Interlayer film for laminated glass and laminated glass

The interlayer film for laminated glass, with a structured resin layer, addresses the issue of varying sound insulation across temperatures, ensuring effective noise reduction from 0°C to 50°C.

JP7569150B2Active Publication Date: 2024-10-17SEKISUI CHEMICAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2019515564
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-02-02
Filing Date
2019-01-30
Publication Date
2024-10-17
Estimated Expiration
2039-01-30

AI Technical Summary

Technical Problem

Conventional laminated glass using interlayer films does not provide effective sound insulation over a wide temperature range, with sound insulation properties decreasing when used at temperatures different from the specific temperature at which they are optimized.

Method used

An interlayer film for laminated glass with a one-layer or multi-layer structure, incorporating a resin layer, designed to maintain a specific ratio of storage moduli and primary loss coefficient across a wide temperature range, enhancing sound insulation properties from 0°C to 50°C.

Benefits of technology

The interlayer film improves sound insulation across a wide temperature range by reducing engine and road noise, maintaining high sound insulation properties from 0°C to 50°C.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569150000005
    Figure 0007569150000005
  • Figure 0007569150000006
    Figure 0007569150000006
  • Figure 0007569150000007
    Figure 0007569150000007
Patent Text Reader

Abstract

To provide an interlayer film for laminated glass that can enhance sound insulation over a wide temperature range of 0°C to 40°C. The interlayer film for laminated glass according to the present invention is an interlayer film for laminated glass having a single-layer structure or a two or more-layer structure, the interlayer film includes a resin layer, and in viscoelasticity measurement of the interlayer film at a frequency of 1 Hz in shear mode, the ratio of a first storage modulus G' at the peak temperature of the maximum peak of tan δ to a second storage modulus G' at a temperature 100°C higher than the peak temperature of the maximum peak of tan δ is 50 or more and 500 or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an interlayer film for laminated glass used to obtain laminated glass. The present invention also relates to laminated glass using the interlayer film for laminated glass. [Background technology]

[0002] Even if laminated glass is broken by an external impact, the amount of glass fragments scattered is small, and therefore, laminated glass is excellent in safety. For this reason, the laminated glass is widely used in automobiles, railroad cars, aircraft, ships, buildings, etc. The laminated glass is manufactured by sandwiching an interlayer film for laminated glass between two glass sheets.

[0003] As an example of the interlayer film for laminated glass, the following Patent Document 1 discloses an interlayer film having a sound insulation layer formed from a composition (A) containing at least one resin (a1) selected from thermoplastic resins and thermosetting resins. The dynamic viscoelasticity of a sheet formed from the composition to a thickness of 0.8 mm was measured at a frequency of 0.3 Hz in a tensile mode, and the tan δ obtained was A In the above dynamic viscoelasticity measurement, T A (℃) is in the range of -50 to 50℃, T A The tan δ at (°C) is 2.5 or more.

[0004] In Patent Document 1, the thermoplastic resins include polyvinyl acetal, polyvinyl alcohol, polyurethane, polyvinyl carboxylate, olefin-vinyl carboxylate copolymer, polyurethane elastomer, polyester elastomer, styrene-diene block copolymer, and chlorinated polyolefin, while the thermosetting resins include epoxy resin, phenol resin, urethane resin, melamine resin, and unsaturated polyester resin.

[0005] Patent Document 1 also describes that the above interlayer film has high sound insulation properties. In the examples of Patent Document 1, the temperature at which the average sound transmission loss was the largest and the sound transmission loss (average value at multiple frequencies) at the temperature at which the average sound transmission loss was the largest are described as measurement results of sound transmission loss at temperatures of 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, and 40°C.

[0006] Furthermore, the following Patent Document 2 discloses a viscoelastic plastic insert (interlayer). Patent Document 2 describes the shear modulus G' of the insert at 10°C to 50°C. Patent Document 2 also describes the dynamic loss factor tan δ of the insert at 10°C to 50°C. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] WO2017 / 170259A1 [Patent Document 2] WO2007 / 135317A1 Summary of the Invention [Problem to be solved by the invention]

[0008] Laminated glass using an interlayer film is used in various temperature environments. Conventional laminated glass using an interlayer film may not be able to improve sound insulation over a wide temperature range. Even if a laminated glass has high sound insulation at one specific temperature, the sound insulation may be reduced when the laminated glass is used at a temperature other than that temperature.

[0009] Patent Document 1 also describes that the above interlayer film has high sound insulation. However, while Patent Document 1 evaluates sound transmission loss at temperatures of 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, and 40°C, it does not describe the results of sound transmission loss at each of the multiple temperatures. Patent Document 1 does not show by examples that sound insulation is high over a wide temperature range.

[0010] Patent Document 2 describes the dynamic loss factor tan δ at temperatures of 10° C., 20° C., 30° C., 40° C., and 50° C. However, there is no example showing that the sound insulation is high over a wide temperature range including 0° C. to 10° C.

[0011] An object of the present invention is to provide an interlayer film for laminated glass that can improve sound insulation over a wide temperature range of 0° C. to 40° C. Another object of the present invention is to provide laminated glass using the interlayer film for laminated glass.

[0012] A further object of the present invention is to provide an interlayer film for laminated glass that can enhance sound insulation over a wide temperature range of 0°C to 50°C. [Means for solving the problem]

[0013] According to a broad aspect of the present invention, there is provided an interlayer film for laminated glass (hereinafter sometimes simply referred to as interlayer film) having a one-layer structure or a two or more layer structure, the interlayer film comprising a resin layer, and in viscoelasticity measurement of the interlayer film at a frequency of 1 Hz in a shear mode, the ratio of a first storage modulus G' at the peak temperature of the maximum peak of tan δ to a second storage modulus G' at a temperature 100°C higher than the peak temperature of the maximum peak of tan δ is 50 or more and 500 or less.

[0014] In one particular aspect, the interlayer film according to the present invention is an interlayer film for laminated glass having a structure of two or more layers.

[0015] In a specific aspect of the interlayer film according to the present invention, the maximum peak value of tan δ is 2.0 or more.

[0016] In a specific aspect of the interlayer film according to the present invention, laminated glass X obtained through the following first, second, and third steps has a primary loss factor of 0.15 or more over the entire temperature range of 0°C or higher and 40°C or lower, when mechanical impedance is measured in accordance with ISO 16940.

[0017] First step: Prepare an interlayer film having a width of 25 mm and a length of 300 mm. Prepare two pieces of clear float glass conforming to JIS R3202, each having a thickness of 2.0 mm, a width of 25 mm, and a length of 300 mm. The interlayer film is sandwiched between the two pieces of clear float glass to obtain a laminate X.

[0018] Second step: The obtained laminate X is placed in a rubber bag and degassed at a vacuum of 2.6 kPa for 20 minutes. Then, in the degassed state, it is transferred to an oven and held at 90°C for a further 30 minutes, where it is vacuum pressed to pre-press the laminate X.

[0019] Third step: The pre-bonded laminate X is subjected to compression bonding in an autoclave at 135° C. and a pressure of 1.2 MPa for 20 minutes to obtain laminated glass X.

[0020] In a specific aspect of the interlayer film according to the present invention, the laminated glass X has a primary loss factor of 0.15 or more over the entire temperature range of 0° C. or more and 50° C. or less, in mechanical impedance measurement in accordance with ISO 16940.

[0021] In a specific aspect of the interlayer film according to the present invention, the peak temperature of the maximum peak of tan δ is -20°C or higher and 20°C or lower.

[0022] In a specific aspect of the interlayer film according to the present invention, the interlayer film has a layer containing a cured material as the resin layer, and the cured material is a cured material obtained by curing a photocurable compound or a moisture-curable compound.

[0023] In a specific aspect of the interlayer film according to the present invention, the cured product is a cured product obtained by curing a photocurable compound.

[0024] In a specific aspect of the interlayer film according to the present invention, the interlayer film includes a layer containing a cured material as the resin layer, and the cured material is a cured material obtained by curing a curable compound having a (meth)acryloyl group.

[0025] In a specific aspect of the interlayer film according to the present invention, the interlayer film has, as the resin layer, a layer containing a resin different from each of the cured product obtained by curing a photocurable compound, the cured product obtained by curing a moisture-curable compound, and the cured product obtained by curing a curable compound having a (meth)acryloyl group.

[0026] In a specific aspect of the interlayer film according to the present invention, the interlayer film has a layer containing the cured product as a first resin layer, and the interlayer film has a layer containing a resin different from the cured product obtained by curing a photocurable compound, the cured product obtained by curing a moisture-curable compound, and the cured product obtained by curing a curable compound having a (meth)acryloyl group as a second resin layer.

[0027] In a specific aspect of the interlayer film according to the present invention, the resin contained in the resin-containing layer is a polyvinyl acetal resin.

[0028] In a specific aspect of the interlayer film according to the present invention, when a sound transmission loss measurement including the following first, second, third, fourth and fifth steps is performed, the interlayer film satisfies the following first feature and the following second feature.

[0029] First configuration: The sound transmission loss at 500 Hz or more and 1000 Hz or less satisfies the following formula (1).

[0030] y≧10.1ln(x)-35...Equation (1)

[0031] In formula (1), x represents frequency (Hz) and y represents sound transmission loss (dB).

[0032] Second configuration: The sound transmission loss in the range of 5000 Hz or more and 10000 Hz or less satisfies the following formula (2).

[0033] y≧12.8ln(x)-68...Equation (2)

[0034] In formula (2), x represents frequency (Hz) and y represents sound transmission loss (dB).

[0035] First step: An interlayer film measuring 500 mm in length and 500 mm in width is prepared. Two sheets of green glass measuring 2 mm in thickness, 500 mm in length and 500 mm in width are prepared. The interlayer film is sandwiched between the two sheets of green glass to obtain a laminate Y.

[0036] Second step: The obtained laminate Y is placed in a rubber bag and degassed at a vacuum of 2.6 kPa for 20 minutes. Then, while still degassed, it is transferred to an oven and held at 90°C for a further 30 minutes to vacuum press and pre-press the laminate Y.

[0037] Third step: The pre-bonded laminate Y is compressed in an autoclave at 135°C and a pressure of 1.2 MPa for 20 minutes, and then stored in an environment of room temperature of 23±2°C and humidity of 25±5% for 84 weeks to obtain laminated glass Y.

[0038] Fourth step: Prepare a reverberation chamber conforming to ISO 10140-5, in which a first reverberation chamber, which is a sound source chamber, and a second reverberation chamber, which is a sound receiving chamber, are connected. The obtained laminated glass Y is installed between the first reverberation chamber and the second reverberation chamber.

[0039] Fifth step: The sound transmission loss at 20°C is measured in a center frequency 1 / 3 octave band by the intensity method in accordance with JIS A1441-1.

[0040] According to a broad aspect of the present invention, there is provided an interlayer film for laminated glass (hereinafter sometimes referred to as interlayer film) having a one-layer structure or a two or more layer structure, the interlayer film comprising a resin layer, and satisfying the following first configuration and the following second configuration when a sound transmission loss measurement including the above-mentioned first, second, third, fourth and fifth steps is carried out.

[0041] According to a broad aspect of the present invention, there is provided laminated glass comprising a first laminated glass component, a second laminated glass component, and the above-mentioned interlayer film for laminated glass, with the interlayer film for laminated glass being disposed between the first laminated glass component and the second laminated glass component.

[0042] According to a broad aspect of the present invention, there is provided a laminated glass comprising a first laminated glass component, a second laminated glass component, and an interlayer film for laminated glass, the interlayer film having a single-layer structure or a two or more-layer structure, the interlayer film comprising a resin layer, and in viscoelasticity measurement of the interlayer film at a frequency of 1 Hz in a shear mode, the ratio of a first storage modulus G' at the peak temperature of the maximum peak of tan δ to a second storage modulus G' at a temperature 100°C higher than the peak temperature of the maximum peak of tan δ is 50 or more and 500 or less, and in mechanical impedance measurement of the laminated glass in accordance with ISO 16940, the laminated glass has a primary loss factor of 0.15 or more over the entire temperature range of 0°C or more and 40°C or less.

[0043] According to a broad aspect of the present invention, there is provided laminated glass comprising a first laminated glass component, a second laminated glass component, and an interlayer film for laminated glass, and which satisfies the following first feature and the following second feature when a sound transmission loss measurement is carried out including the following first, second, and third steps:

[0044] First configuration: The sound transmission loss at 500 Hz or more and 1000 Hz or less satisfies the following formula (1).

[0045] y≧10.1ln(x)-35...Equation (1)

[0046] In formula (1), x represents frequency (Hz) and y represents sound transmission loss (dB).

[0047] Second configuration: The sound transmission loss in the range of 5000 Hz or more and 10000 Hz or less satisfies the following formula (2).

[0048] y≧12.8ln(x)-68...Equation (2)

[0049] In formula (2), x represents frequency (Hz) and y represents sound transmission loss (dB).

[0050] First step: Prepare a laminated glass sheet that is 500 mm long and 500 mm wide.

[0051] Second step: Prepare a reverberation chamber that is in accordance with ISO 10140-5 and is connected to a first reverberation chamber that is a sound source chamber and a second reverberation chamber that is a sound receiving chamber. Install a laminated glass sheet that is 500 mm long and 500 mm wide between the first reverberation chamber and the second reverberation chamber.

[0052] Third step: The sound transmission loss at 20°C is measured in a center frequency 1 / 3 octave band by the intensity method in accordance with JIS A1441-1. Effect of the Invention

[0053] The interlayer film for laminated glass according to the present invention has a one-layer structure or a two or more-layer structure. The interlayer film for laminated glass according to the present invention has a resin layer. In a viscoelasticity measurement of the interlayer film for laminated glass according to the present invention at a frequency of 1 Hz and in a shear mode, the ratio of the first storage modulus G' at the peak temperature of the maximum peak of tan δ to the second storage modulus G' at a temperature 100°C higher than the peak temperature of the maximum peak of tan δ is 50 or more and 500 or less. Since the interlayer film for laminated glass according to the present invention has the above configuration, it can improve sound insulation over a wide temperature range of 0°C to 40°C. Since the interlayer film for laminated glass according to the present invention has the above configuration, it can also improve sound insulation over a wide temperature range of 0°C to 50°C. When the interlayer film for laminated glass according to the present invention is used in a vehicle or the like, since the interlayer film for laminated glass according to the present invention has the above configuration, it can also improve sound insulation of running noise such as engine noise and road noise.

[0054] The interlayer film for laminated glass according to the present invention has a one-layer structure or a two or more layer structure. The interlayer film for laminated glass according to the present invention has a resin layer. The interlayer film for laminated glass according to the present invention satisfies the first feature and the second feature when a sound transmission loss measurement including the first, second, third, fourth and fifth steps is performed. The interlayer film for laminated glass according to the present invention has the above features, and therefore can improve sound insulation over a wide temperature range of 0°C to 40°C. The interlayer film for laminated glass according to the present invention has the above features, and therefore can also improve sound insulation over a wide temperature range of 0°C to 50°C. When the interlayer film for laminated glass according to the present invention is used in a vehicle or the like, the interlayer film for laminated glass according to the present invention has the above features, and therefore can also improve sound insulation against running noise such as engine noise and road noise.

[0055] The laminated glass according to the present invention comprises a first laminated glass member, a second laminated glass member, and an interlayer film for laminated glass. In the laminated glass according to the present invention, the interlayer film has a one-layer structure or a two or more layer structure. In the laminated glass according to the present invention, the interlayer film comprises a resin layer. In the laminated glass according to the present invention, in a viscoelastic measurement of the interlayer film at a frequency of 1 Hz in a shear mode, the ratio of the first storage modulus G' at the peak temperature of the maximum peak of tan δ to the second storage modulus G' at a temperature 100°C higher than the peak temperature of the maximum peak of tan δ is 50 to 500. In a mechanical impedance measurement of the laminated glass according to the present invention in accordance with ISO 16940, the primary loss factor is 0.15 or more over the entire temperature range of 0°C to 40°C. Since the laminated glass according to the present invention has the above configuration, it can improve sound insulation over a wide temperature range of 0°C to 40°C. The laminated glass of the present invention has the above-mentioned configuration, and therefore can improve sound insulation over a wide temperature range of 0° C. to 50° C. When the laminated glass of the present invention is used in a vehicle or the like, the laminated glass of the present invention has the above-mentioned configuration, and therefore can improve sound insulation against running noises such as engine noise and road noise.

[0056] The laminated glass according to the present invention comprises a first laminated glass member, a second laminated glass member, and an interlayer film for laminated glass. The laminated glass according to the present invention satisfies the first feature and the second feature when a sound transmission loss measurement including the first, second, and third steps is performed. Since the laminated glass according to the present invention has the above features, it can improve sound insulation over a wide temperature range of 0°C to 40°C. Since the laminated glass according to the present invention has the above features, it can also improve sound insulation over a wide temperature range of 0°C to 50°C. When the laminated glass according to the present invention is used in a vehicle or the like, since the laminated glass according to the present invention has the above features, it can also improve sound insulation against running noise such as engine noise and road noise. [Brief description of the drawings]

[0057] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic diagram of an interlayer film for laminated glass according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates a schematic diagram of an interlayer film for laminated glass according to a second embodiment of the present invention. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates an example of laminated glass using the interlayer film for laminated glass shown in FIG. [Figure 4] FIG. 4 is a cross-sectional view that illustrates an example of laminated glass using the interlayer film for laminated glass shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0058] The present invention will be described in detail below.

[0059] (Interlayer film for laminated glass) The interlayer film for laminated glass according to the present invention (hereinafter sometimes referred to as interlayer film) has a one-layer structure or a two or more layer structure. The interlayer film according to the present invention may have a one-layer structure, or a two or more layer structure. The interlayer film according to the present invention comprises a resin layer. The interlayer film according to the present invention may have only one of the above-mentioned resin layers, or may have two or more layers. The interlayer film according to the present invention comprises at least one resin layer. The interlayer film according to the present invention may be a single-layer interlayer film having a single-layer structure, or may be a multi-layer interlayer film having a two or more layer structure.

[0060] In a viscoelastic measurement of the interlayer film of the present invention at a frequency of 1 Hz in a shear mode, the ratio of the first storage modulus G' at the peak temperature of the maximum peak of tan δ to the second storage modulus G' at a temperature 100°C higher than the peak temperature of the maximum peak of tan δ (first storage modulus G' / second storage modulus G') is 50 or more and 500 or less.

[0061] The interlayer film according to the present invention has the above-mentioned configuration, and therefore can improve sound insulation over a wide temperature range from 0°C to 40°C. For example, sound insulation can be improved not at one temperature among 0°C, 10°C, 20°C, 30°C, and 40°C, but at all five of these temperatures. Furthermore, the interlayer film according to the present invention has the above-mentioned configuration, and therefore can improve sound insulation over a wide temperature range from 0°C to 50°C. For example, sound insulation can be improved not at one temperature among 0°C, 10°C, 20°C, 30°C, 40°C, and 50°C, but at all six of these temperatures. Therefore, the interlayer film according to the present invention can exhibit high sound insulation even when laminated glass using the interlayer film is used in various temperature environments.

[0062] From the viewpoint of further improving sound insulation over a wide temperature range and further improving sound insulation against running noise such as engine noise and road noise, the above ratio (first storage modulus G' / second storage modulus G') is preferably at least 60, preferably at most 450, more preferably at most 400, even more preferably at most 300, and particularly preferably at most 250. When the above ratio (first storage modulus G' / second storage modulus G') is at least the above lower limit and at most the above upper limit, sound insulation in the low frequency range of 250 Hz to 1000 Hz is further improved, and engine noise is reduced.

[0063] From the viewpoint of effectively improving the sound insulation over a wide temperature range, the first storage modulus G' is preferably 1×10 5 From the viewpoint of effectively improving the sound insulation property over a wide temperature range, the first storage elastic modulus G′ is preferably 1×10 8 Pa or less, more preferably 1×10 7 When the maximum peak value of tan δ is 2.0 or more and the first storage elastic modulus G' is equal to or more than the lower limit, the sound insulation in the high frequency range of 5000 Hz to 10000 Hz is further improved, and road noise is reduced.

[0064] Specifically, the viscoelasticity measurement is performed as follows. Immediately after storing the test piece for 84 weeks or more in an environment of room temperature 23±2°C and humidity 25±5%, the viscoelasticity is measured using a dynamic viscoelasticity measuring device. The measurement is performed in shear mode under conditions of increasing the temperature from -50°C to 200°C at a heating rate of 3°C / min, at a frequency of 1 Hz, and at a strain of 1%.

[0065] The dynamic viscoelasticity measuring device may be, for example, a viscoelasticity measuring device "DVA-200" manufactured by IT Measurement and Control Co., Ltd.

[0066] For example, if the thickness of the interlayer is 0.3 mm or more and 2 mm or less, the viscoelasticity measurement can be easily performed by directly using the interlayer as a test piece. If the thickness of the interlayer is less than 0.3 mm, the interlayer may be stacked multiple times, or an interlayer with only the thickness adjusted may be separately prepared, and a test piece with a thickness of 0.3 mm or more and 2 mm or less may be used to perform the viscoelasticity measurement. If the thickness of the interlayer exceeds 2 mm, the interlayer may be sliced ​​or pressed, or an interlayer with only the thickness adjusted may be separately prepared, and a test piece with a thickness of 0.3 mm or more and 2 mm or less may be used to perform the viscoelasticity measurement.

[0067] In the case of laminated glass, a test piece for measuring viscoelasticity may be obtained as follows. Two sheets of PET film are prepared. After cooling the laminated glass with liquid nitrogen or the like, the laminated glass member and the interlayer are peeled off. The peeled interlayer is sandwiched between two sheets of PET film to obtain a laminate. The obtained laminate is pressure-bonded in an autoclave, and then stored in an environment of room temperature of 23±2°C and humidity of 25±5% for 84 weeks or more to obtain a test piece.

[0068] From the viewpoint of further improving the sound insulation over a wide temperature range and further improving the sound insulation of running sounds such as engine noise and road noise, the peak temperature of the maximum peak of the tan δ is preferably −30° C. or higher, more preferably −25° C. or higher, and even more preferably −20° C. or higher. From the viewpoint of further improving the sound insulation over a wide temperature range and further improving the sound insulation of running sounds such as engine noise and road noise, the peak temperature of the maximum peak of the tan δ is preferably 20° C. or lower, more preferably 10° C. or lower, and even more preferably 0° C. or lower.

[0069] The maximum peak value of tan δ is preferably 2.0 or more, more preferably 2.2 or more, even more preferably 2.4 or more, even more preferably 2.5 or more, even more preferably 2.6 or more, particularly preferably 2.8 or more, and most preferably 3.0 or more. When the maximum peak value of tan δ is equal to or more than the lower limit, the sound insulation can be effectively improved over a wide temperature range, and the sound insulation of running noise such as engine noise and road noise can be further improved. The upper limit of tan δ at the peak temperature of tan δ is not limited. The maximum peak value of tan δ may be 6 or less.

[0070] From the viewpoint of further improving the sound insulation over a wide temperature range, it is preferable that the laminated glass X obtained through the following first, second and third steps has a primary loss factor of 0.15 or more over the entire temperature range of 0°C or more and 40°C or less, when the mechanical impedance is measured in accordance with ISO 16940.

[0071] From the viewpoint of further improving the sound insulation over a wide temperature range, it is preferable that the laminated glass X obtained through the following first, second and third steps has a primary loss factor of 0.15 or more over the entire temperature range of 0°C or higher and 50°C or lower, when the mechanical impedance is measured in accordance with ISO 16940.

[0072] First step: Prepare an interlayer film having a width of 25 mm and a length of 300 mm. Prepare two pieces of clear float glass conforming to JIS R3202, each having a thickness of 2.0 mm, a width of 25 mm, and a length of 300 mm. The interlayer film is sandwiched between the two pieces of clear float glass to obtain a laminate X.

[0073] Second step: The obtained laminate X is placed in a rubber bag and degassed at a vacuum of 2.6 kPa for 20 minutes. Then, in the degassed state, it is transferred to an oven and held at 90°C for a further 30 minutes, where it is vacuum pressed to pre-press the laminate X.

[0074] Third step: The pre-bonded laminate X is subjected to compression bonding in an autoclave at 135° C. and a pressure of 1.2 MPa for 20 minutes to obtain laminated glass X.

[0075] From the viewpoint of effectively improving sound insulation over a wide temperature range, and from the viewpoint of further improving sound insulation against driving noise such as engine noise and road noise, it is preferable that the following first configuration and the following second configuration are satisfied when a sound transmission loss measurement including the following first, second, third, fourth and fifth steps is performed.

[0076] First configuration: The sound transmission loss at 500 Hz or more and 1000 Hz or less satisfies the following formula (1).

[0077] y≧10.1ln(x)-35...Equation (1)

[0078] In formula (1), x represents frequency (Hz) and y represents sound transmission loss (dB).

[0079] Second configuration: The sound transmission loss in the range of 5000 Hz or more and 10000 Hz or less satisfies the following formula (2).

[0080] y≧12.8ln(x)-68...Equation (2)

[0081] In formula (2), x represents frequency (Hz) and y represents sound transmission loss (dB).

[0082] First step: An interlayer film measuring 500 mm in length and 500 mm in width is prepared. Two sheets of green glass measuring 2 mm in thickness, 500 mm in length and 500 mm in width are prepared. The interlayer film is sandwiched between the two sheets of green glass to obtain a laminate Y.

[0083] Second step: The obtained laminate Y is placed in a rubber bag and degassed at a vacuum of 2.6 kPa for 20 minutes. Then, while still degassed, it is transferred to an oven and held at 90°C for a further 30 minutes to vacuum press and pre-press the laminate Y.

[0084] Third step: The pre-bonded laminate Y is compressed in an autoclave at 135°C and a pressure of 1.2 MPa for 20 minutes, and then stored in an environment of room temperature of 23±2°C and humidity of 25±5% for 84 weeks to obtain laminated glass Y.

[0085] Fourth step: Prepare a reverberation chamber conforming to ISO 10140-5, in which a first reverberation chamber, which is a sound source chamber, and a second reverberation chamber, which is a sound receiving chamber, are connected. The obtained laminated glass Y is installed between the first reverberation chamber and the second reverberation chamber.

[0086] Fifth step: The sound transmission loss at 20°C is measured in a center frequency 1 / 3 octave band by the intensity method in accordance with JIS A1441-1.

[0087] The sound transmission loss at 20° C. in the fifth step can be measured, for example, using a sound transmission loss measuring device manufactured by Rion Co., Ltd., such as "Intensity Probe SI-50, Multichannel Analyzer SA-02."

[0088] The laminated glass Y may be produced by peeling off the interlayer film in the laminated glass from the laminated glass members. For example, the laminated glass may be cooled with liquid nitrogen or the like to peel off the interlayer film from the laminated glass members, and the above-mentioned first, second and third steps may be carried out on the obtained interlayer film to obtain laminated glass Y, and the above-mentioned fourth and fifth steps may be carried out on the obtained laminated glass Y. Furthermore, for example, when the thickness of the laminated glass members of the laminated glass is 2 mm and the size of the laminated glass is 500 mm or more in width and 500 mm or more in length, the center may be cut to a width of 500 mm and a length of 500 mm.

[0089] From the viewpoint of effectively improving sound insulation over a wide temperature range and further improving sound insulation of running sounds such as engine noise and road noise, the intermediate film preferably includes a layer (first resin layer) containing a cured product as the resin layer. From the viewpoint of further improving sound insulation over a wide temperature range and further improving sound insulation of running sounds such as engine noise and road noise, the cured product is preferably a cured product obtained by curing a photocurable compound or a moisture curable compound. From the viewpoint of further improving sound insulation over a wide temperature range and further improving sound insulation of running sounds such as engine noise and road noise, the cured product is preferably a cured product obtained by curing a curable compound having a (meth)acryloyl group.

[0090] The curable compound may be a photocurable compound or a moisture-curable compound, or may be a curable compound having a (meth)acryloyl group. The curable compound having a (meth)acryloyl group may be a photocurable compound, a moisture-curable compound, or a curable compound different from both the photocurable compound and the moisture-curable compound. In general, a curable compound having a (meth)acryloyl group has a (meth)acryloyl group, and is cured by irradiation with light.

[0091] From the viewpoint of improving the curing uniformity of the layer containing the cured product, further improving the sound insulation over a wide temperature range, and further improving the sound insulation of running sounds such as engine noise and road noise, the curable compound is preferably a photocurable compound, and is preferably a curable compound having a (meth)acryloyl group. From the viewpoint of improving the curing uniformity of the layer containing the cured product, further improving the sound insulation over a wide temperature range, and further improving the sound insulation of running sounds such as engine noise and road noise, the cured product is preferably a (meth)acrylic polymer.

[0092] From the viewpoint of further improving sound insulation over a wide temperature range and further improving sound insulation against running noise such as engine noise and road noise, the intermediate film preferably has a layer (second resin layer) containing a resin different from the cured product obtained by curing a photocurable compound, the cured product obtained by curing a moisture curable compound, and the cured product obtained by curing a curable compound having a (meth)acryloyl group as the resin layer. The resin in the second resin layer is different from the cured product obtained by curing a photocurable compound, different from the cured product obtained by curing a moisture curable compound, and different from the cured product obtained by curing a curable compound having a (meth)acryloyl group.

[0093] The interlayer film according to the present invention may have a one-layer structure, a two-layer structure, a two or more layer structure, a three-layer structure, a three or more layer structure, a four-layer structure, a four or more layer structure, a five-layer structure, or a five or more layer structure.

[0094] The interlayer film according to the present invention may include a first layer and a second layer disposed on a first surface side of the first layer. In this case, the first layer is preferably a layer containing the cured product.

[0095] From the viewpoint of effectively enhancing sound insulation and adhesion between layers, the interlayer film according to the present invention may comprise a first layer, a second layer disposed on a first surface side of the first layer, and may further comprise a third layer disposed on a second surface side of the first layer opposite to the first surface side. In this case, it is preferable that the first layer is a layer containing the cured product.

[0096] From the viewpoint of effectively enhancing sound insulation and adhesion between layers, the interlayer film according to the present invention may further comprise a fourth layer disposed on the side of the second layer opposite to the first layer side, and may further comprise a fifth layer disposed on the side of the third layer opposite to the first layer side. In this case, it is preferable that the first layer, the second layer, or the third layer is a layer containing the cured product. It is more preferable that the first layer is a layer containing the cured product.

[0097] From the viewpoint of effectively increasing sound insulation and adhesion between the interlayer film and glass, the layer containing the cured product is preferably not a surface layer in the interlayer film, but is preferably an intermediate layer in the interlayer film, although the layer containing the cured product may be a surface layer in the interlayer film.

[0098] From the viewpoint of increasing the transparency of the laminated glass, the visible light transmittance of the interlayer is preferably 70% or more, more preferably 80% or more, and even more preferably 85% or more.

[0099] The visible light transmittance is measured at a wavelength of 380 to 780 nm using a spectrophotometer (Hitachi High-Technologies Corporation, "U-4100") in accordance with JIS R3211:1998.

[0100] The visible light transmittance of the interlayer may be measured by disposing the interlayer between two pieces of clear glass. The thickness of the clear glass is preferably 2.0 mm.

[0101] Hereinafter, specific embodiments of the present invention will be described with reference to the drawings.

[0102] FIG. 1 is a cross-sectional view that illustrates a schematic diagram of an interlayer film for laminated glass according to a first embodiment of the present invention.

[0103] The interlayer film 11 shown in FIG. 1 is a multi-layer interlayer film having a structure of two or more layers. Specifically, the interlayer film 11 has a three-layer structure. The interlayer film 11 is used to obtain laminated glass. The interlayer film 11 is an interlayer film for laminated glass. The interlayer film 11 includes a first layer 1, a second layer 2, and a third layer 3. The second layer 2 is disposed and laminated on the first surface 1a side of the first layer 1. The third layer 3 is disposed and laminated on the second surface 1b side opposite to the first surface 1a of the first layer 1. The first layer 1 is an intermediate layer. The second layer 2 and the third layer 3 are each a protective layer, and in this embodiment, are surface layers. The first layer 1 is disposed and sandwiched between the second layer 2 and the third layer 3. Therefore, the intermediate film 11 has a multilayer structure in which the second layer 2, the first layer 1, and the third layer 3 are laminated in this order (second layer 2 / first layer 1 / third layer 3).

[0104] In the intermediate film 11, the first layer 1 is preferably a layer containing the above-mentioned cured product. The second layer 2 may be a layer containing the above-mentioned cured product, and the third layer 3 may be a layer containing the above-mentioned cured product.

[0105] Other layers may be disposed between the second layer 2 and the first layer 1, and between the first layer 1 and the third layer 3. It is preferable that the second layer 2 and the first layer 1, and the first layer 1 and the third layer 3 are directly laminated to each other. Examples of the other layers include an adhesive layer.

[0106] FIG. 2 is a cross-sectional view that illustrates a schematic diagram of an interlayer film for laminated glass according to a second embodiment of the present invention.

[0107] The interlayer film 11A shown in FIG. 2 is a multi-layer interlayer film having a structure of two or more layers. Specifically, the interlayer film 11A has a structure of five layers. The interlayer film 11A is used to obtain laminated glass. The interlayer film 11A is an interlayer film for laminated glass. The interlayer film 11A includes a first layer 1A, a second layer 2A, a third layer 3A, a fourth layer 4A, and a fifth layer 5A. The second layer 2A is disposed and laminated on the first surface 1a side of the first layer 1A. The third layer 3A is disposed and laminated on the second surface 1b side opposite to the first surface 1a of the first layer 1A. The fourth layer 4A is disposed and laminated on the side opposite to the first layer 1A side of the second layer 2A. The fifth layer 5A is disposed and laminated on the side opposite to the first layer 1A side of the third layer 3A. The first layer 1A, the second layer 2A, and the third layer 3A are each an intermediate layer. The fourth layer 4A and the fifth layer 5A are each a protective layer, which is a surface layer in this embodiment. The first layer 1A is disposed between the second layer 2A and the third layer 3A and sandwiched therebetween. The laminate of the first layer 1A, the second layer 2A, and the third layer 3A is disposed between the fourth layer 4A and the fifth layer 5A and sandwiched therebetween. Therefore, the intermediate film 11A has a multilayer structure (fourth layer 4A / second layer 2A / first layer 1A / third layer 3A / fifth layer 5A) in which the fourth layer 4A, the second layer 2A, the first layer 1A, the third layer 3A, and the fifth layer 5A are laminated in this order.

[0108] In the intermediate film 11A, the first layer 1A, the second layer 2A or the third layer 3A is preferably a layer containing the above-mentioned cured product, and more preferably the first layer 1A is a layer containing the above-mentioned cured product. The fourth layer 4A may be a layer containing the above-mentioned cured product, and the fifth layer 5A may be a layer containing the above-mentioned cured product.

[0109] In addition, other layers may be disposed between the fourth layer 4A and the second layer 2A, between the second layer 2A and the first layer 1A, between the first layer 1A and the third layer 3A, and between the third layer 3A and the fifth layer 5A. It is preferable that the fourth layer 4A and the second layer 2A, the second layer 2A and the first layer 1A, the first layer 1A and the third layer 3A, and the third layer 3A and the fifth layer 5A are directly laminated to each other. Examples of other layers include an adhesive layer.

[0110] Details of the interlayer film according to the present invention, the resin layer (the layer containing the cured product (first resin layer), the layer containing the resin (second resin layer)), the first layer, the second layer, the third layer, the fourth layer, and the fifth layer, as well as details of each component used in the interlayer film, are described below.

[0111] (Resin layer) The intermediate film includes a resin layer.

[0112] The resin layer includes a resin. Examples of the resin include a cured resin (cured product) and a thermoplastic resin. The thermoplastic resin may be a thermoplastic elastomer. A thermoplastic resin is a resin that softens and exhibits plasticity when heated and solidifies when cooled to room temperature. A thermoplastic elastomer means a resin that softens and exhibits plasticity when heated and solidifies and exhibits rubber elasticity when cooled to room temperature (25°C). Examples of the thermoplastic resin include polyolefin resin, vinyl acetate resin, ethylene-vinyl acetate resin, polyester resin, polyvinyl acetal resin, and modified resins obtained by modifying these resins. The cured resin is a cured product obtained by curing a curable compound. Examples of the curable compound include a photocurable compound, a moisture-curable compound, and a thermosetting compound. The resin may be a cured product obtained by curing a photocurable compound or a moisture-curable compound. The cured product obtained by curing the photocurable compound or the moisture-curable compound may be a thermoplastic resin. A thermoplastic resin other than these may be used. The above-listed thermoplastic resins can be turned into thermoplastic elastomers by adjusting the molecular structure, degree of polymerization, and the like of the resin.

[0113] From the viewpoint of further improving sound insulation over a wide temperature range and further improving sound insulation against running noise such as engine noise and road noise, the interlayer preferably comprises a layer (first resin layer) containing the cured product as the resin layer. The interlayer may comprise only the first resin layer as the resin layer. The interlayer may comprise only one layer (first resin layer) containing the cured product, or may comprise two or more layers.

[0114] The intermediate film preferably includes a layer (second resin layer) containing a resin different from the cured product obtained by curing a photocurable compound, the cured product obtained by curing a moisture-curable compound, and the cured product obtained by curing a curable compound having a (meth)acryloyl group. The second resin layer is a resin layer different from the layer (first resin layer) containing the cured product. The intermediate film may include only the second resin layer as the resin layer. The intermediate film may include only one layer (second resin layer) containing the resin, or may include two or more layers.

[0115] The intermediate film preferably includes a layer containing the cured product (first resin layer) and a layer containing the resin (second resin layer). In this case, the intermediate film may include only one layer of the first resin layer and one layer of the second resin layer, or may include two or more layers of each of the first resin layer and the second resin layer.

[0116] In 100% by weight of the composition for forming the resin layer, the content of the resin is preferably 50% by weight or more, more preferably 60% by weight or more, even more preferably 70% by weight or more, and particularly preferably 80% by weight or more. When the content of the resin is equal to or more than the lower limit, the effect of the present invention can be further enhanced. The content of the resin in 100% by weight of the composition for forming the resin layer may be 100% by weight (total amount).

[0117] <Curable compound and cured product for forming a cured product in the layer containing a cured product (first resin layer)> From the viewpoint of further improving sound insulation over a wide temperature range and further improving sound insulation against running noise such as engine noise and road noise, the intermediate film preferably includes a layer (first resin layer) containing the cured product. The curable compound for forming the cured product in the layer containing the cured product is preferably a photocurable compound or a moisture curable compound. The intermediate film does not necessarily have to include the first resin layer as the resin layer.

[0118] The curable compound is preferably a curable compound having a (meth)acryloyl group, and more preferably a (meth)acrylic polymer. The (meth)acrylic polymer may contain other resin components. The resin component is preferably a polyvinyl acetal resin.

[0119] The (meth)acrylic polymer is preferably a polymer of a polymerizable composition containing a curable compound having a (meth)acryloyl group. The polymerizable composition contains a polymerization component. In order to effectively form the cured product in the layer containing the cured product, the polymerizable composition may contain a photoinitiator. The polymerizable composition may contain an auxiliary agent for promoting the curing reaction together with the photoinitiator. The polymerizable composition may contain a resin component such as a polyvinyl acetal resin. A representative example of the curable compound having a (meth)acryloyl group is a (meth)acrylic acid ester. The (meth)acrylic polymer is preferably a poly(meth)acrylic acid ester.

[0120] In order to effectively obtain the effects of the present invention, the polymerization components preferably contain a (meth)acrylic acid ester having an alicyclic structure, a (meth)acrylic acid ester having a cyclic ether structure, a (meth)acrylic acid ester having an aromatic ring, a (meth)acrylic acid ester having a polar group, or an acyclic (meth)acrylic acid ester having 6 or less carbon atoms in the side chain. By using these preferred (meth)acrylic acid esters, both sound insulation properties and foam suppression performance can be improved in a well-balanced manner.

[0121] Examples of the (meth)acrylic acid ester having an alicyclic structure include isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, and dicyclopentanyl acrylate.

[0122] Examples of the (meth)acrylic acid ester having a cyclic ether structure include glycidyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate glycidyl ether, 3-hydroxypropyl (meth)acrylate glycidyl ether, 4-hydroxybutyl acrylate glycidyl ether, 5-hydroxypentyl (meth)acrylate glycidyl ether, 6-hydroxyhexyl (meth)acrylate glycidyl ether; (3-methyloxetan-3-yl)methyl (meth)acrylate, (3-propyloxetan-3-yl)methyl (meth)acrylate, (3-ethyloxetan-3-yl)methyl (meth)acrylate, (3-butyloxetan-3-yl)methyl (meth)acrylate, (3-ethyloxetan-3-yl)ethyl (meth)acrylate, (3-ethyloxetan-3-yl)propyl (meth)acrylate, (3-ethyloxetan-3-yl)butyl (meth)acrylate, ( 3-Ethyloxetan-3-yl)pentyl (meth)acrylate, (3-Ethyloxetan-3-yl)hexyl (meth)acrylate; Tetrahydrofurfuryl (meth)acrylate, (2,2-dimethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, (2-methyl-2-isobutyl-1,3-dioxolan-4-yl)methyl (meth)acrylate Examples of the acrylate include acrylate, (2-cyclohexyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, tetrahydrofurfuryl alcohol acrylic acid polymer ester, tetrahydro-2H-pyran-2-yl-(meth)acrylate, 2-{1-[(tetrahydro-2H-pyran-2-yl)oxy]-2-methylpropyl}(meth)acrylate, cyclic trimethylolpropane formal acrylate, (meth)acryloylmorpholine, etc. From the viewpoint of effectively obtaining the effects of the present invention, tetrahydrofurfuryl (meth)acrylate and cyclic trimethylolpropane formal acrylate are particularly preferred.

[0123] Examples of the (meth)acrylic acid ester having an aromatic ring include benzyl acrylate and phenoxy polyethylene glycol acrylate.

[0124] Examples of the (meth)acrylic acid ester having a polar group include (meth)acrylic acid esters having a hydroxyl group, an amide group, an amino group, an isocyanate group, a carboxyl group, or the like as the polar group.

[0125] Examples of the (meth)acrylic acid ester having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2-hydroxybutyl (meth)acrylate.

[0126] Examples of (meth)acrylic acid esters having an amide group include N,N-dimethylaminopropyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, (meth)acryloylmorpholine, N-isopropyl(meth)acrylamide, and N-hydroxyethyl(meth)acrylamide.

[0127] Examples of the (meth)acrylic acid ester having an amide group or an amino group include N-dialkylaminoalkyl(meth)acrylamide and N,N-dialkylaminoalkyl(meth)acrylamide.

[0128] Examples of the (meth)acrylic acid ester having an isocyanate group include triallyl isocyanurate and its derivatives.

[0129] Examples of the (meth)acrylic acid ester having a carboxyl group include acrylic acid, ω-carboxy-polycaprolactone monoacrylate, and 2-acryloyloxyethyl succinate.

[0130] The (meth)acrylic acid ester may be a polycarboxylic acid ester having a (meth)acryloyl group. Examples of the polycarboxylic acid ester having a (meth)acryloyl group include 2-acryloyloxyethyl succinate.

[0131] From the viewpoint of effectively obtaining the effects of the present invention, a (meth)acrylic acid ester having a hydroxyl group is preferred, and in particular, 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, or 4-hydroxybutyl (meth)acrylate is preferred.

[0132] Examples of the acyclic (meth)acrylic acid ester having 6 or less carbon atoms in the side chain include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, and butyl (meth)acrylate.

[0133] In order to effectively obtain the effects of the present invention, the content of the acyclic (meth)acrylic acid ester having 8 or more carbon atoms in the side chain is preferably less than 20% by weight based on 100% by weight of the above polymerization components.

[0134] Examples of the (meth)acrylic acid ester include, in addition to the above-mentioned compounds, diethylene glycol monoethyl ether (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-acryloyloxyethyl-2-hydroxypropyl phthalate, 2-acryloyloxyethyl-2-hydroxypropyl phthalate; ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 2,2-bis[4-(acryloxyethoxy)phenyl]propane di(meth)acrylate; trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tri(2-acryloyloxyethyl)phosphate, tetramethylolmethane tri(meth)acrylate, tetramethylolpropane tetra(meth)acrylate, and derivatives thereof.

[0135] The (meth)acrylic acid ester may be used alone or in combination of two or more kinds. The (meth)acrylic polymer may be a homopolymer of the (meth)acrylic acid ester or a copolymer of a polymerization component containing the (meth)acrylic acid ester.

[0136] Specific examples of the photoreaction initiator include 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, bis(η5-2,4-cyclopentadiene), 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl dimethyl ketal, 4-(2 -hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-morpholino(4-thiomethylphenyl)propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone oligomer, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzophenone, o- Methyl benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone, 2,4,6-trimethylbenzophenone, 4-benzoyl-N,N-dimethyl-N-[2-(1-oxo-2-propenyloxy)ethyl]benzenemethanaminium bromide, (4-benzoylbenzyl)trimethylammonium chloride, 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2,4-diethylthioxanthone, 2,Examples of the photoinitiator include 4-dichlorothioxanthone, 1-chloro-4-propoxythioxanthone, 2-(3-dimethylamino-2-hydroxy)-3,4-dimethyl-9H-thioxanthone-9-one mesochloride, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and triphenylmethylium tetrakis(pentafluorophenyl)borate. The photoinitiator may be used alone or in combination of two or more.

[0137] Examples of the auxiliary include triethanolamine, triisopropanolamine, 4,4'-dimethylaminobenzophenone (Michler's ketone), 4,4'-diethylaminobenzophenone, 2-dimethylaminoethylbenzoic acid, ethyl 4-dimethylaminobenzoate, (n-butoxy)ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, 2-ethylhexyl 4-dimethylaminobenzoate, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, etc. The auxiliary may be used alone or in combination of two or more.

[0138] The auxiliary is preferably benzyl dimethyl ketal, 1-hydroxycyclohexyl phenyl ketone, benzoyl isopropyl ether, 4-(2-hydroxyethoxy)-phenyl(2-hydroxy-2-propyl) ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, or triphenylmethylium tetrakis(pentafluorophenyl)borate.

[0139] In 100% by weight of the polymerizable composition, the content of the photoreaction initiator is preferably 0.01% by weight or more, more preferably 0.1% by weight or more, and preferably 10% by weight or less, more preferably 5% by weight or less. When the content of the photoreaction initiator is equal to or more than the lower limit and equal to or less than the upper limit, the photocurability and storage stability are further improved.

[0140] When the curable compound for forming the cured product in the layer containing the cured product is a photocurable compound such as a photocurable compound having a (meth)acryloyl group, it is preferable to use a photocuring device such as an ultraviolet ray irradiation device to cure the photocurable compound. Examples of the ultraviolet ray irradiation device include a box type and a belt conveyor type. Examples of the ultraviolet lamp installed in the ultraviolet ray irradiation device include an ultra-high pressure mercury lamp, a high pressure mercury lamp, a low pressure mercury lamp, a chemical lamp, a metal halide lamp, an excimer lamp, and a UV-LED. The ultraviolet ray lamp is preferably a chemical lamp or a UV-LED.

[0141] When the photocurable compound is irradiated with ultraviolet light to obtain the cured product, the ultraviolet light irradiation amount (cumulative irradiation amount) is preferably 500 mJ or more, more preferably 1000 mJ or more, even more preferably 1500 mJ or more, and particularly preferably 2000 mJ or more. The ultraviolet light irradiation amount (cumulative irradiation amount) is preferably 20000 mJ or less, more preferably 10000 mJ or less, and even more preferably 8000 mJ or less. When the ultraviolet light irradiation amount (cumulative irradiation amount) is the lower limit or more, the amount of unreacted monomer can be reduced. When the ultraviolet light irradiation amount (cumulative irradiation amount) is the lower limit or more, the storage stability of the resin is increased. In addition, the irradiation intensity of the ultraviolet light irradiation is preferably 0.1 mW or more, more preferably 0.5 mW or more, even more preferably 1 mW or more, and particularly preferably 2 mW or more.

[0142] In 100% by weight of the composition for forming the layer containing the cured product, the content of the cured product is preferably 50% by weight or more, more preferably 60% by weight or more, even more preferably 70% by weight or more, and particularly preferably 80% by weight or more. When the content of the cured product is equal to or more than the lower limit, the effect of the present invention can be further enhanced. The content of the cured product in 100% by weight of the composition for forming the layer containing the cured product may be 100% by weight (total amount).

[0143] <Resin in layer (second resin layer) containing a resin different from each of the cured product obtained by curing a photocurable compound, the cured product obtained by curing a moisture curable compound, and the cured product obtained by curing a curable compound having a (meth)acryloyl group> The intermediate film preferably includes a layer (second resin layer) containing a resin different from each of the cured product obtained by curing a photocurable compound, the cured product obtained by curing a moisture curable compound, and the cured product obtained by curing a curable compound having a (meth)acryloyl group. The second resin layer is a resin layer different from the layer (first resin layer) containing the cured product. The intermediate film does not necessarily need to include the second resin layer as the resin layer.

[0144] Examples of the resin contained in the second resin layer include a cured product of a thermosetting compound, a thermoplastic resin, etc. The thermoplastic resin may be a thermoplastic elastomer.

[0145] Thermoplastic resins are resins that soften and exhibit plasticity when heated and solidify when cooled to room temperature. Thermoplastic elastomers are specifically resins that soften and exhibit plasticity when heated and solidify and exhibit rubber elasticity when cooled to room temperature (25°C).

[0146] Examples of the thermoplastic resin include polyvinyl acetal resin, polyester resin, aliphatic polyolefin, polystyrene, ethylene-vinyl acetate copolymer resin, ethylene-acrylic acid copolymer resin, polyurethane resin, ionomer resin, polyvinyl alcohol resin, polyvinyl acetate, etc. Thermoplastic resins other than these may also be used.

[0147] The above-listed thermoplastic resins can be turned into thermoplastic elastomers by adjusting the molecular structure, degree of polymerization, and the like of the resin.

[0148] The surface layer of the interlayer film preferably contains a thermoplastic resin. The second layer and the third layer of the interlayer film having a second layer / first layer / third layer structure preferably contain a thermoplastic resin. The fourth layer and the fifth layer of the interlayer film having a fourth layer / second layer / first layer / third layer / fifth layer structure preferably contain a thermoplastic resin.

[0149] In addition, it is preferable that the second layer and the third layer in the interlayer film having a fourth layer / second layer / first layer / third layer / fifth layer structure each contain a thermoplastic resin.

[0150] From the viewpoint of improving the penetration resistance, the thermoplastic resin is preferably a polyvinyl acetal resin, an ionomer resin, or an ethylene-vinyl acetate copolymer resin. From the viewpoint of further improving the penetration resistance, a polyvinyl acetal resin is preferable.

[0151] The polyvinyl acetal resin can be produced, for example, by acetalizing polyvinyl alcohol (PVA) with an aldehyde. The polyvinyl acetal resin is preferably an acetalized product of polyvinyl alcohol. The polyvinyl alcohol can be obtained, for example, by saponifying polyvinyl acetate. The degree of saponification of the polyvinyl alcohol is generally within the range of 70 to 99.9 mol%.

[0152] The average degree of polymerization of the polyvinyl alcohol (PVA) is preferably 200 or more, more preferably 500 or more, even more preferably 1500 or more, even more preferably 1600 or more, and preferably 5000 or less, more preferably 4000 or less, even more preferably 3500 or less, and particularly preferably 3000 or less. When the average degree of polymerization is equal to or more than the lower limit, the penetration resistance of the laminated glass is further improved. When the average degree of polymerization is equal to or less than the upper limit, the interlayer film is easily formed.

[0153] The average degree of polymerization of the polyvinyl alcohol is determined by a method in accordance with JIS K6726 "Testing method for polyvinyl alcohol".

[0154] The number of carbon atoms in the acetal group contained in the polyvinyl acetal resin is not particularly limited. The aldehyde used in producing the polyvinyl acetal resin is not particularly limited. The number of carbon atoms in the acetal group in the polyvinyl acetal resin is preferably 3 to 5, and more preferably 3 or 4. When the number of carbon atoms in the acetal group in the polyvinyl acetal resin is 3 or more, the glass transition temperature of the interlayer film becomes sufficiently low.

[0155] The aldehyde is not particularly limited. In general, an aldehyde having 1 to 10 carbon atoms is preferably used. Examples of the aldehyde having 1 to 10 carbon atoms include formaldehyde, acetaldehyde, propionaldehyde, n-butylaldehyde, isobutylaldehyde, n-valeraldehyde, 2-ethylbutyraldehyde, n-hexylaldehyde, n-octylaldehyde, n-nonylaldehyde, n-decylaldehyde, formaldehyde, acetaldehyde, and benzaldehyde. Propionaldehyde, n-butylaldehyde, isobutylaldehyde, n-hexylaldehyde, or n-valeraldehyde is preferred, propionaldehyde, n-butylaldehyde, or isobutylaldehyde is more preferred, and n-butylaldehyde is even more preferred. The aldehydes may be used alone or in combination of two or more.

[0156] The hydroxyl group content (hydroxyl group amount) of the polyvinyl acetal resin is preferably 15 mol% or more, more preferably 18 mol% or more, and preferably 40 mol% or less, more preferably 35 mol% or less. When the hydroxyl group content is equal to or more than the lower limit, the adhesive strength of the interlayer film is further increased. When the hydroxyl group content is equal to or less than the upper limit, the flexibility of the interlayer film is increased, making it easier to handle.

[0157] The hydroxyl content of the polyvinyl acetal resin is a molar fraction calculated by dividing the amount of ethylene groups to which hydroxyl groups are bonded by the total amount of ethylene groups in the main chain, and expressed as a percentage. The amount of ethylene groups to which hydroxyl groups are bonded can be measured, for example, in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral."

[0158] The degree of acetylation of the polyvinyl acetal resin is preferably 0.01 mol% or more, more preferably 0.5 mol% or more, and preferably 10 mol% or less, more preferably 2 mol% or less. When the degree of acetylation is equal to or more than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetylation is equal to or less than the upper limit, the moisture resistance of the interlayer film and the laminated glass is increased.

[0159] The degree of acetylation is a molar fraction calculated by dividing the amount of ethylene groups to which acetyl groups are bonded by the total amount of ethylene groups in the main chain, expressed as a percentage. The amount of ethylene groups to which acetyl groups are bonded can be measured, for example, in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral."

[0160] The degree of acetalization of the polyvinyl acetal resin (the degree of butyralization in the case of a polyvinyl butyral resin) is preferably 55 mol% or more, more preferably 60 mol% or more, preferably 75 mol% or less, more preferably 71 mol% or less. When the degree of acetalization is equal to or higher than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetalization is equal to or lower than the upper limit, the reaction time required to produce the polyvinyl acetal resin is shortened.

[0161] The degree of acetalization is determined as follows. First, the amount of ethylene groups to which hydroxyl groups are bonded and the amount of ethylene groups to which acetyl groups are bonded are subtracted from the total amount of ethylene groups in the main chain to determine a value. The obtained value is divided by the total amount of ethylene groups in the main chain to determine a molar fraction. The value expressed as a percentage of this molar fraction is the degree of acetalization.

[0162] The hydroxyl group content (hydroxyl group amount), acetalization degree (butyralization degree), and acetylation degree are preferably calculated from the results measured by a method conforming to JIS K6728 "Testing Method for Polyvinyl Butyral". However, measurements according to ASTM D1396-92 may also be used. When the polyvinyl acetal resin is a polyvinyl butyral resin, the hydroxyl group content (hydroxyl group amount), acetalization degree (butyralization degree), and acetylation degree can be calculated from the results measured by a method conforming to JIS K6728 "Testing Method for Polyvinyl Butyral".

[0163] (tackifier resin) The intermediate film preferably contains a tackifier resin. The layer containing the cured product (first resin layer) preferably contains a tackifier resin. The layer containing the resin (second resin layer) preferably contains a tackifier resin. The first layer preferably contains a tackifier resin. Only one type of tackifier resin may be used, or two or more types may be used in combination.

[0164] Examples of the tackifier resin include styrene resin, terpene resin, and rosin resin. From the viewpoint of improving sound insulation over a wide temperature range while maintaining good haze, the tackifier resin is preferably a styrene resin. The styrene resin is preferably a styrene oligomer. An example of a commercially available product of the styrene oligomer is "YS Resin SX100" manufactured by Yasuhara Chemical Co., Ltd.

[0165] In the resin layer containing a tackifier resin, the content of the tackifier resin relative to 100 parts by weight of the resin excluding the tackifier resin contained in the resin layer is preferably 10 parts by weight or more, more preferably 20 parts by weight or more, even more preferably 30 parts by weight or more, preferably 150 parts by weight or less, more preferably 100 parts by weight or less. When the content of the tackifier resin is equal to or more than the lower limit, sound insulation can be improved over a wide temperature range while maintaining good haze.

[0166] (Plasticizer) The intermediate film preferably contains a plasticizer. From the viewpoint of effectively enhancing sound insulation, the layer containing the cured product (first resin layer) preferably contains a plasticizer. The layer containing the resin (second resin layer) preferably contains a plasticizer. Each of the first, second, third, fourth and fifth layers preferably contains a plasticizer. The use of a plasticizer tends to further increase the adhesive strength between the layers. Only one type of the plasticizer may be used, or two or more types may be used in combination.

[0167] Examples of the plasticizer include paraffin oil, benzoic acid ester plasticizer, organic ester plasticizer, and organic phosphoric acid plasticizer. Examples of the organic ester plasticizer include monobasic organic acid ester and polybasic organic acid ester. Examples of the phosphoric acid plasticizer include organic phosphoric acid plasticizer and organic phosphorous acid plasticizer. The plasticizer is preferably a liquid plasticizer.

[0168] Examples of the paraffin oil include naphthenic process oil, white mineral oil, mineral oil, paraffin wax, and liquid paraffin.

[0169] Commercially available paraffin oils include "Diana Process Oil PW-90" manufactured by Idemitsu Kosan Co., Ltd., "Diana Process Oil PW-100" manufactured by Idemitsu Kosan Co., Ltd., and "Diana Process Oil PW-32" manufactured by Idemitsu Kosan Co., Ltd.

[0170] Examples of the organic ester plasticizer include triethylene glycol di-2-ethylpropanoate, triethylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylhexanoate, triethylene glycol dicaprylate, triethylene glycol di-n-octanoate, triethylene glycol di-n-heptanoate, tetraethylene glycol di-n-heptanoate, dibutyl sebacate, dioctyl azelate, dibutyl carbitol adipate, ethylene glycol di-2-ethylbutyrate, 1,3-propylene glycol di-2-ethylbutyrate, 1,4-butylene glycol di-2-ethylbutyrate, diethylene glycol di-2-ethylbutyrate, diethylene glycol di-2-ethylhexanoate, dipropylene glycol di-2-ethylbutyrate, Examples of suitable plasticizers include triethylene glycol di-2-ethylpentanoate, tetraethylene glycol di-2-ethylbutyrate, diethylene glycol dicaprylate, dibutyl maleate, bis(2-butoxyethyl) adipate, dibutyl adipate, diisobutyl adipate, 2,2-butoxyethoxyethyl adipate, glycol benzoate, 1,3-butylene glycol polyester adipate, dihexyl adipate, dioctyl adipate, hexylcyclohexyl adipate, a mixture of heptyl adipate and nonyl adipate, diisononyl adipate, diisodecyl adipate, heptylnonyl adipate, tributyl citrate, tributyl acetyl citrate, diethyl carbonate, dibutyl sebacate, oil-modified alkyd sebacate, and a mixture of a phosphate ester and an adipate ester. Other organic ester plasticizers may also be used. Adipates other than those mentioned above may also be used.

[0171] When expressed by a structural formula, the organic ester plasticizer includes a diester plasticizer represented by the following formula (1).

[0172] [ka]

[0173] In the above formula (1), R1 and R2 each represent an organic group having 2 to 10 carbon atoms, R3 represents an ethylene group, an isopropylene group or an n-propylene group, and p represents an integer of 3 to 10. In the above formula (1), R1 and R2 each represent an organic group having 5 to 10 carbon atoms, and more preferably an organic group having 6 to 10 carbon atoms.

[0174] The plasticizer preferably includes triethylene glycol di-2-ethylhexanoate (3GO), triethylene glycol di-2-ethylbutyrate (3GH) or triethylene glycol di-2-ethylpropanoate.The plasticizer more preferably includes triethylene glycol di-2-ethylhexanoate or triethylene glycol di-2-ethylbutyrate, and even more preferably includes triethylene glycol di-2-ethylhexanoate.

[0175] In the resin layer, the content of the plasticizer relative to 100 parts by weight of the resin is defined as content (0). The content (0) is preferably 5 parts by weight or more, more preferably 10 parts by weight or more, even more preferably 20 parts by weight or more, and preferably 60 parts by weight or less, more preferably 50 parts by weight or less. When the content (0) is equal to or more than the lower limit, sound insulation can be effectively improved. When the content (0) is equal to or less than the upper limit, the penetration resistance of the laminated glass is further improved.

[0176] In the layer (first resin layer) containing the cured product, the content of the plasticizer relative to 100 parts by weight of the cured product is designated as content (1). The content (1) is preferably 5 parts by weight or more, more preferably 10 parts by weight or more, even more preferably 20 parts by weight or more, preferably 60 parts by weight or less, and more preferably 50 parts by weight or less. When the content (1) is equal to or more than the lower limit, sound insulation can be effectively improved. When the content (1) is equal to or less than the upper limit, the penetration resistance of the laminated glass is further improved.

[0177] In the layer (second resin layer) containing the resin, the content of the plasticizer relative to 100 parts by weight of the resin is designated as content (2). The content (2) is preferably 5 parts by weight or more, more preferably 10 parts by weight or more, even more preferably 20 parts by weight or more, preferably 60 parts by weight or less, and more preferably 50 parts by weight or less. When the content (2) is equal to or more than the lower limit, sound insulation can be effectively improved. When the content of the plasticizer is equal to or less than the upper limit, the penetration resistance of the laminated glass is further improved.

[0178] (Heat-shielding material) The intermediate film may contain a heat-shielding material. The resin layer may contain a heat-shielding material. The layer containing the resin may contain a heat-shielding material. The first, second, third, fourth and fifth layers may each contain a heat-shielding material. Only one type of the heat-shielding material may be used, or two or more types may be used in combination.

[0179] The heat-shielding material may contain at least one component X selected from a phthalocyanine compound, a naphthalocyanine compound, and an anthracyanine compound, or may contain heat-shielding particles. In this case, the heat-shielding material may contain both the component X and the heat-shielding particles.

[0180] The intermediate film may contain at least one component X selected from a phthalocyanine compound, a naphthalocyanine compound, and an anthracyanine compound. The layer containing the cured product may contain the component X. The layer containing the resin may contain the component X. The first, second, third, fourth, and fifth layers may each contain the component X. The component X is a heat-shielding material. Only one type of the component X may be used, or two or more types may be used in combination.

[0181] There is no particular limitation on the above-mentioned component X. As the component X, a conventionally known phthalocyanine compound, naphthalocyanine compound, or anthracyanine compound can be used.

[0182] The component X may be phthalocyanine, a derivative of phthalocyanine, naphthalocyanine, a derivative of naphthalocyanine, an anthracyanine, or a derivative of anthracyanine. The phthalocyanine compound and the derivative of phthalocyanine each preferably have a phthalocyanine skeleton. The naphthalocyanine compound and the derivative of naphthalocyanine each preferably have a naphthalocyanine skeleton. The anthracyanine compound and the derivative of anthracyanine each preferably have an anthracyanine skeleton.

[0183] The component X may contain a vanadium atom or a copper atom. The component X may contain a vanadium atom or a copper atom. The component X may be at least one of a phthalocyanine containing a vanadium atom or a copper atom and a derivative of a phthalocyanine containing a vanadium atom or a copper atom.

[0184] The intermediate film may contain heat-shielding particles. The layer containing the cured product may contain heat-shielding particles. The layer containing the resin may contain heat-shielding particles. The first layer may contain heat-shielding particles. The second layer may contain heat-shielding particles. The third layer may contain heat-shielding particles. The heat-shielding particles are a heat-shielding substance. By using the heat-shielding particles, infrared rays (heat rays) can be effectively blocked. Only one type of the heat-shielding particles may be used, or two or more types may be used in combination.

[0185] As the heat shielding particles, metal oxide particles can be used. As the heat shielding particles, particles formed of a metal oxide (metal oxide particles) can be used.

[0186] Infrared rays, which have wavelengths of 780 nm or more, longer than visible light, have a smaller amount of energy than ultraviolet rays. However, infrared rays have a large thermal effect, and when infrared rays are absorbed by a substance, they are released as heat. For this reason, infrared rays are generally called heat rays. By using the above heat-shielding particles, infrared rays (heat rays) can be effectively blocked. Note that heat-shielding particles refer to particles that can absorb infrared rays.

[0187] Specific examples of the heat shielding particles include metal oxide particles such as aluminum-doped tin oxide particles, indium-doped tin oxide particles, antimony-doped tin oxide particles (ATO particles), gallium-doped zinc oxide particles (GZO particles), indium-doped zinc oxide particles (IZO particles), aluminum-doped zinc oxide particles (AZO particles), niobium-doped titanium oxide particles, sodium-doped tungsten oxide particles, cesium-doped tungsten oxide particles, thallium-doped tungsten oxide particles, rubidium-doped tungsten oxide particles, tin-doped indium oxide particles (ITO particles), tin-doped zinc oxide particles, and silicon-doped zinc oxide particles, as well as lanthanum hexaboride (LaB6) particles. Heat shielding particles other than these may also be used.

[0188] (Metal Salts) The interlayer film may contain at least one metal salt selected from alkali metal salts, alkaline earth metal salts, and magnesium salts (hereinafter, may be referred to as metal salt M). The layer containing the cured product may contain the metal salt M. The layer containing the resin may contain the metal salt M. The first, second, third, fourth, and fifth layers may each contain the metal salt M. The use of the metal salt M makes it easy to control the adhesion between the interlayer film and a laminated glass member such as a glass plate, or the adhesion between each layer in the interlayer film. Only one type of the metal salt M may be used, or two or more types may be used in combination.

[0189] The metal salt M may contain at least one metal selected from the group consisting of Li, Na, K, Rb, Cs, Mg, Ca, Sr, and Ba.

[0190] As the metal salt M, an alkali metal salt of an organic acid having 2 to 16 carbon atoms, an alkaline earth metal salt of an organic acid having 2 to 16 carbon atoms, or a magnesium salt of an organic acid having 2 to 16 carbon atoms can be used.

[0191] Examples of the magnesium salt of a carboxylate having 2 to 16 carbon atoms and the potassium salt of a carboxylate having 2 to 16 carbon atoms include magnesium acetate, potassium acetate, magnesium propionate, potassium propionate, magnesium 2-ethylbutyrate, potassium 2-ethylbutanoate, magnesium 2-ethylhexanoate, and potassium 2-ethylhexanoate.

[0192] (UV protection agent) The interlayer film may contain an ultraviolet shielding agent. The layer containing the cured product may contain an ultraviolet shielding agent. The layer containing the resin may contain an ultraviolet shielding agent. The first, second, third, fourth and fifth layers may each contain an ultraviolet shielding agent. By using an ultraviolet shielding agent, the visible light transmittance is more unlikely to decrease even when the interlayer film and the laminated glass are used for a long period of time. The ultraviolet shielding agent may be used alone or in combination of two or more kinds.

[0193] The ultraviolet shielding agent includes an ultraviolet absorbing agent. The ultraviolet shielding agent is preferably an ultraviolet absorbing agent.

[0194] Examples of the ultraviolet ray shielding agent include ultraviolet ray shielding agents containing metal atoms, ultraviolet ray shielding agents containing metal oxides, ultraviolet ray shielding agents having a benzotriazole structure (benzotriazole compounds), ultraviolet ray shielding agents having a benzophenone structure (benzophenone compounds), ultraviolet ray shielding agents having a triazine structure (triazine compounds), ultraviolet ray shielding agents having a malonic acid ester structure (malonic acid ester compounds), ultraviolet ray shielding agents having an oxalic acid anilide structure (oxalic acid anilide compounds), and ultraviolet ray shielding agents having a benzoate structure (benzoate compounds).

[0195] Examples of the ultraviolet shielding agent containing the metal atom include platinum particles, platinum particles whose surfaces are coated with silica, palladium particles, and palladium particles whose surfaces are coated with silica, etc. It is preferable that the ultraviolet shielding agent is not a heat shielding particle.

[0196] Examples of the ultraviolet shielding agent containing the metal oxide include zinc oxide, titanium oxide, and cerium oxide. Furthermore, the ultraviolet shielding agent containing the metal oxide may be surface-coated. Examples of the surface-coating material of the ultraviolet shielding agent containing the metal oxide include insulating metal oxides, hydrolyzable organic silicon compounds, and silicone compounds.

[0197] The insulating metal oxide includes silica, alumina, zirconia, etc. The insulating metal oxide has a band gap energy of, for example, 5.0 eV or more.

[0198] Examples of ultraviolet screening agents having the above-mentioned benzotriazole structure include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole ("Tinuvin P" manufactured by BASF), 2-(2'-hydroxy-3',5'-di-t-butylphenyl)benzotriazole ("Tinuvin 320" manufactured by BASF), 2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole ("Tinuvin 326" manufactured by BASF), and 2-(2'-hydroxy-3',5'-di-amylphenyl)benzotriazole ("Tinuvin 328" manufactured by BASF).

[0199] Examples of the ultraviolet screening agent having a benzophenone structure include octabenzone ("Chimassorb 81" manufactured by BASF).

[0200] Examples of the ultraviolet screening agent having a triazine structure include "LA-F70" manufactured by ADEKA Corporation and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol ("Tinuvin 1577FF" manufactured by BASF).

[0201] Examples of the ultraviolet screening agent having a malonic acid ester structure include dimethyl 2-(p-methoxybenzylidene)malonate, tetraethyl-2,2-(1,4-phenylenedimethylidene)bismalonate, and 2-(p-methoxybenzylidene)-bis(1,2,2,6,6-pentamethyl-4-piperidinyl)malonate.

[0202] Commercially available ultraviolet screening agents having the above malonic acid ester structure include Hostavin B-CAP, Hostavin PR-25, and Hostavin PR-31 (all manufactured by Clariant).

[0203] Examples of ultraviolet screening agents having the above-mentioned oxalic acid anilide structure include oxalic acid diamides having an aryl group substituted on the nitrogen atom, such as N-(2-ethylphenyl)-N'-(2-ethoxy-5-t-butylphenyl)oxalic acid diamide, N-(2-ethylphenyl)-N'-(2-ethoxy-phenyl)oxalic acid diamide, and 2-ethyl-2'-ethoxy-oxyanilide ("Sanduvor VSU" manufactured by Clariant).

[0204] Examples of the ultraviolet screening agent having a benzoate structure include 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate ("Tinuvin 120" manufactured by BASF).

[0205] (Antioxidants) The intermediate film may contain an antioxidant. The layer containing the cured product may contain an antioxidant. The layer containing the resin may contain an antioxidant. The first, second, third, fourth and fifth layers may each contain an antioxidant. Only one type of antioxidant may be used, or two or more types may be used in combination.

[0206] The antioxidants include phenol-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants. The phenol-based antioxidants are antioxidants having a phenol skeleton. The sulfur-based antioxidants are antioxidants containing sulfur atoms. The phosphorus-based antioxidants are antioxidants containing phosphorus atoms.

[0207] The phenol-based antioxidants include 2,6-di-t-butyl-p-cresol (BHT), butyl hydroxyanisole (BHA), 2,6-di-t-butyl-4-ethylphenol, stearyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2'-methylenebis-(4-methyl-6-butylphenol), 2,2'-methylenebis-(4-ethyl-6-t-butylphenol), 4,4'-butylidene-bis-(3-methyl-6-t-butylphenol), 1,1,3-tris-(2-methyl-hydroxy-5- t-butylphenyl)butane, tetrakis[methylene-3-(3',5'-butyl-4-hydroxyphenyl)propionate]methane, 1,3,3-tris-(2-methyl-4-hydroxy-5-t-butylphenol)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis(3,3'-t-butylphenol)butyric acid glycol ester, and bis(3-t-butyl-4-hydroxy-5-methylbenzenepropanoic acid)ethylenebis(oxyethylene). One or more of these antioxidants are preferably used.

[0208] Examples of the phosphorus-based antioxidant include tridecyl phosphite, tris(tridecyl)phosphite, triphenyl phosphite, trinonylphenyl phosphite, bis(tridecyl)pentaerythritol diphosphite, bis(decyl)pentaerythritol diphosphite, tris(2,4-di-t-butylphenyl)phosphite, bis(2,4-di-t-butyl-6-methylphenyl)ethyl ester phosphorous acid, and 2,2'-methylenebis(4,6-di-t-butyl-1-phenyloxy)(2-ethylhexyloxy)phosphorus, etc. One or more of these antioxidants are preferably used.

[0209] Commercially available examples of the antioxidant include "IRGANOX 245" manufactured by BASF, "IRGAFOS 168" manufactured by BASF, "IRGAFOS 38" manufactured by BASF, "Sumilizer BHT" manufactured by Sumitomo Chemical Co., Ltd., "H-BHT" manufactured by Sakai Chemical Industry Co., Ltd., and "IRGANOX 1010" manufactured by BASF.

[0210] (Other ingredients) The intermediate film, the layer containing the cured product, the layer containing the resin, and the first, second, third, fourth, and fifth layers may each contain additives such as coupling agents, dispersants, surfactants, flame retardants, antistatic agents, pigments, dyes, adhesion regulators other than metal salts, moisture-resistant agents, fluorescent brighteners, and infrared absorbing agents, as necessary. These additives may be used alone or in combination of two or more.

[0211] (Other details of interlayer film for laminated glass) The thickness of the interlayer film is not particularly limited. From the viewpoint of practical use and of sufficiently increasing the penetration resistance and bending rigidity of the laminated glass, the thickness of the interlayer film is preferably 0.1 mm or more, more preferably 0.25 mm or more, and preferably 3 mm or less, more preferably 1.5 mm or less. When the thickness of the interlayer film is equal to or more than the lower limit, the penetration resistance and bending rigidity of the laminated glass are further increased. When the thickness of the interlayer film is equal to or less than the upper limit, the transparency of the interlayer film is further improved.

[0212] The thickness of the interlayer is designated as T. The thickness of the layer containing the cured product (thickness per layer) is preferably 0.005T or more, more preferably 0.010T or more, even more preferably 0.020T or more, and preferably 0.180T or less, more preferably 0.120T or less. When the thickness of the layer containing the cured product (thickness per layer) is equal to or more than the above lower limit and equal to or less than the above upper limit, sound insulation can be further improved over a wide temperature range, and sound insulation against running noise such as engine noise and road noise can be further improved.

[0213] The thickness of the layer containing the resin (thickness per layer) is preferably at least 0.300 T, more preferably at least 0.350 T, even more preferably at least 0.400 T, and preferably at most 0.950 T, more preferably at most 0.900 T. When the thickness of the layer containing the resin (thickness per layer) is at least the above lower limit and at most the above upper limit, sound insulation can be further improved over a wide temperature range, and sound insulation against running noise such as engine noise and road noise can be further improved.

[0214] The thickness of the layer containing the cured product (thickness per layer) is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 20 μm or more, preferably 600 μm or less, more preferably 300 μm or less, even more preferably 150 μm or less, and particularly preferably 100 μm or less. When the thickness of the layer containing the cured product (thickness per layer) is equal to or more than the above lower limit and equal to or less than the above upper limit, sound insulation can be further improved over a wide temperature range, and sound insulation against running noise such as engine noise and road noise can be further improved.

[0215] The thickness of the layer containing the resin (thickness per layer) is preferably 200 μm or more, more preferably 300 μm or more, even more preferably 350 μm or more, and preferably 1000 μm or less, more preferably 850 μm or less. When the thickness of the layer containing the resin (thickness per layer) is equal to or more than the above lower limit and equal to or less than the above upper limit, sound insulation over a wide temperature range can be further improved, and sound insulation against running noise such as engine noise and road noise can be further improved.

[0216] The interlayer film may be an interlayer film having a uniform thickness or an interlayer film having a variable thickness. The cross-sectional shape of the interlayer film may be rectangular or wedge-shaped.

[0217] The method for producing the interlayer film according to the present invention is not particularly limited. Examples of the method for producing the interlayer film according to the present invention include a method in which each layer is formed using each resin composition for forming each layer, and then the obtained layers are laminated, and a method in which each layer is laminated by co-extruding each resin composition for forming each layer using an extruder. A production method using extrusion molding is preferred because it is suitable for continuous production.

[0218] In the case where there are two surface layers, it is preferable that the two surface layers contain the same polyvinyl acetal resin, and it is more preferable that the two surface layers contain the same polyvinyl acetal resin and the same plasticizer, because this provides excellent production efficiency for the interlayer film. It is even more preferable that the two surface layers are formed from the same resin composition, because this provides excellent production efficiency for the interlayer film.

[0219] The intermediate film preferably has an uneven shape on at least one of both surfaces. The intermediate film more preferably has an uneven shape on both surfaces. The method for forming the uneven shape is not particularly limited, and examples thereof include a lip embossing method, an embossing roll method, a calendar roll method, and a profile extrusion method. The embossing roll method is preferred because it can form a large number of uneven embossments that are quantitatively uniform uneven patterns.

[0220] (Laminated glass) The laminated glass according to the present invention includes a first laminated glass member, a second laminated glass member, and the above-mentioned interlayer film for laminated glass. In the laminated glass according to the present invention, the interlayer film for laminated glass is disposed between the first laminated glass member and the second laminated glass member.

[0221] The laminated glass according to the present invention comprises a first laminated glass member, a second laminated glass member, and an interlayer film for laminated glass sandwiched between the first laminated glass member and the second laminated glass member. In the laminated glass according to the present invention, the interlayer film has a one-layer structure or a two or more layer structure and comprises a resin layer.

[0222] In the laminated glass of the present invention, in a viscoelastic measurement of the interlayer film at a frequency of 1 Hz in a shear mode, it is preferable that the ratio of the first storage modulus G' at the peak temperature of the maximum peak of tan δ to the second storage modulus G' at a temperature 100° C. higher than the peak temperature of the maximum peak of tan δ is 50 or more and 500 or less.

[0223] From the viewpoint of further improving the sound insulation over a wide temperature range, the laminated glass according to the present invention preferably has a primary loss factor of 0.15 or more over the entire temperature range of 0°C or more and 40°C or less, in mechanical impedance measurement in accordance with ISO 16940.

[0224] From the viewpoint of further improving the sound insulation over a wide temperature range, the laminated glass according to the present invention preferably has a primary loss factor of 0.15 or more over the entire temperature range of 0°C or more and 50°C or less, in mechanical impedance measurement in accordance with ISO 16940.

[0225] From the viewpoint of further improving sound insulation over a wide temperature range and further improving sound insulation against traveling noise such as engine noise and road noise, it is preferable that the laminated glass according to the present invention satisfies the following first and second features when a sound transmission loss measurement including the following first, second and third steps is performed.

[0226] First configuration: The sound transmission loss at 500 Hz or more and 1000 Hz or less satisfies the following formula (1).

[0227] y≧10.1ln(x)-35...Equation (1)

[0228] In formula (1), x represents frequency (Hz) and y represents sound transmission loss (dB).

[0229] Second configuration: The sound transmission loss in the range of 5000 Hz or more and 10000 Hz or less satisfies the following formula (2).

[0230] y≧12.8ln(x)-68...Equation (2)

[0231] In formula (2), x represents frequency (Hz) and y represents sound transmission loss (dB).

[0232] First step: Prepare a laminated glass sheet that is 500 mm long and 500 mm wide.

[0233] Second step: Prepare a reverberation chamber that is in accordance with ISO 10140-5 and is connected to a first reverberation chamber that is a sound source chamber and a second reverberation chamber that is a sound receiving chamber. Install a laminated glass sheet that is 500 mm long and 500 mm wide between the first reverberation chamber and the second reverberation chamber.

[0234] Third step: The sound transmission loss at 20°C is measured in a center frequency 1 / 3 octave band by the intensity method in accordance with JIS A1441-1.

[0235] In the first step, a laminated glass having a length of 500 mm and a width of 500 mm is prepared in order to measure the sound transmission loss. The laminated glass having a length of 500 mm and a width of 500 mm can be obtained, for example, by cutting the laminated glass. For example, when the thickness of the laminated glass member of the laminated glass is 2 mm and the size of the laminated glass is 500 mm or more in width and 500 mm or more in length, the center may be cut to have a width of 500 mm and a length of 500 mm.

[0236] FIG. 3 is a cross-sectional view that illustrates an example of laminated glass using the interlayer film for laminated glass shown in FIG.

[0237] The laminated glass 31 shown in Fig. 3 includes a first laminated glass member 21, a second laminated glass member 22, and an interlayer film 11. The interlayer film 11 is disposed and sandwiched between the first laminated glass member 21 and the second laminated glass member 22.

[0238] A first laminated glass member 21 is laminated on a first surface 11a of the interlayer film 11. A second laminated glass member 22 is laminated on a second surface 11b opposite to the first surface 11a of the interlayer film 11. The first laminated glass member 21 is laminated on an outer surface 2a of the second layer 2. The second laminated glass member 22 is laminated on an outer surface 3a of the third layer 3.

[0239] FIG. 4 is a cross-sectional view that illustrates an example of laminated glass using the interlayer film for laminated glass shown in FIG.

[0240] 4 includes a first laminated glass member 21, a second laminated glass member 22, and an interlayer film 11A. The interlayer film 11A is disposed and sandwiched between the first laminated glass member 21 and the second laminated glass member 22.

[0241] A first laminated glass member 21 is laminated on a first surface 11a of the interlayer film 11A. A second laminated glass member 22 is laminated on a second surface 11b opposite to the first surface 11a of the interlayer film 11A. The first laminated glass member 21 is laminated on the outer surface 4a of the fourth layer 4. The second laminated glass member 22 is laminated on the outer surface 5a of the fifth layer 5A.

[0242] As described above, the laminated glass according to the present invention includes a first laminated glass component, a second laminated glass component, and an interlayer film, and the interlayer film is the interlayer film for laminated glass according to the present invention. In the laminated glass according to the present invention, the interlayer film is disposed between the first laminated glass component and the second laminated glass component.

[0243] The first laminated glass member is preferably a first glass plate, and the second laminated glass member is preferably a second glass plate.

[0244] Examples of the first and second laminated glass members include glass plates and PET (polyethylene terephthalate) films. The laminated glass includes not only a laminated glass having an intermediate film sandwiched between two glass plates, but also a laminated glass having an intermediate film sandwiched between a glass plate and a PET film or the like. The laminated glass is a laminate including glass plates, and preferably includes at least one glass plate. It is preferable that the first laminated glass member and the second laminated glass member are glass plates or PET films, respectively, and that the laminated glass includes a glass plate as at least one of the first laminated glass member and the second laminated glass member. It is particularly preferable that both the first and second laminated glass members are glass plates.

[0245] The glass plate includes inorganic glass and organic glass. The inorganic glass includes float glass plate, heat absorbing glass plate, heat reflecting glass plate, polished glass plate, patterned glass plate, and lined glass plate. The organic glass is a synthetic resin glass that replaces inorganic glass. The organic glass includes polycarbonate plate and poly(meth)acrylic resin plate. The poly(meth)acrylic resin plate includes polymethyl(meth)acrylate plate.

[0246] The thickness of each of the first laminated glass member and the second laminated glass member is preferably 1 mm or more, preferably 5 mm or less, and more preferably 3 mm or less. When the laminated glass member is a glass plate, the thickness of the glass plate is preferably 0.5 mm or more, more preferably 0.7 mm or more, preferably 5 mm or less, and more preferably 3 mm or less. When the laminated glass member is a PET film, the thickness of the PET film is preferably 0.03 mm or more, and preferably 0.5 mm or less.

[0247] The method for producing the laminated glass is not particularly limited. For example, an interlayer film is sandwiched between the first laminated glass member and the second laminated glass member, and the interlayer film is removed by passing the first laminated glass member and the second laminated glass member through a pressing roll or by placing the first laminated glass member and the second laminated glass member in a rubber bag and suctioning the glass under reduced pressure. Then, the glass is pre-bonded at about 70 to 110°C to obtain a laminate. Next, the laminate is placed in an autoclave or pressed to be pressure-bonded at about 120 to 150°C and a pressure of 1 to 1.5 MPa. In this way, a laminated glass can be obtained. During the production of the laminated glass, each layer in the interlayer film may be laminated.

[0248] The interlayer film and the laminated glass can be used in automobiles, railroad vehicles, aircraft, ships, buildings, etc. The interlayer film and the laminated glass can be used for purposes other than these. The interlayer film and the laminated glass are preferably interlayer films and laminated glasses for vehicles or buildings, and more preferably interlayer films and laminated glasses for vehicles. The interlayer film and the laminated glass can be used for automobile front glass, side glass, rear glass, roof glass, etc. The interlayer film and the laminated glass are preferably used in automobiles. The interlayer film is used to obtain laminated glass for automobiles.

[0249] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0250] The following materials were prepared:

[0251] For polyvinyl acetal resin, the degree of acetalization (degree of butyralization), the degree of acetylation, and the content of hydroxyl groups were measured by a method conforming to JIS K6728 "Testing Method for Polyvinyl Butyral". When measured by ASTM D1396-92, the values ​​were similar to those of the method conforming to JIS K6728 "Testing Method for Polyvinyl Butyral". When the type of acetal is acetoacetal, the degree of acetalization is calculated by measuring the degree of acetylation and the content of hydroxyl groups in the same manner, calculating the molar fraction from the measurement results obtained, and then subtracting the degree of acetylation and the content of hydroxyl groups from 100 mol%.

[0252] (resin) Polyvinyl acetal resin (1) (n-butyl aldehyde used, polymerization degree 1700, hydroxyl group content 33 mol%, acetylation degree 1 mol%, acetalization degree 66 mol%) Polyvinyl acetal resin (2) (n-butyl aldehyde used, polymerization degree 800, hydroxyl group content 31 mol%, acetylation degree 1.5 mol%, acetalization degree 67.5 mol%) Polyvinyl acetal resin (X) (wide distribution PVB) (mixture of 50% by weight of polyvinyl acetal resin (XA) and 50% by weight of polyvinyl acetal resin (XB)) (Polyvinyl acetal resin (XA): n-butyl aldehyde used, polymerization degree 1700, hydroxyl group content 9.6 mol%, acetylation degree 1 mol%, acetalization degree 89.4 mol%, Polyvinyl acetal resin (XB): n-butyl aldehyde used, polymerization degree 1700, hydroxyl group content 13 mol%, acetylation degree 1 mol%, acetalization degree 86 mol%) Polyvinyl acetal resin (Y) (n-butyl aldehyde used, polymerization degree 1700, hydroxyl group content 18 mol%, acetylation degree 8 mol%, acetalization degree 74 mol%)

[0253] (cured product) (Meth)acrylic polymer (1): A polymerizable composition was prepared containing the following components:

[0254] Ethyl acrylate 34 parts by weight Benzyl acrylate 38 parts by weight Hydroxypropyl acrylate 28 parts by weight IRGACURE 184 (BASF) 0.2 parts by weight

[0255] This polymerizable composition was sandwiched between two PET sheets (manufactured by Nippa, thickness 50 μm) that had been subjected to a release treatment on one side, to form a polymerizable composition layer with a thickness of 100 μm. Spacers were placed around the periphery of the two PET sheets. A high-pressure mercury UV lamp was used to irradiate the layer with a dose of 3000 mJ / cm. 2 The polymerizable composition layer was irradiated with ultraviolet light at 400 nm to cure the polymerizable composition through a reaction, thereby forming a (meth)acrylic polymer (1) (a layer of the cured product, thickness 100 μm). IRGACURE 184 is 2,2-dimethoxy-1,2-diphenylethan-1-one.

[0256] (Meth)acrylic polymer (2): A polymerizable composition was prepared containing the following components:

[0257] Isobornyl acrylate 60 parts by weight Cyclic trimethylolpropane formal acrylate 40 parts by weight IRGACURE 184 (BASF) 0.2 parts by weight

[0258] This polymerizable composition was sandwiched between two PET sheets (manufactured by Nippa, thickness 50 μm) that had been subjected to a release treatment on one side, to form a polymerizable composition layer with a thickness of 100 μm. Spacers were placed around the periphery of the two PET sheets. A chemical lamp (FL20SBL, manufactured by Toshiba) was used to irradiate the layer with a dose of 3000 mJ / cm. 2 The polymerizable composition layer was irradiated with ultraviolet light at 400 nm, whereby the polymerizable composition was cured by reaction to form a (meth)acrylic polymer (2) (layer of the cured product, thickness 100 μm). IRGACURE184 is 2,2-dimethoxy-1,2-diphenylethan-1-one.

[0259] (Meth)acrylic polymer (3): A polymerizable composition was prepared containing the following components:

[0260] Isobornyl acrylate 70 parts by weight Cyclic trimethylolpropane formal acrylate 25 parts by weight 4-Hydroxybutyl acrylate 5 parts by weight IRGACURE 184 (BASF) 0.2 parts by weight

[0261] This polymerizable composition was sandwiched between two PET sheets (manufactured by Nippa, thickness 50 μm) that had been subjected to a release treatment on one side, to form a polymerizable composition layer with a thickness of 100 μm. Spacers were placed around the periphery of the two PET sheets. A chemical lamp (FL20SBL, manufactured by Toshiba) was used to irradiate the layer with a dose of 3000 mJ / cm. 2 The polymerizable composition layer was irradiated with ultraviolet light at 400 nm, whereby the polymerizable composition was cured by reaction to form a (meth)acrylic polymer (3) (layer of the cured product, thickness 100 μm). IRGACURE184 is 2,2-dimethoxy-1,2-diphenylethan-1-one.

[0262] (Meth)acrylic polymer (4): A polymerizable composition was prepared containing the following components:

[0263] Benzyl acrylate 9.1 parts by weight Cyclic trimethylolpropane triacrylate 38.2 parts by weight Butyl acrylate 43.6 parts by weight Pentaerythritol tetrakis(3-mercaptobutyrate) 0.23 parts by weight Polyvinyl acetal resin (2) 9.1 parts by weight IRGACURE 184 (BASF) 1.8 parts by weight

[0264] Using this polymerizable composition, a (meth)acrylic polymer (4) (layer of cured product, thickness 860 μm) was formed in the same manner as in the case of the (meth)acrylic polymer (1).

[0265] (Meth)acrylic polymer (A): A polymerizable composition was prepared containing the following components:

[0266] Dimethylaminoethyl acrylate 50 parts by weight Hydroxypropyl acrylate 50 parts by weight IRGACURE 184 (BASF) 0.2 parts by weight

[0267] Using this polymerizable composition, a (meth)acrylic polymer (A) (layer of the cured product, thickness 100 μm) was formed in the same manner as in the case of the (meth)acrylic polymer (1).

[0268] (Meth)acrylic polymer (B): A polymerizable composition was prepared containing the following components:

[0269] Benzyl acrylate 7.6 parts by weight Cyclic trimethylolpropane triacrylate 31.8 parts by weight Butyl acrylate 36.4 parts by weight Pentaerythritol tetrakis(3-mercaptobutyrate) 0.19 parts by weight Polyvinyl acetal resin (2) 24.2 parts by weight IRGACURE 184 (BASF) 1.5 parts by weight

[0270] Using this polymerizable composition, a (meth)acrylic polymer (B) (layer of the cured product, thickness 860 μm) was formed in the same manner as in the case of the (meth)acrylic polymer (1).

[0271] (Plasticizer) Triethylene glycol di-2-ethylhexanoate (3GO)

[0272] (Additives) Additive (1): 9,9-Bis-[4-(2-hydroxyethoxy)phenyl]fluorene

[0273] (Metal salt M) Mg mixture (a 50:50 (by weight) mixture of magnesium 2-ethylbutyrate and magnesium acetate)

[0274] (UV protection agent) Tinuvin 326 (2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole, "Tinuvin 326" manufactured by BASF)

[0275] (Antioxidants) BHT (2,6-di-t-butyl-p-cresol)

[0276] Example 1 Preparation of the first layer: An acrylic polymer (1) (layer containing a cured product, thickness 100 μm) was prepared.

[0277] Creating the second and third layers: The following ingredients were mixed and thoroughly kneaded with a mixing roll to obtain a composition for forming the second and third layers.

[0278] Polyvinyl acetal resin (1) 100 parts by weight Plasticizer (3GO) 35 parts by weight Metal salt M (Mg mixture) in an amount of 70 ppm in the resulting second and third layers An ultraviolet ray blocking agent (Tinuvin 326) in an amount of 0.2% by weight in the resulting second and third layers Antioxidant (BHT) in an amount of 0.2% by weight in the resulting second and third layers

[0279] The obtained composition for forming the second and third layers was extruded using an extruder to obtain the second and third layers (each having a thickness of 380 μm).

[0280] Preparation of the interlayer: The release-treated PET sheet laminated on the first layer was peeled off and attached to the second layer using a roll laminator, and the first layer and the second layer were pressure-bonded to obtain a two-layer laminate. Next, the other release-treated PET sheet laminated on the first layer was peeled off, and the first layer and the third layer were pressure-bonded in the same manner as above, to obtain an interlayer film having a second layer / first layer / third layer structure.

[0281] Preparation of specimens for viscoelastic tests: The obtained interlayer film was cut to a size of 25 mm in width and 300 mm in length. A first PET film and a second PET film were prepared, and the cut interlayer film was sandwiched between the two PET films to obtain a laminate. This laminate was placed in a rubber bag and degassed for 20 minutes at a vacuum degree of 2.6 kPa, and then transferred to an oven in the degassed state, and further held at 90°C for 30 minutes to perform vacuum pressing, thereby pre-bonding the laminate. The pre-bonded laminate was compressed for 20 minutes in an autoclave under conditions of 135°C and a pressure of 1.2 MPa, and then stored in an environment of room temperature of 23±2°C and humidity of 25±5% for 84 weeks or more to obtain a test piece.

[0282] Preparation of laminated glass for sound insulation evaluation: The obtained interlayer film was cut to a size of 25 mm in width and 300 mm in length. Two glass plates (clear float glass, width 25 mm, length 300 mm, and thickness 2 mm) were prepared as the first laminated glass member and the second laminated glass member. The interlayer film was sandwiched between the two glass plates to obtain a laminate. This laminate was placed in a rubber bag and degassed for 20 minutes at a vacuum degree of 2.6 kPa, and then transferred to an oven in the degassed state, and further held at 90°C for 30 minutes to perform vacuum pressing, thereby pre-pressing the laminate. The pre-pressed laminate was pressed for 20 minutes in an autoclave under conditions of 135°C and a pressure of 1.2 MPa to obtain laminated glass.

[0283] Example 2 Preparation of the first layer: The following ingredients were mixed and thoroughly kneaded with a mixing roll to obtain a composition for forming a first layer, which was then press-molded to a thickness of 100 μm to obtain a layer containing a cured product.

[0284] (Meth)acrylic polymer (2) 100 parts by weight Plasticizer (3GO) 20 parts by weight

[0285] Creating the second and third layers: The second and third layers similar to those in Example 1 were prepared.

[0286] Preparation of the interlayer: An interlayer film was obtained in the same manner as in Example 1, except that the obtained first layer and the obtained second and third layers were used.

[0287] Preparation of specimens for viscoelastic tests: A test piece was obtained in the same manner as in Example 1, except that the obtained interlayer film was used.

[0288] Preparation of laminated glass for sound insulation evaluation: A laminated glass was obtained in the same manner as in Example 1, except that the obtained interlayer film was used.

[0289] Example 3 Preparation of the first layer: The following ingredients were mixed and thoroughly kneaded with a mixing roll to obtain a composition for forming a first layer, which was then press-molded to a thickness of 100 μm to obtain a layer containing a cured product.

[0290] (Meth)acrylic polymer (3) 100 parts by weight Plasticizer (3GO) 20 parts by weight

[0291] Creating the second and third layers: The second and third layers similar to those in Example 1 were prepared.

[0292] Preparation of the interlayer: An interlayer film was obtained in the same manner as in Example 1, except that the obtained first layer and the obtained second and third layers were used.

[0293] Preparation of specimens for viscoelastic tests: A test piece was obtained in the same manner as in Example 1, except that the obtained interlayer film was used.

[0294] Preparation of laminated glass for sound insulation evaluation: A laminated glass was obtained in the same manner as in Example 1, except that the obtained interlayer film was used.

[0295] Preparation of laminated glass for sound transmission loss measurements: The obtained interlayer film was cut into a size of 500 mm long and 500 mm wide. Two glass plates (green glass, width 500 mm, length 500 mm, and thickness 2 mm) were prepared as the first laminated glass member and the second laminated glass member. The interlayer film was sandwiched between the two glass plates to obtain a laminate. This laminate was placed in a rubber bag and degassed for 20 minutes at a vacuum degree of 2.6 kPa, and then transferred to an oven while degassed, and further held at 90°C for 30 minutes to perform vacuum pressing, thereby pre-pressing the laminate. The pre-pressed laminate was pressed for 20 minutes in an autoclave under conditions of 135°C and a pressure of 1.2 MPa to obtain a laminated glass, which was then stored for 84 weeks in an environment of room temperature 23±2°C and humidity 25±5%, to obtain a laminated glass for measuring sound transmission loss.

[0296] Example 4 Preparation of the interlayer: A (meth)acrylic polymer (4) (layer containing a cured product, thickness 860 μm) was prepared as an interlayer.

[0297] Preparation of specimens for viscoelastic tests: A test piece was obtained in the same manner as in Example 1, except that the obtained interlayer film was used.

[0298] Preparation of laminated glass for sound insulation evaluation: A laminated glass was obtained in the same manner as in Example 1, except that the obtained interlayer film was used.

[0299] Comparative Example 1 Preparation of the first layer: The following ingredients were mixed and thoroughly kneaded with a mixing roll to obtain a composition for forming a first layer, which was then press-molded to a thickness of 250 μm to obtain a layer containing polyvinyl acetal resin (X).

[0300] Polyvinyl acetal resin (X) 100 parts by weight Plasticizer (3GO) 70 parts by weight

[0301] Creating the second and third layers: The second and third layers similar to those in Example 1 were prepared.

[0302] Preparation of the interlayer: An interlayer film was obtained in the same manner as in Example 1, except that the obtained first layer and the obtained second and third layers were used.

[0303] Preparation of specimens for viscoelastic tests: A test piece was obtained in the same manner as in Example 1, except that the obtained interlayer film was used.

[0304] Preparation of laminated glass for sound insulation evaluation: A laminated glass was obtained in the same manner as in Example 1, except that the obtained interlayer film was used.

[0305] Preparation of laminated glass for sound transmission loss measurements: A laminated glass was obtained in the same manner as in Example 3, except that the obtained interlayer film was used.

[0306] Comparative Example 2 Preparation of the first layer: A (meth)acrylic polymer (A) (layer containing a cured product, thickness 100 μm) was prepared.

[0307] Creating the second and third layers: The second and third layers similar to those in Example 1 were prepared.

[0308] Preparation of the interlayer: An interlayer film was obtained in the same manner as in Example 1, except that the obtained first layer and the obtained second and third layers were used.

[0309] Preparation of specimens for viscoelastic tests: A test piece was obtained in the same manner as in Example 1, except that the obtained interlayer film was used.

[0310] Preparation of laminated glass for sound insulation evaluation: A laminated glass was obtained in the same manner as in Example 1, except that the obtained interlayer film was used.

[0311] Comparative Example 3 Preparation of the first layer: The following ingredients were mixed and thoroughly kneaded with a mixing roll to obtain a composition for forming a first layer, which was then press-molded to a thickness of 100 μm to obtain a layer containing polyvinyl acetal resin (Y).

[0312] Polyvinyl acetal resin (Y) 100 parts by weight Triethylene glycol 60 parts by weight Additive (1) 150 parts by weight

[0313] Creating the second and third layers: The second and third layers similar to those in Example 1 were prepared.

[0314] Preparation of the interlayer: An interlayer film was obtained in the same manner as in Example 1, except that the obtained first layer and the obtained second and third layers were used.

[0315] Preparation of specimens for viscoelastic tests: A test piece was obtained in the same manner as in Example 1, except that the obtained interlayer film was used.

[0316] Preparation of laminated glass for sound insulation evaluation: A laminated glass was obtained in the same manner as in Example 1, except that the obtained interlayer film was used.

[0317] Comparative Example 4 Preparation of the interlayer: An acrylic polymer (B) (layer containing a cured product, thickness 860 μm) was prepared as an intermediate film.

[0318] Preparation of specimens for viscoelastic tests: A test piece was obtained in the same manner as in Example 1, except that the obtained interlayer film was used.

[0319] Preparation of laminated glass for sound insulation evaluation: A laminated glass was obtained in the same manner as in Example 1, except that the obtained interlayer film was used.

[0320] (evaluation) (1) Dynamic viscoelasticity measurement The obtained test pieces for viscoelasticity measurement were measured for dynamic viscoelasticity using a dynamic viscoelasticity measuring device (DVA-200, manufactured by IT Measurement & Control Co., Ltd.) under the conditions of heating from -50°C to 200°C at a heating rate of 3°C / min in shear mode, at a frequency of 1 Hz and a strain of 1%, and the following items were evaluated.

[0321] Peak temperature of the maximum peak of tan δ Maximum peak value of tan δ First storage modulus G' at the peak temperature of the maximum peak of tan δ The second storage modulus G' at a temperature 100°C higher than the peak temperature of the maximum peak of tan δ Ratio (first storage modulus G' / second storage modulus G')

[0322] (2) Primary loss factor (sound insulation) The obtained laminated glass for sound insulation evaluation was subjected to mechanical impedance measurement in accordance with ISO 16940. Specifically, the obtained laminated glass for sound insulation evaluation was vibrated by a vibration generator for damping tests ("Vibrator G21-005D" manufactured by Shinken Co., Ltd.). The vibration characteristics obtained from the vibration were amplified by a mechanical impedance measuring device ("XG-81" manufactured by Rion Co., Ltd.), and the vibration spectrum was analyzed by an FFT spectrum analyzer ("FFT Analyzer SA-01A2" manufactured by Rion Co., Ltd.).

[0323] From the above primary loss coefficient, the sound insulation was judged according to the following criteria.

[0324] [Sound insulation evaluation criteria] ○: Primary loss factor is 0.15 or more ×: Primary loss factor is less than 0.15

[0325] (3) Sound transmission loss In a reverberation chamber conforming to ISO 10140-5, in which a first reverberation chamber, which is a sound source chamber, and a second reverberation chamber, which is a sound receiving chamber, are connected, the laminated glass for measuring sound transmission loss obtained in Example 3 and Comparative Example 1 was installed between the first reverberation chamber and the second reverberation chamber (sound source chamber, sound receiving chamber) conforming to ISO 10140-5. The sound transmission loss was measured at 20°C using a sound transmission loss measuring device "Intensity Probe SI-50, Multichannel Analyzer SA-02" manufactured by Rion. Specifically, the sound transmission loss (dB) conforming to JIS A1441-1 was measured by the intensity method. The center frequency was measured in 1 / 3 octave band.

[0326] From the obtained measured values, it was confirmed whether the following formula (1) and formula (2) were satisfied. In Table 3, "◯" is entered when the following formula (1) and formula (2) were satisfied, and "×" is entered when they were not satisfied.

[0327] y≧10.1×ln(x)-35...Equation (1)

[0328] y≧12.8×ln(x)-68...Equation (2)

[0329] In formula (1) and formula (2), x represents frequency (Hz), and y represents sound transmission loss (dB).

[0330] We also checked the sensation of noise felt inside the car when the car was traveling at 60km / h. In Table 3, if the noise felt inside the car was not unpleasant, we marked it with "O", and if it was unpleasant, we marked it with "X". Note that if the engine noise or road noise was not bothersome, it was considered that the noise was not felt to be unpleasant.

[0331] Details and results are shown in Tables 1 to 3 below. In Tables 1 and 2 below, the metal salt M, the UV shielding agent, and the antioxidant are omitted. In Tables 1 and 2, "E+03" means "×10 3 " and "E+04" is "×10 4 " and "E+05" is "×10 5 " and "E+06" is "×10 6 " and "E+07" is "×10 7 " means.

[0332] [Table 1]

[0333] [Table 2]

[0334] [Table 3] [Explanation of symbols]

[0335] 1,1A…First layer 1a...First surface 1b…Second surface 2,2A…Second layer 2a…Outer surface 3,3A…Third layer 3a…Outer surface 4A…fourth layer 4a…Outer surface 5A…5th layer 5a…Outer surface 11,11A…intermediate film 11a...First surface 11b…Second surface 21...First laminated glass member 22...Second laminated glass member 31, 31A…Laminated glass

Claims

1. An interlayer film for laminated glass having a one-layer structure or a two or more layer structure, The intermediate film comprises a resin layer, In a viscoelastic measurement of the interlayer film at a frequency of 1 Hz in a shear mode, the ratio of a first storage modulus G' at a peak temperature of a maximum peak of tan δ to a second storage modulus G' at a temperature 100° C. higher than the peak temperature of a maximum peak of tan δ is 132 or more and 474 or less, the peak temperature of the maximum peak of tan δ is −4° C. or more and 1.1° C. or less; the maximum peak value of tan δ is 2.1 or more and 3.1 or less; the first storage elastic modulus G' is 1.2 x 10 6 Pa or more and 7.5 x 10 6 Pa or less; The interlayer film for laminated glass, wherein the second storage modulus G' is 2.5 x 10 3 Pa or more and 5.7 x 10 4 Pa ​​or less.

2. The interlayer film for laminated glass according to claim 1 , which is an interlayer film for laminated glass having a structure of two or more layers.

3. 3. The interlayer film for laminated glass according to claim 1 or 2, wherein the laminated glass X obtained through the following first, second, and third steps has a primary loss coefficient of 0.15 or more over the entire temperature range of 0° C. or higher and 40° C. or lower, in mechanical impedance measurement in accordance with ISO 16940: First step: Prepare an interlayer film having a width of 25 mm and a length of 300 mm. Prepare two pieces of clear float glass having a thickness of 2.0 mm, a width of 25 mm, and a length of 300 mm conforming to JIS R3202. The interlayer film is sandwiched between the two pieces of clear float glass to obtain a laminate X. Second step: The obtained laminate X is placed in a rubber bag and degassed at a vacuum degree of 2.6 kPa for 20 minutes. Then, in the degassed state, it is transferred into an oven and further held at 90° C. for 30 minutes to vacuum press and pre-press the laminate X. Third step: The pre-bonded laminate X is subjected to pressure bonding in an autoclave at 135° C. and a pressure of 1.2 MPa for 20 minutes to obtain laminated glass X.

4. 4. The interlayer film for laminated glass according to claim 3, wherein the laminated glass X has a primary loss factor of 0.15 or more over the entire temperature range of 0° C. or more and 50° C. or less, in mechanical impedance measurement of the laminated glass X in accordance with ISO 16940.

5. The intermediate film includes a layer containing a cured product as the resin layer, The interlayer film for laminated glass according to any one of claims 1 to 4, wherein the cured product is a cured product obtained by curing a photocurable compound or a moisture-curable compound.

6. The interlayer film for laminated glass according to claim 5 , wherein the cured product is a cured product obtained by curing a photocurable compound.

7. The intermediate film includes a layer containing a cured product as the resin layer, The interlayer film for laminated glass according to any one of claims 1 to 4, wherein the cured product is a cured product obtained by curing a curable compound having a (meth)acryloyl group.

8. The interlayer film for laminated glass according to any one of claims 1 to 4, wherein the resin layer of the interlayer film is a layer containing a resin different from each of the cured product obtained by curing a photocurable compound, the cured product obtained by curing a moisture-curable compound, and the cured product obtained by curing a curable compound having a (meth)acryloyl group.

9. The intermediate film includes a layer containing the cured product as a first resin layer, The interlayer film for laminated glass according to any one of claims 5 to 7, wherein the interlayer film comprises, as a second resin layer, a layer containing a resin different from each of the cured product obtained by curing a photocurable compound, the cured product obtained by curing a moisture-curable compound, and the cured product obtained by curing a curable compound having a (meth)acryloyl group.

10. The interlayer film for laminated glass according to claim 8 or 9, wherein the resin contained in the resin-containing layer is a polyvinyl acetal resin.

11. The interlayer film for laminated glass according to any one of claims 1 to 10, which satisfies the following first feature and the following second feature when a sound transmission loss measurement including the following first, second, third, fourth, and fifth steps is performed. First configuration: The sound transmission loss at 500 Hz or more and 1000 Hz or less satisfies the following formula (1). y≧10.1×ln(x)-35...Formula (1) In formula (1), x represents frequency (Hz) and y represents sound transmission loss (dB). Second configuration: The sound transmission loss in the range of 5,000 Hz or more and 10,000 Hz or less satisfies the following formula (2). y≧12.8×ln(x)-68...Formula (2) In formula (2), x represents frequency (Hz) and y represents sound transmission loss (dB). First step: Prepare an interlayer film having a length of 500 mm and a width of 500 mm. Prepare two sheets of green glass having a thickness of 2 mm, a length of 500 mm, and a width of 500 mm. The interlayer film is sandwiched between the two sheets of green glass to obtain a laminate Y. Second step: The obtained laminate Y is placed in a rubber bag and degassed at a vacuum degree of 2.6 kPa for 20 minutes. Then, in the degassed state, it is transferred into an oven and further held at 90° C. for 30 minutes to vacuum press and pre-press the laminate Y. Third step: The pre-bonded laminate Y is compressed in an autoclave at 135° C. and a pressure of 1.2 MPa for 20 minutes, and then stored in an environment of room temperature of 23±2° C. and humidity of 25±5% for 84 weeks to obtain laminated glass Y. Fourth step: A reverberation chamber conforming to ISO 10140-5 is prepared, in which a first reverberation chamber serving as a sound source chamber and a second reverberation chamber serving as a sound receiving chamber are connected. The obtained laminated glass Y is placed between the first reverberation chamber and the second reverberation chamber. Fifth step: The sound transmission loss at 20° C. is measured in a center frequency ⅓ octave band by the intensity method in accordance with JIS A1441-1.

12. a first laminated glass member; a second laminated glass member; and The interlayer film for laminated glass according to any one of claims 1 to 11, The laminated glass, wherein the interlayer film for laminated glass is disposed between the first laminated glass member and the second laminated glass member.

13. a first laminated glass member; a second laminated glass member; and and an interlayer film for laminated glass, The intermediate film has a one-layer structure or a two-layer or more layer structure, The intermediate film comprises a resin layer, In a viscoelastic measurement of the interlayer film at a frequency of 1 Hz in a shear mode, the ratio of a first storage modulus G' at a peak temperature of a maximum peak of tan δ to a second storage modulus G' at a temperature 100° C. higher than the peak temperature of a maximum peak of tan δ is 132 or more and 474 or less, the peak temperature of the maximum peak of tan δ is −4° C. or more and 1.1° C. or less; the maximum peak value of tan δ is 2.1 or more and 3.1 or less; the first storage elastic modulus G' is 1.2 x 10 6 Pa or more and 7.5 x 10 6 Pa or less; the second storage elastic modulus G' is 2.5 x 10 3 Pa or more and 5.7 x 10 4 Pa ​​or less; A laminated glass having a primary loss factor of 0.15 or more over the entire temperature range of 0°C or higher and 40°C or lower, as measured by mechanical impedance measurement in accordance with ISO 16940.

Citation Information

Patent Citations

  • Laminar glazing assembly having soundproof effect for automobile

    JP1998177390A

  • Acoustic laminated glazing, acoustic interlayer and method for selecting the interlayer for optimal acoustic damping

    WO2007135317A1

  • Laminate and laminated glass

    WO2016076339A1

  • Intermediate film for laminated glass, and laminated glass

    WO2016158696A1

  • Laminate structures with enhanced damping properties

    WO2017023644A2