or a bromide, more preferably PbI2 or PbBr2 or both, and the halide having a second cation disposed on the substrate is preferably a bromide or an iodide, more preferably CsBr or CsI or both. The molar ratio of the halide having a first cation to the halide having a second cation placed on the substrate is not particularly limited, but is usually 1:0.85 to 1:1.15, and preferably 1:0.95 to 1:1.05. In addition, the molar ratio of the halide having a first cation to be placed on the substrate to the organometallic compound containing the first cation is not particularly limited, but is usually 10 or more, and preferably 15 or more, in terms of halide / organometallic compound.

[0026] The method for disposing the halide and the organometallic compound on the substrate is not particularly limited, but typically a coating method is used. For example, a coating liquid is prepared by mixing a mixture of a halide and a solvent and a mixture of an organometallic compound and a solvent, and the coating liquid is applied. The solvent is not particularly limited as long as it dissolves the halide and the organometallic compound, and examples of the solvent include organic solvents such as N,N-dimethylformamide and dimethylsulfoxide.

[0027] Any method can be used as a method for applying the coating liquid, and examples thereof include spin coating, inkjet coating, doctor blade coating, drop casting, reverse roll coating, gravure coating, kiss coating, roll brush coating, spray coating, air knife coating, wire barber coating, pipe doctor coating, impregnation / coating, and curtain coating.

[0028] The heating step is a step of forming an inorganic metal halide perovskite film by heating the halide and organometallic compound placed on the substrate. The heating temperature is not particularly limited, but is usually 350° C. or lower, and preferably 300° C. or lower. There is no lower limit, but it is usually 100° C. or higher, and preferably 150° C. or higher. The heating atmosphere in the heating step is not particularly limited, and may be air or an inert gas atmosphere. If the heating step is in air, the relative humidity is preferably 30% or less. The heating time is not particularly limited, and may be usually 1 minute or more, 5 minutes or more, and is usually 60 minutes or less, and may be 30 minutes or less.

[0029] The inorganic metal halide perovskite film formed by the heating step is produced by the following reaction when the halide containing the first cation is PbI2, the halide containing the second cation is CsBr, and the organometallic compound is lead propionate. Pb(CH3CH2COO)2+PbI2+CsBr+2H2O → CsPbI2Br+2CH3CH2COOH(gas)+Pb(OH)2

[0030] The thickness of the photoelectric conversion layer is not particularly limited, but is usually 100 nm or more, preferably 150 nm or more, and is usually 1000 nm or less, preferably 700 nm or less.

[0031] The electrode has a function of collecting holes and electrons generated by light absorption in the photoelectric conversion layer 103. The photoelectric conversion element 100 according to an embodiment has a pair of electrodes, one of which is called an upper electrode and the other is called a lower electrode. When the photoelectric conversion element 100 has a substrate or is provided on a substrate, the electrode closer to the substrate can be called a lower electrode, and the electrode farther from the substrate can be called an upper electrode. In addition, a transparent electrode can be called a lower electrode, and an electrode less transparent than the lower electrode can be called an upper electrode. The photoelectric conversion element 100 shown in FIG. 1 has a lower electrode 101 and an upper electrode 105.

[0032] The pair of electrodes may be an anode suitable for collecting holes and a cathode suitable for collecting electrons. In this case, the photoelectric conversion element 100 may have a forward configuration in which the lower electrode 101 is an anode and the upper electrode 105 is a cathode, or may have an inverted configuration in which the lower electrode 101 is a cathode and the upper electrode 105 is an anode.

[0033] Either one of the pair of electrodes may be light-transmitting, or both may be light-transmitting. Light-transmitting refers to transmitting 40% or more of sunlight. In addition, a sunlight transmittance of 70% or more of the transparent electrode is preferable so that more light passes through the transparent electrode and reaches the active layer 103. The light transmittance can be measured with a spectrophotometer (e.g., U-4100 manufactured by Hitachi High-Technologies Corporation).

[0034] When the lower electrode and / or the upper electrode are transparent electrodes, the lower electrode and / or the upper electrode are As long as it has the above-mentioned visible light transmittance, it may be formed as a single layer of a transparent conductive layer or a metal layer, or may be formed by laminating a transparent conductive layer and a metal layer. However, if the transparent electrode is formed only from a transparent conductive layer, it may have a high resistance and tend not to show good conductivity, so that the conversion efficiency may decrease. In addition, if the transparent electrode is formed only from a thin metal layer, the metal layer is easily corroded and the photoelectric conversion element tends to deteriorate over time, so that the electrode to be the transparent electrode is preferably formed by laminating a transparent conductive layer and a metal layer.

[0035] The material used for the transparent conductive layer is not particularly limited, but may be tin-doped indium oxide (ITO), zinc-doped indium oxide (IZO), tungsten-doped indium oxide (IWO), zinc-aluminum oxide (AZO), indium oxide (In2O3), etc. Among these, it is preferable to use amorphous oxides such as tin-doped indium oxide (ITO), zinc-doped indium oxide (IZO), tungsten-doped indium oxide (IWO), and zinc-tin composite oxide (ZTO).

[0036] Furthermore, the transparent conductive layer preferably has a sheet resistance of 100 Ω / □ or less, more preferably 50 Ω / □ or less, and more preferably 0.1 Ω / □ or more.

[0037] The material of the metal layer is not particularly limited, and examples thereof include metals such as gold, platinum, silver, aluminum, nickel, titanium, magnesium, calcium, barium, sodium, chromium, copper, and cobalt, or alloys thereof. Among these, the material forming the metal layer is preferably silver or a silver alloy, which exhibits high electrical conductivity and has a high visible light transmittance in a thin film. Examples of silver alloys include silver-gold alloys, silver-copper alloys, silver-palladium alloys, silver-copper-palladium alloys, and silver-platinum alloys, which are less susceptible to sulfurization or chlorination and improve the stability of the thin film.

[0038] The film thickness of the metal layer is not particularly limited as long as it can maintain a visible light transmittance of 70% or more as a transparent electrode, but in order to obtain good electrical conductivity, it is preferably 1 nm or more, and more preferably 5 nm or more, while in order to prevent a decrease in the amount of light incident on the active layer due to a decrease in light transmittance, it is preferably 15 nm or less, and more preferably 10 nm or less.

[0039] As described above, if one of the pair of electrodes is a transparent electrode, the other electrode does not necessarily have to be a transparent electrode, and may be a non-transparent electrode. When a non-transparent electrode is used, there is no particular limitation, but for example, the non-transparent electrode can be formed by thickening the metal layer as described above. In addition, when both the lower electrode and the upper electrode are transparent electrodes, it is preferable that both the lower electrode and the upper electrode have a laminated structure of a metal layer and a transparent conductive layer.

[0040] The total thickness of the lower electrode and the upper electrode is not particularly limited and may be arbitrarily selected in consideration of the optical and electrical properties. In particular, in order to suppress the sheet resistance, the film thickness of each of the lower electrode and the upper electrode is preferably 10 nm or more, more preferably 20 nm or more, and even more preferably 50 nm or more, while in order to maintain a high transmittance, it is preferably 10 μm or less, more preferably 1 μm or less, and even more preferably 500 nm or less.

[0041] The method for forming the lower electrode and the upper electrode is not particularly limited, and they can be formed by a known method according to the material used. Examples of the film formation step in coating include vacuum methods such as deposition and sputtering, and wet methods in which ink containing nanoparticles or precursors is applied. The lower electrode and the upper electrode may be surface-treated to improve electrical properties, wettability, and the like.

[0042] The hole transport layer 104 is a layer located between the photoelectric conversion layer 103 and the electrode 105. The hole transport layer 104 can be used, for example, to improve the efficiency of carrier movement from the photoelectric conversion layer 103 to the upper electrode 105.

[0043] The hole transport layer is not particularly limited, and any known hole transport material can be used. However, it preferably contains a polymer compound, and more preferably contains a hole transport material represented by the following composition formula: [ka] In the above composition formula, n is an integer, preferably 5 or more, and 1,000 or less. In addition, the molecular weight is preferably 2,000 or more and 200,000 or less.

[0044] The hole transport material may be a metal oxide. Examples of the metal oxide include molybdenum dioxide, molybdenum trioxide, copper oxide, and nickel oxide. These metal oxides may be laminated on the hole transport layer described in the above composition formula.

[0045] The hole transport layer is preferably formed by a coating method similar to the inorganic metal halide perovskite film, the details of which are as described above in the section on the inorganic metal halide perovskite film. The thickness of the hole transport layer is not particularly limited, but is usually 5 nm or more, preferably 10 nm or more, and is usually 1000 nm or less, preferably 600 nm or less.

[0046] The electron transport layer 102 is a layer located between the photoelectric conversion layer 103 and the electrode 101. That is, the electron transport layer 102 is provided between the photoelectric conversion layer and one of a pair of electrodes. The electron transport layer 102 can be used, for example, to improve the efficiency of carrier movement from the photoelectric conversion layer 103 to the lower electrode 101.

[0047] In this embodiment, the electron transport layer 102 contains tin oxide (SnO2). The electron transport layer 102 may contain other substances as long as it contains SnO2, but it is preferable that the electron transport layer 102 contains SnO2 on its surface, and is more preferable that the electron transport layer 102 is a SnO2 film. In addition, the SnO2 film is preferably a SnO2 film that has been surface-treated with a SnCl2 solution. In addition, it is preferable that the surface in contact with the photoelectric conversion layer 103 contains an amorphous SnO2 film. The surface of the electron transport layer 102 may have an amorphous portion, and Sn 2+ No peaks attributed to the component were detected. Sn 2+ Since no peaks attributable to the component were detected, it is understood that the electron transport layer 102 has high uniformity. 4+ The photoelectric conversion element 100 has a high open circuit voltage.

[0048] X-ray photoelectron spectroscopy (XPS) revealed that Sn 2+The term "no component is detected" means that no peak (absorption maximum) or sub-peak (inflection point) attributable to the Sn (5s) orbital is observed in the valence band spectrum region, which reflects the difference in the electron configuration of the Sn atom. XPS measurements can be performed using, for example, KRATOS AXIS SUPRA manufactured by Shimadzu Corporation.

[0049] The electron transport layer is preferably formed by a coating method, similar to the inorganic metal halide perovskite film, and more preferably, after forming the SnO2 film by the coating method, the SnO2 film is surface-treated with a SnCl2 solution exposed to the atmosphere for 24 hours or more. Non-Patent Document 3 discloses that the SnO2 film is surface-treated (passivated) with a SnCl2 solution, and the passivation treatment can suppress recombination between the electron transport layer and the perovskite layer. The present inventors have been studying a photoelectric conversion element that produces a higher open circuit voltage, and have produced a highly uniform SnO2 film having an amorphous portion preferably having a thickness of 1 nm to 50 nm by exposing the SnCl2 solution for surface treatment to the air for 24 hours or more and then surface-treating the SnO2 film with the SnCl2 solution. 4+ It was found that a SnO2 film containing the above components could be obtained, resulting in a photoelectric conversion element that produces a high open circuit voltage.

[0050] The details of the coating method are as described in the section on inorganic metal halide perovskite films. The SnCl2 concentration of the SnCl2 solution for surface treatment of the SnO2 film is not particularly limited, but is usually 0.01 mol / L (M) or more in terms of Sn atoms, preferably 0.05 mol / L or more, and 1 mol / L or less, preferably 0.5 mol / L or less. The solvent of the SnCl2 solution may be an aqueous solvent or an organic solvent, but is preferably a mixed solvent containing a polar solvent. The exposure time of the SnCl2 solution to the atmosphere should be at least 24 hours, but not less than 36 hours. It is preferable that the time is 240 hours or less, and it is usually 120 hours or less. The time for surface treatment of the SnO2 film using the SnCl2 solution (contact time with the solution) is not particularly limited, but is usually at least 1 second, preferably at least 5 seconds, and is usually not more than 10 minutes, preferably not more than 5 minutes. The treatment temperature for the surface treatment of the SnO2 film using the SnCl2 solution is not particularly limited, and may be room temperature.

[0051] The thickness of the electron transport layer is not particularly limited, but when a mesoporous metal oxide is used, it is usually 20 nm or more and preferably 250 nm or less, and more preferably 50 nm or more and 150 nm or less. When such an electron transport layer is used, the thickness of the electron transport layer is usually 10 nm or more, preferably 120 nm or less, and more preferably 20 nm or more and 80 nm or less. The band gap of the electron transport layer is preferably 3.9 eV or more.

[0052] The photoelectric conversion element 100 generally has a substrate 106 that serves as a support. The material of the substrate 106 is not particularly limited as long as it does not significantly impair the effects of the present invention, and may be any material described in known documents such as International Publication No. WO 2013 / 171517, International Publication No. WO 2013 / 180230, or JP 2012-191194 A.

[0053] The photoelectric conversion element 100 may have other layers. For example, the photoelectric conversion element 100 may have a work function tuning layer for adjusting the work function of the electrode between the lower electrode 101 and the electron transport layer 102, or between the upper electrode 105 and the hole transport layer 104. The photoelectric conversion element 100 may also have a thin insulator layer between the lower electrode 101 and the photoelectric conversion layer 103, or between the upper electrode 105 and the photoelectric conversion layer 103, for preventing moisture and the like from reaching the photoelectric conversion layer 103. In addition, the photoelectric conversion element 100 may be further sealed to improve durability. For example, the photoelectric conversion element 100 can be sealed by further laminating a sealing plate on the upper electrode 105 and fixing the base material 106 and the sealing plate with an adhesive.

[0054] According to the above-mentioned method, the photoelectric conversion element 100 can be manufactured by forming each layer constituting the photoelectric conversion element 100. There is no particular limitation on the method for forming each layer constituting the photoelectric conversion element 100, and the layers can be formed by a sheet-to-sheet method or a roll-to-roll method.

[0055] The roll-to-roll method is a method in which a flexible substrate wound in a roll is unwound and processed while being transported intermittently or continuously until it is wound up by a take-up roll. The roll-to-roll method allows long substrates on the order of kilometers to be processed in one go, making it more suitable for mass production than the sheet-to-sheet method. However, when attempting to deposit each layer using the roll-to-roll method, due to its structure, the film may be scratched or partially peeled off due to contact between the deposition surface and the roll.

[0056] Furthermore, after laminating the upper electrode 105, the photoelectric conversion element 100 can be heated at a temperature range of 50° C. or higher in one embodiment, 80° C. or higher in another embodiment, 300° C. or lower in one embodiment, 280° C. or lower in another embodiment, and 250° C. or lower in still another embodiment (this step may be referred to as an annealing treatment step). By carrying out the annealing treatment step at a temperature of 50° C. or higher, the effect of improving the adhesion between the layers of the photoelectric conversion element 100, for example, between the electron transport layer 102 and the lower electrode 101, between the electron transport layer 102 and the photoelectric conversion layer 103, etc., can be obtained. By improving the adhesion between the layers, This can improve the thermal stability, durability, etc. of the photoelectric conversion element. Setting the temperature in the annealing process to 300° C. or less reduces the possibility of thermal decomposition of the organic compound contained in the photoelectric conversion element 100. In the annealing process, stepwise heating using different temperatures within the above temperature range may be performed.

[0057] The heating time is 1 minute or more in one embodiment, 3 minutes or more in another embodiment, 180 minutes or less in one embodiment, and 60 minutes or less in another embodiment, in order to improve adhesion while suppressing thermal decomposition. The annealing process can be terminated when the open circuit voltage, short circuit current, and fill factor, which are parameters of the solar cell performance, reach a certain value. In addition, the annealing process can be performed under normal pressure and in an inert gas atmosphere in order to prevent thermal oxidation of the constituent materials. As a heating method, the photoelectric conversion element may be placed on a heat source such as a hot plate, or the photoelectric conversion element may be placed in a heating atmosphere such as an oven. In addition, the heating may be performed in a batch manner or a continuous manner.

[0058] The photoelectric conversion characteristics of the photoelectric conversion element 100 can be determined for each light source used as follows. Light is irradiated onto the photoelectric conversion element 100, and the current-voltage characteristics are measured. From the obtained current-voltage curve, photoelectric conversion characteristics such as photoelectric conversion efficiency (PCE), short-circuit current density (Jsc), open circuit voltage (Voc), fill factor (FF), series resistance, and shunt resistance can be determined.

[0059] The light source used to determine the photoelectric conversion characteristics can be sunlight or an artificial light source, such as a halogen lamp, a xenon lamp, a metal halide lamp, a fluorescent lamp, a white LED lamp, an incandescent LED lamp, a mercury lamp, a sodium lamp, or a combination of these lamps.

[0060] Generally, xenon lamps or metal halide lamps are used as light sources for artificial sunlight, and light with conditions similar to the AM1.5G spectrum is emitted at an irradiation intensity of 100 mW / cm. 2 In addition, although there are no particular limitations on the low-illuminance light source, a white LED lamp is used and used as a measurement light source to obtain the photoelectric conversion characteristics at an illuminance of 1 to 5000 Lx.

[0061] The photoelectric conversion efficiency of the photoelectric conversion element 100 is not particularly limited, but is 5% or more in one embodiment, 8% or more in another embodiment, and 10% or more in yet another embodiment. On the other hand, there is no particular limit on the upper limit, and the higher the better. In addition, there is no particular limit on the fill factor of the photoelectric conversion element 100, but is 0.6 or more in one embodiment, 0.7 or more in another embodiment, and 0.75 or more in yet another embodiment. On the other hand, there is no particular limit on the upper limit, and the higher the better.

[0062] The photoelectric conversion element according to this embodiment has a maximum output (Pmax) retention rate of 60% or more, 80% or more in one embodiment, 90% or more in another embodiment, and 95% or more in still another embodiment after being placed in a test environment at a temperature of 85° C. for one day. For example, the Pmax retention rate can be calculated based on the initial Pmax immediately after the photoelectric conversion element is produced and the Pmax after the photoelectric conversion element is placed in the test environment. The Pmax retention rate can also be measured after sealing the photoelectric conversion element as described above. Here, the Pmax retention rate can be calculated as follows based on the Pmax before and after being placed in the test environment. Pmax maintenance rate (%) = ((Pmax after being placed in the test environment) / (Pmax before being placed in the test environment)) x 100

[0063] In addition, Pmax after being left in a test environment at 85°C for a long period of time (e.g., 60 hours or more) The retention rate is 40% or more, in one embodiment 60% or more, in another embodiment 80% or more, in yet another embodiment 90% or more, and in yet another embodiment 95% or more.

[0064] The photoelectric conversion element 100 can be suitably used as a solar cell, particularly as a solar cell element of a thin-film solar cell. When used as a thin-film solar cell, a known configuration can be applied. EXAMPLES

[0065] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to the following examples.

[0066] [Example 1] (Preparation of Coating Solution for Electron Transport Layer) A coating solution for the electron transport layer was prepared by diluting an aqueous colloidal dispersion (15%) of tin oxide (manufactured by Alfa Aesar) to 1 / 10 with ultrapure water.

[0067] (Preparation of SnCl2 solution for surface treatment) A SnCl2 solution for surface treatment was prepared by dissolving 189 mg of tin(II) chloride (Wako Pure Chemical Industries, Ltd., purity 99.9%) in 10 mL of ethanol, adding 36 μL of water, rotating and stirring in air for 1 hour, and then storing at room temperature for more than 24 hours.

[0068] (Preparation of coating solution for active layer (photoelectric conversion layer)) Lead iodide (II) and cesium bromide were weighed in a vial in a molar ratio of 1:1 in air. Next, lead propionate was weighed in a vial. Next, N,N-dimethylformamide and dimethyl sulfoxide were added as solvents to each vial in a volume ratio of 6:4, and stirred at room temperature for 1 hour to prepare a 1.0 mol / L perovskite precursor solution, i.e., a coating solution for the photoelectric conversion layer. The coating solution for the photoelectric conversion layer was further stirred for 30 minutes and then filtered through a PTFE filter with a pore size of 0.45 μm.

[0069] (Preparation of Coating Solution for Hole Transport Layer) 7 mg of polymer compound was weighed in a vial, 1.0 mL of dehydrated chlorobenzene was added, and the mixture was dissolved by ultrasonication for 60 minutes. The mixture was then filtered through a PTFE filter with a hole diameter of 0.45 μm to prepare a coating solution for the hole transport layer. The polymer compound used was Poly(DTSTPD-r-BThTPD) with the following structure. [ka]

[0070] (Fabrication of photoelectric conversion element) The ITO substrate was washed with an alkaline cleaner (Hellmanex III) with a volume concentration of 2%. The ITO substrate was ultrasonically cleaned with an aqueous solution, then rinsed with water and ultrasonically cleaned with ethanol. The ITO substrate was then subjected to a 10-minute UV ozone treatment. Next, the previously prepared electron transport layer coating solution was spin-coated on the ITO substrate at 5000 rpm for 30 seconds, and heated on a hot plate at 150° C. for 40 minutes. Next, the surface treatment SnCl2 solution was spin-coated at 6000 rpm for 30 seconds, placed on a hot plate, heated at 100° C. for 10 minutes, and further heated at 180° C. for 1 hour to form an electron transport layer.

[0071] Next, in an atmosphere with a relative humidity of 30%, the coating solution for the photoelectric conversion layer was dropped onto the ITO substrate on which the electron transport layer had been formed, and spin-coated at 1000 rpm for 10 seconds and at 3000 rpm for 30 seconds to form a thin film. The thin film was then stored in the atmosphere for 10 minutes, and then heated on a hot plate at 180°C for 10 minutes to form a perovskite photoelectric conversion layer. Next, after the substrate was returned to room temperature, the hole transport layer coating liquid was spin-coated on the photoelectric conversion layer at 4000 rpm for 30 seconds to form a hole transport layer. Next, gold was evaporated onto the hole transport layer by a resistance heating type vacuum evaporation method to form a metal layer. In this manner, a photoelectric conversion element was produced.

[0072] In the photoelectric conversion element thus fabricated, the electron transport layer formed on the ITO substrate had a thickness of approximately 20 nm. Analysis of the composition of the layer revealed that the main component of the electron transport layer was SnO2, with all Sn being tetravalent metal ions (Sn 4+ ) and the divalent metal Sn (Sn 2+ ) was not detected.

[0073] The crystallinity of the electron transport layer made of SnO2 was examined by X-ray diffraction and it was found that the surface of the electron transport layer contained non-crystalline (amorphous) tin oxide (SnO x) was formed, and its thickness was distributed in the range of 5 nm to 10 nm. In addition, as a result of forming various SnO2 films by changing the spin coating conditions, the thickness of the amorphous film was in the range of 1 nm to 50 nm. The properties of the electron transport layer in Example 1 and Comparative Example 1 are shown in Table 1.

[0074] [Table 1]

[0075] [Comparative Example 1] A photoelectric conversion element was produced in the same manner as in Example 1, except that the SnCl2 solution for surface treatment was not stored in the air when the solution was prepared, but was immediately used for the surface treatment of the electron transport layer.

[0076] FIG. 2 shows (a) the UV-Vis spectrum and the calculated ionization potential of the electron transport layer formed under the same conditions as in Example 1. FIG. 3 shows (b) the chlorine atom Cl(2p) XPS spectrum of the electron transport layer formed under the same conditions as in Example 1. Furthermore, the valence band spectrum (XPS) of (c) tin of the electron transport layer formed under the same conditions as in Example 1 is shown in FIG. Here, A-SnO2 is the electron transport layer in Example 1, and F-SnO2 is the electron transport layer in Comparative Example 1.

[0077] [Evaluation of photoelectric conversion elements] The current-voltage characteristics between the lower transparent electrode (FTO) and the upper electrode were measured for the photoelectric conversion elements obtained in Example 1 and Comparative Example 1. A source meter (Model 2400, manufactured by Keithley) was used for the measurement, and the irradiation light source was air mass (AM) 1.5G and irradiance 100mW / cm 2 A solar simulator of this type was used. From the measurement results, the photoelectric conversion efficiency PCE (%) was calculated. These values, which were calculated based on the measurement results immediately after the photoelectric conversion element was fabricated, are shown in Table 2.

[0078] [Table 2]

[0079] As described above, in the photoelectric conversion element obtained in this embodiment, the Sn having high uniformity as the electron transport layer is 4+ The components are amorphous SnO x It is found that a SnO2 film having the following characteristics can be obtained, and that this structure makes it possible to easily manufacture a photoelectric conversion element that produces a high open circuit voltage and photoelectric conversion efficiency. [Explanation of symbols]

[0080] 100 Photoelectric conversion element 101 Lower electrode 102 Electron transport layer 103 Active layer 104 Hole transport layer 105 Upper electrode 106 Base material

Claims

1. A method for manufacturing a photoelectric conversion element having a pair of electrodes composed of an upper electrode and a lower electrode, and an active layer located between the pair of electrodes, comprising the steps of: An electron transport layer is provided between the active layer and at least one of the pair of electrodes, and the electron transport layer is made of SnO 2 and in X-ray photoelectron spectroscopy (XPS) of the surface of the electron transport layer, Sn 2+ This is a layer where the component is not detected. The electron transport layer was exposed to the atmosphere for 24 hours or more. 2 A method for producing a photoelectric conversion element, comprising a step of performing a surface treatment with a solution.

2. The method for producing a photoelectric conversion element according to claim 1 , further comprising heating during the surface treatment.

3. The method for producing a photoelectric conversion element according to claim 1 , wherein the electron transport layer has a band gap of 3.9 eV or more.

4. The method for producing a photoelectric conversion element according to any one of claims 1 to 3, wherein the active layer contains an organic-inorganic hybrid semiconductor compound.

5. The method for producing a photoelectric conversion element according to any one of claims 1 to 3, wherein the active layer contains an inorganic metal halide perovskite compound.

6. The method for producing a photoelectric conversion element according to any one of claims 1 to 5, wherein the photoelectric conversion element comprises a hole transport layer between the active layer and the other electrode of the pair of electrodes, and the hole transport layer contains a polymer compound.

Citation Information

Patent Citations

  • Method utilizing low temperature solution reaction to prepare SnO2 film and method utilizing SnO2 film to prepare perovskite solar energy cell

    CN108054281A

  • Preparation method of planar perovskite solar cell

    CN109904328A

  • Two-component interface hybrid electron transport layer and preparation method and application thereof

    CN109994610A

  • Photoelectric conversion element arranged by use of perovskite compound, and method for manufacturing the same

    JP2016096277A

  • Photoelectric conversion element

    JP2016164915A